Tue Mar 23 11:33:37 2021

Number of Points = 3625
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.806527	0.097013	0.000000	0.000073	0.722600

0.931702	0.129833	0.005005	0.000050	0.722708
1.131530	0.090130	0.010010	0.000013	0.722700
0.860887	0.139667	0.015014	0.000063	0.722703
0.922373	0.017428	0.020019	0.000052	0.722485
0.924875	-0.037100	0.025024	0.000051	0.722378
0.855713	-0.021246	0.030029	0.000064	0.722386
0.953434	-0.043246	0.035034	0.000046	0.722377
0.931988	-0.038072	0.040038	0.000050	0.722380
1.015229	-0.052051	0.045043	0.000034	0.722381
0.898009	-0.033999	0.050048	0.000056	0.722376
0.987585	-0.043781	0.055053	0.000039	0.722388
1.038170	-0.056914	0.060058	0.000029	0.722380
1.168781	-0.079406	0.065062	0.000005	0.722382
1.146742	-0.073331	0.070067	0.000009	0.722386
1.053351	-0.060237	0.075072	0.000026	0.722379
1.053561	-0.056971	0.080077	0.000026	0.722386
0.918537	-0.085935	0.085082	0.000051	0.722282
0.965773	-0.194809	0.090086	0.000043	0.722085
0.876886	-0.178344	0.095091	0.000059	0.722086
0.820655	-0.172181	0.100096	0.000069	0.722079
0.862379	-0.174400	0.105101	0.000062	0.722089
1.044579	-0.210446	0.110106	0.000028	0.722082
0.799164	-0.165916	0.115110	0.000073	0.722084
0.975202	-0.317429	0.120115	0.000040	0.721848
0.758690	-0.329939	0.125120	0.000081	0.721748
0.915423	-0.353311	0.130125	0.000051	0.721757
0.849751	-0.346220	0.135130	0.000064	0.721748
1.146037	-0.395906	0.140134	0.000008	0.721754
0.853069	-0.453467	0.145139	0.000063	0.721539
0.862805	-0.505203	0.150144	0.000061	0.721440
1.074522	-0.536859	0.155149	0.000022	0.721452
1.038293	-0.534253	0.160154	0.000028	0.721445
1.096195	-0.633087	0.165158	0.000017	0.721271
0.970273	-0.680091	0.170163	0.000041	0.721135
0.940516	-0.677922	0.175168	0.000046	0.721129
0.945103	-0.675996	0.180173	0.000045	0.721134
0.951536	-0.788868	0.185178	0.000044	0.720914
0.864672	-0.788348	0.190182	0.000060	0.720885
0.940103	-0.798521	0.195187	0.000046	0.720892
0.738849	-0.854555	0.200192	0.000084	0.720711
0.844164	-0.951356	0.205197	0.000064	0.720558
0.729710	-0.934936	0.210202	0.000085	0.720550
0.723012	-0.988989	0.215206	0.000086	0.720441
0.829828	-1.111702	0.220211	0.000066	0.720237
0.688997	-1.090742	0.225216	0.000093	0.720229
0.775200	-1.164124	0.230221	0.000077	0.720115
0.660951	-1.248419	0.235226	0.000098	0.719909
0.818191	-1.275976	0.240230	0.000068	0.719910
0.872725	-1.374972	0.245235	0.000058	0.719734
0.688855	-1.404224	0.250240	0.000092	0.719612
0.722987	-1.407922	0.255245	0.000086	0.719617
0.736168	-1.581353	0.260250	0.000084	0.719280
0.487048	-1.535644	0.265254	0.000130	0.719282
0.555128	-1.620360	0.270259	0.000117	0.719139
0.331976	-1.668866	0.275264	0.000159	0.718965
0.460932	-1.687196	0.280269	0.000135	0.718975
0.486786	-1.855931	0.285274	0.000130	0.718651
0.546906	-1.864813	0.290278	0.000119	0.718655
0.589226	-1.966222	0.295283	0.000111	0.718469
0.430102	-1.993169	0.300288	0.000140	0.718360
0.470329	-2.070778	0.305293	0.000133	0.718221
0.373062	-2.150947	0.310298	0.000151	0.718029
0.498336	-2.216815	0.315302	0.000127	0.717943
0.324535	-2.299938	0.320307	0.000160	0.717718
0.270276	-2.317195	0.325312	0.000170	0.717664
0.456008	-2.485532	0.330317	0.000135	0.717397
0.329898	-2.485523	0.335322	0.000159	0.717353
-0.568728	-2.456707	0.340326	0.000326	0.717093
-2.362962	-2.136579	0.345331	0.000660	0.717095
-2.236618	-2.259091	0.350336	0.000636	0.716897
-3.091101	-2.172008	0.355341	0.000795	0.716768
-2.978034	-2.195057	0.360346	0.000774	0.716763
-3.351812	-2.192505	0.365350	0.000844	0.716636
-4.194995	-2.131406	0.370355	0.001000	0.716460
-3.880593	-2.190272	0.375360	0.000942	0.716454
-4.294849	-2.112471	0.380365	0.001019	0.716462
-4.537494	-2.195254	0.385370	0.001064	0.716213
-4.833162	-2.176822	0.390374	0.001119	0.716145
-4.689331	-2.201843	0.395379	0.001092	0.716147
-5.320752	-2.095015	0.400384	0.001210	0.716136
-5.409021	-2.172904	0.405389	0.001226	0.715950
-5.491674	-2.188853	0.410394	0.001241	0.715890
-5.919549	-2.113233	0.415398	0.001321	0.715889
-5.587840	-2.168448	0.420403	0.001259	0.715896
-5.945294	-2.190803	0.425408	0.001326	0.715726
-6.937876	-2.097732	0.430413	0.001510	0.715560
-6.642491	-2.153723	0.435418	0.001455	0.715554
-7.037062	-2.083599	0.440422	0.001529	0.715553
-6.755926	-2.131031	0.445427	0.001476	0.715559
-6.983108	-2.169776	0.450432	0.001518	0.715402
-7.713468	-2.118607	0.455437	0.001654	0.715245
-7.453529	-2.167339	0.460442	0.001606	0.715241
-8.036192	-2.063084	0.465446	0.001714	0.715242
-7.800606	-2.103034	0.470451	0.001670	0.715246
-7.349289	-2.203909	0.475456	0.001586	0.715206
-8.378956	-2.163735	0.480461	0.001778	0.714921
-8.955021	-2.063011	0.485466	0.001885	0.714918
-8.724755	-2.104218	0.490470	0.001842	0.714918
-8.016130	-2.229605	0.495475	0.001710	0.714919
-8.690188	-2.113472	0.500480	0.001835	0.714912
-8.852237	-2.117905	0.505485	0.001865	0.714846
-9.200134	-2.172441	0.510490	0.001930	0.714615
-9.156260	-2.181627	0.515494	0.001922	0.714612
-9.556759	-2.106356	0.520499	0.001996	0.714620
-9.583495	-2.106699	0.525504	0.002001	0.714610
-9.124887	-2.185237	0.530509	0.001916	0.714616
-9.517011	-2.159245	0.535514	0.001989	0.714529
-10.354454	-2.134108	0.540518	0.002145	0.714283
-9.912294	-2.209760	0.545523	0.002062	0.714290
-10.819552	-2.051844	0.550528	0.002231	0.714282
-10.391548	-2.123756	0.555533	0.002151	0.714291
-10.047029	-2.188890	0.560538	0.002087	0.714284
-10.609114	-2.088136	0.565542	0.002192	0.714285
-10.813849	-2.180484	0.570547	0.002230	0.714029
-11.477698	-2.090187	0.575552	0.002353	0.713974
-11.424805	-2.095678	0.580557	0.002343	0.713982
-11.443105	-2.095751	0.585562	0.002347	0.713975
-11.626117	-2.063187	0.590566	0.002381	0.713975
-11.002692	-2.171955	0.595571	0.002265	0.713980
-11.157182	-2.148318	0.600576	0.002293	0.713973
-12.081303	-2.135186	0.605581	0.002465	0.713672
-12.251611	-2.110496	0.610586	0.002497	0.713660
-12.311738	-2.099860	0.615590	0.002508	0.713660
-12.085421	-2.138365	0.620595	0.002466	0.713664
-12.581402	-2.055034	0.625600	0.002558	0.713654
-12.176478	-2.123588	0.630605	0.002483	0.713662
-12.249044	-2.110697	0.635610	0.002496	0.713662
-12.842225	-2.130081	0.640614	0.002606	0.713413
-12.984490	-2.124389	0.645619	0.002633	0.713374
-13.269100	-2.079373	0.650624	0.002686	0.713363
-13.063418	-2.111066	0.655629	0.002647	0.713373
-13.038751	-2.117456	0.660634	0.002643	0.713369
-13.380633	-2.057571	0.665638	0.002706	0.713367
-13.235272	-2.080361	0.670643	0.002679	0.713374
-13.450888	-2.172948	0.675648	0.002719	0.713113
-14.057965	-2.102483	0.680653	0.002832	0.713038
-14.184204	-2.084225	0.685658	0.002855	0.713030
-14.364118	-2.052524	0.690662	0.002889	0.713029
-13.796704	-2.150501	0.695667	0.002783	0.713036
-13.827787	-2.147391	0.700672	0.002789	0.713031
-13.985529	-2.115993	0.705677	0.002818	0.713038
-14.404773	-2.158914	0.710682	0.002896	0.712804
-15.283076	-2.046813	0.715686	0.003060	0.712716
-14.878130	-2.115616	0.720691	0.002984	0.712722
-14.986577	-2.100330	0.725696	0.003004	0.712714
-14.976443	-2.097507	0.730701	0.003002	0.712724
-14.790315	-2.132776	0.735706	0.002968	0.712720
-14.964466	-2.102806	0.740710	0.003000	0.712718
-15.076336	-2.170651	0.745715	0.003021	0.712543
-16.432001	-2.006474	0.750720	0.003273	0.712389
-16.099561	-2.060836	0.755725	0.003211	0.712399
-15.958248	-2.087965	0.760730	0.003185	0.712395
-15.857819	-2.108203	0.765734	0.003166	0.712391
-15.865497	-2.101190	0.770739	0.003167	0.712402
-16.287923	-2.032943	0.775744	0.003246	0.712388
-15.951981	-2.086872	0.780749	0.003183	0.712400
-16.329191	-2.158273	0.785754	0.003253	0.712124
-17.136531	-2.029711	0.790758	0.003404	0.712094
-16.783102	-2.088951	0.795763	0.003338	0.712102
-16.449991	-2.151737	0.800768	0.003276	0.712095
-16.911600	-2.065503	0.805773	0.003361	0.712103
-17.058925	-2.040036	0.810778	0.003389	0.712102
-16.651231	-2.114816	0.815782	0.003313	0.712097
-17.032888	-2.174286	0.820787	0.003384	0.711843
-17.912476	-2.056131	0.825792	0.003548	0.711767
-17.687013	-2.092772	0.830797	0.003505	0.711774
-17.445277	-2.136226	0.835802	0.003460	0.711773
-17.968772	-2.046754	0.840806	0.003558	0.711766
-17.604646	-2.106495	0.845811	0.003490	0.711776
-17.772055	-2.082106	0.850816	0.003521	0.711766
-18.123652	-2.119089	0.855821	0.003586	0.711567
-18.858135	-2.039910	0.860826	0.003723	0.711464
-18.643095	-2.079704	0.865830	0.003683	0.711461
-18.548764	-2.093298	0.870835	0.003665	0.711468
-19.100623	-1.999709	0.875840	0.003768	0.711459
-18.716539	-2.064573	0.880845	0.003696	0.711466
-18.688508	-2.072888	0.885850	0.003691	0.711459
-19.030922	-2.012584	0.890854	0.003755	0.711458
-19.036721	-2.159930	0.895859	0.003756	0.711162
-19.334400	-2.117214	0.900864	0.003811	0.711142
-19.718370	-2.044343	0.905869	0.003883	0.711151
-19.483779	-2.087073	0.910874	0.003839	0.711149
-19.766750	-2.038843	0.915878	0.003891	0.711145
-19.516538	-2.079586	0.920883	0.003845	0.711153
-19.463757	-2.093287	0.925888	0.003835	0.711144
-19.902747	-2.141029	0.930893	0.003917	0.710893
-20.163948	-2.100234	0.935898	0.003965	0.710881
-20.566973	-2.031316	0.940902	0.004040	0.710876
-19.943438	-2.136816	0.945907	0.003924	0.710887
-20.290022	-2.081903	0.950912	0.003988	0.710874
-20.294837	-2.078031	0.955917	0.003989	0.710880
-20.176186	-2.153882	0.960922	0.003967	0.710771
-21.294397	-2.073505	0.965926	0.004175	0.710533
-20.758528	-2.165813	0.970931	0.004075	0.710540
-21.497720	-2.038130	0.975936	0.004213	0.710532
-21.318886	-2.066591	0.980941	0.004179	0.710539
-20.888999	-2.144118	0.985946	0.004099	0.710537
-21.602791	-2.018538	0.990950	0.004232	0.710534
-21.267494	-2.133157	0.995955	0.004170	0.710425
-22.221023	-2.065774	1.000960	0.004347	0.710220
-21.950752	-2.108732	1.005965	0.004297	0.710231
-22.228567	-2.060947	1.010970	0.004348	0.710227
-22.127470	-2.080284	1.015974	0.004329	0.710225
-21.951952	-2.109132	1.020979	0.004297	0.710230
-22.583687	-2.001371	1.025984	0.004414	0.710220
-22.194922	-2.094610	1.030989	0.004342	0.710173
-22.870611	-2.108539	1.035994	0.004467	0.709904
-23.169918	-2.057195	1.040998	0.004523	0.709900
-23.278646	-2.035399	1.046003	0.004543	0.709905
-23.164029	-2.059915	1.051008	0.004522	0.709897
-23.138297	-2.061491	1.056013	0.004517	0.709903
-23.000571	-2.086691	1.061018	0.004491	0.709902
-23.076762	-2.075726	1.066022	0.004505	0.709897
-23.316088	-2.151628	1.071027	0.004550	0.709660
-24.330578	-2.001524	1.076032	0.004739	0.709599
-23.958092	-2.063990	1.081037	0.004669	0.709607
-23.629035	-2.123945	1.086042	0.004608	0.709604
-24.312567	-2.005112	1.091046	0.004735	0.709599
-24.018032	-2.052089	1.096051	0.004680	0.709610
-23.887665	-2.082492	1.101056	0.004656	0.709596
-24.187258	-2.132665	1.106061	0.004712	0.709389
-25.169135	-2.017212	1.111066	0.004894	0.709270
-24.904655	-2.065427	1.116070	0.004845	0.709268
-24.484803	-2.135205	1.121075	0.004767	0.709278
-25.118104	-2.026333	1.126080	0.004885	0.709270
-24.992553	-2.046985	1.131085	0.004861	0.709274
-24.830276	-2.076443	1.136090	0.004831	0.709273
-25.177071	-2.081081	1.141094	0.004895	0.709140
-25.947219	-2.029249	1.146099	0.005039	0.708969
-25.866156	-2.047861	1.151104	0.005023	0.708961
-25.945253	-2.030956	1.156109	0.005038	0.708967
-25.809850	-2.054808	1.161114	0.005013	0.708967
-25.593309	-2.096820	1.166118	0.004972	0.708961
-25.573776	-2.095658	1.171123	0.004969	0.708970
-26.137669	-2.005151	1.176128	0.005074	0.708950
-26.292728	-2.128780	1.181133	0.005102	0.708647
-26.225528	-2.140556	1.186138	0.005090	0.708648
-26.814982	-2.037658	1.191142	0.005199	0.708644
-26.686140	-2.055393	1.196147	0.005175	0.708654
-26.755609	-2.047763	1.201152	0.005188	0.708645
-26.503737	-2.090499	1.206157	0.005141	0.708649
-26.404121	-2.141397	1.211162	0.005123	0.708583
-27.538700	-2.053171	1.216166	0.005334	0.708355
-26.853380	-2.171748	1.221171	0.005206	0.708362
-27.511708	-2.057779	1.226176	0.005329	0.708356
-27.720441	-2.016764	1.231181	0.005367	0.708364
-27.528709	-2.053419	1.236186	0.005332	0.708359
-27.379057	-2.080862	1.241190	0.005304	0.708357
-27.316319	-2.166211	1.246195	0.005292	0.708209
-28.465954	-2.056047	1.251200	0.005506	0.708019
-28.179423	-2.104068	1.256205	0.005453	0.708025
-28.348743	-2.074281	1.261210	0.005484	0.708025
-28.786857	-1.999823	1.266214	0.005565	0.708018
-28.103874	-2.117793	1.271219	0.005438	0.708025
-28.400945	-2.068081	1.276224	0.005493	0.708019
-28.597308	-2.097414	1.281229	0.005530	0.707890
-29.077259	-2.102108	1.286234	0.005619	0.707709
-28.833076	-2.148615	1.291238	0.005574	0.707703
-29.564174	-2.014901	1.296243	0.005710	0.707710
-29.777979	-1.982242	1.301248	0.005749	0.707700
-29.099375	-2.098891	1.306253	0.005623	0.707708
-29.320067	-2.057886	1.311258	0.005664	0.707712
-29.744919	-2.006640	1.316262	0.005743	0.707663
-30.081289	-2.080791	1.321267	0.005806	0.707394
-30.183819	-2.069165	1.326272	0.005825	0.707381
-30.684636	-1.975050	1.331277	0.005918	0.707391
-30.157459	-2.070901	1.336282	0.005820	0.707387
-30.356139	-2.038912	1.341286	0.005857	0.707380
-30.440764	-2.020133	1.346291	0.005872	0.707388
-30.265069	-2.056573	1.351296	0.005839	0.707378
-30.075178	-2.173728	1.356301	0.005804	0.707211
-31.416783	-1.995736	1.361306	0.006054	0.707088
-31.495729	-1.983490	1.366310	0.006068	0.707084
-30.990190	-2.070705	1.371315	0.005974	0.707090
-31.235745	-2.031448	1.376320	0.006020	0.707082
-31.206127	-2.033769	1.381325	0.006014	0.707088
-30.905372	-2.088803	1.386330	0.005958	0.707085
-31.261782	-2.096983	1.391334	0.006024	0.706941
-32.042490	-2.046545	1.396339	0.006170	0.706763
-32.012953	-2.057516	1.401344	0.006164	0.706752
-32.098758	-2.037520	1.406349	0.006180	0.706761
-31.919611	-2.070338	1.411354	0.006147	0.706760
-32.132839	-2.034120	1.416358	0.006186	0.706756
-31.763829	-2.096191	1.421363	0.006117	0.706764
-32.050809	-2.107737	1.426368	0.006171	0.706638
-33.208746	-1.994685	1.431373	0.006386	0.706451
-32.812526	-2.066928	1.436378	0.006312	0.706447
-32.944531	-2.044175	1.441382	0.006337	0.706446
-32.591226	-2.103644	1.446387	0.006271	0.706453
-32.777837	-2.074925	1.451392	0.006306	0.706444
-33.014774	-2.029433	1.456397	0.006350	0.706451
-32.817860	-2.123696	1.461402	0.006313	0.706332
-34.065262	-2.000862	1.466406	0.006545	0.706132
-33.496457	-2.099441	1.471411	0.006439	0.706138
-33.880878	-2.035115	1.476416	0.006511	0.706130
-33.921928	-2.024962	1.481421	0.006518	0.706136
-33.550646	-2.090549	1.486426	0.006449	0.706137
-33.987967	-2.015476	1.491430	0.006530	0.706131
-34.048453	-2.022855	1.496435	0.006542	0.706095
-35.018466	-1.962495	1.501440	0.006722	0.705869
-34.383388	-2.073432	1.506445	0.006604	0.705873
-34.195615	-2.107128	1.511450	0.006569	0.705873
-34.626269	-2.032774	1.516454	0.006649	0.705868
-34.354796	-2.076811	1.521459	0.006598	0.705877
-34.253155	-2.099966	1.526464	0.006579	0.705867
-34.561746	-2.140272	1.531469	0.006637	0.705676
-35.561936	-2.032972	1.536474	0.006823	0.705533
-35.366116	-2.071670	1.541478	0.006786	0.705526
-35.273644	-2.082875	1.546483	0.006769	0.705536
-35.702505	-2.008994	1.551488	0.006849	0.705531
-35.356482	-2.068802	1.556493	0.006784	0.705535
-35.270278	-2.085443	1.561498	0.006768	0.705533
-36.046789	-2.062418	1.566502	0.006913	0.705301
-36.304031	-2.055210	1.571507	0.006960	0.705223
-36.342342	-2.052681	1.576512	0.006968	0.705215
-36.394119	-2.041007	1.581517	0.006977	0.705220
-36.419103	-2.036512	1.586522	0.006982	0.705220
-36.145383	-2.089211	1.591526	0.006931	0.705212
-36.050363	-2.100291	1.596531	0.006913	0.705224
-36.820386	-2.092471	1.601536	0.007056	0.704964
-37.325305	-2.036098	1.606541	0.007150	0.704896
-36.766613	-2.135600	1.611546	0.007046	0.704896
-37.497682	-2.008079	1.616550	0.007182	0.704891
-37.408620	-2.018953	1.621555	0.007165	0.704901
-37.328915	-2.038813	1.626560	0.007150	0.704890
-37.228889	-2.055127	1.631565	0.007132	0.704893
-37.312502	-2.132759	1.636570	0.007147	0.704707
-38.447091	-1.987487	1.641574	0.007358	0.704592
-37.801101	-2.099647	1.646579	0.007238	0.704598
-38.238924	-2.024276	1.651584	0.007319	0.704593
-38.408350	-1.991324	1.656589	0.007351	0.704599
-37.828747	-2.093780	1.661594	0.007243	0.704601
-38.289511	-2.015133	1.666598	0.007329	0.704594
-38.245152	-2.113404	1.671603	0.007320	0.704412
-38.780216	-2.092424	1.676608	0.007420	0.704262
-38.998218	-2.050853	1.681613	0.007460	0.704267
-39.242261	-2.008239	1.686618	0.007506	0.704266
-39.183922	-2.021383	1.691622	0.007495	0.704260
-38.723485	-2.098692	1.696627	0.007409	0.704270
-39.229878	-2.013146	1.701632	0.007503	0.704261
-39.267613	-2.076115	1.706637	0.007510	0.704120
-39.696197	-2.080502	1.711642	0.007590	0.703958
-39.911133	-2.045823	1.716646	0.007630	0.703950
-39.850984	-2.050893	1.721651	0.007619	0.703962
-39.872142	-2.050446	1.726656	0.007622	0.703955
-39.564313	-2.102606	1.731661	0.007565	0.703961
-40.119002	-2.005082	1.736666	0.007668	0.703958
-40.271355	-2.055169	1.741670	0.007697	0.703803
-40.770583	-2.044217	1.746675	0.007789	0.703645
-40.876566	-2.029498	1.751680	0.007809	0.703637
-40.927396	-2.019699	1.756685	0.007818	0.703639
-40.734351	-2.052638	1.761690	0.007782	0.703642
-40.922291	-2.021183	1.766694	0.007817	0.703638
-40.736515	-2.050468	1.771699	0.007783	0.703646
-40.602304	-2.118971	1.776704	0.007758	0.703556
-41.617156	-2.040541	1.781709	0.007946	0.703349
-41.594349	-2.043946	1.786714	0.007942	0.703351
-41.877255	-1.997493	1.791718	0.007995	0.703343
-41.342236	-2.087529	1.796723	0.007895	0.703354
-41.731232	-2.022513	1.801728	0.007967	0.703345
-41.983662	-1.976081	1.806733	0.008014	0.703348
-41.446670	-2.115360	1.811738	0.007914	0.703260
-42.536077	-2.044955	1.816742	0.008117	0.703010
-42.398390	-2.066136	1.821747	0.008091	0.703017
-42.719371	-2.014399	1.826752	0.008151	0.703006
-42.422310	-2.063527	1.831757	0.008096	0.703014
-42.192950	-2.103213	1.836762	0.008053	0.703017
-42.703796	-2.015235	1.841766	0.008148	0.703011
-42.680357	-2.079477	1.846771	0.008143	0.702890
-43.505893	-2.027272	1.851776	0.008297	0.702698
-43.351019	-2.053566	1.856781	0.008268	0.702701
-43.141381	-2.089854	1.861786	0.008229	0.702703
-43.282207	-2.067603	1.866790	0.008255	0.702697
-43.047657	-2.105359	1.871795	0.008211	0.702706
-43.256546	-2.071863	1.876800	0.008250	0.702698
-43.576457	-2.131153	1.881805	0.008310	0.702463
-44.498218	-2.009090	1.886810	0.008481	0.702378
-44.566841	-1.999169	1.891814	0.008494	0.702373
-43.749039	-2.141060	1.896819	0.008342	0.702382
-44.113177	-2.081159	1.901824	0.008409	0.702372
-44.568738	-1.997857	1.906829	0.008494	0.702376
-44.175264	-2.066881	1.911834	0.008421	0.702378
-44.241330	-2.151190	1.916838	0.008433	0.702184
-45.257511	-2.019565	1.921843	0.008622	0.702084
-45.199411	-2.034202	1.926848	0.008611	0.702076
-44.739931	-2.114339	1.931853	0.008526	0.702079
-44.824500	-2.097408	1.936858	0.008541	0.702083
-45.285091	-2.018648	1.941862	0.008627	0.702077
-45.301943	-2.012594	1.946867	0.008630	0.702083
-45.446231	-2.113573	1.951872	0.008657	0.701827
-46.211642	-2.015597	1.956877	0.008799	0.701749
-46.090208	-2.034776	1.961882	0.008777	0.701754
-45.915370	-2.070686	1.966886	0.008744	0.701745
-46.085283	-2.034530	1.971891	0.008775	0.701757
-46.308487	-2.001597	1.976896	0.008817	0.701743
-45.923403	-2.068667	1.981901	0.008745	0.701746
-46.003143	-2.126507	1.986906	0.008760	0.701601
-47.246902	-1.986518	1.991910	0.008991	0.701435
-46.489303	-2.116381	1.996915	0.008850	0.701446
-46.946562	-2.037974	2.001920	0.008935	0.701440

-46.794238	-2.064816	2.011917	0.008907	0.701441
-46.923837	-2.040045	2.021914	0.008931	0.701444
-47.287843	-2.064777	2.031910	0.008999	0.701263
-47.930890	-1.997574	2.041907	0.009118	0.701167
-47.553105	-2.023529	2.051904	0.009048	0.701251
-47.234315	-2.042395	2.061901	0.008988	0.701329
-47.070830	-2.040899	2.071898	0.008957	0.701391
-46.537979	-2.110114	2.081894	0.008858	0.701444
-47.115886	-2.008157	2.091891	0.008966	0.701442
-46.885207	-2.050821	2.101888	0.008922	0.701439
-46.882867	-2.050422	2.111885	0.008922	0.701441
-46.796338	-2.064454	2.121882	0.008906	0.701444
-46.736313	-2.075690	2.131878	0.008894	0.701443
-46.938200	-2.038996	2.141875	0.008932	0.701445
-46.447308	-2.045032	2.151872	0.008840	0.701610
-46.073291	-2.043917	2.161869	0.008770	0.701748
-46.109040	-2.037808	2.171866	0.008777	0.701747
-45.935488	-2.066272	2.181862	0.008744	0.701753
-46.010897	-2.053363	2.191859	0.008758	0.701752
-45.486975	-1.986535	2.201856	0.008660	0.702077
-45.271588	-2.024271	2.211853	0.008620	0.702078
-45.153937	-2.044158	2.221850	0.008598	0.702081
-45.148591	-2.024787	2.231846	0.008597	0.702122
-44.425705	-2.026884	2.241843	0.008462	0.702379
-44.112602	-2.082850	2.251840	0.008404	0.702379
-44.475460	-2.020243	2.261837	0.008471	0.702375
-44.154346	-2.021907	2.271834	0.008411	0.702488
-43.151453	-2.095617	2.281830	0.008224	0.702700
-43.607990	-2.016621	2.291827	0.008309	0.702696
-43.541476	-2.029555	2.301824	0.008297	0.702694
-43.280329	-1.970189	2.311821	0.008248	0.702908
-42.416624	-2.074335	2.321818	0.008087	0.703009
-42.773599	-2.009880	2.331814	0.008153	0.703011
-42.618164	-2.011278	2.341811	0.008124	0.703065
-41.955866	-1.991282	2.351808	0.008001	0.703344
-41.840337	-2.010786	2.361805	0.007979	0.703346
-41.658696	-2.041379	2.371802	0.007945	0.703350
-41.214327	-2.020026	2.381798	0.007862	0.703554
-40.996401	-2.016513	2.391795	0.007821	0.703639
-40.764742	-2.058266	2.401792	0.007778	0.703639
-40.936806	-1.999245	2.411789	0.007810	0.703696
-39.935536	-2.046742	2.421786	0.007623	0.703961
-40.009380	-2.034153	2.431782	0.007637	0.703960
-39.939293	-2.047763	2.441779	0.007624	0.703958
-39.825681	-1.967823	2.451776	0.007602	0.704160
-39.037400	-2.056596	2.461773	0.007456	0.704265
-38.949301	-2.070433	2.471770	0.007439	0.704269
-38.954633	-2.068430	2.481766	0.007440	0.704272
-38.380917	-2.009820	2.491763	0.007333	0.704596
-37.967262	-2.085794	2.501760	0.007256	0.704592
-38.077927	-2.066411	2.511757	0.007276	0.704592
-37.874649	-2.062738	2.521754	0.007238	0.704672
-37.364803	-2.043851	2.531750	0.007143	0.704894
-37.160253	-2.081312	2.541747	0.007105	0.704892
-37.504150	-2.020319	2.551744	0.007169	0.704892
-36.587858	-2.050053	2.561741	0.006998	0.705161
-36.423447	-2.052651	2.571738	0.006967	0.705215
-36.339369	-2.067048	2.581734	0.006951	0.705217
-36.358017	-2.030380	2.591731	0.006955	0.705284
-35.506821	-2.059572	2.601728	0.006796	0.705531
-35.474345	-2.065470	2.611725	0.006790	0.705531
-35.334164	-2.089982	2.621722	0.006764	0.705532
-35.208839	-2.012979	2.631718	0.006740	0.705733
