Thu Mar 11 20:08:05 2021

Number of Points = 3625
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.560775	-0.045913	0.000000	-0.000014	0.720883

0.427041	-0.026141	0.005005	0.000011	0.720875
0.442320	-0.027313	0.010010	0.000008	0.720878
0.421741	-0.022734	0.015014	0.000012	0.720880
0.466107	-0.033251	0.020019	0.000003	0.720874
0.584949	-0.052309	0.025024	-0.000019	0.720879
0.391694	-0.019995	0.030029	0.000017	0.720874
0.370476	-0.015461	0.035034	0.000021	0.720876
0.514786	-0.040047	0.040038	-0.000006	0.720878
0.409031	-0.024147	0.045043	0.000014	0.720872
0.355650	-0.009879	0.050048	0.000024	0.720882
0.445200	-0.030148	0.055053	0.000007	0.720873
0.439214	-0.027651	0.060058	0.000008	0.720876
0.608845	-0.055398	0.065062	-0.000023	0.720881
0.531562	-0.046036	0.070067	-0.000009	0.720872
0.419978	-0.031597	0.075072	0.000012	0.720861
0.376192	-0.188600	0.080077	0.000020	0.720537
0.412847	-0.193025	0.085082	0.000013	0.720541
0.418514	-0.192922	0.090086	0.000012	0.720543
0.284189	-0.171655	0.095091	0.000037	0.720538
0.333066	-0.178018	0.100096	0.000028	0.720543
0.351089	-0.185428	0.105101	0.000025	0.720534
0.628250	-0.295990	0.110106	-0.000027	0.720414
0.537656	-0.376600	0.115110	-0.000010	0.720223
0.510795	-0.374073	0.120115	-0.000005	0.720219
0.539507	-0.374032	0.125120	-0.000010	0.720229
0.635726	-0.395723	0.130125	-0.000028	0.720220
0.620511	-0.491236	0.135130	-0.000025	0.720027
0.610030	-0.552828	0.140134	-0.000023	0.719902
0.386503	-0.515158	0.145139	0.000019	0.719897
0.464717	-0.525401	0.150144	0.000004	0.719905
0.625042	-0.629005	0.155149	-0.000026	0.719757
0.640260	-0.709960	0.160154	-0.000029	0.719603
0.742811	-0.726558	0.165158	-0.000048	0.719606
0.587625	-0.702442	0.170163	-0.000019	0.719599
0.771131	-0.887012	0.175168	-0.000053	0.719299
0.542542	-0.861615	0.180173	-0.000010	0.719269
0.439421	-0.843999	0.185178	0.000009	0.719268
0.465400	-0.947272	0.190182	0.000004	0.719073
0.273177	-0.969371	0.195187	0.000040	0.718962
0.243035	-0.959095	0.200192	0.000046	0.718972
0.283557	-1.042888	0.205197	0.000038	0.718821
0.290882	-1.130757	0.210202	0.000037	0.718650
0.406375	-1.150376	0.215206	0.000015	0.718652
0.367946	-1.226517	0.220211	0.000023	0.718488
0.355823	-1.289737	0.225216	0.000025	0.718359
0.181428	-1.261243	0.230221	0.000057	0.718354
0.102042	-1.375337	0.235226	0.000072	0.718100
0.268457	-1.443220	0.240230	0.000041	0.718025
0.017214	-1.416996	0.245235	0.000088	0.717988
0.197436	-1.589664	0.250240	0.000055	0.717710
0.088831	-1.574109	0.255245	0.000075	0.717703
0.128147	-1.667817	0.260250	0.000067	0.717531
0.103931	-1.737597	0.265254	0.000072	0.717385
0.095970	-1.756860	0.270259	0.000074	0.717344
0.265086	-1.914997	0.275264	0.000042	0.717091
0.150474	-1.897539	0.280269	0.000063	0.717085
0.305335	-2.063267	0.285274	0.000035	0.716812
0.449368	-2.113610	0.290278	0.000008	0.716763
0.301910	-2.198971	0.295283	0.000035	0.716542
0.199902	-2.226056	0.300288	0.000055	0.716452
0.176193	-2.318988	0.305293	0.000059	0.716260
0.182325	-2.383562	0.310298	0.000058	0.716134
-0.047970	-2.407820	0.315302	0.000101	0.716005
-0.443741	-2.399831	0.320307	0.000174	0.715881
-0.363638	-2.483849	0.325312	0.000160	0.715743
-3.462766	-2.029844	0.330317	0.000736	0.715548
-2.704290	-2.164368	0.335322	0.000595	0.715549
-3.178623	-2.151863	0.340326	0.000684	0.715407
-4.734331	-1.963816	0.345331	0.000973	0.715230
-3.496743	-2.179682	0.350336	0.000743	0.715239
-4.023357	-2.088935	0.355341	0.000841	0.715233
-4.689306	-2.134067	0.360346	0.000965	0.714908
-4.601289	-2.147700	0.365350	0.000948	0.714912
-5.501802	-1.992462	0.370355	0.001116	0.714902
-5.148195	-2.050500	0.375360	0.001050	0.714912
-5.507797	-2.139435	0.380365	0.001117	0.714608
-5.883458	-2.071682	0.385370	0.001187	0.714610
-6.135433	-2.025335	0.390374	0.001234	0.714613
-6.052251	-2.044240	0.395379	0.001219	0.714604
-5.988719	-2.130951	0.400384	0.001207	0.714455
-6.970954	-2.046187	0.405389	0.001390	0.714276
-6.973624	-2.043430	0.410394	0.001390	0.714280
-7.157929	-2.008353	0.415398	0.001424	0.714285
-7.068081	-2.028444	0.420403	0.001408	0.714276
-6.793653	-2.141299	0.425408	0.001357	0.714149
-8.242671	-1.971795	0.430413	0.001626	0.713973
-8.026086	-2.011559	0.435418	0.001586	0.713971
-7.780099	-2.053537	0.440422	0.001540	0.713975
-8.070820	-2.005863	0.445427	0.001594	0.713966
-7.849172	-2.040009	0.450432	0.001553	0.713977
-8.042596	-2.115699	0.455437	0.001589	0.713758
-9.199095	-1.962689	0.460442	0.001804	0.713653
-8.582455	-2.069490	0.465446	0.001690	0.713659
-8.796177	-2.036434	0.470451	0.001730	0.713649
-9.181758	-1.962003	0.475456	0.001801	0.713660
-8.913791	-2.013041	0.480461	0.001751	0.713654
-8.939079	-2.094655	0.485466	0.001756	0.713482
-9.907362	-1.982178	0.490470	0.001936	0.713363
-10.106578	-1.949625	0.495475	0.001973	0.713357
-9.807217	-1.998526	0.500480	0.001918	0.713366
-9.719401	-2.016367	0.505485	0.001901	0.713361
-9.823114	-1.998828	0.510490	0.001921	0.713360
-9.811546	-2.004380	0.515494	0.001919	0.713353
-10.482096	-2.049557	0.520499	0.002043	0.713025
-10.311639	-2.076396	0.525504	0.002012	0.713032
-10.881507	-1.977956	0.530509	0.002118	0.713026
-10.925275	-1.970626	0.535514	0.002126	0.713025
-10.412414	-2.058708	0.540518	0.002031	0.713032
-10.819382	-1.990941	0.545523	0.002106	0.713022
-10.606888	-2.100646	0.550528	0.002067	0.712879
-11.690106	-1.993505	0.555533	0.002268	0.712708
-11.643232	-2.000992	0.560538	0.002260	0.712710
-11.458197	-2.030196	0.565542	0.002225	0.712717
-11.693230	-1.992080	0.570547	0.002269	0.712710
-11.480567	-2.024520	0.575552	0.002229	0.712721
-11.957464	-1.943897	0.580557	0.002318	0.712712
-11.762576	-2.065366	0.585562	0.002282	0.712539
-12.546511	-1.999553	0.590566	0.002428	0.712392
-12.510867	-2.008919	0.595571	0.002421	0.712386
-12.501538	-2.006974	0.600576	0.002419	0.712393
-12.257588	-2.051772	0.605581	0.002374	0.712391
-12.432003	-2.021201	0.610586	0.002407	0.712390
-12.449937	-2.016515	0.615590	0.002410	0.712393
-12.516451	-2.108016	0.620595	0.002422	0.712187
-13.139287	-2.041884	0.625600	0.002538	0.712097
-13.217652	-2.030190	0.630605	0.002553	0.712093
-13.304742	-2.014631	0.635610	0.002569	0.712093
-13.209809	-2.029194	0.640614	0.002551	0.712098
-13.352979	-2.009126	0.645619	0.002578	0.712087
-13.295697	-2.029905	0.650624	0.002567	0.712066
-14.169176	-2.025447	0.655629	0.002730	0.711764
-14.336995	-1.996050	0.660634	0.002761	0.711763
-14.340341	-1.993063	0.665638	0.002762	0.711768
-14.265004	-2.010244	0.670643	0.002748	0.711761
-14.228976	-2.013177	0.675648	0.002741	0.711768
-14.489524	-1.968823	0.680653	0.002790	0.711763
-14.342652	-1.997497	0.685658	0.002762	0.711758
-14.222783	-2.121996	0.690662	0.002740	0.711553
-15.375328	-1.967531	0.695667	0.002955	0.711451
-15.226452	-1.991358	0.700672	0.002927	0.711457
-14.890839	-2.052334	0.705677	0.002864	0.711454
-15.163718	-2.006015	0.710682	0.002915	0.711450
-15.271769	-1.981124	0.715686	0.002935	0.711461
-15.194791	-2.000435	0.720691	0.002921	0.711450
-15.163134	-2.115896	0.725696	0.002915	0.711231
-16.150539	-1.985472	0.730701	0.003099	0.711140
-16.231424	-1.971486	0.735706	0.003114	0.711139
-15.577772	-2.086164	0.740710	0.002992	0.711143
-16.119298	-1.992831	0.745715	0.003093	0.711136
-15.944485	-2.018857	0.750720	0.003061	0.711146
-16.029470	-2.005823	0.755725	0.003076	0.711142
-16.528936	-2.022913	0.760730	0.003169	0.710930
-16.780230	-2.002684	0.765734	0.003216	0.710881
-16.807366	-2.002734	0.770739	0.003221	0.710872
-16.745166	-2.010140	0.775744	0.003210	0.710879
-16.867804	-1.990044	0.780749	0.003233	0.710876
-16.931447	-1.979834	0.785754	0.003244	0.710873
-16.357019	-2.085089	0.790758	0.003138	0.710868
-17.426978	-2.062024	0.795763	0.003337	0.710533
-17.799336	-1.992032	0.800768	0.003406	0.710540
-17.748611	-2.004156	0.805773	0.003397	0.710534
-17.539232	-2.042639	0.810778	0.003358	0.710532
-17.791226	-1.993744	0.815782	0.003405	0.710540
-18.149804	-1.934726	0.820787	0.003471	0.710530
-17.724596	-2.005887	0.825792	0.003392	0.710539
-18.109204	-2.077334	0.830797	0.003464	0.710259
-19.000420	-1.939953	0.835802	0.003630	0.710216
-18.490894	-2.024973	0.840806	0.003535	0.710228
-18.409660	-2.044642	0.845811	0.003520	0.710218
-18.852575	-1.962857	0.850816	0.003602	0.710223
-18.724574	-1.987306	0.855821	0.003578	0.710220
-18.804239	-1.972131	0.860826	0.003593	0.710222
-18.875550	-2.065256	0.865830	0.003606	0.710011
-19.888062	-1.943455	0.870835	0.003795	0.709893
-19.465303	-2.014891	0.875840	0.003716	0.709901
-19.406025	-2.028576	0.880845	0.003705	0.709895
-19.826066	-1.952350	0.885850	0.003783	0.709898
-19.022320	-2.093283	0.890854	0.003634	0.709902
-19.404485	-2.029039	0.895859	0.003705	0.709894
-20.131128	-2.008953	0.900864	0.003840	0.709676
-20.445976	-1.991866	0.905869	0.003899	0.709598
-20.032619	-2.066077	0.910874	0.003822	0.709597
-20.002548	-2.068859	0.915878	0.003816	0.709602
-20.720809	-1.944440	0.920883	0.003950	0.709595
-20.295452	-2.015327	0.925888	0.003871	0.709604
-20.294693	-2.016280	0.930893	0.003871	0.709603
-20.902832	-2.053932	0.935898	0.003984	0.709311
-20.988581	-2.057722	0.940902	0.004000	0.709272
-21.359432	-1.995253	0.945907	0.004069	0.709265
-21.175439	-2.025078	0.950912	0.004035	0.709271
-21.105452	-2.039890	0.955917	0.004022	0.709266
-21.269400	-2.012580	0.960922	0.004052	0.709263
-21.217241	-2.017115	0.965926	0.004043	0.709272
-22.126956	-2.013616	0.970931	0.004212	0.708955
-21.977892	-2.035152	0.975936	0.004184	0.708965
-22.308101	-1.977701	0.980941	0.004246	0.708962
-22.540949	-1.940644	0.985946	0.004289	0.708953
-22.003198	-2.031025	0.990950	0.004189	0.708964
-22.175653	-2.004030	0.995955	0.004221	0.708956
-22.242037	-1.987167	1.000960	0.004233	0.708966
-22.317077	-2.068751	1.005965	0.004247	0.708776
-23.435693	-1.937192	1.010970	0.004456	0.708641
-23.048353	-2.003303	1.015974	0.004383	0.708646
-23.465865	-1.932862	1.020979	0.004461	0.708638
-23.282862	-1.962554	1.025984	0.004427	0.708644
-22.736265	-2.060790	1.030989	0.004325	0.708643
-23.259534	-1.969397	1.035994	0.004423	0.708639
-23.088335	-2.026794	1.040998	0.004391	0.708585
-23.646759	-2.042154	1.046003	0.004495	0.708355
-23.802320	-2.012127	1.051008	0.004524	0.708359
-24.315047	-1.924636	1.056013	0.004619	0.708352
-24.015731	-1.979306	1.061018	0.004564	0.708349
-23.630257	-2.042866	1.066022	0.004492	0.708359
-23.962894	-1.988758	1.071027	0.004554	0.708349
-23.797512	-2.092700	1.076032	0.004523	0.708200
-24.767283	-2.010615	1.081037	0.004704	0.708018
-25.165911	-1.941354	1.086042	0.004778	0.708014
-24.529809	-2.051459	1.091046	0.004659	0.708021
-24.807985	-2.004289	1.096051	0.004711	0.708016
-24.791271	-2.005436	1.101056	0.004708	0.708020
-24.937580	-1.980252	1.106061	0.004735	0.708018
-24.850334	-2.066534	1.111066	0.004719	0.707876
-25.893921	-1.964045	1.116070	0.004913	0.707708
-26.124303	-1.926793	1.121075	0.004956	0.707701
-25.632051	-2.012001	1.126080	0.004865	0.707706
-25.439671	-2.047651	1.131085	0.004829	0.707703
-25.727186	-1.997219	1.136090	0.004882	0.707701
-25.744936	-1.990706	1.141094	0.004886	0.707708
-25.647240	-2.052633	1.146099	0.004867	0.707619
-26.411259	-2.035999	1.151104	0.005010	0.707379
-26.382921	-2.040698	1.156109	0.005004	0.707380
-26.831542	-1.964116	1.161114	0.005088	0.707373
-26.377215	-2.037977	1.166118	0.005003	0.707387
-26.492270	-2.022951	1.171123	0.005025	0.707376
-26.550397	-2.009360	1.176128	0.005036	0.707383
-26.448094	-2.100905	1.181133	0.005017	0.707236
-27.807427	-1.935710	1.186138	0.005270	0.707081
-27.176068	-2.045331	1.191142	0.005152	0.707087
-27.327254	-2.020946	1.196147	0.005180	0.707082
-27.737189	-1.945502	1.201152	0.005257	0.707086
-27.611482	-1.969618	1.206157	0.005233	0.707083
-27.731314	-1.947984	1.211162	0.005256	0.707083
-27.166836	-2.100616	1.216166	0.005151	0.706979
-28.526929	-1.971044	1.221171	0.005404	0.706752
-28.324394	-2.003841	1.226176	0.005366	0.706759
-28.265874	-2.014231	1.231181	0.005355	0.706759
-28.660657	-1.947239	1.236186	0.005429	0.706752
-28.584501	-1.956187	1.241190	0.005414	0.706762
-28.688688	-1.941927	1.246195	0.005434	0.706753
-28.351286	-1.999309	1.251200	0.005371	0.706758
-28.988825	-2.035474	1.256205	0.005490	0.706457
-29.586190	-1.936407	1.261210	0.005601	0.706443
-29.208879	-2.000400	1.266214	0.005531	0.706449
-29.223224	-2.001337	1.271219	0.005533	0.706442
-29.542159	-1.942735	1.276224	0.005593	0.706446
-29.104281	-2.018768	1.281229	0.005511	0.706450
-29.132368	-2.016555	1.286234	0.005516	0.706444
-29.392584	-2.096226	1.291238	0.005565	0.706191
-30.146457	-1.995462	1.296243	0.005705	0.706123
-30.330574	-1.957048	1.301248	0.005740	0.706134
-30.059540	-2.005943	1.306253	0.005689	0.706133
-30.407707	-1.946944	1.311258	0.005754	0.706127
-30.103140	-1.996536	1.316262	0.005697	0.706136
-30.367411	-1.953269	1.321267	0.005746	0.706129
-30.660807	-1.996458	1.326272	0.005801	0.705937
-30.922677	-1.983307	1.331277	0.005850	0.705869
-31.002718	-1.973034	1.336282	0.005865	0.705861
-31.117024	-1.947338	1.341286	0.005886	0.705872
-31.264616	-1.925955	1.346291	0.005913	0.705862
-30.622606	-2.038614	1.351296	0.005794	0.705866
-30.550067	-2.050030	1.356301	0.005780	0.705869
-31.553945	-2.039189	1.361306	0.005967	0.705530
-31.739031	-2.005455	1.366310	0.006002	0.705532
-31.836208	-1.992551	1.371315	0.006020	0.705523
-31.895793	-1.979638	1.376320	0.006031	0.705528
-31.890595	-1.981145	1.381325	0.006030	0.705526
-32.102706	-1.946161	1.386330	0.006070	0.705521
-31.863579	-1.987392	1.391334	0.006025	0.705524
-32.539032	-2.023066	1.396339	0.006151	0.705209
-32.804614	-1.971841	1.401344	0.006200	0.705217
-33.217569	-1.897252	1.406349	0.006277	0.705219
-33.148748	-1.913861	1.411354	0.006264	0.705210
-32.303145	-2.060225	1.416358	0.006107	0.705219
-32.551576	-2.021711	1.421363	0.006153	0.705208
-33.068079	-1.926724	1.426368	0.006249	0.705213
-32.940502	-2.069479	1.431373	0.006226	0.704972
-33.667968	-1.984744	1.436378	0.006361	0.704881
-33.651584	-1.981346	1.441382	0.006358	0.704894
-33.819447	-1.956378	1.446387	0.006389	0.704884
-33.831902	-1.951598	1.451392	0.006392	0.704889
-33.437293	-2.021286	1.456397	0.006318	0.704891
-33.782663	-1.963356	1.461402	0.006382	0.704883
-33.845141	-2.064462	1.466406	0.006394	0.704657
-34.697170	-1.947773	1.471411	0.006553	0.704586
-34.782101	-1.930731	1.476416	0.006568	0.704590
-34.384670	-2.000808	1.481421	0.006495	0.704591
-34.602502	-1.964954	1.486426	0.006535	0.704585
-34.684294	-1.946457	1.491430	0.006550	0.704593
-34.651316	-1.954426	1.496435	0.006544	0.704589
-34.582382	-2.070663	1.501440	0.006531	0.704380
-35.435203	-1.974723	1.506445	0.006690	0.704267
-35.592139	-1.950381	1.511450	0.006719	0.704259
-35.335824	-1.991314	1.516454	0.006672	0.704269
-35.395793	-1.983873	1.521459	0.006683	0.704262
-35.589331	-1.947314	1.526464	0.006719	0.704266
-35.321431	-1.995190	1.531469	0.006669	0.704266
-35.629499	-2.056897	1.536474	0.006726	0.704031
-36.190919	-1.993645	1.541478	0.006831	0.703957
-36.193635	-1.995752	1.546483	0.006831	0.703951
-35.959863	-2.035493	1.551488	0.006788	0.703955
-35.954878	-2.034251	1.556493	0.006787	0.703960
-36.628073	-1.916975	1.561498	0.006912	0.703954
-36.213968	-1.993589	1.566502	0.006835	0.703949
-36.794640	-2.045436	1.571507	0.006943	0.703635
-37.064366	-1.996918	1.576512	0.006994	0.703636
-37.194281	-1.971820	1.581517	0.007018	0.703640
-37.004489	-2.010027	1.586522	0.006982	0.703631
-36.750236	-2.051952	1.591526	0.006935	0.703638
-37.306214	-1.955918	1.596531	0.007039	0.703632
-37.077107	-2.034668	1.601536	0.006996	0.703555
-37.825790	-2.005241	1.606541	0.007135	0.703345
-38.116689	-1.958168	1.611546	0.007189	0.703335
-38.112844	-1.953013	1.616550	0.007189	0.703347
-37.643229	-2.040298	1.621555	0.007101	0.703340
-38.034467	-1.969921	1.626560	0.007174	0.703341
-37.993964	-1.975169	1.631565	0.007167	0.703345
-37.708253	-2.085529	1.636570	0.007113	0.703225
-38.597152	-2.031666	1.641574	0.007279	0.703014
-38.739297	-2.010919	1.646579	0.007305	0.703005
-39.097606	-1.945330	1.651584	0.007372	0.703008
-38.446709	-2.059798	1.656589	0.007251	0.703011
-38.760102	-2.009174	1.661594	0.007309	0.703001
-39.048466	-1.953660	1.666598	0.007363	0.703009
-38.918474	-2.065899	1.671603	0.007339	0.702829
-40.025619	-1.934278	1.676608	0.007545	0.702696
-39.576538	-2.012147	1.681613	0.007461	0.702701
-39.766278	-1.983064	1.686618	0.007497	0.702691
-39.832173	-1.966562	1.691622	0.007509	0.702701
-39.479352	-2.032829	1.696627	0.007443	0.702694
-39.400337	-2.044714	1.701632	0.007429	0.702698
-39.451097	-2.154418	1.706637	0.007438	0.702458
-40.831951	-1.954919	1.711642	0.007695	0.702364
-40.714502	-1.968871	1.716646	0.007673	0.702378
-40.296940	-2.047840	1.721651	0.007596	0.702369
-40.594252	-1.992856	1.726656	0.007651	0.702373
-40.671671	-1.976540	1.731661	0.007665	0.702378
-40.679354	-1.979686	1.736666	0.007667	0.702369
-40.544485	-2.120422	1.741670	0.007642	0.702133
-41.415505	-1.994323	1.746675	0.007804	0.702074
-41.664091	-1.948722	1.751680	0.007850	0.702076
-40.933034	-2.078149	1.756685	0.007714	0.702078
-41.406054	-1.999089	1.761690	0.007802	0.702068
-41.451664	-1.984818	1.766694	0.007811	0.702080
-41.203773	-2.054140	1.771699	0.007764	0.702029
-42.132632	-2.029173	1.776704	0.007937	0.701745
-41.944455	-2.060642	1.781709	0.007902	0.701749
-42.576290	-1.951678	1.786714	0.008020	0.701741
-42.349842	-1.985575	1.791718	0.007978	0.701754
-42.348285	-1.992909	1.796723	0.007977	0.701740
-42.445438	-1.973770	1.801728	0.007996	0.701744
-42.108663	-2.043926	1.806733	0.007933	0.701723
-43.271829	-1.979808	1.811738	0.008149	0.701433
-43.378803	-1.955218	1.816742	0.008169	0.701444
-43.428791	-1.949540	1.821747	0.008179	0.701438
-43.043237	-2.018945	1.826752	0.008107	0.701437
-43.010284	-2.023817	1.831757	0.008101	0.701439
-43.260884	-1.983908	1.836762	0.008147	0.701429
-43.024361	-2.019220	1.841766	0.008103	0.701443
-43.706978	-2.033717	1.846771	0.008231	0.701167
-44.397502	-1.932545	1.851776	0.008359	0.701122
-43.829152	-2.033083	1.856781	0.008253	0.701124
-43.671243	-2.063051	1.861786	0.008224	0.701120
-43.965299	-2.007414	1.866790	0.008279	0.701127
-44.140110	-1.979129	1.871795	0.008311	0.701121
-43.970551	-2.008361	1.876800	0.008280	0.701123
-44.375068	-2.053237	1.881805	0.008355	0.700886
-44.797977	-1.985678	1.886810	0.008434	0.700870
-44.853474	-1.972082	1.891814	0.008444	0.700878
-44.594150	-2.021213	1.896819	0.008396	0.700872
-44.877312	-1.969984	1.901824	0.008448	0.700873
-44.754284	-1.989186	1.906829	0.008426	0.700879
-45.011003	-2.003993	1.911834	0.008473	0.700756
-45.936727	-1.946500	1.916838	0.008646	0.700538
-45.372383	-2.051527	1.921843	0.008541	0.700529
-45.559595	-2.016753	1.926848	0.008575	0.700532
-45.727150	-1.984137	1.931853	0.008607	0.700537
-45.616051	-2.008414	1.936858	0.008586	0.700528
-45.401744	-2.040199	1.941862	0.008546	0.700541
-45.795265	-2.080927	1.946867	0.008619	0.700317
-46.901399	-1.933313	1.951872	0.008825	0.700216
-46.406158	-2.019897	1.956877	0.008733	0.700219
-46.267725	-2.048623	1.961882	0.008707	0.700211
-46.486273	-2.003643	1.966886	0.008748	0.700223
-46.925781	-1.927995	1.971891	0.008830	0.700218
-46.725789	-1.963966	1.976896	0.008793	0.700217
-46.579609	-2.095307	1.981901	0.008765	0.700004
-47.917541	-1.913444	1.986906	0.009015	0.699889
-47.433119	-1.994678	1.991910	0.008924	0.699899
-47.205320	-2.037647	1.996915	0.008882	0.699894
-47.564949	-1.971284	2.001920	0.008949	0.699899

-47.594144	-1.966882	2.011917	0.008954	0.699897
-47.913221	-2.001626	2.021914	0.009014	0.699711
-48.426722	-1.965061	2.031910	0.009109	0.699599
-48.156028	-2.013063	2.041907	0.009059	0.699600
-48.491758	-1.953454	2.051904	0.009121	0.699599
-48.294583	-1.988884	2.061901	0.009085	0.699599
-47.933038	-1.934688	2.071898	0.009017	0.699840
-47.516049	-1.982205	2.081894	0.008940	0.699894
-47.534531	-1.978751	2.091891	0.008943	0.699895
-47.286141	-2.022774	2.101888	0.008897	0.699895
-47.506512	-1.983239	2.111885	0.008938	0.699896
-47.620126	-1.962434	2.121882	0.008959	0.699897
-47.653489	-1.956903	2.131878	0.008965	0.699896
-47.459954	-1.991953	2.141875	0.008929	0.699895
-47.544287	-1.931767	2.151872	0.008945	0.699986
-46.481773	-2.005205	2.161869	0.008747	0.700222
-46.570769	-1.989522	2.171866	0.008764	0.700221
-46.649477	-1.975559	2.181862	0.008779	0.700221
-46.413618	-2.016191	2.191859	0.008735	0.700224
-46.408196	-1.924738	2.201856	0.008734	0.700411
-45.742762	-1.980915	2.211853	0.008610	0.700538
-45.990514	-1.937192	2.221850	0.008656	0.700537
-45.514560	-2.021255	2.231846	0.008567	0.700539
-45.270808	-1.974650	2.241843	0.008522	0.700721
-44.698952	-2.000068	2.251840	0.008415	0.700876
-44.680029	-2.003824	2.261837	0.008412	0.700876
-44.869008	-1.969542	2.271834	0.008447	0.700877
-44.488840	-1.985873	2.281830	0.008376	0.700981
-44.057970	-1.989978	2.291827	0.008296	0.701128
-44.235234	-1.958286	2.301824	0.008329	0.701129
-44.119999	-1.977249	2.311821	0.008308	0.701132
-43.476363	-1.940073	2.321818	0.008188	0.701439
-43.108078	-2.005045	2.331814	0.008119	0.701441
-43.147658	-1.997597	2.341811	0.008127	0.701442
-42.917573	-1.958819	2.351808	0.008084	0.701603
-42.373374	-1.983640	2.361805	0.007982	0.701749
-42.528771	-1.957510	2.371802	0.008011	0.701746
-42.239196	-1.995121	2.381798	0.007957	0.701774
-41.509121	-1.975834	2.391795	0.007821	0.702077
-41.310840	-2.010799	2.401792	0.007785	0.702078
-41.432569	-1.990944	2.411789	0.007807	0.702074
-41.333604	-1.931298	2.421786	0.007789	0.702230
-40.403720	-2.027678	2.431782	0.007616	0.702371
-40.513167	-2.006535	2.441779	0.007636	0.702374
-40.609943	-1.990590	2.451776	0.007654	0.702371
-39.974674	-1.947763	2.461773	0.007536	0.702687
-39.653512	-2.001348	2.471770	0.007476	0.702694
-39.538145	-2.021799	2.481766	0.007455	0.702694
-39.560168	-1.945343	2.491763	0.007459	0.702841
-38.762686	-2.003343	2.501760	0.007310	0.703011
-38.850614	-1.990176	2.511757	0.007327	0.703006
-39.056758	-1.940261	2.521754	0.007365	0.703032
-37.979120	-1.979284	2.531750	0.007164	0.703342
-38.060981	-1.961084	2.541747	0.007179	0.703349
-37.997286	-1.974255	2.551744	0.007168	0.703345
-37.707449	-1.923903	2.561741	0.007114	0.703551
-37.098379	-1.990627	2.571738	0.007000	0.703636
-37.037280	-2.002291	2.581734	0.006989	0.703634
-37.109312	-1.954624	2.591731	0.007002	0.703704
-36.157228	-1.999775	2.601728	0.006825	0.703956
-36.281176	-1.977401	2.611725	0.006848	0.703956
-36.527834	-1.934971	2.621722	0.006894	0.703953
-35.640175	-1.973006	2.631718	0.006729	0.704195
-35.793531	-1.912285	2.641715	0.006757	0.704263
-35.262499	-2.006994	2.651712	0.006658	0.704263
-35.491369	-1.885079	2.661709	0.006701	0.704426
-34.363034	-2.004835	2.671706	0.006491	0.704590
-34.619620	-1.958971	2.681702	0.006539	0.704590
-34.544923	-1.971702	2.691699	0.006525	0.704592
-33.925680	-1.938793	2.701696	0.006410	0.704880
-33.689712	-1.977713	2.711693	0.006366	0.704887
-33.803794	-1.959893	2.721690	0.006387	0.704881
-33.195255	-1.980052	2.731686	0.006274	0.705059
-32.858037	-1.964124	2.741683	0.006211	0.705212
-32.652222	-2.002247	2.751680	0.006172	0.705210
-32.960888	-1.944421	2.761677	0.006230	0.705215
-32.118784	-1.941822	2.771674	0.006073	0.705523
-32.069843	-1.949883	2.781670	0.006064	0.705524
-31.712850	-2.013363	2.791667	0.005998	0.705524
-31.569642	-1.952811	2.801664	0.005971	0.705697
