Number of Data Points = 30
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
3463_Position 26_00000 LC.hys	256.416717	7999.433979	178.241430	4218771.650546	290.359377	290.076543	76.886568	1.896152	78.267364	237.633841	1.168515	-132.783493	-59.972995	1.492581
3463_Position 26_00001 LC.hys	257.210516	7999.408824	179.802285	4245947.295189	290.820374	290.578038	77.311257	1.884010	58.425142	235.885782	1.229315	-132.776497	-59.972995	0.518335
3463_Position 26_00002 LC.hys	253.157730	7999.222878	175.219727	4108003.323170	287.572122	287.397123	76.595355	1.947229	53.342639	230.738027	1.241094	-132.768997	-59.972995	0.231071
3463_Position 26_00003 LC.hys	256.476188	7999.698417	181.849123	4220804.998356	289.542955	289.469330	78.423893	1.895302	56.446398	234.964741	1.238998	-132.762497	-59.972995	-0.049141
3463_Position 26_00004 LC.hys	246.011261	7999.618275	177.035234	3869655.882958	280.034649	279.901203	79.736720	2.067269	56.599984	224.238606	1.231839	-132.755493	-59.972995	-0.059384
3463_Position 26_00005 LC.hys	241.695904	7999.546840	172.416890	3728785.638328	276.619285	276.493308	79.109917	2.145349	56.629632	219.644617	1.225279	-132.748497	-59.972995	-0.073606
3463_Position 26_00006 LC.hys	254.994142	7999.620004	179.444633	4170261.342877	288.565339	288.429051	77.854490	1.918254	77.701235	236.200748	1.171567	-132.783493	-59.965995	-0.096506
3463_Position 26_00007 LC.hys	260.936006	7999.152032	178.513186	4374507.722128	294.810803	294.543406	75.620673	1.828583	60.654908	239.872416	1.220066	-132.776497	-59.965995	-0.049022
3463_Position 26_00008 LC.hys	251.273831	7999.572884	179.842975	4044563.298451	284.882029	284.634487	79.230517	1.977858	47.725094	228.157832	1.269684	-132.769493	-59.965995	-0.017651
3463_Position 26_00009 LC.hys	267.183029	7999.212019	179.484882	4593826.920552	301.107611	300.608736	74.195128	1.741296	46.246422	243.765815	1.275431	-132.762497	-59.965995	-0.000975
3463_Position 26_00010 LC.hys	254.187582	7999.640326	183.583591	4142866.720740	287.192278	286.868772	79.913142	1.930943	62.391472	233.652549	1.221258	-132.755493	-59.965995	-0.010045
3463_Position 26_00011 LC.hys	259.716242	7999.123779	186.002700	4332231.165629	292.241205	291.970305	79.176858	1.846421	62.575054	239.336375	1.223891	-132.748497	-59.965995	0.047524
3463_Position 26_00012 LC.hys	238.454587	7999.672433	178.438053	3624502.861713	272.325143	272.078325	83.042054	2.207109	43.605913	214.443102	1.285592	-132.783493	-59.958996	0.052937
3463_Position 26_00013 LC.hys	257.495473	7999.357032	178.695091	4255721.422632	291.261024	291.069523	76.746902	1.879671	57.079862	235.898417	1.232450	-132.776497	-59.958996	0.048035
3463_Position 26_00014 LC.hys	243.419469	7999.381411	178.251344	3784772.040339	277.283870	277.077202	81.179763	2.113570	57.772725	221.904066	1.229431	-132.769493	-59.958996	0.088060
3463_Position 26_00015 LC.hys	255.979115	7999.575239	184.044797	4203823.070375	288.583570	288.578142	79.530948	1.902929	65.102586	235.840990	1.213314	-132.762497	-59.958996	0.098932
3463_Position 26_00016 LC.hys	254.491244	7999.567539	179.269347	4153171.246707	288.259198	287.958626	77.938303	1.926135	56.489557	232.835006	1.235314	-132.755493	-59.958996	0.131490
3463_Position 26_00017 LC.hys	261.407302	7999.638034	185.613320	4390890.663636	294.126521	293.731106	78.481565	1.821871	58.515937	240.424235	1.236864	-132.748497	-59.958996	0.096715
3463_Position 26_00018 LC.hys	245.736075	7999.531185	180.031840	3860603.733714	279.421963	279.061560	81.181400	2.072093	52.407609	223.460183	1.251326	-132.783493	-59.951996	0.082985
3463_Position 26_00019 LC.hys	245.604851	7999.618206	176.299826	3856290.475982	279.884931	279.636159	79.542977	2.074434	64.286909	224.940549	1.205411	-132.776497	-59.951996	0.124875
3463_Position 26_00020 LC.hys	252.971133	7999.303842	182.999589	4101700.348226	285.999338	285.755239	80.057676	1.950241	63.292801	232.531532	1.217596	-132.769493	-59.951996	0.118608
3463_Position 26_00021 LC.hys	252.450759	7999.441401	178.892668	4084145.283605	286.189205	285.988081	78.429018	1.958657	58.689009	231.113462	1.227169	-132.762497	-59.951996	0.086835
3463_Position 26_00022 LC.hys	260.139496	7999.084829	184.315436	4346880.646498	293.131654	292.688661	78.326312	1.840190	52.499893	238.142120	1.256865	-132.754997	-59.951996	0.098108
3463_Position 26_00023 LC.hys	251.633173	7999.679430	183.639335	4056630.572371	284.479898	284.304602	80.782597	1.972001	66.951067	231.719471	1.207136	-132.748497	-59.951996	0.115216
3463_Position 26_00024 LC.hys	245.233069	7999.582131	179.193579	3844081.807208	278.937344	278.714663	80.976866	2.081012	62.237470	224.437117	1.215837	-132.783493	-59.944996	0.083287
3463_Position 26_00025 LC.hys	272.339528	7999.265804	187.537505	4778363.630012	304.578233	304.330192	76.012211	1.674060	73.266170	253.400480	1.194013	-132.776497	-59.944996	0.116751
3463_Position 26_00026 LC.hys	277.223102	7999.307721	180.869067	4956026.966443	310.681692	310.393399	71.983390	1.614057	60.335063	256.244867	1.224330	-132.769493	-59.944996	0.088369
3463_Position 26_00027 LC.hys	250.916393	7999.266356	175.380457	4032575.670310	285.302846	285.124593	77.379294	1.983662	68.805274	230.821602	1.190570	-132.762497	-59.944996	0.092252
3463_Position 26_00028 LC.hys	256.089463	7999.465875	181.110383	4207590.382412	289.447871	289.216218	78.227860	1.901199	55.878500	234.446090	1.240013	-132.754997	-59.944996	0.084987
3463_Position 26_00029 LC.hys	245.062849	7999.511245	179.091796	3838497.764324	278.792969	278.563174	80.989715	2.084021	61.399153	224.140170	1.218414	-132.748497	-59.944996	0.105447