-34.610562	-2.054078	2.641715	0.006629	0.705865
-34.810379	-2.019545	2.651712	0.006666	0.705863
-34.505849	-2.045961	2.661709	0.006609	0.705919
-33.972132	-2.036635	2.671706	0.006509	0.706130
-33.851662	-2.056117	2.681702	0.006487	0.706134
-33.812360	-2.064436	2.691699	0.006479	0.706132
-33.282291	-2.023636	2.701696	0.006380	0.706404
-32.987291	-2.055444	2.711693	0.006325	0.706446
-32.966004	-2.058842	2.721690	0.006321	0.706447
-32.710820	-2.041013	2.731686	0.006273	0.706575
-32.123177	-2.057023	2.741683	0.006164	0.706753
-32.141839	-2.055479	2.751680	0.006167	0.706750
-32.016769	-2.076906	2.761677	0.006144	0.706752
-31.478887	-2.014372	2.771674	0.006043	0.707070
-31.230849	-2.051447	2.781670	0.005997	0.707085
-31.124777	-2.070032	2.791667	0.005977	0.707086
-31.145141	-1.985246	2.801664	0.005981	0.707249
-30.412578	-2.050506	2.811661	0.005844	0.707381
-30.468128	-2.039703	2.821658	0.005854	0.707383
-30.504263	-2.000200	2.831654	0.005861	0.707449
-29.741571	-2.007751	2.841651	0.005719	0.707707
-29.553169	-2.042642	2.851648	0.005684	0.707705
-29.630572	-2.029737	2.861645	0.005698	0.707703
-29.072013	-1.985700	2.871642	0.005594	0.707992
-28.611043	-2.054200	2.881638	0.005508	0.708019
-28.470616	-2.080503	2.891635	0.005481	0.708017
-28.586797	-2.001721	2.901632	0.005503	0.708134
-27.646981	-2.058790	2.911629	0.005328	0.708355
-27.782133	-2.033957	2.921626	0.005353	0.708357
-27.668736	-2.054508	2.931622	0.005331	0.708357
-27.295231	-2.006410	2.941619	0.005262	0.708587
-27.121062	-2.007873	2.951616	0.005229	0.708647
-26.785865	-2.069546	2.961613	0.005167	0.708643
-26.823803	-2.008555	2.971610	0.005173	0.708752
-26.105732	-2.031661	2.981606	0.005040	0.708962
-25.802013	-2.086866	2.991603	0.004983	0.708960
-26.112193	-2.031079	3.001600	0.005041	0.708962
-25.224305	-2.055677	3.011597	0.004875	0.709229
-25.241711	-2.031915	3.021594	0.004878	0.709271
-24.869489	-2.098701	3.031590	0.004809	0.709270
-25.321810	-1.966322	3.041587	0.004893	0.709374
-24.332813	-2.028889	3.051584	0.004708	0.709602
-24.344181	-2.027911	3.061581	0.004710	0.709600
-24.241177	-2.046061	3.071578	0.004691	0.709601
-23.550929	-2.037185	3.081574	0.004562	0.709865
-23.478229	-2.030983	3.091571	0.004549	0.709904
-23.404287	-2.046025	3.101568	0.004535	0.709900
-23.297535	-2.008878	3.111565	0.004515	0.710013
-22.633284	-2.021170	3.121562	0.004391	0.710225
-22.331290	-2.075322	3.131558	0.004335	0.710225
-22.691840	-2.009861	3.141555	0.004401	0.710228
-21.765395	-2.032538	3.151552	0.004229	0.710512
-21.859591	-2.001431	3.161549	0.004246	0.710541
-21.749064	-2.020763	3.171546	0.004225	0.710542
-21.437279	-1.990515	3.181542	0.004167	0.710714
-20.999654	-1.987205	3.191539	0.004086	0.710877
-20.901892	-2.004575	3.201536	0.004067	0.710877
-20.925854	-1.979478	3.211533	0.004072	0.710919
-20.051481	-2.022127	3.221530	0.003909	0.711145
-19.897326	-2.049467	3.231526	0.003880	0.711146
-20.127460	-2.009396	3.241523	0.003922	0.711144
-19.408606	-2.022535	3.251520	0.003788	0.711374
-19.366724	-1.988121	3.261517	0.003780	0.711458
-19.068805	-2.038879	3.271514	0.003725	0.711463
-18.947334	-2.014720	3.281510	0.003702	0.711554
-18.257499	-2.031080	3.291507	0.003573	0.711767
-18.199066	-2.042148	3.301504	0.003562	0.711766
-18.281615	-2.030803	3.311501	0.003578	0.711760
-17.599703	-2.029058	3.321498	0.003451	0.712006
-17.191985	-2.056132	3.331494	0.003374	0.712097
-17.348513	-2.030394	3.341491	0.003403	0.712093
-17.261026	-2.031466	3.351488	0.003387	0.712122
-16.925038	-1.956377	3.361485	0.003324	0.712391
-16.378550	-2.053724	3.371482	0.003222	0.712392
-16.660672	-2.003535	3.381478	0.003275	0.712392
-15.761069	-2.029425	3.391475	0.003107	0.712660
-15.537397	-2.042658	3.401472	0.003065	0.712713
-15.370606	-2.071420	3.411469	0.003034	0.712715
-15.557520	-2.020141	3.421466	0.003069	0.712751
-14.738411	-2.026355	3.431462	0.002916	0.713030
-14.699483	-2.033203	3.441459	0.002909	0.713030
-14.757874	-2.023538	3.451456	0.002919	0.713029
-14.488650	-1.956441	3.461453	0.002869	0.713258
-13.482948	-2.081698	3.471450	0.002682	0.713366
-13.909196	-2.004542	3.481446	0.002761	0.713369
-13.789065	-2.007864	3.491443	0.002738	0.713405
-13.075731	-2.006963	3.501440	0.002605	0.713660
-13.020687	-2.015698	3.511437	0.002595	0.713662
-12.773953	-2.060702	3.521434	0.002549	0.713660
-12.576588	-1.996810	3.531430	0.002512	0.713858
-12.123935	-2.017995	3.541427	0.002428	0.713976
-12.206769	-2.002602	3.551424	0.002443	0.713978
-11.910451	-2.037016	3.561421	0.002387	0.714014
-11.141715	-2.038193	3.571418	0.002244	0.714285
-11.075839	-2.049603	3.581414	0.002232	0.714285
-11.230737	-2.020469	3.591411	0.002260	0.714289
-10.692106	-2.017626	3.601408	0.002160	0.714485
-10.200547	-2.041196	3.611405	0.002068	0.714613
-10.262338	-2.028961	3.621402	0.002080	0.714615
-10.292485	-2.023464	3.631398	0.002085	0.714616
-9.039927	-2.099354	3.641395	0.001852	0.714909
-9.020918	-2.099857	3.651392	0.001848	0.714915
-8.958885	-2.111093	3.661389	0.001836	0.714915
-8.782400	-2.141456	3.671386	0.001803	0.714917
-8.516650	-2.076090	3.681382	0.001754	0.715141
-8.034314	-2.111382	3.691379	0.001664	0.715242
-8.078026	-2.105241	3.701376	0.001672	0.715239
-8.189749	-2.085569	3.711373	0.001692	0.715239
-7.217014	-2.117306	3.721370	0.001511	0.715520
-7.302634	-2.082148	3.731366	0.001527	0.715559
-6.844954	-2.165271	3.741363	0.001442	0.715556
-7.361875	-2.072445	3.751360	0.001538	0.715558
-6.195647	-2.111963	3.761357	0.001320	0.715892
-5.909330	-2.163657	3.771354	0.001267	0.715891
-6.085646	-2.130550	3.781350	0.001300	0.715895
-6.138977	-2.121555	3.791347	0.001309	0.715894
-5.643268	-2.087317	3.801344	0.001217	0.716137
-5.373864	-2.135644	3.811341	0.001167	0.716137
-5.337286	-2.139743	3.821338	0.001160	0.716142
-5.195725	-2.088385	3.831334	0.001133	0.716294
-4.475321	-2.133906	3.841331	0.000999	0.716458
-4.772773	-2.080882	3.851328	0.001054	0.716458
-4.449770	-2.125850	3.861325	0.000994	0.716484
-3.897566	-2.083603	3.871322	0.000891	0.716762
-3.572198	-2.140315	3.881318	0.000830	0.716765
-3.481120	-2.156842	3.891315	0.000813	0.716765
-3.367024	-2.083109	3.901312	0.000791	0.716951
-2.579440	-2.153027	3.911309	0.000645	0.717091
-2.469807	-2.171910	3.921306	0.000624	0.717092
-2.631562	-2.141909	3.931302	0.000654	0.717095
-2.302094	-2.075511	3.941299	0.000593	0.717343
-2.227189	-2.064503	3.951296	0.000578	0.717391
-1.653422	-2.167225	3.961293	0.000472	0.717390
-1.882158	-2.047133	3.971290	0.000514	0.717548
-1.516052	-2.028448	3.981286	0.000446	0.717714
-1.096466	-2.102170	3.991283	0.000367	0.717716
-1.766221	-1.906787	4.001280	0.000492	0.717867
-1.371799	-1.896349	4.011277	0.000418	0.718026
-1.067528	-1.948901	4.021274	0.000361	0.718030
-0.992050	-1.791208	4.031270	0.000347	0.718368
-0.604053	-1.861279	4.041267	0.000275	0.718367
-0.688247	-1.762940	4.051264	0.000290	0.718532
-0.769545	-1.688016	4.061261	0.000305	0.718651
-1.083155	-1.547883	4.071258	0.000363	0.718818
-0.995345	-1.486417	4.081254	0.000347	0.718970
-0.625122	-1.428124	4.091251	0.000278	0.719216
-0.489211	-1.412263	4.101248	0.000252	0.719295
-0.613641	-1.230600	4.111245	0.000275	0.719610
-0.282982	-1.223864	4.121242	0.000213	0.719740
-0.639158	-1.073132	4.131238	0.000279	0.719912
-0.740809	-0.896183	4.141235	0.000298	0.720225
-0.315458	-0.869704	4.151232	0.000219	0.720427
-0.135362	-0.801076	4.161229	0.000185	0.720626
0.158638	-0.718712	4.171226	0.000130	0.720891
-0.142368	-0.560231	4.181222	0.000186	0.721098
-0.019164	-0.468466	4.191219	0.000163	0.721322
-0.116588	-0.324986	4.201216	0.000180	0.721570
0.006945	-0.211815	4.211213	0.000157	0.721836
0.177780	-0.097469	4.221210	0.000125	0.722121
0.328777	0.007337	4.231206	0.000097	0.722380
0.168525	0.200837	4.241203	0.000126	0.722704
0.000000	0.396764	4.251200	0.000157	0.723030

-0.076563	1.019110	4.256205	0.000171	0.724224
0.102555	2.233415	4.261210	0.000137	0.726661
0.365231	4.041232	4.266214	0.000087	0.730274
0.801435	6.368276	4.271219	0.000004	0.734931
1.207083	9.209920	4.276224	-0.000073	0.740535
1.571364	12.548202	4.281229	-0.000143	0.747026
2.153138	16.294970	4.286234	-0.000254	0.754304
2.556736	20.489348	4.291238	-0.000332	0.762285
2.819397	25.107361	4.296243	-0.000384	0.770919
3.252713	30.055231	4.301248	-0.000468	0.780111
3.820366	35.341216	4.306253	-0.000577	0.789847
4.148100	40.970890	4.311258	-0.000642	0.799998
4.593008	46.894920	4.316262	-0.000729	0.810573
5.079892	53.089228	4.321267	-0.000824	0.821492
5.655403	59.540477	4.326272	-0.000935	0.832731
6.924505	66.100360	4.331277	-0.001176	0.844209
7.543055	73.004213	4.336282	-0.001296	0.855913
8.141097	80.120499	4.341286	-0.001412	0.867799
9.528020	87.291342	4.346291	-0.001675	0.879837
11.098050	94.615275	4.351296	-0.001972	0.892005
12.841827	102.105258	4.356301	-0.002302	0.904317
13.675552	109.900102	4.361306	-0.002462	0.916688
14.439353	117.825082	4.366310	-0.002609	0.929074
15.086348	125.888285	4.371315	-0.002735	0.941473
15.751494	134.044075	4.376320	-0.002864	0.953853
16.572682	142.258494	4.381325	-0.003023	0.966201
17.174725	150.579315	4.386330	-0.003140	0.978491
18.190508	158.916331	4.391334	-0.003335	0.990754
19.233053	167.296989	4.396339	-0.003535	1.002935
19.825875	175.798144	4.401344	-0.003651	1.015028
20.748322	184.284181	4.406349	-0.003828	1.027037
21.777190	192.791771	4.411354	-0.004025	1.038961
22.493344	201.384548	4.416358	-0.004164	1.050791
22.972329	210.041703	4.421363	-0.004259	1.062520
23.894739	218.639318	4.426368	-0.004437	1.074144
24.813963	227.242326	4.431373	-0.004614	1.085648
25.575125	235.885196	4.436378	-0.004761	1.097048
26.250801	244.548486	4.441382	-0.004892	1.108337
27.129098	253.188647	4.446387	-0.005062	1.119527
27.546199	261.888950	4.451392	-0.005145	1.130582
28.187192	270.558098	4.456397	-0.005270	1.141539
28.771649	279.244669	4.461402	-0.005385	1.152400
29.765651	287.826895	4.466406	-0.005576	1.163118
30.622660	296.424599	4.471411	-0.005741	1.173728
31.131620	305.060820	4.476416	-0.005841	1.184218
31.779553	313.679266	4.481421	-0.005968	1.194622
32.138150	322.310916	4.486426	-0.006040	1.204894
32.799123	330.891939	4.491430	-0.006169	1.215079
33.817347	339.401716	4.496435	-0.006364	1.225168
34.225716	348.018839	4.501440	-0.006446	1.235178
34.901758	356.550615	4.506445	-0.006577	1.245061
35.556827	365.083008	4.511450	-0.006705	1.254863
36.240782	373.586266	4.516454	-0.006838	1.264562
37.145259	382.064138	4.521459	-0.007012	1.274200
37.963509	390.513588	4.526464	-0.007170	1.283717
38.955216	398.968291	4.531469	-0.007360	1.293202
39.192859	407.511326	4.536474	-0.007410	1.302575
39.765111	416.067844	4.541478	-0.007522	1.311957
40.522017	424.534270	4.546483	-0.007669	1.321208
41.072128	432.959013	4.551488	-0.007777	1.330314
41.637407	441.393637	4.556493	-0.007888	1.339370
42.222598	449.789119	4.561498	-0.008002	1.348327
43.041488	458.151160	4.566502	-0.008160	1.357231
43.639816	466.530381	4.571507	-0.008277	1.366057
44.067868	474.940738	4.576512	-0.008362	1.374828
44.839085	483.287310	4.581517	-0.008511	1.383536
45.164396	491.706030	4.586522	-0.008578	1.392188
45.757450	500.049263	4.591526	-0.008693	1.400755
46.480306	508.370280	4.596531	-0.008834	1.409269
46.872103	516.740154	4.601536	-0.008912	1.417725
47.309891	525.083949	4.606541	-0.008999	1.426113
47.887464	533.414244	4.611546	-0.009112	1.434461
48.568188	541.706890	4.616550	-0.009244	1.442740
49.053574	550.036685	4.621555	-0.009340	1.450976
49.404119	558.360682	4.626560	-0.009411	1.459139
50.023235	566.649163	4.631565	-0.009532	1.467264
50.502327	575.005494	4.636570	-0.009626	1.475388
50.971110	583.272689	4.641574	-0.009719	1.483380
51.567941	591.543369	4.646579	-0.009836	1.491352
52.222510	599.785317	4.651584	-0.009963	1.499263
52.784056	608.053174	4.656589	-0.010073	1.507143
53.148031	616.364546	4.661594	-0.010146	1.514992
53.655620	624.612319	4.666598	-0.010246	1.522763
53.931272	632.906709	4.671603	-0.010303	1.530503
54.405432	641.157238	4.676608	-0.010397	1.538192
55.006655	649.381091	4.681613	-0.010514	1.545838
55.412944	657.666364	4.686618	-0.010595	1.553473
55.907606	665.883564	4.691622	-0.010693	1.561022
56.513392	674.092153	4.696627	-0.010811	1.568543
57.088875	682.310556	4.701632	-0.010924	1.576032
57.714216	690.518715	4.706637	-0.011046	1.583483
57.927733	698.795215	4.711642	-0.011091	1.590902
58.430998	707.017806	4.716646	-0.011190	1.598279
59.016707	715.210427	4.721651	-0.011305	1.605607
59.202585	723.472733	4.726656	-0.011345	1.612907
59.969830	731.643303	4.731661	-0.011493	1.620175
60.635743	739.826070	4.736666	-0.011622	1.627406
61.152738	748.091417	4.741670	-0.011724	1.634657
61.628174	756.280402	4.746675	-0.011818	1.641803
61.728704	764.512812	4.751680	-0.011842	1.648905
62.373853	772.686624	4.756685	-0.011968	1.656000
62.713172	780.880477	4.761690	-0.012036	1.663040
63.371133	789.035561	4.766694	-0.012164	1.670060
63.788470	797.253662	4.771699	-0.012247	1.677072
64.239502	805.410940	4.776704	-0.012337	1.684007
64.522378	813.626886	4.781709	-0.012395	1.690941
65.072541	821.805726	4.786714	-0.012503	1.697851
65.415299	829.988065	4.791718	-0.012572	1.704708
65.848990	838.197174	4.796723	-0.012658	1.711572
66.254614	846.380508	4.801728	-0.012739	1.718383
66.650962	854.530920	4.806733	-0.012818	1.725139
67.016510	862.717603	4.811738	-0.012892	1.731895
67.587834	870.855580	4.816742	-0.013003	1.738610
68.205386	878.983976	4.821747	-0.013124	1.745298
68.350190	887.194290	4.826752	-0.013156	1.751966
69.016319	895.324711	4.831757	-0.013286	1.758610
69.328823	903.471818	4.836762	-0.013349	1.765198
69.937671	911.626257	4.841766	-0.013468	1.771804
70.162722	919.824747	4.846771	-0.013515	1.778373
70.517490	927.964820	4.851776	-0.013587	1.784888
71.186740	936.126162	4.856781	-0.013717	1.791433
71.666806	944.287273	4.861786	-0.013811	1.797932
71.946808	952.425996	4.866790	-0.013869	1.804365
72.308141	960.587700	4.871795	-0.013942	1.810803
72.451357	968.763380	4.876800	-0.013974	1.817203
73.038642	976.867511	4.881805	-0.014088	1.823578
73.761469	984.959369	4.886810	-0.014228	1.829937
73.990120	993.147273	4.891814	-0.014276	1.836289
74.200683	1001.301146	4.896819	-0.014321	1.842591
74.720057	1009.410584	4.901824	-0.014423	1.848874
75.399671	1017.528307	4.906829	-0.014555	1.855160
75.779699	1025.663151	4.911834	-0.014631	1.861403
76.019639	1033.823792	4.916838	-0.014681	1.867629
76.504131	1041.979603	4.921843	-0.014777	1.873858
76.928015	1050.080637	4.926848	-0.014861	1.880018
77.405796	1058.194845	4.931853	-0.014955	1.886174
77.761669	1066.340962	4.936858	-0.015027	1.892320
78.161836	1074.476009	4.941862	-0.015107	1.898443
78.376766	1082.626689	4.946867	-0.015152	1.904536
78.624066	1090.767201	4.951872	-0.015204	1.910606
79.135304	1098.888289	4.956877	-0.015304	1.916672
79.443819	1106.998314	4.961882	-0.015367	1.922688
79.758219	1115.122091	4.966886	-0.015431	1.928696
80.545049	1123.202370	4.971891	-0.015583	1.934705
80.944062	1131.302319	4.976896	-0.015663	1.940667
81.479140	1139.419802	4.981901	-0.015768	1.946639
81.930945	1147.578830	4.986906	-0.015857	1.952613
82.222978	1155.708554	4.991910	-0.015917	1.958530
82.680039	1163.795597	4.996915	-0.016007	1.964417
82.872151	1171.912294	5.001920	-0.016048	1.970278
83.292648	1180.032175	5.006925	-0.016132	1.976149
83.457358	1188.165250	5.011930	-0.016168	1.981984
83.884649	1196.251217	5.016934	-0.016253	1.987797
84.530421	1204.344415	5.021939	-0.016379	1.993621
84.692600	1212.468910	5.026944	-0.016414	1.999398
84.921246	1220.576270	5.031949	-0.016462	2.005155
85.603172	1228.648788	5.036954	-0.016594	2.010917
85.873362	1236.776685	5.041958	-0.016650	2.016658
86.314025	1244.874316	5.046963	-0.016738	2.022380
86.649048	1252.985538	5.051968	-0.016805	2.028084
86.920831	1261.140849	5.056973	-0.016861	2.033796
87.256989	1269.227340	5.061978	-0.016929	2.039451
87.680583	1277.284054	5.066982	-0.017013	2.045079
88.266776	1285.370946	5.071987	-0.017128	2.050728
88.522948	1293.489877	5.076992	-0.017181	2.056350
88.918290	1301.588874	5.081997	-0.017260	2.061957
89.050060	1309.709466	5.087002	-0.017290	2.067537
89.640258	1317.789938	5.092006	-0.017405	2.073121
90.141264	1325.877682	5.097011	-0.017504	2.078685
90.675974	1333.930209	5.102016	-0.017609	2.084214
90.989189	1342.050275	5.107021	-0.017672	2.089752
91.185986	1350.199761	5.112026	-0.017714	2.095283
91.456266	1358.283176	5.117030	-0.017770	2.100763
91.931095	1366.364886	5.122035	-0.017864	2.106247
92.198666	1374.511213	5.127040	-0.017919	2.111740
92.687979	1382.616450	5.132045	-0.018015	2.117213
92.968605	1390.676146	5.137050	-0.018073	2.122621
93.660399	1398.700621	5.142054	-0.018207	2.128031
94.052325	1406.819428	5.147059	-0.018286	2.133461
94.222294	1414.911527	5.152064	-0.018323	2.138838
94.575591	1422.985143	5.157069	-0.018394	2.144207
94.896689	1431.085300	5.162074	-0.018459	2.149577
95.240932	1439.189598	5.167078	-0.018528	2.154939
95.732654	1447.242832	5.172083	-0.018625	2.160267
95.931798	1455.324509	5.177088	-0.018668	2.165574
96.350281	1463.412019	5.182093	-0.018751	2.170891
96.775822	1471.507403	5.187098	-0.018835	2.176201
96.979196	1479.595168	5.192102	-0.018879	2.181473
97.224531	1487.715061	5.197107	-0.018930	2.186757
97.508185	1495.813591	5.202112	-0.018988	2.192017
98.034164	1503.888409	5.207117	-0.019091	2.197272
98.084064	1511.964254	5.212122	-0.019106	2.202472
98.359371	1520.037270	5.217126	-0.019162	2.207677
99.054532	1528.084008	5.222131	-0.019297	2.212892
99.366497	1536.166316	5.227136	-0.019361	2.218082
99.501918	1544.269470	5.232141	-0.019391	2.223258
99.750159	1552.346831	5.237146	-0.019443	2.228415
100.249553	1560.427484	5.242150	-0.019541	2.233585
100.602426	1568.498769	5.247155	-0.019612	2.238723
100.713737	1576.577705	5.252160	-0.019638	2.243834
101.036345	1584.658172	5.257165	-0.019704	2.248952
101.535896	1592.727743	5.262170	-0.019802	2.254067
101.932750	1600.785644	5.267174	-0.019881	2.259154
102.425022	1608.846541	5.272179	-0.019978	2.264240
102.570801	1616.950305	5.277184	-0.020011	2.269311
102.862012	1625.127758	5.282189	-0.020070	2.274429
103.161443	1633.168307	5.287194	-0.020131	2.279451
103.739551	1641.170041	5.292198	-0.020244	2.284462
104.114660	1649.242930	5.297203	-0.020319	2.289488
104.054673	1657.370536	5.302208	-0.020314	2.294501
104.702865	1665.393678	5.307213	-0.020440	2.299497
105.156057	1673.429904	5.312218	-0.020529	2.304475
105.474063	1681.504094	5.317222	-0.020594	2.309453
105.801454	1689.617640	5.322227	-0.020660	2.314446
106.156929	1697.645314	5.327232	-0.020732	2.319378
106.244348	1705.742714	5.332237	-0.020753	2.324319
106.417012	1713.820647	5.337242	-0.020791	2.329245
106.934099	1721.870613	5.342246	-0.020892	2.334172
107.606171	1729.901207	5.347251	-0.021023	2.339089
107.866415	1737.968172	5.352256	-0.021077	2.343985
108.312248	1746.063399	5.357261	-0.021165	2.348902
108.599764	1754.169995	5.362266	-0.021224	2.353803
108.778709	1762.238569	5.367270	-0.021263	2.358662
109.206240	1770.272739	5.372275	-0.021348	2.363510
109.533374	1778.323078	5.377280	-0.021414	2.368350
109.941437	1786.419851	5.382285	-0.021495	2.373214
110.121539	1794.494778	5.387290	-0.021534	2.378037
110.442368	1802.540852	5.392294	-0.021599	2.382844
110.738347	1810.622525	5.397299	-0.021659	2.387660
111.078864	1818.685483	5.402304	-0.021728	2.392459
111.463915	1826.760791	5.407309	-0.021805	2.397260
112.014140	1834.779698	5.412314	-0.021913	2.402030
112.159147	1842.853309	5.417318	-0.021945	2.406791
112.577542	1850.943234	5.422323	-0.022029	2.411574
113.096927	1858.978543	5.427328	-0.022131	2.416323
113.300574	1867.072273	5.432333	-0.022174	2.421072
113.354697	1875.146624	5.437338	-0.022189	2.425789
113.664743	1883.204626	5.442342	-0.022252	2.430507
114.072252	1891.358395	5.447347	-0.022334	2.435279
114.146307	1899.385631	5.452352	-0.022353	2.439942
114.343224	1907.426197	5.457357	-0.022395	2.444614
114.694231	1915.472912	5.462362	-0.022465	2.449292
115.023557	1923.538897	5.467366	-0.022532	2.453971
115.553790	1931.566044	5.472371	-0.022636	2.458633
115.961257	1939.601134	5.477376	-0.022717	2.463281
116.013089	1947.701241	5.482381	-0.022732	2.467932
116.314559	1955.780400	5.487386	-0.022794	2.472580
116.608351	1963.837961	5.492390	-0.022854	2.477207
117.001778	1971.875684	5.497395	-0.022932	2.481821
117.058422	1979.933510	5.502400	-0.022948	2.486413
117.496840	1987.991320	5.507405	-0.023035	2.491024
117.842266	1996.038336	5.512410	-0.023105	2.495614
117.986241	2004.107578	5.517414	-0.023137	2.500194
118.180284	2012.153483	5.522419	-0.023178	2.504755
118.664270	2020.178896	5.527424	-0.023274	2.509318
119.214420	2028.279004	5.532429	-0.023382	2.513919
119.244743	2036.360503	5.537434	-0.023393	2.518463
119.596880	2044.361470	5.542438	-0.023464	2.522977
119.754013	2052.436197	5.547443	-0.023498	2.527511
119.958697	2060.495715	5.552448	-0.023542	2.532031
120.524642	2068.536690	5.557453	-0.023652	2.536558
120.862771	2076.584028	5.562458	-0.023721	2.541065
121.264671	2084.607719	5.567462	-0.023801	2.545555
121.381238	2092.715463	5.572467	-0.023828	2.550063
121.713218	2100.775436	5.577472	-0.023895	2.554553
122.128704	2108.805929	5.582477	-0.023978	2.559023
122.238663	2116.863205	5.587482	-0.024003	2.563480
122.430365	2124.922875	5.592486	-0.024044	2.567935
122.979902	2132.977550	5.597491	-0.024152	2.572405
123.209301	2141.037816	5.602496	-0.024200	2.576848
123.560678	2149.076349	5.607501	-0.024271	2.581280
123.975765	2157.100973	5.612506	-0.024353	2.585700
124.267940	2165.178670	5.617510	-0.024413	2.590134
124.526024	2173.449365	5.622515	-0.024467	2.594663
124.679437	2181.430659	5.627520	-0.024501	2.599019
125.048895	2189.419291	5.632525	-0.024575	2.603387
125.364702	2197.451832	5.637530	-0.024639	2.607768
125.651550	2205.476002	5.642534	-0.024697	2.612134
125.995839	2213.533251	5.647539	-0.024767	2.616515
126.256423	2221.538749	5.652544	-0.024821	2.620855
126.476256	2229.596614	5.657549	-0.024867	2.625213
126.780553	2237.639036	5.662554	-0.024929	2.629562
127.098557	2245.695312	5.667558	-0.024993	2.633911
127.273170	2253.775997	5.672563	-0.025031	2.638257
127.482459	2261.788560	5.677568	-0.025076	2.642562
127.804416	2269.826548	5.682573	-0.025141	2.646880
128.219052	2277.879135	5.687578	-0.025223	2.651205
128.312132	2285.964681	5.692582	-0.025246	2.655520
128.865482	2293.985108	5.697587	-0.025354	2.659822
128.990568	2302.024420	5.702592	-0.025383	2.664100