-31.077562	-1.959091	2.811661	0.005879	0.705861
-31.030241	-1.967678	2.821658	0.005870	0.705861
-30.959564	-1.980234	2.831654	0.005857	0.705861
-30.396140	-1.953888	2.841651	0.005752	0.706116
-29.982570	-2.021387	2.851648	0.005675	0.706128
-30.397158	-1.947284	2.861645	0.005753	0.706129
-29.846827	-1.960043	2.871642	0.005650	0.706300
-29.400508	-1.968357	2.881638	0.005567	0.706443
-29.213506	-2.001376	2.891635	0.005532	0.706444
-29.211993	-2.000786	2.901632	0.005532	0.706446
-28.703210	-1.941280	2.911629	0.005437	0.706748
-28.359610	-2.000812	2.921626	0.005373	0.706751
-28.593769	-1.958484	2.931622	0.005417	0.706752
-28.035183	-1.961423	2.941619	0.005313	0.706946
-27.554652	-1.979812	2.951616	0.005223	0.707081
-27.756677	-1.943875	2.961613	0.005261	0.707081
-27.374461	-2.001139	2.971610	0.005190	0.707103
-26.848753	-1.958442	2.981606	0.005092	0.707377
-26.466224	-2.024479	2.991603	0.005021	0.707381
-26.741949	-1.977120	3.001600	0.005072	0.707377
-26.380384	-1.953846	3.011597	0.005005	0.707553
-25.699860	-2.003376	3.021594	0.004878	0.707697
-25.904922	-1.964600	3.031590	0.004916	0.707702
-25.474713	-2.042835	3.041587	0.004836	0.707699
-25.152519	-1.953176	3.051584	0.004776	0.707994
-25.035534	-1.963498	3.061581	0.004754	0.708015
-25.089572	-1.955577	3.071578	0.004764	0.708011
-24.597919	-1.945929	3.081574	0.004673	0.708206
-23.934919	-1.991208	3.091571	0.004549	0.708352
-24.246744	-1.936874	3.101568	0.004608	0.708350
-23.794776	-2.012394	3.111565	0.004523	0.708360
-23.541452	-1.921980	3.121562	0.004476	0.708631
-23.421318	-1.941242	3.131558	0.004454	0.708636
-23.288665	-1.963905	3.141555	0.004429	0.708638
-22.595602	-1.961098	3.151552	0.004300	0.708891
-22.380730	-1.966679	3.161549	0.004260	0.708956
-22.526835	-1.942899	3.171546	0.004287	0.708952
-22.260164	-1.944942	3.181542	0.004238	0.709043
-21.513198	-1.968457	3.191539	0.004099	0.709262
-21.496987	-1.970952	3.201536	0.004096	0.709263
-21.319608	-2.002326	3.211533	0.004063	0.709263
-20.916890	-1.936556	3.221530	0.003988	0.709538
-20.706121	-1.946491	3.231526	0.003948	0.709594
-20.545713	-1.974488	3.241523	0.003918	0.709595
-20.667700	-1.890182	3.251520	0.003941	0.709720
-19.793241	-1.960070	3.261517	0.003778	0.709892
-20.061082	-1.914014	3.271514	0.003828	0.709888
-19.692858	-1.964465	3.281510	0.003760	0.709919
-19.233316	-1.896562	3.291507	0.003674	0.710218
-18.869352	-1.961225	3.301504	0.003606	0.710219
-18.869387	-1.962309	3.311501	0.003606	0.710216
-18.560450	-1.909793	3.321498	0.003549	0.710431
-18.003197	-1.959290	3.331494	0.003445	0.710531
-17.918054	-1.974341	3.341491	0.003429	0.710531
-18.023010	-1.938847	3.351488	0.003449	0.710565
-17.011448	-1.964276	3.361485	0.003260	0.710874
-17.340497	-1.908219	3.371482	0.003322	0.710869
-17.106518	-1.951084	3.381478	0.003278	0.710866
-17.052520	-1.878916	3.391475	0.003268	0.711029
-16.296022	-1.959326	3.401472	0.003127	0.711138
-16.582815	-1.909430	3.411469	0.003181	0.711136
-16.234853	-1.927960	3.421466	0.003116	0.711222
-15.291906	-1.981440	3.431462	0.002940	0.711451
-15.279774	-1.982697	3.441459	0.002938	0.711453
-15.756420	-1.897678	3.451456	0.003027	0.711453
-14.751616	-1.953557	3.461453	0.002840	0.711698
-14.850960	-1.905787	3.471450	0.002858	0.711758
-14.464000	-1.975049	3.481446	0.002786	0.711758
-14.499039	-1.917408	3.491443	0.002793	0.711860
-13.464468	-1.986708	3.501440	0.002600	0.712090
-13.911100	-1.907316	3.511437	0.002683	0.712089
-13.806584	-1.925935	3.521434	0.002664	0.712089
-13.176115	-1.916598	3.531430	0.002546	0.712332
-12.949929	-1.928727	3.541427	0.002504	0.712388
-12.794957	-1.955787	3.551424	0.002475	0.712389
-12.713037	-1.900260	3.561421	0.002460	0.712528
-11.956321	-1.944072	3.571418	0.002319	0.712710
-11.881964	-1.958808	3.581414	0.002305	0.712707
-11.896599	-1.954076	3.591411	0.002308	0.712711
-11.109672	-1.964489	3.601408	0.002162	0.712969
-10.871928	-1.978020	3.611405	0.002117	0.713027
-10.607584	-2.027236	3.621402	0.002068	0.713022
-10.670820	-2.014826	3.631398	0.002080	0.713025
-9.916457	-2.020276	3.641395	0.001939	0.713281
-9.744979	-2.009335	3.651392	0.001908	0.713364
-9.595131	-2.035440	3.661389	0.001880	0.713365
-9.772752	-2.006029	3.671386	0.001913	0.713360
-9.011790	-2.040651	3.681382	0.001771	0.713561
-8.884473	-2.016714	3.691379	0.001747	0.713654
-8.985836	-1.998257	3.701376	0.001766	0.713655
-9.124384	-1.974983	3.711373	0.001792	0.713652
-8.160486	-1.990153	3.721370	0.001613	0.713963
-7.953900	-2.024241	3.731366	0.001574	0.713968
-8.049640	-2.007062	3.741363	0.001592	0.713969
-7.837693	-1.993415	3.751360	0.001552	0.714071
-7.118351	-2.018032	3.761357	0.001419	0.714277
-7.174472	-2.009996	3.771354	0.001429	0.714273
-7.192964	-2.005557	3.781350	0.001432	0.714275
-6.599486	-1.987566	3.791347	0.001322	0.714521
-6.232223	-2.008593	3.801344	0.001254	0.714609
-6.303073	-1.997226	3.811341	0.001267	0.714606
-6.172511	-1.992258	3.821338	0.001242	0.714662
-5.349402	-2.017545	3.831334	0.001089	0.714903
-5.049901	-2.070818	3.841331	0.001033	0.714903
-5.178187	-2.045636	3.851328	0.001057	0.714908
-5.176096	-1.969716	3.861325	0.001057	0.715059
-4.435429	-2.016136	3.871322	0.000919	0.715229
-4.436633	-2.015287	3.881318	0.000919	0.715230
-4.389834	-2.022871	3.891315	0.000911	0.715232
-3.630165	-2.012903	3.901312	0.000769	0.715520
-3.464332	-2.029315	3.911309	0.000738	0.715546
-3.172726	-2.081731	3.921306	0.000684	0.715545
-3.441975	-2.016655	3.931302	0.000734	0.715579
-2.559858	-2.019628	3.941299	0.000570	0.715884
-2.268464	-2.071927	3.951296	0.000516	0.715884
-2.588834	-2.015641	3.961293	0.000575	0.715882
-2.386440	-2.006573	3.971290	0.000538	0.715971
-1.768081	-2.035776	3.981286	0.000422	0.716132
-1.647660	-2.057026	3.991283	0.000400	0.716132
-1.953980	-2.000917	4.001280	0.000457	0.716135
-1.480090	-1.927646	4.011277	0.000369	0.716448
-1.446979	-1.934408	4.021274	0.000363	0.716446
-1.414003	-1.920267	4.031270	0.000356	0.716485
-1.406050	-1.783978	4.041267	0.000355	0.716758
-1.082088	-1.841641	4.051264	0.000295	0.716758
-1.091414	-1.729555	4.061261	0.000296	0.716977
-1.146615	-1.667261	4.071258	0.000307	0.717080
-0.924903	-1.629628	4.081254	0.000265	0.717233
-0.904017	-1.559408	4.091251	0.000261	0.717379
-0.831167	-1.488112	4.101248	0.000248	0.717546
-0.779307	-1.417327	4.111245	0.000238	0.717704
-0.804054	-1.299421	4.121242	0.000243	0.717928
-0.847771	-1.232774	4.131238	0.000251	0.718045
-0.709142	-1.101254	4.141235	0.000225	0.718353
-0.700572	-1.020610	4.151232	0.000223	0.718515
-0.550818	-0.966598	4.161229	0.000195	0.718675
-0.686898	-0.798410	4.171226	0.000220	0.718959
-0.523509	-0.710960	4.181222	0.000190	0.719189
-0.456690	-0.609563	4.191219	0.000177	0.719412
-0.329942	-0.510675	4.201216	0.000154	0.719651
-0.484977	-0.356487	4.211213	0.000183	0.719901
-0.404239	-0.213377	4.221210	0.000167	0.720211
-0.325251	-0.090725	4.231206	0.000153	0.720480
-0.142332	0.024152	4.241203	0.000118	0.720771
0.000000	0.147365	4.251200	0.000092	0.721063

-0.066753	0.788821	4.256205	0.000104	0.722300
-0.069942	2.058821	4.261210	0.000104	0.724789
0.332936	3.847404	4.266214	0.000028	0.728421
0.431331	6.242127	4.271219	0.000008	0.733104
0.618586	9.127615	4.276224	-0.000029	0.738730
0.947259	12.462314	4.281229	-0.000092	0.745217
1.256463	16.260334	4.286234	-0.000153	0.752515
1.605657	20.456308	4.291238	-0.000220	0.760499
1.887124	25.055900	4.296243	-0.000276	0.769123
2.690713	29.938484	4.301248	-0.000428	0.778335
3.182075	35.227573	4.306253	-0.000523	0.788072
3.520299	40.858021	4.311258	-0.000590	0.798248
4.085971	46.755827	4.316262	-0.000699	0.808835
4.700414	52.924863	4.321267	-0.000818	0.819770
5.370131	59.363954	4.326272	-0.000947	0.831038
6.310685	65.980267	4.331277	-0.001126	0.842534
6.765168	72.907051	4.336282	-0.001215	0.854248
7.544969	79.991361	4.341286	-0.001365	0.866155
8.097310	87.297996	4.346291	-0.001473	0.878195
8.731706	94.768662	4.351296	-0.001596	0.890355
9.521903	102.368843	4.356301	-0.001748	0.902598
10.274641	110.127360	4.361306	-0.001893	0.914912
11.489450	117.927098	4.366310	-0.002124	0.927249
12.332298	125.913850	4.371315	-0.002286	0.939607
12.910489	134.062919	4.376320	-0.002399	0.951977
13.665505	142.258902	4.381325	-0.002545	0.964302
14.507445	150.524918	4.386330	-0.002707	0.976595
15.456345	158.873460	4.391334	-0.002889	0.988880
16.025950	167.315969	4.396339	-0.003001	1.001053
16.876879	175.766494	4.401344	-0.003165	1.013159
17.820038	184.243111	4.406349	-0.003346	1.025180
18.363197	192.829674	4.411354	-0.003453	1.037117
19.187064	201.392023	4.416358	-0.003612	1.048950
19.908378	209.987027	4.421363	-0.003752	1.060671
20.412325	218.652912	4.426368	-0.003851	1.072307
20.887544	227.307963	4.431373	-0.003945	1.083798
21.730179	235.909538	4.436378	-0.004108	1.095180
22.580651	244.525796	4.441382	-0.004272	1.106465
23.114499	253.190199	4.446387	-0.004377	1.117628
23.601556	261.872596	4.451392	-0.004473	1.128693
24.209886	270.520948	4.456397	-0.004592	1.139634
24.896564	279.170590	4.461402	-0.004726	1.150488
25.571124	287.816141	4.466406	-0.004857	1.161233
26.004696	296.456717	4.471411	-0.004943	1.171823
26.739013	305.038775	4.476416	-0.005085	1.182310
27.637888	313.603242	4.481421	-0.005258	1.192716
28.378595	322.162050	4.486426	-0.005402	1.202994
29.329028	330.711547	4.491430	-0.005584	1.213215
29.763608	339.311993	4.496435	-0.005671	1.223307
30.337886	347.907290	4.501440	-0.005784	1.233338
30.902479	356.462849	4.506445	-0.005894	1.243241
31.220991	365.032243	4.511450	-0.005959	1.253034
31.971083	373.534776	4.516454	-0.006104	1.262757
32.558709	382.044866	4.521459	-0.006219	1.272384
33.219961	390.522697	4.526464	-0.006348	1.281916
33.705034	399.027230	4.531469	-0.006444	1.291374
34.182955	407.506252	4.536474	-0.006538	1.300734
34.583587	416.056672	4.541478	-0.006618	1.310090
34.880217	424.600955	4.546483	-0.006679	1.319355
35.231825	433.032616	4.551488	-0.006750	1.328444
35.786460	441.430569	4.556493	-0.006859	1.337471
36.209754	449.819007	4.561498	-0.006943	1.346405
36.663131	458.238994	4.566502	-0.007033	1.355318
37.318468	466.569024	4.571507	-0.007161	1.364114
38.076737	474.911839	4.576512	-0.007307	1.372884
38.674857	483.270895	4.581517	-0.007424	1.381588
38.862392	491.692123	4.586522	-0.007464	1.390230
39.674237	500.005428	4.591526	-0.007621	1.398815
39.879630	508.384424	4.596531	-0.007665	1.407312
40.289443	516.734321	4.601536	-0.007746	1.415763
40.894501	525.042123	4.606541	-0.007865	1.424153
41.543889	533.344733	4.611546	-0.007991	1.432496
41.975376	541.675366	4.616550	-0.008077	1.440783
42.370690	549.997231	4.621555	-0.008156	1.449008
42.953178	558.302517	4.626560	-0.008270	1.457200
43.406307	566.609181	4.631565	-0.008359	1.465327
43.624987	574.994295	4.636570	-0.008406	1.473447
44.144765	583.267849	4.641574	-0.008508	1.481464
44.681926	591.517180	4.646579	-0.008613	1.489416
45.111530	599.809324	4.651584	-0.008698	1.497350
45.421834	608.083629	4.656589	-0.008762	1.505207
45.960617	616.335383	4.661594	-0.008867	1.513037
46.360527	624.592423	4.666598	-0.008947	1.520810
46.774422	632.834092	4.671603	-0.009030	1.528531
47.563225	641.037145	4.676608	-0.009182	1.536234
47.946306	649.302639	4.681613	-0.009259	1.543895
48.463781	657.556151	4.686618	-0.009360	1.551526
49.260651	665.757162	4.691622	-0.009514	1.559114
49.636822	673.992570	4.696627	-0.009589	1.566634
49.909191	682.274410	4.701632	-0.009646	1.574145
50.356776	690.499451	4.706637	-0.009734	1.581595
50.605275	698.754944	4.711642	-0.009786	1.589008
50.972888	707.000101	4.716646	-0.009860	1.596394
51.327572	715.207897	4.721651	-0.009931	1.603712
51.826832	723.409854	4.726656	-0.010029	1.611011
52.315459	731.621200	4.731661	-0.010126	1.618284
52.433523	739.852371	4.736666	-0.010153	1.625489
52.959564	748.102005	4.741670	-0.010256	1.632736
53.551504	756.261126	4.746675	-0.010372	1.639881
54.120630	764.419698	4.751680	-0.010483	1.646991
54.422447	772.646740	4.756685	-0.010545	1.654093
54.802592	780.822738	4.761690	-0.010621	1.661132
55.258077	789.015655	4.766694	-0.010711	1.668165
55.750686	797.204751	4.771699	-0.010808	1.675170
55.787273	805.425501	4.776704	-0.010820	1.682112
56.158376	813.604652	4.781709	-0.010895	1.689034
56.531840	821.793124	4.786714	-0.010970	1.695936
57.142594	829.935900	4.791718	-0.011089	1.702804
57.591666	838.113219	4.796723	-0.011178	1.709651
57.998157	846.297805	4.801728	-0.011259	1.716471
58.485085	854.454513	4.806733	-0.011355	1.723251
58.646962	862.632586	4.811738	-0.011390	1.729980
59.173691	870.795432	4.816742	-0.011493	1.736718
59.388155	878.974903	4.821747	-0.011539	1.743403
59.752584	887.138063	4.826752	-0.011612	1.750068
60.266394	895.300692	4.831757	-0.011713	1.756726
60.611215	903.439191	4.836762	-0.011782	1.763318
60.895235	911.618975	4.841766	-0.011841	1.769911
61.414113	919.757771	4.846771	-0.011942	1.776476
62.110486	927.873877	4.851776	-0.012077	1.783021
62.374043	936.068187	4.856781	-0.012132	1.789550
62.668393	944.276853	4.861786	-0.012192	1.796070
63.083091	952.407023	4.866790	-0.012274	1.802520
63.426220	960.527164	4.871795	-0.012344	1.808930
63.997362	968.656251	4.876800	-0.012455	1.815351
64.306029	976.805790	4.881805	-0.012518	1.821735
64.424782	984.976820	4.886810	-0.012546	1.828090
65.035803	993.104316	4.891814	-0.012665	1.834447
65.399730	1001.221880	4.896819	-0.012738	1.840746
65.713520	1009.365333	4.901824	-0.012801	1.847037
65.999176	1017.536485	4.906829	-0.012860	1.853324
66.413986	1025.637186	4.911834	-0.012942	1.859552
66.903507	1033.770071	4.916838	-0.013039	1.865791
67.187693	1041.949214	4.921843	-0.013097	1.872021
67.602108	1050.069359	4.926848	-0.013180	1.878201
68.081832	1058.168064	4.931853	-0.013274	1.884352
68.361363	1066.307671	4.936858	-0.013331	1.890490
68.575771	1074.479093	4.941862	-0.013377	1.896625
68.755977	1082.599731	4.946867	-0.013416	1.902698
69.582359	1090.668170	4.951872	-0.013575	1.908786
69.938583	1098.827084	4.956877	-0.013646	1.914868
70.200714	1106.939669	4.961882	-0.013700	1.920887
70.534845	1115.061348	4.966886	-0.013768	1.926901
70.737095	1123.207283	4.971891	-0.013811	1.932899
71.210740	1131.300465	4.976896	-0.013904	1.938871
71.882876	1139.364102	4.981901	-0.014035	1.944824
72.031708	1147.554838	4.986906	-0.014068	1.950794
72.687806	1155.657223	4.991910	-0.014195	1.956736
73.002426	1163.750910	4.996915	-0.014259	1.962618
73.335932	1171.854619	5.001920	-0.014327	1.968491
73.704159	1179.980697	5.006925	-0.014400	1.974366
74.246697	1188.044616	5.011930	-0.014507	1.980198
74.552649	1196.167144	5.016934	-0.014569	1.986029
74.838235	1204.296426	5.021939	-0.014627	1.991845
74.976842	1212.442268	5.026944	-0.014658	1.997641
75.451632	1220.523151	5.031949	-0.014752	2.003409
75.815533	1228.620016	5.036954	-0.014825	2.009161
76.139844	1236.751592	5.041958	-0.014891	2.014916
76.440238	1244.852974	5.046963	-0.014952	2.020631
76.965317	1252.925632	5.051968	-0.015055	2.026333
77.496445	1261.044111	5.056973	-0.015159	2.032051
77.666840	1269.166869	5.061978	-0.015196	2.037719
78.062570	1277.247510	5.066982	-0.015275	2.043365
78.359227	1285.346175	5.071987	-0.015336	2.048998
78.612454	1293.468989	5.076992	-0.015388	2.054628
79.081117	1301.540963	5.081997	-0.015481	2.060229
79.212453	1309.657269	5.087002	-0.015510	2.065811
79.469364	1317.790567	5.092006	-0.015564	2.071402
79.805644	1325.872877	5.097011	-0.015632	2.076951
80.179688	1333.940583	5.102016	-0.015706	2.082479
80.465449	1342.057150	5.107021	-0.015765	2.088017
80.863095	1350.136779	5.112026	-0.015844	2.093526
81.174565	1358.250976	5.117030	-0.015907	2.099036
81.406086	1366.334502	5.122035	-0.015956	2.104502
81.521894	1374.476686	5.127040	-0.015983	2.109982
82.103422	1382.593186	5.132045	-0.016096	2.115476
82.285919	1390.660150	5.137050	-0.016136	2.120885
82.429432	1398.751832	5.142054	-0.016168	2.126292
82.882183	1406.815528	5.147059	-0.016257	2.131696
83.211525	1414.894674	5.152064	-0.016324	2.137085
83.720228	1422.945358	5.157069	-0.016424	2.142458
84.106112	1431.004162	5.162074	-0.016501	2.147812
84.325628	1439.147785	5.167078	-0.016547	2.153192
84.651990	1447.217418	5.172083	-0.016613	2.158520
84.896305	1455.281724	5.177088	-0.016664	2.163824
85.103889	1463.398519	5.182093	-0.016708	2.169146
85.304164	1471.500483	5.187098	-0.016750	2.174444
85.848662	1479.550871	5.192102	-0.016857	2.179728
86.245732	1487.617302	5.197107	-0.016936	2.184996
86.636725	1495.717171	5.202112	-0.017014	2.190271
86.710618	1503.873743	5.207117	-0.017033	2.195542
87.007759	1511.912607	5.212122	-0.017094	2.200745
87.575207	1519.938672	5.217126	-0.017205	2.205951
87.825434	1528.041012	5.222131	-0.017256	2.211166
88.136816	1536.133534	5.227136	-0.017320	2.216367
88.524687	1544.210055	5.232141	-0.017397	2.221553
88.949562	1552.257321	5.237146	-0.017482	2.226711
89.560196	1560.327084	5.242150	-0.017601	2.231888
89.900723	1568.417798	5.247155	-0.017669	2.237042
90.149501	1576.488802	5.252160	-0.017721	2.242164
90.604313	1584.569786	5.257165	-0.017811	2.247298
90.724952	1592.673656	5.262170	-0.017838	2.252405
91.008342	1600.758187	5.267174	-0.017897	2.257504
91.100345	1608.856596	5.272179	-0.017919	2.262582
91.517904	1616.909354	5.277184	-0.018002	2.267649
92.024662	1625.050059	5.282189	-0.018102	2.272767
92.116886	1633.130130	5.287194	-0.018124	2.277800
92.488492	1641.168402	5.292198	-0.018198	2.282820
92.655566	1649.238718	5.297203	-0.018235	2.287831
93.024428	1657.302857	5.302208	-0.018309	2.292844
93.289908	1665.377587	5.307213	-0.018363	2.297844
93.591580	1673.426006	5.312218	-0.018425	2.302821
94.067062	1681.481200	5.317222	-0.018519	2.307805
94.358074	1689.579669	5.322227	-0.018578	2.312789
94.359022	1697.673100	5.327232	-0.018584	2.317735
94.761035	1705.711891	5.332237	-0.018664	2.322671
95.012563	1713.773695	5.337242	-0.018716	2.327598
95.459009	1721.853756	5.342246	-0.018804	2.332541
95.585832	1729.934650	5.347251	-0.018833	2.337448
95.725550	1738.004512	5.352256	-0.018864	2.342339
96.221346	1746.039700	5.357261	-0.018962	2.347228
96.365577	1754.152563	5.362266	-0.018994	2.352125
96.778948	1762.213549	5.367270	-0.019076	2.357002
96.894280	1770.267392	5.372275	-0.019103	2.361841
97.331882	1778.299095	5.377280	-0.019190	2.366683
97.533302	1786.399490	5.382285	-0.019232	2.371536
97.779122	1794.465823	5.387290	-0.019283	2.376363
97.952189	1802.528807	5.392294	-0.019321	2.381173
98.270491	1810.581119	5.397299	-0.019385	2.385977
99.062205	1818.585999	5.402304	-0.019538	2.390782
99.298399	1826.706336	5.407309	-0.019587	2.395601
99.476084	1834.757768	5.412314	-0.019626	2.400365
99.993136	1842.794171	5.417318	-0.019727	2.405137
100.316929	1850.877385	5.422323	-0.019793	2.409912
100.418775	1858.987423	5.427328	-0.019817	2.414676
100.623707	1867.055564	5.432333	-0.019860	2.419414
100.904932	1875.094517	5.437338	-0.019918	2.424132
101.300411	1883.168251	5.442342	-0.019997	2.428869
101.675641	1891.291842	5.447347	-0.020072	2.433625
102.082085	1899.309073	5.452352	-0.020153	2.438312
102.519654	1907.337364	5.457357	-0.020240	2.442999
102.422768	1915.414901	5.462362	-0.020227	2.447664
102.904459	1923.458630	5.467366	-0.020322	2.452345
103.023002	1931.547215	5.472371	-0.020349	2.457015
103.393336	1939.568877	5.477376	-0.020423	2.461657
103.562543	1947.647455	5.482381	-0.020460	2.466307
103.857423	1955.703730	5.487386	-0.020520	2.470946
103.940531	1963.804029	5.492390	-0.020541	2.475585
104.382851	1971.801411	5.497395	-0.020629	2.480183
104.666798	1979.856162	5.502400	-0.020687	2.484793
104.975406	1987.923688	5.507405	-0.020749	2.489404
105.291753	1995.999321	5.512410	-0.020814	2.494012
105.631505	2004.047638	5.517414	-0.020882	2.498597
105.894195	2012.107103	5.522419	-0.020936	2.503175
106.067934	2020.181893	5.527424	-0.020974	2.507746
106.140828	2028.307810	5.532429	-0.020993	2.512330
106.321327	2036.344795	5.537434	-0.021032	2.516864
106.637135	2044.366782	5.542438	-0.021096	2.521391
107.003582	2052.404150	5.547443	-0.021169	2.525922
107.487774	2060.422130	5.552448	-0.021264	2.530442
108.109911	2068.489452	5.557453	-0.021386	2.534992
108.274667	2076.526025	5.562458	-0.021421	2.539484
108.502031	2084.588618	5.567462	-0.021469	2.543986
108.701116	2092.672898	5.572467	-0.021511	2.548491
109.174114	2100.717389	5.577472	-0.021605	2.552985
109.412067	2108.774823	5.582477	-0.021654	2.557461
109.682346	2116.801154	5.587482	-0.021710	2.561915
110.014803	2124.849346	5.592486	-0.021777	2.566377
110.062974	2132.951891	5.597491	-0.021791	2.570842
110.083812	2141.032778	5.602496	-0.021800	2.575285
110.426793	2149.073731	5.607501	-0.021869	2.579720
110.685152	2157.092594	5.612506	-0.021923	2.584131
111.025419	2165.164192	5.617510	-0.021991	2.588568
111.369005	2173.365356	5.622515	-0.022061	2.593068
111.547217	2181.423329	5.627520	-0.022099	2.597471
111.913687	2189.396346	5.632525	-0.022173	2.601833
112.075332	2197.415981	5.637530	-0.022208	2.606199
112.560365	2205.427369	5.642534	-0.022303	2.610576
112.772319	2213.480367	5.647539	-0.022348	2.614949
112.937657	2221.504191	5.652544	-0.022384	2.619295
113.578638	2229.531773	5.657549	-0.022509	2.623669
113.705005	2237.589493	5.662554	-0.022537	2.628017
113.655142	2245.694023	5.667558	-0.022533	2.632371
114.130071	2253.712332	5.672563	-0.022627	2.636706
114.454792	2261.734629	5.677568	-0.022693	2.641026
114.572238	2269.818509	5.682573	-0.022720	2.645359
114.885029	2277.835889	5.687578	-0.022783	2.649662
115.214556	2285.899600	5.692582	-0.022850	2.653983
115.372384	2293.947182	5.697587	-0.022885	2.658278
115.493360	2302.002973	5.702592	-0.022912	2.662567
115.694961	2310.077905	5.707597	-0.022955	2.666866
115.798285	2318.147285	5.712602	-0.022980	2.671147
115.896941	2326.225523	5.717606	-0.023003	2.675427
116.358180	2334.210651	5.722611	-0.023094	2.679673
116.562049	2342.236341	5.727616	-0.023138	2.683918
117.086140	2350.280654	5.732621	-0.023240	2.688186
117.219655	2358.328151	5.737626	-0.023271	2.692424
117.648768	2366.378982	5.742630	-0.023356	2.696676
117.932566	2374.435218	5.747635	-0.023414	2.700915
117.974772	2382.484928	5.752640	-0.023427	2.705128
118.220083	2390.537814	5.757645	-0.023478	2.709349
118.549057	2398.587398	5.762650	-0.023544	2.713568
118.748703	2406.648365	5.767654	-0.023587	2.717777
119.017365	2414.676452	5.772659	-0.023642	2.721967
119.322556	2422.698271	5.777664	-0.023704	2.726150
119.701611	2430.758169	5.782669	-0.023780	2.730350
119.670322	2438.836573	5.787674	-0.023779	2.734528
120.058072	2446.860095	5.792678	-0.023857	2.738697
120.244988	2454.912581	5.797683	-0.023897	2.742863
120.669748	2462.919589	5.802688	-0.023981	2.747013
121.157196	2470.995347	5.807693	-0.024077	2.751196
121.422998	2479.103100	5.812698	-0.024132	2.755375
121.602718	2487.104870	5.817702	-0.024171	2.759488
121.695377	2495.141118	5.822707	-0.024193	2.763608
121.965074	2503.146662	5.827712	-0.024249	2.767717
122.174148	2511.219712	5.832717	-0.024293	2.771850
122.185839	2519.282635	5.837722	-0.024300	2.775960
122.697576	2527.286309	5.842726	-0.024401	2.780064
122.883092	2535.319799	5.847731	-0.024440	2.784157
123.046692	2543.368387	5.852736	-0.024476	2.788251
123.387619	2551.434841	5.857741	-0.024545	2.792358
123.790032	2559.453137	5.862746	-0.024625	2.796438
123.892810	2567.498858	5.867750	-0.024649	2.800508
124.092621	2575.519754	5.872755	-0.024692	2.804566
