Tue Jun 21 11:27:57 2022

Number of Points = 9928

Depth (nm)	Load (N)	Time (s)
0.132075	114.645601	0.000000
0.720875	118.471547	0.005005
0.551776	114.802945	0.010010
0.616794	104.948628	0.015014
0.533220	97.246180	0.020019
0.402813	100.764383	0.025024
0.320532	76.727243	0.030029
0.246206	57.569069	0.035034
0.026717	50.063987	0.040038
-0.229801	33.493449	0.045043
-0.999533	23.018469	0.050048
-1.499287	10.802913	0.055053
-1.517801	6.754400	0.060058
-2.289319	8.896580	0.065062
-2.228686	2.809541	0.070067
-2.588757	-1.571946	0.075072
-2.899229	0.360491	0.080077
-2.781498	-11.416210	0.085082
-3.996855	-8.281560	0.090086
-4.098970	-16.637801	0.095091
-4.243911	-2.913162	0.100096
-4.378945	-7.714538	0.105101
-3.884178	-21.486339	0.110106
-4.820169	-3.967436	0.115110
-5.018326	-12.795975	0.120115
-5.345320	-8.506431	0.125120
-6.010243	-10.992968	0.130125
-5.993419	-12.040378	0.135130
-6.329132	-8.592197	0.140134
-6.135083	-1.195108	0.145139
-6.331907	-5.013602	0.150144
-6.781421	-3.559365	0.155149
-6.959493	-9.274169	0.160154
-8.022284	1.694376	0.165158
-7.535441	-11.588513	0.170163
-7.503876	-6.538822	0.175168
-7.793788	1.310379	0.180173
-7.884462	-13.196043	0.185178
-8.452518	-11.018885	0.190182
-8.604994	-6.316610	0.195187
-8.778123	-7.378149	0.200192
-9.521256	-7.943531	0.205197
-10.123480	-12.446530	0.210202
-10.505317	-4.905932	0.215206
-9.885804	-16.367504	0.220211
-10.218555	-14.200895	0.225216
-10.476166	-6.090253	0.230221
-10.580620	-16.327472	0.235226
-10.929028	-6.727921	0.240230
-11.082967	-10.987447	0.245235
-11.531870	-15.551551	0.250240
-11.723861	-2.404804	0.255245
-11.461090	-8.739613	0.260250
-12.022543	-8.881413	0.265254
-12.324319	-6.363155	0.270259
-13.087630	-12.109115	0.275264
-13.388013	4.272892	0.280269
-12.877742	-6.516440	0.285274
-13.594356	1.640022	0.290278
-14.066479	-8.938876	0.295283
-14.536284	-9.931357	0.300288
-14.735580	-2.961281	0.305293
-14.728912	-10.981523	0.310298
-15.025443	-11.291708	0.315302
-14.836569	-10.125716	0.320307
-15.174328	-1.954835	0.325312
-15.082849	-3.993771	0.330317
-15.152909	-9.479203	0.335322
-15.822887	-7.442440	0.340326
-16.367736	-11.638023	0.345331
-16.365434	-10.486720	0.350336
-17.511024	1.126210	0.355341
-17.319096	-19.907988	0.360346
-17.686536	3.215333	0.365350
-17.683025	-9.284621	0.370355
-18.005335	-2.472366	0.375360
-18.115535	-10.703739	0.380365
-17.925498	-6.512836	0.385370
-18.172059	-9.697745	0.390374
-18.683802	-12.613190	0.395379
-19.369947	-1.392666	0.400384
-19.621041	0.696685	0.405389
-19.663511	-8.255907	0.410394
-19.897982	3.784728	0.415398
-19.483311	-1.136685	0.420403
-20.211797	-7.531518	0.425408
-21.156862	-3.278940	0.430413
-21.250168	0.268419	0.435418
-21.431662	-7.903987	0.440422
-21.281045	-7.238212	0.445427
-21.178089	-5.589329	0.450432
-21.358147	-10.189072	0.455437
-21.862924	-5.117264	0.460442
-22.510623	-6.451863	0.465446
-22.707203	-12.526691	0.470451
-22.884837	-4.823759	0.475456
-23.102943	-5.114766	0.480461
-22.961834	-11.764498	0.485466
-23.290868	-7.207230	0.490470
-23.833668	-11.913255	0.495475
-24.218267	-7.170569	0.500480
-24.640476	-0.698942	0.505485
-24.233528	-3.837953	0.510490
-24.418011	-3.644551	0.515494
-25.033339	2.206282	0.520499
-25.828705	-4.392765	0.525504
-25.959178	-8.729388	0.530509
-26.327895	-7.919400	0.535514
-26.476945	-5.190621	0.540518
-26.237523	-8.763844	0.545523
-26.262529	-9.358159	0.550528
-26.623742	-9.696310	0.555533
-27.247051	-10.585817	0.560538
-27.559134	-6.144625	0.565542
-27.700675	-1.695167	0.570547
-27.543062	-14.193798	0.575552
-27.822072	-0.452089	0.580557
-28.163747	-7.389111	0.585562
-29.130788	-2.352443	0.590566
-29.487236	-11.497335	0.595571
-29.703244	-9.204821	0.600576
-29.600557	-1.406229	0.605581
-29.790444	-1.959230	0.610586
-29.765084	-2.207279	0.615590
-29.645631	-11.189050	0.620595
-29.259280	-8.373109	0.625600
-30.299273	-4.585116	0.630605
-30.748721	0.059384	0.635610
-30.930762	-2.797193	0.640614
-31.428617	3.009324	0.645619
-31.857269	-5.644097	0.650624
-32.423483	0.892226	0.655629
-32.412305	-8.213301	0.660634
-32.615662	-0.807830	0.665638
-32.705492	-6.031482	0.670643
-32.743059	-10.270812	0.675648
-32.730336	-14.050396	0.680653
-32.928687	-5.605223	0.685658
-33.640339	-8.033303	0.690662
-33.754271	-7.080212	0.695667
-34.288585	-5.110706	0.700672
-34.267814	-0.962615	0.705677
-34.205553	-15.919607	0.710682
-35.218773	-4.422528	0.715686
-35.853726	-14.451917	0.720691
-35.665255	-3.766552	0.725696
-36.101041	-1.275632	0.730701
-36.465940	-5.259083	0.735706
-36.044348	-8.270872	0.740710
-35.693254	-11.144890	0.745715
-36.032054	-6.444321	0.750720
-36.676393	-5.121210	0.755725
-36.810131	-8.970866	0.760730
-37.335762	0.618373	0.765734
-36.975596	-8.658806	0.770739
-37.776833	-11.705683	0.775744
-38.701478	-5.985767	0.780749
-38.756239	-10.680455	0.785754
-38.879356	-6.345739	0.790758
-38.696572	-5.894859	0.795763
-38.766336	-9.576523	0.800768
-39.067751	-6.894144	0.805773
-39.510560	-6.205480	0.810778
-40.240951	5.749152	0.815782
-40.414448	-4.607666	0.820787
-40.486988	-1.527083	0.825792
-40.401355	-4.630250	0.830797
-40.531324	-7.478675	0.835802
-41.388490	-5.924961	0.840806
-41.684413	-6.767055	0.845811
-42.244370	-14.770419	0.850816
-42.517444	-2.640914	0.855821
-42.084194	-16.952100	0.860826
-42.596224	-9.741195	0.865830
-42.457298	-9.914318	0.870835
-42.071645	-4.807432	0.875840
-42.782360	-8.915752	0.880845
-43.224630	-3.918230	0.885850
-43.415153	-5.079697	0.890854
-43.714435	-7.533637	0.895859
-44.016647	-6.824251	0.900864
-44.855516	-0.070307	0.905869
-45.062425	-1.633987	0.910874
-45.700036	-1.190512	0.915878
-45.413671	-3.431230	0.920883
-45.715891	-7.176223	0.925888
-45.747097	-7.635325	0.930893
-45.649119	-11.562622	0.935898
-45.618316	-7.924128	0.940902
-45.850568	-12.926662	0.945907
-46.258388	-9.971907	0.950912
-46.792501	-11.758257	0.955917
-46.970923	-14.003305	0.960922
-47.544849	-5.286173	0.965926
-47.891627	-16.887079	0.970931
-48.340871	-13.438448	0.975936
-48.747882	-12.339538	0.980941
-48.952160	-18.838928	0.985946
-48.683966	-14.954604	0.990950
-48.694086	-13.826700	0.995955
-48.889978	-8.759868	1.000960
-48.990001	-16.411185	1.005965
-49.172123	-14.641292	1.010970
-49.860906	-2.431894	1.015974
-50.309052	-13.095658	1.020979
-50.198944	-7.618926	1.025984
-50.523458	-18.133455	1.030989
-50.748276	-14.587211	1.035994
-51.544630	-13.754751	1.040998
-51.842234	-12.022171	1.046003
-51.757682	-19.244662	1.051008
-52.235266	-13.082560	1.056013
-51.864206	-20.389794	1.061018
-52.071733	-8.227932	1.066022
-52.676135	-12.072656	1.071027
-53.254917	-5.551421	1.076032
-53.453909	-6.957559	1.081037
-53.393732	-16.530780	1.086042
-53.832196	-8.635080	1.091046
-53.796581	-9.736513	1.096051
-53.635462	-11.933204	1.101056
-54.077636	-4.483450	1.106061
-54.840949	-12.811294	1.111066
-55.462162	-1.070303	1.116070
-55.479637	-7.959383	1.121075
-55.250409	-6.368905	1.126080
-55.386636	-6.104166	1.131085
-55.529328	-16.803316	1.136090
-56.344477	0.085036	1.141094
-56.911917	-6.725597	1.146099
-56.614247	-9.836843	1.151104
-56.971986	-7.036208	1.156109
-56.762389	-9.555672	1.161114
-56.936745	1.856761	1.166118
-57.808832	-5.153442	1.171123
-58.122425	-12.071230	1.176128
-58.723540	-4.895889	1.181133
-58.327517	-15.877243	1.186138
-58.526749	-3.817589	1.191142
-58.784383	-7.697638	1.196147
-59.130955	-8.397355	1.201152
-59.865210	-1.318561	1.206157
-59.831291	-11.029319	1.211162
-60.026917	-3.792665	1.216166
-60.258380	-8.042704	1.221171
-59.886698	-0.031735	1.226176
-60.448527	-9.258840	1.231181
-61.133434	-17.542043	1.236186
-61.415889	-3.290455	1.241190
-61.411028	-8.254113	1.246195
-61.729906	-10.667510	1.251200
-62.176711	-7.665054	1.256205
-61.849281	-6.700596	1.261210
-62.103301	-3.276202	1.266214
-62.928821	-6.392855	1.271219
-62.895622	-6.711071	1.276224
-63.117946	-12.028217	1.281229
-63.251922	-15.484153	1.286234
-63.271184	-10.722443	1.291238
-64.313589	-8.392527	1.296243
-64.865030	-12.260030	1.301248
-65.049030	-6.023014	1.306253
-64.755912	-15.352035	1.311258
-64.870025	-3.553931	1.316262
-64.819310	-11.251918	1.321267
-64.927219	-6.938271	1.326272
-65.818719	-7.783359	1.331277
-66.101890	-9.359271	1.336282
-66.655654	-9.378807	1.341286
-66.635384	-11.821925	1.346291
-66.293651	-11.466041	1.351296
-66.655597	-11.839981	1.356301
-66.952605	-12.247565	1.361306
-67.749860	-11.531181	1.366310
-68.020354	-8.360394	1.371315
-68.116748	-9.035830	1.376320
-68.282821	-10.476820	1.381325
-67.870834	-13.107944	1.386330
-68.171891	-10.250787	1.391334
-68.865670	-14.623567	1.396339
-69.548108	-8.713669	1.401344
-69.593453	-11.692532	1.406349
-69.408895	-13.021488	1.411354
-69.816896	-15.135176	1.416358
-70.047612	-22.731495	1.421363
-70.775584	-15.520547	1.426368
-71.535215	-12.388536	1.431373
-71.257095	-10.505028	1.436378
-71.560480	-12.734906	1.441382
-71.418400	-18.680712	1.446387
-71.120954	-5.205366	1.451392
-71.823306	-5.511684	1.456397
-71.432316	-15.937306	1.461402
-72.730747	-6.570354	1.466406
-72.714821	-8.181393	1.471411
-72.943006	-11.623701	1.476416
-73.111666	-9.775130	1.481421
-73.083771	-16.109716	1.486426
-73.728140	-3.032308	1.491430
-74.823617	-12.156034	1.496435
-74.831281	-14.109287	1.501440
-75.086991	-1.707577	1.506445
-74.840895	-15.814708	1.511450
-74.638550	-7.379657	1.516454
-74.672629	-11.141820	1.521459
-74.528173	-11.431102	1.526464
-75.419160	-13.934059	1.531469
-75.727368	-7.884660	1.536474
-76.280678	-9.182390	1.541478
-76.738579	-8.788602	1.546483
-77.246967	-12.365459	1.551488
-77.816652	-6.407731	1.556493
-77.114892	-9.380871	1.561498
-77.572824	-11.171743	1.566502
-77.136487	-12.092479	1.571507
-77.554118	-21.619718	1.576512
-78.185003	-11.063492	1.581517
-78.754260	-10.538981	1.586522
-78.968836	-10.000985	1.591526
-79.410094	-8.310126	1.596531
-79.122283	-14.742615	1.601536
-79.419643	-8.516427	1.606541
-79.032514	-18.229236	1.611546
-80.026005	-9.395853	1.616550
-80.622063	-13.596955	1.621555
-80.531391	-10.315879	1.626560
-81.113134	-10.977240	1.631565
-81.270354	-12.720429	1.636570
-81.162116	-2.845843	1.641574
-81.015224	-7.154001	1.646579
-81.336947	-15.737105	1.651584
-82.252281	-18.974642	1.656589
-82.512978	-12.410972	1.661594
-82.763178	-8.979514	1.666598
-82.540017	-4.638013	1.671603
-82.555743	-9.381786	1.676608
-83.027280	0.842194	1.681613
-83.368168	-12.864035	1.686618
-84.158238	-11.421077	1.691622
-84.216200	-10.923028	1.696627
-84.366152	-15.052377	1.701632
-84.447490	-14.580253	1.706637
-84.327263	-11.059973	1.711642
-84.720347	-7.939725	1.716646
-85.334054	-11.558142	1.721651
-85.379222	-9.689766	1.726656
-85.878843	-9.586054	1.731661
-85.699914	-16.781551	1.736666
-86.589391	-10.306738	1.741670
-87.283578	-6.922518	1.746675
-86.568671	-17.102036	1.751680
-87.113886	-11.132969	1.756685
-86.904866	-21.136747	1.761690
-87.702665	-13.387159	1.766694
-87.514287	-14.786012	1.771699
-87.644303	-11.758467	1.776704
-88.600339	-8.831712	1.781709
-88.089048	-15.120456	1.786714
-88.718910	-10.845674	1.791718
-88.550920	-21.266526	1.796723
-89.282232	-17.815185	1.801728
-89.711062	-17.032533	1.806733
-90.111939	-19.967905	1.811738
-90.716790	-13.665141	1.816742
-90.445240	-10.176237	1.821747
-90.262875	-16.517855	1.826752
-90.683975	-10.202700	1.831757
-90.357793	-11.902613	1.836762
-91.279509	-10.503761	1.841766
-91.993839	-14.245222	1.846771
-91.941408	-3.799986	1.851776
-92.026759	-3.945637	1.856781
-91.578897	-12.487869	1.861786
-92.215231	-7.965744	1.866790
-93.067296	-15.337801	1.871795
-93.435496	-11.576596	1.876800
-93.610107	-5.470782	1.881805
-93.368218	-9.412637	1.886810
-93.630293	-11.591338	1.891814
-93.566184	-16.604665	1.896819
-93.806213	-12.913625	1.901824
-94.982433	-5.504116	1.906829
-95.061819	-19.155372	1.911834
-95.365949	-5.183963	1.916838
-95.070340	-10.063557	1.921843
-95.232365	-13.126102	1.926848
-95.553373	-1.678928	1.931853
-96.109141	-11.285313	1.936858
-96.568772	-2.442067	1.941862
-96.798333	-7.261919	1.946867
-96.980470	-8.904288	1.951872
-97.093462	-0.690712	1.956877
-96.965706	-12.104986	1.961882
-96.994764	-10.055168	1.966886
-98.070980	-0.560631	1.971891
-98.240958	-16.473705	1.976896
-98.742124	-5.351501	1.981901
-98.358042	-14.343940	1.986906
-98.493978	-14.787077	1.991910
-98.762215	1.004504	1.996915
-99.486627	-3.658942	2.006912
-99.099721	-11.879015	2.016909
-98.884438	-0.467487	2.026906
-97.839577	-7.524873	2.036902
-97.755258	-6.435813	2.046899
-96.879352	1.783789	2.056896
-96.143899	-2.884531	2.066893
-96.271718	-6.457127	2.076890
-95.635146	-4.842667	2.086886
-94.978394	-4.709484	2.096883
-94.764957	-9.354380	2.106880
-93.602950	-11.958831	2.116877
-93.291204	-8.903531	2.126874
-93.151311	-16.246910	2.136870
-92.748810	-5.554775	2.146867
-91.914679	-8.808724	2.156864
-91.420119	-10.994603	2.166861
-91.118737	-2.780029	2.176858
-90.008875	-1.469000	2.186854
-89.792874	-2.956915	2.196851
-89.851143	-11.529848	2.206848
-89.302072	-6.781230	2.216845
-89.019829	-11.123163	2.226842
-87.767041	-8.946869	2.236838
-87.267091	-3.294661	2.246835
-87.086280	-9.324755	2.256832
-86.399374	-12.307734	2.266829
-85.738683	-14.569534	2.276826
-85.655363	-10.360050	2.286822
-85.101249	-9.394830	2.296819
-84.304446	-9.427693	2.306816
-84.004992	-8.822778	2.316813
-83.756459	-11.311710	2.326810
-82.769990	-7.764330	2.336806
-82.722613	-8.240741	2.346803
-82.085660	-11.282231	2.356800
-81.181994	-13.667848	2.366797
-81.104231	-10.944861	2.376794
-80.089956	-7.941492	2.386790
-79.566572	-12.824237	2.396787
-79.886742	-9.527753	2.406784
-79.172308	-9.094110	2.416781
-78.395298	-7.549733	2.426778
-77.841559	-9.498233	2.436774
-77.568388	-5.181681	2.446771
-76.863520	-11.660539	2.456768
-76.074353	-12.853143	2.466765
-76.054687	-8.108134	2.476762
-75.696847	-7.059628	2.486758
-75.080089	-4.721687	2.496755
-74.603203	-2.755356	2.506752
-73.537380	-11.930563	2.516749
-73.553471	-10.560703	2.526746
-73.167821	-7.515861	2.536742
-72.302456	2.481190	2.546739
-71.872662	-8.280015	2.556736
-71.672065	-9.093787	2.566733
-70.641599	-19.025417	2.576730
-70.432013	-18.747836	2.586726
-70.169983	-14.479429	2.596723
-69.091951	-12.695045	2.606720
-68.639559	-11.639080	2.616717
-68.460434	-15.086658	2.626714
-68.378350	-13.786602	2.636710
-67.395910	-11.672425	2.646707
-66.814023	-14.647295	2.656704
-66.503010	-13.603483	2.666701
-65.562356	-14.668835	2.676698
-65.405519	-13.756767	2.686694
-65.345006	-11.107388	2.696691
-64.306140	-8.767230	2.706688
-63.738304	-8.343686	2.716685
-63.630972	-14.918603	2.726682
-62.533871	-8.387633	2.736678
-62.110414	-12.708099	2.746675
-62.038006	-7.294106	2.756672
-61.916546	-6.175235	2.766669
-61.162493	-6.820245	2.776666
-60.360101	-6.195478	2.786662
-59.695143	-1.338800	2.796659
-59.283157	-7.133920	2.806656
-59.107719	-7.536302	2.816653
-57.965461	-9.906696	2.826650
-57.505518	-8.096218	2.836646
-57.525375	-7.736775	2.846643
-57.301596	-8.475747	2.856640
-56.504570	-6.728402	2.866637
-56.089448	-7.669379	2.876634
-55.223379	-3.082119	2.886630
-54.819827	-8.551604	2.896627
-54.485077	-7.625134	2.906624
-53.947935	-5.732204	2.916621
-53.014073	-5.994234	2.926618
-52.565231	-5.889446	2.936614
-52.640969	-5.604130	2.946611
-52.226962	-6.759499	2.956608
-51.502937	-2.772491	2.966605
-50.670729	-3.765546	2.976602
-49.944264	-3.464690	2.986598
-49.896859	-12.602833	2.996595
-49.766390	-8.812525	3.006592
-49.291350	-4.259697	3.016589
-48.403451	-9.990378	3.026586
-47.568818	-6.639139	3.036582
-46.952618	-5.538179	3.046579
-47.032120	-5.309343	3.056576
-46.471570	-6.229353	3.066573
-45.861975	-15.900812	3.076570
-45.337467	-10.493521	3.086566
-44.989866	-3.745956	3.096563
-44.310808	-3.531892	3.106560
-43.366367	-8.549566	3.116557
-43.262648	-14.427990	3.126554
-43.164889	-11.595295	3.136550
-42.740590	-6.565392	3.146547
-42.059198	-10.513247	3.156544
-40.838219	-6.622562	3.166541
-40.705312	-11.952386	3.176538
-40.372092	-8.024347	3.186534
-40.167611	-9.549672	3.196531
-39.439588	-12.181627	3.206528
-38.818462	-13.701656	3.216525
-38.567727	-11.752997	3.226522
-37.614492	-7.340212	3.236518
-37.529448	-9.862925	3.246515
-36.856277	-10.917170	3.256512
-36.156171	-17.919820	3.266509
-35.753021	-11.840006	3.276506
-35.651370	-14.257785	3.286502
-34.805877	-10.955960	3.296499
-34.264736	-7.990804	3.306496
-34.018904	-18.750781	3.316493
-33.051780	-10.078391	3.326490
-32.710848	-15.894144	3.336486
-32.576931	-8.352270	3.346483
-31.715905	-7.133585	3.356480
-31.196505	-12.469520	3.366477
-30.953265	-6.501926	3.376474
-30.349091	-4.677393	3.386470
-29.455084	-7.040457	3.396467
-29.109683	-11.300772	3.406464
-29.119308	-10.779424	3.416461
-28.523659	-5.303690	3.426458
-27.634756	-12.710448	3.436454
-27.191683	-10.480467	3.446451
-27.161419	-6.751610	3.456448
-26.118472	-16.316213	3.466445
-25.938138	-1.377528	3.476442
-25.357792	-10.117275	3.486438
-24.521693	-6.896679	3.496435
-24.349336	-7.374028	3.506432
-23.938036	-11.679636	3.516429
-23.074959	-10.304011	3.526426
-22.833078	-8.337090	3.536422
-22.549813	-9.263342	3.546419
-21.530064	-12.741254	3.556416
-21.307463	-11.622533	3.566413
-20.918719	-10.526187	3.576410
-20.147217	-19.420876	3.586406
-19.730223	-12.829039	3.596403
-19.505599	-12.852694	3.606400
-18.737076	-11.146263	3.616397
-17.848850	-13.611704	3.626394
-17.783644	-8.132301	3.636390
-17.685636	-6.613585	3.646387
-16.556883	-10.166451	3.656384
-16.293849	-17.206581	3.666381
-16.112261	-15.025965	3.676378
-14.992264	-11.053545	3.686374
-14.591848	-11.948416	3.696371
-14.574793	-15.069814	3.706368
-14.339852	-15.042620	3.716365
-13.196621	-18.428353	3.726362
-12.413143	-15.349208	3.736358
-12.330171	-20.150717	3.746355
-11.944700	-18.222788	3.756352
-11.399909	-15.879243	3.766349
-10.569663	-18.078417	3.776346
-10.281965	-15.776075	3.786342
-9.819663	-16.061963	3.796339
-8.929430	-22.458091	3.806336
-8.496187	-17.093773	3.816333
-8.451134	-12.419353	3.826330
-8.029291	-18.566615	3.836326
-7.231982	-15.296718	3.846323
-6.721244	-15.070978	3.856320
-6.331681	-13.885458	3.866317
-5.410999	-18.409177	3.876314
-5.336382	-18.544720	3.886310
-5.068816	-9.074417	3.896307
-4.086397	-7.970669	3.906304
-3.998694	-10.018432	3.916301
-3.518617	-5.545267	3.926298
-3.204507	11.135520	3.936294
-2.837088	19.334837	3.946291
-2.324844	39.050160	3.956288
-1.453228	54.523898	3.966285
-1.317208	69.474540	3.976282
-0.691238	86.416546	3.986278
-0.447431	107.584999	3.996275
0.000000	123.022381	4.001280
-0.093151	133.026120	4.006285
0.370567	145.550753	4.011290
0.324683	165.401169	4.016294
0.349102	167.542995	4.021299
0.373995	172.800655	4.026304
0.236928	183.215643	4.031309
0.728014	181.429207	4.036314
0.742983	193.735344	4.041318
1.299912	194.100203	4.046323
1.264079	197.763201	4.051328
0.862545	199.966092	4.056333
0.827452	197.397919	4.061338
1.022595	209.218784	4.066342
1.112319	197.711977	4.071347
1.152863	196.825794	4.076352
1.210483	206.487300	4.081357
1.329695	202.694764	4.086362
0.755903	201.377110	4.091366
1.234090	200.927582	4.096371
1.145796	209.322089	4.101376
1.036339	203.139407	4.106381
1.224553	202.138195	4.111386
0.965785	212.294914	4.116390
1.114650	204.144650	4.121395
1.261660	209.987921	4.126400
1.049018	205.842839	4.131405
1.143808	201.994160	4.136410
1.031214	204.718913	4.141414
1.276069	201.278338	4.146419
1.389924	194.419908	4.151424
1.116170	199.809517	4.156429
1.061405	200.849122	4.161434
1.384757	222.235304	4.166438
1.736614	225.029772	4.171443
1.703429	215.417200	4.176448
1.454740	209.342425	4.181453
1.672498	195.526121	4.186458
1.331721	203.109946	4.191462
1.217219	195.306996	4.196467
1.427679	207.241356	4.201472
1.361434	208.744232	4.206477
1.372847	200.882540	4.211482
1.526207	196.144445	4.216486
1.765530	195.976009	4.221491
1.750348	196.462638	4.226496
1.590132	206.488778	4.231501
1.669519	198.184457	4.236506
1.215082	199.080082	4.241510
1.304379	207.067283	4.246515
1.358042	202.597494	4.251520
1.158303	209.573659	4.256525
1.395083	202.075436	4.261530
1.400173	225.836957	4.266534
1.807940	223.468164	4.271539
1.964848	219.744764	4.276544
1.190674	215.664641	4.281549
1.618213	215.284477	4.286554
1.563826	242.268094	4.291558
1.513556	244.803155	4.296563
1.938106	241.604350	4.301568
1.795759	239.890632	4.306573
1.811360	237.823381	4.311578
1.537988	230.173212	4.316582
1.624210	226.846714	4.321587
1.973846	234.606115	4.326592
1.951263	238.320406	4.331597
2.123967	222.164035	4.336602
1.641074	219.849979	4.341606
1.572885	201.934612	4.346611
1.338270	216.068766	4.351616
1.866498	230.210408	4.356621
1.869967	231.828431	4.361626
2.013260	240.748788	4.366630
1.991043	233.364873	4.371635
1.626701	228.093255	4.376640
1.821759	232.057247	4.381645
2.276052	228.840297	4.386650
1.509875	224.461859	4.391654
1.700235	232.988430	4.396659
2.249608	246.402758	4.401664
2.085847	242.631811	4.406669
2.155861	227.124506	4.411674
1.649487	214.704261	4.416678
2.105512	224.515099	4.421683
1.928051	228.722521	4.426688
2.134448	229.882671	4.431693
1.927087	219.973335	4.436698
1.418827	227.660879	4.441702
1.857822	238.676121	4.446707
2.125956	240.538232	4.451712
2.186073	243.860933	4.456717
1.864581	233.405318	4.461722
2.294319	245.349771	4.466726
2.511311	234.290732	4.471731
2.348818	248.086185	4.476736
2.117372	245.595511	4.481741
2.222748	244.875995	4.486746
2.142476	247.824904	4.491750
1.906069	239.113456	4.496755
1.816874	242.484562	4.501760
1.864660	242.127418	4.506765
1.953664	238.740269	4.511770
1.448197	237.724272	4.516774
1.835779	230.158242	4.521779
1.925935	234.928158	4.526784
1.778151	247.522362	4.531789
2.256511	246.494217	4.536794
2.058827	256.424768	4.541798
2.266095	256.265586	4.546803
2.253279	262.751227	4.551808
2.320307	263.909396	4.556813
2.208149	263.095461	4.561818
1.923461	272.909004	4.566822
2.468649	257.525057	4.571827
2.354314	263.523118	4.576832
1.758778	271.187445	4.581837
2.029624	265.105948	4.586842
1.735481	266.564278	4.591846
2.358639	284.150731	4.596851
2.391531	293.262068	4.601856
2.237768	295.745602	4.606861
2.840449	298.356468	4.611866
2.798137	299.057559	4.616870
2.601512	277.351823	4.621875
2.228723	266.347798	4.626880
2.507196	284.492561	4.631885
2.906192	289.346528	4.636890
2.326513	282.566197	4.641894
2.413489	270.751157	4.646899
2.662375	279.734762	4.651904
2.550127	282.571755	4.656909
2.862231	266.055798	4.661914
2.454886	270.349053	4.666918
2.248435	267.364448	4.671923
2.414498	287.148745	4.676928
2.381698	292.605640	4.681933
2.683706	302.887419	4.686938
2.997497	305.218150	4.691942
2.756811	295.003085	4.696947
2.716047	305.818390	4.701952
3.005070	302.229581	4.706957
3.121998	283.369799	4.711962
2.676124	276.714921	4.716966
2.725075	275.232571	4.721971
2.814230	276.408389	4.726976
2.705828	271.820572	4.731981
2.931258	270.022665	4.736986
2.436383	271.162385	4.741990
2.672678	260.887895	4.746995
2.670108	260.475153	4.752000
2.412041	274.998838	4.757005
2.477135	287.073759	4.762010
2.823274	303.646609	4.767014
3.047830	293.589138	4.772019
3.263365	296.560707	4.777024
2.795895	297.388835	4.782029
2.854094	307.770388	4.787034
2.808025	305.218420	4.792038
3.094015	296.322361	4.797043
3.123097	291.080888	4.802048
2.798355	301.839020	4.807053
3.041442	297.886432	4.812058
2.724275	308.989048	4.817062
2.985339	301.439198	4.822067
2.800835	304.176862	4.827072
2.848355	304.862092	4.832077
3.126551	296.593471	4.837082
3.047094	304.694311	4.842086
3.154081	306.008865	4.847091
3.339419	302.659624	4.852096
2.115526	303.008369	4.857101
2.788658	287.048494	4.862106
2.768595	305.473205	4.867110
2.871595	297.173801	4.872115
3.077278	301.654652	4.877120
2.735838	303.529105	4.882125
3.087216	307.375076	4.887130
2.966499	314.097452	4.892134
3.146138	322.896988	4.897139
3.236910	337.917681	4.902144
3.287854	336.609638	4.907149
3.306271	321.011326	4.912154
3.380267	319.599615	4.917158
3.306132	306.219905	4.922163
3.262345	310.432447	4.927168
2.831197	316.926800	4.932173
3.426150	316.553642	4.937178
3.394268	328.926254	4.942182
3.300364	321.539367	4.947187
3.235988	307.430065	4.952192
2.977535	315.827744	4.957197
3.430073	329.329616	4.962202
3.288983	337.210979	4.967206
3.440114	342.562644	4.972211
3.584363	332.463586	4.977216
3.172966	324.684671	4.982221
3.663642	321.935483	4.987226
3.129231	333.137830	4.992230
3.114642	336.240853	4.997235
3.325348	334.707835	5.002240
3.219966	343.754284	5.007245
3.508096	337.366985	5.012250
3.564429	339.394619	5.017254
3.505314	336.802774	5.022259
3.612501	333.021867	5.027264
3.428989	339.365504	5.032269
3.420035	338.083561	5.037274
3.116423	343.022710	5.042278
3.684565	332.798601	5.047283
3.446023	337.223370	5.052288
3.179263	343.829636	5.057293
3.107656	335.885125	5.062298
3.372605	337.144517	5.067302
3.629482	332.427522	5.072307
3.794714	331.749004	5.077312
3.422749	343.771427	5.082317
3.292640	330.859970	5.087322
3.340470	342.897537	5.092326
3.943071	370.234553	5.097331
3.806380	360.267839	5.102336
3.532192	355.126489	5.107341
4.071682	356.048561	5.112346
3.834048	344.402067	5.117350
3.462420	341.218454	5.122355
3.882320	339.002544	5.127360
3.690037	341.704009	5.132365
3.479869	333.807505	5.137370
3.357945	356.414921	5.142374
3.634419	363.854976	5.147379
3.838111	368.798142	5.152384
3.447738	382.196123	5.157389
3.422596	369.340662	5.162394
3.720830	375.758464	5.167398
3.669202	380.990386	5.172403
4.144909	375.045818	5.177408
3.881491	379.782367	5.182413
4.313584	366.441325	5.187418
4.040349	377.426207	5.192422
3.760335	369.610713	5.197427
4.093314	375.778459	5.202432
3.819179	370.876663	5.207437
3.752620	363.587448	5.212442
3.822444	376.164865	5.217446
3.895282	372.353524	5.222451
3.672060	379.763256	5.227456
3.517021	376.190734	5.232461
3.986080	373.290800	5.237466
3.999767	370.609537	5.242470
3.787259	376.799134	5.247475
4.217399	388.462427	5.252480
3.991642	394.599365	5.257485
4.252769	407.083560	5.262490
3.914225	390.829726	5.267494
4.297165	398.932785	5.272499
3.987356	390.894684	5.277504
3.977560	396.958369	5.282509
4.376017	396.565454	5.287514
4.124799	407.414889	5.292518
4.193176	391.195499	5.297523
4.343241	395.288346	5.302528
4.136181	386.834415	5.307533
4.070094	381.705957	5.312538
3.935038	391.943740	5.317542
4.281406	394.758685	5.322547
4.385815	399.978589	5.327552
4.191320	394.530983	5.332557
4.279040	395.007684	5.337562
3.979808	396.182307	5.342566
4.218390	392.030144	5.347571
4.153811	393.882444	5.352576
4.077024	401.132762	5.357581
4.331919	396.543556	5.362586
4.108951	397.177279	5.367590
4.400010	394.021860	5.372595
4.388926	400.439190	5.377600
4.324875	399.894147	5.382605
4.338513	398.563465	5.387610
4.370860	396.362190	5.392614
4.233323	394.385595	5.397619
4.616347	398.528077	5.402624
4.271879	400.513355	5.407629
4.298675	400.013062	5.412634
4.456288	391.071901	5.417638
4.365770	393.249169	5.422643
4.490534	399.257617	5.427648
4.354031	404.020717	5.432653
4.481931	391.220409	5.437658
4.298164	406.894824	5.442662
4.041277	404.611199	5.447667
4.339841	424.267562	5.452672
4.698510	427.933173	5.457677
4.962400	435.274704	5.462682
4.687405	427.199837	5.467686
4.779870	416.014865	5.472691
4.379392	403.187979	5.477696
4.513153	415.052714	5.482701
4.561611	414.955941	5.487706
4.574355	429.677653	5.492710
4.627905	434.964402	5.497715
4.891006	431.680402	5.502720
4.544469	434.244622	5.507725
4.714436	436.616752	5.512730
4.613220	429.764626	5.517734
4.832585	435.243161	5.522739
4.813457	437.873739	5.527744
4.603049	438.964392	5.532749
4.691887	426.247091	5.537754
4.938703	436.774904	5.542758
5.164416	433.593395	5.547763
5.125523	419.528712	5.552768
4.435336	418.519214	5.557773
4.880993	417.535152	5.562778
4.582458	427.556711	5.567782
4.814596	428.696234	5.572787
4.854909	432.316288	5.577792
4.767256	434.305024	5.582797
4.790825	432.624591	5.587802
4.710276	436.309850	5.592806
5.011316	440.396851	5.597811
4.664007	437.740622	5.602816
4.718205	432.142300	5.607821
4.758869	440.661016	5.612826
4.519341	438.271106	5.617830
4.962274	429.275376	5.622835
4.903225	429.776183	5.627840
4.524771	436.612135	5.632845
4.881498	428.204341	5.637850
4.785904	450.532248	5.642854
4.752040	453.447463	5.647859
5.314746	462.649168	5.652864
4.972944	465.705363	5.657869
5.353803	471.852590	5.662874
5.324631	471.172709	5.667878
5.266402	464.040727	5.672883
5.177452	438.604014	5.677888
4.977809	429.133527	5.682893
5.047827	443.971868	5.687898
5.148067	444.328488	5.692902
5.066825	456.731280	5.697907
5.098595	458.918303	5.702912
4.875166	461.526276	5.707917
5.301823	457.065298	5.712922
5.241804	467.981784	5.717926
5.081686	465.074718	5.722931
5.276949	465.540520	5.727936
5.292027	461.071126	5.732941
5.478231	463.760852	5.737946
5.697103	467.751154	5.742950
5.352883	461.051341	5.747955
5.465509	455.101743	5.752960
4.899937	458.241364	5.757965
5.130684	457.335512	5.762970
4.943193	464.594916	5.767974
5.007882	463.548231	5.772979
5.357220	464.741168	5.777984
4.860854	476.756074	5.782989
5.395840	474.924646	5.787994
5.149369	466.441281	5.792998
5.197545	476.037423	5.798003
5.126165	463.274594	5.803008
5.091496	485.618511	5.808013
5.157305	500.764859	5.813018
5.577462	504.876160	5.818022
5.941088	509.661065	5.823027
5.797234	492.973103	5.828032
5.217462	491.428091	5.833037
5.385843	491.732186	5.838042
5.602665	502.662057	5.843046
5.337783	500.668053	5.848051
5.602784	496.424264	5.853056
5.538140	509.874586	5.858061
5.843920	493.683070	5.863066
5.781664	506.070522	5.868070
5.771564	504.288107	5.873075
6.023995	475.962399	5.878080
5.326418	480.392375	5.883085
5.374250	475.494064	5.888090
5.352026	485.692308	5.893094
5.524186	492.729564	5.898099
5.940657	485.494300	5.903104
5.584263	502.989626	5.908109
6.233453	507.671398	5.913114
5.633136	492.527421	5.918118
5.745183	486.815502	5.923123
5.715727	467.397981	5.928128
5.552076	485.817082	5.933133
5.762479	490.819167	5.938138
6.003765	495.672871	5.943142
5.779175	492.371142	5.948147
5.552214	489.146769	5.953152
5.889088	505.073901	5.958157
5.948651	490.069896	5.963162
5.735451	500.179396	5.968166
6.132292	494.573253	5.973171
5.951877	491.430566	5.978176
5.513329	484.845229	5.983181
5.781163	491.964325	5.988186
5.948187	493.045962	5.993190
5.709384	504.570084	5.998195
5.830565	499.715664	6.003200
5.653987	503.537808	6.008205
5.588882	497.239326	6.013210
4.975340	499.900261	6.018214
5.475655	502.361362	6.023219
6.156735	500.257882	6.028224
5.229671	515.348817	6.033229
5.916887	513.211561	6.038234
6.284776	532.303047	6.043238
5.901001	526.749981	6.048243
6.130199	530.111644	6.053248
6.050045	525.529730	6.058253
6.003647	510.375908	6.063258
5.827211	505.675950	6.068262
6.066709	507.487778	6.073267
6.029472	497.622911	6.078272
5.616352	505.863568	6.083277
6.447199	501.430764	6.088282
6.229611	506.369139	6.093286
6.030661	507.028490	6.098291
6.191438	503.837789	6.103296
6.063172	514.327911	6.108301
6.086769	507.175453	6.113306
6.268119	507.317359	6.118310
6.046656	505.346950	6.123315
6.095017	502.204662	6.128320
5.956201	510.469363	6.133325
6.032818	503.810158	6.138330
5.946131	507.208927	6.143334
6.149750	511.309711	6.148339
6.361423	495.857812	6.153344
5.868417	494.152205	6.158349
5.709751	467.959143	6.163354
5.871284	475.763627	6.168358
5.788990	475.701529	6.173363
6.033890	483.066947	6.178368
5.904987	491.327826	6.183373
5.721844	492.636762	6.188378
5.747432	496.203423	6.193382
5.803242	498.386273	6.198387
6.002002	498.986082	6.203392
6.102011	501.609968	6.208397
6.123549	508.439116	6.213402
5.858542	512.702947	6.218406
5.857085	507.408638	6.223411
5.704744	501.663728	6.228416
5.685379	509.126003	6.233421
5.877610	501.407678	6.238426
5.864106	499.031837	6.243430
6.000468	504.401002	6.248435
5.737077	502.383663	6.253440
5.500375	511.682446	6.258445
6.013417	503.808184	6.263450
5.853259	504.795403	6.268454
5.814499	510.975819	6.273459
6.124485	501.510688	6.278464
6.108105	508.922936	6.283469
6.212132	500.667853	6.288474
6.078010	499.265329	6.293478
6.074567	498.258340	6.298483
6.174338	493.255911	6.303488
5.703141	508.344369	6.308493
5.716407	497.675863	6.313498
5.819958	499.405020	6.318502
5.454155	506.877891	6.323507
5.557014	498.792910	6.328512
5.674327	508.424394	6.333517
5.988415	492.425094	6.338522
6.062151	510.256313	6.343526
6.058441	502.626675	6.348531
6.102201	499.426540	6.353536
5.715978	503.972112	6.358541
5.834301	500.253061	6.363546
5.740665	501.401936	6.368550
5.650109	502.677782	6.373555
5.906757	495.116926	6.378560
5.911445	502.876354	6.383565
6.227316	499.829288	6.388570
6.251756	503.857716	6.393574
5.907864	503.687971	6.398579
6.257623	499.134532	6.403584
5.884250	508.170593	6.408589
5.965807	501.054126	6.413594
6.192240	500.299161	6.418598
5.806925	496.759611	6.423603
6.210316	506.148949	6.428608
5.910050	504.093117	6.433613
5.967877	497.151082	6.438618
6.266310	499.119704	6.443622
5.829894	501.124759	6.448627
6.082147	497.987980	6.453632
5.908606	506.153445	6.458637
5.931302	500.363764	6.463642
6.211854	501.950932	6.468646
6.005656	484.199780	6.473651
5.794688	480.705958	6.478656
5.506788	483.875975	6.483661
6.034812	489.401694	6.488666
5.983804	500.722242	6.493670
5.610616	505.325252	6.498675
6.176892	500.176702	6.503680
5.898165	512.769321	6.508685
6.066881	502.342466	6.513690
5.998463	503.301864	6.518694
6.074504	501.987678	6.523699
6.031382	501.677551	6.528704
6.097747	477.964661	6.533709
5.723428	475.655477	6.538714
5.975402	467.828410	6.543718
5.618544	476.763049	6.548723
5.862426	485.668865	6.553728
5.783828	498.857449	6.558733
5.808708	500.302638	6.563738
6.122300	496.875087	6.568742
6.454044	500.768166	6.573747
5.840935	477.529512	6.578752
5.523075	477.214163	6.583757
5.934615	489.269369	6.588762
5.810587	499.409885	6.593766
6.090390	500.852527	6.598771
6.218384	497.496162	6.603776
5.953272	485.306694	6.608781
5.792731	476.331141	6.613786
6.112329	480.096772	6.618790
5.820297	474.830856	6.623795
5.932081	470.157185	6.628800
5.859251	465.340427	6.633805
6.307255	467.514770	6.638810
5.983719	475.159612	6.643814
5.726033	469.290075	6.648819
5.807575	467.626876	6.653824
5.771477	483.831240	6.658829
6.139386	483.085606	6.663834
5.620657	485.849835	6.668838
5.930379	496.592238	6.673843
6.045503	494.206347	6.678848
5.851395	492.641283	6.683853
5.818715	499.831062	6.688858
6.029269	503.008137	6.693862
6.250246	500.614781	6.698867
6.037694	480.031098	6.703872
5.721253	477.885198	6.708877
5.680742	481.286183	6.713882
5.801453	488.005756	6.718886
6.172281	492.740523	6.723891
6.278440	488.284061	6.728896
6.134014	476.935604	6.733901
5.882067	469.717886	6.738906
6.194307	471.213369	6.743910
5.650512	470.106019	6.748915
5.813428	464.633740	6.753920
5.731104	478.675820	6.758925
5.748527	478.639835	6.763930
5.839338	473.475895	6.768934
5.654662	479.663884	6.773939
6.098253	487.566120	6.778944
6.001456	491.908260	6.783949
6.530438	493.109342	6.788954
5.896006	478.218293	6.793958
5.635086	479.165559	6.798963
5.740766	483.100607	6.803968
5.880085	481.432970	6.808973
5.854835	480.562205	6.813978
5.979784	479.900613	6.818982
5.823836	487.288403	6.823987
5.926101	494.161602	6.828992
5.935029	508.594920	6.833997
6.317773	502.944142	6.839002
6.079376	478.709433	6.844006
5.601927	478.033332	6.849011
5.928766	472.104694	6.854016
5.971371	478.961125	6.859021
5.780664	470.963844	6.864026
5.749531	479.645236	6.869030
5.697528	497.583302	6.874035
6.263678	501.572744	6.879040
6.128965	497.230561	6.884045
6.164467	486.734605	6.889050
5.942300	482.956102	6.894054
5.903860	474.594971	6.899059
5.735157	463.929586	6.904064
5.878426	470.333621	6.909069
6.208353	462.921675	6.914074
5.796854	476.053473	6.919078
5.970716	476.359028	6.924083
5.768480	481.358791	6.929088
5.624453	483.463826	6.934093
5.772540	481.928336	6.939098
6.243592	489.755576	6.944102
5.782294	486.651113	6.949107
6.229942	487.448094	6.954112
5.840185	492.875365	6.959117
5.570587	476.939974	6.964122
6.000227	488.728932	6.969126
6.054240	498.106655	6.974131
6.058693	472.676916	6.979136
5.616690	485.064874	6.984141
5.990035	496.846979	6.989146
6.292974	495.185400	6.994150
6.066926	484.187311	6.999155
5.963474	480.402767	7.004160
6.030670	476.517148	7.009165
5.840848	468.776458	7.014170
5.839350	474.726316	7.019174
5.781509	470.841670	7.024179
5.821211	463.885878	7.029184
5.748742	479.287961	7.034189
5.733875	475.463293	7.039194
6.061616	487.018504	7.044198
5.925051	489.636766	7.049203
6.329797	489.305956	7.054208
5.880891	477.966870	7.059213
5.812954	473.404656	7.064218
5.786027	471.559909	7.069222
5.866562	472.061285	7.074227
5.931623	473.645454	7.079232
5.769500	489.431416	7.084237
6.233905	491.994171	7.089242
6.109786	478.310597	7.094246
5.833408	474.564161	7.099251
5.947524	471.788894	7.104256
5.770221	478.625498	7.109261
5.673571	463.896624	7.114266
5.840804	478.717519	7.119270
5.896861	500.014748	7.124275
6.248459	491.396618	7.129280
5.996363	492.710460	7.134285
5.718413	478.248598	7.139290
5.696254	486.431610	7.144294
5.904139	501.637709	7.149299
6.028367	503.029349	7.154304
6.022323	517.144478	7.159309
6.045737	514.101238	7.164314
6.119768	507.526526	7.169318
5.718002	492.812233	7.174323
5.942735	480.894103	7.179328
5.731470	494.463413	7.184333
5.676102	504.401341	7.189338
5.871007	514.355456	7.194342
5.983984	513.305311	7.199347
5.661357	508.391766	7.204352
5.940126	514.595383	7.209357
6.010805	521.724642	7.214362
6.232543	521.053928	7.219366
6.182726	521.624252	7.224371
6.453635	493.734136	7.229376
5.772433	499.230193	7.234381
5.817918	480.956059	7.239386
5.583707	486.801781	7.244390
5.518265	492.516153	7.249395
5.733918	498.828094	7.254400
5.733639	524.015353	7.259405
5.834702	514.500151	7.264410
6.141639	519.238599	7.269414
5.892703	527.266976	7.274419
5.968759	519.859349	7.279424
5.832441	530.410609	7.284429
5.835158	516.556218	7.289434
5.816577	522.511686	7.294438
5.853670	521.106463	7.299443
6.298212	516.705654	7.304448
6.100323	522.147144	7.309453
5.886109	511.749354	7.314458
6.179558	514.880736	7.319462
6.134529	519.696608	7.324467
6.066622	509.977120	7.329472
5.557451	498.581100	7.334477
5.918050	499.006501	7.339482
6.009653	508.297886	7.344486
5.986477	517.381540	7.349491
6.131775	512.087003	7.354496
5.894598	508.049111	7.359501
5.927291	499.892471	7.364506
5.827736	503.939852	7.369510
5.951834	516.070304	7.374515
6.067736	511.865605	7.379520
5.908047	502.558563	7.384525
5.797224	496.523402	7.389530
5.924684	503.879268	7.394534
5.956896	505.396851	7.399539
5.864941	507.195285	7.404544
5.505636	516.961149	7.409549
5.815386	513.602509	7.414554
6.116740	521.050361	7.419558
5.726047	523.744059	7.424563
6.158507	513.367852	7.429568
5.859518	521.518773	7.434573
5.860742	520.150077	7.439578
6.203631	512.905870	7.444582
6.273036	521.326727	7.449587
5.984443	499.987763	7.454592
5.591170	500.519643	7.459597
5.479490	500.256784	7.464602
6.085342	506.707573	7.469606
5.717755	518.797488	7.474611
5.884653	514.000616	7.479616
5.898026	519.144069	7.484621
5.685852	517.796304	7.489626
5.887038	518.552202	7.494630
5.784102	524.209250	7.499635
5.912944	521.803323	7.504640
5.669789	523.309869	7.509645
5.815518	520.875886	7.514650
5.872098	520.614174	7.519654
5.624262	521.544673	7.524659
5.715566	514.356728	7.529664
5.640673	516.819541	7.534669
6.152593	521.188176	7.539674
6.079990	509.956664	7.544678
5.575479	522.808882	7.549683
5.638546	518.149578	7.554688
5.856639	522.362622	7.559693
6.215960	518.335871	7.564698
6.085006	525.231718	7.569702
5.970984	518.612955	7.574707
6.101781	506.855009	7.579712
5.796930	514.623270	7.584717
6.322306	518.092771	7.589722
6.004965	508.682968	7.594726
6.017687	513.852576	7.599731
5.860575	507.349489	7.604736
6.026518	505.595941	7.609741
6.053108	513.714850	7.614746
5.847481	518.421941	7.619750
5.712473	520.597319	7.624755
5.723594	520.845756	7.629760
5.522444	521.645188	7.634765
5.462140	520.532367	7.639770
5.953932	523.130455	7.644774
6.105834	530.193382	7.649779
6.173766	515.287031	7.654784
5.947785	515.371471	7.659789
5.802828	521.439627	7.664794
5.964046	513.748139	7.669798
5.757457	517.994997	7.674803
6.108303	509.237068	7.679808
5.911603	516.710753	7.684813
6.090352	517.598833	7.689818
6.083469	522.444108	7.694822
6.100639	520.874051	7.699827
6.159207	515.683861	7.704832
5.833723	514.139760	7.709837
6.162407	515.321518	7.714842
6.149000	516.312459	7.719846
5.770925	512.347034	7.724851
5.937578	506.962134	7.729856
5.986610	515.262432	7.734861
6.103348	518.097466	7.739866
5.931879	510.664526	7.744870
5.971380	520.944531	7.749875
6.052500	512.894125	7.754880
5.935314	510.111370	7.759885
5.893146	525.607151	7.764890
6.296110	511.044347	7.769894
6.018366	518.312406	7.774899
6.249985	512.255069	7.779904
6.111967	520.269022	7.784909
6.217287	499.831595	7.789914
6.148431	486.118931	7.794918
5.568234	494.163071	7.799923
5.902718	482.401213	7.804928
5.843236	484.836013	7.809933
5.609691	485.199360	7.814938
5.704283	503.058692	7.819942
5.863946	509.863390	7.824947
5.861215	506.818758	7.829952
5.832678	511.246691	7.834957
5.996301	513.648103	7.839962
6.079056	522.927543	7.844966
5.912915	513.171433	7.849971
5.862553	513.287967	7.854976
5.989238	519.902369	7.859981
5.806804	519.497301	7.864986
6.056227	512.980965	7.869990
