Thu Mar 11 19:40:07 2021

Number of Points = 3622
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.659346	-0.064287	0.000000	-0.000011	0.729717

0.408642	-0.048257	0.005005	0.000035	0.729662
0.408638	-0.051735	0.010010	0.000034	0.729656
0.602939	-0.082641	0.015014	-0.000002	0.729664
0.461163	-0.059925	0.020019	0.000024	0.729660
0.108469	0.004546	0.025024	0.000089	0.729665
0.366927	-0.043483	0.030029	0.000040	0.729662
0.466580	-0.065057	0.035034	0.000021	0.729655
0.740442	-0.107351	0.040038	-0.000030	0.729669
0.693633	-0.105311	0.045043	-0.000022	0.729658
0.879698	-0.135435	0.050048	-0.000057	0.729664
0.802353	-0.122899	0.055053	-0.000044	0.729663
0.919811	-0.146317	0.060058	-0.000066	0.729659
0.833498	-0.128570	0.065062	-0.000050	0.729665
0.710523	-0.111529	0.070067	-0.000028	0.729656
0.653220	-0.141243	0.075072	-0.000018	0.729580
0.555647	-0.249405	0.080077	-0.000000	0.729337
0.443283	-0.231479	0.085082	0.000020	0.729334
0.280925	-0.200320	0.090086	0.000050	0.729339
0.573744	-0.256231	0.095091	-0.000005	0.729333
0.677251	-0.273150	0.100096	-0.000025	0.729336
0.608348	-0.263160	0.105101	-0.000013	0.729333
0.529691	-0.345543	0.110106	0.000002	0.729147
0.722456	-0.441088	0.115110	-0.000035	0.729029
0.644369	-0.432553	0.120115	-0.000021	0.729019
0.690122	-0.438111	0.125120	-0.000030	0.729025
0.722862	-0.444002	0.130125	-0.000036	0.729026
0.857611	-0.592052	0.135130	-0.000062	0.728786
0.753911	-0.610532	0.140134	-0.000043	0.728715
0.580270	-0.585470	0.145139	-0.000011	0.728704
0.661224	-0.595810	0.150144	-0.000027	0.728713
0.352088	-0.643789	0.155149	0.000030	0.728514
0.250340	-0.682774	0.160154	0.000048	0.728404
0.259690	-0.679771	0.165158	0.000046	0.728414
0.316914	-0.695635	0.170163	0.000035	0.728404
0.549378	-0.852632	0.175168	-0.000009	0.728180
0.721978	-0.936172	0.180173	-0.000041	0.728078
0.417544	-0.884618	0.185178	0.000015	0.728074
-0.030031	-0.842699	0.190182	0.000098	0.728001
-0.007910	-0.972411	0.195187	0.000093	0.727757
0.546976	-1.066351	0.200192	-0.000011	0.727768
0.567863	-1.076545	0.205197	-0.000015	0.727756
0.314779	-1.190916	0.210202	0.000032	0.727446
0.251744	-1.178120	0.215206	0.000043	0.727450
0.477481	-1.231901	0.220211	0.000000	0.727425
0.402708	-1.360043	0.225216	0.000014	0.727150
0.076751	-1.302730	0.230221	0.000074	0.727150
0.109699	-1.350173	0.235226	0.000067	0.727070
0.120520	-1.476594	0.240230	0.000065	0.726828
-0.009142	-1.458662	0.245235	0.000088	0.726819
-0.024192	-1.531829	0.250240	0.000091	0.726672
-0.060762	-1.602671	0.255245	0.000097	0.726522
-0.299362	-1.565185	0.260250	0.000141	0.726513
-0.071516	-1.732421	0.265254	0.000098	0.726267
-0.350575	-1.716038	0.270259	0.000149	0.726203
-0.245819	-1.770733	0.275264	0.000129	0.726134
-0.682693	-1.797396	0.280269	0.000210	0.725931
-1.574861	-1.641764	0.285274	0.000376	0.725925
-1.411426	-1.743772	0.290278	0.000345	0.725784
-2.284032	-1.682946	0.295283	0.000507	0.725600
-2.598488	-1.625557	0.300288	0.000565	0.725604
-2.375236	-1.686057	0.305293	0.000523	0.725564
-3.115826	-1.694700	0.310298	0.000660	0.725291
-3.269288	-1.662856	0.315302	0.000688	0.725301
-3.721605	-1.585156	0.320307	0.000772	0.725296
-3.423360	-1.707705	0.325312	0.000716	0.725161
-4.245264	-1.653060	0.330317	0.000868	0.724983
-4.690444	-1.577705	0.335322	0.000951	0.724977
-4.249646	-1.651615	0.340326	0.000868	0.724986
-4.087302	-1.709437	0.345331	0.000837	0.724931
-4.994062	-1.678470	0.350336	0.001006	0.724677
-5.158163	-1.650759	0.355341	0.001036	0.724675
-5.434761	-1.605733	0.360346	0.001086	0.724667
-5.053759	-1.668323	0.365350	0.001015	0.724679
-5.287410	-1.710638	0.370355	0.001058	0.724515
-6.281291	-1.632421	0.375360	0.001243	0.724323
-6.020066	-1.676682	0.380365	0.001193	0.724329
-6.503550	-1.600721	0.385370	0.001283	0.724310
-6.180190	-1.645518	0.390374	0.001222	0.724336
-6.105967	-1.708956	0.395379	0.001208	0.724238
-7.672570	-1.556708	0.400384	0.001499	0.723991
-7.075048	-1.659410	0.405389	0.001387	0.724000
-7.180605	-1.646025	0.410394	0.001406	0.723990
-7.430063	-1.599647	0.415398	0.001452	0.723995
-7.743948	-1.552759	0.420403	0.001510	0.723978
-7.588871	-1.577566	0.425408	0.001481	0.723985
-7.694837	-1.701769	0.430413	0.001500	0.723705
-8.841234	-1.529400	0.435418	0.001713	0.723644
-8.570703	-1.572455	0.440422	0.001662	0.723655
-7.941877	-1.683683	0.445427	0.001544	0.723658
-8.496431	-1.589638	0.450432	0.001647	0.723650
-8.490030	-1.590128	0.455437	0.001645	0.723652
-8.466206	-1.606786	0.460442	0.001640	0.723628
-8.832132	-1.678339	0.465446	0.001708	0.723362
-9.279704	-1.607120	0.470451	0.001791	0.723346
-9.346438	-1.593674	0.475456	0.001803	0.723350
-9.201766	-1.620138	0.480461	0.001775	0.723350
-9.586644	-1.555064	0.485466	0.001846	0.723344
-9.119865	-1.632387	0.490470	0.001759	0.723356
-9.131123	-1.674683	0.495475	0.001761	0.723270
-10.295764	-1.599259	0.500480	0.001977	0.723013
-10.001258	-1.650809	0.505485	0.001921	0.723015
-10.196464	-1.621851	0.510490	0.001957	0.723005
-10.029356	-1.647495	0.515494	0.001926	0.723014
-10.460898	-1.575344	0.520499	0.002005	0.723006
-10.338873	-1.592960	0.525504	0.001982	0.723015
-9.960877	-1.698214	0.530509	0.001911	0.722941
-11.244089	-1.597712	0.535514	0.002150	0.722691
-11.104037	-1.618620	0.540518	0.002123	0.722700
-11.280955	-1.591086	0.545523	0.002155	0.722693
-11.354215	-1.576917	0.550528	0.002169	0.722697
-11.176148	-1.608810	0.555533	0.002135	0.722697
-11.418068	-1.568907	0.560538	0.002179	0.722692
-11.054693	-1.630652	0.565542	0.002111	0.722699
-11.383354	-1.689487	0.570547	0.002172	0.722469
-12.288321	-1.577526	0.575552	0.002340	0.722374
-11.859041	-1.653355	0.580557	0.002259	0.722376
-12.302346	-1.578387	0.585562	0.002341	0.722369
-12.302057	-1.574730	0.590566	0.002341	0.722378
-11.907823	-1.648056	0.595571	0.002267	0.722372
-12.129208	-1.608626	0.600576	0.002308	0.722373
-12.460910	-1.594876	0.605581	0.002369	0.722286
-13.100385	-1.589193	0.610586	0.002487	0.722074
-12.603643	-1.674652	0.615590	0.002394	0.722081
-13.194848	-1.573306	0.620595	0.002504	0.722074
-13.071397	-1.594005	0.625600	0.002480	0.722078
-12.752870	-1.648327	0.630605	0.002421	0.722083
-13.307936	-1.554051	0.635610	0.002523	0.722075
-13.205015	-1.571056	0.640614	0.002504	0.722079
-13.660005	-1.657779	0.645619	0.002588	0.721751
-14.020202	-1.594226	0.650624	0.002654	0.721750
-14.226133	-1.556752	0.655629	0.002692	0.721753
-14.233637	-1.560013	0.660634	0.002693	0.721745
-14.162154	-1.568243	0.665638	0.002679	0.721755
-14.278811	-1.550717	0.670643	0.002700	0.721749
-14.283971	-1.549748	0.675648	0.002701	0.721750
-14.024698	-1.614495	0.680653	0.002652	0.721715
-15.026806	-1.577380	0.685658	0.002838	0.721438
-14.725892	-1.626506	0.690662	0.002782	0.721448
-15.063173	-1.570209	0.695667	0.002844	0.721442
-14.955461	-1.588982	0.700672	0.002823	0.721443
-15.060385	-1.569177	0.705677	0.002842	0.721447
-14.933051	-1.596089	0.710682	0.002818	0.721439
-14.618176	-1.647741	0.715686	0.002759	0.721449
-15.277363	-1.666831	0.720691	0.002881	0.721182
-16.249905	-1.522174	0.725696	0.003062	0.721126
-15.690377	-1.621246	0.730701	0.002957	0.721129
-15.911109	-1.585263	0.735706	0.002997	0.721123
-16.126348	-1.544941	0.740710	0.003037	0.721128
-15.816992	-1.603591	0.745715	0.002979	0.721122
-15.689447	-1.625142	0.750720	0.002955	0.721125
-15.866730	-1.645946	0.755725	0.002987	0.721023
-16.938483	-1.529239	0.760730	0.003186	0.720878
-16.362697	-1.627875	0.765734	0.003078	0.720887
-16.883541	-1.540154	0.770739	0.003175	0.720878
-17.021387	-1.514764	0.775744	0.003200	0.720881
-16.454928	-1.612255	0.780749	0.003094	0.720888
-16.905303	-1.538352	0.785754	0.003177	0.720877
-16.879757	-1.575382	0.790758	0.003172	0.720814
-17.584446	-1.591193	0.795763	0.003303	0.720537
-17.714829	-1.566578	0.800768	0.003326	0.720541
-17.897345	-1.532043	0.805773	0.003360	0.720546
-17.777555	-1.558481	0.810778	0.003337	0.720537
-17.196643	-1.657678	0.815782	0.003228	0.720546
-17.717088	-1.569706	0.820787	0.003325	0.720538
-17.994422	-1.520389	0.825792	0.003376	0.720539
-17.875081	-1.665565	0.830797	0.003353	0.720296
-18.759265	-1.546544	0.835802	0.003517	0.720221
-18.865977	-1.524044	0.840806	0.003537	0.720229
-18.684401	-1.560928	0.845811	0.003502	0.720221
-18.869278	-1.526450	0.850816	0.003536	0.720225
-18.494855	-1.590741	0.855821	0.003466	0.720231
-18.849200	-1.533693	0.860826	0.003531	0.720220
-18.715299	-1.606672	0.865830	0.003506	0.720124
-19.524301	-1.576228	0.870835	0.003656	0.719901
-19.599736	-1.563855	0.875840	0.003669	0.719900
-19.539851	-1.571935	0.880845	0.003658	0.719906
-19.426288	-1.596865	0.885850	0.003636	0.719898
-19.273521	-1.620338	0.890854	0.003607	0.719906
-19.669611	-1.552643	0.895859	0.003680	0.719902
-19.471016	-1.610978	0.900864	0.003643	0.719857
-20.100604	-1.624081	0.905869	0.003760	0.719612
-20.426874	-1.571827	0.910874	0.003820	0.719601
-20.204796	-1.607330	0.915878	0.003778	0.719610
-20.198020	-1.612013	0.920883	0.003776	0.719604
-20.741372	-1.517613	0.925888	0.003877	0.719601
-20.414337	-1.573035	0.930893	0.003815	0.719607
-20.272434	-1.616910	0.935898	0.003788	0.719571
-21.033317	-1.630087	0.940902	0.003930	0.719279
-21.376153	-1.571554	0.945907	0.003993	0.719275
-21.372133	-1.572974	0.950912	0.003992	0.719275
-21.034450	-1.632433	0.955917	0.003928	0.719277
-21.844321	-1.493097	0.960922	0.004078	0.719269
-21.381141	-1.570632	0.965926	0.003992	0.719279
-21.162032	-1.612496	0.970931	0.003950	0.719275
-21.952109	-1.588518	0.975936	0.004097	0.719046
-22.480664	-1.533108	0.980941	0.004195	0.718970
-22.396282	-1.552559	0.985946	0.004179	0.718962
-22.264960	-1.571073	0.990950	0.004154	0.718973
-22.531573	-1.527221	0.995955	0.004203	0.718967
-22.293941	-1.569891	1.000960	0.004158	0.718967
-22.099051	-1.602812	1.005965	0.004121	0.718972
-22.676221	-1.504995	1.010970	0.004228	0.718963
-22.481685	-1.693812	1.015974	0.004191	0.718660
-22.928453	-1.621074	1.020979	0.004274	0.718647
-23.898135	-1.449865	1.025984	0.004454	0.718645
-23.125398	-1.584518	1.030989	0.004310	0.718652
-23.070841	-1.599091	1.035994	0.004299	0.718643
-23.244482	-1.562819	1.040998	0.004331	0.718655
-23.554161	-1.510819	1.046003	0.004388	0.718650
-23.719034	-1.574875	1.051008	0.004418	0.718466
-23.941950	-1.588451	1.056013	0.004459	0.718362
-24.161625	-1.554061	1.061018	0.004499	0.718354
-24.063833	-1.567913	1.066022	0.004481	0.718362
-24.026655	-1.577966	1.071027	0.004473	0.718356
-24.250826	-1.540799	1.076032	0.004514	0.718352
-24.146558	-1.554184	1.081037	0.004494	0.718363
-24.384645	-1.583110	1.086042	0.004538	0.718223
-25.418030	-1.500002	1.091046	0.004730	0.718025
-25.137481	-1.553361	1.096051	0.004677	0.718019
-25.209049	-1.542779	1.101056	0.004690	0.718016
-24.938385	-1.587227	1.106061	0.004639	0.718024
-25.419184	-1.507470	1.111066	0.004728	0.718013
-25.270026	-1.529091	1.116070	0.004700	0.718024
-24.998679	-1.580496	1.121075	0.004649	0.718019
-25.541416	-1.590947	1.126080	0.004749	0.717808
-26.441317	-1.482783	1.131085	0.004916	0.717706
-26.067855	-1.553205	1.136090	0.004846	0.717700
-25.911234	-1.579436	1.141094	0.004817	0.717704
-26.392478	-1.495804	1.146099	0.004906	0.717701
-26.244282	-1.522390	1.151104	0.004878	0.717702
-25.585128	-1.637341	1.156109	0.004754	0.717707
-26.186062	-1.544632	1.161114	0.004866	0.717680
-26.760156	-1.592033	1.166118	0.004972	0.717385
-26.701810	-1.605735	1.171123	0.004961	0.717380
-27.170525	-1.523819	1.176128	0.005047	0.717378
-26.962144	-1.558995	1.181133	0.005008	0.717382
-27.319379	-1.501673	1.186138	0.005074	0.717371
-27.077670	-1.540614	1.191142	0.005029	0.717380
-27.131836	-1.532656	1.196147	0.005038	0.717378
-26.923883	-1.649569	1.201152	0.004999	0.717221
-27.699549	-1.577608	1.206157	0.005143	0.717091
-27.901851	-1.547090	1.211162	0.005180	0.717081
-27.735182	-1.574325	1.216166	0.005148	0.717087
-27.618648	-1.596812	1.221171	0.005126	0.717084
-27.764518	-1.569402	1.226176	0.005153	0.717088
-27.686999	-1.582690	1.231181	0.005138	0.717090
-28.364961	-1.604280	1.236186	0.005263	0.716810
-28.575803	-1.592548	1.241190	0.005302	0.716759
-28.804927	-1.553148	1.246195	0.005344	0.716758
-28.907648	-1.535987	1.251200	0.005363	0.716756
-28.672385	-1.575640	1.256205	0.005319	0.716762
-28.945753	-1.533012	1.261210	0.005369	0.716751
-28.605785	-1.586583	1.266214	0.005305	0.716766
-28.678228	-1.658133	1.271219	0.005318	0.716600
-29.840268	-1.528988	1.276224	0.005534	0.716446
-29.407841	-1.602700	1.281229	0.005453	0.716454
-29.685967	-1.559142	1.286234	0.005504	0.716443
-29.571904	-1.575551	1.291238	0.005482	0.716452
-29.546744	-1.582707	1.296243	0.005477	0.716448
-29.661847	-1.562750	1.301248	0.005498	0.716447
-29.547049	-1.661702	1.306253	0.005476	0.716293
-30.809229	-1.519368	1.311258	0.005711	0.716131
-30.683804	-1.539734	1.316262	0.005687	0.716135
-30.361280	-1.597418	1.321267	0.005626	0.716136
-30.682519	-1.542552	1.326272	0.005685	0.716132
-30.661957	-1.543135	1.331277	0.005681	0.716139
-30.675137	-1.545194	1.336282	0.005683	0.716132
-30.382806	-1.614322	1.341286	0.005628	0.716099
-31.131844	-1.589326	1.346291	0.005767	0.715885
-31.553786	-1.515771	1.351296	0.005845	0.715883
-31.235052	-1.570457	1.356301	0.005785	0.715888
-31.203649	-1.579668	1.361306	0.005779	0.715882
-31.219117	-1.574505	1.366310	0.005781	0.715888
-31.685937	-1.493506	1.371315	0.005867	0.715884
-31.551065	-1.536155	1.376320	0.005842	0.715849
-31.824683	-1.637222	1.381325	0.005892	0.715553
-32.477657	-1.526563	1.386330	0.006013	0.715542
-32.326019	-1.549319	1.391334	0.005985	0.715552
-32.382001	-1.541073	1.396339	0.005994	0.715549
-32.463905	-1.530019	1.401344	0.006009	0.715543
-32.251196	-1.564797	1.406349	0.005969	0.715551
-32.179717	-1.582485	1.411354	0.005955	0.715542
-33.107495	-1.568169	1.416358	0.006127	0.715243
-33.379348	-1.525163	1.421363	0.006178	0.715234
-33.390751	-1.524937	1.426368	0.006179	0.715231
-33.175216	-1.558843	1.431373	0.006138	0.715241
-33.466351	-1.512048	1.436378	0.006192	0.715232
-33.263796	-1.546200	1.441382	0.006154	0.715237
-33.037119	-1.589685	1.446387	0.006111	0.715232
-33.574254	-1.578378	1.451392	0.006211	0.715065
-34.433742	-1.500733	1.456397	0.006370	0.714916
-34.044648	-1.575237	1.461402	0.006297	0.714907
-34.400320	-1.509313	1.466406	0.006363	0.714913
-34.498333	-1.494796	1.471411	0.006381	0.714908
-34.140429	-1.559535	1.476416	0.006313	0.714907
-34.124900	-1.560488	1.481421	0.006310	0.714912
-34.392871	-1.517738	1.486426	0.006359	0.714903
-34.837493	-1.573546	1.491430	0.006442	0.714636
-35.130645	-1.533265	1.496435	0.006496	0.714613
-35.537754	-1.463012	1.501440	0.006571	0.714610
-34.950839	-1.565014	1.506445	0.006461	0.714616
-35.319397	-1.505638	1.511450	0.006529	0.714604
-35.354213	-1.495657	1.516454	0.006535	0.714613
-34.956080	-1.567604	1.521459	0.006461	0.714612
-35.170451	-1.599295	1.526464	0.006500	0.714474
-36.294935	-1.496568	1.531469	0.006709	0.714281
-36.289598	-1.502583	1.536474	0.006707	0.714272
-36.229012	-1.509522	1.541478	0.006695	0.714281
-35.940417	-1.563762	1.546483	0.006641	0.714276
-36.186026	-1.521572	1.551488	0.006686	0.714274
-36.248209	-1.507110	1.556493	0.006697	0.714282
-36.058939	-1.546209	1.561498	0.006662	0.714272
-36.652124	-1.577110	1.566502	0.006772	0.714002
-37.289705	-1.481774	1.571507	0.006890	0.713967
-37.183785	-1.502409	1.576512	0.006870	0.713964
-36.439201	-1.631488	1.581517	0.006730	0.713972
-37.045999	-1.526831	1.586522	0.006843	0.713966
-37.233408	-1.492416	1.591526	0.006877	0.713969
-36.849679	-1.562938	1.596531	0.006805	0.713966
-37.312699	-1.569972	1.601536	0.006891	0.713789
-38.071447	-1.502075	1.606541	0.007032	0.713656
-37.766572	-1.561218	1.611546	0.006974	0.713648
-37.839975	-1.546644	1.616550	0.006987	0.713652
-38.029520	-1.512516	1.621555	0.007022	0.713654
-37.872383	-1.543963	1.626560	0.006992	0.713648
-37.517685	-1.602601	1.631565	0.006926	0.713658
-38.157010	-1.563739	1.636570	0.007044	0.713510
-38.856949	-1.514373	1.641574	0.007174	0.713361
-38.102619	-1.648494	1.646579	0.007033	0.713362
-38.859171	-1.516402	1.651584	0.007174	0.713358
-38.899272	-1.505604	1.656589	0.007180	0.713366
-38.488435	-1.584489	1.661594	0.007103	0.713356
-38.609970	-1.558790	1.666598	0.007126	0.713365
-39.011170	-1.602724	1.671603	0.007200	0.713136
-39.980420	-1.487368	1.676608	0.007380	0.713023
-39.412586	-1.585872	1.681613	0.007273	0.713030
-39.712083	-1.537800	1.686618	0.007329	0.713020
-40.007201	-1.483135	1.691622	0.007383	0.713025
-39.627493	-1.552865	1.696627	0.007312	0.713022
-39.856335	-1.512793	1.701632	0.007354	0.713022
-39.662483	-1.578154	1.706637	0.007317	0.712961
-40.390704	-1.577236	1.711642	0.007452	0.712706
-40.462869	-1.561709	1.716646	0.007465	0.712712
-40.901041	-1.485240	1.721651	0.007546	0.712710
-40.779574	-1.508879	1.726656	0.007523	0.712707
-40.431139	-1.567705	1.731661	0.007458	0.712715
-40.797038	-1.506858	1.736666	0.007525	0.712707
-40.750503	-1.513265	1.741670	0.007516	0.712712
-40.534041	-1.684775	1.746675	0.007475	0.712448
-41.740175	-1.504146	1.751680	0.007699	0.712381
-41.867022	-1.477584	1.756685	0.007722	0.712390
-41.267362	-1.589485	1.761690	0.007610	0.712381
-41.371202	-1.567962	1.766694	0.007629	0.712388
-41.540408	-1.539377	1.771699	0.007660	0.712385
-41.567562	-1.537552	1.776704	0.007665	0.712380
-41.562403	-1.640719	1.781709	0.007663	0.712178
-42.324026	-1.552085	1.786714	0.007804	0.712085
-42.530105	-1.512737	1.791718	0.007842	0.712091
-42.350443	-1.544435	1.796723	0.007808	0.712093
-42.550568	-1.513550	1.801728	0.007845	0.712084
-42.383751	-1.538337	1.806733	0.007813	0.712095
-42.260921	-1.565039	1.811738	0.007790	0.712087
-42.657696	-1.603040	1.816742	0.007863	0.711871
-43.504790	-1.507216	1.821747	0.008021	0.711762
-43.370221	-1.535538	1.826752	0.007995	0.711754
-42.985880	-1.598502	1.831757	0.007923	0.711766
-43.422197	-1.525097	1.836762	0.008004	0.711759
-43.392087	-1.528150	1.841766	0.007997	0.711764
-43.128492	-1.575861	1.846771	0.007948	0.711764
-43.308808	-1.614067	1.851776	0.007981	0.711625
-44.512980	-1.481748	1.856781	0.008205	0.711462
-44.147896	-1.553453	1.861786	0.008136	0.711449
-43.685261	-1.632486	1.866790	0.008049	0.711457
-43.933615	-1.589246	1.871795	0.008095	0.711456
-44.643003	-1.465652	1.876800	0.008227	0.711452
-44.329909	-1.518233	1.881805	0.008168	0.711459
-44.052738	-1.608391	1.886810	0.008116	0.711379
-45.233309	-1.517909	1.891814	0.008335	0.711140
-45.011141	-1.557731	1.896819	0.008293	0.711141
-44.990381	-1.565340	1.901824	0.008289	0.711134
-45.087638	-1.543196	1.906829	0.008306	0.711145
-45.084639	-1.549282	1.911834	0.008305	0.711135
-45.096925	-1.543571	1.916838	0.008307	0.711143
-44.982135	-1.577830	1.921843	0.008285	0.711116
-45.625296	-1.590219	1.926848	0.008404	0.710864
-45.584873	-1.592495	1.931853	0.008396	0.710875
-45.987510	-1.525551	1.936858	0.008471	0.710866
-46.243997	-1.477927	1.941862	0.008518	0.710871
-45.810513	-1.554274	1.946867	0.008437	0.710874
-45.891589	-1.544359	1.951872	0.008451	0.710866
-45.907117	-1.563952	1.956877	0.008454	0.710822
-46.780788	-1.554587	1.961882	0.008616	0.710531
-46.665981	-1.572935	1.966886	0.008594	0.710536
-46.914739	-1.527509	1.971891	0.008640	0.710539
-47.017506	-1.515016	1.976896	0.008658	0.710529
-46.732152	-1.560982	1.981901	0.008605	0.710539
-46.727716	-1.566968	1.986906	0.008603	0.710530
-46.828840	-1.549649	1.991910	0.008622	0.710530
-47.382068	-1.605292	1.996915	0.008724	0.710223
-47.836237	-1.525995	2.001920	0.008808	0.710220

-47.800595	-1.533437	2.011917	0.008800	0.710220
-47.872681	-1.521250	2.021914	0.008813	0.710221
-47.778365	-1.537153	2.031910	0.008794	0.710225
-47.950684	-1.507651	2.041907	0.008825	0.710224
-47.627658	-1.566894	2.051904	0.008764	0.710223
-47.990542	-1.504683	2.061901	0.008830	0.710220
-47.850803	-1.528760	2.071898	0.008803	0.710224
-47.725540	-1.552173	2.081894	0.008779	0.710224
-47.849064	-1.530389	2.091891	0.008801	0.710225
-47.704242	-1.557287	2.101888	0.008773	0.710225
-48.042626	-1.500538	2.111885	0.008835	0.710220
-47.921876	-1.522442	2.121882	0.008811	0.710221
-47.136766	-1.519774	2.131878	0.008664	0.710508
-47.068654	-1.519230	2.141875	0.008650	0.710535
-46.647790	-1.595360	2.151872	0.008571	0.710535
-47.191612	-1.499967	2.161869	0.008671	0.710534
-46.799068	-1.571441	2.171866	0.008597	0.710533
-46.237210	-1.550446	2.181862	0.008491	0.710777
-45.986642	-1.547182	2.191859	0.008444	0.710875
-46.077073	-1.533996	2.201856	0.008459	0.710871
-45.835719	-1.578527	2.211853	0.008413	0.710870
-46.144542	-1.483714	2.221850	0.008470	0.710951
-45.199467	-1.557522	2.231846	0.008293	0.711142
-45.311319	-1.538406	2.241843	0.008313	0.711142
-45.132830	-1.571537	2.251840	0.008278	0.711142
-45.035156	-1.494702	2.261837	0.008259	0.711332
-44.428355	-1.542103	2.271834	0.008145	0.711455
-44.492778	-1.529833	2.281830	0.008156	0.711459
-44.170260	-1.588315	2.291827	0.008095	0.711459
-43.603743	-1.538738	2.301824	0.007988	0.711761
-43.542504	-1.551288	2.311821	0.007976	0.711760
-43.405775	-1.575566	2.321818	0.007949	0.711762
-43.362541	-1.528109	2.331814	0.007940	0.711874
-42.546703	-1.563923	2.341811	0.007787	0.712094
-42.586800	-1.557790	2.351808	0.007794	0.712094
-42.852220	-1.511389	2.361805	0.007842	0.712094
-41.756477	-1.588449	2.371802	0.007637	0.712332
-41.986002	-1.517963	2.381798	0.007679	0.712393
-41.894590	-1.536832	2.391795	0.007660	0.712390
-41.694794	-1.512942	2.401792	0.007622	0.712510
-40.747872	-1.582954	2.411789	0.007445	0.712709
-40.993532	-1.540076	2.421786	0.007490	0.712709
-41.091801	-1.521223	2.431782	0.007507	0.712714
-40.233478	-1.540863	2.441779	0.007346	0.712981
-40.223709	-1.521154	2.451776	0.007343	0.713026
-40.265376	-1.514781	2.461773	0.007350	0.713026
-39.733349	-1.525322	2.471770	0.007250	0.713195
-39.335344	-1.513062	2.481766	0.007174	0.713363
-39.116046	-1.554245	2.491763	0.007133	0.713361
-39.310673	-1.514215	2.501760	0.007168	0.713373
-38.679027	-1.489205	2.511757	0.007049	0.713649
-38.340582	-1.549140	2.521754	0.006985	0.713652
-38.385995	-1.541196	2.531750	0.006992	0.713653
-37.786571	-1.544357	2.541747	0.006880	0.713861
-37.505661	-1.539502	2.551744	0.006826	0.713973
-37.562307	-1.530972	2.561741	0.006836	0.713971
-37.338256	-1.554323	2.571738	0.006793	0.714006
-36.782313	-1.514471	2.581734	0.006688	0.714284
-36.218886	-1.616452	2.591731	0.006583	0.714283
-36.715914	-1.529267	2.601728	0.006674	0.714282
-36.183045	-1.540028	2.611725	0.006574	0.714452
-35.539955	-1.574575	2.621722	0.006453	0.714613
-35.641235	-1.557346	2.631718	0.006471	0.714613
-35.744081	-1.538815	2.641715	0.006489	0.714615
-35.206360	-1.492753	2.651712	0.006388	0.714899
-34.933404	-1.536878	2.661709	0.006336	0.714910
-34.751191	-1.570036	2.671706	0.006301	0.714911
-34.623823	-1.506544	2.681702	0.006276	0.715084
-33.877273	-1.563461	2.691699	0.006136	0.715237
-34.177043	-1.511581	2.701696	0.006191	0.715236
-34.093621	-1.491995	2.711693	0.006174	0.715306
-33.037020	-1.560134	2.721690	0.005976	0.715546
-32.915128	-1.583017	2.731686	0.005953	0.715546
-33.139660	-1.541862	2.741683	0.005993	0.715550
-32.719276	-1.504582	2.751680	0.005914	0.715774
-32.136053	-1.554719	2.761677	0.005804	0.715883
-32.411250	-1.505839	2.771674	0.005855	0.715885
-32.047163	-1.546154	2.781670	0.005786	0.715935
-31.381294	-1.563821	2.791667	0.005661	0.716137