124.380430	2583.560229	5.877760	-0.024751	2.808633
124.784887	2591.630783	5.882765	-0.024831	2.812715
124.953021	2599.682591	5.887770	-0.024868	2.816769
125.247157	2607.711715	5.892774	-0.024928	2.820812
125.680717	2615.715982	5.897779	-0.025014	2.824846
125.824712	2623.785647	5.902784	-0.025046	2.828889
126.348500	2631.849267	5.907789	-0.025149	2.832946
126.236163	2639.917622	5.912794	-0.025133	2.836963
126.549788	2647.932612	5.917798	-0.025196	2.840971
126.797825	2655.951468	5.922803	-0.025248	2.844972
127.022435	2663.983152	5.927808	-0.025295	2.848973
127.277956	2672.064347	5.932813	-0.025348	2.852994
127.390445	2680.093738	5.937818	-0.025374	2.856976
127.697439	2688.128270	5.942822	-0.025436	2.860965
127.966457	2696.148094	5.947827	-0.025492	2.864940
127.963901	2704.209718	5.952832	-0.025496	2.868915
128.348786	2712.273344	5.957837	-0.025573	2.872906
128.520333	2720.315733	5.962842	-0.025611	2.876870
128.773265	2728.346857	5.967846	-0.025663	2.880827
129.015494	2736.359779	5.972851	-0.025713	2.884769
129.277705	2744.400717	5.977856	-0.025767	2.888721
129.490559	2752.464052	5.982861	-0.025812	2.892675
129.567797	2760.516485	5.987866	-0.025832	2.896611
129.955671	2768.541666	5.992870	-0.025909	2.900546
130.240402	2776.548307	5.997875	-0.025967	2.904460
130.369594	2784.622267	6.002880	-0.025997	2.908393
130.449467	2792.752553	6.007885	-0.026017	2.912346
130.779886	2800.771042	6.012890	-0.026084	2.916253
131.016481	2808.757877	6.017894	-0.026133	2.920134
131.286395	2816.776364	6.022899	-0.026188	2.924026
131.352896	2824.808542	6.027904	-0.026206	2.927910
131.657563	2832.868156	6.032909	-0.026268	2.931814
131.729865	2840.923164	6.037914	-0.026287	2.935698
131.974132	2848.907837	6.042918	-0.026337	2.939553
132.403151	2856.940272	6.047923	-0.026423	2.943435
132.427509	2864.973392	6.052928	-0.026432	2.947291
132.754713	2873.042291	6.057933	-0.026498	2.951174
133.142193	2881.052823	6.062938	-0.026576	2.955028
133.290666	2889.093266	6.067942	-0.026609	2.958879
133.563380	2897.131549	6.072947	-0.026665	2.962730
133.596154	2905.170184	6.077952	-0.026676	2.966564
134.094274	2913.202135	6.082957	-0.026774	2.970413
134.293521	2921.245897	6.087962	-0.026816	2.974248
134.670221	2929.260135	6.092966	-0.026892	2.978073
134.980622	2937.301835	6.097971	-0.026955	2.981902
135.258554	2945.331119	6.102976	-0.027012	2.985719
135.528500	2953.388851	6.107981	-0.027067	2.989544
135.507583	2961.479315	6.112986	-0.027069	2.993365
135.815311	2969.483732	6.117990	-0.027131	2.997157
136.075316	2977.522726	6.122995	-0.027185	3.000958
136.362521	2985.488864	6.128000	-0.027244	3.004721
136.786636	2993.537796	6.133005	-0.027328	3.008526
136.901671	3001.618322	6.138010	-0.027354	3.012325
136.958048	3009.672626	6.143014	-0.027370	3.016103
137.333911	3017.667580	6.148019	-0.027445	3.019865
137.594435	3025.685432	6.153024	-0.027499	3.023628
137.658823	3033.778690	6.158029	-0.027516	3.027411
137.744997	3041.830288	6.163034	-0.027538	3.031171
138.056084	3049.844418	6.168038	-0.027601	3.034920
138.388082	3057.857056	6.173043	-0.027668	3.038665
138.511424	3065.873135	6.178048	-0.027696	3.042396
138.928805	3073.929975	6.183053	-0.027779	3.046156
139.053337	3081.961845	6.188058	-0.027807	3.049885
139.146103	3090.023755	6.193062	-0.027830	3.053623
139.420593	3098.048549	6.198067	-0.027886	3.057347
139.478080	3106.066311	6.203072	-0.027902	3.061053
139.647998	3114.110077	6.208077	-0.027939	3.064772
139.977025	3122.133210	6.213082	-0.028006	3.068484
140.187401	3130.249612	6.218086	-0.028050	3.072230
140.535003	3138.313811	6.223091	-0.028120	3.075952
140.798002	3146.264555	6.228096	-0.028174	3.079615
141.098756	3154.274214	6.233101	-0.028235	3.083302
141.202374	3162.308118	6.238106	-0.028260	3.086986
141.520424	3170.331382	6.243110	-0.028324	3.090671
141.671228	3178.390827	6.248115	-0.028358	3.094360
141.844968	3186.424125	6.253120	-0.028395	3.098034
141.948743	3194.461745	6.258125	-0.028420	3.101702
142.218426	3202.467606	6.263130	-0.028475	3.105360
142.609364	3210.497022	6.268134	-0.028553	3.109029
142.651232	3218.572362	6.273139	-0.028566	3.112698
142.749942	3226.616477	6.278144	-0.028590	3.116352
143.168480	3234.627245	6.283149	-0.028673	3.120001
143.310708	3242.640529	6.288154	-0.028705	3.123634
143.410190	3250.673676	6.293158	-0.028729	3.127269
143.886705	3258.706620	6.298163	-0.028823	3.130918
144.108813	3266.745890	6.303168	-0.028869	3.134553
144.362445	3274.775559	6.308173	-0.028922	3.138182
144.452931	3282.818890	6.313178	-0.028944	3.141805
144.630638	3290.830334	6.318182	-0.028982	3.145413
144.813443	3298.874929	6.323187	-0.029021	3.149033
144.933189	3306.934344	6.328192	-0.029049	3.152652
145.287111	3314.981646	6.333197	-0.029120	3.156271
145.525950	3322.941338	6.338202	-0.029170	3.159843
145.531006	3330.972715	6.343206	-0.029176	3.163432
145.976079	3338.995764	6.348211	-0.029264	3.167032
146.196490	3347.052009	6.353216	-0.029310	3.170633
146.193776	3355.113819	6.358221	-0.029315	3.174223
146.651431	3363.120039	6.363226	-0.029405	3.177804
146.951410	3371.141548	6.368230	-0.029466	3.181381
147.120765	3379.177736	6.373235	-0.029503	3.184955
146.894599	3387.226392	6.378240	-0.029466	3.188513
147.347234	3395.278316	6.383245	-0.029556	3.192098
147.782637	3403.291026	6.388250	-0.029642	3.195660
147.831062	3411.308018	6.393254	-0.029656	3.199204
148.058307	3419.357999	6.398259	-0.029704	3.202767
148.192183	3427.373476	6.403264	-0.029734	3.206306
148.540137	3435.430835	6.408269	-0.029804	3.209868
148.602257	3443.479568	6.413274	-0.029821	3.213411
148.779943	3451.512114	6.418278	-0.029859	3.216948
148.793121	3459.546996	6.423283	-0.029867	3.220475
148.931566	3467.514821	6.428288	-0.029898	3.223974
149.437077	3475.556871	6.433293	-0.029997	3.227516
149.515970	3483.607883	6.438298	-0.030017	3.231041
149.697417	3491.696060	6.443302	-0.030056	3.234583
150.024120	3499.694521	6.448307	-0.030122	3.238087
150.431474	3507.667101	6.453312	-0.030203	3.241580
150.718629	3515.666076	6.458317	-0.030262	3.245075
150.619368	3523.722473	6.463322	-0.030249	3.248576
150.770395	3531.785273	6.468326	-0.030282	3.252086
150.924895	3539.847910	6.473331	-0.030316	3.255593
151.220397	3547.797599	6.478336	-0.030376	3.259052
151.322755	3555.847143	6.483341	-0.030401	3.262543
151.431534	3563.892506	6.488346	-0.030426	3.266028
151.568971	3571.927288	6.493350	-0.030457	3.269507
151.971843	3579.979075	6.498355	-0.030537	3.273000
152.048862	3588.007729	6.503360	-0.030557	3.276466
152.205807	3596.030430	6.508365	-0.030591	3.279929
152.297464	3604.042201	6.513370	-0.030614	3.283381
152.600716	3612.038260	6.518374	-0.030675	3.286830
152.827918	3620.092634	6.523379	-0.030723	3.290299
152.807743	3628.150933	6.528384	-0.030724	3.293755
153.292343	3636.164385	6.533389	-0.030820	3.297209
153.459509	3644.174774	6.538394	-0.030856	3.300645
153.498484	3652.182410	6.543398	-0.030869	3.304071
153.770074	3660.241984	6.548403	-0.030924	3.307525
154.046751	3668.251851	6.553408	-0.030981	3.310954
154.479506	3676.336166	6.558413	-0.031067	3.314417
154.831732	3684.318209	6.563418	-0.031138	3.317830
155.012758	3692.361950	6.568422	-0.031177	3.321259
155.578237	3700.340517	6.573427	-0.031287	3.324672
155.719468	3708.376653	6.578432	-0.031319	3.328089
155.734637	3716.445444	6.583437	-0.031327	3.331512
155.860824	3724.487024	6.588442	-0.031356	3.334924
156.068581	3732.464839	6.593446	-0.031399	3.338309
156.274989	3740.528537	6.598451	-0.031443	3.341726
156.352439	3748.523819	6.603456	-0.031463	3.345106
156.674263	3756.565235	6.608461	-0.031528	3.348511
156.686198	3764.641097	6.613466	-0.031535	3.351916
157.002113	3772.664054	6.618470	-0.031599	3.355307
157.422041	3780.655873	6.623475	-0.031683	3.358684
157.517160	3788.696520	6.628480	-0.031706	3.362067
157.853570	3796.698568	6.633485	-0.031774	3.365438
157.917272	3804.744821	6.638490	-0.031791	3.368815
158.112526	3812.780491	6.643494	-0.031832	3.372189
158.329319	3820.844860	6.648499	-0.031878	3.375573
158.542781	3828.828075	6.653504	-0.031923	3.378919
158.857279	3836.870555	6.658509	-0.031987	3.382289
159.106259	3844.904307	6.663514	-0.032038	3.385651
159.047754	3852.925689	6.668518	-0.032033	3.388993
159.310789	3861.041866	6.673523	-0.032087	3.392382
159.419406	3869.080932	6.678528	-0.032112	3.395731
159.666881	3877.024666	6.683533	-0.032164	3.399042
159.768019	3885.044928	6.688538	-0.032188	3.402376
160.252334	3893.035095	6.693542	-0.032283	3.405707
160.453592	3901.050870	6.698547	-0.032326	3.409036
160.600855	3909.100193	6.703552	-0.032358	3.412374
160.774175	3917.167396	6.708557	-0.032396	3.415717
160.981743	3925.131663	6.713562	-0.032440	3.419015
161.035510	3933.190566	6.718566	-0.032455	3.422343
161.425114	3941.189558	6.723571	-0.032533	3.425656
161.458200	3949.195438	6.728576	-0.032544	3.428955
161.753443	3957.297606	6.733581	-0.032604	3.432300
162.244693	3965.278622	6.738586	-0.032701	3.435598
162.555344	3973.248817	6.743590	-0.032764	3.438883
162.816508	3981.312243	6.748595	-0.032818	3.442201
163.115710	3989.330976	6.753600	-0.032879	3.445499
163.433449	3997.364425	6.758605	-0.032943	3.448800
163.491797	4005.428203	6.763610	-0.032959	3.452102
163.750972	4013.475915	6.768614	-0.033013	3.455401
164.005185	4021.496666	6.773619	-0.033065	3.458685
164.123515	4029.511567	6.778624	-0.033093	3.461959
164.240648	4037.546473	6.783629	-0.033120	3.465239
164.528817	4045.577705	6.788634	-0.033179	3.468519
164.619870	4053.642350	6.793638	-0.033201	3.471803
164.691530	4061.693938	6.798643	-0.033219	3.475079
164.684533	4069.677099	6.803648	-0.033223	3.478321
165.109434	4077.685164	6.808653	-0.033308	3.481583
165.171345	4085.696421	6.813658	-0.033324	3.484833
165.242007	4093.681338	6.818662	-0.033343	3.488069
165.668203	4101.756993	6.823667	-0.033427	3.491350
165.645975	4109.776622	6.828672	-0.033428	3.494591
165.986872	4117.795464	6.833677	-0.033497	3.497840
166.107291	4125.823606	6.838682	-0.033525	3.501082
166.330342	4133.814090	6.843686	-0.033572	3.504310
166.747973	4141.848170	6.848691	-0.033655	3.507559
166.864893	4149.895275	6.853696	-0.033682	3.510800
167.153030	4157.928135	6.858701	-0.033740	3.514038
167.073982	4165.953991	6.863706	-0.033731	3.517259
167.209824	4173.976926	6.868710	-0.033761	3.520482
167.540201	4181.969807	6.873715	-0.033828	3.523696
167.635883	4189.991949	6.878720	-0.033851	3.526911
167.916049	4198.041772	6.883725	-0.033909	3.530141
168.212428	4206.058805	6.888730	-0.033969	3.533355
168.458672	4214.065960	6.893734	-0.034020	3.536560
168.545611	4222.153584	6.898739	-0.034042	3.539790
168.605456	4230.167631	6.903744	-0.034058	3.542986
168.926142	4238.189746	6.908749	-0.034123	3.546191
169.249013	4246.164164	6.913754	-0.034188	3.549374
169.433106	4254.285894	6.918758	-0.034228	3.552608
169.663657	4262.375482	6.923763	-0.034276	3.555828
169.805696	4270.308303	6.928768	-0.034308	3.558981
169.891656	4278.342191	6.933773	-0.034329	3.562169
170.018943	4286.324284	6.938778	-0.034358	3.565334
170.127056	4294.327576	6.943782	-0.034383	3.568505
170.149669	4302.432800	6.948787	-0.034393	3.571711
170.546941	4310.388969	6.953792	-0.034472	3.574865
170.906172	4318.416857	6.958797	-0.034544	3.578045
171.160564	4326.461291	6.963802	-0.034596	3.581224
171.179636	4334.421523	6.968806	-0.034605	3.584361
171.444301	4342.498655	6.973811	-0.034660	3.587549
171.558891	4350.515344	6.978816	-0.034686	3.590705
171.630317	4358.562927	6.983821	-0.034705	3.593869
171.823056	4366.583452	6.988826	-0.034746	3.597024
172.090790	4374.543620	6.993830	-0.034801	3.600154
172.350514	4382.599079	6.998835	-0.034855	3.603318
172.140921	4390.621082	7.003840	-0.034821	3.606454
172.385333	4398.646382	7.008845	-0.034872	3.609601
172.486597	4406.701755	7.013850	-0.034896	3.612752
172.699911	4414.712293	7.018854	-0.034941	3.615887
172.838030	4422.739199	7.023859	-0.034972	3.619023
173.095978	4430.733452	7.028864	-0.035025	3.622147
173.470848	4438.757785	7.033869	-0.035100	3.625283
173.703270	4446.799223	7.038874	-0.035148	3.628419
174.056551	4454.824025	7.043878	-0.035219	3.631549
174.364957	4462.885572	7.048883	-0.035282	3.634689
174.352701	4470.885594	7.053888	-0.035285	3.637794
174.648034	4478.928319	7.058893	-0.035345	3.640922
174.843613	4486.897137	7.063898	-0.035387	3.644015
174.940332	4494.915125	7.068902	-0.035410	3.647122
175.148251	4502.973537	7.073907	-0.035454	3.650245
175.201538	4511.016412	7.078912	-0.035469	3.653355
175.503038	4519.041131	7.083917	-0.035530	3.656462
175.562787	4527.048810	7.088922	-0.035547	3.659553
175.573439	4535.056906	7.093926	-0.035554	3.662641
175.835694	4543.115545	7.098931	-0.035608	3.665752
176.093350	4551.106806	7.103936	-0.035661	3.668835
176.062228	4559.171460	7.108941	-0.035661	3.671935
176.429793	4567.198274	7.113946	-0.035734	3.675029
176.521875	4575.174801	7.118950	-0.035757	3.678093
176.762801	4583.223005	7.123955	-0.035807	3.681186
176.943682	4591.199779	7.128960	-0.035846	3.684248
177.091366	4599.271120	7.133965	-0.035878	3.687343
177.352480	4607.269974	7.138970	-0.035932	3.690410
177.584465	4615.297952	7.143974	-0.035981	3.693485
177.626805	4623.358286	7.148979	-0.035994	3.696565
177.573521	4631.354712	7.153984	-0.035989	3.699615
177.946861	4639.363408	7.158989	-0.036064	3.702678
178.336110	4647.392628	7.163994	-0.036142	3.705747
178.336516	4655.394065	7.168998	-0.036147	3.708793
178.461839	4663.491703	7.174003	-0.036176	3.711877
178.611746	4671.537846	7.179008	-0.036209	3.714938
178.787907	4679.515811	7.184013	-0.036247	3.717972
178.918618	4687.526343	7.189018	-0.036276	3.721015
179.002992	4695.463259	7.194022	-0.036297	3.724026
179.365078	4703.532376	7.199027	-0.036370	3.727092
179.384342	4711.557504	7.204032	-0.036379	3.730130
179.420823	4719.611221	7.209037	-0.036391	3.733177
179.618345	4727.646479	7.214042	-0.036433	3.736218
179.626094	4735.604390	7.219046	-0.036439	3.739223
179.889812	4743.660244	7.224051	-0.036494	3.742268
180.094272	4751.629559	7.229056	-0.036537	3.745277
180.370086	4759.683842	7.234061	-0.036593	3.748317
180.701102	4767.771232	7.239066	-0.036660	3.751369
180.910073	4775.757488	7.244070	-0.036705	3.754377
181.294627	4783.788425	7.249075	-0.036781	3.757403
181.030113	4791.805322	7.254080	-0.036737	3.760407
181.052828	4799.825012	7.259085	-0.036747	3.763416
181.233085	4807.871477	7.264090	-0.036786	3.766436
181.662080	4815.840073	7.269094	-0.036871	3.769431
181.663363	4823.908853	7.274099	-0.036876	3.772450
181.953181	4831.895590	7.279104	-0.036935	3.775443
182.159689	4839.945669	7.284109	-0.036979	3.778456
182.154405	4848.008352	7.289114	-0.036983	3.781466
182.289845	4855.955136	7.294118	-0.037014	3.784433
182.553338	4864.022884	7.299123	-0.037068	3.787446
182.586171	4872.037163	7.304128	-0.037079	3.790432
182.847140	4880.077767	7.309133	-0.037133	3.793430
183.084178	4888.151472	7.314138	-0.037183	3.796437
183.361128	4896.072139	7.319142	-0.037239	3.799386
183.429699	4904.119052	7.324147	-0.037257	3.802375
183.475887	4912.113032	7.329152	-0.037271	3.805342
183.858587	4920.096936	7.334157	-0.037348	3.808309
183.992330	4928.184412	7.339162	-0.037378	3.811308
184.161976	4936.185936	7.344166	-0.037415	3.814273
184.419014	4944.234306	7.349171	-0.037468	3.817255
184.421449	4952.194768	7.354176	-0.037473	3.820196
184.532440	4960.214332	7.359181	-0.037499	3.823160
184.987307	4968.242444	7.364186	-0.037589	3.826131
185.191789	4976.246424	7.369190	-0.037632	3.829086
185.324087	4984.349824	7.374195	-0.037662	3.832074
185.507361	4992.320104	7.379200	-0.037702	3.835011
185.835400	5000.329993	7.384205	-0.037768	3.837964
186.149480	5008.357185	7.389210	-0.037832	3.840921
186.155730	5016.339126	7.394214	-0.037838	3.843852
186.486705	5024.408557	7.399219	-0.037905	3.846820
186.747465	5032.426109	7.404224	-0.037959	3.849765
186.941622	5040.475791	7.409229	-0.038000	3.852718
186.851445	5048.541536	7.414234	-0.037988	3.855669
187.185300	5056.514009	7.419238	-0.038056	3.858592
187.492842	5064.518906	7.424243	-0.038118	3.861524
187.486321	5072.531014	7.429248	-0.038122	3.864450
187.813748	5080.588274	7.434253	-0.038189	3.867397
187.887719	5088.638233	7.439258	-0.038208	3.870335
188.017545	5096.845586	7.444262	-0.038237	3.873328
188.108735	5104.871026	7.449267	-0.038259	3.876252
188.301258	5112.728871	7.454272	-0.038300	3.879115
188.485222	5120.741677	7.459277	-0.038340	3.882032
188.770449	5128.711335	7.464282	-0.038398	3.884933
189.062310	5136.705651	7.469286	-0.038458	3.887841
188.889310	5144.781574	7.474291	-0.038431	3.890767
188.960900	5152.797147	7.479296	-0.038449	3.893674
189.339997	5160.841333	7.484301	-0.038525	3.896595
189.352796	5168.804832	7.489306	-0.038533	3.899477
189.376413	5176.840162	7.494310	-0.038542	3.902384
189.813843	5184.831403	7.499315	-0.038629	3.905280
190.090913	5192.844885	7.504320	-0.038686	3.908179
190.330400	5200.900142	7.509325	-0.038736	3.911090
190.342200	5208.961992	7.514330	-0.038743	3.913998
190.556666	5216.946628	7.519334	-0.038788	3.916879
190.792747	5224.923124	7.524339	-0.038837	3.919755
190.794421	5232.951390	7.529344	-0.038843	3.922643
191.215597	5240.960803	7.534349	-0.038926	3.925531
191.205695	5248.995499	7.539354	-0.038930	3.928417
191.210986	5257.008373	7.544358	-0.038936	3.931294
191.536860	5265.052821	7.549363	-0.039002	3.934185
191.699670	5273.076637	7.554368	-0.039037	3.937064
191.890122	5281.077125	7.559373	-0.039078	3.939933
192.025713	5289.100216	7.564378	-0.039109	3.942807
192.378751	5297.059974	7.569382	-0.039180	3.945661
192.311158	5305.136363	7.574387	-0.039172	3.948546
192.427215	5313.186897	7.579392	-0.039199	3.951423
192.757758	5321.222379	7.584397	-0.039266	3.954297
193.008963	5329.223049	7.589402	-0.039318	3.957154
192.838060	5337.193978	7.594406	-0.039291	3.959992
193.144431	5345.222951	7.599411	-0.039354	3.962856
193.422546	5353.222367	7.604416	-0.039410	3.965708
193.706270	5361.224762	7.609421	-0.039469	3.968558
193.649735	5369.308147	7.614426	-0.039463	3.971429
193.975095	5377.323821	7.619430	-0.039529	3.974281
194.304580	5385.361927	7.624435	-0.039596	3.977139
194.162047	5393.337458	7.629440	-0.039574	3.979964
194.328660	5401.371099	7.634445	-0.039611	3.982813
194.589910	5409.391156	7.639450	-0.039664	3.985657
194.774818	5417.373822	7.644454	-0.039704	3.988484
195.095288	5425.438998	7.649459	-0.039769	3.991341
195.143490	5433.478450	7.654464	-0.039783	3.994182
195.121904	5441.535703	7.659469	-0.039784	3.997026
195.328750	5449.522739	7.664474	-0.039828	3.999847
195.662994	5457.511479	7.669478	-0.039896	4.002669
195.855593	5465.549660	7.674483	-0.039937	4.005504
195.916621	5473.558754	7.679488	-0.039953	4.008324
196.084569	5481.592686	7.684493	-0.039990	4.011153
196.371567	5489.640366	7.689498	-0.040048	4.013986
196.380285	5497.658251	7.694502	-0.040055	4.016803
196.527127	5505.681876	7.699507	-0.040088	4.019622
196.801796	5513.696653	7.704512	-0.040144	4.022438
197.043079	5521.699035	7.709517	-0.040194	4.025246
197.085367	5529.747924	7.714522	-0.040208	4.028067
197.025125	5537.726650	7.719526	-0.040201	4.030859
197.620357	5545.842265	7.724531	-0.040318	4.033706
197.589384	5553.864049	7.729536	-0.040317	4.036510
197.631171	5561.756848	7.734541	-0.040330	4.039268
197.962183	5569.834147	7.739546	-0.040397	4.042092
197.965521	5577.779896	7.744550	-0.040403	4.044864
198.513590	5585.807447	7.749555	-0.040510	4.047670
198.516523	5593.850374	7.754560	-0.040516	4.050472
198.774702	5601.890843	7.759565	-0.040569	4.053275
198.726734	5609.925557	7.764570	-0.040565	4.056069
198.816211	5617.879218	7.769574	-0.040587	4.058835
199.128025	5625.910048	7.774579	-0.040650	4.061629
199.131595	5633.924174	7.779584	-0.040656	4.064411
199.481499	5641.952088	7.784589	-0.040727	4.067201
199.852791	5649.995606	7.789594	-0.040801	4.069994
200.097362	5658.016608	7.794598	-0.040852	4.072776
200.452300	5666.017086	7.799603	-0.040923	4.075551
200.629798	5674.002330	7.804608	-0.040961	4.078316
200.865891	5682.024151	7.809613	-0.041011	4.081092
200.982427	5690.020148	7.814618	-0.041038	4.083856
201.156600	5698.068181	7.819622	-0.041075	4.086637
201.535412	5706.119126	7.824627	-0.041151	4.089420
201.410159	5714.157480	7.829632	-0.041133	4.092189
201.517031	5722.174935	7.834637	-0.041158	4.094953
201.715051	5730.165284	7.839642	-0.041200	4.097706
202.031805	5738.131991	7.844646	-0.041264	4.100451
202.283423	5746.179352	7.849651	-0.041316	4.103222
202.326972	5754.238420	7.854656	-0.041330	4.105991
202.333753	5762.233409	7.859661	-0.041336	4.108736
202.452390	5770.314160	7.864666	-0.041364	4.111511
202.603455	5778.332712	7.869670	-0.041397	4.114262
203.039706	5786.372426	7.874675	-0.041483	4.117022
203.049019	5794.317842	7.879680	-0.041490	4.119743
203.216616	5802.317398	7.884685	-0.041527	4.122483
203.518998	5810.348421	7.889690	-0.041588	4.125233
203.743284	5818.326578	7.894694	-0.041635	4.127962
203.882717	5826.427528	7.899699	-0.041666	4.130731
203.771288	5834.457085	7.904704	-0.041651	4.133469
204.238127	5842.455438	7.909709	-0.041743	4.136203
204.421719	5850.458480	7.914714	-0.041782	4.138933
204.249854	5858.524542	7.919718	-0.041756	4.141678
204.463299	5866.501431	7.924723	-0.041801	4.144396
204.617656	5874.529815	7.929728	-0.041835	4.147129
204.826915	5882.531313	7.934733	-0.041879	4.149851
205.058963	5890.634814	7.939738	-0.041927	4.152606
205.207004	5898.607810	7.944742	-0.041960	4.155315
205.395580	5906.635303	7.949747	-0.042000	4.158040
205.368192	5914.639658	7.954752	-0.042001	4.160754
205.579686	5922.619854	7.959757	-0.042045	4.163460
205.890087	5930.680374	7.964762	-0.042108	4.166192
205.959711	5938.651093	7.969766	-0.042126	4.168890
206.277020	5946.717503	7.974771	-0.042191	4.171621
206.252235	5954.723148	7.979776	-0.042191	4.174326
206.309621	5962.732174	7.984781	-0.042207	4.177031
206.687461	5970.787650	7.989786	-0.042283	4.179754
206.787497	5978.737290	7.994790	-0.042307	4.182436
207.004412	5986.789264	7.999795	-0.042352	4.185152
206.957768	5994.823601	8.004800	-0.042349	4.187858
207.210799	6002.815404	8.009805	-0.042401	4.190551
207.618138	6010.960700	8.014810	-0.042482	4.193295
207.787143	6018.962099	8.019814	-0.042519	4.195986
208.053027	6026.900565	8.024819	-0.042574	4.198656
208.089421	6034.908175	8.029824	-0.042586	4.201345
208.268448	6042.864342	8.034829	-0.042624	4.204016
208.382972	6050.952472	8.039834	-0.042651	4.206729
208.473985	6058.904932	8.044838	-0.042673	4.209394
208.788750	6066.934876	8.049843	-0.042737	4.212086
208.812709	6074.988306	8.054848	-0.042746	4.214782
208.882879	6082.956792	8.059853	-0.042765	4.217447
209.168882	6091.015422	8.064858	-0.042823	4.220143
209.262433	6098.980370	8.069862	-0.042846	4.222805
209.445056	6107.013232	8.074867	-0.042885	4.225488
209.420361	6115.052729	8.079872	-0.042886	4.228169
209.670891	6123.092992	8.084877	-0.042937	4.230852
209.827238	6131.162776	8.089882	-0.042972	4.233542
210.123243	6139.118340	8.094886	-0.043032	4.236193
210.478890	6147.107334	8.099891	-0.043104	4.238855
210.456012	6155.129230	8.104896	-0.043105	4.241522
210.572454	6163.084550	8.109901	-0.043131	4.244167
210.697808	6171.165947	8.114906	-0.043160	4.246852
210.967979	6179.122367	8.119910	-0.043215	4.249495
211.324080	6187.243423	8.124915	-0.043287	4.252191
211.558976	6195.270435	8.129920	-0.043336	4.254854