129.544039	2310.058947	5.707597	-0.025491	2.668397
129.651782	2318.187888	5.712602	-0.025517	2.672707
129.664710	2326.246908	5.717606	-0.025525	2.676968
130.113822	2334.247184	5.722611	-0.025613	2.681218
130.229503	2342.289937	5.727616	-0.025640	2.685463
130.599206	2350.320868	5.732621	-0.025715	2.689711
130.875581	2358.391993	5.737626	-0.025771	2.693968
131.297256	2366.416920	5.742630	-0.025855	2.698203
131.707076	2374.441805	5.747635	-0.025937	2.702430
132.064878	2382.467191	5.752640	-0.026009	2.706647
132.260382	2390.555808	5.757645	-0.026050	2.710881
132.640884	2398.603974	5.762650	-0.026127	2.715099
132.778243	2406.639756	5.767654	-0.026157	2.719288
133.207159	2414.669035	5.772659	-0.026243	2.723486
133.588496	2422.688286	5.777664	-0.026319	2.727668
133.966883	2430.753002	5.782669	-0.026395	2.731868
133.998542	2438.856821	5.787674	-0.026406	2.736060
134.132659	2446.890810	5.792678	-0.026436	2.740216
134.705101	2454.898193	5.797683	-0.026548	2.744379
135.019218	2462.956937	5.802688	-0.026612	2.748546
135.081776	2471.083764	5.807693	-0.026629	2.752726
135.275417	2479.169882	5.812698	-0.026670	2.756887
135.535126	2487.152065	5.817702	-0.026724	2.760993
135.780271	2495.171192	5.822707	-0.026775	2.765110
135.875891	2503.208228	5.827712	-0.026798	2.769221
136.254687	2511.264742	5.832717	-0.026874	2.773353
136.419866	2519.308624	5.837722	-0.026910	2.777460
136.427254	2527.352098	5.842726	-0.026917	2.781551
136.953745	2535.367007	5.847731	-0.027020	2.785652
137.221930	2543.382609	5.852736	-0.027075	2.789732
137.355810	2551.476819	5.857741	-0.027106	2.793838
137.605561	2559.515909	5.862746	-0.027157	2.797917
137.726793	2567.540813	5.867750	-0.027185	2.801976
138.048365	2575.573020	5.872755	-0.027251	2.806043
138.313618	2583.610490	5.877760	-0.027305	2.810104
138.621909	2591.683414	5.882765	-0.027368	2.814180
138.915031	2599.722645	5.887770	-0.027428	2.818231
139.127527	2607.747276	5.892774	-0.027473	2.822265
139.591223	2615.806115	5.897779	-0.027564	2.826325
139.996848	2623.824638	5.902784	-0.027645	2.830355
140.215630	2631.931739	5.907789	-0.027691	2.834413
140.410133	2639.947377	5.912794	-0.027733	2.838418
140.654210	2647.971989	5.917798	-0.027784	2.842425
141.196037	2655.987674	5.922803	-0.027890	2.846438
141.166722	2664.038385	5.927808	-0.027890	2.850431
141.359834	2672.118243	5.932813	-0.027931	2.854446
141.819159	2680.123512	5.937818	-0.028022	2.858432
142.008999	2688.146386	5.942822	-0.028062	2.862407
142.380806	2696.197527	5.947827	-0.028137	2.866400
142.672547	2704.223395	5.952832	-0.028197	2.870370
142.988360	2712.299132	5.957837	-0.028261	2.874361
143.264478	2720.312483	5.962842	-0.028317	2.878314
143.337201	2728.357050	5.967846	-0.028336	2.882265
143.632680	2736.407773	5.972851	-0.028397	2.886226
143.716114	2744.431260	5.977856	-0.028418	2.890156
144.347964	2752.486334	5.982861	-0.028540	2.894127
144.591259	2760.517564	5.987866	-0.028591	2.898059
144.470658	2768.601180	5.992870	-0.028574	2.901992
144.972177	2776.606160	5.997875	-0.028673	2.905914
145.245018	2784.638961	6.002880	-0.028729	2.909833
145.650138	2792.764177	6.007885	-0.028810	2.913798
145.821130	2800.775442	6.012890	-0.028847	2.917689
146.194024	2808.770314	6.017894	-0.028921	2.921579
146.629688	2816.773090	6.022899	-0.029008	2.925470
146.556550	2824.822008	6.027904	-0.029000	2.929352
146.877856	2832.892559	6.032909	-0.029065	2.933259
147.154425	2840.926986	6.037914	-0.029122	2.937142
147.205841	2848.969900	6.042918	-0.029136	2.941011
147.550851	2856.978748	6.047923	-0.029206	2.944875
147.780349	2865.014657	6.052928	-0.029254	2.948740
147.956334	2873.077431	6.057933	-0.029292	2.952611
148.276132	2881.137413	6.062938	-0.029357	2.956482
148.305317	2889.109767	6.067942	-0.029368	2.960291
148.744220	2897.152730	6.072947	-0.029455	2.964150
148.945962	2905.195663	6.077952	-0.029498	2.967992
149.117022	2913.262251	6.082957	-0.029535	2.971839
149.354401	2921.314585	6.087962	-0.029584	2.975677
149.396379	2929.325776	6.092966	-0.029597	2.979481
149.589199	2937.376734	6.097971	-0.029639	2.983306
149.921114	2945.391746	6.102976	-0.029706	2.987117
150.207686	2953.431213	6.107981	-0.029764	2.990932
150.268834	2961.530660	6.112986	-0.029781	2.994759
150.522556	2969.512924	6.117990	-0.029834	2.998535
151.007295	2977.521609	6.122995	-0.029929	3.002330
151.023622	2985.578474	6.128000	-0.029938	3.006120
151.197208	2993.597154	6.133005	-0.029975	3.009896
151.567551	3001.654742	6.138010	-0.030050	3.013694
151.732083	3009.681463	6.143014	-0.030086	3.017463
152.044264	3017.728329	6.148019	-0.030149	3.021243
152.290300	3025.724800	6.153024	-0.030200	3.024993
152.622002	3033.782017	6.158029	-0.030267	3.028770
153.023569	3041.836889	6.163034	-0.030347	3.032544
153.093768	3049.880522	6.168038	-0.030366	3.036293
153.548794	3057.879052	6.173043	-0.030456	3.040034
153.574995	3065.914276	6.178048	-0.030466	3.043767
153.626184	3073.981066	6.183053	-0.030481	3.047512
154.205465	3081.988223	6.188058	-0.030594	3.051249
154.473591	3090.039334	6.193062	-0.030649	3.054988
154.663309	3098.089527	6.198067	-0.030690	3.058717
155.031045	3106.076033	6.203072	-0.030764	3.062421
155.223557	3114.125444	6.208077	-0.030805	3.066141
155.485482	3122.166845	6.213082	-0.030859	3.069856
155.721669	3130.260130	6.218086	-0.030908	3.073590
156.365281	3138.289582	6.223091	-0.031033	3.077308
156.505574	3146.280427	6.228096	-0.031065	3.080981
156.519867	3154.293565	6.233101	-0.031073	3.084654
156.933670	3162.314363	6.238106	-0.031155	3.088344
157.157584	3170.355125	6.243110	-0.031202	3.092030
157.302208	3178.463481	6.248115	-0.031234	3.095739
157.368384	3186.451112	6.253120	-0.031252	3.099385
157.737522	3194.456401	6.258125	-0.031326	3.103048
158.008488	3202.504455	6.263130	-0.031382	3.106722
158.037788	3210.549048	6.268134	-0.031392	3.110379
158.449122	3218.601763	6.273139	-0.031474	3.114053
158.652453	3226.624823	6.278144	-0.031518	3.117699
158.788331	3234.649555	6.283149	-0.031548	3.121339
159.129306	3242.662154	6.288154	-0.031617	3.124979
159.279999	3250.687070	6.293158	-0.031650	3.128611
159.545390	3258.759989	6.298163	-0.031705	3.132265
159.821577	3266.779738	6.303168	-0.031762	3.135892
160.110469	3274.788943	6.308173	-0.031821	3.139511
160.235217	3282.849942	6.313178	-0.031849	3.143141
160.551542	3290.846748	6.318182	-0.031914	3.146746
160.956639	3298.911118	6.323187	-0.031994	3.150382
161.061954	3306.977815	6.328192	-0.032019	3.154001
161.208643	3315.016338	6.333197	-0.032052	3.157606
161.524128	3323.002422	6.338202	-0.032116	3.161190
161.687335	3330.999808	6.343206	-0.032152	3.164768
161.898291	3339.045165	6.348211	-0.032196	3.168366
161.982132	3347.116880	6.353216	-0.032217	3.171966
162.543223	3355.100193	6.358221	-0.032327	3.175543
162.564506	3363.189330	6.363226	-0.032336	3.179140
162.618242	3371.194507	6.368230	-0.032352	3.182697
162.939335	3379.229018	6.373235	-0.032417	3.186274
163.294383	3387.258926	6.378240	-0.032488	3.189846
163.400390	3395.318790	6.383245	-0.032513	3.193418
163.794989	3403.351268	6.388250	-0.032592	3.196985
163.988736	3411.346785	6.393254	-0.032633	3.200523
164.144758	3419.387384	6.398259	-0.032668	3.204076
164.244243	3427.428123	6.403264	-0.032692	3.207623
164.544108	3435.456903	6.408269	-0.032753	3.211168
164.836879	3443.510300	6.413274	-0.032813	3.214721
164.866160	3451.519102	6.418278	-0.032823	3.218238
165.321035	3459.556863	6.423283	-0.032913	3.221782
165.525466	3467.542861	6.428288	-0.032957	3.225290
165.433367	3475.615844	6.433293	-0.032945	3.228819
165.621912	3483.709512	6.438298	-0.032985	3.232365
166.013051	3491.716200	6.443302	-0.033063	3.235877
166.481987	3499.685230	6.448307	-0.033156	3.239372
166.749276	3507.687389	6.453312	-0.033211	3.242870
167.062490	3515.723533	6.458317	-0.033275	3.246380
167.296902	3523.747736	6.463322	-0.033324	3.249879
167.540605	3531.778420	6.468326	-0.033374	3.253376
167.898844	3539.839828	6.473331	-0.033446	3.256888
168.327740	3547.815035	6.478336	-0.033532	3.260361
168.550157	3555.853068	6.483341	-0.033578	3.263850
168.688946	3563.921841	6.488346	-0.033609	3.267344
168.983188	3571.914410	6.493350	-0.033670	3.270809
168.975841	3580.020988	6.498355	-0.033674	3.274306
169.283689	3588.033229	6.503360	-0.033736	3.277772
169.452330	3596.072413	6.508365	-0.033773	3.281240
169.699107	3604.063083	6.513370	-0.033824	3.284687
169.759981	3612.098526	6.518374	-0.033841	3.288142
170.314218	3620.146465	6.523379	-0.033949	3.291618
170.324772	3628.164903	6.528384	-0.033957	3.295057
170.528704	3636.181113	6.533389	-0.034000	3.298498
170.850923	3644.226707	6.538394	-0.034065	3.301953
171.132124	3652.206325	6.543398	-0.034123	3.305374
171.652994	3660.262454	6.548403	-0.034225	3.308834
171.719648	3668.326990	6.553408	-0.034243	3.312276
171.858030	3676.384857	6.558413	-0.034274	3.315715
172.284110	3684.356228	6.563418	-0.034359	3.319123
172.155920	3692.377872	6.568422	-0.034340	3.322530
172.362631	3700.412295	6.573427	-0.034384	3.325950
172.535551	3708.419023	6.578432	-0.034421	3.329354
172.991519	3716.440396	6.583437	-0.034511	3.332771
173.126727	3724.514258	6.588442	-0.034542	3.336195
173.259700	3732.496997	6.593446	-0.034572	3.339577
173.569175	3740.542149	6.598451	-0.034635	3.342988
173.777063	3748.577043	6.603456	-0.034679	3.346387
174.130898	3756.586941	6.608461	-0.034750	3.349778
174.354840	3764.671871	6.613466	-0.034797	3.353192
174.424043	3772.707876	6.618470	-0.034815	3.356577
174.663515	3780.704821	6.623475	-0.034865	3.359948
174.997317	3788.712302	6.628480	-0.034933	3.363323
175.025411	3796.775538	6.633485	-0.034943	3.366707
175.198318	3804.812286	6.638490	-0.034981	3.370082
175.373310	3812.836863	6.643494	-0.035019	3.373448
175.795692	3820.888264	6.648499	-0.035103	3.376831
176.052555	3828.863955	6.653504	-0.035156	3.380174
176.208969	3836.878545	6.658509	-0.035190	3.383525
176.480632	3844.937198	6.663514	-0.035246	3.386896
176.826270	3852.938613	6.668518	-0.035316	3.390241
177.262603	3861.068120	6.673523	-0.035402	3.393640
177.424357	3869.113887	6.678528	-0.035438	3.396991
177.639812	3877.056457	6.683533	-0.035483	3.400298
177.649176	3885.063056	6.688538	-0.035490	3.403621
177.946094	3893.058277	6.693542	-0.035551	3.406946
178.213808	3901.084977	6.698547	-0.035606	3.410280
178.423480	3909.138021	6.703552	-0.035650	3.413619
178.548859	3917.187074	6.708557	-0.035679	3.416951
178.988199	3925.179807	6.713562	-0.035766	3.420266
179.220109	3933.177743	6.718566	-0.035815	3.423574
179.273236	3941.278407	6.723571	-0.035830	3.426914
179.296626	3949.263498	6.728576	-0.035839	3.430203
179.582973	3957.322298	6.733581	-0.035898	3.433528
179.658532	3965.361236	6.738586	-0.035917	3.436834
179.757920	3973.351260	6.743590	-0.035941	3.440118
180.286783	3981.365471	6.748595	-0.036045	3.443422
180.329886	3989.396099	6.753600	-0.036058	3.446714
180.505659	3997.422293	6.758605	-0.036096	3.450006
180.779092	4005.476708	6.763610	-0.036153	3.453309
181.081358	4013.530559	6.768614	-0.036214	3.456610
181.446546	4021.522986	6.773619	-0.036288	3.459884
181.532135	4029.559094	6.778624	-0.036309	3.463164
181.570424	4037.595104	6.783629	-0.036321	3.466439
181.862050	4045.624147	6.788634	-0.036381	3.469717
182.187119	4053.637557	6.793638	-0.036447	3.472986
182.460827	4061.695764	6.798643	-0.036503	3.476268
182.504135	4069.675084	6.803648	-0.036516	3.479508
182.918245	4077.668370	6.808653	-0.036599	3.482763
182.983651	4085.718830	6.813658	-0.036616	3.486026
183.216584	4093.709073	6.818662	-0.036665	3.489267
183.485523	4101.793679	6.823667	-0.036720	3.492545
183.430409	4109.808980	6.828672	-0.036715	3.495781
183.749943	4117.809792	6.833677	-0.036780	3.499020
184.132805	4125.849714	6.838682	-0.036857	3.502274
184.170628	4133.839232	6.843686	-0.036869	3.505494
184.503552	4141.902806	6.848691	-0.036936	3.508749
184.541463	4149.956911	6.853696	-0.036949	3.511989
184.872831	4157.940956	6.858701	-0.037016	3.515206
185.184822	4165.967409	6.863706	-0.037079	3.518437
185.236120	4174.014107	6.868710	-0.037094	3.521666
185.566608	4181.980098	6.873715	-0.037161	3.524867
185.597118	4190.045523	6.878720	-0.037172	3.528096
185.941785	4198.077590	6.883725	-0.037241	3.531318
186.314972	4206.119715	6.888730	-0.037316	3.534542
186.589788	4214.115672	6.893734	-0.037373	3.537742
186.928587	4222.173762	6.898739	-0.037441	3.540965
187.106494	4230.181539	6.903744	-0.037479	3.544161
187.440633	4238.189765	6.908749	-0.037547	3.547359
187.721456	4246.254869	6.913754	-0.037605	3.550574
187.861547	4254.340939	6.918758	-0.037636	3.553791
188.035244	4262.417774	6.923763	-0.037674	3.557003
188.271567	4270.333598	6.928768	-0.037723	3.560149
188.431882	4278.352742	6.933773	-0.037758	3.563331
188.812274	4286.383602	6.938778	-0.037834	3.566522
188.675838	4294.384398	6.943782	-0.037814	3.569682
189.009330	4302.446672	6.948787	-0.037882	3.572878
189.165628	4310.453197	6.953792	-0.037916	3.576044
189.205505	4318.454705	6.958797	-0.037929	3.579201
189.513982	4326.493118	6.963802	-0.037991	3.582378
189.866952	4334.450753	6.968806	-0.038062	3.585522
190.063351	4342.530739	6.973811	-0.038104	3.588706
190.083116	4350.571005	6.978816	-0.038113	3.591867
190.472941	4358.560231	6.983821	-0.038191	3.595016
190.858303	4366.574474	6.988826	-0.038268	3.598171
190.936066	4374.582643	6.993830	-0.038288	3.601313
190.999166	4382.633170	6.998835	-0.038305	3.604468
191.430991	4390.624939	7.003840	-0.038391	3.607607
191.555411	4398.659819	7.008845	-0.038419	3.610753
191.599587	4406.746558	7.013850	-0.038433	3.613913
191.892492	4414.720625	7.018854	-0.038493	3.617033
192.103439	4422.738654	7.023859	-0.038537	3.620166
192.225655	4430.781911	7.028864	-0.038565	3.623303
192.736354	4438.776444	7.033869	-0.038666	3.626429
192.772435	4446.810854	7.038874	-0.038678	3.629555
193.004188	4454.868491	7.043878	-0.038726	3.632693
193.313305	4462.926293	7.048883	-0.038789	3.635830
193.533965	4470.919962	7.053888	-0.038835	3.638937
193.879124	4478.923360	7.058893	-0.038905	3.642048
194.238282	4486.920716	7.063898	-0.038977	3.645155
194.434627	4494.956282	7.068902	-0.039019	3.648270
194.667047	4503.006875	7.073907	-0.039068	3.651388
194.643476	4511.063121	7.078912	-0.039069	3.654500
194.965725	4519.066570	7.083917	-0.039134	3.657597
195.254200	4527.093798	7.088922	-0.039193	3.660700
195.213890	4535.097251	7.093926	-0.039191	3.663783
195.536054	4543.166040	7.098931	-0.039256	3.666897
195.575852	4551.152600	7.103936	-0.039269	3.669970
195.867840	4559.182815	7.108941	-0.039328	3.673064
196.144148	4567.235614	7.113946	-0.039385	3.676163
196.232629	4575.171756	7.118950	-0.039407	3.679210
196.521210	4583.228490	7.123955	-0.039466	3.682306
196.787478	4591.234074	7.128960	-0.039521	3.685379
196.821013	4599.281238	7.133965	-0.039532	3.688459
196.988411	4607.346048	7.138970	-0.039569	3.691547
197.185694	4615.323377	7.143974	-0.039611	3.694600
197.363722	4623.379008	7.148979	-0.039649	3.697679
197.573791	4631.363221	7.153984	-0.039694	3.700730
197.793532	4639.364975	7.158989	-0.039740	3.703785
198.048306	4647.428612	7.163994	-0.039793	3.706862
198.149996	4655.419368	7.168998	-0.039817	3.709904
198.512543	4663.529938	7.174003	-0.039890	3.712996
198.501886	4671.597945	7.179008	-0.039893	3.716060
198.584198	4679.522715	7.184013	-0.039914	3.719070
198.925891	4687.554538	7.189018	-0.039983	3.722124
199.023997	4695.502924	7.194022	-0.040006	3.725138
199.276111	4703.581790	7.199027	-0.040059	3.728203
199.613116	4711.586982	7.204032	-0.040127	3.731239
199.868444	4719.597329	7.209037	-0.040179	3.734272
200.158869	4727.673330	7.214042	-0.040239	3.737329
200.335151	4735.636507	7.219046	-0.040277	3.740338
200.726731	4743.670763	7.224051	-0.040355	3.743376
200.745993	4751.716391	7.229056	-0.040364	3.746408
201.035671	4759.747821	7.234061	-0.040423	3.749438
201.152083	4767.813913	7.239066	-0.040450	3.752474
201.427039	4775.788843	7.244070	-0.040507	3.755478
201.507335	4783.825358	7.249075	-0.040527	3.758497
201.852540	4791.830701	7.254080	-0.040597	3.761509
201.867328	4799.810903	7.259085	-0.040605	3.764501
201.981149	4807.879889	7.264090	-0.040631	3.767526
202.130205	4815.867361	7.269094	-0.040664	3.770519
202.439746	4823.961062	7.274099	-0.040727	3.773553
202.650556	4831.977037	7.279104	-0.040772	3.776553
202.882824	4839.936316	7.284109	-0.040820	3.779530
203.082704	4848.013557	7.289114	-0.040863	3.782549
203.374365	4855.968780	7.294118	-0.040922	3.785521
203.774452	4864.057331	7.299123	-0.041002	3.788542
203.743368	4872.074564	7.304128	-0.041002	3.791526
203.984883	4880.142658	7.309133	-0.041052	3.794532
204.309154	4888.148576	7.314138	-0.041118	3.797514
204.348506	4896.094183	7.319142	-0.041130	3.800465
204.747479	4904.111915	7.324147	-0.041210	3.803448
204.794689	4912.132791	7.329152	-0.041224	3.806423
205.027108	4920.150184	7.334157	-0.041273	3.809398
205.378088	4928.193330	7.339162	-0.041343	3.812383
205.591727	4936.190813	7.344166	-0.041388	3.815345
205.694376	4944.233030	7.349171	-0.041413	3.818320
205.946166	4952.243527	7.354176	-0.041465	3.821283
206.173360	4960.238047	7.359181	-0.041513	3.824238
206.390424	4968.304650	7.364186	-0.041558	3.827216
206.445094	4976.308745	7.369190	-0.041574	3.830166
206.858962	4984.344806	7.374195	-0.041656	3.833133
206.955836	4992.371798	7.379200	-0.041679	3.836088
207.190459	5000.331966	7.384205	-0.041728	3.839018
207.344980	5008.434557	7.389210	-0.041763	3.841997
207.456834	5016.354377	7.394214	-0.041789	3.844906
207.714598	5024.454510	7.399219	-0.041842	3.847882
207.929699	5032.445739	7.404224	-0.041887	3.850814
207.964533	5040.503302	7.409229	-0.041899	3.853765
208.289982	5048.558128	7.414234	-0.041965	3.856719
208.310160	5056.499087	7.419238	-0.041974	3.859622
208.665073	5064.563953	7.424243	-0.042045	3.862575
208.758808	5072.596974	7.429248	-0.042068	3.865509
208.763539	5080.621210	7.434253	-0.042074	3.868436
209.165884	5088.667203	7.439258	-0.042155	3.871376
209.289618	5096.864634	7.444262	-0.042183	3.874364
209.549459	5104.857853	7.449267	-0.042237	3.877278
209.620552	5112.780397	7.454272	-0.042255	3.880160
209.862760	5120.759199	7.459277	-0.042306	3.883064
210.159389	5128.780808	7.464282	-0.042366	3.885982
210.118886	5136.760716	7.469286	-0.042364	3.888876
210.438012	5144.821802	7.474291	-0.042429	3.891805
210.551424	5152.816973	7.479296	-0.042455	3.894703
210.624611	5160.837483	7.484301	-0.042474	3.897608
210.854031	5168.862045	7.489306	-0.042522	3.900515
211.119747	5176.860602	7.494310	-0.042577	3.903411
211.142925	5184.880161	7.499315	-0.042586	3.906308
211.138522	5192.890647	7.504320	-0.042591	3.909199
211.427513	5200.953735	7.509325	-0.042650	3.912112
211.632364	5208.969133	7.514330	-0.042693	3.915004
211.719061	5216.954845	7.519334	-0.042715	3.917881
212.080413	5224.972686	7.524339	-0.042788	3.920773
212.227383	5232.990765	7.529344	-0.042820	3.923659
212.422209	5241.018532	7.534349	-0.042862	3.926547
212.629145	5249.007339	7.539354	-0.042906	3.929418
213.021205	5257.061761	7.544358	-0.042984	3.932315
213.039554	5265.113581	7.549363	-0.042993	3.935202
213.345248	5273.105015	7.554368	-0.043055	3.938070
213.452261	5281.094610	7.559373	-0.043080	3.940932
213.635417	5289.148372	7.564378	-0.043119	3.943816
213.758565	5297.108780	7.569382	-0.043148	3.946664
213.915466	5305.171307	7.574387	-0.043182	3.949546
214.022381	5313.218560	7.579392	-0.043207	3.952420
214.143474	5321.242154	7.584397	-0.043235	3.955284
214.440520	5329.272051	7.589402	-0.043296	3.958151
214.646553	5337.219243	7.594406	-0.043340	3.960985
215.030256	5345.220916	7.599411	-0.043416	3.963839
215.177143	5353.240483	7.604416	-0.043449	3.966694
215.434813	5361.277435	7.609421	-0.043502	3.969554
215.601321	5369.342119	7.614426	-0.043539	3.972421
215.798251	5377.330332	7.619430	-0.043581	3.975259
216.346699	5385.374234	7.624435	-0.043688	3.978120
216.515156	5393.346380	7.629440	-0.043725	3.980947
216.491526	5401.370959	7.634445	-0.043726	3.983788
216.802346	5409.409910	7.639450	-0.043789	3.986638
216.848454	5417.419905	7.644454	-0.043803	3.989471
216.972981	5425.502804	7.649459	-0.043831	3.992329
216.974400	5433.556383	7.654464	-0.043837	3.995172
217.354020	5441.557231	7.659469	-0.043913	3.998001
217.698282	5449.554854	7.664474	-0.043982	4.000826
217.731847	5457.525928	7.669478	-0.043994	4.003635
217.931168	5465.594676	7.674483	-0.044036	4.006479
218.221562	5473.608444	7.679488	-0.044095	4.009303
218.448405	5481.643202	7.684493	-0.044143	4.012131
218.715590	5489.701539	7.689498	-0.044198	4.014966
218.961322	5497.668764	7.694502	-0.044249	4.017767
219.214380	5505.691196	7.699507	-0.044302	4.020585
219.200813	5513.692488	7.704512	-0.044304	4.023390
219.404459	5521.685644	7.709517	-0.044347	4.026193
219.742777	5529.772419	7.714522	-0.044416	4.029029
219.865325	5537.769709	7.719526	-0.044444	4.031829
220.081047	5545.927719	7.724531	-0.044489	4.034684
220.114154	5553.902569	7.729536	-0.044501	4.037470
220.392637	5561.831572	7.734541	-0.044558	4.040242
220.569100	5569.843786	7.739546	-0.044596	4.043040
220.720305	5577.819671	7.744550	-0.044630	4.045822
220.935194	5585.841535	7.749555	-0.044675	4.048620
220.843110	5593.903126	7.754560	-0.044663	4.051425
221.187509	5601.906729	7.759565	-0.044733	4.054214
221.646947	5609.976919	7.764570	-0.044823	4.057026
221.637021	5617.926185	7.769574	-0.044827	4.059788
221.823025	5625.952175	7.774579	-0.044867	4.062577
222.104365	5633.955655	7.779584	-0.044924	4.065357
222.423206	5641.985773	7.784589	-0.044989	4.068145
222.532373	5650.003683	7.789594	-0.045015	4.070925
222.643461	5658.018931	7.794598	-0.045041	4.073701
222.897167	5666.058496	7.799603	-0.045093	4.076486
223.208666	5674.038189	7.804608	-0.045157	4.079249
223.391253	5682.067293	7.809613	-0.045196	4.082025
223.567262	5690.082299	7.814618	-0.045234	4.084795
223.679551	5698.136046	7.819622	-0.045260	4.087575
223.983654	5706.125514	7.824627	-0.045322	4.090333
224.125575	5714.186489	7.829632	-0.045354	4.093113
224.189690	5722.194265	7.834637	-0.045371	4.095871
224.522149	5730.211014	7.839642	-0.045438	4.098633
224.630371	5738.221710	7.844646	-0.045464	4.101389
224.925820	5746.206352	7.849651	-0.045524	4.104136
225.014917	5754.239570	7.854656	-0.045546	4.106896
225.144940	5762.249429	7.859661	-0.045575	4.109646
225.390492	5770.357941	7.864666	-0.045627	4.112430
225.523923	5778.359479	7.869670	-0.045657	4.115173
225.671834	5786.400552	7.874675	-0.045690	4.117929
225.883929	5794.390016	7.879680	-0.045734	4.120666