-31.620918	-1.523488	2.801664	0.005704	0.716135
-31.576168	-1.533141	2.811661	0.005695	0.716133
-30.900454	-1.514015	2.821658	0.005568	0.716412
-30.609861	-1.547373	2.831654	0.005513	0.716450
-30.666652	-1.537439	2.841651	0.005522	0.716452
-30.452245	-1.486962	2.851648	0.005481	0.716629
-29.669694	-1.563409	2.861645	0.005335	0.716756
-30.045169	-1.496827	2.871642	0.005403	0.716757
-29.486174	-1.571152	2.881638	0.005298	0.716809
-28.986429	-1.519153	2.891635	0.005204	0.717090
-28.789588	-1.556965	2.901632	0.005166	0.717087
-28.926487	-1.536988	2.911629	0.005191	0.717080
-28.261575	-1.549088	2.921626	0.005066	0.717292
-27.943649	-1.563100	2.931622	0.005006	0.717379
-27.966067	-1.558774	2.941619	0.005009	0.717381
-27.877793	-1.556617	2.951616	0.004991	0.717419
-27.236298	-1.528550	2.961613	0.004871	0.717702
-27.489895	-1.484115	2.971610	0.004917	0.717703
-26.871360	-1.595653	2.981606	0.004801	0.717702
-26.689472	-1.505755	2.991603	0.004766	0.717946
-26.159743	-1.562472	3.001600	0.004666	0.718022
-26.227343	-1.552985	3.011597	0.004678	0.718019
-26.190978	-1.519370	3.021594	0.004670	0.718100
-25.330039	-1.544330	3.031590	0.004509	0.718356
-25.197213	-1.569157	3.041587	0.004483	0.718355
-25.331296	-1.546801	3.051584	0.004507	0.718354
-24.730535	-1.549362	3.061581	0.004394	0.718563
-24.503112	-1.548832	3.071578	0.004350	0.718646
-24.350953	-1.576864	3.081574	0.004321	0.718646
-24.721078	-1.477783	3.091571	0.004389	0.718713
-23.612077	-1.550128	3.101568	0.004181	0.718962
-23.762628	-1.526188	3.111565	0.004208	0.718958
-23.732674	-1.531424	3.121562	0.004202	0.718961
-23.119509	-1.502138	3.131558	0.004086	0.719236
-22.682173	-1.563402	3.141555	0.004004	0.719271
-22.923633	-1.521489	3.151552	0.004048	0.719270
-22.509935	-1.506483	3.161549	0.003970	0.719447
-21.856812	-1.546464	3.171546	0.003847	0.719600
-21.719139	-1.570884	3.181542	0.003820	0.719602
-21.708797	-1.572587	3.191539	0.003817	0.719604
-21.231456	-1.536069	3.201536	0.003727	0.719846
-21.212961	-1.513243	3.211533	0.003723	0.719899
-20.954569	-1.560231	3.221530	0.003674	0.719899
-20.796474	-1.530805	3.231526	0.003643	0.720015
-19.998760	-1.566981	3.241523	0.003494	0.720225
-19.820725	-1.601483	3.251520	0.003459	0.720222
-20.148049	-1.542735	3.261517	0.003519	0.720225
-19.602178	-1.534226	3.271514	0.003417	0.720435
-19.352216	-1.526790	3.281510	0.003369	0.720539
-19.083809	-1.574527	3.291507	0.003318	0.720541
-19.087147	-1.531426	3.301504	0.003318	0.720627
-18.152520	-1.570948	3.311501	0.003142	0.720878
-18.062792	-1.586587	3.321498	0.003125	0.720881
-18.205526	-1.562061	3.331494	0.003150	0.720881
-18.193880	-1.508536	3.341491	0.003147	0.720993
-17.390580	-1.585285	3.351488	0.002996	0.721125
-17.640929	-1.543305	3.361485	0.003042	0.721122
-17.717837	-1.496643	3.371482	0.003055	0.721189
-16.745908	-1.542817	3.381478	0.002873	0.721440
-16.653009	-1.559615	3.391475	0.002855	0.721442
-16.753741	-1.542887	3.401472	0.002873	0.721441
-16.108739	-1.511347	3.411469	0.002751	0.721731
-15.649088	-1.586490	3.421466	0.002665	0.721746
-15.585590	-1.596977	3.431462	0.002652	0.721750
-15.596029	-1.524967	3.441459	0.002653	0.721890
-14.864488	-1.559953	3.451456	0.002515	0.722079
-15.105754	-1.519516	3.461453	0.002559	0.722076
-15.137567	-1.498587	3.471450	0.002564	0.722108
-14.486000	-1.481285	3.481446	0.002442	0.722371
-14.143460	-1.543885	3.491443	0.002377	0.722370
-14.334565	-1.510111	3.501440	0.002411	0.722372
-13.461831	-1.511028	3.511437	0.002248	0.722677
-13.128910	-1.561160	3.521434	0.002185	0.722697
-13.196271	-1.549619	3.531430	0.002196	0.722698
-13.242540	-1.471769	3.541427	0.002204	0.722837
-12.338356	-1.544685	3.551424	0.002035	0.723011
-12.473671	-1.523635	3.561421	0.002059	0.723007
-12.527334	-1.503735	3.571418	0.002068	0.723030
-11.621538	-1.504761	3.581414	0.001898	0.723346
-11.057805	-1.603390	3.591411	0.001792	0.723351
-11.520923	-1.524377	3.601408	0.001877	0.723346
-11.256069	-1.523266	3.611405	0.001827	0.723443
-10.335897	-1.584026	3.621402	0.001654	0.723647
-10.386623	-1.573972	3.631398	0.001663	0.723651
-10.411547	-1.570943	3.641395	0.001666	0.723650
-9.861391	-1.571019	3.651392	0.001563	0.723844
-9.280348	-1.602262	3.661389	0.001454	0.723987
-9.414419	-1.581518	3.671386	0.001477	0.723983
-9.408833	-1.582565	3.681382	0.001475	0.723985
-8.870118	-1.572770	3.691379	0.001374	0.724194
-8.646719	-1.551240	3.701376	0.001331	0.724316
-8.545051	-1.571628	3.711373	0.001311	0.724313
-8.648986	-1.552259	3.721370	0.001330	0.724317
-7.582559	-1.567105	3.731366	0.001130	0.724662
-7.252607	-1.622702	3.741363	0.001068	0.724670
-7.257522	-1.622039	3.751360	0.001067	0.724671
-7.512654	-1.580425	3.761357	0.001114	0.724666
-6.660945	-1.581208	3.771354	0.000954	0.724963
-6.584186	-1.588211	3.781350	0.000939	0.724978
-6.312240	-1.634278	3.791347	0.000887	0.724984
-6.761218	-1.532422	3.801344	0.000970	0.725029
-5.384194	-1.642470	3.811341	0.000712	0.725295
-5.631814	-1.599280	3.821338	0.000757	0.725296
-5.299784	-1.659518	3.831334	0.000694	0.725295
-5.448214	-1.606958	3.841331	0.000721	0.725349
-4.593725	-1.627998	3.851328	0.000561	0.725607
-4.691640	-1.612298	3.861325	0.000578	0.725605
-4.676847	-1.617541	3.871322	0.000574	0.725602
-4.428005	-1.586688	3.881318	0.000527	0.725751
-3.581755	-1.645317	3.891315	0.000368	0.725933
-3.799744	-1.606882	3.901312	0.000408	0.725934
-3.450156	-1.672445	3.911309	0.000342	0.725929
-3.305225	-1.607286	3.921306	0.000313	0.726109
-2.866171	-1.637897	3.931302	0.000231	0.726204
-2.615113	-1.682277	3.941299	0.000183	0.726206
-2.726527	-1.663414	3.951296	0.000203	0.726206
-2.492072	-1.548760	3.961293	0.000158	0.726514
-2.128666	-1.613257	3.971290	0.000089	0.726516
-2.235569	-1.594677	3.981286	0.000108	0.726517
-1.835102	-1.537709	3.991283	0.000032	0.726769
-1.656779	-1.541774	4.001280	-0.000002	0.726825
-1.593369	-1.554712	4.011277	-0.000015	0.726824
-1.476607	-1.441816	4.021274	-0.000038	0.727087
-1.260439	-1.448235	4.031270	-0.000079	0.727151
-1.468008	-1.374817	4.041267	-0.000041	0.727224
-1.539837	-1.245321	4.051264	-0.000029	0.727454
-1.134847	-1.308592	4.061261	-0.000106	0.727473
-0.794340	-1.217624	4.071258	-0.000170	0.727770
-0.754457	-1.224650	4.081254	-0.000179	0.727772
-0.485300	-1.129186	4.091251	-0.000230	0.728053
-0.791625	-1.060303	4.101248	-0.000174	0.728083
-0.794384	-0.904855	4.111245	-0.000175	0.728387
-1.001375	-0.816460	4.121242	-0.000137	0.728489
-0.864758	-0.723939	4.131238	-0.000164	0.728718
-0.491989	-0.677265	4.141235	-0.000234	0.728940
-0.394914	-0.624459	4.151232	-0.000253	0.729078
-0.005179	-0.562934	4.161229	-0.000327	0.729335
-0.425739	-0.387441	4.171226	-0.000250	0.729532
-0.547230	-0.256980	4.181222	-0.000228	0.729746
-0.099950	-0.223924	4.191219	-0.000313	0.729967
-0.154607	-0.057305	4.201216	-0.000304	0.730273
0.120807	0.008798	4.211213	-0.000356	0.730499
0.000000	0.185202	4.221210	-0.000335	0.730801

0.092511	0.807250	4.226214	-0.000353	0.732040
0.460027	2.030646	4.231219	-0.000423	0.734532
0.500561	3.888479	4.236224	-0.000432	0.738124
0.864160	6.257163	4.241229	-0.000502	0.742783
1.468534	9.106747	4.246234	-0.000617	0.748406
1.916647	12.471501	4.251238	-0.000703	0.754903
2.363409	16.278496	4.256243	-0.000789	0.762166
2.906158	20.486685	4.261248	-0.000893	0.770131
3.416274	25.107765	4.266253	-0.000992	0.778756
3.757165	30.119627	4.271258	-0.001059	0.787935
4.263230	35.448787	4.276262	-0.001157	0.797625
4.945590	41.067345	4.281267	-0.001289	0.807760
5.251306	47.053476	4.286272	-0.001350	0.818291
5.954394	53.266284	4.291277	-0.001486	0.829196
6.430153	59.765510	4.296282	-0.001579	0.840375
7.018652	66.464169	4.301286	-0.001693	0.851771
7.595791	73.393107	4.306291	-0.001806	0.863392
8.173438	80.526782	4.311296	-0.001919	0.875189
8.902711	87.817509	4.316301	-0.002060	0.887123
10.365789	95.161826	4.321306	-0.002337	0.899185
11.760389	102.696662	4.326310	-0.002603	0.911365
12.641599	110.464726	4.331315	-0.002772	0.923603
13.453167	118.367665	4.336320	-0.002929	0.935866
14.501650	126.342681	4.341325	-0.003130	0.948140
15.539749	134.428731	4.346330	-0.003329	0.960417
16.359793	142.639264	4.351334	-0.003488	0.972665
16.939691	150.981359	4.356339	-0.003602	0.984889
17.592500	159.399058	4.361344	-0.003729	0.997089
18.208129	167.833862	4.366349	-0.003850	1.009155
19.051360	176.278057	4.371354	-0.004013	1.021146
19.751089	184.790540	4.376358	-0.004149	1.033057
20.509181	193.317142	4.381363	-0.004296	1.044865
21.463152	201.848174	4.386368	-0.004480	1.056592
22.300200	210.432620	4.391373	-0.004642	1.068234
23.127534	219.036065	4.396378	-0.004802	1.079772
24.179330	227.605337	4.401382	-0.005004	1.091194
24.703203	236.285144	4.406387	-0.005108	1.102522
24.955156	245.004773	4.411392	-0.005161	1.113725
25.887146	253.594889	4.416397	-0.005341	1.124801
26.575357	262.239604	4.421402	-0.005475	1.135785
27.859856	270.778104	4.426406	-0.005720	1.146657
28.640825	279.452776	4.431411	-0.005872	1.157489
29.261319	288.074281	4.436416	-0.005994	1.168121
29.999109	296.697659	4.441421	-0.006137	1.178684
30.742676	305.293777	4.446426	-0.006282	1.189121
31.442517	313.895985	4.451430	-0.006418	1.199465
31.911681	322.526413	4.456435	-0.006512	1.209708
32.689860	331.076597	4.461440	-0.006663	1.219832
33.292103	339.667384	4.466445	-0.006781	1.229885
33.911279	348.224570	4.471450	-0.006902	1.239821
34.442812	356.764913	4.476454	-0.007007	1.249642
35.402275	365.246575	4.481459	-0.007192	1.259401
35.879088	373.783649	4.486464	-0.007287	1.269056
36.644993	382.273887	4.491469	-0.007436	1.278639
37.452273	390.727354	4.496474	-0.007592	1.288118
37.872412	399.256233	4.501478	-0.007676	1.297539
38.589028	407.709000	4.506483	-0.007816	1.306863
39.317630	416.272238	4.511488	-0.007958	1.316242
39.846829	424.693599	4.516493	-0.008062	1.325367
40.271600	433.143287	4.521498	-0.008147	1.334441
40.678037	441.567584	4.526502	-0.008229	1.343423
41.217373	449.983841	4.531507	-0.008335	1.352360
41.730782	458.363523	4.536512	-0.008437	1.361196
42.004407	466.789408	4.541517	-0.008494	1.369981
42.836386	475.122943	4.546522	-0.008655	1.378710
43.366741	483.487033	4.551526	-0.008760	1.387364
43.885141	491.889299	4.556531	-0.008862	1.396001
44.260266	500.232573	4.561536	-0.008938	1.404502
44.613414	508.612141	4.566541	-0.009010	1.412983
45.008912	516.948545	4.571546	-0.009089	1.421378
45.256146	525.302313	4.576550	-0.009141	1.429717
46.101325	533.567697	4.581555	-0.009305	1.438017
46.529126	541.862975	4.586560	-0.009390	1.446231
47.104232	550.180899	4.591565	-0.009503	1.454444
47.481702	558.490329	4.596570	-0.009579	1.462571
48.283327	566.752003	4.601574	-0.009735	1.470674
49.143203	575.028507	4.606579	-0.009901	1.478755
49.777443	583.272376	4.611584	-0.010025	1.486727
50.115032	591.604618	4.616589	-0.010093	1.494693
50.442406	599.898507	4.621594	-0.010160	1.502579
50.648770	608.207239	4.626598	-0.010205	1.510419
51.399942	616.439273	4.631603	-0.010351	1.518230
51.894478	624.666782	4.636608	-0.010448	1.525957
52.438803	632.930116	4.641613	-0.010556	1.533686
52.991997	641.166795	4.646618	-0.010665	1.541353
53.304908	649.448136	4.651622	-0.010729	1.548987
53.806502	657.706081	4.656627	-0.010828	1.556590
53.987825	665.961471	4.661632	-0.010868	1.564106
54.419762	674.203219	4.666637	-0.010954	1.571611
54.851835	682.432502	4.671642	-0.011040	1.579069
55.160039	690.664354	4.676646	-0.011104	1.586476
55.592781	698.908386	4.681651	-0.011190	1.593877
55.865032	707.127913	4.686656	-0.011247	1.601199
56.153943	715.365026	4.691661	-0.011307	1.608505
56.629087	723.565765	4.696666	-0.011401	1.615773
57.155978	731.744547	4.701670	-0.011505	1.622996
57.732376	739.966700	4.706675	-0.011618	1.630232
58.338265	748.163225	4.711680	-0.011737	1.637417
58.829947	756.328540	4.716685	-0.011834	1.644528
59.135331	764.550355	4.721690	-0.011897	1.651631
59.172076	772.793062	4.726694	-0.011910	1.658685
59.977108	780.906449	4.731699	-0.012065	1.665703
60.612863	789.070944	4.736704	-0.012190	1.672712
60.992392	797.265446	4.741709	-0.012266	1.679682
61.338951	805.458175	4.746714	-0.012337	1.686618
61.903452	813.632470	4.751718	-0.012447	1.693538
62.393638	821.807937	4.756723	-0.012545	1.700421
62.552800	830.020891	4.761728	-0.012580	1.707264
62.921485	838.235714	4.766733	-0.012655	1.714109
63.103666	846.414049	4.771738	-0.012694	1.720872
63.456006	854.567949	4.776742	-0.012766	1.727610
64.228694	862.702484	4.781747	-0.012916	1.734360
64.707571	870.836066	4.786752	-0.013011	1.741046
65.239481	878.991784	4.791757	-0.013115	1.747730
65.499970	887.197918	4.796762	-0.013170	1.754395
66.006645	895.327393	4.801766	-0.013270	1.761004
66.251234	903.523348	4.806771	-0.013321	1.767609
66.718489	911.672710	4.811776	-0.013414	1.774180
67.764276	919.733940	4.816781	-0.013615	1.780727
68.298265	927.892562	4.821786	-0.013720	1.787265
68.487587	936.160401	4.826790	-0.013761	1.793822
69.095500	944.276300	4.831795	-0.013880	1.800287
69.469155	952.403221	4.836800	-0.013956	1.806709
69.781581	960.589311	4.841805	-0.014020	1.813147
70.115521	968.730649	4.846810	-0.014088	1.819530
70.536945	976.856824	4.851814	-0.014172	1.825889
71.555831	984.931524	4.856819	-0.014367	1.832257
71.918661	993.080568	4.861824	-0.014441	1.838582
72.523250	1001.184497	4.866829	-0.014559	1.844880
72.861400	1009.374918	4.871834	-0.014628	1.851190
73.079975	1017.544518	4.876838	-0.014675	1.857450
73.444457	1025.691221	4.881843	-0.014748	1.863688
73.910152	1033.816495	4.886848	-0.014841	1.869900
74.010864	1042.017047	4.891853	-0.014866	1.876106
74.376832	1050.124723	4.896858	-0.014939	1.882253
74.530075	1058.266409	4.901862	-0.014974	1.888380
75.089565	1066.390334	4.906867	-0.015084	1.894521
75.309136	1074.507581	4.911872	-0.015131	1.900598
75.706421	1082.634619	4.916877	-0.015210	1.906683
76.179866	1090.763176	4.921882	-0.015304	1.912758
76.260414	1098.910712	4.926886	-0.015325	1.918784
76.748783	1106.993303	4.931891	-0.015422	1.924788
77.180138	1115.094628	4.936896	-0.015508	1.930782
77.753468	1123.201432	4.941901	-0.015621	1.936776
78.104288	1131.318236	4.946906	-0.015692	1.942734
78.650342	1139.427962	4.951910	-0.015799	1.948690
79.047265	1147.615554	4.956915	-0.015879	1.954668
79.272362	1155.699622	4.961920	-0.015927	1.960535
79.554638	1163.813020	4.966925	-0.015985	1.966411
80.096379	1171.907189	4.971930	-0.016092	1.972283
80.355914	1180.020909	4.976934	-0.016146	1.978122
80.722458	1188.126701	4.981939	-0.016220	1.983949
81.281732	1196.205804	4.986944	-0.016330	1.989761
81.769463	1204.332199	4.991949	-0.016427	1.995581
82.254404	1212.415356	4.996954	-0.016523	2.001353
82.554517	1220.528397	5.001958	-0.016584	2.007111
82.693669	1228.700597	5.006963	-0.016616	2.012876
83.025631	1236.785891	5.011968	-0.016684	2.018585
83.425808	1244.874690	5.016973	-0.016764	2.024286
83.867462	1252.984337	5.021978	-0.016852	2.029991
84.165214	1261.111398	5.026982	-0.016913	2.035676
84.462272	1269.215584	5.031987	-0.016974	2.041330
84.853242	1277.277654	5.036992	-0.017053	2.046948
85.393843	1285.375385	5.041997	-0.017160	2.052591
85.985652	1293.444285	5.047002	-0.017275	2.058203
86.290159	1301.536707	5.052006	-0.017338	2.063787
86.723803	1309.663287	5.057011	-0.017425	2.069392
86.857294	1317.800611	5.062016	-0.017455	2.074960
87.283696	1325.877994	5.067021	-0.017540	2.080500
87.700843	1333.957429	5.072026	-0.017624	2.086027
87.895617	1342.078232	5.077030	-0.017666	2.091545
88.115893	1350.207464	5.082035	-0.017713	2.097056
88.378639	1358.283429	5.087040	-0.017768	2.102521
88.769729	1366.367184	5.092045	-0.017846	2.107990
88.955376	1374.558381	5.097050	-0.017887	2.113496
89.376336	1382.600102	5.102054	-0.017971	2.118911
89.746805	1390.666021	5.107059	-0.018046	2.124324
89.893517	1398.757259	5.112064	-0.018079	2.129718
90.251297	1406.848246	5.117069	-0.018151	2.135118
90.602459	1414.910393	5.122074	-0.018222	2.140484
91.074952	1422.970226	5.127078	-0.018316	2.145848
91.401706	1431.097094	5.132083	-0.018383	2.151228
91.519496	1439.207055	5.137088	-0.018410	2.156563
91.816280	1447.262270	5.142093	-0.018471	2.161867
92.061236	1455.364744	5.147098	-0.018523	2.167183
92.472742	1463.435320	5.152102	-0.018605	2.172481
93.112170	1471.499305	5.157107	-0.018730	2.177783
93.331197	1479.577290	5.162112	-0.018777	2.183042
93.791560	1487.671177	5.167117	-0.018868	2.188321
94.248742	1495.790500	5.172122	-0.018959	2.193603
94.408493	1503.869093	5.177126	-0.018995	2.198819
94.741140	1511.936523	5.182131	-0.019062	2.204032
94.732610	1520.036262	5.187136	-0.019067	2.209221
95.179307	1528.119849	5.192141	-0.019156	2.214429
95.624937	1536.167823	5.197146	-0.019244	2.219602
95.955924	1544.208012	5.202150	-0.019312	2.224748
96.647008	1552.281360	5.207155	-0.019446	2.229935
96.627270	1560.417466	5.212160	-0.019448	2.235086
96.758374	1568.499574	5.217165	-0.019479	2.240205
97.143300	1576.540568	5.222170	-0.019556	2.245308
97.499039	1584.612162	5.227174	-0.019628	2.250417
97.888688	1592.703623	5.232179	-0.019706	2.255529
98.140273	1600.790736	5.237184	-0.019759	2.260614
98.605931	1608.838785	5.242189	-0.019852	2.265683
98.765430	1616.981965	5.247194	-0.019887	2.270773
98.872235	1625.112891	5.252198	-0.019913	2.275839
99.217463	1633.144721	5.257203	-0.019983	2.280853
99.640515	1641.172638	5.262208	-0.020067	2.285860
99.896293	1649.255674	5.267213	-0.020121	2.290876
100.308667	1657.314036	5.272218	-0.020203	2.295879
100.781939	1665.334909	5.277222	-0.020297	2.300853
101.190001	1673.401265	5.282227	-0.020379	2.305838
101.571345	1681.481636	5.287232	-0.020456	2.310819
102.059367	1689.554643	5.292237	-0.020552	2.315794
102.353551	1697.619302	5.297242	-0.020613	2.320736
102.436145	1705.695045	5.302246	-0.020634	2.325657
102.907296	1713.760522	5.307251	-0.020728	2.330594
103.193163	1721.843619	5.312256	-0.020787	2.335516
103.516221	1729.911270	5.317261	-0.020853	2.340420
103.900198	1737.972537	5.322266	-0.020930	2.345316
104.312599	1746.041881	5.327270	-0.021013	2.350209
104.457806	1754.196450	5.332275	-0.021045	2.355120
104.524086	1762.240167	5.337280	-0.021064	2.359949
105.002838	1770.267263	5.342285	-0.021158	2.364791
105.221806	1778.347165	5.347290	-0.021205	2.369634
105.420385	1786.436270	5.352294	-0.021248	2.374470
105.881672	1794.471804	5.357299	-0.021339	2.379286
105.887036	1802.546874	5.362304	-0.021346	2.384079
106.318254	1810.603109	5.367309	-0.021432	2.388886
106.505986	1818.707352	5.372314	-0.021473	2.393691
106.804737	1826.750956	5.377318	-0.021534	2.398460
107.291879	1834.779835	5.382323	-0.021631	2.403225
107.547668	1842.833694	5.387328	-0.021684	2.407978
107.895182	1850.901317	5.392333	-0.021755	2.412736
108.212174	1858.976608	5.397338	-0.021820	2.417487
108.209502	1867.057117	5.402342	-0.021825	2.422207
108.638392	1875.123382	5.407347	-0.021911	2.426942
108.790646	1883.229342	5.412352	-0.021945	2.431671
108.909978	1891.351496	5.417357	-0.021973	2.436396
109.318838	1899.343272	5.422362	-0.022055	2.441059
109.524306	1907.361952	5.427366	-0.022099	2.445714
109.984184	1915.418398	5.432371	-0.022190	2.450400
109.997886	1923.513821	5.437376	-0.022198	2.455066
110.407126	1931.557945	5.442381	-0.022280	2.459724
110.735437	1939.584075	5.447386	-0.022347	2.464356
110.883589	1947.657222	5.452390	-0.022381	2.468993
110.994861	1955.761661	5.457395	-0.022407	2.473636
111.390837	1963.778122	5.462400	-0.022487	2.478242
111.820308	1971.805680	5.467405	-0.022572	2.482848
112.287607	1979.852862	5.472410	-0.022665	2.487459
112.503171	1987.920918	5.477414	-0.022711	2.492055
112.900282	1995.998457	5.482419	-0.022791	2.496660
113.017558	2004.068193	5.487424	-0.022819	2.501233
113.094136	2012.133672	5.492429	-0.022839	2.505792
113.730810	2020.172284	5.497434	-0.022963	2.510368
113.796547	2028.281318	5.502438	-0.022981	2.514933
113.840857	2036.351675	5.507443	-0.022995	2.519468
114.236384	2044.346707	5.512448	-0.023074	2.523977
114.528223	2052.404195	5.517453	-0.023134	2.528505
114.797166	2060.479806	5.522458	-0.023190	2.533034
115.078245	2068.504871	5.527462	-0.023248	2.537527
115.681131	2076.533959	5.532467	-0.023366	2.542038
116.085927	2084.579256	5.537472	-0.023448	2.546535
116.295758	2092.672250	5.542477	-0.023492	2.551037
116.628335	2100.737016	5.547482	-0.023560	2.555524
116.775135	2108.780871	5.552486	-0.023593	2.559978
117.106213	2116.821207	5.557491	-0.023661	2.564436
117.384009	2124.889851	5.562496	-0.023718	2.568898
117.353690	2132.991346	5.567501	-0.023718	2.573348
117.685719	2141.033076	5.572506	-0.023786	2.577783
118.257248	2149.027688	5.577510	-0.023898	2.582201
118.681473	2157.094545	5.582515	-0.023983	2.586641
118.913249	2165.223963	5.587520	-0.024032	2.591094
118.966221	2173.439483	5.592525	-0.024048	2.595574
119.450195	2181.381625	5.597530	-0.024143	2.599927
119.619797	2189.373973	5.602534	-0.024181	2.604279
120.014602	2197.384628	5.607539	-0.024260	2.608648
120.127842	2205.454629	5.612544	-0.024287	2.613023
120.400179	2213.488711	5.617549	-0.024343	2.617383
120.742643	2221.524488	5.622554	-0.024413	2.621740
120.909321	2229.558741	5.627558	-0.024450	2.626077
121.358288	2237.596234	5.632563	-0.024539	2.630428
121.365231	2245.710538	5.637568	-0.024546	2.634784
121.573735	2253.733582	5.642573	-0.024591	2.639097
122.097301	2261.741388	5.647578	-0.024694	2.643415
122.198526	2269.793364	5.652582	-0.024719	2.647722
122.280249	2277.885816	5.657587	-0.024740	2.652042
122.837143	2285.904059	5.662592	-0.024849	2.656347
123.279557	2293.934927	5.667597	-0.024937	2.660643
123.430038	2302.001094	5.672602	-0.024971	2.664933
123.611247	2310.038276	5.677606	-0.025011	2.669202
124.003701	2318.151391	5.682611	-0.025089	2.673519
124.307963	2326.166066	5.687616	-0.025152	2.677770
124.587637	2334.184791	5.692621	-0.025210	2.682015
125.197633	2342.210878	5.697626	-0.025329	2.686279
125.376620	2350.250392	5.702630	-0.025368	2.690515
125.810976	2358.334439	5.707635	-0.025455	2.694784
125.781002	2366.389627	5.712640	-0.025455	2.699002
126.123107	2374.400755	5.717645	-0.025524	2.703213
126.403496	2382.473272	5.722650	-0.025582	2.707447
126.594683	2390.526131	5.727654	-0.025624	2.711657
127.015969	2398.568317	5.732659	-0.025708	2.715870
126.930528	2406.636240	5.737664	-0.025698	2.720058
127.289669	2414.637688	5.742669	-0.025771	2.724233
127.385660	2422.732982	5.747674	-0.025794	2.728434
127.600555	2430.778984	5.752678	-0.025840	2.732610
127.888316	2438.829995	5.757683	-0.025899	2.736786
127.893534	2446.894219	5.762688	-0.025906	2.740946
128.310095	2454.897818	5.767693	-0.025989	2.745093
128.544673	2462.941318	5.772698	-0.026039	2.749244
128.467757	2471.092233	5.777702	-0.026030	2.753424
128.969377	2479.094211	5.782707	-0.026130	2.757557
129.352737	2487.096126	5.787712	-0.026207	2.761676
129.590373	2495.115682	5.792717	-0.026257	2.765789
129.832696	2503.165749	5.797722	-0.026308	2.769912
130.321088	2511.200435	5.802726	-0.026404	2.774035
130.439645	2519.270849	5.807731	-0.026432	2.778149
130.631527	2527.301101	5.812736	-0.026474	2.782240
130.831068	2535.325157	5.817741	-0.026517	2.786323
131.274039	2543.372942	5.822746	-0.026605	2.790426
131.538962	2551.421957	5.827750	-0.026660	2.794513
132.010338	2559.423158	5.832755	-0.026753	2.798582
132.236708	2567.461468	5.837760	-0.026801	2.802649
132.348613	2575.527266	5.842765	-0.026828	2.806718
132.645217	2583.570539	5.847770	-0.026889	2.810780
