Tue Jun 21 11:01:52 2022

Number of Points = 9927

Depth (nm)	Load (N)	Time (s)
0.589515	94.835626	0.000000
0.288674	87.246560	0.005005
0.765876	98.972119	0.010010
0.412130	110.835291	0.015014
0.803340	103.321647	0.020019
0.471132	96.288726	0.025024
0.355350	92.352836	0.030029
0.344272	89.211240	0.035034
-0.088027	85.581142	0.040038
-0.201014	77.410412	0.045043
-0.388769	74.851005	0.050048
-0.392704	56.732617	0.055053
-0.893264	51.093339	0.060058
-1.286379	55.194779	0.065062
-1.588930	27.516945	0.070067
-2.175937	34.965678	0.075072
-2.119864	32.001821	0.080077
-2.555316	27.726587	0.085082
-2.926686	38.187218	0.090086
-3.198005	35.399528	0.095091
-3.410816	39.178659	0.100096
-3.370138	39.092490	0.105101
-3.654625	34.212293	0.110106
-4.424551	48.203701	0.115110
-4.606375	38.900847	0.120115
-4.958240	38.984466	0.125120
-5.015866	39.274708	0.130125
-5.157819	33.782067	0.135130
-5.320341	43.160674	0.140134
-5.264084	40.237633	0.145139
-6.277119	37.269471	0.150144
-6.177845	36.582192	0.155149
-6.509982	36.492838	0.160154
-6.602691	46.488588	0.165158
-6.543243	30.742531	0.170163
-7.330582	42.061183	0.175168
-8.072221	38.139162	0.180173
-8.155502	31.295733	0.185178
-8.355575	41.662287	0.190182
-8.046512	37.493060	0.195187
-8.330507	32.839913	0.200192
-7.981897	35.205915	0.205197
-9.148961	30.494964	0.210202
-9.576557	42.459704	0.215206
-9.190829	23.726861	0.220211
-9.979701	41.222673	0.225216
-9.667018	30.926060	0.230221
-9.681092	28.810313	0.235226
-10.533772	43.305595	0.240230
-10.928961	29.178366	0.245235
-11.129000	40.456591	0.250240
-10.970282	32.445132	0.255245
-11.211452	30.963727	0.260250
-11.944926	39.297088	0.265254
-12.190186	35.068303	0.270259
-12.434644	32.819029	0.275264
-12.548952	38.166627	0.280269
-12.450259	34.199378	0.285274
-12.760976	36.817830	0.290278
-12.458458	31.373340	0.295283
-13.328612	36.264172	0.300288
-13.777951	35.502379	0.305293
-13.689427	32.885190	0.310298
-14.587093	36.979605	0.315302
-14.883503	29.108835	0.320307
-15.294975	26.568922	0.325312
-15.127659	33.319288	0.330317
-15.366625	27.229801	0.335322
-15.759244	41.492409	0.340326
-15.365372	34.681059	0.345331
-15.532646	40.091893	0.350336
-15.734492	31.433693	0.355341
-16.539320	35.770253	0.360346
-17.057393	32.459056	0.365350
-17.026804	28.165649	0.370355
-17.104798	35.361962	0.375360
-17.715749	29.013607	0.380365
-17.523702	30.875499	0.385370
-18.091551	34.299026	0.390374
-18.225299	42.590300	0.395379
-18.869059	37.395852	0.400384
-18.857056	32.511550	0.405389
-18.485810	35.690760	0.410394
-19.202800	42.416684	0.415398
-19.790022	36.545495	0.420403
-20.022091	38.545308	0.425408
-20.346965	33.881764	0.430413
-20.522319	33.652587	0.435418
-20.686260	41.049022	0.440422
-20.129259	25.700687	0.445427
-20.189991	36.136711	0.450432
-20.915829	36.473281	0.455437
-21.199563	37.206683	0.460442
-21.735293	33.514796	0.465446
-21.735173	35.451294	0.470451
-22.974636	38.030559	0.475456
-23.174161	41.523134	0.480461
-22.796272	33.983708	0.485466
-23.187505	39.784263	0.490470
-23.222716	26.566922	0.495475
-23.415139	35.911996	0.500480
-23.492691	42.762117	0.505485
-23.668379	31.542547	0.510490
-24.242860	42.490287	0.515494
-24.578740	39.821231	0.520499
-25.001812	37.002632	0.525504
-25.097453	27.175608	0.530509
-24.747788	30.767461	0.535514
-25.385857	35.838505	0.540518
-25.797617	30.259520	0.545523
-26.058225	32.705098	0.550528
-26.504108	37.300317	0.555533
-26.659519	31.462010	0.560538
-26.798148	36.614526	0.565542
-26.683816	29.706602	0.570547
-27.398992	38.528292	0.575552
-28.027513	37.772889	0.580557
-28.157998	34.421779	0.585562
-28.081156	38.633053	0.590566
-28.104776	32.773314	0.595571
-28.328020	41.864792	0.600576
-28.227280	28.713736	0.605581
-28.547973	28.920855	0.610586
-29.817054	40.992981	0.615590
-29.825582	36.226333	0.620595
-29.942453	35.889792	0.625600
-30.173383	35.226017	0.630605
-29.886625	35.403974	0.635610
-30.089862	42.934790	0.640614
-31.001744	38.034176	0.645619
-31.511206	43.144901	0.650624
-31.610887	39.126440	0.655629
-31.441591	35.186374	0.660634
-31.678305	47.761035	0.665638
-31.565486	30.682632	0.670643
-32.009900	38.185898	0.675648
-33.100580	32.034996	0.680653
-33.285505	31.633554	0.685658
-33.415593	39.825158	0.690662
-33.274394	23.508898	0.695667
-33.557161	27.920815	0.700672
-33.718483	42.228985	0.705677
-33.130325	37.110543	0.710682
-34.398647	39.458382	0.715686
-34.258013	25.911977	0.720691
-34.648291	30.305389	0.725696
-34.772210	39.374891	0.730701
-35.327466	39.139365	0.735706
-36.098817	34.422285	0.740710
-36.115782	31.899329	0.745715
-36.430061	37.744366	0.750720
-36.461985	33.927805	0.755725
-36.180826	33.948033	0.760730
-36.559815	35.617571	0.765734
-36.509022	29.776690	0.770739
-37.124771	28.886369	0.775744
-38.033335	39.139964	0.780749
-37.792477	30.580921	0.785754
-38.400276	46.401984	0.790758
-38.017590	35.058371	0.795763
-37.866372	40.929722	0.800768
-38.461723	36.293804	0.805773
-38.827358	34.029672	0.810778
-39.626861	38.131120	0.815782
-39.524505	34.981604	0.820787
-39.614650	38.881711	0.825792
-40.607871	44.858528	0.830797
-40.388592	42.155748	0.835802
-40.935821	41.286442	0.840806
-40.823700	38.031906	0.845811
-40.800055	31.796513	0.850816
-41.072541	37.580165	0.855821
-41.070215	32.661552	0.860826
-41.952097	36.379807	0.865830
-42.223425	34.021716	0.870835
-42.473235	30.366744	0.875840
-42.758515	37.649875	0.880845
-42.557041	28.062148	0.885850
-42.837888	32.781982	0.890854
-43.763379	35.508167	0.895859
-43.930914	34.328328	0.900864
-44.139625	35.485807	0.905869
-44.003066	34.492013	0.910874
-44.277160	41.440985	0.915878
-44.042974	32.756161	0.920883
-44.389474	31.542617	0.925888
-45.563719	31.066638	0.930893
-45.861198	33.844119	0.935898
-45.865185	44.239965	0.940902
-45.905532	38.494686	0.945907
-45.889884	44.375071	0.950912
-45.963722	37.628350	0.955917
-45.968246	29.991628	0.960922
-46.704754	49.217869	0.965926
-47.259850	34.744759	0.970931
-47.355512	39.664411	0.975936
-47.251133	34.719622	0.980941
-47.529397	32.662034	0.985946
-48.437734	34.671429	0.990950
-48.837360	29.959293	0.995955
-49.251728	29.057724	1.000960
-48.961318	31.958858	1.005965
-48.935903	33.899454	1.010970
-49.474374	26.191124	1.015974
-49.356434	27.208667	1.020979
-49.477521	26.572878	1.025984
-49.469331	26.823410	1.030989
-50.125761	26.955104	1.035994
-50.547199	38.368855	1.040998
-50.840762	28.517385	1.046003
-51.048468	26.567894	1.051008
-51.336885	47.889793	1.056013
-51.684424	36.135498	1.061018
-52.310377	38.334928	1.066022
-52.286248	30.405749	1.071027
-52.511524	36.233481	1.076032
-52.846911	37.374644	1.081037
-52.605519	24.461372	1.086042
-52.668452	34.733575	1.091046
-53.197329	37.419929	1.096051
-53.216013	33.672019	1.101056
-53.803299	36.702327	1.106061
-53.613391	34.397301	1.111066
-54.521189	36.596640	1.116070
-54.993805	26.872702	1.121075
-55.037103	28.797445	1.126080
-55.458393	27.548140	1.131085
-55.088382	31.199371	1.136090
-55.604071	35.315387	1.141094
-55.568234	32.324295	1.146099
-55.669013	38.933764	1.151104
-56.392006	40.302117	1.156109
-56.430595	34.134257	1.161114
-56.715380	33.675552	1.166118
-56.902683	32.124253	1.171123
-57.487684	36.184260	1.176128
-58.055562	39.215894	1.181133
-57.931968	35.171509	1.186138
-58.306333	39.491645	1.191142
-58.060968	25.977230	1.196147
-58.645292	37.320473	1.201152
-59.017919	36.135134	1.206157
-58.915523	42.169673	1.211162
-59.882853	39.112852	1.216166
-59.960801	32.853240	1.221171
-60.351992	33.926882	1.226176
-60.607425	37.875082	1.231181
-60.108870	33.910877	1.236186
-60.192221	34.560776	1.241190
-60.235910	30.371430	1.246195
-60.709975	41.392129	1.251200
-61.374651	40.030988	1.256205
-61.827934	34.580440	1.261210
-62.101353	39.592479	1.266214
-61.785238	34.173954	1.271219
-61.896320	41.388179	1.276224
-62.526991	37.060034	1.281229
-62.983790	34.065677	1.286234
-63.156543	29.643345	1.291238
-63.596305	31.501535	1.296243
-63.586939	36.038134	1.301248
-63.580273	42.109838	1.306253
-64.063620	33.353620	1.311258
-64.599830	40.177084	1.316262
-64.844981	29.513271	1.321267
-65.088075	32.661216	1.326272
-65.213017	30.219092	1.331277
-64.863476	23.331419	1.336282
-65.393306	38.059362	1.341286
-66.020698	27.823130	1.346291
-66.193432	36.471515	1.351296
-66.625730	36.933723	1.356301
-66.428612	34.861144	1.361306
-66.792063	42.473745	1.366310
-67.095059	26.198690	1.371315
-67.605718	35.524834	1.376320
-67.981199	33.583790	1.381325
-67.820729	27.950693	1.386330
-68.298462	32.743390	1.391334
-68.447725	28.829247	1.396339
-68.540132	34.902161	1.401344
-68.662864	27.837945	1.406349
-68.530490	22.934502	1.411354
-69.398909	27.549577	1.416358
-69.652245	22.910899	1.421363
-69.613230	37.776695	1.426368
-70.359399	30.595111	1.431373
-70.585852	29.300909	1.436378
-71.334623	42.674909	1.441382
-70.931044	33.417591	1.446387
-71.080121	34.015821	1.451392
-71.485280	36.810545	1.456397
-71.211666	34.121459	1.461402
-71.359360	41.246435	1.466406
-71.746066	27.901821	1.471411
-72.387720	30.367883	1.476416
-72.755094	33.404988	1.481421
-72.695821	34.183015	1.486426
-73.438416	39.491994	1.491430
-73.323052	37.361126	1.496435
-73.915551	36.579636	1.501440
-74.475460	37.202691	1.506445
-74.437685	36.060878	1.511450
-74.893055	34.464190	1.516454
-74.624008	31.659830	1.521459
-74.875038	43.340768	1.526464
-74.956722	42.434028	1.531469
-74.833821	31.436348	1.536474
-75.379392	36.207722	1.541478
-75.627176	36.584909	1.546483
-76.255401	35.653838	1.551488
-76.426263	33.816645	1.556493
-76.128772	29.748593	1.561498
-76.988111	35.995292	1.566502
-77.486920	27.730827	1.571507
-77.711081	36.392267	1.576512
-77.858032	40.164833	1.581517
-77.965126	29.536173	1.586522
-78.050370	36.900232	1.591526
-78.150548	28.567774	1.596531
-78.421721	39.796798	1.601536
-78.993632	36.271344	1.606541
-79.107155	32.830997	1.611546
-79.647283	35.762922	1.616550
-79.650633	27.948016	1.621555
-79.694824	30.596130	1.626560
-80.045477	32.593878	1.631565
-80.306570	29.832919	1.636570
-80.441471	35.790327	1.641574
-80.947652	30.727226	1.646579
-80.704067	34.552524	1.651584
-81.492693	38.760710	1.656589
-82.055152	32.107548	1.661594
-82.590666	34.131769	1.666598
-82.498038	29.714425	1.671603
-82.800756	30.947267	1.676608
-82.404654	38.725530	1.681613
-82.539027	30.153056	1.686618
-82.646843	39.465962	1.691622
-83.078171	40.118239	1.696627
-83.528081	31.881787	1.701632
-84.007109	39.981404	1.706637
-83.960188	37.752549	1.711642
-84.280720	38.515335	1.716646
-85.307336	36.728901	1.721651
-85.054850	35.040436	1.726656
-85.154054	28.433293	1.731661
-85.503920	31.491179	1.736666
-85.651633	40.579616	1.741670
-85.625655	32.398534	1.746675
-85.825677	35.158692	1.751680
-86.478693	39.912146	1.756685
-86.593140	39.476538	1.761690
-87.190456	41.911976	1.766694
-87.206457	36.979231	1.771699
-87.329341	31.763455	1.776704
-87.447421	36.832449	1.781709
-87.873050	38.129653	1.786714
-88.674108	37.912743	1.791718
-89.047186	34.957606	1.796723
-88.852941	33.046723	1.801728
-89.186207	33.958039	1.806733
-89.418072	32.598629	1.811738
-89.387731	35.370165	1.816742
-89.363606	38.299216	1.821747
-89.436033	34.553893	1.826752
-89.970182	38.058673	1.831757
-90.345676	30.464450	1.836762
-90.600917	35.785461	1.841766
-90.919621	34.437276	1.846771
-90.817251	34.412914	1.851776
-91.579769	39.691649	1.856781
-91.858545	35.010217	1.861786
-92.187269	39.905519	1.866790
-92.072658	28.677942	1.871795
-92.057789	33.175937	1.876800
-92.396913	50.955431	1.881805
-93.178922	39.472799	1.886810
-93.583250	36.619136	1.891814
-93.739267	37.224634	1.896819
-93.997781	36.016847	1.901824
-94.243001	41.490514	1.906829
-93.948136	34.649384	1.911834
-93.942419	42.156049	1.916838
-94.151653	35.577389	1.921843
-94.793981	39.834163	1.926848
-95.153828	36.011532	1.931853
-95.045479	32.032820	1.936858
-96.028990	36.563955	1.941862
-96.524270	26.233234	1.946867
-96.379299	29.034130	1.951872
-96.482052	37.395052	1.956877
-96.796762	29.691703	1.961882
-97.205673	27.728376	1.966886
-97.329388	29.849168	1.971891
-97.266686	37.233320	1.976896
-97.150395	31.757117	1.981901
-97.748957	24.643842	1.986906
-98.327278	31.888677	1.991910
-98.829936	32.746353	1.996915
-98.874371	31.769112	2.006912
-98.640108	35.325559	2.016909
-97.808043	27.737393	2.026906
-97.479333	31.755958	2.036902
-96.716861	35.618315	2.046899
-96.169663	39.845109	2.056896
-95.975140	33.278931	2.066893
-95.900600	32.329821	2.076890
-94.670643	35.474379	2.086886
-94.361414	39.283769	2.096883
-94.041028	39.938245	2.106880
-93.517562	38.889689	2.116877
-93.160448	37.614590	2.126874
-91.940391	37.245155	2.136870
-91.636560	41.566593	2.146867
-91.826730	37.856995	2.156864
-91.279460	41.360221	2.166861
-90.432529	36.561272	2.176858
-89.742645	38.540614	2.186854
-88.950968	43.291223	2.196851
-88.833100	36.171460	2.206848
-88.768103	34.657650	2.216845
-88.169838	43.086136	2.226842
-87.366024	38.091210	2.236838
-86.884852	39.762901	2.246835
-86.000085	39.063114	2.256832
-85.730405	35.670354	2.266829
-85.454037	36.533855	2.276826
-85.443265	40.120009	2.286822
-84.152649	36.208831	2.296819
-84.015211	34.295757	2.306816
-83.285310	37.077781	2.316813
-82.484217	36.240305	2.326810
-82.339972	40.962993	2.336806
-82.467968	35.126564	2.346803
-81.382655	40.137171	2.356800
-80.996835	41.773085	2.366797
-80.243799	37.980578	2.376794
-79.668809	35.354269	2.386790
-79.757779	38.176084	2.396787
-78.889764	37.012574	2.406784
-78.115747	44.614501	2.416781
-78.026446	30.265476	2.426778
-77.239955	32.083001	2.436774
-76.811139	39.897992	2.446771
-76.611817	44.320122	2.456768
-75.749312	44.815266	2.466765
-75.078542	39.072386	2.476762
-74.840729	42.097733	2.486758
-74.850911	39.698743	2.496755
-74.022230	35.815862	2.506752
-73.319610	34.907956	2.516749
-72.223875	34.131147	2.526746
-72.202174	39.705965	2.536742
-71.650127	36.067274	2.546739
-71.385328	38.825363	2.556736
-71.353150	33.962187	2.566733
-70.374069	38.546812	2.576730
-69.962336	33.577506	2.586726
-68.911052	29.828473	2.596723
-68.561302	31.155806	2.606720
-68.348386	37.381810	2.616717
-68.178145	30.556668	2.626714
-67.493318	38.418174	2.636710
-66.972407	33.689228	2.646707
-66.431524	38.676788	2.656704
-65.313806	39.837023	2.666701
-65.271416	37.730842	2.676698
-65.231179	36.329804	2.686694
-64.323129	41.777986	2.696691
-64.053023	40.990318	2.706688
-63.201728	37.141036	2.716685
-62.273468	39.487732	2.726682
-62.102776	39.345640	2.736678
-62.096746	42.442371	2.746675
-61.837942	43.432868	2.756672
-60.762654	36.331776	2.766669
-60.282475	41.860698	2.776666
-59.570630	38.895786	2.786662
-59.401397	44.484703	2.796659
-59.068119	42.656560	2.806656
-58.115042	41.017209	2.816653
-57.742689	36.913130	2.826650
-57.715864	40.484574	2.836646
-56.358199	39.563028	2.846643
-56.123152	43.301525	2.856640
-55.933667	40.918074	2.866637
-55.715358	28.763010	2.876634
-54.770285	28.404746	2.886630
-54.439485	37.380979	2.896627
-53.817015	35.546437	2.906624
-53.077853	35.366314	2.916621
-53.073578	34.727590	2.926618
-52.290762	43.888792	2.936614
-51.721554	46.009247	2.946611
-51.465027	44.077437	2.956608
-50.221822	43.951755	2.966605
-50.231947	39.545090	2.976602
-49.868709	39.043712	2.986598
-49.789439	43.431390	2.996595
-49.100192	42.469786	3.006592
-48.047712	40.622910	3.016589
-47.320396	43.078959	3.026586
-46.870216	37.829432	3.036582
-46.924275	44.658031	3.046579
-46.899568	34.810221	3.056576
-45.880321	32.164480	3.066573
-45.476582	33.959055	3.076570
-44.258350	35.596613	3.086566
-43.852089	31.655855	3.096563
-43.886218	34.512847	3.106560
-43.803792	44.357311	3.116557
-42.917689	35.258351	3.126554
-42.095656	36.246462	3.136550
-41.872193	39.975616	3.146547
-40.675374	29.958000	3.156544
-40.692271	30.373935	3.166541
-40.270770	25.104859	3.176538
-40.155341	23.968977	3.186534
-39.128484	34.481553	3.196531
-38.947070	31.561810	3.206528
-38.299081	31.447964	3.216525
-37.239885	32.961104	3.226522
-37.157566	32.417731	3.236518
-37.223554	38.765800	3.246515
-36.232317	30.988864	3.256512
-35.593512	30.733488	3.266509
-35.433694	38.470333	3.276506
-34.734911	34.663898	3.286502
-34.105517	32.043403	3.296499
-34.026120	31.771404	3.306496
-33.084401	36.358867	3.316493
-32.457045	32.357983	3.326490
-32.617831	30.403803	3.336486
-31.618487	34.054060	3.346483
-31.595292	30.337379	3.356480
-30.842591	28.343556	3.366477
-29.728303	29.939253	3.376474
-29.550525	33.502690	3.386470
-29.576321	32.685783	3.396467
-28.979520	32.458110	3.406464
-28.124840	27.903686	3.416461
-27.856242	36.205393	3.426458
-27.137718	31.642496	3.436454
-26.509547	36.354992	3.446451
-26.399278	33.455330	3.456448
-25.861340	31.586579	3.466445
-24.560993	33.130720	3.476442
-24.334939	30.730742	3.486438
-24.406447	37.758234	3.496435
-24.524090	33.438530	3.506432
-23.360424	31.933248	3.516429
-22.579006	31.586682	3.526426
-21.779378	35.963540	3.536422
-21.823671	35.981333	3.546419
-21.701472	29.723708	3.556416
-20.617796	35.887712	3.566413
-20.281489	31.823194	3.576410
-19.843035	29.733817	3.586406
-18.482237	34.761456	3.596403
-18.568582	32.916660	3.606400
-18.137432	26.866314	3.616397
-18.131856	29.374513	3.626394
-17.313023	28.355098	3.636390
-16.842186	28.394478	3.646387
-16.141043	32.322135	3.656384
-15.511106	36.021518	3.666381
-15.178051	36.899743	3.676378
-14.788961	37.648952	3.686374
-13.808834	44.344227	3.696371
-13.490971	38.175908	3.706368
-13.620443	40.892006	3.716365
-13.269296	41.873536	3.726362
-12.247826	37.125717	3.736358
-11.285000	31.670376	3.746355
-10.891518	41.133166	3.756352
-10.667106	38.048431	3.766349
-10.599971	35.899029	3.776346
-9.953639	34.300607	3.786342
-8.775868	34.928497	3.796339
-8.916123	37.022998	3.806336
-8.084961	36.263936	3.816333
-7.341491	28.580396	3.826330
-7.106144	29.729094	3.836326
-6.969283	34.222625	3.846323
-6.064041	29.685517	3.856320
-5.588290	37.362341	3.866317
-5.420648	38.086971	3.876314
-4.467162	26.686452	3.886310
-4.717234	34.889113	3.896307
-3.692923	32.631786	3.906304
-2.902411	37.199051	3.916301
-2.766504	34.825857	3.926298
-2.467021	39.901023	3.936294
-2.036081	49.906114	3.946291
-1.737637	69.034350	3.956288
-1.117667	82.796474	3.966285
-0.256636	92.187207	3.976282
-0.033097	101.643996	3.986278
0.000000	128.911485	3.991283
0.258501	121.496967	3.996288
0.416946	135.003391	4.001293
0.352845	143.504595	4.006298
0.768183	139.369443	4.011302
0.801675	144.741147	4.016307
0.769870	140.733519	4.021312
1.073098	154.695309	4.026317
1.142388	155.672177	4.031322
1.188260	154.426992	4.036326
0.786387	162.525930	4.041331
1.353610	172.052935	4.046336
1.173670	167.874272	4.051341
0.971059	153.953021	4.056346
1.212557	163.996512	4.061350
1.211343	173.066100	4.066355
1.630947	165.667112	4.071360
1.037938	157.273120	4.076365
0.832015	162.109049	4.081370
1.430774	170.502868	4.086374
1.206824	173.897100	4.091379
1.681416	173.603309	4.096384
1.273296	167.522634	4.101389
0.739487	160.812755	4.106394
1.358623	168.684801	4.111398
1.603611	177.594431	4.116403
1.689214	173.024287	4.121408
1.053370	167.545502	4.126413
1.145896	166.225299	4.131418
1.155891	168.538074	4.136422
1.189340	186.435216	4.141427
1.584207	177.854336	4.146432
1.481072	185.110136	4.151437
1.539530	183.966860	4.156442
1.496937	187.996673	4.161446
1.453743	188.143828	4.166451
1.332921	186.093295	4.171456
1.275991	187.562894	4.176461
1.324979	184.153218	4.181466
1.855979	185.620769	4.186470
1.446823	183.665936	4.191475
1.740220	185.685904	4.196480
1.661526	183.387844	4.201485
1.323461	179.157219	4.206490
1.680846	181.358794	4.211494
1.436990	184.878081	4.216499
1.904217	176.574709	4.221504
1.736202	186.278731	4.226509
1.518037	180.905810	4.231514
1.706817	176.249512	4.236518
1.466929	176.312615	4.241523
1.602408	176.370981	4.246528
1.908296	186.945311	4.251533
1.629120	174.964877	4.256538
1.529012	169.325939	4.261542
1.597577	178.111062	4.266547
1.769702	181.115683	4.271552
1.785799	190.157353	4.276557
1.672775	187.793542	4.281562
1.935389	184.055448	4.286566
1.395616	186.380135	4.291571
1.788869	183.120059	4.296576
1.283329	191.728136	4.301581
1.362046	188.325770	4.306586
1.946018	179.827042	4.311590
1.864257	190.161869	4.316595
1.713685	189.732631	4.321600
1.835545	189.019701	4.326605
1.873163	184.304960	4.331610
1.590884	193.641330	4.336614
1.430248	196.319019	4.341619
1.699300	179.950238	4.346624
2.146911	189.546395	4.351629
1.750274	186.833302	4.356634
1.780332	190.698545	4.361638
1.703070	188.466157	4.366643
1.746977	187.643986	4.371648
1.784621	200.783104	4.376653
1.979735	208.576400	4.381658
2.203041	203.688625	4.386662
2.311701	209.875329	4.391667
2.297616	190.520386	4.396672
2.080483	193.169936	4.401677
2.091737	186.864503	4.406682
1.933257	186.275155	4.411686
1.646292	189.929652	4.416691
2.190157	194.912369	4.421696
2.098820	207.296142	4.426701
2.043808	206.817532	4.431706
2.414229	203.646876	4.436710
2.099512	195.671502	4.441715
1.948813	182.652723	4.446720
2.021589	197.199332	4.451725
2.153721	209.998393	4.456730
2.134095	209.901686	4.461734
2.151942	212.779125	4.466739
2.342986	205.011654	4.471744
2.370876	203.216116	4.476749
2.107748	210.691810	4.481754
2.443765	205.012212	4.486758
2.264397	217.859114	4.491763
2.166160	205.550125	4.496768
2.268114	201.448896	4.501773
2.011211	207.800328	4.506778
2.115240	209.182298	4.511782
2.152501	212.038367	4.516787
2.085221	212.574709	4.521792
2.164720	218.532008	4.526797
2.069114	221.408502	4.531802
2.542429	208.355828	4.536806
2.372557	216.399010	4.541811
2.474029	205.039877	4.546816
2.260635	211.289385	4.551821
1.973825	217.264523	4.556826
2.335053	209.172471	4.561830
2.092377	216.014493	4.566835
2.429907	212.834877	4.571840
2.462449	216.131390	4.576845
2.402011	218.123524	4.581850
2.554649	220.620677	4.586854
2.111988	228.210175	4.591859
2.653424	233.679936	4.596864
3.018981	241.396479	4.601869
2.656501	228.145145	4.606874
2.398087	218.573466	4.611878
2.298841	227.283593	4.616883
2.711747	230.675582	4.621888
2.646462	219.881594	4.626893
2.265605	229.043881	4.631898
2.821779	232.313675	4.636902
2.726377	249.258574	4.641907
2.811457	240.688901	4.646912
2.725609	223.029072	4.651917
2.410700	231.637571	4.656922
2.576956	212.543805	4.661926
2.612285	235.581271	4.666931
2.879142	238.516343	4.671936
2.867985	241.246445	4.676941
2.637872	238.317508	4.681946
3.031111	222.942816	4.686950
2.280699	222.661651	4.691955
2.759543	232.225233	4.696960
2.904009	238.797532	4.701965
2.719013	243.236535	4.706970
2.954209	243.979324	4.711974
3.055604	243.600910	4.716979
2.962508	232.449210	4.721984
2.566043	222.123480	4.726989
2.870209	234.989978	4.731994
2.933224	241.001126	4.736998
2.948053	253.882401	4.742003
2.856161	239.628383	4.747008
2.951026	236.682927	4.752013
2.965683	235.125392	4.757018
2.923959	214.194340	4.762022
2.992577	233.444167	4.767027
3.073169	227.841194	4.772032
2.700841	225.037241	4.777037
2.620244	238.081123	4.782042
3.023222	239.583496	4.787046
3.008960	248.294560	4.792051
2.958750	253.000144	4.797056
3.252792	241.586993	4.802061
3.032136	254.364591	4.807066
3.068136	240.920175	4.812070
2.672048	248.234383	4.817075
2.830898	254.741160	4.822080
3.318206	242.536657	4.827085
3.016812	248.559806	4.832090
3.379959	242.675800	4.837094
2.939207	249.286209	4.842099
2.990468	241.794457	4.847104
3.134607	244.070032	4.852109
2.829978	249.883161	4.857114
2.768666	233.068194	4.862118
2.976858	249.165979	4.867123
3.010001	245.482052	4.872128
3.252945	244.710785	4.877133
2.983202	242.716479	4.882138
3.155436	244.281533	4.887142
3.263406	249.917012	4.892147
3.314559	257.286418	4.897152
3.367539	254.539113	4.902157
3.054145	258.613986	4.907162
3.267894	249.677269	4.912166
3.182216	267.545095	4.917171
3.583079	269.696266	4.922176
3.774670	266.854373	4.927181
3.234612	265.128409	4.932186
3.169219	241.078600	4.937190
3.499661	254.712148	4.942195
3.586097	252.075928	4.947200
3.426021	247.512899	4.952205
3.334453	252.257498	4.957210
3.487088	241.979946	4.962214
3.219724	244.369842	4.967219
3.058595	258.655687	4.972224
3.027651	268.360742	4.977229
3.581831	274.974730	4.982234
3.483018	267.691340	4.987238
3.517095	278.567477	4.992243
3.491708	266.112386	4.997248
3.650103	269.473713	5.002253
3.427753	271.398537	5.007258
3.587644	254.919487	5.012262
3.753587	275.601889	5.017267
3.527199	269.584221	5.022272
3.626270	266.657797	5.027277
3.614992	275.320824	5.032282
3.664625	264.863768	5.037286
3.074498	278.292011	5.042291
3.332630	272.402099	5.047296
3.490890	275.967692	5.052301
3.412721	278.942740	5.057306
3.766690	274.505136	5.062310
3.114395	274.769142	5.067315
3.397689	287.308208	5.072320
3.803470	296.707313	5.077325
3.980744	300.222206	5.082330
4.183100	288.099783	5.087334
3.886957	279.134807	5.092339
3.721053	282.442884	5.097344
3.694830	277.645347	5.102349
3.676942	269.802527	5.107354
3.699031	259.862319	5.112358
3.638226	276.468416	5.117363
4.017160	290.119026	5.122368
3.784967	282.353721	5.127373
3.727525	297.058938	5.132378
4.029970	295.280873	5.137382
4.085066	288.368829	5.142387
4.058681	291.485675	5.147392
4.309244	279.810726	5.152397
3.961964	274.518552	5.157402
3.784477	270.452923	5.162406
3.819449	268.151814	5.167411
3.906513	270.316075	5.172416
4.132662	265.918782	5.177421
3.779208	278.607488	5.182426
3.652672	266.998351	5.187430
3.984923	285.880560	5.192435
4.063484	289.427387	5.197440
4.230812	293.951917	5.202445
3.801867	290.019488	5.207450
4.431914	284.572176	5.212454
4.300308	277.448726	5.217459
3.932116	266.457209	5.222464
3.637614	272.581249	5.227469
3.895483	290.415496	5.232474
4.448224	289.628446	5.237478
4.127201	304.620437	5.242483
4.183741	303.509438	5.247488
4.498346	296.409769	5.252493
4.041731	286.472447	5.257498
4.074661	282.471033	5.262502
3.946522	283.515531	5.267507
4.194903	295.916330	5.272512
4.411432	302.899418	5.277517
4.211623	299.425539	5.282522
4.392142	299.300819	5.287526
4.355470	305.223320	5.292531
4.029615	294.307259	5.297536
4.027127	303.710830	5.302541
3.947381	305.560341	5.307546
4.228222	299.452548	5.312550
4.164765	308.255265	5.317555
3.939400	307.395784	5.322560
4.143863	302.626146	5.327565
4.004154	299.473050	5.332570
4.139177	295.433414	5.337574
3.955882	303.682120	5.342579
4.461026	326.125886	5.347584
4.493431	329.630439	5.352589
4.144363	330.560366	5.357594
4.616727	332.059152	5.362598
4.465399	334.688554	5.367603
4.593976	328.911441	5.372608
4.662466	327.588298	5.377613
4.320716	321.583399	5.382618
4.405259	313.828577	5.387622
4.366563	322.817040	5.392627
4.296571	331.614143	5.397632
4.542273	331.139999	5.402637
4.507606	334.343671	5.407642
4.881185	332.148296	5.412646
4.860776	333.557198	5.417651
4.886740	335.957735	5.422656
4.874911	310.948180	5.427661
4.504245	319.678244	5.432666
4.674183	302.677695	5.437670
4.458795	307.149967	5.442675
4.344706	312.788300	5.447680
4.507843	315.675640	5.452685
4.395590	333.868022	5.457690
4.935608	325.201062	5.462694
4.476667	321.982621	5.467699
4.547459	329.630211	5.472704
4.737681	332.699355	5.477709
4.637775	342.089283	5.482714
4.838649	326.141704	5.487718
4.769416	343.376207	5.492723
4.794362	332.621268	5.497728
4.972408	329.854818	5.502733
4.675172	334.366701	5.507738
4.728199	335.702269	5.512742
4.963521	335.618991	5.517747
5.004975	337.555392	5.522752
5.251168	326.754347	5.527757
4.832337	330.178122	5.532762
5.211309	322.688896	5.537766
4.706179	315.961373	5.542771
4.896948	322.994123	5.547776
4.648304	322.577766	5.552781
4.506386	339.067713	5.557786
5.001532	330.332206	5.562790
4.794234	340.441054	5.567795
4.993498	331.406441	5.572800
5.134049	335.926341	5.577805
5.217746	335.205713	5.582810
5.385307	331.073062	5.587814
5.022961	331.030740	5.592819
4.984907	324.985810	5.597824
5.281756	326.578584	5.602829
4.732882	323.505475	5.607834
4.857683	323.450366	5.612838
5.009174	321.937455	5.617843
4.634970	327.720890	5.622848
5.105523	320.462973	5.627853
5.040140	328.347814	5.632858
4.951808	323.076482	5.637862
4.799060	331.371057	5.642867
4.819440	327.533920	5.647872
4.818122	331.330393	5.652877
4.564228	328.965023	5.657882
4.797665	343.559955	5.662886
5.070252	356.670364	5.667891
5.155833	363.639643	5.672896
5.129496	364.126388	5.677901
5.256031	370.391104	5.682906
5.361046	364.529868	5.687910
5.260668	367.923807	5.692915
4.967813	362.921358	5.697920
5.447838	360.482993	5.702925
4.925436	370.658644	5.707930
5.305156	358.841282	5.712934
5.181128	364.519562	5.717939
5.085723	361.656702	5.722944
5.361562	360.894388	5.727949
4.897242	367.101051	5.732954
5.409935	359.897508	5.737958
5.133989	364.103356	5.742963
5.368337	374.443977	5.747968
5.867325	377.144286	5.752973
5.469337	377.424591	5.757978
5.773676	364.154676	5.762982
5.466634	361.474865	5.767987
5.386968	371.510106	5.772992
5.345339	359.380078	5.777997
5.132353	374.590655	5.783002
5.194975	367.779748	5.788006
5.251879	379.855537	5.793011
5.358726	388.153529	5.798016
5.786523	388.165068	5.803021
5.676676	396.640439	5.808026
6.075455	390.136166	5.813030
5.766509	376.920438	5.818035
5.469239	369.339916	5.823040
5.531927	361.469300	5.828045
5.376223	368.810853	5.833050
5.706310	377.238226	5.838054
5.224320	377.305702	5.843059
5.354736	383.123010	5.848064
6.294101	388.622047	5.853069
5.819073	389.641114	5.858074
5.534980	387.336780	5.863078
5.829890	388.354644	5.868083
5.889940	391.829768	5.873088
5.971834	381.380710	5.878093
5.425000	372.656307	5.883098
5.484387	368.829276	5.888102
5.707567	385.227633	5.893107
5.638068	389.762796	5.898112
6.204890	392.892134	5.903117
5.609165	396.257007	5.908122
6.050278	385.679392	5.913126
5.757751	383.374088	5.918131
5.711128	396.382876	5.923136
6.217918	390.779717	5.928141
5.852460	388.100694	5.933146
5.623628	362.776914	5.938150
5.884751	383.673992	5.943155
5.690621	390.763407	5.948160
5.835440	384.343816	5.953165
5.680510	395.624105	5.958170
5.880083	391.875286	5.963174
5.798732	395.197013	5.968179
5.846568	398.967010	5.973184
6.204101	399.040901	5.978189
6.080068	403.127078	5.983194
5.787156	395.333092	5.988198
6.179525	395.345170	5.993203
5.791027	394.345554	5.998208
6.306405	392.985106	6.003213
5.658223	397.546835	6.008218
6.045634	391.331767	6.013222
6.477459	394.508917	6.018227
5.742950	400.462751	6.023232
6.103596	396.778822	6.028237
5.700777	399.903166	6.033242
5.889167	395.205821	6.038246
6.090543	399.589766	6.043251
5.944586	403.663589	6.048256
6.113253	396.258291	6.053261
5.831631	398.838041	6.058266
6.004154	399.968527	6.063270
5.976892	403.134282	6.068275
5.957546	406.128424	6.073280
5.955661	392.890645	6.078285
6.087307	403.235268	6.083290
6.245927	398.592186	6.088294
5.944564	404.559741	6.093299
6.024810	397.885616	6.098304
6.334823	397.429435	6.103309
6.111797	401.329931	6.108314
6.092349	392.016946	6.113318
5.899732	400.967795	6.118323
5.749294	397.773831	6.123328
6.173136	392.277156	6.128333
5.725841	397.926493	6.133338
6.051069	394.226526	6.138342
5.927592	396.513288	6.143347
5.960468	400.582163	6.148352
6.470593	395.358720	6.153357
6.180093	395.411851	6.158362
6.207801	398.684142	6.163366
6.268757	400.788610	6.168371
6.304923	396.677503	6.173376
6.266534	376.442675	6.178381
5.963745	374.666751	6.183386
5.754170	372.886441	6.188390
5.915122	367.264980	6.193395
6.159827	378.210304	6.198400
5.894745	361.161156	6.203405
5.921296	372.576349	6.208410
6.041946	380.091780	6.213414
6.014382	377.963616	6.218419
5.808051	383.728548	6.223424
6.114146	379.941569	6.228429
5.804829	396.684065	6.233434
5.796173	399.456996	6.238438
6.281310	396.945159	6.243443
6.204506	386.348918	6.248448
6.291716	393.726232	6.253453
5.855200	385.918931	6.258458
5.879216	371.780181	6.263462
5.866850	375.701830	6.268467
5.864774	384.482191	6.273472
5.950915	388.365429	6.278477
5.978834	393.875094	6.283482
6.176291	397.806206	6.288486
6.272583	396.536076	6.293491
5.674213	400.073071	6.298496
6.389589	399.868265	6.303501
5.686334	390.419872	6.308506
6.282017	390.400650	6.313510
6.142816	389.669965	6.318515
5.916235	381.703579	6.323520
5.836257	379.430172	6.328525
5.716858	388.958533	6.333530
6.091058	396.688721	6.338534
6.170309	399.191149	6.343539
5.886921	409.877422	6.348544
6.180938	394.355399	6.353549
6.246216	395.342024	6.358554
6.038560	378.511666	6.363558
6.002092	367.188675	6.368563
5.813769	377.302101	6.373568
6.007686	379.885785	6.378573
5.961539	394.092132	6.383578
5.971616	404.587327	6.388582
6.024188	387.122841	6.393587
5.973025	400.300911	6.398592
6.489116	398.179807	6.403597
5.911798	393.464811	6.408602
5.825279	375.540487	6.413606
5.618283	379.118242	6.418611
5.610663	390.227906	6.423616
5.977531	400.119955	6.428621
6.205626	399.807187	6.433626
6.395751	388.646363	6.438630
6.273803	389.893692	6.443635
5.827876	391.554615	6.448640
6.088477	385.123547	6.453645
6.049208	392.103450	6.458650
5.745795	386.801012	6.463654
5.969956	389.252604	6.468659
5.976687	397.469695	6.473664
6.234882	395.962984	6.478669
5.889822	401.678670	6.483674
6.083031	397.028874	6.488678
6.126527	398.107908	6.493683
6.207499	389.055357	6.498688
5.992723	376.622067	6.503693
6.465598	370.963554	6.508698
5.865533	365.566192	6.513702
5.790966	360.844913	6.518707
5.692229	365.268087	6.523712
6.148894	365.316287	6.528717
5.998454	373.307393	6.533722
6.240481	371.056047	6.538726
5.788044	364.047649	6.543731
5.740489	371.759850	6.548736
6.310991	385.289823	6.553741
6.248043	376.383856	6.558746
5.802205	370.879650	6.563750
5.989722	363.669964	6.568755
5.758878	365.678692	6.573760
5.795943	384.489529	6.578765
5.981646	398.240710	6.583770
6.265750	393.585927	6.588774
6.252073	389.268965	6.593779
5.547244	378.051909	6.598784
6.224381	385.619443	6.603789
6.125833	402.854525	6.608794
6.005749	391.053401	6.613798
6.026232	383.226863	6.618803
6.028985	380.536398	6.623808
5.756569	370.444789	6.628813
5.907514	381.582851	6.633818
5.980683	392.021610	6.638822
6.375202	400.919237	6.643827
6.035934	395.621747	6.648832
6.310942	368.961036	6.653837
6.038931	379.343478	6.658842
5.800433	370.262933	6.663846
6.079853	358.644125	6.668851
5.863236	364.339119	6.673856
6.165910	368.929074	6.678861
6.306064	372.135180	6.683866
5.857065	365.987786	6.688870
5.669356	364.308248	6.693875
5.658034	373.357723	6.698880
6.201188	381.033086	6.703885
6.417922	390.265823	6.708890
5.949642	382.338278	6.713894
5.926959	364.826881	6.718899
5.674453	364.189948	6.723904
6.475645	376.466313	6.728909
5.991454	376.670513	6.733914
6.110108	364.842702	6.738918
6.020981	368.123875	6.743923
5.379737	370.164256	6.748928
5.955675	368.424959	6.753933
6.029052	385.578270	6.758938
5.920747	385.964726	6.763942
5.999639	394.122504	6.768947
5.712591	389.905079	6.773952
6.307738	395.490326	6.778957
5.901956	392.240374	6.783962
6.188408	388.180965	6.788966
6.084800	393.272349	6.793971
5.867768	400.873507	6.798976
6.146980	396.918897	6.803981
6.205159	398.117060	6.808986
6.053554	379.437840	6.813990
5.826497	375.068007	6.818995
5.965531	383.804675	6.824000
6.109172	388.435771	6.829005
6.042485	391.267054	6.834010
5.991063	379.276570	6.839014
6.147628	378.704111	6.844019
5.790818	383.691589	6.849024
6.006978	388.041508	6.854029
6.335640	385.529142	6.859034
5.916826	376.143769	6.864038
5.939111	364.307250	6.869043
5.824409	368.315503	6.874048
6.232515	374.519781	6.879053
5.968567	374.283758	6.884058
5.550823	365.834776	6.889062
6.001724	374.935189	6.894067
6.169862	390.058791	6.899072
6.203389	382.917023	6.904077
6.135263	387.288366	6.909082
6.125022	372.652669	6.914086
6.119257	363.697970	6.919091
5.986504	363.104157	6.924096
6.030332	353.136016	6.929101
5.907099	365.596634	6.934106
5.586862	373.323404	6.939110
6.170781	378.664228	6.944115
6.092415	393.120015	6.949120
6.165237	375.647650	6.954125
5.878576	379.150586	6.959130
5.756842	370.808677	6.964134
6.392145	382.009995	6.969139
5.505521	384.873059	6.974144
6.048114	383.174211	6.979149
5.871781	396.848983	6.984154
6.061356	395.466710	6.989158
6.189637	401.963614	6.994163
6.242203	396.649782	6.999168
5.996972	374.764737	7.004173
6.025758	373.528481	7.009178
5.948434	369.789605	7.014182
6.154943	362.560988	7.019187
5.905967	371.912078	7.024192
5.972038	355.401885	7.029197
5.988503	363.568604	7.034202
5.715055	377.406259	7.039206
6.357929	389.917832	7.044211
6.173992	387.634406	7.049216
6.216792	374.112379	7.054221
6.206035	373.038765	7.059226
6.295417	368.179431	7.064230
6.303854	361.667979	7.069235
5.850508	367.859801	7.074240
5.873716	362.614582	7.079245
5.729168	372.222874	7.084250
5.929303	369.540575	7.089254
5.846437	366.529212	7.094259
5.799465	372.720442	7.099264
5.758673	367.628494	7.104269
5.493975	378.435184	7.109274
5.927575	390.104248	7.114278
6.268618	392.157400	7.119283
6.122434	390.185436	7.124288
6.268112	392.370003	7.129293
6.214810	378.435072	7.134298
6.025873	372.224087	7.139302
5.930035	361.071762	7.144307
5.703316	372.166585	7.149312
6.247960	371.834155	7.154317
6.206153	381.060761	7.159322
6.056252	370.023154	7.164326
6.394693	361.640370	7.169331
6.302698	373.420731	7.174336
6.263067	367.848273	7.179341
6.173748	370.462677	7.184346
6.230675	359.179875	7.189350
6.054726	369.076939	7.194355
5.975548	369.425615	7.199360
6.208786	361.639041	7.204365
6.322131	369.997122	7.209370
6.175992	370.512783	7.214374
6.220813	358.720489	7.219379
5.910898	374.772775	7.224384
5.918037	364.477006	7.229389
6.018674	363.652338	7.234394
5.956714	368.905934	7.239398
6.094531	367.663859	7.244403
5.760971	371.292961	7.249408
6.140751	361.943089	7.254413
5.861412	359.464710	7.259418
5.699099	364.357615	7.264422
6.195359	367.998092	7.269427
5.919351	374.852019	7.274432
6.041414	361.693199	7.279437
5.687814	373.639033	7.284442
5.778704	368.411416	7.289446
6.251328	360.254267	7.294451
6.193387	371.880393	7.299456
6.378953	361.237959	7.304461
6.163108	367.998643	7.309466
5.893758	370.835263	7.314470
6.167134	371.568777	7.319475
5.926584	374.862792	7.324480
6.230577	367.230064	7.329485
5.982250	368.568177	7.334490
6.190921	367.331537	7.339494
5.946068	354.778133	7.344499
5.845156	356.744032	7.349504
5.975478	366.538674	7.354509
6.151423	371.749915	7.359514
6.060520	365.900401	7.364518
5.902610	362.523369	7.369523
6.109047	364.350953	7.374528
5.997868	371.967720	7.379533
6.015017	364.719941	7.384538
5.998453	367.013463	7.389542
6.305710	363.382982	7.394547
5.585758	362.620002	7.399552
5.889250	362.135498	7.404557
5.807935	372.432287	7.409562
5.742688	373.081372	7.414566
6.034245	365.440443	7.419571
5.784542	376.851854	7.424576
5.883031	365.860736	7.429581
5.457329	372.025880	7.434586
5.908154	371.973813	7.439590
5.757698	361.458656	7.444595
5.952935	373.864964	7.449600
5.981036	368.874090	7.454605
6.162980	370.747565	7.459610
5.875234	375.896076	7.464614
5.830421	367.950116	7.469619
5.777200	376.259413	7.474624
5.982957	372.726251	7.479629
6.087512	365.326058	7.484634
6.207535	369.636046	7.489638
6.398784	363.163783	7.494643
6.217082	365.800588	7.499648
6.282266	370.125578	7.504653
6.182687	371.349862	7.509658
5.818833	369.755931	7.514662
5.966145	365.310293	7.519667
6.206076	366.873029	7.524672
6.329350	368.175655	7.529677
6.244088	376.784290	7.534682
5.927789	380.779162	7.539686
6.274483	376.188219	7.544691
5.870227	376.058115	7.549696
6.201816	373.583351	7.554701
6.142151	371.845706	7.559706
5.837314	376.049435	7.564710
5.845497	363.534438	7.569715
5.466879	373.126830	7.574720
5.599408	364.240399	7.579725
5.713886	371.520438	7.584730
5.948968	364.453641	7.589734
6.433945	369.533785	7.594739
5.770179	378.856674	7.599744
6.068557	374.619072	7.604749
5.921385	374.464748	7.609754
5.618852	377.414610	7.614758
6.015058	368.736512	7.619763
5.633151	375.324600	7.624768
5.720378	376.285487	7.629773
5.819970	379.599151	7.634778
5.894336	398.129923	7.639782
6.236597	402.809633	7.644787
6.204851	401.905849	7.649792
6.083718	392.332838	7.654797
6.086086	384.155670	7.659802
5.834303	384.339145	7.664806
5.933857	379.083646	7.669811
6.188491	396.712532	7.674816
6.043404	391.481161	7.679821
5.926304	378.993805	7.684826
5.876054	378.647209	7.689830
6.060163	388.103405	7.694835
6.133368	396.570959	7.699840
6.096758	382.268187	7.704845
6.229716	371.453499	7.709850
5.986582	383.134968	7.714854
5.823850	381.953712	7.719859
5.695750	374.629734	7.724864
5.985452	388.649823	7.729869
5.949700	400.206780	7.734874
6.175195	398.719298	7.739878
6.253524	394.949510	7.744883
6.215984	386.209829	7.749888
6.074485	374.263274	7.754893
6.117525	376.672829	7.759898
5.877023	377.658190	7.764902
5.860789	365.713198	7.769907
6.191961	376.650517	7.774912
6.025870	372.569753	7.779917
6.034688	383.374764	7.784922
6.007719	377.470652	7.789926
6.104624	371.755601	7.794931
5.956301	374.941990	7.799936
6.146615	363.175328	7.804941
6.272237	373.381805	7.809946
5.609154	370.487640	7.814950
5.969914	363.432986	7.819955
5.892163	378.873962	7.824960
6.097242	371.895406	7.829965
5.900824	379.256532	7.834970
5.949296	376.311037	7.839974
5.997131	363.786908	7.844979
5.988208	372.076435	7.849984
6.152987	368.965060	7.854989
5.828164	369.260679	7.859994
6.011381	373.358919	7.864998
6.307072	369.040856	7.870003
6.070479	370.811562	7.875008
6.064799	370.033903	7.880013
6.082313	372.138457	7.885018
6.188990	371.747127	7.890022
6.353769	370.232997	7.895027
6.111659	371.097261	7.900032
6.017396	366.183484	7.905037
6.185350	372.001281	7.910042
6.158601	375.348693	7.915046