226.190656	5802.363237	7.884685	-0.045797	4.123396
226.361491	5810.396973	7.889690	-0.045834	4.126144
226.476003	5818.414361	7.894694	-0.045860	4.128883
226.799322	5826.445338	7.899699	-0.045926	4.131628
226.790378	5834.480603	7.904704	-0.045930	4.134369
226.789886	5842.496170	7.909709	-0.045935	4.137101
227.052053	5850.506123	7.914714	-0.045989	4.139832
227.216738	5858.537681	7.919718	-0.046025	4.142568
227.510917	5866.540816	7.924723	-0.046085	4.145294
227.771436	5874.587242	7.929728	-0.046139	4.148032
227.740330	5882.584608	7.934733	-0.046138	4.150749
228.000415	5890.642734	7.939738	-0.046192	4.153487
228.012218	5898.671326	7.944742	-0.046200	4.156211
228.346018	5906.664104	7.949747	-0.046267	4.158925
228.440951	5914.661840	7.954752	-0.046290	4.161636
228.493740	5922.604423	7.959757	-0.046305	4.164325
228.862524	5930.714452	7.964762	-0.046379	4.167074
228.896997	5938.710616	7.969766	-0.046391	4.169778
229.166822	5946.747842	7.974771	-0.046446	4.172497
229.217216	5954.783588	7.979776	-0.046461	4.175211
229.290384	5962.772046	7.984781	-0.046480	4.177908
229.663680	5970.760834	7.989786	-0.046555	4.180606
229.618124	5978.784798	7.994790	-0.046552	4.183310
229.893040	5986.812270	7.999795	-0.046608	4.186017
230.190019	5994.853652	8.004800	-0.046669	4.188727
230.191773	6002.878846	8.009805	-0.046674	4.191427
230.459714	6010.975380	8.014810	-0.046730	4.194151
230.466802	6018.973692	8.019814	-0.046736	4.196838
230.780070	6026.912059	8.024819	-0.046800	4.199507
230.894579	6034.908130	8.029824	-0.046826	4.202191
231.260629	6042.878565	8.034829	-0.046900	4.204867
231.436249	6050.981982	8.039834	-0.046938	4.207584
231.535405	6058.940957	8.044838	-0.046962	4.210250
231.763050	6066.986183	8.049843	-0.047009	4.212945
231.801878	6075.010406	8.054848	-0.047022	4.215629
231.916516	6082.991789	8.059853	-0.047048	4.218297
232.201323	6091.022952	8.064858	-0.047107	4.220983
232.536216	6098.995241	8.069862	-0.047174	4.223647
232.687708	6107.031263	8.074867	-0.047208	4.226329
232.601147	6115.086648	8.079872	-0.047197	4.229014
232.740996	6123.110807	8.084877	-0.047229	4.231688
232.911253	6131.152395	8.089882	-0.047266	4.234367
232.808197	6139.174766	8.094886	-0.047252	4.237036
233.244914	6147.142327	8.099891	-0.047338	4.239689
233.431250	6155.200800	8.104896	-0.047378	4.242369
233.394910	6163.106826	8.109901	-0.047377	4.244994
233.625940	6171.240183	8.114906	-0.047425	4.247695
233.914801	6179.160726	8.119910	-0.047484	4.250325
234.023468	6187.261576	8.124915	-0.047510	4.253011
234.188588	6195.258651	8.129920	-0.047546	4.255662
234.417030	6203.308196	8.134925	-0.047594	4.258329
234.787220	6211.323369	8.139930	-0.047668	4.260984
234.716107	6219.343645	8.144934	-0.047660	4.263635
235.164075	6227.345330	8.149939	-0.047749	4.266283
235.204043	6235.403110	8.154944	-0.047761	4.268944
235.192617	6243.406662	8.159949	-0.047765	4.271585
235.662863	6251.517813	8.164954	-0.047857	4.274264
236.055326	6259.516781	8.169958	-0.047936	4.276904
236.109130	6267.439045	8.174963	-0.047951	4.279514
236.313380	6275.483966	8.179968	-0.047994	4.282164
236.309976	6283.418387	8.184973	-0.047999	4.284774
236.661471	6291.542978	8.189978	-0.048070	4.287448
236.612728	6299.444624	8.194982	-0.048066	4.290044
236.967630	6307.605985	8.199987	-0.048138	4.292727
237.172822	6315.591461	8.204992	-0.048181	4.295349
237.455960	6323.582972	8.209997	-0.048239	4.297972
237.582665	6331.597348	8.215002	-0.048268	4.300600
237.706112	6339.607224	8.220006	-0.048296	4.303224
238.023104	6347.596723	8.225011	-0.048361	4.305842
238.062994	6355.647014	8.230016	-0.048373	4.308476
238.122452	6363.645471	8.235021	-0.048390	4.311092
238.323412	6371.709763	8.240026	-0.048432	4.313728
238.470536	6379.698956	8.245030	-0.048465	4.316338
238.940161	6387.695708	8.250035	-0.048558	4.318951
238.995443	6395.704386	8.255040	-0.048573	4.321564
239.037193	6403.717267	8.260045	-0.048586	4.324176
239.244979	6411.777572	8.265050	-0.048630	4.326803
239.310789	6419.720139	8.270054	-0.048648	4.329390
239.589839	6427.801342	8.275059	-0.048705	4.332021
239.733733	6435.845179	8.280064	-0.048737	4.334637
239.913867	6443.856697	8.285069	-0.048776	4.337242
240.130307	6451.839697	8.290074	-0.048822	4.339836
240.235596	6459.820133	8.295078	-0.048847	4.342427
240.424116	6467.808578	8.300083	-0.048887	4.345020
240.573778	6475.888362	8.305088	-0.048920	4.347640
240.685955	6483.891873	8.310093	-0.048946	4.350234
240.833644	6491.981524	8.315098	-0.048979	4.352854
241.007844	6500.034124	8.320102	-0.049017	4.355461
241.475403	6508.022472	8.325107	-0.049109	4.358047
241.591047	6515.970987	8.330112	-0.049136	4.360617
241.648659	6523.950431	8.335117	-0.049152	4.363195
241.907848	6531.980354	8.340122	-0.049206	4.365788
242.015669	6539.985902	8.345126	-0.049231	4.368372
242.247295	6548.016348	8.350131	-0.049280	4.370962
242.384825	6556.044568	8.355136	-0.049311	4.373550
242.577582	6564.109629	8.360141	-0.049352	4.376149
242.645313	6572.102123	8.365146	-0.049370	4.378722
242.593493	6580.059605	8.370150	-0.049365	4.381281
243.005136	6588.080125	8.375155	-0.049447	4.383862
243.053314	6596.142582	8.380160	-0.049462	4.386452
243.226194	6604.130989	8.385165	-0.049499	4.389018
243.485367	6612.202571	8.390170	-0.049553	4.391610
243.419695	6620.195536	8.395174	-0.049546	4.394173
243.519479	6628.251958	8.400179	-0.049570	4.396756
243.889708	6636.218353	8.405184	-0.049644	4.399310
244.202459	6644.237226	8.410189	-0.049707	4.401878
244.308596	6652.229844	8.415194	-0.049732	4.404436
244.358552	6660.248496	8.420198	-0.049747	4.407001
244.761880	6668.256930	8.425203	-0.049827	4.409562
244.708165	6676.321730	8.430208	-0.049823	4.412138
244.789886	6684.321808	8.435213	-0.049843	4.414692
245.152517	6692.438143	8.440218	-0.049916	4.417283
245.363158	6700.348947	8.445222	-0.049961	4.419806
245.461132	6708.420737	8.450227	-0.049984	4.422378
245.766000	6716.378795	8.455232	-0.050046	4.424914
245.950166	6724.428501	8.460237	-0.050086	4.427477
246.044382	6732.443869	8.465242	-0.050109	4.430027
246.226365	6740.496177	8.470246	-0.050148	4.432588
246.423541	6748.503887	8.475251	-0.050190	4.435133
246.430355	6756.535361	8.480256	-0.050196	4.437683
246.471832	6764.476577	8.485261	-0.050209	4.440203
246.689610	6772.578732	8.490266	-0.050255	4.442774
246.797343	6780.504719	8.495270	-0.050281	4.445287
246.924561	6788.589773	8.500275	-0.050310	4.447849
247.036749	6796.522899	8.505280	-0.050336	4.450361
247.585043	6804.610604	8.510285	-0.050443	4.452922
247.616832	6812.647664	8.515290	-0.050454	4.455464
247.758845	6820.644670	8.520294	-0.050486	4.457993
247.912326	6828.659009	8.525299	-0.050520	4.460525
248.043973	6836.691058	8.530304	-0.050550	4.463061
248.130138	6844.634181	8.535309	-0.050571	4.465568
248.508172	6852.713553	8.540314	-0.050647	4.468117
248.570661	6860.691813	8.545318	-0.050664	4.470632
248.649656	6868.722025	8.550323	-0.050684	4.473161
248.896827	6876.794912	8.555328	-0.050735	4.475704
249.057275	6884.772060	8.560333	-0.050770	4.478214
249.156992	6892.765229	8.565338	-0.050794	4.480728
249.184572	6900.769536	8.570343	-0.050805	4.483244
249.482954	6908.739225	8.575347	-0.050865	4.485748
249.754410	6916.827127	8.580352	-0.050921	4.488288
249.790921	6924.787297	8.585357	-0.050933	4.490785
250.101885	6932.875189	8.590362	-0.050997	4.493322
250.357146	6940.889502	8.595367	-0.051050	4.495834
250.509378	6948.916177	8.600371	-0.051083	4.498349
250.530017	6956.882555	8.605376	-0.051092	4.500843
250.906848	6964.901677	8.610381	-0.051168	4.503353
251.105775	6972.910712	8.615386	-0.051210	4.505857
251.132006	6980.963454	8.620391	-0.051220	4.508374
251.399525	6988.941110	8.625395	-0.051275	4.510866
251.455400	6997.027709	8.630400	-0.051291	4.513391
251.728160	7005.027412	8.635405	-0.051347	4.515887
251.856003	7013.068598	8.640410	-0.051376	4.518395
251.939668	7021.007347	8.645415	-0.051397	4.520869
252.187281	7029.050815	8.650419	-0.051449	4.523375
252.308029	7037.023307	8.655424	-0.051476	4.525857
252.445439	7045.033265	8.660429	-0.051507	4.528349
252.854691	7053.078443	8.665434	-0.051589	4.530851
252.894053	7061.099916	8.670439	-0.051601	4.533344
253.122165	7069.093766	8.675443	-0.051649	4.535827
253.157653	7077.144273	8.680448	-0.051661	4.538326
253.321616	7085.105075	8.685453	-0.051697	4.540797
253.628932	7093.157307	8.690458	-0.051759	4.543294
253.673234	7101.129486	8.695463	-0.051773	4.545765
253.767226	7109.186498	8.700467	-0.051796	4.548260
253.946972	7117.189168	8.705472	-0.051835	4.550738
254.173565	7125.220343	8.710477	-0.051882	4.553223
254.475444	7133.284043	8.715482	-0.051944	4.555717
254.583586	7141.242726	8.720487	-0.051969	4.558177
255.040424	7149.225012	8.725491	-0.052059	4.560643
255.286080	7157.311481	8.730496	-0.052110	4.563139
255.356480	7165.282460	8.735501	-0.052129	4.565599
255.625810	7173.319111	8.740506	-0.052184	4.568078
255.581191	7181.300071	8.745511	-0.052181	4.570537
255.638517	7189.361170	8.750515	-0.052197	4.573021
255.908749	7197.364470	8.755520	-0.052253	4.575485
256.021994	7205.437369	8.760525	-0.052279	4.577969
256.248063	7213.416076	8.765530	-0.052327	4.580423
256.413264	7221.427665	8.770535	-0.052363	4.582886
256.617511	7229.398879	8.775539	-0.052406	4.585334
256.706787	7237.478252	8.780544	-0.052428	4.587815
256.788033	7245.464354	8.785549	-0.052448	4.590266
257.149159	7253.561612	8.790554	-0.052521	4.592749
257.345442	7261.562552	8.795559	-0.052563	4.595202
257.620818	7269.615772	8.800563	-0.052619	4.597669
257.698260	7277.506107	8.805568	-0.052639	4.600086
257.637526	7285.592379	8.810573	-0.052633	4.602560
257.768037	7293.574916	8.815578	-0.052663	4.605002
257.957918	7301.586322	8.820583	-0.052703	4.607451
258.076478	7309.577462	8.825587	-0.052731	4.609893
258.237799	7317.694636	8.830592	-0.052766	4.612372
258.456870	7325.666964	8.835597	-0.052812	4.614805
258.556071	7333.732442	8.840602	-0.052836	4.617266
258.535618	7341.627921	8.845607	-0.052837	4.619673
258.807968	7349.684930	8.850611	-0.052893	4.622128
258.832274	7357.673988	8.855616	-0.052903	4.624561
259.002276	7365.691234	8.860621	-0.052940	4.627002
259.314006	7373.747046	8.865626	-0.053004	4.629453
259.466952	7381.771876	8.870631	-0.053037	4.631893
259.614723	7389.785577	8.875635	-0.053070	4.634328
259.695129	7397.809504	8.880640	-0.053090	4.636766
259.941982	7405.778621	8.885645	-0.053142	4.639185
259.916605	7413.763340	8.890650	-0.053142	4.641608
260.232309	7421.761800	8.895655	-0.053206	4.644033
260.473822	7429.811657	8.900659	-0.053257	4.646473
260.551493	7437.861020	8.905664	-0.053276	4.648912
260.578307	7445.859761	8.910669	-0.053287	4.651334
260.902896	7453.916711	8.915674	-0.053352	4.653772
260.948463	7461.916778	8.920679	-0.053366	4.656192
261.076333	7469.920418	8.925683	-0.053395	4.658611
261.381574	7477.936450	8.930688	-0.053457	4.661033
261.605400	7485.890154	8.935693	-0.053504	4.663435
261.857460	7493.943392	8.940698	-0.053557	4.665865
261.728680	7501.950049	8.945703	-0.053538	4.668281
261.970547	7509.966168	8.950707	-0.053588	4.670698
262.178384	7518.086837	8.955712	-0.053632	4.673145
262.473376	7526.074533	8.960717	-0.053693	4.675550
262.611235	7534.173292	8.965722	-0.053724	4.677988
262.758768	7542.067807	8.970727	-0.053756	4.680364
263.137793	7550.073941	8.975731	-0.053832	4.682771
263.188912	7558.044571	8.980736	-0.053847	4.685166
263.485782	7566.064794	8.985741	-0.053908	4.687575
263.739096	7574.088934	8.990746	-0.053960	4.689984
263.782749	7582.104216	8.995751	-0.053973	4.692390
264.177316	7590.123334	9.000755	-0.054052	4.694794
264.156968	7598.168305	9.005760	-0.054054	4.697206
264.086849	7606.129455	9.010765	-0.054046	4.699592
264.405872	7614.219978	9.015770	-0.054111	4.702015
264.559850	7622.137051	9.020775	-0.054145	4.704384
264.671649	7630.211228	9.025779	-0.054171	4.706800
265.122675	7638.199793	9.030784	-0.054260	4.709187
265.285151	7646.226447	9.035789	-0.054296	4.711586
265.289011	7654.278734	9.040794	-0.054302	4.713992
265.497947	7662.317285	9.045799	-0.054346	4.716391
265.709437	7670.277378	9.050803	-0.054391	4.718766
265.898978	7678.288459	9.055808	-0.054431	4.721155
265.900329	7686.309054	9.060813	-0.054437	4.723546
266.130261	7694.351864	9.065818	-0.054485	4.725942
266.366947	7702.373761	9.070823	-0.054534	4.728330
266.477608	7710.383742	9.075827	-0.054560	4.730714
266.699649	7718.435796	9.080832	-0.054607	4.733109
266.693266	7726.405411	9.085837	-0.054611	4.735479
267.174563	7734.465573	9.090842	-0.054706	4.737873
267.170928	7742.353998	9.095847	-0.054710	4.740216
267.563492	7750.488771	9.100851	-0.054789	4.742630
267.620312	7758.432246	9.105856	-0.054805	4.744987
267.400155	7766.505773	9.110861	-0.054769	4.747383
267.755005	7774.487295	9.115866	-0.054840	4.749748
268.160823	7782.503099	9.120871	-0.054921	4.752121
268.194934	7790.609995	9.125875	-0.054933	4.754522
268.361576	7798.606708	9.130880	-0.054969	4.756889
268.357264	7806.546087	9.135885	-0.054974	4.759238
268.635800	7814.587210	9.140890	-0.055031	4.761615
268.838975	7822.550078	9.145895	-0.055074	4.763967
268.981441	7830.590116	9.150899	-0.055106	4.766342
269.120916	7838.608802	9.155904	-0.055137	4.768709
269.194955	7846.603086	9.160909	-0.055156	4.771068
269.232002	7854.649523	9.165914	-0.055168	4.773441
269.291344	7862.688665	9.170919	-0.055185	4.775811
269.581749	7870.676994	9.175923	-0.055244	4.778164
269.772357	7878.690137	9.180928	-0.055285	4.780523
270.022091	7886.681706	9.185933	-0.055337	4.782875
270.234342	7894.686282	9.190938	-0.055381	4.785229
270.205431	7902.737823	9.195943	-0.055381	4.787597
270.696762	7910.708133	9.200947	-0.055478	4.789938
271.093605	7918.855333	9.205952	-0.055557	4.792329
271.066745	7926.829710	9.210957	-0.055558	4.794671
271.220522	7934.879055	9.215962	-0.055592	4.797033
271.559916	7942.718380	9.220967	-0.055660	4.799331
271.659880	7950.857885	9.225971	-0.055684	4.801717
271.741707	7958.805118	9.230976	-0.055705	4.804046
271.798380	7966.820841	9.235981	-0.055720	4.806394
272.029528	7974.860627	9.240986	-0.055769	4.808747
272.287850	7982.883586	9.245991	-0.055822	4.811093
272.484245	7990.440777	9.250995	-0.055864	4.813302
272.661930	7995.192311	9.256000	-0.055900	4.814691

272.611107	7997.759950	9.261005	-0.055892	4.815442
272.700876	7999.036924	9.266010	-0.055910	4.815814
272.701311	7999.684264	9.271015	-0.055910	4.816004
272.636042	7999.642499	9.276019	-0.055898	4.815992
272.902577	7999.854562	9.281024	-0.055948	4.816052
273.074975	8000.428135	9.286029	-0.055981	4.816219
273.321303	8000.223223	9.291034	-0.056027	4.816158
273.267004	8000.288480	9.296039	-0.056017	4.816177
273.346734	8000.189514	9.301043	-0.056031	4.816148
273.458353	8000.313325	9.306048	-0.056052	4.816183
273.344328	8000.211919	9.311053	-0.056031	4.816154
273.401870	8000.299498	9.316058	-0.056042	4.816180
273.483685	8000.300987	9.321063	-0.056057	4.816180
273.603087	8000.154667	9.326067	-0.056080	4.816136
273.741079	8000.191358	9.331072	-0.056105	4.816146
273.720576	8000.188857	9.336077	-0.056102	4.816146
273.844276	8000.296864	9.341082	-0.056125	4.816177
273.710564	8000.453624	9.346087	-0.056100	4.816223
273.681704	8000.323847	9.351091	-0.056095	4.816185
273.914467	8000.252222	9.356096	-0.056138	4.816163
273.900866	8000.254120	9.361101	-0.056136	4.816164
273.983571	8000.210757	9.366106	-0.056151	4.816151
273.988776	8000.348668	9.371111	-0.056152	4.816191
274.095399	8000.477734	9.376115	-0.056172	4.816228
274.088197	8000.298137	9.381120	-0.056171	4.816176
273.940210	8000.289055	9.386125	-0.056143	4.816174
274.125741	8000.141795	9.391130	-0.056178	4.816130
274.133220	8000.153689	9.396135	-0.056179	4.816133
274.025147	8000.200880	9.401139	-0.056159	4.816148
274.382654	8000.072758	9.406144	-0.056226	4.816108
274.153923	8000.370949	9.411149	-0.056184	4.816197
274.189362	8000.194262	9.416154	-0.056190	4.816145
274.312070	8000.293706	9.421159	-0.056213	4.816173
274.387353	8000.192521	9.426163	-0.056227	4.816143
274.403115	8000.360537	9.431168	-0.056230	4.816192
274.421747	8000.344857	9.436173	-0.056234	4.816187
274.453226	8000.258903	9.441178	-0.056240	4.816162
274.473011	8000.407763	9.446183	-0.056244	4.816206
274.454463	8000.371112	9.451187	-0.056240	4.816195
274.469165	8000.347883	9.456192	-0.056243	4.816188
274.588313	8000.236809	9.461197	-0.056265	4.816155
274.636806	8000.297520	9.466202	-0.056274	4.816173
274.583273	8000.330743	9.471207	-0.056264	4.816182
274.704386	8000.309442	9.476211	-0.056287	4.816176
274.680392	8000.159454	9.481216	-0.056283	4.816132
274.697498	8000.400139	9.486221	-0.056286	4.816202
274.784431	8000.121826	9.491226	-0.056302	4.816120
274.819964	8000.367119	9.496231	-0.056309	4.816192
274.582673	8000.304070	9.501235	-0.056265	4.816175
274.772141	8000.281871	9.506240	-0.056300	4.816167
274.790347	8000.417884	9.511245	-0.056304	4.816207
274.884345	8000.067054	9.516250	-0.056321	4.816104
274.893734	8000.244569	9.521255	-0.056323	4.816156
275.071949	8000.226439	9.526259	-0.056356	4.816149
274.939893	8000.096927	9.531264	-0.056332	4.816112
275.063882	8000.421810	9.536269	-0.056355	4.816207
275.141957	8000.211706	9.541274	-0.056369	4.816145
275.010464	8000.415515	9.546279	-0.056345	4.816205
274.995493	8000.359699	9.551283	-0.056342	4.816189
275.027765	8000.368838	9.556288	-0.056349	4.816191
275.004891	8000.422915	9.561293	-0.056344	4.816207
275.036976	8000.133992	9.566298	-0.056350	4.816123
275.012578	8000.368585	9.571303	-0.056346	4.816191
275.210907	7999.903201	9.576307	-0.056383	4.816054
275.204536	8000.069747	9.581312	-0.056382	4.816103
275.121579	8000.463527	9.586317	-0.056367	4.816218
275.293000	8000.155761	9.591322	-0.056398	4.816128
275.148651	8000.125377	9.596327	-0.056372	4.816119
275.233995	8000.203849	9.601331	-0.056388	4.816142
275.311112	8000.155043	9.606336	-0.056402	4.816127
275.236387	8000.277621	9.611341	-0.056388	4.816163
275.342934	8000.069102	9.616346	-0.056408	4.816102
275.239113	8000.503102	9.621351	-0.056389	4.816229
275.361708	8000.320511	9.626355	-0.056412	4.816175
275.265770	8000.298482	9.631360	-0.056394	4.816169
275.132364	8000.210607	9.636365	-0.056369	4.816144
275.319713	8000.052694	9.641370	-0.056404	4.816097
275.272671	8000.439648	9.646375	-0.056396	4.816211
275.420150	8000.438055	9.651379	-0.056423	4.816209
275.279804	8000.102204	9.656384	-0.056397	4.816112
275.175873	8000.200750	9.661389	-0.056378	4.816141
275.405403	8000.005142	9.666394	-0.056420	4.816083
275.320902	8000.076264	9.671399	-0.056405	4.816104
275.545025	8000.295063	9.676403	-0.056447	4.816167
275.682597	8000.189663	9.681408	-0.056472	4.816135
275.259909	8000.199105	9.686413	-0.056394	4.816140
275.509647	7999.978224	9.691418	-0.056440	4.816074
275.625484	8000.057248	9.696423	-0.056462	4.816097
275.441645	8000.096658	9.701427	-0.056428	4.816109
275.429104	8000.155195	9.706432	-0.056425	4.816127
275.424062	8000.316427	9.711437	-0.056425	4.816174
275.641817	7999.981724	9.716442	-0.056465	4.816075
275.515698	8000.177085	9.721447	-0.056442	4.816133
275.556219	8000.150050	9.726451	-0.056449	4.816124
275.735776	7999.883028	9.731456	-0.056483	4.816045
275.437074	8000.224825	9.736461	-0.056427	4.816147
275.535417	7999.837751	9.741466	-0.056446	4.816033
275.626016	8000.121432	9.746471	-0.056463	4.816116
275.487348	8000.204393	9.751475	-0.056437	4.816141
275.440735	8000.079631	9.756480	-0.056428	4.816104
275.500935	8000.373449	9.761485	-0.056440	4.816190
275.685970	7999.896067	9.766490	-0.056474	4.816049
275.696579	8000.233854	9.771495	-0.056476	4.816148
275.693508	7999.899424	9.776499	-0.056476	4.816050
275.727062	8000.119043	9.781504	-0.056482	4.816114
275.566273	8000.189851	9.786509	-0.056452	4.816136
275.677019	7999.949358	9.791514	-0.056473	4.816065
275.620247	8000.346819	9.796519	-0.056463	4.816182
275.588757	8000.317411	9.801523	-0.056457	4.816173
275.704319	8000.070594	9.806528	-0.056478	4.816100
275.795984	8000.229306	9.811533	-0.056495	4.816146
275.802393	7999.933506	9.816538	-0.056497	4.816060
275.798118	8000.257136	9.821543	-0.056496	4.816154
275.728082	8000.147974	9.826547	-0.056483	4.816123
275.863708	8000.059632	9.831552	-0.056508	4.816096
275.727043	8000.274032	9.836557	-0.056483	4.816160
275.624571	8000.127959	9.841562	-0.056464	4.816118
275.766245	8000.205317	9.846567	-0.056490	4.816139
275.826458	8000.113471	9.851571	-0.056502	4.816112
275.580840	7999.966943	9.856576	-0.056456	4.816071
275.705124	8000.229871	9.861581	-0.056479	4.816147
276.019972	7999.909747	9.866586	-0.056538	4.816052
275.738162	8000.125790	9.871591	-0.056486	4.816116
275.927256	8000.113199	9.876595	-0.056521	4.816112
276.141123	7999.983541	9.881600	-0.056561	4.816073
275.795263	8000.250773	9.886605	-0.056496	4.816153
275.919818	7999.927200	9.891610	-0.056520	4.816057
275.894684	8000.319894	9.896615	-0.056515	4.816172
275.864369	8000.104619	9.901619	-0.056509	4.816109
275.859540	8000.070353	9.906624	-0.056509	4.816099
275.746175	8000.281971	9.911629	-0.056488	4.816162
276.177000	8000.209661	9.916634	-0.056568	4.816138
275.806634	8000.240348	9.921639	-0.056499	4.816149
275.831283	8000.137175	9.926643	-0.056504	4.816119
275.948609	7999.992949	9.931648	-0.056526	4.816076
275.994601	8000.041864	9.936653	-0.056534	4.816090
275.800295	7999.980662	9.941658	-0.056498	4.816074
275.902367	8000.092555	9.946663	-0.056517	4.816106
275.909439	8000.041412	9.951667	-0.056519	4.816091
275.940069	7999.981080	9.956672	-0.056524	4.816073
275.780747	8000.201480	9.961677	-0.056495	4.816138
275.916994	8000.055459	9.966682	-0.056520	4.816095
275.815530	8000.175417	9.971687	-0.056502	4.816130
275.802048	8000.098261	9.976691	-0.056499	4.816108
275.845031	7999.944142	9.981696	-0.056507	4.816063
275.884674	8000.183103	9.986701	-0.056515	4.816132
275.969945	7999.893004	9.991706	-0.056530	4.816047
275.909314	8000.210272	9.996711	-0.056519	4.816140
276.073622	8000.145953	10.001715	-0.056550	4.816120
276.192759	8000.067995	10.006720	-0.056572	4.816097
276.173874	8000.336881	10.011725	-0.056569	4.816176
276.225539	7999.985275	10.016730	-0.056578	4.816073
275.914621	8000.156990	10.021735	-0.056521	4.816124
276.034113	7999.917723	10.026739	-0.056543	4.816054
276.230939	7999.941594	10.031744	-0.056580	4.816060
275.981526	7999.943493	10.036749	-0.056533	4.816062
275.951245	7999.898083	10.041754	-0.056528	4.816049
275.901490	8000.207001	10.046759	-0.056519	4.816139
276.055266	7999.925622	10.051763	-0.056547	4.816056
275.915629	7999.956217	10.056768	-0.056521	4.816066