211.663843	6203.284459	8.134925	-0.043361	4.257510
211.671562	6211.292031	8.139930	-0.043367	4.260161
211.873102	6219.283315	8.144934	-0.043410	4.262806
212.181882	6227.331559	8.149939	-0.043473	4.265470
211.982261	6235.363540	8.154944	-0.043441	4.268122
212.220850	6243.390746	8.159949	-0.043491	4.270775
212.447084	6251.445138	8.164954	-0.043538	4.273435
212.552449	6259.496433	8.169958	-0.043563	4.276091
212.907844	6267.444933	8.174963	-0.043634	4.278714
212.785513	6275.497951	8.179968	-0.043617	4.281365
212.806559	6283.410909	8.184973	-0.043626	4.283970
212.933821	6291.515871	8.189978	-0.043655	4.286638
213.321233	6299.471233	8.194982	-0.043732	4.289256
213.700715	6307.543974	8.199987	-0.043808	4.291912
213.518910	6315.560603	8.204992	-0.043779	4.294543
213.618464	6323.558059	8.209997	-0.043803	4.297168
214.113025	6331.536568	8.215002	-0.043900	4.299789
214.100209	6339.550490	8.220006	-0.043903	4.302415
214.217852	6347.559517	8.225011	-0.043930	4.305040
214.362799	6355.604319	8.230016	-0.043963	4.307674
214.546565	6363.606425	8.235021	-0.044002	4.310294
214.869123	6371.700028	8.240026	-0.044067	4.312942
214.839179	6379.682653	8.245030	-0.044067	4.315551
215.142906	6387.699743	8.250035	-0.044129	4.318171
215.148807	6395.718081	8.255040	-0.044135	4.320788
215.245127	6403.629139	8.260045	-0.044158	4.323369
215.574139	6411.735215	8.265050	-0.044225	4.326013
215.494531	6419.707814	8.270054	-0.044215	4.328610
215.612124	6427.738397	8.275059	-0.044242	4.331225
215.812782	6435.809513	8.280064	-0.044285	4.333853
215.899547	6443.800677	8.285069	-0.044306	4.336452
216.105222	6451.830651	8.290074	-0.044350	4.339063
216.313060	6459.833774	8.295078	-0.044394	4.341663
216.730213	6467.824883	8.300083	-0.044476	4.344260
216.619543	6475.839631	8.305088	-0.044461	4.346859
216.744265	6483.869701	8.310093	-0.044490	4.349463
217.072155	6491.929410	8.315098	-0.044556	4.352076
216.980573	6499.999692	8.320102	-0.044544	4.354689
217.191005	6508.055232	8.325107	-0.044588	4.357297
217.262385	6515.943667	8.330112	-0.044607	4.359849
217.432606	6523.938201	8.335117	-0.044644	4.362434
217.685762	6531.920472	8.340122	-0.044696	4.365014
217.657929	6539.958450	8.345126	-0.044696	4.367608
217.855881	6548.001741	8.350131	-0.044738	4.370205
217.993501	6555.984212	8.355136	-0.044769	4.372779
218.152336	6564.028231	8.360141	-0.044804	4.375373
218.425892	6572.042975	8.365146	-0.044860	4.377955
218.490610	6580.060564	8.370150	-0.044877	4.380536
218.690037	6588.041646	8.375155	-0.044920	4.383105
219.034243	6596.095820	8.380160	-0.044989	4.385696
219.158456	6604.136439	8.385165	-0.045017	4.388280
219.305737	6612.158110	8.390170	-0.045050	4.390857
219.337964	6620.162220	8.395174	-0.045061	4.393426
219.605240	6628.219596	8.400179	-0.045116	4.396011
219.881496	6636.181326	8.405184	-0.045173	4.398565
219.941412	6644.201134	8.410189	-0.045189	4.401134
220.840717	6652.163021	8.415194	-0.045362	4.403688
221.847890	6660.181819	8.420198	-0.045555	4.406259
222.166407	6668.209981	8.425203	-0.045619	4.408828
222.382412	6676.297361	8.430208	-0.045665	4.411413
222.544702	6684.275048	8.435213	-0.045700	4.413962
222.845539	6692.384408	8.440218	-0.045761	4.416552
222.960443	6700.330196	8.445222	-0.045788	4.419087
223.207525	6708.401035	8.450227	-0.045839	4.421662
223.516865	6716.326782	8.455232	-0.045902	4.424189
223.676458	6724.371193	8.460237	-0.045937	4.426751
224.002243	6732.433616	8.465242	-0.046003	4.429319
223.823057	6740.443311	8.470246	-0.045975	4.431866
224.064139	6748.529200	8.475251	-0.046025	4.434437
224.334579	6756.513320	8.480256	-0.046080	4.436975
224.454850	6764.467807	8.485261	-0.046108	4.439502
224.452500	6772.537776	8.490266	-0.046113	4.442063
224.454998	6780.465635	8.495270	-0.046118	4.444577
224.825147	6788.562591	8.500275	-0.046193	4.447145
225.068420	6796.524083	8.505280	-0.046243	4.449668
224.978756	6804.532928	8.510285	-0.046232	4.452204
225.308841	6812.579505	8.515290	-0.046298	4.454751
225.433550	6820.620541	8.520294	-0.046327	4.457295
225.489302	6828.632488	8.525299	-0.046342	4.459827
225.613918	6836.640282	8.530304	-0.046371	4.462357
225.941480	6844.606753	8.535309	-0.046437	4.464874
226.120686	6852.676575	8.540314	-0.046476	4.467421
226.132756	6860.668818	8.545318	-0.046483	4.469941
226.281647	6868.724488	8.550323	-0.046516	4.472481
226.324440	6876.726491	8.555328	-0.046529	4.475001
226.474280	6884.698140	8.560333	-0.046562	4.477511
226.677513	6892.752170	8.565338	-0.046605	4.480046
226.619895	6900.737112	8.570343	-0.046600	4.482557
226.725104	6908.750677	8.575347	-0.046625	4.485076
227.003146	6916.815771	8.580352	-0.046682	4.487610
227.199601	6924.792837	8.585357	-0.046724	4.490115
227.272930	6932.835358	8.590362	-0.046742	4.492638
227.074920	6940.856134	8.595367	-0.046711	4.495153
227.503320	6948.867528	8.600371	-0.046796	4.497665
227.642654	6956.854306	8.605376	-0.046827	4.500166
227.684279	6964.860430	8.610381	-0.046840	4.502673
228.062113	6972.865110	8.615386	-0.046915	4.505178
228.009495	6980.881071	8.620391	-0.046911	4.507685
228.339179	6988.937266	8.625395	-0.046978	4.510203
228.515211	6997.053344	8.630400	-0.047016	4.512738
228.735154	7005.033658	8.635405	-0.047062	4.515230
228.933900	7013.014634	8.640410	-0.047104	4.517721
228.862842	7020.977099	8.645415	-0.047096	4.520203
228.929804	7028.990004	8.650419	-0.047114	4.522700
229.160310	7037.006199	8.655424	-0.047162	4.525198
229.088858	7044.998930	8.660429	-0.047154	4.527686
229.301384	7053.010171	8.665434	-0.047198	4.530179
229.272485	7061.075713	8.670439	-0.047198	4.532687
229.469572	7069.119153	8.675443	-0.047240	4.535187
229.673424	7077.115799	8.680448	-0.047283	4.537671
229.697198	7085.072726	8.685453	-0.047293	4.540141
229.911675	7093.132541	8.690458	-0.047338	4.542642
230.027949	7101.120903	8.695463	-0.047365	4.545119
230.069046	7109.158420	8.700467	-0.047378	4.547610
230.181229	7117.155636	8.705472	-0.047404	4.550088
230.383467	7125.209264	8.710477	-0.047447	4.552581
230.698583	7133.280980	8.715482	-0.047511	4.555079
230.737480	7141.243415	8.720487	-0.047523	4.557541
230.751586	7149.237569	8.725491	-0.047531	4.560012
230.790308	7157.234957	8.730496	-0.047544	4.562483
230.975601	7165.219923	8.735501	-0.047583	4.564948
231.256006	7173.306078	8.740506	-0.047641	4.567443
231.310015	7181.277100	8.745511	-0.047656	4.569902
231.625744	7189.360958	8.750515	-0.047720	4.572394
231.552165	7197.362437	8.755520	-0.047712	4.574859
231.686992	7205.342212	8.760525	-0.047742	4.577316
231.819722	7213.404482	8.765530	-0.047772	4.579797
232.041203	7221.379561	8.770535	-0.047818	4.582250
232.290209	7229.387384	8.775539	-0.047870	4.584711
232.536232	7237.446382	8.780544	-0.047921	4.587187
232.756588	7245.450903	8.785549	-0.047967	4.589645
232.897591	7253.514912	8.790554	-0.047999	4.592120
232.823488	7261.538904	8.795559	-0.047990	4.594581
233.157201	7269.559425	8.800563	-0.048057	4.597040
233.383163	7277.519291	8.805568	-0.048105	4.599479
233.467882	7285.511171	8.810573	-0.048126	4.601926
233.666708	7293.536828	8.815578	-0.048168	4.604383
233.838750	7301.542376	8.820583	-0.048205	4.606832
233.937400	7309.551276	8.825587	-0.048229	4.609280
233.913269	7317.609492	8.830592	-0.048230	4.611743
234.083965	7325.588135	8.835597	-0.048267	4.614179
234.413003	7333.686683	8.840602	-0.048333	4.616651
234.269872	7341.619677	8.845607	-0.048312	4.619071
234.364128	7349.678759	8.850611	-0.048334	4.621529
234.387426	7357.659130	8.855616	-0.048344	4.623961
234.633782	7365.682860	8.860621	-0.048395	4.626405
234.869366	7373.678100	8.865626	-0.048444	4.628839
234.940517	7381.721582	8.870631	-0.048463	4.631286
235.244251	7389.759410	8.875635	-0.048524	4.633730
235.207111	7397.844219	8.880640	-0.048523	4.636187
235.486181	7405.735474	8.885645	-0.048580	4.638585
235.549715	7413.791977	8.890650	-0.048597	4.641031
235.792603	7421.751275	8.895655	-0.048647	4.643446
235.959021	7429.814510	8.900659	-0.048684	4.645891
236.188359	7437.827629	8.905664	-0.048731	4.648320
236.148093	7445.817494	8.910669	-0.048729	4.650741
236.213305	7453.873700	8.915674	-0.048747	4.653181
236.059338	7461.878792	8.920679	-0.048723	4.655604
236.439742	7469.882562	8.925683	-0.048799	4.658024
236.498187	7477.881250	8.930688	-0.048815	4.660443
236.603983	7485.884299	8.935693	-0.048840	4.662861
236.864148	7493.952126	8.940698	-0.048894	4.665297
236.870662	7501.967372	8.945703	-0.048900	4.667717
237.063290	7509.945154	8.950707	-0.048941	4.670124
237.343123	7518.097362	8.955712	-0.048999	4.672582
237.485249	7526.094803	8.960717	-0.049030	4.674992
237.661183	7534.066537	8.965722	-0.049068	4.677393
237.819313	7541.967674	8.970727	-0.049103	4.679772
238.040047	7550.021626	8.975731	-0.049149	4.682195
238.039660	7557.979994	8.980736	-0.049154	4.684589
238.138454	7566.037535	8.985741	-0.049178	4.687011
238.381374	7574.039854	8.990746	-0.049229	4.689415
238.446929	7582.125376	8.995751	-0.049246	4.691842
238.505118	7590.092304	9.000755	-0.049262	4.694234
238.770709	7598.152103	9.005760	-0.049317	4.696651
239.087962	7606.107151	9.010765	-0.049381	4.699036
238.980432	7614.153077	9.015770	-0.049366	4.701447
239.002762	7622.080991	9.020775	-0.049376	4.703822
239.243031	7630.152194	9.025779	-0.049426	4.706237
239.468190	7638.161782	9.030784	-0.049473	4.708634
239.313217	7646.207105	9.035789	-0.049449	4.711040
239.775515	7654.286390	9.040794	-0.049540	4.713454
239.924020	7662.257735	9.045799	-0.049573	4.715835
239.994585	7670.236718	9.050803	-0.049592	4.718217
239.883471	7678.266372	9.055808	-0.049576	4.720614
240.453794	7686.282901	9.060813	-0.049688	4.723004
240.352804	7694.309335	9.065818	-0.049674	4.725397
240.528543	7702.306666	9.070823	-0.049712	4.727780
240.838133	7710.362807	9.075827	-0.049775	4.730179
240.940047	7718.382404	9.080832	-0.049799	4.732566
240.938044	7726.428193	9.085837	-0.049804	4.734960
240.925361	7734.419152	9.090842	-0.049807	4.737336
241.126793	7742.388944	9.095847	-0.049849	4.739705
241.247234	7750.436614	9.100851	-0.049877	4.742095
241.368187	7758.435822	9.105856	-0.049905	4.744470
241.806566	7766.462432	9.110861	-0.049992	4.746851
241.999597	7774.489559	9.115866	-0.050033	4.749231
241.894495	7782.508056	9.120871	-0.050018	4.751609
242.444641	7790.540993	9.125875	-0.050126	4.753988
242.690120	7798.561015	9.130880	-0.050177	4.756362
242.363311	7806.479397	9.135885	-0.050121	4.758708
242.546552	7814.556351	9.140890	-0.050161	4.761097
242.733858	7822.535065	9.145895	-0.050201	4.763456
242.860591	7830.581524	9.150899	-0.050230	4.765834
242.915767	7838.556133	9.155904	-0.050245	4.768190
243.050741	7846.561092	9.160909	-0.050275	4.770553
243.245314	7854.649130	9.165914	-0.050317	4.772940
243.176839	7862.659577	9.170919	-0.050309	4.775303
243.428965	7870.666516	9.175923	-0.050362	4.777663
243.671878	7878.663621	9.180928	-0.050412	4.780019
243.702149	7886.650247	9.185933	-0.050423	4.782371
243.919361	7894.662470	9.190938	-0.050469	4.784729
244.221128	7902.738275	9.195943	-0.050530	4.787104
244.311692	7910.714382	9.200947	-0.050552	4.789450
244.281046	7918.800003	9.205952	-0.050552	4.791827
244.457759	7926.758718	9.210957	-0.050590	4.794165
244.678082	7934.840059	9.215962	-0.050636	4.796537
244.788233	7942.758964	9.220967	-0.050662	4.798861
244.900278	7950.780771	9.225971	-0.050688	4.801214
245.205038	7958.772225	9.230976	-0.050750	4.803556
245.092135	7966.811341	9.235981	-0.050734	4.805913
245.209751	7974.805735	9.240986	-0.050761	4.808255
245.447454	7982.816641	9.245991	-0.050811	4.810599
245.715386	7990.364701	9.250995	-0.050865	4.812807
245.801260	7995.069930	9.256000	-0.050884	4.814183

245.989064	7997.718944	9.261005	-0.050921	4.814957
246.101996	7999.064745	9.266010	-0.050943	4.815350
246.058860	7999.423810	9.271015	-0.050935	4.815456
246.103188	8000.512409	9.276019	-0.050944	4.815774
246.288497	8000.475915	9.281024	-0.050979	4.815762
246.253058	8000.582103	9.286029	-0.050972	4.815793
246.237980	8000.604279	9.291034	-0.050969	4.815800
246.238415	8000.580797	9.296039	-0.050969	4.815793
246.436927	8000.484730	9.301043	-0.051006	4.815764
246.422202	8000.593390	9.306048	-0.051004	4.815796
246.518790	8000.590688	9.311053	-0.051022	4.815795
246.684272	8000.425754	9.316058	-0.051052	4.815746
246.484769	8000.616826	9.321063	-0.051015	4.815803
246.508013	8000.409013	9.326067	-0.051019	4.815742
246.507359	8000.584095	9.331072	-0.051019	4.815793
246.375750	8000.479465	9.336077	-0.050995	4.815763
246.484090	8000.599732	9.341082	-0.051015	4.815798
246.552827	8000.478069	9.346087	-0.051028	4.815762
246.603773	8000.588863	9.351091	-0.051037	4.815794
246.627493	8000.477145	9.356096	-0.051042	4.815761
246.677956	8000.583662	9.361101	-0.051051	4.815792
246.838843	8000.526486	9.366106	-0.051081	4.815774
246.805218	8000.518466	9.371111	-0.051075	4.815772
246.821138	8000.524063	9.376115	-0.051078	4.815774
246.928456	8000.427581	9.381120	-0.051098	4.815745
246.875296	8000.589001	9.386125	-0.051088	4.815793
246.993369	8000.503371	9.391130	-0.051110	4.815767
246.843483	8000.590619	9.396135	-0.051082	4.815793
246.929282	8000.511938	9.401139	-0.051098	4.815770
246.965472	8000.602209	9.406144	-0.051105	4.815796
246.834181	8000.503988	9.411149	-0.051080	4.815768
247.181304	8000.523504	9.416154	-0.051145	4.815772
247.040101	8000.592744	9.421159	-0.051119	4.815793
246.908409	8000.504125	9.426163	-0.051094	4.815768
247.276876	8000.503703	9.431168	-0.051163	4.815766
247.194697	8000.602728	9.436173	-0.051147	4.815795
246.879433	8000.514330	9.441178	-0.051089	4.815771
246.917259	8000.593951	9.446183	-0.051096	4.815794
247.224612	8000.524207	9.451187	-0.051153	4.815772
247.449213	8000.511840	9.456192	-0.051195	4.815767
247.196459	8000.610230	9.461197	-0.051148	4.815797
247.348151	8000.597746	9.466202	-0.051176	4.815793
247.488985	8000.521026	9.471207	-0.051202	4.815770
247.390216	8000.502339	9.476211	-0.051184	4.815765
247.348207	8000.374605	9.481216	-0.051176	4.815728
247.421942	8000.606418	9.486221	-0.051190	4.815795
247.351535	8000.418433	9.491226	-0.051176	4.815740
247.302320	8000.493437	9.496231	-0.051167	4.815763
247.468600	8000.519626	9.501235	-0.051198	4.815769
247.442407	8000.506389	9.506240	-0.051193	4.815766
247.339690	8000.537818	9.511245	-0.051174	4.815775
247.588182	8000.518365	9.516250	-0.051221	4.815769
247.595305	8000.619910	9.521255	-0.051222	4.815798
247.433948	8000.534010	9.526259	-0.051192	4.815774
247.452522	8000.522567	9.531264	-0.051195	4.815770
247.429934	8000.602275	9.536269	-0.051191	4.815794
247.462160	8000.530197	9.541274	-0.051197	4.815773
247.242197	8000.608834	9.546279	-0.051156	4.815797
247.547136	8000.525171	9.551283	-0.051213	4.815771
247.657316	8000.449021	9.556288	-0.051233	4.815748
247.428226	8000.560607	9.561293	-0.051191	4.815782
247.662778	8000.624207	9.566298	-0.051234	4.815799
247.628430	8000.493393	9.571303	-0.051228	4.815761
247.564032	8000.512632	9.576307	-0.051216	4.815767
247.498720	8000.515842	9.581312	-0.051204	4.815768
247.480761	8000.605234	9.586317	-0.051201	4.815794
247.513646	8000.509678	9.591322	-0.051207	4.815766
247.523669	8000.613405	9.596327	-0.051209	4.815797
247.652426	8000.484173	9.601331	-0.051232	4.815758
247.638431	8000.616336	9.606336	-0.051230	4.815797
247.637828	8000.522371	9.611341	-0.051230	4.815769
247.682817	8000.613854	9.616346	-0.051238	4.815796
247.629361	8000.575617	9.621351	-0.051228	4.815785
247.489953	8000.588299	9.626355	-0.051202	4.815789
247.684540	8000.618152	9.631360	-0.051239	4.815797
247.726294	8000.488574	9.636365	-0.051246	4.815759
247.680128	8000.545478	9.641370	-0.051238	4.815776
247.462729	8000.513119	9.646375	-0.051197	4.815768
247.726685	8000.521678	9.651379	-0.051246	4.815769
247.693861	8000.539295	9.656384	-0.051240	4.815774
247.534076	8000.513210	9.661389	-0.051210	4.815767
247.566826	8000.538298	9.666394	-0.051217	4.815774
247.567859	8000.508420	9.671399	-0.051217	4.815766
247.716587	8000.489483	9.676403	-0.051244	4.815759
247.805481	8000.544310	9.681408	-0.051261	4.815775
247.735686	8000.608304	9.686413	-0.051248	4.815794
247.903241	8000.517071	9.691418	-0.051279	4.815767
247.988172	8000.499232	9.696423	-0.051295	4.815761
248.129148	8000.464154	9.701427	-0.051321	4.815750
247.961564	8000.555387	9.706432	-0.051290	4.815778
247.958728	8000.590574	9.711437	-0.051290	4.815788
248.031938	8000.620591	9.716442	-0.051303	4.815796
248.079175	8000.503913	9.721447	-0.051312	4.815762
248.042916	8000.627175	9.726451	-0.051305	4.815798
248.029409	8000.537270	9.731456	-0.051303	4.815772
247.981152	8000.608020	9.736461	-0.051294	4.815793
248.063249	8000.516466	9.741466	-0.051309	4.815766
247.679332	8000.581762	9.746471	-0.051237	4.815787
247.854717	8000.611304	9.751475	-0.051270	4.815794
248.091304	8000.505176	9.756480	-0.051314	4.815762
247.933211	8000.609376	9.761485	-0.051285	4.815793
248.112237	8000.624029	9.766490	-0.051318	4.815797
248.045139	8000.523644	9.771495	-0.051306	4.815768
247.939298	8000.609474	9.776499	-0.051286	4.815793
247.972250	8000.509647	9.781504	-0.051292	4.815764
247.909629	8000.619668	9.786509	-0.051280	4.815797
247.981827	8000.459622	9.791514	-0.051294	4.815749
248.056411	8000.613512	9.796519	-0.051308	4.815794
247.983554	8000.504492	9.801523	-0.051294	4.815763
248.130863	8000.546389	9.806528	-0.051321	4.815774
247.967781	8000.608868	9.811533	-0.051291	4.815793
248.053591	8000.526983	9.816538	-0.051307	4.815769
248.038266	8000.529936	9.821543	-0.051304	4.815770
247.804651	8000.609420	9.826547	-0.051261	4.815794
247.718651	8000.587736	9.831552	-0.051245	4.815788
247.933889	8000.541052	9.836557	-0.051285	4.815774
247.920630	8000.552581	9.841562	-0.051282	4.815777
247.840775	8000.623886	9.846567	-0.051268	4.815798
247.883753	8000.503936	9.851571	-0.051275	4.815763
248.142803	8000.544446	9.856576	-0.051324	4.815774
248.003661	8000.511222	9.861581	-0.051298	4.815764
248.102907	8000.617468	9.866586	-0.051316	4.815795
248.152891	8000.621483	9.871591	-0.051326	4.815796
247.985355	8000.511992	9.876595	-0.051294	4.815765
247.953123	8000.629981	9.881600	-0.051288	4.815799
247.935402	8000.486623	9.886605	-0.051285	4.815758
248.052106	8000.537632	9.891610	-0.051307	4.815772
248.031602	8000.523419	9.896615	-0.051303	4.815768
247.987356	8000.615589	9.901619	-0.051295	4.815795
248.152205	8000.436761	9.906624	-0.051325	4.815742
248.064994	8000.604038	9.911629	-0.051309	4.815791
247.915036	8000.539675	9.916634	-0.051281	4.815773
247.945192	8000.407773	9.921639	-0.051287	4.815734
248.023394	8000.433600	9.926643	-0.051301	4.815742
247.998066	8000.539956	9.931648	-0.051297	4.815773
248.015386	8000.475109	9.936653	-0.051300	4.815754
248.268262	8000.558226	9.941658	-0.051347	4.815777
248.207287	8000.534813	9.946663	-0.051336	4.815770
248.059455	8000.506787	9.951667	-0.051308	4.815763
248.254873	8000.516368	9.956672	-0.051344	4.815765
248.205201	8000.527305	9.961677	-0.051335	4.815768
248.143123	8000.631997	9.966682	-0.051324	4.815799
247.994904	8000.467301	9.971687	-0.051296	4.815752
248.100790	8000.637715	9.976691	-0.051316	4.815801
248.090334	8000.634342	9.981696	-0.051314	4.815800
248.217407	8000.522164	9.986701	-0.051338	4.815767
248.335350	8000.548637	9.991706	-0.051359	4.815774
248.113834	8000.524751	9.996711	-0.051318	4.815768
248.341874	8000.637361	10.001715	-0.051361	4.815800
248.196916	8000.432145	10.006720	-0.051334	4.815740
248.098854	8000.503154	10.011725	-0.051315	4.815762
248.019752	8000.546711	10.016730	-0.051301	4.815775
248.426006	8000.625916	10.021735	-0.051376	4.815796
248.456585	8000.515372	10.026739	-0.051382	4.815764
248.414790	8000.528573	10.031744	-0.051374	4.815768
248.170528	8000.640981	10.036749	-0.051329	4.815802
248.393134	8000.405437	10.041754	-0.051370	4.815732
248.389931	8000.537777	10.046759	-0.051370	4.815770
248.198814	8000.488761	10.051763	-0.051334	4.815757
248.252126	8000.537673	10.056768	-0.051344	4.815771
248.156904	8000.448576	10.061773	-0.051326	4.815745
248.238672	8000.398655	10.066778	-0.051341	4.815730
248.191923	8000.487581	10.071783	-0.051333	4.815757
248.323847	8000.501469	10.076787	-0.051357	4.815760
248.308244	8000.209739	10.081792	-0.051354	4.815675
248.194081	8000.629618	10.086797	-0.051333	4.815798
248.254704	8000.453367	10.091802	-0.051344	4.815746
248.259981	8000.468400	10.096807	-0.051345	4.815751
248.258433	8000.629595	10.101811	-0.051345	4.815798
248.590093	8000.501523	10.106816	-0.051407	4.815759
248.394295	8000.592298	10.111821	-0.051370	4.815786
248.324627	8000.634941	10.116826	-0.051357	4.815799
248.402226	8000.541177	10.121831	-0.051372	4.815771
248.417908	8000.644999	10.126835	-0.051375	4.815802
248.425826	8000.421980	10.131840	-0.051376	4.815736
248.323783	8000.634927	10.136845	-0.051357	4.815799
248.599573	8000.533707	10.141850	-0.051409	4.815768
248.386638	8000.602849	10.146855	-0.051369	4.815789
248.260706	8000.530335	10.151859	-0.051345	4.815769
248.521328	8000.548450	10.156864	-0.051394	4.815773
248.526370	8000.615797	10.161869	-0.051395	4.815793
248.410700	8000.553058	10.166874	-0.051373	4.815775
248.247213	8000.529047	10.171879	-0.051343	4.815769
248.323888	8000.519616	10.176883	-0.051357	4.815765
248.285900	8000.538217	10.181888	-0.051350	4.815771
248.156237	8000.468846	10.186893	-0.051326	4.815751
248.312753	8000.627272	10.191898	-0.051355	4.815797
248.362411	8000.514903	10.196903	-0.051364	4.815764
248.421391	8000.411228	10.201907	-0.051375	4.815733
248.571399	8000.400853	10.206912	-0.051403	4.815729
248.614771	8000.639653	10.211917	-0.051411	4.815799
248.621470	8000.435832	10.216922	-0.051413	4.815739
248.462283	8000.418298	10.221927	-0.051383	4.815735
248.428037	8000.438027	10.226931	-0.051377	4.815741
248.517941	8000.413863	10.231936	-0.051393	4.815734
248.175322	8000.626104	10.236941	-0.051330	4.815797
248.500485	8000.542770	10.241946	-0.051390	4.815771
248.457930	8000.481220	10.246951	-0.051382	4.815754
248.339600	8000.646924	10.251955	-0.051360	4.815803
248.533090	8000.421582	10.256960	-0.051396	4.815736
248.398941	8000.623331	10.261965	-0.051371	4.815795
248.493612	8000.509559	10.266970	-0.051389	4.815762
248.545079	8000.501853	10.271975	-0.051398	4.815759
248.388224	8000.648781	10.276979	-0.051369	4.815803
248.660813	8000.428995	10.281984	-0.051420	4.815737
248.563751	8000.566218	10.286989	-0.051402	4.815778
248.648236	8000.488581	10.291994	-0.051418	4.815755
248.695885	8000.523522	10.296999	-0.051426	4.815765
248.476743	8000.644880	10.302003	-0.051386	4.815801
248.613662	8000.526456	10.307008	-0.051411	4.815766
248.637678	8000.614397	10.312013	-0.051416	4.815792
248.529089	8000.542164	10.317018	-0.051395	4.815771
248.416155	8000.528584	10.322023	-0.051374	4.815768
248.596656	8000.623339	10.327027	-0.051408	4.815794
248.808323	8000.563785	10.332032	-0.051447	4.815776
248.424172	8000.515901	10.337037	-0.051376	4.815764
248.743288	8000.521087	10.342042	-0.051435	4.815764
248.717832	8000.469424	10.347047	-0.051430	4.815749
248.727395	8000.517625	10.352051	-0.051432	4.815763
248.685204	8000.554309	10.357056	-0.051424	4.815774
248.641190	8000.483125	10.362061	-0.051416	4.815753
248.643159	8000.530136	10.367066	-0.051417	4.815767
248.468246	8000.372478	10.372071	-0.051384	4.815722
248.511106	8000.555749	10.377075	-0.051392	4.815775
248.720516	8000.437435	10.382080	-0.051431	4.815739