5.506635	522.254604	7.874995
6.146365	515.391441	7.880000
6.010878	515.737960	7.885005
6.125318	517.263833	7.890010
5.921609	518.424424	7.895014
6.216885	524.218201	7.900019
6.041953	506.376990	7.905024
5.788151	509.638062	7.910029
5.950635	512.167736	7.915034
6.155239	517.650718	7.920038
5.810081	503.106817	7.925043
5.558391	492.304781	7.930048
5.883518	506.861172	7.935053
5.980581	511.393815	7.940058
6.025273	508.377641	7.945062
5.697245	511.966944	7.950067
6.049879	509.765899	7.955072
5.789510	507.002314	7.960077
5.966572	515.877179	7.965082
6.101020	518.395709	7.970086
5.850521	517.930672	7.975091
6.019463	509.397835	7.980096
5.758799	522.096994	7.985101
5.849373	514.737287	7.990106
6.106196	518.092596	7.995110
6.059809	518.577496	8.000115
6.117606	509.132440	8.005133
5.730208	495.273292	8.010150
5.533514	504.119614	8.015168
5.705119	510.042966	8.020186
5.808051	509.758869	8.025203
6.013542	505.447463	8.030221
6.019138	511.794141	8.035238
5.954173	523.081860	8.040256
6.104829	515.176652	8.045274
5.761031	523.844996	8.050291
6.115693	509.248831	8.055309
5.654199	511.740672	8.060326
5.662671	515.961051	8.065344
5.750926	514.654462	8.070362
5.803942	521.807403	8.075379
6.280400	517.693036	8.080397
5.818256	518.300677	8.085414
6.168457	515.562431	8.090432
6.003167	519.845047	8.095450
5.629070	520.248949	8.100467
6.245734	518.477330	8.105485
6.090867	515.571358	8.110502
6.039576	514.425464	8.115520
6.286452	509.548782	8.120538
6.089546	518.076863	8.125555
6.005300	511.098283	8.130573
6.271937	508.464025	8.135590
5.497273	523.398524	8.140608
6.109099	512.386077	8.145626
5.967522	513.561652	8.150643
5.880493	518.447010	8.155661
5.947884	520.072396	8.160678
6.088043	517.874600	8.165696
6.148360	509.505846	8.170714
5.985576	518.595558	8.175731
6.060068	525.393593	8.180749
6.136188	516.661222	8.185766
5.825182	518.982092	8.190784
6.438050	531.567314	8.195802
6.278539	531.554610	8.200819
6.242697	516.561718	8.205837
6.161051	520.936775	8.210854
6.249669	520.354873	8.215872
6.103955	515.052683	8.220890
5.914198	520.715822	8.225907
6.123214	515.523974	8.230925
5.920033	522.089859	8.235942
5.818212	528.036252	8.240960
6.315007	537.083286	8.245978
6.414989	553.379367	8.250995
6.485863	539.848201	8.256013
6.212531	528.105805	8.261030
5.936491	520.148622	8.266048
6.160967	521.806653	8.271066
5.691532	531.868538	8.276083
5.901713	544.666896	8.281101
6.450588	544.910683	8.286118
6.323446	549.389337	8.291136
6.276944	548.317642	8.296154
6.300902	543.413693	8.301171
6.095196	544.882350	8.306189
6.542586	546.571577	8.311206
6.382750	549.601421	8.316224
6.442126	542.657504	8.321242
6.129732	542.938403	8.326259
5.898947	548.307974	8.331277
6.481905	542.161349	8.336294
6.276736	551.418519	8.341312
6.371243	535.858198	8.346330
6.538325	550.229527	8.351347
6.186812	534.576737	8.356365
6.115475	528.750650	8.361382
6.233809	540.501891	8.366400
6.276595	539.575832	8.371418
6.396614	551.642921	8.376435
6.241976	540.103680	8.381453
6.426080	548.121279	8.386470
6.063601	549.403116	8.391488
6.522743	537.110321	8.396506
6.563934	540.830641	8.401523
6.187266	539.392783	8.406541
6.362115	539.445176	8.411558
6.543965	547.372800	8.416576
6.614090	535.295397	8.421594
6.029392	528.482743	8.426611
6.213681	529.845483	8.431629
6.166675	537.503344	8.436646
5.874043	551.817540	8.441664
6.385850	543.535411	8.446682
6.324804	548.565678	8.451699
6.467818	545.548962	8.456717
6.062930	556.595574	8.461734
6.064347	551.111342	8.466752
6.121126	551.289972	8.471770
6.183982	547.676337	8.476787
6.144889	549.717951	8.481805
6.207716	553.797066	8.486822
6.085825	572.306717	8.491840
6.638083	574.436227	8.496858
6.446509	574.567208	8.501875
6.121743	578.297351	8.506893
6.682534	580.564219	8.511910
6.404763	579.370198	8.516928
6.762524	577.927251	8.521946
6.241454	583.368325	8.526963
6.201727	574.899378	8.531981
6.687108	573.518166	8.536998
6.382386	582.886912	8.542016
6.610764	587.554721	8.547034
6.524090	582.978310	8.552051
6.452267	577.569578	8.557069
6.573559	574.006099	8.562087
6.243684	582.928255	8.567104
6.837014	568.395656	8.572122
6.419074	577.230036	8.577139
6.094575	575.775663	8.582157
6.317028	581.454025	8.587175
6.211880	578.101059	8.592192
6.538036	579.931223	8.597210
6.528401	575.896151	8.602227
6.574136	583.884519	8.607245
6.576828	582.205112	8.612263
6.494909	582.532881	8.617280
6.837269	581.161770	8.622298
6.647724	577.581261	8.627315
6.193360	581.376170	8.632333
6.530563	581.444786	8.637351
6.360303	583.378212	8.642368
6.878117	586.710981	8.647386
6.626089	581.247251	8.652403
6.543485	582.932714	8.657421
6.397438	576.540872	8.662439
6.651934	586.567360	8.667456
6.705935	577.569936	8.672474
6.605650	578.640457	8.677491
6.745635	589.135680	8.682509
6.924142	583.009361	8.687527
6.523541	588.195466	8.692544
6.949263	581.929400	8.697562
6.812752	578.296018	8.702579
6.592729	580.742373	8.707597
6.697494	568.442294	8.712615
6.932865	570.480979	8.717632
6.544310	581.316848	8.722650
6.525694	574.637783	8.727667
6.443967	586.147206	8.732685
6.591903	571.530100	8.737703
6.257974	577.353934	8.742720
6.664749	591.825955	8.747738
6.746336	605.401706	8.752755
6.733407	608.907201	8.757773
7.001483	611.744160	8.762791
6.767479	606.056587	8.767808
6.636485	591.197087	8.772826
6.510274	598.725978	8.777843
6.940453	605.144504	8.782861
6.988923	603.890161	8.787879
6.760384	604.581161	8.792896
6.764788	597.757142	8.797914
6.917961	589.865061	8.802931
6.654410	597.079905	8.807949
6.977823	596.055213	8.812967
6.981872	592.956585	8.817984
6.813641	585.761776	8.823002
6.783252	579.394281	8.828019
6.602009	585.222754	8.833037
6.876269	586.336169	8.838055
6.803852	591.704923	8.843072
6.737784	595.739846	8.848090
7.063770	600.059630	8.853107
6.641701	598.895801	8.858125
7.208876	591.173337	8.863143
6.583428	585.234470	8.868160
6.807352	592.190652	8.873178
6.725149	603.465144	8.878195
6.998239	607.625787	8.883213
6.907340	601.484233	8.888231
6.706821	610.706025	8.893248
6.848580	614.371917	8.898266
6.951794	602.826937	8.903283
6.769806	611.695489	8.908301
7.069574	605.708914	8.913319
6.649936	616.476928	8.918336
6.808558	599.053889	8.923354
7.032234	609.572076	8.928371
6.994426	611.895946	8.933389
7.157336	604.228214	8.938407
6.835804	610.066147	8.943424
6.935472	611.543491	8.948442
7.035131	614.626631	8.953459
7.027064	614.590228	8.958477
7.151508	607.206797	8.963495
6.973375	611.508492	8.968512
6.836095	607.129220	8.973530
6.883447	608.206593	8.978547
6.765936	607.970020	8.983565
7.052971	605.023532	8.988583
6.679830	606.844700	8.993600
6.702908	614.109130	8.998618
6.960753	609.820127	9.003635
6.648158	609.447956	9.008653
7.060800	608.341563	9.013671
6.973039	607.323543	9.018688
7.015312	599.527177	9.023706
7.077654	606.890213	9.028723
6.865357	607.190363	9.033741
6.911043	604.100781	9.038759
7.141788	607.732253	9.043776
6.969246	621.727435	9.048794
7.583257	613.466533	9.053811
7.332362	616.800031	9.058829
7.209242	613.271503	9.063847
6.757272	604.515119	9.068864
7.265040	614.148136	9.073882
7.363222	602.263068	9.078899
7.091352	597.544299	9.083917
7.218961	600.024228	9.088935
6.993843	601.904146	9.093952
6.544144	610.420008	9.098970
7.341029	601.674924	9.103987
6.733907	610.032417	9.109005
7.174984	615.234659	9.114023
7.452765	641.287729	9.119040
7.210002	625.609162	9.124058
7.464075	607.598693	9.129075
6.948391	616.986843	9.134093
7.425854	597.013740	9.139111
7.047785	612.672164	9.144128
7.210786	610.602257	9.149146
7.024103	608.738866	9.154163
7.072819	631.967450	9.159181
7.477615	629.684876	9.164199
7.208336	629.644879	9.169216
7.139180	632.622127	9.174234
7.360171	633.188302	9.179251
7.195162	637.680928	9.184269
7.306466	644.471936	9.189287
7.512878	641.315972	9.194304
7.240976	632.183715	9.199322
7.335765	613.967543	9.204339
7.200645	613.642751	9.209357
7.610004	614.964096	9.214375
7.354464	618.324740	9.219392
7.478443	619.930924	9.224410
7.689699	618.678166	9.229427
7.240874	617.262877	9.234445
7.053053	615.211694	9.239463
7.702448	613.885795	9.244480
7.774496	617.697080	9.249498
7.545009	613.131317	9.254515
7.141556	620.406737	9.259533
7.324535	613.559243	9.264551
7.111583	612.620610	9.269568
6.992349	615.632720	9.274586
7.052546	601.710383	9.279603
7.227790	617.416943	9.284621
7.232853	603.222060	9.289639
7.313448	621.169537	9.294656
7.451638	638.847081	9.299674
7.576302	627.624690	9.304691
7.424634	627.200085	9.309709
7.531388	617.303018	9.314727
7.379494	613.714692	9.319744
6.880563	614.926812	9.324762
7.467411	629.340313	9.329779
7.435005	641.642146	9.334797
7.371243	643.139863	9.339815
7.340491	642.421238	9.344832
7.478605	637.270025	9.349850
7.543555	641.956646	9.354867
7.296082	643.610168	9.359885
7.261287	645.193042	9.364903
7.482245	644.536273	9.369920
7.340233	642.545607	9.374938
7.500560	643.571010	9.379955
7.575473	643.678335	9.384973
7.664768	646.213825	9.389991
7.542642	645.321564	9.395008
7.641161	643.121788	9.400026
7.848842	634.220529	9.405043
7.701404	641.406325	9.410061
7.294542	644.923715	9.415079
7.529173	636.614015	9.420096
7.436051	646.268802	9.425114
7.900974	639.880481	9.430131
7.340905	639.719158	9.435149
7.009185	648.566072	9.440167
7.317667	650.090136	9.445184
7.087819	641.609330	9.450202
7.656271	639.921464	9.455219
7.052599	647.828632	9.460237
7.610539	651.550807	9.465255
7.766361	662.271198	9.470272
7.356660	671.365077	9.475290
7.820824	665.490027	9.480307
7.703747	669.375158	9.485325
7.788396	672.894429	9.490343
7.737153	660.203996	9.495360
7.418369	655.185124	9.500378
7.670927	659.228126	9.505395
7.603194	668.335451	9.510413
7.910700	670.063996	9.515431
7.796050	669.954302	9.520448
7.440579	663.800041	9.525466
7.924666	665.978055	9.530483
7.592127	655.988165	9.535501
7.731306	663.563489	9.540519
8.087029	659.156894	9.545536
7.509781	655.068163	9.550554
7.779355	648.307489	9.555571
7.639043	654.255973	9.560589
7.924939	666.741324	9.565607
7.955514	648.944576	9.570624
7.573298	654.633137	9.575642
7.842375	648.305981	9.580659
7.880141	648.293088	9.585677
7.605283	647.144639	9.590695
8.002209	645.953254	9.595712
7.722273	648.356394	9.600730
7.567213	641.597931	9.605747
7.854994	659.830218	9.610765
7.929364	662.034739	9.615783
8.024093	657.930203	9.620800
8.021676	652.838474	9.625818
8.168418	637.800861	9.630835
7.848164	638.832422	9.635853
7.945532	638.059120	9.640871
8.111644	638.286374	9.645888
7.759278	642.723221	9.650906
7.814299	630.907086	9.655923
8.218793	639.600985	9.660941
8.068242	636.207104	9.665959
8.151975	634.103866	9.670976
7.898528	640.028955	9.675994
8.165920	633.068268	9.681011
8.149877	642.248116	9.686029
7.849093	647.877327	9.691047
8.489561	644.467610	9.696064
7.977271	648.707332	9.701082
7.918754	640.664071	9.706099
8.238981	636.185215	9.711117
8.028215	643.086833	9.716135
7.877311	638.316527	9.721152
7.978381	643.086137	9.726170
8.010682	635.739996	9.731187
7.759452	635.118112	9.736205
7.487108	635.897071	9.741223
7.831694	637.529912	9.746240
7.860311	636.720162	9.751258
7.778064	635.951998	9.756275
8.028509	644.471422	9.761293
8.042158	641.167468	9.766311
8.133886	635.873750	9.771328
7.932223	650.650894	9.776346
7.923327	634.980439	9.781363
7.961495	641.051125	9.786381
8.022256	635.834381	9.791399
8.096901	634.436144	9.796416
8.046371	642.970762	9.801434
8.015431	636.800369	9.806451
7.923879	635.789864	9.811469
7.955526	641.224075	9.816487
8.216093	636.638964	9.821504
8.010460	641.180244	9.826522
7.894648	641.237661	9.831539
7.883731	640.419302	9.836557
7.981110	659.386218	9.841575
8.174918	661.944166	9.846592
8.138696	669.195018	9.851610
8.467032	664.221340	9.856627
8.301732	669.472242	9.861645
7.949137	663.737556	9.866663
8.442183	659.992821	9.871680
8.056459	665.896520	9.876698
8.327016	655.097756	9.881715
8.076381	662.814789	9.886733
7.989990	669.598980	9.891751
8.138040	654.492636	9.896768
7.957647	668.272639	9.901786
8.358629	661.573658	9.906803
8.178302	665.692870	9.911821
7.992604	670.621581	9.916839
8.232392	667.246516	9.921856
8.190131	669.625262	9.926874
8.397462	670.814526	9.931891
8.647847	666.998365	9.936909
8.060517	677.227494	9.941927
8.259278	672.600051	9.946944
8.481837	670.792894	9.951962
8.332840	661.538896	9.956979
8.349241	669.998474	9.961997
7.880965	680.844267	9.967015
8.165868	662.967400	9.972032
8.284418	667.065466	9.977050
8.495689	660.692565	9.982067
8.544694	665.957189	9.987085
8.473587	668.384607	9.992103
8.750419	660.189551	9.997120
8.432950	671.339675	10.002138
8.437385	665.106921	10.007155
8.416357	658.257757	10.012173
8.271741	671.684225	10.017191
8.342554	670.993069	10.022208
8.181444	661.290909	10.027226
8.375119	662.458813	10.032243
8.244753	657.799266	10.037261
8.252185	666.143996	10.042279
8.395682	665.584890	10.047296
8.495434	662.473550	10.052314
8.552223	657.220451	10.057331
8.216988	662.148725	10.062349
8.206030	668.722406	10.067367
8.188024	663.349021	10.072384
8.304537	667.347038	10.077402
8.250804	673.724077	10.082419
8.428673	682.587409	10.087437
8.936360	689.164384	10.092455
8.586940	684.992254	10.097472
8.459971	671.360278	10.102490
8.384534	665.691108	10.107507
8.358118	675.928923	10.112525
8.304904	692.035177	10.117543
8.635340	697.264036	10.122560
8.811570	698.414754	10.127578
8.247130	707.101429	10.132595
8.256358	692.649295	10.137613
8.563829	703.676078	10.142631
8.637638	705.138226	10.147648
8.669292	712.155825	10.152666
8.417788	696.333958	10.157683
8.917880	694.979235	10.162701
8.591786	709.000513	10.167719
8.931989	704.529550	10.172736
8.865892	699.685737	10.177754
8.809957	696.332667	10.182771
8.994103	685.808410	10.187789
8.749280	670.698015	10.192807
8.750689	666.500275	10.197824
8.432468	669.547905	10.202842
8.339347	672.189978	10.207859
8.644100	681.915706	10.212877
8.594618	693.961370	10.217895
8.615367	701.568134	10.222912
8.530248	690.173559	10.227930
8.516906	698.765825	10.232947
8.853728	692.726627	10.237965
8.635488	696.610211	10.242983
8.812108	693.982758	10.248000
8.714319	697.323202	10.253018
8.637517	697.545408	10.258035
8.776896	691.434187	10.263053
8.792431	703.755295	10.268071
8.868174	703.243625	10.273088
8.613994	695.618537	10.278106
8.567809	699.480717	10.283123
8.662693	700.560265	10.288141
8.487696	702.338791	10.293159
8.867955	696.129417	10.298176
8.880642	699.063010	10.303194
8.699256	700.962665	10.308211
8.950153	694.459378	10.313229
8.740906	701.605834	10.318247
8.521064	696.765040	10.323264
8.985545	703.478696	10.328282
8.609408	711.107093	10.333299
9.113877	710.450813	10.338317
9.162721	717.872236	10.343335
9.071976	702.572920	10.348352
9.041701	694.120256	10.353370
8.798988	702.580831	10.358387
9.206329	690.074460	10.363405
8.914848	706.461900	10.368423
9.011889	700.448232	10.373440
9.180394	697.050911	10.378458
8.823706	703.571823	10.383475
8.998084	701.473447	10.388493
8.968761	698.271079	10.393511
9.085569	690.349931	10.398528
8.908235	701.086542	10.403546
8.888429	698.440436	10.408563
9.112086	689.872108	10.413581
8.819809	697.586605	10.418599
8.598107	698.749676	10.423616
9.316694	706.041296	10.428634
9.033141	717.426962	10.433651
8.911271	701.167508	10.438669
9.018193	724.158654	10.443687
9.324087	719.412677	10.448704
9.354816	714.128443	10.453722
9.013560	706.827197	10.458739
9.252942	695.783977	10.463757
8.969751	700.565268	10.468775
9.188587	689.741188	10.473792
9.266677	690.772338	10.478810
9.070632	701.178998	10.483827
9.152891	705.454136	10.488845
8.934159	699.247889	10.493863
9.139776	700.166590	10.498880
9.321719	693.300336	10.503898
9.028686	698.654480	10.508915
8.774918	697.414746	10.513933
8.964394	711.956128	10.518951
9.247160	728.229212	10.523968
9.501483	731.196023	10.528986
9.298472	732.398912	10.534003
9.398163	730.973882	10.539021
9.145829	723.099671	10.544039
9.310413	710.029582	10.549056
9.341141	716.220223	10.554074
9.329479	704.422159	10.559091
9.232738	705.218498	10.564109
9.247589	702.322967	10.569127
9.193998	701.155591	10.574144
9.277925	702.903053	10.579162
9.506409	725.260724	10.584179
9.223627	717.312822	10.589197
9.146129	712.216184	10.594215
8.987005	725.315790	10.599232
8.974809	724.524999	10.604250
8.804375	732.454363	10.609267
9.333143	725.575150	10.614285
9.452769	729.636639	10.619303
9.210148	728.078147	10.624320
9.423821	729.219911	10.629338
9.092122	730.062243	10.634355
9.451848	728.518175	10.639373
9.432422	734.219521	10.644391
9.283788	733.973730	10.649408
9.393986	729.057017	10.654426
9.243738	735.400460	10.659443
9.546945	734.725935	10.664461
9.576994	726.012098	10.669479
9.240666	732.911911	10.674496
9.657789	727.255047	10.679514
9.506010	728.907299	10.684531
9.512609	718.439189	10.689549
9.573325	732.729094	10.694567
9.598622	734.401628	10.699584
9.471470	731.881159	10.704602
9.358376	733.236472	10.709619
9.636070	725.966182	10.714637
9.697093	726.089194	10.719655
9.595691	739.045797	10.724672
9.661055	731.634297	10.729690
9.726390	733.189971	10.734707
9.575522	726.770126	10.739725
9.606455	726.913473	10.744743
9.310827	728.870236	10.749760
9.294882	725.472745	10.754778
9.190909	730.215708	10.759795
9.241324	718.048715	10.764813
9.581747	738.421851	10.769831
9.784974	761.765587	10.774848
9.947128	743.456027	10.779866
9.726754	741.329711	10.784883
9.859802	730.472961	10.789901
10.118432	721.497274	10.794919
9.700701	727.453143	10.799936
9.695430	719.993112	10.804954
9.653434	734.716537	10.809971
9.417365	734.064777	10.814989
9.342633	729.874707	10.820007
9.284076	736.231312	10.825024
9.864817	736.009619	10.830042
9.870042	746.106619	10.835059
10.071743	736.708880	10.840077
9.685579	733.712828	10.845095
9.719328	733.414791	10.850112
9.887500	729.567152	10.855130
9.665744	734.315448	10.860147
9.697557	732.489085	10.865165
9.917744	731.729100	10.870183
9.634370	734.875100	10.875200
9.702162	731.114944	10.880218
9.375121	736.688499	10.885235
9.562210	751.979874	10.890253
10.020019	765.621020	10.895271
9.955644	766.451763	10.900288
10.014799	764.625199	10.905306
9.947958	764.730016	10.910323
9.803300	761.328635	10.915341
10.164139	764.154987	10.920359
9.878329	754.419484	10.925376
9.946581	736.578604	10.930394
9.896493	743.166866	10.935411
9.841987	753.264314	10.940429
9.873165	751.124293	10.945447
9.972592	762.528854	10.950464
10.360977	756.122453	10.955482
9.922442	740.063417	10.960499
9.755043	728.415525	10.965517
10.090614	733.197510	10.970535
9.801802	744.901371	10.975552
10.254215	741.862910	10.980570
9.891482	734.595127	10.985587
9.959770	740.598861	10.990605
10.142152	755.374515	10.995623
10.066965	744.543969	11.000640
10.098301	726.870226	11.005658
9.602077	736.077479	11.010675
9.929772	754.705607	11.015693
10.342572	755.283330	11.020711
10.367811	762.778757	11.025728
10.446513	752.687245	11.030746
10.252386	736.285004	11.035763
9.921451	728.000209	11.040781
10.139907	729.226215	11.045799
9.883157	725.172972	11.050816
9.990836	722.800223	11.055834
9.852249	728.363040	11.060851
10.118322	757.822367	11.065869
10.194950	747.367444	11.070887
10.115664	758.042979	11.075904
10.239159	757.519069	11.080922
10.193936	761.197652	11.085939
10.365946	757.272604	11.090957
10.436637	757.406613	11.095975
10.287008	745.601837	11.100992
10.053384	721.805419	11.106010
10.094925	726.271939	11.111027
10.284872	747.111315	11.116045
10.594252	752.701532	11.121063
10.257896	732.871871	11.126080
10.173990	723.462382	11.131098
10.008457	730.337455	11.136115
10.122778	748.492670	11.141133
10.211286	756.683482	11.146151
10.035700	753.935217	11.151168
10.220604	763.614310	11.156186
10.446544	765.292597	11.161203
10.211280	760.233090	11.166221
10.046790	764.253057	11.171239
9.980098	755.529634	11.176256
10.327949	759.232493	11.181274
10.046332	762.901404	11.186291
10.245986	758.837534	11.191309
10.441379	772.063504	11.196327
10.072022	760.491547	11.201344
10.094918	758.472575	11.206362
9.994643	764.303060	11.211379
10.302192	783.501060	11.216397
10.508646	779.968311	11.221415
10.450307	781.532265	11.226432
10.873060	782.646499	11.231450
10.733973	784.505697	11.236467
10.611094	783.795825	11.241485
10.581987	765.287608	11.246503
10.700687	766.291567	11.251520
10.148533	752.211453	11.256538
10.349442	758.035762	11.261555
10.604158	775.386311	11.266573
10.542735	777.480666	11.271591
10.504925	776.939374	11.276608
10.878103	769.993785	11.281626
10.398949	768.949624	11.286643
10.506188	772.980107	11.291661
10.679183	768.199825	11.296679
10.212343	761.883071	11.301696
10.724074	763.615997	11.306714
10.851733	768.892236	11.311731
10.643077	773.865920	11.316749
10.867500	766.370983	11.321767
10.723194	767.851144	11.326784
10.800143	754.360910	11.331802
10.689822	755.336260	11.336819
10.364148	749.914585	11.341837
10.798273	746.544526	11.346855
10.301021	758.582500	11.351872
10.765330	761.740123	11.356890
10.868410	769.522647	11.361907
10.664067	779.115426	11.366925
10.931000	771.900831	11.371943
10.642932	767.816545	11.376960
10.774030	764.376194	11.381978
10.798333	759.588648	11.386995
10.690046	774.689994	11.392013
11.141652	759.175627	11.397031
10.780460	765.821319	11.402048
10.530069	752.451821	11.407066
10.903464	754.418270	11.412083
10.615558	765.384245	11.417101
10.917038	765.736715	11.422119
10.758368	775.915595	11.427136
10.748332	772.488377	11.432154
10.876813	778.749859	11.437171
10.964761	774.724166	11.442189
11.090733	769.491855	11.447207
10.860278	774.032954	11.452224
10.754448	767.566660	11.457242
10.930889	766.170648	11.462259
11.038027	763.024012	11.467277
11.290182	766.092757	11.472295
10.814365	753.936500	11.477312
10.771136	754.912551	11.482330
10.901222	765.753411	11.487347
10.856513	764.192850	11.492365
11.317861	768.333583	11.497383
10.763395	762.851763	11.502400
11.003926	766.005892	11.507418
11.008332	773.200856	11.512435
10.979554	771.082177	11.517453
10.802125	767.939356	11.522471
11.376310	769.372587	11.527488
11.144309	766.377377	11.532506
11.054135	769.012680	11.537523
10.817458	771.191562	11.542541
10.974397	769.706659	11.547559
10.992652	771.852776	11.552576
11.124711	780.978065	11.557594
11.002200	777.478531	11.562611
11.038306	775.840811	11.567629
11.291342	772.475537	11.572647
10.923352	769.662678	11.577664
11.007774	770.979776	11.582682
11.486145	768.450367	11.587699
11.281986	764.697048	11.592717
11.390729	766.130978	11.597735
11.027908	756.442476	11.602752
11.092760	768.928294	11.607770
11.538498	766.767260	11.612787
11.187224	779.417261	11.617805
11.696809	771.658185	11.622823
11.523666	766.480916	11.627840
10.875386	755.278358	11.632858
11.373475	753.782239	11.637875
11.354594	767.580268	11.642893
11.546556	764.338095	11.647911
11.090289	743.273626	11.652928
11.011486	751.624415	11.657946
11.459045	759.131795	11.662963
11.208623	764.289547	11.667981
11.434702	767.989739	11.672999
11.249357	765.047036	11.678016
11.243388	771.073313	11.683034
11.440965	764.103264	11.688051
11.176051	770.822774	11.693069
11.141230	761.290967	11.698087
11.156235	774.414928	11.703104
11.375627	763.709201	11.708122
11.392519	770.469051	11.713139
11.408215	768.843372	11.718157
11.351914	767.637465	11.723175
10.882213	772.026853	11.728192
11.194450	770.101297	11.733210
11.197785	761.073379	11.738227
10.801204	770.671609	11.743245
11.248550	790.291718	11.748263
11.413463	802.220474	11.753280
11.775226	794.091005	11.758298
11.716392	791.624564	11.763315
11.662673	800.208613	11.768333
11.520377	790.994567	11.773351
11.591047	795.622417	11.778368
11.635103	804.563091	11.783386
11.872035	792.458063	11.788403
11.551503	810.470803	11.793421
11.774580	801.193888	11.798439
11.857918	782.484758	11.803456
11.603732	776.772905	11.808474
11.678124	761.102113	11.813491
11.464912	768.516169	11.818509
11.642021	766.426780	11.823527
11.508220	774.934317	11.828544
11.426607	791.366618	11.833562
11.773971	785.933084	11.838579
11.716707	791.603317	11.843597
11.731172	796.624309	11.848615
11.925451	793.376628	11.853632
11.556656	801.980176	11.858650
12.077508	798.502836	11.863667
11.958818	788.893567	11.868685
11.775582	780.843720	11.873703
11.811042	772.217145	11.878720
11.421195	778.302660	11.883738
11.934927	778.282209	11.888755
11.713097	797.478520	11.893773
11.931254	796.930273	11.898791
11.771910	793.788783	11.903808
11.477306	806.935299	11.908826
11.668908	803.601057	11.913843
11.504222	808.554086	11.918861
11.562318	798.452177	11.923879
11.801310	803.620628	11.928896
11.780455	803.838689	11.933914
11.815254	800.356800	11.938931
11.737480	798.224578	11.943949
11.811339	802.163357	11.948967
12.000028	798.463083	11.953984
11.678622	794.855542	11.959002
11.794096	796.924938	11.964019
12.063117	794.198314	11.969037
11.858834	804.972135	11.974055
11.946242	803.040893	11.979072
12.105917	820.357234	11.984090
12.210771	809.518482	11.989107
11.973795	808.641686	11.994125
11.751525	802.692662	11.999143
11.919368	813.368256	12.004160
12.422262	821.806609	12.009178
12.272253	810.575831	12.014195
12.174539	815.711462	12.019213
12.491616	801.357455	12.024231
12.601382	798.055267	12.029248
12.071993	800.780232	12.034266
12.663944	787.093279	12.039283
12.404138	797.862116	12.044301
12.362670	792.664215	12.049319
12.602479	788.629119	12.054336
12.408690	792.425612	12.059354
12.642049	785.733864	12.064371
12.187984	773.437383	12.069389
12.018003	756.776018	12.074407
12.076188	763.749880	12.079424
11.700387	767.990261	12.084442
12.129065	785.306111	12.089459
12.260583	800.671693	12.094477
12.159828	797.985828	12.099495
12.501003	788.548822	12.104512
12.322829	794.179632	12.109530
12.103528	785.323203	12.114547
12.062309	791.858052	12.119565
11.993888	791.170656	12.124583
12.092098	793.905077	12.129600
12.198746	797.238460	12.134618
12.068210	797.292410	12.139635
12.126061	795.529834	12.144653
12.205700	793.897501	12.149671
12.232881	796.859026	12.154688
12.072119	801.602360	12.159706
12.440164	812.636119	12.164723
12.215687	820.228040	12.169741
12.195242	813.451542	12.174759
12.276259	821.840467	12.179776
12.193473	829.532938	12.184794
12.323489	826.140782	12.189811
12.598109	828.954259	12.194829
12.477269	819.415796	12.199847
12.607729	817.900235	12.204864
12.534137	820.266280	12.209882
12.601768	821.850321	12.214899
12.586668	829.283173	12.219917
12.466354	826.276544	12.224935
12.585346	822.062244	12.229952
12.490947	837.789270	12.234970
12.837449	832.072413	12.239987
12.564440	824.923975	12.245005
12.277009	821.781642	12.250023
12.802103	819.847211	12.255040
12.672223	824.961402	12.260058
12.569756	825.507921	12.265075
12.751566	822.990604	12.270093
12.529637	827.357482	12.275111
12.586640	825.923371	12.280128
12.176613	836.449408	12.285146
12.674767	827.213538	12.290163
12.529804	840.204209	12.295181
12.357262	837.939256	12.300199
12.766378	831.678596	12.305216
13.015683	849.584819	12.310234
12.977426	836.654899	12.315251
12.472987	835.352730	12.320269
12.936412	835.397693	12.325287
12.817284	821.671771	12.330304
12.872342	829.241423	12.335322
12.829233	813.463664	12.340339
12.752586	827.151240	12.345357
12.670300	830.580872	12.350375
13.218580	842.593808	12.355392
12.696352	837.014502	12.360410
12.712598	832.962086	12.365427
13.191578	843.219272	12.370445
13.265583	836.103126	12.375463
13.062350	814.690378	12.380480
12.687813	833.582904	12.385498
12.705018	824.573124	12.390515
13.037995	825.964417	12.395533
13.196223	833.684301	12.400551
12.961417	826.012241	12.405568
12.768248	831.099120	12.410586
12.940483	842.133437	12.415603
13.408965	840.254044	12.420621
12.899616	836.829575	12.425639
12.918065	820.835327	12.430656
12.940878	835.831958	12.435674
13.184906	834.329085	12.440691
13.457730	842.732715	12.445709
12.913288	837.986569	12.450727
12.857645	820.487350	12.455744
12.964970	832.355590	12.460762
13.216291	840.834823	12.465779
13.351255	849.704174	12.470797
12.884635	855.153647	12.475815
13.065370	855.221406	12.480832
13.052458	847.864936	12.485850
13.048193	848.758560	12.490867
13.523630	848.134247	12.495885
13.171165	847.604901	12.500903
13.454909	846.793444	12.505920
13.264933	851.182988	12.510938
13.247573	846.105086	12.515955
13.602743	845.422346	12.520973
13.329944	830.623103	12.525991
13.477146	812.028158	12.531008
13.173789	821.860182	12.536026
13.493982	818.721953	12.541043
13.247085	813.436415	12.546061
13.188184	813.300954	12.551079
13.409567	809.142139	12.556096
13.231780	816.415714	12.561114
13.199017	819.698569	12.566131
13.502303	832.616978	12.571149
13.394995	846.870247	12.576167
13.730646	836.564095	12.581184
13.379403	828.128287	12.586202
13.300794	824.392744	12.591219
13.560651	818.026891	12.596237
13.227482	818.854511	12.601255
13.350870	830.604348	12.606272
13.835427	841.975509	12.611290
13.670095	838.025596	12.616307
13.750813	818.824756	12.621325
13.249824	823.764584	12.626343
13.373537	808.572558	12.631360
13.448999	829.203061	12.636378
13.364294	841.396397	12.641395
13.623475	839.560717	12.646413
13.441061	844.921396	12.651431
13.439504	843.305653	12.656448
13.680076	842.259232	12.661466
13.701570	844.915031	12.666483
13.713284	836.576982	12.671501
13.518184	848.729945	12.676519
13.533957	847.306991	12.681536
13.369463	844.955670	12.686554
13.682250	845.072425	12.691571
13.821421	842.470045	12.696589
13.587476	850.063547	12.701607
13.625110	844.517116	12.706624
13.624479	844.366100	12.711642
13.499126	848.676443	12.716659
14.017964	845.391543	12.721677
13.527743	845.805036	12.726695
13.823640	840.920921	12.731712
13.702547	845.468734	12.736730
13.733280	851.972010	12.741747
13.816889	839.544320	12.746765
13.616435	846.425621	12.751783
13.570882	849.329912	12.756800
13.736150	858.811146	12.761818
13.773553	872.097220	12.766835
14.368763	868.141829	12.771853
14.204780	862.464612	12.776871
14.138512	848.953130	12.781888
14.257564	841.142158	12.786906
13.818750	846.522460	12.791923
14.088937	839.484845	12.796941
13.900382	849.049464	12.801959
13.751857	835.568542	12.806976
14.427348	836.806276	12.811994
13.889435	843.196633	12.817011
14.480233	838.275891	12.822029
14.126821	835.354706	12.827047
14.147084	826.172774	12.832064
14.185985	839.421172	12.837082
13.815606	841.493469	12.842099
14.128102	833.130025	12.847117
14.085417	843.160223	12.852135
13.958812	840.123926	12.857152
14.027386	840.280331	12.862170
13.765044	837.999542	12.867187
14.004939	834.156142	12.872205
14.165474	848.578042	12.877223
14.063133	847.658084	12.882240
14.111636	841.576024	12.887258
13.852863	841.217374	12.892275
14.419433	857.072754	12.897293
14.418347	854.424310	12.902311
13.809752	849.041573	12.907328
13.912969	866.816503	12.912346
14.148869	867.751853	12.917363
14.289987	864.748774	12.922381
14.209011	877.027736	12.927399
14.147250	874.213754	12.932416
14.747470	872.548358	12.937434
14.113667	873.489932	12.942451
14.540379	865.112675	12.947469
14.591698	866.557304	12.952487
14.410218	872.094993	12.957504
14.809556	873.009579	12.962522
14.560061	880.260807	12.967539
14.655664	869.419609	12.972557
14.713285	873.105597	12.977575
14.670848	858.858309	12.982592
14.593892	841.463376	12.987610
14.423657	851.633986	12.992627
14.575072	844.183381	12.997645
14.321412	855.196896	13.002663
14.078603	838.297516	13.007680
14.642079	848.961951	13.012698
14.786478	869.988947	13.017715
14.861364	857.076493	13.022733
14.627154	858.057798	13.027751
14.519391	845.275986	13.032768
14.759437	842.160473	13.037786
14.274305	852.069462	13.042803
14.600069	836.988432	13.047821
14.406251	849.747450	13.052839
14.811826	861.925756	13.057856
14.949954	859.630223	13.062874
14.787771	853.457067	13.067891
14.792586	839.319289	13.072909
14.339630	843.179180	13.077927
14.559309	851.165654	13.082944
14.964247	862.396873	13.087962
14.814583	871.035036	13.092979
15.004621	864.339404	13.097997
14.925616	858.015867	13.103015
14.716174	846.326424	13.108032
14.820728	842.956590	13.113050
14.930902	839.357098	13.118067
14.740362	836.951433	13.123085
14.857866	841.366827	13.128103
14.657260	854.530101	13.133120
14.981100	858.937711	13.138138
14.915866	861.703932	13.143155
14.763813	857.391204	13.148173
15.021778	859.630704	13.153191
14.907535	864.315176	13.158208
14.684688	862.419948	13.163226
14.920745	869.492744	13.168243
15.227414	862.312864	13.173261
15.382688	862.401373	13.178279
14.948277	852.181780	13.183296
14.861011	843.077876	13.188314
14.661229	862.323763	13.193331
15.043761	866.714570	13.198349
15.077726	875.012108	13.203367
14.963555	874.807063	13.208384
15.026078	865.967697	13.213402
14.919140	868.823498	13.218419
14.689103	868.262461	13.223437
14.866733	869.531852	13.228455
14.932074	860.884138	13.233472
15.281491	860.637366	13.238490
15.065761	861.661278	13.243507
15.137983	862.346580	13.248525
14.858022	864.131088	13.253543
14.945714	859.859365	13.258560
15.377090	868.958371	13.263578
15.271147	882.416607	13.268595
14.910030	879.057342	13.273613
15.274346	888.740269	13.278631
15.045559	892.021348	13.283648
15.478865	883.537483	13.288666
15.488358	886.211024	13.293683
15.417762	889.453310	13.298701
15.390314	898.386589	13.303719
15.497583	888.991010	13.308736
15.552606	881.316991	13.313754
15.401732	887.644853	13.318771
15.783732	875.953905	13.323789
15.207145	870.824115	13.328807
15.206841	867.309442	13.333824
15.390047	873.835115	13.338842
15.467173	890.671923	13.343859
15.617989	887.317252	13.348877
15.752414	898.599983	13.353895
15.567754	880.273283	13.358912
15.587835	857.981808	13.363930
15.452726	869.105223	13.368947
15.692365	858.960616	13.373965
15.665263	857.169977	13.378983
15.454409	856.223895	13.384000
15.394604	848.214201	13.389018
15.527129	870.662378	13.394035
15.362012	876.581592	13.399053
16.079266	870.639559	13.404071
15.746560	890.196452	13.409088
15.983405	868.033235	13.414106
15.499201	855.180291	13.419123
15.431613	864.381994	13.424141
15.557235	877.529849	13.429159
15.599050	882.538860	13.434176
15.861999	873.406474	13.439194
15.825109	883.577463	13.444211
15.736007	877.255984	13.449229
15.798032	882.554941	13.454247
15.864596	887.670874	13.459264
16.009923	882.753807	13.464282
15.326883	891.050008	13.469299
15.848128	884.445186	13.474317
15.759228	882.277395	13.479335
15.315056	887.484591	13.484352
15.790066	876.998652	13.489370
15.760060	883.113987	13.494387
15.752299	876.558578	13.499405
15.847761	877.723865	13.504423
15.621782	888.858404	13.509440
16.143805	885.856025	13.514458
15.741242	883.467352	13.519475
15.719462	885.723258	13.524493
16.187679	893.498529	13.529511
16.125798	899.471519	13.534528
16.161312	904.785109	13.539546
16.142257	904.824537	13.544563
16.281115	896.645315	13.549581
16.406271	883.412719	13.554599
15.914364	878.085056	13.559616
16.249679	874.988011	13.564634
16.186575	879.307739	13.569651
16.028754	874.171201	13.574669
16.105793	882.854504	13.579687
16.032422	876.916620	13.584704
16.231582	883.171166	13.589722
16.408332	895.655486	13.594739
15.954812	889.210101	13.599757
16.536598	888.394564	13.604775
16.234431	878.569569	13.609792
16.437530	867.383817	13.614810
16.093010	881.258310	13.619827
16.138113	871.725404	13.624845
16.336635	880.539763	13.629863
16.401633	895.038548	13.634880
16.568023	892.309218	13.639898
16.532267	895.663840	13.644915
16.191895	887.000620	13.649933
16.478609	883.607700	13.654951
16.366226	888.020625	13.659968
16.597184	893.899062	13.664986
16.608039	888.136981	13.670003
16.082475	883.134165	13.675021
16.835492	886.429038	13.680039
16.340117	882.849495	13.685056
16.275725	884.021175	13.690074
16.438479	890.623860	13.695091
16.469865	895.181476	13.700109
16.851243	892.721256	13.705127
16.594979	907.994078	13.710144
16.932384	898.863914	13.715162
16.869092	889.764280	13.720179
16.456658	875.241646	13.725197
16.356211	879.415203	13.730215
16.474271	891.593900	13.735232
16.572756	891.046570	13.740250
16.530287	893.419283	13.745267
16.531550	895.817037	13.750285
16.747712	889.696567	13.755303
16.637830	894.143329	13.760320
16.751964	882.952220	13.765338
16.708642	888.529634	13.770355
16.527256	892.328034	13.775373
16.862333	895.328353	13.780391
16.761697	903.293882	13.785408
16.732675	894.216128	13.790426
16.528910	894.636517	13.795443
16.644529	905.095637	13.800461
16.594257	890.291377	13.805479
16.991891	898.892864	13.810496
16.813030	899.184726	13.815514
16.617690	897.355408	13.820531
16.500159	917.536121	13.825549
17.263045	917.989744	13.830567
17.042868	938.814222	13.835584
16.849546	933.928019	13.840602
17.001272	937.801186	13.845619
17.358731	935.890957	13.850637
17.405900	923.228301	13.855655
17.248358	908.744921	13.860672
17.344636	893.059348	13.865690
17.362535	897.020410	13.870707
16.957947	896.419381	13.875725
17.041921	890.453469	13.880743
17.143274	894.165290	13.885760
17.343911	889.260715	13.890778
17.197125	888.437086	13.895795
17.114038	889.571706	13.900813
17.606626	889.745298	13.905831
16.995006	897.851733	13.910848
17.466390	885.857015	13.915866
17.570536	883.107286	13.920883
17.082922	890.709743	13.925901
17.255427	887.001105	13.930919
17.228538	895.086302	13.935936
17.193733	894.450418	13.940954
17.094123	885.883939	13.945971
17.097781	894.531764	13.950989
17.348725	881.920435	13.956007
16.965506	893.558154	13.961024
17.185533	902.615409	13.966042
17.541354	914.024476	13.971059
17.423231	919.803647	13.976077
17.708379	913.050515	13.981095
17.512983	919.272382	13.986112
17.455495	913.169657	13.991130
17.418765	908.439807	13.996147
17.285583	918.553146	14.001165
17.500740	917.780207	14.006183
17.241949	927.319892	14.011200
17.430883	924.849803	14.016218
17.500933	916.717001	14.021235
17.128014	921.034895	14.026253
17.801924	908.435786	14.031271
17.524033	921.737105	14.036288
17.869928	920.461438	14.041306
17.630216	912.564962	14.046323
17.742649	925.303645	14.051341
17.934767	911.317848	14.056359
17.849222	930.516952	14.061376
17.450209	926.885618	14.066394
17.593807	916.943088	14.071411
17.533811	924.200358	14.076429
17.639734	923.856903	14.081447
17.509567	927.490145	14.086464
17.546691	920.804456	14.091482
17.876017	927.104785	14.096499
17.678833	926.156828	14.101517
17.846264	936.192450	14.106535
18.340872	948.286794	14.111552
17.878338	929.040740	14.116570
18.260134	918.942237	14.121587
17.823030	914.385369	14.126605
18.114847	905.176927	14.131623
18.078990	911.871954	14.136640
18.005758	914.964296	14.141658
17.982878	911.238008	14.146675
18.020054	918.814601	14.151693
18.027068	912.180356	14.156711
17.947123	911.102362	14.161728
18.054860	914.385593	14.166746
18.178612	911.248380	14.171763
18.104599	912.018525	14.176781
18.209998	910.239796	14.181799
17.981258	914.080686	14.186816
18.174958	924.148957	14.191834
18.033656	912.145834	14.196851
17.971111	920.716058	14.201869
18.202597	922.929638	14.206887
17.861073	929.710325	14.211904
17.847897	938.688112	14.216922
18.299312	936.556035	14.221939
18.237668	941.531019	14.226957
18.378280	939.937392	14.231975
18.465374	944.541307	14.236992
18.299831	947.277305	14.242010
18.605515	941.598268	14.247027
18.344113	950.311274	14.252045
18.472174	928.854926	14.257063
18.382110	940.878370	14.262080
18.191035	937.684233	14.267098
18.396902	936.011693	14.272115
18.445045	945.137197	14.277133
18.391449	934.410811	14.282151
18.686539	938.092137	14.287168
18.607112	942.922041	14.292186
18.599730	936.109470	14.297203
18.346959	936.206494	14.302221
18.770418	936.280516	14.307239
18.628424	937.753224	14.312256
18.511700	936.313226	14.317274
18.622354	932.308928	14.322291
18.424376	941.485026	14.327309
18.295137	928.731503	14.332327
18.411152	944.647801	14.337344
18.216297	945.269068	14.342362
18.770730	938.106786	14.347379
18.802898	943.711875	14.352397
18.520142	941.438386	14.357415
18.638115	942.278313	14.362432
18.407246	947.749407	14.367450
18.774619	956.956304	14.372467
19.148970	975.349818	14.377485
19.299833	954.082171	14.382503
18.690434	942.243145	14.387520
18.400240	935.622278	14.392538
19.162206	951.824124	14.397555
18.823744	967.346431	14.402573
18.797293	959.151244	14.407591
19.063185	965.644368	14.412608
18.676104	962.731488	14.417626
18.850905	959.689351	14.422643
18.968683	966.880592	14.427661
19.112942	951.157489	14.432679
19.064606	962.099681	14.437696
18.792134	965.275809	14.442714
19.032524	958.143079	14.447731
18.915840	969.070610	14.452749
19.082781	958.497839	14.457767
19.323250	963.994431	14.462784
19.171156	962.922475	14.467802
19.227669	959.048389	14.472819
19.149444	967.793669	14.477837
19.025574	960.607086	14.482855
19.206780	957.740652	14.487872
19.282177	960.947362	14.492890
19.418118	957.827805	14.497907
19.359768	962.272353	14.502925
19.435297	958.584874	14.507943
19.374396	947.136888	14.512960
19.406264	953.195946	14.517978
19.072756	954.837369	14.522995
19.105746	960.790737	14.528013
19.090718	949.947329	14.533031
19.280596	959.436361	14.538048
19.217766	954.734046	14.543066
19.154304	947.802809	14.548083
19.156357	955.058480	14.553101
19.526672	955.347985	14.558119
19.708082	950.898128	14.563136
19.150624	954.687559	14.568154
19.285372	957.518316	14.573171
19.465872	968.150585	14.578189
19.910933	978.202465	14.583207
19.840875	960.550362	14.588224
19.446637	956.050554	14.593242
19.544380	943.564538	14.598259
19.569463	942.058935	14.603277
19.419405	962.759635	14.608295
19.818240	966.367100	14.613312
19.651150	972.400450	14.618330
20.340017	965.517850	14.623347
19.945141	956.884874	14.628365