275.911994	8000.209351	10.061773	-0.056521	4.816140
276.161212	7999.972433	10.066778	-0.056567	4.816069
276.023162	8000.058610	10.071783	-0.056542	4.816095
275.878244	7999.906428	10.076787	-0.056515	4.816051
276.038225	7999.910402	10.081792	-0.056545	4.816052
276.059522	8000.091341	10.086797	-0.056549	4.816104
276.033852	7999.956275	10.091802	-0.056544	4.816065
275.944775	8000.167265	10.096807	-0.056528	4.816127
276.099961	7999.872023	10.101811	-0.056556	4.816040
276.237564	8000.087119	10.106816	-0.056582	4.816102
276.170859	8000.253646	10.111821	-0.056570	4.816151
276.218714	7999.987439	10.116826	-0.056579	4.816073
276.128844	8000.050986	10.121831	-0.056562	4.816092
276.265098	7999.895350	10.126835	-0.056587	4.816046
276.319728	7999.924124	10.131840	-0.056598	4.816054
276.326254	8000.171034	10.136845	-0.056599	4.816126
276.413734	7999.983532	10.141850	-0.056615	4.816071
276.173289	8000.133022	10.146855	-0.056571	4.816116
276.367723	8000.054291	10.151859	-0.056607	4.816092
276.410795	7999.911924	10.156864	-0.056615	4.816050
276.255142	8000.162304	10.161869	-0.056586	4.816124
276.288690	8000.038993	10.166874	-0.056593	4.816088
276.279895	8000.127513	10.171879	-0.056591	4.816114
276.114674	8000.109570	10.176883	-0.056560	4.816109
276.265322	7999.965947	10.181888	-0.056588	4.816067
276.223553	8000.261125	10.186893	-0.056581	4.816153
276.397493	7999.989723	10.191898	-0.056613	4.816073
276.349930	8000.128820	10.196903	-0.056605	4.816114
276.270193	8000.141271	10.201907	-0.056590	4.816118
276.348347	8000.058297	10.206912	-0.056604	4.816093
276.225204	8000.234484	10.211917	-0.056582	4.816145
276.485862	7999.865300	10.216922	-0.056630	4.816036
276.359562	7999.902547	10.221927	-0.056607	4.816048
276.319443	8000.100536	10.226931	-0.056599	4.816106
276.377516	8000.051385	10.231936	-0.056610	4.816091
276.433931	7999.944513	10.236941	-0.056621	4.816059
276.232825	7999.954765	10.241946	-0.056583	4.816064
276.084689	8000.033281	10.246951	-0.056556	4.816087
276.246800	7999.885593	10.251955	-0.056586	4.816043
276.275547	7999.981202	10.256960	-0.056591	4.816071
276.180822	7999.957058	10.261965	-0.056574	4.816064
276.158958	7999.857316	10.266970	-0.056570	4.816035
276.069780	8000.097148	10.271975	-0.056553	4.816106
276.199029	8000.034330	10.276979	-0.056578	4.816087
276.278669	7999.975954	10.281984	-0.056592	4.816069
276.190879	7999.998943	10.286989	-0.056576	4.816077
276.333477	7999.924615	10.291994	-0.056603	4.816054
276.201429	7999.897659	10.296999	-0.056578	4.816047
276.198669	7999.803605	10.302003	-0.056578	4.816020
276.247866	8000.074788	10.307008	-0.056587	4.816099
276.288724	8000.116133	10.312013	-0.056595	4.816110
276.503957	7999.813431	10.317018	-0.056635	4.816021
276.608683	7999.990542	10.322023	-0.056655	4.816072
276.420009	7999.832223	10.327027	-0.056619	4.816027
276.202901	7999.900943	10.332032	-0.056579	4.816048
276.399491	8000.074376	10.337037	-0.056616	4.816098
276.538709	7999.820508	10.342042	-0.056642	4.816023
276.262708	7999.904186	10.347047	-0.056590	4.816049
276.324598	7999.946979	10.352051	-0.056602	4.816061
276.456482	7999.932283	10.357056	-0.056627	4.816056
276.429419	7999.940347	10.362061	-0.056622	4.816058
276.389857	7999.986644	10.367066	-0.056614	4.816072
276.467563	8000.173950	10.372071	-0.056629	4.816126
276.537993	8000.082289	10.377075	-0.056642	4.816099
276.551573	8000.087884	10.382080	-0.056645	4.816101
276.357248	8000.159153	10.387085	-0.056609	4.816123
276.534732	7999.848288	10.392090	-0.056642	4.816031
276.466504	8000.142987	10.397095	-0.056629	4.816117
276.579125	7999.943120	10.402099	-0.056650	4.816058
276.675258	7999.895727	10.407104	-0.056668	4.816044
276.369362	7999.994887	10.412109	-0.056611	4.816074
276.596582	7999.807782	10.417114	-0.056654	4.816019
276.679741	7999.926812	10.422119	-0.056669	4.816053
276.475263	7999.889996	10.427123	-0.056631	4.816043
276.397667	7999.912101	10.432128	-0.056617	4.816050
276.439199	7999.978029	10.437133	-0.056625	4.816069
276.429426	7999.806928	10.442138	-0.056623	4.816019
276.511746	7999.970812	10.447143	-0.056638	4.816067
276.403567	7999.808611	10.452147	-0.056618	4.816020
276.641113	7999.912277	10.457152	-0.056663	4.816049
276.435797	7999.972664	10.462157	-0.056625	4.816068
276.604334	7999.935129	10.467162	-0.056656	4.816056
276.493588	8000.057056	10.472167	-0.056635	4.816092
276.514986	7999.969848	10.477171	-0.056639	4.816066
276.599528	7999.903014	10.482176	-0.056655	4.816046
276.623546	7999.972899	10.487181	-0.056660	4.816067
276.550234	7999.886111	10.492186	-0.056646	4.816042
276.624987	7999.869312	10.497191	-0.056660	4.816036
276.610274	7999.881873	10.502195	-0.056658	4.816040
276.783261	7999.912792	10.507200	-0.056690	4.816048
276.622625	7999.917367	10.512205	-0.056660	4.816050
276.566488	7999.916357	10.517210	-0.056650	4.816050
276.648823	7999.993708	10.522215	-0.056665	4.816073
276.688558	8000.086313	10.527219	-0.056673	4.816099
276.803822	7999.872605	10.532224	-0.056694	4.816036
276.583233	7999.985064	10.537229	-0.056653	4.816070
276.718305	7999.852909	10.542234	-0.056678	4.816031
276.519356	8000.025586	10.547239	-0.056641	4.816083
276.579637	8000.041643	10.552243	-0.056653	4.816087
276.422145	8000.143493	10.557248	-0.056624	4.816118
276.498159	8000.133126	10.562253	-0.056638	4.816114
276.534323	8000.063279	10.567258	-0.056645	4.816094
276.710742	8000.101739	10.572263	-0.056677	4.816104
276.715590	7999.952268	10.577267	-0.056678	4.816060
276.571349	7999.860990	10.582272	-0.056652	4.816034
276.487826	8000.109474	10.587277	-0.056636	4.816107
276.621135	7999.927075	10.592282	-0.056661	4.816053
276.574433	8000.022386	10.597287	-0.056652	4.816081
276.800134	7999.954906	10.602291	-0.056695	4.816060
276.813119	7999.928440	10.607296	-0.056697	4.816053
276.714963	8000.128585	10.612301	-0.056679	4.816112
276.826704	7999.880627	10.617306	-0.056700	4.816039
276.806802	8000.021294	10.622311	-0.056696	4.816080
276.670200	8000.135275	10.627315	-0.056671	4.816114
276.655528	7999.911734	10.632320	-0.056668	4.816049
276.720479	7999.970609	10.637325	-0.056680	4.816065
276.898888	7999.926843	10.642330	-0.056713	4.816052
276.840517	7999.987756	10.647335	-0.056703	4.816070
276.613222	8000.047744	10.652339	-0.056661	4.816089
276.738063	8000.106637	10.657344	-0.056684	4.816105
276.805361	8000.131368	10.662349	-0.056697	4.816112
276.646704	7999.952224	10.667354	-0.056667	4.816060
276.769404	7999.926678	10.672359	-0.056690	4.816052
276.807253	7999.929508	10.677363	-0.056697	4.816053
276.728449	7999.937703	10.682368	-0.056682	4.816056
276.688124	8000.186971	10.687373	-0.056675	4.816129
276.718895	7999.839258	10.692378	-0.056681	4.816027
276.875722	7999.883772	10.697383	-0.056710	4.816039
276.593833	7999.972685	10.702387	-0.056658	4.816067
276.684334	7999.925189	10.707392	-0.056675	4.816052
276.579546	8000.163674	10.712397	-0.056655	4.816123
276.773729	7999.834948	10.717402	-0.056691	4.816025
276.753234	7999.890137	10.722407	-0.056688	4.816042
276.910046	7999.901533	10.727411	-0.056717	4.816044
277.089248	7999.900515	10.732416	-0.056750	4.816043
276.605788	8000.102223	10.737421	-0.056661	4.816104
276.600689	7999.890608	10.742426	-0.056659	4.816043
276.736174	8000.134515	10.747431	-0.056685	4.816113
276.633567	7999.892287	10.752435	-0.056666	4.816043
276.803769	8000.000076	10.757440	-0.056698	4.816074
276.795130	8000.028772	10.762445	-0.056696	4.816082
276.753187	7999.879521	10.767450	-0.056688	4.816039
276.893926	7999.894899	10.772455	-0.056715	4.816042
276.812517	8000.018427	10.777459	-0.056700	4.816079
276.736597	7999.958300	10.782464	-0.056685	4.816062
276.820246	8000.079477	10.787469	-0.056701	4.816097
276.814050	7999.859295	10.792474	-0.056700	4.816032
276.777276	7999.999656	10.797479	-0.056693	4.816074
276.728321	8000.065014	10.802483	-0.056684	4.816093
276.851219	7999.967893	10.807488	-0.056707	4.816064
276.666659	8000.138695	10.812493	-0.056673	4.816115
276.840857	7999.913235	10.817498	-0.056705	4.816048
276.786042	8000.081047	10.822503	-0.056695	4.816097
276.794232	8000.032059	10.827507	-0.056697	4.816083
276.843447	8000.036164	10.832512	-0.056706	4.816084
276.833944	8000.147107	10.837517	-0.056705	4.816116
276.970820	8000.008574	10.842522	-0.056730	4.816075
277.021584	8000.258428	10.847527	-0.056740	4.816148
276.815321	8000.140382	10.852531	-0.056701	4.816114
276.789504	7999.852539	10.857536	-0.056696	4.816030
276.833331	8000.220850	10.862541	-0.056705	4.816138
276.959907	7999.903717	10.867546	-0.056728	4.816045
277.009133	8000.009314	10.872551	-0.056738	4.816075
276.796055	7999.847346	10.877555	-0.056698	4.816029
277.013445	7999.916461	10.882560	-0.056739	4.816048
277.056474	7999.981349	10.887565	-0.056747	4.816067
276.811147	7999.848710	10.892570	-0.056701	4.816029
276.909088	7999.928481	10.897575	-0.056719	4.816052
276.975379	7999.956398	10.902579	-0.056732	4.816060
277.137961	7999.831152	10.907584	-0.056762	4.816022
277.168221	7999.831708	10.912589	-0.056768	4.816022
276.981097	7999.851828	10.917594	-0.056733	4.816029
277.191635	7999.984920	10.922599	-0.056772	4.816067
277.168075	7999.995184	10.927603	-0.056768	4.816070
277.161917	7999.906408	10.932608	-0.056767	4.816044
277.120102	8000.005013	10.937613	-0.056759	4.816073
277.083310	8000.016106	10.942618	-0.056753	4.816077
277.025177	7999.911430	10.947623	-0.056742	4.816046
276.962514	8000.083374	10.952627	-0.056730	4.816097
277.042431	7999.945945	10.957632	-0.056745	4.816056
277.161078	8000.052801	10.962637	-0.056767	4.816087
277.016126	7999.857880	10.967642	-0.056740	4.816031
276.817465	8000.172653	10.972647	-0.056704	4.816124
276.960003	7999.935935	10.977651	-0.056730	4.816054
276.982137	7999.855150	10.982656	-0.056734	4.816030
276.864405	8000.146818	10.987661	-0.056713	4.816116
276.929509	7999.974933	10.992666	-0.056725	4.816065
276.933853	8000.111768	10.997671	-0.056726	4.816105
276.960198	8000.033195	11.002675	-0.056731	4.816082
276.955148	8000.009608	11.007680	-0.056730	4.816075
277.028412	8000.201110	11.012685	-0.056744	4.816131
276.937346	7999.947336	11.017690	-0.056726	4.816057
276.976075	8000.177740	11.022695	-0.056734	4.816124
277.114010	7999.878974	11.027699	-0.056759	4.816036
277.287659	7999.907769	11.032704	-0.056792	4.816044
277.076082	8000.087698	11.037709	-0.056753	4.816098
277.147478	7999.937294	11.042714	-0.056766	4.816053
277.153034	8000.034622	11.047719	-0.056767	4.816082
277.083334	7999.971402	11.052723	-0.056754	4.816064
277.029606	7999.783477	11.057728	-0.056744	4.816009
276.940290	8000.010490	11.062733	-0.056728	4.816076
277.056707	8000.028633	11.067738	-0.056750	4.816080
276.918256	8000.027199	11.072743	-0.056724	4.816081
276.734040	8000.174504	11.077747	-0.056690	4.816125
276.983535	8000.023056	11.082752	-0.056736	4.816079
276.958483	8000.332432	11.087757	-0.056732	4.816170
276.781534	8000.140132	11.092762	-0.056699	4.816114
276.943831	7999.909114	11.097767	-0.056729	4.816046
277.041412	7999.919437	11.102771	-0.056747	4.816049
276.961698	7999.910522	11.107776	-0.056732	4.816046
276.928289	7999.920607	11.112781	-0.056726	4.816049
276.970325	7999.834841	11.117786	-0.056734	4.816024
277.008235	8000.029974	11.122791	-0.056741	4.816081
276.956633	7999.870932	11.127795	-0.056732	4.816035
277.149424	7999.797513	11.132800	-0.056768	4.816012
277.072825	8000.268342	11.137805	-0.056754	4.816150
276.957598	7999.844263	11.142810	-0.056732	4.816027
277.112202	8000.044716	11.147815	-0.056761	4.816085
277.084963	7999.938464	11.152819	-0.056756	4.816054
277.134365	7999.889155	11.157824	-0.056765	4.816039
277.221093	7999.961245	11.162829	-0.056782	4.816060
277.251824	7999.789806	11.167834	-0.056787	4.816010
277.155947	7999.877817	11.172839	-0.056770	4.816036
277.151376	7999.874537	11.177843	-0.056769	4.816035
277.249533	7999.854956	11.182848	-0.056787	4.816029
277.143390	7999.837015	11.187853	-0.056767	4.816024
277.001021	7999.862219	11.192858	-0.056741	4.816032
276.963065	7999.876496	11.197863	-0.056734	4.816036
277.115221	7999.833322	11.202867	-0.056762	4.816023
277.169327	7999.914436	11.207872	-0.056773	4.816046
277.168963	7999.989221	11.212877	-0.056773	4.816068
277.123581	7999.879435	11.217882	-0.056764	4.816036
277.027528	7999.875565	11.222887	-0.056746	4.816036
276.970750	7999.855314	11.227891	-0.056736	4.816030
277.164679	7999.905843	11.232896	-0.056772	4.816044
276.999594	7999.961617	11.237901	-0.056742	4.816061
277.074272	7999.876442	11.242906	-0.056755	4.816036
277.162841	7999.871645	11.247911	-0.056772	4.816034
277.157773	8000.047838	11.252915	-0.056771	4.816085
277.164706	7999.991349	11.257920	-0.056773	4.816069
276.936079	8000.020331	11.262925	-0.056730	4.816079
277.255864	7999.876566	11.267930	-0.056790	4.816035
277.279309	8000.057550	11.272935	-0.056794	4.816088
277.093199	8000.042432	11.277939	-0.056760	4.816084
277.141432	7999.915112	11.282944	-0.056769	4.816047
277.223502	8000.023442	11.287949	-0.056784	4.816078
277.105690	7999.866404	11.292954	-0.056762	4.816033
277.126148	8000.017419	11.297959	-0.056766	4.816077
277.071740	7999.956613	11.302963	-0.056756	4.816059
277.200079	7999.869206	11.307968	-0.056780	4.816033
277.178163	8000.031205	11.312973	-0.056776	4.816080
277.359274	7999.874243	11.317978	-0.056810	4.816034
277.171207	7999.961651	11.322983	-0.056775	4.816060
277.048475	8000.222248	11.327987	-0.056752	4.816137
277.162312	8000.004239	11.332992	-0.056773	4.816073
277.172456	8000.040754	11.337997	-0.056775	4.816083
277.031453	8000.042479	11.343002	-0.056749	4.816084
277.197157	8000.148052	11.348007	-0.056780	4.816114
277.300681	8000.009982	11.353011	-0.056799	4.816074
277.420847	7999.982254	11.358016	-0.056822	4.816065
277.239759	7999.924493	11.363021	-0.056788	4.816049
277.270045	7999.887658	11.368026	-0.056794	4.816038
277.308343	7999.971691	11.373031	-0.056801	4.816062
277.009108	7999.941702	11.378035	-0.056745	4.816055
277.220132	7999.876092	11.383040	-0.056785	4.816035
277.161582	8000.235074	11.388045	-0.056774	4.816140
277.344833	7999.855932	11.393050	-0.056808	4.816028
277.263450	8000.046768	11.398055	-0.056793	4.816084
277.248599	7999.904415	11.403059	-0.056790	4.816043
277.248436	7999.884122	11.408064	-0.056790	4.816037
277.254460	7999.907742	11.413069	-0.056792	4.816044
277.119815	7999.874327	11.418074	-0.056767	4.816035
277.155460	8000.027754	11.423079	-0.056773	4.816079
277.138599	7999.890708	11.428083	-0.056770	4.816040
277.283839	7999.854887	11.433088	-0.056797	4.816028
277.381406	8000.004096	11.438093	-0.056816	4.816071
277.432603	7999.830890	11.443098	-0.056825	4.816020
277.370128	8000.136383	11.448103	-0.056814	4.816110
277.349771	7999.882821	11.453107	-0.056810	4.816036
277.416885	7999.915027	11.458112	-0.056823	4.816045
277.216460	7999.865463	11.463117	-0.056785	4.816032
277.216246	7999.845168	11.468122	-0.056785	4.816026
277.504703	7999.894207	11.473127	-0.056839	4.816039
277.434158	7999.863022	11.478131	-0.056826	4.816030
277.351165	7999.832680	11.483136	-0.056811	4.816021
277.484864	7999.905621	11.488141	-0.056836	4.816042
277.432013	7999.879031	11.493146	-0.056826	4.816035
277.449402	7999.799227	11.498151	-0.056829	4.816011
277.319822	8000.025513	11.503155	-0.056805	4.816078
277.421852	7999.902373	11.508160	-0.056824	4.816041
277.250730	7999.991157	11.513165	-0.056793	4.816068
277.396707	7999.789756	11.518170	-0.056820	4.816009
277.217072	7999.953169	11.523175	-0.056786	4.816057
277.280695	8000.009884	11.528179	-0.056798	4.816074
277.536627	7999.808340	11.533184	-0.056846	4.816013
277.334332	7999.911515	11.538189	-0.056808	4.816045
277.351085	7999.946014	11.543194	-0.056812	4.816054
277.322334	7999.777770	11.548199	-0.056806	4.816005
277.267335	7999.968014	11.553203	-0.056796	4.816061
277.334853	7999.862411	11.558208	-0.056809	4.816030
277.168144	8000.037811	11.563213	-0.056778	4.816082
277.265070	7999.883596	11.568218	-0.056796	4.816037
277.361405	7999.920606	11.573223	-0.056814	4.816047
277.224092	7999.871117	11.578227	-0.056789	4.816033
277.210543	7999.895451	11.583232	-0.056786	4.816040
277.205695	7999.903917	11.588237	-0.056785	4.816043
277.234203	7999.888416	11.593242	-0.056791	4.816038
277.323735	7999.945601	11.598247	-0.056807	4.816054
277.254712	7999.875983	11.603251	-0.056795	4.816035
277.496967	7999.929526	11.608256	-0.056840	4.816049
277.424000	7999.826718	11.613261	-0.056826	4.816019
277.321012	7999.910326	11.618266	-0.056807	4.816044
277.312976	7999.901641	11.623271	-0.056806	4.816042
277.353399	7999.872468	11.628275	-0.056813	4.816033
277.275998	7999.831544	11.633280	-0.056799	4.816021
277.268250	7999.890170	11.638285	-0.056798	4.816039
277.331667	8000.057990	11.643290	-0.056810	4.816087
277.246324	7999.883378	11.648295	-0.056794	4.816037
277.266779	7999.885893	11.653299	-0.056798	4.816037
277.513875	7999.903199	11.658304	-0.056844	4.816041
277.556024	7999.830255	11.663309	-0.056852	4.816020
277.284386	7999.872346	11.668314	-0.056801	4.816033
277.535450	7999.886519	11.673319	-0.056848	4.816036
277.267213	7999.944697	11.678323	-0.056798	4.816054
277.380740	7999.845270	11.683328	-0.056819	4.816025
277.210761	8000.019542	11.688333	-0.056788	4.816077
277.351147	7999.888551	11.693338	-0.056814	4.816038
277.394115	7999.843398	11.698343	-0.056822	4.816024
277.247031	7999.898430	11.703347	-0.056795	4.816041
277.393749	7999.874389	11.708352	-0.056822	4.816033
277.379692	7999.961746	11.713357	-0.056820	4.816059
277.329374	7999.772813	11.718362	-0.056810	4.816004
277.505070	7999.920231	11.723367	-0.056843	4.816046
277.239270	7999.963497	11.728371	-0.056794	4.816060
277.515287	7999.899065	11.733376	-0.056845	4.816040
277.414275	7999.874806	11.738381	-0.056826	4.816033
277.518043	7999.899130	11.743386	-0.056846	4.816040
277.511028	7999.838114	11.748391	-0.056845	4.816022
277.492902	7999.890142	11.753395	-0.056841	4.816037
277.548557	7999.887954	11.758400	-0.056852	4.816036
277.393225	7999.919333	11.763405	-0.056823	4.816046
277.245582	7999.789531	11.768410	-0.056795	4.816009
277.354881	7999.962455	11.773415	-0.056816	4.816059
277.503647	7999.817727	11.778419	-0.056844	4.816016
277.616475	7999.925547	11.783424	-0.056865	4.816047
277.357193	7999.768081	11.788429	-0.056817	4.816002
277.389444	7999.888327	11.793434	-0.056823	4.816037
277.573568	7999.888467	11.798439	-0.056857	4.816036
277.341475	7999.912045	11.803443	-0.056814	4.816045
277.426886	7999.836680	11.808448	-0.056830	4.816022
277.533550	7999.886696	11.813453	-0.056850	4.816036
277.501016	7999.863679	11.818458	-0.056844	4.816030
277.533476	7999.946538	11.823463	-0.056850	4.816054
277.504968	7999.813553	11.828467	-0.056845	4.816015
277.453251	7999.897023	11.833472	-0.056835	4.816040
277.537922	8000.033178	11.838477	-0.056851	4.816079
277.712775	7999.822684	11.843482	-0.056884	4.816016
277.652502	7999.842966	11.848487	-0.056872	4.816023
277.578731	7999.887576	11.853491	-0.056859	4.816036
277.628219	7999.881002	11.858496	-0.056868	4.816034
277.778965	7999.911520	11.863501	-0.056896	4.816042
277.698199	7999.858782	11.868506	-0.056881	4.816027
277.639509	7999.920758	11.873511	-0.056870	4.816045
277.608981	7999.863590	11.878515	-0.056865	4.816029
277.686724	7999.920561	11.883520	-0.056879	4.816045
277.504974	7999.864925	11.888525	-0.056846	4.816030
277.729493	7999.820926	11.893530	-0.056887	4.816016
277.626367	7999.944062	11.898535	-0.056868	4.816052
277.345417	7999.989189	11.903539	-0.056816	4.816067
277.550693	7999.844417	11.908544	-0.056854	4.816024
277.435763	7999.874391	11.913549	-0.056833	4.816033
277.454922	7999.835217	11.918554	-0.056837	4.816021
277.512692	7999.842682	11.923559	-0.056848	4.816023
277.562667	7999.951499	11.928563	-0.056857	4.816055
277.640757	7999.804421	11.933568	-0.056872	4.816011
277.546792	7999.967252	11.938573	-0.056854	4.816059
277.624658	7999.876792	11.943578	-0.056869	4.816033
277.553907	7999.956712	11.948583	-0.056856	4.816056
277.688505	7999.982664	11.953587	-0.056881	4.816063
277.889207	7999.894431	11.958592	-0.056918	4.816036
277.641557	7999.916658	11.963597	-0.056872	4.816044
277.710568	7999.788646	11.968602	-0.056885	4.816006
277.678376	7999.930161	11.973607	-0.056879	4.816048
277.689298	7999.811779	11.978611	-0.056881	4.816013
277.831720	7999.825052	11.983616	-0.056908	4.816016
277.622351	7999.905664	11.988621	-0.056869	4.816041
277.814996	7999.866430	11.993626	-0.056905	4.816029
277.815261	7999.888878	11.998631	-0.056905	4.816035
277.535554	7999.908387	12.003635	-0.056853	4.816042
277.556431	7999.902363	12.008640	-0.056857	4.816040
277.646857	7999.965974	12.013645	-0.056874	4.816059
277.724817	7999.818894	12.018650	-0.056889	4.816015
277.676378	7999.878919	12.023655	-0.056880	4.816033
277.492719	7999.837137	12.028659	-0.056846	4.816022
277.705056	7999.912573	12.033664	-0.056885	4.816043
277.682574	7999.876918	12.038669	-0.056881	4.816032
277.804597	7999.768028	12.043674	-0.056904	4.816000
277.762984	7999.883732	12.048679	-0.056896	4.816034
277.662276	8000.004775	12.053683	-0.056878	4.816070
277.774354	7999.862586	12.058688	-0.056898	4.816028
277.994259	7999.931751	12.063693	-0.056939	4.816047
277.931838	7999.847294	12.068698	-0.056928	4.816022
277.621482	7999.948511	12.073703	-0.056870	4.816054
277.776530	7999.819922	12.078707	-0.056899	4.816015
277.835804	7999.824209	12.083712	-0.056910	4.816016
277.545529	7999.928995	12.088717	-0.056856	4.816048
277.572742	7999.789542	12.093722	-0.056861	4.816007
277.771858	7999.967301	12.098727	-0.056899	4.816058
277.714718	7999.856231	12.103731	-0.056888	4.816026
277.685578	7999.843959	12.108736	-0.056883	4.816023
277.731934	7999.811688	12.113741	-0.056891	4.816013
277.699437	7999.949993	12.118746	-0.056885	4.816054
277.581809	7999.800435	12.123751	-0.056864	4.816010
277.718988	7999.911901	12.128755	-0.056889	4.816042
277.926479	7999.837680	12.133760	-0.056928	4.816020
277.761525	7999.930850	12.138765	-0.056897	4.816048
277.679292	7999.833214	12.143770	-0.056882	4.816020
277.667499	7999.842623	12.148775	-0.056880	4.816022
277.774136	7999.892640	12.153779	-0.056900	4.816036
277.768461	7999.808144	12.158784	-0.056899	4.816012
277.822141	7999.839039	12.163789	-0.056909	4.816020
277.857939	7999.903797	12.168794	-0.056916	4.816039
277.564658	7999.841865	12.173799	-0.056861	4.816023
277.675008	7999.841736	12.178803	-0.056882	4.816022
277.826907	7999.954539	12.183808	-0.056910	4.816054
277.696117	8000.017345	12.188813	-0.056886	4.816073