132.832602	2591.639414	5.852774	-0.026930	2.814843
133.273824	2599.666649	5.857779	-0.027018	2.818893
133.491542	2607.703192	5.862784	-0.027064	2.822929
133.768679	2615.747077	5.867789	-0.027121	2.826967
134.055242	2623.818446	5.872794	-0.027180	2.831013
134.358363	2631.870816	5.877798	-0.027243	2.835045
134.678400	2639.884580	5.882803	-0.027308	2.839053
134.796205	2647.926524	5.887808	-0.027336	2.843057
135.095705	2655.946704	5.892813	-0.027397	2.847056
135.196968	2664.029118	5.897818	-0.027422	2.851068
135.303444	2672.063068	5.902822	-0.027447	2.855051
135.509036	2680.117356	5.907827	-0.027491	2.859044
135.762145	2688.135907	5.912832	-0.027544	2.863017
135.935642	2696.160742	5.917837	-0.027582	2.866982
136.486034	2704.221166	5.922842	-0.027691	2.870981
136.649412	2712.274178	5.927846	-0.027727	2.874948
136.924051	2720.290340	5.932851	-0.027784	2.878899
136.980604	2728.336264	5.937856	-0.027800	2.882846
137.184427	2736.371750	5.942861	-0.027844	2.886791
137.328301	2744.428207	5.947866	-0.027876	2.890737
137.463541	2752.477521	5.952870	-0.027907	2.894675
137.907526	2760.490218	5.957875	-0.027996	2.898605
138.015619	2768.540917	5.962880	-0.028022	2.902531
138.219956	2776.568184	5.967885	-0.028065	2.906445
138.688882	2784.614554	5.972890	-0.028159	2.910377
138.992278	2792.745686	5.977894	-0.028221	2.914336
139.119645	2800.753825	5.982899	-0.028250	2.918221
139.332404	2808.743972	5.987904	-0.028296	2.922096
139.562138	2816.779217	5.992909	-0.028344	2.925989
139.620751	2824.827791	5.997914	-0.028361	2.929874
140.049244	2832.846763	6.002918	-0.028446	2.933759
140.197195	2840.890896	6.007923	-0.028480	2.937636
140.376778	2848.935804	6.012928	-0.028519	2.941510
140.699885	2856.940696	6.017933	-0.028585	2.945368
141.041319	2864.986229	6.022938	-0.028654	2.949240
141.366239	2873.034518	6.027942	-0.028720	2.953108
141.506609	2881.081410	6.032947	-0.028752	2.956960
141.746247	2889.090224	6.037952	-0.028803	2.960795
142.039396	2897.117570	6.042957	-0.028863	2.964636
142.200375	2905.186077	6.047962	-0.028899	2.968485
142.387039	2913.217711	6.052966	-0.028939	2.972312
142.706306	2921.275245	6.057971	-0.029005	2.976154
142.582221	2929.328729	6.062976	-0.028987	2.979966
142.833504	2937.330067	6.067981	-0.029040	2.983768
143.120824	2945.372270	6.072986	-0.029099	2.987586
143.317041	2953.425326	6.077990	-0.029141	2.991399
143.577995	2961.493174	6.082995	-0.029196	2.995218
143.825890	2969.489292	6.088000	-0.029248	2.998998
143.928605	2977.504977	6.093005	-0.029273	3.002774
144.241492	2985.540591	6.098010	-0.029337	3.006566
144.549759	2993.545073	6.103014	-0.029400	3.010338
144.911400	3001.599484	6.108019	-0.029473	3.014131
145.164971	3009.632182	6.113024	-0.029526	3.017904
145.440722	3017.652709	6.118029	-0.029583	3.021668
145.719058	3025.701851	6.123034	-0.029641	3.025440
145.848822	3033.732456	6.128038	-0.029670	3.029192
146.347595	3041.791742	6.133043	-0.029769	3.032970
146.690839	3049.829135	6.138048	-0.029839	3.036726
146.825034	3057.847886	6.143053	-0.029870	3.040458
146.997256	3065.881390	6.148058	-0.029907	3.044195
147.229842	3073.913915	6.153062	-0.029956	3.047929
147.883146	3081.939418	6.158067	-0.030084	3.051675
148.426270	3089.999293	6.163072	-0.030191	3.055428
148.974428	3097.964666	6.168077	-0.030299	3.059132
149.421580	3106.019414	6.173082	-0.030388	3.062868
149.537529	3114.048908	6.178086	-0.030415	3.066572
149.753545	3122.118712	6.183091	-0.030461	3.070295
149.859217	3130.285126	6.188096	-0.030486	3.074053
150.042553	3138.271968	6.193101	-0.030526	3.077727
150.457854	3146.268786	6.198106	-0.030609	3.081412
150.581967	3154.252333	6.203110	-0.030638	3.085073
150.880645	3162.298161	6.208115	-0.030700	3.088767
151.258387	3170.351965	6.213120	-0.030776	3.092463
151.450947	3178.386992	6.218125	-0.030817	3.096137
151.564092	3186.412911	6.223130	-0.030844	3.099800
151.417559	3194.453825	6.228134	-0.030823	3.103453
151.733794	3202.498395	6.233139	-0.030887	3.107124
152.031427	3210.528364	6.238144	-0.030949	3.110784
152.266614	3218.543863	6.243149	-0.030998	3.114430
152.643256	3226.578950	6.248154	-0.031074	3.118087
152.744171	3234.599947	6.253158	-0.031099	3.121720
152.857779	3242.639459	6.258163	-0.031125	3.125359
153.107663	3250.670088	6.263168	-0.031178	3.128995
153.287889	3258.718452	6.268173	-0.031217	3.132632
153.651695	3266.760965	6.273178	-0.031291	3.136270
153.896299	3274.776805	6.278182	-0.031342	3.139886
154.031985	3282.807140	6.283187	-0.031373	3.143500
154.051221	3290.867243	6.288192	-0.031382	3.147119
154.153059	3298.912540	6.293197	-0.031407	3.150729
154.636316	3306.966216	6.298202	-0.031503	3.154357
154.730081	3314.963938	6.303206	-0.031526	3.157938
154.925103	3322.984036	6.308211	-0.031568	3.161529
155.054317	3330.992433	6.313216	-0.031598	3.165108
155.105693	3339.009087	6.318221	-0.031613	3.168683
155.206638	3347.092493	6.323226	-0.031638	3.172286
155.403036	3355.138722	6.328230	-0.031680	3.175873
155.682271	3363.114455	6.333235	-0.031738	3.179428
155.911227	3371.162522	6.338240	-0.031786	3.183008
155.981846	3379.186301	6.343245	-0.031805	3.186567
156.237681	3387.234560	6.348250	-0.031859	3.190141
156.369017	3395.269236	6.353254	-0.031889	3.193699
156.775626	3403.301602	6.358259	-0.031970	3.197264
156.912436	3411.329118	6.363264	-0.032001	3.200812
156.897178	3419.292846	6.368269	-0.032004	3.204321
157.377948	3427.364562	6.373274	-0.032100	3.207895
157.715927	3435.409277	6.378278	-0.032168	3.211446
158.084640	3443.438133	6.383283	-0.032243	3.214988
158.008164	3451.485841	6.388288	-0.032234	3.218516
158.341316	3459.491096	6.393293	-0.032302	3.222038
158.440918	3467.554259	6.398298	-0.032326	3.225572
158.487228	3475.573442	6.403302	-0.032341	3.229081
158.596145	3483.673488	6.408307	-0.032367	3.232624
158.861415	3491.720690	6.413312	-0.032422	3.236146
159.084257	3499.666787	6.418317	-0.032469	3.239619
159.299510	3507.688951	6.423322	-0.032515	3.243120
159.355226	3515.711663	6.428326	-0.032531	3.246612
159.695083	3523.717556	6.433331	-0.032600	3.250104
159.941813	3531.777515	6.438336	-0.032652	3.253612
160.287670	3539.786757	6.443341	-0.032722	3.257098
160.444854	3547.842970	6.448346	-0.032757	3.260593
160.261800	3555.868988	6.453350	-0.032729	3.264058
160.640539	3563.892659	6.458355	-0.032805	3.267540
160.932496	3571.919960	6.463360	-0.032865	3.271017
160.898144	3579.979812	6.468365	-0.032865	3.274491
161.146407	3587.990679	6.473370	-0.032917	3.277951
161.460470	3595.993295	6.478374	-0.032981	3.281407
161.506594	3604.039603	6.483379	-0.032995	3.284868
161.734092	3612.073720	6.488384	-0.033043	3.288326
161.982876	3620.078087	6.493389	-0.033095	3.291769
162.346563	3628.143351	6.498394	-0.033169	3.295239
162.511221	3636.140973	6.503398	-0.033205	3.298668
162.731170	3644.180056	6.508403	-0.033252	3.302114
163.039302	3652.204433	6.513408	-0.033315	3.305553
163.011670	3660.245223	6.518413	-0.033316	3.308983
163.263419	3668.312064	6.523418	-0.033368	3.312431
163.595962	3676.330400	6.528422	-0.033436	3.315858
163.994604	3684.299952	6.533427	-0.033516	3.319263
164.194717	3692.340232	6.538432	-0.033559	3.322687
164.388055	3700.354918	6.543437	-0.033601	3.326096
164.584356	3708.395348	6.548442	-0.033643	3.329513
164.354655	3716.466696	6.553446	-0.033606	3.332923
164.642090	3724.517265	6.558451	-0.033665	3.336340
165.035678	3732.508605	6.563456	-0.033744	3.339733
164.989036	3740.520670	6.568461	-0.033742	3.343115
165.239785	3748.573519	6.573466	-0.033794	3.346521
165.482638	3756.569418	6.578470	-0.033845	3.349900
165.684596	3764.647532	6.583475	-0.033888	3.353308
165.714273	3772.699802	6.588480	-0.033900	3.356696
165.840809	3780.664915	6.593485	-0.033929	3.360047
166.532977	3788.683277	6.598490	-0.034064	3.363437
166.430184	3796.723750	6.603494	-0.034050	3.366805
166.654004	3804.768195	6.608499	-0.034098	3.370183
166.840193	3812.815822	6.613504	-0.034138	3.373557
166.879903	3820.838479	6.618509	-0.034151	3.376912
167.040130	3828.863404	6.623514	-0.034187	3.380269
167.087168	3836.865543	6.628518	-0.034201	3.383610
167.361563	3844.906632	6.633523	-0.034258	3.386971
167.503443	3852.930252	6.638528	-0.034290	3.390317
167.539151	3861.063165	6.643533	-0.034303	3.393701
167.988817	3869.050737	6.648538	-0.034392	3.397036
167.764469	3877.041076	6.653542	-0.034356	3.400345
168.059276	3885.006308	6.658547	-0.034417	3.403659
168.285061	3893.058325	6.663552	-0.034465	3.407003
168.554581	3901.062664	6.668557	-0.034521	3.410325
168.557338	3909.130294	6.673562	-0.034527	3.413661
168.843205	3917.138557	6.678566	-0.034586	3.416979
169.225816	3925.130114	6.683571	-0.034663	3.420291
169.404563	3933.159262	6.688576	-0.034702	3.423607
169.386981	3941.188143	6.693581	-0.034704	3.426914
170.088267	3949.209916	6.698586	-0.034841	3.430238
170.201863	3957.268082	6.703590	-0.034868	3.433555
170.108195	3965.321337	6.708595	-0.034856	3.436859
170.301176	3973.336915	6.713600	-0.034898	3.440154
170.491078	3981.311758	6.718605	-0.034939	3.443430
170.810545	3989.364654	6.723610	-0.035004	3.446738
170.910757	3997.388179	6.728614	-0.035028	3.450024
171.064728	4005.452524	6.733619	-0.035063	3.453325
170.995239	4013.525031	6.738624	-0.035056	3.456619
171.035493	4021.496878	6.743629	-0.035069	3.459873
171.415969	4029.529518	6.748634	-0.035146	3.463159
171.647912	4037.554974	6.753638	-0.035195	3.466434
171.654961	4045.571480	6.758643	-0.035202	3.469695
172.198880	4053.651300	6.763648	-0.035309	3.472997
172.314993	4061.667550	6.768653	-0.035336	3.476255
172.506223	4069.644636	6.773658	-0.035377	3.479497
172.765545	4077.628518	6.778662	-0.035431	3.482741
173.092367	4085.664812	6.783667	-0.035498	3.486005
173.315291	4093.665978	6.788672	-0.035545	3.489248
173.097011	4101.760225	6.793677	-0.035510	3.492512
173.484669	4109.795332	6.798682	-0.035588	3.495769
173.796405	4117.744131	6.803686	-0.035652	3.498985
173.826295	4125.802887	6.808691	-0.035664	3.502233
174.118160	4133.837999	6.813696	-0.035724	3.505477
174.308417	4141.831080	6.818701	-0.035765	3.508698
174.371904	4149.927647	6.823706	-0.035782	3.511954
174.521401	4157.960581	6.828710	-0.035816	3.515183
174.830473	4165.910876	6.833715	-0.035879	3.518382
175.081583	4173.961841	6.838720	-0.035932	3.521616
175.355414	4181.935903	6.843725	-0.035989	3.524817
175.660051	4189.993089	6.848730	-0.036051	3.528049
175.855200	4198.044237	6.853734	-0.036093	3.531273
175.706309	4206.111667	6.858739	-0.036071	3.534489
176.127390	4214.126133	6.863744	-0.036155	3.537699
176.357003	4222.139767	6.868749	-0.036204	3.540900
176.552727	4230.142915	6.873754	-0.036246	3.544092
176.582153	4238.214514	6.878758	-0.036257	3.547304
176.861809	4246.230746	6.883763	-0.036315	3.550498
176.883100	4254.403372	6.888768	-0.036325	3.553744
176.885817	4262.343957	6.893773	-0.036331	3.556895
177.052706	4270.318032	6.898778	-0.036368	3.560061
177.182956	4278.299631	6.903782	-0.036398	3.563225
177.385666	4286.350150	6.908787	-0.036441	3.566417
177.403010	4294.363145	6.913792	-0.036450	3.569585
177.640590	4302.394799	6.918797	-0.036500	3.572764
178.102205	4310.422876	6.923802	-0.036592	3.575945
177.990340	4318.397962	6.928806	-0.036577	3.579086
178.418185	4326.433512	6.933811	-0.036663	3.582264
178.580563	4334.446459	6.938816	-0.036699	3.585422
178.689536	4342.489483	6.943821	-0.036725	3.588588
178.759340	4350.555215	6.948826	-0.036743	3.591759
178.995350	4358.534187	6.953830	-0.036793	3.594897
179.268615	4366.535093	6.958835	-0.036850	3.598043
179.153331	4374.618782	6.963840	-0.036834	3.601207
179.421901	4382.546492	6.968845	-0.036890	3.604318
179.762006	4390.597466	6.973850	-0.036959	3.607476
179.850209	4398.619997	6.978854	-0.036981	3.610614
179.922196	4406.709900	6.983859	-0.037000	3.613775
180.156972	4414.741785	6.988864	-0.037050	3.616914
180.010276	4422.739516	6.993869	-0.037028	3.620028
180.280328	4430.756510	6.998874	-0.037084	3.623157
180.524727	4438.793600	7.003878	-0.037135	3.626291
180.652728	4446.804112	7.008883	-0.037165	3.629409
180.853421	4454.899341	7.013888	-0.037208	3.632558
180.945826	4462.907807	7.018893	-0.037231	3.635669
181.333512	4470.893868	7.023898	-0.037309	3.638776
181.482924	4478.909844	7.028902	-0.037343	3.641885
181.519523	4486.915501	7.033907	-0.037355	3.644985
181.823513	4494.955668	7.038912	-0.037418	3.648103
181.777954	4502.991230	7.043917	-0.037415	3.651207
182.022744	4511.025116	7.048922	-0.037466	3.654315
182.081286	4519.034110	7.053926	-0.037483	3.657406
182.199829	4527.070962	7.058931	-0.037511	3.660507
182.332656	4535.083713	7.063936	-0.037541	3.663596
182.708733	4543.089309	7.068941	-0.037617	3.666686
182.917212	4551.138301	7.073946	-0.037661	3.669786
183.002930	4559.174794	7.078950	-0.037683	3.672875
183.057135	4567.213699	7.083955	-0.037699	3.675962
183.357166	4575.176200	7.088960	-0.037761	3.679023
183.359906	4583.196232	7.093965	-0.037767	3.682096
183.565613	4591.225009	7.098970	-0.037811	3.685175
183.596046	4599.244432	7.103974	-0.037822	3.688243
183.733702	4607.303527	7.108979	-0.037854	3.691327
183.920911	4615.325277	7.113984	-0.037894	3.694395
184.093359	4623.320373	7.118989	-0.037932	3.697450
184.333759	4631.358687	7.123994	-0.037983	3.700520
184.343795	4639.359770	7.128998	-0.037990	3.703568
184.692504	4647.400433	7.134003	-0.038061	3.706637
185.052496	4655.428302	7.139008	-0.038134	3.709699
185.125085	4663.488109	7.144013	-0.038153	3.712763
185.116689	4671.549959	7.149018	-0.038157	3.715824
185.527240	4679.485350	7.154022	-0.038240	3.718844
185.616989	4687.511364	7.159027	-0.038262	3.721888
185.749100	4695.504182	7.164032	-0.038292	3.724919
185.628081	4703.504822	7.169037	-0.038276	3.727943
186.147180	4711.531618	7.174042	-0.038378	3.730991
186.196591	4719.574243	7.179046	-0.038393	3.734030
186.311942	4727.625088	7.184051	-0.038420	3.737072
186.705416	4735.652653	7.189056	-0.038499	3.740109
186.646136	4743.641526	7.194061	-0.038494	3.743118
186.783256	4751.692559	7.199066	-0.038525	3.746153
186.953140	4759.701664	7.204070	-0.038563	3.749171
187.295188	4767.736528	7.209075	-0.038632	3.752199
187.409879	4775.788782	7.214080	-0.038659	3.755227
187.471541	4783.781795	7.219085	-0.038676	3.758228
187.866266	4791.871524	7.224090	-0.038756	3.761271
187.975545	4799.807943	7.229094	-0.038782	3.764248
187.771202	4807.857444	7.234099	-0.038750	3.767257
187.958862	4815.877743	7.239104	-0.038790	3.770262
188.143613	4823.920582	7.244109	-0.038830	3.773273
188.424749	4831.993369	7.249114	-0.038889	3.776295
188.580735	4839.931345	7.254118	-0.038923	3.779261
188.811851	4847.975804	7.259123	-0.038972	3.782266
188.886003	4855.985885	7.264128	-0.038992	3.785253
189.279298	4864.012632	7.269133	-0.039071	3.788250
189.519475	4872.050834	7.274138	-0.039121	3.791246
189.416503	4880.104945	7.279142	-0.039108	3.794238
189.401288	4888.108896	7.284147	-0.039111	3.797210
189.700469	4896.108163	7.289152	-0.039172	3.800186
189.833618	4904.066326	7.294157	-0.039203	3.803140
190.124412	4912.104107	7.299162	-0.039263	3.806125
190.209314	4920.111428	7.304166	-0.039284	3.809092
190.198357	4928.178728	7.309171	-0.039288	3.812077
190.406597	4936.202476	7.314176	-0.039332	3.815048
190.520547	4944.211815	7.319181	-0.039359	3.818009
190.982626	4952.226846	7.324186	-0.039451	3.820977
190.921974	4960.225815	7.329190	-0.039446	3.823926
190.911364	4968.231469	7.334195	-0.039449	3.826877
191.200119	4976.312748	7.339200	-0.039509	3.829859
191.442950	4984.319040	7.344205	-0.039560	3.832810
191.530577	4992.393916	7.349210	-0.039582	3.835781
191.839360	5000.344462	7.354214	-0.039645	3.838708
191.788084	5008.366549	7.359219	-0.039641	3.841652
192.012900	5016.369942	7.364224	-0.039689	3.844593
192.263153	5024.373889	7.369229	-0.039741	3.847532
192.519485	5032.429779	7.374234	-0.039795	3.850488
192.672897	5040.459284	7.379238	-0.039829	3.853430
192.687874	5048.527414	7.384243	-0.039838	3.856381
193.036217	5056.552620	7.389248	-0.039908	3.859320
193.031976	5064.527319	7.394253	-0.039913	3.862232
193.060571	5072.559318	7.399258	-0.039924	3.865164
193.049271	5080.582477	7.404262	-0.039928	3.868089
193.526105	5088.610937	7.409267	-0.040023	3.871023
193.644965	5096.924164	7.414272	-0.040051	3.874052
193.678607	5104.816663	7.419277	-0.040063	3.876923
193.961916	5112.747173	7.424282	-0.040121	3.879811
194.063132	5120.726998	7.429286	-0.040146	3.882712
194.185455	5128.716879	7.434291	-0.040174	3.885614
194.343006	5136.731592	7.439296	-0.040209	3.888524
194.727256	5144.760212	7.444301	-0.040287	3.891441
194.972273	5152.815306	7.449306	-0.040338	3.894362
194.893376	5160.809850	7.454310	-0.040329	3.897253
195.116891	5168.803119	7.459315	-0.040376	3.900148
195.125562	5176.846479	7.464320	-0.040384	3.903054
195.021153	5184.861925	7.469325	-0.040370	3.905946
195.491810	5192.866506	7.474330	-0.040463	3.908843
195.490271	5200.930164	7.479334	-0.040469	3.911750
195.553586	5208.937542	7.484339	-0.040486	3.914635
195.673503	5216.948836	7.489344	-0.040515	3.917521
195.829368	5224.913903	7.494349	-0.040549	3.920389
195.969095	5232.938702	7.499354	-0.040581	3.923276
195.818617	5241.010244	7.504358	-0.040559	3.926172
196.215635	5248.946108	7.509363	-0.040638	3.929028
196.589367	5257.015365	7.514368	-0.040714	3.931928
196.579382	5265.044569	7.519373	-0.040718	3.934805
196.695819	5273.091674	7.524378	-0.040745	3.937689
196.944412	5281.053520	7.529382	-0.040797	3.940543
197.043058	5289.071458	7.534387	-0.040821	3.943412
197.194873	5297.138119	7.539392	-0.040855	3.946297
197.449482	5305.117373	7.544397	-0.040909	3.949150
197.720084	5313.183140	7.549402	-0.040965	3.952033
197.603314	5321.242222	7.554406	-0.040949	3.954904
197.779595	5329.205263	7.559411	-0.040987	3.957744
198.123048	5337.220433	7.564416	-0.041057	3.960604
198.182101	5345.195516	7.569421	-0.041074	3.963442
198.498030	5353.237854	7.574426	-0.041138	3.966306
198.703327	5361.226361	7.579430	-0.041182	3.969148
198.565538	5369.302957	7.584435	-0.041162	3.972012
198.800148	5377.359808	7.589440	-0.041212	3.974874
198.944194	5385.348421	7.594445	-0.041244	3.977708
199.034892	5393.399086	7.599450	-0.041267	3.980562
199.069857	5401.384941	7.604454	-0.041279	3.983389
199.475081	5409.401662	7.609459	-0.041361	3.986231
199.750131	5417.409105	7.614464	-0.041417	3.989066
199.422410	5425.468724	7.619469	-0.041362	3.991907
199.491239	5433.532565	7.624474	-0.041381	3.994755
199.892758	5441.522348	7.629478	-0.041461	3.997579
200.053579	5449.523598	7.634483	-0.041497	4.000402
200.175128	5457.547429	7.639488	-0.041525	4.003229
200.265146	5465.582854	7.644493	-0.041548	4.006059
200.427217	5473.586136	7.649498	-0.041584	4.008876
200.489365	5481.635141	7.654502	-0.041601	4.011706
200.687160	5489.634022	7.659507	-0.041644	4.014518
200.971835	5497.668567	7.664512	-0.041703	4.017343
200.978106	5505.649052	7.669517	-0.041709	4.020141
201.421197	5513.655120	7.674522	-0.041798	4.022954
201.720444	5521.680414	7.679526	-0.041859	4.025769
201.477923	5529.724355	7.684531	-0.041820	4.028580
201.672807	5537.791465	7.689536	-0.041862	4.031405
201.984184	5545.869123	7.694541	-0.041926	4.034232
202.154949	5553.836111	7.699546	-0.041963	4.037017
202.205513	5561.803979	7.704550	-0.041978	4.039798
202.305832	5569.793159	7.709555	-0.042003	4.042586
202.543449	5577.836750	7.714560	-0.042053	4.045393
202.666522	5585.821815	7.719565	-0.042081	4.048175
202.746701	5593.846543	7.724570	-0.042102	4.050969
203.007103	5601.877399	7.729574	-0.042156	4.053766
203.227423	5609.900310	7.734579	-0.042203	4.056557
203.238182	5617.900658	7.739584	-0.042211	4.059336
203.362608	5625.926111	7.744589	-0.042240	4.062123
203.657924	5633.906898	7.749594	-0.042300	4.064895
203.800382	5641.959884	7.754598	-0.042333	4.067688
204.033282	5649.958887	7.759603	-0.042382	4.070462
204.380006	5658.027429	7.764608	-0.042452	4.073259
204.240430	5666.060746	7.769613	-0.042432	4.076035
204.248050	5674.067389	7.774618	-0.042439	4.078803
204.571426	5682.055136	7.779622	-0.042505	4.081566
204.808380	5690.011149	7.784627	-0.042555	4.084315
204.787657	5698.084216	7.789632	-0.042557	4.087099
205.036425	5706.070652	7.794637	-0.042609	4.089855
205.087520	5714.156453	7.799642	-0.042624	4.092641
205.352957	5722.163239	7.804646	-0.042679	4.095401
205.467154	5730.139632	7.809651	-0.042706	4.098146
205.633911	5738.211170	7.814656	-0.042743	4.100923
205.739423	5746.168772	7.819661	-0.042769	4.103657
205.880527	5754.226817	7.824666	-0.042801	4.106425
206.200312	5762.252635	7.829670	-0.042866	4.109183
206.160246	5770.305761	7.834675	-0.042864	4.111943
206.496161	5778.371147	7.839680	-0.042933	4.114710
206.650237	5786.301114	7.844685	-0.042967	4.117427
207.124159	5794.315796	7.849690	-0.043061	4.120175
207.353738	5802.350543	7.854694	-0.043110	4.122925
207.516079	5810.329242	7.859699	-0.043145	4.125653
207.687029	5818.377927	7.864704	-0.043183	4.128403
207.663682	5826.437293	7.869709	-0.043185	4.131153
207.912349	5834.460131	7.874714	-0.043237	4.133891
208.023390	5842.514433	7.879718	-0.043263	4.136637
208.238676	5850.433753	7.884723	-0.043309	4.139336
208.429721	5858.519812	7.889728	-0.043350	4.142090
208.254792	5866.511330	7.894733	-0.043323	4.144806
208.962322	5874.564272	7.899738	-0.043461	4.147551
209.024591	5882.556232	7.904742	-0.043478	4.150266
208.795290	5890.610537	7.909747	-0.043441	4.152997
209.031207	5898.638303	7.914752	-0.043491	4.155722
209.452150	5906.595049	7.919757	-0.043575	4.158424
209.270362	5914.652462	7.924762	-0.043547	4.161151
209.326137	5922.643349	7.929766	-0.043563	4.163857
209.714012	5930.654079	7.934771	-0.043641	4.166571
209.960132	5938.686056	7.939776	-0.043693	4.169289
209.744485	5946.731430	7.944781	-0.043658	4.172004
210.078594	5954.744263	7.949786	-0.043726	4.174713
210.165795	5962.768755	7.954790	-0.043748	4.177422
210.241885	5970.748847	7.959795	-0.043768	4.180113
210.554777	5978.775510	7.964800	-0.043832	4.182821
210.512181	5986.743002	7.969805	-0.043830	4.185504
210.810889	5994.847503	7.974810	-0.043891	4.188234
210.752511	6002.855581	7.979814	-0.043886	4.190926
210.946822	6010.974108	7.984819	-0.043928	4.193657
211.059865	6019.010392	7.989824	-0.043955	4.196357
211.144711	6026.876934	7.994829	-0.043977	4.198998
211.276711	6034.931348	7.999834	-0.044007	4.201701
211.428275	6042.837607	8.004838	-0.044041	4.204353
211.527543	6050.887588	8.009843	-0.044065	4.207051
211.856144	6058.909620	8.014848	-0.044132	4.209740
212.104999	6066.945892	8.019853	-0.044184	4.212431
212.148918	6075.001103	8.024858	-0.044198	4.215125
212.240500	6082.993694	8.029862	-0.044221	4.217796
212.353311	6090.976735	8.034867	-0.044248	4.220463
212.650241	6099.012746	8.039872	-0.044309	4.223148
212.615642	6107.046005	8.044877	-0.044308	4.225826
212.738613	6115.037562	8.049882	-0.044337	4.228491
212.727437	6123.115018	8.054886	-0.044340	4.231181
212.981745	6131.112993	8.059891	-0.044393	4.233846
213.359887	6139.150109	8.064896	-0.044470	4.236523
213.506083	6147.107974	8.069901	-0.044503	4.239170
213.618347	6155.157386	8.074906	-0.044529	4.241845
213.729183	6163.158359	8.079910	-0.044556	4.244503
213.860592	6171.134645	8.084915	-0.044586	4.247150
214.329540	6179.200770	8.089920	-0.044679	4.249829
214.260596	6187.225775	8.094925	-0.044672	4.252488
214.450997	6195.286395	8.099930	-0.044713	4.255159
214.627420	6203.283663	8.104934	-0.044752	4.257808