19.698656	947.453746	14.633383
19.787137	940.078474	14.638400
19.610069	945.614672	14.643418
19.702179	951.543680	14.648435
19.816390	955.534476	14.653453
19.784214	951.871919	14.658471
19.541083	951.699643	14.663488
19.592413	968.744734	14.668506
19.960625	968.717280	14.673523
20.140645	974.978182	14.678541
20.285452	984.559334	14.683559
20.440380	969.244664	14.688576
19.890107	965.649390	14.693594
20.044886	946.099530	14.698611
20.147031	945.427189	14.703629
20.119887	941.150444	14.708647
20.009630	938.195668	14.713664
19.867350	939.463316	14.718682
19.884628	935.760292	14.723699
19.836867	948.699921	14.728717
20.222917	954.788123	14.733735
20.485517	957.348902	14.738752
20.204502	966.134846	14.743770
20.405148	959.629140	14.748787
20.463836	951.822596	14.753805
19.952373	945.833611	14.758823
20.506385	935.811693	14.763840
20.424191	932.085773	14.768858
20.271197	937.475862	14.773875
19.967436	936.429416	14.778893
19.989876	952.950559	14.783911
20.413056	953.771049	14.788928
20.210422	964.263224	14.793946
20.389594	953.644732	14.798963
20.126493	961.103359	14.803981
20.250537	962.306831	14.808999
20.390824	956.745723	14.814016
20.177381	968.317987	14.819034
20.297595	967.995786	14.824051
20.409596	959.083217	14.829069
20.230289	968.967623	14.834087
20.352077	962.754882	14.839104
20.215018	963.122890	14.844122
20.511511	964.044276	14.849139
20.709920	979.730835	14.854157
20.464619	991.450117	14.859175
20.644936	985.790249	14.864192
20.711788	997.163371	14.869210
20.559815	981.247962	14.874227
20.440102	987.201823	14.879245
20.725901	982.977181	14.884263
21.050913	986.580339	14.889280
20.780184	990.298679	14.894298
20.683979	988.997398	14.899315
20.827448	995.826540	14.904333
20.672014	995.033863	14.909351
20.772393	982.379277	14.914368
20.464287	992.375966	14.919386
20.811654	988.240335	14.924403
21.292075	985.832595	14.929421
21.053259	986.132418	14.934439
21.103541	989.468877	14.939456
21.079836	992.727829	14.944474
21.066900	983.814674	14.949491
21.212052	990.323471	14.954509
20.935260	993.666848	14.959527
21.336821	985.818079	14.964544
21.124138	986.994636	14.969562
21.489313	963.209317	14.974579
20.938264	956.643052	14.979597
20.897377	952.155598	14.984615
21.235505	954.371602	14.989632
20.755305	966.021498	14.994650
21.236007	971.156282	14.999667
21.429778	979.848262	15.004685
21.342406	982.373693	15.009703
21.504612	970.054532	15.014720
21.129268	955.088299	15.019738
21.299632	960.683896	15.024755
21.252289	961.516553	15.029773
20.967838	979.012514	15.034791
21.223683	977.469090	15.039808
21.189625	984.941375	15.044826
21.427322	981.894330	15.049843
21.347705	971.713935	15.054861
21.123372	986.716993	15.059879
21.206788	979.368524	15.064896
21.055211	985.798113	15.069914
21.223864	983.469949	15.074931
21.128963	978.917025	15.079949
21.361018	990.791898	15.084967
21.638178	993.922688	15.089984
21.454343	1014.170409	15.095002
21.443341	1011.887343	15.100019
21.731477	1008.584708	15.105037
21.623442	1008.635720	15.110055
21.611370	1009.247194	15.115072
21.656499	1000.314573	15.120090
21.342523	1008.685938	15.125107
21.601761	995.946377	15.130125
21.533588	1002.525540	15.135143
22.162286	1006.191799	15.140160
21.618503	1010.602573	15.145178
21.897215	1010.106101	15.150195
21.900302	1005.914486	15.155213
21.486690	1007.180220	15.160231
21.835295	998.303250	15.165248
21.998840	1006.584914	15.170266
21.781189	1003.495946	15.175283
21.871298	1005.765625	15.180301
21.804322	1009.892338	15.185319
21.759084	1008.172004	15.190336
21.709006	1006.137524	15.195354
21.856947	1012.245886	15.200371
22.137703	1006.741025	15.205389
21.675292	1011.832390	15.210407
21.925161	1025.081052	15.215424
22.024115	1036.256377	15.220442
22.108203	1034.263455	15.225459
22.214910	1034.011596	15.230477
22.387024	1032.496992	15.235495
22.806833	1019.313518	15.240512
22.745004	1014.367722	15.245530
22.250842	999.681345	15.250547
22.475494	996.004989	15.255565
22.194311	997.712159	15.260583
22.273894	993.303559	15.265600
22.353722	992.028639	15.270618
22.359493	998.749487	15.275635
22.083929	991.305343	15.280653
22.314152	997.035130	15.285671
22.667245	991.241537	15.290688
22.319699	994.383647	15.295706
22.410209	999.551556	15.300723
22.678938	993.786497	15.305741
22.554366	997.541265	15.310759
22.414248	988.518070	15.315776
22.288623	995.460665	15.320794
22.546199	995.440507	15.325811
22.411977	993.738059	15.330829
22.108316	998.907459	15.335847
22.782997	1003.973128	15.340864
22.759333	1009.083570	15.345882
22.524138	1010.265826	15.350899
23.012141	1008.806786	15.355917
22.739845	1002.145133	15.360935
22.590568	1002.219902	15.365952
22.733931	997.739325	15.370970
22.492063	1003.614212	15.375987
22.592285	1017.332509	15.381005
22.679081	1026.851643	15.386023
22.797566	1026.601772	15.391040
22.978876	1022.946366	15.396058
22.675743	1025.722088	15.401075
22.740118	1021.409302	15.406093
22.609074	1030.189346	15.411111
23.017207	1028.961237	15.416128
22.910978	1020.537111	15.421146
22.634307	1028.154310	15.426163
22.964396	1019.929579	15.431181
22.821246	1025.378696	15.436199
22.743362	1017.350649	15.441216
23.110046	1026.660059	15.446234
23.054471	1028.172795	15.451251
23.201863	1014.082111	15.456269
22.594982	1027.405320	15.461287
23.190666	1042.537205	15.466304
23.268968	1050.586955	15.471322
23.120296	1043.369796	15.476339
23.251393	1047.912522	15.481357
23.239920	1053.990999	15.486375
23.510736	1052.395485	15.491392
23.777805	1046.599975	15.496410
23.542544	1032.263988	15.501427
23.436810	1015.442105	15.506445
23.185612	1013.144877	15.511463
23.293598	1017.648508	15.516480
23.234523	1023.826585	15.521498
23.645325	1035.766379	15.526515
23.362011	1014.566212	15.531533
22.817545	1025.423284	15.536551
23.264645	1040.047509	15.541568
23.191868	1047.227429	15.546586
23.290098	1042.929108	15.551603
23.733957	1039.839254	15.556621
23.482240	1041.833663	15.561639
23.702188	1042.737022	15.566656
23.780080	1037.386209	15.571674
23.967814	1031.966030	15.576691
24.535025	1033.197697	15.581709
24.182541	1047.960628	15.586727
24.018850	1019.199223	15.591744
24.145810	1004.198585	15.596762
23.901192	1007.544511	15.601779
23.868833	1007.025142	15.606797
24.114682	1009.797356	15.611815
24.039081	1004.684166	15.616832
24.011633	1004.052965	15.621850
23.883184	1001.888163	15.626867
24.349390	994.579842	15.631885
24.047271	1008.244285	15.636903
24.240713	1005.966736	15.641920
24.336076	1002.827513	15.646938
23.675065	1009.882780	15.651955
23.929535	993.537867	15.656973
24.068371	1000.059525	15.661991
23.766305	994.522834	15.667008
23.856414	996.793298	15.672026
23.670886	991.559738	15.677043
24.308380	994.339144	15.682061
24.228068	1000.504586	15.687079
24.064185	1006.453958	15.692096
24.215092	1001.061541	15.697114
23.909083	1006.596671	15.702131
23.995093	997.550201	15.707149
24.012917	1003.857262	15.712167
24.095375	1015.808105	15.717184
24.131855	1033.365154	15.722202
24.532638	1036.906174	15.727219
24.281712	1027.819418	15.732237
24.154586	1029.066847	15.737255
24.241416	1037.263204	15.742272
24.310866	1029.086744	15.747290
23.895082	1036.821072	15.752307
24.364586	1027.702422	15.757325
24.490067	1031.833492	15.762343
24.377505	1036.828354	15.767360
24.319909	1028.016659	15.772378
24.080562	1030.070040	15.777395
24.451433	1041.325141	15.782413
24.297146	1059.822826	15.787431
24.531592	1057.245577	15.792448
24.918187	1061.250745	15.797466
24.819699	1063.086325	15.802483
24.891125	1059.884127	15.807501
24.903608	1063.447325	15.812519
24.575582	1067.603501	15.817536
25.164829	1063.815185	15.822554
25.065932	1055.433919	15.827571
25.368578	1060.113196	15.832589
25.438147	1051.439087	15.837607
24.813411	1038.582094	15.842624
25.233619	1030.221968	15.847642
25.155629	1025.539463	15.852659
24.895087	1018.911681	15.857677
24.864806	1024.803506	15.862695
25.277182	1024.166009	15.867712
24.961852	1018.326794	15.872730
24.897439	1034.503761	15.877747
24.755909	1024.430822	15.882765
24.801702	1021.186029	15.887783
24.833160	1029.461625	15.892800
24.926423	1049.262739	15.897818
24.897250	1054.433162	15.902835
25.283465	1059.334025	15.907853
25.328285	1062.661562	15.912871
25.435228	1057.274044	15.917888
25.442020	1057.988298	15.922906
25.236085	1057.218546	15.927923
25.269433	1059.125599	15.932941
25.323978	1051.224813	15.937959
25.365788	1053.058419	15.942976
25.699126	1048.203866	15.947994
25.325017	1053.977444	15.953011
25.202042	1051.166479	15.958029
25.307373	1053.638754	15.963047
25.255277	1052.747470	15.968064
25.741512	1051.111168	15.973082
25.356710	1054.283867	15.978099
25.454932	1051.275652	15.983117
25.657983	1062.806185	15.988135
25.428451	1052.215538	15.993152
25.427449	1050.076867	15.998170
25.555509	1058.269164	16.003187
25.614554	1058.210229	16.008205
25.536347	1049.394062	16.013223
25.405254	1069.399273	16.018240
25.895744	1065.140322	16.023258
25.909969	1072.437731	16.028275
25.885797	1071.624496	16.033293
25.881500	1072.248071	16.038311
25.664812	1081.076969	16.043328
25.981804	1076.132204	16.048346
25.714250	1076.939522	16.053363
25.979906	1067.552646	16.058381
25.747313	1075.939704	16.063399
26.009416	1076.079421	16.068416
26.055229	1067.705288	16.073434
25.667719	1078.803720	16.078451
26.119935	1068.161197	16.083469
26.340148	1062.613587	16.088487
25.679071	1072.306190	16.093504
26.249113	1067.028199	16.098522
26.268481	1070.994574	16.103539
26.108689	1071.379734	16.108557
26.252582	1068.012391	16.113575
26.148499	1066.213215	16.118592
26.523039	1073.828508	16.123610
26.169383	1074.426470	16.128627
26.205281	1065.139054	16.133645
26.291044	1065.073727	16.138663
26.259748	1075.372258	16.143680
26.322437	1071.385315	16.148698
26.283514	1082.085885	16.153715
26.388657	1095.044018	16.158733
26.696305	1097.246588	16.163751
26.783318	1105.486255	16.168768
26.585670	1082.597068	16.173786
26.506618	1074.423915	16.178803
26.685113	1091.292973	16.183821
26.916250	1084.173135	16.188839
26.213542	1081.090456	16.193856
26.741951	1083.441108	16.198874
26.687484	1100.801096	16.203891
26.773367	1098.322454	16.208909
26.975234	1089.022503	16.213927
26.663514	1085.356991	16.218944
26.689894	1084.118078	16.223962
26.847501	1094.710133	16.228979
26.673752	1099.349807	16.233997
26.899667	1102.691853	16.239015
26.622723	1103.701114	16.244032
26.851828	1102.848694	16.249050
26.901673	1092.189320	16.254067
26.608431	1092.396978	16.259085
26.991373	1097.162967	16.264103
26.780568	1099.306902	16.269120
27.044747	1090.567083	16.274138
26.904938	1100.830452	16.279155
26.994155	1097.761909	16.284173
27.079858	1103.207016	16.289191
26.674259	1108.883865	16.294208
26.773371	1099.428094	16.299226
27.171407	1120.843338	16.304243
27.100632	1125.624624	16.309261
27.491322	1125.983593	16.314279
27.261512	1126.964578	16.319296
27.700580	1120.633098	16.324314
27.528602	1123.226103	16.329331
27.281821	1129.843556	16.334349
27.892250	1123.613617	16.339367
27.401796	1105.517198	16.344384
27.289917	1091.946129	16.349402
27.083426	1103.808276	16.354419
27.490137	1115.905891	16.359437
27.875717	1110.941490	16.364455
27.532208	1126.117560	16.369472
27.546811	1122.962552	16.374490
27.416275	1122.999180	16.379507
27.492001	1122.526081	16.384525
27.731962	1115.105959	16.389543
27.572618	1135.524974	16.394560
27.676774	1124.802649	16.399578
27.536087	1123.327626	16.404595
27.859570	1122.258011	16.409613
27.994484	1111.144002	16.414631
27.843060	1128.167332	16.419648
27.732084	1115.459054	16.424666
27.621240	1122.629171	16.429683
27.900274	1120.066182	16.434701
28.070193	1115.193000	16.439719
28.013314	1113.578909	16.444736
27.951720	1113.692307	16.449754
28.020765	1114.735613	16.454771
28.238079	1111.991908	16.459789
28.284291	1109.069062	16.464807
27.946650	1117.584162	16.469824
28.402146	1108.672895	16.474842
28.452831	1103.752139	16.479859
28.130459	1121.959238	16.484877
28.035150	1107.183881	16.489895
27.718297	1114.479047	16.494912
27.692018	1112.076847	16.499930
27.971413	1118.846136	16.504947
28.415726	1130.703687	16.509965
28.747730	1135.846614	16.514983
28.245588	1136.092800	16.520000
28.340926	1136.818773	16.525018
28.723843	1144.815771	16.530035
28.323038	1142.585814	16.535053
28.496256	1129.210016	16.540071
28.654064	1143.643668	16.545088
28.553266	1130.172695	16.550106
28.458322	1128.867256	16.555123
28.572547	1144.001408	16.560141
28.657183	1135.446406	16.565159
28.501087	1141.700434	16.570176
28.744397	1133.989208	16.575194
28.785996	1138.373951	16.580211
28.570889	1142.572470	16.585229
28.827704	1133.838570	16.590247
28.392027	1137.915348	16.595264
28.564259	1136.548740	16.600282
28.417656	1135.431770	16.605299
28.342402	1143.494003	16.610317
28.543446	1137.354680	16.615335
28.566307	1143.998355	16.620352
28.847631	1158.045439	16.625370
28.902659	1162.800394	16.630387
28.665742	1164.667568	16.635405
29.041401	1156.890716	16.640423
28.715972	1161.561429	16.645440
28.992331	1156.680845	16.650458
28.983399	1156.358766	16.655475
29.184321	1166.023257	16.660493
28.974101	1166.639202	16.665511
29.088965	1167.101322	16.670528
29.301855	1162.457616	16.675546
29.225190	1155.126516	16.680563
29.324185	1163.697684	16.685581
28.840325	1161.738555	16.690599
29.169221	1177.647008	16.695616
29.515354	1180.827438	16.700634
29.610014	1178.118991	16.705651
29.607762	1180.106361	16.710669
29.953397	1166.831504	16.715687
29.878433	1165.847546	16.720704
29.821222	1154.537374	16.725722
29.573492	1147.608606	16.730739
29.532095	1159.824154	16.735757
29.886323	1143.091319	16.740775
29.954735	1145.733889	16.745792
30.206395	1151.188540	16.750810
30.024765	1151.191504	16.755827
29.945172	1150.846874	16.760845
29.864242	1142.648012	16.765863
29.784914	1141.264005	16.770880
29.808945	1145.178841	16.775898
30.134290	1141.930645	16.780915
30.089501	1144.626604	16.785933
30.002094	1139.866886	16.790951
30.020053	1146.926320	16.795968
30.057630	1149.757849	16.800986
30.087924	1129.521701	16.806003
30.020658	1119.423019	16.811021
29.959780	1118.769397	16.816039
29.782465	1129.125605	16.821056
29.837675	1142.528251	16.826074
30.244605	1131.039276	16.831091
30.091500	1142.958752	16.836109
30.268118	1145.467268	16.841127
30.358484	1155.640593	16.846144
30.262614	1143.943535	16.851162
30.433826	1134.565565	16.856179
30.087941	1141.223054	16.861197
29.804681	1142.870742	16.866215
29.904206	1149.683608	16.871232
29.925865	1148.587199	16.876250
30.183272	1151.070134	16.881267
30.183420	1166.949944	16.886285
30.289413	1168.105242	16.891303
30.520438	1176.780930	16.896320
30.399595	1184.117292	16.901338
30.717416	1177.292103	16.906355
30.210388	1183.658586	16.911373
30.260044	1167.869434	16.916391
30.686356	1171.951517	16.921408
30.658617	1169.529471	16.926426
30.578273	1172.872640	16.931443
30.471776	1181.102265	16.936461
30.741761	1168.034416	16.941479
30.975597	1169.264606	16.946496
31.034401	1166.067626	16.951514
30.847363	1163.427872	16.956531
30.753088	1173.535722	16.961549
30.945312	1169.291486	16.966567
30.952145	1170.261242	16.971584
30.764740	1175.507510	16.976602
30.913317	1170.148097	16.981619
31.053268	1193.474226	16.986637
31.406231	1202.245875	16.991655
30.932939	1200.519628	16.996672
31.200779	1204.408675	17.001690
31.634983	1189.525088	17.006707
30.975920	1174.464286	17.011725
31.153758	1176.081689	17.016743
31.216794	1185.595014	17.021760
31.268470	1191.923317	17.026778
31.389446	1185.040958	17.031795
31.564178	1190.407970	17.036813
31.504040	1192.775387	17.041831
31.478557	1188.847501	17.046848
31.464338	1192.711597	17.051866
31.742296	1182.865149	17.056883
31.562938	1178.466303	17.061901
31.361088	1176.914792	17.066919
31.758729	1178.548553	17.071936
31.548770	1193.425813	17.076954
31.598948	1184.176511	17.081971
31.490909	1188.366762	17.086989
31.694526	1192.996339	17.092007
31.828839	1184.390566	17.097024
31.505377	1196.270970	17.102042
31.860164	1193.356461	17.107059
31.454856	1193.157886	17.112077
31.608352	1192.138854	17.117095
31.593134	1193.372490	17.122112
31.334368	1188.819473	17.127130
31.791548	1196.492400	17.132147
32.248486	1208.676651	17.137165
32.318406	1206.167959	17.142183
31.611295	1198.247943	17.147200
31.831994	1207.591085	17.152218
32.368682	1209.854956	17.157235
32.184466	1222.059558	17.162253
32.229636	1220.079749	17.167271
32.506376	1212.080280	17.172288
32.501648	1213.993263	17.177306
32.303652	1188.115090	17.182323
32.221673	1184.054044	17.187341
32.253641	1181.998082	17.192359
32.563612	1180.697637	17.197376
32.206513	1187.766832	17.202394
32.370303	1194.417113	17.207411
32.328534	1209.109850	17.212429
32.248270	1207.229944	17.217447
32.199606	1212.289477	17.222464
32.484421	1222.333801	17.227482
32.745488	1218.639946	17.232499
32.405865	1218.351757	17.237517
32.121923	1219.434229	17.242535
32.246609	1217.129058	17.247552
32.261900	1220.262313	17.252570
32.430811	1209.592984	17.257587
32.267983	1229.867430	17.262605
32.371422	1231.388893	17.267623
32.707619	1241.347165	17.272640
32.787091	1254.004965	17.277658
32.969655	1237.310689	17.282675
33.281128	1242.022812	17.287693
33.227127	1239.552349	17.292711
33.027360	1230.059376	17.297728
33.116870	1244.400103	17.302746
33.102100	1239.220071	17.307763
33.017932	1239.749401	17.312781
33.344456	1237.273803	17.317799
33.038779	1231.445506	17.322816
33.136021	1243.313764	17.327834
33.552235	1235.299456	17.332851
33.406839	1236.808187	17.337869
33.301232	1226.157926	17.342887
33.478836	1229.728072	17.347904
32.980876	1235.408842	17.352922
33.195195	1234.023841	17.357939
33.010970	1233.173321	17.362957
33.417591	1235.230393	17.367975
33.446102	1223.115448	17.372992
33.290041	1231.222208	17.378010
33.768625	1223.364897	17.383027
33.622154	1233.196398	17.388045
33.431687	1231.604414	17.393063
33.710786	1237.562411	17.398080
33.594730	1229.357903	17.403098
33.545800	1228.764500	17.408115
33.628996	1232.912074	17.413133
33.654185	1256.426194	17.418151
34.132899	1257.298530	17.423168
34.016159	1267.020407	17.428186
34.050582	1253.597014	17.433203
34.005384	1239.699821	17.438221
33.598824	1238.201884	17.443239
33.956520	1237.262025	17.448256
33.714318	1252.543881	17.453274
34.152271	1256.531148	17.458291
34.364227	1249.168354	17.463309
33.964671	1264.467222	17.468327
34.440924	1255.682353	17.473344
34.243638	1255.178474	17.478362
34.092920	1260.925375	17.483379
34.120045	1251.229469	17.488397
34.093427	1258.581366	17.493415
34.348465	1260.520632	17.498432
34.145083	1260.647666	17.503450
34.356443	1261.835917	17.508467
34.443269	1265.265202	17.513485
34.377538	1257.299976	17.518503
34.477552	1257.639758	17.523520
33.906051	1257.455316	17.528538
34.207358	1261.319545	17.533555
34.171692	1261.663683	17.538573
34.381961	1284.585404	17.543591
34.749542	1284.286803	17.548608
34.862330	1292.362465	17.553626
35.083005	1277.208647	17.558643
35.406355	1269.030175	17.563661
34.766037	1259.010541	17.568679
34.823258	1247.058141	17.573696
34.566402	1250.439215	17.578714
34.583311	1241.561519	17.583731
34.725871	1244.367415	17.588749
34.975491	1268.540829	17.593767
35.262307	1268.228831	17.598784
34.834460	1273.164560	17.603802
35.024419	1271.084001	17.608819
35.324365	1267.451412	17.613837
35.201211	1272.867384	17.618855
35.369650	1268.334154	17.623872
35.234184	1269.139294	17.628890
35.098996	1246.255663	17.633907
35.443940	1262.091864	17.638925
35.349078	1266.392549	17.643943
35.628621	1246.504337	17.648960
35.362053	1246.431209	17.653978
35.470597	1244.684204	17.658995
35.764253	1232.097407	17.664013
35.205632	1240.757036	17.669031
34.911085	1239.094886	17.674048
34.891827	1253.781576	17.679066
35.422939	1268.970046	17.684083
35.286448	1271.008394	17.689101
35.392542	1268.190954	17.694119
35.679636	1257.579187	17.699136
35.295808	1269.121621	17.704154
35.143153	1260.911344	17.709171
36.016871	1278.102487	17.714189
36.008252	1293.242166	17.719207
36.103664	1285.257724	17.724224
35.737602	1282.310593	17.729242
36.159973	1284.735921	17.734259
36.102581	1271.465506	17.739277
35.889685	1266.243470	17.744295
36.116809	1270.642018	17.749312
36.011139	1270.920191	17.754330
36.189332	1278.063780	17.759347
36.600562	1274.424574	17.764365
36.307028	1271.542599	17.769383
35.910730	1262.138052	17.774400
36.195780	1258.129202	17.779418
36.190628	1268.653054	17.784435
36.094344	1275.746030	17.789453
36.055704	1293.981151	17.794471
36.260457	1288.293112	17.799488
36.341136	1286.695200	17.804506
36.461167	1292.404368	17.809523
36.583293	1285.058400	17.814541
36.509467	1281.707771	17.819559
36.554939	1284.370699	17.824576
36.879486	1286.176415	17.829594
36.550582	1276.966599	17.834611
36.541289	1285.797098	17.839629
36.688335	1291.050623	17.844647
36.919133	1287.333813	17.849664
36.588291	1291.896802	17.854682
36.914822	1276.353025	17.859699
36.953813	1280.551238	17.864717
36.797994	1290.199288	17.869735
37.066607	1281.138951	17.874752
36.830612	1283.822501	17.879770
36.742640	1284.056407	17.884787
36.969801	1276.608013	17.889805
36.523008	1283.152747	17.894823
36.716099	1293.858352	17.899840
36.891354	1303.860636	17.904858
36.823618	1308.812730	17.909875
37.265837	1313.998491	17.914893
37.103572	1323.851561	17.919911
37.327467	1314.021856	17.924928
37.421602	1311.797713	17.929946
37.670402	1310.766042	17.934963
37.614959	1310.159148	17.939981
37.529855	1313.059051	17.944999
37.402074	1311.778325	17.950016
37.488477	1317.763143	17.955034
37.524155	1313.593607	17.960051
37.649636	1301.484196	17.965069
37.402109	1310.165972	17.970087
37.497738	1306.953023	17.975104
37.477733	1314.802265	17.980122
37.441829	1313.913009	17.985139
37.553287	1304.565696	17.990157
37.437157	1308.897866	17.995175
37.473709	1312.009903	18.000192
38.003748	1318.000395	18.005210
37.646627	1331.460062	18.010227
37.795756	1337.702212	18.015245
37.854103	1338.069367	18.020263
38.129053	1326.740288	18.025280
37.942875	1339.997251	18.030298
38.262039	1330.200973	18.035315
38.560223	1327.653283	18.040333
38.256106	1329.009175	18.045351
38.048059	1328.228735	18.050368
38.214509	1325.120195	18.055386
38.289963	1337.177955	18.060403
38.465342	1324.365792	18.065421
38.336754	1330.681876	18.070439
38.648891	1326.754349	18.075456
38.445777	1331.247775	18.080474
37.894017	1327.266447	18.085491
38.648714	1319.557852	18.090509
38.173714	1333.773243	18.095527
38.485450	1322.485319	18.100544
38.375291	1324.781119	18.105562
38.165300	1330.133538	18.110579
38.505972	1332.053123	18.115597
38.183846	1346.672336	18.120615
38.090135	1354.325539	18.125632
38.158503	1356.084313	18.130650
38.706083	1354.941751	18.135667
38.829853	1352.119401	18.140685
38.576242	1368.422923	18.145703
39.068891	1381.986017	18.150720
39.002686	1379.836838	18.155738
39.451426	1383.118823	18.160755
39.624624	1380.624103	18.165773
39.327631	1367.040137	18.170791
39.321350	1356.007205	18.175808
39.304697	1354.633666	18.180826
39.249284	1345.375375	18.185843
39.677747	1341.452992	18.190861
39.378286	1344.037221	18.195879
39.219719	1345.415469	18.200896
39.428006	1346.489277	18.205914
39.143095	1343.284215	18.210931
39.431330	1336.690228	18.215949
39.270080	1345.320337	18.220967
39.348785	1345.122716	18.225984
39.353871	1362.762895	18.231002
39.671107	1370.874035	18.236019
39.208879	1367.327862	18.241037
39.523451	1383.616846	18.246055
39.335714	1379.790579	18.251072
39.650834	1368.476865	18.256090
40.189029	1377.419121	18.261107
40.009639	1374.330041	18.266125
40.110564	1374.251180	18.271143
39.980539	1373.497975	18.276160
40.153121	1375.125718	18.281178
39.815655	1373.778921	18.286195
40.048510	1368.226354	18.291213
39.997127	1365.928663	18.296231
39.831699	1377.384227	18.301248
40.257143	1367.201831	18.306266
39.820426	1367.071050	18.311283
40.052475	1371.664084	18.316301
39.964574	1372.107424	18.321319
39.731305	1369.698513	18.326336
40.184818	1378.181965	18.331354
40.162600	1388.109524	18.336371
40.168199	1393.817992	18.341389
40.148528	1390.961119	18.346407
40.467031	1400.342514	18.351424
40.603169	1391.531209	18.356442
39.881067	1389.061507	18.361459
40.637072	1398.188966	18.366477
40.773685	1405.232020	18.371495
40.864758	1409.561799	18.376512
40.829907	1390.502612	18.381530
40.964521	1380.814417	18.386547
40.698700	1379.914802	18.391565
40.100289	1388.280319	18.396583
40.742916	1404.093753	18.401600
41.058223	1399.832618	18.406618
40.885816	1410.066943	18.411635
41.069586	1412.274324	18.416653
41.195311	1404.261573	18.421671
41.249191	1410.761252	18.426688
41.440730	1411.716975	18.431706
40.987395	1407.118551	18.436723
41.390417	1412.745473	18.441741
41.395082	1404.251989	18.446759
41.349681	1407.232736	18.451776
41.674639	1405.243190	18.456794
41.668850	1410.356316	18.461811
41.609768	1396.456951	18.466829
41.585469	1399.975531	18.471847
41.628109	1398.963030	18.476864
41.632924	1394.385598	18.481882
41.695132	1409.941608	18.486899
42.000511	1402.875865	18.491917
41.888095	1399.664669	18.496935
42.121574	1405.920045	18.501952
42.236204	1387.308937	18.506970
41.674580	1377.218321	18.511987
41.891354	1374.681742	18.517005
41.967759	1367.769675	18.522023
41.914066	1373.433624	18.527040
41.801015	1363.215594	18.532058
41.670585	1383.155748	18.537075
41.826214	1385.610693	18.542093
41.656683	1395.629970	18.547111
41.783763	1399.270332	18.552128
42.359163	1388.186730	18.557146
41.905148	1398.958613	18.562163
42.002548	1391.153311	18.567181
42.230494	1388.581022	18.572199
42.006376	1394.932241	18.577216
42.391817	1407.758006	18.582234
42.493988	1415.035897	18.587251
42.906195	1408.663475	18.592269
42.873391	1401.482867	18.597287
42.485509	1397.788945	18.602304
42.672510	1382.672883	18.607322
42.507349	1390.212740	18.612339
42.200515	1395.036739	18.617357
42.137671	1396.397567	18.622375
42.508058	1417.691428	18.627392
42.799010	1419.418472	18.632410
42.262659	1431.911069	18.637427
42.710001	1416.926273	18.642445
42.818239	1423.935058	18.647463
42.681677	1422.884906	18.652480
42.628930	1425.841283	18.657498
42.946720	1444.595506	18.662515
43.276718	1451.546719	18.667533
43.402288	1448.234297	18.672551
43.159000	1448.567149	18.677568
43.500247	1449.631155	18.682586
43.395913	1449.472896	18.687603
43.128339	1440.705576	18.692621
43.407935	1436.693253	18.697639
43.355457	1442.107818	18.702656
43.560542	1443.579008	18.707674
43.494063	1443.434953	18.712691
43.421561	1457.197202	18.717709
43.767829	1448.743586	18.722727
43.521733	1451.418601	18.727744
43.740954	1444.538756	18.732762
43.545234	1450.888445	18.737779
43.588388	1445.911348	18.742797
44.119526	1439.427884	18.747815
43.713284	1440.281411	18.752832
43.845170	1440.785209	18.757850
43.855174	1444.281190	18.762867
43.848616	1441.317807	18.767885
43.685484	1439.725999	18.772903
43.836519	1438.309727	18.777920
44.024167	1440.063721	18.782938
43.972972	1440.667518	18.787955
44.195298	1438.964642	18.792973
44.001434	1442.182573	18.797991
43.845993	1450.292101	18.803008
44.202824	1449.420090	18.808026
44.122279	1470.587905	18.813043
44.266380	1467.246426	18.818061
44.388182	1460.400816	18.823079
44.332377	1460.658138	18.828096
44.486730	1458.676361	18.833114
44.273702	1456.188102	18.838131
44.462336	1464.417040	18.843149
44.792903	1457.444739	18.848167
44.303667	1466.111506	18.853184
44.704334	1459.063031	18.858202
44.645886	1470.655279	18.863219
44.691782	1485.429431	18.868237
44.975941	1485.982032	18.873255
44.967433	1486.927970	18.878272
45.010455	1479.602095	18.883290
45.108777	1480.920496	18.888307
45.179028	1483.336052	18.893325
45.238175	1476.759073	18.898343
45.253609	1480.953367	18.903360
45.359539	1471.382462	18.908378
45.464212	1484.115018	18.913395
45.352189	1478.072674	18.918413
45.751432	1467.131175	18.923431
45.315112	1458.409502	18.928448
45.124616	1447.916448	18.933466
45.440583	1452.228292	18.938483
45.507278	1460.669936	18.943501
45.417042	1456.996400	18.948519
45.559859	1471.858033	18.953536
45.642674	1469.260944	18.958554
45.363678	1474.289410	18.963571
45.737831	1469.488204	18.968589
45.760086	1473.227829	18.973607
45.570348	1468.279839	18.978624
45.541811	1468.975159	18.983642
45.465190	1469.215455	18.988659
45.436804	1475.100051	18.993677
45.591524	1472.246177	18.998695
45.554536	1488.295062	19.003712
45.885249	1495.128855	19.008730
45.846318	1494.678273	19.013747
46.102592	1507.522359	19.018765
45.939325	1500.394408	19.023783
45.868259	1511.024220	19.028800
45.999416	1493.829524	19.033818
46.006437	1506.628267	19.038835
45.986886	1520.162515	19.043853
46.630911	1523.055113	19.048871
46.476154	1531.401181	19.053888
46.799915	1527.414200	19.058906
46.485415	1523.442352	19.063923
46.609568	1530.565872	19.068941
47.045071	1509.311356	19.073959
46.834418	1526.168554	19.078976
47.124410	1517.888391	19.083994
46.842377	1519.544969	19.089011
46.626136	1520.646170	19.094029
47.033627	1515.697306	19.099047
47.229703	1516.481026	19.104064
47.002647	1520.262731	19.109082
47.453080	1520.055132	19.114099
47.291593	1518.516192	19.119117
47.261970	1506.513406	19.124135
46.862651	1497.502516	19.129152
47.158880	1503.357782	19.134170
47.294330	1515.995899	19.139187
47.216230	1518.477756	19.144205
47.447613	1516.764318	19.149223
47.206889	1519.259716	19.154240
47.452669	1519.957255	19.159258
47.462638	1510.759298	19.164275
47.457387	1516.651102	19.169293
47.463326	1511.964002	19.174311
47.420510	1518.357297	19.179328
47.291692	1522.460528	19.184346
47.163105	1522.389747	19.189363
47.330134	1537.541919	19.194381
47.915050	1546.172998	19.199399
48.112358	1548.598234	19.204416
48.095064	1538.952416	19.209434
48.154895	1546.001555	19.214451
48.025016	1541.831418	19.219469
48.428056	1540.762383	19.224487
48.273194	1550.221461	19.229504
48.253063	1535.628913	19.234522
48.318586	1540.110596	19.239539
48.279121	1536.007772	19.244557
47.942109	1532.991609	19.249575
48.156576	1539.698608	19.254592
48.282950	1538.678139	19.259610
48.424551	1542.316525	19.264627
48.074362	1546.198151	19.269645
48.613349	1532.624041	19.274663
48.029061	1541.542807	19.279680
48.488408	1534.208994	19.284698
48.547597	1537.129928	19.289715
48.208379	1555.943468	19.294733
48.740342	1557.794794	19.299751
48.557456	1571.144716	19.304768
48.490976	1568.131389	19.309786
48.743537	1566.843963	19.314803
48.445128	1576.416982	19.319821
48.812305	1562.752004	19.324839
48.895799	1574.748383	19.329856
49.174263	1575.332246	19.334874
49.520030	1579.766356	19.339891
49.435823	1576.518169	19.344909
49.577263	1565.740153	19.349927
49.163047	1566.542645	19.354944
49.652831	1551.983366	19.359962
49.303081	1552.964157	19.364979
49.160289	1560.387795	19.369997
49.699709	1565.608728	19.375015
49.705578	1563.577904	19.380032
49.336605	1556.708001	19.385050
49.683565	1564.117084	19.390067
49.651754	1574.872328	19.395085
50.002750	1586.046870	19.400103
49.785185	1578.947558	19.405120
49.820120	1578.776080	19.410138
50.038361	1569.886514	19.415155
49.704268	1577.105223	19.420173
49.907956	1577.197533	19.425191
49.881142	1584.206312	19.430208
49.759103	1575.166788	19.435226
49.931975	1571.590210	19.440243
49.936300	1579.547762	19.445261
50.201541	1576.902339	19.450279
49.890183	1581.228328	19.455296
50.246230	1601.963404	19.460314
50.582903	1605.199034	19.465331
50.335748	1611.376204	19.470349
50.527672	1605.388600	19.475367
50.621204	1608.232208	19.480384
50.663221	1622.829968	19.485402
50.722382	1604.441170	19.490419
50.776790	1607.914481	19.495437
50.828240	1604.076900	19.500455
50.811896	1607.014291	19.505472
50.492949	1611.682095	19.510490
50.622030	1605.924580	19.515507
50.359512	1606.053927	19.520525
50.574784	1598.159320	19.525543
50.599928	1606.448869	19.530560
50.771421	1627.273199	19.535578
51.066070	1626.928403	19.540595
51.029149	1630.443219	19.545613
51.157964	1624.135350	19.550631
51.403991	1621.597826	19.555648
51.325795	1625.496639	19.560666
51.353130	1622.815798	19.565683
51.690139	1626.501769	19.570701
51.826761	1625.895344	19.575719
51.664837	1621.824979	19.580736
51.749520	1624.052735	19.585754
52.098763	1620.996547	19.590771
52.050325	1626.024287	19.595789
52.299292	1624.135879	19.600807
52.283643	1626.658594	19.605824
52.017184	1605.024508	19.610842
51.911531	1589.642530	19.615859
51.982616	1596.536287	19.620877
52.269507	1584.041664	19.625895
52.196166	1580.902306	19.630912
51.974773	1578.323679	19.635930
52.284934	1581.252279	19.640947
52.167312	1589.105618	19.645965
52.310291	1585.561546	19.650983
52.177626	1585.926477	19.656000
52.022060	1587.521570	19.661018
52.245764	1590.440865	19.666035
52.088346	1609.823578	19.671053
52.314658	1612.615674	19.676071
52.731983	1609.681679	19.681088
52.503158	1608.480650	19.686106
52.610727	1605.358576	19.691123
52.540751	1606.363911	19.696141
52.471811	1608.987179	19.701159
52.893913	1602.322490	19.706176
52.651170	1609.458372	19.711194
53.091543	1611.448886	19.716211
52.553516	1615.275804	19.721229
52.835401	1620.249242	19.726247
52.869778	1631.442384	19.731264
52.650988	1638.623919	19.736282
53.189376	1632.356105	19.741299
52.881891	1640.368072	19.746317
53.290634	1636.732346	19.751335
53.151039	1638.990152	19.756352
53.197369	1643.547877	19.761370
53.337798	1640.681378	19.766387
53.058280	1670.706802	19.771405
53.619751	1672.179242	19.776423
53.664498	1672.441965	19.781440
53.764889	1676.051772	19.786458
53.766286	1662.309083	19.791475
53.345300	1672.715842	19.796493
53.341869	1659.594821	19.801511
53.676929	1662.415377	19.806528
53.453848	1663.666539	19.811546
54.118727	1677.398621	19.816563
53.960613	1692.095332	19.821581
54.290794	1687.328114	19.826599
54.510198	1691.986723	19.831616
54.477585	1687.061071	19.836634
54.188410	1669.558612	19.841651
54.154037	1670.169081	19.846669
54.358897	1681.244266	19.851687
54.931048	1682.798010	19.856704
54.362223	1687.059178	19.861722
54.600413	1684.610343	19.866739
54.550482	1678.831261	19.871757
54.666332	1685.157409	19.876775
54.675460	1678.189020	19.881792
54.690371	1684.132668	19.886810
54.971179	1676.400792	19.891827
54.584556	1672.030611	19.896845
54.912957	1681.118807	19.901863
54.836437	1680.563813	19.906880
54.659972	1687.682457	19.911898
55.070119	1676.506329	19.916915
55.122863	1679.317334	19.921933
54.663760	1668.420573	19.926951
55.130089	1677.947347	19.931968
54.808894	1696.208072	19.936986
55.422632	1698.822256	19.942003
55.338901	1700.903892	19.947021
55.250311	1698.554831	19.952039
55.669958	1693.069646	19.957056
55.306350	1702.596845	19.962074
55.486307	1694.349375	19.967091
55.396602	1691.137900	19.972109
55.325946	1688.390202	19.977127
55.546806	1691.482428	19.982144
55.383456	1694.985122	19.987162
55.823291	1708.637566	19.992179
55.689641	1722.602694	19.997197
55.372150	1720.587988	20.002215
55.717047	1724.128582	20.007232
55.898569	1727.216305	20.012250
56.265842	1723.949632	20.017267
55.939958	1724.448921	20.022285
56.308571	1717.558000	20.027303
56.572305	1713.067131	20.032320
56.167553	1716.079090	20.037338
56.622292	1730.103889	20.042355
56.623097	1730.645543	20.047373
56.684227	1718.200792	20.052391
56.371127	1715.266460	20.057408
56.630525	1740.614981	20.062426
57.115383	1732.595354	20.067443
56.869699	1737.165237	20.072461
56.621350	1740.037918	20.077479
57.265603	1738.185228	20.082496
57.178501	1727.841005	20.087514
57.209321	1716.693798	20.092531
57.089465	1707.845568	20.097549
56.776715	1711.710798	20.102567
57.202829	1714.920619	20.107584
57.190413	1730.076314	20.112602
57.549505	1731.240536	20.117619
57.824489	1724.050154	20.122637
57.486504	1728.536104	20.127655
57.668738	1707.598057	20.132672
57.362943	1714.311749	20.137690
57.395084	1717.420267	20.142707
57.799551	1724.742740	20.147725
57.649544	1726.832204	20.152743
57.624280	1726.391164	20.157760
57.762165	1730.571943	20.162778
58.061383	1724.915348	20.167795
57.821963	1733.062944	20.172813
57.597891	1729.750481	20.177831
57.864555	1721.141788	20.182848
57.855865	1721.407848	20.187866
57.834172	1731.174908	20.192883
57.926758	1722.708030	20.197901
57.713153	1738.917521	20.202919
58.110149	1747.680618	20.207936
57.898000	1755.627646	20.212954
58.137475	1755.064030	20.217971
58.103418	1756.788628	20.222989
58.003075	1765.868336	20.228007
58.191091	1768.046326	20.233024
58.345967	1785.692107	20.238042
58.504958	1785.308745	20.243059
58.643495	1787.866981	20.248077
58.851845	1779.956498	20.253095
58.951717	1774.476595	20.258112
58.773115	1779.406645	20.263130
58.946689	1771.592083	20.268147
58.916007	1788.283939	20.273165
59.050243	1812.340694	20.278183
59.298117	1806.704777	20.283200
59.300717	1810.901678	20.288218
59.151881	1805.796411	20.293235
59.431736	1798.561881	20.298253
59.574968	1808.669402	20.303271
59.580217	1792.278301	20.308288
59.618501	1805.523298	20.313306
59.987853	1797.525519	20.318323
59.682594	1785.251617	20.323341
59.956915	1782.259772	20.328359
59.951600	1765.936196	20.333376
59.431038	1769.723644	20.338394
59.390084	1782.216383	20.343411
59.985077	1797.001490	20.348429
59.653199	1796.051369	20.353447
60.146007	1789.705605	20.358464
60.046731	1795.574895	20.363482
60.315338	1787.852071	20.368499
60.005647	1786.756150	20.373517
60.131508	1795.451174	20.378535
60.280903	1788.572111	20.383552
60.496860	1794.320701	20.388570
60.272147	1799.943437	20.393587
60.669576	1794.989065	20.398605
60.492037	1792.569284	20.403623
60.697625	1789.803781	20.408640
60.372166	1803.351919	20.413658
60.115559	1811.716182	20.418675
60.691520	1817.727223	20.423693
60.640994	1834.203121	20.428711
60.710942	1821.785961	20.433728
60.669050	1824.861483	20.438746
60.565351	1839.024515	20.443763
61.139893	1853.562667	20.448781
61.015615	1859.697147	20.453799
61.038386	1853.734700	20.458816
61.124313	1852.809886	20.463834
60.902085	1847.334075	20.468851
61.428685	1845.258726	20.473869
61.435286	1853.913293	20.478887
61.318923	1856.343664	20.483904
61.870627	1865.005621	20.488922
62.142181	1871.630871	20.493939
62.035631	1857.915331	20.498957
61.689481	1854.996286	20.503975
61.837919	1840.325146	20.508992
62.165349	1855.367999	20.514010
62.092608	1850.038305	20.519027
62.343858	1846.943968	20.524045
62.042395	1841.980890	20.529063
61.830742	1844.706174	20.534080
62.188834	1858.239607	20.539098
62.323980	1863.707111	20.544115
62.692013	1864.092295	20.549133
62.518482	1868.027821	20.554151
62.859854	1853.979455	20.559168
62.761273	1863.256174	20.564186
62.479032	1860.406469	20.569203
62.718357	1863.268505	20.574221
62.690411	1855.093956	20.579239
62.649617	1860.649647	20.584256
62.834061	1850.396997	20.589274
62.886347	1860.916465	20.594291
62.803750	1849.481246	20.599309
62.775260	1862.212933	20.604327
62.784867	1856.112899	20.609344
62.913714	1856.782178	20.614362
62.752778	1859.804188	20.619379
63.248023	1870.817650	20.624397
63.082397	1878.714911	20.629415
62.955233	1882.206537	20.634432
63.014886	1874.234406	20.639450
63.409857	1882.896340	20.644467
63.466107	1874.340512	20.649485
63.566628	1876.169221	20.654503
63.506423	1891.371569	20.659520
63.693107	1903.227887	20.664538
63.444587	1909.531385	20.669555
63.943863	1898.821845	20.674573
63.852046	1911.554215	20.679591
63.644890	1899.812018	20.684608
63.750006	1900.736806	20.689626
63.803390	1908.318288	20.694643
63.972172	1909.365608	20.699661
64.024386	1927.008863	20.704679
64.191234	1925.885603	20.709696
64.249017	1935.729005	20.714714
64.358653	1930.123018	20.719731
64.509606	1922.482996	20.724749
64.259446	1930.632079	20.729767
64.498284	1924.034607	20.734784
64.177069	1933.691937	20.739802
64.617224	1952.952512	20.744819
64.888982	1956.406056	20.749837
64.992885	1954.386901	20.754855
65.240303	1950.729783	20.759872
65.179538	1955.304545	20.764890
65.217028	1958.917353	20.769907
65.575468	1951.212252	20.774925
65.349013	1944.481967	20.779943
65.758508	1949.953684	20.784960
65.452874	1949.069680	20.789978
65.557203	1948.956001	20.794995
65.803049	1940.351028	20.800013
65.485114	1948.860561	20.805031
65.586005	1938.654365	20.810048
65.611021	1938.852642	20.815066
65.516163	1939.616052	20.820083
66.036759	1932.634124	20.825101
66.013491	1945.742186	20.830119
65.996977	1928.534845	20.835136
66.224794	1936.407543	20.840154
66.008305	1935.933196	20.845171
66.137005	1943.522698	20.850189
66.041803	1941.301075	20.855207
65.971702	1931.648007	20.860224
65.720994	1941.581074	20.865242
65.908504	1962.709115	20.870259
66.330123	1963.201967	20.875277
66.406412	1972.102153	20.880295
66.275270	1962.172554	20.885312
66.394043	1973.327559	20.890330
66.239772	1979.953676	20.895347
66.750805	1983.001459	20.900365
66.991397	1992.240208	20.905383
67.068670	1997.738209	20.910400
66.829660	1994.407294	20.915418
66.825240	1995.533299	20.920435
67.391871	1983.200312	20.925453
67.584999	1987.531072	20.930471
67.281638	1981.605252	20.935488
67.803705	1981.966118	20.940506
67.401333	1991.212503	20.945523
67.641700	1983.260789	20.950541
67.688908	1985.539291	20.955559
67.589320	1986.454670	20.960576
67.694318	1979.910439	20.965594
67.593489	1983.661512	20.970611
67.516521	1972.936700	20.975629
67.399631	1987.316228	20.980647
67.443216	1997.951800	20.985664
68.165343	2008.232505	20.990682
68.091822	2019.061106	20.995699
68.201797	2004.338698	21.000717
68.072006	2024.237836	21.005735
68.007575	2017.151157	21.010752
68.280240	2015.094209	21.015770
68.177180	2012.981359	21.020787
68.174625	2013.513736	21.025805