277.663029	7999.860772	12.193818	-0.056880	4.816028
277.790489	7999.927192	12.198823	-0.056904	4.816046
277.957394	7999.869329	12.203827	-0.056935	4.816029
277.893862	7999.862843	12.208832	-0.056923	4.816027
277.744360	7999.927447	12.213837	-0.056895	4.816047
277.887594	7999.798643	12.218842	-0.056922	4.816008
277.943837	7999.838131	12.223847	-0.056933	4.816020
277.712714	7999.936511	12.228851	-0.056890	4.816049
277.935433	7999.860429	12.233856	-0.056931	4.816026
277.595761	7999.833980	12.238861	-0.056868	4.816020
277.772060	7999.929062	12.243866	-0.056901	4.816047
277.766378	7999.891574	12.248871	-0.056900	4.816036
277.664853	7999.856623	12.253875	-0.056881	4.816026
277.873425	7999.877505	12.258880	-0.056920	4.816031
277.823811	7999.831742	12.263885	-0.056911	4.816018
277.716808	7999.835152	12.268890	-0.056891	4.816020
277.908570	7999.965771	12.273895	-0.056927	4.816057
277.901892	7999.898350	12.278899	-0.056926	4.816037
277.945747	7999.861760	12.283904	-0.056934	4.816026
277.827778	7999.794459	12.288909	-0.056912	4.816007
277.562091	8000.000117	12.293914	-0.056863	4.816069
277.611803	7999.839704	12.298919	-0.056872	4.816022
277.657690	7999.828791	12.303923	-0.056880	4.816018
277.864725	7999.929772	12.308928	-0.056919	4.816047
277.850604	7999.833372	12.313933	-0.056917	4.816019
277.911753	7999.825941	12.318938	-0.056928	4.816016
277.877995	7999.935377	12.323943	-0.056922	4.816048
277.835637	7999.800004	12.328947	-0.056914	4.816009
277.882977	7999.928004	12.333952	-0.056923	4.816046
277.669031	7999.909176	12.338957	-0.056883	4.816042
277.664935	7999.815094	12.343962	-0.056882	4.816014
277.922545	7999.905240	12.348967	-0.056931	4.816039
277.921843	7999.791989	12.353971	-0.056930	4.816006
277.919608	7999.884903	12.358976	-0.056930	4.816033
277.874283	7999.931097	12.363981	-0.056922	4.816047
278.002109	7999.870389	12.368986	-0.056946	4.816029
277.946683	7999.860845	12.373991	-0.056935	4.816026
277.678585	7999.916888	12.378995	-0.056886	4.816044
278.006929	7999.805329	12.384000	-0.056947	4.816010
277.832593	7999.996618	12.389005	-0.056914	4.816066
277.743691	7999.850785	12.394010	-0.056898	4.816024
277.622410	7999.809065	12.399015	-0.056875	4.816013
277.738539	7999.894509	12.404019	-0.056897	4.816037
277.961471	7999.884670	12.409024	-0.056939	4.816033
277.954097	7999.896295	12.414029	-0.056937	4.816036
277.925504	7999.832751	12.419034	-0.056932	4.816018
277.931782	7999.948256	12.424039	-0.056933	4.816052
277.676745	7999.873128	12.429043	-0.056886	4.816031
277.908756	7999.919008	12.434048	-0.056929	4.816043
277.950796	7999.824693	12.439053	-0.056937	4.816015
277.811522	7999.848885	12.444058	-0.056911	4.816023
277.848383	7999.857039	12.449063	-0.056918	4.816025
277.869485	7999.884138	12.454067	-0.056922	4.816033
277.896081	7999.846167	12.459072	-0.056927	4.816022
277.786517	7999.862350	12.464077	-0.056907	4.816027
277.998784	7999.905736	12.469082	-0.056947	4.816039
278.009287	7999.854652	12.474087	-0.056949	4.816024
277.774163	7999.801253	12.479091	-0.056905	4.816010
277.820253	7999.949530	12.484096	-0.056914	4.816053
277.822085	7999.898289	12.489101	-0.056914	4.816038
277.907361	7999.801553	12.494106	-0.056930	4.816009
277.928550	7999.863910	12.499111	-0.056934	4.816027
278.013212	7999.912460	12.504115	-0.056950	4.816041
278.142678	7999.877422	12.509120	-0.056974	4.816030
277.865512	7999.859585	12.514125	-0.056922	4.816026
277.929764	7999.804134	12.519130	-0.056934	4.816010
278.083081	7999.968244	12.524135	-0.056963	4.816057
277.967536	7999.821928	12.529139	-0.056942	4.816015
278.060316	7999.894129	12.534144	-0.056959	4.816035
278.106286	7999.852236	12.539149	-0.056968	4.816023
278.010390	7999.923153	12.544154	-0.056950	4.816044
277.821709	7999.901578	12.549159	-0.056915	4.816039
278.002199	7999.877080	12.554163	-0.056949	4.816030
278.032181	7999.881905	12.559168	-0.056954	4.816032
277.782155	7999.834645	12.564173	-0.056908	4.816019
277.793534	7999.855158	12.569178	-0.056910	4.816025
277.806863	7999.790237	12.574183	-0.056912	4.816006
277.900493	7999.911598	12.579187	-0.056930	4.816041
277.742667	7999.899129	12.584192	-0.056901	4.816038
277.916994	7999.876657	12.589197	-0.056933	4.816031
278.117782	7999.898467	12.594202	-0.056971	4.816036
278.049883	7999.867329	12.599207	-0.056958	4.816027
277.966467	7999.882918	12.604211	-0.056943	4.816032
277.951904	7999.815355	12.609216	-0.056940	4.816013
277.834534	7999.831397	12.614221	-0.056918	4.816018
277.930488	7999.939980	12.619226	-0.056936	4.816049
277.821538	7999.870706	12.624231	-0.056916	4.816030
277.904905	7999.862609	12.629235	-0.056932	4.816027
277.781361	7999.898838	12.634240	-0.056909	4.816038
277.861910	7999.902443	12.639245	-0.056924	4.816039
277.811768	7999.775475	12.644250	-0.056914	4.816002
277.982899	7999.969822	12.649255	-0.056946	4.816058
277.765532	7999.895376	12.654259	-0.056906	4.816037
277.960011	7999.848697	12.659264	-0.056942	4.816022
277.988418	7999.914389	12.664269	-0.056948	4.816041
277.790399	7999.753758	12.669274	-0.056911	4.815995
277.872768	7999.926196	12.674279	-0.056926	4.816045
277.870405	7999.860991	12.679283	-0.056926	4.816026
278.079790	7999.814582	12.684288	-0.056965	4.816012
278.092464	7999.929134	12.689293	-0.056967	4.816045
278.148325	7999.868189	12.694298	-0.056978	4.816027
277.911723	7999.907710	12.699303	-0.056934	4.816040
277.734800	7999.775239	12.704307	-0.056901	4.816002
277.855794	7999.945172	12.709312	-0.056924	4.816051
278.015263	7999.878627	12.714317	-0.056953	4.816031
277.902342	7999.858425	12.719322	-0.056933	4.816025
277.947508	7999.859252	12.724327	-0.056941	4.816025
277.900798	7999.829567	12.729331	-0.056932	4.816017
278.016511	7999.876543	12.734336	-0.056954	4.816030
278.052365	8000.007542	12.739341	-0.056961	4.816068
278.056016	7999.766165	12.744346	-0.056961	4.815998
277.967100	7999.916268	12.749351	-0.056945	4.816042
277.786978	8000.061513	12.754355	-0.056912	4.816085
278.145825	7999.887473	12.759360	-0.056978	4.816033
278.061609	7999.937235	12.764365	-0.056963	4.816048
278.083066	7999.885282	12.769370	-0.056967	4.816032
278.272845	7999.826765	12.774375	-0.057002	4.816014
278.216914	7999.894134	12.779379	-0.056992	4.816034
278.085210	7999.828720	12.784384	-0.056968	4.816016
278.196272	7999.939715	12.789389	-0.056988	4.816048
278.201996	7999.794528	12.794394	-0.056989	4.816005
278.238239	7999.844337	12.799399	-0.056996	4.816020
277.818796	7999.862381	12.804403	-0.056918	4.816027
278.134247	7999.856356	12.809408	-0.056977	4.816024
278.155742	7999.868505	12.814413	-0.056981	4.816027
277.855373	7999.915417	12.819418	-0.056925	4.816042
278.030863	7999.949589	12.824423	-0.056958	4.816051
277.940352	7999.904152	12.829427	-0.056941	4.816039
278.029902	7999.791468	12.834432	-0.056958	4.816005
278.103390	7999.956268	12.839437	-0.056972	4.816053
278.154981	7999.872810	12.844442	-0.056981	4.816028
278.198968	7999.888572	12.849447	-0.056990	4.816033
278.162201	7999.877230	12.854451	-0.056983	4.816030
278.011864	7999.836050	12.859456	-0.056955	4.816018
278.128475	7999.843514	12.864461	-0.056977	4.816020
278.074195	7999.918391	12.869466	-0.056967	4.816042
278.185301	7999.822124	12.874471	-0.056988	4.816013
278.176984	7999.856168	12.879475	-0.056986	4.816023
278.199818	7999.882230	12.884480	-0.056990	4.816031
278.220711	7999.931762	12.889485	-0.056994	4.816045
278.294808	7999.802772	12.894490	-0.057008	4.816007
278.178202	7999.840195	12.899495	-0.056987	4.816019
277.904995	7999.896146	12.904499	-0.056936	4.816036
278.194856	7999.843717	12.909504	-0.056990	4.816020
278.332724	7999.885754	12.914509	-0.057016	4.816031
278.147643	7999.890953	12.919514	-0.056981	4.816034
278.259311	7999.873754	12.924519	-0.057002	4.816028
278.132607	7999.794542	12.929523	-0.056979	4.816005
278.009519	7999.835053	12.934528	-0.056956	4.816018
277.938416	7999.955565	12.939533	-0.056943	4.816054
278.137535	7999.788244	12.944538	-0.056980	4.816004
278.090051	7999.889954	12.949543	-0.056971	4.816034
278.058860	7999.924652	12.954547	-0.056965	4.816044
278.173884	7999.801746	12.959552	-0.056987	4.816007
278.287551	7999.932019	12.964557	-0.057008	4.816045
278.171894	7999.802793	12.969562	-0.056987	4.816008
278.151411	7999.922087	12.974567	-0.056983	4.816043
278.028203	7999.877126	12.979571	-0.056960	4.816030
278.180280	7999.766644	12.984576	-0.056988	4.815997
278.052413	7999.900015	12.989581	-0.056965	4.816037
278.195805	7999.868435	12.994586	-0.056991	4.816027
278.138448	7999.849241	12.999591	-0.056981	4.816021
277.960687	7999.806496	13.004595	-0.056948	4.816010
278.083020	7999.908079	13.009600	-0.056971	4.816039
278.134173	7999.859869	13.014605	-0.056980	4.816025
278.205199	7999.800268	13.019610	-0.056994	4.816007
278.159496	7999.969317	13.024615	-0.056985	4.816056
278.200491	7999.776694	13.029619	-0.056993	4.816000
278.260353	7999.882486	13.034624	-0.057004	4.816030
277.906345	7999.805564	13.039629	-0.056938	4.816010
277.967506	7999.899628	13.044634	-0.056950	4.816037
278.221451	7999.861505	13.049639	-0.056997	4.816025
278.209156	7999.901887	13.054643	-0.056995	4.816036
278.178336	7999.838302	13.059648	-0.056989	4.816018
278.013651	7999.906905	13.064653	-0.056959	4.816039
277.942065	7999.783821	13.069658	-0.056945	4.816003
278.116283	7999.934422	13.074663	-0.056978	4.816046
278.276560	7999.898874	13.079667	-0.057008	4.816035
278.175671	7999.824403	13.084672	-0.056989	4.816014
277.987866	7999.837031	13.089677	-0.056954	4.816019
278.157686	7999.836913	13.094682	-0.056986	4.816018
278.214382	7999.941580	13.099687	-0.056997	4.816048
278.042018	7999.809190	13.104691	-0.056964	4.816010
278.290436	7999.853231	13.109696	-0.057011	4.816022
278.337330	7999.898960	13.114701	-0.057020	4.816035
278.287502	7999.831825	13.119706	-0.057010	4.816015
278.339038	7999.891528	13.124711	-0.057020	4.816033
278.331473	7999.897809	13.129715	-0.057019	4.816035
278.274348	7999.857250	13.134720	-0.057008	4.816023
278.093185	7999.940511	13.139725	-0.056975	4.816048
278.118265	7999.841615	13.144730	-0.056979	4.816019
278.221104	7999.846692	13.149735	-0.056999	4.816020
277.998551	8000.003989	13.154739	-0.056957	4.816067
278.150505	7999.891367	13.159744	-0.056986	4.816034
278.095775	7999.855126	13.164749	-0.056975	4.816023
278.058885	7999.841645	13.169754	-0.056969	4.816020
278.119218	7999.820310	13.174759	-0.056980	4.816013
278.302538	7999.967872	13.179763	-0.057014	4.816055
278.483338	7999.809834	13.184768	-0.057048	4.816008
278.162903	7999.916210	13.189773	-0.056988	4.816041
278.176194	7999.772229	13.194778	-0.056991	4.815999
278.336670	7999.964248	13.199783	-0.057021	4.816054
278.086621	7999.811218	13.204787	-0.056974	4.816010
278.278712	7999.840349	13.209792	-0.057010	4.816018
278.322755	7999.907394	13.214797	-0.057018	4.816037
278.252969	7999.853786	13.219802	-0.057006	4.816022
278.132695	7999.868707	13.224807	-0.056983	4.816027
278.211647	7999.887240	13.229811	-0.056998	4.816032
278.335817	7999.823260	13.234816	-0.057021	4.816013
278.158899	7999.854248	13.239821	-0.056988	4.816023
278.125209	7999.907063	13.244826	-0.056982	4.816038
278.152328	7999.891536	13.249831	-0.056987	4.816034
278.406374	7999.817091	13.254835	-0.057035	4.816010
278.537685	7999.808796	13.259840	-0.057059	4.816007
278.482522	7999.941350	13.264845	-0.057049	4.816046
278.339471	7999.779576	13.269850	-0.057022	4.816000
278.367003	7999.900809	13.274855	-0.057028	4.816035
278.348671	7999.854544	13.279859	-0.057024	4.816022
278.489424	7999.903044	13.284864	-0.057051	4.816035
278.347003	7999.838503	13.289869	-0.057024	4.816017
278.285708	7999.761545	13.294874	-0.057013	4.815995
278.252842	7999.968221	13.299879	-0.057007	4.816055
278.172828	7999.827889	13.304883	-0.056992	4.816015
278.187762	7999.865560	13.309888	-0.056995	4.816026
278.268656	7999.883060	13.314893	-0.057010	4.816030
278.413537	7999.860054	13.319898	-0.057037	4.816023
278.379705	7999.878679	13.324903	-0.057031	4.816029
278.215911	7999.939819	13.329907	-0.057000	4.816047
278.259231	7999.854074	13.334912	-0.057008	4.816022
278.304535	7999.867723	13.339917	-0.057017	4.816026
278.300264	7999.921072	13.344922	-0.057016	4.816041
278.477771	7999.887974	13.349927	-0.057049	4.816031
278.428602	7999.864654	13.354931	-0.057040	4.816024
278.431134	7999.875391	13.359936	-0.057041	4.816027
278.377048	7999.872281	13.364941	-0.057031	4.816027
278.414343	7999.823819	13.369946	-0.057038	4.816012
278.405360	7999.846100	13.374951	-0.057036	4.816019
278.053979	7999.871787	13.379955	-0.056971	4.816028
278.367551	7999.826199	13.384960	-0.057029	4.816013
278.251454	7999.920255	13.389965	-0.057008	4.816041
278.150853	7999.898139	13.394970	-0.056989	4.816035
278.350598	7999.866512	13.399975	-0.057027	4.816025
278.377549	7999.861667	13.404979	-0.057032	4.816024
278.328010	7999.914195	13.409984	-0.057023	4.816039
278.214846	7999.896125	13.414989	-0.057002	4.816035
278.431210	7999.854115	13.419994	-0.057042	4.816021
278.504025	7999.874674	13.424999	-0.057055	4.816027
278.125657	7999.871026	13.430003	-0.056985	4.816028
278.367983	7999.956624	13.435008	-0.057030	4.816051
278.429756	7999.860529	13.440013	-0.057042	4.816023
278.370012	7999.872274	13.445018	-0.057031	4.816027
278.350726	7999.866590	13.450023	-0.057027	4.816025
278.257078	7999.766610	13.455027	-0.057010	4.815996
278.281736	7999.893132	13.460032	-0.057015	4.816033
278.401045	7999.810901	13.465037	-0.057037	4.816009
278.245391	7999.904240	13.470042	-0.057008	4.816037
278.500844	7999.861871	13.475047	-0.057056	4.816023
278.360398	7999.809119	13.480051	-0.057030	4.816008
278.486343	7999.911837	13.485056	-0.057053	4.816038
278.305810	7999.972674	13.490061	-0.057020	4.816056
278.364193	7999.797458	13.495066	-0.057030	4.816005
278.455895	7999.855752	13.500071	-0.057048	4.816021
278.479156	7999.864729	13.505075	-0.057052	4.816024
278.402335	7999.822745	13.510080	-0.057038	4.816012
278.246819	7999.966300	13.515085	-0.057009	4.816055
278.262464	7999.771079	13.520090	-0.057012	4.815998
278.364379	7999.860541	13.525095	-0.057031	4.816023
278.205828	7999.935665	13.530099	-0.057002	4.816046
278.367976	7999.769810	13.535104	-0.057032	4.815997
278.310878	7999.961089	13.540109	-0.057021	4.816053
278.296894	7999.787767	13.545114	-0.057019	4.816002
278.438643	7999.940985	13.550119	-0.057045	4.816046
278.358510	7999.827360	13.555123	-0.057030	4.816014
278.239516	7999.888244	13.560128	-0.057008	4.816032
278.330218	7999.880281	13.565133	-0.057025	4.816029
278.500050	7999.876958	13.570138	-0.057057	4.816027
278.567101	7999.889934	13.575143	-0.057070	4.816031
278.403733	7999.874158	13.580147	-0.057039	4.816027
278.486633	7999.872464	13.585152	-0.057055	4.816026
278.557108	7999.925032	13.590157	-0.057068	4.816041
278.383785	7999.789418	13.595162	-0.057036	4.816002
278.361502	7999.891585	13.600167	-0.057032	4.816032
278.384715	7999.959321	13.605171	-0.057036	4.816052
278.397662	7999.846316	13.610176	-0.057039	4.816019
278.376119	7999.938881	13.615181	-0.057035	4.816046
278.489804	7999.906762	13.620186	-0.057056	4.816036
278.431032	7999.872584	13.625191	-0.057045	4.816026
278.321050	7999.918675	13.630195	-0.057025	4.816040
278.411775	7999.851951	13.635200	-0.057042	4.816020
278.467823	7999.849770	13.640205	-0.057052	4.816020
278.468300	7999.796367	13.645210	-0.057052	4.816004
278.333907	7999.945647	13.650215	-0.057027	4.816048
278.426458	7999.813786	13.655219	-0.057045	4.816009
278.441096	7999.838632	13.660224	-0.057047	4.816016
278.523907	7999.937364	13.665229	-0.057063	4.816045
278.476257	7999.779456	13.670234	-0.057054	4.815999
278.581297	7999.926667	13.675239	-0.057074	4.816041
278.373200	7999.845978	13.680243	-0.057035	4.816019
278.500754	7999.848298	13.685248	-0.057059	4.816019
278.639700	7999.934160	13.690253	-0.057085	4.816043
278.337699	7999.841083	13.695258	-0.057029	4.816018
278.363225	7999.936639	13.700263	-0.057034	4.816045
278.316234	7999.792633	13.705267	-0.057025	4.816004
278.423692	7999.900358	13.710272	-0.057045	4.816035
278.313627	7999.910121	13.715277	-0.057025	4.816038
278.575704	7999.883899	13.720282	-0.057073	4.816029
278.645936	7999.931120	13.725287	-0.057087	4.816042
278.464073	7999.780394	13.730291	-0.057053	4.815999
278.521241	7999.914985	13.735296	-0.057064	4.816038
278.559894	7999.845180	13.740301	-0.057071	4.816018
278.573257	7999.905260	13.745306	-0.057073	4.816035
278.454154	7999.802680	13.750311	-0.057051	4.816006
278.295296	7999.913055	13.755315	-0.057022	4.816039
278.463840	7999.895819	13.760320	-0.057053	4.816033
278.580968	7999.838122	13.765325	-0.057075	4.816015
278.498376	7999.865478	13.770330	-0.057060	4.816024
278.487642	7999.939009	13.775335	-0.057058	4.816045
278.371200	7999.906990	13.780339	-0.057036	4.816037
278.498937	7999.797135	13.785344	-0.057060	4.816004
278.538197	7999.823495	13.790349	-0.057067	4.816011
278.534139	7999.905694	13.795354	-0.057067	4.816035
278.676636	7999.852730	13.800359	-0.057093	4.816019
278.543922	7999.873835	13.805363	-0.057069	4.816026
278.613353	7999.783221	13.810368	-0.057082	4.815999
278.381609	7999.946762	13.815373	-0.057039	4.816048
278.414023	7999.788169	13.820378	-0.057045	4.816002
278.580008	7999.858494	13.825383	-0.057076	4.816021
278.616524	7999.852754	13.830387	-0.057083	4.816020
278.312616	7999.848319	13.835392	-0.057026	4.816020
278.438935	7999.918993	13.840397	-0.057050	4.816040
278.549213	7999.856898	13.845402	-0.057070	4.816021
278.518570	7999.877717	13.850407	-0.057065	4.816027
278.419844	7999.911191	13.855411	-0.057047	4.816038
278.400715	7999.927946	13.860416	-0.057043	4.816043
278.596530	7999.828940	13.865421	-0.057080	4.816013
278.458195	7999.816823	13.870426	-0.057054	4.816010
278.397972	7999.935397	13.875431	-0.057043	4.816045
278.305761	7999.806596	13.880435	-0.057026	4.816008
278.302501	7999.848211	13.885440	-0.057025	4.816020
278.393271	7999.873369	13.890445	-0.057042	4.816027
278.608842	7999.900790	13.895450	-0.057082	4.816034
278.520580	7999.856462	13.900455	-0.057066	4.816021
278.427834	7999.775728	13.905459	-0.057049	4.815998
278.631483	7999.901223	13.910464	-0.057087	4.816034
278.313352	7999.887983	13.915469	-0.057028	4.816031
278.386181	7999.836961	13.920474	-0.057041	4.816016
278.620157	7999.823049	13.925479	-0.057085	4.816011
278.655608	7999.889939	13.930483	-0.057092	4.816030
278.609290	7999.845303	13.935488	-0.057083	4.816017
278.498791	7999.866811	13.940493	-0.057063	4.816024
278.541603	7999.799218	13.945498	-0.057071	4.816004
278.786297	7999.948964	13.950503	-0.057116	4.816047
278.238216	7999.825784	13.955507	-0.057014	4.816014
278.371391	7999.801497	13.960512	-0.057039	4.816006
278.560796	7999.969469	13.965517	-0.057075	4.816054
278.384210	7999.838069	13.970522	-0.057042	4.816016
278.442552	7999.816699	13.975527	-0.057053	4.816010
278.433083	7999.865680	13.980531	-0.057051	4.816024
278.405403	7999.885484	13.985536	-0.057046	4.816030
278.413612	7999.980727	13.990541	-0.057047	4.816058
278.437779	7999.835873	13.995546	-0.057052	4.816015
278.390287	7999.902327	14.000551	-0.057043	4.816035
278.380143	7999.851937	14.005555	-0.057041	4.816020
278.528198	7999.857834	14.010560	-0.057069	4.816021
278.588344	7999.897394	14.015565	-0.057080	4.816033
278.436121	7999.871137	14.020570	-0.057052	4.816026
278.556714	7999.796408	14.025575	-0.057075	4.816003
278.520734	7999.942131	14.030579	-0.057068	4.816046
278.557198	7999.771860	14.035584	-0.057075	4.815996
278.565213	7999.915175	14.040589	-0.057076	4.816038
278.491722	7999.879662	14.045594	-0.057063	4.816028
278.640286	7999.852449	14.050599	-0.057091	4.816019
278.607655	7999.976866	14.055603	-0.057085	4.816056
278.403618	7999.799027	14.060608	-0.057047	4.816005
278.555221	7999.816741	14.065613	-0.057075	4.816009
278.443543	7999.868142	14.070618	-0.057054	4.816025
278.439372	7999.787946	14.075623	-0.057053	4.816001
278.613287	7999.995168	14.080627	-0.057086	4.816061
278.479121	7999.847442	14.085632	-0.057061	4.816019
278.479842	7999.829301	14.090637	-0.057061	4.816013
278.505936	7999.874653	14.095642	-0.057066	4.816026
278.604580	7999.850809	14.100647	-0.057085	4.816019
278.428631	7999.889292	14.105651	-0.057052	4.816031
278.621032	7999.762447	14.110656	-0.057088	4.815993
278.784944	7999.916069	14.115661	-0.057119	4.816037
278.614724	7999.747390	14.120666	-0.057087	4.815989
278.629827	7999.886561	14.125671	-0.057090	4.816029
278.347250	7999.925247	14.130675	-0.057037	4.816042
278.496082	7999.783723	14.135680	-0.057065	4.816000
278.404894	7999.909214	14.140685	-0.057048	4.816037
278.616479	7999.862845	14.145690	-0.057088	4.816022
278.849030	7999.882027	14.150695	-0.057131	4.816027
278.597271	7999.873195	14.155699	-0.057084	4.816025
278.592857	7999.780174	14.160704	-0.057083	4.815998
278.743225	7999.896157	14.165709	-0.057112	4.816031
278.558686	7999.858629	14.170714	-0.057077	4.816021
278.679028	7999.840520	14.175719	-0.057100	4.816015
278.512158	7999.859937	14.180723	-0.057069	4.816022
278.612591	7999.804074	14.185728	-0.057087	4.816005
278.513211	7999.949716	14.190733	-0.057069	4.816048
278.596563	7999.848670	14.195738	-0.057085	4.816018
278.795713	7999.874725	14.200743	-0.057122	4.816025
278.701658	7999.988413	14.205747	-0.057104	4.816059
278.736333	7999.857638	14.210752	-0.057111	4.816020
278.603267	7999.837070	14.215757	-0.057086	4.816015
278.400845	7999.871868	14.220762	-0.057049	4.816026
278.577918	7999.857993	14.225767	-0.057082	4.816021
278.548939	7999.911962	14.230771	-0.057076	4.816037
278.566991	7999.837510	14.235776	-0.057080	4.816015
278.680166	7999.868417	14.240781	-0.057101	4.816024
278.681471	7999.878063	14.245786	-0.057101	4.816026
278.937344	7999.805788	14.250791	-0.057149	4.816004
278.753999	7999.876189	14.255795	-0.057115	4.816025
278.798520	7999.582131	14.260800	-0.057123	4.815939

278.875709	7996.339218	14.265805	-0.057135	4.814991
278.543060	7990.721048	14.270810	-0.057070	4.813351
278.810503	7984.019342	14.275815	-0.057115	4.811389
278.714902	7976.655630	14.280819	-0.057093	4.809235
278.704897	7969.042946	14.285824	-0.057086	4.807007
278.566424	7961.233341	14.290829	-0.057055	4.804721
278.326738	7953.366134	14.295834	-0.057006	4.802417
278.475757	7945.379423	14.300839	-0.057028	4.800075
278.185637	7937.453126	14.305843	-0.056969	4.797752
278.077819	7929.417827	14.310848	-0.056944	4.795395
278.429230	7921.390787	14.315853	-0.057004	4.793037
278.386653	7913.391015	14.320858	-0.056991	4.790688