6.390186	366.552222	7.920051
6.255237	370.242761	7.925056
6.259593	367.040141	7.930061
6.247321	356.122232	7.935066
5.969223	350.165587	7.940070
5.900244	335.700876	7.945075
5.946864	347.382683	7.950080
5.959835	343.908882	7.955085
5.748978	345.988497	7.960090
5.979279	365.975802	7.965094
6.384741	370.434084	7.970099
5.632176	370.517357	7.975104
5.848474	361.237774	7.980109
5.914419	367.604088	7.985114
5.782471	373.459510	7.990118
6.011254	368.040345	7.995136
6.188169	373.323286	8.000154
6.430756	374.716353	8.005171
6.041467	367.181360	8.010189
5.918055	374.306599	8.015206
5.945343	372.367691	8.020224
6.037590	369.529913	8.025242
6.053671	380.748438	8.030259
6.233890	378.795227	8.035277
5.974892	375.589664	8.040294
6.633067	366.231552	8.045312
5.914474	359.183735	8.050330
5.840808	347.666902	8.055347
5.712139	362.120326	8.060365
5.981384	368.059179	8.065382
6.160616	363.776017	8.070400
5.862192	375.689675	8.075418
6.158374	377.465959	8.080435
6.183260	373.747875	8.085453
6.045514	379.008523	8.090470
6.461461	369.829878	8.095488
5.997372	371.092548	8.100506
6.192979	372.594960	8.105523
6.055733	364.349587	8.110541
5.875280	366.432143	8.115558
6.142199	365.059210	8.120576
6.251172	376.079687	8.125594
6.154105	373.566147	8.130611
6.241781	370.641928	8.135629
6.095395	370.508598	8.140646
6.251908	363.041478	8.145664
6.312334	375.271859	8.150682
5.920336	364.830870	8.155699
6.238108	370.226694	8.160717
6.125386	367.848807	8.165734
6.229538	370.556616	8.170752
6.025848	374.701507	8.175770
5.863088	377.067330	8.180787
6.322694	369.304958	8.185805
6.350469	366.627647	8.190822
6.360155	363.950183	8.195840
6.209132	378.490978	8.200858
6.478888	380.150586	8.205875
6.415271	374.760096	8.210893
6.106704	373.674768	8.215910
6.264648	370.414137	8.220928
6.061480	374.406002	8.225946
6.264758	373.528015	8.230963
6.191690	370.665845	8.235981
6.059931	362.392599	8.240998
6.395426	366.433240	8.246016
6.084296	371.143906	8.251034
6.269360	373.323794	8.256051
6.174595	369.870189	8.261069
5.784735	371.169382	8.266086
5.968160	375.512350	8.271104
6.112626	371.319976	8.276122
6.141903	374.972389	8.281139
6.310046	359.126696	8.286157
6.076700	373.147306	8.291174
6.131303	375.079137	8.296192
6.321728	379.653014	8.301210
6.483876	402.849112	8.306227
6.715801	399.044379	8.311245
6.597344	384.000782	8.316262
6.639522	368.743607	8.321280
6.426390	375.720333	8.326298
6.147032	373.404878	8.331315
6.350066	367.480512	8.336333
6.166566	378.640754	8.341350
6.264311	368.430053	8.346368
6.278812	363.556703	8.351386
6.035014	373.971087	8.356403
6.060327	379.806453	8.361421
6.140942	398.099140	8.366438
6.498085	400.254669	8.371456
6.446963	405.890910	8.376474
6.483179	401.579259	8.381491
6.599743	400.461715	8.386509
6.749754	407.946776	8.391526
6.796978	396.837608	8.396544
6.555170	383.521186	8.401562
6.436510	386.632006	8.406579
6.477785	375.294330	8.411597
6.125342	374.079075	8.416614
6.159682	370.697980	8.421632
6.116528	381.471629	8.426650
6.281878	397.266240	8.431667
6.553845	400.676126	8.436685
6.506400	408.070470	8.441702
6.312758	408.782888	8.446720
6.731162	408.313333	8.451738
6.501529	406.189819	8.456755
6.563766	409.621053	8.461773
6.533029	415.603498	8.466790
6.490724	408.837729	8.471808
6.552119	411.632935	8.476826
6.502468	409.622124	8.481843
6.591152	408.359602	8.486861
6.611034	405.211781	8.491878
6.562822	410.900883	8.496896
6.761731	407.082719	8.501914
6.274371	409.502497	8.506931
6.639542	406.824617	8.511949
6.367862	418.372295	8.516966
6.534550	411.423306	8.521984
6.374521	407.738197	8.527002
6.380312	406.181553	8.532019
6.893371	406.032713	8.537037
6.277249	415.826947	8.542054
6.432511	411.530420	8.547072
6.823084	415.621792	8.552090
6.844451	406.400996	8.557107
6.730926	403.325656	8.562125
6.582478	408.226895	8.567143
6.854775	410.180353	8.572160
6.907376	401.759636	8.577178
6.622726	402.681005	8.582195
6.734320	397.621108	8.587213
6.457114	390.450189	8.592231
6.561811	395.202623	8.597248
6.401871	406.679823	8.602266
6.393501	402.357251	8.607283
6.215197	398.633835	8.612301
6.656780	418.499509	8.617319
6.473782	401.170905	8.622336
6.628553	402.400382	8.627354
6.184719	409.623970	8.632371
6.229752	399.920558	8.637389
6.362188	404.075538	8.642407
6.536824	423.331146	8.647424
6.721789	429.166666	8.652442
6.771720	435.626863	8.657459
6.825741	439.078163	8.662477
6.734082	439.523517	8.667495
6.617281	441.413076	8.672512
6.938924	436.484708	8.677530
6.771203	438.079180	8.682547
6.842877	445.378231	8.687565
6.548464	438.145971	8.692583
6.656941	440.994404	8.697600
6.776622	443.759886	8.702618
6.956939	446.120674	8.707635
6.851834	441.443864	8.712653
6.958144	444.070036	8.717671
6.856549	431.205513	8.722688
6.708276	411.301081	8.727706
6.670131	418.947610	8.732723
7.089856	423.170168	8.737741
6.839676	413.613855	8.742759
6.269201	404.283211	8.747776
6.880059	423.274472	8.752794
6.959431	435.482474	8.757811
6.472960	430.498574	8.762829
6.781913	435.554571	8.767847
6.817433	445.046834	8.772864
6.988151	448.884685	8.777882
6.674316	446.218658	8.782899
7.162885	443.339250	8.787917
6.889166	441.083674	8.792935
6.933972	446.704240	8.797952
7.230360	428.091791	8.802970
6.944141	435.852040	8.807987
7.132495	438.784481	8.813005
7.021976	417.131017	8.818023
6.656661	415.657282	8.823040
7.069548	401.239203	8.828058
6.878545	405.600881	8.833075
6.684153	412.228485	8.838093
6.830558	420.397360	8.843111
6.934270	433.972281	8.848128
7.142044	432.021587	8.853146
6.892863	439.754249	8.858163
6.943494	439.737100	8.863181
7.124826	440.879707	8.868199
6.895923	431.593065	8.873216
7.109943	435.795562	8.878234
6.550991	438.962573	8.883251
6.861501	428.593381	8.888269
6.787027	445.070616	8.893287
6.836202	442.477340	8.898304
6.957250	440.940580	8.903322
6.785947	447.324434	8.908339
7.033162	445.850042	8.913357
6.817192	437.047634	8.918375
6.991039	439.332530	8.923392
7.186513	438.806985	8.928410
6.961527	441.753155	8.933427
7.230043	435.413030	8.938445
7.136009	429.896466	8.943463
7.097982	441.506444	8.948480
7.582934	436.458913	8.953498
7.090809	442.588634	8.958515
6.980142	443.150513	8.963533
7.406530	435.047180	8.968551
6.854955	442.015025	8.973568
7.156534	440.716852	8.978586
6.810769	438.623981	8.983603
6.978371	443.676815	8.988621
7.051218	437.089587	8.993639
6.816548	444.827919	8.998656
7.054578	437.510047	9.003674
6.651939	436.176338	9.008691
6.889172	442.494506	9.013709
6.785046	438.245846	9.018727
6.909977	447.080050	9.023744
7.060635	452.310678	9.028762
7.149692	464.186810	9.033779
7.182240	461.290600	9.038797
7.300362	463.549297	9.043815
7.471483	467.096951	9.048832
7.225096	450.200213	9.053850
6.903890	457.107477	9.058867
7.445890	469.522535	9.063885
7.341842	450.493730	9.068903
6.764048	449.701189	9.073920
7.522332	459.494016	9.078938
7.335529	470.238959	9.083955
7.124074	452.045788	9.088973
7.340627	452.409397	9.093991
7.110159	446.450693	9.099008
7.292187	456.418268	9.104026
7.469991	457.808095	9.109043
7.217879	447.354318	9.114061
7.356845	437.154658	9.119079
7.438310	436.630671	9.124096
7.088704	428.564512	9.129114
7.022826	439.029391	9.134131
7.222178	453.663798	9.139149
7.430672	456.039802	9.144167
7.398132	451.368294	9.149184
7.116146	436.460576	9.154202
7.467423	450.056124	9.159219
7.480748	452.701436	9.164237
7.442975	440.660521	9.169255
6.838222	439.280759	9.174272
7.152535	448.328661	9.179290
7.496101	457.991360	9.184307
7.259253	466.479217	9.189325
7.551212	457.765506	9.194343
7.132482	463.281751	9.199360
6.971635	465.933665	9.204378
6.996183	459.223727	9.209395
7.523464	459.838023	9.214413
7.443773	456.810805	9.219431
7.173844	461.559357	9.224448
7.065487	455.116095	9.229466
7.387586	462.246530	9.234483
7.511196	462.564512	9.239501
7.531993	466.318934	9.244519
7.566358	470.229956	9.249536
7.559739	470.903729	9.254554
7.529306	466.864888	9.259571
7.437573	459.454577	9.264589
7.461502	458.144315	9.269607
7.349260	466.509577	9.274624
7.762564	457.198456	9.279642
7.608439	466.875077	9.284659
7.470988	469.136731	9.289677
7.778018	455.755146	9.294695
7.670802	461.605600	9.299712
7.423902	465.562804	9.304730
7.653624	457.768186	9.309747
7.173756	466.997215	9.314765
7.707873	465.541251	9.319783
7.394173	464.263671	9.324800
7.363521	454.181058	9.329818
7.612472	465.694716	9.334835
7.241264	463.585978	9.339853
7.632137	460.851476	9.344871
7.241080	460.134301	9.349888
7.485573	461.509739	9.354906
7.739194	467.859650	9.359923
7.278366	462.901412	9.364941
7.588608	459.312614	9.369959
7.615760	464.592240	9.374976
7.378449	466.771029	9.379994
7.679886	466.962326	9.385011
6.960030	467.560524	9.390029
7.556309	478.686387	9.395047
7.373853	488.899759	9.400064
7.564188	491.701381	9.405082
7.750969	490.006695	9.410099
7.630117	493.569045	9.415117
7.735813	484.061032	9.420135
7.555201	496.899884	9.425152
7.990137	493.695910	9.430170
7.880937	490.758211	9.435187
7.712957	501.986439	9.440205
8.058168	479.518895	9.445223
7.503584	474.788170	9.450240
7.629393	458.390178	9.455258
7.696031	463.440054	9.460275
7.636034	465.312139	9.465293
7.586234	481.374139	9.470311
7.920768	490.062446	9.475328
7.858558	482.539566	9.480346
7.958176	476.822426	9.485363
7.576851	472.193513	9.490381
7.794358	467.289072	9.495399
7.764728	461.078027	9.500416
7.909626	462.606364	9.505434
7.834846	461.380749	9.510451
7.724468	463.416676	9.515469
7.766775	462.943657	9.520487
7.876131	462.549292	9.525504
7.816688	463.902035	9.530522
7.825181	457.614212	9.535539
7.594296	466.309332	9.540557
7.911874	462.123697	9.545575
8.173557	453.071722	9.550592
7.849056	465.608418	9.555610
7.823252	457.742147	9.560627
7.611523	466.415987	9.565645
7.820366	455.834694	9.570663
7.937719	468.502930	9.575680
7.530268	464.895391	9.580698
7.770571	480.587526	9.585715
7.913638	488.715852	9.590733
8.262973	482.308588	9.595751
8.101440	474.845070	9.600768
7.946750	470.079423	9.605786
8.043028	462.410632	9.610803
7.636673	465.110091	9.615821
7.898548	463.415373	9.620839
7.832841	468.839698	9.625856
7.877696	484.586642	9.630874
8.066149	484.183902	9.635891
7.991183	492.800072	9.640909
7.840039	489.354989	9.645927
7.917364	485.224880	9.650944
8.136189	483.104645	9.655962
7.846890	489.791893	9.660979
7.909840	493.418287	9.665997
7.931003	483.551466	9.671015
7.871968	495.120675	9.676032
7.999229	485.446110	9.681050
7.859477	485.455172	9.686067
8.065740	493.444306	9.691085
8.077995	488.150061	9.696103
8.051162	490.128854	9.701120
8.184937	499.269472	9.706138
8.304307	492.307615	9.711155
8.354519	498.344006	9.716173
8.141595	483.330718	9.721191
8.063125	468.572324	9.726208
7.863656	465.362396	9.731226
8.214045	475.524921	9.736243
7.867546	493.664057	9.741261
8.020187	495.890667	9.746279
8.385120	496.766083	9.751296
8.279761	487.053272	9.756314
8.155203	475.516427	9.761331
7.756127	479.934233	9.766349
8.126268	489.491771	9.771367
8.333686	490.631047	9.776384
8.008139	495.190606	9.781402
8.046304	493.025883	9.786419
8.299690	495.908593	9.791437
8.207633	495.682216	9.796455
8.156977	495.511183	9.801472
7.975909	497.248805	9.806490
8.419778	492.303132	9.811507
8.147161	502.079116	9.816525
8.455670	496.339581	9.821543
8.324943	490.960163	9.826560
8.258130	500.929607	9.831578
8.502826	484.469974	9.836595
8.131449	475.603719	9.841613
8.271843	470.889395	9.846631
8.015524	468.083732	9.851648
8.438827	487.605895	9.856666
8.192434	477.726696	9.861683
8.041176	492.301689	9.866701
8.049851	488.606733	9.871719
8.204114	492.837643	9.876736
8.007624	488.939082	9.881754
8.273821	489.940090	9.886771
8.182808	505.340881	9.891789
8.288469	492.060519	9.896807
8.218466	497.301722	9.901824
7.930424	501.127569	9.906842
8.087223	498.648932	9.911859
7.837622	500.005610	9.916877
8.040738	496.188893	9.921895
8.706424	503.188834	9.926912
8.565039	504.397681	9.931930
8.188562	499.115645	9.936947
8.574626	505.583196	9.941965
8.138268	500.515783	9.946983
8.255268	508.618517	9.952000
8.240042	514.364985	9.957018
9.021958	518.639395	9.962035
8.662098	507.300535	9.967053
8.206252	508.494533	9.972071
8.331558	496.364566	9.977088
8.263107	502.759362	9.982106
8.544765	511.886522	9.987123
8.511181	526.644605	9.992141
8.499502	512.038088	9.997159
8.599977	517.132769	10.002176
8.465260	511.425683	10.007194
8.584984	507.434598	10.012211
8.090050	502.198946	10.017229
8.302132	512.845387	10.022247
8.745716	517.894863	10.027264
8.682212	531.454453	10.032282
8.732488	524.325887	10.037299
8.381978	519.856805	10.042317
8.681208	525.627183	10.047335
8.490278	523.181716	10.052352
8.574256	517.577970	10.057370
8.610049	504.346959	10.062387
8.555137	519.229227	10.067405
8.580430	518.401768	10.072423
8.913441	519.839121	10.077440
8.131612	516.166213	10.082458
8.449372	512.663160	10.087475
8.224182	522.608061	10.092493
8.656654	530.469603	10.097511
9.094727	528.571895	10.102528
8.532421	535.218551	10.107546
8.829241	528.705013	10.112563
8.503454	517.053636	10.117581
8.727065	529.992495	10.122599
8.862901	517.842659	10.127616
8.717553	519.319466	10.132634
8.730877	514.954887	10.137651
8.601256	524.472380	10.142669
8.766376	524.047915	10.147687
8.730017	515.600729	10.152704
8.618578	531.355099	10.157722
8.966535	519.069749	10.162739
8.778331	511.221093	10.167757
8.231893	506.892915	10.172775
8.464755	506.770398	10.177792
8.387199	521.223970	10.182810
8.798060	514.661043	10.187827
8.636069	528.924093	10.192845
8.650757	530.141149	10.197863
8.454740	518.194681	10.202880
8.574624	533.721588	10.207898
8.709801	518.427411	10.212915
8.839234	517.254581	10.217933
9.106749	527.415905	10.222951
9.289650	517.897841	10.227968
8.806376	532.281217	10.232986
8.757463	523.095807	10.238003
8.734151	523.565276	10.243021
8.658687	522.418110	10.248039
8.944210	527.604385	10.253056
8.955872	526.713243	10.258074
9.039010	530.668562	10.263091
8.288967	518.352849	10.268109
8.291635	524.077658	10.273127
8.931853	523.135575	10.278144
8.671577	544.488202	10.283162
8.962917	549.784931	10.288179
9.281942	557.434385	10.293197
8.758353	548.443107	10.298215
8.971341	536.363742	10.303232
9.034354	551.051526	10.308250
8.925445	551.178503	10.313267
8.959672	545.738288	10.318285
9.009818	543.906589	10.323303
9.146830	543.999732	10.328320
8.976103	538.352926	10.333338
8.851549	533.820440	10.338355
8.833073	548.954163	10.343373
8.942683	559.650083	10.348391
9.205354	558.027266	10.353408
9.100735	569.820599	10.358426
8.844650	558.689893	10.363443
9.009909	564.746428	10.368461
9.163250	560.815506	10.373479
9.020664	553.007696	10.378496
8.738016	569.374468	10.383514
8.732598	558.986842	10.388531
9.124688	557.281968	10.393549
9.273486	560.232399	10.398567
9.260275	559.739637	10.403584
9.428451	557.871659	10.408602
9.443069	556.007656	10.413619
9.141683	538.616816	10.418637
8.677382	538.597149	10.423655
9.300574	539.549673	10.428672
9.507825	552.418430	10.433690
9.358894	548.806444	10.438707
9.118320	525.009171	10.443725
9.139420	531.490322	10.448743
8.970292	520.552119	10.453760
8.958386	541.666974	10.458778
9.114143	550.009947	10.463795
9.522198	544.195844	10.468813
9.255522	558.353824	10.473831
9.325832	551.148311	10.478848
9.121592	551.658568	10.483866
9.139629	550.988793	10.488883
9.397826	544.354292	10.493901
9.209822	560.741206	10.498919
9.297888	544.161592	10.503936
9.352718	554.994130	10.508954
9.344650	549.895145	10.513971
9.270554	552.093764	10.518989
8.908257	547.633121	10.524007
9.392306	552.885341	10.529024
9.416955	557.176706	10.534042
9.229106	562.812025	10.539059
9.374635	553.506018	10.544077
9.195037	560.343818	10.549095
9.247973	552.691609	10.554112
9.213998	552.425694	10.559130
9.015324	555.338396	10.564147
9.499024	550.921502	10.569165
9.290525	552.147766	10.574183
9.448482	556.203095	10.579200
9.256676	560.820835	10.584218
9.153208	556.529124	10.589235
9.634543	564.301496	10.594253
9.296665	560.767643	10.599271
9.601914	556.464348	10.604288
9.500943	551.256740	10.609306
9.192453	551.322089	10.614323
9.536865	551.741097	10.619341
9.046062	560.640324	10.624359
9.379347	557.839756	10.629376
9.566665	559.477408	10.634394
9.476658	562.197917	10.639411
9.302603	550.757592	10.644429
9.063942	561.351158	10.649447
9.461683	552.678731	10.654464
9.573612	569.423241	10.659482
9.581101	578.680088	10.664499
9.982770	571.707075	10.669517
9.622765	563.453211	10.674535
9.405753	559.411387	10.679552
9.462649	561.057843	10.684570
9.062669	553.774707	10.689587
9.542501	570.197093	10.694605
9.499008	581.801979	10.699623
9.397346	585.290902	10.704640
9.867565	594.608327	10.709658
9.618288	587.501977	10.714675
10.028825	587.490578	10.719693
9.607839	589.723813	10.724711
9.656574	592.579411	10.729728
9.621862	578.768913	10.734746
9.486504	596.022478	10.739763
9.722915	582.558390	10.744781
9.528295	585.702103	10.749799
9.311279	586.128656	10.754816
9.456880	592.012485	10.759834
9.157169	598.218270	10.764851
9.349773	593.440346	10.769869
9.587517	589.111018	10.774887
9.488439	591.871417	10.779904
9.601795	588.605724	10.784922
9.410089	601.995871	10.789939
9.888459	610.437411	10.794957
9.860591	623.864811	10.799975
10.024595	603.458845	10.804992
10.075249	600.858605	10.810010
9.993213	593.096058	10.815027
10.036372	585.596622	10.820045
10.136596	585.973790	10.825063
10.051575	582.415185	10.830080
10.324891	590.801110	10.835098
10.007890	583.043622	10.840115
10.100571	585.606529	10.845133
9.849222	588.014217	10.850151
9.901301	575.923478	10.855168
9.967127	585.074415	10.860186
9.990336	588.042697	10.865203
10.044851	580.547288	10.870221
9.775603	581.390728	10.875239
9.936791	584.693615	10.880256
9.797394	577.789530	10.885274
10.007048	579.369356	10.890291
9.932904	579.726977	10.895309
9.946422	588.454523	10.900327
9.904393	586.686898	10.905344
10.007814	574.570730	10.910362
9.890167	585.386381	10.915379
10.194380	589.665710	10.920397
9.992737	590.065309	10.925415
9.859953	582.065520	10.930432
9.882650	583.896762	10.935450
10.067070	590.563280	10.940467
10.054235	581.850960	10.945485
9.715129	589.739327	10.950503
10.066675	575.844791	10.955520
10.028961	585.386273	10.960538
9.804662	592.702912	10.965555
9.812358	569.775220	10.970573
9.684589	580.949015	10.975591
9.621212	586.029516	10.980608
9.867522	577.963016	10.985626
10.299746	594.493698	10.990643
10.204125	587.235731	10.995661
10.144267	584.433927	11.000679
9.851469	582.075394	11.005696
10.147083	599.383768	11.010714
10.066737	614.239041	11.015731
10.379783	607.684794	11.020749
10.186166	624.288635	11.025767
10.126801	622.970696	11.030784
10.411885	624.680939	11.035802
10.318039	606.446656	11.040819
10.012509	592.782756	11.045837
10.004954	608.259586	11.050855
10.241844	617.655622	11.055872
10.562529	611.638653	11.060890
10.025409	607.845678	11.065907
10.225739	609.848084	11.070925
10.324223	619.554421	11.075943
10.175774	610.747819	11.080960
10.618580	623.039673	11.085978
10.326388	615.299122	11.090995
10.425622	601.242226	11.096013
10.146700	597.936970	11.101031
10.105927	604.783492	11.106048
10.331804	606.324612	11.111066
10.290046	616.575198	11.116083
10.283541	612.932132	11.121101
10.230644	618.070156	11.126119
10.329874	622.502722	11.131136
10.511743	609.451355	11.136154
10.241755	626.712092	11.141171
10.508960	609.936415	11.146189
10.324812	622.072856	11.151207
10.482707	606.781719	11.156224
10.543542	612.977604	11.161242
10.378156	616.765059	11.166259
10.445458	617.306133	11.171277
10.301266	616.391389	11.176295
10.227207	618.213462	11.181312
10.299501	607.048027	11.186330
10.342394	611.105693	11.191347
10.347700	617.614495	11.196365
10.335461	615.011873	11.201383
9.622020	618.302329	11.206400
10.279682	621.852908	11.211418
10.411680	646.116692	11.216435
10.977788	643.056507	11.221453
10.766816	633.047729	11.226471
10.638586	625.476268	11.231488
10.925880	614.278964	11.236506
10.446283	613.204619	11.241523
10.974864	615.051298	11.246541
10.643006	615.461241	11.251559
10.190356	614.992431	11.256576
10.492023	615.480720	11.261594
10.144745	619.813221	11.266611
10.564047	621.821294	11.271629
10.762811	636.077848	11.276647
10.861100	641.299301	11.281664
11.054675	623.898247	11.286682
10.752815	621.563057	11.291699
10.734501	613.503157	11.296717
10.804787	612.072811	11.301735
10.625667	625.195164	11.306752
10.883121	613.633536	11.311770
10.494913	621.654844	11.316787
10.708707	603.895961	11.321805
10.892978	619.395561	11.326823
10.588473	619.474619	11.331840
10.545979	609.806239	11.336858
10.561840	613.389281	11.341875
10.823500	629.875810	11.346893
11.119647	631.079729	11.351911
10.751176	630.231452	11.356928
10.636057	621.282325	11.361946
10.519243	625.735905	11.366963
10.875292	635.299805	11.371981
10.982430	642.412774	11.376999
10.984389	646.981131	11.382016
10.816252	644.737960	11.387034
10.812571	641.596354	11.392051
10.962132	644.988771	11.397069
11.013327	639.655942	11.402087
10.852372	631.948175	11.407104
10.872141	634.711340	11.412122
10.985436	637.913712	11.417139
10.649805	636.070693	11.422157
10.882223	630.889342	11.427175
10.889494	646.213962	11.432192
11.004924	645.862285	11.437210
10.895090	649.621258	11.442227
10.941105	647.355615	11.447245
10.997021	647.299994	11.452263
10.723944	656.491741	11.457280
10.737147	641.155638	11.462298
11.268041	642.049442	11.467315
10.908939	642.622745	11.472333
11.153909	636.590158	11.477351
10.959073	643.566729	11.482368
11.093774	637.601216	11.487386
10.961139	643.716955	11.492403
10.941712	642.760683	11.497421
11.099486	638.490054	11.502439
10.887381	653.782116	11.507456
10.647351	639.675271	11.512474
11.014103	649.276183	11.517491
10.808466	642.339144	11.522509
10.899560	657.507385	11.527527
11.113753	661.455208	11.532544
11.239002	671.724037	11.537562
11.438269	674.701170	11.542579
11.025493	654.928803	11.547597
11.220628	658.110934	11.552615
11.214399	662.336580	11.557632
11.319213	652.255813	11.562650
11.195578	652.382670	11.567667
10.860600	645.726283	11.572685
11.254621	659.587360	11.577703
11.176205	675.341722	11.582720
11.376028	682.896616	11.587738
11.256680	683.858930	11.592755
11.292591	685.110474	11.597773
11.508006	678.602087	11.602791
11.282779	682.859674	11.607808
11.261723	681.503892	11.612826
11.474060	672.646761	11.617843
11.014146	685.410965	11.622861
11.332510	679.726814	11.627879
11.345579	680.529414	11.632896
11.032638	678.727905	11.637914
11.165754	681.540021	11.642931
11.060556	685.285244	11.647949
11.146344	682.038269	11.652967
11.130035	690.064559	11.657984
11.019651	677.443986	11.663002
11.107414	684.592859	11.668019
11.252776	691.159792	11.673037
11.422126	702.814557	11.678055
11.124467	715.467080	11.683072
11.499763	704.475400	11.688090
11.883316	717.626104	11.693107
11.429723	710.931657	11.698125
11.656215	710.587963	11.703143
11.694197	714.757093	11.708160
11.579334	705.418136	11.713178
11.453785	708.445521	11.718195
11.372958	716.697848	11.723213
11.662230	711.746803	11.728231
11.249422	717.837317	11.733248
11.645069	705.971061	11.738266
11.633676	710.690852	11.743283
11.035860	712.802411	11.748301
11.403781	706.609681	11.753319
11.492970	714.466161	11.758336
11.472616	705.991025	11.763354
11.544400	704.841114	11.768371
11.503274	714.451346	11.773389
11.081354	714.269354	11.778407
11.565300	712.993712	11.783424
11.753275	720.652351	11.788442
11.582171	713.341868	11.793459
11.681255	731.701965	11.798477
11.798959	740.655242	11.803495
11.581708	747.170836	11.808512
11.818609	738.067291	11.813530
11.915607	749.071121	11.818547
11.514832	745.214590	11.823565
11.604787	735.337398	11.828583
11.939760	746.559282	11.833600
11.842118	744.592200	11.838618
11.915968	743.180148	11.843635
11.609671	745.015499	11.848653
12.090065	743.069225	11.853671
12.196082	749.651359	11.858688
11.685850	731.244557	11.863706
11.955797	722.109173	11.868723
11.751824	717.750010	11.873741
11.795072	721.589944	11.878759
12.031483	744.782131	11.883776
11.998117	732.437325	11.888794
11.979211	724.636308	11.893811
11.652852	723.402335	11.898829
11.890896	734.240680	11.903847
11.865030	740.173038	11.908864
12.089809	749.118037	11.913882
12.120232	747.529329	11.918899
12.014053	746.704535	11.923917
12.141969	736.679726	11.928935
11.848585	721.180153	11.933952
11.754385	738.220774	11.938970
12.153589	744.552006	11.943987
11.728786	750.647668	11.949005
11.703518	756.310264	11.954023
11.895512	745.449298	11.959040
11.816673	755.470106	11.964058
12.027403	744.905626	11.969075
11.825829	755.714429	11.974093
12.199794	741.324724	11.979111
12.172827	739.363261	11.984128
12.000978	750.709625	11.989146
11.988008	756.862280	11.994163
12.062180	756.874498	11.999181
11.918129	748.413918	12.004199
12.054727	754.555584	12.009216
11.969469	752.310482	12.014234
12.160421	750.996354	12.019251
12.287013	762.420463	12.024269
11.867718	754.751871	12.029287
11.903785	769.790760	12.034304
12.164278	783.585483	12.039322
12.232644	781.559017	12.044339
12.279758	789.104017	12.049357
12.245393	781.459065	12.054375
12.371758	787.170180	12.059392
12.302363	793.081028	12.064410
12.729664	785.208452	12.069427
12.731461	788.747410	12.074445
12.386416	768.016493	12.079463
12.352452	764.545645	12.084480
11.754246	759.594706	12.089498
12.204392	768.738997	12.094515
12.353550	775.611619	12.099533
12.132213	788.953489	12.104551
12.828674	778.989614	12.109568
12.420199	782.653987	12.114586
12.664812	773.978254	12.119603
12.524175	784.566368	12.124621
12.328135	782.847058	12.129639
12.226235	782.869142	12.134656
12.179327	778.930383	12.139674
12.628086	774.560353	12.144691
12.524482	778.121093	12.149709
12.387662	779.100873	12.154727
12.642685	776.006552	12.159744
12.567748	780.115269	12.164762
12.782641	777.587402	12.169779
12.584646	782.014512	12.174797
12.806484	782.988046	12.179815
12.732916	780.241033	12.184832
12.450209	775.016991	12.189850
12.479856	765.042687	12.194867
12.192527	786.264307	12.199885
12.630343	783.175540	12.204903
12.580750	782.986612	12.209920
12.478641	778.225940	12.214938
12.312190	778.205961	12.219955
12.207889	786.966514	12.224973
12.456288	788.490342	12.229991
12.583414	787.948153	12.235008
12.562807	788.781137	12.240026
12.698316	780.318337	12.245043
12.562597	785.367775	12.250061
12.593405	790.528213	12.255079
12.575784	786.516890	12.260096
12.607824	813.713658	12.265114
12.983593	808.702592	12.270131
12.916136	814.545415	12.275149
12.811193	807.704219	12.280167
12.763278	796.684924	12.285184
12.637425	799.534828	12.290202
12.928776	810.241965	12.295219
12.950512	812.574153	12.300237
12.957405	810.303547	12.305255
13.105199	788.646943	12.310272
12.766373	781.758667	12.315290
12.619054	773.785987	12.320307
13.122454	787.344438	12.325325
13.189782	792.627956	12.330343
12.700171	780.900365	12.335360
12.609271	781.466264	12.340378
13.297334	793.153698	12.345395
12.681335	789.022578	12.350413
12.531830	798.066590	12.355431
12.768631	814.932805	12.360448
12.513671	822.487294	12.365466
13.177004	809.812107	12.370483
12.786072	811.754783	12.375501
13.118412	818.364031	12.380519
13.384358	812.427503	12.385536
12.931169	823.918929	12.390554
12.981413	817.158717	12.395571
13.379382	817.716888	12.400589
13.251179	825.718078	12.405607
13.333745	824.806910	12.410624
12.797965	824.387092	12.415642
12.803580	806.205391	12.420659
13.071292	821.813809	12.425677
12.972962	819.295288	12.430695
13.283550	815.836659	12.435712
12.746874	828.247767	12.440730
12.839435	822.390732	12.445747
13.355977	819.862117	12.450765
12.900124	818.497619	12.455783
13.285984	815.090696	12.460800
13.141092	820.650691	12.465818
13.133434	813.019017	12.470835
13.222048	814.416166	12.475853
13.246616	829.350330	12.480871
13.402655	824.522487	12.485888
13.045184	835.048124	12.490906
13.167671	834.523629	12.495923
13.345033	842.328567	12.500941
13.153648	843.116609	12.505959
13.520005	843.443808	12.510976
13.084535	851.672656	12.515994
13.203043	851.122050	12.521011
13.164303	841.501522	12.526029
13.264372	850.403849	12.531047
13.594121	841.499031	12.536064
13.344889	858.219412	12.541082
13.438037	837.449695	12.546099
13.583768	841.866750	12.551117
13.346699	847.809715	12.556135
13.382794	837.308341	12.561152
13.433458	843.937081	12.566170
13.521578	850.545449	12.571187
13.621230	839.682387	12.576205
13.422619	847.273616	12.581223
13.808468	841.654211	12.586240
13.330573	849.781821	12.591258
13.729752	845.319200	12.596275
13.646903	842.291839	12.601293
13.466460	845.303932	12.606311
13.872693	829.197085	12.611328
13.438484	844.439505	12.616346
13.742379	837.417215	12.621363
13.339749	846.563799	12.626381
13.416289	840.120465	12.631399
13.800094	835.686769	12.636416
13.505014	844.107313	12.641434
13.492259	841.965147	12.646451
13.706653	841.151039	12.651469
13.473297	843.060537	12.656487
13.491576	838.519269	12.661504
13.627801	837.897623	12.666522
13.689196	840.378750	12.671539
13.684965	850.182552	12.676557
13.798565	863.761921	12.681575
14.100694	866.429554	12.686592
13.727827	854.702258	12.691610
13.657929	850.537379	12.696627
13.705864	852.693983	12.701645
13.669431	868.581542	12.706663
14.078655	869.298866	12.711680
13.830779	869.941549	12.716698
13.945896	876.759619	12.721715
13.903285	870.135621	12.726733
13.669610	876.989404	12.731751
14.110292	863.827450	12.736768
13.913009	871.955451	12.741786
13.803881	877.191056	12.746803
14.041075	875.935005	12.751821
13.693069	879.766937	12.756839
13.972246	873.543564	12.761856
13.861914	876.779474	12.766874
14.151941	876.746893	12.771891
14.332178	870.316294	12.776909
14.065810	874.116597	12.781927
14.135696	869.469534	12.786944
13.907092	877.883025	12.791962
13.801978	877.037184	12.796979
14.007679	873.458517	12.801997
14.109796	875.113658	12.807015
14.100437	871.651703	12.812032
14.254852	874.705590	12.817050
13.858831	872.880416	12.822067
14.076100	874.403897	12.827085
13.706028	882.983723	12.832103
14.127169	872.338646	12.837120
13.862556	876.985858	12.842138
14.185031	875.597580	12.847155
14.335032	881.515042	12.852173
13.777077	882.498427	12.857191
14.017169	878.126311	12.862208
14.422713	881.870858	12.867226
14.465242	882.339474	12.872243
14.401865	881.999292	12.877261
14.044817	873.711703	12.882279
14.442672	883.052112	12.887296
14.441634	877.499517	12.892314
14.070491	880.370764	12.897331
14.195815	890.529102	12.902349
14.170863	904.319236	12.907367
14.133679	902.537781	12.912384
14.584111	909.027912	12.917402
14.460370	907.717460	12.922419
14.479418	912.211022	12.927437
13.945445	913.828595	12.932455
14.471068	910.294969	12.937472
14.586974	919.106134	12.942490
14.553946	911.984887	12.947507
14.680111	908.440248	12.952525
14.376400	912.087697	12.957543
14.637757	915.654958	12.962560
14.120452	915.921807	12.967578
14.148209	910.406162	12.972595
14.272972	906.116912	12.977613
14.037785	914.305539	12.982631
14.714887	914.243111	12.987648
14.562717	912.024813	12.992666
14.426770	916.142488	12.997683
14.318245	908.671164	13.002701
14.101373	911.418843	13.007719
14.352931	936.208728	13.012736
14.679541	944.174426	13.017754
14.423304	951.427234	13.022771
14.707682	941.788962	13.027789
14.229742	954.760495	13.032807
14.648450	951.628405	13.037824
14.339955	953.281475	13.042842
14.400828	949.859445	13.047859
14.890374	943.301222	13.052877
14.439022	949.134441	13.057895
14.757673	957.686082	13.062912
14.852174	957.496517	13.067930
14.804882	958.600058	13.072947
15.184969	962.990544	13.077965
14.966334	959.485669	13.082983
14.737324	956.400603	13.088000
14.820416	952.462319	13.093018
14.732635	966.785721	13.098035
15.316030	963.689346	13.103053
15.012507	955.575912	13.108071
14.839991	953.586951	13.113088
14.792381	950.391931	13.118106
14.415211	957.293919	13.123123
14.976622	958.820259	13.128141
14.888559	973.252371	13.133159
14.971157	967.831950	13.138176
15.197737	967.678779	13.143194
15.174752	970.838829	13.148211
15.645542	963.380203	13.153229
15.272398	950.791897	13.158247
15.035080	944.040275	13.163264
15.126437	939.370739	13.168282
15.001241	949.828069	13.173299
15.283466	945.046220	13.178317
14.912613	940.462672	13.183335
14.753946	945.537220	13.188352
15.004873	947.699198	13.193370
14.827425	966.568335	13.198387
15.068626	963.387294	13.203405
14.977472	971.666268	13.208423
14.702074	963.010796	13.213440
15.255205	972.303501	13.218458
14.985464	971.012890	13.223475
15.409931	959.157023	13.228493
15.135516	966.540795	13.233511
15.373420	969.311991	13.238528
15.353815	958.744959	13.243546
15.305723	977.315535	13.248563
15.633022	971.491223	13.253581
15.151923	975.540484	13.258599
15.135586	974.046106	13.263616
15.084777	969.643006	13.268634
15.087284	972.742933	13.273651
15.752516	964.855669	13.278669
15.339989	970.186033	13.283687
15.236979	964.876266	13.288704
15.568673	965.778867	13.293722
15.221705	969.944491	13.298739
15.526177	963.646424	13.303757
15.559476	973.638962	13.308775
15.298677	971.866578	13.313792
15.635023	966.357683	13.318810
15.251339	972.289936	13.323827
15.588533	991.950613	13.328845
15.559430	1000.236649	13.333863
15.450186	993.535447	13.338880
15.735001	1002.997006	13.343898
15.326008	1003.928960	13.348915
15.699960	992.120409	13.353933
15.820037	1009.274262	13.358951
15.612464	1007.173782	13.363968
15.818037	997.099727	13.368986
15.611811	1006.026487	13.374003
15.729475	999.426284	13.379021
15.477764	1002.687601	13.384039
15.491482	1006.651387	13.389056
16.091143	998.992278	13.394074
15.421040	1006.384115	13.399091
15.560656	998.714970	13.404109
15.696703	1001.234546	13.409127
15.301510	1010.898476	13.414144
15.851205	999.902511	13.419162
15.534287	1009.531825	13.424179
15.573012	1001.104224	13.429197
15.465199	1003.070508	13.434215
15.453713	1010.161165	13.439232
15.560260	1025.185874	13.444250
15.537477	1037.601416	13.449267
15.359783	1032.301632	13.454285
15.631595	1039.792222	13.459303
15.685162	1033.417177	13.464320
16.104358	1031.144796	13.469338
15.517703	1035.445007	13.474355
15.956380	1030.746668	13.479373
16.051558	1033.038382	13.484391
15.570805	1037.837176	13.489408
16.075193	1046.723054	13.494426
16.119946	1055.297271	13.499443
16.438909	1052.224984	13.504461
16.235468	1042.907578	13.509479
16.280449	1029.143322	13.514496
16.349390	1025.610101	13.519514
16.053292	1031.103481	13.524531
16.315267	1028.003235	13.529549
15.730519	1032.281477	13.534567
15.717243	1042.403026	13.539584
16.067648	1039.499543	13.544602
16.027336	1060.307026	13.549619
16.154250	1058.816083	13.554637
16.460416	1067.802118	13.559655
16.262594	1073.236721	13.564672
16.350867	1060.811671	13.569690
16.474260	1072.305040	13.574707
16.371693	1054.211038	13.579725
16.454096	1036.337598	13.584743
16.260514	1036.941770	13.589760
16.473147	1020.951426	13.594778
16.164126	1026.264275	13.599795
16.078278	1026.186068	13.604813
16.112766	1040.113323	13.609831
15.995263	1063.135862	13.614848
16.462506	1051.811009	13.619866
16.516019	1053.486422	13.624883
16.556354	1066.203727	13.629901
16.543937	1061.319065	13.634919
16.087158	1065.807218	13.639936
16.213359	1042.767671	13.644954
16.475895	1062.401826	13.649971
16.560927	1055.842828	13.654989
16.756404	1060.111556	13.660007
16.441469	1065.140763	13.665024
16.629084	1064.428713	13.670042
16.424955	1066.988490	13.675059
16.660717	1062.170600	13.680077
16.725337	1061.041139	13.685095
16.477612	1059.218550	13.690112
17.023106	1052.998641	13.695130
16.972238	1056.014120	13.700147
16.714699	1055.991507	13.705165
17.390905	1058.896823	13.710183
16.475051	1060.941806	13.715200
16.549947	1058.904775	13.720218
16.666171	1060.224149	13.725235
16.486186	1063.493678	13.730253
16.502101	1053.609648	13.735271
16.472011	1070.084134	13.740288
16.631206	1065.579698	13.745306
16.778369	1072.613012	13.750323
16.365091	1069.515919	13.755341
16.707162	1060.117617	13.760359
16.640599	1066.833185	13.765376
16.872659	1072.406829	13.770394
16.975601	1093.214255	13.775411
16.880507	1091.524648	13.780429
16.939747	1089.942551	13.785447
16.621485	1099.056414	13.790464
17.058180	1091.309684	13.795482
16.903202	1091.748416	13.800499
16.847745	1092.473805	13.805517
16.852171	1084.379778	13.810535
17.049083	1099.223066	13.815552
16.919713	1094.010136	13.820570
16.920880	1099.460220	13.825587
16.819594	1094.722936	13.830605
17.003517	1090.043144	13.835623
16.685776	1091.356040	13.840640
17.080787	1092.264305	13.845658
17.315769	1086.398940	13.850675
16.899771	1092.521228	13.855693
17.197309	1089.083598	13.860711
17.097279	1085.630311	13.865728
17.195146	1089.267598	13.870746
17.142693	1086.078862	13.875763
17.055487	1095.068639	13.880781
17.548284	1081.682525	13.885799
17.330420	1096.765355	13.890816
17.142629	1090.187744	13.895834
17.122839	1084.680697	13.900851
17.292052	1090.815915	13.905869
17.613724	1088.104969	13.910887
17.179846	1087.849363	13.915904
17.243595	1081.984796	13.920922
17.318555	1108.217924	13.925939
17.262863	1113.442792	13.930957
17.598647	1122.496392	13.935975
17.470551	1125.232951	13.940992
17.676835	1129.064885	13.946010
17.335204	1114.938605	13.951027
17.349851	1113.668996	13.956045
17.403815	1118.167466	13.961063
17.200693	1118.882271	13.966080
17.556331	1123.990998	13.971098
17.529131	1127.480113	13.976115
17.522334	1125.236531	13.981133
17.518269	1121.083118	13.986151
17.106420	1111.674596	13.991168
17.513168	1117.431919	13.996186
17.742496	1124.595346	14.001203
17.577398	1128.254535	14.006221
17.894917	1116.856401	14.011239
17.670847	1120.624169	14.016256
17.777890	1122.469853	14.021274
17.758950	1118.862978	14.026291
17.671868	1121.608098	14.031309
17.846622	1110.424154	14.036327
17.852753	1125.882896	14.041344
17.700659	1123.543694	14.046362
17.965008	1118.124224	14.051379
17.707065	1119.987436	14.056397
17.420120	1121.171617	14.061415
17.316593	1126.841796	14.066432
17.478479	1125.910389	14.071450
18.012564	1142.080904	14.076467
17.744785	1144.503996	14.081485
17.902854	1148.082904	14.086503
18.027395	1167.400684	14.091520
17.871125	1156.727019	14.096538
17.799006	1155.926090	14.101555
17.920048	1150.584275	14.106573
17.943970	1161.717424	14.111591
17.930828	1160.479577	14.116608
18.025461	1153.080394	14.121626
18.042095	1157.088223	14.126643
17.881616	1161.079715	14.131661
18.203126	1166.584252	14.136679
18.234489	1165.805161	14.141696
18.019873	1159.072519	14.146714
18.263949	1148.353823	14.151731
18.003884	1162.993327	14.156749
18.095717	1147.724409	14.161767
18.158353	1159.163732	14.166784
18.014893	1152.031134	14.171802
18.309540	1152.021410	14.176819
17.977802	1156.369988	14.181837
18.312719	1155.903217	14.186855
18.379939	1152.110419	14.191872
18.382331	1151.242428	14.196890
18.357731	1150.793067	14.201907
18.585043	1156.549805	14.206925
18.543911	1150.232518	14.211943
18.182193	1150.602340	14.216960
18.022311	1159.744341	14.221978
18.461522	1154.565973	14.226995
17.869069	1161.901325	14.232013
18.194752	1149.927818	14.237031
18.186241	1156.654283	14.242048
18.267992	1149.330462	14.247066
18.231476	1159.605537	14.252083
18.197266	1178.177598	14.257101
18.447728	1174.676881	14.262119
18.418811	1188.418319	14.267136
18.397314	1183.903614	14.272154
18.407817	1190.188377	14.277171
18.164357	1192.735790	14.282189
18.683161	1177.242207	14.287207
18.636286	1186.637548	14.292224
18.518432	1177.360611	14.297242
18.318453	1189.883961	14.302259
18.474879	1186.072446	14.307277
18.759147	1182.347633	14.312295
18.602772	1186.812845	14.317312
18.602463	1182.706035	14.322330
19.070265	1195.087708	14.327347
18.737846	1199.191143	14.332365
18.854570	1194.655908	14.337383
18.455190	1190.891944	14.342400
18.750882	1203.324170	14.347418
18.875806	1207.083378	14.352435
18.990871	1213.668148	14.357453
19.366428	1204.538616	14.362471
19.161692	1187.932591	14.367488
19.057535	1189.775462	14.372506
19.334765	1182.690505	14.377523
19.070706	1180.748956	14.382541
19.195095	1181.494173	14.387559
19.035958	1180.582066	14.392576
18.963704	1181.896442	14.397594
18.888195	1179.535888	14.402611
18.572436	1174.333324	14.407629
18.704784	1170.350216	14.412647
18.741154	1181.108101	14.417664
18.845004	1198.629799	14.422682
19.300153	1203.090205	14.427699
18.925198	1209.807298	14.432717
18.995986	1201.565217	14.437735
18.851946	1204.871341	14.442752
18.981844	1214.799614	14.447770
19.103930	1208.515117	14.452787
19.346328	1213.091068	14.457805
19.295427	1218.068334	14.462823
19.442306	1215.016244	14.467840
19.096751	1211.930742	14.472858
19.559301	1208.365764	14.477875
19.439934	1214.766921	14.482893
19.426897	1213.051508	14.487911
18.981767	1210.714756	14.492928
18.976652	1207.196907	14.497946
19.093162	1197.887841	14.502963
18.992560	1212.828534	14.507981
19.400184	1202.284681	14.512999
19.446237	1213.672068	14.518016
19.210172	1208.836205	14.523034
19.368376	1205.518864	14.528051
19.440921	1232.863198	14.533069
19.644619	1232.010685	14.538087
19.767970	1227.635362	14.543104
19.404255	1227.520886	14.548122
19.437669	1208.334140	14.553139
19.441157	1220.785634	14.558157
19.541710	1227.685403	14.563175
19.404193	1240.868903	14.568192
19.640251	1241.026750	14.573210
19.559166	1234.047167	14.578227
19.265056	1243.213413	14.583245
19.241095	1238.608945	14.588263
19.461087	1232.829076	14.593280
19.508405	1245.805206	14.598298
19.451067	1243.642021	14.603315
19.650988	1254.250830	14.608333
19.860299	1257.324442	14.613351
19.629251	1262.735480	14.618368
20.007410	1273.252584	14.623386
19.944545	1263.208242	14.628403
20.002447	1267.159661	14.633421