248.700244	8000.528927	10.387085	-0.051427	4.815766
248.601225	8000.626614	10.392090	-0.051409	4.815795
248.662017	8000.551795	10.397095	-0.051420	4.815773
248.455874	8000.544174	10.402099	-0.051382	4.815772
248.655606	8000.436380	10.407104	-0.051419	4.815739
248.676453	8000.569112	10.412109	-0.051423	4.815778
248.623849	8000.362193	10.417114	-0.051413	4.815718
248.483162	8000.455998	10.422119	-0.051387	4.815746
248.504992	8000.532159	10.427123	-0.051391	4.815768
248.570002	8000.449935	10.432128	-0.051403	4.815744
248.497729	8000.548056	10.437133	-0.051390	4.815773
248.580006	8000.412728	10.442138	-0.051405	4.815733
248.823080	8000.526651	10.447143	-0.051450	4.815765
248.560708	8000.543740	10.452147	-0.051401	4.815771
248.712740	8000.561159	10.457152	-0.051430	4.815776
248.657005	8000.507936	10.462157	-0.051419	4.815760
248.762979	8000.540621	10.467162	-0.051439	4.815769
248.769458	8000.624007	10.472167	-0.051440	4.815794
248.659530	8000.620084	10.477171	-0.051420	4.815793
248.849172	8000.550563	10.482176	-0.051455	4.815772
248.648805	8000.554780	10.487181	-0.051418	4.815774
248.630803	8000.379386	10.492186	-0.051414	4.815723
248.732463	8000.559342	10.497191	-0.051433	4.815775
248.496416	8000.592875	10.502195	-0.051389	4.815786
248.610900	8000.544554	10.507200	-0.051411	4.815771
248.713816	8000.530211	10.512205	-0.051430	4.815767
248.923556	8000.430053	10.517210	-0.051469	4.815736
248.859265	8000.328645	10.522215	-0.051457	4.815707
248.617758	8000.507295	10.527219	-0.051412	4.815760
248.864185	8000.539060	10.532224	-0.051458	4.815769
248.696338	8000.533129	10.537229	-0.051426	4.815768
248.496461	8000.561911	10.542234	-0.051389	4.815777
248.682336	8000.640739	10.547239	-0.051424	4.815799
248.724199	8000.539987	10.552243	-0.051432	4.815769
248.638295	8000.445702	10.557248	-0.051416	4.815742
248.479020	8000.625689	10.562253	-0.051386	4.815796
248.654404	8000.505754	10.567258	-0.051419	4.815760
248.557903	8000.512727	10.572263	-0.051401	4.815762
248.431415	8000.644133	10.577267	-0.051377	4.815801
248.628066	8000.420978	10.582272	-0.051414	4.815735
248.686551	8000.631196	10.587277	-0.051425	4.815796
248.581707	8000.521655	10.592282	-0.051405	4.815765
248.630427	8000.617471	10.597287	-0.051414	4.815793
248.654898	8000.537791	10.602291	-0.051419	4.815769
248.618651	8000.650378	10.607296	-0.051412	4.815802
248.627849	8000.525607	10.612301	-0.051414	4.815766
248.896230	8000.647416	10.617306	-0.051464	4.815800
248.787183	8000.511113	10.622311	-0.051443	4.815761
248.870655	8000.558380	10.627315	-0.051459	4.815774
249.034609	8000.380604	10.632320	-0.051489	4.815721
248.762755	8000.629230	10.637325	-0.051439	4.815795
248.710638	8000.425520	10.642330	-0.051429	4.815736
248.608202	8000.503932	10.647335	-0.051410	4.815759
248.715987	8000.513158	10.652339	-0.051430	4.815762
248.526571	8000.644609	10.657344	-0.051395	4.815801
248.500538	8000.548093	10.662349	-0.051390	4.815773
248.628918	8000.526690	10.667354	-0.051414	4.815766
248.698756	8000.629256	10.672359	-0.051427	4.815796
248.539427	8000.510287	10.677363	-0.051397	4.815762
248.708578	8000.659311	10.682368	-0.051429	4.815804
248.824843	8000.513858	10.687373	-0.051450	4.815761
248.783269	8000.598598	10.692378	-0.051443	4.815786
248.694986	8000.533101	10.697383	-0.051426	4.815768
248.739241	8000.490044	10.702387	-0.051434	4.815755
248.907081	8000.534412	10.707392	-0.051466	4.815767
248.789230	8000.623251	10.712397	-0.051444	4.815793
248.804693	8000.542357	10.717402	-0.051447	4.815770
249.041925	8000.536604	10.722407	-0.051491	4.815767
248.772666	8000.425457	10.727411	-0.051441	4.815736
249.110933	8000.625277	10.732416	-0.051504	4.815793
249.059003	8000.472818	10.737421	-0.051494	4.815748
248.959273	8000.549139	10.742426	-0.051475	4.815771
248.807220	8000.641693	10.747431	-0.051447	4.815799
248.931415	8000.520926	10.752435	-0.051470	4.815763
249.010758	8000.422919	10.757440	-0.051485	4.815734
248.750546	8000.631162	10.762445	-0.051437	4.815796
248.848975	8000.529195	10.767450	-0.051455	4.815766
248.945934	8000.517958	10.772455	-0.051473	4.815762
248.702783	8000.597287	10.777459	-0.051428	4.815786
248.792571	8000.524007	10.782464	-0.051444	4.815764
248.995421	8000.505949	10.787469	-0.051482	4.815758
249.060428	8000.544376	10.792474	-0.051494	4.815769
248.872152	8000.529570	10.797479	-0.051459	4.815766
248.711753	8000.656155	10.802483	-0.051429	4.815803
248.933105	8000.546576	10.807488	-0.051470	4.815770
248.704258	8000.528976	10.812493	-0.051428	4.815766
248.724804	8000.552799	10.817498	-0.051432	4.815773
248.925330	8000.510147	10.822503	-0.051469	4.815760
248.938512	8000.624606	10.827507	-0.051471	4.815793
249.164500	8000.320780	10.832512	-0.051513	4.815703
249.039913	8000.492790	10.837517	-0.051490	4.815754
249.020030	8000.562936	10.842522	-0.051487	4.815775
248.840013	8000.441495	10.847527	-0.051453	4.815740
248.940393	8000.538151	10.852531	-0.051472	4.815768
249.093468	8000.414650	10.857536	-0.051500	4.815731
248.935562	8000.525260	10.862541	-0.051471	4.815764
248.897061	8000.518228	10.867546	-0.051464	4.815762
249.056522	8000.479179	10.872551	-0.051493	4.815750
248.942926	8000.549936	10.877555	-0.051472	4.815771
248.837390	8000.540747	10.882560	-0.051453	4.815769
248.871836	8000.612843	10.887565	-0.051459	4.815790
248.991327	8000.481322	10.892570	-0.051481	4.815751
248.871590	8000.600026	10.897575	-0.051459	4.815786
248.687655	8000.579953	10.902579	-0.051425	4.815781
248.996588	8000.642630	10.907584	-0.051482	4.815798
248.893087	8000.411392	10.912589	-0.051463	4.815731
248.999915	8000.357607	10.917594	-0.051483	4.815715
248.946620	8000.527573	10.922599	-0.051473	4.815765
248.883045	8000.543623	10.927603	-0.051461	4.815770
249.140294	8000.395122	10.932608	-0.051509	4.815725
249.075395	8000.654588	10.937613	-0.051497	4.815801
249.051642	8000.617899	10.942618	-0.051492	4.815791
249.101158	8000.411569	10.947623	-0.051502	4.815730
249.226223	8000.611127	10.952627	-0.051525	4.815788
249.279594	8000.530849	10.957632	-0.051535	4.815764
249.233743	8000.632604	10.962637	-0.051526	4.815794
248.984210	8000.544198	10.967642	-0.051480	4.815769
249.202243	8000.395060	10.972647	-0.051520	4.815725
249.175340	8000.562252	10.977651	-0.051515	4.815774
248.998808	8000.552976	10.982656	-0.051483	4.815772
248.804903	8000.604277	10.987661	-0.051447	4.815788
249.180311	8000.529233	10.992666	-0.051516	4.815764
249.230973	8000.624015	10.997671	-0.051526	4.815792
249.046268	8000.622080	11.002675	-0.051491	4.815792
249.192887	8000.449359	11.007680	-0.051519	4.815741
248.859058	8000.530417	11.012685	-0.051457	4.815766
248.992539	8000.533654	11.017690	-0.051481	4.815766
249.065371	8000.626661	11.022695	-0.051495	4.815793
249.099315	8000.520441	11.027699	-0.051501	4.815762
248.943013	8000.404725	11.032704	-0.051472	4.815729
248.972763	8000.628358	11.037709	-0.051478	4.815794
249.020842	8000.533045	11.042714	-0.051487	4.815766
248.918926	8000.649904	11.047719	-0.051468	4.815801
248.858528	8000.604078	11.052723	-0.051456	4.815788
249.207073	8000.554223	11.057728	-0.051521	4.815771
249.119400	8000.553866	11.062733	-0.051505	4.815772
249.017622	8000.534060	11.067738	-0.051486	4.815766
248.936069	8000.611744	11.072743	-0.051471	4.815789
249.123276	8000.587027	11.077747	-0.051506	4.815781
249.131824	8000.633077	11.082752	-0.051507	4.815795
248.999211	8000.425922	11.087757	-0.051483	4.815735
249.161831	8000.532132	11.092762	-0.051513	4.815765
249.116006	8000.514304	11.097767	-0.051504	4.815760
248.912847	8000.634855	11.102771	-0.051467	4.815796
249.186585	8000.543211	11.107776	-0.051517	4.815768
249.128934	8000.505972	11.112781	-0.051507	4.815758
249.030184	8000.631424	11.117786	-0.051488	4.815795
249.263467	8000.541257	11.122791	-0.051532	4.815767
249.274238	8000.543568	11.127795	-0.051534	4.815768
249.404082	8000.545678	11.132800	-0.051558	4.815768
249.232901	8000.564249	11.137805	-0.051526	4.815774
249.200967	8000.544511	11.142810	-0.051520	4.815769
249.182570	8000.527129	11.147815	-0.051517	4.815764
249.244220	8000.633834	11.152819	-0.051528	4.815794
249.319603	8000.439668	11.157824	-0.051542	4.815737
249.150383	8000.481761	11.162829	-0.051511	4.815750
249.068627	8000.519937	11.167834	-0.051495	4.815762
249.155855	8000.444480	11.172839	-0.051512	4.815739
249.216873	8000.537295	11.177843	-0.051523	4.815766
249.108575	8000.449050	11.182848	-0.051503	4.815741
248.953652	8000.628041	11.187853	-0.051474	4.815794
249.373090	8000.496057	11.192858	-0.051552	4.815754
249.367477	8000.538674	11.197863	-0.051551	4.815766
249.079061	8000.571355	11.202867	-0.051497	4.815777
249.259136	8000.615924	11.207872	-0.051531	4.815789
249.319654	8000.499459	11.212877	-0.051542	4.815755
249.209145	8000.548912	11.217882	-0.051522	4.815770
249.087667	8000.439099	11.222887	-0.051499	4.815738
249.218016	8000.543717	11.227891	-0.051523	4.815768
249.271731	8000.432481	11.232896	-0.051533	4.815735
249.102137	8000.618709	11.237901	-0.051502	4.815791
249.304542	8000.555801	11.242906	-0.051539	4.815771
249.208205	8000.538219	11.247911	-0.051521	4.815767
249.207267	8000.540339	11.252915	-0.051521	4.815767
249.295236	8000.544972	11.257920	-0.051538	4.815768
249.352290	8000.512800	11.262925	-0.051548	4.815759
249.230920	8000.424342	11.267930	-0.051526	4.815733
249.226632	8000.522502	11.272935	-0.051525	4.815762
249.377145	8000.637059	11.277939	-0.051553	4.815795
249.381393	8000.527152	11.282944	-0.051554	4.815763
249.287126	8000.524552	11.287949	-0.051536	4.815762
249.264736	8000.644840	11.292954	-0.051532	4.815798
249.742034	8000.396347	11.297959	-0.051621	4.815723
249.322195	8000.650044	11.302963	-0.051543	4.815799
249.468735	8000.410055	11.307968	-0.051570	4.815728
249.514154	8000.535716	11.312973	-0.051578	4.815764
249.351884	8000.530942	11.317978	-0.051548	4.815764
249.266108	8000.490042	11.322983	-0.051532	4.815752
249.106743	8000.591019	11.327987	-0.051503	4.815783
249.440479	8000.438423	11.332992	-0.051565	4.815736
249.154213	8000.635567	11.337997	-0.051511	4.815795
249.268809	8000.502898	11.343002	-0.051533	4.815756
249.293786	8000.510778	11.348007	-0.051537	4.815758
249.161512	8000.499018	11.353011	-0.051513	4.815755
249.340018	8000.662077	11.358016	-0.051546	4.815802
249.377457	8000.492919	11.363021	-0.051553	4.815753
249.386110	8000.516549	11.368026	-0.051555	4.815759
249.368458	8000.548293	11.373031	-0.051551	4.815769
249.377223	8000.532420	11.378035	-0.051553	4.815764
249.417064	8000.380384	11.383040	-0.051560	4.815720
249.217917	8000.499934	11.388045	-0.051523	4.815755
249.246356	8000.432062	11.393050	-0.051528	4.815735
249.481559	8000.377161	11.398055	-0.051572	4.815718
249.297595	8000.649641	11.403059	-0.051538	4.815799
249.274650	8000.457079	11.408064	-0.051534	4.815743
249.334256	8000.444167	11.413069	-0.051545	4.815739
249.297162	8000.528981	11.418074	-0.051538	4.815764
249.246259	8000.644534	11.423079	-0.051529	4.815798
249.157519	8000.537388	11.428083	-0.051512	4.815767
249.375014	8000.661576	11.433088	-0.051553	4.815802
249.447553	8000.449211	11.438093	-0.051566	4.815739
249.166009	8000.494817	11.443098	-0.051513	4.815754
249.284224	8000.540514	11.448103	-0.051536	4.815767
249.317357	8000.636080	11.453107	-0.051542	4.815795
249.343025	8000.401600	11.458112	-0.051546	4.815726
249.388819	8000.510183	11.463117	-0.051555	4.815758
249.255178	8000.514416	11.468122	-0.051530	4.815759
249.340731	8000.655678	11.473127	-0.051546	4.815800
249.263562	8000.520959	11.478131	-0.051532	4.815761
249.495614	8000.557830	11.483136	-0.051575	4.815771
249.340863	8000.538231	11.488141	-0.051546	4.815766
249.437178	8000.546202	11.493146	-0.051564	4.815768
249.536288	8000.481615	11.498151	-0.051582	4.815749
249.417677	8000.600339	11.503155	-0.051560	4.815784
249.362050	8000.433939	11.508160	-0.051550	4.815735
249.521051	8000.503789	11.513165	-0.051580	4.815755
249.534965	8000.431410	11.518170	-0.051582	4.815734
249.633455	8000.424469	11.523175	-0.051600	4.815731
249.549305	8000.630239	11.528179	-0.051585	4.815792
249.502524	8000.383903	11.533184	-0.051576	4.815720
249.359479	8000.507568	11.538189	-0.051549	4.815757
249.337658	8000.555260	11.543194	-0.051545	4.815771
249.373528	8000.392483	11.548199	-0.051552	4.815723
249.322165	8000.430085	11.553203	-0.051542	4.815734
249.232475	8000.422221	11.558208	-0.051526	4.815733
249.150823	8000.423029	11.563213	-0.051511	4.815733
249.225325	8000.540620	11.568218	-0.051524	4.815767
249.302946	8000.537611	11.573223	-0.051539	4.815766
249.130864	8000.626637	11.578227	-0.051507	4.815793
249.412004	8000.418732	11.583232	-0.051559	4.815731
249.271463	8000.545640	11.588237	-0.051533	4.815769
249.260679	8000.636221	11.593242	-0.051531	4.815795
249.488010	8000.390071	11.598247	-0.051573	4.815722
249.354419	8000.522431	11.603251	-0.051549	4.815761
249.507765	8000.546278	11.608256	-0.051577	4.815768
249.578826	8000.546365	11.613261	-0.051590	4.815767
249.488717	8000.523546	11.618266	-0.051574	4.815761
249.437547	8000.438364	11.623271	-0.051564	4.815736
249.397074	8000.553019	11.628275	-0.051556	4.815770
249.464644	8000.540237	11.633280	-0.051569	4.815766
249.309472	8000.348730	11.638285	-0.051540	4.815711
249.281327	8000.631216	11.643290	-0.051535	4.815793
249.396728	8000.545539	11.648295	-0.051556	4.815768
249.391032	8000.432269	11.653299	-0.051555	4.815735
249.456846	8000.367140	11.658304	-0.051567	4.815715
249.507108	8000.441629	11.663309	-0.051577	4.815737
249.338315	8000.474120	11.668314	-0.051545	4.815747
249.323043	8000.506970	11.673319	-0.051543	4.815757
249.383420	8000.535712	11.678323	-0.051554	4.815765
249.618743	8000.648446	11.683328	-0.051598	4.815797
249.364712	8000.438246	11.688333	-0.051550	4.815737
249.224216	8000.544868	11.693338	-0.051524	4.815769
249.348150	8000.536206	11.698343	-0.051547	4.815765
249.470953	8000.513644	11.703347	-0.051570	4.815758
249.327047	8000.449378	11.708352	-0.051543	4.815740
249.290170	8000.397528	11.713357	-0.051536	4.815725
249.454574	8000.413013	11.718362	-0.051567	4.815729
249.472845	8000.390887	11.723367	-0.051570	4.815722
249.347659	8000.509504	11.728371	-0.051547	4.815758
249.552889	8000.462657	11.733376	-0.051585	4.815743
249.549282	8000.426296	11.738381	-0.051585	4.815732
249.422134	8000.521391	11.743386	-0.051561	4.815761
249.574297	8000.426702	11.748391	-0.051589	4.815732
249.577869	8000.629627	11.753395	-0.051590	4.815792
249.546222	8000.408095	11.758400	-0.051584	4.815727
249.581645	8000.470598	11.763405	-0.051591	4.815745
249.689723	8000.538553	11.768410	-0.051611	4.815764
249.513822	8000.423583	11.773415	-0.051578	4.815732
249.527307	8000.526303	11.778419	-0.051581	4.815762
249.872487	8000.262850	11.783424	-0.051645	4.815683
249.663606	8000.371564	11.788429	-0.051606	4.815716
249.428158	8000.548180	11.793434	-0.051562	4.815769
249.513297	8000.395813	11.798439	-0.051578	4.815724
249.448316	8000.641399	11.803443	-0.051566	4.815796
249.500223	8000.552554	11.808448	-0.051576	4.815769
249.751428	8000.409293	11.813453	-0.051622	4.815726
249.703295	8000.631664	11.818458	-0.051613	4.815792
249.511329	8000.563411	11.823463	-0.051578	4.815773
249.471686	8000.523261	11.828467	-0.051570	4.815761
249.669434	8000.390876	11.833472	-0.051607	4.815721
249.684284	8000.313174	11.838477	-0.051610	4.815699
249.606556	8000.420817	11.843482	-0.051595	4.815730
249.954386	8000.268449	11.848487	-0.051660	4.815684
249.792880	8000.456945	11.853491	-0.051630	4.815740
249.682520	8000.299264	11.858496	-0.051609	4.815695
249.582767	8000.434310	11.863501	-0.051591	4.815734
249.812516	8000.029113	11.868506	-0.051633	4.815615
249.527582	8000.249767	11.873511	-0.051580	4.815681
249.428036	8000.415778	11.878515	-0.051562	4.815730
249.552030	8000.464773	11.883520	-0.051585	4.815744
249.575806	8000.516410	11.888525	-0.051590	4.815759
249.588295	8000.469633	11.893530	-0.051592	4.815745
249.704744	8000.540928	11.898535	-0.051614	4.815765
249.452144	8000.595545	11.903539	-0.051567	4.815782
249.615418	8000.455125	11.908544	-0.051597	4.815740
249.505852	8000.504594	11.913549	-0.051577	4.815755
249.316378	8000.405420	11.918554	-0.051541	4.815727
249.630586	8000.270657	11.923559	-0.051600	4.815686
249.609597	8000.499874	11.928563	-0.051596	4.815754
249.717412	8000.358553	11.933568	-0.051616	4.815712
249.560711	8000.499079	11.938573	-0.051587	4.815754
249.509605	8000.552701	11.943578	-0.051577	4.815769
249.662524	8000.459093	11.948583	-0.051606	4.815741
249.653045	8000.498444	11.953587	-0.051604	4.815753
249.724585	8000.451560	11.958592	-0.051617	4.815739
249.461469	8000.531631	11.963597	-0.051568	4.815764
249.525974	8000.563644	11.968602	-0.051580	4.815773
249.887520	8000.444598	11.973607	-0.051648	4.815736
249.445139	8000.536704	11.978611	-0.051565	4.815765
249.562512	8000.546086	11.983616	-0.051587	4.815767
249.652274	8000.450383	11.988621	-0.051604	4.815739
249.514550	8000.431060	11.993626	-0.051578	4.815734
249.645610	8000.527150	11.998631	-0.051603	4.815761
249.690336	8000.454204	12.003635	-0.051611	4.815740
249.788349	8000.283895	12.008640	-0.051629	4.815690
249.717788	8000.521916	12.013645	-0.051616	4.815759
249.575525	8000.542025	12.018650	-0.051590	4.815766
249.701674	8000.394596	12.023655	-0.051613	4.815722
249.569661	8000.524846	12.028659	-0.051588	4.815761
249.646030	8000.550645	12.033664	-0.051603	4.815768
249.686085	8000.457337	12.038669	-0.051610	4.815741
249.618659	8000.548064	12.043674	-0.051598	4.815768
249.674238	8000.540426	12.048679	-0.051608	4.815765
249.660657	8000.546611	12.053683	-0.051605	4.815767
249.726782	8000.579718	12.058688	-0.051618	4.815776
249.681956	8000.553364	12.063693	-0.051609	4.815769
249.558285	8000.523592	12.068698	-0.051586	4.815761
249.793136	8000.449466	12.073703	-0.051630	4.815738
249.531824	8000.627798	12.078707	-0.051581	4.815791
249.530051	8000.546622	12.083712	-0.051581	4.815768
249.904504	8000.429922	12.088717	-0.051651	4.815732
249.956985	8000.543954	12.093722	-0.051661	4.815765
249.636131	8000.570768	12.098727	-0.051601	4.815774
249.625877	8000.532164	12.103731	-0.051599	4.815763
249.885896	8000.527849	12.108736	-0.051647	4.815760
249.819322	8000.375150	12.113741	-0.051635	4.815716
249.741590	8000.543654	12.118746	-0.051620	4.815766
249.987013	8000.435533	12.123751	-0.051666	4.815733
250.000776	8000.638625	12.128755	-0.051669	4.815792
249.980895	8000.423688	12.133760	-0.051665	4.815729
249.869878	8000.528655	12.138765	-0.051644	4.815761
249.798507	8000.563797	12.143770	-0.051631	4.815771
250.027202	8000.369987	12.148775	-0.051673	4.815714
249.757997	8000.640015	12.153779	-0.051623	4.815794
249.890496	8000.295159	12.158784	-0.051648	4.815692
249.819212	8000.500070	12.163789	-0.051635	4.815753
249.707843	8000.488649	12.168794	-0.051614	4.815750
249.854666	8000.557235	12.173799	-0.051641	4.815769
249.995735	8000.360932	12.178803	-0.051668	4.815711
249.807415	8000.500945	12.183808	-0.051633	4.815753
249.831733	8000.397771	12.188813	-0.051637	4.815723
249.993126	8000.562689	12.193818	-0.051667	4.815770
249.790119	8000.437668	12.198823	-0.051629	4.815734
249.866896	8000.638581	12.203827	-0.051644	4.815793
250.006356	8000.445454	12.208832	-0.051670	4.815736
249.855597	8000.295658	12.213837	-0.051641	4.815693
249.590104	8000.463244	12.218842	-0.051592	4.815743
250.042607	8000.532529	12.223847	-0.051676	4.815761
249.979099	8000.521886	12.228851	-0.051665	4.815758
249.981749	8000.486694	12.233856	-0.051665	4.815748
249.771961	8000.442710	12.238861	-0.051626	4.815736
249.711286	8000.475890	12.243866	-0.051615	4.815746
249.918860	8000.575360	12.248871	-0.051653	4.815774
249.828455	8000.532248	12.253875	-0.051636	4.815762
249.783199	8000.531512	12.258880	-0.051628	4.815762
249.725035	8000.528431	12.263885	-0.051617	4.815761
249.623380	8000.525710	12.268890	-0.051598	4.815761
249.985117	8000.434429	12.273895	-0.051666	4.815733
249.796333	8000.609669	12.278899	-0.051631	4.815785
249.643714	8000.482264	12.283904	-0.051602	4.815748
249.851361	8000.358581	12.288909	-0.051641	4.815711
250.087677	8000.472398	12.293914	-0.051685	4.815743
250.052648	8000.431255	12.298919	-0.051678	4.815731
249.612157	8000.499901	12.303923	-0.051596	4.815754
249.622270	8000.645276	12.308928	-0.051598	4.815796
249.929589	8000.540297	12.313933	-0.051655	4.815764
249.756043	8000.560965	12.318938	-0.051623	4.815771
249.813099	8000.385718	12.323943	-0.051634	4.815719
249.758772	8000.476659	12.328947	-0.051623	4.815746
249.715502	8000.335017	12.333952	-0.051615	4.815705
249.770374	8000.417055	12.338957	-0.051626	4.815729
249.781003	8000.430040	12.343962	-0.051628	4.815732
250.114366	8000.458950	12.348967	-0.051690	4.815739
249.845225	8000.621139	12.353971	-0.051640	4.815788
250.023281	8000.553564	12.358976	-0.051673	4.815767
249.945062	8000.554427	12.363981	-0.051658	4.815768
249.747815	8000.467937	12.368986	-0.051621	4.815744
249.957790	8000.352834	12.373991	-0.051660	4.815709
249.819842	8000.449889	12.378995	-0.051635	4.815738
249.687185	8000.390075	12.384000	-0.051610	4.815721
249.643007	8000.537770	12.389005	-0.051602	4.815764
249.670599	8000.307592	12.394010	-0.051607	4.815697
249.874696	8000.397394	12.399015	-0.051645	4.815722
249.869601	8000.629007	12.404019	-0.051644	4.815790
249.945822	8000.404956	12.409024	-0.051658	4.815724
250.046620	8000.292349	12.414029	-0.051677	4.815691
249.880054	8000.451934	12.419034	-0.051646	4.815738
249.902682	8000.539855	12.424039	-0.051650	4.815764
250.009693	8000.650504	12.429043	-0.051670	4.815796
249.806836	8000.535093	12.434048	-0.051632	4.815763
249.788281	8000.308435	12.439053	-0.051629	4.815697
249.757026	8000.543892	12.444058	-0.051623	4.815766
249.895192	8000.413741	12.449063	-0.051649	4.815727
249.831980	8000.557924	12.454067	-0.051637	4.815769
250.044848	8000.536827	12.459072	-0.051677	4.815762
249.965592	8000.519522	12.464077	-0.051662	4.815758
249.785085	8000.545415	12.469082	-0.051628	4.815766
249.800654	8000.546736	12.474087	-0.051631	4.815766
249.786408	8000.638329	12.479091	-0.051629	4.815793
249.955187	8000.549249	12.484096	-0.051660	4.815766
249.887326	8000.554551	12.489101	-0.051647	4.815768
249.871878	8000.517997	12.494106	-0.051644	4.815758
249.926342	8000.484715	12.499111	-0.051655	4.815748
249.891355	8000.641102	12.504115	-0.051648	4.815793
250.119586	8000.527363	12.509120	-0.051691	4.815759
250.068506	8000.543616	12.514125	-0.051681	4.815764
249.849165	8000.549659	12.519130	-0.051640	4.815767
250.022566	8000.539665	12.524135	-0.051673	4.815763
250.106322	8000.640327	12.529139	-0.051688	4.815792
250.152144	8000.538569	12.534144	-0.051697	4.815762
250.011654	8000.441256	12.539149	-0.051670	4.815734
249.889091	8000.551375	12.544154	-0.051648	4.815767
250.193899	8000.430339	12.549159	-0.051704	4.815730
250.012996	8000.532034	12.554163	-0.051671	4.815761
250.036454	8000.644528	12.559168	-0.051675	4.815794
250.075472	8000.428413	12.564173	-0.051682	4.815730
249.826862	8000.622967	12.569178	-0.051636	4.815789
249.952177	8000.556670	12.574183	-0.051659	4.815769
249.975908	8000.538905	12.579187	-0.051664	4.815763
250.201616	8000.524423	12.584192	-0.051706	4.815758
250.133989	8000.635436	12.589197	-0.051693	4.815791
249.996065	8000.433527	12.594202	-0.051667	4.815732
250.294822	8000.379659	12.599207	-0.051723	4.815715