68.190185	2008.594966	21.030823
68.599353	2011.385601	21.035840
68.764147	2026.452400	21.040858
68.593338	2029.123707	21.045875
68.742132	2034.642163	21.050893
68.927927	2026.176223	21.055911
68.798639	2024.273625	21.060928
69.294042	2026.150751	21.065946
69.067978	2030.296201	21.070963
69.102017	2027.662212	21.075981
69.382152	2026.085927	21.080999
69.094523	2026.282032	21.086016
69.213821	2014.967990	21.091034
69.367859	2014.772456	21.096051
69.128014	2012.383035	21.101069
69.229340	2033.718359	21.106087
69.508963	2047.581494	21.111104
69.559180	2044.662927	21.116122
69.285239	2049.304510	21.121139
69.945691	2046.890036	21.126157
69.649799	2052.592366	21.131175
69.827350	2052.155925	21.136192
69.537827	2052.352738	21.141210
69.872309	2068.530486	21.146227
70.112357	2073.182644	21.151245
69.929160	2079.000580	21.156263
70.170621	2090.755450	21.161280
70.577292	2082.034399	21.166298
70.191726	2076.647757	21.171315
70.536133	2069.819748	21.176333
70.367114	2086.989172	21.181351
70.418337	2098.805862	21.186368
70.876930	2097.487431	21.191386
70.937674	2106.035534	21.196403
71.114004	2096.296285	21.201421
71.238099	2103.216924	21.206439
71.395757	2101.365627	21.211456
71.166352	2090.167141	21.216474
71.050178	2102.500540	21.221491
71.398301	2093.232862	21.226509
71.341786	2094.552938	21.231527
71.125738	2101.050748	21.236544
71.367139	2098.235166	21.241562
71.498548	2096.625230	21.246579
71.478354	2093.917924	21.251597
71.573263	2086.724120	21.256615
71.309466	2096.074397	21.261632
71.875799	2105.573461	21.266650
72.085532	2117.588336	21.271667
72.173786	2114.740233	21.276685
72.432296	2120.114566	21.281703
72.255782	2121.223010	21.286720
72.333651	2123.269677	21.291738
71.830061	2116.587565	21.296755
71.937335	2114.248531	21.301773
72.502347	2116.507856	21.306791
72.189092	2115.995980	21.311808
72.319633	2120.165876	21.316826
72.181961	2116.296488	21.321843
72.502866	2115.436693	21.326861
72.672621	2127.136926	21.331879
72.454569	2139.857706	21.336896
72.833820	2136.986615	21.341914
72.702099	2145.140215	21.346931
73.141965	2135.864015	21.351949
73.026204	2138.008101	21.356967
73.170560	2136.229477	21.361984
73.527449	2130.901387	21.367002
73.427120	2134.846119	21.372019
73.309235	2129.687193	21.377037
73.620718	2127.167492	21.382055
73.423694	2134.165330	21.387072
73.421848	2127.246984	21.392090
73.536357	2135.307053	21.397107
73.501068	2131.243145	21.402125
73.688594	2147.896896	21.407143
73.554905	2162.220310	21.412160
73.916348	2173.901439	21.417178
73.731975	2156.630690	21.422195
73.682791	2164.374954	21.427213
74.211783	2168.937566	21.432231
73.955500	2161.477062	21.437248
73.836736	2182.832890	21.442266
73.932544	2198.825875	21.447283
74.061261	2192.690634	21.452301
74.689985	2183.545346	21.457319
74.183912	2198.146205	21.462336
74.840423	2205.238981	21.467354
74.964670	2212.890772	21.472371
74.979331	2210.292245	21.477389
75.001543	2207.727904	21.482407
74.805894	2214.233407	21.487424
75.090802	2209.903070	21.492442
74.992368	2211.613180	21.497459
75.196511	2205.642616	21.502477
75.282567	2197.838394	21.507495
75.028256	2207.153702	21.512512
75.090574	2213.955874	21.517530
75.355225	2225.334947	21.522547
75.265350	2233.842308	21.527565
75.771131	2236.918968	21.532583
75.693576	2236.642481	21.537600
75.741492	2241.356818	21.542618
75.977019	2235.657041	21.547635
75.933872	2233.295649	21.552653
76.079263	2235.053583	21.557671
75.910452	2243.294482	21.562688
75.951035	2237.443510	21.567706
76.474945	2254.498389	21.572723
76.498940	2265.172821	21.577741
76.568971	2262.203294	21.582759
76.658639	2263.273187	21.587776
77.119979	2259.413642	21.592794
77.087324	2257.095000	21.597811
77.199197	2244.285901	21.602829
77.221116	2221.763411	21.607847
76.903062	2222.451581	21.612864
77.100473	2216.803792	21.617882
77.256475	2216.831561	21.622899
76.871308	2217.828490	21.627917
77.131100	2214.259029	21.632935
77.391126	2236.156171	21.637952
77.350367	2239.421752	21.642970
77.393552	2242.379723	21.647987
77.687634	2247.427727	21.653005
77.504488	2232.116605	21.658023
77.155198	2242.192961	21.663040
77.497253	2239.268953	21.668058
77.703399	2238.876987	21.673075
77.576489	2240.693000	21.678093
77.606014	2235.337578	21.683111
77.836403	2258.466081	21.688128
77.831173	2265.601913	21.693146
78.097481	2277.983151	21.698163
78.017374	2271.050926	21.703181
78.134146	2270.585565	21.708199
77.912484	2272.506643	21.713216
78.356096	2266.501918	21.718234
78.337855	2279.642108	21.723251
78.446091	2289.560455	21.728269
78.837326	2301.070206	21.733287
78.585164	2304.570023	21.738304
78.526237	2299.019767	21.743322
78.871285	2306.229517	21.748339
78.875749	2297.402493	21.753357
79.068883	2292.498329	21.758375
78.971855	2315.347649	21.763392
79.252269	2329.950306	21.768410
79.522671	2329.755188	21.773427
79.497949	2330.401094	21.778445
79.664565	2322.320075	21.783463
79.378779	2323.205670	21.788480
79.749328	2319.197357	21.793498
79.892056	2321.488441	21.798515
79.768437	2331.386539	21.803533
79.791926	2322.743366	21.808551
79.953295	2320.381959	21.813568
79.850966	2322.570699	21.818586
79.641398	2328.797046	21.823603
80.017377	2343.024035	21.828621
80.068835	2345.244010	21.833639
80.017777	2343.072503	21.838656
80.260523	2350.351970	21.843674
80.523212	2351.644808	21.848691
80.276507	2372.057863	21.853709
80.709675	2370.410142	21.858727
80.692743	2379.017715	21.863744
80.763670	2380.111980	21.868762
80.980874	2378.274020	21.873779
80.884306	2371.094465	21.878797
81.247654	2373.219889	21.883815
80.810449	2367.290882	21.888832
81.154283	2366.146163	21.893850
81.361964	2384.794951	21.898867
81.472263	2386.808331	21.903885
81.651679	2388.029128	21.908903
81.462843	2398.865669	21.913920
81.678066	2386.003120	21.918938
81.672324	2388.814882	21.923955
81.834853	2383.742126	21.928973
81.861679	2383.751912	21.933991
81.905920	2383.518252	21.939008
82.050881	2385.297535	21.944026
82.506340	2376.343036	21.949043
81.994827	2383.530857	21.954061
82.200334	2393.360327	21.959079
82.391240	2404.909230	21.964096
82.596021	2408.188131	21.969114
82.344117	2410.331959	21.974131
82.453952	2416.875161	21.979149
83.100247	2417.498556	21.984167
82.559451	2412.303647	21.989184
82.519348	2410.748062	21.994202
82.680429	2416.477622	21.999219
82.980196	2429.503472	22.004237
83.309949	2434.717294	22.009255
82.966312	2441.630090	22.014272
83.537929	2437.127410	22.019290
83.729541	2443.464554	22.024307
83.237223	2441.648390	22.029325
83.536466	2437.297112	22.034343
83.334442	2442.608038	22.039360
83.525814	2442.932328	22.044378
83.993337	2433.239937	22.049395
83.498888	2433.694709	22.054413
83.636127	2436.974169	22.059431
83.880316	2449.408814	22.064448
83.792523	2459.855420	22.069466
84.087606	2460.216086	22.074483
84.017648	2465.637444	22.079501
84.236787	2457.367335	22.084519
84.131785	2464.556394	22.089536
83.965832	2459.527764	22.094554
84.652258	2474.594069	22.099571
84.931421	2482.498704	22.104589
85.100147	2471.230086	22.109607
85.132672	2482.692272	22.114624
85.232477	2470.960239	22.119642
85.318383	2468.173093	22.124659
85.061274	2475.646016	22.129677
85.780427	2471.418915	22.134695
85.523059	2468.444104	22.139712
85.733779	2470.383384	22.144730
86.100799	2467.597335	22.149747
85.488713	2467.745977	22.154765
85.643985	2465.704866	22.159783
85.792662	2470.786074	22.164800
85.722539	2477.730769	22.169818
85.846043	2468.350053	22.174835
85.450178	2473.730487	22.179853
85.737739	2463.174915	22.184871
85.508158	2491.106932	22.189888
85.620320	2499.546733	22.194906
86.007773	2497.365201	22.199923
86.073829	2509.032496	22.204941
86.178135	2530.970404	22.209959
86.367118	2522.485950	22.214976
86.131291	2527.361139	22.219994
86.775600	2527.189550	22.225011
86.445016	2539.183577	22.230029
86.668000	2549.640208	22.235047
86.975770	2555.014806	22.240064
86.901996	2570.679932	22.245082
87.248112	2554.617832	22.250099
87.167073	2555.784911	22.255117
87.408770	2552.237663	22.260135
87.296945	2551.271136	22.265152
87.450521	2555.946814	22.270170
88.036801	2569.421041	22.275187
87.758576	2580.826476	22.280205
87.999739	2576.175703	22.285223
88.086731	2575.569980	22.290240
88.159861	2577.795850	22.295258
88.417478	2568.620047	22.300275
88.602811	2569.495766	22.305293
88.502830	2573.537801	22.310311
88.516219	2567.447887	22.315328
88.663010	2569.333194	22.320346
88.553349	2567.000088	22.325363
88.423088	2569.416333	22.330381
89.005586	2562.483726	22.335399
88.567545	2562.890970	22.340416
88.587324	2567.841968	22.345434
88.817484	2554.359450	22.350451
88.743636	2569.179264	22.355469
88.742843	2559.070999	22.360487
88.961952	2564.563435	22.365504
88.844080	2584.872756	22.370522
89.199597	2593.151049	22.375539
88.971120	2598.361677	22.380557
89.125673	2592.313345	22.385575
89.626373	2594.226284	22.390592
89.350085	2607.156311	22.395610
89.355943	2622.040935	22.400627
89.534028	2622.422158	22.405645
89.758035	2615.075626	22.410663
89.916570	2624.992946	22.415680
89.657524	2631.245717	22.420698
89.921798	2644.507166	22.425715
90.044999	2655.356003	22.430733
90.292742	2652.536517	22.435751
90.448772	2652.541447	22.440768
90.415952	2659.395396	22.445786
90.799511	2664.405887	22.450803
90.982975	2677.362613	22.455821
90.864972	2671.088100	22.460839
91.114135	2674.409319	22.465856
91.056822	2678.202569	22.470874
91.436889	2675.433616	22.475891
91.279475	2679.135558	22.480909
91.577125	2667.975383	22.485927
91.531501	2663.621296	22.490944
91.144877	2667.733257	22.495962
91.868272	2668.277754	22.500979
91.831122	2673.403576	22.505997
91.839944	2668.812112	22.511015
91.758510	2668.661858	22.516032
91.873615	2686.678658	22.521050
92.042857	2685.478173	22.526067
92.069564	2696.192612	22.531085
91.733005	2698.094179	22.536103
92.168078	2696.474065	22.541120
92.186833	2696.281236	22.546138
92.529887	2707.513029	22.551155
92.202905	2722.001646	22.556173
92.469537	2718.943965	22.561191
92.597803	2723.715623	22.566208
92.738619	2720.630738	22.571226
93.002325	2722.007304	22.576243
93.108241	2738.325965	22.581261
93.341089	2752.023840	22.586279
93.927495	2755.136868	22.591296
93.534647	2754.323163	22.596314
93.613735	2750.394497	22.601331
93.711038	2751.387171	22.606349
94.013540	2747.228589	22.611367
93.653838	2744.973866	22.616384
93.603063	2745.555199	22.621402
93.912648	2738.635415	22.626419
93.847902	2742.849231	22.631437
93.577943	2743.947597	22.636455
93.948316	2744.396993	22.641472
93.648935	2757.873130	22.646490
94.029366	2767.634896	22.651507
94.268252	2764.215634	22.656525
93.975627	2776.062602	22.661543
94.560798	2781.687828	22.666560
94.661495	2797.306577	22.671578
94.911972	2784.935537	22.676595
94.803758	2796.982320	22.681613
94.823997	2799.324073	22.686631
94.660075	2795.984489	22.691648
95.023894	2805.411604	22.696666
95.168685	2810.973523	22.701683
95.157764	2813.978752	22.706701
95.538631	2813.839363	22.711719
95.893603	2814.994119	22.716736
95.426523	2817.287415	22.721754
95.795114	2804.501893	22.726771
96.012525	2802.379185	22.731789
95.667701	2804.039596	22.736807
96.309159	2808.880260	22.741824
96.206982	2827.719869	22.746842
96.258854	2830.914326	22.751859
96.465232	2828.292617	22.756877
96.452186	2830.053622	22.761895
96.796357	2824.302176	22.766912
96.956760	2824.386310	22.771930
97.058110	2824.351865	22.776947
96.984758	2827.573749	22.781965
96.998071	2820.962056	22.786983
97.155486	2821.427421	22.792000
96.797055	2837.641951	22.797018
97.211528	2821.024125	22.802035
97.626659	2825.089215	22.807053
97.370968	2821.777418	22.812071
97.615839	2817.268885	22.817088
97.370724	2842.569658	22.822106
97.499949	2849.401586	22.827123
97.859412	2850.453625	22.832141
97.598007	2856.435989	22.837159
97.877041	2850.541370	22.842176
97.892176	2854.879009	22.847194
98.019287	2877.030181	22.852211
98.122087	2879.263781	22.857229
98.392578	2883.126439	22.862247
98.337858	2871.826806	22.867264
98.034377	2881.620376	22.872282
98.348448	2880.986100	22.877299
98.698094	2898.828082	22.882317
98.897078	2905.500836	22.887335
99.180593	2902.385990	22.892352
99.146035	2904.856920	22.897370
99.395090	2899.751166	22.902387
99.440340	2902.458901	22.907405
99.527423	2895.349492	22.912423
99.668655	2896.425460	22.917440
99.497430	2899.041467	22.922458
99.625219	2901.356767	22.927475
99.761145	2915.574023	22.932493
99.922319	2928.521656	22.937511
100.032221	2926.693132	22.942528
99.843938	2931.559392	22.947546
99.971797	2925.160205	22.952563
100.250919	2918.818660	22.957581
100.285359	2918.457865	22.962599
100.759359	2927.716407	22.967616
100.562987	2940.692930	22.972634
100.862123	2945.479283	22.977651
100.732480	2948.540025	22.982669
100.659451	2944.894390	22.987687
100.951986	2947.884052	22.992704
100.744700	2945.512717	22.997722
100.888028	2944.052703	23.002739
101.099626	2965.096616	23.007757
100.920062	2970.142169	23.012775
101.377856	2971.755937	23.017792
101.116233	2974.553078	23.022810
101.253248	2973.413425	23.027827
101.427110	2984.995111	23.032845
101.330211	3001.891373	23.037863
101.443807	3001.481641	23.042880
101.793754	3008.036129	23.047898
102.007667	3021.748008	23.052915
102.465615	3022.494753	23.057933
102.163736	3025.385584	23.062951
102.734175	3025.315997	23.067968
102.634368	3024.618340	23.072986
102.466579	3014.053528	23.078003
103.011634	3013.228630	23.083021
102.804614	3018.422457	23.088039
103.226263	3014.865392	23.093056
103.150204	3015.489902	23.098074
103.028342	3014.410824	23.103091
103.172978	3023.726711	23.108109
103.544094	3032.648383	23.113127
103.553365	3041.088976	23.118144
103.810723	3035.210083	23.123162
103.895363	3041.369890	23.128179
103.963136	3034.504975	23.133197
103.660825	3040.915478	23.138215
104.025245	3040.215376	23.143232
103.932846	3040.409089	23.148250
103.958293	3051.759864	23.153267
104.168864	3067.351637	23.158285
104.157883	3070.446698	23.163303
104.653475	3065.180771	23.168320
104.661103	3062.081647	23.173338
104.689537	3063.168822	23.178355
104.985558	3060.250318	23.183373
104.707423	3073.072363	23.188391
105.073073	3080.714932	23.193408
105.069692	3089.832904	23.198426
104.740296	3092.638924	23.203443
105.346647	3093.013433	23.208461
105.299918	3098.618977	23.213479
105.490529	3115.120090	23.218496
105.646952	3126.985898	23.223514
105.752280	3121.889695	23.228531
106.034456	3117.949362	23.233549
106.041199	3124.481581	23.238567
106.265767	3121.419763	23.243584
106.009338	3121.118540	23.248602
106.298391	3132.268234	23.253619
106.580195	3143.880203	23.258637
106.614579	3143.923781	23.263655
106.681723	3139.289448	23.268672
106.779961	3143.660657	23.273690
107.028658	3138.157604	23.278707
107.150179	3131.803087	23.283725
106.966990	3142.013557	23.288743
107.200315	3131.105458	23.293760
107.188480	3131.988262	23.298778
106.990721	3153.113197	23.303795
107.313507	3158.113438	23.308813
107.353240	3163.125500	23.313831
107.837591	3151.630105	23.318848
107.460551	3160.613901	23.323866
107.579964	3174.990836	23.328883
108.195922	3184.739858	23.333901
107.906991	3190.633984	23.338919
108.355624	3184.794240	23.343936
108.094248	3187.201576	23.348954
108.250010	3183.173091	23.353971
108.544184	3191.991047	23.358989
108.862173	3207.451779	23.364007
108.960943	3210.061722	23.369024
108.999046	3210.848851	23.374042
109.107664	3209.061062	23.379059
109.300457	3205.682411	23.384077
108.853718	3206.434447	23.389095
109.338532	3204.128030	23.394112
109.421218	3213.890551	23.399130
109.374281	3207.373717	23.404147
109.351262	3200.649757	23.409165
109.250004	3215.216035	23.414183
110.168366	3230.086790	23.419200
109.871505	3234.281288	23.424218
110.103355	3234.861127	23.429235
110.181652	3235.649872	23.434253
109.991304	3241.078044	23.439271
110.265865	3227.641932	23.444288
110.324760	3243.798811	23.449306
110.311358	3262.360046	23.454323
110.501222	3262.465293	23.459341
110.718681	3256.790975	23.464359
110.835487	3253.120532	23.469376
110.977875	3275.418575	23.474394
110.811177	3282.318193	23.479411
111.181721	3280.654371	23.484429
111.203144	3288.220555	23.489447
111.370472	3286.440755	23.494464
111.801797	3297.911143	23.499482
111.572102	3303.644307	23.504499
111.868045	3314.892215	23.509517
112.183471	3302.999042	23.514535
112.194561	3309.003004	23.519552
112.206067	3302.897365	23.524570
112.338044	3297.925052	23.529587
112.562568	3306.421499	23.534605
112.377508	3305.746606	23.539623
112.596856	3316.026779	23.544640
112.528070	3324.438318	23.549658
112.443560	3328.294895	23.554675
112.593483	3327.381056	23.559693
112.862281	3352.338092	23.564711
112.868161	3362.728842	23.569728
113.229636	3359.507290	23.574746
113.240327	3362.607482	23.579763
113.259019	3357.094398	23.584781
113.068938	3368.808287	23.589799
113.600881	3390.135993	23.594816
113.854545	3387.644567	23.599834
113.686614	3381.741066	23.604851
113.872251	3390.488512	23.609869
114.055496	3414.022250	23.614887
114.656878	3415.280368	23.619904
114.727590	3412.259718	23.624922
114.309428	3415.606533	23.629939
114.406051	3411.590144	23.634957
114.650429	3415.838010	23.639975
115.073089	3424.825398	23.644992
115.120048	3431.645608	23.650010
115.251694	3444.079209	23.655027
115.670317	3436.863870	23.660045
115.597365	3437.873752	23.665063
115.630764	3431.123027	23.670080
115.721883	3424.285575	23.675098
115.510094	3437.000071	23.680115
115.995084	3431.587337	23.685133
116.035597	3427.449116	23.690151
115.907985	3422.314208	23.695168
115.982178	3446.863013	23.700186
116.117537	3457.177659	23.705203
116.360535	3452.678705	23.710221
116.359213	3460.588147	23.715239
116.576605	3454.070366	23.720256
116.338563	3454.904409	23.725274
116.396544	3466.389878	23.730291
116.676435	3475.506457	23.735309
117.005620	3479.449321	23.740327
117.206895	3480.770931	23.745344
117.272228	3481.757134	23.750362
117.080676	3487.721872	23.755379
117.458898	3494.853056	23.760397
117.715673	3506.471803	23.765415
117.696110	3501.842269	23.770432
118.164608	3501.975017	23.775450
117.932073	3502.113975	23.780467
118.357638	3499.377510	23.785485
118.031961	3498.104557	23.790503
118.092740	3500.570034	23.795520
118.608721	3507.841427	23.800538
118.703516	3518.077780	23.805555
118.559176	3514.049678	23.810573
118.777847	3518.034474	23.815591
118.625048	3520.445540	23.820608
118.792056	3521.712978	23.825626
119.076156	3544.228916	23.830643
119.385731	3547.278874	23.835661
119.681318	3548.245859	23.840679
119.702479	3550.151693	23.845696
119.932651	3554.570080	23.850714
119.739386	3549.096350	23.855731
120.185271	3550.974391	23.860749
120.131418	3546.322565	23.865767
120.054352	3555.476633	23.870784
120.322581	3565.689422	23.875802
120.296752	3575.018505	23.880819
120.165876	3577.372794	23.885837
120.566002	3574.925209	23.890855
120.528826	3576.572562	23.895872
120.721665	3594.827965	23.900890
120.636622	3602.356016	23.905907
121.165733	3599.312199	23.910925
121.014663	3604.840304	23.915943
121.060329	3601.187465	23.920960
121.293772	3615.640427	23.925978
121.807085	3623.461598	23.930995
121.447664	3626.110457	23.936013
121.778877	3622.850550	23.941031
122.035734	3626.063602	23.946048
121.700632	3640.335484	23.951066
121.954205	3653.944886	23.956083
122.232191	3646.829123	23.961101
122.591624	3654.704531	23.966119
122.402149	3659.745251	23.971136
122.916385	3664.578902	23.976154
122.815900	3676.050205	23.981171
122.935340	3670.953062	23.986189
122.998743	3675.503832	23.991207
123.105615	3672.228688	23.996224
123.324465	3669.254731	24.001242
122.988773	3678.039038	24.006259
123.471591	3693.168593	24.011277
123.484070	3708.550466	24.016295
123.599470	3700.007471	24.021312
123.968611	3707.209163	24.026330
123.914474	3718.928762	24.031347
123.946617	3733.215528	24.036365
124.548939	3729.914258	24.041383
124.236896	3731.563034	24.046400
124.637853	3725.000181	24.051418
124.727624	3731.692552	24.056435
124.821698	3728.039544	24.061453
124.327629	3729.966520	24.066471
124.282363	3755.032109	24.071488
124.801314	3749.861710	24.076506
125.180914	3753.656909	24.081523
125.038465	3760.147944	24.086541
125.548510	3770.705529	24.091559
125.107195	3782.625516	24.096576
125.926832	3779.476865	24.101594
125.864138	3779.608180	24.106611
125.776877	3779.651031	24.111629
126.007376	3787.412794	24.116647
126.038287	3806.118539	24.121664
126.511005	3805.952127	24.126682
126.288171	3815.928621	24.131699
126.535572	3813.070793	24.136717
126.732851	3814.725424	24.141735
126.920176	3825.721962	24.146752
127.211612	3829.172278	24.151770
127.017103	3842.469755	24.156787
127.199099	3832.522556	24.161805
127.112451	3831.954591	24.166823
126.890638	3848.036111	24.171840
127.534076	3861.859139	24.176858
127.470792	3864.795670	24.181875
127.811839	3870.250662	24.186893
127.911364	3878.112119	24.191911
128.070446	3892.998180	24.196928
128.684112	3878.910404	24.201946
128.333659	3892.184915	24.206963
128.671816	3887.671264	24.211981
128.875625	3880.072726	24.216999
128.715223	3884.104626	24.222016
129.132853	3893.432143	24.227034
129.062770	3902.524225	24.232051
129.218865	3911.732825	24.237069
129.168848	3904.132985	24.242087
129.290072	3906.224687	24.247104
129.468843	3904.994184	24.252122
129.620861	3916.553404	24.257139
129.874584	3932.824824	24.262157
129.785266	3921.950693	24.267175
129.448433	3939.140088	24.272192
129.974681	3942.071958	24.277210
129.904446	3955.219014	24.282227
130.014563	3953.731331	24.287245
130.301760	3969.672003	24.292263
130.620289	3978.639545	24.297280
130.684743	3977.457101	24.302298
131.012742	3989.297521	24.307315
131.253801	4001.480740	24.312333
131.636784	4003.680716	24.317351
131.549112	4016.779129	24.322368
131.782898	4005.860897	24.327386
131.749714	4006.558674	24.332403
131.864074	4012.357198	24.337421
132.059583	4000.438070	24.342439
131.728625	3999.472292	24.347456
132.080086	4012.122352	24.352474
132.442834	4020.428957	24.357491
132.490693	4033.866418	24.362509
132.641732	4025.229932	24.367527
132.431289	4032.365895	24.372544
132.669001	4037.186382	24.377562
132.715084	4046.936976	24.382579
132.694381	4058.702089	24.387597
133.601357	4047.330592	24.392615
133.304004	4057.629465	24.397632
133.477354	4057.602394	24.402650
133.616611	4060.439671	24.407667
133.590605	4074.817096	24.412685
133.948075	4072.629294	24.417703
133.808031	4085.032389	24.422720
134.150684	4084.885148	24.427738
134.541410	4089.393660	24.432755
134.335285	4093.811194	24.437773
134.714719	4076.842672	24.442791
134.652241	4103.428042	24.447808
134.657992	4114.335928	24.452826
134.832380	4120.072577	24.457843
134.567581	4126.009519	24.462861
134.970310	4118.392896	24.467879
134.900277	4138.247816	24.472896
135.307911	4145.844584	24.477914
135.428976	4133.832151	24.482931
135.254900	4157.934909	24.487949
135.627166	4165.224106	24.492967
135.708977	4164.215180	24.497984
135.943057	4164.341073	24.503002
136.377711	4187.767413	24.508019
136.158185	4193.668534	24.513037
136.997341	4191.006417	24.518055
136.825229	4192.039064	24.523072
136.985850	4188.023694	24.528090
137.234026	4186.886421	24.533107
137.134912	4212.532219	24.538125
137.201914	4218.016561	24.543143
137.572204	4221.611023	24.548160
137.454534	4224.665697	24.553178
137.689927	4227.269730	24.558195
137.649866	4221.483345	24.563213
138.201583	4234.658004	24.568231
137.998195	4251.503940	24.573248
138.015608	4251.120732	24.578266
138.079100	4241.195258	24.583283
137.878254	4258.973217	24.588301
138.555874	4271.139497	24.593319
138.793167	4271.187681	24.598336
138.600739	4273.659367	24.603354
139.066642	4293.439143	24.608371
138.905361	4309.949769	24.613389
139.253786	4300.116478	24.618407
139.136002	4314.823543	24.623424
139.570901	4321.307822	24.628442
139.837335	4331.419818	24.633459
140.028528	4331.156682	24.638477
140.304515	4323.924785	24.643495
139.864485	4335.433488	24.648512
140.208765	4336.668102	24.653530
140.420730	4347.029324	24.658547
140.287650	4357.164952	24.663565
140.728289	4355.594947	24.668583
140.833289	4351.984088	24.673600
140.979287	4375.553003	24.678618
141.495763	4368.788446	24.683635
141.454009	4378.960158	24.688653
141.548145	4371.718181	24.693671
141.323008	4369.209399	24.698688
141.700909	4379.782583	24.703706
141.945296	4388.223173	24.708723
141.708612	4401.613552	24.713741
142.298404	4396.347344	24.718759
142.342542	4406.499341	24.723776
142.400557	4394.986210	24.728794
142.442434	4398.677612	24.733811
142.375736	4431.015630	24.738829
142.830352	4423.904535	24.743847
142.799850	4427.870177	24.748864
142.624365	4413.913363	24.753882
142.959749	4434.374096	24.758899
143.656126	4442.071263	24.763917
143.491904	4438.474242	24.768935
143.617080	4450.221009	24.773952
143.857301	4444.566911	24.778970
144.371318	4452.385630	24.783987
144.193849	4459.928999	24.789005
144.642917	4464.739041	24.794023
144.521831	4469.772634	24.799040
144.636113	4472.832270	24.804058
144.629075	4468.672902	24.809075
144.530431	4473.828788	24.814093
144.805198	4474.835509	24.819111
145.043053	4488.716005	24.824128
145.258795	4495.278379	24.829146
145.595064	4499.417219	24.834163
145.060579	4496.151610	24.839181
145.614191	4511.914059	24.844199
145.494580	4530.659369	24.849216
145.753743	4534.261276	24.854234
146.116282	4531.129882	24.859251
146.381288	4550.119470	24.864269
146.483786	4549.348085	24.869287
146.421543	4558.350649	24.874304
146.285051	4556.107527	24.879322
146.387221	4561.255397	24.884339
146.437900	4584.779766	24.889357
146.971398	4585.419190	24.894375
147.233006	4598.076726	24.899392
147.458552	4603.503452	24.904410
147.583988	4599.552870	24.909427
147.624332	4611.309077	24.914445
147.882623	4624.849239	24.919463
148.216116	4630.013964	24.924480
148.219554	4634.540288	24.929498
148.249793	4630.670824	24.934515
148.272307	4634.041016	24.939533
148.614472	4642.332460	24.944551
148.914123	4661.938613	24.949568
149.028147	4662.523842	24.954586
149.255369	4654.728892	24.959603
149.015780	4666.128258	24.964621
149.492177	4685.842214	24.969639
149.460548	4688.485019	24.974656
149.550317	4697.912977	24.979674
149.901634	4696.965720	24.984691
149.592543	4709.218518	24.989709
149.951897	4721.769403	24.994727
149.998178	4721.182941	24.999744
150.253587	4730.164517	25.004762
150.761403	4748.684929	25.009779
150.754582	4751.214168	25.014797
151.150541	4758.060264	25.019815
151.252888	4751.781511	25.024832
151.210046	4752.436028	25.029850
151.627816	4754.622480	25.034867
151.764246	4766.868507	25.039885
152.042418	4758.429513	25.044903
151.861935	4771.164317	25.049920
151.905034	4767.106828	25.054938
152.029656	4765.351261	25.059955
152.195454	4781.420753	25.064973
151.985061	4790.518069	25.069991
152.439424	4798.817798	25.075008
152.475521	4795.004817	25.080026
152.823909	4786.225772	25.085043
152.484221	4812.618028	25.090061
152.706051	4817.305926	25.095079
153.073526	4823.303053	25.100096
153.156724	4832.803847	25.105114
153.576805	4844.732843	25.110131
153.260698	4857.398812	25.115149
153.453157	4864.172325	25.120167
153.864813	4877.065140	25.125184
153.515061	4880.748248	25.130202
153.985604	4886.547196	25.135219
154.148397	4900.794099	25.140237
154.183494	4904.077209	25.145255
154.499586	4914.895682	25.150272
154.610888	4934.122248	25.155290
155.116612	4929.838490	25.160307
155.037077	4943.985364	25.165325
155.383569	4952.599946	25.170343
155.860519	4958.427788	25.175360
155.607515	4957.127714	25.180378
156.118821	4953.480955	25.185395
156.018859	4961.102301	25.190413
156.459971	4975.941125	25.195431
156.654746	4974.426730	25.200448
156.482875	4993.083583	25.205466
156.935368	4984.621123	25.210483
156.847492	4977.916195	25.215501
156.821012	4986.948523	25.220519
157.411570	5003.246411	25.225536
157.473123	5003.285891	25.230554
157.315982	5006.799315	25.235571
157.241942	5010.069012	25.240589
157.578696	5025.471733	25.245607
157.939970	5033.864181	25.250624
158.005882	5041.013127	25.255642
158.473261	5041.099619	25.260659
158.340956	5070.134138	25.265677
158.629788	5069.320854	25.270695
158.567115	5065.892743	25.275712
158.494925	5073.852927	25.280730
158.878739	5091.155422	25.285747
159.177647	5088.951190	25.290765
159.086121	5100.851668	25.295783
159.719074	5115.283192	25.300800
159.584742	5126.177167	25.305818
159.826923	5123.010454	25.310835
159.783840	5131.682542	25.315853
160.019059	5143.688049	25.320871
160.295992	5153.413714	25.325888
160.335640	5159.851155	25.330906
160.645202	5158.253159	25.335923
161.074349	5179.598754	25.340941
161.067382	5196.223374	25.345959
161.549170	5183.900762	25.350976
161.006979	5184.896290	25.355994
161.453665	5189.398223	25.361011
161.778246	5199.972914	25.366029
161.657177	5206.558268	25.371047
161.988021	5208.920630	25.376064
161.862666	5216.098170	25.381082
162.372181	5214.237881	25.386099
162.848004	5231.370933	25.391117
162.830787	5228.441675	25.396135
163.341593	5220.003302	25.401152
162.756870	5235.674556	25.406170
163.035302	5232.449839	25.411187
163.039731	5232.286130	25.416205
163.009275	5246.544862	25.421223
163.667420	5259.030173	25.426240
163.242298	5260.618276	25.431258
163.768214	5265.490667	25.436275
164.144236	5280.105856	25.441293
164.087660	5287.848553	25.446311
164.238065	5278.140374	25.451328
164.238955	5290.515571	25.456346
164.314522	5297.871746	25.461363
164.613008	5307.007188	25.466381
164.953241	5307.751101	25.471399
165.303948	5320.218051	25.476416
165.134793	5340.328745	25.481434
165.313447	5343.480282	25.486451
165.727973	5346.489596	25.491469
165.470675	5347.206419	25.496487
166.246380	5351.595648	25.501504
166.010831	5360.345405	25.506522
166.375448	5366.571615	25.511539
166.394391	5379.025015	25.516557
166.457559	5388.104163	25.521575
166.972736	5396.664287	25.526592
166.911870	5397.988114	25.531610
167.192222	5402.550725	25.536627
167.648575	5412.205105	25.541645
167.320594	5426.874759	25.546663
167.729268	5417.865647	25.551680
167.656282	5422.720673	25.556698
167.967175	5434.279126	25.561715
168.212542	5431.407171	25.566733
168.191218	5449.050425	25.571751
168.485876	5451.079363	25.576768
168.579547	5464.818411	25.581786
168.575311	5472.202055	25.586803
169.067861	5473.429545	25.591821
169.071878	5494.304085	25.596839
169.293685	5500.338977	25.601856
169.218990	5508.579391	25.606874
169.534437	5521.535133	25.611891
169.709694	5537.016286	25.616909
169.800925	5546.160188	25.621927
170.106173	5539.644332	25.626944
170.371229	5558.776898	25.631962
170.635617	5562.337225	25.636979
170.455626	5556.913756	25.641997
170.956524	5576.123864	25.647015
171.238936	5584.592672	25.652032
171.173823	5591.391025	25.657050
171.747303	5586.275988	25.662067
171.732826	5591.633318	25.667085
171.778790	5607.484063	25.672103
171.959373	5618.568036	25.677120
172.080483	5617.211483	25.682138
172.341856	5618.804898	25.687156
172.621103	5618.835119	25.692173
172.487575	5641.734703	25.697191
172.823103	5631.290758	25.702208
172.971664	5641.772809	25.707226
172.757861	5653.763255	25.712244
173.181468	5664.732206	25.717261
173.241823	5679.035365	25.722279
173.739665	5679.123911	25.727296
173.297364	5693.782808	25.732314
173.532489	5693.840024	25.737332
174.078490	5709.159944	25.742349
173.644122	5732.849811	25.747367
173.961092	5730.751979	25.752384
174.271883	5747.267867	25.757402
174.555388	5762.700604	25.762420
174.609724	5759.329369	25.767437
174.969338	5784.967941	25.772455
175.275349	5795.012109	25.777472
175.128780	5803.376415	25.782490
175.390955	5813.968939	25.787508
175.618627	5810.491024	25.792525
175.832727	5820.081797	25.797543
176.398278	5833.543781	25.802560
176.493596	5839.372912	25.807578
176.709035	5834.974724	25.812596
177.353526	5836.971003	25.817613
176.960788	5836.808454	25.822631
177.388582	5841.290864	25.827648
177.210213	5857.322343	25.832666
177.796462	5858.091716	25.837684
177.819177	5863.078317	25.842701
177.374081	5873.980934	25.847719
177.799612	5877.906100	25.852736
178.065697	5895.499122	25.857754
178.138204	5896.656778	25.862772
178.443450	5912.334949	25.867789
178.474966	5922.168666	25.872807
178.835518	5929.652019	25.877824
178.923529	5942.407900	25.882842
178.882574	5951.835409	25.887860
179.489923	5955.732858	25.892877
179.604818	5970.500609	25.897895
179.848050	5965.307017	25.902912
179.993275	5982.448362	25.907930
179.743732	5987.968397	25.912948
179.856657	5996.949870	25.917965
179.974122	6023.453553	25.922983
180.501564	6028.966268	25.928000
180.738902	6051.526231	25.933018
180.597060	6058.621030	25.938036
181.421067	6070.798352	25.943053
181.386449	6086.893691	25.948071
181.515649	6075.840912	25.953088
181.687816	6088.529420	25.958106
181.948703	6098.537933	25.963124
181.971045	6097.869534	25.968141
182.209746	6108.318857	25.973159
182.365856	6112.639177	25.978176
182.476966	6132.028698	25.983194
182.561780	6148.195692	25.988212
183.278290	6147.174509	25.993229
182.900699	6148.922591	25.998247
183.210602	6158.674926	26.003264
183.456876	6183.012058	26.008282
183.715665	6193.492768	26.013300
184.363548	6184.330994	26.018317
184.083062	6205.782857	26.023335
183.827814	6207.179100	26.028352
184.513055	6220.208097	26.033370
184.246535	6232.300646	26.038388
184.896145	6243.015989	26.043405
184.854148	6249.873809	26.048423
185.164035	6267.790800	26.053440
185.432359	6284.084292	26.058458
185.448437	6289.080002	26.063476
185.648579	6298.306339	26.068493
185.800371	6316.511052	26.073511
186.017452	6307.887592	26.078528
186.558786	6325.398509	26.083546
186.617900	6331.700095	26.088564
186.696789	6331.327927	26.093581
186.936189	6340.728946	26.098599
187.054780	6344.003260	26.103616
187.541494	6357.506312	26.108634
187.232624	6365.970244	26.113652
187.971930	6362.181459	26.118669
187.791948	6366.285753	26.123687
187.997341	6381.117670	26.128704
188.258857	6377.269353	26.133722
187.894923	6385.901515	26.138740
188.163493	6394.970868	26.143757
188.468534	6418.963888	26.148775
188.573691	6421.540230	26.153792
188.976383	6437.782494	26.158810
189.297536	6447.734781	26.163828
189.312665	6445.395399	26.168845
189.425679	6469.565212	26.173863
190.012731	6474.606659	26.178880
190.042046	6482.674406	26.183898
190.096587	6491.282244	26.188916
190.195643	6494.490510	26.193933
190.365796	6511.041507	26.198951
190.560629	6528.320157	26.203968
190.890841	6538.588423	26.208986
191.076269	6541.566586	26.214004
191.056846	6548.831160	26.219021
191.367715	6570.224214	26.224039
191.409369	6582.885103	26.229056
191.594852	6597.744936	26.234074
191.689312	6613.660336	26.239092
192.549969	6614.575725	26.244109
192.716713	6628.639226	26.249127
192.680127	6638.301138	26.254144
192.906595	6655.026485	26.259162
192.903253	6665.043656	26.264180
193.532619	6668.678504	26.269197
193.581630	6684.870088	26.274215
193.788600	6678.341684	26.279232
193.928614	6681.067465	26.284250
194.159729	6707.343963	26.289268
194.571477	6707.653140	26.294285
194.660293	6725.105511	26.299303
194.787009	6723.573866	26.304320
195.475656	6736.457800	26.309338
194.954215	6746.679725	26.314356
195.013541	6741.340679	26.319373
195.465965	6767.754713	26.324391
195.690576	6763.531976	26.329408
195.791773	6768.606689	26.334426
195.824495	6789.380515	26.339444
196.149349	6799.007896	26.344461
196.274226	6810.633597	26.349479
196.325001	6828.141214	26.354496
196.564862	6838.300970	26.359514
196.382665	6859.464125	26.364532
196.928276	6870.706731	26.369549
197.078230	6891.712547	26.374567
197.660872	6898.374297	26.379584
197.896251	6904.798951	26.384602
197.745640	6926.276757	26.389620
198.018133	6925.279414	26.394637
198.139295	6935.198165	26.399655
198.512660	6954.598052	26.404672
198.786820	6958.255538	26.409690
199.145480	6978.882710	26.414708
199.195554	6978.152183	26.419725
199.138200	6993.757549	26.424743
199.140388	7017.090347	26.429760
199.703154	7018.145659	26.434778
199.591915	7022.397062	26.439796
200.196351	7032.100392	26.444813
200.282928	7042.581030	26.449831
200.178032	7047.589917	26.454848
200.688999	7072.260316	26.459866
200.619142	7084.955031	26.464884
200.829482	7080.991354	26.469901
201.140846	7101.024732	26.474919
201.500728	7119.648044	26.479936
201.591247	7112.832335	26.484954
201.710844	7131.986159	26.489972
202.103430	7137.749230	26.494989
202.393438	7146.594129	26.500007
202.388817	7164.133341	26.505024
202.879158	7160.565967	26.510042
202.909695	7182.100775	26.515060
203.176801	7191.351993	26.520077
203.477860	7194.463948	26.525095
203.439011	7197.981901	26.530112
203.660406	7213.643736	26.535130
203.856838	7231.715294	26.540148
203.917148	7247.860684	26.545165
204.425700	7250.526343	26.550183
204.420010	7253.571725	26.555200
204.688569	7279.768142	26.560218
204.883850	7284.591142	26.565236
205.392532	7301.261788	26.570253
205.759016	7315.799313	26.575271
205.576388	7320.851872	26.580288
205.854437	7324.856957	26.585306
205.742282	7349.951529	26.590324
205.839493	7351.981109	26.595341
206.321452	7372.137037	26.600359
206.408238	7381.668702	26.605376
206.745406	7401.863603	26.610394
206.888810	7413.347258	26.615412
207.318886	7420.232197	26.620429
207.259777	7438.972506	26.625447
207.274580	7453.401384	26.630464
207.838766	7458.089325	26.635482
207.690871	7470.813019	26.640500
208.168888	7489.451868	26.645517
208.428210	7502.694220	26.650535
208.603154	7512.973069	26.655552
209.003052	7517.414107	26.660570
209.258887	7530.199410	26.665588
209.310517	7549.608386	26.670605
209.623180	7556.691628	26.675623
209.713544	7552.987155	26.680640
210.360837	7567.526475	26.685658
210.275662	7590.183765	26.690676
210.234066	7588.288414	26.695693
210.565837	7604.549919	26.700711
210.554402	7623.159670	26.705728
211.038788	7635.191992	26.710746
211.036271	7651.776701	26.715764
210.961616	7658.972943	26.720781
211.727094	7676.949231	26.725799
211.530392	7691.191993	26.730816
212.032829	7704.434441	26.735834
212.209514	7720.217607	26.740852
212.316195	7740.289613	26.745869
212.477816	7743.961187	26.750887
212.626279	7767.888430	26.755904
213.020352	7773.512064	26.760922
213.165742	7786.780603	26.765940
213.842714	7798.646471	26.770957
214.029551	7807.984595	26.775975
214.270350	7815.487095	26.780992
214.650925	7806.790864	26.786010
214.510004	7816.596008	26.791028
214.567476	7834.655807	26.796045
215.124801	7832.069713	26.801063
214.986058	7836.979684	26.806080
215.332882	7845.602887	26.811098
216.002709	7856.981602	26.816116
215.867819	7859.561681	26.821133
216.460585	7864.065416	26.826151
216.122331	7866.559429	26.831168
216.792982	7877.969531	26.836186
216.633582	7892.639538	26.841204
216.768192	7890.499938	26.846221
217.248421	7905.668249	26.851239
216.958878	7914.439370	26.856256
217.105886	7922.231571	26.861274
217.193970	7944.801604	26.866292
217.370238	7960.107721	26.871309
218.099052	7975.930503	26.876327
218.003115	7989.203712	26.881344
217.842977	8008.818450	26.886362
218.463334	8020.665499	26.891380
218.558763	8041.679497	26.896397
218.651294	8054.003080	26.901415
218.637894	8072.719235	26.906432
219.216604	8095.026300	26.911450
219.229836	8118.219454	26.916468
219.873243	8130.566125	26.921485
220.032635	8142.572284	26.926503
219.735887	8169.271786	26.931520
220.422803	8184.618836	26.936538
220.838415	8203.900611	26.941556
220.844009	8211.546213	26.946573
221.536566	8229.679355	26.951591
221.391587	8244.668691	26.956608
221.841641	8258.993163	26.961626
222.117180	8270.510704	26.966644
222.160683	8279.747582	26.971661
222.790678	8302.701054	26.976679
222.620541	8306.668722	26.981696
223.091659	8324.341570	26.986714
223.263256	8337.802375	26.991732
223.339377	8337.820549	26.996749
223.922092	8343.554952	27.001767
223.910313	8360.772118	27.006784
224.205197	8361.173153	27.011802
224.399553	8377.963135	27.016820
224.650780	8391.704629	27.021837
224.927340	8394.185175	27.026855
225.325883	8414.300305	27.031872
225.024586	8421.554889	27.036890
225.201519	8428.209616	27.041908
225.372615	8444.666365	27.046925
225.898478	8450.717437	27.051943
226.091227	8475.051186	27.056960
226.693435	8481.258208	27.061978
226.805659	8490.076570	27.066996
226.843544	8507.507816	27.072013
227.196785	8503.255453	27.077031
227.153482	8517.342790	27.082048
227.259474	8534.806117	27.087066
227.693000	8552.019884	27.092084
227.825913	8561.401249	27.097101
228.251384	8568.964914	27.102119
227.893645	8579.087641	27.107136
228.297677	8603.500046	27.112154
228.414814	8611.576391	27.117172
228.769077	8630.830239	27.122189
228.944614	8631.947409	27.127207
229.178771	8667.415732	27.132224
229.149032	8668.609424	27.137242
229.746935	8688.217673	27.142260
230.101060	8706.727210	27.147277
230.533269	8712.387405	27.152295
230.498064	8734.945090	27.157312
230.731404	8731.608191	27.162330
230.592298	8747.896819	27.167348
231.200962	8770.674101	27.172365
231.351874	8768.103147	27.177383
231.393502	8797.893978	27.182400
231.616349	8803.278487	27.187418
232.081112	8818.813387	27.192436
231.882996	8841.386372	27.197453
232.517212	8854.173911	27.202471
232.498554	8868.411091	27.207488
233.203275	8883.347810	27.212506
233.806570	8884.757348	27.217524
233.612087	8907.247109	27.222541
233.989381	8924.170448	27.227559
234.414221	8936.544476	27.232576
234.399663	8952.069833	27.237594
234.445697	8951.094103	27.242612
234.535341	8969.082898	27.247629
235.119254	8979.923632	27.252647
234.942732	8996.577927	27.257664
235.048027	9001.862222	27.262682
235.517569	9021.657561	27.267700
235.520977	9044.742608	27.272717