278.107715	7905.406322	14.325863	-0.056934	4.788343
278.256520	7897.420664	14.330867	-0.056957	4.785995
278.304816	7889.430959	14.335872	-0.056961	4.783644
278.037563	7881.423390	14.340877	-0.056906	4.781289
277.878130	7873.411959	14.345882	-0.056871	4.778931
278.069825	7865.440495	14.350887	-0.056901	4.776582
278.050645	7857.425316	14.355891	-0.056893	4.774220
277.866580	7849.363042	14.360896	-0.056853	4.771844
277.864041	7841.368819	14.365901	-0.056848	4.769485
277.800561	7833.375586	14.370906	-0.056831	4.767126
277.867446	7825.381810	14.375911	-0.056838	4.764765
277.789412	7817.422746	14.380915	-0.056818	4.762414
277.854213	7809.403055	14.385920	-0.056825	4.760043
277.741214	7801.433527	14.390925	-0.056799	4.757687
277.431238	7793.349388	14.395930	-0.056736	4.755296
277.454518	7785.388661	14.400935	-0.056735	4.752939
277.359654	7777.290227	14.405939	-0.056713	4.750541
277.392450	7769.335501	14.410944	-0.056714	4.748183
277.475774	7761.337970	14.415949	-0.056724	4.745812
277.442567	7753.348263	14.420954	-0.056713	4.743442
277.408724	7745.338374	14.425959	-0.056701	4.741065
277.016856	7737.343043	14.430963	-0.056623	4.738692
277.219728	7729.336668	14.435968	-0.056656	4.736313
277.068804	7721.341789	14.440973	-0.056622	4.733937
277.004853	7713.258549	14.445978	-0.056605	4.731533
277.100956	7705.382613	14.450983	-0.056618	4.729190
276.874949	7697.290051	14.455987	-0.056571	4.726781
276.746765	7689.332689	14.460992	-0.056542	4.724412
276.742351	7681.402655	14.465997	-0.056536	4.722049
276.902758	7673.290879	14.471002	-0.056561	4.719630
276.908403	7665.383616	14.476007	-0.056557	4.717271
276.611937	7657.294340	14.481011	-0.056496	4.714858
276.696738	7649.264198	14.486016	-0.056507	4.712460
276.548185	7641.295483	14.491021	-0.056474	4.710080
276.519075	7633.288101	14.496026	-0.056464	4.707686
276.491118	7625.287953	14.501031	-0.056453	4.705294
276.542270	7617.372911	14.506035	-0.056458	4.702926
276.703897	7609.316826	14.511040	-0.056483	4.700514
276.560166	7601.347709	14.516045	-0.056451	4.698127
276.443455	7593.286061	14.521050	-0.056424	4.695712
276.402469	7585.340612	14.526055	-0.056411	4.693329
276.175470	7577.239611	14.531059	-0.056364	4.690900
276.407448	7569.278476	14.536064	-0.056402	4.688510
276.390663	7561.267500	14.541069	-0.056393	4.686105
276.217195	7553.298998	14.546074	-0.056356	4.683711
276.141456	7545.342600	14.551079	-0.056337	4.681319
275.974418	7537.340904	14.556083	-0.056301	4.678913
275.887042	7529.296212	14.561088	-0.056279	4.676493
275.880175	7521.251063	14.566093	-0.056273	4.674071
276.030663	7513.173774	14.571098	-0.056296	4.671638
275.997920	7505.193781	14.576103	-0.056284	4.669233
275.751998	7497.207355	14.581107	-0.056233	4.666825
275.884664	7489.229367	14.586112	-0.056253	4.664418
275.826932	7481.278197	14.591117	-0.056237	4.662018
275.638319	7473.205406	14.596122	-0.056197	4.659580
275.671999	7465.289897	14.601127	-0.056198	4.657189
275.593858	7457.248848	14.606131	-0.056178	4.654758
275.547921	7449.228700	14.611136	-0.056165	4.652332
275.597231	7441.203907	14.616141	-0.056169	4.649903
275.493365	7433.267165	14.621146	-0.056144	4.647500
275.328438	7425.238510	14.626151	-0.056108	4.645068
275.231638	7417.274122	14.631155	-0.056085	4.642654
275.382704	7409.196485	14.636160	-0.056108	4.640205
275.403511	7401.268675	14.641165	-0.056107	4.637799
275.153138	7393.176495	14.646170	-0.056055	4.635343
275.259631	7385.198748	14.651175	-0.056070	4.632919
275.375459	7377.173817	14.656179	-0.056086	4.630480
275.415393	7369.192903	14.661184	-0.056089	4.628054
275.244846	7361.198193	14.666189	-0.056052	4.625622
275.076855	7353.206743	14.671194	-0.056015	4.623189
275.297249	7345.231680	14.676199	-0.056051	4.620760
275.171073	7337.217034	14.681203	-0.056023	4.618318
274.821957	7329.222674	14.686208	-0.055952	4.615881
275.117438	7321.201967	14.691213	-0.056002	4.613435
274.687540	7313.113852	14.696218	-0.055917	4.610966
274.792711	7305.222010	14.701223	-0.055932	4.608557
274.790451	7297.148227	14.706227	-0.055926	4.606090
274.721306	7289.194105	14.711232	-0.055908	4.603658
274.647958	7281.191151	14.716237	-0.055889	4.601211
274.483535	7273.183278	14.721242	-0.055853	4.598760
274.529961	7265.211388	14.726247	-0.055857	4.596320
274.426818	7257.165270	14.731251	-0.055833	4.593855
274.455940	7249.122475	14.736256	-0.055833	4.591390
274.455687	7241.133879	14.741261	-0.055828	4.588940
274.289962	7233.093708	14.746266	-0.055792	4.586473
274.322875	7225.150297	14.751271	-0.055793	4.584034
274.283537	7217.153260	14.756275	-0.055780	4.581578
274.382015	7209.145139	14.761280	-0.055793	4.579117
274.264195	7201.183207	14.766285	-0.055766	4.576668
274.041459	7193.129377	14.771290	-0.055720	4.574190
274.229508	7185.151273	14.776295	-0.055750	4.571735
273.959472	7177.093162	14.781299	-0.055694	4.569253
274.074066	7169.106576	14.786304	-0.055710	4.566792
274.155089	7161.130411	14.791309	-0.055720	4.564332
273.874584	7153.166522	14.796314	-0.055663	4.561875
273.986093	7145.155410	14.801319	-0.055679	4.559403
273.536342	7137.170467	14.806323	-0.055590	4.556936
273.797532	7129.134272	14.811328	-0.055633	4.554453
273.655183	7121.137022	14.816333	-0.055602	4.551981
273.602242	7113.052050	14.821338	-0.055586	4.549480
273.789887	7105.152176	14.826343	-0.055616	4.547035
273.556090	7097.106950	14.831347	-0.055568	4.544543
273.554994	7089.172058	14.836352	-0.055562	4.542085
273.551984	7081.147849	14.841357	-0.055557	4.539597
273.541622	7073.143174	14.846362	-0.055550	4.537114
273.464979	7065.153261	14.851367	-0.055530	4.534634
273.369211	7057.103522	14.856371	-0.055507	4.532135
273.372504	7049.089914	14.861376	-0.055503	4.529645
273.333100	7041.134156	14.866381	-0.055490	4.527172
273.212745	7033.065809	14.871386	-0.055463	4.524662
273.223472	7025.158706	14.876391	-0.055460	4.522201
273.231805	7017.119605	14.881395	-0.055456	4.519698
273.096298	7009.196031	14.886400	-0.055426	4.517229
273.009092	7001.110343	14.891405	-0.055404	4.514708
272.946797	6993.018045	14.896410	-0.055387	4.512184
272.951606	6985.027874	14.901415	-0.055383	4.509690
272.719392	6977.046749	14.906419	-0.055335	4.507198
272.947116	6969.050917	14.911424	-0.055372	4.504700
272.731927	6961.123547	14.916429	-0.055327	4.502222
272.679033	6953.077687	14.921434	-0.055312	4.499705
272.871378	6945.092333	14.926439	-0.055343	4.497207
272.811567	6937.061489	14.931443	-0.055326	4.494692
272.467537	6929.043426	14.936448	-0.055257	4.492179
272.530174	6921.073450	14.941453	-0.055264	4.489681
272.425380	6913.057557	14.946458	-0.055239	4.487166
272.503986	6905.083416	14.951463	-0.055248	4.484664
272.413468	6897.075430	14.956467	-0.055226	4.482149
272.576274	6889.056791	14.961472	-0.055252	4.479630
272.404414	6881.115181	14.966477	-0.055215	4.477133
272.095340	6873.035480	14.971482	-0.055152	4.474591
272.249584	6865.075073	14.976487	-0.055175	4.472086
272.314444	6857.038670	14.981491	-0.055182	4.469556
272.031607	6849.030078	14.986496	-0.055125	4.467032
272.050161	6841.049802	14.991501	-0.055123	4.464516
272.105881	6833.049891	14.996506	-0.055128	4.461993
272.278417	6825.058203	15.001511	-0.055155	4.459471
272.124015	6817.038909	15.006515	-0.055121	4.456938
272.173368	6809.031891	15.011520	-0.055125	4.454409
272.166028	6801.017207	15.016525	-0.055119	4.451875
271.784516	6792.989632	15.021530	-0.055043	4.449334
271.916651	6785.021032	15.026535	-0.055062	4.446812
271.887372	6777.009523	15.031539	-0.055051	4.444275
271.716227	6769.021044	15.036544	-0.055014	4.441743
271.713541	6761.031218	15.041549	-0.055009	4.439210
271.768035	6753.014758	15.046554	-0.055014	4.436667
271.645127	6745.002150	15.051559	-0.054986	4.434123
271.495395	6736.966039	15.056563	-0.054953	4.431570
271.514420	6728.978610	15.061568	-0.054951	4.429032
271.555718	6721.012156	15.066573	-0.054954	4.426499
271.410839	6712.996809	15.071578	-0.054922	4.423949
271.461667	6705.009984	15.076583	-0.054926	4.421406
271.522225	6696.982532	15.081587	-0.054932	4.418850
271.478277	6688.977809	15.086592	-0.054919	4.416299
271.369880	6681.048135	15.091597	-0.054893	4.413769
271.192629	6672.970464	15.096602	-0.054855	4.411191
271.152490	6665.000216	15.101607	-0.054843	4.408647
270.967595	6656.942921	15.106611	-0.054803	4.406072
271.005204	6649.005264	15.111616	-0.054805	4.403535
271.143551	6640.998441	15.116621	-0.054826	4.400975
270.935858	6632.987851	15.121626	-0.054782	4.398410
271.010009	6624.976697	15.126631	-0.054790	4.395846
270.847079	6616.983646	15.131635	-0.054755	4.393284
270.666088	6608.948882	15.136640	-0.054716	4.390708
270.621767	6600.998460	15.141645	-0.054703	4.388157
270.569767	6592.943893	15.146650	-0.054688	4.385572
270.710451	6585.062969	15.151655	-0.054709	4.383042
270.644259	6577.006399	15.156659	-0.054692	4.380453
270.738743	6569.001436	15.161664	-0.054704	4.377880
270.665990	6561.015635	15.166669	-0.054685	4.375310
270.597334	6552.996677	15.171674	-0.054667	4.372729
270.665502	6544.973327	15.176679	-0.054675	4.370145
270.615807	6537.001325	15.181683	-0.054661	4.367575
270.359749	6528.968991	15.186688	-0.054608	4.364984
270.297464	6521.038655	15.191693	-0.054591	4.362425
270.139599	6512.983266	15.196698	-0.054557	4.359823
270.275467	6505.063590	15.201703	-0.054577	4.357266
270.022677	6496.980959	15.206707	-0.054524	4.354652
269.990514	6488.887573	15.211712	-0.054513	4.352034
269.995605	6480.914103	15.216717	-0.054509	4.349453
269.942539	6472.902146	15.221722	-0.054494	4.346859
270.014229	6464.942679	15.226727	-0.054502	4.344280
270.039112	6456.995571	15.231731	-0.054502	4.341704
269.815108	6448.944559	15.236736	-0.054455	4.339091
269.643256	6440.985917	15.241741	-0.054418	4.336506
269.569762	6432.949396	15.246746	-0.054399	4.333896
269.882483	6424.935835	15.251751	-0.054452	4.331294
269.619784	6416.952217	15.256755	-0.054398	4.328696
269.597478	6408.961811	15.261760	-0.054389	4.326096
269.788827	6400.991890	15.266765	-0.054419	4.323502
269.671860	6392.950794	15.271770	-0.054392	4.320882
269.535310	6385.018457	15.276775	-0.054362	4.318295
269.406634	6376.939575	15.281779	-0.054333	4.315660
269.525389	6368.916744	15.286784	-0.054350	4.313042
269.342518	6360.955043	15.291789	-0.054310	4.310441
269.493648	6352.903936	15.296794	-0.054333	4.307811
269.512513	6344.932231	15.301799	-0.054332	4.305205
269.432629	6336.947538	15.306803	-0.054312	4.302592
269.398954	6328.949527	15.311808	-0.054300	4.299974
269.329065	6321.005831	15.316813	-0.054282	4.297371
268.994918	6312.918812	15.321818	-0.054215	4.294718
269.106081	6304.961714	15.326823	-0.054231	4.292109
269.033193	6296.924331	15.331827	-0.054212	4.289471
268.957242	6288.909112	15.336832	-0.054192	4.286839
268.912731	6280.930401	15.341837	-0.054179	4.284217
268.872574	6272.928016	15.346842	-0.054166	4.281586
268.893749	6264.977474	15.351847	-0.054165	4.278970
268.657046	6256.924313	15.356851	-0.054116	4.276318
268.757997	6248.898261	15.361856	-0.054130	4.273675
268.799942	6240.904173	15.366861	-0.054132	4.271041
268.629051	6232.873012	15.371866	-0.054095	4.268391
268.550484	6224.916469	15.376871	-0.054076	4.265764
268.353221	6216.934798	15.381875	-0.054034	4.263127
268.333213	6208.886549	15.386880	-0.054025	4.260468
268.229121	6200.932360	15.391885	-0.054000	4.257837
268.380139	6192.898201	15.396890	-0.054023	4.255181
268.376506	6184.894740	15.401895	-0.054018	4.252531
268.267879	6176.873605	15.406899	-0.053992	4.249874
268.231469	6168.908354	15.411904	-0.053980	4.247233
268.319388	6160.908048	15.416909	-0.053992	4.244581
268.200928	6152.949316	15.421914	-0.053964	4.241939
268.222171	6144.949509	15.426919	-0.053963	4.239283
268.144842	6136.938624	15.431923	-0.053944	4.236620
267.976109	6128.941904	15.436928	-0.053907	4.233960
268.086959	6120.902189	15.441933	-0.053923	4.231286
267.999217	6112.917132	15.446938	-0.053901	4.228627
268.024036	6104.920856	15.451943	-0.053901	4.225964
267.887057	6096.938885	15.456947	-0.053870	4.223302
267.909689	6088.916283	15.461952	-0.053869	4.220626
267.884592	6080.989913	15.466957	-0.053859	4.217981
267.807457	6072.915834	15.471962	-0.053840	4.215284
267.627899	6064.965756	15.476967	-0.053801	4.212625
267.530764	6056.939959	15.481971	-0.053778	4.209941
267.491538	6048.933477	15.486976	-0.053766	4.207261
267.372912	6040.977357	15.491981	-0.053738	4.204596
267.286048	6032.958313	15.496986	-0.053717	4.201909
267.344466	6025.003379	15.501991	-0.053723	4.199243
267.345993	6016.977981	15.506995	-0.053718	4.196551
267.199394	6008.892521	15.512000	-0.053685	4.193835
267.129616	6000.857397	15.517005	-0.053667	4.191136
267.099833	5992.840181	15.522010	-0.053657	4.188441
267.269588	5984.879481	15.527015	-0.053683	4.185765
267.288095	5976.912772	15.532019	-0.053681	4.183084
267.045058	5968.917690	15.537024	-0.053631	4.180389
267.015997	5960.971114	15.542029	-0.053620	4.177711
267.009655	5952.895643	15.547034	-0.053614	4.174988
267.028177	5944.924553	15.552039	-0.053612	4.172299
266.911280	5936.893638	15.557043	-0.053586	4.169586
266.788251	5928.900537	15.562048	-0.053558	4.166885
266.945343	5920.920156	15.567053	-0.053582	4.164188
266.850210	5912.906113	15.572058	-0.053559	4.161476
266.947365	5904.938935	15.577063	-0.053572	4.158780
266.658937	5896.926122	15.582067	-0.053513	4.156063
266.788093	5888.888151	15.587072	-0.053532	4.153340
266.842355	5880.885527	15.592077	-0.053537	4.150626
266.655918	5872.879705	15.597082	-0.053497	4.147907
266.547217	5864.902306	15.602087	-0.053472	4.145197
266.484710	5856.923088	15.607091	-0.053455	4.142484
266.537334	5848.902036	15.612096	-0.053459	4.139757
266.440438	5840.957460	15.617101	-0.053436	4.137053
266.220693	5832.864753	15.622106	-0.053390	4.134294
266.416821	5824.876577	15.627111	-0.053422	4.131575
266.328816	5816.884358	15.632115	-0.053400	4.128849
266.250905	5808.875150	15.637120	-0.053380	4.126115
266.311126	5800.913913	15.642125	-0.053386	4.123398
266.159387	5792.912500	15.647130	-0.053353	4.120662
266.159819	5784.967601	15.652135	-0.053348	4.117946
266.079011	5776.925060	15.657139	-0.053328	4.115194
265.934625	5768.881135	15.662144	-0.053296	4.112438
266.042074	5760.869911	15.667149	-0.053311	4.109695
265.883404	5752.887429	15.672154	-0.053276	4.106957
265.697756	5744.925898	15.677159	-0.053236	4.104223
265.701958	5736.921792	15.682163	-0.053232	4.101476
265.740372	5728.903606	15.687168	-0.053234	4.098723
265.887038	5720.930324	15.692173	-0.053256	4.095984
265.660794	5712.905604	15.697178	-0.053209	4.093221
265.495895	5704.891333	15.702183	-0.053173	4.090460
265.373221	5696.901781	15.707187	-0.053145	4.087707
265.318013	5688.858038	15.712192	-0.053130	4.084934
265.478876	5680.945403	15.717197	-0.053155	4.082207
265.410625	5672.922962	15.722202	-0.053137	4.079438
265.503776	5664.984681	15.727207	-0.053149	4.076698
265.285121	5656.947387	15.732211	-0.053103	4.073917
265.362477	5648.941057	15.737216	-0.053112	4.071150
265.075899	5640.931060	15.742221	-0.053054	4.068374
265.122904	5632.913427	15.747226	-0.053057	4.065598
265.129582	5624.973114	15.752231	-0.053054	4.062847
265.181407	5616.925674	15.757235	-0.053058	4.060057
265.081015	5608.954633	15.762240	-0.053034	4.057289
264.993438	5600.959800	15.767245	-0.053013	4.054512
264.820158	5592.929962	15.772250	-0.052975	4.051720
264.997211	5584.920157	15.777255	-0.053003	4.048937
264.716368	5576.925607	15.782259	-0.052946	4.046151
264.887296	5568.959297	15.787264	-0.052972	4.043380
265.015955	5560.950872	15.792269	-0.052991	4.040591
264.698100	5552.954870	15.797274	-0.052927	4.037798
264.743015	5544.943115	15.802279	-0.052930	4.035004
264.715278	5536.820179	15.807283	-0.052920	4.032167
264.617714	5528.856874	15.812288	-0.052897	4.029383
264.415355	5520.924091	15.817293	-0.052854	4.026606
264.393646	5512.920499	15.822298	-0.052845	4.023806
264.341102	5504.916684	15.827303	-0.052830	4.021002
264.216848	5496.936704	15.832307	-0.052801	4.018204
264.245451	5488.899667	15.837312	-0.052802	4.015387
264.292150	5480.932412	15.842317	-0.052805	4.012592
264.234203	5472.870371	15.847322	-0.052789	4.009760
264.152046	5464.928807	15.852327	-0.052769	4.006969
264.068874	5456.888128	15.857331	-0.052748	4.004140
263.934399	5448.946795	15.862336	-0.052718	4.001344
263.883631	5440.959502	15.867341	-0.052703	3.998531
263.751704	5432.918590	15.872346	-0.052674	3.995695
263.915471	5424.917129	15.877351	-0.052699	3.992876
263.901515	5416.884135	15.882355	-0.052691	3.990042
263.671403	5408.909039	15.887360	-0.052643	3.987222
263.738408	5400.903261	15.892365	-0.052651	3.984394
263.419840	5392.931286	15.897370	-0.052586	3.981570
263.767397	5384.949654	15.902375	-0.052646	3.978751
263.659859	5376.961820	15.907379	-0.052621	3.975920
263.635613	5368.934495	15.912384	-0.052611	3.973075
263.433195	5360.921187	15.917389	-0.052568	3.970230
263.288677	5352.922456	15.922394	-0.052536	3.967389
263.305369	5344.920238	15.927399	-0.052534	3.964548
263.369224	5336.968967	15.932403	-0.052541	3.961723
263.305343	5328.985484	15.937408	-0.052524	3.958882
263.377851	5321.017102	15.942413	-0.052532	3.956048
263.185113	5312.962724	15.947418	-0.052491	3.953176
263.164690	5304.935846	15.952423	-0.052482	3.950314
263.145220	5296.943628	15.957427	-0.052473	3.947463
263.137051	5288.948787	15.962432	-0.052467	3.944610
262.987001	5281.025999	15.967437	-0.052434	3.941777
262.903474	5272.981778	15.972442	-0.052413	3.938900
262.884541	5265.008384	15.977447	-0.052404	3.936047
262.769295	5256.992310	15.982451	-0.052378	3.933176
262.663470	5248.941610	15.987456	-0.052353	3.930290
262.814825	5241.020889	15.992461	-0.052376	3.927453
262.588140	5233.009689	15.997466	-0.052329	3.924575
262.563343	5225.027485	16.002471	-0.052319	3.921708
262.429526	5217.002710	16.007475	-0.052289	3.918823
262.385982	5209.009776	16.012480	-0.052276	3.915948
262.522408	5201.020640	16.017485	-0.052296	3.913076
262.188823	5192.989937	16.022490	-0.052229	3.910178
262.464435	5184.987346	16.027495	-0.052275	3.907299
262.382516	5176.985333	16.032499	-0.052254	3.904412
262.232885	5168.995327	16.037504	-0.052221	3.901526
262.314731	5161.023655	16.042509	-0.052232	3.898648
262.234648	5152.991035	16.047514	-0.052211	3.895743
262.049956	5144.995727	16.052519	-0.052172	3.892848
262.098949	5136.964181	16.057523	-0.052176	3.889942
262.002950	5129.025417	16.062528	-0.052153	3.887064
262.110875	5121.005326	16.067533	-0.052168	3.884159
261.836558	5113.002602	16.072538	-0.052112	3.881250
261.920689	5105.051638	16.077543	-0.052122	3.878365
261.811027	5096.981925	16.082547	-0.052097	3.875431
261.801064	5088.780923	16.087552	-0.052090	3.872449
261.849815	5080.863577	16.092557	-0.052094	3.869569
261.808401	5072.913212	16.097562	-0.052081	3.866673
261.687516	5064.936257	16.102567	-0.052053	3.863764
261.592712	5056.993062	16.107571	-0.052030	3.860865
261.601387	5049.013535	16.112576	-0.052027	3.857953
261.661117	5040.997970	16.117581	-0.052033	3.855026
261.563279	5032.985929	16.122586	-0.052009	3.852096
261.473407	5025.017990	16.127591	-0.051988	3.849179
261.342329	5016.989340	16.132595	-0.051958	3.846237
261.297304	5009.030318	16.137600	-0.051945	3.843320
261.377587	5001.055992	16.142605	-0.051954	3.840398
261.232967	4993.041454	16.147610	-0.051922	3.837454
261.279084	4985.053150	16.152615	-0.051926	3.834522
261.094523	4977.027736	16.157619	-0.051886	3.831569
261.080424	4969.027925	16.162624	-0.051878	3.828626
260.976273	4961.060521	16.167629	-0.051854	3.825691
260.869238	4953.048611	16.172634	-0.051829	3.822738
260.966971	4945.073717	16.177639	-0.051842	3.819800
261.130067	4937.091915	16.182643	-0.051867	3.816859
260.933320	4929.090162	16.187648	-0.051825	3.813901
260.848258	4921.073137	16.192653	-0.051804	3.810937
260.918901	4913.061079	16.197658	-0.051812	3.807975
261.020568	4905.047545	16.202663	-0.051826	3.805012
260.576773	4897.142422	16.207667	-0.051739	3.802075
260.438876	4889.123203	16.212672	-0.051708	3.799100
260.508195	4881.122711	16.217677	-0.051715	3.796133
260.434547	4873.077924	16.222682	-0.051697	3.793145
260.319621	4865.052845	16.227687	-0.051670	3.790161
260.374835	4857.055228	16.232691	-0.051675	3.787189
260.317182	4849.081411	16.237696	-0.051659	3.784220
260.372805	4841.116419	16.242701	-0.051665	3.781255
260.212682	4833.107622	16.247706	-0.051630	3.778267
260.363226	4825.089303	16.252711	-0.051653	3.775280
260.371132	4817.089949	16.257715	-0.051649	3.772294
260.298780	4809.071654	16.262720	-0.051630	3.769297
260.227366	4801.122320	16.267725	-0.051612	3.766323
260.138903	4793.111103	16.272730	-0.051590	3.763323
260.127254	4785.137517	16.277735	-0.051583	3.760337
260.118313	4777.153459	16.282739	-0.051576	3.757345
259.816973	4769.102008	16.287744	-0.051515	3.754318
259.728761	4761.124012	16.292749	-0.051493	3.751321
259.607515	4753.092986	16.297754	-0.051466	3.748301
259.853559	4745.087469	16.302759	-0.051506	3.745297
259.644724	4737.156065	16.307763	-0.051462	3.742307
259.603318	4729.098948	16.312768	-0.051449	3.739272
259.633980	4721.154889	16.317773	-0.051450	3.736279
259.539596	4713.136428	16.322778	-0.051427	3.733252
259.502302	4705.109389	16.327783	-0.051415	3.730221
259.481143	4697.158098	16.332787	-0.051406	3.727216
259.421111	4689.160374	16.337792	-0.051390	3.724191
259.343885	4681.224691	16.342797	-0.051370	3.721186
259.089130	4673.209425	16.347802	-0.051318	3.718144
259.278198	4665.202395	16.352807	-0.051348	3.715114
259.072149	4657.073890	16.357811	-0.051304	3.712025
259.001593	4649.111297	16.362816	-0.051286	3.709000
259.055368	4641.150583	16.367821	-0.051291	3.705976
259.041800	4633.163735	16.372826	-0.051283	3.702939
259.128053	4625.182779	16.377831	-0.051294	3.699903
258.951179	4617.229393	16.382835	-0.051256	3.696869
258.831134	4609.199546	16.387840	-0.051229	3.693805
258.802377	4601.195858	16.392845	-0.051218	3.690750
258.784906	4593.201349	16.397850	-0.051210	3.687697
258.728644	4585.219272	16.402855	-0.051194	3.684645
258.715760	4577.254055	16.407859	-0.051187	3.681598
258.603529	4569.244901	16.412864	-0.051161	3.678529
258.780813	4561.236466	16.417869	-0.051188	3.675465
258.576052	4553.233809	16.422874	-0.051145	3.672391
258.674865	4545.242249	16.427879	-0.051158	3.669327
258.690922	4537.234386	16.432883	-0.051156	3.666251
258.555086	4529.232801	16.437888	-0.051126	3.663172
258.303015	4521.281462	16.442893	-0.051074	3.660106
258.342930	4513.268724	16.447898	-0.051076	3.657021
258.269082	4505.273614	16.452903	-0.051057	3.653938
258.254372	4497.253801	16.457907	-0.051049	3.650844