250.242093	8000.545368	12.604211	-0.051713	4.815764
250.134821	8000.441121	12.609216	-0.051693	4.815734
250.271198	8000.499928	12.614221	-0.051719	4.815750
250.006757	8000.554353	12.619226	-0.051670	4.815768
250.132008	8000.386621	12.624231	-0.051693	4.815718
250.250752	8000.558321	12.629235	-0.051715	4.815768
250.346652	8000.639961	12.634240	-0.051733	4.815791
250.075069	8000.549057	12.639245	-0.051682	4.815766
249.945253	8000.545878	12.644250	-0.051658	4.815765
250.197234	8000.547840	12.649255	-0.051705	4.815765
250.106998	8000.553846	12.654259	-0.051688	4.815767
249.993966	8000.545602	12.659264	-0.051667	4.815765
250.184806	8000.440864	12.664269	-0.051703	4.815734
250.017874	8000.637815	12.669274	-0.051672	4.815792
249.996407	8000.457019	12.674279	-0.051668	4.815739
250.054008	8000.515613	12.679283	-0.051678	4.815756
250.215419	8000.592979	12.684288	-0.051708	4.815778
250.221945	8000.527953	12.689293	-0.051710	4.815759
250.126260	8000.541345	12.694298	-0.051692	4.815763
250.167719	8000.421366	12.699303	-0.051699	4.815728
250.147919	8000.527816	12.704307	-0.051696	4.815759
250.113264	8000.432225	12.709312	-0.051689	4.815731
250.107932	8000.536775	12.714317	-0.051688	4.815762
250.038343	8000.549524	12.719322	-0.051675	4.815766
250.201164	8000.560714	12.724327	-0.051706	4.815769
249.997873	8000.516834	12.729331	-0.051668	4.815757
250.062048	8000.441001	12.734336	-0.051680	4.815734
250.138083	8000.374970	12.739341	-0.051694	4.815715
249.887534	8000.539597	12.744346	-0.051647	4.815764
249.991993	8000.541295	12.749351	-0.051667	4.815764
250.032089	8000.540879	12.754355	-0.051674	4.815764
250.187920	8000.558361	12.759360	-0.051703	4.815768
250.202819	8000.548994	12.764365	-0.051706	4.815765
250.273499	8000.553346	12.769370	-0.051719	4.815766
250.022611	8000.447832	12.774375	-0.051672	4.815736
250.004450	8000.512668	12.779379	-0.051669	4.815755
250.104224	8000.595438	12.784384	-0.051688	4.815779
250.096376	8000.550465	12.789389	-0.051686	4.815766
250.157772	8000.640086	12.794394	-0.051698	4.815792
250.105651	8000.459858	12.799399	-0.051688	4.815739
250.291272	8000.648663	12.804403	-0.051723	4.815794
250.109039	8000.553873	12.809408	-0.051689	4.815767
250.086301	8000.541758	12.814413	-0.051684	4.815764
250.079161	8000.564065	12.819418	-0.051683	4.815770
250.168803	8000.502526	12.824423	-0.051700	4.815752
250.106100	8000.636041	12.829427	-0.051688	4.815791
250.142753	8000.504237	12.834432	-0.051695	4.815752
250.207599	8000.551204	12.839437	-0.051707	4.815766
250.036938	8000.533480	12.844442	-0.051675	4.815761
250.302563	8000.506836	12.849447	-0.051724	4.815752
250.178518	8000.538986	12.854451	-0.051701	4.815762
250.195195	8000.612931	12.859456	-0.051705	4.815784
250.182295	8000.559334	12.864461	-0.051702	4.815768
249.932082	8000.523233	12.869466	-0.051656	4.815759
250.200612	8000.535073	12.874471	-0.051706	4.815761
250.188820	8000.628842	12.879475	-0.051703	4.815789
250.174536	8000.611526	12.884480	-0.051701	4.815784
250.209516	8000.508524	12.889485	-0.051707	4.815753
250.095254	8000.582475	12.894490	-0.051686	4.815775
250.120418	8000.462230	12.899495	-0.051691	4.815740
250.001796	8000.629003	12.904499	-0.051669	4.815789
249.940001	8000.420858	12.909504	-0.051657	4.815729
249.945763	8000.649446	12.914509	-0.051658	4.815796
250.170117	8000.632807	12.919514	-0.051700	4.815790
250.181223	8000.322278	12.924519	-0.051702	4.815699
250.105793	8000.514310	12.929523	-0.051688	4.815755
250.204540	8000.538338	12.934528	-0.051706	4.815762
250.439556	8000.402286	12.939533	-0.051750	4.815721
250.406927	8000.551239	12.944538	-0.051744	4.815765
250.250321	8000.252931	12.949543	-0.051715	4.815678
250.260420	8000.402576	12.954547	-0.051717	4.815722
250.104429	8000.362670	12.959552	-0.051687	4.815711
250.205995	8000.442265	12.964557	-0.051706	4.815734
250.135736	8000.556437	12.969562	-0.051693	4.815768
250.036607	8000.356228	12.974567	-0.051675	4.815710
250.127705	8000.395079	12.979571	-0.051692	4.815720
250.107449	8000.534622	12.984576	-0.051688	4.815761
250.259519	8000.533891	12.989581	-0.051716	4.815760
250.127836	8000.629981	12.994586	-0.051692	4.815789
250.264355	8000.521157	12.999591	-0.051717	4.815757
250.418135	8000.533267	13.004595	-0.051746	4.815759
250.358298	8000.521616	13.009600	-0.051735	4.815756
250.380105	8000.551868	13.014605	-0.051739	4.815765
250.488737	8000.506654	13.019610	-0.051759	4.815751
250.591133	8000.401545	13.024615	-0.051778	4.815720
250.331156	8000.497684	13.029619	-0.051730	4.815749
250.304291	8000.654205	13.034624	-0.051725	4.815795
250.360419	8000.534463	13.039629	-0.051735	4.815760
250.355140	8000.646490	13.044634	-0.051734	4.815793
250.451712	8000.431309	13.049639	-0.051752	4.815729
250.294300	8000.460781	13.054643	-0.051723	4.815739
250.148635	8000.621775	13.059648	-0.051696	4.815787
250.299009	8000.551615	13.064653	-0.051724	4.815765
250.185091	8000.527339	13.069658	-0.051703	4.815759
250.443276	8000.552893	13.074663	-0.051751	4.815765
250.345629	8000.400754	13.079667	-0.051732	4.815721
250.422552	8000.537607	13.084672	-0.051747	4.815761
250.249616	8000.563623	13.089677	-0.051715	4.815769
250.332043	8000.535067	13.094682	-0.051730	4.815760
250.324042	8000.563765	13.099687	-0.051728	4.815769
250.517166	8000.525264	13.104691	-0.051764	4.815757
250.409381	8000.537392	13.109696	-0.051744	4.815761
250.291455	8000.557896	13.114701	-0.051722	4.815767
250.287107	8000.531132	13.119706	-0.051722	4.815759
250.271853	8000.543696	13.124711	-0.051719	4.815763
250.076609	8000.513828	13.129715	-0.051682	4.815755
250.158370	8000.548257	13.134720	-0.051698	4.815765
250.339899	8000.543735	13.139725	-0.051731	4.815763
250.154722	8000.616532	13.144730	-0.051697	4.815785
250.050252	8000.362849	13.149735	-0.051677	4.815711
250.107116	8000.519662	13.154739	-0.051688	4.815757
250.316183	8000.641581	13.159744	-0.051727	4.815792
250.294629	8000.283539	13.164749	-0.051723	4.815687
250.022277	8000.420051	13.169754	-0.051672	4.815728
250.157635	8000.208707	13.174759	-0.051697	4.815666
250.182071	8000.498457	13.179763	-0.051702	4.815750
250.118705	8000.409873	13.184768	-0.051690	4.815725
250.280561	8000.330289	13.189773	-0.051720	4.815701
250.091728	8000.564255	13.194778	-0.051685	4.815770
250.086503	8000.308983	13.199783	-0.051684	4.815695
250.222215	8000.527938	13.204787	-0.051709	4.815759
250.291290	8000.653987	13.209792	-0.051722	4.815795
250.148576	8000.338820	13.214797	-0.051696	4.815704
250.131573	8000.634305	13.219802	-0.051693	4.815790
250.319497	8000.307431	13.224807	-0.051727	4.815694
250.273002	8000.398499	13.229811	-0.051719	4.815721
250.292803	8000.365722	13.234816	-0.051722	4.815711
250.432833	8000.301799	13.239821	-0.051748	4.815692
250.211962	8000.535244	13.244826	-0.051707	4.815761
250.386605	8000.409955	13.249831	-0.051740	4.815724
250.385973	8000.414216	13.254835	-0.051740	4.815725
250.368220	8000.519633	13.259840	-0.051737	4.815756
250.266203	8000.523312	13.264845	-0.051718	4.815757
250.451363	8000.641640	13.269850	-0.051752	4.815791
250.575120	8000.301976	13.274855	-0.051775	4.815691
250.545440	8000.543869	13.279859	-0.051770	4.815762
250.331169	8000.560671	13.284864	-0.051730	4.815768
250.390718	8000.234914	13.289869	-0.051741	4.815672
250.327012	8000.407917	13.294874	-0.051729	4.815723
250.277542	8000.443415	13.299879	-0.051720	4.815734
250.317400	8000.541227	13.304883	-0.051727	4.815762
250.414542	8000.574839	13.309888	-0.051745	4.815772
250.216568	8000.359140	13.314893	-0.051708	4.815710
250.219290	8000.415774	13.319898	-0.051709	4.815726
250.364814	8000.563352	13.324903	-0.051736	4.815769
250.317993	8000.425920	13.329907	-0.051727	4.815729
250.202593	8000.435789	13.334912	-0.051706	4.815732
250.235347	8000.474759	13.339917	-0.051712	4.815743
250.423071	8000.504505	13.344922	-0.051747	4.815751
250.366216	8000.501445	13.349927	-0.051736	4.815750
250.399153	8000.413359	13.354931	-0.051742	4.815724
250.505963	8000.551766	13.359936	-0.051762	4.815764
250.654398	8000.369461	13.364941	-0.051790	4.815710
250.453925	8000.411046	13.369946	-0.051752	4.815724
250.459218	8000.429283	13.374951	-0.051753	4.815729
250.313426	8000.506992	13.379955	-0.051726	4.815752
250.365120	8000.464055	13.384960	-0.051736	4.815739
250.423482	8000.267474	13.389965	-0.051747	4.815682
250.429266	8000.429863	13.394970	-0.051748	4.815729
250.237116	8000.406451	13.399975	-0.051712	4.815723
250.464737	8000.302312	13.404979	-0.051754	4.815692
250.512551	8000.469655	13.409984	-0.051763	4.815740
250.387402	8000.472958	13.414989	-0.051740	4.815742
250.139681	8000.450778	13.419994	-0.051694	4.815737
250.469328	8000.448665	13.424999	-0.051755	4.815734
250.685976	8000.492762	13.430003	-0.051796	4.815746
250.587398	8000.412146	13.435008	-0.051777	4.815723
250.453682	8000.362991	13.440013	-0.051752	4.815710
250.294975	8000.433016	13.445018	-0.051723	4.815731
250.409044	8000.383619	13.450023	-0.051744	4.815716
250.573957	8000.425807	13.455027	-0.051775	4.815727
250.552039	8000.493786	13.460032	-0.051771	4.815747
250.756416	8000.578259	13.465037	-0.051809	4.815771
250.396434	8000.436800	13.470042	-0.051742	4.815731
250.447919	8000.401334	13.475047	-0.051751	4.815721
250.431865	8000.448053	13.480051	-0.051748	4.815734
250.181887	8000.419430	13.485056	-0.051702	4.815727
250.350790	8000.325013	13.490061	-0.051733	4.815699
250.552600	8000.476710	13.495066	-0.051771	4.815742
250.547751	8000.585540	13.500071	-0.051770	4.815774
250.409016	8000.435936	13.505075	-0.051744	4.815731
250.472892	8000.460464	13.510080	-0.051756	4.815738
250.467496	8000.448631	13.515085	-0.051755	4.815734
250.444773	8000.544358	13.520090	-0.051751	4.815763
250.422012	8000.329373	13.525095	-0.051746	4.815700
250.605719	8000.338766	13.530099	-0.051781	4.815702
250.392632	8000.481581	13.535104	-0.051741	4.815744
250.353393	8000.393388	13.540109	-0.051734	4.815719
250.176883	8000.370231	13.545114	-0.051701	4.815713
250.365639	8000.344472	13.550119	-0.051736	4.815705
250.386534	8000.425959	13.555123	-0.051740	4.815728
250.396699	8000.489120	13.560128	-0.051742	4.815747
250.468056	8000.434758	13.565133	-0.051755	4.815730
250.348595	8000.496879	13.570138	-0.051733	4.815749
250.301445	8000.475825	13.575143	-0.051724	4.815743
250.438489	8000.516492	13.580147	-0.051749	4.815754
250.526260	8000.532868	13.585152	-0.051766	4.815759
250.468773	8000.396330	13.590157	-0.051755	4.815719
250.536736	8000.547987	13.595162	-0.051768	4.815763
250.435928	8000.550618	13.600167	-0.051749	4.815764
250.423810	8000.475679	13.605171	-0.051747	4.815743
250.370874	8000.483359	13.610176	-0.051737	4.815745
250.521182	8000.604323	13.615181	-0.051765	4.815780
250.365801	8000.584712	13.620186	-0.051736	4.815775
250.604495	8000.400671	13.625191	-0.051780	4.815720
250.756242	8000.297433	13.630195	-0.051808	4.815689
250.510525	8000.503781	13.635200	-0.051763	4.815750
250.488239	8000.489538	13.640205	-0.051759	4.815746
250.287629	8000.600523	13.645210	-0.051721	4.815780
250.484385	8000.399785	13.650215	-0.051758	4.815720
250.246220	8000.536853	13.655219	-0.051714	4.815761
250.315395	8000.551858	13.660224	-0.051727	4.815765
250.419296	8000.570632	13.665229	-0.051746	4.815770
250.403369	8000.558627	13.670234	-0.051743	4.815767
250.512412	8000.440814	13.675239	-0.051763	4.815732
250.622922	8000.532301	13.680243	-0.051784	4.815758
250.644928	8000.580708	13.685248	-0.051788	4.815772
250.428898	8000.531281	13.690253	-0.051748	4.815759
250.542073	8000.542731	13.695258	-0.051769	4.815762
250.453562	8000.557307	13.700263	-0.051752	4.815766
250.423709	8000.497028	13.705267	-0.051747	4.815749
250.328522	8000.540325	13.710272	-0.051729	4.815762
250.390103	8000.449501	13.715277	-0.051740	4.815735
250.235303	8000.540944	13.720282	-0.051712	4.815763
250.239596	8000.530336	13.725287	-0.051712	4.815759
250.463820	8000.618334	13.730291	-0.051754	4.815784
250.418780	8000.570621	13.735296	-0.051746	4.815770
250.437892	8000.420380	13.740301	-0.051749	4.815726
250.365694	8000.429883	13.745306	-0.051736	4.815729
250.549335	8000.443547	13.750311	-0.051770	4.815733
250.578358	8000.448290	13.755315	-0.051775	4.815734
250.428442	8000.551558	13.760320	-0.051748	4.815765
250.550699	8000.453178	13.765325	-0.051770	4.815735
250.621952	8000.555772	13.770330	-0.051784	4.815765
250.588678	8000.514657	13.775335	-0.051777	4.815753
250.570566	8000.535717	13.780339	-0.051774	4.815759
250.621969	8000.628379	13.785344	-0.051784	4.815786
250.609955	8000.538493	13.790349	-0.051781	4.815760
250.448740	8000.486754	13.795354	-0.051751	4.815746
250.485032	8000.622948	13.800359	-0.051758	4.815785
250.446612	8000.502735	13.805363	-0.051751	4.815750
250.426599	8000.572880	13.810368	-0.051747	4.815771
250.692093	8000.568657	13.815373	-0.051797	4.815769
250.614749	8000.521485	13.820378	-0.051782	4.815755
250.562760	8000.430949	13.825383	-0.051772	4.815729
250.695780	8000.363710	13.830387	-0.051797	4.815709
250.506610	8000.544284	13.835392	-0.051762	4.815762
250.598527	8000.431531	13.840397	-0.051779	4.815729
250.539503	8000.532006	13.845402	-0.051768	4.815759
250.627981	8000.421332	13.850407	-0.051785	4.815726
250.585899	8000.531692	13.855411	-0.051777	4.815758
250.543989	8000.652734	13.860416	-0.051769	4.815794
250.582210	8000.454754	13.865421	-0.051776	4.815736
250.563513	8000.433095	13.870426	-0.051773	4.815729
250.553245	8000.548244	13.875431	-0.051771	4.815763
250.544709	8000.453076	13.880435	-0.051769	4.815735
250.626623	8000.525947	13.885440	-0.051784	4.815756
250.681214	8000.546054	13.890445	-0.051795	4.815762
250.416844	8000.512925	13.895450	-0.051745	4.815754
250.491977	8000.532298	13.900455	-0.051759	4.815759
250.662669	8000.547888	13.905459	-0.051791	4.815763
250.374347	8000.538927	13.910464	-0.051737	4.815761
250.491305	8000.532287	13.915469	-0.051759	4.815759
250.542019	8000.619599	13.920474	-0.051769	4.815784
250.291892	8000.536517	13.925479	-0.051722	4.815761
250.405236	8000.641932	13.930483	-0.051743	4.815791
250.437742	8000.534618	13.935488	-0.051749	4.815760
250.402643	8000.573554	13.940493	-0.051743	4.815771
250.448510	8000.481406	13.945498	-0.051751	4.815744
250.479708	8000.598297	13.950503	-0.051757	4.815778
250.657880	8000.415408	13.955507	-0.051790	4.815724
250.416507	8000.592998	13.960512	-0.051745	4.815777
250.396515	8000.537150	13.965517	-0.051742	4.815761
250.460433	8000.549934	13.970522	-0.051753	4.815764
250.592791	8000.567035	13.975527	-0.051778	4.815769
250.376222	8000.514397	13.980531	-0.051738	4.815754
250.554713	8000.636887	13.985536	-0.051771	4.815789
250.524546	8000.546705	13.990541	-0.051765	4.815763
250.514704	8000.525190	13.995546	-0.051764	4.815757
250.452149	8000.414196	14.000551	-0.051752	4.815724
250.488077	8000.452151	14.005555	-0.051758	4.815735
250.552830	8000.630449	14.010560	-0.051771	4.815787
250.485810	8000.432894	14.015565	-0.051758	4.815730
250.502211	8000.533528	14.020570	-0.051761	4.815759
250.211066	8000.402801	14.025575	-0.051707	4.815722
250.392343	8000.620363	14.030579	-0.051741	4.815785
250.434643	8000.521751	14.035584	-0.051749	4.815756
250.533416	8000.426193	14.040589	-0.051767	4.815728
250.347058	8000.634575	14.045594	-0.051732	4.815789
250.529597	8000.513685	14.050599	-0.051766	4.815753
250.604281	8000.556542	14.055603	-0.051780	4.815765
250.547375	8000.531058	14.060608	-0.051770	4.815758
250.562999	8000.449096	14.065613	-0.051772	4.815734
250.289315	8000.629363	14.070618	-0.051722	4.815788
250.331645	8000.417572	14.075623	-0.051729	4.815726
250.444808	8000.424751	14.080627	-0.051750	4.815728
250.476339	8000.513885	14.085632	-0.051756	4.815754
250.683926	8000.392336	14.090637	-0.051795	4.815717
250.483593	8000.521477	14.095642	-0.051758	4.815756
250.639453	8000.537893	14.100647	-0.051787	4.815760
250.607026	8000.546975	14.105651	-0.051781	4.815763
250.420138	8000.547138	14.110656	-0.051746	4.815764
250.458708	8000.533885	14.115661	-0.051753	4.815759
250.552755	8000.531143	14.120666	-0.051771	4.815758
250.346063	8000.658046	14.125671	-0.051732	4.815796
250.387005	8000.483602	14.130675	-0.051740	4.815745
250.288723	8000.587709	14.135680	-0.051721	4.815776
250.539985	8000.533070	14.140685	-0.051768	4.815759
250.631854	8000.583681	14.145690	-0.051785	4.815773
250.672306	8000.586474	14.150695	-0.051793	4.815774
250.713334	8000.439792	14.155699	-0.051800	4.815731
250.588051	8000.533851	14.160704	-0.051777	4.815759
250.723249	8000.517898	14.165709	-0.051802	4.815754
250.648780	8000.629868	14.170714	-0.051788	4.815787
250.636891	8000.534645	14.175719	-0.051786	4.815759
250.503051	8000.475878	14.180723	-0.051761	4.815742
250.486488	8000.555689	14.185728	-0.051758	4.815766
250.723926	8000.558483	14.190733	-0.051802	4.815765
250.774991	8000.395948	14.195738	-0.051812	4.815718
250.561061	8000.427704	14.200743	-0.051772	4.815728
250.634105	8000.407537	14.205747	-0.051786	4.815722
250.517085	8000.416311	14.210752	-0.051764	4.815725
250.664962	8000.400564	14.215757	-0.051791	4.815720
250.613842	8000.540675	14.220762	-0.051782	4.815761
250.463866	8000.526490	14.225767	-0.051754	4.815757
250.537484	8000.567194	14.230771	-0.051768	4.815769
250.478856	8000.547021	14.235776	-0.051757	4.815763
250.555474	8000.419070	14.240781	-0.051771	4.815725
250.258226	8000.452674	14.245786	-0.051716	4.815737
250.260910	8000.370503	14.250791	-0.051716	4.815713
250.622686	8000.619831	14.255795	-0.051784	4.815784
250.774263	7999.472365	14.260800	-0.051811	4.815448

250.856496	7996.280573	14.265805	-0.051824	4.814514
250.683392	7990.665976	14.270810	-0.051788	4.812872
250.618322	7983.945692	14.275815	-0.051772	4.810906
250.431859	7976.676114	14.280819	-0.051732	4.808779
250.281131	7969.024596	14.285824	-0.051699	4.806538
250.387002	7961.242163	14.290829	-0.051714	4.804257
250.218009	7953.367677	14.295834	-0.051677	4.801950
250.200351	7945.399279	14.300839	-0.051669	4.799612
250.294272	7937.468330	14.305843	-0.051681	4.797285
250.190813	7929.433085	14.310848	-0.051657	4.794926
250.088866	7921.369986	14.315853	-0.051632	4.792558
250.105692	7913.392255	14.320858	-0.051630	4.790213
250.177240	7905.408582	14.325863	-0.051639	4.787866
250.053588	7897.416569	14.330867	-0.051610	4.785515
250.053938	7889.400528	14.335872	-0.051605	4.783156
250.114723	7881.415758	14.340877	-0.051611	4.780804
249.981314	7873.427045	14.345882	-0.051581	4.778451
249.716570	7865.386615	14.350887	-0.051527	4.776082
249.913834	7857.420759	14.355891	-0.051558	4.773732
249.747837	7849.296559	14.360896	-0.051522	4.771336
249.840617	7841.407049	14.365901	-0.051534	4.769007
249.679328	7833.359742	14.370906	-0.051499	4.766630
249.655222	7825.377319	14.375911	-0.051489	4.764272
249.581749	7817.442624	14.380915	-0.051470	4.761926
249.553418	7809.349896	14.385920	-0.051460	4.759533
249.342910	7801.442690	14.390925	-0.051415	4.757193
249.413934	7793.324417	14.395930	-0.051423	4.754789
249.318908	7785.334831	14.400935	-0.051400	4.752423
249.300934	7777.292186	14.405939	-0.051392	4.750039
249.370153	7769.322941	14.410944	-0.051400	4.747676
249.274837	7761.326465	14.415949	-0.051377	4.745304
249.298573	7753.327897	14.420954	-0.051376	4.742929
249.373313	7745.338051	14.425959	-0.051384	4.740556
249.283344	7737.348456	14.430963	-0.051363	4.738183
249.091214	7729.325169	14.435968	-0.051322	4.735798
249.220379	7721.324801	14.440973	-0.051340	4.733418
249.096608	7713.276763	14.445978	-0.051312	4.731024
248.882196	7705.294930	14.450983	-0.051267	4.728648
248.907692	7697.347630	14.455987	-0.051266	4.726280
248.899407	7689.283579	14.460992	-0.051260	4.723877
248.837193	7681.358214	14.465997	-0.051243	4.721514
248.750080	7673.285986	14.471002	-0.051221	4.719106
248.752109	7665.351447	14.476007	-0.051217	4.716738
248.874685	7657.354971	14.481011	-0.051234	4.714349
248.684269	7649.253528	14.486016	-0.051194	4.711929
248.867041	7641.311590	14.491021	-0.051222	4.709555
248.522125	7633.317526	14.496026	-0.051153	4.707164
248.534382	7625.260346	14.501031	-0.051150	4.704753
248.479633	7617.327760	14.506035	-0.051135	4.702378
248.330561	7609.300627	14.511040	-0.051102	4.699974
248.355499	7601.340259	14.516045	-0.051101	4.697588
248.465301	7593.303289	14.521050	-0.051116	4.695178
248.474267	7585.303077	14.526055	-0.051113	4.692778
248.369674	7577.262607	14.531059	-0.051088	4.690365
248.237150	7569.297872	14.536064	-0.051058	4.687973
248.209253	7561.305648	14.541069	-0.051048	4.685571
248.134937	7553.304831	14.546074	-0.051029	4.683166
248.035237	7545.288312	14.551079	-0.051005	4.680755
248.008063	7537.291894	14.556083	-0.050995	4.678349
247.794022	7529.286263	14.561088	-0.050950	4.675938
247.874281	7521.224059	14.566093	-0.050959	4.673509
247.862987	7513.136621	14.571098	-0.050952	4.671072
247.867331	7505.229430	14.576103	-0.050948	4.668687
247.968127	7497.242889	14.581107	-0.050961	4.666277
247.730896	7489.231215	14.586112	-0.050912	4.663859
247.780410	7481.270323	14.591117	-0.050916	4.661454
247.681119	7473.234511	14.596122	-0.050892	4.659026
247.556470	7465.250338	14.601127	-0.050864	4.656612
247.371870	7457.216524	14.606131	-0.050824	4.654182
247.377059	7449.217445	14.611136	-0.050820	4.651761
247.453806	7441.238191	14.616141	-0.050829	4.649345
247.340422	7433.261554	14.621146	-0.050802	4.646928
247.463709	7425.211422	14.626151	-0.050820	4.644487
247.479725	7417.285652	14.631155	-0.050818	4.642083
247.177641	7409.194693	14.636160	-0.050756	4.639628
247.133692	7401.267930	14.641165	-0.050743	4.637221
247.158383	7393.221096	14.646170	-0.050742	4.634777
247.109858	7385.179433	14.651175	-0.050728	4.632333
246.997907	7377.190205	14.656179	-0.050702	4.629903
247.018558	7369.189965	14.661184	-0.050701	4.627469
247.053982	7361.175493	14.666189	-0.050702	4.625029
246.912045	7353.243017	14.671194	-0.050671	4.622613
246.808505	7345.208254	14.676199	-0.050646	4.620164
246.943298	7337.239265	14.681203	-0.050666	4.617735
246.952983	7329.160862	14.686208	-0.050662	4.615270
247.015004	7321.174708	14.691213	-0.050669	4.612832
246.792882	7313.120306	14.696218	-0.050622	4.610373
246.720235	7305.159077	14.701223	-0.050603	4.607940
246.550754	7297.176640	14.706227	-0.050567	4.605499
246.430163	7289.148465	14.711232	-0.050539	4.603044
246.457637	7281.189726	14.716237	-0.050539	4.600608
246.416489	7273.181271	14.721242	-0.050526	4.598156
246.386794	7265.186263	14.726247	-0.050515	4.595706
246.708603	7257.161330	14.731251	-0.050570	4.593246
246.253461	7249.095264	14.736256	-0.050480	4.590772
246.257258	7241.127347	14.741261	-0.050476	4.588327
246.390138	7233.120692	14.746266	-0.050495	4.585869
246.275520	7225.130083	14.751271	-0.050469	4.583414
246.201068	7217.168070	14.756275	-0.050449	4.580966
246.115619	7209.144413	14.761280	-0.050428	4.578499
246.060496	7201.183861	14.766285	-0.050413	4.576049
245.783299	7193.131006	14.771290	-0.050356	4.573570
245.587282	7185.095525	14.776295	-0.050314	4.571094
245.809527	7177.125733	14.781299	-0.050350	4.568638
245.664785	7169.119056	14.786304	-0.050318	4.566169
245.471445	7161.127088	14.791309	-0.050277	4.563703
245.481085	7153.158882	14.796314	-0.050274	4.561243
245.659801	7145.140670	14.801319	-0.050302	4.558767
245.764357	7137.187696	14.806323	-0.050316	4.556309
245.633481	7129.141196	14.811328	-0.050286	4.553821
245.579850	7121.113898	14.816333	-0.050271	4.551337