236.189153	9053.004468	27.277735
236.392139	9077.641517	27.282752
236.325888	9090.117439	27.287770
236.945182	9097.141159	27.292788
237.242647	9117.279422	27.297805
237.689253	9130.513397	27.302823
237.853810	9139.985184	27.307840
238.024445	9145.035770	27.312858
238.620860	9152.428830	27.317876
238.513408	9157.764148	27.322893
238.958731	9169.117949	27.327911
239.205441	9188.621879	27.332928
239.327119	9186.477946	27.337946
239.603582	9189.622729	27.342964
239.532290	9211.170825	27.347981
240.182853	9209.764932	27.352999
240.273359	9227.250484	27.358016
240.263485	9234.081422	27.363034
240.702120	9243.928575	27.368052
240.737911	9271.080618	27.373069
240.819932	9272.384262	27.378087
241.346567	9293.616065	27.383104
241.620164	9308.606431	27.388122
241.710616	9319.473937	27.393140
241.863766	9339.533957	27.398157
242.224189	9342.479743	27.403175
242.351390	9366.435745	27.408192
242.080397	9378.786649	27.413210
242.906664	9396.625629	27.418228
243.369626	9417.331653	27.423245
243.370168	9424.337412	27.428263
243.716844	9436.627869	27.433280
243.969960	9465.902019	27.438298
244.380101	9464.048261	27.443316
244.367310	9478.331490	27.448333
244.515692	9479.611562	27.453351
244.796845	9493.054417	27.458368
244.910729	9503.684195	27.463386
245.223213	9514.174754	27.468404
245.314086	9529.353920	27.473421
245.823664	9547.731559	27.478439
245.831668	9559.067432	27.483456
245.921935	9582.025431	27.488474
246.287544	9593.083126	27.493492
246.512934	9603.261225	27.498509
246.704074	9610.445068	27.503527
247.125240	9645.988590	27.508544
247.279790	9644.790029	27.513562
247.821161	9662.555145	27.518580
247.689906	9678.256505	27.523597
248.139703	9694.358012	27.528615
248.529117	9709.723483	27.533632
248.139775	9736.070648	27.538650
248.895156	9747.590183	27.543668
248.867199	9775.278306	27.548685
248.998185	9788.880194	27.553703
249.218541	9809.564648	27.558720
249.844854	9828.364458	27.563738
250.420615	9840.469985	27.568756
250.357849	9861.221855	27.573773
250.704617	9868.608517	27.578791
251.068499	9875.596083	27.583808
251.210519	9898.014195	27.588826
251.764769	9912.243337	27.593844
252.066729	9929.603266	27.598861
252.296533	9937.574183	27.603879
252.546180	9952.818065	27.608896
252.602191	9966.094542	27.613914
253.156689	9967.189258	27.618932
252.980602	9982.836885	27.623949
253.577412	9989.236837	27.628967
253.902905	10002.858705	27.633984
253.935771	10021.205504	27.639002
254.016371	10030.256841	27.644020
254.070089	10054.188216	27.649037
254.548301	10068.751514	27.654055
254.916961	10081.596604	27.659072
254.960899	10098.326628	27.664090
255.301465	10107.625682	27.669108
255.481274	10130.876893	27.674125
255.748245	10152.273354	27.679143
256.222411	10157.177115	27.684160
256.135128	10187.307778	27.689178
256.674809	10191.562567	27.694196
256.873175	10220.527297	27.699213
257.129736	10228.179587	27.704231
257.258688	10243.918784	27.709248
257.279575	10272.916926	27.714266
258.222580	10270.536054	27.719284
258.323074	10292.054010	27.724301
258.692327	10312.312671	27.729319
258.752785	10324.598403	27.734336
259.117075	10338.495391	27.739354
259.176652	10356.905117	27.744372
259.385101	10363.098490	27.749389
259.610658	10381.669849	27.754407
259.759726	10393.580138	27.759424
260.146257	10414.154353	27.764442
260.886639	10425.984908	27.769460
260.991478	10435.974713	27.774477
261.154032	10448.837669	27.779495
261.700026	10464.456840	27.784512
261.826594	10474.877172	27.789530
261.957739	10481.552939	27.794548
262.239081	10490.607546	27.799565
262.841800	10496.242521	27.804583
262.581310	10492.311827	27.809600
263.012018	10520.961319	27.814618
263.577449	10516.234483	27.819636
263.294332	10526.000212	27.824653
263.870779	10538.734066	27.829671
263.995230	10557.629623	27.834688
264.037239	10569.308017	27.839706
264.490681	10581.392599	27.844724
264.287996	10593.119392	27.849741
264.643245	10610.202581	27.854759
264.917625	10628.057082	27.859776
265.150358	10652.840527	27.864794
265.516970	10660.529169	27.869812
265.612832	10690.030903	27.874829
265.537944	10708.395532	27.879847
265.967648	10724.696001	27.884864
266.498801	10751.495947	27.889882
266.567112	10772.154808	27.894900
266.849391	10800.707250	27.899917
267.309586	10814.220058	27.904935
267.664947	10830.025560	27.909952
267.943110	10858.433819	27.914970
268.512470	10862.939143	27.919988
268.377054	10889.391120	27.925005
268.778710	10909.582141	27.930023
269.014139	10931.567088	27.935040
269.354564	10950.220936	27.940058
269.797797	10955.293940	27.945076
270.341739	10980.768542	27.950093
270.237405	10989.967633	27.955111
271.067237	11000.067839	27.960128
271.049784	11005.455050	27.965146
271.453912	11024.303284	27.970164
271.916571	11033.463698	27.975181
271.796613	11043.034127	27.980199
272.347386	11058.328484	27.985216
271.987162	11063.934753	27.990234
272.488693	11094.952116	27.995252
272.538730	11103.407182	28.000269
272.754712	11124.385562	28.005287
273.555556	11138.849156	28.010304
273.759408	11173.579547	28.015322
273.887103	11168.263957	28.020340
274.160672	11190.721970	28.025357
274.233394	11198.480002	28.030375
274.711916	11210.907571	28.035392
274.709183	11246.494855	28.040410
274.975583	11254.124734	28.045428
275.162912	11276.709020	28.050445
275.573641	11298.977451	28.055463
276.073805	11320.433774	28.060480
275.812450	11337.569373	28.065498
276.430365	11352.972655	28.070516
277.010239	11379.095881	28.075533
277.113212	11393.048065	28.080551
277.633907	11400.957378	28.085568
277.765524	11435.506469	28.090586
277.977528	11446.244986	28.095604
278.541052	11457.571393	28.100621
278.298018	11483.489056	28.105639
279.276347	11487.775591	28.110656
279.535424	11502.523010	28.115674
279.728978	11508.502621	28.120692
279.892289	11518.970334	28.125709
280.247487	11527.245897	28.130727
280.586001	11533.989413	28.135744
280.807993	11543.325473	28.140762
281.106005	11555.737490	28.145780
281.350466	11566.620415	28.150797
281.195487	11571.948637	28.155815
281.732010	11580.474703	28.160832
281.805050	11598.289543	28.165850
281.871880	11611.308729	28.170868
282.239031	11633.398891	28.175885
282.488251	11655.426663	28.180903
282.835872	11662.102543	28.185920
282.932957	11697.909089	28.190938
283.342641	11716.044952	28.195956
283.660157	11729.397778	28.200973
283.934416	11750.357869	28.205991
284.376545	11757.642164	28.211008
284.489155	11793.228890	28.216026
284.735037	11801.806333	28.221044
285.260294	11819.119520	28.226061
285.444357	11833.584982	28.231079
285.980701	11852.617155	28.236096
286.109243	11875.078064	28.241114
286.211142	11886.036803	28.246132
286.606239	11904.742586	28.251149
286.526533	11930.395979	28.256167
287.261814	11946.464309	28.261184
287.151628	11967.546621	28.266202
287.696709	11984.522630	28.271220
287.898214	12007.037828	28.276237
287.790965	12030.214009	28.281255
288.231377	12043.945438	28.286272
288.459679	12075.178523	28.291290
289.004945	12102.733202	28.296308
289.552125	12123.878674	28.301325
289.809868	12144.821524	28.306343
290.456832	12165.767737	28.311360
290.541337	12185.848963	28.316378
290.756583	12200.319045	28.321396
290.888364	12207.984265	28.326413
291.159139	12235.838317	28.331431
291.715769	12244.911380	28.336448
292.045261	12273.658740	28.341466
292.325282	12290.540268	28.346484
292.748049	12308.201873	28.351501
292.775683	12326.032907	28.356519
293.191702	12337.961115	28.361536
293.265018	12360.313646	28.366554
293.667560	12375.586515	28.371572
293.969749	12390.485194	28.376589
294.155488	12421.259533	28.381607
294.262854	12438.469208	28.386624
294.490629	12462.693660	28.391642
294.915411	12493.431721	28.396660
295.337662	12502.468865	28.401677
295.433584	12529.996215	28.406695
295.807378	12537.599470	28.411712
296.255128	12561.155732	28.416730
296.351896	12580.857204	28.421748
297.274109	12607.285053	28.426765
297.362307	12622.416351	28.431783
297.649392	12633.715276	28.436800
297.842944	12654.894761	28.441818
298.125331	12675.547403	28.446836
298.180010	12695.497092	28.451853
298.352142	12718.965252	28.456871
299.081260	12732.004938	28.461888
299.647048	12751.663655	28.466906
299.630400	12773.703858	28.471924
299.810280	12783.679540	28.476941
299.930992	12809.721911	28.481959
300.259912	12823.721449	28.486976
300.277099	12846.370753	28.491994
300.607273	12870.441760	28.497012
301.106735	12890.685255	28.502029
301.151605	12912.091401	28.507047
301.699771	12931.486923	28.512064
302.093268	12941.181501	28.517082
302.142484	12964.942994	28.522100
302.701145	12992.224334	28.527117
302.833767	13013.154342	28.532135
303.245417	13032.539487	28.537152
303.573986	13057.296564	28.542170
303.387457	13077.037647	28.547188
304.100717	13102.485991	28.552205
304.548359	13117.621291	28.557223
304.863801	13130.507563	28.562240
305.151634	13163.679166	28.567258
305.126839	13184.974277	28.572276
305.789592	13201.724062	28.577293
305.732906	13233.350096	28.582311
306.467967	13249.087237	28.587328
306.971087	13276.745443	28.592346
306.961586	13302.001690	28.597364
307.271164	13314.682629	28.602381
307.596569	13335.147755	28.607399
308.015166	13363.340163	28.612416
308.388360	13377.961659	28.617434
308.488754	13398.089028	28.622452
309.271605	13420.287750	28.627469
309.390581	13442.588505	28.632487
309.944089	13444.674929	28.637504
310.488951	13464.651591	28.642522
310.300006	13476.709137	28.647540
310.815725	13492.637264	28.652557
310.877343	13517.565303	28.657575
311.546561	13530.142757	28.662592
311.845859	13553.783339	28.667610
312.192369	13571.655939	28.672628
312.562052	13582.673937	28.677645
312.357083	13594.582928	28.682663
312.794545	13612.408998	28.687680
312.971812	13629.557930	28.692698
312.964825	13655.476221	28.697716
314.003876	13680.928283	28.702733
313.818098	13697.918314	28.707751
314.095251	13725.587892	28.712768
314.785711	13747.343739	28.717786
315.103107	13766.239464	28.722804
315.567534	13786.478843	28.727821
315.420919	13805.104693	28.732839
315.806555	13827.240485	28.737856
315.798583	13849.862248	28.742874
316.015774	13871.654042	28.747892
316.742271	13895.010075	28.752909
316.967470	13922.548320	28.757927
317.331638	13950.240125	28.762944
317.893424	13971.429715	28.767962
318.099122	13999.786120	28.772980
318.494452	14017.778786	28.777997
318.693644	14040.826722	28.783015
318.807649	14064.126770	28.788032
319.388103	14078.590085	28.793050
319.376975	14106.632684	28.798068
319.953331	14124.595505	28.803085
320.458557	14149.605535	28.808103
320.528358	14162.780719	28.813120
321.162139	14179.624568	28.818138
321.242941	14200.714398	28.823156
321.533783	14215.963356	28.828173
321.524392	14238.341604	28.833191
321.578169	14253.766950	28.838208
322.314997	14275.396050	28.843226
322.408068	14303.757437	28.848244
322.740492	14323.373150	28.853261
323.485453	14352.641703	28.858279
323.472803	14372.295676	28.863296
324.023122	14403.390087	28.868314
324.084098	14427.224256	28.873332
324.555026	14442.602801	28.878349
324.649169	14472.056513	28.883367
325.401877	14489.122136	28.888384
325.834806	14512.433079	28.893402
325.622941	14544.664169	28.898420
326.359144	14552.581918	28.903437
326.715112	14588.738098	28.908455
326.811840	14606.456163	28.913472
327.512324	14629.708804	28.918490
327.824592	14650.507153	28.923508
328.061946	14656.620948	28.928525
328.525124	14685.194400	28.933543
328.745574	14700.001548	28.938560
329.162060	14725.730082	28.943578
329.387019	14745.997676	28.948596
329.945044	14764.809022	28.953613
330.013229	14795.125005	28.958631
329.786548	14817.231090	28.963648
330.502384	14840.710025	28.968666
330.664604	14860.414444	28.973684
331.044556	14896.167002	28.978701
331.506732	14918.291603	28.983719
331.839523	14948.234666	28.988736
332.374635	14975.754910	28.993754
332.310304	15009.056314	28.998772
332.772206	15019.467401	29.003789
333.049404	15056.859141	29.008807
333.515651	15067.554818	29.013824
333.933642	15098.845824	29.018842
334.244098	15132.306104	29.023860
334.933527	15148.410419	29.028877
335.114245	15185.433845	29.033895
335.349963	15204.899549	29.038912
335.590047	15227.488457	29.043930
336.003380	15250.518413	29.048948
336.458520	15267.839000	29.053965
336.558436	15293.986485	29.058983
336.742703	15321.804951	29.064000
337.485900	15348.416619	29.069018
337.555629	15369.535000	29.074036
338.026604	15391.926729	29.079053
338.596339	15419.222901	29.084071
338.774642	15448.577745	29.089088
339.007691	15466.348253	29.094106
339.348723	15487.502267	29.099124
339.449392	15505.009442	29.104141
339.924108	15538.024101	29.109159
340.112494	15569.346124	29.114176
340.801905	15602.120475	29.119194
341.259733	15626.724495	29.124212
341.459461	15644.535387	29.129229
341.691600	15668.800117	29.134247
342.028806	15688.575866	29.139264
342.699736	15713.281873	29.144282
342.795852	15745.354004	29.149300
343.257373	15761.176678	29.154317
343.624311	15784.604380	29.159335
343.757839	15813.636284	29.164352
344.486779	15819.431147	29.169370
344.361023	15829.886423	29.174388
344.544497	15862.752911	29.179405
345.221542	15874.538057	29.184423
345.508202	15904.492073	29.189440
345.988998	15923.374275	29.194458
346.092386	15943.951912	29.199476
346.288914	15966.462352	29.204493
346.467709	15987.580812	29.209511
346.875753	16023.936437	29.214528
347.472301	16047.217750	29.219546
347.527559	16078.614789	29.224564
347.781651	16105.713723	29.229581
348.409925	16138.887014	29.234599
348.765032	16156.467833	29.239616
349.394779	16181.827614	29.244634
349.573522	16216.762027	29.249652
349.977390	16238.221852	29.254669
350.112663	16261.904518	29.259687
350.304254	16277.532777	29.264704
350.750147	16305.572833	29.269722
351.046724	16340.793796	29.274740
351.898978	16367.199916	29.279757
352.265690	16397.067493	29.284775
352.529144	16420.051384	29.289792
353.018592	16440.386051	29.294810
352.992125	16461.813357	29.299828
353.504273	16488.469841	29.304845
353.938857	16516.573602	29.309863
354.084111	16546.854829	29.314880
354.801456	16565.496855	29.319898
354.966834	16598.019447	29.324916
355.329183	16608.960310	29.329933
355.892202	16639.821987	29.334951
356.322511	16676.489041	29.339968
357.062555	16687.097902	29.344986
356.792387	16712.292185	29.350004
357.339526	16738.640636	29.355021
357.722737	16756.141783	29.360039
358.044377	16787.738827	29.365056
358.427276	16809.866483	29.370074
358.839162	16836.456579	29.375092
359.204866	16851.269995	29.380109
359.224421	16874.499802	29.385127
359.456561	16907.104952	29.390144
359.811903	16930.435317	29.395162
360.381292	16956.140455	29.400180
360.444970	16981.015073	29.405197
361.004464	17019.160572	29.410215
361.057546	17047.158134	29.415232
361.631433	17080.265078	29.420250
362.035634	17115.477759	29.425268
362.306757	17144.271694	29.430285
363.116495	17168.602240	29.435303
363.183412	17195.918368	29.440320
363.766331	17219.183101	29.445338
363.866116	17246.358308	29.450356
364.238997	17274.424703	29.455373
364.828836	17292.959397	29.460391
365.381253	17327.960416	29.465408
365.774079	17346.411127	29.470426
365.898440	17369.882801	29.475444
366.366278	17393.162096	29.480461
366.605071	17411.392463	29.485479
366.907220	17442.051326	29.490496
367.084522	17460.200496	29.495514
367.703398	17486.011765	29.500532
368.057259	17514.169989	29.505549
368.548809	17531.869987	29.510567
368.641235	17556.625635	29.515584
369.185395	17579.566254	29.520602
369.175755	17597.213703	29.525620
369.667018	17629.246153	29.530637
370.096477	17655.601353	29.535655
370.075121	17699.305091	29.540672
370.470147	17703.901102	29.545690
371.010987	17743.857880	29.550708
371.137757	17773.266361	29.555725
371.913541	17793.700332	29.560743
372.008499	17825.962694	29.565760
372.738647	17860.137770	29.570778
372.723818	17889.798469	29.575796
373.429017	17923.776027	29.580813
373.781287	17935.201814	29.585831
374.306813	17974.745513	29.590848
374.451549	18006.959001	29.595866
374.895253	18027.240135	29.600884
375.219323	18060.478660	29.605901
375.827595	18079.570810	29.610919
375.922674	18116.283917	29.615936
376.451042	18139.874254	29.620954
376.581870	18175.758687	29.625972
377.130272	18203.810215	29.630989
377.466212	18232.484959	29.636007
377.492352	18274.167674	29.641024
378.286006	18294.719115	29.646042
378.789235	18327.187600	29.651060
378.738834	18358.847630	29.656077
379.671626	18383.695587	29.661095
379.873454	18426.186694	29.666112
380.334537	18446.667248	29.671130
380.723764	18471.904821	29.676148
381.316409	18507.199615	29.681165
382.041270	18516.874187	29.686183
382.157245	18552.593208	29.691200
382.746249	18567.702258	29.696218
382.687475	18595.758771	29.701236
383.049970	18624.938992	29.706253
383.108954	18642.092215	29.711271
383.741512	18687.031887	29.716288
384.262039	18715.834561	29.721306
384.748597	18743.249305	29.726324
385.062521	18772.570246	29.731341
385.696618	18796.505029	29.736359
385.882739	18829.750578	29.741376
386.195167	18850.161643	29.746394
386.762465	18887.160883	29.751412
386.776905	18912.081217	29.756429
387.383113	18937.400245	29.761447
387.787147	18964.343452	29.766464
387.901828	18990.692956	29.771482
388.396112	19023.507954	29.776500
388.939935	19052.969484	29.781517
389.772226	19081.180453	29.786535
389.690038	19111.970633	29.791552
389.962543	19133.156410	29.796570
390.458191	19159.600782	29.801588
390.980235	19189.811847	29.806605
391.372312	19221.311995	29.811623
391.166797	19245.403719	29.816640
391.737661	19279.582847	29.821658
392.300945	19313.752265	29.826676
392.289791	19347.428775	29.831693
393.097061	19377.004929	29.836711
393.244194	19404.338199	29.841728
393.403961	19445.267052	29.846746
394.238505	19474.890892	29.851764
394.509290	19502.686279	29.856781
394.671212	19517.994575	29.861799
394.943412	19558.181463	29.866816
395.169968	19589.269839	29.871834
395.787095	19614.701600	29.876852
396.136598	19645.886400	29.881869
396.583518	19683.266780	29.886887
396.784114	19732.930028	29.891904
397.284942	19748.045285	29.896922
398.211232	19789.295867	29.901940
398.329024	19821.324967	29.906957
398.632836	19853.391136	29.911975
399.138247	19881.854628	29.916992
399.399883	19911.865724	29.922010
400.261668	19948.495378	29.927028
400.625913	19979.558539	29.932045
400.973970	20007.838600	29.937063
401.294024	20038.461431	29.942080
401.772371	20071.369411	29.947098
402.220941	20097.490396	29.952116
402.328239	20137.280279	29.957133
403.130126	20160.076169	29.962151
403.292335	20206.106789	29.967168
403.476162	20229.764984	29.972186
404.244381	20270.202577	29.977204
404.147359	20296.149291	29.982221
404.587896	20326.467340	29.987239
405.199458	20361.663592	29.992256
405.506176	20409.632173	29.997274
405.952745	20436.085107	30.002292
406.343084	20472.670951	30.007309
407.022722	20499.285646	30.012327
407.135568	20546.167289	30.017344
407.874668	20576.288175	30.022362
408.551064	20608.782885	30.027380
408.893012	20649.061744	30.032397
409.061063	20667.085065	30.037415
409.492825	20703.051238	30.042432
410.119974	20741.813678	30.047450
410.672144	20767.046666	30.052468
410.876067	20798.763807	30.057485
411.342496	20822.141144	30.062503
411.324236	20861.794274	30.067520
411.882345	20893.049350	30.072538
412.477751	20924.498550	30.077556
412.963822	20963.005775	30.082573
413.002805	20985.725652	30.087591
413.419337	21025.617819	30.092608
413.907363	21062.284955	30.097626
414.512802	21107.453188	30.102644
414.948505	21130.602688	30.107661
415.537662	21162.433350	30.112679
415.629557	21196.187952	30.117696
416.073717	21229.368742	30.122714
416.802760	21263.768548	30.127732
417.127009	21297.349302	30.132749
417.897582	21318.986763	30.137767
417.781062	21354.819592	30.142784
418.315688	21383.354899	30.147802
418.760725	21408.671225	30.152820
419.488767	21444.764965	30.157837
420.071261	21468.347887	30.162855
420.098723	21502.298240	30.167872
420.041585	21535.847980	30.172890
420.548088	21571.865130	30.177908
420.698553	21609.205822	30.182925
421.182068	21635.810625	30.187943
421.638179	21665.284950	30.192960
421.698417	21704.682670	30.197978
422.416605	21730.490369	30.202996
422.719681	21776.681710	30.208013
423.506725	21807.586821	30.213031
424.027424	21844.154068	30.218048
424.581572	21884.353455	30.223066
424.901416	21906.744272	30.228084
425.220671	21948.715552	30.233101
425.593393	21967.182575	30.238119
425.906350	22003.205869	30.243136
426.200831	22044.380483	30.248154
426.800278	22073.781343	30.253172
427.162088	22108.467548	30.258189
427.578900	22143.840085	30.263207
427.980429	22190.071448	30.268224
428.106430	22236.376915	30.273242
428.928161	22266.201750	30.278260
429.288722	22316.366471	30.283277
429.481512	22356.842803	30.288295
430.070115	22388.795706	30.293312
430.559408	22434.962754	30.298330
430.735328	22474.166513	30.303348
431.365930	22522.680375	30.308365
431.833706	22551.138838	30.313383
432.210544	22589.270484	30.318400
432.507424	22636.095923	30.323418
433.415686	22671.105978	30.328436
433.438245	22718.721308	30.333453
433.723454	22751.444143	30.338471
434.660407	22790.598379	30.343488
435.099518	22830.393298	30.348506
435.510934	22870.779485	30.353524
435.825640	22915.365183	30.358541
436.395434	22958.281459	30.363559
437.329412	22983.435655	30.368576
437.307492	23030.232939	30.373594
438.066846	23067.099203	30.378612
438.649888	23095.864340	30.383629
438.738488	23125.050379	30.388647
439.472309	23167.544243	30.393664
439.576735	23201.827439	30.398682
440.272553	23231.458777	30.403700
440.482178	23263.542272	30.408717
440.748202	23299.793693	30.413735
441.223267	23338.656637	30.418752
441.668710	23387.418068	30.423770
442.545954	23421.419279	30.428788
442.937092	23456.775146	30.433805
443.379590	23498.822897	30.438823
443.853903	23528.133449	30.443840
443.666627	23564.756908	30.448858
444.640040	23597.960405	30.453876
444.562211	23645.599667	30.458893
445.374269	23683.977129	30.463911
445.747884	23724.647559	30.468928
446.036912	23765.995975	30.473946
446.725706	23796.408469	30.478964
447.134849	23835.493188	30.483981
447.825826	23869.472503	30.488999
447.959112	23902.374076	30.494016
448.384325	23955.935993	30.499034
448.961941	23978.122879	30.504052
449.329963	24027.439848	30.509069
450.108853	24061.152684	30.514087
450.613880	24094.440968	30.519104
450.934571	24129.368335	30.524122
451.498814	24154.575991	30.529140
451.912055	24189.068689	30.534157
452.089234	24223.209429	30.539175
452.660608	24257.909491	30.544192
453.440191	24289.477964	30.549210
453.611585	24300.753507	30.554228
453.866228	24334.632486	30.559245
454.451617	24366.640102	30.564263
454.750297	24393.390202	30.569280
455.117241	24437.491826	30.574298
455.565087	24466.377848	30.579316
456.063021	24504.049023	30.584333
456.280139	24539.193069	30.589351
456.671038	24571.769437	30.594368
456.663029	24626.089565	30.599386
457.707852	24673.116957	30.604404
458.083925	24717.457498	30.609421
458.604628	24754.513569	30.614439
459.141670	24797.651215	30.619456
459.685132	24837.614907	30.624474
460.118439	24877.205813	30.629492
460.265325	24914.122228	30.634509
460.705538	24951.879637	30.639527
461.278964	25002.849713	30.644544
461.354784	25050.303437	30.649562
462.259720	25087.088473	30.654580
462.630510	25148.397033	30.659597
463.069233	25185.546455	30.664615
463.641566	25229.398491	30.669632
464.065910	25284.503929	30.674650
464.524068	25315.859383	30.679668
464.974281	25362.608565	30.684685
465.373484	25420.661442	30.689703
466.151194	25462.672741	30.694720
466.200211	25508.561377	30.699738
466.665158	25546.735510	30.704756
467.359368	25602.150579	30.709773
467.989098	25654.608369	30.714791
468.781556	25695.703072	30.719808
468.618794	25739.403633	30.724826
469.388057	25781.934406	30.729844
469.863060	25832.686660	30.734861
470.249044	25875.798388	30.739879
470.966467	25913.641363	30.744896
471.432514	25970.142591	30.749914
471.708134	26009.992462	30.754932
472.348094	26050.491853	30.759949
472.724088	26089.574575	30.764967
473.407233	26127.922074	30.769984
473.865037	26172.476798	30.775002
474.778911	26223.949316	30.780020
475.039921	26250.951425	30.785037
475.335880	26294.987546	30.790055
475.831386	26333.398096	30.795072
476.613317	26369.890801	30.800090
476.814876	26405.485997	30.805108
477.431218	26442.334310	30.810125
477.417120	26492.144269	30.815143
478.064206	26530.990715	30.820160
478.696664	26575.864561	30.825178
479.252098	26612.013577	30.830196
479.699566	26654.678615	30.835213
480.267623	26707.499953	30.840231
480.664549	26737.587435	30.845248
480.754694	26784.608247	30.850266
481.609339	26813.869366	30.855284
482.112393	26858.131316	30.860301
482.258575	26893.752452	30.865319
483.206264	26929.215797	30.870336
483.470917	26973.252517	30.875354
483.845389	27013.403791	30.880372
484.279917	27039.583492	30.885389
484.869325	27082.131463	30.890407
485.410618	27124.078682	30.895424
485.921504	27160.807181	30.900442
486.156761	27195.379521	30.905460
486.710763	27234.536321	30.910477
487.235464	27280.540216	30.915495
487.862570	27313.126846	30.920512
487.693110	27351.132349	30.925530
488.232345	27400.367556	30.930548
488.921080	27438.657105	30.935565
489.058477	27497.826520	30.940583
489.697810	27536.026667	30.945600
489.782935	27582.993691	30.950618
490.432341	27638.056774	30.955636
490.712974	27688.420767	30.960653
491.463857	27749.375972	30.965671
492.093347	27800.108435	30.970688
492.412786	27855.441322	30.975706
492.925324	27906.001014	30.980724
493.851859	27947.725592	30.985741
494.104481	28007.303550	30.990759
494.642275	28048.209392	30.995776
495.302446	28105.849535	31.000794
496.317601	28148.197175	31.005812
496.782202	28184.314027	31.010829
496.994738	28247.905893	31.015847
497.817429	28282.086649	31.020864
498.137573	28329.338576	31.025882
498.557943	28373.832595	31.030900
499.440103	28411.089082	31.035917
500.086608	28465.814556	31.040935
500.331842	28495.851320	31.045952
500.652086	28549.990632	31.050970
501.140503	28579.129207	31.055988
501.962275	28628.797509	31.061005
501.862609	28681.211649	31.066023
502.647152	28717.617382	31.071040
503.261666	28774.648956	31.076058
503.595342	28816.278123	31.081076
504.357917	28859.612576	31.086093
504.413479	28909.515726	31.091111
505.087293	28950.063614	31.096128
505.242444	29008.888188	31.101146
505.761724	29062.882581	31.106164
506.901318	29106.486522	31.111181
506.892461	29158.748252	31.116199
507.810068	29198.142710	31.121216
508.326999	29248.516276	31.126234
508.482137	29294.261691	31.131252
509.306252	29339.161441	31.136269
509.599669	29390.187604	31.141287
510.233843	29437.450509	31.146304
510.596693	29493.393457	31.151322
510.814732	29543.085386	31.156340
512.178176	29582.078826	31.161357
512.198902	29639.542743	31.166375
512.839019	29683.091954	31.171392
513.012111	29734.883600	31.176410
513.777211	29775.901009	31.181428
514.228633	29822.157206	31.186445
514.604726	29868.277705	31.191463
515.506895	29906.997994	31.196480
515.673430	29964.574512	31.201498
516.286435	30003.674137	31.206516
517.254246	30045.396908	31.211533
517.216955	30090.718762	31.216551
517.827305	30130.333379	31.221568
518.548136	30175.807652	31.226586
518.324639	30224.842599	31.231604
518.997877	30270.350232	31.236621
519.333532	30329.651021	31.241639
520.151896	30364.010102	31.246656
520.487632	30411.366030	31.251674
520.742668	30469.115706	31.256692
521.826455	30511.129596	31.261709
522.212053	30571.647117	31.266727
522.723035	30615.765846	31.271744
523.200929	30671.340136	31.276762
523.468327	30732.584518	31.281780
524.041362	30780.665719	31.286797
524.467645	30835.968259	31.291815
525.272802	30875.833133	31.296832
525.657739	30945.997406	31.301850
526.053026	30993.767840	31.306868
527.028849	31045.499934	31.311885
527.083862	31112.397033	31.316903
527.704206	31162.822083	31.321920
528.268491	31217.951535	31.326938
528.839290	31288.468199	31.331956
529.727154	31335.877239	31.336973
529.895632	31393.095247	31.341991
530.783730	31449.910395	31.347008
531.264929	31507.869004	31.352026
531.453537	31567.835652	31.357044
532.581890	31608.292386	31.362061
532.698519	31667.192169	31.367079
533.521041	31725.565156	31.372096
533.946605	31778.482188	31.377114
534.512223	31836.102905	31.382132
535.160588	31884.875136	31.387149
535.610554	31943.824810	31.392167
536.247758	31991.772478	31.397184
536.766092	32051.036200	31.402202
537.084074	32110.162879	31.407220
537.841365	32156.314638	31.412237
538.387251	32223.393455	31.417255
539.298578	32260.271494	31.422272
539.652949	32309.349128	31.427290
540.069015	32366.131727	31.432308
540.629949	32415.058724	31.437325
541.217493	32480.894688	31.442343
541.368430	32532.903308	31.447360
542.157053	32586.920737	31.452378
542.754602	32646.400534	31.457396
543.645752	32680.638492	31.462413
543.639344	32744.222866	31.467431
544.491168	32791.537640	31.472448
545.270434	32848.567771	31.477466
545.490316	32900.502948	31.482484
546.273791	32945.409151	31.487501
546.914559	32995.217554	31.492519
547.390422	33059.900277	31.497536
547.897911	33101.283602	31.502554
547.993917	33165.556225	31.507572
549.197101	33216.057929	31.512589
549.365357	33275.247967	31.517607
549.176455	33322.805776	31.522624
549.993222	33381.560682	31.527642
550.570616	33439.970402	31.532660
551.237636	33499.586715	31.537677
551.609160	33559.643419	31.542695
552.349875	33619.828580	31.547712
553.020103	33660.526744	31.552730
553.698286	33714.594272	31.557748
554.105661	33756.629974	31.562765
554.690248	33812.799190	31.567783
555.037877	33863.513715	31.572800
555.669541	33911.344406	31.577818
556.166741	33969.478802	31.582836
557.227512	34026.431414	31.587853
557.641614	34076.352924	31.592871
557.668587	34123.896078	31.597888
558.548353	34184.621858	31.602906
558.802113	34231.619698	31.607924
559.242231	34289.770891	31.612941
559.690154	34343.771124	31.617959
560.048931	34411.984194	31.622976
561.060035	34469.091601	31.627994
561.335736	34535.447492	31.633012
562.204752	34594.428119	31.638029
562.489455	34665.693473	31.643047
562.942678	34730.543780	31.648064
563.699181	34786.712855	31.653082
564.235619	34850.502081	31.658100
564.792533	34913.167806	31.663117
565.511504	34969.302637	31.668135
566.042624	35046.436566	31.673152
566.902557	35104.189568	31.678170
567.293174	35176.787002	31.683188
568.384634	35227.802055	31.688205
568.884232	35282.686538	31.693223
569.650891	35338.540066	31.698240
570.196945	35388.591725	31.703258
570.487980	35451.407465	31.708276
570.963340	35512.649647	31.713293
571.767877	35563.088239	31.718311
572.279351	35633.250023	31.723328
572.858096	35680.469299	31.728346
573.463768	35746.686695	31.733364
573.882718	35802.122631	31.738381
574.238159	35869.527522	31.743399
574.845784	35930.717681	31.748416
575.698818	35984.289712	31.753434
576.469073	36046.097194	31.758452
577.145269	36107.488064	31.763469
577.608325	36160.544421	31.768487
578.156579	36214.341149	31.773504
578.932288	36267.582799	31.778522
579.493949	36338.805792	31.783540
580.319677	36389.659802	31.788557
580.892563	36435.408106	31.793575
581.346427	36490.098682	31.798592
581.642173	36546.289515	31.803610
581.999359	36614.918336	31.808628
582.956539	36666.322645	31.813645
583.181214	36724.836123	31.818663
583.737198	36787.416987	31.823680
584.418667	36848.541224	31.828698
585.185396	36914.158664	31.833716
585.616167	36970.438940	31.838733
586.221145	37028.192946	31.843751
586.784831	37098.468559	31.848768
587.352825	37153.265349	31.853786
587.754796	37224.890687	31.858804
588.473371	37286.903493	31.863821
588.991972	37335.481627	31.868839
589.559739	37405.344277	31.873856
590.510310	37459.797782	31.878874
590.698434	37519.345675	31.883892
590.996289	37584.683292	31.888909
591.883200	37641.584578	31.893927
592.246118	37699.327109	31.898944
592.969497	37753.452945	31.903962
592.952219	37826.810273	31.908980
593.638106	37892.656103	31.913997
594.507443	37956.540093	31.919015
594.797013	38019.731123	31.924032
595.749392	38082.367654	31.929050
596.087122	38148.066840	31.934068
596.918711	38210.161947	31.939085
597.558862	38281.051301	31.944103
597.757342	38347.948453	31.949120
598.561893	38415.364250	31.954138
599.346885	38492.593955	31.959156
600.032748	38556.122153	31.964173
600.515812	38622.783837	31.969191
601.085780	38683.462366	31.974208
601.693531	38756.615853	31.979226
602.226482	38816.780118	31.984244
602.594813	38878.992024	31.989261
603.505694	38954.365728	31.994279
604.351029	39027.035911	31.999296
605.078529	39089.236458	32.004314
605.727017	39158.420110	32.009332
606.373357	39218.708985	32.014349
607.232643	39273.782777	32.019367
607.598417	39340.368623	32.024384
608.368063	39398.702662	32.029402
609.222070	39467.869264	32.034420
609.539040	39530.208676	32.039437
609.859715	39591.575424	32.044455
610.591322	39662.464469	32.049472
611.237923	39720.949316	32.054490
611.814565	39793.165073	32.059508
612.666815	39866.942299	32.064525
613.458927	39924.377778	32.069543
613.751583	39983.272417	32.074560
614.584669	40042.283025	32.079578
614.980617	40105.877189	32.084596
615.700231	40176.104119	32.089613
616.410031	40245.534269	32.094631
617.068944	40319.465256	32.099648
617.747212	40375.269961	32.104666
618.073854	40445.692364	32.109684
618.610048	40497.192913	32.114701
619.592676	40573.868336	32.119719
619.764206	40647.265683	32.124736
620.358564	40715.558129	32.129754
621.010315	40780.056208	32.134772
621.576871	40843.621534	32.139789
621.721467	40921.687185	32.144807
622.462521	40999.300910	32.149824
623.574377	41067.171248	32.154842
623.851645	41144.455065	32.159860
624.453532	41218.317007	32.164877
625.362249	41282.610166	32.169895
625.952482	41358.305646	32.174912
626.781520	41423.389099	32.179930
627.344739	41497.321692	32.184948
627.793910	41567.330311	32.189965
628.554002	41631.816596	32.194983
629.336953	41711.892031	32.200000
630.011474	41779.853125	32.205018
630.823482	41850.620468	32.210036
631.349143	41912.870259	32.215053
632.088301	41976.631918	32.220071
632.550977	42044.594301	32.225088
633.073442	42106.415902	32.230106
633.721532	42166.947756	32.235124
634.163170	42228.088563	32.240141
634.702304	42291.852825	32.245159
635.015541	42366.812115	32.250176
635.771636	42428.450905	32.255194
636.525628	42503.037893	32.260212
637.444031	42575.315321	32.265229
637.813612	42629.690850	32.270247
638.029828	42708.992952	32.275264
638.963987	42773.883789	32.280282
639.574007	42842.872916	32.285300
640.143245	42914.795826	32.290317
640.762247	42992.254958	32.295335
641.430104	43068.790715	32.300352
642.196240	43139.895755	32.305370
642.868732	43212.137404	32.310388
643.299375	43287.737692	32.315405
644.667550	43362.387536	32.320423
644.691730	43431.005312	32.325440
645.509013	43501.894884	32.330458
645.890442	43581.056533	32.335476
646.485710	43667.160970	32.340493
647.104032	43737.051882	32.345511
647.581777	43830.719548	32.350528
648.486142	43901.653062	32.355546
649.074556	43971.925533	32.360564
649.955629	44067.286352	32.365581
650.673575	44140.291327	32.370599
650.906108	44228.172857	32.375616
651.409059	44321.257825	32.380634
652.139758	44384.069232	32.385652
652.525446	44479.198346	32.390669
653.595054	44555.102203	32.395687
654.161263	44652.810459	32.400704
655.018784	44728.074384	32.405722
655.947561	44809.594622	32.410740
656.564415	44893.607638	32.415757
657.616093	44965.846995	32.420775
658.129824	45051.431318	32.425792
658.589653	45127.031029	32.430810
659.418370	45198.146153	32.435828
660.083450	45277.255392	32.440845
660.698818	45346.268634	32.445863
661.250400	45432.587320	32.450880
661.640974	45507.075874	32.455898
662.601442	45588.471090	32.460916
663.043550	45676.542585	32.465933
664.423990	45749.668405	32.470951
664.837284	45834.537140	32.475968
665.184204	45906.713542	32.480986
666.378212	45979.192174	32.486004
667.040290	46068.814310	32.491021
667.644324	46139.846997	32.496039
668.040739	46217.668866	32.501056
668.798787	46288.272431	32.506074
669.402865	46365.327937	32.511092
670.033875	46452.452858	32.516109
670.795280	46531.264042	32.521127
671.642876	46605.709734	32.526144
672.017934	46689.350731	32.531162
673.034782	46761.249034	32.536180
673.111341	46849.708558	32.541197
674.134376	46917.523237	32.546215
674.369062	47018.364909	32.551232
675.215982	47094.666346	32.556250
676.324137	47174.954451	32.561268
676.808648	47261.077814	32.566285
677.646095	47325.034005	32.571303
678.017186	47394.073008	32.576320
678.918253	47471.554412	32.581338
679.513741	47539.448353	32.586356
680.318055	47620.031769	32.591373
680.844081	47678.150902	32.596391
681.346435	47757.739533	32.601408
681.876467	47831.712001	32.606426
682.736259	47907.130300	32.611444
683.133546	47995.693669	32.616461
683.776255	48059.100287	32.621479
684.591573	48141.124185	32.626496
685.398500	48226.270075	32.631514
686.013927	48302.229345	32.636532
686.553497	48395.053493	32.641549
687.264750	48464.703310	32.646567
687.810584	48559.883229	32.651584
688.631531	48638.210069	32.656602
689.446952	48723.157795	32.661620
690.002268	48807.182503	32.666637
690.668239	48890.267062	32.671655
691.325710	48971.196287	32.676672
692.006523	49064.761453	32.681690
692.781746	49131.762783	32.686708
693.451595	49234.429649	32.691725
694.612908	49316.293958	32.696743
695.143024	49402.372034	32.701760
695.381371	49485.725723	32.706778
696.587948	49567.030899	32.711796
697.135798	49662.408605	32.716813
697.762149	49749.571431	32.721831
698.700295	49835.849252	32.726848
699.487678	49924.319081	32.731866
700.609505	50003.037574	32.736884
701.348731	50086.724760	32.741901
701.923864	50164.634189	32.746919
702.774632	50236.614088	32.751936
703.213274	50326.766909	32.756954
704.125412	50405.458562	32.761972
704.346923	50486.185159	32.766989
705.261630	50568.995763	32.772007
705.946648	50659.646330	32.777024
706.386346	50736.692914	32.782042
707.535691	50812.194740	32.787060
707.967564	50914.385583	32.792077
708.879583	50994.260963	32.797095
709.775081	51072.774883	32.802112
710.313405	51161.860122	32.807130
711.140341	51239.457421	32.812148
711.464016	51327.662922	32.817165
712.514124	51412.286753	32.822183
713.088161	51499.763029	32.827200
713.507679	51580.695166	32.832218
714.497868	51653.074214	32.837236
714.846708	51750.848362	32.842253
715.802405	51839.817126	32.847271
716.338992	51927.566854	32.852288
717.212287	52022.665433	32.857306
718.338560	52104.923238	32.862324
718.617166	52190.872096	32.867341
719.659740	52273.542466	32.872359
720.320642	52354.425251	32.877376
720.901204	52449.182639	32.882394
721.962247	52526.777933	32.887412
722.483309	52620.642563	32.892429
723.107942	52693.446056	32.897447
724.088323	52774.378817	32.902464
724.381923	52868.831910	32.907482
725.724156	52945.295690	32.912500
726.429500	53025.295720	32.917517
726.985915	53087.062023	32.922535
727.450289	53174.507083	32.927552
727.946800	53254.548910	32.932570
728.958452	53333.596066	32.937588
729.634287	53415.921264	32.942605
730.283099	53484.781274	32.947623
730.807525	53563.511916	32.952640
731.270809	53643.023790	32.957658
732.435913	53724.694407	32.962676
732.790081	53810.625232	32.967693
733.545950	53902.782856	32.972711
734.153495	53992.905722	32.977728
734.762023	54087.944400	32.982746
736.092946	54174.157517	32.987764
736.733553	54263.814923	32.992781
737.234416	54356.035804	32.997799
738.071978	54440.480438	33.002816
738.441694	54538.884226	33.007834
739.525793	54622.379015	33.012852
740.161587	54724.631835	33.017869
740.626124	54819.735765	33.022887
741.716018	54916.240507	33.027904
742.329144	55014.442118	33.032922
743.232921	55102.473855	33.037940
743.737653	55199.910819	33.042957
744.419743	55298.626872	33.047975
745.543058	55392.708389	33.052992
745.695056	55499.158656	33.058010
746.641278	55597.655585	33.063028
747.348571	55704.299440	33.068045
748.552218	55797.699807	33.073063
749.169404	55891.873730	33.078080
749.807391	55995.510235	33.083098
751.270053	56099.510060	33.088116
751.517587	56189.904681	33.093133
752.246050	56286.918198	33.098151
753.495690	56378.872979	33.103168
754.474122	56478.898129	33.108186
755.231289	56567.813674	33.113204
755.909461	56652.698509	33.118221
756.682838	56738.673790	33.123239
757.685156	56829.268732	33.128256
757.860696	56928.885503	33.133274
759.000872	57005.253092	33.138292
759.916946	57095.130486	33.143309
760.582075	57185.883925	33.148327
761.423697	57267.414124	33.153344
761.949336	57372.485550	33.158362
762.755499	57452.208743	33.163380
763.576654	57546.679019	33.168397
764.330880	57638.999600	33.173415
764.860232	57717.493130	33.178432
765.784107	57817.534004	33.183450
766.748869	57903.975548	33.188468
767.132992	57998.596074	33.193485
767.964647	58093.199895	33.198503
768.897830	58181.088696	33.203520
769.765166	58273.829532	33.208538
770.331065	58363.568309	33.213556
770.935968	58460.164106	33.218573
771.755483	58549.343555	33.223591
772.755041	58649.553000	33.228608
773.407495	58748.392109	33.233626
774.341073	58833.970693	33.238644
775.209186	58920.299878	33.243661
775.605457	59025.843718	33.248679
776.447723	59102.041053	33.253696
776.788109	59197.496012	33.258714
777.990235	59286.343681	33.263732
778.594865	59373.476766	33.268749
778.959447	59461.894950	33.273767
779.988602	59549.508406	33.278784
780.228541	59650.853331	33.283802
780.804763	59736.058766	33.288820