214.743677	6211.292336	8.109939	-0.044779	4.260458
214.871763	6219.304790	8.114944	-0.044809	4.263107
215.173376	6227.312941	8.119949	-0.044871	4.265755
215.297333	6235.322382	8.124954	-0.044899	4.268401
215.230018	6243.406237	8.129958	-0.044893	4.271067
215.374787	6251.412880	8.134963	-0.044925	4.273708
215.558709	6259.475658	8.139968	-0.044965	4.276367
215.450479	6267.392660	8.144973	-0.044951	4.278973
215.747610	6275.491068	8.149978	-0.045012	4.281641
215.861933	6283.438808	8.154982	-0.045039	4.284256
215.973760	6291.500782	8.159987	-0.045066	4.286907
216.197303	6299.486113	8.164992	-0.045113	4.289532
216.368004	6307.553842	8.169997	-0.045151	4.292181
216.556928	6315.579546	8.175002	-0.045192	4.294816
216.689121	6323.556399	8.180006	-0.045222	4.297433
216.955083	6331.533046	8.185011	-0.045277	4.300049
217.206339	6339.617056	8.190016	-0.045330	4.302698
216.858834	6347.565771	8.195021	-0.045271	4.305297
216.938375	6355.638013	8.200026	-0.045291	4.307938
217.406974	6363.631656	8.205030	-0.045384	4.310554
217.454501	6371.688846	8.210035	-0.045399	4.313187
217.575910	6379.730161	8.215040	-0.045427	4.315813
217.743332	6387.664357	8.220045	-0.045464	4.318403
217.953723	6395.702026	8.225050	-0.045509	4.321025
217.950159	6403.700579	8.230054	-0.045514	4.323632
218.161340	6411.722222	8.235059	-0.045559	4.326246
218.674720	6419.721066	8.240064	-0.045661	4.328853
218.819406	6427.721451	8.245069	-0.045693	4.331457
218.738906	6435.837245	8.250074	-0.045684	4.334094
219.082537	6443.861422	8.255078	-0.045754	4.336704
219.217865	6451.795922	8.260083	-0.045785	4.339281
219.389894	6459.813349	8.265088	-0.045823	4.341884
219.306609	6467.796675	8.270093	-0.045813	4.344472
219.643449	6475.867623	8.275098	-0.045881	4.347090
219.612723	6483.901907	8.280102	-0.045881	4.349693
219.777939	6491.957300	8.285107	-0.045918	4.352301
220.093940	6500.001070	8.290112	-0.045982	4.354906
219.957917	6507.969885	8.295117	-0.045963	4.357481
220.075886	6515.946118	8.300122	-0.045991	4.360059
220.465065	6523.980848	8.305126	-0.046069	4.362657
220.611195	6531.942957	8.310131	-0.046102	4.365227
220.776195	6539.992732	8.315136	-0.046138	4.367825
220.815026	6548.004219	8.320141	-0.046151	4.370408
221.142718	6556.031562	8.325146	-0.046218	4.372996
221.248535	6564.059165	8.330150	-0.046243	4.375581
221.450882	6572.007312	8.335155	-0.046287	4.378140
221.719108	6580.100786	8.340160	-0.046343	4.380744
221.937043	6588.064058	8.345165	-0.046389	4.383305
221.999977	6596.098016	8.350170	-0.046406	4.385886
222.238466	6604.117135	8.355174	-0.046456	4.388462
222.253143	6612.128390	8.360179	-0.046465	4.391032
222.557792	6620.227055	8.365184	-0.046528	4.393630
222.707989	6628.239698	8.370189	-0.046561	4.396199
222.798874	6636.199579	8.375194	-0.046584	4.398749
222.915504	6644.251511	8.380198	-0.046611	4.401326
223.071620	6652.197256	8.385203	-0.046646	4.403869
223.381119	6660.265343	8.390208	-0.046710	4.406450
223.401983	6668.252965	8.395213	-0.046719	4.409002
223.478946	6676.343127	8.400218	-0.046739	4.411586
223.530790	6684.334734	8.405222	-0.046755	4.414137
223.934670	6692.338324	8.410227	-0.046836	4.416691
223.997373	6700.363638	8.415232	-0.046853	4.419250
223.873042	6708.374867	8.420237	-0.046836	4.421801
224.166918	6716.340375	8.425242	-0.046896	4.424339
224.355352	6724.446569	8.430246	-0.046937	4.426919
224.516594	6732.387103	8.435251	-0.046973	4.429445
224.902966	6740.475452	8.440256	-0.047050	4.432018
224.847849	6748.509945	8.445261	-0.047046	4.434570
224.904683	6756.505213	8.450266	-0.047062	4.437108
225.051247	6764.455642	8.455270	-0.047095	4.439631
225.117005	6772.483635	8.460275	-0.047113	4.442177
225.518716	6780.515778	8.465280	-0.047194	4.444725
225.574146	6788.545366	8.470285	-0.047210	4.447268
225.745340	6796.577114	8.475290	-0.047248	4.449811
225.986567	6804.614624	8.480294	-0.047298	4.452355
225.881232	6812.588050	8.485299	-0.047284	4.454876
226.144509	6820.635572	8.490304	-0.047339	4.457420
226.284322	6828.583488	8.495309	-0.047371	4.459931
226.542260	6836.599847	8.500314	-0.047425	4.462462
226.666350	6844.631335	8.505318	-0.047454	4.464996
226.975336	6852.658395	8.510323	-0.047517	4.467528
227.123734	6860.690955	8.515328	-0.047550	4.470060
227.063280	6868.753251	8.520333	-0.047545	4.472599
227.250009	6876.740039	8.525338	-0.047585	4.475113
227.472264	6884.786617	8.530342	-0.047632	4.477645
227.334298	6892.726392	8.535347	-0.047612	4.480141
227.598612	6900.754870	8.540352	-0.047667	4.482664
227.813928	6908.747707	8.545357	-0.047713	4.485175
227.748993	6916.772761	8.550362	-0.047707	4.487693
227.616609	6924.816899	8.555366	-0.047688	4.490216
228.194304	6932.853794	8.560371	-0.047801	4.492738
228.330109	6940.906528	8.565376	-0.047832	4.495261
228.334325	6948.890253	8.570381	-0.047839	4.497761
228.345432	6956.866395	8.575386	-0.047847	4.500258
228.664741	6964.863262	8.580391	-0.047912	4.502760
228.770065	6972.859542	8.585395	-0.047937	4.505260
229.184570	6980.941698	8.590400	-0.048020	4.507786
229.218621	6988.926648	8.595405	-0.048032	4.510280
229.260839	6997.026041	8.600410	-0.048046	4.512808
229.396522	7005.031162	8.605415	-0.048077	4.515305
229.581796	7012.962268	8.610419	-0.048117	4.517778
229.848982	7020.993418	8.615424	-0.048173	4.520281
229.687670	7028.994092	8.620429	-0.048148	4.522772
230.146943	7036.987776	8.625434	-0.048240	4.525261
230.288265	7045.028362	8.630439	-0.048272	4.527762
230.320935	7053.018924	8.635443	-0.048284	4.530246
230.438285	7061.104815	8.640448	-0.048311	4.532759
230.530992	7069.097853	8.645453	-0.048334	4.535241
230.634210	7077.149587	8.650458	-0.048359	4.537740
230.826998	7085.126764	8.655463	-0.048401	4.540215
231.078098	7093.113088	8.660467	-0.048453	4.542692
231.308207	7101.131202	8.665472	-0.048502	4.545176
231.514220	7109.177122	8.670477	-0.048546	4.547668
231.831277	7117.166450	8.675482	-0.048611	4.550142
232.063300	7125.251527	8.680487	-0.048660	4.552643
232.102178	7133.219820	8.685491	-0.048673	4.555107
232.376739	7141.277314	8.690496	-0.048730	4.557597
232.464238	7149.239001	8.695501	-0.048752	4.560056
232.598201	7157.293876	8.700506	-0.048782	4.562542
232.683449	7165.277469	8.705511	-0.048804	4.565005
232.802664	7173.257190	8.710515	-0.048832	4.567465
232.869617	7181.325562	8.715520	-0.048850	4.569952
232.963523	7189.372926	8.720525	-0.048874	4.572430
233.331155	7197.403574	8.725530	-0.048948	4.574903
233.592581	7205.456280	8.730535	-0.049002	4.577380
233.453751	7213.373358	8.735539	-0.048982	4.579814
233.565540	7221.408807	8.740544	-0.049009	4.582284
233.678289	7229.401873	8.745549	-0.049035	4.584739
234.042327	7237.501496	8.750554	-0.049109	4.587226
234.070446	7245.497393	8.755559	-0.049120	4.589679
234.224998	7253.538109	8.760563	-0.049154	4.592145
234.613847	7261.562485	8.765568	-0.049233	4.594604
234.709609	7269.573354	8.770573	-0.049256	4.597058
234.807652	7277.501845	8.775578	-0.049280	4.599486
235.061788	7285.548731	8.780583	-0.049333	4.601948
235.111887	7293.507261	8.785587	-0.049348	4.604382
235.344163	7301.587425	8.790592	-0.049397	4.606852
235.581933	7309.535045	8.795597	-0.049447	4.609280
235.494688	7317.594393	8.800602	-0.049437	4.611740
235.551795	7325.653936	8.805607	-0.049453	4.614200
235.899774	7333.648259	8.810611	-0.049524	4.616638
235.958366	7341.635556	8.815616	-0.049540	4.619073
235.963758	7349.664988	8.820621	-0.049547	4.621519
236.208965	7357.620947	8.825626	-0.049599	4.623942
236.560275	7365.711600	8.830631	-0.049670	4.626404
236.678532	7373.695551	8.835635	-0.049698	4.628833
236.614751	7381.750257	8.840640	-0.049691	4.631282
236.866240	7389.797386	8.845645	-0.049744	4.633727
237.015502	7397.800360	8.850650	-0.049778	4.636158
236.914773	7405.752576	8.855655	-0.049765	4.638571
237.143306	7413.764180	8.860659	-0.049813	4.641002
237.557968	7421.793914	8.865664	-0.049896	4.643436
237.414868	7429.830712	8.870669	-0.049875	4.645872
237.772670	7437.825650	8.875674	-0.049947	4.648294
237.987014	7445.871926	8.880679	-0.049993	4.650729
238.070195	7453.862239	8.885683	-0.050014	4.653147
238.408729	7461.927824	8.890688	-0.050083	4.655586
238.479609	7469.899711	8.895693	-0.050102	4.657996
238.747858	7477.881671	8.900698	-0.050158	4.660407
238.740530	7485.952629	8.905703	-0.050162	4.662844
238.790907	7493.921475	8.910707	-0.050177	4.665249
239.290201	7501.985444	8.915712	-0.050276	4.667680
239.269276	7509.973774	8.920717	-0.050278	4.670089
239.397373	7518.058135	8.925722	-0.050307	4.672524
239.813373	7526.154413	8.930727	-0.050391	4.674962
239.794983	7534.040181	8.935731	-0.050393	4.677336
239.955124	7542.010831	8.940736	-0.050428	4.679733
240.107670	7550.063487	8.945741	-0.050463	4.682155
240.114075	7557.990701	8.950746	-0.050470	4.684537
240.347897	7566.078204	8.955751	-0.050519	4.686966
240.328306	7574.037399	8.960755	-0.050521	4.689356
240.596231	7582.149199	8.965760	-0.050577	4.691789
240.736396	7590.086445	8.970765	-0.050608	4.694169
240.837108	7598.187951	8.975770	-0.050633	4.696598
241.130566	7606.115744	8.980775	-0.050693	4.698972
241.082617	7614.145370	8.985779	-0.050690	4.701377
241.413304	7622.170369	8.990784	-0.050758	4.703778
241.631699	7630.189373	8.995789	-0.050804	4.706176
241.627238	7638.166988	9.000794	-0.050809	4.708561
241.982824	7646.248665	9.005799	-0.050881	4.710976
242.106805	7654.243901	9.010803	-0.050910	4.713363
242.255825	7662.308311	9.015808	-0.050943	4.715770
242.230590	7670.315781	9.020813	-0.050944	4.718160
242.308828	7678.281081	9.025818	-0.050965	4.720535
242.689540	7686.302340	9.030823	-0.051041	4.722925
242.906263	7694.327387	9.035827	-0.051087	4.725315
242.871540	7702.358469	9.040832	-0.051087	4.727706
243.060614	7710.371584	9.045837	-0.051128	4.730091
243.316884	7718.392619	9.050842	-0.051181	4.732476
243.419044	7726.432053	9.055847	-0.051206	4.734866
243.337654	7734.398101	9.060851	-0.051196	4.737233
243.667114	7742.421711	9.065856	-0.051263	4.739615
243.768808	7750.414519	9.070861	-0.051288	4.741988
243.948432	7758.395362	9.075866	-0.051327	4.744355
244.143702	7766.546814	9.080871	-0.051370	4.746772
244.248505	7774.482374	9.085875	-0.051395	4.749124
244.341228	7782.575677	9.090880	-0.051418	4.751521
244.455044	7790.578436	9.095885	-0.051445	4.753890
244.638200	7798.568104	9.100890	-0.051485	4.756254
244.879093	7806.506553	9.105895	-0.051535	4.758602
244.956816	7814.529458	9.110899	-0.051555	4.760974
245.347501	7822.538008	9.115904	-0.051634	4.763339
245.398937	7830.526427	9.120909	-0.051649	4.765698
245.304532	7838.595285	9.125914	-0.051637	4.768081
245.559597	7846.609095	9.130919	-0.051691	4.770444
245.676683	7854.643206	9.135923	-0.051718	4.772813
245.796607	7862.719537	9.140928	-0.051746	4.775193
246.087457	7870.673977	9.145933	-0.051806	4.777536
246.177683	7878.657304	9.150938	-0.051829	4.779886
246.285707	7886.690470	9.155943	-0.051855	4.782250
246.255305	7894.632328	9.160947	-0.051855	4.784587
246.415528	7902.721996	9.165952	-0.051890	4.786965
246.748380	7910.711968	9.170957	-0.051958	4.789312
246.803532	7918.768950	9.175962	-0.051974	4.791678
247.072380	7926.811807	9.180967	-0.052030	4.794038
246.991712	7934.818429	9.185971	-0.052021	4.796388
247.284939	7942.834585	9.190976	-0.052081	4.798738
247.424798	7950.799193	9.195981	-0.052113	4.801073
247.609119	7958.822778	9.200986	-0.052153	4.803423
247.727346	7966.807754	9.205991	-0.052181	4.805761
247.494918	7974.819924	9.210995	-0.052143	4.808107
248.073588	7982.885216	9.216000	-0.052257	4.810465
248.235137	7990.311517	9.221005	-0.052292	4.812636
248.387588	7994.790798	9.226010	-0.052324	4.813944

248.551506	7997.356044	9.231015	-0.052357	4.814693
248.914388	7998.682454	9.236019	-0.052426	4.815079
248.947815	7999.165947	9.241024	-0.052433	4.815220
249.008021	8000.045212	9.246029	-0.052445	4.815477
249.272491	8000.034651	9.251034	-0.052495	4.815473
249.693780	8000.077958	9.256039	-0.052574	4.815483
249.433374	8000.012818	9.261043	-0.052526	4.815465
249.592305	8000.028301	9.266048	-0.052556	4.815469
249.698933	8000.069635	9.271053	-0.052576	4.815481
249.692434	8000.043932	9.276058	-0.052576	4.815473
249.514190	8000.060278	9.281063	-0.052543	4.815479
249.783496	8000.082920	9.286067	-0.052594	4.815484
249.925923	8000.090653	9.291072	-0.052621	4.815486
249.914417	8000.058457	9.296077	-0.052619	4.815476
249.922529	8000.020173	9.301082	-0.052621	4.815465
249.797966	8000.066250	9.306087	-0.052598	4.815479
249.924551	8000.034190	9.311091	-0.052622	4.815469
250.224447	8000.066952	9.316096	-0.052679	4.815477
250.271578	8000.070980	9.321101	-0.052688	4.815478
250.277134	8000.066845	9.326106	-0.052690	4.815477
250.310421	8000.103768	9.331111	-0.052696	4.815488
250.359247	8000.065085	9.336115	-0.052706	4.815476
250.533271	8000.049832	9.341120	-0.052739	4.815471
250.562618	8000.119813	9.346125	-0.052745	4.815491
250.337896	8000.069147	9.351130	-0.052704	4.815477
250.633900	8000.106122	9.356135	-0.052759	4.815487
250.625692	8000.082527	9.361139	-0.052758	4.815480
250.433260	8000.043077	9.366144	-0.052723	4.815469
250.436731	8000.050661	9.371149	-0.052724	4.815471
250.461942	8000.029753	9.376154	-0.052729	4.815465
250.539720	8000.065271	9.381159	-0.052744	4.815475
250.498836	8000.058234	9.386163	-0.052737	4.815473
250.531364	8000.057748	9.391168	-0.052744	4.815473
250.437645	8000.093648	9.396173	-0.052727	4.815484
250.426102	8000.064656	9.401178	-0.052725	4.815475
250.665431	8000.073986	9.406183	-0.052770	4.815477
250.412193	8000.064521	9.411187	-0.052724	4.815475
250.650691	8000.101617	9.416192	-0.052769	4.815485
250.812878	8000.107540	9.421197	-0.052800	4.815486
250.676320	8000.107475	9.426202	-0.052775	4.815487
250.549272	8000.100088	9.431207	-0.052751	4.815485
250.605878	8000.061533	9.436211	-0.052763	4.815473
251.179055	8000.092387	9.441216	-0.052870	4.815480
250.836523	8000.115643	9.446221	-0.052807	4.815488
250.685467	8000.088627	9.451226	-0.052779	4.815481
250.873754	8000.085363	9.456231	-0.052815	4.815479
250.836089	8000.034571	9.461235	-0.052808	4.815464
250.749705	8000.048154	9.466240	-0.052792	4.815469
250.755228	8000.091031	9.471245	-0.052794	4.815481
250.995915	8000.064055	9.476250	-0.052839	4.815472
250.883425	8000.103921	9.481255	-0.052819	4.815484
250.862933	8000.041658	9.486259	-0.052816	4.815466
251.092611	8000.098911	9.491264	-0.052859	4.815482
251.082232	8000.104129	9.496269	-0.052858	4.815483
250.997858	8000.104924	9.501274	-0.052842	4.815484
251.120956	8000.103792	9.506279	-0.052866	4.815483
251.189571	8000.107106	9.511283	-0.052879	4.815484
251.336557	8000.107437	9.516288	-0.052907	4.815483
251.273986	8000.106453	9.521293	-0.052896	4.815483
251.253768	8000.070906	9.526298	-0.052893	4.815473
251.035083	8000.099407	9.531303	-0.052853	4.815482
250.955335	8000.073565	9.536307	-0.052838	4.815475
251.335004	8000.091618	9.541312	-0.052909	4.815478
251.263740	8000.096902	9.546317	-0.052897	4.815480
251.046114	8000.039940	9.551322	-0.052857	4.815465
251.135698	8000.107708	9.556327	-0.052874	4.815484
251.186912	8000.082955	9.561331	-0.052884	4.815477
251.182270	8000.088268	9.566336	-0.052884	4.815478
251.275784	8000.148622	9.571341	-0.052902	4.815495
251.361888	8000.110552	9.576346	-0.052918	4.815484
251.585794	8000.162370	9.581351	-0.052960	4.815498
251.264724	8000.064169	9.586355	-0.052901	4.815471
251.401339	8000.070740	9.591360	-0.052927	4.815472
251.180143	8000.075692	9.596365	-0.052886	4.815474
251.111944	8000.103465	9.601370	-0.052874	4.815483
251.368283	8000.118418	9.606375	-0.052923	4.815486
251.400746	8000.068780	9.611379	-0.052929	4.815471
251.329250	8000.155266	9.616384	-0.052916	4.815497
251.183101	8000.163591	9.621389	-0.052890	4.815500
251.259968	8000.099725	9.626394	-0.052904	4.815481
251.268316	8000.143718	9.631399	-0.052907	4.815494
251.381388	8000.110367	9.636403	-0.052928	4.815483
251.399043	8000.122458	9.641408	-0.052932	4.815487
251.504548	8000.132791	9.646413	-0.052952	4.815489
251.288247	8000.094014	9.651418	-0.052912	4.815479
251.385536	8000.108485	9.656423	-0.052931	4.815483
251.449822	8000.054029	9.661427	-0.052943	4.815467
251.485392	8000.112361	9.666432	-0.052951	4.815483
251.281340	8000.174225	9.671437	-0.052913	4.815503
251.457737	8000.102382	9.676442	-0.052947	4.815481
251.601163	8000.109066	9.681447	-0.052974	4.815482
251.560351	8000.081728	9.686451	-0.052967	4.815474
251.406941	8000.091001	9.691456	-0.052939	4.815478
251.268108	8000.074871	9.696461	-0.052913	4.815473
251.400943	8000.068557	9.701466	-0.052939	4.815471
251.662775	8000.138096	9.706471	-0.052988	4.815490
251.308158	8000.066054	9.711475	-0.052922	4.815471
251.426586	8000.111860	9.716480	-0.052945	4.815483
251.455142	8000.130542	9.721485	-0.052951	4.815489
251.514664	8000.112336	9.726490	-0.052962	4.815483
251.620981	8000.160080	9.731495	-0.052983	4.815497
251.591893	8000.121181	9.736499	-0.052978	4.815485
251.791587	8000.122381	9.741504	-0.053016	4.815485
251.841700	8000.202324	9.746509	-0.053026	4.815508
251.616103	8000.162324	9.751514	-0.052984	4.815497
251.536036	8000.152504	9.756519	-0.052970	4.815495
251.686513	8000.090919	9.761523	-0.052998	4.815476
251.812904	8000.062061	9.766528	-0.053022	4.815467
251.644232	8000.082837	9.771533	-0.052991	4.815474
251.710210	8000.061531	9.776538	-0.053004	4.815467
251.755375	8000.125364	9.781543	-0.053013	4.815486
251.804512	8000.147591	9.786547	-0.053023	4.815492
251.714307	8000.160043	9.791552	-0.053007	4.815496
251.733534	8000.134762	9.796557	-0.053011	4.815488
251.635123	8000.134256	9.801562	-0.052993	4.815489
251.703821	8000.129023	9.806567	-0.053006	4.815487
251.751752	8000.143750	9.811571	-0.053016	4.815491
251.931914	8000.171342	9.816576	-0.053050	4.815498
251.839370	8000.185891	9.821581	-0.053033	4.815503
251.849956	8000.099563	9.826586	-0.053035	4.815478
251.989004	8000.152121	9.831591	-0.053062	4.815492
251.774432	8000.135810	9.836595	-0.053023	4.815488
251.847344	8000.124236	9.841600	-0.053037	4.815485
252.015930	8000.128129	9.846605	-0.053069	4.815485
251.863104	8000.090397	9.851610	-0.053041	4.815475
251.761354	8000.137919	9.856615	-0.053022	4.815489
251.755776	8000.103681	9.861619	-0.053022	4.815479
252.068479	8000.100332	9.866624	-0.053080	4.815477
251.936569	8000.089657	9.871629	-0.053056	4.815474
251.839846	8000.115892	9.876634	-0.053039	4.815482
252.165620	8000.112758	9.881639	-0.053100	4.815480
252.036775	8000.087175	9.886643	-0.053077	4.815473
252.069947	8000.074946	9.891648	-0.053083	4.815469
251.962063	8000.086037	9.896653	-0.053064	4.815473
252.021330	8000.073170	9.901658	-0.053075	4.815469
252.240574	8000.147352	9.906663	-0.053117	4.815489
252.015115	8000.082778	9.911667	-0.053075	4.815472
251.952451	8000.101025	9.916672	-0.053064	4.815477
251.934460	8000.125352	9.921677	-0.053061	4.815484
251.978630	8000.106893	9.926682	-0.053070	4.815479
252.212439	8000.151396	9.931687	-0.053114	4.815491
252.050541	8000.108172	9.936691	-0.053084	4.815479
252.021241	8000.107736	9.941696	-0.053080	4.815479
252.109534	8000.132745	9.946701	-0.053097	4.815486
252.187319	8000.143690	9.951706	-0.053112	4.815488
252.054144	8000.172530	9.956711	-0.053087	4.815498
252.230114	8000.125255	9.961715	-0.053121	4.815483
252.211154	8000.127127	9.966720	-0.053118	4.815483
252.174776	8000.135122	9.971725	-0.053111	4.815486
252.069856	8000.107796	9.976730	-0.053092	4.815478
252.217650	8000.213925	9.981735	-0.053120	4.815509
252.152681	8000.134899	9.986739	-0.053109	4.815486
252.227789	8000.109470	9.991744	-0.053123	4.815478
252.060663	8000.175149	9.996749	-0.053093	4.815498
252.301239	8000.097952	10.001754	-0.053138	4.815474
252.126699	8000.148549	10.006759	-0.053106	4.815490
252.223446	8000.086078	10.011763	-0.053125	4.815471
252.380719	8000.126115	10.016768	-0.053154	4.815482
252.385419	8000.134788	10.021773	-0.053156	4.815485
252.194525	8000.075057	10.026778	-0.053121	4.815468
252.174019	8000.159180	10.031783	-0.053118	4.815493
252.045219	8000.090855	10.036787	-0.053094	4.815473
252.134335	8000.112673	10.041792	-0.053111	4.815479
252.269730	8000.160897	10.046797	-0.053137	4.815493
252.308160	8000.135933	10.051802	-0.053145	4.815485
252.077252	8000.116147	10.056807	-0.053102	4.815481
252.087928	8000.123849	10.061811	-0.053105	4.815483
252.224996	8000.098373	10.066816	-0.053131	4.815475
252.325347	8000.143883	10.071821	-0.053150	4.815488
252.209091	8000.129192	10.076826	-0.053129	4.815484
252.380582	8000.208999	10.081831	-0.053161	4.815506
252.455339	8000.126932	10.086835	-0.053176	4.815482
252.406679	8000.141137	10.091840	-0.053167	4.815486
252.347128	8000.153024	10.096845	-0.053157	4.815490
252.474185	8000.083573	10.101850	-0.053181	4.815469
252.292939	8000.134060	10.106855	-0.053148	4.815485
252.111038	8000.102259	10.111859	-0.053114	4.815476
252.226206	8000.128780	10.116864	-0.053136	4.815483
252.125178	8000.134641	10.121869	-0.053118	4.815486
252.126925	8000.081291	10.126874	-0.053119	4.815470
252.315245	8000.135730	10.131879	-0.053154	4.815485
252.194046	8000.111341	10.136883	-0.053132	4.815478
252.170254	8000.108858	10.141888	-0.053128	4.815478
252.391941	8000.091188	10.146893	-0.053170	4.815472
252.332222	8000.083839	10.151898	-0.053160	4.815470
252.284416	8000.138662	10.156903	-0.053151	4.815486
252.316015	8000.089008	10.161907	-0.053158	4.815471
252.293855	8000.106855	10.166912	-0.053154	4.815477
252.373709	8000.110355	10.171917	-0.053170	4.815477
252.350995	8000.046984	10.176922	-0.053166	4.815459
252.576410	8000.094556	10.181927	-0.053208	4.815472
252.586363	8000.136439	10.186931	-0.053211	4.815484
252.460856	8000.107704	10.191936	-0.053188	4.815476
252.324609	8000.123671	10.196941	-0.053163	4.815481
252.509655	8000.073341	10.201946	-0.053198	4.815466
252.625035	8000.128716	10.206951	-0.053220	4.815481
252.351490	8000.090061	10.211955	-0.053170	4.815471
252.431139	8000.092489	10.216960	-0.053185	4.815472
252.519069	8000.123904	10.221965	-0.053202	4.815480
252.509764	8000.084262	10.226970	-0.053201	4.815469
252.489112	8000.112819	10.231975	-0.053197	4.815477
252.436174	8000.091691	10.236979	-0.053188	4.815471
252.374801	8000.115303	10.241984	-0.053177	4.815478
252.294885	8000.137540	10.246989	-0.053163	4.815485
252.476225	8000.097834	10.251994	-0.053197	4.815473
252.805945	8000.135372	10.256999	-0.053259	4.815482
252.469007	8000.079644	10.262003	-0.053197	4.815468
252.498739	8000.069495	10.267008	-0.053203	4.815464
252.883786	8000.145344	10.272013	-0.053275	4.815485
252.500828	8000.101680	10.277018	-0.053204	4.815474
252.540164	8000.139774	10.282023	-0.053212	4.815485
252.446430	8000.135070	10.287027	-0.053195	4.815484
252.419311	8000.095134	10.292032	-0.053191	4.815472
252.485988	8000.075977	10.297037	-0.053204	4.815466
252.346436	8000.070519	10.302042	-0.053178	4.815465
252.528125	8000.110959	10.307047	-0.053213	4.815476
252.438646	8000.103120	10.312051	-0.053196	4.815474
252.365144	8000.074173	10.317056	-0.053183	4.815466
252.525131	8000.109981	10.322061	-0.053214	4.815476
252.597851	8000.055663	10.327066	-0.053228	4.815460
252.542219	8000.100740	10.332071	-0.053218	4.815473
252.485337	8000.061382	10.337075	-0.053208	4.815462
252.513685	8000.080061	10.342080	-0.053214	4.815467
252.714759	8000.083422	10.347085	-0.053252	4.815467
252.467890	8000.058029	10.352090	-0.053206	4.815461
252.732750	8000.123348	10.357095	-0.053256	4.815479