19.877435	1260.757796	14.638439
19.921804	1247.922556	14.643456
19.853669	1251.601150	14.648474
20.283220	1250.547461	14.653491
19.945679	1253.802570	14.658509
19.594285	1242.985965	14.663527
20.018984	1261.394734	14.668544
19.956645	1266.491230	14.673562
20.265088	1269.488194	14.678579
20.100152	1267.161332	14.683597
19.962326	1270.932177	14.688615
20.034531	1264.367735	14.693632
20.180772	1269.934009	14.698650
20.622778	1269.771934	14.703667
20.321171	1252.683863	14.708685
20.254366	1244.466512	14.713703
20.101889	1237.924721	14.718720
19.853466	1246.713335	14.723738
20.293734	1245.038993	14.728755
19.991730	1260.427244	14.733773
20.201708	1267.271903	14.738791
20.098369	1266.917858	14.743808
20.146667	1269.803574	14.748826
20.273854	1265.353199	14.753843
20.011666	1274.281112	14.758861
20.007180	1262.159049	14.763879
20.098648	1268.800111	14.768896
19.932238	1271.576504	14.773914
20.343383	1274.187575	14.778931
20.508466	1298.058131	14.783949
20.809018	1294.846724	14.788967
20.677819	1285.387684	14.793984
20.200622	1273.303341	14.799002
20.435994	1276.096664	14.804019
20.517005	1293.800594	14.809037
20.654159	1300.067185	14.814055
20.833449	1296.039264	14.819072
20.359982	1278.940647	14.824090
20.715675	1285.250568	14.829107
20.676166	1297.189966	14.834125
20.662799	1292.788054	14.839143
20.998142	1288.177615	14.844160
20.611370	1272.635081	14.849178
20.449486	1266.001531	14.854195
20.861867	1288.416200	14.859213
20.734290	1293.230602	14.864231
21.043831	1282.455305	14.869248
20.771771	1286.575932	14.874266
20.636609	1276.109707	14.879283
21.163674	1277.115011	14.884301
21.001091	1277.278243	14.889319
20.569883	1261.808824	14.894336
21.058915	1272.948889	14.899354
20.930523	1270.072683	14.904371
20.921180	1274.873012	14.909389
20.601586	1270.376937	14.914407
20.811019	1276.773277	14.919424
21.057310	1292.028247	14.924442
21.192115	1301.854585	14.929459
21.321462	1297.959340	14.934477
21.006868	1302.777549	14.939495
21.316400	1295.204134	14.944512
20.992406	1290.041082	14.949530
21.131250	1288.966635	14.954547
21.125165	1304.449231	14.959565
21.030968	1305.541273	14.964583
21.170763	1298.243989	14.969600
21.220421	1310.545000	14.974618
20.948306	1302.317130	14.979635
21.271418	1301.259411	14.984653
21.362665	1302.180984	14.989671
21.453608	1295.276033	14.994688
20.822218	1305.494598	14.999706
21.069373	1307.327732	15.004723
21.219776	1298.302357	15.009741
21.130679	1302.504105	15.014759
21.366056	1291.586757	15.019776
21.465231	1298.981261	15.024794
21.471936	1303.691148	15.029811
21.395351	1293.397490	15.034829
21.154536	1302.129759	15.039847
21.384220	1304.937021	15.044864
21.346722	1302.673694	15.049882
21.505400	1298.322029	15.054899
21.662718	1296.986655	15.059917
21.284721	1301.613399	15.064935
21.874471	1314.739521	15.069952
21.514536	1321.003004	15.074970
21.862422	1314.602728	15.079987
21.890980	1304.687311	15.085005
21.798715	1300.939390	15.090023
21.802714	1300.504973	15.095040
21.652538	1304.816834	15.100058
21.328881	1304.880758	15.105075
21.605629	1303.312619	15.110093
21.447329	1319.616873	15.115111
22.006609	1315.163039	15.120128
21.953511	1324.743349	15.125146
21.811185	1318.754948	15.130163
21.825567	1320.756547	15.135181
21.826064	1322.758478	15.140199
22.092834	1318.780237	15.145216
22.032577	1326.458629	15.150234
22.310993	1319.815136	15.155251
22.133029	1299.295203	15.160269
21.571320	1294.453791	15.165287
22.097600	1300.158713	15.170304
22.030114	1314.009008	15.175322
21.869995	1319.999251	15.180339
22.205638	1312.388433	15.185357
22.081815	1326.494519	15.190375
22.187897	1316.412324	15.195392
22.290204	1329.582170	15.200410
21.965888	1323.629415	15.205427
22.222999	1319.306324	15.210445
21.794138	1324.182043	15.215463
22.039414	1318.984556	15.220480
22.359475	1323.507917	15.225498
22.109064	1325.741943	15.230515
22.594782	1322.148695	15.235533
22.552667	1324.011229	15.240551
22.435461	1315.022677	15.245568
22.394638	1323.215947	15.250586
22.199118	1323.239755	15.255603
22.201993	1323.870852	15.260621
22.171796	1324.568842	15.265639
22.579888	1322.252985	15.270656
21.970006	1327.288205	15.275674
21.844533	1328.912974	15.280691
21.899474	1322.371445	15.285709
22.187156	1332.289020	15.290727
22.347110	1347.041030	15.295744
22.438690	1355.426954	15.300762
22.563549	1352.594227	15.305779
22.324111	1349.994262	15.310797
22.253194	1351.192686	15.315815
22.533295	1350.604281	15.320832
22.641131	1354.758867	15.325850
22.735034	1357.393745	15.330867
22.751696	1343.828778	15.335885
22.465324	1351.781234	15.340903
22.876232	1354.124254	15.345920
22.752892	1355.703792	15.350938
22.881825	1353.710923	15.355955
23.080694	1345.520783	15.360973
22.473117	1356.941317	15.365991
23.007383	1338.438779	15.371008
22.830022	1348.559353	15.376026
22.587472	1361.511535	15.381043
23.156130	1343.492656	15.386061
22.804105	1347.647800	15.391079
23.065981	1344.393969	15.396096
22.870000	1342.564745	15.401114
22.780227	1356.714431	15.406131
23.223253	1365.535854	15.411149
23.075719	1374.448775	15.416167
22.990406	1369.409949	15.421184
23.330557	1378.240540	15.426202
23.124645	1372.970901	15.431219
23.373355	1374.367574	15.436237
23.093244	1368.688579	15.441255
23.078414	1367.139190	15.446272
23.195853	1366.945036	15.451290
23.551072	1381.950566	15.456307
23.621651	1368.290036	15.461325
23.373112	1352.065883	15.466343
23.171719	1346.643540	15.471360
23.287338	1344.106432	15.476378
23.083715	1345.250848	15.481395
23.377007	1354.958458	15.486413
23.595579	1368.549625	15.491431
23.646215	1361.519039	15.496448
23.321492	1345.662620	15.501466
23.389092	1363.289324	15.506483
23.647476	1354.170840	15.511501
23.261405	1356.042698	15.516519
23.738375	1360.608195	15.521536
23.850350	1360.405497	15.526554
23.333284	1353.574038	15.531571
23.662643	1350.708235	15.536589
23.226746	1359.545279	15.541607
23.857052	1368.606158	15.546624
23.692670	1365.754397	15.551642
23.400163	1367.381634	15.556659
23.941519	1368.421585	15.561677
23.857786	1362.262444	15.566695
23.577072	1361.638956	15.571712
23.760557	1364.646396	15.576730
23.589787	1372.109651	15.581747
23.612375	1365.504171	15.586765
23.510309	1362.898779	15.591783
23.952695	1359.623715	15.596800
23.747934	1359.621888	15.601818
23.414886	1372.315449	15.606835
24.005460	1360.298310	15.611853
23.837678	1366.422908	15.616871
23.756694	1365.023054	15.621888
23.778686	1367.287567	15.626906
23.929825	1380.099771	15.631923
24.342193	1394.578143	15.636941
24.148798	1385.323039	15.641959
24.013668	1386.278954	15.646976
24.328781	1384.280447	15.651994
23.749011	1387.668213	15.657011
24.534024	1386.403295	15.662029
24.427909	1398.537261	15.667047
24.331364	1386.609870	15.672064
24.384694	1371.036484	15.677082
24.326694	1365.412046	15.682099
24.531787	1356.717730	15.687117
24.460315	1368.635705	15.692135
24.520448	1355.185180	15.697152
24.106608	1358.010828	15.702170
24.005733	1361.569281	15.707187
24.448767	1363.370773	15.712205
24.066760	1371.194591	15.717223
24.365528	1389.179887	15.722240
24.551835	1382.176037	15.727258
24.080261	1393.111487	15.732275
24.137949	1390.057991	15.737293
24.555289	1396.366017	15.742311
24.646684	1399.934372	15.747328
24.883737	1391.584344	15.752346
24.475970	1402.736789	15.757363
24.536699	1395.077363	15.762381
24.473395	1392.707275	15.767399
24.039930	1395.306263	15.772416
24.526389	1389.960941	15.777434
24.425972	1397.924754	15.782451
24.500201	1415.071294	15.787469
25.047549	1421.381031	15.792487
24.855488	1412.652845	15.797504
25.139064	1409.674142	15.802522
24.961844	1418.940030	15.807539
24.819404	1409.296559	15.812557
24.928756	1412.431636	15.817575
25.025603	1416.981752	15.822592
25.048624	1404.620381	15.827610
25.254505	1408.120174	15.832627
25.005283	1395.477127	15.837645
24.977302	1401.104975	15.842663
25.162746	1398.915344	15.847680
25.214828	1383.319712	15.852698
24.905023	1390.752850	15.857715
25.046628	1384.862286	15.862733
24.839883	1382.446268	15.867751
24.733229	1393.803957	15.872768
24.971268	1396.709852	15.877786
24.857472	1417.294553	15.882803
24.830660	1410.950379	15.887821
25.311877	1406.220476	15.892839
25.382376	1407.024627	15.897856
25.243440	1407.052844	15.902874
24.895661	1415.923753	15.907891
25.083203	1413.742041	15.912909
25.577916	1425.855668	15.917927
25.198539	1419.172636	15.922944
25.342199	1417.818254	15.927962
25.185744	1432.914862	15.932979
25.601735	1442.546304	15.937997
25.170377	1438.123411	15.943015
25.266228	1440.039489	15.948032
25.470867	1434.903416	15.953050
25.292429	1436.453503	15.958067
25.814089	1439.294330	15.963085
25.852226	1444.828569	15.968103
25.663992	1442.094915	15.973120
25.657235	1432.457307	15.978138
25.686725	1434.519018	15.983155
25.637093	1431.513599	15.988173
25.782379	1430.565239	15.993191
25.780911	1443.195288	15.998208
25.645889	1440.798487	16.003226
25.903948	1445.246326	16.008243
25.853913	1445.401945	16.013261
25.999432	1432.308074	16.018279
25.840470	1433.351795	16.023296
25.578474	1435.280674	16.028314
25.829087	1439.855726	16.033331
26.035108	1450.793970	16.038349
26.143071	1437.547655	16.043367
25.737476	1444.450627	16.048384
26.443274	1452.934497	16.053402
26.085065	1446.368025	16.058419
26.015292	1433.399566	16.063437
26.310374	1443.909285	16.068455
25.864368	1455.302741	16.073472
26.109982	1466.495066	16.078490
25.996915	1464.299346	16.083507
26.259749	1462.470508	16.088525
26.782862	1462.158389	16.093543
26.424687	1467.652753	16.098560
26.668898	1459.934565	16.103578
26.246348	1451.405153	16.108595
25.739788	1443.625865	16.113613
26.237535	1442.220721	16.118631
26.527141	1456.564364	16.123648
26.390440	1459.579568	16.128666
26.771838	1462.022766	16.133683
26.634855	1468.332457	16.138701
26.718258	1461.381438	16.143719
26.439883	1463.900819	16.148736
26.676749	1453.287044	16.153754
26.461071	1462.171536	16.158771
26.627183	1459.950847	16.163789
26.493191	1461.729007	16.168807
25.940908	1461.069383	16.173824
26.824804	1458.531018	16.178842
26.609850	1455.800211	16.183859
26.502357	1454.083878	16.188877
26.805605	1455.408143	16.193895
26.600392	1453.535947	16.198912
27.005570	1458.199582	16.203930
27.077383	1459.566108	16.208947
26.462628	1453.473605	16.213965
27.186317	1456.210902	16.218983
26.991218	1461.325902	16.224000
26.929224	1449.958480	16.229018
26.620173	1459.113154	16.234035
26.668716	1467.686577	16.239053
26.863784	1469.085843	16.244071
26.635814	1487.669494	16.249088
26.998892	1491.734213	16.254106
26.861009	1491.120925	16.259123
26.772777	1493.689139	16.264141
26.936533	1487.070074	16.269159
26.645834	1492.960747	16.274176
26.843646	1489.883634	16.279194
27.024738	1496.522551	16.284211
27.138014	1509.013576	16.289229
27.790523	1506.450135	16.294247
27.551733	1509.869651	16.299264
27.936947	1495.060858	16.304282
27.939545	1486.549606	16.309299
27.629925	1484.132498	16.314317
27.818182	1474.179505	16.319335
27.668410	1486.477460	16.324352
27.659805	1474.222057	16.329370
27.962668	1477.088886	16.334387
27.520820	1482.176643	16.339405
27.820328	1469.726917	16.344423
27.897022	1474.533927	16.349440
27.642486	1447.305706	16.354458
27.670244	1444.660299	16.359475
27.384635	1451.126483	16.364493
27.940770	1456.567470	16.369511
27.941936	1468.074286	16.374528
27.679118	1454.032674	16.379546
27.753760	1452.706253	16.384563
27.758203	1466.899099	16.389581
28.118591	1468.030835	16.394599
27.373689	1455.446591	16.399616
27.676467	1464.498772	16.404634
28.070982	1470.978323	16.409651
27.782483	1475.446599	16.414669
27.784686	1464.665378	16.419687
27.706472	1469.585044	16.424704
27.837312	1467.896565	16.429722
27.573070	1468.761661	16.434739
27.691685	1470.613345	16.439757
27.709276	1471.897907	16.444775
27.719869	1487.290524	16.449792
27.991141	1501.368351	16.454810
28.065265	1505.606905	16.459827
28.005999	1514.648595	16.464845
28.006200	1498.931124	16.469863
27.976759	1502.946279	16.474880
28.137879	1501.597266	16.479898
28.490415	1499.327591	16.484915
28.192625	1501.616337	16.489933
28.231334	1491.940062	16.494951
28.392655	1502.080636	16.499968
28.471268	1499.837423	16.504986
28.418698	1503.833574	16.510003
28.105243	1510.731553	16.515021
28.712921	1515.537262	16.520039
28.878391	1532.142058	16.525056
28.760507	1517.479544	16.530074
28.825904	1509.442521	16.535091
28.663848	1504.015183	16.540109
28.150134	1496.863423	16.545127
28.256596	1508.205197	16.550144
28.865998	1525.699061	16.555162
28.729676	1526.542978	16.560179
28.647309	1532.017283	16.565197
29.166889	1523.682604	16.570215
29.154823	1530.057068	16.575232
28.920037	1509.876971	16.580250
29.019871	1504.805473	16.585267
28.529230	1496.800296	16.590285
29.021742	1496.646392	16.595303
28.838158	1521.604151	16.600320
29.160293	1518.224953	16.605338
28.906413	1521.555632	16.610355
28.717605	1531.479798	16.615373
28.949336	1530.882074	16.620391
29.075018	1541.791954	16.625408
28.718403	1532.482688	16.630426
29.027958	1530.313826	16.635443
28.719642	1532.292905	16.640461
28.980004	1531.664850	16.645479
28.992570	1537.056902	16.650496
28.663323	1530.268671	16.655514
28.932831	1554.351068	16.660531
28.822768	1561.944911	16.665549
28.918940	1552.860653	16.670567
29.273805	1556.627933	16.675584
28.844848	1564.808043	16.680602
29.469454	1572.019609	16.685619
29.596039	1591.760411	16.690637
29.912819	1573.865258	16.695655
30.081856	1556.061126	16.700672
29.860029	1559.593590	16.705690
30.060406	1543.711825	16.710707
29.877777	1545.546867	16.715725
29.999616	1545.067339	16.720743
29.928029	1546.956827	16.725760
29.799825	1545.060843	16.730778
30.193629	1540.832379	16.735795
30.125541	1530.089523	16.740813
29.964193	1519.444007	16.745831
29.900995	1508.940904	16.750848
29.633608	1506.279006	16.755866
29.977303	1497.647880	16.760883
29.614151	1508.440261	16.765901
29.904762	1495.770337	16.770919
29.924181	1509.267049	16.775936
29.977393	1527.023487	16.780954
30.304100	1531.382425	16.785971
29.549422	1521.482789	16.790989
30.132993	1530.946381	16.796007
30.151910	1530.540195	16.801024
30.061481	1535.160333	16.806042
30.591532	1534.235654	16.811059
30.225554	1541.977375	16.816077
30.139259	1542.882694	16.821095
30.150050	1545.864435	16.826112
30.031737	1543.963271	16.831130
30.376406	1535.450860	16.836147
30.443487	1542.394894	16.841165
30.093265	1536.782169	16.846183
30.209401	1537.292946	16.851200
30.173685	1534.877323	16.856218
30.411518	1533.643556	16.861235
30.433232	1530.912521	16.866253
30.495799	1537.045892	16.871271
30.682759	1533.842616	16.876288
30.124180	1532.501754	16.881306
30.414197	1528.064891	16.886323
30.283065	1530.287068	16.891341
30.500124	1535.347228	16.896359
30.547723	1551.727472	16.901376
30.307084	1569.099549	16.906394
30.725117	1565.775720	16.911411
30.468023	1566.322712	16.916429
30.999053	1569.653740	16.921447
30.973274	1568.119137	16.926464
31.239616	1569.591255	16.931482
31.242989	1574.249414	16.936499
31.169209	1572.131031	16.941517
31.175463	1568.278937	16.946535
30.894523	1551.723722	16.951552
30.972680	1557.823810	16.956570
31.044768	1561.961930	16.961587
30.939844	1573.562770	16.966605
30.934051	1570.752032	16.971623
31.255346	1563.869447	16.976640
30.937797	1572.182293	16.981658
31.191802	1567.803350	16.986675
31.059524	1566.023393	16.991693
31.254947	1570.717071	16.996711
31.065458	1566.368654	17.001728
31.084728	1579.454039	17.006746
31.282851	1564.756475	17.011763
30.944707	1567.936158	17.016781
31.262545	1565.973005	17.021799
31.416761	1569.670759	17.026816
31.091788	1574.249432	17.031834
31.143576	1580.139724	17.036851
31.492970	1594.115724	17.041869
31.235465	1591.458474	17.046887
31.591224	1582.402472	17.051904
31.313950	1591.209836	17.056922
31.582867	1591.014612	17.061939
31.473302	1596.895015	17.066957
31.366503	1597.310428	17.071975
31.600379	1599.523747	17.076992
31.666944	1622.868995	17.082010
31.680885	1619.803407	17.087027
31.868143	1620.294536	17.092045
31.876613	1628.067601	17.097063
32.078622	1608.759530	17.102080
32.169407	1624.414199	17.107098
32.213254	1615.879510	17.112115
31.862830	1610.249075	17.117133
31.642964	1617.181210	17.122151
32.002082	1615.151373	17.127168
31.742387	1620.592081	17.132186
31.861480	1616.625226	17.137203
31.669394	1621.948834	17.142221
31.885422	1617.417899	17.147239
31.904140	1613.169637	17.152256
32.284348	1632.098418	17.157274
32.409751	1630.365941	17.162291
32.503364	1643.330013	17.167309
32.586042	1638.118400	17.172327
32.436271	1617.577629	17.177344
32.599311	1607.907465	17.182362
32.445364	1605.806683	17.187379
32.409843	1613.930725	17.192397
32.677278	1606.738931	17.197415
32.872391	1607.124429	17.202432
32.428012	1608.377234	17.207450
32.469351	1608.742132	17.212467
32.459348	1605.936416	17.217485
32.829501	1618.744834	17.222503
32.924372	1611.315867	17.227520
32.407679	1609.614520	17.232538
32.716537	1603.730035	17.237555
32.570046	1610.731512	17.242573
32.383042	1638.317571	17.247591
32.833808	1625.887162	17.252608
32.574757	1638.319080	17.257626
33.347136	1633.306251	17.262643
32.816003	1638.500575	17.267661
32.826793	1633.833543	17.272679
33.109467	1636.065558	17.277696
32.881676	1638.746669	17.282714
33.046254	1638.222266	17.287731
33.131275	1628.503985	17.292749
32.597611	1642.316020	17.297767
33.229739	1625.081185	17.302784
32.983051	1630.576042	17.307802
32.964244	1634.413879	17.312819
33.237124	1641.604193	17.317837
33.203332	1650.616154	17.322855
33.522513	1642.481527	17.327872
33.041065	1640.607018	17.332890
33.550435	1647.762111	17.337907
33.773409	1662.355562	17.342925
33.590646	1656.419395	17.347943
33.624798	1639.943798	17.352960
33.694156	1632.600542	17.357978
33.758474	1629.708498	17.362995
33.568575	1623.426676	17.368013
33.654446	1626.766078	17.373031
33.757447	1625.506206	17.378048
33.418688	1627.059632	17.383066
33.849625	1622.683659	17.388083
33.690647	1628.204147	17.393101
33.296253	1632.451027	17.398119
34.224999	1644.892561	17.403136
34.142902	1663.341243	17.408154
34.151012	1648.710104	17.413171
34.060686	1634.681497	17.418189
33.835189	1626.554394	17.423207
34.003605	1619.896312	17.428224
33.663312	1635.568045	17.433242
33.869280	1646.282815	17.438259
34.183258	1658.464743	17.443277
34.007548	1663.197859	17.448295
34.288650	1661.440383	17.453312
33.984366	1666.220774	17.458330
34.134802	1660.349510	17.463347
34.054552	1662.930208	17.468365
33.975212	1654.570228	17.473383
34.201047	1651.123089	17.478400
34.031806	1653.385846	17.483418
33.860450	1657.897768	17.488435
34.213335	1659.898870	17.493453
34.157387	1688.134967	17.498471
34.780559	1678.423605	17.503488
34.462289	1686.861435	17.508506
34.637857	1675.106478	17.513523
34.435260	1683.601529	17.518541
34.499223	1685.071344	17.523559
34.858561	1674.110367	17.528576
35.242353	1678.692571	17.533594
35.094821	1663.680892	17.538611
35.331641	1660.805948	17.543629
34.836496	1646.206964	17.548647
35.080042	1636.327783	17.553664
35.173129	1634.790419	17.558682
35.188841	1641.154029	17.563699
35.462596	1628.536001	17.568717
35.092839	1638.163034	17.573735
35.134262	1634.258643	17.578752
35.379479	1630.136255	17.583770
35.321340	1633.321946	17.588787
35.548784	1630.308403	17.593805
35.538850	1610.501962	17.598823
34.887074	1605.309617	17.603840
35.141117	1604.070798	17.608858
35.163435	1606.799857	17.613875
34.906153	1607.939791	17.618893
34.792832	1620.145989	17.623911
35.200149	1623.512477	17.628928
34.994414	1633.572581	17.633946
35.177614	1638.941530	17.638963
35.415999	1626.045110	17.643981
35.087576	1637.114504	17.648999
35.244905	1633.870446	17.654016
35.212671	1637.969955	17.659034
34.908763	1654.610088	17.664051
35.702771	1661.150733	17.669069
35.675156	1663.989645	17.674087
35.948179	1662.682325	17.679104
35.728510	1669.309333	17.684122
35.450210	1673.924007	17.689139
35.750773	1658.303094	17.694157
35.508632	1676.345617	17.699175
35.433779	1657.360889	17.704192
35.665073	1661.582909	17.709210
35.634745	1667.258486	17.714227
35.867004	1680.539002	17.719245
35.608402	1697.064984	17.724263
35.995838	1694.536353	17.729280
35.826243	1693.188150	17.734298
35.927328	1694.516780	17.739315
36.362832	1686.735702	17.744333
36.071899	1691.044993	17.749351
36.077151	1689.987522	17.754368
36.383198	1689.647566	17.759386
36.105177	1680.130707	17.764403
36.438213	1677.468174	17.769421
36.560396	1684.125195	17.774439
36.426712	1681.280496	17.779456
36.388715	1682.637667	17.784474
36.323862	1681.970152	17.789491
36.675285	1677.269536	17.794509
36.419698	1680.938326	17.799527
36.359438	1690.206267	17.804544
36.308219	1682.906969	17.809562
36.501969	1703.534036	17.814579
36.758750	1698.786093	17.819597
36.803207	1706.224498	17.824615
36.773394	1706.656693	17.829632
36.975678	1704.789823	17.834650
37.078421	1710.938263	17.839667
37.086862	1695.166472	17.844685
36.785089	1683.066930	17.849703
36.801774	1676.161902	17.854720
36.973535	1688.347325	17.859738
36.912159	1698.349708	17.864755
37.091711	1691.400776	17.869773
37.127803	1704.818126	17.874791
37.205220	1706.305006	17.879808
37.093516	1698.527133	17.884826
36.956172	1704.415720	17.889843
37.250101	1700.761626	17.894861
37.263920	1694.055884	17.899879
37.331322	1698.924344	17.904896
37.609820	1697.932650	17.909914
37.155366	1701.998943	17.914931
37.323903	1700.263252	17.919949
37.251755	1698.536707	17.924967
37.383900	1700.300352	17.929984
37.387009	1692.607800	17.935002
37.417351	1694.336726	17.940019
37.539898	1696.618102	17.945037
37.788229	1708.500704	17.950055
37.355232	1704.602019	17.955072
37.782947	1701.296638	17.960090
37.592014	1694.981494	17.965107
37.438975	1694.367164	17.970125
37.631230	1704.510229	17.975143
37.257192	1708.820688	17.980160
37.511172	1717.246058	17.985178
37.747817	1733.128653	17.990195
38.063352	1733.716655	17.995213
37.977357	1737.349502	18.000231
37.978914	1724.039853	18.005248
38.114969	1726.893013	18.010266
38.279332	1729.889911	18.015283
38.278852	1727.316455	18.020301
38.119281	1732.773299	18.025319
38.185208	1731.269951	18.030336
38.385179	1723.666439	18.035354
38.221267	1730.280303	18.040371
38.132137	1727.188060	18.045389
38.254660	1721.854860	18.050407
38.374162	1723.332411	18.055424
38.470901	1719.133012	18.060442
38.396146	1729.323457	18.065459
38.480568	1726.893029	18.070477
38.427096	1718.863376	18.075495
38.353378	1734.177285	18.080512
38.539501	1725.879607	18.085530
38.445989	1736.438125	18.090547
38.488514	1734.053610	18.095565
38.688674	1744.334369	18.100583
38.711851	1747.037326	18.105600
38.899118	1744.658369	18.110618
38.683736	1752.752030	18.115635
38.893333	1751.603631	18.120653
38.790290	1741.539254	18.125671
38.758774	1744.550480	18.130688
38.774555	1740.292040	18.135706
38.722028	1744.854782	18.140723
38.713267	1748.772087	18.145741
38.942581	1746.757822	18.150759
38.934466	1768.183759	18.155776
39.261546	1774.873427	18.160794
38.868365	1774.393740	18.165811
39.011286	1773.221342	18.170829
39.320325	1774.411605	18.175847
39.368938	1773.959551	18.180864
39.509380	1776.224982	18.185882
39.423051	1783.868941	18.190899
39.276242	1772.536980	18.195917
39.740699	1767.441240	18.200935
39.240358	1777.909277	18.205952
39.498539	1767.222467	18.210970
39.345987	1769.373028	18.215987
39.595063	1763.874762	18.221005
39.579424	1766.419976	18.226023
39.868128	1776.746332	18.231040
39.927286	1768.923594	18.236058
39.675849	1775.223623	18.241075
39.866111	1775.001263	18.246093
39.841734	1767.195509	18.251111
39.332997	1784.009855	18.256128
39.596527	1792.313606	18.261146
39.969761	1793.147176	18.266163
39.869520	1788.716595	18.271181
40.213701	1789.899859	18.276199
40.257939	1786.832371	18.281216
40.524715	1787.350890	18.286234
40.530897	1792.216525	18.291251
40.393885	1781.340418	18.296269
40.647132	1777.812335	18.301287
40.727417	1777.826692	18.306304
40.581742	1757.124426	18.311322
40.681532	1757.549335	18.316339
40.964674	1749.209988	18.321357
40.786951	1746.145010	18.326375
40.430721	1755.341133	18.331392
40.836775	1737.369986	18.336410
40.374547	1751.290760	18.341427
40.748789	1747.092252	18.346445
40.731230	1738.200340	18.351463
40.431212	1745.106828	18.356480
40.482620	1744.564153	18.361498
40.728607	1746.299503	18.366515
40.750243	1746.237351	18.371533
40.684404	1747.381027	18.376551
40.593989	1767.590666	18.381568
41.046602	1772.794971	18.386586
40.889583	1779.481337	18.391603
41.119340	1789.231632	18.396621
40.983546	1783.203386	18.401639
41.067324	1779.518718	18.406656
41.294992	1778.409451	18.411674
40.942700	1787.374625	18.416691
40.910691	1785.713865	18.421709
40.984097	1774.155279	18.426727
40.959383	1778.972482	18.431744
40.975708	1781.538784	18.436762
41.183462	1792.112414	18.441779
41.174653	1801.840803	18.446797
41.250957	1811.392505	18.451815
40.963466	1813.343760	18.456832
41.471867	1805.746224	18.461850
41.346340	1814.126221	18.466867
41.587882	1806.340194	18.471885
41.952679	1806.575551	18.476903
41.787331	1818.228311	18.481920
41.897493	1802.620671	18.486938
41.686051	1809.840475	18.491955
41.797272	1809.203248	18.496973
41.837990	1800.951262	18.501991
41.949641	1814.645961	18.507008
42.094204	1814.176443	18.512026
41.773657	1817.437514	18.517043
41.908531	1826.866533	18.522061
42.416752	1829.747457	18.527079
42.362660	1827.435619	18.532096
42.389630	1823.118610	18.537114
42.507987	1809.757263	18.542131
42.145176	1798.953967	18.547149
42.431742	1788.937643	18.552167
42.190506	1783.919382	18.557184
42.448699	1800.635098	18.562202
42.372244	1814.675121	18.567219
42.680805	1819.467860	18.572237
42.878572	1809.474888	18.577255
42.553134	1797.511065	18.582272
42.596499	1786.841308	18.587290
42.716893	1789.839987	18.592307
42.702488	1801.033879	18.597325
42.890067	1773.642503	18.602343
42.564036	1779.792286	18.607360
42.370017	1780.374902	18.612378
42.882801	1797.702005	18.617395
42.892696	1808.417465	18.622413
43.417368	1809.646436	18.627431
42.785794	1805.358557	18.632448
42.741345	1809.793995	18.637466
42.829163	1810.190179	18.642483
42.911697	1817.954225	18.647501
43.045756	1815.868716	18.652519
43.510806	1814.991402	18.657536
43.334507	1812.950985	18.662554
43.346928	1806.770233	18.667571
43.276249	1809.188346	18.672589
43.418582	1810.504644	18.677607
43.137186	1807.996982	18.682624
42.966850	1806.167392	18.687642
43.022975	1806.448350	18.692659
43.101816	1819.172101	18.697677
43.220612	1816.622187	18.702695
43.574062	1827.998494	18.707712
43.205052	1847.624049	18.712730
43.580923	1846.385511	18.717747
43.352887	1845.909973	18.722765
43.559672	1836.917469	18.727783
43.471917	1847.356604	18.732800
43.485706	1845.797704	18.737818
43.840568	1851.209170	18.742835
43.747636	1868.535469	18.747853
44.136329	1871.462965	18.752871
44.029818	1863.140048	18.757888
44.188755	1868.628845	18.762906
44.348610	1867.307570	18.767923
44.224352	1862.921889	18.772941
44.461889	1853.878614	18.777959
44.118944	1859.511538	18.782976
44.465447	1854.957354	18.787994
44.868760	1858.049358	18.793011
44.300625	1857.408873	18.798029
44.717520	1858.092303	18.803047
44.659835	1856.760594	18.808064
44.267091	1850.500456	18.813082
44.698700	1854.390538	18.818099
44.728926	1859.804974	18.823117
44.494170	1845.600090	18.828135
44.426326	1854.560327	18.833152
44.449098	1860.429940	18.838170
44.998933	1851.594011	18.843187
44.706497	1856.564232	18.848205
44.819171	1857.554339	18.853223
44.962089	1856.393746	18.858240
44.420201	1858.064688	18.863258
44.692590	1848.813673	18.868275
44.420650	1854.607674	18.873293
44.725725	1860.226602	18.878311
44.822696	1876.720275	18.883328
45.147493	1897.087315	18.888346
45.406210	1883.369588	18.893363
45.151665	1888.308348	18.898381
45.507284	1881.103008	18.903399
45.380604	1887.081238	18.908416
45.249186	1879.198268	18.913434
45.546820	1880.792009	18.918451
45.798876	1876.530234	18.923469
45.757993	1869.823631	18.928487
45.784773	1875.677232	18.933504
45.638570	1868.199477	18.938522
45.892973	1863.251089	18.943539
46.135196	1878.671094	18.948557
45.836192	1874.462773	18.953575
45.652605	1873.899163	18.958592
45.702237	1877.962739	18.963610
45.847369	1873.447407	18.968627
45.797729	1880.646357	18.973645
46.038770	1874.586384	18.978663
45.801637	1870.355614	18.983680
46.100196	1871.186200	18.988698
45.989073	1862.837668	18.993715
45.853375	1869.408730	18.998733
45.821230	1868.908233	19.003751
46.064974	1866.721877	19.008768
46.010937	1872.931382	19.013786
45.760259	1873.285980	19.018803
46.038232	1896.381277	19.023821
45.929256	1896.574220	19.028839
46.061449	1897.957560	19.033856
46.134086	1899.043277	19.038874
46.505051	1901.104411	19.043891
46.188815	1915.035409	19.048909
46.806969	1919.686361	19.053927
46.305563	1936.837852	19.058944
46.912855	1923.518676	19.063962
46.919666	1927.431873	19.068979
46.541745	1927.713839	19.073997
46.922276	1926.121369	19.079015
46.716582	1926.852776	19.084032
46.535109	1936.792127	19.089050
46.885819	1934.796714	19.094067
46.819008	1926.570340	19.099085
47.259254	1951.177062	19.104103
46.942760	1943.818415	19.109120
47.178794	1950.765365	19.114138
47.548286	1956.019325	19.119155
47.464297	1954.692356	19.124173
47.458088	1951.874532	19.129191
47.577994	1954.342606	19.134208
47.662048	1951.519678	19.139226
47.639083	1929.458650	19.144243
47.244210	1922.905524	19.149261
47.739901	1935.551684	19.154279
47.865551	1947.487857	19.159296
47.648325	1942.100208	19.164314
47.995715	1940.994335	19.169331
47.709281	1943.876942	19.174349
47.914992	1938.113745	19.179367
48.095234	1939.699371	19.184384
47.958165	1937.187081	19.189402
48.423008	1931.223494	19.194419
47.972164	1919.894918	19.199437
48.046263	1903.465183	19.204455
48.110167	1908.220902	19.209472
47.862544	1904.259185	19.214490
48.377903	1916.116630	19.219507
48.114028	1934.547702	19.224525
48.472793	1934.379331	19.229543
48.232639	1937.273172	19.234560
47.944860	1931.672796	19.239578
48.094112	1935.901390	19.244595
48.023940	1940.098602	19.249613
48.182098	1933.384210	19.254631
48.105806	1939.522229	19.259648
48.116127	1957.562644	19.264666
48.461755	1965.504070	19.269683
48.385329	1973.118922	19.274701
48.342195	1971.734793	19.279719
48.548816	1955.030693	19.284736
48.482522	1963.871443	19.289754
48.689816	1961.448586	19.294771
48.792978	1976.855101	19.299789
48.811055	1990.158356	19.304807
49.091834	1980.001133	19.309824
49.146555	1996.119639	19.314842
49.389533	1986.173793	19.319859
49.211324	1994.670487	19.324877
49.303252	1989.482422	19.329895
49.386933	1989.137155	19.334912
49.234162	1982.680925	19.339930
49.886731	1984.618668	19.344947
49.812696	1999.767534	19.349965
49.963518	1982.493106	19.354983
49.619919	1960.727257	19.360000
49.405240	1963.910984	19.365018
49.820824	1949.066417	19.370035
49.475739	1964.299502	19.375053
49.648845	1973.830157	19.380071
49.555058	1980.334875	19.385088
49.835723	1977.684507	19.390106
50.070668	1984.693465	19.395123
49.373053	1985.429558	19.400141
49.918687	1984.258571	19.405159
49.988676	1979.795022	19.410176
49.990963	1981.317598	19.415194
49.862021	1981.154393	19.420211
49.939210	1981.720848	19.425229
50.040640	1986.364863	19.430247
49.970305	1987.938836	19.435264
50.275312	2014.395253	19.440282
50.556514	2010.296335	19.445299
50.182226	2008.247731	19.450317
50.224826	2011.173507	19.455335
50.378027	2007.509180	19.460352
50.274836	2012.322127	19.465370
50.507014	2005.990337	19.470387
50.615591	2010.644594	19.475405
50.581366	2013.294502	19.480423
50.859882	2006.569598	19.485440
50.406087	2011.816986	19.490458
50.753832	2021.657736	19.495475
51.039106	2027.009919	19.500493
51.031915	2038.429564	19.505511
51.233251	2036.113196	19.510528
51.044434	2040.275748	19.515546
51.080453	2029.262939	19.520563
51.264313	2036.210693	19.525581
51.244744	2041.520051	19.530599
51.529477	2031.435370	19.535616
51.240152	2032.631033	19.540634
51.330398	2037.006043	19.545651
51.532036	2031.362780	19.550669
51.307914	2031.635422	19.555687
51.557715	2026.978695	19.560704
51.390437	2034.529092	19.565722
51.458768	2026.522419	19.570739
51.743599	2022.983933	19.575757
51.457505	2033.311150	19.580775
51.759408	2033.552596	19.585792
51.305842	2033.985281	19.590810
51.480350	2042.670845	19.595827
51.539020	2059.184047	19.600845
51.615793	2056.555617	19.605863
51.930084	2055.243401	19.610880
52.118052	2060.112484	19.615898
52.006599	2059.589286	19.620915
52.403750	2052.917948	19.625933
52.183505	2058.790867	19.630951
52.582067	2054.444941	19.635968
52.290572	2056.376416	19.640986
52.052905	2053.580363	19.646003
52.233151	2060.266515	19.651021
52.212263	2061.835458	19.656039
52.643760	2053.493826	19.661056
52.427460	2064.228413	19.666074
52.517307	2079.410852	19.671091
52.675988	2075.097160	19.676109
52.825711	2080.532045	19.681127
53.093271	2075.747951	19.686144
53.005867	2074.171925	19.691162
52.755483	2071.515774	19.696179
53.161976	2070.774918	19.701197
52.971486	2073.963323	19.706215
53.084208	2071.382876	19.711232
53.081260	2065.854188	19.716250
52.940959	2066.320830	19.721267
53.003665	2067.792858	19.726285
52.843972	2066.080768	19.731303
53.375724	2064.918768	19.736320
52.822986	2066.411207	19.741338
53.269588	2079.497515	19.746355
53.666151	2074.676705	19.751373
53.302921	2092.845670	19.756391
53.813294	2093.792774	19.761408
53.386564	2104.244902	19.766426
53.601584	2100.007704	19.771443
53.983754	2099.462218	19.776461
53.677456	2099.271684	19.781479
53.905076	2099.854180	19.786496
53.540442	2098.788243	19.791514
53.626167	2099.813538	19.796531
54.033444	2105.859739	19.801549
53.713674	2098.025957	19.806567
53.823344	2083.175224	19.811584
54.117350	2103.358654	19.816602
54.301434	2116.029395	19.821619
54.511408	2112.744629	19.826637
54.267201	2122.402746	19.831655
54.549577	2110.794346	19.836672
54.893708	2110.823678	19.841690
54.549251	2111.700121	19.846707
54.984326	2114.205013	19.851725
54.291012	2103.295201	19.856743
54.569412	2097.710859	19.861760
54.772584	2106.326751	19.866778
54.836612	2108.986391	19.871795
54.988129	2108.198776	19.876813
54.767323	2110.452813	19.881831
54.682584	2100.056028	19.886848
54.373924	2108.543282	19.891866
54.785269	2102.051861	19.896883
55.225920	2106.310993	19.901901
54.911363	2112.892088	19.906919
55.225566	2104.070625	19.911936
55.213262	2101.240396	19.916954
55.176188	2111.712262	19.921971
55.332167	2137.319920	19.926989
55.031072	2133.067777	19.932007
55.515624	2139.352384	19.937024
55.217154	2140.049162	19.942042
55.173104	2134.630014	19.947059
55.628626	2133.893636	19.952077
55.589572	2139.394841	19.957095
55.565881	2133.414432	19.962112
55.570752	2132.616451	19.967130
55.468027	2138.312062	19.972147
55.884936	2143.160585	19.977165
55.454330	2153.739770	19.982183
55.632653	2158.880962	19.987200
55.850499	2158.018579	19.992218
55.897405	2165.578457	19.997235
56.348774	2152.647515	20.002253
56.055888	2154.763490	20.007271
56.487850	2149.239531	20.012288
56.413424	2153.500892	20.017306
56.420349	2151.502534	20.022323
56.607894	2149.687660	20.027341
56.974946	2149.104911	20.032359
56.581120	2149.860787	20.037376
56.679722	2153.374578	20.042394
56.692345	2146.249928	20.047411
57.008301	2150.399008	20.052429
56.554236	2151.566839	20.057447
56.676171	2150.971133	20.062464
56.529436	2149.705326	20.067482
56.719594	2177.404303	20.072499
57.054365	2171.856665	20.077517
56.989535	2187.082932	20.082535
56.878355	2184.546234	20.087552
57.054420	2167.289075	20.092570
57.075547	2178.842328	20.097587
57.159202	2171.211007	20.102605
57.262859	2181.412759	20.107623
57.512074	2177.337206	20.112640
57.389649	2179.087545	20.117658
57.418654	2180.934074	20.122675
57.537496	2178.012428	20.127693
57.331663	2185.948822	20.132711
57.906005	2189.138956	20.137728
58.008007	2201.212709	20.142746
57.821816	2206.167022	20.147763
58.089133	2192.518468	20.152781
58.113878	2198.908372	20.157799
58.097801	2192.230200	20.162816
58.469805	2193.395899	20.167834
58.154204	2181.464795	20.172851
58.126639	2160.949525	20.177869
58.310723	2175.540452	20.182887
58.304695	2182.966973	20.187904
58.711520	2180.468522	20.192922
58.633869	2178.456998	20.197939
58.724576	2159.185572	20.202957
58.434560	2160.772709	20.207975
58.494490	2151.790562	20.212992
58.828129	2154.974875	20.218010
58.407924	2163.810953	20.223027
58.542559	2175.854873	20.228045
58.436829	2176.218546	20.233063
58.683547	2181.666541	20.238080
58.754207	2176.192162	20.243098
59.019281	2181.565068	20.248115
59.076887	2181.841457	20.253133
58.704080	2180.072121	20.258151
58.729877	2180.404960	20.263168
59.135300	2184.814834	20.268186
59.000935	2213.261728	20.273203
59.292658	2206.631799	20.278221
58.717820	2213.843455	20.283239
59.050711	2214.655778	20.288256
59.415115	2212.035208	20.293274
59.462908	2218.891792	20.298291
59.632590	2207.166149	20.303309
59.544167	2221.156551	20.308327
59.623996	2210.396605	20.313344
59.852574	2212.727825	20.318362
59.459585	2217.942770	20.323379
59.629377	2221.033358	20.328397
60.074279	2235.767381	20.333415
59.543686	2235.872261	20.338432
60.177185	2241.577897	20.343450
60.102888	2236.714922	20.348467
60.252743	2228.888353	20.353485
60.228732	2236.145037	20.358503
60.193740	2236.446996	20.363520
60.465437	2230.832614	20.368538
60.288084	2233.551143	20.373555
60.286965	2233.857730	20.378573
60.441627	2228.950153	20.383591
60.708358	2229.903751	20.388608
60.731201	2230.249286	20.393626
60.724702	2249.229472	20.398643
60.856884	2248.414735	20.403661
60.795376	2263.069639	20.408679
60.983449	2259.505389	20.413696
61.338629	2257.796608	20.418714
61.159191	2266.222391	20.423731
61.114983	2265.822308	20.428749
61.478486	2261.387245	20.433767
61.360750	2245.507043	20.438784
61.646158	2230.916450	20.443802
60.833713	2239.785629	20.448819
61.340004	2245.358388	20.453837
61.119368	2257.863968	20.458855
61.023443	2259.947343	20.463872
61.389623	2261.337642	20.468890
61.100383	2259.829665	20.473907
61.481956	2254.475437	20.478925
61.470373	2274.463619	20.483943
61.453064	2279.854182	20.488960
61.966612	2283.041804	20.493978
61.567353	2287.864882	20.498995
61.981702	2276.849491	20.504013
62.156068	2273.331997	20.509031
61.903903	2277.178318	20.514048
62.182984	2272.176107	20.519066
62.126953	2277.893172	20.524083
62.199771	2287.641815	20.529101
62.398122	2306.127897	20.534119
62.318266	2302.990693	20.539136
62.728593	2294.245337	20.544154
62.512794	2303.564597	20.549171
62.999014	2306.397286	20.554189
62.869386	2302.158044	20.559207
62.790300	2302.318088	20.564224
63.305679	2295.723925	20.569242
62.797274	2296.944859	20.574259
62.954445	2299.398158	20.579277
62.955877	2298.390493	20.584295
62.849574	2299.936593	20.589312
63.322052	2294.900383	20.594330
63.071567	2303.849387	20.599347
63.324954	2292.508655	20.604365
63.336578	2298.376737	20.609383
63.253775	2292.052497	20.614400
63.312988	2289.258425	20.619418
63.120480	2290.067983	20.624435
63.296968	2290.032158	20.629453
63.155101	2293.497607	20.634471
63.412611	2300.777393	20.639488
63.659250	2307.951104	20.644506
63.723791	2311.749716	20.649523
63.676418	2314.231374	20.654541
63.941906	2310.382629	20.659559
63.897760	2316.263101	20.664576
64.034249	2313.071174	20.669594
64.089227	2316.695774	20.674611
63.947933	2320.883604	20.679629
63.878968	2305.389375	20.684647
64.006328	2315.710524	20.689664
64.155085	2327.406146	20.694682
64.479011	2346.281342	20.699699
64.224995	2344.317899	20.704717
64.400265	2347.406030	20.709735
64.435256	2350.387462	20.714752
64.639983	2341.682817	20.719770
64.548280	2344.060791	20.724787
64.700379	2339.853239	20.729805
64.928794	2338.615853	20.734823
64.802676	2342.764560	20.739840
65.038487	2337.973439	20.744858
65.004022	2346.720943	20.749875
65.234502	2354.470998	20.754893
65.142652	2364.403262	20.759911
65.227327	2361.290380	20.764928
65.257201	2365.011278	20.769946
65.378177	2367.790279	20.774963
65.234929	2368.880279	20.779981
65.336312	2364.044870	20.784999
65.583962	2373.516576	20.790016
65.611311	2364.804672	20.795034
65.695296	2358.911470	20.800051
65.926729	2361.073729	20.805069
65.900347	2359.805694	20.810087
65.843949	2359.700553	20.815104
65.824803	2351.614492	20.820122
65.942965	2358.976044	20.825139
65.974793	2377.910669	20.830157
66.157075	2383.447361	20.835175
66.337178	2387.186304	20.840192
66.436431	2380.795267	20.845210
66.476109	2378.590660	20.850227
66.671591	2377.837092	20.855245
67.053712	2381.556757	20.860263
66.647806	2384.636793	20.865280
66.844067	2375.372482	20.870298
66.897769	2378.379957	20.875315
66.674795	2382.939612	20.880333
66.967676	2370.430027	20.885351
66.760703	2374.977187	20.890368
67.188760	2370.946384	20.895386
66.854250	2374.887863	20.900403
66.847865	2376.797758	20.905421
66.911400	2369.051557	20.910439
66.784264	2369.320743	20.915456
66.677221	2375.172280	20.920474
66.918021	2385.461699	20.925491
67.156309	2397.007109	20.930509
67.132960	2389.548919	20.935527
66.922996	2392.250433	20.940544
67.365588	2400.950473	20.945562
67.480251	2422.542032	20.950579
67.450082	2424.461383	20.955597
67.741321	2421.456419	20.960615
67.413468	2432.525887	20.965632
67.402396	2431.654149	20.970650
67.538507	2435.415742	20.975667
67.960371	2449.698251	20.980685
68.144735	2452.085650	20.985703
68.066773	2457.871377	20.990720
68.211766	2441.799826	20.995738
68.386631	2453.477439	21.000755
68.150973	2444.732659	21.005773
68.453816	2440.726508	21.010791
68.442396	2441.657277	21.015808
68.501885	2441.316794	21.020826