781.876917	59840.825143	33.293837
782.647856	59942.380736	33.298855
783.298139	60038.173919	33.303872
783.701019	60146.705582	33.308890
784.646006	60253.195232	33.313908
785.615427	60363.334465	33.318925
786.401283	60475.457602	33.323943
787.376878	60567.135572	33.328960
788.125501	60681.895227	33.333978
788.799494	60784.065166	33.338996
790.011121	60882.992840	33.344013
790.439142	60995.247548	33.349031
791.593724	61103.141703	33.354048
792.266865	61205.345495	33.359066
793.174702	61312.491513	33.364084
793.727619	61415.152351	33.369101
794.134645	61525.934447	33.374119
795.357655	61630.735647	33.379136
796.070955	61751.366326	33.384154
796.865160	61853.806157	33.389172
797.914134	61955.761914	33.394189
798.636508	62071.469172	33.399207
799.466439	62177.115630	33.404224
800.193538	62287.918430	33.409242
801.488026	62397.686182	33.414260
802.169716	62501.734380	33.419277
802.692085	62609.747361	33.424295
804.071442	62714.079456	33.429312
804.568282	62818.033409	33.434330
805.159050	62930.176973	33.439348
805.775394	63042.158890	33.444365
806.605742	63155.559859	33.449383
807.766115	63270.556668	33.454400
808.588485	63375.407749	33.459418
809.214925	63478.199470	33.464436
810.210220	63594.047132	33.469453
810.865014	63702.884647	33.474471
812.021049	63803.207295	33.479488
812.372466	63922.753756	33.484506
813.388548	64036.280546	33.489524
814.458942	64140.860595	33.494541
815.218881	64251.813895	33.499559
816.137924	64347.955699	33.504576
816.878242	64471.998736	33.509594
817.568802	64572.964705	33.514612
818.554321	64674.887499	33.519629
819.564207	64788.097029	33.524647
820.430368	64892.347993	33.529664
821.107262	64999.633543	33.534682
821.931926	65105.763632	33.539700
823.214646	65207.538734	33.544717
823.849484	65309.870329	33.549735
824.659340	65417.003279	33.554752
825.562666	65521.352389	33.559770
826.175489	65628.873032	33.564788
827.186014	65712.849201	33.569805
827.905797	65833.022134	33.574823
829.080887	65929.489234	33.579840
830.075703	66029.609052	33.584858
830.569204	66123.547215	33.589876
831.588543	66215.508561	33.594893
832.150742	66309.935632	33.599911
833.233455	66394.288239	33.604928
833.849375	66480.829953	33.609946
834.618213	66579.251207	33.614964
835.028491	66668.957137	33.619981
835.717987	66772.462748	33.624999
836.611547	66875.214391	33.630016
837.701124	66985.887446	33.635034
838.126271	67080.460767	33.640052
838.813808	67170.622435	33.645069
839.433107	67289.233430	33.650087
840.664901	67398.728153	33.655104
841.207894	67508.375299	33.660122
841.914520	67626.006422	33.665140
842.762517	67734.112211	33.670157
843.610332	67855.792904	33.675175
844.434724	67970.529746	33.680192
845.397028	68091.396225	33.685210
846.095427	68205.990795	33.690228
847.241713	68312.520143	33.695245
847.655231	68442.533349	33.700263
848.514552	68553.069336	33.705280
849.587388	68673.541492	33.710298
850.730595	68801.912444	33.715316
851.471818	68928.213554	33.720333
852.355272	69049.623320	33.725351
853.169636	69165.215534	33.730368
854.022049	69284.342899	33.735386
854.937131	69397.093384	33.740404
856.224503	69515.460906	33.745421
856.807871	69635.134240	33.750439
857.314648	69757.944485	33.755456
858.578490	69886.529648	33.760474
859.341508	69991.240189	33.765492
859.984243	70108.592099	33.770509
861.162374	70240.064264	33.775527
861.798602	70357.677864	33.780544
862.803816	70494.422123	33.785562
863.610643	70602.460754	33.790580
864.547688	70725.749187	33.795597
865.268727	70846.860879	33.800615
866.659724	70967.723340	33.805632
867.590110	71090.717768	33.810650
867.875401	71210.891826	33.815668
868.902879	71342.635946	33.820685
869.952528	71468.508967	33.825703
870.989813	71579.650861	33.830720
872.024755	71694.031397	33.835738
872.730943	71821.202701	33.840756
873.649571	71932.758102	33.845773
874.601440	72051.941287	33.850791
875.818357	72173.035328	33.855808
876.725599	72281.046793	33.860826
877.585312	72387.877781	33.865844
878.458792	72495.162336	33.870861
879.248303	72617.872563	33.875879
879.975072	72741.466557	33.880896
881.205629	72852.209913	33.885914
881.720158	72967.094292	33.890932
882.599737	73079.269150	33.895949
883.506441	73196.809204	33.900967
884.475935	73313.409871	33.905984
885.562098	73431.218743	33.911002
886.058542	73541.170016	33.916020
887.026156	73652.315080	33.921037
888.210904	73769.597219	33.926055
888.735191	73895.685035	33.931072
889.389380	73999.724665	33.936090
890.212351	74109.953662	33.941108
891.488953	74218.818030	33.946125
892.191263	74336.151370	33.951143
893.003359	74433.083660	33.956160
893.758628	74542.434290	33.961178
894.468323	74660.609292	33.966196
895.503594	74779.059961	33.971213
895.954492	74895.596711	33.976231
896.724121	75014.611191	33.981248
897.867974	75132.293184	33.986266
898.311887	75265.352886	33.991284
899.508202	75394.399293	33.996301
900.071600	75517.043003	34.001319
901.207694	75649.724917	34.006336
901.980491	75773.594047	34.011354
903.150167	75902.515011	34.016372
903.996763	76028.650298	34.021389
904.991833	76167.740418	34.026407
905.744506	76300.021601	34.031424
906.872129	76420.609962	34.036442
907.464622	76556.410542	34.041460
908.427391	76682.795991	34.046477
909.279444	76821.376233	34.051495
910.118587	76959.820321	34.056512
911.618243	77086.650591	34.061530
912.177309	77235.958722	34.066548
913.206100	77358.567279	34.071565
913.763727	77502.855205	34.076583
914.379567	77638.253705	34.081600
915.545752	77777.097883	34.086618
916.638518	77931.224548	34.091636
917.556736	78069.124786	34.096653
918.572880	78204.302380	34.101671
919.445828	78337.429705	34.106688
920.556050	78481.335259	34.111706
921.490360	78619.084407	34.116724
922.629980	78760.127726	34.121741
923.855620	78896.628531	34.126759
924.532539	79040.653604	34.131776
925.476847	79166.176875	34.136794
926.072783	79313.063663	34.141812
927.263837	79446.410634	34.146829
928.527918	79582.567647	34.151847
929.346245	79715.705836	34.156864
930.011606	79844.593777	34.161882
931.147663	79996.582952	34.166900
932.193167	80119.463187	34.171917
933.508800	80266.344699	34.176935
934.360404	80386.759662	34.181952
935.462556	80513.415662	34.186970
936.215385	80650.669499	34.191988
937.085025	80781.597639	34.197005
938.225636	80911.064651	34.202023
939.091953	81041.918925	34.207040
940.393912	81167.786381	34.212058
941.395096	81301.669120	34.217076
942.383160	81417.303249	34.222093
943.130566	81544.719554	34.227111
943.579690	81672.673030	34.232128
944.736269	81796.929453	34.237146
945.645833	81937.632027	34.242164
946.561975	82072.861917	34.247181
947.237771	82203.368433	34.252199
948.340443	82346.205275	34.257216
949.154898	82478.487188	34.262234
949.843384	82618.148639	34.267252
951.117535	82744.143253	34.272269
952.014632	82881.519493	34.277287
952.362164	83017.772682	34.282304
953.863077	83135.475464	34.287322
954.527300	83265.781141	34.292340
955.275468	83406.721861	34.297357
955.975947	83533.385079	34.302375
956.755168	83677.770504	34.307392
957.628751	83801.306343	34.312410
958.563261	83956.417437	34.317428
960.081341	84090.351171	34.322445
960.989139	84238.040556	34.327463
961.574265	84375.413995	34.332480
962.953965	84512.157007	34.337498
963.726172	84656.809107	34.342516
964.682234	84803.526038	34.347533
965.712213	84948.681475	34.352551
966.710749	85093.887308	34.357568
967.913260	85229.917211	34.362586
968.720553	85387.159590	34.367604
969.400539	85516.924810	34.372621
970.828782	85672.383319	34.377639
971.522906	85816.644235	34.382656
972.469888	85955.878075	34.387674
973.539567	86113.088273	34.392692
974.564220	86265.605499	34.397709
975.641384	86406.048057	34.402727
976.448907	86561.887201	34.407744
977.987473	86702.236251	34.412762
978.754174	86855.673198	34.417780
979.899821	86994.658871	34.422797
980.889572	87145.308192	34.427815
981.589792	87286.577685	34.432832
982.816251	87437.632689	34.437850
983.829415	87583.693134	34.442868
984.575367	87733.272782	34.447885
986.065879	87875.066906	34.452903
986.997953	88029.496629	34.457920
987.799796	88170.476155	34.462938
989.104526	88320.188597	34.467956
989.817739	88461.469276	34.472973
991.336108	88606.256440	34.477991
991.628100	88760.461352	34.483008
993.037962	88901.610467	34.488026
993.932012	89043.351982	34.493044
994.733214	89194.577081	34.498061
996.336327	89348.252572	34.503079
996.895345	89487.577674	34.508096
998.193516	89633.882040	34.513114
999.198399	89785.836629	34.518132
1000.042251	89931.395213	34.523149
1001.206354	90081.458392	34.528167
1001.904929	90233.466464	34.533184
1003.196400	90364.100101	34.538202
1004.422256	90509.845849	34.543220
1005.365845	90657.746661	34.548237
1006.303251	90800.117950	34.553255
1006.892769	90946.433566	34.558272
1008.455064	91095.861298	34.563290
1009.103634	91242.732223	34.568308
1010.214865	91386.603520	34.573325
1011.528512	91522.859963	34.578343
1012.317969	91681.608931	34.583360
1013.915837	91810.566825	34.588378
1014.906338	91966.999594	34.593396
1016.078877	92105.497864	34.598413
1017.152591	92232.304119	34.603431
1017.839669	92366.339731	34.608448
1018.793889	92498.344499	34.613466
1019.822373	92640.002653	34.618484
1020.532432	92773.226543	34.623501
1021.685961	92898.269823	34.628519
1022.622155	93028.444904	34.633536
1023.562929	93144.315241	34.638554
1024.512762	93285.667340	34.643572
1025.471271	93425.588336	34.648589
1026.423199	93553.845749	34.653607
1026.763889	93690.990441	34.658624
1028.249170	93834.440899	34.663642
1028.816193	93987.082861	34.668660
1029.527553	94139.486693	34.673677
1030.758526	94286.703737	34.678695
1031.498065	94437.952734	34.683712
1032.746906	94600.208390	34.688730
1033.696735	94765.147799	34.693748
1034.635059	94931.653711	34.698765
1036.190879	95090.361363	34.703783
1036.913646	95246.783365	34.708800
1038.060323	95388.089662	34.713818
1039.434841	95556.667223	34.718836
1040.236137	95718.073677	34.723853
1041.636138	95871.001002	34.728871
1042.228541	96031.690736	34.733888
1043.396452	96189.070568	34.738906
1044.467834	96358.349371	34.743924
1045.493179	96513.532878	34.748941
1046.731232	96679.323592	34.753959
1047.343493	96843.952782	34.758976
1048.605069	97008.121191	34.763994
1049.344837	97175.200366	34.769012
1050.143498	97346.778285	34.774029
1051.759071	97517.177758	34.779047
1052.987260	97686.047110	34.784064
1053.538724	97849.831977	34.789082
1054.904741	98026.454926	34.794100
1055.985332	98193.775730	34.799117
1057.242834	98367.836049	34.804135
1057.879181	98550.325368	34.809152
1059.432829	98712.367412	34.814170
1060.581297	98886.822854	34.819188
1061.614862	99060.912303	34.824205
1062.807681	99222.238552	34.829223
1063.530620	99394.482330	34.834240
1064.737840	99561.113800	34.839258
1066.025986	99732.557331	34.844276
1066.973544	99903.754429	34.849293
1067.833335	100056.631876	34.854311
1068.769369	100240.976819	34.859328
1070.115273	100408.996444	34.864346
1071.551785	100573.178038	34.869364
1072.172506	100754.989279	34.874381
1073.484729	100917.794385	34.879399
1074.544813	101096.027769	34.884416
1075.695001	101261.641375	34.889434
1076.808673	101442.502222	34.894452
1077.744608	101603.430081	34.899469
1078.729717	101774.462494	34.904487
1079.909490	101951.675269	34.909504
1080.939089	102115.142512	34.914522
1082.463244	102292.319680	34.919540
1082.970397	102458.547485	34.924557
1084.165055	102634.109858	34.929575
1085.412465	102802.813553	34.934592
1086.354644	102978.584625	34.939610
1087.177311	103152.761980	34.944628
1088.271884	103325.002260	34.949645
1089.731692	103496.816033	34.954663
1090.568973	103671.735290	34.959680
1091.478235	103839.931708	34.964698
1092.623908	104004.088161	34.969716
1094.168610	104163.785087	34.974733
1095.132817	104316.613436	34.979751
1095.951696	104489.388212	34.984768
1097.073908	104651.450259	34.989786
1098.209788	104812.383874	34.994804
1099.443530	104977.836328	34.999821
1100.630897	105136.977663	35.004839
1101.332602	105299.265192	35.009856
1102.492604	105471.660716	35.014874
1103.810502	105644.398551	35.019892
1104.387987	105819.919635	35.024909
1105.837061	105991.472837	35.029927
1106.496233	106166.995375	35.034944
1107.613192	106343.633950	35.039962
1108.860324	106524.849802	35.044980
1109.872762	106709.816744	35.049997
1111.083080	106891.256489	35.055015
1112.241101	107074.150026	35.060032
1113.336117	107259.398436	35.065050
1114.174817	107439.598741	35.070068
1115.255999	107635.884190	35.075085
1116.390228	107818.862739	35.080103
1117.336115	108014.109352	35.085120
1118.460084	108213.862524	35.090138
1119.714965	108398.395703	35.095156
1120.356009	108599.561553	35.100173
1121.817687	108791.397201	35.105191
1123.287399	109001.321071	35.110208
1123.943910	109188.783263	35.115226
1125.197270	109387.966371	35.120244
1126.447638	109595.790382	35.125261
1127.730886	109790.310012	35.130279
1128.766714	109989.533487	35.135296
1129.850011	110198.263754	35.140314
1130.754435	110388.606710	35.145332
1132.013978	110607.229576	35.150349
1133.558904	110796.481413	35.155367
1134.468284	111002.535688	35.160384
1135.595858	111212.672481	35.165402
1137.019307	111412.842981	35.170420
1137.907803	111613.192050	35.175437
1139.218799	111809.140235	35.180455
1140.050974	112017.191084	35.185472
1141.418669	112220.480367	35.190490
1142.989161	112420.241143	35.195508
1143.851711	112629.634416	35.200525
1144.925663	112831.760565	35.205543
1146.075188	113045.505521	35.210560
1147.497975	113250.364148	35.215578
1148.871025	113435.456432	35.220596
1149.524806	113650.909590	35.225613
1150.998492	113850.582608	35.230631
1152.082593	114048.003004	35.235648
1152.907530	114252.055621	35.240666
1154.444629	114461.439790	35.245684
1155.231702	114678.196404	35.250701
1156.747307	114880.391023	35.255719
1157.847702	115085.683760	35.260736
1158.850349	115295.960661	35.265754
1160.249110	115492.642327	35.270772
1160.978621	115708.732188	35.275789
1162.588119	115902.341091	35.280807
1163.893093	116105.504183	35.285824
1164.267583	116315.955828	35.290842
1165.731530	116512.317020	35.295860
1166.598659	116727.264208	35.300877
1167.782309	116926.880175	35.305895
1168.935786	117117.506473	35.310912
1170.170708	117324.516301	35.315930
1171.446040	117515.568570	35.320948
1172.596771	117729.336026	35.325965
1173.684726	117926.541975	35.330983
1174.959867	118134.298559	35.336000
1175.955227	118330.927044	35.341018
1177.136697	118529.629503	35.346036
1177.955128	118739.835430	35.351053
1179.285192	118937.933249	35.356071
1180.489858	119153.526977	35.361088
1181.167467	119363.608636	35.366106
1182.534888	119580.977973	35.371124
1183.748968	119802.251805	35.376141
1184.824709	120016.086514	35.381159
1185.704399	120240.992374	35.386176
1187.086873	120464.828433	35.391194
1188.602314	120687.110900	35.396212
1189.772054	120914.254933	35.401229
1191.155272	121130.441960	35.406247
1192.372048	121360.179460	35.411264
1193.457262	121582.552465	35.416282
1194.512617	121797.455288	35.421300
1195.704728	122039.811294	35.426317
1196.727497	122265.672038	35.431335
1197.840008	122496.892934	35.436352
1199.012185	122737.876578	35.441370
1200.126904	122969.151458	35.446388
1201.592628	123216.008731	35.451405
1202.717624	123447.070157	35.456423
1203.991887	123683.431480	35.461440
1205.356843	123924.849036	35.466458
1206.566813	124155.775123	35.471476
1207.652634	124396.494856	35.476493
1209.178641	124634.152743	35.481511
1210.626387	124873.878590	35.486528
1211.434965	125110.796982	35.491546
1212.801716	125341.414687	35.496564
1213.692760	125582.860416	35.501581
1215.232361	125826.342791	35.506599
1216.377317	126058.789642	35.511616
1217.730790	126300.849012	35.516634
1218.868924	126539.168883	35.521652
1220.134703	126792.057976	35.526669
1221.284158	127023.446713	35.531687
1222.710321	127268.530933	35.536704
1223.760541	127520.042042	35.541722
1225.661918	127744.961760	35.546740
1226.694516	127985.401607	35.551757
1227.674259	128219.172221	35.556775
1229.249178	128456.965678	35.561792
1230.104940	128694.562936	35.566810
1231.709082	128925.041430	35.571828
1233.144343	129171.026415	35.576845
1234.223476	129405.980977	35.581863
1235.474739	129636.041347	35.586880
1237.033018	129876.700374	35.591898
1238.047962	130099.869495	35.596916
1239.239061	130344.560353	35.601933
1240.567139	130575.096557	35.606951
1242.056019	130807.243091	35.611968
1242.808761	131058.007767	35.616986
1244.322731	131279.467451	35.622004
1245.318844	131509.013150	35.627021
1246.834200	131745.510187	35.632039
1248.137964	131983.210202	35.637056
1249.044442	132218.721176	35.642074
1250.503686	132423.413748	35.647092
1251.805214	132648.416826	35.652109
1253.191368	132873.901892	35.657127
1254.424360	133080.841841	35.662144
1255.546178	133310.937414	35.667162
1256.948422	133518.359273	35.672180
1258.201711	133744.607644	35.677197
1259.382221	133967.548118	35.682215
1260.437948	134180.951859	35.687232
1261.388557	134410.576403	35.692250
1262.868217	134638.390939	35.697268
1263.965958	134869.743911	35.702285
1265.141721	135101.795579	35.707303
1266.453081	135333.458810	35.712320
1267.190321	135578.378427	35.717338
1268.788190	135811.354214	35.722356
1270.129111	136055.201363	35.727373
1271.300286	136296.770897	35.732391
1272.653599	136541.709912	35.737408
1273.734669	136790.892330	35.742426
1274.974169	137029.184816	35.747444
1276.142225	137286.623038	35.752461
1277.357495	137543.193272	35.757479
1278.741956	137783.901504	35.762496
1279.780766	138049.012334	35.767514
1281.242722	138303.696455	35.772532
1282.382957	138566.271435	35.777549
1283.416006	138825.138443	35.782567
1285.008067	139086.856658	35.787584
1286.130344	139350.835412	35.792602
1287.331571	139602.478570	35.797620
1288.828256	139878.533919	35.802637
1290.041625	140160.394960	35.807655
1291.653074	140421.435485	35.812672
1292.601558	140699.654872	35.817690
1293.644178	140965.979669	35.822708
1295.368495	141235.376583	35.827725
1296.531306	141507.125493	35.832743
1297.854335	141771.254481	35.837760
1298.995181	142050.137659	35.842778
1300.594591	142319.132480	35.847796
1302.113608	142602.357738	35.852813
1303.197035	142877.148450	35.857831
1304.655021	143137.892358	35.862848
1306.276816	143408.400860	35.867866
1307.559373	143682.353357	35.872884
1309.148947	143953.226426	35.877901
1310.248441	144215.483193	35.882919
1311.707015	144491.023370	35.887936
1312.639872	144763.342696	35.892954
1314.261672	145029.082624	35.897972
1315.616564	145295.299815	35.902989
1316.842069	145568.046114	35.908007
1318.279839	145838.108888	35.913024
1319.674161	146110.336800	35.918042
1321.098070	146379.518177	35.923060
1322.736210	146646.104353	35.928077
1323.117533	146913.077752	35.933095
1324.867944	147184.113467	35.938112
1326.475305	147457.483039	35.943130
1327.888864	147720.043125	35.948148
1329.321004	147984.428315	35.953165
1330.141118	148263.590451	35.958183
1331.694358	148520.502043	35.963200
1332.934840	148784.988065	35.968218
1334.629082	149053.358073	35.973236
1336.106920	149324.429232	35.978253
1337.220766	149585.428672	35.983271
1338.545934	149829.627758	35.988288
1339.604532	150086.492408	35.993306
1341.450980	150336.176631	35.998324
1342.797724	150572.564008	36.003341
1343.586886	150824.049692	36.008359
1345.316296	151073.301539	36.013376
1346.729959	151322.975040	36.018394
1348.078179	151572.622949	36.023412
1349.099612	151821.730361	36.028429
1350.416293	152086.506082	36.033447
1351.751610	152337.442219	36.038464
1352.483099	152600.643912	36.043482
1353.859972	152870.742461	36.048500
1355.564943	153136.323793	36.053517
1356.700728	153409.142358	36.058535
1358.294970	153678.589103	36.063552
1359.501388	153955.040299	36.068570
1360.364125	154216.582306	36.073588
1361.843568	154499.042846	36.078605
1363.554846	154788.228159	36.083623
1365.120892	155063.879366	36.088640
1366.044883	155350.839527	36.093658
1367.453562	155622.195042	36.098676
1368.753100	155904.771528	36.103693
1369.802169	156200.850566	36.108711
1371.118665	156490.544897	36.113728
1372.684647	156778.550985	36.118746
1374.084318	157072.574245	36.123764
1375.432656	157380.042314	36.128781
1376.810885	157667.388101	36.133799
1378.286569	157964.082024	36.138816
1379.693861	158258.975328	36.143834
1380.598269	158560.778994	36.148852
1382.667244	158851.659940	36.153869
1383.985713	159158.436018	36.158887
1385.221290	159451.184288	36.163904
1386.612742	159753.753574	36.168922
1388.044789	160051.801964	36.173940
1389.623234	160354.915654	36.178957
1391.110925	160659.974942	36.183975
1392.692643	160957.979743	36.188992
1394.172512	161258.147594	36.194010
1395.408218	161560.121443	36.199028
1397.029228	161850.894523	36.204045
1398.234035	162151.431398	36.209063
1400.126310	162448.152124	36.214080
1401.578329	162750.859993	36.219098
1402.828849	163043.466045	36.224116
1404.690515	163326.026085	36.229133
1405.766792	163629.360541	36.234151
1407.033868	163918.353873	36.239168
1408.790801	164219.702239	36.244186
1410.036762	164514.412569	36.249204
1411.784711	164799.335657	36.254221
1412.810508	165097.194884	36.259239
1414.176484	165388.998442	36.264256
1416.194837	165683.652502	36.269274
1417.621833	165973.457825	36.274292
1418.709052	166263.143568	36.279309
1420.181568	166555.901598	36.284327
1421.509109	166850.398477	36.289344
1423.023886	167143.178781	36.294362
1424.264504	167434.407534	36.299380
1426.101903	167723.775826	36.304397
1427.251311	168017.865742	36.309415
1428.769515	168312.619911	36.314432
1430.149637	168605.609667	36.319450
1431.206795	168897.956786	36.324468
1432.653470	169167.540412	36.329485
1433.950187	169451.819235	36.334503
1435.607576	169734.631707	36.339520
1436.849568	170016.956231	36.344538
1438.038757	170300.420581	36.349556
1439.480671	170586.243248	36.354573
1440.767645	170877.143777	36.359591
1442.185923	171167.999051	36.364608
1443.537929	171459.704623	36.369626
1444.693529	171763.284168	36.374644
1446.314420	172061.357469	36.379661
1447.146992	172363.433397	36.384679
1448.933060	172675.480454	36.389696
1450.594178	172982.283758	36.394714
1451.547102	173293.190828	36.399732
1453.243815	173591.844980	36.404749
1454.528758	173921.584610	36.409767
1456.272035	174228.674214	36.414784
1457.738927	174549.923460	36.419802
1459.167450	174868.884149	36.424820
1460.426962	175183.103104	36.429837
1462.015989	175512.727165	36.434855
1463.487774	175841.687502	36.439872
1465.228414	176153.904145	36.444890
1466.414052	176483.474451	36.449908
1468.038268	176799.877108	36.454925
1469.465622	177127.000403	36.459943
1471.044638	177453.580430	36.464960
1472.532335	177796.118190	36.469978
1474.130084	178116.594815	36.474996
1475.760957	178445.355650	36.480013
1477.100375	178777.974292	36.485031
1478.642163	179101.360090	36.490048
1480.384751	179435.185571	36.495066
1481.447296	179766.117583	36.500084
1483.482211	180092.410744	36.505101
1484.776249	180427.052887	36.510119
1486.661108	180750.481163	36.515136
1488.301864	181079.320617	36.520154
1489.587898	181406.342267	36.525172
1491.250271	181726.399059	36.530189
1492.624342	182054.780956	36.535207
1494.498479	182384.681523	36.540224
1496.404471	182710.491815	36.545242
1497.560573	183034.054439	36.550260
1499.140887	183362.042180	36.555277
1500.522976	183670.555635	36.560295
1502.340714	184004.537169	36.565312
1503.645944	184337.970771	36.570330
1505.090862	184652.546681	36.575348
1506.872754	184978.492611	36.580365
1508.456774	185287.032564	36.585383
1510.011795	185611.737677	36.590400
1511.426984	185930.489172	36.595418
1512.961452	186254.642900	36.600436
1514.682261	186561.758301	36.605453
1516.091485	186888.855889	36.610471
1517.097631	187212.518488	36.615488
1518.876243	187524.846666	36.620506
1520.586084	187866.942340	36.625524
1522.105449	188177.463593	36.630541
1523.713094	188493.087613	36.635559
1525.036226	188819.448770	36.640576
1526.336945	189138.655952	36.645594
1527.729261	189463.968349	36.650612
1529.557321	189783.320397	36.655629
1531.243340	190121.015596	36.660647
1532.063456	190432.184779	36.665664
1533.853789	190740.465964	36.670682
1534.784504	191053.168823	36.675700
1536.482969	191361.366810	36.680717
1538.139373	191680.084515	36.685735
1539.659208	191996.896849	36.690752
1540.807692	192310.852368	36.695770
1541.554809	192642.242408	36.700788
1543.414166	192971.546217	36.705805
1545.280462	193303.440410	36.710823
1546.476109	193621.368318	36.715840
1548.192758	193963.230990	36.720858
1549.701540	194306.970666	36.725876
1550.960024	194633.703780	36.730893
1552.607468	194981.537468	36.735911
1554.272397	195326.996110	36.740928
1555.872788	195670.778767	36.745946
1557.377000	196017.587986	36.750964
1558.908364	196354.530060	36.755981
1560.306035	196708.343144	36.760999
1561.725946	197073.606034	36.766016
1563.745089	197421.696037	36.771034
1565.122401	197778.158930	36.776052
1566.548504	198135.402806	36.781069
1568.384545	198494.294813	36.786087
1569.792684	198857.169812	36.791104
1571.683716	199219.116318	36.796122
1572.976771	199579.487621	36.801140
1574.499631	199941.803460	36.806157
1576.295747	200304.774343	36.811175
1577.572547	200676.187161	36.816192
1579.406169	201042.723363	36.821210
1581.380973	201411.917113	36.826228
1583.391182	201774.910970	36.831245
1584.798800	202130.807190	36.836263
1586.414819	202497.818488	36.841280
1587.963043	202854.812350	36.846298
1589.590318	203224.898079	36.851316
1591.159665	203582.945833	36.856333
1592.918928	203934.539257	36.861351
1594.247393	204307.498491	36.866368
1596.039683	204666.733534	36.871386
1597.642535	205037.441749	36.876404
1599.317453	205410.476158	36.881421
1601.048636	205779.770076	36.886439
1602.397835	206144.303863	36.891456
1604.705264	206499.576996	36.896474
1605.773375	206879.308692	36.901492
1607.320844	207233.974240	36.906509
1609.105810	207611.318160	36.911527
1611.110256	207979.917000	36.916544
1612.647043	208339.211166	36.921562
1614.562376	208701.695018	36.926580
1616.061459	209053.684643	36.931597
1617.856726	209417.118434	36.936615
1619.336221	209783.894753	36.941632
1621.219334	210138.365130	36.946650
1622.709650	210494.273280	36.951668
1624.201682	210855.490449	36.956685
1626.169162	211209.367254	36.961703
1627.644241	211571.504508	36.966720
1629.685727	211930.603707	36.971738
1631.118716	212279.722440	36.976756
1632.634657	212630.682815	36.981773
1634.182367	212985.194887	36.986791
1635.904830	213346.003333	36.991808
1637.802818	213699.292102	36.996826
1638.943609	214054.154967	37.001844
1640.860910	214408.179809	37.006861
1642.724615	214733.541282	37.011879
1644.283361	215073.633976	37.016896
1645.840637	215410.731242	37.021914
1647.229747	215749.127370	37.026932
1649.045325	216083.009657	37.031949
1650.614521	216418.483071	37.036967
1651.715337	216751.850806	37.041984
1653.685676	217106.435717	37.047002
1655.355067	217446.645535	37.052020
1656.370174	217797.200048	37.057037
1658.372568	218146.373584	37.062055
1659.696921	218496.498480	37.067072
1661.325308	218853.355729	37.072090
1662.868232	219219.930556	37.077108
1664.806196	219572.954783	37.082125
1666.034619	219936.968036	37.087143
1667.442635	220314.718997	37.092160
1669.739404	220670.024310	37.097178
1671.286486	221059.819375	37.102196
1672.747746	221434.289011	37.107213
1674.380910	221805.048659	37.112231
1675.689893	222194.353702	37.117248
1677.730658	222574.903465	37.122266
1679.552987	222956.760557	37.127284
1681.576986	223338.890405	37.132301
1683.344765	223715.552142	37.137319
1684.863523	224105.692618	37.142336
1686.639217	224514.155916	37.147354
1688.432487	224927.316664	37.152372
1689.849064	225307.521222	37.157389
1691.972873	225690.429531	37.162407
1693.609303	226072.428929	37.167424
1695.416975	226456.458612	37.172442
1697.021431	226846.314264	37.177460
1698.890584	227232.241138	37.182477
1700.701053	227610.736557	37.187495
1702.172576	227998.179189	37.192512
1704.056555	228387.205848	37.197530
1705.702094	228766.722412	37.202548
1707.340517	229160.389343	37.207565
1709.415956	229540.675250	37.212583
1710.847025	229933.057778	37.217600
1712.545044	230319.809112	37.222618
1714.360214	230713.247967	37.227636
1715.960597	231118.915818	37.232653
1717.654268	231500.514598	37.237671
1719.379969	231914.343036	37.242688
1721.053493	232294.143663	37.247706
1722.901810	232696.752044	37.252724
1724.365750	233098.434293	37.257741
1726.244939	233495.019496	37.262759
1727.732240	233893.296086	37.267776
1729.496449	234290.257826	37.272794
1731.380744	234698.707563	37.277812
1733.132951	235102.963431	37.282829
1734.934349	235499.794834	37.287847
1736.336876	235911.324393	37.292864
1737.943316	236312.812919	37.297882
1740.044589	236719.783592	37.302900
1741.714317	237127.436077	37.307917
1743.686327	237522.109929	37.312935
1745.198978	237928.545368	37.317952
1747.592243	238332.931041	37.322970
1748.861804	238740.500574	37.327988
1750.507042	239154.054572	37.333005
1752.705233	239531.446964	37.338023
1754.326432	239953.922658	37.343040
1755.995867	240353.452949	37.348058
1758.079020	240721.797789	37.353076
1759.664653	241109.277162	37.358093
1761.289464	241480.518578	37.363111
1762.838117	241863.966319	37.368128
1764.615336	242241.762966	37.373146
1766.525062	242623.551898	37.378164
1767.855671	243008.612369	37.383181
1769.873963	243396.735150	37.388199
1771.583803	243788.465805	37.393216
1773.416599	244182.183520	37.398234
1775.046363	244572.582161	37.403252
1776.777652	244966.724163	37.408269
1778.539761	245365.891340	37.413287
1780.026996	245765.790309	37.418304
1781.924203	246167.527282	37.423322
1783.519314	246581.838249	37.428340
1785.464353	246996.371361	37.433357
1787.299301	247393.649161	37.438375
1789.289431	247819.988137	37.443392
1790.969116	248228.418965	37.448410
1792.836965	248645.964220	37.453428
1794.364335	249064.582255	37.458445
1796.197944	249485.410994	37.463463
1797.801849	249906.074841	37.468480
1799.613520	250335.443417	37.473498
1801.324326	250768.334655	37.478516
1802.760328	251193.193441	37.483533
1805.040580	251618.243365	37.488551
1806.557376	252066.816009	37.493568
1807.922161	252496.107657	37.498586
1810.372858	252945.898449	37.503604
1812.078000	253393.043702	37.508621
1813.900558	253833.895220	37.513639
1815.630387	254282.535674	37.518656
1817.565914	254719.380662	37.523674
1819.440056	255170.563415	37.528692
1820.781326	255621.123052	37.533709
1823.054639	256070.944635	37.538727
1824.750513	256525.205672	37.543744
1826.830057	256980.622810	37.548762
1828.895575	257439.573407	37.553780
1830.741808	257884.410640	37.558797
1832.860925	258337.128674	37.563815
1834.587982	258797.202219	37.568832
1836.301275	259246.761059	37.573850
1838.187744	259692.404565	37.578868
1840.010407	260143.672685	37.583885
1842.312986	260593.311871	37.588903
1844.117800	261045.217848	37.593920
1845.627491	261491.532913	37.598938
1848.017648	261953.274640	37.603956
1849.947782	262396.014314	37.608973
1851.739226	262846.854944	37.613991
1853.686359	263296.450298	37.619008
1855.535696	263738.034152	37.624026
1857.482460	264186.536749	37.629044
1859.170471	264647.681787	37.634061
1861.201718	265095.179130	37.639079
1863.022426	265544.997209	37.644096
1864.713456	265987.952110	37.649114
1866.797712	266430.765511	37.654132
1868.400970	266886.461128	37.659149
1870.397261	267329.262869	37.664167
1872.155934	267784.246088	37.669184
1873.751597	268237.706178	37.674202
1876.108075	268682.733367	37.679220
1877.873330	269143.328105	37.684237
1879.650815	269570.921869	37.689255
1881.177907	270014.611126	37.694272
1883.028547	270442.953877	37.699290
1885.217897	270873.272391	37.704308
1886.636217	271304.124119	37.709325
1888.614829	271729.014706	37.714343
1890.355286	272175.079118	37.719360
1892.326343	272612.442470	37.724378
1894.646322	273043.193663	37.729396
1896.189498	273505.470112	37.734413
1897.848372	273941.892260	37.739431
1899.508783	274382.504857	37.744448
1901.786924	274834.064780	37.749466
1903.209387	275285.688987	37.754484
1904.977553	275743.453459	37.759501
1907.225599	276206.446900	37.764519
1909.145839	276666.191251	37.769536
1910.892068	277136.835561	37.774554
1912.636308	277596.099017	37.779572
1914.593958	278066.223766	37.784589
1916.576049	278540.915801	37.789607
1918.567456	279011.490072	37.794624
1920.369490	279481.484862	37.799642
1922.568223	279956.645807	37.804660
1924.284144	280441.792010	37.809677
1926.313229	280913.371509	37.814695
1928.412519	281393.828793	37.819712
1930.496023	281879.748747	37.824730
1932.211196	282356.304200	37.829748
1934.105127	282847.409267	37.834765
1936.181104	283341.276997	37.839783
1938.318970	283823.092802	37.844800
1939.868997	284316.612613	37.849818
1942.014321	284800.075335	37.854836
1943.899991	285298.058056	37.859853
1945.974427	285792.629654	37.864871
1948.053602	286282.245662	37.869888
1949.622585	286783.501672	37.874906
1952.067112	287277.803978	37.879924
1953.674891	287776.510044	37.884941
1955.536149	288283.503868	37.889959
1957.900946	288783.579953	37.894976
1959.622417	289293.818967	37.899994
1961.727268	289782.300880	37.905012
1963.555057	290299.935336	37.910029
1965.736628	290798.383034	37.915047
1968.224151	291309.046450	37.920064
1969.661657	291810.127599	37.925082
1971.930433	292309.850263	37.930100
1973.616125	292818.811023	37.935117
1975.830476	293321.942025	37.940135
1977.759011	293832.864900	37.945152
1980.063408	294329.703029	37.950170
1981.831366	294830.666050	37.955188
1983.753882	295341.684775	37.960205
1985.862613	295852.060828	37.965223
1988.042773	296371.363118	37.970240
1989.980727	296873.076170	37.975258
1991.814817	297371.222805	37.980276
1993.833951	297886.480529	37.985293
1995.511403	298393.385250	37.990311
1997.772035	298901.207110	37.995328
1999.590024	299408.261372	38.000346
2001.328354	299922.767833	38.005364
2003.550174	300433.966258	38.010381
2005.713610	300944.714488	38.015399
2008.127711	301456.790098	38.020416
2009.407173	301973.164681	38.025434
2011.303554	302472.672343	38.030452
2013.622317	302974.596512	38.035469
2015.685450	303467.721976	38.040487
2017.503432	303951.437591	38.045504
2019.042572	304450.282333	38.050522
2021.285542	304945.071598	38.055540
2023.302350	305437.330380	38.060557
2025.024091	305938.396839	38.065575
2026.969128	306439.575898	38.070592
2029.050829	306955.611532	38.075610
2030.772037	307460.986468	38.080628
2032.688933	307974.554257	38.085645
2034.680155	308499.864736	38.090663
2036.914021	309028.636348	38.095680
2038.509220	309547.402646	38.100698
2040.919943	310080.099816	38.105716
2042.732618	310609.844756	38.110733
2044.446161	311149.328670	38.115751
2046.768156	311686.524454	38.120768
2048.512906	312235.442408	38.125786
2050.749143	312772.822485	38.130804
2052.573278	313327.483900	38.135821
2054.732368	313881.324079	38.140839
2056.987106	314440.527760	38.145856
2058.502765	315007.644962	38.150874
2061.171451	315554.659078	38.155892
2063.159559	316118.566169	38.160909
2065.168600	316684.852250	38.165927
2067.425561	317250.229490	38.170944
2069.381507	317818.749708	38.175962
2071.892988	318393.013728	38.180980
2073.574786	318959.386024	38.185997
2076.194419	319521.282149	38.191015
2078.337919	320083.049034	38.196032
2080.304894	320662.334941	38.201050
2082.563821	321223.336727	38.206068
2085.088134	321795.588823	38.211085
2086.846676	322363.112649	38.216103
2089.103394	322929.076556	38.221120
2090.998260	323500.680999	38.226138
2093.101907	324077.349167	38.231156
2095.507870	324645.126460	38.236173
2097.454726	325215.411721	38.241191
2099.800453	325789.104157	38.246208
2101.659804	326371.249849	38.251226
2103.759839	326938.066130	38.256244
2105.873832	327510.739481	38.261261
2107.842259	328107.651759	38.266279
2110.208630	328680.602133	38.271296
2112.066213	329276.708358	38.276314
2114.478001	329847.786393	38.281332
2116.804057	330425.575125	38.286349
2118.767833	330999.025832	38.291367
2120.937911	331581.195078	38.296384
2123.194002	332166.923558	38.301402
2124.770103	332746.005369	38.306420
2127.430656	333327.313734	38.311437
2129.224942	333910.155122	38.316455
2131.753793	334497.489123	38.321472
2133.658955	335084.285034	38.326490
2136.174558	335665.820597	38.331508
2138.675180	336249.941469	38.336525
2140.223329	336838.807631	38.341543
2142.339943	337409.829890	38.346560
2143.891723	337996.169319	38.351578
2146.367170	338580.141227	38.356596
2148.676105	339162.331731	38.361613
2150.548528	339768.828202	38.366631
2152.861020	340342.831222	38.371648
2154.827254	340909.650856	38.376666
2157.027797	341469.952930	38.381684
2159.198053	342022.588359	38.386701
2161.389854	342589.782897	38.391719
2163.356240	343146.551011	38.396736
2165.695803	343705.053135	38.401754
2167.731456	344281.466779	38.406772
2169.846548	344848.342762	38.411789
2171.918856	345414.609893	38.416807
2174.241956	345987.376728	38.421824
2176.153977	346569.873880	38.426842
2178.326544	347149.909708	38.431860
2180.157930	347737.024419	38.436877
2182.022665	348326.054840	38.441895
2184.194841	348931.294139	38.446912
2186.610553	349528.947976	38.451930
2188.551297	350126.418472	38.456948
2191.013595	350732.499148	38.461965
2192.922378	351350.310728	38.466983
2195.423571	351961.697165	38.472000
2197.539065	352574.813509	38.477018
2199.688015	353193.980406	38.482036
2202.017726	353802.831645	38.487053
2204.107295	354435.439260	38.492071
2206.444397	355039.425055	38.497088
2208.734805	355666.652525	38.502106
2211.349134	356297.090357	38.507124
2213.341508	356907.500330	38.512141
2215.035265	357545.505545	38.517159
2217.597395	358165.647559	38.522176
2220.203030	358803.457341	38.527194
2221.948139	359430.184865	38.532212
2224.490178	360067.071879	38.537229
2226.504081	360715.351376	38.542247
2229.089302	361341.783546	38.547264
2230.995751	362002.339114	38.552282
2233.171853	362635.947283	38.557300
2235.982090	363275.833581	38.562317
2238.185062	363934.683980	38.567335
2240.648072	364565.270597	38.572352
2242.867847	365213.238702	38.577370
2244.776850	365854.803759	38.582388
2247.475140	366497.851200	38.587405
2249.869938	367146.011109	38.592423
2252.146114	367786.468065	38.597440
2254.293689	368436.675712	38.602458
2256.425273	369081.598605	38.607476
2258.680513	369720.985621	38.612493
2260.838394	370379.248703	38.617511
2263.424853	371023.123863	38.622528
2265.874701	371677.738899	38.627546
2267.933926	372323.833783	38.632564
2270.678362	372962.930645	38.637581
2272.946187	373609.221462	38.642599
2275.566965	374247.656183	38.647616
2278.099424	374889.416221	38.652634
2280.225686	375522.456701	38.657652
2282.813464	376148.562212	38.662669
2284.630036	376797.252517	38.667687
2287.075926	377427.010080	38.672704
2289.557936	378067.071180	38.677722
2291.748873	378712.772505	38.682740
2294.155551	379339.027084	38.687757
2296.137496	379971.730209	38.692775
2298.550708	380617.130147	38.697792
2300.837214	381244.636808	38.702810
2302.774021	381886.084418	38.707828
2305.448162	382515.962527	38.712845
2307.331164	383136.729876	38.717863
2309.768108	383741.141722	38.722880
2312.034686	384350.641268	38.727898
2313.684663	384968.471020	38.732916
2316.218333	385578.917430	38.737933
2318.511742	386203.690754	38.742951
2320.660402	386822.923597	38.747968
2322.812562	387447.492974	38.752986
2324.675627	388083.328261	38.758004
2326.892654	388723.832830	38.763021
2329.051204	389371.203800	38.768039
2331.476288	390026.096828	38.773056
2333.418035	390683.539962	38.778074
2335.662560	391340.310726	38.783092
2337.893972	392005.206259	38.788109
2340.140481	392678.322691	38.793127
2342.558092	393357.935419	38.798144
2344.661333	394032.185968	38.803162
2347.122046	394723.648117	38.808180
2349.079828	395409.854786	38.813197
2351.359778	396112.212905	38.818215
2353.645680	396811.917590	38.823232
2356.098680	397517.178910	38.828250
2358.489879	398237.005441	38.833268
2361.206445	398945.229862	38.838285
2363.146190	399662.485317	38.843303
2365.467264	400373.476843	38.848320
2367.766041	401096.972429	38.853338
2370.049698	401834.464876	38.858356
2372.624891	402562.894763	38.863373
2374.661497	403297.045129	38.868391
2377.074353	404032.431760	38.873408
2379.941529	404765.595763	38.878426
2382.249561	405519.354956	38.883444
2384.756070	406254.540638	38.888461
2387.435489	407011.440694	38.893479
2389.751625	407746.491131	38.898496
2392.718466	408484.859686	38.903514
2395.073323	409229.946262	38.908532
2397.634820	409972.014301	38.913549
2399.834672	410713.640189	38.918567
2402.669872	411448.757323	38.923584
2405.230673	412176.655038	38.928602
2407.574789	412929.137760	38.933620
2410.455832	413655.928619	38.938637
2413.118824	414390.054994	38.943655
2415.288175	415128.395767	38.948672
2417.944318	415864.634410	38.953690
2419.959013	416592.473814	38.958708
2422.753789	417325.102223	38.963725
2425.164762	418067.092243	38.968743
2427.758610	418790.291128	38.973760
2430.275171	419530.220402	38.978778
2432.538252	420269.562052	38.983796
2435.254088	420985.992815	38.988813
2437.537947	421729.972324	38.993831
2440.047568	422460.396920	38.998848
2443.014110	423181.457823	39.003866
2445.060712	423923.663526	39.008884
2447.926059	424638.065025	39.013901
2450.177285	425383.534592	39.018919
2451.799359	426105.237512	39.023936
2454.653632	426826.766233	39.028954
2457.324491	427584.351309	39.033972
2459.760218	428299.171267	39.038989