252.514828	8000.098432	10.362099	-0.053216	4.815473
252.481564	8000.122507	10.367104	-0.053210	4.815480
252.688024	8000.091764	10.372109	-0.053249	4.815470
252.707719	8000.089998	10.377114	-0.053253	4.815469
252.636612	8000.110244	10.382119	-0.053241	4.815475
252.679146	8000.094964	10.387123	-0.053249	4.815471
252.737530	8000.117344	10.392128	-0.053261	4.815477
252.677808	8000.140983	10.397133	-0.053250	4.815484
252.770337	8000.085922	10.402138	-0.053268	4.815468
252.882945	8000.102784	10.407143	-0.053289	4.815472
252.854827	8000.086339	10.412147	-0.053284	4.815467
252.799408	8000.107912	10.417152	-0.053275	4.815474
252.958829	8000.147986	10.422157	-0.053305	4.815485
252.768665	8000.074374	10.427162	-0.053270	4.815464
252.646557	8000.107670	10.432167	-0.053248	4.815474
252.778026	8000.087445	10.437171	-0.053273	4.815468
252.843614	8000.109944	10.442176	-0.053286	4.815474
252.547424	8000.111520	10.447181	-0.053231	4.815476
252.617035	8000.069972	10.452186	-0.053244	4.815464
252.635966	8000.121621	10.457191	-0.053249	4.815478
252.661013	8000.125287	10.462195	-0.053254	4.815479
252.660270	8000.101813	10.467200	-0.053254	4.815473
252.692993	8000.105605	10.472205	-0.053261	4.815473
252.718896	8000.066543	10.477210	-0.053266	4.815462
252.741813	8000.139628	10.482215	-0.053271	4.815483
252.692120	8000.119622	10.487219	-0.053262	4.815478
252.837844	8000.106043	10.492224	-0.053290	4.815473
252.752153	8000.138871	10.497229	-0.053274	4.815483
252.670249	8000.085209	10.502234	-0.053260	4.815468
252.864875	8000.104492	10.507239	-0.053296	4.815472
252.772672	8000.081648	10.512243	-0.053280	4.815466
252.792416	8000.051032	10.517248	-0.053284	4.815457
252.695221	8000.107179	10.522253	-0.053266	4.815474
252.576840	8000.071081	10.527258	-0.053245	4.815464
252.696281	8000.119044	10.532263	-0.053268	4.815477
252.775937	8000.096896	10.537267	-0.053283	4.815470
252.688427	8000.095500	10.542272	-0.053267	4.815470
252.631799	8000.125601	10.547277	-0.053257	4.815479
252.619474	8000.065607	10.552282	-0.053255	4.815462
252.797502	8000.111330	10.557287	-0.053289	4.815474
253.015784	8000.071164	10.562291	-0.053330	4.815462
252.767235	8000.091691	10.567296	-0.053285	4.815469
252.921331	8000.073975	10.572301	-0.053314	4.815463
252.936939	8000.094582	10.577306	-0.053317	4.815469
252.897073	8000.140988	10.582311	-0.053310	4.815483
252.716033	8000.125227	10.587315	-0.053277	4.815479
252.797702	8000.089221	10.592320	-0.053293	4.815468
252.994997	8000.169457	10.597325	-0.053330	4.815490
252.900859	8000.070713	10.602330	-0.053313	4.815462
252.882977	8000.138852	10.607335	-0.053310	4.815482
252.910298	8000.136144	10.612339	-0.053316	4.815481
252.739969	8000.091710	10.617344	-0.053285	4.815469
252.909719	8000.092417	10.622349	-0.053317	4.815468
252.922685	8000.089472	10.627354	-0.053320	4.815467
253.002161	8000.126092	10.632359	-0.053335	4.815478
252.882066	8000.093171	10.637363	-0.053313	4.815468
252.928257	8000.096116	10.642368	-0.053323	4.815469
252.937230	8000.133710	10.647373	-0.053325	4.815480
252.855783	8000.099289	10.652378	-0.053310	4.815470
252.900627	8000.090458	10.657383	-0.053319	4.815468
252.938851	8000.109301	10.662387	-0.053327	4.815473
252.722486	8000.126083	10.667392	-0.053287	4.815479
252.923590	8000.098457	10.672397	-0.053325	4.815470
252.940066	8000.088090	10.677402	-0.053328	4.815467
252.857493	8000.128449	10.682407	-0.053314	4.815479
252.727757	8000.095370	10.687411	-0.053290	4.815470
252.786392	8000.098520	10.692416	-0.053301	4.815470
252.909392	8000.117692	10.697421	-0.053325	4.815475
252.758620	8000.076785	10.702426	-0.053297	4.815464
252.787533	8000.121119	10.707431	-0.053303	4.815477
252.874333	8000.101226	10.712435	-0.053320	4.815471
252.820119	8000.107859	10.717440	-0.053310	4.815473
252.941031	8000.154778	10.722445	-0.053333	4.815486
252.887206	8000.087687	10.727450	-0.053324	4.815467
253.014593	8000.141125	10.732455	-0.053348	4.815482
252.819279	8000.116581	10.737459	-0.053312	4.815475
252.882322	8000.147586	10.742464	-0.053325	4.815484
252.866726	8000.116388	10.747469	-0.053322	4.815475
252.670028	8000.143112	10.752474	-0.053286	4.815484
253.032437	8000.152339	10.757479	-0.053354	4.815485
252.986767	8000.165524	10.762483	-0.053346	4.815489
252.932815	8000.149722	10.767488	-0.053337	4.815484
253.002906	8000.180844	10.772493	-0.053350	4.815493
253.045946	8000.133515	10.777498	-0.053359	4.815479
252.995744	8000.176545	10.782503	-0.053350	4.815492
253.067791	8000.164957	10.787507	-0.053364	4.815488
253.068901	8000.143651	10.792512	-0.053365	4.815482
253.025454	8000.150462	10.797517	-0.053357	4.815484
252.908087	8000.094077	10.802522	-0.053336	4.815468
253.004116	8000.109598	10.807527	-0.053354	4.815472
253.391517	8000.134198	10.812531	-0.053427	4.815478
253.168977	8000.111341	10.817536	-0.053386	4.815472
253.251290	8000.138391	10.822541	-0.053402	4.815479
253.095021	8000.126244	10.827546	-0.053373	4.815477
253.109813	8000.132946	10.832551	-0.053376	4.815478
253.056123	8000.109668	10.837555	-0.053367	4.815472
253.072128	8000.106773	10.842560	-0.053370	4.815471
253.210828	8000.139027	10.847565	-0.053397	4.815480
253.150813	8000.088930	10.852570	-0.053386	4.815465
253.001438	8000.150628	10.857575	-0.053359	4.815484
253.043119	8000.109688	10.862579	-0.053367	4.815472
253.094131	8000.090273	10.867584	-0.053377	4.815466
253.113492	8000.101325	10.872589	-0.053381	4.815469
253.036319	8000.088345	10.877594	-0.053368	4.815466
253.179588	8000.095029	10.882599	-0.053395	4.815467
253.271960	8000.114764	10.887603	-0.053412	4.815472
253.250672	8000.108049	10.892608	-0.053409	4.815470
253.431758	8000.155961	10.897613	-0.053443	4.815483
253.252451	8000.094280	10.902618	-0.053410	4.815466
253.012580	8000.127772	10.907623	-0.053366	4.815477
253.081473	8000.111858	10.912627	-0.053380	4.815472
253.030298	8000.103581	10.917632	-0.053371	4.815470
253.083401	8000.115189	10.922637	-0.053381	4.815473
252.989847	8000.089116	10.927642	-0.053364	4.815466
253.210356	8000.161187	10.932647	-0.053406	4.815486
253.088745	8000.149611	10.937651	-0.053384	4.815483
253.096262	8000.101697	10.942656	-0.053386	4.815469
253.140036	8000.174059	10.947661	-0.053394	4.815490
253.025509	8000.092076	10.952666	-0.053373	4.815467
253.160474	8000.136022	10.957671	-0.053399	4.815479
253.208525	8000.101598	10.962675	-0.053409	4.815468
253.138189	8000.096211	10.967680	-0.053396	4.815467
253.151043	8000.132801	10.972685	-0.053399	4.815478
253.035888	8000.080727	10.977690	-0.053378	4.815463
253.174516	8000.125802	10.982695	-0.053404	4.815476
253.009426	8000.111373	10.987699	-0.053374	4.815472
253.143418	8000.081572	10.992704	-0.053400	4.815463
253.291099	8000.115042	10.997709	-0.053428	4.815472
253.121335	8000.073821	11.002714	-0.053397	4.815461
253.030565	8000.075577	11.007719	-0.053380	4.815462
252.977171	8000.080087	11.012723	-0.053371	4.815463
253.175087	8000.072711	11.017728	-0.053408	4.815460
252.970294	8000.136701	11.022733	-0.053371	4.815480
252.801708	8000.088020	11.027738	-0.053340	4.815466
253.128003	8000.115886	11.032743	-0.053401	4.815473
252.991056	8000.092304	11.037747	-0.053376	4.815467
252.997069	8000.077490	11.042752	-0.053378	4.815462
253.222386	8000.107966	11.047757	-0.053420	4.815470
252.927135	8000.050786	11.052762	-0.053366	4.815455
252.936823	8000.101214	11.057767	-0.053368	4.815469
253.065358	8000.110860	11.062771	-0.053393	4.815472
253.331128	8000.103535	11.067776	-0.053443	4.815468
253.317784	8000.102293	11.072781	-0.053441	4.815468
253.025138	8000.064390	11.077786	-0.053387	4.815458
253.221011	8000.131780	11.082791	-0.053424	4.815477
253.150712	8000.138148	11.087795	-0.053411	4.815479
252.938573	8000.115463	11.092800	-0.053372	4.815473
253.094648	8000.123426	11.097805	-0.053402	4.815475
253.088966	8000.081705	11.102810	-0.053401	4.815463
253.071487	8000.109246	11.107815	-0.053398	4.815471
253.059305	8000.098406	11.112819	-0.053397	4.815468
253.278975	8000.088184	11.117824	-0.053438	4.815464
253.291873	8000.111952	11.122829	-0.053441	4.815471
253.228240	8000.085304	11.127834	-0.053430	4.815463
253.229769	8000.153764	11.132839	-0.053431	4.815483
253.369753	8000.111240	11.137843	-0.053457	4.815470
253.281531	8000.095940	11.142848	-0.053441	4.815466
253.553835	8000.167798	11.147853	-0.053492	4.815486
253.236668	8000.069649	11.152858	-0.053434	4.815459
253.131330	8000.117113	11.157863	-0.053415	4.815473
253.193033	8000.126726	11.162867	-0.053427	4.815475
253.274800	8000.115298	11.167872	-0.053443	4.815472
253.231020	8000.149886	11.172877	-0.053435	4.815482
253.117713	8000.101047	11.177882	-0.053414	4.815468
253.308395	8000.102101	11.182887	-0.053450	4.815468
253.281111	8000.109178	11.187891	-0.053446	4.815470
253.249745	8000.092679	11.192896	-0.053441	4.815465
253.359984	8000.127669	11.197901	-0.053462	4.815475
253.264944	8000.099435	11.202906	-0.053444	4.815467
253.300061	8000.144941	11.207911	-0.053452	4.815480
253.052683	8000.122743	11.212915	-0.053406	4.815475
253.315937	8000.107896	11.217920	-0.053456	4.815469
253.582829	8000.154019	11.222925	-0.053506	4.815481
253.324385	8000.142324	11.227930	-0.053458	4.815479
253.445709	8000.176429	11.232935	-0.053481	4.815488
253.264104	8000.135012	11.237939	-0.053448	4.815477
253.280864	8000.103278	11.242944	-0.053452	4.815468
253.415197	8000.140803	11.247949	-0.053477	4.815478
253.354980	8000.081085	11.252954	-0.053467	4.815461
253.320855	8000.119038	11.257959	-0.053461	4.815472
253.238622	8000.159403	11.262963	-0.053446	4.815484
253.220691	8000.129234	11.267968	-0.053443	4.815476
253.250120	8000.123355	11.272973	-0.053449	4.815474
253.127428	8000.098939	11.277978	-0.053427	4.815467
253.318970	8000.116036	11.282983	-0.053463	4.815471
253.429942	8000.083718	11.287987	-0.053484	4.815461
253.303372	8000.051758	11.292992	-0.053461	4.815453
253.250001	8000.102216	11.297997	-0.053452	4.815468
253.387847	8000.086370	11.303002	-0.053478	4.815462
253.190120	8000.100254	11.308007	-0.053442	4.815467
253.220237	8000.092249	11.313011	-0.053448	4.815465
253.250538	8000.091727	11.318016	-0.053454	4.815464
253.446523	8000.127063	11.323021	-0.053491	4.815474
253.226872	8000.064716	11.328026	-0.053451	4.815457
253.303051	8000.100213	11.333031	-0.053465	4.815467
253.253238	8000.091959	11.338035	-0.053457	4.815464
253.224634	8000.094739	11.343040	-0.053452	4.815465
253.214023	8000.113846	11.348045	-0.053450	4.815471
253.368972	8000.099350	11.353050	-0.053480	4.815466
253.222074	8000.126895	11.358055	-0.053453	4.815475
253.164095	8000.093929	11.363059	-0.053443	4.815465
253.319553	8000.091196	11.368064	-0.053472	4.815464
253.194952	8000.125520	11.373069	-0.053449	4.815474
253.229998	8000.079127	11.378074	-0.053456	4.815461
253.149341	8000.081050	11.383079	-0.053442	4.815462
253.286891	8000.104736	11.388083	-0.053468	4.815468
253.123616	8000.095679	11.393088	-0.053438	4.815466
253.181648	8000.091340	11.398093	-0.053450	4.815464
253.393067	8000.118382	11.403098	-0.053490	4.815471
253.452064	8000.115128	11.408103	-0.053501	4.815470
253.366366	8000.120173	11.413107	-0.053486	4.815472
253.359942	8000.103017	11.418112	-0.053485	4.815467
253.308981	8000.093674	11.423117	-0.053476	4.815464
253.225075	8000.103023	11.428122	-0.053461	4.815468
253.239283	8000.104373	11.433127	-0.053464	4.815468
253.361883	8000.140636	11.438131	-0.053487	4.815478
253.141181	8000.094301	11.443136	-0.053447	4.815465
253.087708	8000.113768	11.448141	-0.053437	4.815471
253.126470	8000.075986	11.453146	-0.053445	4.815460
253.491964	8000.147243	11.458151	-0.053514	4.815479
253.297630	8000.097068	11.463155	-0.053478	4.815465
253.260527	8000.095434	11.468160	-0.053472	4.815465
253.510372	8000.124179	11.473165	-0.053519	4.815472
253.559164	8000.117550	11.478170	-0.053528	4.815470
253.527708	8000.141656	11.483175	-0.053523	4.815477
253.794772	8000.131147	11.488179	-0.053573	4.815473
253.523315	8000.072219	11.493184	-0.053523	4.815457
253.302939	8000.097483	11.498189	-0.053483	4.815465
253.298922	8000.058995	11.503194	-0.053483	4.815454
253.343848	8000.093977	11.508199	-0.053491	4.815464
253.411895	8000.087666	11.513203	-0.053505	4.815462
253.339302	8000.060870	11.518208	-0.053492	4.815454
253.576513	8000.076584	11.523213	-0.053536	4.815458
253.408938	8000.053564	11.528218	-0.053506	4.815452
253.478317	8000.085744	11.533223	-0.053519	4.815461
253.328324	8000.121786	11.538227	-0.053492	4.815472
253.420131	8000.070986	11.543232	-0.053509	4.815457
253.544067	8000.092312	11.548237	-0.053533	4.815463
253.322758	8000.076954	11.553242	-0.053492	4.815459
253.518073	8000.116554	11.558247	-0.053529	4.815470
253.502013	8000.113130	11.563251	-0.053527	4.815469
253.435779	8000.111016	11.568256	-0.053515	4.815468
253.542799	8000.122445	11.573261	-0.053535	4.815471
253.452991	8000.066513	11.578266	-0.053519	4.815455
253.246031	8000.090930	11.583271	-0.053481	4.815464
253.583789	8000.092273	11.588275	-0.053545	4.815462
253.528849	8000.081797	11.593280	-0.053535	4.815459
253.315553	8000.105040	11.598285	-0.053496	4.815467
253.347306	8000.056456	11.603290	-0.053502	4.815453
253.726755	8000.100161	11.608295	-0.053573	4.815464
253.581061	8000.075365	11.613299	-0.053547	4.815457
253.421447	8000.090945	11.618304	-0.053518	4.815463
253.593117	8000.126950	11.623309	-0.053550	4.815472
253.596951	8000.098208	11.628314	-0.053551	4.815464
253.636354	8000.124551	11.633319	-0.053559	4.815471
253.700044	8000.120305	11.638323	-0.053572	4.815470
253.631280	8000.122424	11.643328	-0.053559	4.815471
253.817415	8000.112718	11.648333	-0.053594	4.815467
253.702978	8000.109808	11.653338	-0.053574	4.815467
253.749046	8000.110615	11.658343	-0.053583	4.815467
253.760826	8000.162149	11.663347	-0.053586	4.815482
253.619309	8000.089334	11.668352	-0.053560	4.815461
253.780059	8000.154011	11.673357	-0.053590	4.815479
253.649010	8000.136936	11.678362	-0.053566	4.815475
253.467498	8000.128646	11.683367	-0.053533	4.815473
253.429339	8000.114172	11.688371	-0.053526	4.815469
253.605781	8000.119266	11.693376	-0.053560	4.815470
253.503522	8000.132586	11.698381	-0.053541	4.815474
253.183366	8000.102776	11.703386	-0.053482	4.815467
253.523392	8000.152243	11.708391	-0.053546	4.815480
253.561275	8000.171080	11.713395	-0.053554	4.815485
253.375916	8000.094338	11.718400	-0.053520	4.815464
253.588741	8000.145981	11.723405	-0.053560	4.815478
253.673673	8000.075833	11.728410	-0.053576	4.815457
253.647483	8000.114986	11.733415	-0.053572	4.815468
253.529132	8000.137658	11.738419	-0.053550	4.815475
253.463200	8000.078914	11.743424	-0.053539	4.815459
253.544091	8000.152959	11.748429	-0.053554	4.815480
253.477273	8000.108092	11.753434	-0.053542	4.815467
253.497417	8000.127705	11.758439	-0.053547	4.815473
253.602600	8000.155133	11.763443	-0.053567	4.815480
253.543158	8000.136034	11.768448	-0.053556	4.815475
253.480699	8000.125433	11.773453	-0.053545	4.815472
253.427256	8000.083992	11.778458	-0.053536	4.815460
253.499742	8000.111949	11.783463	-0.053550	4.815468
253.666614	8000.096583	11.788467	-0.053581	4.815463
253.759289	8000.089609	11.793472	-0.053599	4.815460
253.590547	8000.145645	11.798477	-0.053568	4.815477
253.616207	8000.101235	11.803482	-0.053573	4.815464
253.773821	8000.111362	11.808487	-0.053603	4.815466
253.847706	8000.121176	11.813491	-0.053618	4.815469
253.628590	8000.137912	11.818496	-0.053577	4.815475
253.478204	8000.136546	11.823501	-0.053550	4.815475
253.500425	8000.139097	11.828506	-0.053554	4.815476
253.509421	8000.102960	11.833511	-0.053557	4.815465
253.451195	8000.118076	11.838515	-0.053546	4.815470
253.575595	8000.089185	11.843520	-0.053570	4.815461
253.789760	8000.147263	11.848525	-0.053610	4.815477
253.561397	8000.104005	11.853530	-0.053568	4.815465
253.732446	8000.130382	11.858535	-0.053601	4.815472
253.893974	8000.114928	11.863539	-0.053631	4.815467
253.535335	8000.114402	11.868544	-0.053565	4.815468
253.686863	8000.141526	11.873549	-0.053594	4.815475
253.713864	8000.140949	11.878554	-0.053600	4.815475
253.548650	8000.154300	11.883559	-0.053569	4.815480
253.674390	8000.191684	11.888563	-0.053593	4.815490
253.832404	8000.117399	11.893568	-0.053623	4.815468
253.882442	8000.158878	11.898573	-0.053633	4.815479
253.740544	8000.157653	11.903578	-0.053607	4.815480
253.723754	8000.138188	11.908583	-0.053605	4.815474
253.796453	8000.135160	11.913587	-0.053619	4.815473
253.722355	8000.133984	11.918592	-0.053605	4.815473
253.407768	8000.122431	11.923597	-0.053547	4.815471
253.637995	8000.134824	11.928602	-0.053591	4.815473
253.856535	8000.140613	11.933607	-0.053632	4.815474
253.725823	8000.147052	11.938611	-0.053608	4.815477
253.598239	8000.150337	11.943616	-0.053585	4.815478
253.947333	8000.183927	11.948621	-0.053650	4.815486
253.590295	8000.137477	11.953626	-0.053584	4.815474
253.541051	8000.146329	11.958631	-0.053576	4.815477
253.739944	8000.181715	11.963635	-0.053613	4.815487
253.905184	8000.138538	11.968640	-0.053645	4.815473
253.794674	8000.144242	11.973645	-0.053625	4.815475
253.850565	8000.145211	11.978650	-0.053636	4.815475
253.836810	8000.134345	11.983655	-0.053634	4.815472
253.757170	8000.077511	11.988659	-0.053619	4.815456
253.845314	8000.085423	11.993664	-0.053636	4.815458
253.671456	8000.121072	11.998669	-0.053604	4.815469
253.410654	8000.086896	12.003674	-0.053556	4.815460
253.541109	8000.116878	12.008679	-0.053581	4.815468
253.787365	8000.130605	12.013683	-0.053627	4.815471
253.781709	8000.118804	12.018688	-0.053627	4.815468
253.729516	8000.154322	12.023693	-0.053618	4.815478
253.738369	8000.098948	12.028698	-0.053620	4.815462
253.671061	8000.119256	12.033703	-0.053608	4.815468
253.605200	8000.107531	12.038707	-0.053596	4.815465
253.635868	8000.084574	12.043712	-0.053602	4.815459
253.753341	8000.170978	12.048717	-0.053625	4.815483
253.732356	8000.137552	12.053722	-0.053621	4.815473
253.717037	8000.146964	12.058727	-0.053619	4.815476
253.862847	8000.176131	12.063731	-0.053647	4.815484
253.877355	8000.121919	12.068736	-0.053650	4.815468
253.732272	8000.147356	12.073741	-0.053624	4.815476
253.710549	8000.114986	12.078746	-0.053620	4.815467
253.591113	8000.118406	12.083751	-0.053598	4.815468
253.501283	8000.091325	12.088755	-0.053582	4.815461
253.589288	8000.093892	12.093760	-0.053599	4.815461
253.984454	8000.107938	12.098765	-0.053673	4.815464
253.765253	8000.081928	12.103770	-0.053633	4.815457
253.753066	8000.087117	12.108775	-0.053631	4.815459
253.888390	8000.163130	12.113779	-0.053657	4.815480
253.752648	8000.087204	12.118784	-0.053632	4.815459
253.679007	8000.090310	12.123789	-0.053619	4.815460
253.660904	8000.079373	12.128794	-0.053616	4.815457
253.942915	8000.109718	12.133799	-0.053669	4.815464
253.919266	8000.133953	12.138803	-0.053665	4.815471
253.818639	8000.115242	12.143808	-0.053647	4.815466
253.794050	8000.130912	12.148813	-0.053643	4.815471
253.673711	8000.122562	12.153818	-0.053621	4.815469
253.752102	8000.117491	12.158823	-0.053636	4.815467
253.912242	8000.169335	12.163827	-0.053667	4.815482
253.635003	8000.078252	12.168832	-0.053615	4.815456
253.486357	8000.133551	12.173837	-0.053588	4.815473
253.490417	8000.100538	12.178842	-0.053590	4.815464
253.662925	8000.136557	12.183847	-0.053622	4.815473
253.464022	8000.126911	12.188851	-0.053586	4.815471
253.500408	8000.109392	12.193856	-0.053593	4.815466
253.684069	8000.132772	12.198861	-0.053628	4.815472
253.706354	8000.139598	12.203866	-0.053633	4.815474
253.808341	8000.159494	12.208871	-0.053652	4.815479
253.857125	8000.169963	12.213875	-0.053662	4.815482
253.847498	8000.124970	12.218880	-0.053660	4.815469
253.952374	8000.195138	12.223885	-0.053680	4.815489
253.760795	8000.136457	12.228890	-0.053645	4.815473
253.911560	8000.127236	12.233895	-0.053674	4.815469
253.731471	8000.176673	12.238899	-0.053641	4.815484
253.404601	8000.126447	12.243904	-0.053581	4.815471
253.514880	8000.134724	12.248909	-0.053602	4.815473
253.543198	8000.161953	12.253914	-0.053607	4.815481
253.798398	8000.142701	12.258919	-0.053655	4.815474
253.716577	8000.177731	12.263923	-0.053641	4.815485
253.574626	8000.116663	12.268928	-0.053615	4.815468
253.702499	8000.173318	12.273933	-0.053639	4.815483
253.490251	8000.114296	12.278938	-0.053600	4.815467
253.667138	8000.149319	12.283943	-0.053634	4.815477
253.751760	8000.145419	12.288947	-0.053650	4.815475
253.806180	8000.117511	12.293952	-0.053661	4.815467
253.870672	8000.146406	12.298957	-0.053673	4.815475
253.886864	8000.164886	12.303962	-0.053677	4.815480
253.842403	8000.147102	12.308967	-0.053669	4.815475
253.614523	8000.130566	12.313971	-0.053627	4.815471
253.665635	8000.149622	12.318976	-0.053637	4.815477
253.677119	8000.195809	12.323981	-0.053640	4.815490
253.559277	8000.147961	12.328986	-0.053618	4.815477
253.753069	8000.173646	12.333991	-0.053655	4.815483
253.790899	8000.177523	12.338995	-0.053663	4.815484
253.614253	8000.104128	12.344000	-0.053630	4.815464
253.665777	8000.140289	12.349005	-0.053640	4.815474
253.757756	8000.100178	12.354010	-0.053658	4.815462
253.864110	8000.129763	12.359015	-0.053678	4.815470
253.965775	8000.181712	12.364019	-0.053698	4.815484
253.831234	8000.121834	12.369024	-0.053673	4.815468
253.961240	8000.167839	12.374029	-0.053698	4.815480
253.747289	8000.123748	12.379034	-0.053659	4.815468
253.973789	8000.138218	12.384039	-0.053701	4.815472
253.988159	8000.138502	12.389043	-0.053705	4.815472
253.785911	8000.156584	12.394048	-0.053667	4.815478
253.934412	8000.195414	12.399053	-0.053696	4.815488
253.901080	8000.186362	12.404058	-0.053690	4.815486
253.803065	8000.124950	12.409063	-0.053672	4.815468
253.787013	8000.209152	12.414067	-0.053670	4.815493
253.728510	8000.123814	12.419072	-0.053659	4.815468
253.787306	8000.163300	12.424077	-0.053671	4.815480
253.519247	8000.091603	12.429082	-0.053621	4.815460
253.839678	8000.125788	12.434087	-0.053682	4.815468
253.975709	8000.209294	12.439091	-0.053708	4.815492
253.772825	8000.147220	12.444096	-0.053670	4.815475
253.873165	8000.158540	12.449101	-0.053690	4.815478
253.937409	8000.183156	12.454106	-0.053702	4.815485
253.924669	8000.174444	12.459111	-0.053700	4.815482
253.782325	8000.225572	12.464115	-0.053674	4.815498
253.561851	8000.114053	12.469120	-0.053634	4.815466
253.826831	8000.130226	12.474125	-0.053684	4.815470
253.910551	8000.144478	12.479130	-0.053700	4.815473
253.977909	8000.132813	12.484135	-0.053713	4.815470
253.895391	8000.157144	12.489139	-0.053698	4.815477
253.686927	8000.132380	12.494144	-0.053660	4.815471
253.791668	8000.098891	12.499149	-0.053680	4.815461
253.929192	8000.115099	12.504154	-0.053706	4.815465
253.947454	8000.111172	12.509159	-0.053710	4.815464
253.794968	8000.110841	12.514163	-0.053682	4.815464
253.772913	8000.106249	12.519168	-0.053678	4.815463
253.891265	8000.113592	12.524173	-0.053701	4.815464
253.665020	8000.146238	12.529178	-0.053659	4.815475
253.584202	8000.126786	12.534183	-0.053645	4.815470
253.913539	8000.116237	12.539187	-0.053707	4.815465
253.931722	8000.134750	12.544192	-0.053710	4.815470
253.791033	8000.117515	12.549197	-0.053685	4.815466
253.724458	8000.190198	12.554202	-0.053673	4.815488
253.798118	8000.166882	12.559207	-0.053687	4.815480
253.879462	8000.149036	12.564211	-0.053703	4.815475
253.775029	8000.109959	12.569216	-0.053684	4.815464
253.867910	8000.111538	12.574221	-0.053702	4.815464