68.854502	2438.413480	21.025843
68.546528	2447.098843	21.030861
68.871017	2465.133499	21.035879
68.892273	2464.377672	21.040896
69.021189	2467.884153	21.045914
69.057068	2473.348658	21.050931
68.961508	2482.203997	21.055949
69.581908	2460.305778	21.060967
69.224969	2471.441511	21.065984
69.586152	2471.822764	21.071002
69.774040	2471.104309	21.076019
69.503285	2475.999085	21.081037
69.967740	2464.335863	21.086055
70.074919	2468.257775	21.091072
69.495101	2452.988940	21.096090
69.691953	2453.673401	21.101107
69.604437	2464.370009	21.106125
69.835785	2464.436917	21.111143
69.882972	2464.883550	21.116160
69.951416	2465.641638	21.121178
70.182661	2459.808664	21.126195
69.735546	2467.927286	21.131213
69.998625	2460.090515	21.136231
69.890093	2462.137025	21.141248
69.907838	2474.992304	21.146266
70.083043	2480.099866	21.151283
70.154372	2492.428543	21.156301
70.499060	2490.385632	21.161319
70.596033	2489.366860	21.166336
70.597063	2495.026128	21.171354
70.744254	2492.844650	21.176371
70.504563	2494.030159	21.181389
70.953213	2513.013653	21.186407
70.968620	2518.570939	21.191424
71.221544	2524.208982	21.196442
71.332431	2511.993214	21.201459
70.871288	2519.681878	21.206477
71.201242	2518.922180	21.211495
71.185532	2511.367386	21.216512
71.259282	2517.797734	21.221530
71.461509	2507.470883	21.226547
71.206956	2518.740491	21.231565
71.294434	2519.674180	21.236583
71.627944	2535.527780	21.241600
71.482104	2536.072915	21.246618
71.802976	2541.105981	21.251635
71.769745	2538.098419	21.256653
71.859884	2534.363305	21.261671
72.010861	2538.880771	21.266688
71.944409	2531.369017	21.271706
71.838476	2534.578161	21.276723
72.172594	2560.989744	21.281741
72.554737	2554.173034	21.286759
72.848897	2564.928566	21.291776
72.484253	2568.917605	21.296794
73.007545	2559.625414	21.301811
72.649402	2553.124993	21.306829
72.866413	2529.967414	21.311847
73.034611	2530.392829	21.316864
72.684541	2526.008915	21.321882
72.733346	2518.903302	21.326899
73.053168	2547.848861	21.331917
73.017393	2549.014784	21.336935
73.006105	2553.569753	21.341952
73.053224	2559.859638	21.346970
72.962615	2553.558633	21.351987
72.844831	2560.374670	21.357005
73.085802	2557.666603	21.362023
73.001844	2558.823968	21.367040
72.993087	2571.979007	21.372058
73.416539	2576.543499	21.377075
73.300791	2593.985413	21.382093
73.302001	2585.981692	21.387111
73.652987	2582.377007	21.392128
73.409745	2605.515569	21.397146
73.974529	2610.518507	21.402163
73.806141	2623.863811	21.407181
74.054501	2618.250004	21.412199
74.571248	2606.765431	21.417216
74.147262	2605.011211	21.422234
74.495983	2606.754455	21.427251
74.281896	2608.993276	21.432269
74.318839	2607.745445	21.437287
74.372228	2605.173160	21.442304
74.237823	2612.621537	21.447322
74.764585	2623.584673	21.452339
74.725175	2631.851631	21.457357
74.573273	2635.520404	21.462375
75.075737	2635.158540	21.467392
74.703114	2624.128323	21.472410
75.306884	2632.878583	21.477427
74.942829	2630.865601	21.482445
75.002109	2633.077666	21.487463
74.927281	2642.399377	21.492480
75.282128	2657.181787	21.497498
75.880270	2645.129737	21.502515
75.762901	2661.197108	21.507533
75.988193	2659.931866	21.512551
75.906267	2655.458631	21.517568
75.792317	2660.288126	21.522586
76.358622	2652.795170	21.527603
76.218141	2647.447720	21.532621
76.188539	2645.636066	21.537639
76.559062	2642.728175	21.542656
76.269318	2622.813616	21.547674
76.636782	2612.425869	21.552691
76.175658	2600.933522	21.557709
76.218092	2613.047775	21.562727
76.464560	2620.189768	21.567744
76.566314	2630.106681	21.572762
76.688066	2634.272694	21.577779
76.860172	2635.797926	21.582797
76.711346	2637.034546	21.587815
76.722957	2634.632963	21.592832
76.478843	2640.277754	21.597850
76.446512	2631.122407	21.602867
76.583643	2641.638623	21.607885
76.937423	2653.579300	21.612903
76.860028	2663.920410	21.617920
76.863035	2668.179327	21.622938
77.181248	2660.995574	21.627955
77.144162	2674.667626	21.632973
77.029658	2678.104612	21.637991
77.117776	2694.015149	21.643008
77.049397	2701.217187	21.648026
77.516600	2695.942732	21.653043
77.427097	2697.209300	21.658061
77.540625	2711.924232	21.663079
77.764235	2723.095126	21.668096
78.016518	2723.024309	21.673114
78.078531	2726.200172	21.678131
78.147476	2726.841647	21.683149
78.116512	2728.369016	21.688167
78.632729	2715.154809	21.693184
78.530639	2712.853148	21.698202
78.481425	2713.336224	21.703219
78.358502	2724.106593	21.708237
78.481605	2722.083413	21.713255
78.470683	2713.330404	21.718272
78.698781	2735.239069	21.723290
79.126628	2734.443467	21.728307
79.353097	2739.371355	21.733325
79.591358	2743.970892	21.738343
79.689578	2726.723248	21.743360
79.108862	2720.415526	21.748378
79.157183	2707.350852	21.753395
79.374121	2716.517991	21.758413
79.471057	2729.272172	21.763431
79.645185	2733.477180	21.768448
79.451988	2742.316155	21.773466
79.665598	2729.743420	21.778483
79.711389	2733.902744	21.783501
79.713290	2732.185478	21.788519
80.076372	2731.317523	21.793536
79.799986	2738.661507	21.798554
79.832648	2734.336215	21.803571
79.927918	2738.456638	21.808589
79.816104	2745.466662	21.813607
80.353290	2757.243183	21.818624
80.707032	2761.282229	21.823642
80.624939	2754.506865	21.828659
80.517777	2756.699653	21.833677
80.078166	2760.742100	21.838695
80.331368	2757.371298	21.843712
80.237356	2761.960500	21.848730
80.709272	2774.109284	21.853747
80.766489	2784.871129	21.858765
80.743781	2783.772148	21.863783
80.990455	2781.367057	21.868800
80.889716	2778.292274	21.873818
81.156206	2787.950498	21.878835
81.278046	2797.727567	21.883853
81.583136	2797.686592	21.888871
81.725142	2799.547951	21.893888
81.637361	2805.215738	21.898906
81.838880	2798.531594	21.903923
81.751812	2796.104984	21.908941
81.754047	2800.577072	21.913959
82.149734	2800.373448	21.918976
81.802854	2799.736044	21.923994
81.816018	2799.765062	21.929011
81.987995	2794.158722	21.934029
81.926349	2801.998319	21.939047
82.087464	2811.256259	21.944064
82.038686	2822.874324	21.949082
82.603486	2820.562625	21.954099
83.187799	2817.385035	21.959117
82.775382	2827.084431	21.964135
83.036770	2818.969789	21.969152
82.923912	2817.355379	21.974170
82.771731	2818.565794	21.979187
82.891227	2815.636047	21.984205
82.873880	2813.428221	21.989223
83.222754	2813.373304	21.994240
83.237862	2816.196295	21.999258
83.265813	2813.907736	22.004275
82.928198	2809.432301	22.009293
83.188600	2829.276547	22.014311
83.479081	2837.346067	22.019328
83.694821	2840.364994	22.024346
83.503736	2847.909488	22.029363
83.648535	2846.499281	22.034381
83.486560	2844.692985	22.039399
83.576711	2844.136772	22.044416
83.838456	2859.396636	22.049434
83.928484	2866.680797	22.054451
84.343751	2866.470780	22.059469
84.032726	2871.764501	22.064487
84.044397	2861.302421	22.069504
84.467421	2874.848068	22.074522
84.158127	2866.996016	22.079539
84.423622	2882.315129	22.084557
84.758975	2897.011225	22.089575
84.608524	2899.106075	22.094592
84.891303	2901.311095	22.099610
84.701448	2890.410279	22.104627
85.244510	2893.307691	22.109645
85.054745	2892.154467	22.114663
85.234586	2885.799490	22.119680
85.520748	2888.938666	22.124698
85.756984	2882.271180	22.129715
85.882022	2877.961658	22.134733
85.443076	2875.553532	22.139751
85.684473	2874.776590	22.144768
85.455792	2881.887922	22.149786
85.749525	2898.428454	22.154803
86.108189	2909.056607	22.159821
85.989988	2907.244631	22.164839
86.109946	2913.182415	22.169856
86.348538	2912.192926	22.174874
86.223569	2905.649417	22.179891
86.295217	2907.303524	22.184909
86.614395	2914.946253	22.189927
86.674314	2906.312125	22.194944
86.694011	2907.283442	22.199962
86.884752	2907.373615	22.204979
87.183467	2902.019895	22.209997
86.740340	2903.390704	22.215015
86.772510	2896.944024	22.220032
86.794501	2897.309795	22.225050
86.904483	2914.857223	22.230067
87.355234	2917.970333	22.235085
87.270469	2928.311264	22.240103
87.338874	2917.342862	22.245120
87.195395	2922.262768	22.250138
87.251226	2928.430878	22.255155
87.106892	2922.849699	22.260173
87.432500	2936.056776	22.265191
88.016154	2940.598789	22.270208
87.846045	2953.343036	22.275226
87.792133	2952.649636	22.280243
88.232192	2945.182171	22.285261
88.155139	2946.707742	22.290279
88.273709	2951.244870	22.295296
88.170674	2942.712906	22.300314
88.352955	2939.042760	22.305331
88.516193	2939.035116	22.310349
88.419530	2960.069451	22.315367
88.565038	2965.880967	22.320384
88.809541	2976.665482	22.325402
88.659586	2968.119619	22.330419
88.731711	2965.863884	22.335437
88.496606	2973.772843	22.340455
88.596073	2969.629354	22.345472
89.025103	2983.020938	22.350490
89.225704	2995.916848	22.355507
89.386141	2988.036962	22.360525
89.552523	2997.935140	22.365543
89.558258	2998.061065	22.370560
89.605109	2997.749831	22.375578
89.477567	2994.142784	22.380595
89.557288	2993.133923	22.385613
89.602098	2997.189535	22.390631
89.655272	3002.284402	22.395648
89.860556	3015.098837	22.400666
89.855124	3021.940570	22.405683
90.388777	3010.741511	22.410701
90.324279	3014.926260	22.415719
90.380703	3006.805297	22.420736
90.507351	3007.396676	22.425754
90.436540	3008.071541	22.430771
90.785295	3025.438602	22.435789
90.953941	3034.778900	22.440807
90.781624	3041.615594	22.445824
90.992761	3034.405695	22.450842
90.947348	3037.732492	22.455859
91.118885	3036.952935	22.460877
91.383622	3030.798035	22.465895
91.212620	3033.091991	22.470912
91.352263	3022.284176	22.475930
91.334985	3036.870274	22.480947
91.585035	3036.069450	22.485965
91.785432	3064.265206	22.490983
91.585185	3057.617551	22.496000
92.070190	3052.535718	22.501018
92.004386	3065.075367	22.506035
92.103614	3054.280521	22.511053
91.994996	3052.609867	22.516071
91.964402	3053.891121	22.521088
92.198429	3062.064210	22.526106
92.360353	3075.531600	22.531123
92.842569	3071.490472	22.536141
92.701123	3087.990653	22.541159
93.169090	3085.451229	22.546176
93.012991	3080.148344	22.551194
93.185747	3070.828059	22.556211
93.224631	3072.386026	22.561229
93.091273	3079.181243	22.566247
93.136702	3077.518153	22.571264
93.366693	3061.196044	22.576282
93.212325	3070.171306	22.581299
93.359962	3070.531633	22.586317
93.694732	3078.485275	22.591335
93.545605	3066.764527	22.596352
94.003685	3064.858689	22.601370
93.691222	3074.854707	22.606387
93.777693	3088.811810	22.611405
93.963071	3081.094692	22.616423
93.637707	3084.172156	22.621440
94.303416	3080.171910	22.626458
93.855109	3092.233528	22.631475
94.343001	3089.801444	22.636493
94.491859	3109.997225	22.641511
94.527103	3116.431046	22.646528
94.915436	3117.211405	22.651546
94.814619	3115.516616	22.656563
94.668130	3114.784595	22.661581
94.715129	3111.698671	22.666599
94.682309	3121.135771	22.671616
94.694580	3117.735487	22.676634
94.638864	3138.267174	22.681651
95.059519	3133.760589	22.686669
95.112903	3145.235983	22.691687
95.174539	3143.569415	22.696704
95.368489	3140.405999	22.701722
95.229778	3168.703373	22.706739
95.503041	3178.657204	22.711757
95.629612	3178.413483	22.716775
95.839027	3171.588883	22.721792
96.379151	3163.687778	22.726810
96.088690	3170.952397	22.731827
96.086346	3163.868740	22.736845
96.441010	3168.473937	22.741863
96.748379	3186.385483	22.746880
96.771961	3191.039599	22.751898
96.754164	3188.873925	22.756915
97.079057	3183.105500	22.761933
97.224544	3186.727129	22.766951
97.116747	3194.331234	22.771968
97.276253	3190.743549	22.776986
97.107538	3192.751294	22.782003
97.243045	3188.856136	22.787021
97.157865	3189.296357	22.792039
97.015439	3190.694180	22.797056
97.367128	3181.634782	22.802074
97.175960	3189.601147	22.807091
97.398128	3193.430575	22.812109
97.695861	3214.147169	22.817127
97.711829	3213.117745	22.822144
97.971147	3204.346883	22.827162
97.792089	3209.589336	22.832179
98.138762	3205.900177	22.837197
98.237170	3221.863887	22.842215
98.393810	3233.143490	22.847232
98.748337	3232.862419	22.852250
98.616627	3236.197640	22.857267
99.006901	3228.312258	22.862285
99.125823	3218.934651	22.867303
99.048489	3222.472304	22.872320
99.117301	3220.140696	22.877338
98.980560	3229.185185	22.882355
98.749312	3228.679417	22.887373
99.311047	3227.908087	22.892391
99.174177	3242.250373	22.897408
99.320146	3250.566894	22.902426
99.616669	3268.020047	22.907443
99.701535	3260.497061	22.912461
99.752207	3253.124242	22.917479
99.657229	3258.522885	22.922496
99.834694	3251.963016	22.927514
99.744805	3267.507510	22.932531
100.080836	3274.208555	22.937549
99.949458	3277.996926	22.942567
99.789252	3289.430618	22.947584
100.249672	3287.194018	22.952602
100.621512	3297.358792	22.957619
100.377133	3301.439135	22.962637
100.726286	3308.668392	22.967655
100.676154	3305.747741	22.972672
101.166910	3304.748371	22.977690
101.106667	3305.667193	22.982707
101.102939	3307.694491	22.987725
101.306702	3302.429200	22.992743
101.293472	3322.998587	22.997760
101.716227	3324.264255	23.002778
101.824838	3325.410266	23.007795
101.885384	3327.312739	23.012813
101.693138	3326.062637	23.017831
101.620691	3326.340107	23.022848
101.952197	3330.336130	23.027866
101.871829	3321.569079	23.032883
101.674310	3321.930256	23.037901
102.056094	3323.092854	23.042919
101.941098	3346.062442	23.047936
102.678600	3345.584086	23.052954
102.781972	3347.334967	23.057971
102.623562	3344.243633	23.062989
102.859208	3342.970719	23.068007
102.754794	3346.717630	23.073024
103.231428	3345.439857	23.078042
102.974552	3346.125069	23.083059
102.879277	3346.550429	23.088077
103.392409	3348.647682	23.093095
103.069457	3356.970634	23.098112
103.487919	3353.905056	23.103130
103.744921	3358.224085	23.108147
103.772416	3365.879109	23.113165
103.783418	3356.431878	23.118183
103.919520	3366.629824	23.123200
104.307149	3351.926369	23.128218
103.844332	3363.291309	23.133235
103.955785	3369.699624	23.138253
104.383424	3376.649748	23.143271
104.088547	3387.397071	23.148288
104.249971	3387.610619	23.153306
104.226501	3393.400662	23.158323
104.385438	3392.917302	23.163341
104.839893	3405.798295	23.168359
104.996143	3424.056037	23.173376
104.894480	3419.169267	23.178394
104.802223	3418.208149	23.183411
104.763118	3421.538313	23.188429
105.177386	3429.936505	23.193447
105.482317	3441.681919	23.198464
105.743345	3440.861145	23.203482
105.934422	3442.069503	23.208499
105.850125	3438.294544	23.213517
106.030321	3433.028387	23.218535
106.062927	3445.376830	23.223552
106.229939	3427.879200	23.228570
106.148318	3435.993319	23.233587
106.344259	3436.210603	23.238605
106.654907	3448.544118	23.243623
106.396983	3456.551203	23.248640
107.058975	3451.563181	23.253658
106.934170	3449.210835	23.258675
106.939660	3453.534917	23.263693
107.091388	3455.049038	23.268711
106.763044	3462.922493	23.273728
107.015967	3448.554674	23.278746
107.019544	3453.227144	23.283763
107.095771	3473.149168	23.288781
107.389536	3477.262121	23.293799
107.030978	3483.715623	23.298816
107.476065	3487.841324	23.303834
107.685073	3490.902837	23.308851
107.656557	3497.640714	23.313869
107.834108	3503.401058	23.318887
107.831221	3511.489186	23.323904
108.163687	3507.990521	23.328922
108.282138	3505.394716	23.333939
108.290526	3515.214253	23.338957
108.647237	3528.238318	23.343975
108.332130	3533.589634	23.348992
108.596261	3529.349828	23.354010
108.714349	3534.958987	23.359027
108.946817	3535.641934	23.364045
108.980151	3528.074589	23.369063
109.268282	3529.886643	23.374080
109.344702	3548.243585	23.379098
109.653629	3548.842999	23.384115
109.224455	3568.526346	23.389133
109.423852	3549.161970	23.394151
109.796614	3549.988638	23.399168
109.981784	3548.672879	23.404186
110.070478	3551.621238	23.409203
109.459397	3548.747350	23.414221
109.830324	3557.455973	23.419239
109.644208	3581.664995	23.424256
110.155071	3577.665067	23.429274
110.377119	3584.573331	23.434291
110.527602	3583.194406	23.439309
110.569992	3604.001046	23.444327
110.661640	3605.982272	23.449344
110.882707	3610.869990	23.454362
111.176150	3602.726406	23.459379
110.877385	3613.605252	23.464397
110.997641	3603.493245	23.469415
111.434432	3622.117419	23.474432
111.407879	3638.318806	23.479450
111.455270	3623.485189	23.484467
111.364428	3633.768135	23.489485
111.872872	3630.251332	23.494503
111.717668	3635.046220	23.499520
111.915961	3654.350945	23.504538
112.350791	3650.437613	23.509555
112.440525	3655.638072	23.514573
112.612763	3650.640910	23.519591
112.598407	3658.885363	23.524608
112.594646	3656.816132	23.529626
112.831773	3639.288544	23.534643
112.851164	3647.425422	23.539661
112.883574	3646.361354	23.544679
112.935845	3661.764971	23.549696
113.090724	3667.763017	23.554714
113.297431	3673.365034	23.559731
113.420477	3672.423376	23.564749
114.067668	3665.026410	23.569767
113.796081	3674.901852	23.574784
113.983248	3671.524466	23.579802
113.876099	3663.459777	23.584819
113.448073	3677.561655	23.589837
113.921218	3675.556391	23.594855
113.860801	3695.548573	23.599872
113.999717	3698.625670	23.604890
114.156173	3695.217926	23.609907
114.129487	3711.620224	23.614925
114.575363	3722.550680	23.619943
114.694782	3731.888915	23.624960
114.752030	3723.169729	23.629978
114.942927	3724.346246	23.634995
114.652255	3731.246148	23.640013
115.171051	3750.327825	23.645031
115.048449	3757.705097	23.650048
115.463326	3756.288680	23.655066
115.582561	3752.194869	23.660083
115.725057	3751.443713	23.665101
116.175511	3755.763505	23.670119
116.187574	3762.885774	23.675136
116.307786	3773.895780	23.680154
116.458546	3770.511407	23.685171
116.574378	3769.978473	23.690189
116.704042	3768.580141	23.695207
116.867973	3746.836036	23.700224
116.672667	3736.163906	23.705242
116.850592	3734.354778	23.710259
117.099536	3756.654395	23.715277
117.207595	3757.694610	23.720295
116.985484	3757.657845	23.725312
116.780987	3764.419068	23.730330
117.372702	3754.353330	23.735347
117.257345	3760.954892	23.740365
117.268926	3764.661828	23.745383
117.350955	3761.769215	23.750400
117.274398	3781.976413	23.755418
117.856890	3780.464517	23.760435
117.583859	3790.286720	23.765453
117.754952	3793.091543	23.770471
117.702098	3807.681101	23.775488
117.812066	3824.327070	23.780506
118.164673	3821.595580	23.785523
118.111755	3823.846079	23.790541
118.001476	3837.421804	23.795559
118.227293	3839.593079	23.800576
118.280360	3853.475283	23.805594
118.529114	3869.368692	23.810611
118.572929	3870.479796	23.815629
118.885616	3876.570709	23.820647
119.513592	3887.476643	23.825664
119.369859	3901.350916	23.830682
120.271485	3894.377138	23.835699
119.848531	3891.840197	23.840717
120.108622	3890.878592	23.845735
120.169541	3884.253098	23.850752
120.293374	3885.315911	23.855770
120.655475	3884.152745	23.860787
120.426730	3886.825334	23.865805
120.416639	3882.866303	23.870823
120.820099	3902.597273	23.875840
120.629752	3911.830977	23.880858
121.360654	3904.574787	23.885875
121.086202	3914.945806	23.890893
121.068795	3900.704628	23.895911
121.328478	3908.017887	23.900928
121.092569	3901.770713	23.905946
121.561959	3904.529711	23.910963
121.634041	3900.446425	23.915981
121.539836	3922.195526	23.920999
121.951608	3919.130162	23.926016
121.505446	3926.555965	23.931034
122.161414	3921.854665	23.936051
121.805038	3922.403990	23.941069
122.639902	3939.423044	23.946087
122.634963	3951.577681	23.951104
122.400082	3956.845768	23.956122
122.860966	3954.638533	23.961139
122.941146	3957.739582	23.966157
123.037983	3946.447990	23.971175
122.992624	3950.636512	23.976192
123.212363	3950.544703	23.981210
123.532930	3943.434792	23.986227
123.266426	3952.602377	23.991245
123.398263	3971.838960	23.996263
123.650518	3977.336680	24.001280
123.402385	3986.416192	24.006298
123.789259	3974.837940	24.011315
123.327676	3984.252048	24.016333
123.527394	4006.841315	24.021351
124.177382	4005.472184	24.026368
123.963126	4014.249996	24.031386
124.083671	4020.937430	24.036403
124.275027	4031.321573	24.041421
124.482258	4040.934475	24.046439
124.790585	4040.890605	24.051456
124.885299	4041.747588	24.056474
125.160626	4060.768761	24.061491
125.427781	4065.701756	24.066509
125.240302	4066.755879	24.071527
125.717128	4056.033673	24.076544
125.521479	4058.302719	24.081562
125.676556	4056.682405	24.086579
125.982334	4055.401762	24.091597
125.988524	4056.274190	24.096615
126.259625	4037.050907	24.101632
126.314430	4053.566468	24.106650
126.513774	4063.173602	24.111667
126.613629	4074.580951	24.116685
126.703693	4080.410333	24.121703
126.701156	4075.371491	24.126720
126.969168	4081.720314	24.131738
127.130838	4081.911782	24.136755
127.291915	4069.768391	24.141773
127.314606	4078.809416	24.146791
127.337952	4077.607822	24.151808
127.435033	4097.046799	24.156826
127.895528	4105.177429	24.161843
127.905194	4110.192446	24.166861
127.829529	4113.893040	24.171879
128.397521	4110.007163	24.176896
128.094238	4116.046589	24.181914
128.095795	4105.759787	24.186931
128.339858	4115.068953	24.191949
128.156124	4129.261516	24.196967
128.559333	4129.627201	24.201984
128.528580	4136.242869	24.207002
128.701137	4133.974670	24.212019
128.538821	4152.232850	24.217037
128.530916	4157.399634	24.222055
129.144129	4159.951374	24.227072
129.179717	4177.041203	24.232090
129.442977	4178.316816	24.237107
130.018581	4190.335354	24.242125
129.763777	4186.704605	24.247143
129.883980	4184.028465	24.252160
129.998128	4185.423269	24.257178
130.219640	4195.417428	24.262195
130.681866	4193.440685	24.267213
130.792292	4210.683542	24.272231
131.051183	4197.212622	24.277248
131.214169	4200.998940	24.282266
131.072444	4196.029569	24.287283
131.295827	4202.392918	24.292301
131.136175	4199.229166	24.297319
131.444156	4195.421757	24.302336
131.198427	4198.131467	24.307354
131.321396	4206.095950	24.312371
131.508926	4210.330249	24.317389
131.347360	4224.738161	24.322407
131.382872	4221.371198	24.327424
131.468508	4234.072566	24.332442
131.579679	4249.548912	24.337459
132.091014	4257.690892	24.342477
132.113253	4253.863051	24.347495
132.545368	4262.434754	24.352512
132.371804	4289.757083	24.357530
132.783275	4286.709025	24.362547
133.094050	4271.817405	24.367565
133.010475	4287.019682	24.372583
133.403898	4279.744776	24.377600
133.024009	4302.488712	24.382618
133.421241	4308.898136	24.387635
133.872777	4315.797082	24.392653
133.424838	4314.064735	24.397671
133.815517	4301.858736	24.402688
133.790947	4305.005155	24.407706
134.007623	4317.071406	24.412723
134.370219	4326.525667	24.417741
134.350047	4333.852385	24.422759
134.507866	4332.237102	24.427776
134.602734	4331.591459	24.432794
134.290471	4335.749459	24.437811
134.786641	4338.176489	24.442829
134.809736	4348.999795	24.447847
134.973222	4364.313236	24.452864
135.242920	4365.416904	24.457882
135.232596	4369.943104	24.462899
135.756162	4380.622142	24.467917
135.758718	4388.915369	24.472935
136.128397	4386.208916	24.477952
136.209952	4385.801736	24.482970
136.283409	4391.605633	24.487987
136.423691	4383.072367	24.493005
136.231434	4388.157131	24.498023
136.587573	4385.395430	24.503040
137.079121	4415.568999	24.508058
136.779121	4412.780470	24.513075
137.046624	4413.067827	24.518093
136.617262	4413.796602	24.523111
137.162820	4398.497422	24.528128
137.135439	4418.978843	24.533146
137.121748	4422.066781	24.538163
137.654780	4433.721626	24.543181
137.321265	4433.551700	24.548199
137.548418	4449.047630	24.553216
137.755897	4447.146899	24.558234
137.899213	4446.937403	24.563251
138.289100	4460.346983	24.568269
138.452835	4473.374256	24.573287
138.740472	4470.271063	24.578304
139.011033	4474.701173	24.583322
139.168301	4467.707056	24.588339
139.242400	4473.017088	24.593357
138.983989	4481.048792	24.598375
139.442686	4481.107609	24.603392
139.521508	4506.533866	24.608410
139.631589	4505.488775	24.613427
139.915089	4497.334958	24.618445
140.118056	4503.071776	24.623463
139.966645	4495.382950	24.628480
140.174885	4500.947210	24.633498
140.103638	4510.863247	24.638515
140.661199	4524.758599	24.643533
140.387600	4530.920062	24.648551
140.608810	4524.168923	24.653568
140.619606	4527.952955	24.658586
140.643526	4553.953835	24.663603
140.783043	4553.124381	24.668621
141.074774	4565.354019	24.673639
141.540990	4559.769610	24.678656
141.744939	4574.707985	24.683674
141.789570	4590.381546	24.688691
141.852263	4580.760027	24.693709
141.719006	4591.971659	24.698727
141.978172	4590.230889	24.703744
141.953440	4597.606526	24.708762
142.321074	4607.748441	24.713779
142.566944	4614.352376	24.718797
142.447336	4607.753710	24.723815
142.778933	4609.343303	24.728832
143.024172	4613.554769	24.733850
142.852609	4621.402842	24.738867
143.430649	4624.538546	24.743885
143.273232	4634.876879	24.748903
143.650543	4629.721416	24.753920
143.130397	4626.514881	24.758938
143.492999	4639.978747	24.763955
143.946523	4650.923948	24.768973
143.934174	4662.344001	24.773991
143.855504	4656.552865	24.779008
144.240246	4657.046844	24.784026
143.903410	4673.370370	24.789043
144.263347	4674.129136	24.794061
144.239226	4688.235135	24.799079
144.507050	4704.639720	24.804096
144.741644	4715.096702	24.809114
144.796999	4717.393588	24.814131
145.536822	4728.993940	24.819149
145.504848	4740.006984	24.824167
145.512254	4738.559898	24.829184
146.056922	4735.815752	24.834202
145.723464	4738.084870	24.839219
146.330868	4745.070034	24.844237
146.185793	4752.012823	24.849255
146.605940	4753.893342	24.854272
146.944380	4757.248307	24.859290
146.592050	4759.561506	24.864307
147.273115	4759.407098	24.869325
146.740717	4754.013157	24.874343
147.253023	4769.047938	24.879360
147.557626	4772.956648	24.884378
147.378926	4780.288556	24.889395
147.742843	4774.548534	24.894413
147.666234	4782.536903	24.899431
147.659423	4774.243569	24.904448
147.624704	4802.492019	24.909466
147.609631	4809.746446	24.914483
148.138461	4809.638507	24.919501
148.366395	4819.349268	24.924519
148.410674	4834.600998	24.929536
148.845747	4838.435357	24.934554
148.761339	4846.278562	24.939571
149.215784	4842.772801	24.944589
149.539436	4858.813115	24.949607
149.411084	4867.208599	24.954624
149.444375	4864.341968	24.959642
149.630083	4873.280855	24.964659
149.899276	4866.253855	24.969677
149.862337	4877.771857	24.974695
149.989164	4878.636958	24.979712
150.071282	4887.116529	24.984730
150.268957	4889.248116	24.989747
150.322317	4889.466191	24.994765
150.466222	4921.553790	24.999783
150.713231	4913.851562	25.004800
151.175407	4912.515820	25.009818
151.046122	4922.801641	25.014835
151.616798	4921.030526	25.019853
151.621953	4935.116148	25.024871
151.831377	4941.299395	25.029888
152.368672	4932.691438	25.034906
152.127177	4943.612515	25.039923
152.366523	4939.229557	25.044941
152.425597	4929.834456	25.049959
152.216122	4937.534599	25.054976
152.636879	4926.392654	25.059994
152.315090	4952.909006	25.065011
152.880720	4952.887119	25.070029
152.979235	4964.117348	25.075047
152.857681	4966.355352	25.080064
153.115666	4956.860359	25.085082
153.241485	4969.624188	25.090099
153.244548	4981.775934	25.095117
153.430637	4992.857010	25.100135
153.272128	4992.075300	25.105152
153.755364	5003.817574	25.110170
153.989378	5021.074724	25.115187
154.202534	5019.535268	25.120205
154.371763	5019.160025	25.125223
154.502491	5037.725120	25.130240
154.765551	5036.015948	25.135258
154.646221	5039.985462	25.140275
155.135465	5039.921093	25.145293
155.593864	5048.632216	25.150311
155.398247	5061.327264	25.155328
155.547895	5064.943523	25.160346
155.541632	5073.681974	25.165363
155.806859	5059.919443	25.170381
155.922545	5071.610785	25.175399
156.113309	5089.488690	25.180416
156.031084	5091.147635	25.185434
156.225482	5093.471173	25.190451
156.081385	5100.515550	25.195469
156.664401	5112.450092	25.200487
156.804681	5127.071117	25.205504
157.342058	5125.222798	25.210522
157.117732	5139.624610	25.215539
157.559229	5142.055309	25.220557
157.813177	5138.527549	25.225575
157.646752	5141.759051	25.230592
157.799585	5143.742158	25.235610
158.188937	5155.481975	25.240627
158.166121	5161.229638	25.245645
158.851235	5166.016603	25.250663
159.001776	5169.401192	25.255680
159.357747	5159.789045	25.260698
158.764339	5172.609108	25.265715
159.018288	5164.138509	25.270733
159.296865	5175.613154	25.275751
159.150492	5197.108423	25.280768
159.372063	5184.901390	25.285786
159.662381	5191.506874	25.290803
159.934899	5212.323226	25.295821
159.824257	5219.393620	25.300839
159.839574	5224.623066	25.305856
160.151048	5215.444333	25.310874
159.856568	5243.467228	25.315891
160.037791	5243.270349	25.320909
160.484060	5252.357696	25.325927
160.514663	5274.939772	25.330944
160.939099	5274.682150	25.335962
161.042983	5290.864827	25.340979
161.755043	5294.079294	25.345997
161.878331	5289.953304	25.351015
161.708651	5304.010708	25.356032
161.901743	5295.723383	25.361050
162.167976	5298.793502	25.366067
162.270653	5320.792713	25.371085
162.633029	5319.349812	25.376103
162.873850	5328.227854	25.381120
162.894710	5321.549713	25.386138
162.835731	5319.084980	25.391155
163.163788	5320.676022	25.396173
163.264862	5308.579416	25.401191
163.011551	5336.422391	25.406208
163.207531	5336.520776	25.411226
163.284160	5348.542487	25.416243
163.683971	5349.400225	25.421261
163.909366	5359.481119	25.426279
164.145809	5370.847107	25.431296
164.155878	5374.937834	25.436314
164.454255	5372.215457	25.441331
164.444591	5367.445160	25.446349
164.718923	5374.998473	25.451367
164.608154	5388.157800	25.456384
164.975547	5395.071945	25.461402
165.055314	5408.879433	25.466419
165.429952	5425.872745	25.471437
165.709043	5414.414461	25.476455
165.679593	5419.205608	25.481472
165.963768	5427.958390	25.486490
166.564242	5427.530644	25.491507
166.657060	5439.270937	25.496525
166.895486	5434.717877	25.501543
166.675384	5448.763280	25.506560
166.846328	5431.613644	25.511578
167.158278	5423.167959	25.516595
167.083767	5435.142301	25.521613
167.283657	5443.519189	25.526631
167.262086	5459.181735	25.531648
167.469673	5459.725551	25.536666
167.377175	5467.211262	25.541683
167.497061	5482.602321	25.546701
167.584621	5489.548660	25.551719
167.342319	5516.812824	25.556736
167.939922	5519.306738	25.561754
168.088068	5540.049603	25.566771
168.083633	5557.981623	25.571789
168.937450	5572.320321	25.576807
168.911151	5575.048277	25.581824
169.372175	5580.637230	25.586842
169.539323	5592.370845	25.591859
169.561142	5605.934492	25.596877
170.062842	5594.081655	25.601895
170.155519	5598.221771	25.606912
170.432649	5601.389383	25.611930
170.575099	5595.516399	25.616947
170.367656	5616.533250	25.621965
171.141655	5616.562720	25.626983
171.149398	5628.643306	25.632000
171.364920	5621.159388	25.637018
171.534812	5627.462866	25.642035
171.116438	5624.648033	25.647053
171.689254	5623.884619	25.652071
171.643538	5641.195851	25.657088
171.734780	5643.045875	25.662106
172.262964	5644.830648	25.667123
172.329562	5647.332161	25.672141
172.896284	5657.244898	25.677159
172.915542	5666.393730	25.682176
173.149167	5665.620311	25.687194
173.167461	5661.076852	25.692212
173.120724	5667.175205	25.697229
173.493350	5663.956898	25.702247
173.265630	5668.636028	25.707264
173.588746	5680.933801	25.712282
174.016045	5689.948147	25.717300
174.088716	5690.429247	25.722317
174.096779	5686.871190	25.727335
174.066146	5703.502655	25.732352
174.138038	5715.690827	25.737370
174.474346	5717.894090	25.742388
174.349519	5727.302306	25.747405
174.668193	5732.137514	25.752423
174.944416	5753.760477	25.757440
175.065035	5752.574943	25.762458
175.204983	5756.878973	25.767476
175.316127	5780.418770	25.772493
175.507014	5784.267801	25.777511
175.774907	5783.260297	25.782528
175.950569	5801.245475	25.787546
176.498907	5817.018802	25.792564
176.410091	5811.101327	25.797581
176.482033	5820.025721	25.802599
176.651278	5847.096302	25.807616
176.543901	5845.695685	25.812634
176.892538	5848.686899	25.817652
177.041728	5862.596706	25.822669
177.408547	5865.637683	25.827687
177.211941	5883.942136	25.832704
177.901194	5887.203037	25.837722
178.175177	5889.097660	25.842740
178.409962	5889.766946	25.847757
178.790088	5893.386983	25.852775
178.761988	5910.645974	25.857792
178.802384	5907.070700	25.862810
179.105202	5908.188690	25.867828
178.922478	5914.070217	25.872845
179.219310	5933.509899	25.877863
179.494383	5937.264693	25.882880
179.533388	5942.658218	25.887898
179.869496	5953.954570	25.892916
179.677415	5970.661876	25.897933
179.994887	5966.327925	25.902951
180.028771	5987.774735	25.907968
180.407006	5988.523454	25.912986
180.836338	5995.919873	25.918004
180.895919	6012.250033	25.923021
181.294328	6019.920948	25.928039
181.428540	6028.776868	25.933056
181.447405	6027.995668	25.938074
181.774534	6043.171023	25.943092
181.837658	6057.165349	25.948109
182.032386	6056.800827	25.953127
181.960800	6065.610500	25.958144
182.670520	6077.930431	25.963162
182.880212	6076.909704	25.968180
182.547131	6078.017991	25.973197
182.992557	6091.824611	25.978215
183.379516	6103.771893	25.983232
183.323798	6104.969733	25.988250
183.731569	6094.317448	25.993268
183.718182	6115.444606	25.998285
184.222124	6121.314131	26.003303
184.236095	6138.158415	26.008320
184.224314	6137.230272	26.013338
184.619255	6122.092994	26.018356
184.683265	6148.464775	26.023373
184.933173	6150.323247	26.028391
184.935165	6157.400616	26.033408
185.045036	6155.442596	26.038426
185.379438	6181.783845	26.043444
185.491889	6193.784518	26.048461
185.786452	6186.051748	26.053479
185.700004	6204.935355	26.058496
185.617767	6217.278603	26.063514
186.076779	6218.808679	26.068532
186.116904	6230.641774	26.073549
186.358091	6254.012672	26.078567
186.599049	6247.421360	26.083584
186.663030	6263.628181	26.088602
186.971561	6271.585832	26.093620
187.324118	6279.199092	26.098637
187.716953	6285.928265	26.103655
187.655693	6299.028956	26.108672
187.735341	6304.900271	26.113690
188.080870	6294.929220	26.118708
188.001028	6314.967323	26.123725
188.028084	6323.631637	26.128743
188.454593	6327.199990	26.133760
188.545017	6360.773822	26.138778
188.553869	6355.702435	26.143796
188.885308	6384.311329	26.148813
189.368569	6388.358635	26.153831
189.228800	6388.164479	26.158848
189.580962	6404.519857	26.163866
189.792195	6422.872406	26.168884
189.951333	6418.059670	26.173901
189.845508	6433.277935	26.178919
190.384331	6451.891340	26.183936
190.165091	6455.332699	26.188954
190.457996	6468.629305	26.193972
191.247021	6476.662678	26.198989
191.573695	6491.442356	26.204007
191.930642	6498.482379	26.209024
192.090529	6500.036014	26.214042
192.280039	6498.183701	26.219060
192.480473	6497.648095	26.224077
192.646928	6495.950827	26.229095
192.773139	6515.347797	26.234112
192.642736	6524.568373	26.239130
193.084609	6520.829615	26.244148
193.073451	6533.314144	26.249165
193.023443	6536.224199	26.254183
192.904146	6550.155431	26.259200
193.595672	6571.287793	26.264218
193.757686	6574.885814	26.269236
194.211832	6582.546202	26.274253
194.273781	6592.105955	26.279271
194.653347	6598.225457	26.284288
194.464353	6611.029342	26.289306
194.934637	6609.077762	26.294324
194.988438	6620.933301	26.299341
195.121374	6630.622314	26.304359
195.554332	6624.925337	26.309376
195.373261	6639.283541	26.314394
195.643574	6659.863511	26.319412
195.707872	6673.044544	26.324429
196.024133	6684.789729	26.329447
196.600674	6693.508205	26.334464
196.535154	6701.733577	26.339482
196.948976	6709.561384	26.344500
197.191660	6719.840352	26.349517
197.382742	6732.526277	26.354535
197.890090	6726.597980	26.359552
197.272819	6726.231608	26.364570
197.810040	6735.344931	26.369588
197.563721	6739.598180	26.374605
197.841874	6764.259404	26.379623
198.096812	6776.075460	26.384640
198.074025	6789.747539	26.389658
198.490028	6797.148118	26.394676
198.328014	6819.479155	26.399693
198.926836	6837.685316	26.404711
199.353887	6846.217532	26.409728
199.334902	6853.331766	26.414746
199.556013	6865.512662	26.419764
199.927322	6866.611508	26.424781
200.034059	6875.798542	26.429799
200.251312	6885.371357	26.434816
200.479064	6896.106604	26.439834
200.564320	6902.263133	26.444852
200.527647	6913.363535	26.449869
200.992171	6916.017554	26.454887
201.163092	6928.625845	26.459904
201.198312	6942.314445	26.464922
201.740205	6956.493385	26.469940
201.758172	6962.340497	26.474957
201.704268	6971.469113	26.479975
202.187387	6981.851014	26.484992
202.223621	7000.385224	26.490010
202.621128	7000.248619	26.495028
202.766437	7018.960135	26.500045
202.884918	7033.329753	26.505063
203.368131	7034.480189	26.510080
203.570235	7047.706458	26.515098
203.604035	7061.473376	26.520116
203.597888	7063.653971	26.525133
203.563972	7077.914167	26.530151
204.018988	7083.820512	26.535168
203.980886	7102.030023	26.540186
204.606596	7116.541020	26.545204
204.784098	7137.372489	26.550221
204.969181	7145.918145	26.555239
205.416640	7151.314565	26.560256
205.476186	7166.276941	26.565274
205.980161	7163.901462	26.570292
206.150383	7174.704711	26.575309
206.030456	7196.915884	26.580327
206.562264	7195.607035	26.585344
206.350158	7203.364634	26.590362
206.722193	7216.948875	26.595380
206.924510	7221.084657	26.600397
206.962042	7233.026841	26.605415
207.464255	7241.783133	26.610432
207.295089	7251.326406	26.615450
207.464373	7271.211045	26.620468
207.905912	7285.268262	26.625485
208.206864	7295.196891	26.630503
208.867051	7308.071066	26.635520
208.761245	7314.308221	26.640538
208.571448	7324.793872	26.645556
209.381002	7330.732200	26.650573
209.129505	7343.921171	26.655591
209.438195	7350.266163	26.660608
209.489175	7375.816646	26.665626
209.551101	7379.039152	26.670644
210.090916	7391.144848	26.675661
210.130963	7404.542390	26.680679
210.452877	7412.073839	26.685696
210.761048	7438.831907	26.690714
210.852461	7435.828372	26.695732
211.279490	7455.131792	26.700749
210.944597	7469.589463	26.705767
211.601509	7482.017702	26.710784
211.753662	7493.563013	26.715802
211.821502	7501.865969	26.720820
212.173618	7517.568721	26.725837
212.040595	7536.481311	26.730855
212.667403	7537.729320	26.735872
212.680195	7561.151771	26.740890
213.050550	7554.647990	26.745908
213.521520	7568.010565	26.750925
213.523556	7591.137879	26.755943
214.164519	7581.317983	26.760960
214.274994	7597.939887	26.765978
214.381781	7574.038544	26.770996
214.618998	7598.065868	26.776013
214.465869	7611.061543	26.781031
214.967083	7607.805025	26.786048
215.169526	7611.446214	26.791066
215.274759	7619.097916	26.796084
215.527479	7631.124505	26.801101
215.774170	7641.438854	26.806119
216.100990	7635.968620	26.811136
216.421461	7639.320096	26.816154
216.336302	7659.260734	26.821172
216.576390	7663.944921	26.826189
216.224987	7675.320088	26.831207
216.877115	7677.317747	26.836224
217.300193	7691.462666	26.841242
217.015037	7702.502352	26.846260
217.233666	7705.077485	26.851277
217.338583	7732.676304	26.856295
218.058662	7733.200744	26.861312
218.003478	7752.399244	26.866330
218.196140	7771.344057	26.871348
218.321021	7785.928340	26.876365
218.730910	7802.670248	26.881383
218.958011	7802.623291	26.886400
218.850190	7814.936566	26.891418
219.327408	7839.759495	26.896436
219.742903	7837.322161	26.901453
219.418052	7857.120765	26.906471
219.976609	7866.885011	26.911488
220.031405	7884.905954	26.916506
220.497173	7908.734431	26.921524
221.015306	7914.972508	26.926541
221.117408	7933.278704	26.931559
221.413511	7942.453123	26.936576
221.434297	7954.564828	26.941594
221.407701	7974.802586	26.946612
221.987422	7971.180103	26.951629
222.131774	8008.122273	26.956647
222.401677	8000.832258	26.961664
222.625928	8017.717767	26.966682
222.887253	8034.115861	26.971700
223.157801	8027.446450	26.976717
223.387839	8041.309338	26.981735
223.883698	8052.270384	26.986752
224.170758	8055.688135	26.991770
224.233610	8063.100511	26.996788
224.566542	8072.009749	27.001805
224.419180	8081.998120	27.006823
224.674947	8082.091360	27.011840
224.802249	8103.384557	27.016858
225.400755	8111.526724	27.021876
225.753045	8108.181329	27.026893
225.416751	8141.153694	27.031911
225.843216	8134.085046	27.036928
225.907913	8150.511084	27.041946
226.219013	8162.983716	27.046964
226.193599	8156.220668	27.051981
226.275954	8189.772126	27.056999
226.660136	8192.041078	27.062016
226.681456	8213.396867	27.067034
227.287569	8230.766071	27.072052
227.416132	8245.525040	27.077069
227.557601	8267.538459	27.082087
228.362121	8274.702117	27.087104
228.495606	8282.165920	27.092122
228.544946	8291.702786	27.097140
228.843475	8283.659559	27.102157
228.839351	8310.058808	27.107175
229.043167	8318.508254	27.112192
229.006571	8321.186396	27.117210
229.282089	8344.658668	27.122228
229.886366	8350.463583	27.127245
229.626693	8360.197377	27.132263
229.756741	8378.454556	27.137280
230.288550	8385.876099	27.142298
230.468910	8407.049060	27.147316
230.530398	8411.106849	27.152333
230.824757	8433.322055	27.157351
230.899266	8449.244986	27.162368
231.580441	8463.488085	27.167386
231.705196	8484.182741	27.172404
232.002083	8503.368762	27.177421
232.190174	8517.298877	27.182439
232.470493	8520.739902	27.187456
232.729531	8540.469473	27.192474
232.662119	8549.624859	27.197492
233.323439	8561.730244	27.202509
233.517771	8574.663666	27.207527
233.681907	8587.392557	27.212544
233.982625	8593.439237	27.217562
233.895656	8611.164642	27.222580
234.364473	8626.924007	27.227597
234.409195	8643.780818	27.232615
234.408188	8651.256817	27.237632
235.015569	8667.864535	27.242650
234.896959	8677.840641	27.247668
235.459176	8696.181039	27.252685
235.982530	8711.973999	27.257703
235.969486	8730.985515	27.262720
236.436382	8739.132463	27.267738
236.390873	8751.163578	27.272756
236.782012	8770.693534	27.277773