245.336158	7113.099061	14.821338	-0.050221	4.548856
245.301473	7105.107724	14.826343	-0.050209	4.546381
245.533884	7097.130342	14.831347	-0.050247	4.543909
245.349920	7089.161647	14.836352	-0.050208	4.541438
245.257881	7081.149532	14.841357	-0.050185	4.538952
245.236922	7073.188671	14.846362	-0.050176	4.536481
245.417203	7065.105257	14.851367	-0.050204	4.533971
245.298647	7057.116612	14.856371	-0.050177	4.531489
245.170079	7049.062195	14.861376	-0.050148	4.528984
245.334877	7041.120615	14.866381	-0.050173	4.526514
245.057168	7033.094226	14.871386	-0.050116	4.524015
244.839808	7025.146109	14.876391	-0.050071	4.521539
245.060787	7017.103973	14.881395	-0.050107	4.519034
244.971471	7009.144704	14.886400	-0.050085	4.516552
244.920578	7001.098499	14.891405	-0.050070	4.514042
244.802406	6993.030344	14.896410	-0.050043	4.511524
244.936805	6985.001627	14.901415	-0.050063	4.509017
244.891113	6977.078751	14.906419	-0.050049	4.506541
244.502279	6969.042446	14.911424	-0.049971	4.504027
244.714656	6961.100224	14.916429	-0.050006	4.501544
244.831650	6953.066448	14.921434	-0.050022	4.499029
244.575924	6945.099390	14.926439	-0.049969	4.496534
244.642251	6937.087990	14.931443	-0.049977	4.494024
244.577649	6929.036520	14.936448	-0.049959	4.491499
244.557756	6921.003100	14.941453	-0.049950	4.488979
244.556106	6913.064514	14.946458	-0.049945	4.486487
244.483134	6905.008835	14.951463	-0.049926	4.483957
244.351633	6897.111317	14.956467	-0.049896	4.481475
244.106552	6889.021890	14.961472	-0.049846	4.478931
244.257392	6881.108486	14.966477	-0.049868	4.476442
244.229218	6873.083405	14.971482	-0.049858	4.473916
244.013677	6865.027318	14.976487	-0.049813	4.471379
244.133927	6857.036446	14.981491	-0.049830	4.468861
244.121151	6849.050593	14.986496	-0.049822	4.466343
244.228425	6841.047062	14.991501	-0.049837	4.463819
244.144322	6833.073064	14.996506	-0.049816	4.461301
244.041691	6825.040586	15.001511	-0.049792	4.458764
244.172911	6817.044401	15.006515	-0.049811	4.456238
244.067315	6808.983627	15.011520	-0.049786	4.453689
243.963852	6801.009374	15.016525	-0.049762	4.451165
243.918993	6793.028086	15.021530	-0.049748	4.448639
243.773013	6785.000461	15.026535	-0.049716	4.446096
243.536726	6777.078172	15.031539	-0.049666	4.443584
243.589740	6769.015789	15.036544	-0.049671	4.441028
243.417221	6761.018192	15.041549	-0.049634	4.438489
243.411171	6753.064218	15.046554	-0.049627	4.435964
243.495428	6744.982823	15.051559	-0.049638	4.433398
243.255502	6736.954917	15.056563	-0.049588	4.430845
242.996122	6728.976189	15.061568	-0.049534	4.428307
243.266385	6720.977679	15.066573	-0.049580	4.425763
243.402165	6713.003319	15.071578	-0.049600	4.423225
243.060450	6704.977996	15.076583	-0.049531	4.420667
243.046007	6697.004354	15.081587	-0.049523	4.418125
243.045356	6688.945067	15.086592	-0.049517	4.415555
243.037696	6680.957099	15.091597	-0.049511	4.413005
242.740695	6672.955869	15.096602	-0.049450	4.410449
242.898422	6664.991173	15.101607	-0.049475	4.407905
242.992501	6657.007648	15.106611	-0.049487	4.405354
242.893079	6648.979210	15.111616	-0.049463	4.402785
242.756663	6641.018533	15.116621	-0.049432	4.400237
242.694795	6633.001823	15.121626	-0.049416	4.397669
242.594470	6624.999248	15.126631	-0.049392	4.395105
242.703975	6617.009460	15.131635	-0.049407	4.392544
242.626086	6608.929295	15.136640	-0.049387	4.389951
242.594874	6601.031061	15.141645	-0.049376	4.387416
242.388937	6592.992812	15.146650	-0.049333	4.384833
242.310917	6585.017302	15.151655	-0.049313	4.382269
242.569100	6576.974376	15.156659	-0.049356	4.379685
242.212513	6569.028895	15.161664	-0.049284	4.377126
242.389803	6561.006546	15.166669	-0.049312	4.374545
242.553677	6552.999779	15.171674	-0.049337	4.371966
242.342471	6544.939915	15.176679	-0.049293	4.369367
242.119933	6537.004191	15.181683	-0.049246	4.366807
242.206946	6528.981146	15.186688	-0.049257	4.364218
242.150375	6521.022672	15.191693	-0.049241	4.361648
241.920222	6513.009554	15.196698	-0.049193	4.359058
241.839856	6505.045620	15.201703	-0.049173	4.356483
242.040369	6496.982360	15.206707	-0.049205	4.353876
241.726742	6488.911166	15.211712	-0.049142	4.351262
241.571110	6480.879300	15.216717	-0.049107	4.348659
241.691187	6472.930393	15.221722	-0.049124	4.346084
241.573703	6464.927595	15.226727	-0.049097	4.343489
241.572717	6456.971429	15.231731	-0.049092	4.340908
241.557903	6448.961651	15.236736	-0.049084	4.338307
241.638631	6440.982501	15.241741	-0.049094	4.335716
241.572550	6432.971909	15.246746	-0.049076	4.333112
241.498525	6424.932751	15.251751	-0.049057	4.330497
241.575182	6416.926812	15.256755	-0.049066	4.327892
241.269890	6408.921713	15.261760	-0.049004	4.325283
241.256155	6400.992620	15.266765	-0.048997	4.322700
241.316229	6393.001507	15.271770	-0.049003	4.320095
241.335794	6384.959672	15.276775	-0.049001	4.317472
241.115710	6376.958844	15.281779	-0.048955	4.314859
241.026731	6368.903532	15.286784	-0.048933	4.312228
241.059732	6360.907626	15.291789	-0.048934	4.309615
241.241208	6352.954098	15.296794	-0.048962	4.307015
240.809910	6344.916879	15.301799	-0.048877	4.304382
240.896452	6336.960985	15.306803	-0.048888	4.301778
240.833403	6328.929662	15.311808	-0.048871	4.299147
240.891268	6320.970798	15.316813	-0.048876	4.296538
240.713091	6312.965463	15.321818	-0.048838	4.293911
240.652692	6304.903228	15.326823	-0.048822	4.291265
240.681160	6296.915058	15.331827	-0.048822	4.288641
240.655848	6288.917928	15.336832	-0.048812	4.286013
240.589528	6280.922965	15.341837	-0.048794	4.283384
240.468681	6272.930545	15.346842	-0.048766	4.280753
240.534966	6264.908886	15.351847	-0.048774	4.278113
240.552506	6256.981538	15.356851	-0.048772	4.275502
240.216325	6248.916781	15.361856	-0.048704	4.272841
240.133940	6240.863757	15.366861	-0.048683	4.270184
240.296889	6232.911411	15.371866	-0.048708	4.267561
240.309244	6224.833718	15.376871	-0.048705	4.264893
240.359397	6216.937630	15.381875	-0.048710	4.262285
239.999603	6208.875299	15.386880	-0.048637	4.259616
240.077423	6200.956216	15.391885	-0.048647	4.256996
240.102769	6192.886932	15.396890	-0.048646	4.254325
239.927270	6184.887629	15.401895	-0.048608	4.251673
240.046614	6176.908713	15.406899	-0.048625	4.249030
240.023453	6168.948133	15.411904	-0.048616	4.246389
239.857030	6160.900653	15.416909	-0.048580	4.243717
239.948509	6152.963751	15.421914	-0.048591	4.241082
239.823016	6144.921509	15.426919	-0.048563	4.238408
239.769526	6136.988386	15.431923	-0.048548	4.235770
239.825403	6128.886340	15.436928	-0.048553	4.233074
239.770042	6120.911743	15.441933	-0.048537	4.230419
239.471438	6112.926857	15.446938	-0.048476	4.227756
239.610863	6104.869557	15.451943	-0.048497	4.225071
239.593747	6096.925852	15.456947	-0.048489	4.222421
239.441423	6088.944453	15.461952	-0.048455	4.219756
239.384371	6080.958748	15.466957	-0.048439	4.217088
239.385832	6072.947400	15.471962	-0.048434	4.214411
239.293585	6064.919751	15.476967	-0.048412	4.211725
239.218888	6056.900458	15.481971	-0.048393	4.209041
238.898807	6048.951709	15.486976	-0.048328	4.206376
239.211822	6040.939033	15.491981	-0.048381	4.203694
239.085377	6032.973990	15.496986	-0.048352	4.201022
238.888415	6024.931643	15.501991	-0.048311	4.198322
238.965986	6016.956497	15.506995	-0.048320	4.195646
239.156856	6008.863874	15.512000	-0.048350	4.192929
239.180299	6000.792020	15.517005	-0.048349	4.190216
239.210498	5992.893120	15.522010	-0.048350	4.187560
238.930788	5984.854449	15.527015	-0.048292	4.184851
239.114343	5976.906030	15.532019	-0.048321	4.182176
238.685943	5968.893864	15.537024	-0.048236	4.179471
238.807344	5960.926247	15.542029	-0.048254	4.176786
238.769119	5952.935731	15.547034	-0.048241	4.174089
238.569743	5944.916980	15.552039	-0.048199	4.171379
238.511036	5936.895096	15.557043	-0.048183	4.168668
238.605661	5928.935114	15.562048	-0.048195	4.165978
238.399693	5920.950817	15.567053	-0.048152	4.163274
238.229959	5912.913401	15.572058	-0.048115	4.160551
238.012693	5904.923499	15.577063	-0.048069	4.157842
238.202671	5896.913739	15.582067	-0.048099	4.155129
237.901053	5888.854508	15.587072	-0.048038	4.152391
238.100072	5880.829150	15.592077	-0.048070	4.149670
238.246914	5872.905465	15.597082	-0.048092	4.146980
237.908217	5864.856231	15.602087	-0.048024	4.144240
238.080735	5856.924561	15.607091	-0.048051	4.141545
237.856452	5848.926002	15.612096	-0.048004	4.138820
237.742545	5840.896760	15.617101	-0.047977	4.136084
237.630331	5832.900299	15.622106	-0.047951	4.133357
237.590919	5824.867163	15.627111	-0.047939	4.130618
237.628194	5816.907914	15.632115	-0.047940	4.127902
237.607113	5808.861899	15.637120	-0.047931	4.125154
237.592916	5800.907779	15.642125	-0.047923	4.122436
237.530587	5792.910504	15.647130	-0.047906	4.119701
237.277056	5784.952170	15.652135	-0.047854	4.116975
237.334361	5776.943790	15.657139	-0.047859	4.114234
237.223287	5768.876033	15.662144	-0.047834	4.111468
237.318238	5760.867842	15.667149	-0.047846	4.108724
237.143573	5752.869795	15.672154	-0.047808	4.105978
237.095945	5744.878673	15.677159	-0.047794	4.103234
237.132960	5736.918734	15.682163	-0.047796	4.100500
236.972205	5728.920911	15.687168	-0.047761	4.097749
237.020649	5720.906783	15.692173	-0.047765	4.094993
237.112303	5712.927176	15.697178	-0.047776	4.092247
236.945586	5704.888750	15.702183	-0.047740	4.089476
236.882388	5696.945022	15.707187	-0.047723	4.086737
236.784218	5688.925700	15.712192	-0.047700	4.083970
236.798957	5680.967942	15.717197	-0.047697	4.081223
236.925234	5672.976734	15.722202	-0.047716	4.078465
236.869858	5664.961179	15.727207	-0.047700	4.075694
236.734576	5656.946218	15.732211	-0.047670	4.072920
236.658102	5648.895614	15.737216	-0.047650	4.070133
236.517707	5640.889221	15.742221	-0.047619	4.067358
236.395302	5632.945253	15.747226	-0.047591	4.064603
236.278094	5624.953419	15.752231	-0.047564	4.061830
236.452447	5616.954121	15.757235	-0.047591	4.059056
236.465547	5608.948064	15.762240	-0.047588	4.056276
236.274270	5600.950657	15.767245	-0.047547	4.053494
236.146160	5592.914891	15.772250	-0.047518	4.050698
236.132504	5584.918467	15.777255	-0.047511	4.047915
236.236623	5576.940486	15.782259	-0.047525	4.045138
235.967646	5568.964135	15.787264	-0.047469	4.042354
235.914180	5560.964487	15.792269	-0.047454	4.039564
236.294213	5552.966075	15.797274	-0.047520	4.036779
236.163924	5544.909267	15.802279	-0.047490	4.033963
235.941507	5536.841599	15.807283	-0.047444	4.031141
235.847920	5528.874920	15.812288	-0.047421	4.028353
235.905948	5520.869709	15.817293	-0.047427	4.025553
235.975046	5512.927495	15.822298	-0.047434	4.022773
235.588877	5504.930691	15.827303	-0.047357	4.019964
235.712192	5496.925065	15.832307	-0.047375	4.017159
235.712421	5488.913571	15.837312	-0.047370	4.014348
235.639938	5480.905615	15.842317	-0.047351	4.011534
235.489082	5472.923709	15.847322	-0.047318	4.008727
235.454700	5464.905823	15.852327	-0.047306	4.005907
235.428945	5456.930463	15.857331	-0.047296	4.003100
235.238432	5448.916809	15.862336	-0.047255	4.000275
235.101085	5440.945440	15.867341	-0.047225	3.997463
235.213400	5432.931119	15.872346	-0.047240	3.994639
235.316098	5424.880422	15.877351	-0.047254	3.991800
235.364116	5416.883016	15.882355	-0.047258	3.988976
235.184836	5408.900938	15.887360	-0.047219	3.986152
234.913924	5400.923579	15.892365	-0.047164	3.983326
235.058675	5392.968683	15.897370	-0.047185	3.980513
234.937570	5384.982515	15.902375	-0.047158	3.977683
234.934449	5376.955130	15.907379	-0.047152	3.974838
234.809701	5368.909351	15.912384	-0.047123	3.971982
234.872125	5360.875453	15.917389	-0.047130	3.969132
235.097241	5352.923880	15.922394	-0.047166	3.966311
234.909276	5344.893220	15.927399	-0.047126	3.963454
234.868002	5336.995611	15.932403	-0.047113	3.960644
234.798616	5329.023449	15.937408	-0.047095	3.957805
234.775114	5321.003121	15.942413	-0.047086	3.954948
234.654653	5313.012597	15.947418	-0.047058	3.952098
234.513415	5304.947550	15.952423	-0.047027	3.949218
234.651082	5297.003251	15.957427	-0.047047	3.946385
234.496564	5288.989922	15.962432	-0.047013	3.943519
234.442722	5280.985356	15.967437	-0.046998	3.940657
234.471249	5273.010454	15.972442	-0.046998	3.937804
234.355754	5264.985756	15.977447	-0.046971	3.934929
234.463660	5257.003686	15.982451	-0.046986	3.932071
234.410029	5248.953690	15.987456	-0.046971	3.929184
234.064547	5241.016585	15.992461	-0.046901	3.926330
234.360641	5233.003323	15.997466	-0.046951	3.923458
234.210145	5224.978595	16.002471	-0.046918	3.920572
234.102601	5217.040099	16.007475	-0.046893	3.917715
233.854977	5209.003626	16.012480	-0.046841	3.914818
233.882124	5200.951266	16.017485	-0.046841	3.911919
234.092390	5192.975939	16.022490	-0.046875	3.909049
233.959421	5184.980928	16.027495	-0.046845	3.906163
234.005325	5177.018892	16.032499	-0.046848	3.903290
233.893392	5169.001832	16.037504	-0.046822	3.900392
233.675499	5161.026561	16.042509	-0.046777	3.897505
233.649374	5153.022183	16.047514	-0.046767	3.894609
233.730320	5144.973288	16.052519	-0.046776	3.891697
233.501394	5137.006267	16.057523	-0.046729	3.888806
233.508484	5128.995695	16.062528	-0.046725	3.885902
233.574866	5121.013753	16.067533	-0.046732	3.883007
233.382521	5113.006919	16.072538	-0.046691	3.880096
233.314712	5105.018377	16.077543	-0.046673	3.877192
233.348676	5097.024351	16.082547	-0.046674	3.874286
233.271367	5088.748202	16.087552	-0.046654	3.871273
233.224757	5080.833338	16.092557	-0.046640	3.868389
233.276973	5072.886468	16.097562	-0.046645	3.865494
233.198426	5064.949278	16.102567	-0.046625	3.862597
233.241590	5056.954108	16.107571	-0.046628	3.859680
233.075605	5049.020934	16.112576	-0.046592	3.856779
233.105877	5041.011233	16.117581	-0.046592	3.853851
233.052543	5033.011404	16.122586	-0.046577	3.850923
232.936775	5024.997302	16.127591	-0.046550	3.847987
232.973132	5017.008119	16.132595	-0.046552	3.845060
232.749775	5009.037036	16.137600	-0.046505	3.842133
232.616568	5001.057698	16.142605	-0.046475	3.839202
232.616072	4993.081265	16.147610	-0.046470	3.836272
232.519827	4985.043337	16.152615	-0.046447	3.833316
232.609911	4977.048568	16.157619	-0.046458	3.830377
232.650657	4969.025417	16.162624	-0.046461	3.827425
232.527395	4961.011912	16.167629	-0.046432	3.824470
232.566417	4953.069822	16.172634	-0.046435	3.821543
232.287885	4945.098836	16.177639	-0.046377	3.818596
232.307484	4937.084758	16.182643	-0.046376	3.815637
232.361262	4929.088422	16.187648	-0.046381	3.812684
232.104755	4921.067399	16.192653	-0.046328	3.809712
232.135407	4913.076441	16.197658	-0.046328	3.806755
232.308438	4905.065640	16.202663	-0.046355	3.803792
232.262083	4897.130331	16.207667	-0.046341	3.800849
231.863326	4889.137031	16.212672	-0.046262	3.797875
231.847342	4881.094718	16.217677	-0.046254	3.794889
231.922169	4873.049993	16.222682	-0.046262	3.791901
231.926652	4865.028365	16.227687	-0.046258	3.788919
231.814335	4857.083776	16.232691	-0.046232	3.785960
231.934510	4849.092121	16.237696	-0.046249	3.782986
231.873845	4841.083261	16.242701	-0.046233	3.779999
231.882743	4833.125087	16.247706	-0.046229	3.777031
231.639935	4825.097302	16.252711	-0.046179	3.774029
231.811541	4817.096770	16.257715	-0.046205	3.771043
231.674680	4809.076245	16.262720	-0.046175	3.768041
231.525635	4801.063756	16.267725	-0.046142	3.765039
231.573868	4793.139786	16.272730	-0.046145	3.762073
231.531117	4785.087770	16.277735	-0.046132	3.759054
231.247251	4777.166122	16.282739	-0.046074	3.756076
231.196524	4769.102608	16.287744	-0.046060	3.753047
231.112378	4761.095884	16.292749	-0.046039	3.750037
231.155369	4753.112606	16.297754	-0.046041	3.747036
231.063147	4745.100213	16.302759	-0.046019	3.744019
231.158685	4737.133924	16.307763	-0.046032	3.741021
231.204430	4729.127442	16.312768	-0.046035	3.738004
231.037752	4721.115168	16.317773	-0.045999	3.734978
230.972131	4713.145228	16.322778	-0.045981	3.731967
230.971364	4705.126429	16.327783	-0.045976	3.728937
230.869209	4697.152796	16.332787	-0.045952	3.725919
230.693265	4689.153280	16.337792	-0.045914	3.722888
230.863355	4681.174448	16.342797	-0.045940	3.719870
230.764986	4673.226682	16.347802	-0.045917	3.716854
230.678045	4665.172810	16.352807	-0.045895	3.713797
230.779701	4657.097807	16.357811	-0.045909	3.710733
230.610072	4649.112721	16.362816	-0.045872	3.707694
230.459898	4641.108381	16.367821	-0.045839	3.704646
230.456783	4633.214248	16.372826	-0.045833	3.701642
230.434565	4625.171319	16.377831	-0.045824	3.698577
230.361927	4617.222685	16.382835	-0.045805	3.695545
230.369441	4609.218091	16.387840	-0.045801	3.692490
230.130982	4601.197951	16.392845	-0.045752	3.689421
230.138833	4593.239324	16.397850	-0.045748	3.686380
230.101672	4585.207047	16.402855	-0.045736	3.683306
230.019664	4577.248061	16.407859	-0.045715	3.680257
229.992731	4569.272489	16.412864	-0.045705	3.677200
229.876758	4561.234666	16.417869	-0.045678	3.674115
230.037155	4553.225743	16.422874	-0.045703	3.671045
230.080356	4545.182606	16.427879	-0.045706	3.667956
229.994928	4537.205245	16.432883	-0.045685	3.664887
229.894316	4529.269701	16.437888	-0.045661	3.661831
229.851474	4521.243719	16.442893	-0.045647	3.658739
229.631380	4513.290869	16.447898	-0.045601	3.655668
229.564067	4505.250236	16.452903	-0.045584	3.652564
229.587178	4497.220786	16.457907	-0.045583	3.649464
229.581629	4489.250999	16.462912	-0.045576	3.646385
229.306797	4481.248412	16.467917	-0.045520	3.643282
229.311224	4473.287489	16.472922	-0.045516	3.640201
229.272168	4465.302493	16.477927	-0.045503	3.637106
229.156593	4457.293415	16.482931	-0.045476	3.633998
229.360759	4449.256907	16.487936	-0.045509	3.630884
229.322811	4441.254568	16.492941	-0.045497	3.627775
229.012911	4433.263716	16.497946	-0.045434	3.624660
228.888436	4425.319787	16.502951	-0.045406	3.621566
229.127788	4417.320213	16.507955	-0.045445	3.618458
229.024257	4409.342827	16.512960	-0.045421	3.615346
228.610700	4401.334323	16.517965	-0.045338	3.612210
228.793011	4393.299433	16.522970	-0.045367	3.609078
228.711869	4385.310170	16.527975	-0.045347	3.605954
228.604572	4377.360859	16.532979	-0.045322	3.602842
228.583085	4369.378842	16.537984	-0.045312	3.599717
228.744419	4361.371529	16.542989	-0.045337	3.596584
228.902786	4353.373728	16.547994	-0.045361	3.593453
228.574914	4345.367840	16.552999	-0.045295	3.590301
228.719304	4337.373879	16.558003	-0.045317	3.587165
228.584230	4329.381731	16.563008	-0.045286	3.584019
228.436282	4321.415051	16.568013	-0.045254	3.580880
228.589480	4313.427119	16.573018	-0.045277	3.577738
228.444122	4305.401483	16.578023	-0.045245	3.574570
228.357991	4297.422981	16.583027	-0.045223	3.571420
228.223289	4289.421946	16.588032	-0.045193	3.568256
228.141845	4281.391776	16.593037	-0.045173	3.565080
228.097277	4273.469414	16.598042	-0.045159	3.561945
227.854522	4265.448948	16.603047	-0.045109	3.558762
228.004880	4257.449080	16.608051	-0.045132	3.555596
228.120732	4249.352639	16.613056	-0.045148	3.552388
227.933050	4241.330943	16.618061	-0.045108	3.549197
227.791660	4233.376691	16.623066	-0.045076	3.546032
227.668138	4225.400024	16.628071	-0.045048	3.542856
227.636873	4217.434601	16.633075	-0.045037	3.539684
227.435471	4209.493094	16.638080	-0.044994	3.536513
227.460383	4201.457957	16.643085	-0.044994	3.533310
227.483738	4193.441164	16.648090	-0.044993	3.530110
227.334614	4185.436161	16.653095	-0.044960	3.526907
227.354952	4177.450552	16.658099	-0.044958	3.523715
227.403626	4169.505094	16.663104	-0.044962	3.520536
227.199362	4161.535550	16.668109	-0.044919	3.517337
227.331681	4153.517145	16.673114	-0.044939	3.514125
227.453297	4145.465633	16.678119	-0.044956	3.510897
227.134700	4137.504403	16.683123	-0.044891	3.507689
227.018219	4129.484518	16.688128	-0.044865	3.504461
227.082360	4121.513890	16.693133	-0.044871	3.501255
227.139112	4113.551113	16.698138	-0.044877	3.498049
226.927745	4105.552291	16.703143	-0.044832	3.494817
226.893632	4097.554844	16.708147	-0.044821	3.491588
226.943725	4089.555898	16.713152	-0.044825	3.488358
226.527052	4081.569374	16.718157	-0.044742	3.485116
226.778852	4073.598741	16.723162	-0.044784	3.481898
226.718329	4065.609183	16.728167	-0.044767	3.478660
226.770199	4057.626669	16.733171	-0.044771	3.475425
226.782940	4049.580860	16.738176	-0.044769	3.472160
226.553774	4041.570307	16.743181	-0.044721	3.468898
226.638653	4033.595315	16.748186	-0.044731	3.465658
226.470780	4025.602710	16.753191	-0.044695	3.462400
226.486452	4017.595348	16.758195	-0.044693	3.459138
226.302239	4009.660564	16.763200	-0.044653	3.455896
226.199299	4001.626618	16.768205	-0.044629	3.452614
226.099226	3993.626867	16.773210	-0.044605	3.449342
225.929379	3985.651847	16.778215	-0.044568	3.446076
226.023653	3977.650097	16.783219	-0.044580	3.442803
226.126230	3969.663619	16.788224	-0.044594	3.439535
225.881309	3961.685608	16.793229	-0.044543	3.436255
226.033626	3953.679854	16.798234	-0.044567	3.432974
225.948621	3945.619092	16.803239	-0.044545	3.429659
225.886734	3937.690219	16.808243	-0.044529	3.426395
225.858102	3929.683577	16.813248	-0.044518	3.423098
225.686751	3921.719149	16.818253	-0.044481	3.419811
225.627476	3913.762283	16.823258	-0.044465	3.416526
225.501538	3905.727170	16.828263	-0.044436	3.413205
225.598689	3897.704075	16.833267	-0.044449	3.409892
225.540325	3889.734111	16.838272	-0.044433	3.406593
225.407519	3881.760022	16.843277	-0.044403	3.403287
225.606907	3873.786307	16.848282	-0.044435	3.399989
225.384813	3865.828479	16.853287	-0.044388	3.396679
225.424318	3857.785915	16.858291	-0.044391	3.393341
225.352718	3849.712564	16.863296	-0.044372	3.389982
225.402744	3841.732978	16.868301	-0.044376	3.386663
225.401166	3833.766308	16.873306	-0.044371	3.383345
225.243623	3825.793734	16.878311	-0.044336	3.380015
225.248961	3817.834699	16.883315	-0.044332	3.376694
224.915392	3809.847366	16.888320	-0.044265	3.373345
224.830047	3801.808889	16.893325	-0.044243	3.369981
224.935155	3793.847923	16.898330	-0.044258	3.366652
224.803471	3785.830185	16.903335	-0.044228	3.363288
224.714474	3777.877131	16.908339	-0.044206	3.359949
224.826301	3769.897643	16.913344	-0.044222	3.356602
224.749720	3761.862877	16.918349	-0.044202	3.353223
224.553834	3753.887366	16.923354	-0.044161	3.349860
224.597959	3745.864328	16.928359	-0.044164	3.346483
224.836381	3737.868764	16.933363	-0.044203	3.343122
224.579716	3729.922763	16.938368	-0.044150	3.339759
224.392853	3721.958852	16.943373	-0.044110	3.336388
224.521800	3713.938563	16.948378	-0.044129	3.333002
224.414428	3705.898425	16.953383	-0.044104	3.329595
224.289385	3697.952083	16.958387	-0.044075	3.326223
224.220584	3689.969916	16.963392	-0.044057	3.322835
224.211753	3681.986961	16.968397	-0.044050	3.319446
224.130055	3674.044309	16.973402	-0.044030	3.316067
224.130736	3666.001276	16.978407	-0.044025	3.312646
224.092922	3657.975837	16.983411	-0.044012	3.309226
224.062691	3649.991711	16.988416	-0.044002	3.305822
223.834831	3642.019563	16.993421	-0.043954	3.302411
223.895238	3634.030727	16.998426	-0.043960	3.299000
223.952333	3626.044587	17.003431	-0.043965	3.295587
223.879736	3618.061574	17.008435	-0.043947	3.292167
223.926349	3610.039035	17.013440	-0.043950	3.288731
223.910892	3602.033367	17.018445	-0.043942	3.285296
223.818479	3594.105528	17.023450	-0.043920	3.281888
223.610873	3586.125266	17.028455	-0.043876	3.278450
223.689248	3578.152184	17.033459	-0.043885	3.275022