253.816844	8000.139595	12.579226	-0.053693	4.815472
253.806925	8000.125586	12.584231	-0.053691	4.815468
253.751102	8000.142878	12.589235	-0.053682	4.815473
253.642118	8000.086628	12.594240	-0.053662	4.815458
253.928972	8000.103163	12.599245	-0.053716	4.815461
254.042653	8000.120046	12.604250	-0.053737	4.815465
253.923397	8000.139497	12.609255	-0.053716	4.815472
253.944951	8000.130282	12.614259	-0.053720	4.815469
253.648039	8000.091235	12.619264	-0.053666	4.815459
253.944017	8000.135703	12.624269	-0.053721	4.815470
253.874680	8000.099342	12.629274	-0.053709	4.815460
253.814026	8000.119761	12.634279	-0.053698	4.815466
254.090004	8000.137184	12.639283	-0.053750	4.815470
253.798219	8000.085398	12.644288	-0.053696	4.815456
253.764760	8000.142598	12.649293	-0.053690	4.815473
253.765889	8000.115948	12.654298	-0.053691	4.815465
253.928577	8000.135777	12.659303	-0.053722	4.815470
253.773416	8000.143950	12.664307	-0.053694	4.815473
253.783545	8000.098214	12.669312	-0.053696	4.815460
253.991895	8000.111316	12.674317	-0.053735	4.815463
253.834170	8000.125858	12.679322	-0.053707	4.815468
253.682302	8000.106301	12.684327	-0.053679	4.815463
253.837221	8000.137757	12.689331	-0.053708	4.815471
253.821479	8000.140750	12.694336	-0.053706	4.815472
253.899627	8000.145292	12.699341	-0.053721	4.815473
254.039206	8000.135887	12.704346	-0.053747	4.815470
253.931906	8000.122409	12.709351	-0.053728	4.815466
254.046448	8000.132895	12.714355	-0.053750	4.815469
253.976662	8000.090114	12.719360	-0.053737	4.815457
254.178339	8000.145851	12.724365	-0.053775	4.815472
253.981289	8000.130892	12.729370	-0.053739	4.815468
253.878757	8000.139933	12.734375	-0.053721	4.815472
254.078656	8000.127249	12.739379	-0.053758	4.815467
253.983175	8000.090456	12.744384	-0.053741	4.815457
254.015609	8000.154086	12.749389	-0.053748	4.815475
253.820441	8000.117786	12.754394	-0.053712	4.815465
253.898712	8000.072106	12.759399	-0.053727	4.815452
254.101860	8000.134278	12.764403	-0.053765	4.815469
253.942267	8000.098565	12.769408	-0.053736	4.815459
253.920650	8000.126039	12.774413	-0.053733	4.815467
254.105246	8000.151572	12.779418	-0.053768	4.815474
253.832772	8000.113996	12.784423	-0.053717	4.815464
253.914856	8000.146387	12.789427	-0.053733	4.815473
254.017595	8000.116071	12.794432	-0.053753	4.815464
254.092625	8000.157964	12.799437	-0.053767	4.815476
253.866092	8000.130763	12.804442	-0.053726	4.815469
253.848547	8000.140138	12.809447	-0.053723	4.815472
253.756460	8000.129048	12.814451	-0.053706	4.815469
253.772857	8000.096238	12.819456	-0.053710	4.815459
253.939370	8000.093690	12.824461	-0.053741	4.815458
253.712108	8000.095330	12.829466	-0.053700	4.815459
253.581467	8000.103907	12.834471	-0.053676	4.815462
253.799363	8000.128921	12.839475	-0.053717	4.815468
253.785051	8000.082782	12.844480	-0.053715	4.815455
253.901824	8000.129637	12.849485	-0.053737	4.815468
253.754810	8000.137944	12.854490	-0.053710	4.815471
253.955652	8000.140237	12.859495	-0.053748	4.815471
254.063660	8000.176262	12.864499	-0.053769	4.815481
253.934774	8000.132506	12.869504	-0.053745	4.815469
254.024018	8000.155398	12.874509	-0.053763	4.815475
253.997247	8000.105846	12.879514	-0.053758	4.815461
253.836760	8000.101108	12.884519	-0.053729	4.815460
254.122536	8000.171056	12.889523	-0.053783	4.815479
253.922252	8000.129328	12.894528	-0.053746	4.815468
254.027940	8000.154628	12.899533	-0.053766	4.815475
253.779432	8000.125996	12.904538	-0.053720	4.815468
253.883421	8000.142720	12.909543	-0.053740	4.815472
253.998050	8000.180991	12.914547	-0.053762	4.815483
253.766143	8000.132329	12.919552	-0.053719	4.815469
253.978979	8000.158329	12.924557	-0.053759	4.815476
254.074544	8000.171708	12.929562	-0.053778	4.815479
253.989332	8000.150045	12.934567	-0.053762	4.815473
253.844166	8000.198990	12.939571	-0.053736	4.815488
253.907135	8000.169086	12.944576	-0.053748	4.815479
254.126547	8000.195195	12.949581	-0.053790	4.815486
253.875490	8000.198579	12.954586	-0.053743	4.815488
253.659982	8000.157668	12.959591	-0.053704	4.815477
253.861610	8000.212335	12.964595	-0.053742	4.815492
253.773696	8000.154295	12.969600	-0.053726	4.815476
253.897789	8000.190585	12.974605	-0.053750	4.815486
254.078939	8000.160495	12.979610	-0.053784	4.815476
253.964053	8000.143685	12.984615	-0.053763	4.815472
253.990892	8000.159135	12.989619	-0.053769	4.815476
253.819193	8000.161692	12.994624	-0.053737	4.815478
253.700883	8000.157649	12.999629	-0.053716	4.815477
253.919678	8000.195502	13.004634	-0.053757	4.815487
254.078942	8000.175737	13.009639	-0.053787	4.815480
254.200464	8000.257936	13.014643	-0.053810	4.815504
254.110693	8000.168874	13.019648	-0.053794	4.815478
253.969095	8000.156967	13.024653	-0.053768	4.815475
254.079913	8000.146019	13.029658	-0.053789	4.815472
253.884345	8000.111849	13.034663	-0.053753	4.815463
253.942826	8000.158811	13.039667	-0.053765	4.815476
254.111128	8000.109273	13.044672	-0.053797	4.815461
254.251939	8000.159732	13.049677	-0.053824	4.815475
253.983513	8000.162829	13.054682	-0.053774	4.815477
253.926508	8000.173690	13.059687	-0.053764	4.815480
254.099301	8000.173383	13.064691	-0.053797	4.815479
253.892105	8000.167873	13.069696	-0.053759	4.815479
253.953580	8000.167866	13.074701	-0.053771	4.815478
253.976913	8000.204631	13.079706	-0.053776	4.815489
253.916569	8000.151320	13.084711	-0.053765	4.815474
254.049655	8000.163180	13.089715	-0.053790	4.815477
254.013479	8000.150875	13.094720	-0.053784	4.815473
253.938847	8000.145416	13.099725	-0.053771	4.815472
253.937809	8000.146515	13.104730	-0.053771	4.815472
253.913029	8000.149358	13.109735	-0.053767	4.815473
254.308420	8000.218980	13.114739	-0.053841	4.815492
254.025601	8000.172682	13.119744	-0.053789	4.815479
254.060446	8000.206432	13.124749	-0.053796	4.815489
254.256019	8000.209707	13.129754	-0.053833	4.815489
254.100393	8000.155891	13.134759	-0.053804	4.815474
253.940692	8000.196047	13.139763	-0.053775	4.815487
253.900632	8000.148414	13.144768	-0.053768	4.815473
254.058014	8000.142509	13.149773	-0.053798	4.815470
254.016079	8000.181403	13.154778	-0.053791	4.815482
253.822794	8000.206044	13.159783	-0.053755	4.815490
254.020608	8000.257443	13.164787	-0.053793	4.815504
253.928820	8000.160868	13.169792	-0.053776	4.815476
254.011770	8000.223195	13.174797	-0.053792	4.815494
253.812081	8000.206054	13.179802	-0.053755	4.815490
253.957382	8000.171098	13.184807	-0.053783	4.815479
253.995774	8000.179258	13.189811	-0.053791	4.815481
253.826455	8000.153001	13.194816	-0.053760	4.815474
254.077756	8000.155058	13.199821	-0.053807	4.815474
254.023262	8000.152069	13.204826	-0.053797	4.815473
253.919349	8000.143989	13.209831	-0.053779	4.815471
254.020651	8000.157463	13.214835	-0.053798	4.815475
253.966489	8000.126694	13.219840	-0.053788	4.815466
253.921792	8000.168748	13.224845	-0.053781	4.815478
253.942965	8000.133880	13.229850	-0.053785	4.815468
254.221852	8000.128912	13.234855	-0.053838	4.815465
254.127235	8000.166936	13.239859	-0.053820	4.815477
254.088578	8000.144973	13.244864	-0.053814	4.815471
254.091197	8000.156818	13.249869	-0.053815	4.815474
254.209863	8000.231490	13.254874	-0.053837	4.815495
253.997521	8000.146817	13.259879	-0.053798	4.815472
253.862943	8000.194868	13.264883	-0.053774	4.815486
254.067064	8000.203627	13.269888	-0.053812	4.815488
254.118603	8000.183152	13.274893	-0.053823	4.815482
253.862516	8000.208893	13.279898	-0.053775	4.815490
253.963769	8000.139014	13.284903	-0.053795	4.815469
254.156169	8000.188187	13.289907	-0.053831	4.815483
253.996793	8000.150339	13.294912	-0.053802	4.815473
253.880677	8000.200832	13.299917	-0.053781	4.815488
253.858610	8000.162044	13.304922	-0.053777	4.815477
253.947236	8000.144319	13.309927	-0.053794	4.815471
253.894748	8000.152048	13.314931	-0.053785	4.815473
253.849714	8000.148146	13.319936	-0.053777	4.815473
253.688250	8000.153009	13.324941	-0.053748	4.815475
254.024089	8000.208823	13.329946	-0.053811	4.815489
254.038742	8000.172779	13.334951	-0.053814	4.815479
254.031739	8000.253926	13.339955	-0.053813	4.815503
253.854445	8000.223262	13.344960	-0.053781	4.815494
253.830885	8000.184450	13.349965	-0.053777	4.815483
253.799811	8000.256650	13.354970	-0.053772	4.815504
253.658698	8000.195594	13.359975	-0.053746	4.815487
253.838029	8000.206081	13.364979	-0.053780	4.815489
253.852563	8000.196750	13.369984	-0.053783	4.815487
254.224433	8000.249955	13.374989	-0.053853	4.815500
253.961839	8000.271314	13.379994	-0.053805	4.815508
253.943432	8000.189841	13.384999	-0.053802	4.815484
254.050834	8000.219445	13.390003	-0.053822	4.815492
254.032596	8000.209574	13.395008	-0.053819	4.815489
253.909174	8000.184074	13.400013	-0.053797	4.815483
254.146924	8000.217966	13.405018	-0.053842	4.815491
254.120913	8000.250711	13.410023	-0.053837	4.815501
254.176030	8000.248462	13.415027	-0.053848	4.815500
254.080803	8000.221290	13.420032	-0.053831	4.815493
253.900994	8000.235467	13.425037	-0.053798	4.815498
253.953880	8000.219289	13.430042	-0.053808	4.815493
254.110704	8000.208032	13.435047	-0.053838	4.815488
254.149452	8000.256807	13.440051	-0.053846	4.815503
253.827446	8000.178872	13.445056	-0.053786	4.815481
254.102833	8000.185602	13.450061	-0.053838	4.815482
254.200483	8000.217182	13.455066	-0.053857	4.815491
253.855417	8000.215808	13.460071	-0.053793	4.815492
253.993480	8000.250192	13.465075	-0.053819	4.815501
254.128748	8000.222551	13.470080	-0.053845	4.815493
254.188124	8000.268460	13.475085	-0.053857	4.815506
253.941854	8000.266579	13.480090	-0.053811	4.815506
253.820048	8000.213321	13.485095	-0.053789	4.815491
253.939018	8000.291205	13.490099	-0.053812	4.815513
253.907591	8000.209517	13.495104	-0.053807	4.815490
253.976375	8000.247033	13.500109	-0.053820	4.815500
253.974956	8000.222478	13.505114	-0.053820	4.815493
253.849322	8000.200147	13.510119	-0.053797	4.815487
254.013455	8000.226413	13.515123	-0.053828	4.815494
253.940297	8000.173958	13.520128	-0.053815	4.815479
253.935221	8000.213460	13.525133	-0.053815	4.815491
253.926365	8000.195194	13.530138	-0.053814	4.815485
254.056019	8000.147156	13.535143	-0.053838	4.815471
254.208648	8000.196742	13.540147	-0.053867	4.815484
253.994985	8000.160135	13.545152	-0.053828	4.815475
254.067852	8000.183825	13.550157	-0.053842	4.815481
254.136311	8000.194620	13.555162	-0.053855	4.815484
253.910294	8000.184524	13.560167	-0.053814	4.815482
254.024799	8000.235618	13.565171	-0.053836	4.815497
253.870218	8000.190368	13.570176	-0.053808	4.815484
253.942550	8000.194815	13.575181	-0.053822	4.815485
253.941070	8000.232240	13.580186	-0.053822	4.815496
253.947090	8000.177886	13.585191	-0.053823	4.815480
254.017454	8000.258173	13.590195	-0.053837	4.815503
253.814139	8000.221736	13.595200	-0.053800	4.815493
253.933576	8000.210931	13.600205	-0.053823	4.815490
254.053384	8000.243946	13.605210	-0.053845	4.815499
253.896505	8000.166599	13.610215	-0.053817	4.815477
253.954500	8000.225309	13.615219	-0.053828	4.815494
253.972832	8000.178639	13.620224	-0.053832	4.815480
254.032414	8000.158297	13.625229	-0.053844	4.815474
253.876332	8000.160042	13.630234	-0.053815	4.815475
253.880264	8000.193281	13.635239	-0.053816	4.815485
254.329163	8000.199670	13.640243	-0.053900	4.815484
254.036057	8000.180986	13.645248	-0.053846	4.815480
253.997569	8000.200701	13.650253	-0.053840	4.815486
254.028585	8000.213015	13.655258	-0.053846	4.815490
254.083192	8000.169081	13.660263	-0.053857	4.815477
254.120937	8000.212496	13.665267	-0.053864	4.815489
254.037869	8000.162015	13.670272	-0.053849	4.815475
254.129235	8000.162501	13.675277	-0.053867	4.815474
254.288828	8000.213271	13.680282	-0.053897	4.815488
254.221247	8000.199379	13.685287	-0.053885	4.815485
254.251184	8000.205263	13.690291	-0.053891	4.815486
254.091483	8000.163134	13.695296	-0.053862	4.815475
254.125568	8000.166950	13.700301	-0.053869	4.815476
253.985672	8000.155070	13.705306	-0.053843	4.815473
254.121928	8000.166984	13.710311	-0.053869	4.815476
254.263082	8000.186459	13.715315	-0.053896	4.815481
254.109403	8000.167939	13.720320	-0.053868	4.815476
254.316839	8000.217362	13.725325	-0.053907	4.815489
253.932946	8000.231375	13.730330	-0.053836	4.815495
253.916631	8000.165967	13.735335	-0.053834	4.815476
254.006788	8000.212384	13.740339	-0.053851	4.815489
253.973783	8000.192651	13.745344	-0.053845	4.815484
253.993736	8000.176998	13.750349	-0.053850	4.815479
254.133678	8000.176149	13.755354	-0.053876	4.815478
254.114687	8000.179088	13.760359	-0.053873	4.815479
254.105094	8000.266605	13.765363	-0.053872	4.815505
253.955199	8000.252422	13.770368	-0.053845	4.815501
254.146550	8000.271658	13.775373	-0.053881	4.815506
254.074751	8000.257695	13.780378	-0.053868	4.815502
254.056913	8000.268134	13.785383	-0.053865	4.815505
254.303315	8000.247670	13.790387	-0.053911	4.815498
254.116938	8000.132434	13.795392	-0.053877	4.815465
254.215676	8000.182199	13.800397	-0.053896	4.815479
254.081619	8000.268730	13.805402	-0.053872	4.815505
254.227331	8000.228437	13.810407	-0.053899	4.815493
254.289035	8000.267973	13.815411	-0.053911	4.815504
254.033360	8000.228534	13.820416	-0.053864	4.815494
254.143116	8000.236805	13.825421	-0.053885	4.815496
254.190991	8000.260084	13.830426	-0.053895	4.815502
254.142458	8000.178113	13.835431	-0.053886	4.815478
254.392528	8000.239995	13.840435	-0.053933	4.815495
254.265943	8000.212304	13.845440	-0.053910	4.815488
254.210498	8000.211436	13.850445	-0.053901	4.815488
254.356181	8000.276938	13.855450	-0.053928	4.815506
254.280228	8000.274662	13.860455	-0.053915	4.815506
254.314413	8000.272068	13.865459	-0.053922	4.815505
254.208315	8000.214794	13.870464	-0.053902	4.815489
254.277814	8000.205301	13.875469	-0.053916	4.815486
254.215864	8000.258826	13.880474	-0.053905	4.815502
254.010974	8000.193510	13.885479	-0.053867	4.815483
254.177251	8000.213400	13.890483	-0.053899	4.815488
254.338319	8000.217174	13.895488	-0.053929	4.815489
254.297215	8000.205856	13.900493	-0.053922	4.815486
254.426562	8000.252922	13.905498	-0.053947	4.815499
254.307118	8000.168711	13.910503	-0.053925	4.815475
254.386695	8000.191445	13.915507	-0.053940	4.815481
254.425080	8000.171821	13.920512	-0.053948	4.815475
254.367427	8000.240378	13.925517	-0.053938	4.815495
254.398031	8000.280470	13.930522	-0.053944	4.815507
254.091983	8000.239130	13.935527	-0.053887	4.815496
254.345848	8000.264741	13.940531	-0.053935	4.815503
254.369248	8000.267312	13.945536	-0.053940	4.815503
254.232855	8000.250146	13.950541	-0.053915	4.815499
254.413836	8000.305545	13.955546	-0.053950	4.815514
254.377541	8000.215226	13.960551	-0.053943	4.815488
254.391899	8000.181313	13.965555	-0.053946	4.815478
254.347531	8000.174216	13.970560	-0.053939	4.815476
254.329286	8000.181442	13.975565	-0.053936	4.815478
254.341758	8000.214823	13.980570	-0.053939	4.815488
254.155093	8000.181866	13.985575	-0.053904	4.815479
254.299904	8000.204608	13.990579	-0.053932	4.815485
254.371712	8000.201566	13.995584	-0.053946	4.815484
254.491804	8000.228174	14.000589	-0.053969	4.815491
254.412078	8000.338045	14.005594	-0.053955	4.815523
254.307465	8000.223087	14.010599	-0.053936	4.815490
254.279104	8000.238696	14.015603	-0.053931	4.815495
254.444143	8000.223301	14.020608	-0.053962	4.815490
254.389293	8000.194657	14.025613	-0.053952	4.815482
254.268532	8000.247211	14.030618	-0.053930	4.815498
254.166392	8000.211375	14.035623	-0.053912	4.815488
254.296964	8000.230676	14.040627	-0.053937	4.815493
254.470494	8000.214353	14.045632	-0.053970	4.815487
254.345193	8000.164242	14.050637	-0.053947	4.815473
254.367912	8000.226645	14.055642	-0.053952	4.815491
254.322627	8000.204571	14.060647	-0.053944	4.815485
254.303502	8000.268421	14.065651	-0.053941	4.815503
254.257353	8000.246333	14.070656	-0.053933	4.815497
254.229931	8000.188221	14.075661	-0.053928	4.815480
254.309359	8000.208815	14.080666	-0.053943	4.815486
254.177501	8000.198135	14.085671	-0.053919	4.815483
254.182747	8000.230328	14.090675	-0.053921	4.815493
254.203280	8000.198655	14.095680	-0.053925	4.815483
254.323997	8000.188940	14.100685	-0.053948	4.815480
254.172500	8000.198240	14.105690	-0.053920	4.815483
254.157386	8000.126439	14.110695	-0.053918	4.815463
254.331504	8000.196685	14.115699	-0.053951	4.815482
254.182885	8000.192141	14.120704	-0.053924	4.815482
254.407394	8000.184139	14.125709	-0.053966	4.815478
254.343176	8000.219460	14.130714	-0.053955	4.815489
254.161392	8000.184446	14.135719	-0.053922	4.815479
254.275328	8000.203473	14.140723	-0.053943	4.815484
254.285465	8000.237883	14.145728	-0.053946	4.815494
254.183947	8000.196714	14.150733	-0.053927	4.815483
254.362252	8000.223215	14.155738	-0.053961	4.815490
254.312398	8000.174350	14.160743	-0.053952	4.815476
254.565604	8000.223461	14.165747	-0.054000	4.815489
254.285334	8000.175066	14.170752	-0.053948	4.815476
254.187035	8000.172421	14.175757	-0.053931	4.815476
254.364903	8000.249141	14.180762	-0.053964	4.815497
254.234142	8000.202146	14.185767	-0.053940	4.815484
254.200148	8000.232622	14.190771	-0.053935	4.815493
254.387132	8000.227208	14.195776	-0.053970	4.815491
254.417216	8000.221339	14.200781	-0.053976	4.815489
254.358964	8000.288818	14.205786	-0.053966	4.815509
254.365968	8000.230205	14.210791	-0.053968	4.815492
254.548394	8000.232195	14.215795	-0.054002	4.815491
254.402873	8000.195643	14.220800	-0.053975	4.815481
254.479898	8000.229021	14.225805	-0.053990	4.815491
254.472582	7999.284287	14.230810	-0.053989	4.815215

254.153161	7996.035176	14.235815	-0.053928	4.814267
254.332386	7990.611717	14.240819	-0.053958	4.812681
254.421739	7983.896720	14.245824	-0.053971	4.810717
254.189803	7976.625478	14.250829	-0.053924	4.808591
254.130210	7968.992270	14.255834	-0.053908	4.806358
254.068555	7961.192030	14.260839	-0.053892	4.804074
254.376076	7953.409731	14.265843	-0.053945	4.801793
254.211116	7945.349055	14.270848	-0.053909	4.799432
253.834824	7937.405285	14.275853	-0.053835	4.797105
254.005097	7929.396998	14.280858	-0.053862	4.794755
254.208336	7921.416459	14.285863	-0.053895	4.792412
253.969021	7913.349400	14.290867	-0.053846	4.790044
253.870035	7905.398919	14.295872	-0.053822	4.787709
253.767108	7897.369476	14.300877	-0.053799	4.785349
253.825352	7889.452410	14.305882	-0.053805	4.783021
253.577937	7881.356788	14.310887	-0.053754	4.780640
253.501579	7873.401205	14.315891	-0.053735	4.778298
253.476337	7865.384525	14.320896	-0.053726	4.775937
253.357858	7857.397092	14.325901	-0.053699	4.773584
253.561994	7849.414622	14.330906	-0.053732	4.771230
253.493720	7841.350028	14.335911	-0.053715	4.768852
253.307018	7833.453019	14.340915	-0.053675	4.766522
253.402431	7825.343514	14.345920	-0.053688	4.764128
253.648999	7817.438539	14.350925	-0.053730	4.761792
253.458795	7809.389582	14.355930	-0.053690	4.759414
253.174993	7801.367913	14.360935	-0.053632	4.757043
253.278563	7793.337933	14.365939	-0.053647	4.754667
253.230488	7785.295456	14.370944	-0.053633	4.752287
253.155910	7777.332630	14.375949	-0.053614	4.749929
252.963290	7769.337739	14.380954	-0.053574	4.747561
252.951205	7761.297259	14.385959	-0.053567	4.745178
252.818625	7753.341652	14.390963	-0.053538	4.742819
252.728539	7745.348424	14.395968	-0.053516	4.740447
252.782546	7737.339672	14.400973	-0.053522	4.738070
252.828754	7729.328544	14.405978	-0.053525	4.735690
252.854858	7721.320187	14.410983	-0.053526	4.733310
252.756703	7713.334612	14.415987	-0.053503	4.730936
252.808464	7705.278949	14.420992	-0.053508	4.728540
252.665849	7697.308423	14.425997	-0.053476	4.726168
252.621004	7689.323971	14.431002	-0.053463	4.723791
252.502249	7681.310436	14.436007	-0.053437	4.721403
252.523041	7673.337809	14.441011	-0.053436	4.719027
252.443540	7665.336957	14.446016	-0.053416	4.716641
252.587175	7657.237414	14.451021	-0.053438	4.714224
252.663604	7649.304544	14.456026	-0.053448	4.711856
252.309181	7641.235375	14.461031	-0.053377	4.709447
252.520759	7633.327288	14.466035	-0.053412	4.707083
252.206061	7625.330452	14.471040	-0.053349	4.704693
252.051453	7617.283667	14.476045	-0.053315	4.702286
252.118340	7609.337530	14.481050	-0.053323	4.699908
251.989390	7601.325261	14.486055	-0.053294	4.697509
252.002635	7593.278499	14.491059	-0.053292	4.695098
251.705860	7585.318213	14.496064	-0.053232	4.692712
251.567805	7577.272547	14.501069	-0.053202	4.690300
251.872286	7569.296181	14.506074	-0.053254	4.687906
251.813566	7561.256145	14.511079	-0.053238	4.685492
251.706857	7553.304179	14.516083	-0.053213	4.683104
251.934223	7545.316608	14.521088	-0.053251	4.680703
251.972375	7537.279113	14.526093	-0.053254	4.678286
251.691735	7529.282524	14.531098	-0.053197	4.675881
251.524134	7521.250278	14.536103	-0.053161	4.673464
251.712604	7513.162789	14.541107	-0.053191	4.671028
251.587895	7505.218921	14.546112	-0.053163	4.668634
251.461189	7497.201519	14.551117	-0.053135	4.666218
251.547302	7489.219218	14.556122	-0.053146	4.663810
251.244088	7481.219827	14.561127	-0.053085	4.661396
251.283779	7473.251833	14.566131	-0.053088	4.658991
251.291160	7465.278532	14.571136	-0.053085	4.656582
251.080881	7457.253898	14.576141	-0.053041	4.654157
250.997319	7449.267997	14.581146	-0.053020	4.651742
251.105538	7441.197103	14.586151	-0.053036	4.649300
251.275035	7433.246065	14.591155	-0.053063	4.646893
251.146243	7425.173624	14.596160	-0.053034	4.644448
250.916537	7417.250476	14.601165	-0.052987	4.642047
251.127181	7409.197634	14.606170	-0.053021	4.639605
251.209396	7401.265994	14.611175	-0.053032	4.637199
251.019739	7393.187814	14.616179	-0.052992	4.634748
251.059544	7385.217141	14.621184	-0.052995	4.632327
250.980632	7377.152867	14.626189	-0.052975	4.629877
251.039181	7369.193687	14.631194	-0.052981	4.627457
250.821602	7361.143960	14.636199	-0.052936	4.625009
250.863688	7353.217780	14.641203	-0.052939	4.622597
250.550154	7345.210414	14.646208	-0.052876	4.620159
250.460388	7337.193161	14.651213	-0.052855	4.617717
250.745072	7329.191553	14.656218	-0.052903	4.615278
250.556276	7321.152079	14.661223	-0.052863	4.612826
250.549434	7313.140463	14.666227	-0.052857	4.610382
250.509994	7305.153565	14.671232	-0.052845	4.607943
250.478596	7297.121864	14.676237	-0.052835	4.605490
250.411505	7289.212958	14.681242	-0.052818	4.603073
250.421570	7281.198948	14.686247	-0.052815	4.600623
250.558675	7273.213558	14.691251	-0.052836	4.598180
250.407406	7265.163400	14.696256	-0.052803	4.595715
250.215586	7257.104439	14.701261	-0.052762	4.593247
250.171634	7249.096497	14.706266	-0.052749	4.590793
250.064843	7241.108249	14.711271	-0.052725	4.588344
250.017292	7233.118087	14.716275	-0.052711	4.585893
250.029159	7225.165647	14.721280	-0.052709	4.583452
249.932051	7217.097782	14.726285	-0.052686	4.580975
249.976538	7209.151786	14.731290	-0.052690	4.578533
250.143089	7201.114236	14.736295	-0.052716	4.576062
249.961905	7193.115511	14.741299	-0.052678	4.573602
249.749990	7185.109097	14.746304	-0.052634	4.571138
249.727118	7177.111511	14.751309	-0.052625	4.568675
249.820972	7169.133027	14.756314	-0.052637	4.566217
249.656182	7161.128408	14.761319	-0.052602	4.563750
249.623855	7153.122598	14.766323	-0.052591	4.561280
249.704005	7145.114603	14.771328	-0.052602	4.558809
249.627392	7137.141941	14.776333	-0.052583	4.556348
249.553755	7129.142291	14.781338	-0.052564	4.553876
249.566699	7121.083999	14.786343	-0.052562	4.551385