237.089246	8788.578388	27.282791
237.389412	8799.301359	27.287808
237.652975	8803.888255	27.292826
237.711805	8810.859711	27.297844
237.878662	8819.633008	27.302861
238.312286	8836.551684	27.307879
238.428636	8852.756411	27.312896
238.722947	8865.650673	27.317914
238.420111	8882.838624	27.322932
239.042877	8893.074198	27.327949
239.298602	8915.126313	27.332967
239.888961	8922.925996	27.337984
240.038372	8926.379328	27.343002
239.869248	8950.012751	27.348020
240.527969	8946.950470	27.353037
240.714830	8967.547241	27.358055
241.134986	8988.765566	27.363072
241.282643	8997.113595	27.368090
241.559935	9004.526358	27.373108
241.701357	9012.587103	27.378125
242.095394	9024.074576	27.383143
242.098770	9045.655021	27.388160
242.634834	9045.732592	27.393178
242.827947	9067.551074	27.398196
243.190869	9076.878156	27.403213
243.280109	9084.055032	27.408231
243.409115	9095.450933	27.413248
243.366977	9106.362334	27.418266
243.677600	9116.418121	27.423284
243.868272	9125.022211	27.428301
244.069531	9147.268002	27.433319
244.335183	9159.717427	27.438336
244.689175	9170.291514	27.443354
244.392701	9191.226974	27.448372
244.447261	9194.141471	27.453389
244.755162	9213.749557	27.458407
245.118079	9233.942545	27.463424
245.648016	9243.956592	27.468442
245.751994	9264.870761	27.473460
246.333552	9285.880785	27.478477
246.538233	9296.722309	27.483495
246.716401	9318.213526	27.488512
246.894552	9324.250051	27.493530
247.086776	9343.914472	27.498548
247.616587	9355.884677	27.503565
247.584843	9376.100636	27.508583
247.939357	9395.788673	27.513600
248.228701	9413.521994	27.518618
248.605483	9423.251120	27.523636
248.996499	9424.340592	27.528653
249.304639	9446.793624	27.533671
249.425801	9450.611765	27.538688
250.270776	9473.243816	27.543706
250.114641	9486.598376	27.548724
250.217208	9479.813583	27.553741
250.285888	9500.912731	27.558759
250.397951	9509.901879	27.563776
250.757885	9527.770170	27.568794
250.830081	9537.799517	27.573812
251.227775	9563.727812	27.578829
251.622308	9570.829159	27.583847
251.604253	9597.273010	27.588864
252.023485	9599.987774	27.593882
252.081115	9629.691655	27.598900
252.154539	9642.488396	27.603917
252.848123	9651.629516	27.608935
253.300920	9665.252899	27.613952
253.706297	9675.081434	27.618970
253.739642	9693.547556	27.623988
254.205541	9703.121871	27.629005
254.557993	9718.774743	27.634023
254.763348	9726.536142	27.639040
255.117579	9736.942763	27.644058
255.108727	9748.006650	27.649076
255.223543	9755.542770	27.654093
255.569543	9781.294053	27.659111
255.766417	9784.192190	27.664128
256.176110	9795.949420	27.669146
256.101200	9811.506900	27.674164
256.554140	9830.831756	27.679181
256.789496	9839.422531	27.684199
256.533699	9854.712993	27.689216
257.177466	9864.194149	27.694234
257.396776	9891.193987	27.699252
257.513200	9912.734036	27.704269
258.166534	9927.355692	27.709287
258.421363	9942.034662	27.714304
258.711232	9949.107023	27.719322
259.077280	9973.540436	27.724340
259.571935	9973.402710	27.729357
260.223940	9985.263350	27.734375
259.885268	9997.799285	27.739392
259.987107	9990.848956	27.744410
260.172740	10006.797581	27.749428
260.372230	10025.372085	27.754445
260.628332	10031.425123	27.759463
260.654240	10050.148138	27.764480
260.719052	10063.870751	27.769498
261.173657	10092.343013	27.774516
261.603339	10099.050382	27.779533
261.602625	10123.001139	27.784551
261.862594	10141.709937	27.789568
262.206252	10150.284527	27.794586
262.078467	10161.843443	27.799604
262.888816	10181.020534	27.804621
263.210145	10188.956764	27.809639
263.224484	10211.006501	27.814656
263.898557	10215.945763	27.819674
263.533566	10244.088361	27.824692
263.679039	10258.968500	27.829709
264.402925	10271.108162	27.834727
264.470221	10293.517163	27.839744
264.769054	10305.538134	27.844762
265.032611	10330.151348	27.849780
265.371839	10345.927560	27.854797
265.591347	10359.078061	27.859815
265.952147	10376.325555	27.864832
266.465160	10404.264004	27.869850
266.363152	10407.405537	27.874868
266.599369	10431.152873	27.879885
267.073559	10433.806688	27.884903
266.945305	10460.594787	27.889920
267.396572	10480.906289	27.894938
267.846239	10490.235596	27.899956
267.936886	10510.624951	27.904973
268.682692	10539.218399	27.909991
268.779423	10550.708914	27.915008
269.043073	10560.347950	27.920026
269.625935	10579.348882	27.925044
269.435404	10603.773754	27.930061
270.041137	10603.287532	27.935079
269.810596	10619.542797	27.940096
270.502887	10641.130307	27.945114
270.545717	10658.318865	27.950132
270.608215	10686.885449	27.955149
271.176317	10687.719587	27.960167
271.439415	10716.396406	27.965184
271.396517	10721.586081	27.970202
271.504827	10748.095203	27.975220
271.835533	10775.686306	27.980237
272.461718	10785.084258	27.985255
272.565950	10813.623674	27.990272
273.258105	10828.571415	27.995290
273.586450	10844.742270	28.000308
274.034690	10864.241690	28.005325
274.243546	10873.280182	28.010343
274.148472	10893.840216	28.015360
274.853136	10904.050924	28.020378
275.185595	10918.780965	28.025396
275.029719	10922.771374	28.030413
275.450042	10938.605651	28.035431
275.288329	10956.387766	28.040448
276.064497	10971.589608	28.045466
276.159565	10987.202021	28.050484
276.570519	11007.980975	28.055501
276.614776	11019.818504	28.060519
276.614058	11048.404070	28.065536
276.990068	11059.242848	28.070554
277.277672	11084.641889	28.075572
277.267924	11117.972042	28.080589
277.718878	11134.332466	28.085607
277.593349	11161.768116	28.090624
277.902073	11180.547262	28.095642
278.747990	11206.605706	28.100660
278.883684	11225.311123	28.105677
279.495308	11242.606268	28.110695
279.728271	11263.812104	28.115712
279.678369	11278.813767	28.120730
280.643858	11293.546516	28.125748
280.588155	11306.960801	28.130765
280.768924	11311.481762	28.135783
280.938292	11337.108772	28.140800
281.102182	11349.008678	28.145818
281.537592	11369.623322	28.150836
281.446839	11385.704942	28.155853
282.162598	11396.711467	28.160871
282.248460	11422.927591	28.165888
282.722352	11440.627084	28.170906
282.979127	11456.247850	28.175924
283.224272	11471.134668	28.180941
283.336476	11482.499587	28.185959
283.752850	11507.064876	28.190976
283.918607	11526.036697	28.195994
284.430286	11540.602123	28.201012
284.792187	11561.511245	28.206029
284.924756	11569.956079	28.211047
285.157453	11593.652132	28.216064
285.516481	11611.255794	28.221082
286.132203	11628.605829	28.226100
285.878719	11637.291090	28.231117
286.522502	11648.040243	28.236135
286.824387	11670.982758	28.241152
287.043915	11693.885361	28.246170
287.588290	11708.089396	28.251188
287.679901	11728.153149	28.256205
287.850146	11747.833598	28.261223
288.032367	11764.213932	28.266240
288.438591	11785.820391	28.271258
288.824860	11797.437992	28.276276
288.919752	11825.462298	28.281293
289.487059	11837.492763	28.286311
289.414753	11852.914678	28.291328
289.772815	11875.350228	28.296346
290.067293	11887.336070	28.301364
290.586815	11915.586496	28.306381
291.090563	11935.495615	28.311399
290.947632	11955.765510	28.316416
291.492049	11971.840272	28.321434
291.893558	11987.355650	28.326452
292.145253	12012.131761	28.331469
292.512488	12018.123818	28.336487
292.581458	12033.867627	28.341504
292.947615	12050.752010	28.346522
293.125397	12066.364379	28.351540
293.250101	12087.214166	28.356557
293.458038	12101.034580	28.361575
294.057815	12133.808934	28.366592
294.224760	12146.848254	28.371610
294.624401	12160.414793	28.376628
294.657850	12187.836893	28.381645
294.887046	12210.475459	28.386663
294.947935	12225.376137	28.391680
295.410913	12254.719122	28.396698
295.969711	12273.611001	28.401716
296.197708	12302.539123	28.406733
296.673200	12321.547278	28.411751
296.958023	12344.351743	28.416768
297.237863	12372.150972	28.421786
297.851829	12370.678435	28.426804
297.836626	12397.270583	28.431821
298.624512	12410.205755	28.436839
298.851850	12426.728998	28.441856
298.786521	12446.260183	28.446874
299.269520	12458.695884	28.451892
299.907838	12479.082948	28.456909
299.880573	12501.920384	28.461927
299.950538	12504.509088	28.466944
299.976047	12528.162008	28.471962
300.833136	12527.730267	28.476980
300.854713	12555.424427	28.481997
300.986037	12574.395295	28.487015
301.279331	12590.441325	28.492032
301.394534	12601.912116	28.497050
301.970657	12622.200920	28.502068
302.296842	12646.522846	28.507085
302.507042	12664.915019	28.512103
302.589588	12683.244822	28.517120
302.837609	12710.900187	28.522138
303.376378	12715.480476	28.527156
303.588681	12748.567626	28.532173
303.989303	12768.824203	28.537191
304.299029	12790.312448	28.542208
304.239942	12807.567430	28.547226
304.540631	12828.702643	28.552244
304.897320	12865.401747	28.557261
305.365331	12889.717895	28.562279
305.806286	12908.576440	28.567296
305.948875	12941.614061	28.572314
306.734264	12943.386283	28.577332
306.748191	12958.887951	28.582349
306.924552	12989.288295	28.587367
307.303675	13012.119062	28.592384
307.423084	13037.498574	28.597402
308.143883	13059.079876	28.602420
308.328986	13078.472658	28.607437
308.772567	13100.706635	28.612455
308.982298	13113.437069	28.617472
309.183785	13138.818912	28.622490
309.733048	13150.837585	28.627508
309.774429	13179.180388	28.632525
309.865886	13200.457881	28.637543
310.475628	13221.421101	28.642560
310.876519	13255.024915	28.647578
311.081280	13276.247506	28.652596
311.469379	13304.971251	28.657613
311.667927	13320.122784	28.662631
312.094290	13344.033606	28.667648
312.226799	13357.870727	28.672666
312.679977	13386.334842	28.677684
312.958547	13413.707399	28.682701
313.336237	13437.933728	28.687719
313.789284	13461.332845	28.692736
313.841646	13486.292338	28.697754
314.141520	13503.899967	28.702772
314.634057	13528.933230	28.707789
314.661494	13544.880795	28.712807
315.232873	13574.826002	28.717824
315.388722	13602.474497	28.722842
315.866666	13623.601890	28.727860
316.467263	13647.760115	28.732877
316.645018	13671.116845	28.737895
317.290486	13686.522549	28.742912
317.138365	13709.029318	28.747930
317.711106	13729.900031	28.752948
318.100148	13740.774700	28.757965
318.451900	13761.852240	28.762983
318.716206	13773.015496	28.768000
318.631442	13805.539322	28.773018
318.909771	13821.798652	28.778036
319.115613	13849.064201	28.783053
319.518620	13873.588003	28.788071
319.995356	13894.968109	28.793088
320.083891	13915.094954	28.798106
320.648994	13937.814282	28.803124
320.626640	13967.738711	28.808141
321.132775	13991.837433	28.813159
321.383047	14011.657094	28.818176
321.090765	14049.831114	28.823194
322.122883	14065.204698	28.828212
322.271654	14091.774039	28.833229
322.699340	14110.371400	28.838247
322.937947	14130.946479	28.843264
322.947088	14154.022906	28.848282
323.439331	14172.199884	28.853300
323.697715	14203.364319	28.858317
324.066923	14230.901334	28.863335
324.611894	14256.844292	28.868352
325.082045	14287.904490	28.873370
325.443802	14298.796656	28.878388
325.822364	14322.385854	28.883405
325.974985	14347.757174	28.888423
326.653881	14363.982263	28.893440
326.797913	14375.706426	28.898458
327.441917	14410.634090	28.903476
327.659907	14426.376030	28.908493
327.851009	14441.663801	28.913511
328.404687	14461.938128	28.918528
328.627732	14485.988297	28.923546
328.821622	14498.331570	28.928564
328.935586	14517.936420	28.933581
329.494346	14552.069972	28.938599
329.735131	14561.218712	28.943616
329.772174	14591.515856	28.948634
330.048004	14617.018502	28.953652
330.822576	14650.043228	28.958669
331.033692	14673.652768	28.963687
331.336145	14688.359677	28.968704
331.611823	14728.947241	28.973722
332.045316	14744.051750	28.978740
332.231374	14770.663302	28.983757
332.698041	14808.155525	28.988775
333.167277	14823.555226	28.993792
332.820788	14846.275399	28.998810
333.538482	14871.456280	29.003828
333.844439	14898.904018	29.008845
333.870990	14930.889956	29.013863
334.190190	14957.273302	29.018880
334.771320	14995.702130	29.023898
334.796228	15020.438389	29.028916
335.322902	15045.578655	29.033933
335.391867	15078.924356	29.038951
336.208657	15108.537018	29.043968
336.307861	15132.950652	29.048986
336.718426	15171.638239	29.054004
337.111285	15197.555853	29.059021
337.190702	15223.050971	29.064039
338.302700	15253.587510	29.069056
338.637376	15284.638921	29.074074
339.003273	15305.909974	29.079092
339.346349	15329.984067	29.084109
339.662389	15346.801355	29.089127
339.992756	15381.352712	29.094144
340.463707	15391.311789	29.099162
340.818484	15411.394824	29.104180
341.222981	15427.518230	29.109197
341.505438	15448.281571	29.114215
341.772755	15468.992278	29.119232
341.955993	15491.590984	29.124250
342.178755	15511.629793	29.129268
342.642639	15525.439115	29.134285
343.123275	15561.453878	29.139303
343.270045	15580.071035	29.144320
343.600917	15608.278700	29.149338
343.746321	15621.302292	29.154356
344.380998	15651.623834	29.159373
344.470661	15670.223750	29.164391
344.801733	15676.896178	29.169408
344.766425	15705.847105	29.174426
345.429460	15735.524178	29.179444
345.663927	15765.299034	29.184461
345.567754	15788.589056	29.189479
345.653111	15817.225457	29.194496
346.665442	15850.520607	29.199514
346.462928	15879.244168	29.204532
347.072338	15910.341130	29.209549
347.099045	15946.408224	29.214567
347.945733	15973.126739	29.219584
348.282527	16009.462616	29.224602
348.564201	16044.524658	29.229620
349.261137	16072.362014	29.234637
349.441380	16105.901010	29.239655
349.869728	16129.192963	29.244672
350.615930	16159.839023	29.249690
350.897284	16180.861970	29.254708
351.182679	16211.412588	29.259725
351.783433	16226.910057	29.264743
351.871080	16245.536174	29.269760
352.594371	16267.795936	29.274778
352.621272	16293.031864	29.279796
352.942922	16311.769068	29.284813
353.105116	16347.111608	29.289831
353.441769	16372.980478	29.294848
353.954518	16403.823256	29.299866
354.302683	16439.398446	29.304884
354.681029	16456.074150	29.309901
354.612921	16496.076703	29.314919
355.615805	16515.185296	29.319936
355.677341	16533.776653	29.324954
355.847909	16564.419437	29.329972
356.200258	16589.351324	29.334989
356.527047	16624.746027	29.340007
357.040794	16651.057326	29.345024
357.429970	16680.716803	29.350042
357.837026	16711.550853	29.355060
358.429111	16725.529118	29.360077
358.141099	16765.125783	29.365095
358.645753	16787.657302	29.370112
358.946318	16826.064329	29.375130
359.575926	16857.452924	29.380148
360.078215	16892.675710	29.385165
360.365484	16921.529659	29.390183
360.732006	16941.451832	29.395200
360.842976	16973.134560	29.400218
361.128630	17009.389674	29.405236
361.740768	17030.530770	29.410253
361.883376	17065.222340	29.415271
362.450410	17089.711183	29.420288
362.994328	17120.003158	29.425306
363.277988	17145.710189	29.430324
363.727293	17171.801265	29.435341
364.156977	17211.494585	29.440359
364.280561	17226.945868	29.445376
364.866453	17265.033982	29.450394
365.033351	17284.486759	29.455412
365.412357	17306.907370	29.460429
365.298125	17350.039182	29.465447
366.290766	17377.741523	29.470464
366.446101	17411.202162	29.475482
366.565257	17447.897217	29.480500
367.168073	17471.535781	29.485517
367.336661	17506.796187	29.490535
367.918159	17525.529591	29.495552
368.352998	17555.194110	29.500570
368.602096	17591.601572	29.505588
368.827937	17608.787622	29.510605
369.001434	17635.177294	29.515623
369.629610	17655.220962	29.520640
369.990856	17693.708231	29.525658
370.181080	17727.813197	29.530676
370.681627	17749.757142	29.535693
370.974497	17774.467353	29.540711
371.186528	17810.667041	29.545728
371.743335	17845.911204	29.550746
371.855995	17879.520146	29.555764
372.619942	17917.293386	29.560781
372.610654	17947.861296	29.565799
373.133718	17977.382702	29.570816
373.593086	18009.191027	29.575834
373.922604	18050.089960	29.580852
374.365689	18070.000817	29.585869
374.476807	18103.872151	29.590887
374.982672	18146.846643	29.595904
375.353242	18182.565316	29.600922
375.705668	18214.473706	29.605940
376.657168	18238.809183	29.610957
376.464064	18279.096821	29.615975
377.091447	18303.421403	29.620992
377.468219	18336.457874	29.626010
377.879520	18381.542124	29.631028
378.363050	18398.802998	29.636045
378.588426	18430.291427	29.641063
378.879622	18458.518394	29.646080
379.256070	18497.005004	29.651098
379.926298	18536.284904	29.656116
380.140170	18567.319901	29.661133
380.595869	18606.794696	29.666151
381.082460	18637.954945	29.671168
381.669648	18666.830072	29.676186
381.532232	18708.659191	29.681204
381.807423	18736.071091	29.686221
382.421941	18777.842144	29.691239
382.802420	18798.415319	29.696256
383.272662	18829.443055	29.701274
383.653256	18867.731197	29.706292
384.300818	18895.225187	29.711309
384.660534	18929.693951	29.716327
384.654746	18961.986239	29.721344
385.409985	18989.408963	29.726362
385.517400	19035.454911	29.731380
385.902749	19063.672048	29.736397
386.059674	19100.027115	29.741415
386.314043	19131.367028	29.746432
387.053124	19169.708462	29.751450
387.193846	19200.108795	29.756468
387.572486	19240.096018	29.761485
387.883509	19288.778007	29.766503
388.176200	19316.684567	29.771520
388.922005	19356.669632	29.776538
389.307386	19391.560762	29.781556
389.919008	19426.264751	29.786573
389.900999	19462.061508	29.791591
390.293820	19502.933026	29.796608
391.063579	19536.507491	29.801626
391.452245	19573.137386	29.806644
391.857385	19607.648901	29.811661
392.307674	19631.735143	29.816679
392.731451	19671.394308	29.821696
393.454583	19688.104482	29.826714
393.708422	19722.981813	29.831732
393.895595	19758.242319	29.836749
394.263462	19784.548038	29.841767
394.636491	19805.910394	29.846784
394.962668	19826.703507	29.851802
395.560316	19864.724673	29.856820
395.943266	19881.281657	29.861837
396.368593	19914.614337	29.866855
396.210221	19942.178797	29.871872
396.716025	19959.158546	29.876890
397.101267	20007.228083	29.881908
397.690981	20032.045435	29.886925
398.259165	20057.541169	29.891943
398.259952	20101.277483	29.896960
398.719894	20130.570349	29.901978
399.353094	20168.256810	29.906996
399.390898	20198.075298	29.912013
399.818520	20234.813706	29.917031
399.973838	20274.584945	29.922048
400.583115	20312.427044	29.927066
400.591238	20361.819726	29.932084
401.392294	20403.956544	29.937101
402.266090	20429.170500	29.942119
402.338369	20469.851469	29.947136
402.692308	20495.727034	29.952154
403.121575	20531.584479	29.957172
403.625504	20567.410724	29.962189
403.858522	20601.914931	29.967207
404.058278	20655.667716	29.972224
404.838025	20681.876717	29.977242
405.179507	20725.835757	29.982260
405.659531	20761.472443	29.987277
405.985389	20810.578932	29.992295
405.897640	20845.179294	29.997312
406.532948	20881.151591	30.002330
407.172454	20927.221872	30.007348
407.487547	20969.002218	30.012365
408.087829	21009.335374	30.017383
408.179741	21047.748794	30.022400
408.861195	21080.429641	30.027418
409.037826	21122.108723	30.032436
409.423969	21157.678220	30.037453
410.307595	21191.867834	30.042471
410.419181	21237.693651	30.047488
411.040631	21261.944685	30.052506
411.358372	21301.483340	30.057524
412.113802	21337.912898	30.062541
412.589142	21370.775055	30.067559
412.806656	21418.247267	30.072576
413.529145	21444.695560	30.077594
413.741054	21472.067213	30.082612
414.024609	21518.682075	30.087629
414.562050	21545.799727	30.092647
414.602531	21592.338343	30.097664
415.528534	21613.959939	30.102682
415.850566	21655.797598	30.107700
416.250064	21692.403508	30.112717
416.990191	21716.432156	30.117735
417.377004	21743.349580	30.122752
417.422456	21774.848826	30.127770
417.768987	21803.374994	30.132788
418.013785	21844.823830	30.137805
418.609779	21886.123192	30.142823
418.735479	21924.794754	30.147840
419.576097	21960.803176	30.152858
419.392687	21994.485116	30.157876
419.917747	22034.317565	30.162893
420.633708	22072.781402	30.167911
420.672993	22115.384427	30.172928
420.926009	22152.378235	30.177946
421.619373	22195.532310	30.182964
421.935959	22239.729619	30.187981
422.401078	22269.591416	30.192999
422.767318	22306.612549	30.198016
423.315175	22340.517894	30.203034
423.418731	22375.524919	30.208052
423.957705	22421.775171	30.213069
424.496490	22451.539949	30.218087
424.778052	22504.879826	30.223104
425.663537	22534.464380	30.228122
426.004450	22577.600494	30.233140
426.056686	22612.405204	30.238157
426.427707	22644.432456	30.243175
426.822775	22690.989512	30.248192
427.102354	22735.039704	30.253210
427.655040	22781.142019	30.258228
428.360157	22822.829278	30.263245
428.911677	22863.037739	30.268263
429.116531	22903.368318	30.273280
429.775070	22933.202427	30.278298
430.491651	22978.942284	30.283316
431.013492	23021.474025	30.288333
431.651062	23053.055833	30.293351
431.641824	23099.209432	30.298368
432.226309	23127.190692	30.303386
432.885759	23162.055300	30.308404
433.079471	23201.543220	30.313421
433.636391	23229.440905	30.318439
433.971940	23264.116485	30.323456
434.330150	23293.854279	30.328474
434.802298	23335.329048	30.333492
435.346134	23378.745836	30.338509
435.996811	23405.352579	30.343527
436.131612	23455.980640	30.348544
436.492798	23488.727027	30.353562
436.906681	23519.916225	30.358580
437.360030	23567.040029	30.363597
437.879472	23598.382208	30.368615
438.110562	23644.355585	30.373632
438.512558	23686.052548	30.378650
438.817858	23723.597776	30.383668
439.247694	23774.881269	30.388685
439.743626	23808.782368	30.393703
440.163786	23865.303184	30.398720
440.591997	23899.562599	30.403738
441.492686	23948.103642	30.408756
441.722942	23988.479892	30.413773
442.535543	24018.392911	30.418791
442.803194	24066.181186	30.423808
443.029614	24101.508892	30.428826
443.972003	24136.897958	30.433844
444.276495	24181.595900	30.438861
444.741305	24213.784049	30.443879
445.231846	24249.487827	30.448896
445.524070	24280.503002	30.453914
446.096885	24314.900173	30.458932
446.241248	24351.535106	30.463949
447.034103	24387.116599	30.468967
447.024219	24430.895789	30.473984
447.854764	24464.020548	30.479002
448.434863	24501.615051	30.484020
448.511619	24534.915157	30.489037
449.303291	24574.222133	30.494055
449.352396	24616.184777	30.499072
449.909125	24648.771712	30.504090
450.314304	24689.688394	30.509108
450.732537	24730.319148	30.514125
451.320259	24753.823787	30.519143
451.463245	24787.280587	30.524160
451.846524	24822.236873	30.529178
452.285021	24852.945012	30.534196
452.579575	24897.226973	30.539213
453.284236	24946.645435	30.544231
453.204033	24988.797556	30.549248
453.687167	25030.011251	30.554266
454.205413	25078.587254	30.559284
454.663297	25122.432731	30.564301
455.366412	25161.585388	30.569319
455.636121	25206.610326	30.574336
456.195192	25250.862040	30.579354
456.661861	25295.946087	30.584372
457.162979	25339.810198	30.589389
457.508875	25380.937051	30.594407
458.060367	25422.780673	30.599424
458.335056	25485.194529	30.604442
458.999038	25517.831605	30.609460
459.464885	25566.411350	30.614477
459.640374	25612.153176	30.619495
460.229034	25657.454548	30.624512
460.926174	25713.367857	30.629530
461.140864	25746.694796	30.634548
461.109346	25802.643814	30.639565
462.201656	25847.852878	30.644583
462.716283	25902.115783	30.649600
463.069753	25949.683760	30.654618
463.697892	25990.636036	30.659636
464.533425	26040.783553	30.664653
465.200265	26073.124707	30.669671
465.220366	26120.372962	30.674688
465.942054	26162.616050	30.679706
466.075851	26212.574226	30.684724
466.219735	26252.364457	30.689741
467.279535	26300.223422	30.694759
467.754946	26335.788943	30.699776
468.149769	26385.117712	30.704794
468.240812	26420.119297	30.709812
468.852599	26478.049078	30.714829
469.478839	26519.359369	30.719847
469.903587	26567.617527	30.724864
470.184204	26619.486223	30.729882
470.752924	26656.390200	30.734900
471.252956	26714.112149	30.739917
471.996045	26749.539593	30.744935
472.384778	26803.157426	30.749952
472.594655	26856.107891	30.754970
473.191116	26895.417783	30.759988
473.416970	26941.899243	30.765005
474.243552	26986.830362	30.770023
474.572246	27036.342273	30.775040
475.041711	27088.941353	30.780058
475.645770	27121.228617	30.785076
476.243167	27166.008859	30.790093
476.666191	27212.433180	30.795111
477.175942	27258.496277	30.800128
477.228024	27299.963383	30.805146
478.200951	27349.956321	30.810164
478.399212	27401.503451	30.815181
478.939367	27451.527290	30.820199
479.756022	27498.600166	30.825216
480.176589	27522.552653	30.830234
480.883145	27562.896312	30.835252
481.166536	27609.316412	30.840269
481.742748	27652.826967	30.845287
482.155922	27700.774736	30.850304
482.315220	27738.329219	30.855322
483.348745	27762.398271	30.860340
483.822520	27807.708519	30.865357
484.220077	27838.255244	30.870375
484.665873	27869.866614	30.875392
484.897493	27909.876418	30.880410
485.305678	27938.068202	30.885428
485.406349	27982.153555	30.890445
486.029495	28025.534245	30.895463
486.591638	28063.379242	30.900480
486.731748	28114.991739	30.905498
487.474515	28164.441499	30.910516
487.479057	28221.051677	30.915533
488.449775	28268.574351	30.920551
488.964492	28309.569812	30.925568
489.339096	28361.169472	30.930586
489.704571	28394.157923	30.935604
490.233562	28456.843253	30.940621
490.879116	28498.265480	30.945639
491.502032	28544.745459	30.950656
491.868549	28597.738401	30.955674
492.533030	28640.220987	30.960692
492.811474	28681.063981	30.965709
493.196692	28735.454966	30.970727
494.203810	28776.625581	30.975744
494.275011	28832.608371	30.980762
495.154205	28865.436989	30.985780
495.199665	28926.219645	30.990797
495.941878	28973.214190	30.995815
496.278555	29019.973105	31.000832
496.705279	29079.734133	31.005850
497.716844	29121.393829	31.010868
497.769121	29181.119366	31.015885
498.005204	29230.542421	31.020903
498.770413	29268.605667	31.025920
499.185739	29332.382452	31.030938
500.203488	29382.436916	31.035956
500.537353	29437.466408	31.040973
500.658163	29490.534264	31.045991
501.321499	29544.077236	31.051008
501.745267	29592.037915	31.056026
502.058841	29633.063459	31.061044
502.771899	29697.590506	31.066061
503.112672	29747.436234	31.071079
503.945099	29798.771923	31.076096
504.522873	29860.823217	31.081114
505.151627	29908.608867	31.086132
505.335529	29958.313938	31.091149
506.101828	30009.004944	31.096167
506.671065	30054.434581	31.101184
506.969534	30114.526398	31.106202
507.531341	30161.787460	31.111220
507.848465	30204.006357	31.116237
508.609766	30259.892125	31.121255
509.230209	30311.024608	31.126272
509.697553	30371.953848	31.131290
510.369271	30411.738793	31.136308
510.934619	30457.488779	31.141325
511.412076	30517.328342	31.146343
511.993589	30553.298238	31.151360
512.205864	30610.377106	31.156378
512.739502	30655.271506	31.161396
513.456980	30701.826753	31.166413
513.873450	30752.104523	31.171431
514.563290	30795.626186	31.176448
514.696588	30843.379624	31.181466
515.321983	30890.244038	31.186484
515.687613	30941.313242	31.191501
516.270568	30992.864083	31.196519
517.079185	31031.949413	31.201536
517.183375	31082.727838	31.206554
517.724387	31121.750371	31.211572
518.198122	31160.408653	31.216589
518.663898	31215.125288	31.221607
519.312214	31263.409909	31.226624
519.602775	31313.145325	31.231642
520.321964	31362.750004	31.236660
520.791225	31399.087282	31.241677
520.859982	31442.495603	31.246695
521.519909	31502.775296	31.251712
521.824775	31561.214462	31.256730
522.512444	31623.424168	31.261748
523.174408	31672.635309	31.266765
523.708325	31728.194191	31.271783
524.224861	31781.317053	31.276800
524.591531	31849.228711	31.281818
525.409120	31893.006458	31.286836
526.039274	31953.507178	31.291853
526.527329	32009.670895	31.296871
527.198799	32044.344712	31.301888
527.423447	32112.444959	31.306906
528.154978	32151.397221	31.311924
528.554836	32214.278242	31.316941
529.290612	32267.268467	31.321959
529.607035	32318.611689	31.326976
530.178753	32373.200779	31.331994
530.818675	32426.604925	31.337012
531.140765	32481.036860	31.342029
531.757109	32540.756160	31.347047
532.424356	32597.848194	31.352064
532.828434	32664.422016	31.357082
533.481834	32701.258463	31.362100
533.781471	32763.981306	31.367117
534.438090	32817.686794	31.372135
535.235348	32878.598478	31.377152
535.573606	32940.520360	31.382170
536.161880	32997.396391	31.387188
536.734267	33050.049945	31.392205
536.889909	33119.295154	31.397223
537.507947	33167.211307	31.402240
538.140786	33235.548089	31.407258
538.898232	33296.221655	31.412276
539.359920	33350.513236	31.417293
539.761935	33407.932607	31.422311
540.760787	33458.560319	31.427328
540.989117	33518.877252	31.432346
541.593811	33567.850673	31.437364
542.283589	33626.681041	31.442381
542.859099	33680.393086	31.447399
543.343201	33735.114455	31.452416
543.679236	33793.719897	31.457434
544.228661	33851.630680	31.462452
544.832885	33909.649345	31.467469
545.124658	33967.375925	31.472487
545.909439	34014.982751	31.477504
546.398327	34079.414551	31.482522
547.392793	34136.750857	31.487540
547.938651	34185.057221	31.492557
548.041775	34248.682473	31.497575
549.041756	34299.116728	31.502592
549.365908	34356.081819	31.507610
549.796346	34411.565214	31.512628
550.557677	34470.755749	31.517645
550.785038	34523.931488	31.522663
551.851614	34574.055697	31.527680
552.293334	34624.927229	31.532698
552.509785	34684.246499	31.537716
553.411436	34728.143550	31.542733
553.702912	34780.271165	31.547751
554.290875	34823.974199	31.552768
554.733572	34882.969505	31.557786
554.899763	34929.870061	31.562804
555.816011	34988.604317	31.567821
555.991229	35038.937278	31.572839
556.786082	35096.467483	31.577856
557.277624	35153.094970	31.582874
557.892992	35210.134509	31.587892
558.419528	35263.950929	31.592909
558.880410	35319.394222	31.597927
559.629409	35377.030747	31.602944
560.298158	35436.826799	31.607962
560.375163	35496.073984	31.612980
561.079942	35557.565551	31.617997
561.336972	35629.609358	31.623015
562.064001	35688.254126	31.628032
562.614940	35743.172548	31.633050
563.410711	35814.711357	31.638068
564.185470	35871.565662	31.643085
564.503452	35931.374053	31.648103
564.998961	35980.589900	31.653120
565.685325	36040.113617	31.658138
566.187448	36106.816562	31.663156
566.993734	36164.051615	31.668173
567.314064	36234.701835	31.673191
567.961541	36301.195237	31.678208
568.542599	36355.602403	31.683226
569.024204	36428.622202	31.688244
569.799264	36486.182214	31.693261
570.547543	36559.060575	31.698279
570.981050	36608.228423	31.703296
571.896827	36667.659438	31.708314
572.083680	36727.097634	31.713332
572.892249	36784.277464	31.718349
573.109002	36853.741565	31.723367
573.658072	36911.551791	31.728384
574.326866	36979.527587	31.733402
574.574030	37035.857384	31.738420
575.782294	37114.598785	31.743437
575.897885	37183.837856	31.748455
576.570678	37240.173613	31.753472
577.374859	37302.118644	31.758490
577.486213	37367.865093	31.763508
578.475937	37444.677705	31.768525
578.927422	37501.660063	31.773543
579.723851	37573.290938	31.778560
580.371599	37634.975760	31.783578
580.681592	37697.508926	31.788596
581.431680	37764.208505	31.793613
581.764741	37832.890104	31.798631
582.447911	37892.890739	31.803648
583.155732	37956.962424	31.808666
583.524841	38028.918310	31.813684
583.997020	38089.431124	31.818701
584.702468	38161.426577	31.823719
585.098403	38232.081525	31.828736
585.670047	38291.255995	31.833754
586.394742	38368.163705	31.838772
587.417560	38427.702719	31.843789
587.857464	38500.674613	31.848807
588.537428	38562.215202	31.853824
589.340614	38619.524802	31.858842
589.897619	38690.508406	31.863860
590.570127	38735.213836	31.868877
591.104450	38807.467423	31.873895
591.472216	38863.258925	31.878912
591.934145	38919.508504	31.883930
592.501793	38984.935911	31.888948
593.134935	39022.937648	31.893965
593.818595	39101.461943	31.898983
594.203378	39157.548248	31.904000
594.804159	39206.689125	31.909018
594.880147	39281.747744	31.914036
595.624052	39339.691270	31.919053
596.096281	39408.980781	31.924071
597.090931	39473.872098	31.929088
597.855422	39537.103429	31.934106
597.960525	39599.077228	31.939124
598.925566	39673.346385	31.944141
599.367016	39743.867056	31.949159
599.759259	39805.143756	31.954176
600.568002	39864.997507	31.959194
601.112898	39941.597491	31.964212
601.845075	40005.040970	31.969229
602.477961	40075.793252	31.974247
603.084890	40151.493635	31.979264
603.718835	40204.495609	31.984282
604.253487	40282.399308	31.989300
604.906676	40357.111114	31.994317
605.299756	40425.618875	31.999335
606.050663	40490.301566	32.004352
607.042311	40559.998787	32.009370
607.287786	40630.968829	32.014388
608.170692	40698.146438	32.019405
608.616696	40769.165913	32.024423
609.392056	40835.528396	32.029440
610.544549	40894.261586	32.034458
610.622394	40967.325280	32.039476
611.492116	41030.995777	32.044493
611.928818	41090.694082	32.049511
612.162117	41159.654035	32.054528
612.907181	41223.484726	32.059546
613.697950	41294.041926	32.064564
614.291766	41355.451434	32.069581
615.176019	41431.524751	32.074599
615.630797	41498.558273	32.079616
616.269396	41561.062853	32.084634
616.785932	41643.931832	32.089652
617.825072	41696.315411	32.094669
618.455142	41761.199341	32.099687
618.923047	41827.073236	32.104704
619.587459	41892.712800	32.109722
620.119631	41961.986197	32.114740
620.800129	42023.734016	32.119757
621.103915	42096.281738	32.124775
621.534443	42173.216134	32.129792
622.482718	42236.003254	32.134810
622.625101	42317.500640	32.139828
623.444915	42381.395567	32.144845
623.929986	42455.354366	32.149863
624.473082	42520.094320	32.154880
625.675432	42599.267521	32.159898
625.841248	42671.019436	32.164916
626.544723	42743.740345	32.169933
627.126964	42823.402278	32.174951
627.490580	42897.294522	32.179968
628.503439	42960.654339	32.184986
629.191519	43056.878585	32.190004
630.113961	43107.372141	32.195021
630.512251	43183.444630	32.200039
631.066189	43257.066856	32.205056
631.690660	43327.798216	32.210074
631.908600	43409.363645	32.215092
632.863947	43477.047666	32.220109
633.719231	43548.546800	32.225127
634.066005	43612.631563	32.230144
634.601481	43669.937985	32.235162
635.324332	43743.594171	32.240180
635.978561	43811.973333	32.245197
636.537881	43878.912875	32.250215
636.854096	43945.798154	32.255232
637.593766	44019.263195	32.260250
638.070542	44098.821713	32.265268
638.958111	44166.399458	32.270285
639.500648	44239.427514	32.275303
639.904686	44318.828495	32.280320
640.966600	44393.406805	32.285338
641.299252	44472.037181	32.290356
642.230050	44539.091284	32.295373
642.635739	44612.481287	32.300391
642.998076	44698.130083	32.305408
643.815334	44769.100222	32.310426
643.999492	44870.848178	32.315444
645.083808	44938.563505	32.320461
646.143143	45027.982338	32.325479
646.853653	45110.342006	32.330496
647.420040	45179.912163	32.335514
648.186772	45263.163125	32.340532
648.646989	45338.109974	32.345549
649.670210	45416.693196	32.350567
649.687427	45497.195703	32.355584
650.314625	45573.669446	32.360602
650.817788	45652.987023	32.365620
651.682065	45738.049104	32.370637
652.399964	45825.570411	32.375655
652.827564	45917.639965	32.380672
654.039174	45991.435662	32.385690
654.707059	46078.922206	32.390708
655.313050	46169.962454	32.395725
656.012349	46235.778824	32.400743
656.684180	46320.660632	32.405760
657.309417	46391.191808	32.410778
657.993015	46476.331310	32.415796
658.526733	46558.508643	32.420813
659.459394	46630.256154	32.425831
659.938892	46720.678922	32.430848
660.725716	46793.262756	32.435866
661.073161	46882.666031	32.440884
661.926572	46965.401714	32.445901
662.756109	47042.239494	32.450919
663.043748	47130.112744	32.455936
663.779749	47211.728897	32.460954
664.352277	47294.490375	32.465972
665.146627	47373.624860	32.470989
666.018548	47462.268274	32.476007
666.771186	47551.658182	32.481024
667.954763	47611.613679	32.486042
668.272834	47702.832064	32.491060
668.591747	47780.616292	32.496077
669.753267	47859.613099	32.501095
670.219695	47938.851552	32.506112
670.894924	48013.880765	32.511130
671.152680	48102.897200	32.516148
671.942002	48189.703837	32.521165
672.764646	48272.908215	32.526183
673.228310	48356.829244	32.531200
674.088877	48439.064829	32.536218
674.477168	48519.752429	32.541236
675.105804	48598.366720	32.546253
676.619017	48680.899624	32.551271
676.942275	48760.449403	32.556288
677.893103	48835.881554	32.561306
678.203394	48906.442553	32.566324
679.256276	48974.944940	32.571341
680.115750	49041.287720	32.576359
680.087441	49117.505145	32.581376
681.051095	49186.973696	32.586394
681.559068	49244.121495	32.591412
681.780675	49326.978241	32.596429
683.177032	49399.771183	32.601447
683.734098	49476.632239	32.606464
684.244052	49550.472524	32.611482
684.559756	49629.174387	32.616500
685.243076	49710.124539	32.621517
685.640849	49796.971636	32.626535
686.155487	49885.167386	32.631552
687.001898	49969.281650	32.636570
687.858892	50062.809864	32.641588
688.380171	50157.117358	32.646605
689.196212	50239.740712	32.651623
689.748665	50339.786054	32.656640
690.547338	50427.454041	32.661658
691.476114	50514.342858	32.666676
691.977403	50612.875668	32.671693
692.775667	50689.338418	32.676711
693.249378	50785.817294	32.681728
694.139088	50876.074913	32.686746
694.509250	50968.471990	32.691764
695.255279	51068.091086	32.696781
696.053177	51157.297591	32.701799
696.768494	51242.494059	32.706816
697.811808	51342.166458	32.711834
698.442625	51442.267698	32.716852
699.026323	51528.952820	32.721869
699.842627	51619.106008	32.726887
700.063612	51719.434406	32.731904
701.037347	51814.786978	32.736922
701.939082	51907.858676	32.741940
702.489901	52008.854194	32.746957
702.948804	52095.492990	32.751975
703.678145	52194.697339	32.756992
705.031626	52291.303481	32.762010
705.709707	52398.256433	32.767028
706.112481	52494.098476	32.772045
707.311972	52569.921020	32.777063
707.867831	52664.753011	32.782080
708.606796	52756.453144	32.787098
709.081247	52850.130713	32.792116
709.734762	52952.402950	32.797133
710.493924	53034.321037	32.802151
711.234288	53124.563237	32.807168
712.026777	53217.930917	32.812186
712.870132	53318.417278	32.817204
713.444082	53414.677763	32.822221
714.416615	53487.173923	32.827239
714.834860	53595.623220	32.832256
715.625386	53691.514377	32.837274
716.379071	53775.053890	32.842292
716.816939	53883.387801	32.847309
717.406495	53970.910449	32.852327
718.502484	54067.169904	32.857344
719.024245	54163.316322	32.862362
719.974227	54251.469280	32.867380
720.444153	54354.619511	32.872397
721.485773	54446.062643	32.877415
721.955394	54543.281015	32.882432
722.559268	54650.113183	32.887450
723.469028	54733.782582	32.892468
724.089855	54834.945335	32.897485
724.904064	54912.312859	32.902503
725.682710	55007.719543	32.907520
726.302308	55104.195553	32.912538
727.011695	55190.433761	32.917556
727.567670	55276.880960	32.922573
728.350240	55360.921575	32.927591
728.830488	55453.277332	32.932608
729.565467	55547.973516	32.937626
730.371769	55639.448457	32.942644
730.746993	55745.130120	32.947661
731.800747	55833.020212	32.952679
731.987293	55940.800360	32.957696
732.765977	56037.166127	32.962714
733.836522	56143.493143	32.967732
734.481423	56253.063221	32.972749
735.382044	56341.404258	32.977767
735.853020	56448.805201	32.982784
736.323785	56555.726513	32.987802
737.329178	56667.330819	32.992820
737.740553	56781.492125	32.997837
738.856246	56878.532903	33.002855
739.812085	56991.132995	33.007872
740.265737	57093.112141	33.012890
741.138018	57202.194835	33.017908
741.774696	57314.830587	33.022925
742.522497	57425.571769	33.027943
743.137711	57534.401792	33.032960
744.104511	57651.566317	33.037978
744.874854	57748.662124	33.042996
745.187296	57866.612318	33.048013
746.260242	57980.481437	33.053031
747.100229	58083.962613	33.058048
747.700756	58194.587053	33.063066
748.633201	58305.422615	33.068084
749.538812	58412.743226	33.073101
750.380248	58519.499941	33.078119
751.276519	58632.984885	33.083136
751.821226	58745.289967	33.088154
752.872901	58850.319985	33.093172
753.454062	58959.586770	33.098189
754.427008	59060.978097	33.103207
755.098012	59170.837861	33.108224
755.570191	59275.074853	33.113242
756.711718	59390.160323	33.118260
757.137625	59503.683726	33.123277
757.819369	59603.053010	33.128295
758.853502	59725.761043	33.133312
759.492025	59828.835772	33.138330
760.542757	59938.415686	33.143348
761.147340	60051.944202	33.148365
761.891310	60161.917350	33.153383
762.714340	60261.930102	33.158400
763.593566	60381.823661	33.163418
764.341437	60480.781810	33.168436
764.909729	60585.603734	33.173453
765.948810	60691.764064	33.178471
766.653894	60807.700840	33.183488
767.163357	60918.905088	33.188506
768.314139	61023.462261	33.193524
768.804938	61123.249781	33.198541
769.658824	61234.683196	33.203559
770.156873	61342.864146	33.208576
770.753336	61462.513767	33.213594
771.684366	61568.987277	33.218612
772.149364	61690.594066	33.223629
773.092798	61794.778646	33.228647
774.104220	61915.234519	33.233664
774.790816	62032.508634	33.238682
775.516049	62142.318568	33.243700
776.297858	62254.148695	33.248717
776.889292	62357.281903	33.253735
778.122940	62449.431261	33.258752
778.969400	62559.229692	33.263770
779.726834	62658.386418	33.268788
780.324832	62761.040178	33.273805
781.175839	62859.164725	33.278823
781.908258	62955.413062	33.283840
782.300660	63078.032459	33.288858
783.433026	63186.491133	33.293876
783.769711	63290.107302	33.298893
784.328200	63399.332054	33.303911