2462.049344	429039.053740	39.044007
2464.523999	429766.530297	39.049024
2467.338891	430487.701784	39.054042
2469.516158	431201.262013	39.059060
2472.103309	431893.270244	39.064077
2474.362583	432593.360357	39.069095
2476.313181	433289.734728	39.074112
2479.053407	433985.907289	39.079130
2481.302533	434701.069318	39.084148
2483.886150	435396.668351	39.089165
2486.282059	436124.819663	39.094183
2488.383625	436823.137168	39.099200
2491.051694	437535.965210	39.104218
2493.192403	438273.958139	39.109236
2496.023016	438991.622138	39.114253
2498.198223	439734.267612	39.119271
2500.305495	440450.283736	39.124288
2503.169996	441200.002559	39.129306
2505.360269	441949.453082	39.134324
2508.028763	442692.727808	39.139341
2510.592966	443452.336376	39.144359
2512.965467	444208.105227	39.149376
2515.668617	444959.948470	39.154394
2518.084459	445724.308416	39.159412
2520.900672	446488.524698	39.164429
2523.604444	447247.269241	39.169447
2525.733456	448014.478542	39.174464
2528.366052	448784.915557	39.179482
2530.912251	449561.711909	39.184500
2533.812618	450321.831915	39.189517
2536.379370	451105.193794	39.194535
2538.558392	451885.808868	39.199552
2541.569931	452651.895048	39.204570
2544.039071	453441.102461	39.209588
2546.613911	454221.413003	39.214605
2549.296504	454995.709489	39.219623
2551.823018	455786.587665	39.224640
2554.434083	456573.426951	39.229658
2556.730513	457357.911475	39.234676
2559.489289	458160.996048	39.239693
2561.764828	458948.456014	39.244711
2564.786620	459754.821114	39.249728
2567.364485	460547.830698	39.254746
2569.613275	461361.942609	39.259764
2572.055516	462162.594051	39.264781
2574.815385	462956.893050	39.269799
2577.406003	463765.037141	39.274816
2580.164855	464578.528292	39.279834
2583.071732	465404.040303	39.284852
2585.390907	466207.125023	39.289869
2588.445625	467016.372200	39.294887
2590.687680	467822.788666	39.299904
2593.590882	468626.687370	39.304922
2596.313115	469438.363815	39.309940
2599.102978	470243.021913	39.314957
2602.026975	471046.613412	39.319975
2604.628777	471846.384301	39.324992
2607.144605	472638.860552	39.330010
2609.843562	473436.830326	39.335028
2612.651367	474235.455451	39.340045
2615.057240	475030.071616	39.345063
2617.512119	475832.121620	39.350080
2620.669502	476626.495074	39.355098
2623.089222	477429.340389	39.360116
2625.774951	478216.096522	39.365133
2628.473894	479014.331552	39.370151
2631.361517	479817.954747	39.375168
2634.066534	480614.603731	39.380186
2636.537919	481401.409390	39.385204
2638.934456	482199.655452	39.390221
2641.769901	482971.083231	39.395239
2643.964898	483735.363384	39.400256
2646.935297	484494.080741	39.405274
2649.163223	485253.140707	39.410292
2651.671715	486016.867448	39.415309
2654.251123	486775.097520	39.420327
2656.479036	487544.408003	39.425344
2659.072530	488318.369390	39.430362
2661.292964	489111.286261	39.435380
2663.882163	489890.276770	39.440397
2666.063412	490689.235522	39.445415
2668.577722	491487.395968	39.450432
2671.532535	492280.097505	39.455450
2674.177623	493107.381055	39.460468
2676.387442	493913.048757	39.465485
2679.102748	494734.691392	39.470503
2681.363286	495574.937238	39.475520
2684.497474	496413.483770	39.480538
2686.702934	497258.750981	39.485556
2689.252744	498111.133120	39.490573
2691.832003	498961.903289	39.495591
2694.318355	499819.858896	39.500608
2697.378859	500682.366606	39.505626
2700.236209	501559.691794	39.510644
2702.610924	502417.884595	39.515661
2705.541243	503298.887963	39.520679
2708.317215	504177.448862	39.525696
2711.001156	505068.181148	39.530714
2713.482804	505957.637496	39.535732
2716.563277	506846.290859	39.540749
2719.437641	507738.811643	39.545767
2722.272887	508636.734384	39.550784
2724.911435	509524.405434	39.555802
2727.825463	510424.029900	39.560820
2730.638850	511329.417054	39.565837
2733.727526	512232.489359	39.570855
2735.936312	513128.296546	39.575872
2738.810402	514027.219028	39.580890
2741.369590	514941.966365	39.585908
2744.215047	515857.872832	39.590925
2747.134270	516758.697028	39.595943
2749.731718	517676.502548	39.600960
2752.694867	518592.480248	39.605978
2755.624158	519510.424354	39.610996
2758.125030	520431.860354	39.616013
2761.433459	521349.631800	39.621031
2764.073877	522280.403809	39.626048
2766.962241	523190.879908	39.631066
2769.458060	524114.310056	39.636084
2772.261485	525030.632490	39.641101
2775.651919	525959.543284	39.646119
2778.333677	526883.880505	39.651136
2781.204386	527794.181348	39.656154
2783.992434	528725.587307	39.661172
2786.827308	529648.871413	39.666189
2789.642262	530568.224552	39.671207
2792.135243	531493.865963	39.676224
2795.138071	532410.656391	39.681242
2798.240798	533335.225008	39.686260
2801.037096	534259.382775	39.691277
2804.059290	535175.341549	39.696295
2806.388256	536101.371294	39.701312
2809.632514	537016.019112	39.706330
2812.591924	537932.064539	39.711348
2815.326080	538853.069678	39.716365
2818.568319	539764.774708	39.721383
2820.855555	540685.684640	39.726400
2823.694956	541592.609563	39.731418
2826.320198	542502.730873	39.736436
2829.038410	543389.791206	39.741453
2832.417843	544267.633062	39.746471
2834.822682	545159.109279	39.751488
2837.574850	546026.281799	39.756506
2840.581738	546908.142410	39.761524
2843.070169	547791.088270	39.766541
2845.781531	548659.208766	39.771559
2848.292288	549564.914701	39.776576
2851.311014	550452.881267	39.781594
2854.030401	551353.859495	39.786612
2856.448911	552263.021250	39.791629
2859.629073	553164.859087	39.796647
2862.254070	554087.636605	39.801664
2864.908916	555003.058838	39.806682
2868.101452	555923.104132	39.811700
2870.236762	556859.843026	39.816717
2873.287157	557795.460896	39.821735
2875.909976	558750.828884	39.826752
2878.560119	559691.805438	39.831770
2881.347770	560659.065974	39.836788
2883.983109	561632.860986	39.841805
2887.100976	562596.659548	39.846823
2889.651112	563569.470905	39.851840
2892.346143	564547.007004	39.856858
2895.464342	565537.205088	39.861876
2898.211708	566549.833762	39.866893
2901.533115	567541.552123	39.871911
2904.411174	568544.864506	39.876928
2907.215359	569560.108622	39.881946
2910.434728	570562.704579	39.886964
2912.739521	571568.233425	39.891981
2915.966534	572580.707606	39.896999
2918.900866	573616.384663	39.902016
2921.812241	574639.083948	39.907034
2924.643779	575670.895497	39.912052
2927.413253	576708.251585	39.917069
2930.573869	577741.393296	39.922087
2933.418232	578792.359768	39.927104
2936.203967	579830.355671	39.932122
2939.315827	580880.899952	39.937140
2942.127145	581934.363038	39.942157
2945.413314	582989.412486	39.947175
2948.601863	584036.063246	39.952192
2951.295620	585096.593988	39.957210
2954.214589	586144.110492	39.962228
2957.144531	587222.163698	39.967245
2960.287179	588270.962700	39.972263
2963.250012	589337.041585	39.977280
2966.302348	590407.671601	39.982298
2969.420880	591465.265784	39.987316
2972.439234	592549.138867	39.992333
2975.477862	593607.757900	39.997351
2978.321447	594677.486109	40.002368
2981.223857	595737.389223	40.007386
2984.658323	596810.582830	40.012404
2987.418476	597879.131225	40.017421
2990.854368	598949.273094	40.022439
2993.577299	600018.582602	40.027456
2996.630872	601081.930604	40.032474
2999.382148	602151.338484	40.037492
3002.579610	603229.334074	40.042509
3006.130991	604292.453224	40.047527
3009.122130	605367.077727	40.052544
3012.059097	606433.301859	40.057562
3015.060964	607497.563512	40.062580
3018.375882	608565.226079	40.067597
3021.464740	609626.320464	40.072615
3024.433544	610667.623203	40.077632
3027.221821	611696.002742	40.082650
3030.298062	612714.836445	40.087668
3032.820384	613721.964737	40.092685
3036.021617	614742.392456	40.097703
3039.138564	615756.039175	40.102720
3041.987950	616783.237094	40.107738
3044.960720	617801.219369	40.112756
3047.757691	618837.882935	40.117773
3051.151670	619865.102152	40.122791
3054.178776	620904.830484	40.127808
3056.573854	621939.515750	40.132826
3059.589395	622986.892760	40.137844
3062.471401	624052.228441	40.142861
3065.956544	625099.572494	40.147879
3068.914155	626183.570188	40.152896
3071.656285	627249.060987	40.157914
3074.784282	628319.676109	40.162932
3077.455105	629406.190381	40.167949
3080.787820	630484.993471	40.172967
3083.728362	631579.779225	40.177984
3086.786458	632681.870840	40.183002
3089.214825	633785.148609	40.188020
3092.100353	634905.605548	40.193037
3095.420550	636027.168081	40.198055
3098.217125	637152.838021	40.203072
3101.532389	638293.968749	40.208090
3104.685510	639427.016919	40.213108
3107.360915	640577.729685	40.218125
3110.481059	641722.952396	40.223143
3113.846355	642889.304209	40.228160
3116.119852	644062.684559	40.233178
3119.802999	645228.516244	40.238196
3122.923683	646412.206253	40.243213
3126.007173	647583.000732	40.248231
3129.112999	648775.140018	40.253248
3131.749100	649963.626245	40.258266
3134.949633	651163.739198	40.263284
3138.403270	652370.891210	40.268301
3141.471096	653572.977473	40.273319
3144.783322	654786.036693	40.278336
3148.055064	655989.887411	40.283354
3151.130395	657204.679974	40.288372
3153.952306	658426.435199	40.293389
3157.227577	659642.684583	40.298407
3160.512607	660866.049242	40.303424
3163.550382	662100.998851	40.308442
3167.016126	663319.244552	40.313460
3170.016318	664558.564498	40.318477
3173.426358	665799.398516	40.323495
3176.668841	667025.620259	40.328512
3179.779255	668267.625799	40.333530
3183.504287	669495.240731	40.338548
3186.694241	670732.533008	40.343565
3190.141842	671956.293034	40.348583
3193.258321	673197.898547	40.353600
3196.282066	674426.378883	40.358618
3199.780531	675638.960777	40.363636
3203.153536	676878.593436	40.368653
3206.419754	678111.120612	40.373671
3209.714241	679324.348160	40.378688
3212.670978	680550.439336	40.383706
3215.895637	681785.513179	40.388724
3218.971916	683025.114094	40.393741
3221.924904	684256.571289	40.398759
3225.281092	685492.661920	40.403776
3228.412494	686731.997506	40.408794
3231.805958	687974.942711	40.413812
3235.033706	689200.222216	40.418829
3237.815301	690393.793981	40.423847
3240.986224	691598.109439	40.428864
3243.892759	692787.917309	40.433882
3247.170818	693992.388084	40.438900
3250.343766	695193.339803	40.443917
3253.346604	696401.447363	40.448935
3256.611241	697618.818076	40.453952
3259.461148	698832.865837	40.458970
3262.600276	700051.705106	40.463988
3265.420332	701298.185732	40.469005
3268.512637	702525.758465	40.474023
3271.524348	703777.998072	40.479040
3274.407606	705056.189412	40.484058
3277.555371	706320.078595	40.489076
3280.654726	707611.578121	40.494093
3284.044990	708909.620297	40.499111
3286.681685	710203.430186	40.504128
3289.707586	711523.962655	40.509146
3293.344343	712849.288006	40.514164
3296.893319	714172.787114	40.519181
3299.826015	715493.755445	40.524199
3302.740475	716841.485483	40.529216
3306.054357	718193.385536	40.534234
3309.521951	719539.897486	40.539252
3312.788574	720912.930563	40.544269
3315.387311	722294.499841	40.549287
3318.821722	723674.118784	40.554304
3322.144147	725068.057836	40.559322
3325.358194	726459.455575	40.564340
3328.721866	727863.390357	40.569357
3331.877507	729272.947766	40.574375
3335.312229	730693.131533	40.579392
3338.463477	732124.571140	40.584410
3341.770504	733551.435640	40.589428
3345.003804	734986.353620	40.594445
3348.669904	736428.742773	40.599463
3352.015263	737866.927187	40.604480
3355.017951	739323.362851	40.609498
3358.513860	740769.287498	40.614516
3362.381399	742232.791711	40.619533
3365.541243	743696.535582	40.624551
3369.071786	745161.375773	40.629568
3372.282196	746619.389058	40.634586
3375.586652	748086.035739	40.639604
3379.450756	749561.725995	40.644621
3382.800885	751031.061487	40.649639
3386.657299	752495.305279	40.654656
3389.603583	753982.223581	40.659674
3393.629210	755445.237403	40.664692
3396.913583	756911.293584	40.669709
3400.635728	758376.208171	40.674727
3404.059506	759830.850130	40.679744
3407.363571	761311.113160	40.684762
3411.308990	762762.398868	40.689780
3414.639927	764231.211975	40.694797
3418.042698	765705.577194	40.699815
3421.735590	767148.384223	40.704832
3424.991321	768615.364602	40.709850
3428.730405	770053.274567	40.714868
3432.458305	771517.734969	40.719885
3435.962766	772971.919632	40.724903
3439.544419	774418.681982	40.729920
3442.558369	775870.506520	40.734938
3446.401147	777310.318998	40.739956
3449.882882	778751.673221	40.744973
3453.187368	780199.641076	40.749991
3457.024977	781644.188957	40.755008
3460.014998	783066.048403	40.760013
3463.326350	784446.434179	40.765018
3466.963553	785756.637491	40.770023
3470.304643	787010.955565	40.775028
3473.645470	788197.573017	40.780032
3476.357270	789325.029723	40.785037
3479.449551	790376.236327	40.790042
3482.365812	791367.775261	40.795047
3484.820381	792287.143834	40.800052
3487.621416	793124.021274	40.805056
3490.085227	793890.777420	40.810061
3492.516239	794607.713721	40.815066
3494.781586	795256.406149	40.820071
3496.958101	795848.741821	40.825076
3499.370685	796370.445132	40.830080
3500.993968	796841.826724	40.835085
3502.983809	797251.858654	40.840090
3504.647423	797597.868180	40.845095
3506.069770	797907.188474	40.850100
3508.088084	798153.037025	40.855104
3509.065251	798369.258872	40.860109
3510.510149	798537.695633	40.865114
3512.096479	798660.024006	40.870119
3513.010893	798758.463774	40.875124
3514.211312	798800.714930	40.880128
3515.272744	798821.396395	40.885133
3516.243656	798799.644084	40.890138
3517.182169	798749.924886	40.895143
3517.677475	798680.452267	40.900148
3518.795902	798582.805311	40.905152
3519.375351	798452.462992	40.910157
3519.771366	798306.492848	40.915162
3520.434610	798128.869169	40.920167
3521.057024	797950.413331	40.925172
3521.476839	797727.567890	40.930176
3521.880663	797529.602908	40.935181
3522.758934	797277.954131	40.940186
3523.020272	797018.642293	40.945191
3523.184881	796751.433560	40.950196
3523.681150	796464.671179	40.955200
3523.658778	796183.284425	40.960205
3524.060610	795875.354659	40.965210
3524.652090	795559.279161	40.970215
3524.700467	795233.066318	40.975220
3524.979942	794891.087822	40.980224
3525.423636	794565.122435	40.985229
3525.565682	794208.991471	40.990234
3525.743274	793839.822807	40.995239
3525.419590	793475.186431	41.000244
3526.082580	793099.416202	41.005248
3525.888752	792736.242614	41.010253
3526.272285	792347.953626	41.015258
3526.277276	791968.940477	41.020263
3526.125515	791579.911410	41.025268
3526.368463	791183.230283	41.030272
3526.307867	790791.588127	41.035277
3526.541471	790383.268967	41.040282
3526.519379	789970.840981	41.045287
3526.397095	789565.235707	41.050292
3526.479742	789164.241855	41.055296
3526.119031	788745.999701	41.060301
3526.155261	788339.905068	41.065306
3526.654460	787922.652266	41.070311
3526.016075	787509.445472	41.075316
3526.337095	787092.763191	41.080320
3526.007196	786682.701844	41.085325
3525.965829	786266.178424	41.090330
3525.945221	785846.284119	41.095335
3525.786755	785428.895360	41.100340
3525.976789	785010.834778	41.105344
3525.996702	784597.793418	41.110349
3525.777506	784171.195199	41.115354
3525.621773	783752.282155	41.120359
3525.531638	783351.530905	41.125364
3525.546099	782930.427079	41.130368
3525.257316	782505.757907	41.135373
3525.030855	782087.890789	41.140378
3525.232500	781683.260092	41.145383
3525.093093	781276.842655	41.150388
3524.828484	780860.288139	41.155392
3524.823368	780456.114689	41.160397
3524.595242	780046.001740	41.165402
3524.568067	779637.702284	41.170407
3524.312469	779238.521155	41.175412
3524.329960	778824.263399	41.180416
3524.112336	778425.671030	41.185421
3524.172676	778017.019841	41.190426
3524.268493	777616.658055	41.195431
3523.811165	777215.873149	41.200436
3524.050244	776808.404429	41.205440
3523.859002	776412.946329	41.210445
3523.704314	776012.389975	41.215450
3523.479463	775615.614202	41.220455
3523.071966	775231.746899	41.225460
3523.541692	774829.742703	41.230464
3523.058657	774443.433781	41.235469
3522.886698	774044.889910	41.240474
3522.763402	773663.060303	41.245479
3522.636702	773282.147135	41.250484
3522.712415	772895.270633	41.255488
3522.178489	772507.390624	41.260493
3521.723863	772129.968869	41.265498
3521.840109	771744.699948	41.270503
3521.464291	771388.605900	41.275508
3521.538642	771017.838207	41.280512
3521.093312	770661.277139	41.285517
3521.226689	770295.439424	41.290522
3521.292503	769934.669741	41.295527
3520.905247	769576.322287	41.300532
3520.683822	769213.889498	41.305536
3520.574624	768866.549121	41.310541
3520.272582	768507.741743	41.315546
3520.288589	768163.994677	41.320551
3520.114968	767817.946525	41.325556
3520.073676	767472.205489	41.330560
3520.001612	767130.643146	41.335565
3519.166675	766786.824791	41.340570
3519.567781	766450.575508	41.345575
3519.191631	766119.171658	41.350580
3519.153950	765785.922557	41.355584
3518.823610	765466.412600	41.360589
3518.707695	765135.464556	41.365594
3518.851222	764808.452891	41.370599
3518.415197	764499.864928	41.375604
3518.671764	764166.791096	41.380608
3518.710792	763857.062898	41.385613
3518.256763	763532.658270	41.390618
3518.225948	763206.641095	41.395623
3518.068477	762905.684322	41.400628
3518.300929	762589.559285	41.405632
3517.796323	762272.901226	41.410637
3517.683405	761964.846403	41.415642
3517.840795	761653.725547	41.420647
3517.405829	761350.729987	41.425652
3517.417918	761055.048149	41.430656
3517.445175	760753.037715	41.435661
3516.839553	760447.419425	41.440666
3516.930567	760135.654979	41.445671
3516.526034	759865.896788	41.450676
3516.484923	759572.139272	41.455680
3516.459717	759279.749325	41.460685
3516.273242	759009.036554	41.465690
3516.202872	758716.188239	41.470695
3515.944853	758443.197186	41.475700
3516.255839	758155.001747	41.480704
3515.847727	757876.636019	41.485709
3515.622755	757612.344807	41.490714
3515.689094	757324.256926	41.495719
3515.643288	757055.573675	41.500724
3515.558199	756781.112539	41.505728
3515.380062	756514.751867	41.510733
3515.342916	756246.334849	41.515738
3515.527918	755982.511941	41.520743
3515.027517	755723.186336	41.525748
3514.926463	755439.942047	41.530752
3514.569394	755189.707575	41.535757
3514.472461	754930.584835	41.540762
3514.417590	754681.518216	41.545767
3514.325230	754429.832903	41.550772
3514.195544	754175.281739	41.555776
3513.871891	753926.333634	41.560781
3513.829572	753685.675992	41.565786
3513.828493	753441.300551	41.570791
3513.971741	753202.868680	41.575796
3513.938182	752962.977074	41.580800
3514.081125	752723.048910	41.585805
3513.706193	752482.260272	41.590810
3513.339769	752241.314543	41.595815
3513.298368	752006.777662	41.600820
3513.162485	751779.904708	41.605824
3512.940645	751543.210296	41.610829
3512.978299	751326.667690	41.615834
3512.833527	751096.614964	41.620839
3512.812345	750886.293431	41.625844
3512.414719	750645.945198	41.630848
3512.761022	750432.537535	41.635853
3512.348762	750211.097941	41.640858
3512.526443	749992.321305	41.645863
3512.127451	749779.512472	41.650868
3512.334673	749564.621737	41.655872
3512.218765	749354.175403	41.660877
3511.936326	749143.355545	41.665882
3511.925889	748931.447570	41.670887
3511.836610	748737.136657	41.675892
3512.256895	748525.245459	41.680896
3511.842597	748316.697804	41.685901
3511.345138	748114.334960	41.690906
3511.415167	747893.145088	41.695911
3511.076540	747712.290530	41.700916
3511.392867	747499.894397	41.705920
3511.286788	747310.146455	41.710925
3511.089846	747122.583342	41.715930
3511.135708	746927.562550	41.720935
3510.525514	746733.435740	41.725940
3510.976518	746546.493360	41.730944
3510.671256	746363.081422	41.735949
3510.890705	746172.757955	41.740954
3510.787206	745991.182232	41.745959
3510.472913	745814.925840	41.750964
3510.609381	745616.150289	41.755968
3510.226464	745439.402452	41.760973
3510.313993	745250.462352	41.765978
3510.288787	745072.362071	41.770983
3510.144238	744905.647211	41.775988
3509.746600	744726.067978	41.780992
3510.157099	744552.827612	41.785997
3509.682648	744376.021445	41.791002
3510.100182	744213.994689	41.796007
3509.778974	744045.609768	41.801012
3509.852411	743866.922052	41.806016
3509.736028	743709.768596	41.811021
3509.774330	743547.098405	41.816026
3509.583233	743358.850896	41.821031
3509.394518	743203.231993	41.826036
3509.636532	743040.418879	41.831040
3509.478772	742877.074911	41.836045
3509.209644	742709.443958	41.841050
3509.267578	742555.551740	41.846055
3508.593661	742390.749829	41.851060
3509.212840	742235.621553	41.856064
3509.009091	742088.093016	41.861069
3508.640290	741923.923402	41.866074
3508.859002	741768.011234	41.871079
3508.704307	741623.532058	41.876084
3508.860382	741477.317552	41.881088
3508.965113	741320.426230	41.886093
3508.547258	741169.206584	41.891098
3508.853423	741010.396546	41.896103
3508.332786	740877.141604	41.901108
3508.362796	740721.487200	41.906112
3508.566734	740589.591837	41.911117
3508.417716	740445.980522	41.916122
3508.435383	740301.844513	41.921127
3508.201858	740154.383744	41.926132
3508.391032	740002.745023	41.931136
3508.096475	739884.423896	41.936141
3507.939670	739733.677951	41.941146
3507.900732	739588.796321	41.946151
3507.648150	739458.787666	41.951156
3507.709521	739320.909077	41.956160
3507.407627	739197.384687	41.961165
3507.228544	739071.908795	41.966170
3507.479839	738951.505014	41.971175
3507.385555	738827.149125	41.976180
3507.264815	738687.706461	41.981184
3507.015247	738561.294145	41.986189
3507.331198	738452.943717	41.991194
3507.449668	738330.078711	41.996199
3507.144025	738211.586083	42.001204
3507.330973	738075.396876	42.006208
3507.392812	737961.292870	42.011213
3507.080685	737830.426305	42.016218
3507.249611	737708.483490	42.021223
3507.282383	737593.043076	42.026228
3507.079221	737476.303898	42.031232
3507.164901	737357.090849	42.036237
3506.673076	737243.859507	42.041242
3507.005940	737121.633309	42.046247
3506.763105	737013.751270	42.051252
3506.850370	736893.442411	42.056256
3506.914507	736775.857210	42.061261
3506.665610	736668.020987	42.066266
3506.688410	736548.756756	42.071271
3506.681718	736442.510625	42.076276
3506.690828	736318.197566	42.081280
3506.440166	736210.751369	42.086285
3506.204360	736103.647704	42.091290
3506.629925	735996.681080	42.096295
3506.249243	735893.953553	42.101300
3506.376860	735793.467022	42.106304
3506.310291	735685.884469	42.111309
3506.303606	735582.893365	42.116314
3505.877570	735470.863378	42.121319
3505.873482	735377.322311	42.126324
3506.367463	735274.096269	42.131328
3505.832396	735179.056572	42.136333
3505.549035	735081.004568	42.141338
3505.853647	734978.399869	42.146343
3505.739843	734899.621036	42.151348
3505.848143	734790.859255	42.156352
3505.816049	734695.681462	42.161357
3505.723531	734608.481686	42.166362
3505.781798	734510.564420	42.171367
3505.445141	734412.958528	42.176372
3505.619699	734309.574734	42.181376
3505.530851	734229.547723	42.186381
3505.669948	734152.798914	42.191386
3506.048526	734056.951886	42.196391
3505.690777	733956.373841	42.201396
3505.801508	733858.291486	42.206400
3505.650769	733764.310285	42.211405
3505.669135	733673.963405	42.216410
3505.795937	733579.934323	42.221415
3505.637774	733487.733274	42.226420
3505.715211	733396.680483	42.231424
3505.556190	733311.655855	42.236429
3505.177732	733219.933594	42.241434
3505.488045	733117.502266	42.246439
3505.406608	733029.837999	42.251444
3505.351700	732934.296588	42.256448
3505.616329	732860.930869	42.261453
3505.320543	732775.180488	42.266458
3505.491073	732682.470490	42.271463
3505.100866	732601.041173	42.276468
3505.323476	732511.687339	42.281472
3505.159017	732427.396952	42.286477
3505.092172	732350.268830	42.291482
3504.856903	732251.827858	42.296487
3504.835489	732190.089099	42.301492
3505.256172	732100.301980	42.306496
3505.276652	732021.769959	42.311501
3504.990025	731939.772255	42.316506
3505.171276	731846.159640	42.321511
3504.670767	731780.386948	42.326516
3504.872978	731706.922012	42.331520
3505.236906	731629.022812	42.336525
3504.673948	731547.858925	42.341530
3504.820182	731465.190886	42.346535
3504.762051	731392.162130	42.351540
3504.811630	731307.082031	42.356544
3504.828309	731234.633748	42.361549
3504.873820	731168.122366	42.366554
3505.213173	731074.573823	42.371559
3504.847154	730999.264829	42.376564
3504.799150	730915.137579	42.381568
3504.905164	730841.829214	42.386573
3504.548172	730774.390499	42.391578
3504.775429	730702.150370	42.396583
3504.527145	730631.919326	42.401588
3504.543493	730555.404190	42.406592
3504.617956	730486.158686	42.411597
3504.297961	730406.082358	42.416602
3504.481816	730334.638491	42.421607
3504.232319	730274.408440	42.426612
3504.181859	730196.613291	42.431616
3504.463231	730138.028135	42.436621
3504.045821	730076.932828	42.441626
3504.265737	730002.756182	42.446631
3504.126319	729940.920679	42.451636
3504.255505	729868.738824	42.456640
3504.416780	729808.982438	42.461645
3504.278130	729736.843543	42.466650
3504.687799	729675.163187	42.471655
3504.082593	729601.217889	42.476660
3504.284970	729537.292322	42.481664
3504.211314	729461.673241	42.486669
3503.638032	729418.033043	42.491674
3504.031430	729349.666374	42.496679
3503.902127	729291.439972	42.501684
3504.309381	729230.152888	42.506688
3504.232679	729160.128503	42.511693
3503.988910	729112.767049	42.516698
3504.330767	729035.985853	42.521703
3503.753592	728981.595472	42.526708
3503.835086	728915.406448	42.531712
3503.891047	728851.994957	42.536717
3503.918844	728804.487898	42.541722
3503.880835	728731.332837	42.546727
3503.989000	728681.533255	42.551732
3503.851372	728620.579041	42.556736
3504.127559	728561.686194	42.561741
3503.696791	728503.206619	42.566746
3504.283247	728426.329847	42.571751
3503.953510	728382.891644	42.576756
3503.880215	728318.803799	42.581760
3503.752291	728265.672097	42.586765
3503.844708	728202.843994	42.591770
3503.941496	728139.271624	42.596775
3503.510662	728091.340603	42.601780
3503.492600	728029.421051	42.606784
3503.729032	727974.939426	42.611789
3503.568725	727925.823471	42.616794
3503.654032	727859.080323	42.621799
3503.775135	727802.734060	42.626804
3503.458391	727751.364008	42.631808
3503.810207	727697.356921	42.636813
3503.711381	727643.225567	42.641818
3503.748511	727586.148538	42.646823
3503.658085	727536.919648	42.651828
3503.789583	727482.452032	42.656832
3503.577837	727434.233344	42.661837
3503.563143	727388.756264	42.666842
3503.801891	727320.645800	42.671847
3503.408493	727269.533060	42.676852
3503.677843	727209.244395	42.681856
3503.789115	727159.633197	42.686861
3503.675057	727107.036652	42.691866
3503.606855	727049.923694	42.696871
3503.470260	727001.442350	42.701876
3503.686180	726952.902635	42.706880
3503.521143	726898.876354	42.711885
3503.350263	726838.360224	42.716890
3503.394179	726794.505185	42.721895
3503.539636	726743.696737	42.726900
3503.819366	726698.365492	42.731904
3503.700989	726633.380028	42.736909
3503.566031	726593.517121	42.741914
3503.856153	726540.602606	42.746919
3503.346966	726487.670809	42.751924
3503.334104	726426.035549	42.756928
3503.359336	726374.253661	42.761933
3503.564450	726332.946101	42.766938
3503.394081	726279.164353	42.771943
3503.310319	726231.264330	42.776948
3503.516460	726182.523470	42.781952
3503.372874	726130.272364	42.786957
3502.880329	726082.488376	42.791962
3503.289590	726033.168111	42.796967
3503.487217	725990.472652	42.801972
3503.411976	725938.803672	42.806977
3503.332624	725894.666825	42.811981
3503.194203	725860.053344	42.816986
3503.670828	725807.252026	42.821991
3503.334863	725757.260068	42.826996
3503.507157	725708.224658	42.832001
3503.296943	725659.648401	42.837005
3503.320254	725600.329950	42.842010
3503.635040	725558.356236	42.847015
3503.397351	725514.193879	42.852020
3503.323140	725464.553436	42.857025
3503.134074	725417.557983	42.862029
3503.312043	725363.514621	42.867034
3503.661296	725318.610295	42.872039
3503.222399	725256.788680	42.877044
3503.086448	725216.473249	42.882049
3503.334000	725164.399323	42.887053
3503.196684	725125.173893	42.892058
3503.141418	725075.230642	42.897063
3503.119035	725040.099023	42.902068
3503.449447	724997.624311	42.907073
3503.466502	724937.013633	42.912077
3503.054608	724899.566861	42.917082
3503.246575	724838.678852	42.922087
3503.267965	724794.023918	42.927092
3502.821478	724752.518434	42.932097
3503.212581	724720.588153	42.937101
3502.968505	724675.332058	42.942106
3503.171478	724631.389700	42.947111
3503.108941	724585.607612	42.952116
3503.093649	724546.260196	42.957121
3503.189998	724511.751029	42.962125
3503.003762	724465.691299	42.967130
3502.983662	724394.130026	42.972135
3503.235266	724361.378817	42.977140
3502.932869	724331.692396	42.982145
3503.011855	724288.561609	42.987149
3502.724476	724240.039238	42.992154
3503.247445	724205.805425	42.997159
3503.400286	724171.880264	43.002164
3503.473796	724118.440681	43.007169
3503.511991	724077.050175	43.012173
3502.719268	724019.242523	43.017178
3503.174430	723973.817796	43.022183
3503.288315	723946.688220	43.027188
3502.971306	723908.130914	43.032193
3503.015991	723858.213376	43.037197
3502.703179	723812.319538	43.042202
3503.117088	723772.600327	43.047207
3503.124804	723740.828556	43.052212
3502.967803	723690.298900	43.057217
3503.382830	723636.155583	43.062221
3503.243460	723607.877068	43.067226
3503.076498	723551.549104	43.072231
3503.085073	723513.580654	43.077236
3503.032404	723473.738623	43.082241
3503.257962	723428.546994	43.087245
3502.878494	723381.472157	43.092250
3503.082873	723348.129915	43.097255
3502.882564	723307.072243	43.102260
3502.911630	723267.760985	43.107265
3502.656101	723223.539709	43.112269
3502.517207	723192.583060	43.117274
3503.028756	723158.346794	43.122279
3503.068060	723120.173202	43.127284
3503.003563	723065.609482	43.132289
3503.005857	723037.156965	43.137293
3503.038514	722998.934340	43.142298
3503.295787	722948.778003	43.147303
3503.134246	722911.330505	43.152308
3503.026155	722860.143310	43.157313
3502.956185	722816.484113	43.162317
3502.871694	722786.012674	43.167322
3503.195229	722739.264469	43.172327
3502.781640	722698.189343	43.177332
3502.876480	722663.028283	43.182337
3502.973958	722618.646463	43.187341
3502.900455	722580.340254	43.192346
3502.978629	722525.055463	43.197351
3502.746715	722501.200263	43.202356
3503.040769	722468.434560	43.207361
3503.192969	722421.117929	43.212365
3502.903950	722379.326683	43.217370
3503.193967	722326.236413	43.222375
3503.180483	722301.452339	43.227380
3503.125998	722256.201305	43.232385
3503.177918	722210.337612	43.237389
3502.916505	722173.398960	43.242394
3502.924479	722134.383233	43.247399
3502.823852	722089.188463	43.252404
3503.246855	722052.334796	43.257409
3503.566382	721994.032237	43.262413
3503.394957	721953.607554	43.267418
3503.328061	721912.471399	43.272423
3503.002128	721866.221884	43.277428
3502.604904	721817.653801	43.282433
3503.113872	721777.859787	43.287437
3503.024712	721749.566641	43.292442
3503.136972	721694.865607	43.297447
3503.098680	721672.413830	43.302452
3503.018164	721627.758571	43.307457
3503.033787	721591.515328	43.312461
3502.896426	721543.547321	43.317466
3502.790070	721506.381836	43.322471
3502.945144	721455.687950	43.327476
3502.626943	721417.962040	43.332481
3502.927185	721383.654114	43.337485
3502.757825	721351.852768	43.342490
3503.262997	721306.058127	43.347495
3502.897939	721274.040834	43.352500
3502.757771	721234.896547	43.357505
3502.888070	721190.402514	43.362509
3502.821517	721153.972583	43.367514
3502.912844	721112.707231	43.372519
3502.451743	721075.399947	43.377524
3502.607068	721048.154886	43.382529
3503.072971	721015.503875	43.387533
3502.742016	720980.455420	43.392538
3503.007774	720923.641625	43.397543
3502.652477	720893.158263	43.402548
3502.526592	720857.183037	43.407553
3502.588412	720828.961037	43.412557
3502.758332	720800.820293	43.417562
3502.551445	720760.593964	43.422567
3502.685185	720732.756443	43.427572
3502.451553	720697.145351	43.432577
3502.893650	720660.084038	43.437581
3502.697787	720633.837554	43.442586
3502.648972	720595.666856	43.447591
3502.632531	720556.102318	43.452596
3502.595455	720510.590978	43.457601
3502.916634	720482.424234	43.462605
3502.336410	720448.356694	43.467610
3502.681577	720408.979793	43.472615
3502.471906	720382.437286	43.477620
3502.576382	720343.446824	43.482625
3502.833395	720316.529704	43.487629
3502.665640	720295.682243	43.492634
3502.929478	720240.797907	43.497639
3502.643232	720210.151904	43.502644
3502.667178	720169.785511	43.507649
3502.879093	720139.057164	43.512653
3502.591119	720099.931883	43.517658
3502.829938	720063.694786	43.522663
3502.601880	720038.245104	43.527668
3502.646312	719999.808376	43.532673
3502.578843	719958.563463	43.537677
3502.135817	719943.165430	43.542682
3502.949550	719894.684083	43.547687
3502.646098	719869.543830	43.552692
3502.678115	719829.025693	43.557697
3502.330007	719793.528768	43.562701
3502.661467	719763.820683	43.567706
3502.666837	719731.686817	43.572711
3502.756243	719697.902567	43.577716
3502.430907	719668.054420	43.582721
3502.568212	719626.327825	43.587725
3502.390323	719614.307116	43.592730
3502.631737	719569.240631	43.597735
3502.418791	719531.340040	43.602740
3502.477895	719501.031236	43.607745
3502.563764	719462.486022	43.612749
3502.330253	719438.771045	43.617754
3502.418073	719393.679329	43.622759
3502.432436	719368.485195	43.627764
3502.720184	719330.253240	43.632769
3502.754663	719302.328114	43.637773
3502.226786	719278.066093	43.642778
3502.299651	719234.414114	43.647783
3502.703211	719210.692699	43.652788
3502.616764	719169.149459	43.657793
3502.824748	719147.642114	43.662797
3502.442327	719129.207497	43.667802
3502.675765	719087.412776	43.672807
3502.411769	719071.041378	43.677812
3502.712506	719039.897612	43.682817
3502.581328	718998.559262	43.687821
3502.482695	718962.422578	43.692826
3502.642379	718920.738360	43.697831
3502.458734	718900.137987	43.702836
3502.248313	718868.532282	43.707841
3502.584791	718844.275356	43.712845
3502.313255	718823.986837	43.717850
3502.254578	718769.096365	43.722855
3502.378935	718750.577407	43.727860
3502.394681	718716.107004	43.732865
3502.073338	718689.676688	43.737869
3502.355619	718653.525498	43.742874
3502.516885	718628.701682	43.747879
3502.403517	718600.203433	43.752884
3502.503771	718577.075742	43.757889
3502.612137	718544.920335	43.762893
3502.266805	718515.666495	43.767898
3502.674029	718480.188304	43.772903
3502.726227	718450.223992	43.777908
3502.554182	718417.271170	43.782913
3502.835201	718382.706087	43.787917
3502.755796	718348.448230	43.792922
3502.523880	718310.892394	43.797927
3502.915813	718286.178345	43.802932
3502.355779	718253.189612	43.807937
3501.959318	718220.124199	43.812941
3502.195349	718196.923487	43.817946
3502.610741	718165.063212	43.822951
3502.724942	718138.757776	43.827956
3502.677579	718106.874333	43.832961
3502.356717	718072.208749	43.837965
3502.591339	718041.022562	43.842970
3502.599875	717994.299618	43.847975
3502.755604	717977.212134	43.852980
3502.649586	717933.334842	43.857985
3502.722754	717911.747337	43.862989
3502.724078	717870.728766	43.867994
3502.780756	717827.121704	43.872999
3502.497059	717789.026461	43.878004
3502.241210	717765.211207	43.883009
3502.880130	717727.955662	43.888013
3502.798084	717706.839603	43.893018
3502.820776	717660.211663	43.898023
3503.005843	717625.113661	43.903028
3502.684794	717589.751698	43.908033
3502.529427	717560.909621	43.913037
3502.763815	717519.305315	43.918042
3502.969055	717482.368145	43.923047
3502.905024	717461.050093	43.928052
3502.602922	717429.950068	43.933057
3502.642122	717383.119459	43.938061
3502.623554	717355.593389	43.943066
3502.728904	717311.033178	43.948071
3502.588253	717286.007119	43.953076
3502.381706	717249.186374	43.958081
3502.776045	717206.462899	43.963085
3502.362206	717180.142253	43.968090
3502.641838	717158.121962	43.973095
3502.415895	717116.740319	43.978100
3502.548693	717090.329321	43.983105
3502.729132	717058.652370	43.988109
3502.629327	717034.412492	43.993114
3502.862418	716985.960386	43.998119
3502.805649	716944.500413	44.003124
3502.714682	716908.502406	44.008129
3502.776812	716882.747262	44.013133
3502.589656	716853.759172	44.018138
3502.765264	716798.717965	44.023143
3502.629935	716773.788710	44.028148
3502.779193	716741.371616	44.033153
3502.679064	716699.669549	44.038157
3502.654593	716679.781568	44.043162
3502.598281	716651.664132	44.048167
3502.501440	716608.572091	44.053172
3502.537503	716581.183298	44.058177
3502.365156	716538.897050	44.063181
3502.166270	716522.460319	44.068186
3502.429884	716475.091593	44.073191
3502.388713	716464.184791	44.078196
3501.943174	716430.078631	44.083201
3502.373122	716408.478079	44.088205
3502.141446	716385.250209	44.093210
3502.600531	716345.289733	44.098215
3502.200387	716319.112948	44.103220
3502.055524	716289.371814	44.108225
3502.603364	716257.581698	44.113229
3502.663397	716236.636961	44.118234
3502.479338	716211.118758	44.123239
3502.731913	716169.703206	44.128244
3502.550651	716129.499951	44.133249
3502.544021	716108.367441	44.138253
3502.297851	716081.966106	44.143258
3502.182295	716044.380934	44.148263
3502.160846	716018.934573	44.153268
3502.072099	716000.791928	44.158273
3502.389013	715959.166298	44.163277
3502.043321	715941.561967	44.168282
3501.843205	715904.138932	44.173287
3502.191844	715895.399647	44.178292
3502.165053	715867.274721	44.183297
3502.181307	715831.055984	44.188301
3502.021342	715821.259368	44.193306
3502.056022	715790.742716	44.198311
3502.041305	715781.864738	44.203316
3502.186928	715748.749855	44.208321
3502.465123	715721.070305	44.213325
3501.813691	715701.878657	44.218330
3502.138177	715678.160296	44.223335
3502.275775	715648.717638	44.228340
3501.973809	715625.251186	44.233345
3502.364302	715602.712435	44.238349
3502.071147	715574.382356	44.243354
3502.245576	715551.482168	44.248359
3502.007415	715521.108721	44.253364
3501.847776	715502.331712	44.258369
3502.570644	715477.257203	44.263373
3502.255055	715464.310559	44.268378
3502.252227	715433.501113	44.273383
3502.395640	715405.693895	44.278388
3502.016590	715376.285800	44.283393
3502.258260	715349.107186	44.288397
3502.180454	715335.277725	44.293402
3502.141510	715296.188161	44.298407
3502.123721	715270.093946	44.303412
3502.311174	715248.679224	44.308417
3502.630482	715215.831317	44.313421
3502.057992	715198.461256	44.318426
3502.247028	715153.429285	44.323431
3502.576127	715153.077421	44.328436
3502.330782	715117.593332	44.333441
3502.329437	715077.355403	44.338445
3502.150663	715045.134672	44.343450
3502.283533	715029.384593	44.348455
3502.387399	714992.949352	44.353460
3502.201451	714981.717169	44.358465
3502.541043	714944.250552	44.363469
3502.306464	714930.644724	44.368474
3502.455472	714885.220984	44.373479
3502.343960	714851.301459	44.378484
3501.833713	714840.817160	44.383489
3502.117878	714821.717421	44.388493
3502.067029	714794.138664	44.393498
3501.847784	714770.358492	44.398503
3502.341226	714740.357855	44.403508
3502.087252	714719.907644	44.408513
3502.473315	714684.168839	44.413517
3502.144665	714679.261244	44.418522
3502.163203	714629.788950	44.423527
3502.146402	714615.253599	44.428532
3501.956109	714584.819267	44.433537
3502.235397	714556.788389	44.438541
3502.297523	714544.423135	44.443546
3502.333511	714511.271838	44.448551
3502.295537	714487.361761	44.453556
3502.268158	714464.045302	44.458561
3502.555142	714436.757047	44.463565
3502.297661	714417.050970	44.468570
3501.996036	714381.970012	44.473575
3502.359203	714351.542884	44.478580
3502.372280	714321.768773	44.483585
3502.318807	714291.310838	44.488589
3502.148714	714270.746475	44.493594
3502.262387	714237.730166	44.498599
3502.437239	714213.536143	44.503604
3502.106451	714195.876078	44.508609
3502.327534	714151.577795	44.513613
3502.174719	714121.482964	44.518618
3502.023452	714115.156415	44.523623
3501.979110	714101.220172	44.528628
3501.863533	714091.414226	44.533633
3502.193570	714040.348887	44.538637
3501.899177	714028.587461	44.543642
3502.203216	714009.730724	44.548647
3502.025236	713995.568217	44.553652
3502.071245	713955.069024	44.558657
3502.278914	713933.052170	44.563661
3502.307673	713922.279420	44.568666
3502.244225	713879.515267	44.573671
3502.452363	713849.608107	44.578676
3502.053970	713836.126747	44.583681
3502.433449	713801.873987	44.588685
3502.247502	713779.871969	44.593690
3501.665006	713751.881174	44.598695
3501.938495	713724.146233	44.603700
3501.830565	713717.117514	44.608705
3501.958981	713687.222915	44.613709
3501.903195	713676.265286	44.618714
3502.005667	713654.016921	44.623719
3502.156756	713619.801057	44.628724
3501.628130	713604.852059	44.633729
3502.212623	713586.394788	44.638733
3502.138881	713566.408326	44.643738
3502.231315	713542.722211	44.648743
3501.830154	713506.016398	44.653748
3501.504012	713505.474691	44.658753
3501.738742	713484.891335	44.663757
3501.567873	713456.037733	44.668762
3501.707022	713456.560736	44.673767
3501.887942	713434.596619	44.678772
3501.886568	713415.292630	44.683777
3502.182913	713389.488219	44.688781
3501.718648	713379.193018	44.693786
3501.929548	713346.405337	44.698791
3502.066076	713321.520318	44.703796