249.654475	7113.068099	14.791347	-0.052574	4.548907
249.448565	7105.112527	14.796352	-0.052531	4.546445
249.524141	7097.079194	14.801357	-0.052540	4.543958
249.326256	7089.173671	14.806362	-0.052498	4.541508
249.242000	7081.064397	14.811367	-0.052478	4.538995
249.139068	7073.171124	14.816371	-0.052454	4.536547
249.108761	7065.104671	14.821376	-0.052444	4.534044
249.083046	7057.095946	14.826381	-0.052434	4.531558
249.172026	7049.072800	14.831386	-0.052446	4.529066
249.011133	7041.114971	14.836391	-0.052412	4.526592
249.114172	7033.064386	14.841395	-0.052426	4.524089
249.017133	7025.149052	14.846400	-0.052403	4.521626
248.990092	7017.085169	14.851405	-0.052394	4.519115
249.073584	7009.170253	14.856410	-0.052405	4.516650
248.888372	7001.072416	14.861415	-0.052365	4.514126
248.803812	6993.027441	14.866419	-0.052345	4.511617
248.879986	6985.017695	14.871424	-0.052354	4.509119
248.738914	6977.033159	14.876429	-0.052323	4.506626
248.618691	6969.034941	14.881434	-0.052296	4.504127
248.452737	6961.108523	14.886439	-0.052261	4.501649
248.543746	6953.074472	14.891443	-0.052273	4.499137
248.576212	6945.097283	14.896448	-0.052274	4.496642
248.404964	6937.036666	14.901453	-0.052238	4.494118
248.377197	6929.067984	14.906458	-0.052228	4.491622
248.266585	6920.995994	14.911463	-0.052203	4.489092
248.137650	6913.039267	14.916467	-0.052174	4.486596
248.294334	6905.006572	14.921472	-0.052198	4.484077
248.194655	6897.059498	14.926477	-0.052175	4.481582
248.232660	6889.071743	14.931482	-0.052178	4.479073
248.163990	6881.082633	14.936487	-0.052160	4.476562
248.072534	6873.046674	14.941491	-0.052138	4.474034
247.969624	6865.012448	14.946496	-0.052115	4.471506
248.040483	6857.001693	14.951501	-0.052123	4.468985
247.954819	6849.010098	14.956506	-0.052102	4.466467
247.975930	6840.976262	14.961511	-0.052102	4.463935
247.892292	6833.071930	14.966515	-0.052081	4.461442
247.833285	6825.024375	14.971520	-0.052066	4.458903
247.820413	6817.021408	14.976525	-0.052059	4.456376
247.697117	6809.048067	14.981530	-0.052031	4.453857
247.434120	6801.003032	14.986535	-0.051977	4.451313
247.530733	6792.947275	14.991539	-0.051991	4.448766
247.640523	6784.996538	14.996544	-0.052006	4.446250
247.431481	6777.000227	15.001549	-0.051963	4.443718
247.383465	6769.083268	15.006554	-0.051949	4.441210
247.581703	6761.011907	15.011559	-0.051981	4.438652
247.504950	6753.049269	15.016563	-0.051962	4.436126
247.320113	6745.001236	15.021568	-0.051923	4.433572
247.190465	6736.941418	15.026573	-0.051894	4.431012
247.318110	6728.964182	15.031578	-0.051914	4.428478
247.164224	6720.935649	15.036583	-0.051880	4.425925
247.114574	6712.946595	15.041587	-0.051866	4.423384
247.009572	6704.993382	15.046592	-0.051842	4.420852
247.102213	6696.986912	15.051597	-0.051855	4.418303
247.119823	6689.002829	15.056602	-0.051853	4.415759
246.926245	6680.974720	15.061607	-0.051813	4.413199
246.617268	6672.945331	15.066611	-0.051750	4.410636
246.778440	6664.947523	15.071616	-0.051776	4.408084
246.686081	6656.930009	15.076621	-0.051754	4.405523
246.724482	6648.986381	15.081626	-0.051756	4.402985
246.699246	6640.982968	15.086631	-0.051747	4.400426
246.776729	6632.996181	15.091635	-0.051757	4.397871
246.908617	6625.004322	15.096640	-0.051776	4.395314
246.711489	6616.957370	15.101645	-0.051735	4.392735
246.766691	6608.966404	15.106650	-0.051741	4.390175
246.716601	6600.968288	15.111655	-0.051727	4.387610
246.541328	6592.927467	15.116659	-0.051689	4.385029
246.414909	6584.978082	15.121664	-0.051661	4.382476
246.200598	6576.960153	15.126669	-0.051616	4.379899
246.190654	6569.041396	15.131674	-0.051610	4.377353
246.464357	6560.981342	15.136679	-0.051656	4.374763
246.419252	6552.973572	15.141683	-0.051643	4.372186
246.360102	6544.981475	15.146688	-0.051627	4.369612
245.962581	6536.957896	15.151693	-0.051549	4.367024
246.195529	6528.969783	15.156698	-0.051587	4.364451
246.092011	6520.966670	15.161703	-0.051563	4.361868
246.045194	6512.999149	15.166707	-0.051550	4.359296
245.930555	6505.059919	15.171712	-0.051524	4.356732
246.023002	6496.936822	15.176717	-0.051537	4.354107
246.025665	6488.866728	15.181722	-0.051532	4.351498
245.941369	6480.873665	15.186727	-0.051512	4.348911
245.925294	6472.947633	15.191731	-0.051504	4.346345
245.729856	6464.897034	15.196736	-0.051463	4.343736
245.701856	6456.942232	15.201741	-0.051453	4.341158
245.594529	6448.994808	15.206746	-0.051429	4.338580
245.611672	6440.941791	15.211751	-0.051427	4.335967
245.555244	6432.905780	15.216755	-0.051412	4.333357
245.490041	6424.943995	15.221760	-0.051395	4.330770
245.283293	6416.936327	15.226765	-0.051352	4.328165
245.462722	6408.939456	15.231770	-0.051381	4.325565
245.284863	6400.956226	15.236775	-0.051343	4.322965
245.402978	6392.947284	15.241779	-0.051360	4.320358
245.414040	6384.955135	15.246784	-0.051358	4.317753
245.249577	6376.946925	15.251789	-0.051322	4.315141
245.327668	6368.920844	15.256794	-0.051332	4.312523
245.399561	6360.876811	15.261799	-0.051341	4.309897
245.267293	6352.929374	15.266803	-0.051312	4.307300
245.003452	6344.901092	15.271808	-0.051258	4.304674
244.974050	6336.935231	15.276813	-0.051248	4.302068
245.268300	6328.925452	15.281818	-0.051298	4.299449
244.990658	6320.902804	15.286823	-0.051241	4.296820
244.985843	6312.910928	15.291827	-0.051236	4.294201
244.980992	6304.906801	15.296832	-0.051230	4.291577
244.828460	6296.880790	15.301837	-0.051197	4.288942
244.653167	6288.927848	15.306842	-0.051160	4.286330
244.625526	6280.870656	15.311847	-0.051150	4.283683
244.668281	6272.955315	15.316851	-0.051153	4.281082
244.485508	6264.901537	15.321856	-0.051114	4.278432
244.240440	6256.891418	15.326861	-0.051064	4.275794
244.469521	6248.877861	15.331866	-0.051102	4.273157
244.433292	6240.819254	15.336871	-0.051091	4.270501
244.505940	6232.888720	15.341875	-0.051099	4.267887
244.508377	6224.868384	15.346880	-0.051095	4.265241
244.360729	6216.921325	15.351885	-0.051063	4.262617
244.418350	6208.875447	15.356890	-0.051069	4.259960
244.413707	6200.946737	15.361895	-0.051064	4.257339
244.181150	6192.895123	15.366899	-0.051016	4.254674
244.099011	6184.914317	15.371904	-0.050996	4.252032
243.796786	6176.834321	15.376909	-0.050935	4.249354
244.004534	6168.905477	15.381914	-0.050969	4.246729
244.063534	6160.839723	15.386919	-0.050975	4.244055
243.772486	6152.949778	15.391923	-0.050916	4.241435
243.857286	6144.915952	15.396928	-0.050927	4.238768
243.855754	6136.929084	15.401933	-0.050922	4.236115
243.982217	6128.900348	15.406938	-0.050941	4.233448
243.870495	6120.876026	15.411943	-0.050916	4.230778
243.924130	6112.883881	15.416947	-0.050921	4.228119
243.621933	6104.938130	15.421952	-0.050860	4.225470
243.554546	6096.919365	15.426957	-0.050843	4.222797
243.660765	6088.970743	15.431962	-0.050858	4.220148
243.637770	6080.911215	15.436967	-0.050849	4.217458
243.531620	6072.926658	15.441971	-0.050824	4.214791
243.421359	6064.904355	15.446976	-0.050799	4.212110
243.361575	6056.891271	15.451981	-0.050783	4.209431
243.438964	6048.931353	15.456986	-0.050793	4.206769
243.264373	6040.919904	15.461991	-0.050756	4.204086
243.072133	6032.996198	15.466995	-0.050715	4.201430
243.361502	6024.898607	15.472000	-0.050765	4.198719
243.048935	6016.944223	15.477005	-0.050702	4.196048
243.280037	6008.892236	15.482010	-0.050740	4.193349
243.101262	6000.773844	15.487015	-0.050702	4.190621
243.117502	5992.806887	15.492019	-0.050700	4.187944
243.125665	5984.864777	15.497024	-0.050697	4.185273
243.132105	5976.898110	15.502029	-0.050694	4.182593
242.950078	5968.930660	15.507034	-0.050655	4.179909
242.710197	5960.898048	15.512039	-0.050606	4.177200
242.901297	5952.867612	15.517043	-0.050637	4.174495
242.881256	5944.884489	15.522048	-0.050628	4.171802
242.642601	5936.868542	15.527053	-0.050579	4.169094
242.726817	5928.926511	15.532058	-0.050590	4.166413
242.778484	5920.882625	15.537063	-0.050595	4.163695
242.530032	5912.933554	15.542067	-0.050544	4.161003
242.600132	5904.915197	15.547072	-0.050553	4.158291
242.445083	5896.882150	15.552077	-0.050519	4.155569
242.363073	5888.879540	15.557082	-0.050499	4.152856
242.242820	5880.837509	15.562087	-0.050472	4.150128
242.162025	5872.861988	15.567091	-0.050452	4.147420
242.204945	5864.839561	15.572096	-0.050456	4.144697
242.056417	5856.897147	15.577101	-0.050423	4.141997
242.157122	5848.854722	15.582106	-0.050437	4.139264
242.025244	5840.885525	15.587111	-0.050408	4.136551
242.074308	5832.889437	15.592115	-0.050412	4.133830
241.975073	5824.875563	15.597120	-0.050389	4.131099
242.046796	5816.835184	15.602125	-0.050398	4.128359
242.001735	5808.882160	15.607130	-0.050385	4.125645
241.597587	5800.902782	15.612135	-0.050305	4.122917
241.755959	5792.874275	15.617139	-0.050330	4.120177
241.915004	5784.893028	15.622144	-0.050355	4.117451
241.788437	5776.888429	15.627149	-0.050326	4.114712
241.611018	5768.899333	15.632154	-0.050289	4.111975
241.665662	5760.835803	15.637159	-0.050294	4.109214
241.701896	5752.837568	15.642163	-0.050296	4.106474
241.512596	5744.859626	15.647168	-0.050256	4.103736
241.631694	5736.861643	15.652173	-0.050274	4.100993
241.728043	5728.866208	15.657178	-0.050287	4.098248
241.561697	5720.887163	15.662183	-0.050251	4.095504
241.585851	5712.897060	15.667187	-0.050251	4.092757
241.747231	5704.862512	15.672192	-0.050277	4.089995
241.228001	5696.903559	15.677197	-0.050175	4.087248
241.420609	5688.891298	15.682202	-0.050206	4.084490
241.489081	5680.926409	15.687207	-0.050215	4.081744
241.448514	5672.857223	15.692211	-0.050202	4.078960
241.351390	5664.928717	15.697216	-0.050180	4.076221
241.086952	5656.891267	15.702221	-0.050126	4.073441
241.199764	5648.892920	15.707226	-0.050142	4.070677
240.771086	5640.923760	15.712231	-0.050057	4.067914
240.837345	5632.894926	15.717235	-0.050065	4.065136
241.051678	5624.948371	15.722240	-0.050100	4.062386
240.983613	5616.935921	15.727245	-0.050083	4.059607
240.808349	5608.952321	15.732250	-0.050046	4.056835
240.763511	5600.905901	15.737255	-0.050033	4.054041
240.835219	5592.899715	15.742259	-0.050041	4.051261
240.878605	5584.916349	15.747264	-0.050045	4.048487
240.522619	5576.896966	15.752269	-0.049974	4.045692
240.829885	5568.933187	15.757274	-0.050026	4.042924
240.652145	5560.930868	15.762279	-0.049988	4.040134
240.636148	5552.945151	15.767283	-0.049981	4.037350
240.666070	5544.931668	15.772288	-0.049982	4.034555
240.542688	5536.810539	15.777293	-0.049954	4.031719
240.315155	5528.857834	15.782298	-0.049907	4.028937
240.382743	5520.846095	15.787303	-0.049915	4.026138
240.455124	5512.864678	15.792307	-0.049924	4.023347
240.165911	5504.892169	15.797312	-0.049865	4.020552
240.146215	5496.892953	15.802317	-0.049857	4.017750
240.099517	5488.898748	15.807322	-0.049843	4.014947
239.968702	5480.895209	15.812327	-0.049814	4.012137
239.828109	5472.848876	15.817331	-0.049783	4.009311
239.897142	5464.910819	15.822336	-0.049792	4.006523
239.968995	5456.870709	15.827341	-0.049800	4.003698
239.840273	5448.905657	15.832346	-0.049772	4.000894
239.763649	5440.898666	15.837351	-0.049753	3.998074
239.694256	5432.898804	15.842355	-0.049735	3.995255
239.736020	5424.892445	15.847360	-0.049738	3.992434
239.718321	5416.831659	15.852365	-0.049730	3.989590
239.722527	5408.904694	15.857370	-0.049726	3.986792
239.693562	5400.881477	15.862375	-0.049716	3.983957
239.281453	5392.946293	15.867379	-0.049635	3.981145
239.549980	5384.942690	15.872384	-0.049680	3.978318
239.331012	5376.915571	15.877389	-0.049635	3.975472
239.369559	5368.937641	15.882394	-0.049637	3.972647
239.334553	5360.873793	15.887399	-0.049626	3.969787
239.232153	5352.918382	15.892403	-0.049602	3.966963
239.157230	5344.941881	15.897408	-0.049584	3.964130
239.101726	5336.985999	15.902413	-0.049569	3.961302
239.227129	5328.953383	15.907418	-0.049587	3.958448
239.199784	5320.961089	15.912423	-0.049577	3.955604
238.847011	5312.907095	15.917427	-0.049507	3.952730
239.023889	5304.898108	15.922432	-0.049535	3.949880
238.942101	5296.929373	15.927437	-0.049515	3.947037
238.804494	5288.942925	15.932442	-0.049485	3.944185
238.895741	5280.975499	15.937447	-0.049497	3.941341
238.830091	5272.954316	15.942451	-0.049481	3.938474
238.983711	5264.958651	15.947456	-0.049504	3.935617
238.826558	5256.935407	15.952461	-0.049470	3.932743
238.657660	5248.951802	15.957466	-0.049434	3.929881
238.420442	5240.974044	15.962471	-0.049386	3.927017
238.526217	5232.957921	15.967475	-0.049401	3.924144
238.590799	5224.996669	15.972480	-0.049408	3.921288
238.498819	5216.968359	15.977485	-0.049386	3.918402
238.282117	5209.012282	15.982490	-0.049341	3.915538
238.212303	5200.938340	15.987495	-0.049323	3.912633
238.154548	5192.929628	15.992499	-0.049308	3.909749
238.170536	5184.967228	15.997504	-0.049306	3.906880
238.100881	5176.930281	16.002509	-0.049289	3.903982
238.235662	5168.995095	16.007514	-0.049309	3.901121
238.310180	5160.972017	16.012519	-0.049318	3.898226
237.955804	5152.979084	16.017523	-0.049247	3.895331
237.887857	5145.000481	16.022528	-0.049230	3.892445
238.088032	5136.922255	16.027533	-0.049263	3.889526
238.255587	5128.964636	16.032538	-0.049289	3.886647
237.859224	5120.984287	16.037543	-0.049211	3.883747
237.823738	5112.997689	16.042547	-0.049199	3.880850
237.880852	5104.984600	16.047552	-0.049205	3.877943
237.866325	5096.983072	16.052557	-0.049198	3.875036
237.481920	5088.797180	16.057562	-0.049122	3.872053
237.523201	5080.801457	16.062567	-0.049125	3.869145
237.444551	5072.864544	16.067571	-0.049105	3.866254
237.541918	5064.900019	16.072576	-0.049119	3.863355
237.566649	5056.924872	16.077581	-0.049119	3.860448
237.476326	5048.962048	16.082586	-0.049097	3.857540
237.401797	5040.940302	16.087591	-0.049079	3.854610
237.390211	5032.944269	16.092595	-0.049072	3.851687
237.457137	5024.964462	16.097600	-0.049080	3.848771
237.332243	5016.953618	16.102605	-0.049052	3.845836
237.365438	5009.022758	16.107610	-0.049053	3.842932
237.286924	5000.994318	16.112615	-0.049034	3.839988
237.056453	4993.035078	16.117619	-0.048986	3.837063
237.066217	4985.039537	16.122624	-0.048984	3.834128
237.058405	4976.998451	16.127629	-0.048977	3.831174
237.165318	4969.008827	16.132634	-0.048993	3.828239
236.849679	4960.981553	16.137639	-0.048929	3.825278
236.970921	4953.022061	16.142643	-0.048947	3.822350
236.834546	4945.050397	16.147648	-0.048917	3.819409
236.600475	4937.064337	16.152653	-0.048869	3.816459
236.527706	4929.041408	16.157658	-0.048850	3.813496
236.660619	4921.011125	16.162663	-0.048870	3.810533
236.540297	4913.033862	16.167667	-0.048843	3.807581
236.643875	4905.046386	16.172672	-0.048858	3.804629
236.584336	4897.105820	16.177677	-0.048842	3.801687
236.501064	4889.097025	16.182682	-0.048822	3.798718
236.343497	4881.079562	16.187687	-0.048788	3.795741
236.330805	4873.017840	16.192691	-0.048781	3.792749
236.428513	4865.038277	16.197696	-0.048795	3.789788
236.162214	4857.023635	16.202701	-0.048740	3.786803
236.427961	4849.050743	16.207706	-0.048785	3.783843
236.072451	4841.082675	16.212711	-0.048714	3.780869
235.934474	4833.081985	16.217715	-0.048684	3.777885
236.039778	4825.072998	16.222720	-0.048699	3.774901
235.955290	4817.052526	16.227725	-0.048678	3.771906
235.925000	4809.063584	16.232730	-0.048668	3.768921
235.795136	4801.042805	16.237735	-0.048639	3.765920
235.828672	4793.081896	16.242739	-0.048641	3.762943
235.937310	4785.070989	16.247744	-0.048656	3.759947
235.703574	4777.086655	16.252749	-0.048608	3.756950
235.719236	4769.090079	16.257754	-0.048606	3.753952
235.647582	4761.062883	16.262759	-0.048588	3.750938
235.618152	4753.052849	16.267763	-0.048578	3.747929
235.676780	4745.048761	16.272768	-0.048584	3.744922
235.558519	4737.096149	16.277773	-0.048558	3.741928
235.593314	4729.082340	16.282778	-0.048559	3.738911
235.400342	4721.135690	16.287783	-0.048519	3.735913
235.468332	4713.091329	16.292787	-0.048527	3.732881
235.472363	4705.079850	16.297792	-0.048523	3.729858
235.209329	4697.090165	16.302797	-0.048469	3.726834
235.053731	4689.131618	16.307802	-0.048436	3.723821
235.035292	4681.177426	16.312807	-0.048427	3.720812
235.025065	4673.152504	16.317811	-0.048421	3.717773
235.150636	4665.183903	16.322816	-0.048440	3.714757
235.038044	4657.086481	16.327821	-0.048414	3.711683
235.162030	4649.069332	16.332826	-0.048432	3.708643
234.881349	4641.091503	16.337831	-0.048375	3.705606
234.869920	4633.140602	16.342835	-0.048369	3.702583
234.764506	4625.155581	16.347840	-0.048344	3.699542
234.523506	4617.158180	16.352845	-0.048295	3.696491
234.632517	4609.190393	16.357850	-0.048310	3.693457
234.515706	4601.160513	16.362855	-0.048284	3.690391
234.538185	4593.162507	16.367859	-0.048283	3.687338
234.380322	4585.169983	16.372864	-0.048249	3.684280
234.382866	4577.208617	16.377869	-0.048245	3.681236
234.580434	4569.209060	16.382874	-0.048277	3.678180
234.262277	4561.227678	16.387879	-0.048213	3.675114
234.178498	4553.176358	16.392883	-0.048193	3.672026
234.414951	4545.152653	16.397888	-0.048232	3.668954
234.256225	4537.174363	16.402893	-0.048198	3.665886
234.439997	4529.201626	16.407898	-0.048228	3.662827
234.363991	4521.197894	16.412903	-0.048209	3.659746
234.299588	4513.247167	16.417907	-0.048192	3.656684
234.242939	4505.214321	16.422912	-0.048177	3.653587
234.121381	4497.200841	16.427917	-0.048150	3.650494
234.047232	4489.220073	16.432922	-0.048131	3.647412
234.022115	4481.212829	16.437927	-0.048122	3.644318
233.911176	4473.264322	16.442931	-0.048096	3.641243
234.096794	4465.265810	16.447936	-0.048126	3.638153
234.013090	4457.253182	16.452941	-0.048106	3.635048
233.705432	4449.250919	16.457946	-0.048044	3.631938
233.581867	4441.242026	16.462951	-0.048016	3.628828
233.671547	4433.228382	16.467955	-0.048028	3.625719
233.828589	4425.250587	16.472960	-0.048053	3.622623
233.478483	4417.220480	16.477965	-0.047983	3.619490
233.547663	4409.300239	16.482970	-0.047991	3.616409
233.474497	4401.278224	16.487975	-0.047973	3.613282
233.467533	4393.279313	16.492979	-0.047967	3.610163
233.350564	4385.331914	16.497984	-0.047941	3.607058
233.356634	4377.276400	16.502989	-0.047937	3.603912
233.104972	4369.338913	16.507994	-0.047885	3.600801
233.305573	4361.318609	16.512999	-0.047918	3.597669
233.143279	4353.334436	16.518003	-0.047883	3.594537
233.147930	4345.332547	16.523008	-0.047879	3.591401
232.733790	4337.326507	16.528013	-0.047798	3.588249
232.764239	4329.341621	16.533018	-0.047799	3.585114
232.762848	4321.374754	16.538023	-0.047794	3.581983
232.763286	4313.363951	16.543027	-0.047789	3.578832
232.835717	4305.405685	16.548032	-0.047798	3.575701
232.749106	4297.347994	16.553037	-0.047777	3.572523
232.686204	4289.342460	16.558042	-0.047761	3.569364
232.878820	4281.395619	16.563047	-0.047792	3.566233
232.610816	4273.396425	16.568051	-0.047737	3.563065
232.607407	4265.407013	16.573056	-0.047732	3.559905
232.654056	4257.419415	16.578061	-0.047736	3.556745
232.539378	4249.394167	16.583066	-0.047710	3.553562
232.475588	4241.290527	16.588071	-0.047693	3.550347
232.280922	4233.333772	16.593075	-0.047652	3.547184
232.547536	4225.352815	16.598080	-0.047697	3.544022
232.190816	4217.393472	16.603085	-0.047626	3.540847
232.070445	4209.400122	16.608090	-0.047599	3.537662
232.171536	4201.397321	16.613095	-0.047613	3.534478
232.222360	4193.362440	16.618099	-0.047618	3.531276
232.085782	4185.403782	16.623104	-0.047588	3.528096
231.751255	4177.398657	16.628109	-0.047521	3.524889
231.892754	4169.445095	16.633114	-0.047543	3.521714
232.122103	4161.437339	16.638119	-0.047581	3.518517
231.950902	4153.445627	16.643123	-0.047544	3.515311
231.678307	4145.455840	16.648128	-0.047489	3.512100
231.642972	4137.441221	16.653133	-0.047477	3.508884
231.760223	4129.447060	16.658138	-0.047495	3.505677
231.617976	4121.498876	16.663143	-0.047463	3.502478
231.563817	4113.480606	16.668147	-0.047449	3.499251
231.700171	4105.530115	16.673152	-0.047469	3.496053
231.437699	4097.507218	16.678157	-0.047416	3.492811
231.390012	4089.503728	16.683162	-0.047402	3.489581
231.481753	4081.529980	16.688167	-0.047415	3.486364
231.278383	4073.537319	16.693171	-0.047372	3.483127
231.354147	4065.584974	16.698176	-0.047382	3.479913
231.413586	4057.581126	16.703181	-0.047388	3.476673
231.289757	4049.573037	16.708186	-0.047360	3.473424
231.003124	4041.559263	16.713191	-0.047302	3.470163
231.072424	4033.522553	16.718195	-0.047310	3.466902
231.229017	4025.553213	16.723200	-0.047335	3.463668
230.974673	4017.573455	16.728205	-0.047283	3.460413
231.119523	4009.590812	16.733210	-0.047305	3.457167
231.253353	4001.582803	16.738215	-0.047325	3.453908
230.994722	3993.548102	16.743219	-0.047272	3.450621
230.986587	3985.614061	16.748224	-0.047266	3.447381
230.848552	3977.585009	16.753229	-0.047236	3.444094
230.932497	3969.637978	16.758234	-0.047247	3.440846
230.921786	3961.639057	16.763239	-0.047240	3.437569
230.815798	3953.615948	16.768243	-0.047216	3.434277
230.782347	3945.631927	16.773248	-0.047205	3.431000
230.666108	3937.610665	16.778253	-0.047179	3.427701
230.575661	3929.638330	16.783258	-0.047157	3.424421
230.429570	3921.695695	16.788263	-0.047125	3.421147
230.266052	3913.664446	16.793267	-0.047090	3.417834
230.347152	3905.699569	16.798272	-0.047100	3.414552
230.251602	3897.673013	16.803277	-0.047078	3.411237
230.289011	3889.705970	16.808282	-0.047080	3.407947
230.233303	3881.688701	16.813287	-0.047065	3.404629
230.283899	3873.733737	16.818291	-0.047070	3.401339
230.256475	3865.771883	16.823296	-0.047060	3.398039
229.995946	3857.755291	16.828301	-0.047007	3.394705
229.969252	3849.681969	16.833306	-0.046997	3.391353
230.158444	3841.665311	16.838311	-0.047028	3.388028
230.073268	3833.661573	16.843315	-0.047007	3.384696
229.881077	3825.783476	16.848320	-0.046967	3.381409
229.769923	3817.761764	16.853325	-0.046941	3.378062
229.721648	3809.806295	16.858330	-0.046928	3.374742
229.362187	3801.829126	16.863335	-0.046856	3.371398
229.374416	3793.780563	16.868339	-0.046854	3.368034
229.519708	3785.768930	16.873344	-0.046876	3.364687
229.383550	3777.810183	16.878349	-0.046846	3.361348
229.323165	3769.849180	16.883354	-0.046830	3.358008
229.360794	3761.849030	16.888359	-0.046833	3.354652
229.342886	3753.795557	16.893363	-0.046825	3.351268
229.156807	3745.840456	16.898368	-0.046785	3.347916
229.140425	3737.822372	16.903373	-0.046777	3.344540
229.120723	3729.862297	16.908378	-0.046769	3.341185
228.985707	3721.884018	16.913383	-0.046739	3.337815
229.053264	3713.888801	16.918387	-0.046747	3.334442
229.033477	3705.893041	16.923392	-0.046739	3.331062
228.788728	3697.888985	16.928397	-0.046689	3.327666
228.627893	3689.907214	16.933402	-0.046654	3.324280
228.868017	3681.927070	16.938407	-0.046694	3.320905
228.910478	3673.923834	16.943411	-0.046697	3.317511
228.810096	3665.953152	16.948416	-0.046674	3.314121
228.551085	3657.921816	16.953421	-0.046621	3.310696
228.731036	3649.940573	16.958426	-0.046650	3.307305
228.636836	3641.955214	16.963431	-0.046628	3.303898
228.399458	3634.008462	16.968435	-0.046579	3.300499
228.377434	3626.022999	16.973440	-0.046570	3.297089
228.382684	3617.992273	16.978445	-0.046566	3.293656
228.227971	3610.005423	16.983450	-0.046533	3.290232
228.350865	3602.015834	16.988455	-0.046551	3.286815
228.408549	3594.011997	16.993459	-0.046557	3.283385
228.398082	3586.048096	16.998464	-0.046550	3.279966
228.366391	3578.077727	17.003469	-0.046540	3.276540