785.374436	63507.503248	33.308928
786.078311	63627.817737	33.313946
787.012372	63738.650950	33.318964
787.826434	63864.631363	33.323981
788.351624	63976.778769	33.328999
789.365864	64087.998831	33.334016
790.001985	64213.170059	33.339034
791.341008	64332.517554	33.344052
791.810427	64440.321247	33.349069
792.670391	64565.805254	33.354087
793.617903	64685.782148	33.359104
793.904821	64798.871057	33.364122
794.780184	64911.129944	33.369140
795.532723	65037.361543	33.374157
796.402645	65162.360733	33.379175
797.380023	65276.033404	33.384192
797.473387	65418.515605	33.389210
798.637311	65532.013414	33.394228
799.383809	65658.142295	33.399245
800.363560	65789.385653	33.404263
801.824534	65911.769151	33.409280
802.097853	66041.967716	33.414298
803.089196	66148.789868	33.419316
803.992696	66284.151883	33.424333
804.858700	66396.749039	33.429351
805.850221	66521.584508	33.434368
806.311734	66644.162886	33.439386
807.303578	66769.644628	33.444404
807.939264	66892.233575	33.449421
808.737903	67007.652190	33.454439
809.669954	67134.397793	33.459456
810.309423	67255.755392	33.464474
811.057510	67375.243284	33.469492
812.186243	67499.783675	33.474509
812.856901	67630.432129	33.479527
814.047907	67745.353636	33.484544
814.525223	67872.216817	33.489562
815.786781	67992.040551	33.494580
816.413963	68117.002628	33.499597
817.131331	68242.886266	33.504615
818.239866	68359.184102	33.509632
818.699915	68483.404623	33.514650
819.730454	68609.636965	33.519668
820.488077	68731.887625	33.524685
821.658467	68851.712328	33.529703
822.440015	68963.350781	33.534720
823.220201	69092.112252	33.539738
823.952555	69209.115565	33.544756
824.932242	69318.282482	33.549773
825.649326	69438.735558	33.554791
826.598415	69551.519123	33.559808
827.260496	69679.089663	33.564826
828.087085	69784.509457	33.569844
828.592319	69911.266361	33.574861
829.595608	70035.968829	33.579879
830.556647	70146.540470	33.584896
831.395934	70261.736089	33.589914
831.880360	70375.195230	33.594932
832.748804	70489.628466	33.599949
833.378005	70600.434384	33.604967
834.316461	70726.681825	33.609984
834.703918	70840.690620	33.615002
835.879559	70949.846095	33.620020
836.336543	71083.605231	33.625037
837.123833	71213.889577	33.630055
838.285949	71325.306666	33.635072
838.783230	71461.767934	33.640090
839.820576	71585.746557	33.645108
840.687956	71714.357583	33.650125
841.267955	71838.900220	33.655143
842.292245	71973.557526	33.660160
843.117485	72104.372156	33.665178
843.741049	72236.441417	33.670196
844.981318	72362.465122	33.675213
845.475618	72503.960864	33.680231
846.605255	72627.525467	33.685248
847.258458	72767.567452	33.690266
848.194780	72903.269554	33.695284
849.196360	73036.368876	33.700301
849.646909	73166.492999	33.705319
850.722649	73296.324775	33.710336
851.568700	73445.015830	33.715354
852.460665	73577.327102	33.720372
853.491212	73716.718308	33.725389
854.227985	73848.721710	33.730407
855.492398	73989.391413	33.735424
855.977372	74127.616945	33.740442
856.920990	74255.711797	33.745460
858.013675	74397.272634	33.750477
858.960112	74536.973897	33.755495
859.878036	74669.749162	33.760512
860.345728	74808.873592	33.765530
861.414632	74944.534814	33.770548
862.538484	75071.440903	33.775565
863.488401	75209.438232	33.780583
864.615504	75338.331250	33.785600
865.261325	75464.534411	33.790618
865.876527	75599.971124	33.795636
867.092906	75724.342107	33.800653
867.896717	75869.097269	33.805671
868.995863	75991.699230	33.810688
869.484895	76132.820801	33.815706
870.641420	76251.164394	33.820724
871.431409	76390.137960	33.825741
872.246567	76523.984995	33.830759
873.351383	76655.507924	33.835776
874.126978	76786.036121	33.840794
874.995711	76911.622430	33.845812
876.181417	77033.077316	33.850829
877.057152	77172.743686	33.855847
877.813516	77294.150827	33.860864
878.657457	77428.978956	33.865882
879.421470	77558.033487	33.870900
880.718314	77681.769607	33.875917
881.350666	77815.515484	33.880935
882.055195	77942.279646	33.885952
883.101605	78071.246160	33.890970
883.920219	78205.722615	33.895988
884.806279	78325.171992	33.901005
885.668725	78461.502428	33.906023
886.524057	78589.712837	33.911040
887.283031	78712.367055	33.916058
888.011540	78840.492334	33.921076
889.072698	78970.568568	33.926093
889.702839	79102.513340	33.931111
890.631134	79215.539868	33.936128
891.743772	79346.792677	33.941146
892.461462	79468.433067	33.946164
893.258871	79595.064676	33.951181
894.138582	79721.974376	33.956199
895.063653	79848.099198	33.961216
895.946945	79980.494333	33.966234
896.305547	80105.967813	33.971252
897.610261	80229.375057	33.976269
898.149796	80369.920312	33.981287
899.169203	80509.849356	33.986304
900.079883	80645.969927	33.991322
900.623520	80781.595310	33.996340
901.948032	80922.330473	34.001357
902.576866	81059.468043	34.006375
903.827755	81194.649957	34.011392
904.213034	81344.950269	34.016410
905.580182	81486.187973	34.021428
906.982193	81614.837546	34.026445
907.670227	81767.425016	34.031463
908.428239	81899.396536	34.036480
909.108100	82045.470925	34.041498
910.262454	82189.677355	34.046516
911.460906	82323.647269	34.051533
911.845522	82468.577453	34.056551
913.236192	82600.720429	34.061568
914.037527	82740.964934	34.066586
914.921942	82890.420978	34.071604
916.081552	83028.494846	34.076621
916.883797	83172.993446	34.081639
917.565670	83309.832024	34.086656
918.918258	83455.044892	34.091674
919.742977	83591.475574	34.096692
920.846996	83733.390667	34.101709
921.742119	83875.980209	34.106727
922.423977	84014.638822	34.111744
923.258097	84162.175331	34.116762
924.278318	84309.308701	34.121780
925.236963	84450.872603	34.126797
926.261224	84598.475350	34.131815
927.296150	84739.705709	34.136832
927.712645	84890.251762	34.141850
928.834203	85037.094579	34.146868
930.247007	85184.333075	34.151885
930.934231	85327.263292	34.156903
931.793102	85465.578584	34.161920
932.704090	85610.194599	34.166938
933.654068	85761.929878	34.171956
934.822268	85906.441914	34.176973
935.546692	86062.436942	34.181991
936.675224	86205.052764	34.187008
937.731543	86347.795294	34.192026
938.394283	86497.266894	34.197044
939.513412	86639.418657	34.202061
940.682105	86785.657184	34.207079
941.509680	86928.365133	34.212096
942.215791	87065.360957	34.217114
943.120521	87212.183655	34.222132
944.370180	87355.672333	34.227149
944.968407	87509.021084	34.232167
946.087565	87646.875866	34.237184
947.036371	87786.575784	34.242202
947.955387	87935.039585	34.247220
948.984363	88078.303360	34.252237
950.218054	88223.299717	34.257255
951.176338	88363.425458	34.262272
952.250633	88499.444770	34.267290
952.952052	88638.659040	34.272308
954.162576	88756.779805	34.277325
954.608605	88887.551448	34.282343
955.692483	89009.086421	34.287360
956.997669	89146.178720	34.292378
957.494260	89282.500547	34.297396
958.351321	89405.283788	34.302413
959.311627	89552.042145	34.307431
959.988018	89688.437809	34.312448
961.179020	89826.926200	34.317466
961.856423	89979.834763	34.322484
962.692823	90115.927937	34.327501
963.783304	90269.143427	34.332519
964.613467	90415.504562	34.337536
965.676804	90567.631562	34.342554
966.566747	90721.933683	34.347572
967.495194	90868.958509	34.352589
968.714792	91021.594163	34.357607
969.292539	91168.944627	34.362624
970.111842	91324.996425	34.367642
971.105263	91481.248284	34.372660
972.476695	91633.185481	34.377677
973.526921	91794.043883	34.382695
974.247807	91954.578061	34.387712
975.141796	92106.597176	34.392730
976.142652	92270.631513	34.397748
976.838707	92431.059015	34.402765
978.020601	92598.939167	34.407783
978.841131	92753.208730	34.412800
979.965306	92918.714445	34.417818
980.879759	93093.243828	34.422836
982.157738	93253.295679	34.427853
982.954590	93417.105615	34.432871
984.052089	93587.569989	34.437888
985.274226	93749.792716	34.442906
986.149423	93915.479262	34.447924
987.025501	94077.033458	34.452941
988.113867	94241.022226	34.457959
989.099498	94402.452836	34.462976
990.433364	94567.390633	34.467994
991.382299	94733.944012	34.473012
992.357974	94896.784741	34.478029
993.383010	95056.187526	34.483047
994.542266	95220.734449	34.488064
995.632049	95379.856419	34.493082
996.409111	95544.987759	34.498100
997.675002	95696.784021	34.503117
998.835096	95859.391684	34.508135
999.712669	96018.957972	34.513152
1001.059576	96176.947400	34.518170
1001.744469	96331.787186	34.523188
1003.019154	96482.352374	34.528205
1003.999929	96650.970707	34.533223
1004.698307	96801.595133	34.538240
1005.965330	96956.671714	34.543258
1006.618693	97127.094604	34.548276
1007.864393	97269.610580	34.553293
1008.897020	97443.410394	34.558311
1009.874250	97596.778947	34.563328
1011.048279	97757.738024	34.568346
1011.711623	97915.319674	34.573364
1013.018484	98073.460630	34.578381
1014.097875	98223.922955	34.583399
1015.051175	98389.309802	34.588416
1016.287366	98547.060238	34.593434
1017.055555	98701.356395	34.598452
1018.314649	98844.714745	34.603469
1019.263088	98996.102312	34.608487
1020.216262	99143.691387	34.613504
1021.240225	99277.676838	34.618522
1021.979731	99433.862515	34.623540
1023.630056	99575.476232	34.628557
1024.253417	99712.189287	34.633575
1025.081325	99859.689267	34.638592
1026.184319	100013.007339	34.643610
1026.830414	100165.243257	34.648628
1028.091914	100304.278843	34.653645
1029.146343	100452.238631	34.658663
1029.709872	100616.944646	34.663680
1030.819685	100767.600599	34.668698
1031.889244	100931.712117	34.673716
1033.287734	101086.792225	34.678733
1033.972109	101241.693765	34.683751
1034.936027	101402.976565	34.688768
1036.103826	101570.950844	34.693786
1037.134776	101734.206430	34.698804
1037.957301	101904.487709	34.703821
1039.344330	102077.418415	34.708839
1040.107989	102235.719287	34.713856
1041.446463	102396.211870	34.718874
1042.255681	102566.246427	34.723892
1043.326522	102730.147547	34.728909
1044.568374	102894.831914	34.733927
1045.464698	103068.508885	34.738944
1046.245582	103236.443957	34.743962
1047.685684	103408.944177	34.748980
1048.683556	103572.324436	34.753997
1049.693377	103738.299921	34.759015
1050.500193	103920.786383	34.764032
1051.967491	104081.331369	34.769050
1052.615509	104270.128092	34.774068
1053.635728	104436.346904	34.779085
1054.694726	104615.592348	34.784103
1055.733221	104794.880397	34.789120
1056.971887	104973.933931	34.794138
1058.051430	105153.040321	34.799156
1059.024045	105319.031939	34.804173
1060.619536	105505.122510	34.809191
1060.947793	105686.079189	34.814208
1062.469009	105854.744481	34.819226
1063.898542	106028.580820	34.824244
1064.988018	106201.296634	34.829261
1066.112777	106383.760218	34.834279
1067.134940	106556.400808	34.839296
1068.578919	106727.262900	34.844314
1069.460086	106889.087096	34.849332
1070.549618	107052.397727	34.854349
1071.550038	107222.741031	34.859367
1072.507228	107399.248262	34.864384
1073.493808	107568.126789	34.869402
1074.607656	107744.927047	34.874420
1075.765037	107927.079112	34.879437
1076.918590	108087.294885	34.884455
1077.838835	108266.258529	34.889472
1078.926804	108437.646375	34.894490
1079.992664	108617.601597	34.899508
1081.156793	108781.733731	34.904525
1082.439079	108949.318021	34.909543
1083.360686	109125.551108	34.914560
1084.775983	109299.765673	34.919578
1085.546684	109471.668532	34.924596
1086.720677	109644.582502	34.929613
1087.543395	109806.826553	34.934631
1088.752900	109993.493419	34.939648
1090.203221	110158.992624	34.944666
1091.087740	110331.338112	34.949684
1092.128991	110483.023432	34.954701
1093.324500	110637.774972	34.959719
1094.123788	110805.577217	34.964736
1095.263018	110960.922598	34.969754
1096.452956	111122.226998	34.974772
1097.509414	111280.767486	34.979789
1098.576349	111452.722491	34.984807
1099.139018	111616.603744	34.989824
1100.522802	111781.680361	34.994842
1101.722785	111951.412232	34.999860
1102.649407	112112.132552	35.004877
1103.921410	112291.165754	35.009895
1104.525184	112463.710358	35.014912
1105.531625	112633.389729	35.019930
1106.731752	112815.237928	35.024948
1108.371299	113003.209631	35.029965
1109.360768	113167.118165	35.034983
1110.300186	113352.965618	35.040000
1111.527752	113531.000645	35.045018
1112.734856	113713.423649	35.050036
1113.849840	113886.145918	35.055053
1114.938176	114060.913385	35.060071
1115.984677	114248.940841	35.065088
1117.097541	114427.000525	35.070106
1118.141746	114611.711434	35.075124
1118.851363	114798.949415	35.080141
1120.279422	114978.404791	35.085159
1121.202289	115169.461510	35.090176
1122.480514	115362.576609	35.095194
1123.846737	115550.255808	35.100212
1124.749025	115744.208517	35.105229
1125.916905	115927.982676	35.110247
1127.207678	116127.499236	35.115264
1128.295455	116319.550037	35.120282
1129.585537	116511.720728	35.125300
1130.599193	116700.416071	35.130317
1132.036035	116882.378076	35.135335
1132.749964	117072.899280	35.140352
1133.982475	117268.277529	35.145370
1135.267895	117462.533346	35.150388
1136.472722	117642.283158	35.155405
1137.787757	117840.401199	35.160423
1138.923632	118031.023715	35.165440
1140.457542	118206.845355	35.170458
1141.791232	118404.672755	35.175476
1142.535492	118592.157941	35.180493
1144.072785	118774.381393	35.185511
1145.085672	118956.933442	35.190528
1146.334730	119133.897534	35.195546
1147.312645	119324.288575	35.200564
1148.351121	119512.313943	35.205581
1149.885127	119682.999873	35.210599
1150.489000	119880.818585	35.215616
1151.716358	120068.423485	35.220634
1152.947972	120250.719377	35.225652
1154.267215	120432.735806	35.230669
1155.647984	120624.335902	35.235687
1156.189462	120817.634666	35.240704
1157.873597	120999.290149	35.245722
1158.731772	121190.359387	35.250740
1160.027584	121378.265461	35.255757
1161.231089	121560.966955	35.260775
1162.131886	121759.066010	35.265792
1163.413890	121946.433056	35.270810
1164.727960	122137.230273	35.275828
1165.662342	122312.161855	35.280845
1166.998081	122504.985486	35.285863
1168.045334	122687.871815	35.290880
1169.255020	122862.672404	35.295898
1170.500408	123043.018905	35.300916
1171.327178	123216.947061	35.305933
1172.756431	123383.717661	35.310951
1173.789296	123558.133325	35.315968
1174.752989	123743.473179	35.320986
1176.058540	123914.347989	35.326004
1176.947894	124105.532129	35.331021
1177.971242	124279.003030	35.336039
1178.939610	124473.192742	35.341056
1180.114214	124665.169726	35.346074
1181.445415	124855.677225	35.351092
1182.606216	125053.590291	35.356109
1183.819268	125236.312597	35.361127
1184.828834	125447.193342	35.366144
1186.163525	125643.471893	35.371162
1187.312297	125836.474471	35.376180
1188.461901	126041.873589	35.381197
1189.732707	126234.757111	35.386215
1190.736051	126439.156445	35.391232
1191.786606	126636.400893	35.396250
1193.073012	126842.530551	35.401268
1194.497502	127063.062587	35.406285
1195.501343	127257.048652	35.411303
1196.808116	127473.141548	35.416320
1197.939361	127680.468538	35.421338
1199.134500	127884.744339	35.426356
1200.175434	128104.447268	35.431373
1201.651658	128307.538619	35.436391
1202.744055	128521.291303	35.441408
1204.047315	128736.785148	35.446426
1205.709317	128950.700118	35.451444
1206.536321	129155.247903	35.456461
1207.525995	129372.433109	35.461479
1208.831954	129593.775877	35.466496
1210.088172	129800.361082	35.471514
1211.684371	130014.306849	35.476532
1212.465515	130235.335247	35.481549
1213.829636	130452.263175	35.486567
1215.113537	130663.045228	35.491584
1216.549807	130873.841523	35.496602
1217.358040	131088.786786	35.501620
1218.587758	131314.844436	35.506637
1220.068104	131535.170501	35.511655
1221.397037	131749.729905	35.516672
1222.477974	131975.778794	35.521690
1223.989590	132193.416761	35.526708
1225.151593	132410.657628	35.531725
1226.167303	132619.417911	35.536743
1227.791693	132844.698518	35.541760
1228.465136	133068.096874	35.546778
1229.894266	133286.617901	35.551796
1231.226472	133510.645692	35.556813
1232.016934	133721.339233	35.561831
1233.528766	133946.265783	35.566848
1234.479262	134168.992038	35.571866
1235.693048	134404.962458	35.576884
1237.103715	134635.590065	35.581901
1238.131381	134846.517887	35.586919
1239.688604	135079.114804	35.591936
1240.923036	135313.896627	35.596954
1242.168998	135536.684751	35.601972
1243.447468	135769.484757	35.606989
1244.530572	135988.651535	35.612007
1245.805296	136218.006830	35.617024
1246.919657	136447.085933	35.622042
1248.506673	136666.478174	35.627060
1249.564071	136904.901229	35.632077
1250.801294	137109.330063	35.637095
1251.816429	137341.322449	35.642112
1253.016884	137556.448293	35.647130
1254.466719	137758.576432	35.652148
1255.319578	137982.041795	35.657165
1256.266228	138192.674577	35.662183
1257.938399	138424.591188	35.667200
1258.438478	138664.881255	35.672218
1260.040413	138888.114678	35.677236
1261.338695	139126.145942	35.682253
1262.448553	139354.928607	35.687271
1263.988905	139586.583319	35.692288
1264.763616	139822.956207	35.697306
1266.033317	140054.734906	35.702324
1267.109759	140307.304063	35.707341
1268.270931	140551.149935	35.712359
1269.587679	140791.510163	35.717376
1270.703348	141042.341060	35.722394
1272.018185	141292.456122	35.727412
1273.468944	141546.468744	35.732429
1274.752539	141812.481174	35.737447
1276.315157	142058.376257	35.742464
1277.271720	142319.653380	35.747482
1278.760432	142571.891920	35.752500
1280.007165	142827.900426	35.757517
1281.657083	143086.798802	35.762535
1282.759834	143334.300559	35.767552
1283.912495	143594.933387	35.772570
1285.529358	143851.864598	35.777588
1286.827013	144104.450039	35.782605
1288.323822	144362.076896	35.787623
1289.798781	144616.855907	35.792640
1290.577589	144878.409603	35.797658
1292.179798	145126.335875	35.802676
1293.325150	145393.019525	35.807693
1294.500809	145656.123879	35.812711
1296.087731	145913.303144	35.817728
1297.391187	146176.922815	35.822746
1298.910460	146427.344744	35.827764
1300.187034	146696.235699	35.832781
1301.777578	146947.943022	35.837799
1302.745198	147204.625063	35.842816
1303.863709	147468.500272	35.847834
1305.613680	147720.300713	35.852852
1306.851489	147988.345180	35.857869
1308.064155	148253.136301	35.862887
1309.402632	148504.502819	35.867904
1310.803332	148767.630474	35.872922
1311.878553	149021.694740	35.877940
1313.650325	149287.998915	35.882957
1314.984561	149546.513762	35.887975
1316.073542	149805.400700	35.892992
1317.307939	150077.709719	35.898010
1318.732854	150325.472190	35.903028
1320.024045	150589.759624	35.908045
1321.158435	150853.643587	35.913063
1322.464508	151127.305501	35.918080
1323.678449	151389.087247	35.923098
1324.918337	151655.026813	35.928116
1326.459227	151925.028089	35.933133
1327.394719	152182.459986	35.938151
1329.110955	152453.514161	35.943168
1330.050018	152730.064123	35.948186
1331.619181	152995.146801	35.953204
1333.036983	153271.735691	35.958221
1334.335266	153538.249470	35.963239
1336.014221	153808.076262	35.968256
1337.349021	154066.938848	35.973274
1338.801959	154323.716020	35.978292
1339.812636	154575.570159	35.983309
1340.860059	154815.140868	35.988327
1342.716064	155068.431393	35.993344
1343.398690	155328.780097	35.998362
1344.654267	155592.181740	36.003380
1346.414568	155842.651590	36.008397
1347.091989	156116.782499	36.013415
1348.808904	156370.129733	36.018432
1350.082605	156639.484787	36.023450
1351.498413	156897.604138	36.028468
1352.582892	157167.767845	36.033485
1354.034732	157443.555864	36.038503
1355.408947	157701.446232	36.043520
1356.566349	157987.384544	36.048538
1358.084455	158256.671990	36.053556
1359.478703	158522.391536	36.058573
1360.760292	158803.240648	36.063591
1362.227677	159079.265588	36.068608
1363.266207	159366.070529	36.073626
1364.830253	159639.698241	36.078644
1365.961978	159927.379748	36.083661
1367.489188	160215.365811	36.088679
1369.107664	160492.846913	36.093696
1370.062625	160793.301079	36.098714
1371.533200	161083.801824	36.103732
1372.850478	161376.956123	36.108749
1374.282954	161665.767157	36.113767
1375.787552	161959.985660	36.118784
1377.017388	162251.219383	36.123802
1378.903037	162551.291276	36.128820
1380.153822	162843.489849	36.133837
1381.338939	163136.005781	36.138855
1383.001634	163427.442476	36.143872
1384.446400	163727.963466	36.148890
1385.796707	164016.017439	36.153908
1387.462191	164301.940450	36.158925
1388.808712	164599.349870	36.163943
1390.222405	164888.541101	36.168960
1391.646579	165183.327966	36.173978
1393.162049	165458.422404	36.178996
1394.614753	165752.980015	36.184013
1395.886257	166050.767009	36.189031
1397.682989	166343.292346	36.194048
1398.789518	166641.034462	36.199066
1400.629935	166925.448486	36.204084
1402.132619	167217.165371	36.209101
1403.327876	167499.989408	36.214119
1405.119464	167784.696141	36.219136
1406.453787	168072.677854	36.224154
1407.781494	168349.927625	36.229172
1409.168480	168646.558189	36.234189
1410.552469	168924.525461	36.239207
1411.938517	169202.849392	36.244224
1413.268492	169498.682835	36.249242
1414.852203	169789.235545	36.254260
1416.456813	170057.833879	36.259277
1417.739184	170365.177428	36.264295
1419.231880	170651.245839	36.269312
1420.540844	170930.151321	36.274330
1421.677605	171217.855569	36.279348
1423.390582	171505.593269	36.284365
1424.508692	171796.996914	36.289383
1426.331609	172079.123712	36.294400
1427.924733	172376.772079	36.299418
1429.168894	172660.267004	36.304436
1430.842932	172931.700313	36.309453
1432.073481	173225.530718	36.314471
1433.862728	173486.351740	36.319488
1435.088660	173752.571884	36.324506
1436.226670	174012.361248	36.329524
1437.926673	174271.627663	36.334541
1439.083721	174548.866335	36.339559
1440.731000	174812.827220	36.344576
1441.803864	175083.090262	36.349594
1443.097716	175355.589950	36.354612
1444.484648	175632.213021	36.359629
1445.747684	175908.274339	36.364647
1447.040775	176189.738640	36.369664
1448.541480	176482.668428	36.374682
1449.885740	176768.277572	36.379700
1450.901638	177063.867220	36.384717
1452.271228	177355.186630	36.389735
1454.022863	177656.369322	36.394752
1455.509790	177959.272841	36.399770
1456.936188	178261.096701	36.404788
1458.961137	178547.885336	36.409805
1460.102255	178852.945467	36.414823
1461.351908	179152.874674	36.419840
1462.652682	179464.803735	36.424858
1464.320601	179771.381458	36.429876
1466.290515	180070.118172	36.434893
1467.633136	180379.773962	36.439911
1469.047427	180677.336767	36.444928
1470.631512	180979.797813	36.449946
1472.068600	181297.134948	36.454964
1473.586941	181595.663077	36.459981
1474.908252	181908.085660	36.464999
1476.561781	182221.648287	36.470016
1477.928138	182530.868552	36.475034
1479.516980	182847.136379	36.480052
1481.060466	183151.025389	36.485069
1482.414904	183466.954802	36.490087
1483.805125	183781.674314	36.495104
1485.551223	184098.583503	36.500122
1486.745687	184419.622084	36.505140
1488.599879	184735.311251	36.510157
1489.970010	185055.194819	36.515175
1491.380410	185371.659080	36.520192
1493.086486	185710.670510	36.525210
1494.503376	186023.380153	36.530228
1496.410940	186331.567725	36.535245
1497.479025	186661.639832	36.540263
1499.428968	186970.128532	36.545280
1500.935889	187289.380238	36.550298
1502.077843	187606.574167	36.555316
1503.912858	187928.136271	36.560333
1505.393841	188252.424397	36.565351
1506.844534	188561.511903	36.570368
1508.711457	188873.020317	36.575386
1509.941211	189198.015318	36.580404
1511.529564	189505.155556	36.585421
1512.934043	189833.133725	36.590439
1514.131374	190138.996269	36.595456
1516.124105	190459.797246	36.600474
1517.537508	190780.314834	36.605492
1519.243136	191100.417703	36.610509
1520.555464	191422.288337	36.615527
1521.875011	191740.478022	36.620544
1523.970032	192053.755309	36.625562
1525.244265	192376.792500	36.630580
1526.867458	192686.456781	36.635597
1528.431785	193015.085915	36.640615
1529.784060	193322.487655	36.645632
1531.605186	193636.998859	36.650650
1532.973797	193952.068826	36.655668
1534.411164	194239.110672	36.660685
1535.877881	194543.757307	36.665703
1537.437473	194846.574624	36.670720
1539.016847	195138.789456	36.675738
1540.254040	195447.820147	36.680756
1541.915329	195739.516353	36.685773
1543.182810	196053.128008	36.690791
1544.723531	196353.771878	36.695808
1546.320406	196666.849621	36.700826
1547.674305	196968.593611	36.705844
1549.511881	197288.083972	36.710861
1550.587598	197604.502387	36.715879
1552.114013	197917.813508	36.720896
1553.630638	198242.465223	36.725914
1555.147402	198568.578520	36.730932
1557.006119	198889.786973	36.735949
1558.211359	199218.798783	36.740967
1559.709991	199555.406825	36.745984
1561.442720	199886.213714	36.751002
1562.893730	200223.010618	36.756020
1564.751528	200551.032198	36.761037
1566.156111	200890.226907	36.766055
1567.918145	201218.102362	36.771072
1569.205395	201552.202923	36.776090
1570.658852	201902.630873	36.781108
1572.572612	202236.783474	36.786125
1574.291290	202582.358854	36.791143
1575.639362	202915.909722	36.796160
1577.146425	203262.856453	36.801178
1578.785186	203614.112719	36.806196
1580.634427	203949.439219	36.811213
1581.899508	204292.329614	36.816231
1583.719394	204638.443861	36.821248
1585.180937	204985.380729	36.826266
1586.891031	205347.171978	36.831284
1588.904935	205684.358166	36.836301
1589.954062	206027.584099	36.841319
1591.669264	206380.478512	36.846336
1593.492646	206738.461030	36.851354
1595.094391	207098.780048	36.856372
1596.478246	207434.185954	36.861389
1598.129818	207794.093571	36.866407
1599.751948	208142.274997	36.871424
1601.562534	208496.128078	36.876442
1602.983973	208858.630704	36.881460
1604.862779	209200.692006	36.886477
1606.337669	209563.874593	36.891495
1607.658510	209916.329039	36.896512
1609.725084	210275.061567	36.901530
1611.082237	210639.296808	36.906548
1613.088482	210992.302812	36.911565
1614.416122	211344.635097	36.916583
1616.072216	211709.358823	36.921600
1618.124011	212046.387241	36.926618
1619.471522	212418.275948	36.931636
1621.192185	212756.961786	36.936653
1623.012592	213122.121368	36.941671
1624.533876	213476.385759	36.946688
1625.913634	213820.236725	36.951706
1627.494096	214185.745011	36.956724
1629.298805	214544.995374	36.961741
1630.938779	214897.290072	36.966759
1632.597041	215251.843453	36.971776
1634.037113	215610.218451	36.976794
1635.574117	215977.569559	36.981812
1637.501987	216328.475957	36.986829
1639.397592	216687.744852	36.991847
1640.690195	217033.450603	36.996864
1642.643898	217372.825843	37.001882
1644.125486	217721.906124	37.006900
1645.484048	218039.615787	37.011917
1647.219320	218377.532039	37.016935
1648.677860	218716.130093	37.021952
1650.145755	219049.775028	37.026970
1652.083039	219405.871989	37.031988
1653.664168	219755.907941	37.037005
1655.253041	220089.891807	37.042023
1656.656019	220447.121915	37.047040
1658.416578	220791.061339	37.052058
1659.867545	221156.667503	37.057076
1661.233848	221510.452934	37.062093
1663.143677	221875.274523	37.067111
1664.440352	222236.642716	37.072128
1666.324238	222604.391882	37.077146
1667.552425	222971.590178	37.082164
1669.406284	223345.594940	37.087181
1671.215594	223738.149922	37.092199
1672.318069	224170.370185	37.097216
1674.561175	224541.596709	37.102234
1676.000535	224925.682447	37.107252
1677.552435	225311.935199	37.112269
1679.364140	225698.527250	37.117287
1680.946734	226082.237353	37.122304
1682.726232	226473.586931	37.127322
1684.207354	226867.095219	37.132340
1686.271039	227252.405798	37.137357
1687.748649	227651.606709	37.142375
1689.650417	228048.224123	37.147392
1691.326500	228439.698299	37.152410
1693.102347	228840.987142	37.157428
1694.539894	229231.105968	37.162445
1696.756901	229628.412531	37.167463
1698.262497	230030.460673	37.172480
1700.024645	230419.081327	37.177498
1701.786960	230824.213585	37.182516
1703.500492	231228.262777	37.187533
1705.023568	231622.463521	37.192551
1706.804177	232035.800588	37.197568
1708.492189	232434.446783	37.202586
1710.755213	232840.162164	37.207604
1712.330188	233237.533607	37.212621
1714.228519	233646.308634	37.217639
1715.749351	234038.026478	37.222656
1717.608690	234447.190957	37.227674
1719.443160	234849.070290	37.232692
1720.981281	235256.714878	37.237709
1722.900908	235651.596566	37.242727
1724.235349	236064.255393	37.247744
1726.005422	236465.564811	37.252762
1727.833536	236872.225305	37.257780
1729.508875	237276.193913	37.262797
1731.248339	237684.699730	37.267815
1733.038101	238102.088795	37.272832
1734.814957	238498.752795	37.277850
1736.416008	238913.761524	37.282868
1738.244689	239323.856271	37.287885
1739.993564	239736.479814	37.292903
1741.568187	240150.631661	37.297920
1743.424903	240558.539528	37.302938
1745.520142	240962.903211	37.307956
1746.945782	241380.689053	37.312973
1749.042945	241792.395142	37.317991
1750.580402	242212.094548	37.323008
1752.306136	242606.005419	37.328026
1753.965442	243024.695355	37.333044
1755.843156	243425.796698	37.338061
1758.098629	243807.987496	37.343079
1759.556588	244198.109170	37.348096
1761.301457	244574.339524	37.353114
1763.035702	244968.684264	37.358132
1764.515998	245355.196615	37.363149
1765.904367	245743.020177	37.368167
1767.562388	246152.087240	37.373184
1769.413815	246543.975943	37.378202
1771.069992	246938.412236	37.383220
1772.538020	247353.634230	37.388237
1773.987246	247761.010297	37.393255
1775.603856	248183.651744	37.398272
1777.378381	248604.921208	37.403290
1779.090481	249027.700196	37.408308
1780.773911	249464.456015	37.413325
1782.343165	249895.947281	37.418343
1783.826114	250333.168897	37.423360
1785.970102	250774.905086	37.428378
1787.325066	251214.434883	37.433396
1789.167738	251672.454184	37.438413
1791.163752	252119.372732	37.443431
1792.803280	252572.142405	37.448448
1794.842791	253026.065674	37.453466
1796.538207	253497.828315	37.458484
1798.156681	253952.405952	37.463501
1800.164952	254409.129527	37.468519
1801.650769	254877.675916	37.473536
1803.583355	255342.439840	37.478554
1805.711689	255816.291385	37.483572
1807.226301	256281.327895	37.488589
1809.289919	256746.121435	37.493607
1810.912227	257222.800496	37.498624
1812.859615	257704.252573	37.503642
1814.993230	258175.436414	37.508660
1816.646127	258651.297673	37.513677
1818.854851	259121.249775	37.518695
1820.773348	259605.755070	37.523712
1822.723105	260066.909515	37.528730
1824.551664	260539.362965	37.533748
1826.338756	261009.816299	37.538765
1828.565254	261487.055820	37.543783
1830.034204	261963.454972	37.548800
1832.259762	262438.077768	37.553818
1834.319117	262905.081426	37.558836
1836.135635	263366.663266	37.563853
1837.864045	263835.804168	37.568871
1839.739367	264306.876573	37.573888
1841.860790	264780.880199	37.578906
1843.602541	265239.932918	37.583924
1845.375662	265725.348584	37.588941
1847.279215	266191.740761	37.593959
1849.257972	266664.547102	37.598976
1851.258238	267122.920500	37.603994
1852.849254	267590.125105	37.609012
1854.775125	268070.508907	37.614029
1857.018774	268530.288669	37.619047
1858.630521	269009.021281	37.624064
1860.414245	269464.608235	37.629082
1862.768076	269933.081372	37.634100
1864.105075	270404.744772	37.639117
1866.463213	270860.539937	37.644135
1868.555229	271334.744658	37.649152
1870.142080	271792.571113	37.654170
1871.860630	272261.857177	37.659188
1874.058300	272729.107374	37.664205
1875.878605	273186.842341	37.669223
1877.282627	273657.473623	37.674240
1879.372359	274114.349675	37.679258
1881.366381	274556.888321	37.684276
1883.114100	275000.533782	37.689293
1885.194530	275434.394380	37.694311
1886.920738	275871.005354	37.699328
1888.732654	276318.575177	37.704346
1890.328601	276762.699686	37.709364
1892.156871	277213.491143	37.714381
1894.212049	277657.156995	37.719399
1895.799536	278116.013430	37.724416
1897.794291	278567.028572	37.729434
1899.642752	279025.992307	37.734452
1901.311228	279484.730694	37.739469
1903.305960	279950.171033	37.744487
1904.913137	280415.877456	37.749504
1906.696255	280881.401258	37.754522
1908.813768	281362.033472	37.759540
1910.366064	281830.412547	37.764557
1912.332321	282311.219584	37.769575
1914.048025	282805.707257	37.774592
1916.139591	283288.294355	37.779610
1918.010306	283773.659863	37.784628
1919.572958	284283.434601	37.789645
1922.106412	284766.630169	37.794663
1923.576752	285271.133514	37.799680
1925.313751	285766.472201	37.804698
1927.356436	286270.852312	37.809716
1929.051752	286780.317430	37.814733
1931.346871	287290.748545	37.819751
1933.560559	287805.280784	37.824768
1935.109716	288309.659039	37.829786
1937.239270	288815.768437	37.834804
1939.056199	289328.277660	37.839821
1941.178490	289853.790227	37.844839
1943.520368	290367.783544	37.849856
1945.253734	290885.913903	37.854874
1947.292708	291398.302084	37.859892
1949.154742	291917.956337	37.864909
1951.484307	292441.214151	37.869927
1953.438969	292959.959669	37.874944
1955.228095	293477.307886	37.879962
1957.536748	293989.945338	37.884980
1959.116350	294516.568919	37.889997
1961.270874	295040.047227	37.895015
1963.337698	295561.531047	37.900032
1965.252338	296078.795914	37.905050
1967.549743	296591.550329	37.910068
1969.397058	297117.558546	37.915085
1971.471898	297646.117241	37.920103
1973.454103	298158.814534	37.925120
1975.410954	298678.878982	37.930138
1977.741831	299196.059819	37.935156
1979.782973	299718.238461	37.940173
1981.756620	300243.320867	37.945191
1983.715604	300756.745301	37.950208
1985.493801	301283.886200	37.955226
1988.020020	301792.741464	37.960244
1989.985886	302318.017026	37.965261
1991.898399	302825.926740	37.970279
1994.014623	303341.546139	37.975296
1995.477542	303859.860986	37.980314
1998.029301	304366.793083	37.985332
1999.471316	304899.505364	37.990349
2001.735853	305408.993201	37.995367
2003.668311	305930.012046	38.000384
2005.528870	306456.068064	38.005402
2007.813311	306970.114714	38.010420
2009.422095	307500.396179	38.015437
2011.914188	308010.745167	38.020455
2013.961161	308514.256904	38.025472
2015.631262	309002.895266	38.030490
2017.352828	309484.944812	38.035508
2019.601564	309992.070972	38.040525
2021.464603	310492.477130	38.045543
2023.489270	310985.184196	38.050560
2025.242907	311493.220459	38.055578
2027.406524	311981.378015	38.060596
2028.913124	312500.926698	38.065613
2031.000008	313017.328717	38.070631
2033.085581	313531.086430	38.075648
2034.999977	314062.238183	38.080666
2037.074593	314572.841646	38.085684
2038.833555	315095.428547	38.090701
2040.873761	315634.089921	38.095719
2042.887591	316168.384000	38.100736
2044.806803	316699.591752	38.105754
2046.887438	317243.541328	38.110772
2048.908440	317791.229188	38.115789
2051.040126	318338.132658	38.120807
2053.231761	318877.328073	38.125824
2054.998486	319450.411240	38.130842
2057.154171	319985.871130	38.135860
2059.318863	320551.109321	38.140877
2061.444098	321107.589226	38.145895
2063.704858	321659.598598	38.150912
2065.637367	322226.993461	38.155930
2067.791425	322778.325318	38.160948
2069.929400	323342.375586	38.165965
2072.035964	323896.447701	38.170983
2074.329030	324461.833369	38.176000
2076.223711	325036.013674	38.181018
2078.698803	325591.634724	38.186036
2080.960070	326163.078046	38.191053
2082.784628	326727.428397	38.196071
2084.956926	327278.894754	38.201088
2087.325299	327854.315671	38.206106
2089.252831	328421.374880	38.211124
2091.293674	328984.271653	38.216141
2093.406249	329561.215885	38.221159
2095.914610	330125.090635	38.226176
2097.387613	330695.579079	38.231194
2099.999196	331266.940055	38.236212
2102.166762	331838.825479	38.241229
2104.116525	332400.535666	38.246247
2106.556744	332975.766139	38.251264
2108.647648	333557.572411	38.256282
2110.473129	334124.895732	38.261300
2112.562293	334695.951978	38.266317
2114.820852	335263.953357	38.271335
2117.126452	335844.125596	38.276352
2119.391026	336424.196698	38.281370
2121.472853	336988.654877	38.286388
2123.381229	337566.030607	38.291405
2125.506283	338147.755485	38.296423
2127.803977	338724.114760	38.301440
2129.835684	339296.653193	38.306458
2132.014425	339864.033547	38.311476
2134.335670	340450.167006	38.316493
2136.100021	341024.100525	38.321511
2138.426651	341602.503308	38.326528
2140.478427	342188.153029	38.331546
2142.816998	342763.189759	38.336564
2144.587275	343346.968398	38.341581
2146.610773	343930.875818	38.346599
2148.489123	344508.835681	38.351616
2150.622959	345093.116726	38.356634
2153.031384	345677.395962	38.361652
2154.786650	346253.527416	38.366669
2156.940110	346817.429408	38.371687
2159.517791	347366.433263	38.376704
2161.328255	347937.306586	38.381722
2163.252256	348497.368299	38.386740
2165.493191	349066.050010	38.391757
2167.371042	349637.499878	38.396775
2169.793949	350221.439581	38.401792
2171.327008	350791.789617	38.406810
2173.360059	351375.727727	38.411828
2175.722683	351966.937399	38.416845
2177.576280	352558.882864	38.421863
2179.961122	353158.776598	38.426880
2182.045843	353758.305523	38.431898
2184.181770	354360.735707	38.436916
2186.307201	354972.496890	38.441933
2188.342131	355581.473017	38.446951
2190.480993	356194.711319	38.451968
2192.669268	356820.923601	38.456986
2194.936246	357440.288120	38.462004
2197.292926	358069.016373	38.467021
2199.229011	358701.128157	38.472039
2201.368327	359317.415342	38.477056
2203.555525	359950.861658	38.482074
2205.951168	360589.439266	38.487092
2207.897431	361237.341098	38.492109
2210.442856	361882.850143	38.497127
2212.785798	362527.392628	38.502144
2214.902002	363177.898360	38.507162
2217.291619	363819.367515	38.512180
2219.563926	364470.383947	38.517197
2221.595292	365117.522458	38.522215
2224.375195	365766.733446	38.527232
2226.386118	366419.916080	38.532250
2228.573323	367066.818111	38.537268
2231.106426	367721.566185	38.542285
2233.280645	368373.800060	38.547303
2235.691301	369024.360058	38.552320
2237.828196	369681.878396	38.557338
2240.304293	370333.342935	38.562356
2242.413006	370994.976716	38.567373
2244.577423	371646.266249	38.572391
2247.280170	372293.270238	38.577408
2249.225672	372964.507398	38.582426
2251.490876	373616.200995	38.587444
2254.150409	374279.762867	38.592461
2256.288233	374931.478564	38.597479
2258.934824	375589.742667	38.602496
2260.855389	376255.316461	38.607514
2263.192564	376916.472170	38.612532
2265.685052	377576.448371	38.617549
2268.061186	378240.919548	38.622567
2270.045683	378898.392780	38.627584
2272.757023	379551.397086	38.632602
2274.883158	380203.420296	38.637620
2277.307030	380860.453026	38.642637
2279.709585	381518.820189	38.647655
2282.014261	382165.146399	38.652672
2284.318132	382827.459260	38.657690
2286.633392	383480.172734	38.662708
2289.163695	384123.101589	38.667725
2291.069422	384787.671492	38.672743
2293.629170	385439.291005	38.677760
2295.734745	386091.048293	38.682778
2297.845923	386750.371661	38.687796
2300.621054	387407.847836	38.692813
2302.622863	388062.953536	38.697831
2305.164036	388701.985650	38.702848
2307.445573	389326.243067	38.707866
2309.567055	389944.937452	38.712884
2311.653970	390569.987811	38.717901
2313.980098	391189.003736	38.722919
2315.863378	391816.039559	38.727936
2317.950133	392457.324950	38.732954
2320.226247	393097.805140	38.737972
2322.709013	393736.108547	38.742989
2324.576332	394380.405589	38.748007
2326.894641	395024.538301	38.753024
2329.041460	395688.733163	38.758042
2331.188150	396343.637165	38.763060
2333.414546	397007.003621	38.768077
2335.399740	397681.900678	38.773095
2337.914741	398350.359079	38.778112
2340.168902	399033.264729	38.783130
2342.219561	399717.454916	38.788148
2344.781445	400413.860077	38.793165
2346.999879	401107.340197	38.798183
2349.231510	401798.748772	38.803200
2351.296845	402516.621723	38.808218
2353.380145	403216.381966	38.813236
2356.029988	403933.286181	38.818253
2358.062001	404658.964531	38.823271
2360.719558	405380.492250	38.828288
2362.947217	406113.523787	38.833306
2365.438744	406846.466929	38.838324
2368.431040	407570.491505	38.843341
2370.527802	408305.411398	38.848359
2372.884153	409027.171444	38.853376
2375.265422	409777.381463	38.858394
2377.578102	410517.246603	38.863412
2380.550292	411240.441424	38.868429
2382.566334	411991.308169	38.873447
2385.505519	412731.844199	38.878464
2387.812364	413469.905558	38.883482
2390.251668	414207.392387	38.888500
2392.978998	414945.140087	38.893517
2395.232996	415689.479162	38.898535
2397.612343	416434.561205	38.903552
2400.151941	417173.770453	38.908570
2402.341052	417922.234226	38.913588
2405.305242	418661.760827	38.918605
2407.559785	419407.941559	38.923623
2410.043115	420149.149989	38.928640
2412.282621	420898.504912	38.933658
2414.752947	421646.609214	38.938676
2417.835863	422399.147489	38.943693
2420.030778	423134.820361	38.948711
2422.607366	423873.952851	38.953728
2425.115563	424618.188492	38.958746
2427.388530	425368.516281	38.963764
2430.187416	426098.633273	38.968781
2432.395690	426844.470477	38.973799
2434.707895	427584.799537	38.978816
2437.341487	428335.785684	38.983834
2440.305781	429075.252253	38.988852
2442.746702	429800.506194	38.993869
2444.666489	430550.021460	38.998887
2447.156937	431277.044298	39.003904
2449.507433	432024.467287	39.008922
2451.915225	432775.096442	39.013940
2454.224552	433516.100575	39.018957
2457.140993	434268.115993	39.023975
2459.454930	435016.511568	39.028992
2461.791009	435758.603318	39.034010
2463.918099	436513.863924	39.039028
2466.620370	437242.486084	39.044045
2468.810354	437972.636931	39.049063
2471.255463	438685.061072	39.054080