3501.917504	713307.848071	44.708801
3501.570518	713291.230926	44.713805
3501.564384	713284.036195	44.718810
3501.575050	713267.707456	44.723815
3501.869184	713243.292501	44.728820
3502.022245	713229.917813	44.733825
3501.791953	713210.799956	44.738829
3501.937366	713183.878377	44.743834
3502.278377	713166.452849	44.748839
3501.762957	713136.066868	44.753844
3501.626402	713126.709901	44.758849
3502.080873	713110.704751	44.763853
3501.852645	713079.973483	44.768858
3501.670940	713068.192149	44.773863
3501.898174	713059.618833	44.778868
3501.819667	713034.123243	44.783873
3502.106044	713015.912367	44.788877
3501.600920	712994.407544	44.793882
3502.175821	712964.039802	44.798887
3502.294315	712951.464420	44.803892
3502.179379	712930.242539	44.808897
3502.000020	712909.031221	44.813901
3502.312543	712883.520376	44.818906
3501.938889	712854.102592	44.823911
3502.293560	712830.669049	44.828916
3501.753038	712822.321255	44.833921
3501.844446	712796.598438	44.838925
3501.937392	712772.463424	44.843930
3501.872211	712755.501016	44.848935
3502.415030	712727.718439	44.853940
3501.905083	712708.298119	44.858945
3501.992830	712684.858526	44.863949
3502.239211	712657.720121	44.868954
3502.105297	712629.999100	44.873959
3502.217030	712604.818283	44.878964
3502.184521	712590.579821	44.883969
3501.882478	712547.649732	44.888973
3502.093617	712545.183100	44.893978
3502.212653	712512.854008	44.898983
3502.170767	712490.626375	44.903988
3502.290053	712469.017330	44.908993
3502.261027	712433.833737	44.913997
3502.096210	712415.398131	44.919002
3502.302140	712395.362823	44.924007
3502.088881	712369.043702	44.929012
3502.038153	712339.322762	44.934017
3502.485873	712318.205165	44.939021
3502.373608	712297.179786	44.944026
3502.066828	712267.302256	44.949031
3502.315331	712248.698920	44.954036
3502.192021	712226.781805	44.959041
3502.283806	712185.472491	44.964045
3502.070963	712174.191368	44.969050
3502.142043	712144.995637	44.974055
3502.508848	712106.767494	44.979060
3501.996451	712083.226594	44.984065
3502.232759	712067.106531	44.989069
3502.194701	712036.141608	44.994074
3501.963474	712015.830002	44.999079
3502.237488	711982.728852	45.004084
3501.949466	711984.166109	45.009089
3502.090892	711943.045971	45.014093
3502.267681	711918.199837	45.019098
3502.124760	711904.127319	45.024103
3502.255622	711877.055089	45.029108
3501.767368	711854.800070	45.034113
3502.464105	711815.771739	45.039117
3502.368863	711797.025515	45.044122
3501.986458	711775.646275	45.049127
3502.354459	711759.106850	45.054132
3502.078391	711733.292455	45.059137
3502.207073	711702.993738	45.064141
3502.297000	711680.494087	45.069146
3501.944563	711659.407430	45.074151
3502.351471	711626.680084	45.079156
3502.062728	711609.950766	45.084161
3502.398327	711576.242255	45.089165
3502.150386	711569.830455	45.094170
3502.263298	711529.805014	45.099175
3502.511680	711501.918044	45.104180
3502.570205	711475.749915	45.109185
3502.403826	711450.214407	45.114189
3502.266373	711421.000912	45.119194
3502.155643	711383.940223	45.124199
3502.651622	711353.679016	45.129204
3502.362666	711330.744495	45.134209
3502.417896	711300.754274	45.139213
3502.316550	711276.895214	45.144218
3502.153444	711248.032817	45.149223
3502.071802	711221.738089	45.154228
3502.168519	711194.172930	45.159233
3502.259299	711170.381191	45.164237
3502.103302	711158.493687	45.169242
3502.349238	711127.131188	45.174247
3502.264168	711090.362824	45.179252
3502.041507	711073.720838	45.184257
3502.227328	711048.572843	45.189261
3502.031817	711034.209712	45.194266
3501.869860	710997.403976	45.199271
3502.426626	710974.924818	45.204276
3502.277292	710958.816561	45.209281
3502.418415	710923.052640	45.214285
3502.338062	710896.111372	45.219290
3501.995628	710867.376512	45.224295
3502.255025	710842.712189	45.229300
3501.630840	710836.113625	45.234305
3501.944793	710797.987597	45.239309
3502.192621	710786.281236	45.244314
3501.980731	710762.786434	45.249319
3502.082105	710758.848149	45.254324
3502.323302	710738.257081	45.259329
3502.291228	710704.754629	45.264333
3502.232723	710682.574647	45.269338
3502.076444	710653.163051	45.274343
3502.172501	710623.660134	45.279348
3502.273958	710593.808732	45.284353
3502.298053	710568.884537	45.289357
3502.202267	710541.497913	45.294362
3502.213516	710520.695997	45.299367
3502.006007	710486.973384	45.304372
3502.050647	710476.292929	45.309377
3502.360724	710440.449502	45.314381
3501.802504	710423.017605	45.319386
3501.787371	710396.163295	45.324391
3502.347117	710364.597357	45.329396
3502.163240	710361.003749	45.334401
3502.113155	710329.984955	45.339405
3502.236104	710316.858869	45.344410
3502.240793	710274.661047	45.349415
3502.594642	710251.816274	45.354420
3501.950317	710233.951381	45.359425
3502.337465	710200.477159	45.364429
3502.287329	710160.720374	45.369434
3502.338292	710146.662643	45.374439
3502.317426	710120.006987	45.379444
3502.110873	710096.261243	45.384449
3502.004995	710058.052152	45.389453
3502.175431	710060.456728	45.394458
3502.215518	710022.074490	45.399463
3502.249044	709999.182532	45.404468
3501.838717	709975.718255	45.409473
3501.864161	709944.834551	45.414477
3502.171337	709943.741430	45.419482
3501.986157	709918.949111	45.424487
3502.123486	709904.926397	45.429492
3501.880014	709864.653983	45.434497
3502.644802	709842.634037	45.439501
3502.290560	709819.060794	45.444506
3502.022414	709794.629309	45.449511
3502.101088	709758.821150	45.454516
3501.702119	709742.304904	45.459521
3502.137077	709725.502277	45.464525
3501.907659	709704.738027	45.469530
3501.749735	709681.082408	45.474535
3502.168628	709668.055504	45.479540
3501.645128	709636.863958	45.484545
3502.091061	709624.974425	45.489549
3502.255909	709598.634073	45.494554
3502.098255	709584.361553	45.499559
3502.131165	709552.283653	45.504564
3502.053888	709523.947399	45.509569
3502.201222	709496.070525	45.514573
3502.190449	709473.383050	45.519578
3502.026976	709452.259781	45.524583
3502.282590	709431.365297	45.529588
3501.677737	709401.030321	45.534593
3501.867042	709382.678735	45.539597
3502.283078	709371.042022	45.544602
3502.365520	709338.011825	45.549607
3502.473078	709321.113405	45.554612
3501.978392	709282.170517	45.559617
3502.369624	709260.458878	45.564621
3502.019353	709240.011309	45.569626
3502.226237	709220.812434	45.574631
3502.679070	709191.940883	45.579636
3502.261816	709177.015355	45.584641
3502.262860	709136.748868	45.589645
3502.331185	709117.274689	45.594650
3502.032579	709084.157346	45.599655
3502.423812	709064.729143	45.604660
3501.789621	709038.369773	45.609665
3502.253151	709006.020267	45.614669
3502.326403	708984.956138	45.619674
3502.191544	708962.585661	45.624679
3502.441336	708938.761503	45.629684
3502.154376	708909.216473	45.634689
3502.034369	708880.338958	45.639693
3502.156690	708860.656691	45.644698
3502.278569	708835.115502	45.649703
3502.136875	708820.491509	45.654708
3502.210571	708796.795277	45.659713
3502.393390	708759.873424	45.664717
3502.204265	708723.757491	45.669722
3502.191013	708710.701035	45.674727
3502.192323	708676.887209	45.679732
3502.124566	708653.710419	45.684737
3502.222513	708634.726794	45.689741
3502.108904	708603.662545	45.694746
3502.122352	708579.528758	45.699751
3502.240567	708547.135112	45.704756
3502.021716	708536.148073	45.709761
3501.871806	708500.024733	45.714765
3501.878013	708493.717693	45.719770
3501.762983	708474.272264	45.724775
3502.103168	708441.444410	45.729780
3501.789266	708425.954338	45.734785
3502.306586	708412.313459	45.739789
3502.196711	708384.078110	45.744794
3501.967242	708349.357576	45.749799
3502.007150	708326.261469	45.754804
3502.264166	708328.701927	45.759809
3501.989865	708285.199568	45.764813
3502.101635	708246.251342	45.769818
3502.020090	708178.683362	45.774823
3502.485441	708026.062331	45.779828
3501.848492	707835.780957	45.784833
3501.587319	707582.415906	45.789837
3502.024995	707286.319103	45.794842
3501.232536	706921.035564	45.799847
3501.348329	706506.815358	45.804852
3501.084917	706045.005971	45.809857
3500.897531	705505.870999	45.814861
3500.556055	704914.271333	45.819866
3499.524016	704262.783193	45.824871
3499.929443	703549.104840	45.829876
3499.291081	702784.561065	45.834881
3498.652933	701955.400667	45.839885
3498.287120	701089.639156	45.844890
3497.343786	700153.658291	45.849895
3496.919141	699145.962693	45.854900
3496.464110	698109.571046	45.859905
3495.601900	696993.274573	45.864909
3495.128022	695822.919172	45.869914
3494.484240	694580.025287	45.874919
3493.366048	693296.447177	45.879924
3492.727714	691951.663614	45.884929
3491.981386	690531.613835	45.889933
3491.082814	689072.996123	45.894938
3490.149476	687545.013873	45.899943
3489.188966	685958.035916	45.904948
3488.207544	684307.799207	45.909953
3486.932639	682606.516444	45.914957
3485.843472	680871.564535	45.919962
3484.807535	679049.143579	45.924967
3483.534249	677178.765760	45.929972
3482.155794	675271.645792	45.934977
3481.040048	673293.206598	45.939981
3479.714229	671262.380255	45.944986
3478.212805	669176.885365	45.949991
3476.964046	667048.340241	45.954996
3475.286945	664872.141014	45.960001
3473.933954	662635.358316	45.965005
3472.478267	660348.655922	45.970010
3470.895028	658008.261324	45.975015
3469.543558	655631.010482	45.980020
3467.445047	653217.541345	45.985025
3466.097268	650732.058651	45.990029
3464.541779	648202.109211	45.995034
3462.803594	645622.110755	46.000039
3460.822791	643011.091344	46.005044
3458.822505	640344.536843	46.010049
3456.878295	637640.107640	46.015053
3455.037550	634887.662920	46.020058
3452.846010	632095.554830	46.025063
3451.219632	629261.253531	46.030068
3448.925691	626394.851379	46.035073
3446.867025	623467.674652	46.040077
3444.798944	620526.174434	46.045082
3442.472331	617528.933879	46.050087
3440.525519	614498.221578	46.055092
3438.596475	611428.309890	46.060097
3436.416115	608304.469816	46.065101
3433.961973	605168.920670	46.070106
3431.344233	601976.417929	46.075111
3429.285249	598748.694901	46.080116
3426.892254	595492.256904	46.085121
3424.574757	592177.030703	46.090125
3422.118978	588845.775503	46.095130
3419.246759	585476.065572	46.100135
3416.867612	582080.902294	46.105140
3413.850142	578655.734155	46.110145
3411.290410	575203.837588	46.115149
3408.710869	571710.385522	46.120154
3405.842071	568197.848619	46.125159
3403.677904	564638.921386	46.130164
3400.280807	561073.179539	46.135169
3397.755336	557464.969445	46.140173
3394.983712	553842.520281	46.145178
3392.578861	550189.855378	46.150183
3389.655494	546498.387391	46.155188
3386.520577	542784.336761	46.160193
3383.659099	539048.123634	46.165197
3380.752038	535286.315498	46.170202
3377.437182	531492.505996	46.175207
3374.854807	527684.872250	46.180212
3371.565760	523855.374245	46.185217
3368.366919	519990.190929	46.190221
3365.554050	516117.452266	46.195226
3362.270389	512217.954840	46.200231
3359.500874	508299.871949	46.205236
3356.141537	504357.118474	46.210241
3352.872661	500382.854398	46.215245
3349.699515	496396.141999	46.220250
3346.592868	492398.562147	46.225255
3343.660044	488370.572250	46.230260
3339.956179	484340.062236	46.235265
3336.747423	480275.701819	46.240269
3333.156031	476208.824476	46.245274
3329.647354	472129.188256	46.250279
3326.383523	468020.867694	46.255284
3322.929335	463913.830761	46.260289
3319.591246	459784.325742	46.265293
3315.976595	455645.652415	46.270298
3312.762426	451501.818649	46.275303
3309.143738	447325.383977	46.280308
3305.424025	443149.521507	46.285313
3301.946769	438964.351233	46.290317
3298.508727	434770.884106	46.295322
3294.672948	430563.319050	46.300327
3291.230707	426351.739652	46.305332
3287.665472	422134.775509	46.310337
3283.989677	417904.519332	46.315341
3280.393518	413662.881966	46.320346
3276.744213	409411.041741	46.325351
3273.154973	405156.944920	46.330356
3269.227022	400896.534468	46.335361
3265.376746	396626.099341	46.340365
3261.537788	392350.417619	46.345370
3257.787724	388085.963247	46.350375
3254.318144	383810.944325	46.355380
3250.208874	379536.154395	46.360385
3246.503557	375248.372053	46.365389
3242.748466	370963.554390	46.370394
3238.577827	366682.850425	46.375399
3235.082083	362387.381377	46.380404
3231.206258	358111.981498	46.385409
3227.533009	353817.810047	46.390413
3223.786555	349521.743718	46.395418
3219.895069	345225.187383	46.400423
3215.989169	340923.634792	46.405428
3211.375927	336634.854773	46.410433
3207.494147	332324.349904	46.415437
3203.899531	328034.332965	46.420442
3199.709281	323751.966065	46.425447
3196.241143	319456.025637	46.430452
3192.077681	315180.010632	46.435457
3187.946876	310900.782855	46.440461
3183.883064	306623.269294	46.445466
3179.683198	302348.694152	46.450471
3175.894345	298087.172140	46.455476
3171.804759	293842.966509	46.460481
3168.014242	289579.609261	46.465485
3163.800444	285331.844803	46.470490
3159.852882	281096.600003	46.475495
3155.920857	276849.716426	46.480500
3151.626741	272623.567307	46.485505
3147.331912	268394.656567	46.490509
3143.658741	264182.052039	46.495514
3139.386373	259964.911443	46.500519
3135.426884	255765.336458	46.505524
3131.086373	251583.230368	46.510529
3127.129003	247392.227386	46.515533
3123.080418	243222.348354	46.520538
3118.727826	239060.657016	46.525543
3114.538636	234905.972965	46.530548
3110.559077	230764.824930	46.535553
3106.326480	226632.085169	46.540557
3101.830642	222510.241919	46.545562
3097.722140	218408.956374	46.550567
3093.745502	214308.730203	46.555572
3089.788944	210186.556333	46.560577
3085.859174	206055.845712	46.565581
3081.581796	201994.148462	46.570586
3077.337695	197939.635834	46.575591
3073.108122	193902.177237	46.580596
3069.017197	189880.339796	46.585601
3064.621424	185860.198283	46.590605
3060.637059	181849.781492	46.595610
3056.118243	177857.517023	46.600615
3051.886862	173881.703181	46.605620
3047.765138	169925.243224	46.610625
3043.657242	165987.031194	46.615629
3039.409241	162053.899730	46.620634
3035.343700	158141.936311	46.625639
3031.105988	154228.876740	46.630644
3026.742823	150351.871753	46.635649
3022.329742	146482.291769	46.640653
3018.148307	142619.619277	46.645658
3013.779946	138782.151429	46.650663
3009.982319	134962.307914	46.655668
3005.407107	131164.525553	46.660673
3000.740955	127369.089529	46.665677
2996.702892	123598.548493	46.670682
2991.899577	119849.236187	46.675687
2987.802866	116124.395540	46.680692
2983.535373	112416.592242	46.685697
2978.959845	108732.369675	46.690701
2974.688333	105060.291101	46.695706
2970.034926	101404.990385	46.700711
2966.048893	97785.143827	46.705716
2961.194492	94184.660496	46.710721
2956.864560	90600.909297	46.715725
2952.305307	87054.263012	46.720730
2947.647026	83520.146672	46.725735
2943.052102	80010.437032	46.730740
2938.738010	76535.998594	46.735745
2934.310211	73081.699405	46.740749
2929.464707	69654.284890	46.745754
2924.657007	66254.590121	46.750759
2920.022884	62874.661521	46.755764
2915.038891	59554.662127	46.760769
2910.300204	56240.238621	46.765773
2905.447835	52972.609501	46.770778
2900.276675	49740.293559	46.775783
2895.232734	46541.463891	46.780788
2889.800404	43391.239586	46.785793
2884.068916	40294.254866	46.790797
2878.224373	37255.251120	46.795802
2871.466117	34273.377087	46.800807
2863.192400	31405.174265	46.805812
2852.146647	28676.272418	46.810817
2841.214859	26080.292111	46.815821
2829.541345	23640.927138	46.820826
2816.880447	21390.484091	46.825831
2804.713823	19321.949839	46.830836
2792.238350	17437.921054	46.835841
2780.026660	15743.310683	46.840845
2768.401357	14249.328777	46.845850
2757.496902	12932.085964	46.850855
2747.854777	11785.332055	46.855860
2739.195569	10801.376143	46.860865
2730.929681	9950.545172	46.865869
2724.087923	9220.042797	46.870874
2718.024340	8606.522187	46.875879
2712.659320	8078.035075	46.880884
2707.706004	7634.997914	46.885889
2703.727450	7251.663092	46.890893
2700.425444	6907.882907	46.895898
2696.995560	6620.206658	46.900903
2693.679697	6357.295892	46.905908
2690.835711	6129.296692	46.910913
2688.367738	5900.952083	46.915917
2685.874548	5690.033551	46.920922
2683.156023	5481.787632	46.925927
2681.038410	5271.448357	46.930932
2678.725091	5077.740145	46.935937
2676.171487	4859.910692	46.940941
2673.733126	4657.470064	46.945946
2670.871899	4438.504129	46.950951
2668.625178	4216.328163	46.955956
2665.865358	3995.757523	46.960961
2663.085710	3764.361517	46.965965
2660.800940	3529.791114	46.970970
2657.542436	3285.765010	46.975975
2654.625999	3032.353514	46.980980
2651.916620	2783.686013	46.985985
2648.710492	2512.676893	46.990989
2646.022261	2260.721696	46.995994
2642.196693	2001.746588	47.000999
2639.638723	1725.952842	47.006004
2636.190222	1468.822975	47.011009
2632.783378	1203.630969	47.016013
2629.375913	932.349824	47.021018
2625.622207	673.570886	47.026023
2622.018817	421.380494	47.031028
2617.436325	189.333926	47.036033
2605.169184	185.009935	47.041037
2595.100031	178.126453	47.046042
2588.666418	189.016184	47.051047
2585.515208	176.548137	47.056052
2583.857542	183.104477	47.061057
2582.300648	184.385070	47.066061
2580.250728	171.696210	47.071066
2577.358653	175.501295	47.076071
2574.152236	179.716235	47.081076
2570.986520	180.114807	47.086081
2567.754231	176.216236	47.091085
2564.718506	169.082793	47.096090
2560.958849	175.111427	47.101095
2557.827881	162.488910	47.106100
2554.281356	172.369773	47.111105
2550.963817	170.150637	47.116109
2548.188810	162.522667	47.121114
2544.509991	180.236091	47.126119
2541.507505	170.777049	47.131124
2538.018204	168.621199	47.136129
2534.357618	177.071440	47.141133
2530.643840	168.694004	47.146138
2527.146810	168.589207	47.151143
2524.595123	173.057643	47.156148
2520.638639	175.090292	47.161153
2517.320727	174.330767	47.166157
2514.439080	167.113320	47.171162
2510.838494	171.931102	47.176167
2507.201423	177.786604	47.181172
2503.488193	169.307075	47.186177
2500.241930	171.971621	47.191181
2497.365809	159.206447	47.196186
2493.959454	165.351853	47.201191
2489.856543	172.523150	47.206196
2486.332980	162.013874	47.211201
2483.614792	168.620358	47.216205
2480.103588	157.299168	47.221210
2476.398172	167.511783	47.226215
2473.184440	161.757788	47.231220
2469.697032	158.405995	47.236225
2466.306809	167.668105	47.241229
2462.842683	147.534063	47.246234
2458.662791	159.084420	47.251239
2455.176200	163.565705	47.256244
2452.033926	147.338567	47.261249
2448.937487	158.584985	47.266253
2446.049451	150.570209	47.271258
2442.380878	162.810543	47.276263
2438.982183	151.729335	47.281268
2434.929491	152.955812	47.286273
2431.541196	170.850839	47.291277
2428.252579	156.176065	47.296282
2424.492873	161.780122	47.301287
2421.390872	150.240477	47.306292
2418.226018	152.891832	47.311297
2414.126179	157.824843	47.316301
2410.747282	152.979083	47.321306
2407.225296	148.967420	47.326311
2403.476787	146.097069	47.331316
2400.481204	149.099385	47.336321
2396.680327	161.828490	47.341325
2393.580900	152.185859	47.346330
2389.942919	159.124780	47.351335
2386.573307	147.993231	47.356340
2382.868644	152.565418	47.361345
2379.312060	151.342171	47.366349
2376.039917	138.996500	47.371354
2372.273495	145.676209	47.376359
2369.004216	141.397698	47.381364
2365.780588	139.825858	47.386369
2362.438547	154.592741	47.391373
2358.742098	146.388036	47.396378
2355.497131	144.558250	47.401383
2351.916342	152.957733	47.406388
2348.505703	149.671900	47.411393
2344.426377	152.130889	47.416397
2341.124190	136.784927	47.421402
2337.712882	152.372148	47.426407
2334.245228	141.674598	47.431412
2330.552354	146.943455	47.436417
2327.464557	149.659896	47.441421
2324.238989	148.064525	47.446426
2320.109048	154.946172	47.451431
2316.794983	144.414304	47.456436
2313.215894	140.110805	47.461441
2310.027607	144.458869	47.466445
2306.236333	148.485358	47.471450
2302.904942	152.523944	47.476455
2299.509817	137.766235	47.481460
2295.972943	149.447749	47.486465
2292.160313	150.060452	47.491469
2289.082258	147.754012	47.496474
2285.747052	150.510534	47.501479
2281.889410	136.677756	47.506484
2278.492613	147.321042	47.511489
2274.937157	146.704701	47.516493
2271.298918	146.357780	47.521498
2267.696591	150.634510	47.526503
2264.812062	149.632517	47.531508
2261.333749	142.940402	47.536513
2257.782580	151.572058	47.541517
2254.344596	143.667944	47.546522
2250.478077	152.360153	47.551527
2247.298220	138.235927	47.556532
2243.560802	141.045066	47.561537
2240.114360	139.318284	47.566541
2236.677016	143.434788	47.571546
2232.837160	147.341477	47.576551
2228.994937	148.848522	47.581556
2226.081558	144.345587	47.586561
2222.582486	140.886976	47.591565
2219.549535	147.310517	47.596570
2215.685346	146.973119	47.601575
2212.443162	138.947515	47.606580
2208.590692	142.992072	47.611585
2204.823957	140.452275	47.616589
2201.678736	137.055240	47.621594
2198.500543	145.570291	47.626599
2194.846076	143.001703	47.631604
2191.444239	138.004396	47.636609
2187.637135	145.650215	47.641613
2184.030550	135.256940	47.646618
2180.766336	135.534677	47.651623
2177.269800	140.601116	47.656628
2173.668379	146.339252	47.661633
2170.034468	140.124019	47.666637
2166.870146	134.544635	47.671642
2163.145713	143.609105	47.676647
2160.264476	139.950845	47.681652
2156.286331	144.529866	47.686657
2152.697310	139.289391	47.691661
2149.416713	134.949364	47.696666
2145.269836	139.883046	47.701671
2142.271009	137.900084	47.706676
2138.979575	136.556667	47.711681
2135.049665	138.542403	47.716685
2131.990035	133.472455	47.721690
2128.532028	136.355128	47.726695
2124.844341	130.472846	47.731700
2121.050002	137.492418	47.736705
2117.635650	138.392530	47.741709
2114.232116	135.201014	47.746714
2110.543128	140.368936	47.751719
2107.214199	136.961846	47.756724
2104.226621	129.252259	47.761729
2100.334423	141.001045	47.766733
2096.949770	141.606179	47.771738
2093.244313	141.821067	47.776743
2089.742296	137.847991	47.781748
2086.587154	130.132933	47.786753
2082.500474	134.070820	47.791757
2079.356422	130.468248	47.796762
2075.677005	139.458443	47.801767
2072.229959	134.354236	47.806772
2069.028137	135.518056	47.811777
2065.228842	146.139919	47.816781
2062.252153	134.413903	47.821786
2058.661142	137.816670	47.826791
2054.673521	134.601671	47.831796
2051.020558	133.744268	47.836801
2047.274473	134.838927	47.841805
2044.525678	140.115277	47.846810
2040.629288	143.408644	47.851815
2037.270139	133.747609	47.856820
2034.198055	134.504823	47.861825
2030.213590	134.032723	47.866829
2026.891923	127.549172	47.871834
2023.073611	134.244204	47.876839
2019.696612	134.642698	47.881844
2016.564728	138.033611	47.886849
2012.770772	140.095266	47.891853
2009.703473	137.814863	47.896858
2006.064607	135.241282	47.901863
2002.360627	135.836070	47.906868
1998.955551	133.510223	47.911873
1994.994925	134.257911	47.916877
1992.219845	136.395423	47.921882
1988.588271	141.146643	47.926887
1984.811877	134.129826	47.931892
1981.385330	142.999783	47.936897
1977.491202	127.035165	47.941901
1974.227097	136.033403	47.946906
1970.393057	133.137468	47.951911
1967.444264	130.950991	47.956916
1964.007526	130.434269	47.961921
1960.293114	131.771620	47.966925
1956.939333	129.067521	47.971930
1953.560560	136.200130	47.976935
1949.966025	135.121411	47.981940
1946.641913	128.741533	47.986945
1942.438303	130.787821	47.991949
1939.492274	125.922435	47.996954
1935.493205	133.155726	48.001959
1932.879698	134.351527	48.006964
1928.996171	121.697929	48.011969
1925.220337	133.490560	48.016973
1921.858633	125.521827	48.021978
1918.253587	128.684482	48.026983
1914.798905	130.162296	48.031988
1911.456759	128.344922	48.036993
1907.620517	128.883482	48.041997
1904.744974	126.016761	48.047002
1900.904111	131.473756	48.052007
1897.672837	118.455129	48.057012
1894.319599	124.843338	48.062017
1890.237879	116.346291	48.067021
1886.770748	117.228049	48.072026
1883.216430	124.205181	48.077031
1879.990169	118.462582	48.082036
1876.091822	124.220359	48.087041
1872.260574	124.995915	48.092045
1869.427217	116.651844	48.097050
1865.824830	124.851542	48.102055
1862.139090	115.463848	48.107060
1858.884311	123.569231	48.112065
1855.285560	127.902290	48.117069
1851.965371	122.332898	48.122074
1848.647195	125.479002	48.127079
1845.045998	125.136747	48.132084
1841.705492	116.625452	48.137089
1837.747940	130.121186	48.142093
1834.410894	123.580531	48.147098
1830.644468	129.588090	48.152103
1827.212052	120.547532	48.157108
1823.999102	126.342897	48.162113
1819.837389	130.248990	48.167117
1816.794570	133.218401	48.172122
1813.130430	135.872488	48.177127
1809.662213	127.733768	48.182132
1806.441467	129.265172	48.187137
1802.756381	130.000063	48.192141
1799.744676	124.805409	48.197146
1796.091626	133.286643	48.202151
1792.398226	123.031392	48.207156
1789.158882	130.874771	48.212161
1785.529240	125.019495	48.217165
1781.971965	126.953428	48.222170
1777.763509	126.265358	48.227175
1774.705378	128.625577	48.232180
1771.036286	126.910861	48.237185
1767.864667	126.050729	48.242189
1764.497215	116.651191	48.247194
1760.853317	123.620115	48.252199
1757.027979	123.512094	48.257204
1753.728551	125.653281	48.262209
1750.319170	125.405113	48.267213
1747.143790	124.699540	48.272218
1743.309078	131.708291	48.277223
1739.827668	122.663662	48.282228
1736.395735	119.654135	48.287233
1732.495048	115.378577	48.292237
1729.556378	121.843049	48.297242
1725.350267	122.840298	48.302247
1722.225126	120.268508	48.307252
1719.058672	111.820914	48.312257
1715.492672	123.776152	48.317261
1711.983694	121.377897	48.322266
1708.055931	125.107689	48.327271
1704.468654	122.469191	48.332276
1701.076269	110.426545	48.337281
1697.397308	119.196483	48.342285
1694.568610	114.964476	48.347290
1691.242636	115.231239	48.352295
1687.645584	125.789149	48.357300
1683.832822	116.755900	48.362305
1679.886717	124.421288	48.367309
1676.650993	109.059611	48.372314
1673.342671	119.281710	48.377319
1669.685435	114.244914	48.382324
1666.258565	113.107338	48.387329
1662.582801	112.333336	48.392333
1659.320392	114.046562	48.397338
1655.600162	118.535402	48.402343
1652.103791	111.122149	48.407348
1649.076712	116.287399	48.412353
1645.187665	128.854525	48.417357
1641.847409	113.796086	48.422362
1637.907344	113.810523	48.427367
1634.825719	120.317019	48.432372
1631.735702	111.888042	48.437377
1627.636889	118.970899	48.442381
1624.291341	115.121920	48.447386
1620.704723	113.647277	48.452391
1616.989504	115.410484	48.457396
1613.763326	111.790830	48.462401
1609.895506	120.382265	48.467405
1607.130638	115.807452	48.472410
1603.331221	121.399903	48.477415
1599.740539	117.402989	48.482420
1596.494973	114.408360	48.487425
1592.687728	111.163177	48.492429
1589.060461	111.700814	48.497434
1585.549744	115.396918	48.502439
1581.999585	120.446764	48.507444
1578.942997	107.541825	48.512449
1575.165326	109.083315	48.517453
1571.557878	100.753900	48.522458
1568.108236	112.269865	48.527463
1564.427462	108.239127	48.532468
1561.168477	104.376685	48.537473
1557.579181	119.531743	48.542477
1554.116341	107.411276	48.547482
1551.021372	105.108329	48.552487
1547.128634	106.224846	48.557492
1544.245946	103.469656	48.562497
1540.129166	118.714848	48.567501
1536.855278	112.273517	48.572506
1533.058925	118.838977	48.577511
1529.404335	105.705713	48.582516
1526.151650	109.005393	48.587521
1522.417478	110.640773	48.592525
1518.963755	104.822371	48.597530
1515.734442	108.964377	48.602535
1512.130308	110.503486	48.607540
1508.934315	106.760520	48.612545
1505.256415	114.541952	48.617549
1501.888192	110.859815	48.622554
1498.049564	110.656719	48.627559
1494.743410	109.877025	48.632564
1491.373902	107.835375	48.637569
1487.546661	112.506405	48.642573
1483.685625	110.310960	48.647578
1480.733832	102.242291	48.652583
1477.278148	104.833366	48.657588
1473.743736	110.185766	48.662593
1469.704638	112.768871	48.667597
1466.610576	104.478432	48.672602
1463.052728	105.146382	48.677607
1459.236208	110.873191	48.682612
1456.193836	100.723791	48.687617
1452.775260	101.359458	48.692621
1449.171792	93.124809	48.697626
1445.425470	109.542784	48.702631
1441.711223	110.417753	48.707636
1438.412720	108.468996	48.712641
1435.128406	109.270943	48.717645
1431.694419	106.645418	48.722650
1427.786764	116.506919	48.727655
1424.372610	110.937208	48.732660
1421.363963	110.167599	48.737665
1417.637049	110.374723	48.742669
1413.873370	111.329517	48.747674
1410.497516	111.494807	48.752679
1406.668434	114.754655	48.757684
1403.792803	105.878973	48.762689
1399.773757	118.860449	48.767693
1396.796312	111.210285	48.772698
1393.392705	111.483579	48.777703
1389.553875	116.540422	48.782708
1386.286624	107.816306	48.787713
1382.645856	119.799306	48.792717
1379.175503	104.402865	48.797722
1375.295895	114.953209	48.802727
1371.920515	111.955732	48.807732
1368.664594	107.801854	48.812737
1364.798930	113.749588	48.817741
1361.529184	104.578346	48.822746
1358.027975	107.979798	48.827751
1354.397437	111.688372	48.832756
1351.131887	106.348724	48.837761
1347.627940	113.239944	48.842765
1344.106130	106.010732	48.847770
1340.665570	111.152942	48.852775
1336.818340	110.846617	48.857780
1333.442389	105.064844	48.862785
1329.782351	114.307884	48.867789
1326.662410	108.727708	48.872794
1322.999707	100.813365	48.877799
1319.441913	117.455620	48.882804
1316.242002	102.871570	48.887809
1312.062413	116.633273	48.892813
1309.006003	109.731898	48.897818
1305.373603	108.352295	48.902823
1301.889733	104.443548	48.907828
1298.781740	99.522301	48.912833
1295.145582	103.508119	48.917837
1291.764413	101.272789	48.922842
1287.690738	98.478227	48.927847
1284.342238	106.577540	48.932852
1281.272902	100.026626	48.937857
1277.231034	116.018777	48.942861
1274.102892	107.681822	48.947866
1270.577649	101.252652	48.952871
1266.740515	107.323026	48.957876
1263.211089	99.246005	48.962881
1260.006094	102.743011	48.967885
1256.511425	103.264908	48.972890
1252.532500	111.774132	48.977895
1249.421597	107.174663	48.982900
1246.186406	103.948880	48.987905
1242.329361	109.126066	48.992909
1238.751033	102.518622	48.997914
1235.499832	106.550172	49.002919
1231.545169	107.964314	49.007924
1228.826946	102.779374	49.012929
1225.281498	107.167812	49.017933
1221.460427	100.427055	49.022938
1217.986959	100.451149	49.027943
1214.331565	117.253064	49.032948
1210.706452	99.788825	49.037953
1206.947424	112.590501	49.042957
1204.166170	102.548695	49.047962
1200.247152	105.050411	49.052967
1196.900543	112.201861	49.057972
1193.698551	104.108655	49.062977
1189.941558	109.785968	49.067981
1186.346135	102.772317	49.072986
1182.571269	107.218646	49.077991
1179.253895	113.598821	49.082996
1175.803540	111.129530	49.088001
1172.302860	109.107044	49.093005
1168.779948	108.792827	49.098010
1165.350183	105.345695	49.103015
1161.896467	108.538944	49.108020
1158.612170	97.625036	49.113025
1154.728819	102.034658	49.118029
1151.239267	95.600875	49.123034
1147.876558	99.197241	49.128039
1143.976227	109.109047	49.133044
1140.983047	96.715151	49.138049
1137.424374	104.657101	49.143053
1133.806315	102.843101	49.148058
1130.468186	102.255443	49.153063
1126.970627	103.611070	49.158068
1123.213085	102.286642	49.163073
1119.623975	111.067583	49.168077
1116.245875	99.342182	49.173082
1113.059272	99.234861	49.178087
1109.018592	105.852480	49.183092
1106.018885	103.921662	49.188097
1102.094250	102.778801	49.193101
1098.828430	98.342801	49.198106
1095.470305	101.078062	49.203111
1091.993765	104.102861	49.208116
1088.703167	109.682219	49.213121
1084.389761	100.558854	49.218125
1081.160269	102.331170	49.223130
1077.569442	106.722484	49.228135
1073.781297	105.618254	49.233140
1070.544485	99.970374	49.238145
1067.612574	98.522700	49.243149
1064.314592	98.779958	49.248154
1060.320751	103.611479	49.253159
1056.540933	91.895727	49.258164
1053.232539	91.448647	49.263169
1049.420447	105.560828	49.268173
1046.613855	100.375031	49.273178
1042.883809	102.237048	49.278183
1038.989804	95.129042	49.283188
1035.881777	100.679231	49.288193
1032.351073	107.036759	49.293197
1028.560781	99.968445	49.298202
1025.065551	107.269496	49.303207
1021.537785	103.719295	49.308212
1018.265260	103.019047	49.313217
1014.400915	113.011041	49.318221
1011.131264	103.176232	49.323226
1007.744827	107.468878	49.328231
1003.862330	108.198958	49.333236
1001.351050	96.870232	49.338241
997.472518	100.643369	49.343245
993.769757	95.265596	49.348250
990.224263	105.387018	49.353255
986.856642	111.176123	49.358260
983.264014	110.512455	49.363265
979.460330	97.863966	49.368269
975.956396	99.743899	49.373274
972.977099	103.561939	49.378279
969.130637	96.953684	49.383284
965.634841	104.162121	49.388289
961.792776	105.029212	49.393293
958.438301	100.072806	49.398298
954.990070	106.526864	49.403303
951.706265	106.799423	49.408308
948.510833	98.381502	49.413313
944.873046	102.762132	49.418317
941.318983	94.268945	49.423322
937.545071	103.892804	49.428327
933.635148	101.304149	49.433332
930.588998	95.082176	49.438337
927.110609	103.251154	49.443341
923.615158	92.090376	49.448346
920.273449	101.011296	49.453351
916.397152	99.282018	49.458356
913.460584	106.362684	49.463361
909.372695	97.079862	49.468365
905.953754	102.037450	49.473370
902.754685	105.047087	49.478375
899.040326	101.316106	49.483380
896.190242	96.295080	49.488385
892.175075	106.847082	49.493389
888.855545	101.531524	49.498394
885.075316	93.529862	49.503399
881.535955	94.136992	49.508404
877.996236	98.444225	49.513409
874.190233	95.010615	49.518413
871.385520	102.448380	49.523418
867.411558	96.215131	49.528423
863.549741	102.246093	49.533428
860.700718	91.995328	49.538433
857.074172	99.111602	49.543437
853.699992	104.086294	49.548442
850.365730	99.884006	49.553447
846.471357	101.073609	49.558452
843.225914	103.437777	49.563457
839.510565	98.300010	49.568461
836.036064	90.786752	49.573466
832.401814	101.680530	49.578471
828.834316	98.539429	49.583476
825.757548	91.069718	49.588481
821.491687	104.971567	49.593485
818.386488	97.763492	49.598490
815.013397	105.425937	49.603495
811.401754	103.107147	49.608500
808.351684	98.819603	49.613505
804.576752	93.769870	49.618509
801.175903	96.070575	49.623514
797.781423	91.870596	49.628519
794.100155	94.648868	49.633524
790.408186	84.874245	49.638529
786.686160	98.292676	49.643533
783.257530	89.137939	49.648538
780.056320	93.165868	49.653543
776.418720	96.130911	49.658548
773.169606	96.877980	49.663553
769.434686	97.656273	49.668557
765.751357	98.524308	49.673562
762.627840	104.047042	49.678567
759.079575	97.666124	49.683572
755.590718	93.149871	49.688577
751.882902	101.560966	49.693581
748.326501	89.551431	49.698586
745.141548	95.905250	49.703591
741.207867	103.251598	49.708596
738.072101	99.763676	49.713601
734.496029	90.071953	49.718605
731.130006	95.249029	49.723610
727.383763	97.703817	49.728615
723.764685	97.043751	49.733620
720.653234	94.724781	49.738625
716.775733	99.428416	49.743629
712.914545	92.857768	49.748634
709.958824	94.662805	49.753639
706.370070	93.995172	49.758644
703.339722	94.525342	49.763649
699.700528	96.551592	49.768653
695.883466	93.141481	49.773658
692.335480	87.916568	49.778663
688.917507	100.551078	49.783668
685.707706	95.198194	49.788673
682.099011	97.276640	49.793677
678.576809	91.416394	49.798682
674.573678	85.674198	49.803687
671.083671	90.115639	49.808692
668.181564	89.213277	49.813697
664.163836	92.801925	49.818701
660.780879	95.708948	49.823706
657.485129	92.132707	49.828711
653.799433	93.435561	49.833716
650.570857	91.216138	49.838721
646.696406	101.037014	49.843725
643.076741	91.302068	49.848730
640.037458	99.502987	49.853735
636.215138	101.715481	49.858740
633.132315	92.381512	49.863745
629.095003	103.943201	49.868749
625.970479	102.033960	49.873754
622.422883	100.305224	49.878759
618.514118	94.935426	49.883764
615.176562	92.756754	49.888769
611.902281	98.520017	49.893773
608.258702	93.097475	49.898778
604.943868	94.460173	49.903783
601.299852	98.738103	49.908788
597.973678	94.723135	49.913793
594.421921	100.807405	49.918797
590.993858	92.210016	49.923802
587.565278	96.038500	49.928807
583.531470	93.317136	49.933812
580.287955	90.711687	49.938817
576.649032	94.308974	49.943821
573.236027	100.450025	49.948826
569.522160	93.458888	49.953831
566.288290	99.876371	49.958836
562.830722	95.962501	49.963841
559.075854	92.459145	49.968845
555.812871	98.251362	49.973850
552.677005	87.166208	49.978855
548.661389	94.006487	49.983860
545.272696	80.972860	49.988865
541.525773	96.453978	49.993869
538.478469	99.472104	49.998874
534.557273	97.861895	50.003879
531.045251	102.109555	50.008884
528.050085	86.173542	50.013889
524.056018	92.792813	50.018893
520.595602	91.590238	50.023898
517.261666	95.919735	50.028903
513.743838	86.586017	50.033908
510.284572	94.206685	50.038913
506.965622	95.836343	50.043917
503.264646	94.701214	50.048922
499.567509	94.275661	50.053927
496.231944	92.236466	50.058932
492.868569	89.338735	50.063937
489.140335	88.151692	50.068941
485.871641	93.061827	50.073946
482.467076	92.171499	50.078951
478.709853	100.649583	50.083956
475.271745	92.332595	50.088961
471.316392	91.794098	50.093965
468.171049	101.240490	50.098970
464.854046	90.735157	50.103975
461.186554	100.135351	50.108980
457.634095	85.107799	50.113985
453.742549	96.770809	50.118989
450.650133	92.811998	50.123994
446.888355	101.393475	50.128999
443.905637	97.161755	50.134004
440.398179	97.126567	50.139009
436.733152	90.607588	50.144013
433.335779	97.905097	50.149018
429.713627	90.705132	50.154023
425.894091	98.459879	50.159028
422.627869	98.076348	50.164033
419.182085	100.365636	50.169037
415.576807	97.352697	50.174042
412.646942	101.287430	50.179047
408.550144	105.249132	50.184052
405.058578	92.953709	50.189057
401.728289	98.661266	50.194061
397.683174	100.279167	50.199066
394.577669	105.191370	50.204071
390.989837	102.622329	50.209076
387.770401	94.471691	50.214081
383.857471	97.218978	50.219085
380.731101	96.662951	50.224090
376.965085	92.847054	50.229095
373.272421	97.917226	50.234100
370.113631	89.466092	50.239105
366.720401	90.397941	50.244109
363.062912	87.165967	50.249114
360.141632	87.131311	50.254119
355.898539	94.400915	50.259124
352.677730	94.132664	50.264129
349.005365	94.686458	50.269133
345.527416	90.966375	50.274138
342.035204	88.157775	50.279143
338.273279	89.675184	50.284148
335.007337	78.748305	50.289153
331.782403	87.725268	50.294157
328.199988	87.899912	50.299162
324.868290	80.074771	50.304167
320.896719	93.349139	50.309172
317.751898	86.001601	50.314177
314.377302	93.233657	50.319181
310.667977	89.101781	50.324186
306.871040	94.305296	50.329191
303.267652	90.084062	50.334196
300.019680	90.386894	50.339201
296.500359	88.936137	50.344205
293.257289	95.926214	50.349210
289.509763	86.049573	50.354215
285.613340	90.540817	50.359220
282.248826	78.015120	50.364225
278.941971	83.984492	50.369229
275.514682	80.059344	50.374234
272.196651	82.359763	50.379239
268.325868	99.154312	50.384244
265.233190	84.978709	50.389249
261.553792	93.110582	50.394253
257.980516	86.145408	50.399258
254.746912	87.417568	50.404263
250.864748	87.660049	50.409268
247.474105	88.890524	50.414273
244.014049	88.701622	50.419277
240.087752	94.279242	50.424282
237.134560	83.394014	50.429287
233.646390	90.610788	50.434292
230.041441	86.297526	50.439297
226.205805	88.868368	50.444301
222.702198	93.742194	50.449306
219.544721	89.918256	50.454311
215.810501	86.164339	50.459316
212.697511	86.138234	50.464321
209.165279	89.703749	50.469325
205.448443	92.739989	50.474330
202.037196	86.894751	50.479335
198.254648	94.258952	50.484340
195.142480	96.352091	50.489345
191.654262	87.669705	50.494349
187.693616	89.551465	50.499354
184.155242	85.617944	50.504359
180.435510	90.829502	50.509364
177.395502	80.180303	50.514369
173.899250	88.540429	50.519373
170.611568	81.426232	50.524378
167.004573	79.356461	50.529383
163.163318	87.633406	50.534388
159.898846	79.083127	50.539393
156.584365	82.128967	50.544397
152.980670	93.255167	50.549402
149.309340	88.830422	50.554407
145.470840	92.899375	50.559412
142.090343	86.248711	50.564417
139.307522	80.539447	50.569421
135.227281	85.310681	50.574426
131.847720	79.789610	50.579431
128.581014	85.287722	50.584436
124.927217	86.267044	50.589441
121.547212	89.722571	50.594445
118.085704	95.607751	50.599450
114.270677	82.281619	50.604455
110.850186	84.744755	50.609460
107.323138	86.375226	50.614465
103.775069	84.803296	50.619469
99.993538	92.815057	50.624474
97.014827	80.016282	50.629479
93.144449	92.461257	50.634484
89.985834	68.916876	50.639489
86.280312	85.921771	50.644493
82.699925	87.321530	50.649498
79.368840	83.128229	50.654503
75.817557	86.673519	50.659508
72.496881	88.965845	50.664513
68.839958	90.119978	50.669517
65.158684	90.257931	50.674522
61.774430	71.274416	50.679527
58.360694	90.991718	50.684532
55.051782	77.256053	50.689537
51.067945	85.704698	50.694541
47.534694	91.587995	50.699546
44.200573	89.208326	50.704551
40.420437	96.797415	50.709556
37.561778	79.114536	50.714561
34.070178	85.900061	50.719565
30.402945	84.761339	50.724570
27.112260	86.734578	50.729575
23.172079	84.029830	50.734580
19.946414	85.146930	50.739585
16.014821	95.241403	50.744589
12.451271	93.188448	50.749594
9.497145	83.495652	50.754599
5.583370	88.685415	50.759604
2.585213	89.343943	50.764609