223.737104	3570.103992	17.038464	-0.043889	3.271557
223.571155	3562.100435	17.043469	-0.043853	3.268099
223.338530	3554.142602	17.048474	-0.043804	3.264654
223.176650	3546.166593	17.053479	-0.043769	3.261201
223.137324	3538.169121	17.058483	-0.043756	3.257740
223.196539	3530.176160	17.063488	-0.043762	3.254280
223.186078	3522.142669	17.068493	-0.043755	3.250797
223.115151	3514.176581	17.073498	-0.043737	3.247337
223.042508	3506.176807	17.078503	-0.043718	3.243858
223.111215	3498.219186	17.083507	-0.043725	3.240400
223.027012	3490.251264	17.088512	-0.043705	3.236928
222.945989	3482.227927	17.093517	-0.043684	3.233427
223.009825	3474.194807	17.098522	-0.043691	3.229925
222.720213	3466.193402	17.103527	-0.043632	3.226418
222.740955	3458.204603	17.108531	-0.043630	3.222925
222.809940	3450.234899	17.113536	-0.043638	3.219439
222.745024	3442.272858	17.118541	-0.043621	3.215947
222.609122	3434.292762	17.123546	-0.043590	3.212441
222.515539	3426.272695	17.128551	-0.043568	3.208914
222.534105	3418.299140	17.133555	-0.043566	3.205409
222.576147	3410.347672	17.138560	-0.043569	3.201911
222.395709	3402.344576	17.143565	-0.043530	3.198377
222.529735	3394.370000	17.148570	-0.043549	3.194865
222.279339	3386.354597	17.153575	-0.043498	3.191314
222.194192	3378.364206	17.158579	-0.043477	3.187778
222.093700	3370.387016	17.163584	-0.043453	3.184243
222.182710	3362.392104	17.168589	-0.043464	3.180704
222.107418	3354.423253	17.173594	-0.043445	3.177166
222.205434	3346.392520	17.178599	-0.043458	3.173604
222.126944	3338.394115	17.183603	-0.043438	3.170044
222.085877	3330.452291	17.188608	-0.043425	3.166508
221.939600	3322.449732	17.193613	-0.043393	3.162936
222.102837	3314.475192	17.198618	-0.043418	3.159385
221.880965	3306.528847	17.203623	-0.043371	3.155827
221.517002	3298.504939	17.208627	-0.043298	3.152223
221.500384	3290.494098	17.213632	-0.043290	3.148637
221.704059	3282.455514	17.218637	-0.043323	3.145043
221.740380	3274.521717	17.223642	-0.043324	3.141486
221.399933	3266.545694	17.228647	-0.043256	3.137888
221.385628	3258.555204	17.233651	-0.043248	3.134294
221.448662	3250.548930	17.238656	-0.043254	3.130693
221.403133	3242.564649	17.243661	-0.043241	3.127092
221.354549	3234.599573	17.248666	-0.043227	3.123496
221.257713	3226.625693	17.253671	-0.043203	3.119889
221.201209	3218.655695	17.258675	-0.043188	3.116282
221.147053	3210.673359	17.263680	-0.043172	3.112665
220.862604	3202.648986	17.268685	-0.043114	3.109015
220.894227	3194.672693	17.273690	-0.043115	3.105396
220.898019	3186.698861	17.278695	-0.043110	3.101773
220.866863	3178.702189	17.283699	-0.043099	3.098134
220.917103	3170.713595	17.288704	-0.043103	3.094498
220.711693	3162.719762	17.293709	-0.043060	3.090843
220.665121	3154.741322	17.298714	-0.043046	3.087198
220.703793	3146.764387	17.303719	-0.043048	3.083554
220.752928	3138.777397	17.308723	-0.043052	3.079901
220.675167	3130.825004	17.313728	-0.043032	3.076254
220.515842	3122.755704	17.318733	-0.042997	3.072545
220.636142	3114.735663	17.323738	-0.043015	3.068867
220.423366	3106.780231	17.328743	-0.042970	3.065199
220.370316	3098.811310	17.333747	-0.042955	3.061528
220.604105	3090.829339	17.338752	-0.042993	3.057860
220.449034	3082.839300	17.343757	-0.042959	3.054166
220.169344	3074.896146	17.348762	-0.042902	3.050482
220.303480	3066.864083	17.353767	-0.042921	3.046773
220.369957	3058.895880	17.358771	-0.042929	3.043086
220.315848	3050.930269	17.363776	-0.042913	3.039389
220.141339	3042.984845	17.368781	-0.042876	3.035692
220.023849	3034.994945	17.373786	-0.042849	3.031972
219.887345	3026.984714	17.378791	-0.042818	3.028237
219.873265	3018.978368	17.383795	-0.042810	3.024505
219.822908	3011.037193	17.388800	-0.042796	3.020798
219.700188	3003.063276	17.393805	-0.042768	3.017067
219.628999	2995.078544	17.398810	-0.042749	3.013328
219.701226	2987.032067	17.403815	-0.042757	3.009563
219.674313	2979.050636	17.408819	-0.042747	3.005820
219.691292	2971.089158	17.413824	-0.042745	3.002082
219.419401	2963.118314	17.418829	-0.042689	2.998322
219.589891	2955.137323	17.423834	-0.042716	2.994574
219.340799	2947.138547	17.428839	-0.042664	2.990792
219.167279	2939.153896	17.433843	-0.042627	2.987016
219.307791	2931.159896	17.438848	-0.042648	2.983246
219.090486	2923.185043	17.443853	-0.042602	2.979462
219.110755	2915.245131	17.448858	-0.042601	2.975702
219.219320	2907.209753	17.453863	-0.042615	2.971897
219.118052	2899.218264	17.458867	-0.042591	2.968097
219.059883	2891.256060	17.463872	-0.042575	2.964308
218.974338	2883.286041	17.468877	-0.042554	2.960509
218.973408	2875.328964	17.473882	-0.042549	2.956716
218.880565	2867.318156	17.478887	-0.042526	2.952888
218.743448	2859.325839	17.483891	-0.042496	2.949061
218.889218	2851.353098	17.488896	-0.042518	2.945253
218.740109	2843.369849	17.493901	-0.042485	2.941419
218.749020	2835.411772	17.498906	-0.042481	2.937602
218.692799	2827.409436	17.503911	-0.042465	2.933754
218.835002	2819.377825	17.508915	-0.042487	2.929898
218.532511	2811.470724	17.513920	-0.042425	2.926073
218.432586	2803.492439	17.518925	-0.042401	2.922219
218.509810	2795.522746	17.523930	-0.042411	2.918374
218.369179	2787.520356	17.528935	-0.042379	2.914497
218.066140	2779.458943	17.533939	-0.042317	2.910577
218.100418	2771.483961	17.538944	-0.042319	2.906712
218.033259	2763.515351	17.543949	-0.042301	2.902839
217.932480	2755.571398	17.548954	-0.042277	2.898971
217.882494	2747.572876	17.553959	-0.042262	2.895074
218.052817	2739.576052	17.558963	-0.042289	2.891185
218.074868	2731.598719	17.563968	-0.042288	2.887291
217.846728	2723.631921	17.568973	-0.042240	2.883385
217.717409	2715.694336	17.573978	-0.042211	2.879492
217.542745	2707.744616	17.578983	-0.042173	2.875586
217.502814	2699.699176	17.583987	-0.042161	2.871635
217.491817	2691.732676	17.588992	-0.042153	2.867718
217.451491	2683.713804	17.593997	-0.042141	2.863769
217.442741	2675.760063	17.599002	-0.042134	2.859849
217.409136	2667.793487	17.604007	-0.042122	2.855915
217.533373	2659.760110	17.609011	-0.042140	2.851952
217.293015	2651.837074	17.614016	-0.042090	2.848017
217.009616	2643.856974	17.619021	-0.042032	2.844046
217.272427	2635.891543	17.624026	-0.042076	2.840108
217.205534	2627.936845	17.629031	-0.042058	2.836151
216.846124	2619.944484	17.634035	-0.041986	2.832152
217.018673	2611.917933	17.639040	-0.042013	2.828162
217.038309	2603.915717	17.644045	-0.042012	2.824169
216.942729	2595.987310	17.649050	-0.041989	2.820201
216.753886	2588.027825	17.654055	-0.041948	2.816207
216.725072	2580.024629	17.659059	-0.041938	2.812194
216.853534	2572.015398	17.664064	-0.041956	2.808181
216.597278	2564.053816	17.669069	-0.041904	2.804164
216.803003	2556.088253	17.674074	-0.041937	2.800166
216.591595	2548.138867	17.679079	-0.041892	2.796147
216.542493	2540.142059	17.684083	-0.041878	2.792107
216.399264	2532.174559	17.689088	-0.041846	2.788070
216.498310	2524.160326	17.694093	-0.041859	2.784019
216.495654	2516.194770	17.699098	-0.041853	2.779980
216.271541	2508.259856	17.704103	-0.041806	2.775937
216.218795	2500.252803	17.709107	-0.041791	2.771863
216.147865	2492.302563	17.714112	-0.041773	2.767810
216.006345	2484.303156	17.719117	-0.041741	2.763721
215.990684	2476.344257	17.724122	-0.041733	2.759655
216.078914	2468.373903	17.729127	-0.041745	2.755583
215.960413	2460.313566	17.734131	-0.041717	2.751447
215.982350	2452.335193	17.739136	-0.041716	2.747355
215.880942	2444.361409	17.744141	-0.041692	2.743252
215.903636	2436.409780	17.749146	-0.041691	2.739161
215.495112	2428.493888	17.754151	-0.041610	2.735057
215.547276	2420.479805	17.759155	-0.041614	2.730924
215.686474	2412.479543	17.764160	-0.041635	2.726797
215.697865	2404.505331	17.769165	-0.041632	2.722669
215.555926	2396.584359	17.774170	-0.041600	2.718553
215.481045	2388.613980	17.779175	-0.041581	2.714410
215.293520	2380.626106	17.784179	-0.041541	2.710244
215.414043	2372.632255	17.789184	-0.041558	2.706088
215.302388	2364.659358	17.794189	-0.041532	2.701921
215.272011	2356.713525	17.799194	-0.041522	2.697768
215.232343	2348.727410	17.804199	-0.041509	2.693586
215.390440	2340.701881	17.809203	-0.041533	2.689390
215.245533	2332.790772	17.814208	-0.041501	2.685228
214.900644	2324.856285	17.819213	-0.041432	2.681034
215.052499	2316.862931	17.824218	-0.041455	2.676835
215.175932	2308.834614	17.829223	-0.041472	2.672609
215.056522	2300.854360	17.834227	-0.041445	2.668386
214.885782	2292.898954	17.839232	-0.041408	2.664166
214.966799	2284.911995	17.844237	-0.041418	2.659938
215.016211	2276.965643	17.849242	-0.041422	2.655724
214.631496	2269.009891	17.854247	-0.041345	2.651470
214.412152	2261.044808	17.859251	-0.041299	2.647214
214.509763	2253.066320	17.864256	-0.041312	2.642966
214.292385	2245.112178	17.869261	-0.041266	2.638702
214.345753	2237.147000	17.874266	-0.041271	2.634444
214.310864	2229.135411	17.879271	-0.041259	2.630148
214.386836	2221.152870	17.884275	-0.041268	2.625868
214.245621	2213.219741	17.889280	-0.041237	2.621593
214.284707	2205.206911	17.894285	-0.041239	2.617281
214.327610	2197.249002	17.899290	-0.041242	2.612991
214.120400	2189.278936	17.904295	-0.041198	2.608670
213.931981	2181.333108	17.909299	-0.041158	2.604357
214.032327	2173.381517	17.914304	-0.041171	2.600053
213.885849	2165.421580	17.919309	-0.041139	2.595721
214.033395	2157.263042	17.924314	-0.041161	2.591293
213.894520	2149.282762	17.929319	-0.041130	2.586935
213.840120	2141.343985	17.934323	-0.041115	2.582599
213.489722	2133.452915	17.939328	-0.041044	2.578260
213.482693	2125.475439	17.944333	-0.041038	2.573891
213.477814	2117.493894	17.949338	-0.041032	2.569512
213.526756	2109.539310	17.954343	-0.041035	2.565145
213.301049	2101.614548	17.959347	-0.040988	2.560767
213.558002	2093.638674	17.964352	-0.041031	2.556387
213.304222	2085.673026	17.969357	-0.040978	2.551970
213.097769	2077.729967	17.974362	-0.040935	2.547560
213.045230	2069.761222	17.979367	-0.040920	2.543140
213.053544	2061.782595	17.984371	-0.040916	2.538710
213.106222	2053.812502	17.989376	-0.040921	2.534281
213.093772	2045.819559	17.994381	-0.040913	2.529827
212.826337	2037.900431	17.999386	-0.040858	2.525388
212.642351	2029.953171	18.004391	-0.040819	2.520931
212.816778	2021.966270	18.009395	-0.040846	2.516470
212.963062	2013.966464	18.014400	-0.040868	2.511991
212.533863	2006.021901	18.019405	-0.040783	2.507494
212.396847	1998.060545	18.024410	-0.040752	2.503001
212.497767	1990.090856	18.029415	-0.040766	2.498512
212.430647	1982.133697	18.034419	-0.040748	2.494010
212.275977	1974.156555	18.039424	-0.040714	2.489482
212.180391	1966.199549	18.044429	-0.040691	2.484962
212.170978	1958.237100	18.049434	-0.040684	2.480436
212.122839	1950.291205	18.054439	-0.040670	2.475909
212.097683	1942.309295	18.059443	-0.040660	2.471355
212.239957	1934.336092	18.064448	-0.040682	2.466809
212.050214	1926.379189	18.069453	-0.040641	2.462240
211.923002	1918.446390	18.074458	-0.040612	2.457681
211.799398	1910.477969	18.079463	-0.040584	2.453093
211.683263	1902.494017	18.084467	-0.040557	2.448488
211.765741	1894.523922	18.089472	-0.040567	2.443897
211.573461	1886.599511	18.094477	-0.040526	2.439304
211.545355	1878.678467	18.099482	-0.040516	2.434716
211.360405	1870.620996	18.104487	-0.040476	2.430028
211.146917	1862.666947	18.109491	-0.040431	2.425389
211.326281	1854.699532	18.114496	-0.040460	2.420764
211.344045	1846.734433	18.119501	-0.040458	2.416118
211.284777	1838.779119	18.124506	-0.040441	2.411464
211.405462	1830.799022	18.129511	-0.040459	2.406799
211.360628	1822.847845	18.134515	-0.040445	2.402130
211.164876	1814.950045	18.139520	-0.040404	2.397472
211.161975	1806.960950	18.144525	-0.040398	2.392765
211.044790	1799.007606	18.149530	-0.040371	2.388062
211.048578	1791.045886	18.154535	-0.040366	2.383353
210.906010	1783.106358	18.159539	-0.040335	2.378637
210.804568	1775.168469	18.164544	-0.040311	2.373916
210.579859	1767.198004	18.169549	-0.040264	2.369156
210.643386	1759.245675	18.174554	-0.040270	2.364420
210.367853	1751.316328	18.179559	-0.040214	2.359662
210.645140	1743.320650	18.184563	-0.040260	2.354898
210.624203	1735.345942	18.189568	-0.040251	2.350114
210.498643	1727.378817	18.194573	-0.040222	2.345315
210.463607	1719.435469	18.199578	-0.040211	2.340529
210.505601	1711.482411	18.204583	-0.040213	2.335733
210.337333	1703.524228	18.209587	-0.040177	2.330907
210.369675	1695.574339	18.214592	-0.040178	2.326092
210.041613	1687.656664	18.219597	-0.040111	2.321257
210.016566	1679.714806	18.224602	-0.040102	2.316423
210.154189	1671.719198	18.229607	-0.040122	2.311559
210.177265	1663.752181	18.234611	-0.040121	2.306693
210.041021	1655.839852	18.239616	-0.040091	2.301836
209.775925	1647.907369	18.244621	-0.040036	2.296946
209.822382	1639.925752	18.249626	-0.040040	2.292042
209.886351	1631.951929	18.254631	-0.040046	2.287133
209.722497	1624.031146	18.259635	-0.040011	2.282227
209.512993	1616.132541	18.264640	-0.039966	2.277321
209.508465	1608.095524	18.269645	-0.039960	2.272335
209.475058	1600.113497	18.274650	-0.039949	2.267371
209.346358	1592.182458	18.279655	-0.039920	2.262418
209.326862	1584.226714	18.284659	-0.039911	2.257450
209.188016	1576.309079	18.289664	-0.039880	2.252483
209.212760	1568.325778	18.294669	-0.039879	2.247479
209.208147	1560.391861	18.299674	-0.039873	2.242492
209.157919	1552.462399	18.304679	-0.039859	2.237492
208.986385	1544.524184	18.309683	-0.039822	2.232465
209.077910	1536.555274	18.314688	-0.039834	2.227431
209.092915	1528.603727	18.319693	-0.039831	2.222389
209.090363	1520.668493	18.324698	-0.039825	2.217345
208.947091	1512.735366	18.329703	-0.039794	2.212278
208.882365	1504.771589	18.334707	-0.039776	2.207187
208.988663	1496.830110	18.339712	-0.039791	2.202114
208.791768	1488.921712	18.344717	-0.039749	2.197022
208.682380	1480.967503	18.349722	-0.039724	2.191898
208.415937	1473.027106	18.354727	-0.039669	2.186756
208.236819	1465.092211	18.359731	-0.039630	2.181613
208.286522	1457.145090	18.364736	-0.039634	2.176471
208.152854	1449.192809	18.369741	-0.039604	2.171297
208.282874	1441.221298	18.374746	-0.039623	2.166122
208.226828	1433.299795	18.379751	-0.039608	2.160950
208.142457	1425.383677	18.384755	-0.039587	2.155767
208.222814	1417.417175	18.389760	-0.039597	2.150554
207.939870	1409.486563	18.394765	-0.039539	2.145317
207.962498	1401.554191	18.399770	-0.039538	2.140095
207.918222	1393.630910	18.404775	-0.039524	2.134860
207.877004	1385.660911	18.409779	-0.039512	2.129582
207.704657	1377.760340	18.414784	-0.039474	2.124324
207.685083	1369.819213	18.419789	-0.039465	2.119040
207.542949	1361.901543	18.424794	-0.039434	2.113747
207.415969	1353.894780	18.429799	-0.039405	2.108383
207.245539	1345.959190	18.434803	-0.039368	2.103048
207.483845	1338.015253	18.439808	-0.039407	2.097734
207.129646	1330.109850	18.444813	-0.039336	2.092375
207.063713	1322.168989	18.449818	-0.039319	2.087006
207.454309	1314.191626	18.454823	-0.039386	2.081643
207.171406	1306.316979	18.459827	-0.039328	2.076270
207.028152	1298.397644	18.464832	-0.039297	2.070867
207.033719	1290.436665	18.469837	-0.039292	2.065435
207.016658	1282.511075	18.474842	-0.039284	2.060011
206.808256	1274.623454	18.479847	-0.039240	2.054580
206.565690	1266.672305	18.484851	-0.039190	2.049087
206.906316	1258.716706	18.489856	-0.039248	2.043635
206.650154	1250.832798	18.494861	-0.039195	2.038158
206.755205	1242.876847	18.499866	-0.039210	2.032652
206.425078	1234.964994	18.504871	-0.039143	2.027118
206.396977	1227.020127	18.509875	-0.039133	2.021577
206.347147	1219.111848	18.514880	-0.039118	2.016043
206.143614	1211.176425	18.519885	-0.039075	2.010460
206.316248	1203.230521	18.524890	-0.039102	2.004893
206.064049	1195.352069	18.529895	-0.039050	1.999313
206.080749	1187.417696	18.534899	-0.039048	1.993706
206.078023	1179.479682	18.539904	-0.039042	1.988079
205.661673	1171.602903	18.544909	-0.038959	1.982436
205.773281	1163.667301	18.549914	-0.038975	1.976791
205.851571	1155.714746	18.554919	-0.038984	1.971113
205.843346	1147.779681	18.559923	-0.038978	1.965423
205.742178	1139.902077	18.564928	-0.038954	1.959747
205.537659	1131.997778	18.569933	-0.038911	1.954025
205.510535	1124.020762	18.574938	-0.038900	1.948252
205.505939	1116.104174	18.579943	-0.038894	1.942509
205.180891	1108.219551	18.584947	-0.038829	1.936736
205.330584	1100.274775	18.589952	-0.038851	1.930955
205.322334	1092.342962	18.594957	-0.038845	1.925148
205.290695	1084.454509	18.599962	-0.038834	1.919353
205.066079	1076.569737	18.604967	-0.038787	1.913522
204.976687	1068.636146	18.609971	-0.038765	1.907651
204.839840	1060.749987	18.614976	-0.038734	1.901793
204.681980	1052.841910	18.619981	-0.038700	1.895897
204.875906	1044.890648	18.624986	-0.038731	1.889991
204.798210	1036.994532	18.629991	-0.038711	1.884077
204.653752	1029.104952	18.634995	-0.038679	1.878141
204.812585	1021.168668	18.640000	-0.038703	1.872186
204.631639	1013.262086	18.645005	-0.038664	1.866195
204.583723	1005.364579	18.650010	-0.038650	1.860208
204.641089	997.462233	18.655015	-0.038656	1.854209
204.520801	989.542081	18.660019	-0.038628	1.848157
204.245339	981.693355	18.665024	-0.038572	1.842121
204.164915	973.798140	18.670029	-0.038552	1.836053
204.112320	965.882677	18.675034	-0.038537	1.829952
203.995642	957.997640	18.680039	-0.038510	1.823847
203.783086	950.114254	18.685043	-0.038465	1.817710
203.859277	942.192803	18.690048	-0.038474	1.811558
203.750820	934.290562	18.695053	-0.038449	1.805378
203.743802	926.414851	18.700058	-0.038443	1.799210
203.827172	918.485667	18.705063	-0.038453	1.792989
203.538754	910.569651	18.710067	-0.038394	1.786712
203.472100	902.696444	18.715072	-0.038376	1.780474
203.381446	894.812588	18.720077	-0.038354	1.774202
203.490355	886.891926	18.725082	-0.038370	1.767903
203.399347	879.030719	18.730087	-0.038347	1.761605
203.177453	871.176754	18.735091	-0.038301	1.755273
203.271107	863.265781	18.740096	-0.038313	1.748912
203.210269	855.373908	18.745101	-0.038297	1.742524
203.055101	847.531335	18.750106	-0.038263	1.736140
202.883574	839.654656	18.755111	-0.038226	1.729703
202.857723	831.758984	18.760115	-0.038216	1.723245
202.817368	823.905797	18.765120	-0.038203	1.716795
202.562158	816.023070	18.770125	-0.038151	1.710269
202.803295	808.093677	18.775130	-0.038190	1.703744
202.781976	800.235804	18.780135	-0.038181	1.697219
202.480315	792.383243	18.785139	-0.038120	1.690636
202.420571	784.519312	18.790144	-0.038104	1.684050
202.452411	776.645662	18.795149	-0.038104	1.677443
202.283475	768.792111	18.800154	-0.038068	1.670799
202.405571	760.899022	18.805159	-0.038085	1.664134
202.142987	753.068477	18.810163	-0.038031	1.657443
202.241998	745.184073	18.815168	-0.038045	1.650729
201.934139	737.350982	18.820173	-0.037982	1.643975
202.122978	729.479395	18.825178	-0.038012	1.637229
201.932464	721.597103	18.830183	-0.037972	1.630393
201.681346	713.731840	18.835187	-0.037920	1.623535
201.712719	705.882836	18.840192	-0.037921	1.616701
201.781870	697.996766	18.845197	-0.037928	1.609811
201.557212	690.183859	18.850202	-0.037881	1.602914
201.398056	682.365448	18.855207	-0.037847	1.595992
201.402842	674.485612	18.860211	-0.037842	1.589008
201.456194	666.633387	18.865216	-0.037847	1.582025
201.221997	658.824976	18.870221	-0.037798	1.575009
201.216344	650.967119	18.875226	-0.037792	1.567950
201.294782	643.118552	18.880231	-0.037802	1.560880
201.088220	635.311472	18.885235	-0.037758	1.553774
201.030513	627.460548	18.890240	-0.037742	1.546616
200.981407	619.633655	18.895245	-0.037728	1.539449
200.810864	611.812581	18.900250	-0.037691	1.532236
200.684606	603.988527	18.905255	-0.037663	1.524992
200.535599	596.185939	18.910259	-0.037630	1.517730
200.529483	588.344537	18.915264	-0.037624	1.510419
200.431016	580.522179	18.920269	-0.037600	1.503075
200.240390	572.727819	18.925274	-0.037560	1.495708
200.359718	564.884591	18.930279	-0.037577	1.488306
200.259870	557.071489	18.935283	-0.037553	1.480862
200.081540	549.293291	18.940288	-0.037515	1.473401
200.154764	541.407138	18.945293	-0.037523	1.465838
199.857894	533.653269	18.950298	-0.037463	1.458304
199.772972	525.853358	18.955303	-0.037442	1.450721
199.813944	518.027534	18.960307	-0.037445	1.443093
199.834476	510.244871	18.965312	-0.037443	1.435463
199.642274	502.459145	18.970317	-0.037402	1.427755
199.346723	494.709904	18.975322	-0.037342	1.420024
199.592091	486.877865	18.980327	-0.037383	1.412257
199.407030	479.103083	18.985331	-0.037343	1.404434
199.160789	471.382349	18.990336	-0.037292	1.396611
198.989590	463.587728	18.995341	-0.037256	1.388681
198.973282	455.795340	19.000346	-0.037247	1.380734
198.988145	448.026427	19.005351	-0.037245	1.372771
198.838599	440.254369	19.010355	-0.037212	1.364729
198.769099	432.516785	19.015360	-0.037194	1.356690
198.577313	424.769381	19.020365	-0.037153	1.348571
198.607458	416.994754	19.025370	-0.037154	1.340413
198.533128	409.259631	19.030375	-0.037135	1.332229
198.440655	401.506444	19.035379	-0.037113	1.323972
198.394967	393.784448	19.040384	-0.037099	1.315704
198.313905	385.907224	19.045389	-0.037079	1.307210
198.194667	378.195849	19.050394	-0.037052	1.298834
198.037147	370.490085	19.055399	-0.037017	1.290402
198.050486	362.760110	19.060403	-0.037015	1.281920
198.116545	355.046375	19.065408	-0.037022	1.273410
197.971474	347.339155	19.070413	-0.036990	1.264809
197.624315	339.693962	19.075418	-0.036921	1.256181
197.660403	331.972724	19.080423	-0.036922	1.247481
197.596394	324.283158	19.085427	-0.036905	1.238736
197.557671	316.588291	19.090432	-0.036893	1.229928
197.387016	308.907951	19.095437	-0.036856	1.221047
197.448767	301.212292	19.100442	-0.036863	1.212129
197.175367	293.582743	19.105447	-0.036807	1.203155
197.014103	285.932617	19.110451	-0.036772	1.194113
197.181502	278.235900	19.115456	-0.036798	1.185012
196.892732	270.622864	19.120461	-0.036739	1.175848
196.719199	262.989691	19.125466	-0.036702	1.166612
196.730828	255.355405	19.130471	-0.036699	1.157339
196.557425	247.692749	19.135475	-0.036662	1.147917
196.495879	240.078026	19.140480	-0.036645	1.138500
196.539643	232.431549	19.145485	-0.036649	1.128988
196.311781	224.856581	19.150490	-0.036601	1.119426
196.289780	217.253269	19.155495	-0.036592	1.109791
196.101080	209.676072	19.160499	-0.036552	1.100068
196.239000	202.067375	19.165504	-0.036573	1.090290
195.952317	194.538978	19.170509	-0.036515	1.080433
195.737332	186.997652	19.175514	-0.036470	1.070484
195.598509	179.447808	19.180519	-0.036439	1.060448
195.510174	171.904532	19.185523	-0.036417	1.050337
195.478292	164.373560	19.190528	-0.036407	1.040157
195.216079	156.882332	19.195533	-0.036353	1.029877
194.931482	149.401869	19.200538	-0.036295	1.019502
194.867459	141.903193	19.205543	-0.036278	1.009048
194.686940	134.432386	19.210547	-0.036240	0.998496
194.497086	126.949036	19.215552	-0.036200	0.987811
194.264980	119.501389	19.220557	-0.036151	0.977049
193.767798	112.113907	19.225562	-0.036054	0.966188
193.316044	104.745246	19.230567	-0.035965	0.955243
193.156434	97.318704	19.235571	-0.035931	0.944160
192.685973	89.976433	19.240576	-0.035838	0.932991
192.121422	82.652765	19.245581	-0.035728	0.921690
191.792528	75.305564	19.250586	-0.035662	0.910275
191.439501	67.974765	19.255591	-0.035592	0.898735
190.938289	60.911658	19.260595	-0.035494	0.887428