2473.889098	439406.084638	39.059098
2476.091714	440119.059890	39.064116
2478.490107	440838.709810	39.069133
2480.626829	441564.906740	39.074151
2482.846383	442291.875710	39.079168
2485.257584	443030.982398	39.084186
2487.262248	443770.687793	39.089204
2490.362274	444525.263614	39.094221
2492.303788	445285.518671	39.099239
2494.672552	446029.792031	39.104256
2497.276066	446791.807253	39.109274
2499.145484	447568.080139	39.114292
2501.969309	448340.019661	39.119309
2503.914930	449123.456724	39.124327
2506.583240	449899.411748	39.129344
2509.180879	450699.171565	39.134362
2511.673823	451497.401029	39.139380
2514.161247	452289.178261	39.144397
2516.636419	453099.588132	39.149415
2519.370826	453904.462197	39.154432
2521.805334	454723.058071	39.159450
2523.961333	455527.155262	39.164468
2526.847923	456341.566935	39.169485
2529.137484	457177.330772	39.174503
2532.136274	457992.365853	39.179520
2534.325917	458812.607880	39.184538
2536.719209	459656.846989	39.189556
2539.270449	460478.275930	39.194573
2541.675986	461330.328756	39.199591
2544.333803	462173.356483	39.204608
2547.042465	463022.152798	39.209626
2549.366028	463878.507219	39.214644
2551.715304	464722.033067	39.219661
2554.522449	465573.381759	39.224679
2557.147132	466451.306003	39.229696
2559.689595	467306.716055	39.234714
2562.136645	468191.817265	39.239732
2564.965707	469064.535883	39.244749
2567.490307	469934.940714	39.249767
2569.933495	470794.708876	39.254784
2572.766988	471669.227685	39.259802
2575.369141	472554.000058	39.264820
2578.155033	473425.363639	39.269837
2580.711855	474302.230859	39.274855
2583.107328	475183.831896	39.279872
2586.030358	476065.455690	39.284890
2589.047508	476936.869670	39.289908
2591.312986	477821.346791	39.294925
2593.783252	478692.111391	39.299943
2596.892643	479579.495824	39.304960
2599.658916	480446.946348	39.309978
2601.829944	481338.136806	39.314996
2604.940841	482213.323490	39.320013
2607.232886	483089.562092	39.325031
2609.963625	483961.949299	39.330048
2612.696435	484847.319296	39.335066
2615.433964	485718.660200	39.340084
2618.262312	486591.609215	39.345101
2620.779332	487473.299437	39.350119
2623.357707	488337.419741	39.355136
2626.370447	489210.157910	39.360154
2628.945521	490085.599662	39.365172
2631.464528	490945.159097	39.370189
2634.510761	491827.198197	39.375207
2636.669355	492687.285596	39.380224
2639.365542	493537.956247	39.385242
2641.862844	494386.649517	39.390260
2644.458155	495208.895309	39.395277
2647.047283	496049.821042	39.400295
2649.470399	496885.434924	39.405312
2652.297880	497729.214471	39.410330
2654.973543	498571.614638	39.415348
2657.387635	499399.739762	39.420365
2660.289059	500237.529184	39.425383
2662.576787	501082.943566	39.430400
2665.388429	501933.322533	39.435418
2667.740020	502793.416981	39.440436
2670.082933	503644.692788	39.445453
2672.854895	504510.881476	39.450471
2675.467994	505377.907679	39.455488
2678.308192	506250.245559	39.460506
2680.843533	507126.368362	39.465524
2683.368816	508026.393928	39.470541
2685.973599	508901.803796	39.475559
2688.567148	509798.038534	39.480576
2691.345786	510683.707248	39.485594
2693.952463	511594.407275	39.490612
2696.555567	512490.992891	39.495629
2699.275481	513392.649283	39.500647
2701.641706	514321.779386	39.505664
2704.494073	515231.472915	39.510682
2707.184326	516158.878294	39.515700
2710.006589	517086.005098	39.520717
2712.952323	518011.544531	39.525735
2715.419784	518950.710866	39.530752
2718.275149	519886.783508	39.535770
2721.054938	520827.093528	39.540788
2724.093106	521759.142498	39.545805
2726.819528	522694.762150	39.550823
2729.451901	523639.254680	39.555840
2732.421313	524584.035507	39.560858
2734.944708	525525.254956	39.565876
2737.673686	526477.611316	39.570893
2740.912653	527419.802237	39.575911
2743.562688	528377.035494	39.580928
2746.174262	529319.360528	39.585946
2749.391301	530274.665749	39.590964
2751.933713	531225.187435	39.595981
2755.007580	532178.630563	39.600999
2757.653115	533132.585511	39.606016
2760.708331	534076.394324	39.611034
2763.431009	535047.223205	39.616052
2766.322048	535994.708787	39.621069
2768.997580	536943.123737	39.626087
2771.842150	537896.681330	39.631104
2774.961586	538852.142657	39.636122
2777.782615	539806.381674	39.641140
2780.611737	540758.341677	39.646157
2783.661026	541696.367377	39.651175
2786.312527	542643.148859	39.656192
2789.690586	543583.107332	39.661210
2792.264022	544541.342305	39.666228
2794.958598	545474.848556	39.671245
2797.926159	546424.188581	39.676263
2800.944253	547367.923920	39.681280
2803.366787	548308.022467	39.686298
2806.354160	549261.035986	39.691316
2809.047649	550199.552704	39.696333
2812.017036	551135.094061	39.701351
2814.649689	552092.342374	39.706368
2817.682190	553026.989224	39.711386
2820.566948	553983.207994	39.716404
2822.942789	554918.887776	39.721421
2826.206251	555845.260166	39.726439
2828.625272	556752.813704	39.731456
2831.618374	557664.280916	39.736474
2834.257026	558562.932129	39.741492
2836.975293	559469.648263	39.746509
2839.851562	560376.929291	39.751527
2842.348533	561287.274687	39.756544
2845.026932	562192.855792	39.761562
2847.386851	563111.184293	39.766580
2850.276961	564038.551552	39.771597
2852.828429	564970.930521	39.776615
2855.504648	565928.480241	39.781632
2858.351677	566855.050838	39.786650
2861.223126	567812.679774	39.791668
2863.661318	568769.405161	39.796685
2866.882057	569718.048621	39.801703
2869.337485	570703.491753	39.806720
2871.944824	571682.057562	39.811738
2874.742611	572658.960657	39.816756
2877.379018	573662.111789	39.821773
2880.480660	574648.948140	39.826791
2882.954872	575662.956140	39.831808
2885.997278	576666.252052	39.836826
2889.033516	577679.000381	39.841844
2891.596339	578712.161306	39.846861
2894.548905	579736.042665	39.851879
2897.313209	580769.450047	39.856896
2900.755531	581802.207515	39.861914
2903.274240	582839.292908	39.866932
2906.202176	583884.346117	39.871949
2909.129586	584929.811186	39.876967
2912.198165	585980.377003	39.881984
2915.118658	587033.282311	39.887002
2918.362780	588086.643861	39.892020
2921.355530	589145.818788	39.897037
2924.125838	590211.903043	39.902055
2927.201965	591278.994276	39.907072
2930.184947	592331.373568	39.912090
2933.133766	593401.702455	39.917108
2935.648088	594467.847822	39.922125
2939.168148	595543.699690	39.927143
2941.680739	596611.354208	39.932160
2944.856550	597692.775781	39.937178
2947.944286	598779.219802	39.942196
2950.893146	599858.223951	39.947213
2954.134288	600939.032153	39.952231
2957.100482	602032.401269	39.957248
2960.228787	603106.516062	39.962266
2963.010703	604185.843333	39.967284
2965.856656	605276.019584	39.972301
2968.951655	606357.742482	39.977319
2971.914224	607445.439299	39.982336
2975.038396	608538.208833	39.987354
2978.508444	609623.410485	39.992372
2980.873798	610713.091953	39.997389
2984.185595	611804.862456	40.002407
2987.405151	612897.391679	40.007424
2990.494737	613987.284327	40.012442
2993.269630	615069.820441	40.017460
2996.486469	616171.029105	40.022477
2999.596485	617245.395888	40.027495
3002.190002	618345.389602	40.032512
3005.693123	619423.127654	40.037530
3008.578570	620522.454129	40.042548
3011.544517	621601.064862	40.047565
3014.651453	622687.141043	40.052583
3017.265542	623779.335463	40.057600
3020.294571	624864.155904	40.062618
3023.634104	625944.968678	40.067636
3026.386242	627005.437901	40.072653
3029.231106	628048.104481	40.077671
3032.339172	629107.456566	40.082688
3035.092929	630147.085213	40.087706
3038.551083	631203.173459	40.092724
3041.183784	632258.343270	40.097741
3044.257408	633299.505421	40.102759
3047.014510	634368.720689	40.107776
3049.975882	635438.391747	40.112794
3052.819409	636506.774488	40.117812
3055.684904	637578.836277	40.122829
3058.624274	638665.744302	40.127847
3061.532083	639755.586448	40.132864
3064.419811	640849.806269	40.137882
3067.343964	641954.228914	40.142900
3070.365617	643069.389270	40.147917
3073.187195	644176.431189	40.152935
3076.351689	645314.960764	40.157952
3079.001520	646442.677262	40.162970
3082.500152	647566.039677	40.167988
3085.311927	648720.346129	40.173005
3088.542309	649871.260677	40.178023
3091.231812	651021.135061	40.183040
3094.360664	652181.368610	40.188058
3097.727688	653351.890735	40.193076
3100.604400	654528.383436	40.198093
3104.138058	655694.913774	40.203111
3107.194785	656880.261574	40.208128
3109.964145	658069.945748	40.213146
3113.202614	659254.876270	40.218164
3116.090031	660448.184720	40.223181
3119.073836	661653.477766	40.228199
3122.204492	662855.559995	40.233216
3125.159998	664062.846737	40.238234
3128.748290	665270.126319	40.243252
3131.550995	666493.704040	40.248269
3135.100073	667713.220747	40.253287
3138.227074	668939.316657	40.258304
3141.277960	670162.232507	40.263322
3144.731386	671388.305638	40.268340
3147.757738	672613.046454	40.273357
3151.090357	673839.764746	40.278375
3154.247368	675073.808230	40.283392
3157.059476	676296.859560	40.288410
3160.477206	677547.432654	40.293428
3163.732570	678790.459461	40.298445
3167.052155	680025.209496	40.303463
3170.673859	681263.420502	40.308480
3173.626470	682498.445333	40.313498
3177.068863	683740.275410	40.318516
3180.312506	684968.709938	40.323533
3183.691415	686208.823298	40.328551
3186.958168	687448.984012	40.333568
3190.235097	688677.754222	40.338586
3193.467081	689900.954165	40.343604
3196.768105	691145.811493	40.348621
3200.189919	692371.967762	40.353639
3203.364063	693600.278440	40.358656
3206.154640	694838.949396	40.363674
3209.787141	696060.990555	40.368692
3212.752331	697305.834408	40.373709
3215.796717	698527.035734	40.378727
3218.934905	699771.402853	40.383744
3222.195907	701007.344087	40.388762
3225.693522	702230.234249	40.393780
3228.645252	703473.608454	40.398797
3232.428432	704701.455621	40.403815
3235.314565	705919.912665	40.408832
3238.336237	707117.171995	40.413850
3241.709738	708295.930361	40.418868
3244.911942	709487.529522	40.423885
3247.895158	710670.878052	40.428903
3251.102807	711869.422210	40.433920
3254.044515	713069.375546	40.438938
3257.641839	714263.804366	40.443956
3260.274272	715470.100077	40.448973
3263.769802	716664.205442	40.453991
3266.949700	717874.172637	40.459008
3269.701058	719084.678517	40.464026
3273.115507	720302.812813	40.469044
3275.976100	721539.601955	40.474061
3279.491462	722769.028247	40.479079
3282.793054	724022.580160	40.484096
3285.652753	725273.097929	40.489114
3289.189986	726511.749141	40.494132
3292.472432	727780.051520	40.499149
3295.862531	729029.809548	40.504167
3298.913357	730304.476647	40.509184
3302.062993	731579.519992	40.514202
3306.042528	732853.682456	40.519220
3308.949588	734138.337263	40.524237
3311.953549	735422.030420	40.529255
3315.769724	736705.680370	40.534272
3318.630925	738002.902458	40.539290
3322.260603	739294.161645	40.544308
3325.707064	740608.083234	40.549325
3328.922381	741904.363257	40.554343
3332.175164	743214.282839	40.559360
3335.517921	744540.291337	40.564378
3339.068513	745854.800649	40.569396
3342.445780	747178.582018	40.574413
3345.724407	748498.359958	40.579431
3349.335504	749818.598217	40.584448
3352.391455	751157.769957	40.589466
3356.345950	752475.429002	40.594484
3359.408938	753805.174650	40.599501
3363.084661	755137.100454	40.604519
3366.776486	756462.686777	40.609536
3369.839536	757808.673601	40.614554
3373.538514	759139.011013	40.619572
3377.143794	760472.821140	40.624589
3380.456855	761795.816975	40.629607
3383.875865	763132.877782	40.634624
3387.161422	764476.657403	40.639642
3390.655252	765798.279482	40.644660
3394.053162	767133.548002	40.649677
3397.419401	768476.250646	40.654695
3401.267351	769809.932052	40.659712
3404.138173	771147.022953	40.664730
3407.680838	772488.133402	40.669748
3411.311647	773837.777369	40.674765
3414.843161	775170.687967	40.679783
3418.544851	776511.233023	40.684800
3421.735798	777860.059759	40.689818
3425.491867	779190.136541	40.694836
3428.589071	780528.567743	40.699853
3432.367609	781870.809358	40.704871
3435.901001	783204.354409	40.709888
3439.116887	784543.737032	40.714906
3442.614118	785888.069898	40.719924
3445.889628	787225.616233	40.724941
3449.307167	788559.750552	40.729959
3453.014918	789906.280058	40.734976
3456.290647	791253.996535	40.739994
3459.896729	792589.447058	40.745012
3463.222756	793919.642813	40.750016
3466.393888	795207.305277	40.755021
3469.998495	796434.818183	40.760026
3473.325816	797605.912693	40.765031
3476.505786	798709.798951	40.770036
3479.635221	799744.088291	40.775040
3482.593726	800707.359509	40.780045
3485.601114	801596.662516	40.785050
3488.045283	802432.971947	40.790055
3490.545571	803177.461238	40.795060
3493.301718	803879.508289	40.800064
3495.424937	804511.666798	40.805069
3497.943692	805086.975404	40.810074
3499.932833	805600.404095	40.815079
3502.088891	806017.389351	40.820084
3503.655072	806423.269887	40.825088
3505.466086	806769.432508	40.830093
3507.410771	807050.905074	40.835098
3508.624557	807298.471356	40.840103
3510.421704	807503.096408	40.845108
3511.466069	807652.408521	40.850112
3512.771706	807764.770002	40.855117
3514.094099	807822.040499	40.860122
3515.160906	807873.373522	40.865127
3515.870991	807869.188864	40.870132
3517.155573	807852.167169	40.875136
3517.778861	807791.390909	40.880141
3519.055092	807700.169227	40.885146
3519.610312	807591.323139	40.890151
3520.429925	807444.398449	40.895156
3520.995675	807292.169985	40.900160
3521.368104	807102.669982	40.905165
3522.049809	806884.488386	40.910170
3522.397188	806664.688303	40.915175
3522.636245	806419.261846	40.920180
3523.102490	806175.799011	40.925184
3523.311917	805907.662192	40.930189
3523.832689	805627.305329	40.935194
3523.817035	805344.868171	40.940199
3524.246266	805029.790581	40.945204
3524.870117	804732.710081	40.950208
3524.667676	804405.057691	40.955213
3525.158761	804073.989949	40.960218
3525.313511	803737.812601	40.965223
3525.459416	803393.479435	40.970228
3525.724753	803046.510033	40.975232
3525.394812	802687.997282	40.980237
3526.019287	802314.201580	40.985242
3525.840314	801932.375435	40.990247
3525.919817	801565.201821	40.995252
3526.009884	801186.920094	41.000256
3525.880651	800798.645632	41.005261
3525.994499	800412.418988	41.010266
3525.821119	800039.760059	41.015271
3525.931719	799643.432713	41.020276
3526.082851	799256.890137	41.025280
3525.834168	798849.732025	41.030285
3525.878340	798454.770835	41.035290
3525.628571	798062.976680	41.040295
3525.348380	797653.594179	41.045300
3525.532208	797270.420509	41.050304
3525.724112	796871.418323	41.055309
3525.571809	796472.057299	41.060314
3525.443566	796082.291670	41.065319
3525.344645	795670.308186	41.070324
3525.244256	795270.673525	41.075328
3525.079234	794871.321293	41.080333
3525.078446	794465.781194	41.085338
3524.936332	794076.789990	41.090343
3524.763236	793666.812443	41.095348
3524.694559	793280.858939	41.100352
3524.747924	792878.508734	41.105357
3524.450573	792485.673100	41.110362
3524.374313	792097.494710	41.115367
3524.623371	791689.297157	41.120372
3524.115126	791301.833854	41.125376
3523.974848	790906.477122	41.130381
3523.704362	790511.807561	41.135386
3523.517683	790121.769940	41.140391
3523.614385	789732.794283	41.145396
3522.925297	789350.904606	41.150400
3523.299120	788978.352861	41.155405
3523.438578	788589.258268	41.160410
3522.777840	788216.345536	41.165415
3522.948601	787828.481954	41.170420
3522.798263	787461.441870	41.175424
3522.405875	787089.507186	41.180429
3522.625735	786703.343809	41.185434
3522.237867	786332.401186	41.190439
3522.271881	785967.220195	41.195444
3522.058576	785597.292199	41.200448
3521.786471	785240.040170	41.205453
3521.931575	784871.785642	41.210458
3521.465560	784505.284759	41.215463
3521.653545	784139.985113	41.220468
3521.555239	783766.943851	41.225472
3521.220938	783424.906009	41.230477
3521.255124	783069.265802	41.235482
3520.793169	782704.787149	41.240487
3520.812968	782361.804211	41.245492
3520.757666	782018.964878	41.250496
3520.435883	781658.296173	41.255501
3520.549544	781319.724706	41.260506
3520.368352	780976.266195	41.265511
3520.446845	780630.239369	41.270516
3520.152355	780303.003433	41.275520
3519.710051	779950.239985	41.280525
3519.882558	779600.556482	41.285530
3519.252465	779277.610464	41.290535
3519.631766	778933.322890	41.295540
3519.633852	778620.774675	41.300544
3519.067359	778290.293763	41.305549
3519.220874	777961.549457	41.310554
3518.775585	777644.997101	41.315559
3518.696240	777319.658335	41.320564
3518.737378	777000.192112	41.325568
3518.126183	776695.981140	41.330573
3518.464117	776376.487905	41.335578
3518.026499	776072.813079	41.340583
3517.907144	775753.564849	41.345588
3518.002059	775464.300646	41.350592
3517.698723	775150.816870	41.355597
3517.919476	774843.634374	41.360602
3517.524188	774557.467905	41.365607
3517.201331	774250.054637	41.370612
3517.344014	773958.950342	41.375616
3516.821654	773673.311982	41.380621
3516.936164	773365.789590	41.385626
3516.668223	773099.589521	41.390631
3516.664129	772796.741670	41.395636
3516.504156	772519.125412	41.400640
3516.226397	772235.804342	41.405645
3516.209367	771963.660306	41.410650
3516.455983	771677.374379	41.415655
3515.904619	771398.795183	41.420660
3516.029556	771129.355638	41.425664
3515.226096	770854.935606	41.430669
3515.845774	770583.670339	41.435674
3515.664469	770322.380955	41.440679
3515.403142	770052.374559	41.445684
3515.165049	769787.331035	41.450688
3515.310081	769528.916232	41.455693
3515.358575	769257.745773	41.460698
3515.217739	768998.817555	41.465703
3514.995299	768742.062054	41.470708
3514.575599	768497.157708	41.475712
3514.560422	768237.886551	41.480717
3514.298932	767979.238352	41.485722
3514.207118	767742.042083	41.490727
3514.393547	767499.272155	41.495732
3514.268693	767253.686806	41.500736
3513.816558	767014.505850	41.505741
3514.222310	766766.943965	41.510746
3513.678103	766539.593204	41.515751
3513.593662	766296.779443	41.520756
3513.976783	766067.831931	41.525760
3513.759493	765825.813504	41.530765
3513.595066	765589.250895	41.535770
3513.624461	765368.573442	41.540775
3513.297840	765132.861254	41.545780
3513.158010	764908.993395	41.550784
3513.002338	764678.760905	41.555789
3512.792264	764447.692066	41.560794
3512.813925	764233.836270	41.565799
3512.660754	764011.571011	41.570804
3512.648602	763805.844893	41.575808
3512.653393	763586.203875	41.580813
3512.658527	763372.572833	41.585818
3512.413556	763164.993547	41.590823
3512.144277	762943.307602	41.595828
3512.386557	762730.852201	41.600832
3511.971844	762526.094452	41.605837
3512.008718	762314.006378	41.610842
3511.760301	762112.958473	41.615847
3511.921662	761900.986232	41.620852
3512.020813	761710.129868	41.625856
3511.856015	761512.998270	41.630861
3511.420062	761295.040157	41.635866
3511.314366	761101.094431	41.640871
3511.522933	760898.902942	41.645876
3511.292934	760707.828821	41.650880
3510.953559	760518.889248	41.655885
3510.969468	760317.996650	41.660890
3510.634867	760135.213596	41.665895
3510.839971	759948.390196	41.670900
3510.805722	759764.068567	41.675904
3510.481751	759589.016759	41.680909
3510.737501	759402.516938	41.685914
3510.556724	759215.887090	41.690919
3510.310995	759034.937857	41.695924
3510.287742	758870.527446	41.700928
3510.184148	758692.013847	41.705933
3510.406912	758518.919780	41.710938
3509.936629	758352.992725	41.715943
3509.798039	758164.158765	41.720948
3509.870260	757996.802117	41.725952
3509.568924	757837.745008	41.730957
3509.710007	757666.619056	41.735962
3509.553028	757500.424364	41.740967
3509.741282	757353.170636	41.745972
3509.573541	757189.241232	41.750976
3509.405105	757029.306294	41.755981
3509.533897	756863.741622	41.760986
3509.249220	756700.018397	41.765991
3509.680422	756550.685440	41.770996
3509.401586	756385.621798	41.776000
3509.223493	756223.993308	41.781005
3509.404095	756063.190825	41.786010
3509.093253	755916.583968	41.791015
3509.277011	755754.589745	41.796020
3509.031143	755597.698192	41.801024
3509.069438	755466.723479	41.806029
3509.178733	755297.721792	41.811034
3509.043516	755147.862361	41.816039
3509.144660	754999.047183	41.821044
3508.820949	754843.535347	41.826048
3508.560807	754698.476657	41.831053
3508.599639	754555.587721	41.836058
3508.517916	754405.655587	41.841063
3508.304087	754262.259710	41.846068
3508.638470	754113.339539	41.851072
3508.305052	753976.129933	41.856077
3508.576026	753830.226669	41.861082
3507.899375	753706.647505	41.866087
3507.901414	753554.857970	41.871092
3508.350186	753421.015467	41.876096
3508.031479	753295.148614	41.881101
3508.247410	753152.648821	41.886106
3508.107574	753019.587664	41.891111
3507.978087	752878.028585	41.896116
3507.869967	752743.278394	41.901120
3507.946208	752629.582828	41.906125
3507.895776	752486.768909	41.911130
3507.963557	752357.810510	41.916135
3507.852160	752230.311713	41.921140
3507.338645	752097.592523	41.926144
3507.326946	751976.740518	41.931149
3507.028383	751853.661955	41.936154
3506.828210	751735.948790	41.941159
3507.137175	751616.717589	41.946164
3506.908988	751506.513022	41.951168
3507.001966	751392.598898	41.956173
3507.241994	751259.296589	41.961178
3506.885215	751152.269347	41.966183
3506.654658	751044.676480	41.971188
3506.942006	750924.894825	41.976192
3506.546566	750829.428081	41.981197
3506.879567	750703.164545	41.986202
3506.920829	750602.633929	41.991207
3506.661253	750486.442852	41.996212
3506.828186	750368.549575	42.001216
3506.687125	750263.796259	42.006221
3506.722820	750149.823876	42.011226
3506.374252	750045.052392	42.016231
3506.587350	749935.246738	42.021236
3506.689902	749819.232992	42.026240
3506.431297	749719.530771	42.031245
3506.439070	749618.153041	42.036250
3506.277023	749515.813874	42.041255
3506.539483	749403.374106	42.046260
3506.409752	749308.882350	42.051264
3506.537364	749209.752218	42.056269
3506.640003	749094.913391	42.061274
3506.606193	748992.546195	42.066279
3506.190136	748889.795955	42.071284
3506.344160	748787.543335	42.076288
3506.427629	748673.343758	42.081293
3506.239823	748575.097475	42.086298
3506.382844	748479.068361	42.091303
3506.068566	748373.280428	42.096308
3506.123675	748266.787826	42.101312
3505.676341	748175.842924	42.106317
3505.504551	748081.738482	42.111322
3505.820676	747991.159762	42.116327
3505.393774	747902.234285	42.121332
3505.700329	747815.707131	42.126336
3505.977638	747725.823541	42.131341
3505.812899	747622.669235	42.136346
3506.018298	747531.708088	42.141351
3505.543316	747445.107928	42.146356
3505.868303	747347.305252	42.151360
3505.411813	747262.726177	42.156365
3505.759145	747158.492973	42.161370
3505.726567	747074.830405	42.166375
3505.614811	746992.613190	42.171380
3505.670170	746888.029118	42.176384
3505.280297	746812.873674	42.181389
3505.618933	746718.223870	42.186394
3505.407901	746636.562910	42.191399
3505.040264	746555.470559	42.196404
3505.473984	746464.657052	42.201408
3505.293049	746385.064315	42.206413
3505.473698	746304.175560	42.211418
3505.175581	746218.965974	42.216423
3505.150374	746130.992049	42.221428
3505.367725	746057.508625	42.226432
3505.168744	745969.017818	42.231437
3505.507985	745871.490889	42.236442
3505.435013	745804.626830	42.241447
3505.483818	745721.727220	42.246452
3505.850191	745638.922694	42.251456
3505.277517	745544.606571	42.256461
3505.480826	745448.975116	42.261466
3505.442867	745367.914986	42.266471
3505.281766	745286.676583	42.271476
3505.105714	745199.359654	42.276480
3505.264524	745114.013314	42.281485
3505.046741	745035.401574	42.286490
3505.155167	744948.034972	42.291495
3504.744721	744875.978622	42.296500
3504.890674	744791.174663	42.301504
3504.767244	744731.873265	42.306509
3504.888893	744649.939017	42.311514
3504.533278	744572.185748	42.316519
3504.975465	744506.412194	42.321524
3504.836199	744429.313972	42.326528
3504.751070	744364.219359	42.331533
3504.873961	744280.402432	42.336538
3504.759384	744208.340634	42.341543
3504.455851	744137.545280	42.346548
3504.531546	744066.142969	42.351552
3504.466240	744002.030873	42.356557
3504.616077	743927.994790	42.361562
3504.473422	743860.927881	42.366567
3504.567743	743788.728934	42.371572
3504.343008	743724.245314	42.376576
3504.308404	743658.345466	42.381581
3504.544046	743596.652566	42.386586
3504.664910	743529.292198	42.391591
3504.225305	743460.935857	42.396596
3504.093062	743388.869458	42.401600
3504.168903	743334.221805	42.406605
3504.461105	743262.578752	42.411610
3504.345964	743204.105010	42.416615
3504.411406	743136.157075	42.421620
3504.576066	743065.126583	42.426624
3504.155183	743003.339433	42.431629
3504.368645	742927.256172	42.436634
3504.298655	742856.855824	42.441639
3504.187939	742797.883870	42.446644
3504.346157	742736.938705	42.451648
3504.133095	742681.542969	42.456653
3504.331299	742612.579685	42.461658
3504.375515	742553.283682	42.466663
3504.260245	742485.211567	42.471668
3504.680839	742424.072405	42.476672
3504.415551	742361.611739	42.481677
3504.748383	742284.563064	42.486682
3504.419793	742216.474329	42.491687
3503.970548	742155.872025	42.496692
3504.248265	742092.132922	42.501696
3504.195992	742020.683708	42.506701
3504.349370	741965.766537	42.511706
3504.071400	741918.931403	42.516711
3504.148326	741837.173070	42.521716
3504.412462	741776.054676	42.526720
3504.340034	741722.409362	42.531725
3504.163229	741637.871901	42.536730
3504.134438	741578.184970	42.541735
3504.027797	741519.895161	42.546740
3504.417301	741456.231424	42.551744
3504.170802	741395.342595	42.556749
3504.161172	741330.457757	42.561754
3503.754553	741277.754705	42.566759
3504.079190	741215.731794	42.571764
3504.002187	741163.468239	42.576768
3503.666934	741105.806537	42.581773
3503.802663	741044.654195	42.586778
3504.267669	740988.046769	42.591783
3503.757966	740931.550087	42.596788
3504.131055	740870.555126	42.601792
3504.128848	740814.666417	42.606797
3504.388626	740758.190085	42.611802
3504.283152	740701.724076	42.616807
3503.781143	740630.633170	42.621812
3504.299544	740568.870034	42.626816
3503.881702	740510.970299	42.631821
3504.193817	740451.268160	42.636826
3504.011140	740389.668610	42.641831
3503.740701	740332.732529	42.646836
3503.911065	740284.725663	42.651840
3504.165393	740225.080806	42.656845
3504.038194	740156.149730	42.661850
3503.979116	740108.723705	42.666855
3503.733631	740050.544885	42.671860
3504.066723	739983.218251	42.676864
3503.961809	739929.170420	42.681869
3504.366666	739868.360383	42.686874
3503.833075	739799.740499	42.691879
3503.923136	739751.298446	42.696884
3503.803379	739690.029358	42.701888
3503.605223	739633.274211	42.706893
3504.112166	739579.073711	42.711898
3503.760668	739527.091933	42.716903
3503.626472	739475.618156	42.721908
3503.809490	739422.805601	42.726912
3503.379869	739377.860212	42.731917
3503.656926	739324.586292	42.736922
3503.718947	739268.676109	42.741927
3503.636905	739215.559568	42.746932
3503.914779	739162.680186	42.751936
3503.615071	739105.690653	42.756941
3503.795542	739058.367295	42.761946
3503.799659	739007.263458	42.766951
3503.621209	738949.708647	42.771956
3503.789013	738885.665055	42.776960
3503.527104	738848.456077	42.781965
3503.393252	738792.871655	42.786970
3503.557693	738737.188222	42.791975
3503.579344	738698.695005	42.796980
3503.689655	738639.160927	42.801985
3503.585940	738608.108901	42.806989
3503.392611	738544.369436	42.811994
3503.461858	738487.957839	42.816999
3503.362826	738454.381262	42.822004
3503.648755	738404.315553	42.827009
3503.257191	738368.313083	42.832013
3503.491968	738307.271770	42.837018
3503.513549	738260.068800	42.842023
3503.245257	738209.351056	42.847028
3503.504031	738169.084554	42.852033
3503.197439	738119.263116	42.857037
3503.565882	738058.445256	42.862042
3503.580998	738016.140106	42.867047
3503.590544	737978.684423	42.872052
3503.411239	737916.224029	42.877057
3503.178780	737881.083735	42.882061
3503.643710	737830.787022	42.887066
3503.582746	737796.013920	42.892071
3503.315854	737750.686169	42.897076
3503.395651	737696.246379	42.902081
3503.042615	737656.721330	42.907085
3503.324856	737602.445460	42.912090
3503.600441	737562.173127	42.917095
3503.448043	737504.653059	42.922100
3503.480664	737463.579100	42.927105
3503.769305	737417.564152	42.932109
3503.480851	737362.786921	42.937114
3503.293589	737303.242422	42.942119
3503.152488	737257.990105	42.947124
3503.517777	737211.417042	42.952129
3503.232902	737169.503209	42.957133
3503.332271	737125.892918	42.962138
3503.352997	737068.885492	42.967143
3503.322377	737032.866994	42.972148
3503.246930	736979.882912	42.977153
3503.428104	736947.490905	42.982157
3503.557535	736896.204438	42.987162
3503.408339	736846.893440	42.992167
3503.253904	736807.479912	42.997172
3503.668500	736758.025982	43.002177
3503.355624	736714.134980	43.007181
3503.367536	736657.422983	43.012186
3503.329932	736610.764354	43.017191
3503.615095	736564.794560	43.022196
3503.675657	736519.257401	43.027201
3503.315104	736473.492453	43.032205
3503.418268	736412.705785	43.037210
3503.256764	736364.086654	43.042215
3503.296219	736323.104684	43.047220
3503.679360	736269.396994	43.052225
3503.284163	736232.049302	43.057229
3503.262640	736178.655123	43.062234
3503.362463	736138.602541	43.067239
3503.173684	736109.435377	43.072244
3503.051560	736059.917111	43.077249
3503.116162	736027.194166	43.082253
3503.150761	735981.163332	43.087258
3503.234005	735934.233399	43.092263
3503.150195	735890.003188	43.097268
3503.092352	735858.339024	43.102273
3503.270931	735821.389774	43.107277
3503.247556	735766.557925	43.112282
3503.407720	735729.759761	43.117287
3503.105481	735684.772550	43.122292
3503.190111	735638.682014	43.127297
3503.387258	735596.779494	43.132301
3503.410059	735546.095856	43.137306
3503.043614	735504.038256	43.142311
3503.147760	735466.901668	43.147316
3503.635679	735410.498352	43.152321
3503.190527	735375.382084	43.157325
3503.547587	735329.195388	43.162330
3503.335963	735291.219132	43.167335
3503.260196	735241.985137	43.172340
3503.357225	735187.228477	43.177345
3503.170467	735155.978737	43.182349
3503.168782	735104.850894	43.187354
3503.323567	735065.427333	43.192359
3502.910953	735028.027398	43.197364
3503.402796	734972.857751	43.202369
3503.108436	734931.280226	43.207373
3503.327938	734891.746158	43.212378
3503.311142	734858.289413	43.217383
3503.202451	734805.395419	43.222388
3503.526416	734743.074808	43.227393
3503.048939	734700.783803	43.232397
3503.230096	734674.619307	43.237402
3502.800433	734634.646466	43.242407
3503.010786	734595.260941	43.247412
3503.274381	734541.808886	43.252417
3502.889001	734519.301128	43.257421
3503.189138	734471.534928	43.262426
3503.244797	734423.957226	43.267431
3502.810040	734390.072409	43.272436
3502.904673	734342.537303	43.277441
3502.949808	734319.067049	43.282445
3502.822048	734275.478681	43.287450
3502.724562	734234.013606	43.292455
3502.859378	734196.767095	43.297460
3503.362106	734150.896135	43.302465
3502.870457	734118.653077	43.307469
3502.963577	734080.917889	43.312474
3502.936744	734039.489671	43.317479
3502.761573	733999.174722	43.322484
3502.957032	733958.848003	43.327489
3502.798723	733932.489520	43.332493
3502.748281	733882.104469	43.337498
3503.081863	733857.446781	43.342503
3502.729671	733810.774204	43.347508
3502.889329	733776.046307	43.352513
3502.475987	733744.976922	43.357517
3502.752120	733710.724585	43.362522
3502.862315	733679.766698	43.367527
3502.686162	733649.103394	43.372532
3502.980994	733609.699130	43.377537
3502.896570	733569.664103	43.382541
3502.886034	733535.210734	43.387546
3503.008891	733493.557023	43.392551
3502.920492	733464.116179	43.397556
3503.444132	733418.881179	43.402561
3502.897785	733378.426261	43.407565
3502.870399	733324.122972	43.412570
3503.097450	733291.758172	43.417575
3502.842981	733256.997265	43.422580
3503.048564	733217.655299	43.427585
3502.744477	733185.922166	43.432589
3503.106431	733143.088591	43.437594
3503.165643	733104.166247	43.442599
3503.057134	733070.915215	43.447604
3503.303427	733020.822437	43.452609
3503.141285	732985.253019	43.457613
3503.220358	732943.009583	43.462618
3503.092177	732903.325015	43.467623
3503.167630	732865.587051	43.472628
3503.100342	732829.951809	43.477633
3502.989554	732785.461418	43.482637
3503.171172	732746.517181	43.487642
3502.837998	732706.617875	43.492647
3502.751293	732677.223389	43.497652
3503.182104	732621.800165	43.502657
3502.968593	732593.218432	43.507661
3503.118534	732551.010780	43.512666
3503.077238	732504.725004	43.517671
3502.599705	732467.422875	43.522676
3502.909766	732442.814259	43.527681
3502.932390	732405.132359	43.532685
3503.015389	732353.676027	43.537690
3503.158225	732324.192921	43.542695
3502.809892	732279.837910	43.547700
3502.999866	732247.821626	43.552705
3502.687310	732209.005739	43.557709
3502.817153	732165.908157	43.562714
3502.712323	732144.387296	43.567719
3502.765267	732097.984636	43.572724
3502.845884	732055.686794	43.577729
3502.653328	732030.615093	43.582733
3502.586524	731998.491592	43.587738
3503.082514	731967.067457	43.592743
3502.830013	731927.695665	43.597748
3503.025426	731895.924665	43.602753
3502.599542	731862.968527	43.607757
3502.544458	731823.860790	43.612762
3502.672649	731791.753852	43.617767
3502.607332	731753.786315	43.622772
3502.471139	731720.039126	43.627777
3502.751941	731681.320996	43.632781
3502.745134	731656.564140	43.637786
3502.887965	731615.986816	43.642791
3502.613750	731590.580591	43.647796
3502.785725	731560.693770	43.652801
3502.778048	731519.298976	43.657805
3502.688750	731485.345012	43.662810
3502.810478	731451.603721	43.667815
3502.608813	731418.460272	43.672820
3503.012588	731369.717816	43.677825
3502.907711	731341.410862	43.682829
3502.663734	731312.631546	43.687834
3502.919790	731270.597805	43.692839
3502.587814	731246.190386	43.697844
3502.725272	731196.450878	43.702849
3502.819812	731176.479199	43.707853
3502.603088	731144.277972	43.712858
3502.901098	731116.052403	43.717863
3502.561926	731082.633119	43.722868
3502.497716	731043.968795	43.727873
3502.468627	731011.835164	43.732877
3502.500728	730987.218412	43.737882
3502.943978	730951.144125	43.742887
3502.654105	730915.834249	43.747892
3502.668877	730878.295099	43.752897
3502.984814	730849.025707	43.757901
3502.834757	730810.820108	43.762906
3502.870435	730771.642813	43.767911
3502.793729	730738.525513	43.772916
3502.911520	730696.709669	43.777921
3502.862559	730675.423307	43.782925
3502.928282	730629.901532	43.787930
3502.627789	730580.973252	43.792935
3502.990241	730569.374803	43.797940
3502.975715	730522.033301	43.802945
3503.018901	730486.171442	43.807949
3502.862174	730443.706202	43.812954
3502.978992	730412.833770	43.817959
3502.809920	730365.566344	43.822964
3502.965664	730336.767221	43.827969
3503.010551	730305.510040	43.832973
3502.936780	730261.742543	43.837978
3502.967402	730234.796090	43.842983
3502.813779	730190.892794	43.847988
3503.109995	730154.938254	43.852993
3502.858037	730130.415235	43.857997
3503.113298	730082.729565	43.863002
3503.151229	730037.852888	43.868007
3503.017901	730004.989554	43.873012
3503.148084	729953.213051	43.878017
3503.082946	729919.545710	43.883021
3502.736033	729878.594657	43.888026
3502.840696	729843.611319	43.893031
3502.925190	729812.741934	43.898036
3503.059303	729764.480031	43.903041
3502.847728	729741.781711	43.908045
3502.776169	729694.989594	43.913050
3503.026897	729649.927127	43.918055
3502.626397	729625.526116	43.923060
3503.057113	729587.219061	43.928065
3502.953097	729558.261869	43.933069
3502.806428	729518.514230	43.938074
3502.718722	729478.558563	43.943079
3502.825116	729451.398911	43.948084
3502.840944	729407.364401	43.953089
3502.733630	729380.140666	43.958093
3502.483033	729341.152236	43.963098
3502.874118	729308.694981	43.968103
3502.787618	729286.172901	43.973108
3502.914495	729247.567600	43.978113
3502.987392	729202.928210	43.983117
3502.766210	729161.160325	43.988122
3503.009875	729128.429455	43.993127
3502.809013	729097.009997	43.998132
3502.706016	729063.246286	44.003137
3502.824461	729026.969335	44.008141
3502.894628	728982.874044	44.013146
3503.086534	728944.008928	44.018151
3502.614380	728912.930658	44.023156
3503.215847	728870.233201	44.028161
3503.070432	728833.156801	44.033165
3503.074657	728790.705939	44.038170
3503.240973	728757.639591	44.043175
3502.971852	728724.842994	44.048180
3502.785806	728689.258657	44.053185
3502.877924	728650.755327	44.058189
3502.752253	728611.841888	44.063194
3502.628569	728570.897000	44.068199
3502.967069	728543.349332	44.073204
3502.869385	728499.576297	44.078209
3502.874570	728464.157607	44.083213
3503.057362	728432.573298	44.088218
3502.898586	728397.131798	44.093223
3502.898285	728349.131341	44.098228
3502.895807	728318.468772	44.103233
3502.816150	728284.598917	44.108237
3502.774556	728247.255060	44.113242
3502.839843	728214.797604	44.118247
3502.516952	728178.589602	44.123252
3502.834237	728136.826814	44.128257
3502.847478	728104.872873	44.133261
3503.015160	728072.348441	44.138266
3502.660948	728031.686522	44.143271
3502.952156	727998.745137	44.148276
3502.683813	727961.833645	44.153281
3502.552534	727931.091767	44.158285
3502.909960	727895.761188	44.163290
3502.698087	727863.397544	44.168295
3502.532330	727843.757816	44.173300
3502.765378	727806.218070	44.178305
3502.413621	727774.570678	44.183309
3502.499288	727744.535448	44.188314
3502.871330	727708.607172	44.193319
3502.515235	727672.105151	44.198324
3502.932416	727641.569053	44.203329
3502.546901	727600.018409	44.208333
3502.484535	727569.660142	44.213338
3502.981656	727541.736178	44.218343
3502.574474	727507.223488	44.223348
3502.568540	727479.184035	44.228353
3502.576418	727451.439461	44.233357
3502.492691	727428.961336	44.238362
3502.651410	727382.266627	44.243367
3502.473567	727349.598086	44.248372
3502.539425	727310.399171	44.253377
3502.832400	727287.511786	44.258381
3502.523913	727256.251597	44.263386
3502.937644	727221.800607	44.268391
3502.827810	727192.191908	44.273396
3503.258123	727156.449782	44.278401
3503.130010	727109.156712	44.283405
3502.804111	727062.490489	44.288410
3503.020274	727030.944811	44.293415
3502.623181	727004.652694	44.298420
3502.633197	726962.240919	44.303425
3502.578020	726934.703163	44.308429
3502.639003	726900.606216	44.313434
3502.810830	726871.594033	44.318439
3502.307420	726845.764831	44.323444
3502.091269	726811.069085	44.328449
3502.263246	726776.606513	44.333453
3502.188275	726750.656868	44.338458
3502.460605	726736.194171	44.343463
3502.168616	726717.811191	44.348468
3502.739828	726670.994911	44.353473
3502.456740	726645.326957	44.358477
3502.513077	726619.900274	44.363482
3502.858211	726577.728570	44.368487
3502.693702	726554.567694	44.373492
3502.804157	726515.704458	44.378497
3502.608810	726482.787602	44.383501
3502.490187	726448.867014	44.388506
3502.572598	726419.521130	44.393511
3502.362681	726393.988975	44.398516
3502.768318	726368.206666	44.403521
3502.882809	726335.634552	44.408525
3502.545390	726305.118722	44.413530
3502.771347	726269.505504	44.418535
3502.549660	726229.159622	44.423540
3502.710906	726197.570239	44.428545
3502.461133	726174.967382	44.433549
3502.621082	726135.549145	44.438554
3502.930595	726104.579121	44.443559
3502.578363	726076.591928	44.448564
3502.849294	726041.069409	44.453569
3502.898131	726009.051871	44.458573
3502.499365	725975.175483	44.463578
3503.021653	725936.538949	44.468583
3502.898496	725912.427975	44.473588
3502.999493	725865.040419	44.478593
3503.238167	725829.423198	44.483597
3503.107707	725784.055379	44.488602
3503.116327	725744.412440	44.493607
3502.729763	725714.249373	44.498612
3502.696590	725674.266116	44.503617
3503.269875	725623.330665	44.508621
3503.121258	725597.637269	44.513626
3502.933759	725552.178461	44.518631
3502.568968	725509.920041	44.523636
3502.923703	725473.439743	44.528641
3502.971473	725455.443927	44.533645
3502.608565	725406.742660	44.538650
3502.815994	725375.043397	44.543655
3502.530590	725351.254835	44.548660
3502.574689	725300.949685	44.553665
3502.776627	725285.405833	44.558669
3502.639695	725259.313014	44.563674
3502.526296	725212.254351	44.568679
3502.334311	725184.039484	44.573684
3502.420806	725155.035298	44.578689
3502.530610	725133.807436	44.583693
3502.432325	725101.067264	44.588698
3502.531699	725070.177528	44.593703
3502.505960	725036.235795	44.598708
3502.574999	725007.233965	44.603713
3502.309215	724986.364949	44.608717
3502.330202	724950.185110	44.613722
3502.171512	724924.739054	44.618727
3502.191817	724901.344827	44.623732
3502.152303	724874.887835	44.628737
3502.090920	724859.039666	44.633741
3502.359029	724820.935355	44.638746
3502.144295	724797.480446	44.643751
3501.857031	724763.778914	44.648756
3502.468365	724750.842729	44.653761
3502.343210	724718.006343	44.658765
3502.165047	724704.109893	44.663770
3502.451127	724666.200138	44.668775
3502.363084	724647.977141	44.673780
3502.874042	724621.279952	44.678785
3502.578258	724596.896208	44.683789
3502.277653	724552.392128	44.688794
3502.529205	724527.620634	44.693799
3502.521519	724517.908332	44.698804
3502.407562	724476.594455	44.703809
3502.458312	724452.450540	44.708813
3502.322425	724422.489219	44.713818
3502.479642	724394.065420	44.718823
3502.296087	724362.872729	44.723828