228.288844	3570.057488	17.008474	-0.046521	3.273087
228.072515	3562.054746	17.013479	-0.046476	3.269632
228.003124	3554.069622	17.018483	-0.046458	3.266188
228.381553	3546.058582	17.023488	-0.046524	3.262746
228.114978	3538.085210	17.028493	-0.046470	3.259291
227.637465	3530.190994	17.033498	-0.046376	3.255858
227.664388	3522.128529	17.038503	-0.046376	3.252369
227.668125	3514.125800	17.043507	-0.046372	3.248901
227.685078	3506.149816	17.048512	-0.046371	3.245442
227.619961	3498.163335	17.053517	-0.046354	3.241971
227.738650	3490.162671	17.058522	-0.046371	3.238497
227.689703	3482.189683	17.063527	-0.046358	3.235025
227.686681	3474.112153	17.068531	-0.046352	3.231506
227.691417	3466.123540	17.073536	-0.046349	3.228022
227.569050	3458.131844	17.078541	-0.046321	3.224527
227.494115	3450.188691	17.083546	-0.046303	3.221052
227.438092	3442.223851	17.088551	-0.046287	3.217564
227.404692	3434.232786	17.093555	-0.046277	3.214062
227.303138	3426.237658	17.098560	-0.046253	3.210552
227.144931	3418.260938	17.103565	-0.046219	3.207044
227.090514	3410.278950	17.108570	-0.046204	3.203533
227.072564	3402.297319	17.113575	-0.046196	3.200021
227.042339	3394.319962	17.118579	-0.046186	3.196506
227.103211	3386.325745	17.123584	-0.046192	3.192983
226.804046	3378.299733	17.128589	-0.046132	3.189427
226.745096	3370.310701	17.133594	-0.046116	3.185894
226.883928	3362.348298	17.138599	-0.046137	3.182377
226.850382	3354.346358	17.143603	-0.046127	3.178832
226.861337	3346.399751	17.148608	-0.046124	3.175308
226.541746	3338.371498	17.153613	-0.046060	3.171731
226.859006	3330.336632	17.158618	-0.046114	3.168174
226.626967	3322.398822	17.163623	-0.046066	3.164632
226.475651	3314.436973	17.168627	-0.046033	3.161079
226.347754	3306.483278	17.173632	-0.046005	3.157527
226.462370	3298.448608	17.178637	-0.046022	3.153945
226.312935	3290.413145	17.183642	-0.045989	3.150347
226.402472	3282.447972	17.188647	-0.046001	3.146787
226.097306	3274.444725	17.193651	-0.045940	3.143189
226.253197	3266.481421	17.198656	-0.045964	3.139624
226.156910	3258.523368	17.203661	-0.045941	3.136047
225.975629	3250.522421	17.208666	-0.045903	3.132443
226.181371	3242.500227	17.213671	-0.045936	3.128842
226.021418	3234.505995	17.218675	-0.045902	3.125233
226.024476	3226.569960	17.223680	-0.045898	3.121654
225.833821	3218.612499	17.228685	-0.045858	3.118052
225.751493	3210.618362	17.233690	-0.045838	3.114434
225.817903	3202.606334	17.238695	-0.045845	3.110811
225.810775	3194.586849	17.243699	-0.045839	3.107177
225.660574	3186.628195	17.248704	-0.045807	3.103559
225.627300	3178.653444	17.253709	-0.045796	3.099935
225.580661	3170.679772	17.258714	-0.045783	3.096307
225.734015	3162.670000	17.263719	-0.045806	3.092668
225.576567	3154.641347	17.268723	-0.045772	3.089001
225.430445	3146.714829	17.273728	-0.045741	3.085377
225.302520	3138.739180	17.278733	-0.045712	3.081727
225.371592	3130.759901	17.283738	-0.045720	3.078080
225.445978	3122.759530	17.288743	-0.045729	3.074420
225.186069	3114.685621	17.293747	-0.045676	3.070705
225.082405	3106.739575	17.298752	-0.045652	3.067053
224.967980	3098.746449	17.303757	-0.045626	3.063373
225.212897	3090.744526	17.308762	-0.045667	3.059702
225.273836	3082.806154	17.313767	-0.045674	3.056048
225.034892	3074.797797	17.318771	-0.045625	3.052342
224.948384	3066.837646	17.323776	-0.045604	3.048662
224.949709	3058.835592	17.328781	-0.045600	3.044962
224.922463	3050.882606	17.333786	-0.045590	3.041278
224.835179	3042.927307	17.338791	-0.045569	3.037587
224.802631	3034.894708	17.343795	-0.045558	3.033857
224.867550	3026.882025	17.348800	-0.045566	3.030137
224.588739	3018.939054	17.353805	-0.045509	3.026428
224.447684	3010.964813	17.358810	-0.045478	3.022706
224.431913	3002.989389	17.363815	-0.045471	3.018986
224.278518	2995.007470	17.368819	-0.045437	3.015251
224.494869	2986.993427	17.373824	-0.045473	3.011515
224.224202	2979.006372	17.378829	-0.045418	3.007762
224.221146	2971.028561	17.383834	-0.045413	3.004023
224.207189	2963.081114	17.388839	-0.045405	3.000292
224.292941	2955.081906	17.393843	-0.045417	2.996538
224.157781	2947.077585	17.398848	-0.045387	2.992765
224.028979	2939.082754	17.403853	-0.045358	2.988993
224.158505	2931.077272	17.408858	-0.045378	2.985223
224.163379	2923.108965	17.413863	-0.045374	2.981460
223.843368	2915.155644	17.418867	-0.045310	2.977683
223.821348	2907.199221	17.423872	-0.045301	2.973915
223.824957	2899.165916	17.428877	-0.045297	2.970107
223.667217	2891.212778	17.433882	-0.045263	2.966323
223.568520	2883.239901	17.438887	-0.045240	2.962529
223.407579	2875.243338	17.443891	-0.045205	2.958715
223.543292	2867.266463	17.448896	-0.045226	2.954921
223.346912	2859.260402	17.453901	-0.045184	2.951091
223.254786	2851.273811	17.458906	-0.045163	2.947270
223.573160	2843.294908	17.463911	-0.045217	2.943470
223.173853	2835.332354	17.468915	-0.045138	2.939635
223.214488	2827.371617	17.473920	-0.045141	2.935819
223.165214	2819.364734	17.478925	-0.045127	2.931971
223.262607	2811.340714	17.483930	-0.045141	2.928118
223.092777	2803.391389	17.488935	-0.045104	2.924281
223.053684	2795.417569	17.493939	-0.045092	2.920435
223.079834	2787.471032	17.498944	-0.045093	2.916600
222.988994	2779.416129	17.503949	-0.045071	2.912701
222.906897	2771.393653	17.508954	-0.045051	2.908813
222.789577	2763.441824	17.513959	-0.045024	2.904952
222.654895	2755.487761	17.518963	-0.044995	2.901084
222.652386	2747.518202	17.523968	-0.044990	2.897211
222.587214	2739.525217	17.528973	-0.044973	2.893318
222.686073	2731.516497	17.533978	-0.044987	2.889420
222.694113	2723.556756	17.538983	-0.044983	2.885536
222.615635	2715.585440	17.543987	-0.044964	2.881637
222.704071	2707.628010	17.548992	-0.044976	2.877748
222.617435	2699.637181	17.553997	-0.044955	2.873828
222.390749	2691.644367	17.559002	-0.044908	2.869894
222.364247	2683.658597	17.564007	-0.044899	2.865969
222.350030	2675.688107	17.569011	-0.044891	2.862047
222.198194	2667.740236	17.574016	-0.044858	2.858123
222.062416	2659.769933	17.579021	-0.044828	2.854183
222.072167	2651.748174	17.584026	-0.044826	2.850221
222.010249	2643.798642	17.589031	-0.044809	2.846285
222.018569	2635.789206	17.594035	-0.044806	2.842317
221.968225	2627.848543	17.599040	-0.044792	2.838375
221.865794	2619.864573	17.604045	-0.044768	2.834403
221.605909	2611.865886	17.609050	-0.044715	2.830409
221.723712	2603.886264	17.614055	-0.044733	2.826440
221.695539	2595.891317	17.619059	-0.044723	2.822450
221.586295	2587.930083	17.624064	-0.044698	2.818466
221.498679	2579.957106	17.629069	-0.044677	2.814472
221.671990	2571.919447	17.634074	-0.044704	2.810455
221.628180	2563.983447	17.639079	-0.044691	2.806471
221.458981	2556.018551	17.644083	-0.044655	2.802459
221.395189	2548.080263	17.649088	-0.044639	2.798461
221.325780	2540.092710	17.654093	-0.044621	2.794432
221.115672	2532.086644	17.659098	-0.044577	2.790380
221.282102	2524.091232	17.664103	-0.044604	2.786349
221.244369	2516.118076	17.669107	-0.044592	2.782312
221.102456	2508.171715	17.674112	-0.044561	2.778276
220.969628	2500.204572	17.679117	-0.044532	2.774224
221.003667	2492.189761	17.684122	-0.044533	2.770152
221.016898	2484.228979	17.689127	-0.044531	2.766100
220.837348	2476.249815	17.694131	-0.044493	2.762022
220.861718	2468.317870	17.699136	-0.044493	2.757973
220.852243	2460.310017	17.704141	-0.044486	2.753878
220.867745	2452.231943	17.709146	-0.044484	2.749743
220.568841	2444.318663	17.714151	-0.044424	2.745666
220.665607	2436.316501	17.719155	-0.044438	2.741562
220.476107	2428.403196	17.724160	-0.044398	2.737480
220.315862	2420.409920	17.729165	-0.044363	2.733352
220.366138	2412.411674	17.734170	-0.044368	2.729229
220.319692	2404.465360	17.739175	-0.044354	2.725120
220.120755	2396.516060	17.744179	-0.044313	2.720994
220.176921	2388.541875	17.749184	-0.044319	2.716864
220.070883	2380.540264	17.754189	-0.044294	2.712704
220.101601	2372.538818	17.759194	-0.044295	2.708546
219.917967	2364.603490	17.764199	-0.044256	2.704403
220.029081	2356.603760	17.769203	-0.044272	2.700238
219.945690	2348.666572	17.774208	-0.044252	2.696088
219.944461	2340.667945	17.779213	-0.044247	2.691904
219.705581	2332.693750	17.784218	-0.044198	2.687711
219.829423	2324.725160	17.789223	-0.044217	2.683537
219.630076	2316.765863	17.794227	-0.044175	2.679342
219.749554	2308.816646	17.799232	-0.044192	2.675165
219.611200	2300.789185	17.804237	-0.044162	2.670924
219.498161	2292.796873	17.809242	-0.044136	2.666697
219.585154	2284.854863	17.814247	-0.044148	2.662502
219.322689	2276.897279	17.819251	-0.044094	2.658270
219.267222	2268.946037	17.824256	-0.044079	2.654048
219.373636	2260.919280	17.829261	-0.044094	2.649789
219.244697	2252.963802	17.834266	-0.044066	2.645546
219.108424	2245.030249	17.839271	-0.044036	2.641308
218.940270	2237.058512	17.844275	-0.044000	2.637040
219.059853	2229.071921	17.849280	-0.044017	2.632776
219.074324	2221.063994	17.854285	-0.044015	2.628487
218.735635	2213.117691	17.859290	-0.043948	2.624201
218.735684	2205.165869	17.864295	-0.043943	2.619927
218.668290	2197.193947	17.869299	-0.043926	2.615631
218.924697	2189.179929	17.874304	-0.043969	2.611327
218.725257	2181.224658	17.879309	-0.043927	2.607016
218.623816	2173.264690	17.884314	-0.043903	2.602703
218.687291	2165.312950	17.889319	-0.043911	2.598398
218.615556	2157.316239	17.894323	-0.043892	2.594052
218.738447	2149.155455	17.899328	-0.043911	2.589623
218.468801	2141.243560	17.904333	-0.043856	2.585296
218.278194	2133.317141	17.909338	-0.043816	2.580958
218.413490	2125.369483	17.914343	-0.043836	2.576624
218.315184	2117.396986	17.919347	-0.043813	2.572253
218.213978	2109.444716	17.924352	-0.043790	2.567885
218.169964	2101.499379	17.929357	-0.043777	2.563518
217.937811	2093.571829	17.934362	-0.043729	2.559140
218.022158	2085.607436	17.939367	-0.043740	2.554756
217.973773	2077.608519	17.944371	-0.043726	2.550336
217.966891	2069.645854	17.949376	-0.043720	2.545931
217.995287	2061.671367	17.954381	-0.043721	2.541515
217.797884	2053.725710	17.959386	-0.043680	2.537091
217.758845	2045.766248	17.964391	-0.043668	2.532663
217.620005	2037.787832	17.969395	-0.043637	2.528210
217.778298	2029.819072	17.974400	-0.043662	2.523775
217.622712	2021.879607	17.979405	-0.043628	2.519326
217.605775	2013.907769	17.984410	-0.043621	2.514861
217.600738	2005.912138	17.989415	-0.043615	2.510376
217.549995	1997.920856	17.994419	-0.043601	2.505882
217.315595	1990.006398	17.999424	-0.043553	2.501410
217.184805	1982.055795	18.004429	-0.043524	2.496916
217.127977	1974.074126	18.009434	-0.043508	2.492403
217.126857	1966.096973	18.014439	-0.043503	2.487888
216.886580	1958.162561	18.019443	-0.043454	2.483371
217.174410	1950.160402	18.024448	-0.043503	2.478847
216.997120	1942.239198	18.029453	-0.043465	2.474326
216.775240	1934.258237	18.034458	-0.043419	2.469759
216.917029	1926.274208	18.039463	-0.043441	2.465209
216.672356	1918.338419	18.044467	-0.043391	2.460650
216.656494	1910.388903	18.049472	-0.043383	2.456091
216.556671	1902.415736	18.054477	-0.043360	2.451504
216.787926	1894.402174	18.059482	-0.043398	2.446910
216.536252	1886.497811	18.064487	-0.043347	2.442334
216.424900	1878.547556	18.069491	-0.043321	2.437733
216.678356	1870.538686	18.074496	-0.043364	2.433117
216.524140	1862.529537	18.079501	-0.043331	2.428462
216.423537	1854.577065	18.084506	-0.043307	2.423834
216.385743	1846.651078	18.089511	-0.043295	2.419218
216.335830	1838.692101	18.094515	-0.043282	2.414573
216.109205	1830.749506	18.099520	-0.043235	2.409914
216.198365	1822.764699	18.104525	-0.043247	2.405247
216.235231	1814.810262	18.109530	-0.043249	2.400584
216.230272	1806.882130	18.114535	-0.043243	2.395924
215.995080	1798.909591	18.119539	-0.043195	2.391211
215.902164	1790.961372	18.124544	-0.043173	2.386514
215.865325	1783.002347	18.129549	-0.043161	2.381806
215.771938	1775.061391	18.134554	-0.043139	2.377095
215.813322	1767.088963	18.139559	-0.043142	2.372366
215.827410	1759.093062	18.144563	-0.043140	2.367612
215.680996	1751.182706	18.149568	-0.043108	2.362886
215.496406	1743.258675	18.154573	-0.043069	2.358140
215.499136	1735.266764	18.159578	-0.043065	2.353359
215.379739	1727.309682	18.164583	-0.043038	2.348578
215.277915	1719.339234	18.169587	-0.043015	2.343782
215.375172	1711.376540	18.174592	-0.043028	2.338996
215.194107	1703.448230	18.179597	-0.042990	2.334199
215.053004	1695.487553	18.184602	-0.042959	2.329375
215.086187	1687.522792	18.189607	-0.042960	2.324553
215.073084	1679.578524	18.194611	-0.042953	2.319730
214.932794	1671.655077	18.199616	-0.042923	2.314899
214.845864	1663.680834	18.204621	-0.042902	2.310031
214.945278	1655.685405	18.209626	-0.042916	2.305156
215.015355	1647.755924	18.214631	-0.042924	2.300308
214.836358	1639.820886	18.219635	-0.042886	2.295425
214.838445	1631.855603	18.224640	-0.042882	2.290529
214.820703	1623.896906	18.229645	-0.042874	2.285625
214.668990	1615.981096	18.234650	-0.042841	2.280725
214.638600	1608.043195	18.239655	-0.042831	2.275811
214.685946	1599.991484	18.244659	-0.042835	2.270823
214.680822	1592.035446	18.249664	-0.042829	2.265878
214.470143	1584.125029	18.254669	-0.042785	2.260934
214.485045	1576.173725	18.259674	-0.042783	2.255973
214.451448	1568.223951	18.264679	-0.042772	2.250997
214.238695	1560.284884	18.269683	-0.042728	2.246002
214.247526	1552.353793	18.274688	-0.042725	2.241019
214.307020	1544.401794	18.279693	-0.042732	2.236017
214.032098	1536.462925	18.284698	-0.042676	2.230983
213.922637	1528.518727	18.289703	-0.042651	2.225948
213.972966	1520.557852	18.294707	-0.042655	2.220906
213.911595	1512.631431	18.299712	-0.042639	2.215863
213.693137	1504.690823	18.304717	-0.042594	2.210787
213.691714	1496.725322	18.309722	-0.042589	2.205702
213.775402	1488.784445	18.314727	-0.042600	2.200629
213.517995	1480.871319	18.319731	-0.042547	2.195531
213.542246	1472.891062	18.324736	-0.042547	2.190404
213.538837	1464.923934	18.329741	-0.042542	2.185270
213.280721	1457.026357	18.334746	-0.042489	2.180146
213.298277	1449.080189	18.339751	-0.042488	2.175004
213.131668	1441.123706	18.344755	-0.042452	2.169826
213.312484	1433.157463	18.349760	-0.042481	2.164661
213.017588	1425.281495	18.354765	-0.042422	2.159499
212.855135	1417.350301	18.359770	-0.042387	2.154300
212.987569	1409.359545	18.364775	-0.042407	2.149077
213.147017	1401.382805	18.369779	-0.042432	2.143854
212.988745	1393.491988	18.374784	-0.042398	2.138644
213.073997	1385.523410	18.379789	-0.042409	2.133393
212.878833	1377.604066	18.384794	-0.042368	2.128136
212.750643	1369.689134	18.389799	-0.042340	2.122874
212.697268	1361.753807	18.394803	-0.042325	2.117593
212.868234	1353.764755	18.399808	-0.042352	2.112284
212.776060	1345.791898	18.404813	-0.042330	2.106948
212.570731	1337.887539	18.409818	-0.042287	2.101633
212.455349	1329.988188	18.414823	-0.042261	2.096317
212.370686	1322.047526	18.419827	-0.042241	2.090962
212.322434	1314.108101	18.424832	-0.042227	2.085597
212.399076	1306.174174	18.429837	-0.042237	2.080235
212.214892	1298.269202	18.434842	-0.042198	2.074853
212.165796	1290.316348	18.439847	-0.042184	2.069438
212.150744	1282.359927	18.444851	-0.042177	2.064010
212.050203	1274.464733	18.449856	-0.042153	2.058600
211.774241	1266.568513	18.454861	-0.042097	2.053158
211.630916	1258.621370	18.459866	-0.042066	2.047680
211.846021	1250.671229	18.464871	-0.042101	2.042221
211.734004	1242.761143	18.469875	-0.042076	2.036742
211.585546	1234.828511	18.474880	-0.042044	2.031229
211.515203	1226.868311	18.479885	-0.042026	2.025689
211.582134	1218.939406	18.484890	-0.042034	2.020171
211.391665	1211.063650	18.489895	-0.041994	2.014648
211.276584	1203.115708	18.494899	-0.041968	2.009066
211.613675	1195.148663	18.499904	-0.042026	2.003503
211.333838	1187.281685	18.504909	-0.041969	1.997931
211.298643	1179.332131	18.509914	-0.041958	1.992310
211.363309	1171.391699	18.514919	-0.041965	1.986690
211.147381	1163.491524	18.519923	-0.041920	1.981053
211.128621	1155.591581	18.524928	-0.041912	1.975422
210.845728	1147.684665	18.529933	-0.041855	1.969741
210.893727	1139.745862	18.534938	-0.041859	1.964056
210.671749	1131.874934	18.539943	-0.041813	1.958374
210.773493	1123.895249	18.544947	-0.041828	1.952632
210.599245	1115.965673	18.549952	-0.041791	1.946880
210.590326	1108.038459	18.554957	-0.041784	1.941130
210.481753	1100.140055	18.559962	-0.041759	1.935373
210.642860	1092.190832	18.564967	-0.041785	1.929591
210.420293	1084.301191	18.569971	-0.041739	1.923794
210.359807	1076.406549	18.574976	-0.041723	1.917993
210.276286	1068.491231	18.579981	-0.041703	1.912157
210.055243	1060.585475	18.584986	-0.041657	1.906294
210.001283	1052.682650	18.589991	-0.041642	1.900435
209.819407	1044.791740	18.594995	-0.041604	1.894551
210.084130	1036.819535	18.600000	-0.041648	1.888639
209.852151	1028.946978	18.605005	-0.041601	1.882727
209.825706	1021.049505	18.610010	-0.041591	1.876801
209.741502	1013.127567	18.615015	-0.041571	1.870831
209.730473	1005.189423	18.620019	-0.041564	1.864838
209.846281	997.293181	18.625024	-0.041581	1.858872
209.556656	989.423296	18.630029	-0.041522	1.852860
209.492892	981.499560	18.635034	-0.041506	1.846813
209.743713	973.577143	18.640039	-0.041548	1.840785
209.485776	965.710663	18.645043	-0.041495	1.834720
209.450032	957.798132	18.650048	-0.041484	1.828625
209.255977	949.913557	18.655053	-0.041443	1.822513
209.197576	942.029611	18.660058	-0.041428	1.816397
209.465637	934.084127	18.665063	-0.041473	1.810251
209.016111	926.240350	18.670067	-0.041385	1.804077
209.044113	918.356021	18.675072	-0.041385	1.797909
208.963066	910.430090	18.680077	-0.041366	1.791673
208.857544	902.498220	18.685082	-0.041341	1.785407
208.763353	894.645074	18.690087	-0.041319	1.779183
208.739624	886.735073	18.695091	-0.041310	1.772901
208.823328	878.827152	18.700096	-0.041321	1.766611
208.423886	871.007812	18.705101	-0.041242	1.760310
208.246260	863.137688	18.710106	-0.041205	1.753973
208.304160	855.214411	18.715111	-0.041211	1.747599
208.459615	847.293092	18.720115	-0.041235	1.741216
208.402412	839.433372	18.725120	-0.041220	1.734833
208.376631	831.548472	18.730125	-0.041210	1.728410
208.316881	823.668070	18.735130	-0.041195	1.721962
208.212616	815.826278	18.740135	-0.041171	1.715516
208.124306	807.924271	18.745139	-0.041150	1.708997
208.202772	800.038393	18.750144	-0.041160	1.702489
207.899093	792.209257	18.755149	-0.041098	1.695953
207.701882	784.335735	18.760154	-0.041057	1.689369
207.843611	776.443877	18.765159	-0.041079	1.682788
207.705747	768.590802	18.770163	-0.041049	1.676177
207.584806	760.723037	18.775168	-0.041022	1.669529
207.617824	752.842699	18.780173	-0.041023	1.662865
207.371942	745.005018	18.785178	-0.040973	1.656173
207.552465	737.114881	18.790183	-0.041002	1.649466
207.393078	729.258204	18.795187	-0.040967	1.642715
207.199042	721.443257	18.800192	-0.040927	1.635967
207.415346	713.487453	18.805197	-0.040962	1.629125
207.333187	705.624725	18.810202	-0.040942	1.622295
207.233783	697.801289	18.815207	-0.040919	1.615467
206.906947	689.979047	18.820211	-0.040854	1.608579
206.912973	682.123316	18.825216	-0.040851	1.601679
206.807763	674.289574	18.830221	-0.040826	1.594753
206.785297	666.415418	18.835226	-0.040818	1.587772
206.932276	658.550461	18.840231	-0.040840	1.580794
206.773152	650.731217	18.845235	-0.040806	1.573781
206.810307	642.873770	18.850240	-0.040808	1.566730
206.544018	635.088198	18.855245	-0.040754	1.559669
206.454210	627.247829	18.860250	-0.040733	1.552551
206.304682	619.411194	18.865255	-0.040701	1.545396
206.322222	611.559311	18.870259	-0.040699	1.538217
206.252525	603.736279	18.875264	-0.040682	1.531019
206.297493	595.892584	18.880269	-0.040686	1.523785
206.101844	588.096799	18.885274	-0.040645	1.516524
206.096446	580.256347	18.890279	-0.040639	1.509215
205.766975	572.476078	18.895283	-0.040573	1.501878
206.006251	564.618534	18.900288	-0.040613	1.494520
206.107810	556.773763	18.905293	-0.040627	1.487116
205.954698	548.988086	18.910298	-0.040594	1.479691
205.683903	541.210175	18.915303	-0.040539	1.472218
205.475291	533.375355	18.920307	-0.040496	1.464662
205.386150	525.591482	18.925312	-0.040475	1.457134
205.325241	517.779966	18.930317	-0.040459	1.449545
205.417060	509.956233	18.935322	-0.040471	1.441929
205.571301	502.149662	18.940327	-0.040496	1.434300
205.211943	494.390300	18.945331	-0.040424	1.426592
205.037656	486.628958	18.950336	-0.040387	1.418871
205.025306	478.828970	18.955341	-0.040380	1.411096
204.909309	471.052839	18.960346	-0.040354	1.403285
204.852042	463.294073	18.965351	-0.040339	1.395457
204.910832	455.467980	18.970355	-0.040345	1.387536
204.789481	447.710044	18.975360	-0.040318	1.379608
204.679967	439.953002	18.980365	-0.040293	1.371638
204.548516	432.191429	18.985370	-0.040264	1.363612
204.300486	424.473569	18.990375	-0.040214	1.355565
204.130079	416.704060	18.995379	-0.040177	1.347428
204.036629	408.960847	19.000384	-0.040155	1.339284
204.048952	401.192354	19.005389	-0.040153	1.331081
203.818901	393.472568	19.010394	-0.040106	1.322836
203.853277	385.705661	19.015399	-0.040108	1.314537
203.832766	377.827079	19.020403	-0.040099	1.306054
203.597737	370.152153	19.025408	-0.040051	1.297698
203.560389	362.420791	19.030413	-0.040040	1.289262
203.328069	354.728027	19.035418	-0.039992	1.280777
203.447602	347.002500	19.040423	-0.040010	1.272264
203.148199	339.313859	19.045427	-0.039949	1.263657
203.191385	331.597397	19.050432	-0.039953	1.255024
203.470162	323.846452	19.055437	-0.040000	1.246338
203.225631	316.199197	19.060442	-0.039950	1.237608
203.124493	308.512062	19.065447	-0.039927	1.228798
202.856786	300.846982	19.070451	-0.039873	1.219917
202.839972	293.162124	19.075456	-0.039865	1.210997
202.727611	285.507705	19.080461	-0.039840	1.202028
202.782464	277.826110	19.085466	-0.039845	1.192993
202.660178	270.177746	19.090471	-0.039818	1.183892
202.446844	262.554745	19.095475	-0.039774	1.174733
202.225784	254.930520	19.100480	-0.039728	1.165498
202.099769	247.314950	19.105485	-0.039701	1.156221
201.800509	239.667894	19.110490	-0.039640	1.146792
201.522258	232.081391	19.115495	-0.039584	1.137365
201.213233	224.484707	19.120499	-0.039522	1.127840
201.032366	216.897041	19.125504	-0.039484	1.118273
200.650191	209.331483	19.130509	-0.039409	1.108607
200.459144	201.740365	19.135514	-0.039369	1.098865
200.352509	194.156622	19.140519	-0.039344	1.089064
199.884613	186.643393	19.145523	-0.039253	1.079185
199.697223	179.070385	19.150528	-0.039213	1.069200
199.408329	171.538104	19.155533	-0.039155	1.059151
199.024970	164.011563	19.160538	-0.039080	1.048992
198.543354	156.541341	19.165543	-0.038986	1.038786
197.995554	149.057939	19.170547	-0.038879	1.028445
197.824108	141.540374	19.175552	-0.038843	1.018042
197.197002	134.103089	19.180557	-0.038722	1.007533
196.515934	126.686147	19.185562	-0.038591	0.996928
196.213738	119.181809	19.190567	-0.038530	0.986178
195.527008	111.781057	19.195571	-0.038398	0.975363
195.371817	104.304864	19.200576	-0.038365	0.964451
195.110522	96.881510	19.205581	-0.038312	0.953465
194.498766	89.511931	19.210586	-0.038194	0.942339
193.877979	82.177862	19.215591	-0.038074	0.931132
193.464589	74.807145	19.220595	-0.037992	0.919787
192.957878	67.474381	19.225600	-0.037894	0.908334
192.581115	60.364876	19.230605	-0.037820	0.897121