Number of Data Points = 29
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
KGT3462_Position 5_00000 LC.hys	221.459258	7999.284287	182.383567	3099488.193344	254.565604	254.354016	91.785809	2.580840	50.193368	198.951113	1.263185	-130.981498	-93.353500	0.567824
KGT3462_Position 5_00001 LC.hys	195.003119	7999.447740	167.474044	2357293.763233	230.933496	230.827093	96.644130	3.393488	53.519287	172.104870	1.229391	-130.974495	-93.353500	0.120710
KGT3462_Position 5_00002 LC.hys	211.047275	7999.489888	171.391412	2796279.014456	246.150540	246.052631	90.809991	2.860762	49.789631	187.743373	1.249293	-130.967499	-93.353500	-0.048358
KGT3462_Position 5_00003 LC.hys	219.975658	7999.465302	181.910235	3055417.761110	253.176275	252.956755	92.205465	2.618125	47.834080	197.015562	1.272119	-130.960495	-93.353500	-0.112877
KGT3462_Position 5_00004 LC.hys	218.820551	7999.516920	176.193295	3021303.498882	252.979690	252.872003	89.810483	2.647704	52.088279	196.247349	1.247186	-130.953499	-93.353500	-0.131420
KGT3462_Position 5_00005 LC.hys	218.684328	7999.450051	174.028794	3017291.848618	253.185373	253.159011	88.766128	2.651202	54.699011	196.416751	1.234433	-130.946495	-93.353500	-0.109512
KGT3462_Position 5_00006 LC.hys	219.627880	7999.475742	179.024604	3045128.403401	253.313945	253.140630	90.895994	2.626975	56.570812	197.970129	1.234691	-130.981498	-93.346496	-0.043276
KGT3462_Position 5_00007 LC.hys	208.601049	7999.369894	173.475204	2727115.020697	243.263878	243.185401	93.072313	2.933272	50.458835	185.561452	1.249639	-130.974495	-93.346000	-0.049564
KGT3462_Position 5_00008 LC.hys	211.456162	7999.419480	173.559284	2807917.250185	246.223312	246.023973	91.767843	2.848880	67.080439	191.030837	1.193158	-130.967499	-93.346496	0.001607
KGT3462_Position 5_00009 LC.hys	216.058847	7999.472365	173.125634	2940447.256433	250.856496	250.713474	89.451887	2.720495	62.134296	194.904143	1.207833	-130.960495	-93.346496	-0.002353
KGT3462_Position 5_00010 LC.hys	222.935946	7999.549366	170.838922	3143636.895279	258.048163	258.054770	85.370035	2.544680	71.991389	203.020682	1.175312	-130.953499	-93.346496	-0.009914
KGT3462_Position 5_00011 LC.hys	203.328271	7999.372234	171.590517	2580749.684696	238.524360	238.292494	94.635737	3.099631	39.051928	177.810770	1.297363	-130.946495	-93.346496	0.036653
KGT3462_Position 5_00012 LC.hys	207.765781	7999.518206	170.753784	2703681.200771	243.233168	242.901979	92.008388	2.958751	46.788719	183.843811	1.260627	-130.981498	-93.339500	0.034201
KGT3462_Position 5_00013 LC.hys	203.857557	7999.512083	166.727916	2595273.588173	240.133074	239.842137	91.696250	3.082339	45.552821	179.389086	1.259978	-130.974495	-93.339500	0.065192
KGT3462_Position 5_00014 LC.hys	212.834845	7999.591589	166.635312	2847322.059710	249.271512	248.839781	87.495067	2.809514	57.019034	190.478897	1.215685	-130.967499	-93.339500	0.038897
KGT3462_Position 5_00015 LC.hys	235.230240	7999.172143	180.056713	3522074.292082	268.881870	268.549626	85.005082	2.271154	45.853248	211.776436	1.277931	-130.960495	-93.339500	0.084301
KGT3462_Position 5_00017 LC.hys	222.036189	7999.673840	170.433590	3116703.111591	257.580070	257.239081	85.534693	2.566710	57.415464	199.987838	1.219742	-130.946495	-93.339500	0.099850
KGT3462_Position 5_00018 LC.hys	209.728918	7999.714707	163.229449	2758905.331584	246.695594	246.485680	87.069278	2.899597	71.245470	189.303485	1.166769	-130.981498	-93.332496	0.068402
KGT3462_Position 5_00019 LC.hys	223.217283	7999.223464	179.369955	3152080.069970	256.956592	256.664454	89.512958	2.537760	52.134598	200.854514	1.251450	-130.974495	-93.332000	0.057428
KGT3462_Position 5_00020 LC.hys	238.008937	7999.364023	170.927355	3610267.897832	273.274552	273.108778	79.703370	2.215726	44.164607	213.568362	1.272237	-130.967499	-93.332496	0.068818
KGT3462_Position 5_00021 LC.hys	237.607221	7999.400837	170.180157	3597457.671964	272.887323	272.861335	79.496114	2.223626	68.310711	217.165950	1.184870	-130.960495	-93.332496	0.084770
KGT3462_Position 5_00022 LC.hys	215.226262	7999.305704	174.607128	2916267.112420	249.741583	249.586138	90.590602	2.742995	48.566170	191.915723	1.258817	-130.953499	-93.332496	0.058051
KGT3462_Position 5_00023 LC.hys	217.307604	7999.501631	168.931407	2976884.366572	253.118517	252.822765	86.748954	2.687206	66.239027	196.507181	1.189258	-130.946495	-93.332496	0.108993
KGT3462_Position 5_00024 LC.hys	217.638081	7999.527095	176.826929	2986561.421183	251.925971	251.567558	90.656199	2.678507	43.964207	193.585568	1.281673	-130.981498	-93.324997	0.030154
KGT3462_Position 5_00025 LC.hys	246.252302	7999.254464	163.819092	3877592.534533	283.142496	282.874657	73.708616	2.062944	49.262133	222.309747	1.240327	-130.974495	-93.325500	0.090127
KGT3462_Position 5_00026 LC.hys	221.809310	7999.549652	174.716258	3109928.156279	256.381236	256.148771	87.779473	2.572262	57.573522	200.050937	1.225219	-130.967499	-93.325500	0.034715
KGT3462_Position 5_00027 LC.hys	200.652961	7999.524944	172.701500	2507915.846313	235.769954	235.392924	96.621652	3.189710	50.754863	177.614475	1.247377	-130.960495	-93.325500	0.060033
KGT3462_Position 5_00028 LC.hys	229.561365	7999.048395	174.401178	3345178.179541	264.065622	263.960710	84.484029	2.391217	58.079685	207.864942	1.223041	-130.953499	-93.325500	0.048630
KGT3462_Position 5_00029 LC.hys	218.156949	7999.589006	170.271397	3001783.767844	253.595933	253.393001	87.073665	2.664945	58.019780	196.196075	1.217438	-130.946495	-93.325500	0.060573