3502.676760	724322.021739	44.728833
3502.570907	724306.625880	44.733837
3502.317914	724273.560982	44.738842
3502.675100	724242.179611	44.743847
3502.297717	724222.268706	44.748852
3502.210957	724187.738795	44.753857
3502.721143	724161.882795	44.758861
3502.305940	724135.287083	44.763866
3502.377009	724093.742551	44.768871
3502.256094	724080.925980	44.773876
3502.582885	724042.709279	44.778881
3502.293796	724017.975778	44.783885
3502.294643	723994.681308	44.788890
3502.491489	723958.121196	44.793895
3502.359288	723932.370329	44.798900
3502.666882	723897.774222	44.803905
3502.390215	723877.399817	44.808909
3502.352047	723847.271612	44.813914
3502.501720	723805.464858	44.818919
3502.183892	723796.199319	44.823924
3502.619196	723756.476498	44.828929
3502.691014	723737.630376	44.833933
3502.549607	723705.585659	44.838938
3502.693603	723675.972020	44.843943
3502.288357	723652.247853	44.848948
3502.307171	723611.849493	44.853953
3502.547795	723595.800435	44.858957
3502.258220	723564.622191	44.863962
3502.230806	723535.829338	44.868967
3502.256853	723497.857934	44.873972
3502.381734	723479.250307	44.878977
3502.627192	723456.855763	44.883981
3502.302602	723436.289899	44.888986
3502.124114	723398.401307	44.893991
3502.083650	723391.667053	44.898996
3502.426926	723346.752965	44.904001
3502.153425	723328.111509	44.909005
3502.208925	723299.056334	44.914010
3502.299292	723272.671931	44.919015
3502.000566	723248.829914	44.924020
3502.619043	723226.373281	44.929025
3502.588994	723205.163500	44.934029
3502.159805	723180.500137	44.939034
3502.709034	723145.761933	44.944039
3502.176968	723117.001206	44.949044
3502.525240	723082.147144	44.954049
3502.440605	723072.148410	44.959053
3502.183947	723028.967203	44.964058
3502.541391	723009.923651	44.969063
3502.260090	722980.575874	44.974068
3502.246087	722963.130052	44.979073
3502.065928	722921.571450	44.984077
3501.998529	722909.289499	44.989082
3502.350273	722865.908050	44.994087
3502.198185	722863.107743	44.999092
3502.089958	722833.681356	45.004097
3502.377744	722816.036787	45.009101
3502.254132	722776.946627	45.014106
3502.457521	722766.057372	45.019111
3502.053884	722732.713697	45.024116
3502.511313	722697.988743	45.029121
3502.265757	722678.795939	45.034125
3502.496833	722658.929705	45.039130
3502.757705	722621.014721	45.044135
3502.539224	722610.095634	45.049140
3502.546504	722569.545368	45.054145
3502.424063	722543.044989	45.059149
3502.035334	722506.376661	45.064154
3502.355849	722493.336170	45.069159
3502.381644	722469.785431	45.074164
3502.549140	722443.088242	45.079169
3502.736615	722409.298857	45.084173
3502.344527	722369.556999	45.089178
3502.809464	722332.598519	45.094183
3502.491179	722297.256117	45.099188
3502.516114	722277.621227	45.104193
3502.800723	722249.119489	45.109197
3502.716218	722221.620368	45.114202
3502.754287	722191.225696	45.119207
3502.323633	722156.049926	45.124212
3502.527177	722128.602179	45.129217
3502.541998	722103.069251	45.134221
3502.245138	722074.117410	45.139226
3502.546250	722035.300781	45.144231
3502.433316	722015.291392	45.149236
3502.437829	721988.074274	45.154241
3502.331986	721963.849742	45.159245
3502.684351	721936.178537	45.164250
3502.556580	721898.820039	45.169255
3502.230514	721885.389384	45.174260
3502.415369	721839.898327	45.179265
3502.390696	721828.500091	45.184269
3502.173729	721793.089264	45.189274
3502.499207	721775.138817	45.194279
3502.241652	721746.377656	45.199284
3502.432863	721726.515758	45.204289
3502.315723	721689.699905	45.209293
3502.734456	721663.652880	45.214298
3502.480801	721629.635546	45.219303
3502.436369	721608.671927	45.224308
3502.471318	721569.946556	45.229313
3502.647350	721543.046755	45.234317
3502.180507	721514.715895	45.239322
3502.394195	721471.895256	45.244327
3502.501840	721457.202572	45.249332
3502.593123	721423.226709	45.254337
3502.331511	721400.612695	45.259341
3502.391043	721367.732557	45.264346
3502.568532	721340.583968	45.269351
3502.246619	721306.824449	45.274356
3502.134859	721280.467007	45.279361
3502.371765	721248.499169	45.284365
3502.296080	721228.531321	45.289370
3502.501605	721200.039014	45.294375
3502.153289	721193.552015	45.299380
3502.462007	721161.819908	45.304385
3502.393149	721139.669218	45.309389
3502.403713	721102.631397	45.314394
3502.433910	721079.918845	45.319399
3502.112529	721053.843124	45.324404
3502.245763	721040.533735	45.329409
3502.339981	721004.721202	45.334413
3502.165189	720977.232830	45.339418
3502.075934	720940.607380	45.344423
3502.035119	720929.508054	45.349428
3502.190893	720900.328783	45.354433
3502.292692	720882.413268	45.359437
3502.052965	720867.776782	45.364442
3502.588480	720826.387228	45.369447
3502.419775	720814.813007	45.374452
3502.518443	720781.725773	45.379457
3502.294358	720748.939502	45.384461
3502.527322	720724.903433	45.389466
3502.173011	720686.039753	45.394471
3502.167051	720672.405634	45.399476
3502.324502	720631.870731	45.404481
3502.410371	720608.056894	45.409485
3502.301809	720591.216657	45.414490
3502.556254	720553.243706	45.419495
3502.350470	720534.188125	45.424500
3502.290080	720505.737257	45.429505
3502.326083	720475.534977	45.434509
3502.358611	720453.861589	45.439514
3502.693633	720413.940956	45.444519
3502.361212	720403.285650	45.449524
3502.398600	720356.620752	45.454529
3502.177948	720341.484348	45.459533
3502.363254	720319.140836	45.464538
3502.512639	720296.704013	45.469543
3502.359435	720265.887547	45.474548
3502.470725	720250.894622	45.479553
3502.606961	720210.509919	45.484557
3502.014903	720181.897622	45.489562
3502.471067	720144.187081	45.494567
3502.285151	720131.920543	45.499572
3502.247202	720093.299474	45.504577
3501.815914	720089.453336	45.509581
3501.933092	720055.418031	45.514586
3502.348820	720022.820985	45.519591
3502.278863	720015.394636	45.524596
3502.259886	719983.612863	45.529601
3502.349919	719965.895661	45.534605
3502.267004	719935.661431	45.539610
3502.335447	719911.154255	45.544615
3502.127971	719893.684271	45.549620
3502.296114	719864.697681	45.554625
3502.266721	719830.090558	45.559629
3502.119130	719813.949403	45.564634
3502.176642	719773.030086	45.569639
3502.140703	719764.011094	45.574644
3502.360311	719734.420515	45.579649
3502.059501	719717.659774	45.584653
3502.308549	719694.064378	45.589658
3502.409326	719663.005475	45.594663
3502.157468	719648.468014	45.599668
3502.074615	719609.653747	45.604673
3502.332814	719588.188865	45.609677
3502.282296	719558.493406	45.614682
3502.574677	719539.105512	45.619687
3502.441257	719510.960813	45.624692
3502.303628	719488.866646	45.629697
3502.478428	719458.935347	45.634701
3502.188101	719440.982166	45.639706
3502.490657	719409.442762	45.644711
3502.242935	719389.945157	45.649716
3502.444161	719352.620180	45.654721
3502.594529	719324.775223	45.659725
3502.265654	719311.687991	45.664730
3502.512832	719274.603046	45.669735
3502.465835	719259.485649	45.674740
3502.209791	719214.400024	45.679745
3502.027118	719193.304320	45.684749
3502.030581	719180.410076	45.689754
3502.139019	719133.825805	45.694759
3502.173876	719134.415254	45.699764
3502.099987	719097.035283	45.704769
3502.208280	719078.420533	45.709773
3502.470957	719058.986828	45.714778
3502.558429	719034.374756	45.719783
3502.293545	719000.398100	45.724788
3502.547597	718980.320931	45.729793
3502.342227	718935.175854	45.734797
3501.858905	718919.088285	45.739802
3502.024794	718887.966176	45.744807
3501.927134	718871.914154	45.749812
3502.183801	718853.423233	45.754817
3502.148243	718808.894205	45.759821
3501.577661	718725.224222	45.764826
3501.768950	718593.916055	45.769831
3502.074030	718422.414458	45.774836
3502.032092	718175.678000	45.779841
3501.688033	717865.993244	45.784845
3501.567231	717512.511975	45.789850
3501.657070	717084.724420	45.794855
3500.841515	716613.212066	45.799860
3500.496211	716072.985595	45.804865
3500.513072	715482.853097	45.809869
3500.258510	714844.645145	45.814874
3499.639226	714135.193166	45.819879
3498.980265	713374.871544	45.824884
3498.777331	712557.579720	45.829889
3498.268527	711684.022565	45.834893
3497.544338	710754.217629	45.839898
3497.145457	709745.468295	45.844903
3496.126888	708704.477197	45.849908
3495.319491	707586.750202	45.854913
3494.744788	706411.574367	45.859917
3493.750582	705191.402759	45.864922
3493.220848	703902.423186	45.869927
3492.563664	702569.249151	45.874932
3491.631078	701154.911377	45.879937
3490.594560	699692.098332	45.884941
3489.618665	698176.633300	45.889946
3488.646889	696600.444380	45.894951
3487.351499	694972.107945	45.899956
3486.257473	693270.469610	45.904961
3485.226350	691528.396720	45.909965
3483.751282	689750.379376	45.914970
3482.955093	687882.211721	45.919975
3481.708137	685993.669852	45.924980
3480.016397	684032.958613	45.929985
3478.740458	682019.364624	45.934989
3477.127173	679961.447890	45.939994
3476.188172	677853.583517	45.944999
3474.662131	675691.014161	45.950004
3473.238063	673483.012414	45.955009
3471.625142	671207.110001	45.960013
3469.754941	668893.894381	45.965018
3468.315159	666529.759421	45.970023
3466.853886	664136.900229	45.975028
3464.901311	661673.302193	45.980033
3463.409002	659163.470732	45.985037
3460.833677	656624.807118	45.990042
3459.643865	654024.919006	45.995047
3457.770675	651401.276522	46.000052
3455.401441	648729.846533	46.005057
3453.873159	646001.827564	46.010061
3451.392671	643250.227280	46.015066
3449.538935	640442.211106	46.020071
3447.273102	637611.330797	46.025076
3445.601169	634726.780868	46.030081
3443.593376	631805.997067	46.035085
3441.108483	628848.328471	46.040090
3438.846806	625839.711868	46.045095
3436.322790	622807.847609	46.050100
3434.156717	619745.354978	46.055105
3431.983021	616645.609259	46.060109
3429.730438	613502.080293	46.065114
3427.411135	610312.981911	46.070119
3425.027413	607107.784954	46.075124
3422.465672	603852.125963	46.080129
3419.787527	600564.234167	46.085133
3416.971121	597242.337858	46.090138
3415.055101	593896.393187	46.095143
3411.934248	590522.717545	46.100148
3409.342780	587107.140697	46.105153
3407.111278	583661.027362	46.110157
3404.198655	580203.039821	46.115162
3401.689549	576703.323170	46.120167
3399.118091	573169.427563	46.125172
3396.075632	569618.817315	46.130177
3393.196292	566031.299218	46.135181
3390.526231	562423.011887	46.140186
3387.361414	558773.414837	46.145191
3384.588633	555118.012993	46.150196
3381.628462	551426.520155	46.155201
3378.541661	547718.419704	46.160205
3375.551154	543979.102117	46.165210
3372.498638	540226.689883	46.170215
3369.485387	536443.057582	46.175220
3366.281498	532643.977991	46.180225
3363.188165	528819.459573	46.185229
3360.422962	524990.314513	46.190234
3357.417428	521119.628087	46.195239
3354.075974	517238.164517	46.200244
3350.784919	513327.221815	46.205249
3347.459885	509412.280845	46.210253
3344.219715	505466.490266	46.215258
3341.108874	501512.439620	46.220263
3337.645496	497537.674948	46.225268
3334.472872	493543.457686	46.230273
3331.309340	489528.875684	46.235277
3327.528940	485509.218970	46.240282
3324.133831	481460.490986	46.245287
3320.769282	477420.168322	46.250292
3317.203566	473352.503764	46.255297
3313.797917	469274.154534	46.260301
3310.096845	465193.009367	46.265306
3306.862022	461092.994159	46.270311
3303.101291	456991.563789	46.275316
3299.285684	452868.022257	46.280321
3296.161642	448735.587948	46.285325
3292.692771	444612.703751	46.290330
3288.889000	440452.770756	46.295335
3285.141959	436303.974515	46.300340
3281.322215	432137.129664	46.305345
3277.774605	427967.313507	46.310349
3274.167858	423798.303328	46.315354
3270.530471	419615.109266	46.320359
3266.550716	415435.136296	46.325364
3262.380522	411233.948880	46.330369
3259.157343	407043.853746	46.335373
3255.200405	402853.288361	46.340378
3251.364820	398643.684453	46.345383
3247.943847	394436.933273	46.350388
3243.860034	390236.053256	46.355393
3240.403443	386025.754593	46.360397
3236.643151	381820.949671	46.365402
3232.986575	377595.125544	46.370407
3228.932577	373381.380037	46.375412
3224.521296	369160.148323	46.380417
3220.674832	364934.219168	46.385421
3216.761102	360724.749221	46.390426
3213.321045	356507.583006	46.395431
3209.033698	352296.056510	46.400436
3205.124206	348088.028697	46.405441
3201.516968	343871.343019	46.410445
3197.267260	339671.924480	46.415450
3193.795728	335447.238512	46.420455
3189.558105	331237.715013	46.425460
3185.205803	327029.472554	46.430465
3181.980583	322822.859551	46.435469
3177.293634	318637.057854	46.440474
3173.528251	314437.887560	46.445479
3169.728415	310256.583196	46.450484
3165.466577	306073.580097	46.455489
3161.642996	301902.904583	46.460493
3157.481516	297733.092798	46.465498
3153.233364	293564.961505	46.470503
3149.546771	289415.076034	46.475508
3145.375911	285264.630513	46.480513
3141.280521	281114.747016	46.485517
3136.875256	276981.627354	46.490522
3132.733716	272857.504033	46.495527
3128.686205	268737.201710	46.500532
3124.456485	264629.467826	46.505537
3120.370683	260529.834381	46.510541
3116.315529	256455.859168	46.515546
3112.686088	252374.843386	46.520551
3108.165183	248310.094914	46.525556
3104.050373	244252.909613	46.530561
3099.956500	240202.093689	46.535565
3095.633904	236169.979229	46.540570
3091.681061	232142.017690	46.545575
3087.752953	228134.324872	46.550580
3083.424119	224124.627062	46.555585
3079.215791	220126.069946	46.560589
3074.869727	216142.249894	46.565594
3070.818873	212169.086320	46.570599
3066.685752	208156.854863	46.575604
3062.554679	204186.752117	46.580609
3058.925204	200249.616212	46.585613
3054.246763	196329.802296	46.590618
3050.114389	192418.009975	46.595623
3045.861213	188520.203917	46.600628
3041.626312	184646.604457	46.605633
3037.653478	180768.219180	46.610637
3033.026618	176919.454284	46.615642
3029.017596	173069.127371	46.620647
3024.617070	169260.495192	46.625652
3020.602330	165454.138791	46.630657
3016.840273	161657.610387	46.635661
3012.470961	157880.270831	46.640666
3008.302393	154114.428211	46.645671
3003.873014	150344.642410	46.650676
2999.740555	146614.498027	46.655681
2995.686699	142893.812303	46.660685
2991.215365	139190.787137	46.665690
2987.055642	135491.772455	46.670695
2982.813907	131831.565865	46.675700
2978.342850	128175.193760	46.680705
2974.491166	124526.834411	46.685709
2970.283321	120915.904097	46.690714
2965.950623	117295.793306	46.695719
2961.689244	113704.602123	46.700724
2957.419345	110135.600714	46.705729
2953.125445	106568.705905	46.710733
2948.824257	103041.627712	46.715738
2944.372059	99513.038035	46.720743
2940.187167	96025.832670	46.725748
2935.663795	92546.505010	46.730753
2931.590050	89084.849132	46.735757
2926.905091	85665.904203	46.740762
2922.705997	82234.539006	46.745767
2918.029559	78836.380558	46.750772
2913.912284	75472.705070	46.755777
2909.485103	72124.693368	46.760781
2904.602358	68807.667903	46.765786
2899.893085	65514.148779	46.770791
2895.141299	62245.633590	46.775796
2890.334335	59009.952879	46.780801
2885.208946	55804.286052	46.785805
2880.221104	52645.850165	46.790810
2874.982347	49531.271775	46.795815
2868.552485	46472.900811	46.800820
2859.824035	43536.030707	46.805825
2849.468437	40725.381302	46.810829
2838.976372	38021.557350	46.815834
2828.846151	35432.863904	46.820839
2819.478452	32955.824025	46.825844
2810.337830	30624.969640	46.830849
2802.080667	28430.225826	46.835853
2793.454702	26364.521526	46.840858
2785.469249	24405.236609	46.845863
2777.702473	22575.125468	46.850868
2770.418599	20854.083072	46.855873
2763.802287	19243.855330	46.860877
2757.040299	17746.284266	46.865882
2750.540454	16328.943246	46.870887
2744.155404	15009.664485	46.875892
2737.803364	13783.210200	46.880897
2731.395803	12650.208311	46.885901
2724.629288	11619.159514	46.890906
2717.718196	10650.036573	46.895911
2711.552201	9777.518472	46.900916
2705.211511	8989.460102	46.905921
2699.671800	8264.343208	46.910925
2693.589680	7612.435912	46.915930
2688.464470	7028.962471	46.920935
2683.492325	6506.113379	46.925940
2678.783404	6011.870086	46.930945
2674.351805	5561.322216	46.935949
2669.894421	5169.318149	46.940954
2666.831519	4800.113486	46.945959
2662.795595	4455.134819	46.950964
2659.251724	4123.827160	46.955969
2655.894351	3834.008358	46.960973
2652.615337	3539.222930	46.965978
2649.619601	3256.807087	46.970983
2646.447516	2992.396091	46.975988
2643.041130	2733.855452	46.980993
2639.701749	2479.678182	46.985997
2637.171878	2242.289689	46.991002
2634.073596	1987.831959	46.996007
2631.284290	1749.876026	47.001012
2627.708566	1502.276840	47.006017
2624.728031	1253.180189	47.011021
2621.461381	1025.919904	47.016026
2618.075031	787.942239	47.021031
2614.630649	552.970737	47.026036
2610.615015	335.703933	47.031041
2605.822820	171.311526	47.036045
2592.440632	234.794757	47.041050
2584.987645	225.108576	47.046055
2580.782107	227.849366	47.051060
2578.360899	225.157514	47.056065
2577.027680	221.545284	47.061069
2574.916252	236.895688	47.066074
2572.753361	233.180815	47.071079
2570.115886	229.496120	47.076084
2566.885402	224.693087	47.081089
2563.774788	227.146026	47.086093
2560.256773	237.872621	47.091098
2557.193646	226.637280	47.096103
2553.674483	215.547469	47.101108
2550.114222	226.152566	47.106113
2547.000234	216.555076	47.111117
2543.883219	227.420329	47.116122
2540.636613	224.874790	47.121127
2537.224721	222.260824	47.126132
2533.645147	224.601340	47.131137
2530.294390	226.280102	47.136141
2527.244126	223.756435	47.141146
2523.464549	217.117230	47.146151
2520.615095	216.638815	47.151156
2516.937122	218.274106	47.156161
2514.069358	219.846321	47.161165
2510.307510	215.420928	47.166170
2507.003394	214.455933	47.171175
2503.613645	217.607189	47.176180
2500.134866	223.146360	47.181185
2496.458726	211.753739	47.186189
2493.216930	215.629883	47.191194
2490.117059	211.579319	47.196199
2486.626079	214.923717	47.201204
2483.103857	210.543059	47.206209
2480.440761	210.644281	47.211213
2476.179450	222.282373	47.216218
2472.646825	212.012829	47.221223
2468.721928	215.511942	47.226228
2465.309547	217.795504	47.231233
2462.673461	207.883376	47.236237
2459.535297	218.396748	47.241242
2455.374976	224.635532	47.246247
2451.263461	215.207900	47.251252
2447.997335	216.633964	47.256257
2445.335682	218.133714	47.261261
2441.664299	218.969533	47.266266
2438.649768	219.456964	47.271271
2435.324538	215.784047	47.276276
2431.525525	210.132662	47.281281
2428.483165	210.846503	47.286285
2424.468800	212.353863	47.291290
2421.300591	214.375535	47.296295
2417.693279	213.980049	47.301300
2413.702021	221.307706	47.306305
2410.625795	210.456500	47.311309
2407.194863	221.796934	47.316314
2403.350214	218.065724	47.321319
2400.444636	208.223775	47.326324
2397.370878	212.987896	47.331329
2393.428084	206.716357	47.336333
2389.832916	211.316919	47.341338
2386.935153	216.989360	47.346343
2383.039931	222.350478	47.351348
2379.184290	218.699446	47.356353
2375.732228	210.225505	47.361357
2372.394982	213.818311	47.366362
2369.136940	217.129860	47.371367
2365.779700	204.893380	47.376372
2362.225985	219.931144	47.381377
2358.935125	205.406800	47.386381
2354.944839	209.103871	47.391386
2351.326403	192.688641	47.396391
2348.074160	205.980298	47.401396
2344.582297	213.275288	47.406401
2341.504774	200.200926	47.411405
2337.853995	204.373594	47.416410
2333.945250	204.412352	47.421415
2330.906945	204.773923	47.426420
2326.617384	209.309783	47.431425
2324.110876	196.115120	47.436429
2320.070146	200.001504	47.441434
2316.832079	201.291394	47.446439
2313.413121	199.347347	47.451444
2309.839352	204.351541	47.456449
2306.728938	199.336472	47.461453
2302.717556	192.580624	47.466458
2299.208839	202.336287	47.471463
2296.170046	191.911569	47.476468
2292.635747	201.612651	47.481473
2289.472692	195.069601	47.486477
2285.612040	202.253035	47.491482
2282.099979	192.074005	47.496487
2278.498991	196.021814	47.501492
2274.755304	203.344409	47.506497
2271.691306	196.198129	47.511501
2267.866478	201.877853	47.516506
2264.297401	199.756156	47.521511
2261.234953	183.523130	47.526516
2257.491492	195.517906	47.531521
2254.090927	187.410715	47.536525
2250.267733	192.859884	47.541530
2247.007298	198.162466	47.546535
2244.030368	195.841190	47.551540
2239.807260	196.982563	47.556545
2236.642220	191.649375	47.561549
2232.945974	192.302967	47.566554
2229.565652	194.524163	47.571559
2226.449701	191.713559	47.576564
2222.972168	197.433063	47.581569
2219.565264	189.452255	47.586573
2215.263464	192.377960	47.591578
2212.204816	199.876393	47.596583
2208.796280	194.423781	47.601588
2205.171286	193.737534	47.606593
2201.685444	190.650966	47.611597
2197.928541	200.556601	47.616602
2194.748491	194.581014	47.621607
2191.363694	197.191141	47.626612
2187.376131	196.719291	47.631617
2184.066172	195.713450	47.636621
2180.883725	190.857185	47.641626
2176.905610	193.835053	47.646631
2173.783825	193.436936	47.651636
2170.605604	199.061072	47.656641
2167.223513	187.725583	47.661645
2163.264585	195.953270	47.666650
2159.620277	197.858748	47.671655
2156.643010	187.574152	47.676660
2152.919567	193.313585	47.681665
2149.118930	190.526106	47.686669
2145.424589	195.088150	47.691674
2142.127537	193.038848	47.696679
2138.940287	197.924471	47.701684
2135.301650	194.949617	47.706689
2131.843903	188.951654	47.711693
2128.168893	190.572136	47.716698
2124.635383	186.714600	47.721703
2121.456249	181.212535	47.726708
2117.814060	188.222660	47.731713
2114.599705	184.527726	47.736717
2110.899416	187.703086	47.741722
2107.026514	192.652025	47.746727
2103.845007	185.705247	47.751732
2100.359591	188.569054	47.756737
2097.303572	185.930786	47.761741
2093.576143	188.154927	47.766746
2090.005816	191.939340	47.771751
2086.940084	188.029844	47.776756
2082.880114	190.218528	47.781761
2079.420497	181.705238	47.786765
2075.651385	181.843890	47.791770
2072.062494	188.822551	47.796775
2068.612635	182.154555	47.801780
2064.796631	188.176730	47.806785
2061.983885	183.504594	47.811789
2058.409289	178.880130	47.816794
2054.939269	186.034930	47.821799
2051.289020	180.043369	47.826804
2047.869234	185.648857	47.831809
2044.667299	176.429590	47.836813
2040.809548	177.626633	47.841818
2037.447318	178.090625	47.846823
2034.167390	172.399250	47.851828
2030.474125	176.737017	47.856833
2027.036331	175.426593	47.861837
2023.367390	174.877396	47.866842
2019.707141	187.810145	47.871847
2016.727557	180.872513	47.876852
2012.661766	184.417341	47.881857
2009.067088	170.544989	47.886861
2005.801413	189.281832	47.891866
2002.319363	175.401142	47.896871
1999.004664	180.401433	47.901876
1995.148494	187.372980	47.906881
1992.085201	178.295040	47.911885
1988.487991	180.297453	47.916890
1985.384772	174.467602	47.921895
1981.826572	173.378778	47.926900
1977.984187	184.623799	47.931905
1974.468384	173.752010	47.936909
1971.005613	183.354640	47.941914
1966.936748	183.894148	47.946919
1963.788851	177.008232	47.951924
1960.125895	183.834026	47.956929
1956.921232	178.127907	47.961933
1953.289500	180.837390	47.966938
1949.717272	179.752880	47.971943
1946.706079	171.985186	47.976948
1942.759153	183.596787	47.981953
1939.836699	167.168047	47.986957
1935.973859	177.922137	47.991962
1932.312881	186.998668	47.996967
1929.075792	169.491744	48.001972
1925.277182	172.771294	48.006977
1921.667637	170.163398	48.011981
1918.326964	182.152042	48.016986
1914.958638	178.316525	48.021991
1911.640453	171.970871	48.026996
1908.047759	176.514318	48.032001
1904.441942	174.573416	48.037005
1901.046392	183.051799	48.042010
1897.748077	181.780197	48.047015
1893.839070	173.171187	48.052020
1889.890846	180.257077	48.057025
1886.800948	175.258655	48.062029
1883.519365	179.574704	48.067034
1879.712954	180.970798	48.072039
1876.426196	171.547812	48.077044
1872.622948	171.135768	48.082049
1869.603780	180.683339	48.087053
1866.030064	172.973299	48.092058
1862.176507	177.721292	48.097063
1859.232262	169.584435	48.102068
1855.306445	172.316519	48.107073
1852.035000	173.036985	48.112077
1848.545246	175.933257	48.117082
1845.173047	172.207956	48.122087
1841.349812	165.300491	48.127092
1837.412895	178.081119	48.132097
1834.167752	169.335861	48.137101
1830.917903	171.119191	48.142106
1827.398216	171.026601	48.147111
1824.094247	176.089365	48.152116
1820.300648	177.060887	48.157121
1817.021599	170.333898	48.162125
1813.342705	171.273650	48.167130
1809.947491	171.594260	48.172135
1806.307064	166.739335	48.177140
1802.566824	171.156463	48.182145
1799.357846	166.696777	48.187149
1795.999366	170.942307	48.192154
1792.270625	180.123267	48.197159
1788.982002	170.811958	48.202164
1785.204375	183.736615	48.207169
1782.093197	173.305898	48.212173
1778.657610	177.358949	48.217178
1774.865465	174.826327	48.222183
1771.855683	174.620531	48.227188
1767.905011	161.909944	48.232193
1764.507283	172.944888	48.237197
1760.689111	181.867529	48.242202
1757.289289	182.764771	48.247207
1753.918217	174.504320	48.252212
1750.175970	176.706895	48.257217
1747.011865	176.038593	48.262221
1743.298746	171.109688	48.267226
1739.592898	180.022863	48.272231
1736.363634	173.831969	48.277236
1732.770722	174.488408	48.282241
1729.556444	172.758045	48.287245
1725.906896	177.131437	48.292250
1722.125092	178.493594	48.297255
1719.200440	183.307077	48.302260
1715.029964	182.542012	48.307265
1711.693826	174.581106	48.312269
1708.582623	167.944478	48.317274
1704.699951	168.086991	48.322279
1701.294842	165.892069	48.327284
1697.685278	174.415999	48.332289
1694.409902	165.805499	48.337293
1690.722906	172.680442	48.342298
1686.938836	182.714041	48.347303
1684.014735	176.417707	48.352308
1680.217158	170.514540	48.357313
1676.691811	164.466350	48.362317
1673.547816	176.608133	48.367322
1670.145867	180.750226	48.372327
1666.815390	174.067171	48.377332
1662.612524	177.810170	48.382337
1659.288356	176.855396	48.387341
1656.018120	176.443471	48.392346
1652.116820	171.754520	48.397351
1648.847835	170.247957	48.402356
1645.235001	170.121954	48.407361
1641.925610	167.415548	48.412365
1638.305593	169.272801	48.417370
1634.627014	169.830197	48.422375
1631.513154	168.090415	48.427380
1627.541304	170.519086	48.432385
1624.106879	173.372038	48.437389
1620.605504	167.196003	48.442394
1617.593621	170.768097	48.447399
1614.362939	168.596910	48.452404
1610.557860	172.679555	48.457409
1606.772176	160.093420	48.462413
1603.116283	172.751204	48.467418
1599.978461	170.008191	48.472423
1596.092860	170.281520	48.477428
1592.072341	169.478764	48.482433
1589.211274	164.741711	48.487437
1585.657470	171.278387	48.492442
1582.708894	161.940659	48.497447
1579.471041	159.729243	48.502452
1575.215222	162.985352	48.507457
1571.903132	148.089703	48.512461
1568.249425	163.413567	48.517466
1564.343315	168.470227	48.522471
1561.379673	163.548661	48.527476
1557.864724	167.567023	48.532481
1554.523947	161.199334	48.537485
1550.802255	166.153106	48.542490
1546.965715	164.079720	48.547495
1543.822530	168.156243	48.552500
1540.077773	167.373084	48.557505
1536.612369	162.461241	48.562509
1532.936002	167.707293	48.567514
1529.400335	168.257534	48.572519
1526.336433	164.792139	48.577524
1522.752782	164.353957	48.582529
1519.272713	159.201630	48.587533
1516.013712	169.361299	48.592538
1512.094364	166.654359	48.597543
1508.921720	158.072026	48.602548
1505.074879	160.183145	48.607553
1501.594925	161.698653	48.612557
1497.937754	153.762567	48.617562
1494.633053	162.771426	48.622567
1491.535514	164.116588	48.627572
1487.422721	174.487630	48.632577
1484.059108	163.491466	48.637581
1480.781110	167.385670	48.642586
1476.927801	171.705498	48.647591
1473.932713	164.202882	48.652596
1470.007046	166.494795	48.657601
1467.012227	158.677389	48.662605
1463.242325	165.300776	48.667610
1459.237244	170.832291	48.672615
1456.154760	163.820309	48.677620
1452.654904	176.983836	48.682625
1449.404394	164.417341	48.687629
1445.622119	161.833441	48.692634
1441.833082	177.749477	48.697639
1438.925781	166.857903	48.702644
1435.378638	172.847945	48.707649
1431.572467	164.878125	48.712653
1428.052077	166.468649	48.717658
1424.260369	164.602858	48.722663
1421.112355	157.770853	48.727668
1417.436987	171.587387	48.732673
1414.271714	156.299370	48.737677
1410.822871	159.108282	48.742682
1407.349456	160.274478	48.747687
1403.939932	161.765196	48.752692
1399.984264	164.719258	48.757697
1396.662114	158.516748	48.762701
1392.876926	157.517402	48.767706
1389.240578	167.755105	48.772711
1386.499049	159.553907	48.777716
1382.526120	157.520965	48.782721
1379.344814	156.911804	48.787725
1375.559603	160.283299	48.792730
1371.837102	160.861976	48.797735
1368.754515	157.242899	48.802740
1365.409841	160.041335	48.807745
1361.551722	158.884952	48.812749
1358.265238	151.886244	48.817754
1354.630182	158.166550	48.822759
1351.163601	158.110535	48.827764
1347.213338	161.637999	48.832769
1343.976635	154.310005	48.837773
1340.611483	163.319085	48.842778
1336.979289	161.135337	48.847783
1334.064793	162.998351	48.852788
1329.881272	169.751384	48.857793
1326.544194	156.987369	48.862797
1322.999553	164.957747	48.867802
1319.308435	163.982182	48.872807
1316.203680	165.059484	48.877812
1312.427881	162.305508	48.882817
1308.956194	158.586806	48.887821
1305.778341	156.412637	48.892826
1301.900838	163.715207	48.897831
1298.500937	149.396131	48.902836
1294.732776	156.878164	48.907841
1291.613462	154.265120	48.912845
1288.108847	161.057315	48.917850
1284.414289	165.338421	48.922855
1280.967637	157.341280	48.927860
1277.158754	161.263785	48.932865
1274.092418	157.458565	48.937869
1270.569639	160.910688	48.942874
1267.228521	166.164071	48.947879
1263.812215	144.553376	48.952884
1259.966227	152.710165	48.957889
1256.749204	154.483722	48.962893
1253.066356	161.554642	48.967898
1249.341169	171.344768	48.972903
1245.863391	149.829494	48.977908
1242.289369	162.579154	48.982913
1239.014474	154.213249	48.987917
1235.581695	159.507854	48.992922
1231.906101	156.247790	48.997927
1228.758072	164.858935	49.002932
1224.825018	148.091695	49.007937
1221.498977	153.595994	49.012941
1217.830053	169.869620	49.017946
1214.354273	153.580712	49.022951
1211.079723	155.604561	49.027956
1207.599162	160.835847	49.032961
1204.473338	159.212994	49.037965
1200.814129	160.730931	49.042970
1196.761927	161.034311	49.047975
1193.281294	151.677886	49.052980
1189.476922	149.667177	49.057985
1186.215311	155.941709	49.062989
1183.071902	154.348814	49.067994
1179.473651	154.484410	49.072999
1176.152101	149.880407	49.078004
1172.550470	152.213912	49.083009
1168.687692	157.426325	49.088013
1165.525651	151.803157	49.093018
1161.789289	160.866818	49.098023
1158.398492	151.039327	49.103028
1155.115302	153.721775	49.108033
1151.504076	157.406863	49.113037
1147.794426	152.493689	49.118042
1144.020356	158.789634	49.123047
1140.855198	160.002547	49.128052
1137.366509	146.100473	49.133057
1133.976615	147.189916	49.138061
1130.379528	152.774217	49.143066
1126.936546	152.980087	49.148071
1123.586781	150.006451	49.153076
1119.825016	163.599076	49.158081
1116.258776	156.482434	49.163085
1112.927172	158.131769	49.168090
1109.171757	162.445371	49.173095
1105.804197	155.268260	49.178100
1102.305342	161.110245	49.183105
1098.955127	157.995407	49.188109
1095.206407	158.561279	49.193114
1091.672359	155.264905	49.198119
1088.204469	157.774684	49.203124
1084.945152	158.400736	49.208129
1081.191423	154.707344	49.213133
1077.569469	151.203120	49.218138
1074.230409	151.826578	49.223143
1071.295427	151.767730	49.228148
1067.483022	155.759459	49.233153
1063.924871	159.041164	49.238157
1060.531053	150.841495	49.243162
1056.843554	160.976189	49.248167
1053.726293	146.620664	49.253172
1049.558710	163.369548	49.258177
1046.114569	145.369010	49.263181
1042.697715	153.303844	49.268186
1039.285933	152.931161	49.273191
1035.847815	151.098205	49.278196
1032.016826	153.629391	49.283201
1028.813398	149.162065	49.288205
1025.441201	151.972198	49.293210
1021.509014	157.118062	49.298215
1018.241877	152.651609	49.303220
1014.884744	156.724581	49.308225
1011.454786	150.799510	49.313229
1008.178325	145.636433	49.318234
1004.174648	144.796093	49.323239
1000.694674	147.081392	49.328244
997.036161	146.677714	49.333249
993.963260	147.127172	49.338253
990.053897	141.888804	49.343258
986.137126	141.257889	49.348263
983.388125	142.863065	49.353268
979.698324	144.300000	49.358273
976.446747	141.849957	49.363277
972.798164	136.479680	49.368282
969.300092	139.812692	49.373287
965.657422	141.771691	49.378292
962.128705	138.096450	49.383297
958.384914	131.729993	49.388301
955.351271	144.397957	49.393306
951.787564	138.471380	49.398311
948.605362	131.117728	49.403316
944.710582	138.558204	49.408321
941.129316	133.059999	49.413325
937.739576	126.837672	49.418330
934.103458	142.023638	49.423335
930.747218	132.549398	49.428340
927.195436	143.199468	49.433345
923.964378	133.291110	49.438349
920.648529	135.988791	49.443354
916.765883	143.001828	49.448359
913.221302	137.064426	49.453364
909.225530	140.682067	49.458369
905.863398	141.818790	49.463373
902.795597	144.979654	49.468378
899.388152	138.359098	49.473383
895.763247	140.161095	49.478388
892.041413	135.906112	49.483393
888.590981	130.664755	49.488397
885.064468	134.984477	49.493402
881.781671	137.846626	49.498407
878.215130	133.815798	49.503412
874.651487	135.300032	49.508417
871.087886	140.522397	49.513421
867.964405	139.052730	49.518426
863.797419	138.087383	49.523431
860.530356	139.869293	49.528436
856.893064	147.364146	49.533441
853.888645	142.156590	49.538445
850.285200	137.587241	49.543450
846.249463	141.636609	49.548455
843.433576	139.531770	49.553460
839.923673	146.062889	49.558465
835.751607	145.777245	49.563469
832.436034	140.301685	49.568474
829.003537	155.091151	49.573479
825.845310	140.305504	49.578484
822.142282	152.179288	49.583489
818.822582	137.296432	49.588493
815.085496	145.141121	49.593498
811.245224	142.844821	49.598503
808.061810	135.890690	49.603508
804.528084	143.797456	49.608513
801.404986	141.939021	49.613517
797.622013	142.032464	49.618522
794.033803	141.491819	49.623527
790.578748	135.585299	49.628532
786.670764	141.372242	49.633537
783.524931	141.063115	49.638541
780.179705	132.910910	49.643546
776.574172	137.655230	49.648551
773.498136	131.521451	49.653556
769.932638	141.766990	49.658561
766.224116	137.436704	49.663565
762.596226	131.561168	49.668570
758.773559	139.317046	49.673575
755.436354	130.640400	49.678580
751.657896	144.493352	49.683585
748.341001	139.906683	49.688589
745.119708	130.150981	49.693594
741.758237	140.508224	49.698599
738.053577	127.543696	49.703604
734.372279	139.784732	49.708609
730.937910	129.672382	49.713613
727.632627	136.325032	49.718618
723.892842	143.186124	49.723623
720.540631	140.450803	49.728628
716.523492	134.805463	49.733633
713.329643	142.270078	49.738637
709.829239	138.517744	49.743642
706.257375	142.568243	49.748647
703.162073	139.913374	49.753652
699.697820	145.217114	49.758657
696.086080	139.264566	49.763661
692.947986	133.712203	49.768666
688.574501	144.626846	49.773671
685.426640	140.285177	49.778676
681.710556	144.200700	49.783681
678.462086	134.507169	49.788685
675.234939	142.475590	49.793690
671.297461	135.914304	49.798695
668.077109	135.392429	49.803700
664.601711	133.779258	49.808705
661.184547	133.363162	49.813709
657.643819	128.472014	49.818714
654.036610	136.059716	49.823719
650.477452	125.478301	49.828724
646.664479	130.761232	49.833729
643.565289	130.952825	49.838733
639.850179	130.737594	49.843738
636.318728	136.981749	49.848743
633.049642	131.109518	49.853748
629.306353	134.807383	49.858753
625.728578	132.518536	49.863757
622.469261	129.783514	49.868762
618.901096	135.112594	49.873767
615.890857	127.295238	49.878772
611.774490	130.567427	49.883777
608.096933	132.357646	49.888781
604.816896	131.540022	49.893786
601.339750	135.775026	49.898791
598.098690	124.988487	49.903796
594.233026	137.304525	49.908801
590.631693	127.401873	49.913805
587.664836	127.854785	49.918810
583.819018	135.939640	49.923815
580.490421	123.636477	49.928820
576.922460	137.816631	49.933825
573.609783	137.016271	49.938829
569.984960	138.991579	49.943834
566.287808	137.192389	49.948839
562.800316	130.062231	49.953844
559.221828	139.586636	49.958849
556.192305	133.391059	49.963853
552.407406	134.050200	49.968858
548.533212	143.041605	49.973863
545.488672	123.983649	49.978868
541.457399	144.283885	49.983873
537.918800	131.056455	49.988877
534.695470	126.295428	49.993882
530.886240	133.443835	49.998887
528.326277	127.387451	50.003892
524.332636	135.180092	50.008897
521.140020	132.016945	50.013901
517.465329	130.133372	50.018906
513.506754	132.923695	50.023911
510.468418	121.266197	50.028916
507.170737	126.269003	50.033921
503.210938	131.430912	50.038925
500.054944	131.371130	50.043930
495.992567	139.997664	50.048935
492.801014	129.288466	50.053940
488.975826	141.986639	50.058945
485.419131	135.537557	50.063949
482.393890	126.256391	50.068954
478.797913	136.439885	50.073959
475.140375	127.392815	50.078964
471.960231	135.225911	50.083969
468.555389	140.953730	50.088973
464.974189	132.387765	50.093978
461.062641	133.342636	50.098983
458.185956	127.719570	50.103988
454.096450	131.367918	50.108993
450.465049	129.644382	50.113997
447.119214	127.815967	50.119002
443.676076	131.448918	50.124007
440.540136	131.000662	50.129012
436.454989	123.554928	50.134017
433.019877	127.841118	50.139021
429.759832	134.913517	50.144026
426.273986	136.035161	50.149031
422.835679	127.854664	50.154036
419.130863	132.027634	50.159041
415.909375	128.000087	50.164045
412.380589	131.833915	50.169050
408.893692	137.484583	50.174055
405.086116	132.075216	50.179060
401.325299	143.696800	50.184065
397.962760	138.680675	50.189069
394.824484	133.266512	50.194074
391.213093	139.785352	50.199079
387.946038	119.768819	50.204084
384.155425	129.549665	50.209089
380.615593	131.733654	50.214093
377.175805	130.861540	50.219098
373.668081	127.042230	50.224103
370.286515	127.021259	50.229108
366.414165	144.526316	50.234113
363.023897	129.249256	50.239117
360.082178	126.193695	50.244122
355.926446	130.779976	50.249127
352.657930	135.448320	50.254132
349.247359	123.493219	50.259137
345.655893	126.564118	50.264141
342.177599	131.312183	50.269146
338.225239	136.224166	50.274151
335.339257	128.434808	50.279156
331.678040	132.149130	50.284161
327.631775	131.495250	50.289165
324.821966	123.321517	50.294170
320.967810	129.213599	50.299175
317.716337	128.593340	50.304180
314.089053	134.598839	50.309185
310.881000	136.725992	50.314189
307.139161	133.273263	50.319194
303.266556	138.754213	50.324199
300.275012	133.848047	50.329204
296.571047	134.813302	50.334209
292.978378	129.375769	50.339213
289.512470	127.536375	50.344218
285.861073	132.575592	50.349223
283.017039	126.572708	50.354228
279.300602	135.959322	50.359233
275.504876	133.915434	50.364237
271.967445	135.856983	50.369242
268.365607	136.134221	50.374247
265.193832	128.911808	50.379252
261.571370	126.254550	50.384257
257.955427	137.035486	50.389261
254.997987	125.814926	50.394266
250.785104	140.219279	50.399271
247.742877	136.705451	50.404276
243.814934	131.438510	50.409281
240.436723	128.136005	50.414285
237.369741	128.175148	50.419290
233.698849	138.041280	50.424295
230.252397	121.181363	50.429300
226.256872	131.421512	50.434305
222.705251	137.371933	50.439309
219.183450	138.240201	50.444314
215.806189	132.796873	50.449319
212.608086	129.358607	50.454324
209.332222	132.025916	50.459329
205.666942	132.861905	50.464333
202.379736	124.448206	50.469338
198.583916	131.214397	50.474343
194.879816	126.285186	50.479348
190.778574	131.629637	50.484353
187.726226	134.996411	50.489357
184.952779	129.272782	50.494362
181.156038	142.659122	50.499367
177.923695	126.677858	50.504372
174.266701	134.052359	50.509377
170.396862	128.546372	50.514381
166.795399	133.900256	50.519386
163.145690	133.316053	50.524391
159.738402	127.082293	50.529396
156.255499	133.664301	50.534401
152.946034	135.479601	50.539405
149.600764	130.563048	50.544410
145.997797	131.506185	50.549415
142.651247	127.458122	50.554420
138.851792	134.231872	50.559425
135.431917	125.583069	50.564429
131.830344	118.154085	50.569434
128.245102	127.504486	50.574439
125.200386	124.362351	50.579444
121.557832	131.396665	50.584449
118.195412	122.067628	50.589453
114.624233	133.404842	50.594458
110.626826	128.538283	50.599463
107.461572	129.955199	50.604468
103.635649	128.628451	50.609473
100.082531	132.883125	50.614477
96.867173	129.313422	50.619482
93.039499	129.083954	50.624487
90.051045	128.122938	50.629492
86.724656	119.173358	50.634497
83.230074	130.211578	50.639501
79.758558	129.106186	50.644506
75.526066	136.459433	50.649511
72.502163	124.151271	50.654516
68.564514	128.691643	50.659521
65.326402	130.777382	50.664525
61.888273	130.459167	50.669530
58.316686	133.979101	50.674535
55.062251	126.895857	50.679540
51.436306	127.339873	50.684545
47.579910	127.439620	50.689549
44.227161	132.209551	50.694554
40.794805	129.225401	50.699559
37.861955	117.635688	50.704564
34.227208	119.512045	50.709569
30.094098	120.530042	50.714573
26.646728	128.266191	50.719578
22.901395	127.745897	50.724583
19.918827	126.771327	50.729588
16.642775	137.583182	50.734593
12.727753	130.894707	50.739597
9.481423	126.919355	50.744602
5.437209	134.746070	50.749607
2.409002	123.512376	50.754612