258.232131	4489.259900	16.462912	-0.051040	3.647757
258.192181	4481.280441	16.467917	-0.051028	3.644673
257.973428	4473.315876	16.472922	-0.050982	3.641587
257.896907	4465.313804	16.477927	-0.050962	3.638488
257.929959	4457.323184	16.482931	-0.050963	3.635394
257.856723	4449.258106	16.487936	-0.050945	3.632265
257.851304	4441.248432	16.492941	-0.050938	3.629156
257.876001	4433.264444	16.497946	-0.050938	3.626056
258.041661	4425.291182	16.502951	-0.050964	3.622961
257.778351	4417.302261	16.507955	-0.050909	3.619846
257.564383	4409.355381	16.512960	-0.050864	3.616746
257.718515	4401.322494	16.517965	-0.050888	3.613620
257.485871	4393.292330	16.522970	-0.050840	3.610481
257.457967	4385.344435	16.527975	-0.050829	3.607378
257.488188	4377.324237	16.532979	-0.050830	3.604245
257.364338	4369.356178	16.537984	-0.050802	3.601125
257.223965	4361.408212	16.542989	-0.050770	3.598010
257.207230	4353.375590	16.547994	-0.050762	3.594863
257.366835	4345.358175	16.552999	-0.050787	3.591724
257.246687	4337.365256	16.558003	-0.050759	3.588584
257.289795	4329.368520	16.563008	-0.050762	3.585444
257.333825	4321.422367	16.568013	-0.050765	3.582321
257.225932	4313.401252	16.573018	-0.050740	3.579162
257.131618	4305.422745	16.578023	-0.050717	3.576017
257.095660	4297.395630	16.583027	-0.050705	3.572852
257.048582	4289.364590	16.588032	-0.050691	3.569683
256.932066	4281.434266	16.593037	-0.050665	3.566548
256.828404	4273.446869	16.598042	-0.050640	3.563388
256.806632	4265.438541	16.603047	-0.050631	3.560219
256.657257	4257.487685	16.608051	-0.050598	3.557067
256.806839	4249.414908	16.613056	-0.050621	3.553872
256.610593	4241.344887	16.618061	-0.050579	3.550666
256.522698	4233.366221	16.623066	-0.050558	3.547496
256.545110	4225.391282	16.628071	-0.050557	3.544328
256.454762	4217.462436	16.633075	-0.050535	3.541172
256.377437	4209.465262	16.638080	-0.050515	3.537986
256.365139	4201.467349	16.643085	-0.050508	3.534799
256.227671	4193.430461	16.648090	-0.050477	3.531590
256.252971	4185.423925	16.653095	-0.050477	3.528395
256.168047	4177.404800	16.658099	-0.050456	3.525188
256.020065	4169.475026	16.663104	-0.050423	3.522013
256.220226	4161.509798	16.668109	-0.050455	3.518831
255.888147	4153.505541	16.673114	-0.050388	3.515614
255.789678	4145.494139	16.678119	-0.050365	3.512399
256.078849	4137.517367	16.683123	-0.050413	3.509207
255.961585	4129.486310	16.688128	-0.050386	3.505977
255.951074	4121.524393	16.693133	-0.050379	3.502775
255.688363	4113.521657	16.698138	-0.050325	3.499546
255.960843	4105.560408	16.703143	-0.050371	3.496348
255.831151	4097.539818	16.708147	-0.050342	3.493110
255.626641	4089.525555	16.713152	-0.050298	3.489870
255.590884	4081.590734	16.718157	-0.050287	3.486663
255.608904	4073.583417	16.723162	-0.050285	3.483426
255.668565	4065.602657	16.728167	-0.050291	3.480198
255.382629	4057.656268	16.733171	-0.050232	3.476971
255.418807	4049.565954	16.738176	-0.050234	3.473692
255.488073	4041.580631	16.743181	-0.050242	3.470453
255.207827	4033.602578	16.748186	-0.050184	3.467203
255.187401	4025.613949	16.753191	-0.050176	3.463955
255.096624	4017.642992	16.758195	-0.050154	3.460708
255.019322	4009.624107	16.763200	-0.050134	3.457439
254.977025	4001.664402	16.768205	-0.050121	3.454192
255.130732	3993.588021	16.773210	-0.050144	3.450901
255.096147	3985.632852	16.778215	-0.050133	3.447650
254.762513	3977.661065	16.783219	-0.050066	3.444379
254.777160	3969.674403	16.788224	-0.050063	3.441111
254.729295	3961.718635	16.793229	-0.050049	3.437850
254.736204	3953.667101	16.798234	-0.050045	3.434548
254.680438	3945.655745	16.803239	-0.050030	3.431258
254.724862	3937.656899	16.808243	-0.050033	3.427973
254.445858	3929.676036	16.813248	-0.049976	3.424681
254.483534	3921.741634	16.818253	-0.049978	3.421416
254.711365	3913.700069	16.823258	-0.050015	3.418111
254.498741	3905.721124	16.828263	-0.049970	3.414813
254.614565	3897.697363	16.833267	-0.049987	3.411504
254.453370	3889.717695	16.838272	-0.049952	3.408201
254.467209	3881.729916	16.843277	-0.049949	3.404897
254.287127	3873.794538	16.848282	-0.049910	3.401605
254.281321	3865.783240	16.853287	-0.049904	3.398285
254.137575	3857.810779	16.858291	-0.049872	3.394972
254.086322	3849.700219	16.863296	-0.049858	3.391602
254.164519	3841.737843	16.868301	-0.049867	3.388295
254.021051	3833.746233	16.873306	-0.049835	3.384965
253.956216	3825.788191	16.878311	-0.049818	3.381648
253.811251	3817.812534	16.883315	-0.049786	3.378318
253.910891	3809.816757	16.888320	-0.049799	3.374984
253.978778	3801.850936	16.893325	-0.049807	3.371659
253.788505	3793.825964	16.898330	-0.049766	3.368297
253.803052	3785.837968	16.903335	-0.049764	3.364954
253.809348	3777.894357	16.908339	-0.049760	3.361626
253.676319	3769.884167	16.913344	-0.049730	3.358261
253.685792	3761.901131	16.918349	-0.049727	3.354910
253.579566	3753.860227	16.923354	-0.049702	3.351527
253.482721	3745.886035	16.928359	-0.049679	3.348169
253.428802	3737.863593	16.933363	-0.049663	3.344789
253.309092	3729.932684	16.938368	-0.049636	3.341442
253.448670	3721.926030	16.943373	-0.049657	3.338068
253.243496	3713.929147	16.948378	-0.049613	3.334683
253.138651	3705.942861	16.953383	-0.049589	3.331303
253.095932	3697.938696	16.958387	-0.049576	3.327913
253.002398	3689.916937	16.963392	-0.049553	3.324511
253.160273	3681.989658	16.968397	-0.049577	3.321155
253.055463	3673.993331	16.973402	-0.049553	3.317757
253.031112	3665.988654	16.978407	-0.049543	3.314354
253.030606	3657.960045	16.983411	-0.049538	3.310938
252.751213	3650.000181	16.988416	-0.049481	3.307538
253.070665	3642.009713	16.993421	-0.049535	3.304144
252.786723	3634.032399	16.998426	-0.049477	3.300729
252.742995	3626.054612	17.003431	-0.049464	3.297320
252.831269	3618.042730	17.008435	-0.049475	3.293897
252.619110	3610.020683	17.013440	-0.049431	3.290455
252.599297	3602.089012	17.018445	-0.049422	3.287055
252.419981	3594.084525	17.023450	-0.049383	3.283615
252.650423	3586.083053	17.028455	-0.049421	3.280188
252.577820	3578.136646	17.033459	-0.049402	3.276769
252.342422	3570.107347	17.038464	-0.049353	3.273305
252.374528	3562.117596	17.043469	-0.049354	3.269865
252.111003	3554.152828	17.048474	-0.049300	3.266420
252.124167	3546.155633	17.053479	-0.049297	3.262968
252.117159	3538.150676	17.058483	-0.049291	3.259509
252.006146	3530.175225	17.063488	-0.049265	3.256054
251.965635	3522.176652	17.068493	-0.049252	3.252589
251.889218	3514.159675	17.073498	-0.049233	3.249110
252.080221	3506.168547	17.078503	-0.049263	3.245650
251.964433	3498.202504	17.083507	-0.049237	3.242184
251.966160	3490.217016	17.088512	-0.049232	3.238712
251.961923	3482.251395	17.093517	-0.049226	3.235243
251.750357	3474.194622	17.098522	-0.049182	3.231723
251.702479	3466.197381	17.103527	-0.049167	3.228232
251.838431	3458.193920	17.108531	-0.049188	3.224742
251.509041	3450.252283	17.113536	-0.049121	3.221256
251.594874	3442.286454	17.118541	-0.049132	3.217772
251.561793	3434.268390	17.123546	-0.049121	3.214257
251.513723	3426.281145	17.128551	-0.049107	3.210751
251.394932	3418.312119	17.133555	-0.049079	3.207246
251.205226	3410.342200	17.138560	-0.049039	3.203734
251.249999	3402.356222	17.143565	-0.049042	3.200221
251.123859	3394.398647	17.148570	-0.049014	3.196709
250.953069	3386.383366	17.153575	-0.048977	3.193167
251.013681	3378.333260	17.158579	-0.048983	3.189614
251.045298	3370.340721	17.163584	-0.048984	3.186082
250.935547	3362.416295	17.168589	-0.048958	3.182570
251.157280	3354.365582	17.173594	-0.048994	3.179012
250.979873	3346.414625	17.178599	-0.048956	3.175478
250.897882	3338.433273	17.183603	-0.048936	3.171930
250.822052	3330.413281	17.188608	-0.048916	3.168361
250.965541	3322.449309	17.193613	-0.048938	3.164822
250.595618	3314.501557	17.198618	-0.048864	3.161265
250.628894	3306.514273	17.203623	-0.048865	3.157704
250.699117	3298.502374	17.208627	-0.048873	3.154129
250.657212	3290.445478	17.213632	-0.048860	3.150525
250.438893	3282.529259	17.218637	-0.048814	3.146972
250.444001	3274.513339	17.223642	-0.048810	3.143380
250.488846	3266.521490	17.228647	-0.048813	3.139797
250.474740	3258.568812	17.233651	-0.048806	3.136224
250.385989	3250.557562	17.238656	-0.048784	3.132618
250.396466	3242.572201	17.243661	-0.048781	3.129023
250.388886	3234.581170	17.248666	-0.048774	3.125422
250.257969	3226.633617	17.253671	-0.048745	3.121830
250.069067	3218.673366	17.258675	-0.048704	3.118225
249.971202	3210.646506	17.263680	-0.048681	3.114591
250.044705	3202.655524	17.268685	-0.048690	3.110976
249.684528	3194.677559	17.273690	-0.048617	3.107343
249.703363	3186.684521	17.278695	-0.048616	3.103716
249.800168	3178.697866	17.283699	-0.048629	3.100092
249.613495	3170.714481	17.288704	-0.048589	3.096451
249.870521	3162.700357	17.293709	-0.048632	3.092813
249.788012	3154.724739	17.298714	-0.048611	3.089172
249.581249	3146.740275	17.303719	-0.048567	3.085518
249.477040	3138.796712	17.308723	-0.048543	3.081882
249.659326	3130.788728	17.313728	-0.048572	3.078226
249.563662	3122.799142	17.318733	-0.048549	3.074561
249.368385	3114.729215	17.323738	-0.048507	3.070850
249.466507	3106.763074	17.328743	-0.048520	3.067196
249.568760	3098.784245	17.333747	-0.048534	3.063532
249.324092	3090.798673	17.338752	-0.048484	3.059845
249.331445	3082.882478	17.343757	-0.048480	3.056196
249.027786	3074.879688	17.348762	-0.048418	3.052489
248.972952	3066.886322	17.353767	-0.048403	3.048793
248.860594	3058.913292	17.358771	-0.048377	3.045099
248.869587	3050.932825	17.363776	-0.048373	3.041403
248.973001	3042.959074	17.368781	-0.048388	3.037711
248.813116	3034.964303	17.373786	-0.048353	3.033991
248.814775	3026.938582	17.378791	-0.048348	3.030260
248.944206	3018.979248	17.383795	-0.048367	3.026562
248.653231	3011.020247	17.388800	-0.048308	3.022839
248.656459	3003.047347	17.393805	-0.048303	3.019119
248.676098	2995.041827	17.398810	-0.048302	3.015380
248.729218	2987.036069	17.403815	-0.048306	3.011638
248.486629	2979.077767	17.408819	-0.048256	3.007899
248.604112	2971.066544	17.413824	-0.048273	3.004149
248.490056	2963.122091	17.418829	-0.048246	3.000413
248.341290	2955.169334	17.423834	-0.048214	2.996667
248.420165	2947.133053	17.428839	-0.048223	2.992889
248.222492	2939.163828	17.433843	-0.048181	2.989123
248.098678	2931.148023	17.438848	-0.048153	2.985335
248.002217	2923.191735	17.443853	-0.048130	2.981571
247.945820	2915.218218	17.448858	-0.048114	2.977796
247.825500	2907.244501	17.453863	-0.048087	2.974013
247.821651	2899.227821	17.458867	-0.048081	2.970211
247.951731	2891.232765	17.463872	-0.048100	2.966421
248.058371	2883.265453	17.468877	-0.048115	2.962638
247.769071	2875.314556	17.473882	-0.048056	2.958838
247.693762	2867.347832	17.478887	-0.048037	2.955036
247.670699	2859.334156	17.483891	-0.048027	2.951210
247.816767	2851.299648	17.488896	-0.048049	2.947377
247.728986	2843.363286	17.493901	-0.048028	2.943575
247.519295	2835.384621	17.498906	-0.047984	2.939740
247.762054	2827.381875	17.503911	-0.048024	2.935913
247.517104	2819.416923	17.508915	-0.047973	2.932074
247.392085	2811.423584	17.513920	-0.047945	2.928222
247.455333	2803.443685	17.518925	-0.047951	2.924381
247.148718	2795.491866	17.523930	-0.047889	2.920530
247.263782	2787.527964	17.528935	-0.047905	2.916689
247.475285	2779.451058	17.533939	-0.047940	2.912794
247.057202	2771.445381	17.538944	-0.047857	2.908895
247.038852	2763.477603	17.543949	-0.047848	2.905030
247.080136	2755.537661	17.548954	-0.047851	2.901177
247.283892	2747.555717	17.553959	-0.047883	2.897307
247.195389	2739.593477	17.558963	-0.047862	2.893426
246.952252	2731.582251	17.563968	-0.047811	2.889507
247.046283	2723.624610	17.568973	-0.047824	2.885627
246.801852	2715.676197	17.573978	-0.047773	2.881729
246.728313	2707.705043	17.578983	-0.047754	2.877823
246.746934	2699.705860	17.583987	-0.047753	2.873903
246.697811	2691.682542	17.588992	-0.047738	2.869962
246.647517	2683.724354	17.593997	-0.047724	2.866047
246.585586	2675.737799	17.599002	-0.047707	2.862113
246.698365	2667.768014	17.604007	-0.047723	2.858191
246.619820	2659.797699	17.609011	-0.047703	2.854253
246.314855	2651.801377	17.614016	-0.047641	2.850284
246.444004	2643.855112	17.619021	-0.047660	2.846359
246.387499	2635.867653	17.624026	-0.047645	2.842397
246.247821	2627.908299	17.629031	-0.047614	2.838439
246.373956	2619.925024	17.634035	-0.047632	2.834478
246.291315	2611.889997	17.639040	-0.047611	2.830474
246.120106	2603.942165	17.644045	-0.047575	2.826504
245.933702	2595.971694	17.649050	-0.047535	2.822515
245.919077	2587.994894	17.654055	-0.047527	2.818527
245.979634	2580.012707	17.659059	-0.047533	2.814535
245.826418	2571.999027	17.664064	-0.047499	2.810510
245.943998	2564.034892	17.669069	-0.047516	2.806519
245.592384	2556.102946	17.674074	-0.047446	2.802512
245.643173	2548.119569	17.679079	-0.047450	2.798496
245.733760	2540.135615	17.684083	-0.047462	2.794476
245.429397	2532.139420	17.689088	-0.047400	2.790422
245.293452	2524.176292	17.694093	-0.047369	2.786388
245.348363	2516.197762	17.699098	-0.047374	2.782351
245.492353	2508.217995	17.704103	-0.047396	2.778314
245.346088	2500.269307	17.709107	-0.047364	2.774269
245.069874	2492.262127	17.714112	-0.047307	2.770180
245.355980	2484.278005	17.719117	-0.047355	2.766131
245.039466	2476.347573	17.724122	-0.047291	2.762068
244.906934	2468.375119	17.729127	-0.047262	2.757987
244.951447	2460.365761	17.734131	-0.047265	2.753893
244.996051	2452.300686	17.739136	-0.047268	2.749764
244.904659	2444.348184	17.744141	-0.047246	2.745678
244.852883	2436.379231	17.749146	-0.047231	2.741580
244.884948	2428.423861	17.754151	-0.047232	2.737488
244.592595	2420.499282	17.759155	-0.047172	2.733386
244.516889	2412.488626	17.764160	-0.047153	2.729247
244.514880	2404.522475	17.769165	-0.047148	2.725128
244.420556	2396.576902	17.774170	-0.047125	2.721009
244.458956	2388.592753	17.779175	-0.047127	2.716871
244.499499	2380.587447	17.784179	-0.047129	2.712717
244.596613	2372.564846	17.789184	-0.047142	2.708550
244.334970	2364.646467	17.794189	-0.047088	2.704409
244.329072	2356.676298	17.799194	-0.047082	2.700250
244.059888	2348.733821	17.804199	-0.047027	2.696083
244.363323	2340.708855	17.809203	-0.047078	2.691903
244.103944	2332.749519	17.814208	-0.047025	2.687715
244.245666	2324.788931	17.819213	-0.047046	2.683545
243.882311	2316.858203	17.824218	-0.046974	2.679352
243.779736	2308.889654	17.829223	-0.046949	2.675149
243.841233	2300.855881	17.834227	-0.046956	2.670915
243.990350	2292.848405	17.839232	-0.046978	2.666695
244.066634	2284.886525	17.844237	-0.046987	2.662487
243.795708	2276.955241	17.849242	-0.046932	2.658266
243.711802	2268.974570	17.854247	-0.046911	2.654025
243.578562	2261.002155	17.859251	-0.046881	2.649778
243.593702	2253.009542	17.864256	-0.046879	2.645522
243.709112	2245.081557	17.869261	-0.046895	2.641301
243.568935	2237.114853	17.874266	-0.046864	2.637036
243.441316	2229.130719	17.879271	-0.046835	2.632756
243.416113	2221.144729	17.884275	-0.046825	2.628474
243.264835	2213.183501	17.889280	-0.046792	2.624190
243.360790	2205.215328	17.894285	-0.046805	2.619912
243.115130	2197.273614	17.899290	-0.046754	2.615618
242.996120	2189.277382	17.904295	-0.046727	2.611296
243.153774	2181.300887	17.909299	-0.046751	2.606997
242.861272	2173.336814	17.914304	-0.046691	2.602666
243.061535	2165.372125	17.919309	-0.046723	2.598361
243.147467	2157.340826	17.924314	-0.046734	2.594006
242.786818	2149.258199	17.929319	-0.046662	2.589584
242.818225	2141.310951	17.934323	-0.046663	2.585256
242.689766	2133.394690	17.939328	-0.046634	2.580926
242.785148	2125.447783	17.944333	-0.046646	2.576588
242.690645	2117.463400	17.949338	-0.046624	2.572208
242.697780	2109.489567	17.954343	-0.046620	2.567834
242.576214	2101.572463	17.959347	-0.046592	2.563475
242.252347	2093.647349	17.964352	-0.046527	2.559090
242.338127	2085.674139	17.969357	-0.046538	2.554699
242.344646	2077.666998	17.974362	-0.046534	2.550276
242.302486	2069.697655	17.979367	-0.046521	2.545863
242.348074	2061.755787	17.984371	-0.046524	2.541464
242.231786	2053.790327	17.989376	-0.046497	2.537033
242.305009	2045.827090	17.994381	-0.046506	2.532609
242.131788	2037.855361	17.999386	-0.046468	2.528154
242.055088	2029.889104	18.004391	-0.046449	2.523702
242.107223	2021.940571	18.009395	-0.046454	2.519261
241.796726	2013.997559	18.014400	-0.046391	2.514789
241.717736	2005.997235	18.019405	-0.046371	2.510294
241.643372	1998.007363	18.024410	-0.046352	2.505797
241.701168	1990.065565	18.029415	-0.046358	2.501328
241.676322	1982.104880	18.034419	-0.046348	2.496835
241.525403	1974.123464	18.039424	-0.046315	2.492312
241.559401	1966.169380	18.044429	-0.046316	2.487811
241.327144	1958.215704	18.049434	-0.046268	2.483282
241.284368	1950.272997	18.054439	-0.046254	2.478764
241.317285	1942.298543	18.059443	-0.046255	2.474226
241.248295	1934.300253	18.064448	-0.046237	2.469659
241.254914	1926.346531	18.069453	-0.046234	2.465114
241.155651	1918.397288	18.074458	-0.046210	2.460555
241.080132	1910.452936	18.079463	-0.046191	2.455993
241.044859	1902.477422	18.084467	-0.046179	2.451407
241.110197	1894.491494	18.089472	-0.046186	2.446814
241.245706	1886.532135	18.094477	-0.046206	2.442233
241.007892	1878.609349	18.099482	-0.046157	2.437637
240.989806	1870.610826	18.104487	-0.046148	2.433004
240.927721	1862.623116	18.109491	-0.046132	2.428365
240.714150	1854.675228	18.114496	-0.046087	2.423730
240.726933	1846.726988	18.119501	-0.046084	2.419102
240.771500	1838.740024	18.124506	-0.046087	2.414445
240.518087	1830.805212	18.129511	-0.046035	2.409787
240.422596	1822.863629	18.134515	-0.046012	2.405128
240.385985	1814.903361	18.139520	-0.046000	2.400454
240.507572	1806.954550	18.144525	-0.046018	2.395789
240.418909	1798.970781	18.149530	-0.045996	2.391079
240.234180	1791.023265	18.154535	-0.045957	2.386373
240.220221	1783.080859	18.159539	-0.045949	2.381674
240.160420	1775.114474	18.164544	-0.045933	2.376948
240.297113	1767.138694	18.169549	-0.045953	2.372222
240.044927	1759.190247	18.174554	-0.045901	2.367472
239.980526	1751.250728	18.179559	-0.045884	2.362734
240.240243	1743.290879	18.184563	-0.045927	2.357999
239.727623	1735.378722	18.189568	-0.045827	2.353221
239.800595	1727.367566	18.194573	-0.045835	2.348422
239.520531	1719.442477	18.199578	-0.045778	2.343635
239.411079	1711.485038	18.204583	-0.045752	2.338834
239.499815	1703.520767	18.209587	-0.045764	2.334034
239.288529	1695.563497	18.214592	-0.045719	2.329204
239.301957	1687.595672	18.219597	-0.045717	2.324376
239.317881	1679.648407	18.224602	-0.045715	2.319551
239.323094	1671.699899	18.229607	-0.045710	2.314714
239.284191	1663.728243	18.234611	-0.045698	2.309849
239.145576	1655.771967	18.239616	-0.045667	2.304975
239.289499	1647.826526	18.244621	-0.045689	2.300121
239.283401	1639.861143	18.249626	-0.045683	2.295232
239.124037	1631.919813	18.254631	-0.045648	2.290334
239.196707	1623.964943	18.259635	-0.045656	2.285437
239.026895	1616.036954	18.264640	-0.045620	2.280525
238.986900	1608.123119	18.269645	-0.045607	2.275623
238.734570	1600.103341	18.274650	-0.045555	2.270626
238.712780	1592.137730	18.279655	-0.045546	2.265672
238.751677	1584.206421	18.284659	-0.045548	2.260733
238.532173	1576.269287	18.289664	-0.045502	2.255758
238.502182	1568.311293	18.294669	-0.045491	2.250774
238.391630	1560.361245	18.299674	-0.045466	2.245778
238.241529	1552.438176	18.304679	-0.045432	2.240784
238.387303	1544.495090	18.309683	-0.045455	2.235792
238.166247	1536.529955	18.314688	-0.045408	2.230743
238.226998	1528.567014	18.319693	-0.045414	2.225709
238.249198	1520.623249	18.324698	-0.045413	2.220672
238.063305	1512.701379	18.329703	-0.045374	2.215619
238.214561	1504.726649	18.334707	-0.045397	2.210550
237.882265	1496.806791	18.339712	-0.045330	2.205462
238.023654	1488.866538	18.344717	-0.045351	2.200392
237.854006	1480.944319	18.349722	-0.045314	2.195293
237.702702	1472.968204	18.354727	-0.045281	2.190149
237.796990	1464.997256	18.359731	-0.045294	2.185019
237.628286	1457.067197	18.364736	-0.045257	2.179879
237.713312	1449.129863	18.369741	-0.045268	2.174746
237.603696	1441.174450	18.374746	-0.045242	2.169571
237.675936	1433.229971	18.379751	-0.045251	2.164407
237.530129	1425.337554	18.384755	-0.045218	2.159245
237.445923	1417.375213	18.389760	-0.045198	2.154030
237.503937	1409.423562	18.394765	-0.045203	2.148823
237.437309	1401.484017	18.399770	-0.045186	2.143600
237.333221	1393.565900	18.404775	-0.045161	2.138374
237.355089	1385.626723	18.409779	-0.045160	2.133134
237.404790	1377.654983	18.414784	-0.045164	2.127862
237.249425	1369.761058	18.419789	-0.045130	2.122608
236.896285	1361.876078	18.424794	-0.045060	2.117329
236.974706	1353.864936	18.429799	-0.045069	2.111994
237.091445	1345.878924	18.434803	-0.045086	2.106665
236.821320	1337.965849	18.439808	-0.045030	2.101335
236.851635	1330.038872	18.444813	-0.045031	2.096011
236.804151	1322.101143	18.449818	-0.045017	2.090658
236.689620	1314.180320	18.454823	-0.044991	2.085297
236.466467	1306.297545	18.459827	-0.044944	2.079937
236.460734	1298.355183	18.464832	-0.044938	2.074544
236.518388	1290.379115	18.469837	-0.044943	2.069120
236.530691	1282.440782	18.474842	-0.044941	2.063703
236.274074	1274.553395	18.479847	-0.044888	2.058280
236.329679	1266.608624	18.484851	-0.044893	2.052834
236.061792	1258.685072	18.489856	-0.044838	2.047356
236.109622	1250.761058	18.494861	-0.044842	2.041895
236.059052	1242.852108	18.499866	-0.044827	2.036420
235.972362	1234.888157	18.504871	-0.044806	2.030888
236.120640	1226.925954	18.509875	-0.044829	2.025366
236.021053	1219.016915	18.514880	-0.044805	2.019841
236.055317	1211.114064	18.519885	-0.044806	2.014318
235.835119	1203.173036	18.524890	-0.044760	2.008727
235.767497	1195.262962	18.529895	-0.044743	2.003159
235.785787	1187.358431	18.534899	-0.044741	1.997587
235.634748	1179.426279	18.539904	-0.044708	1.991963
235.536673	1171.504145	18.544909	-0.044684	1.986336
235.378026	1163.604967	18.549914	-0.044650	1.980702
235.545897	1155.658778	18.554919	-0.044676	1.975053
235.304589	1147.753638	18.559923	-0.044626	1.969374
235.270926	1139.819399	18.564928	-0.044614	1.963680
235.260677	1131.924611	18.569933	-0.044608	1.958000
235.033907	1123.997598	18.574938	-0.044560	1.952257
234.941211	1116.043391	18.579943	-0.044538	1.946492
235.124185	1108.108389	18.584947	-0.044567	1.940753
234.935493	1100.215447	18.589952	-0.044527	1.934988
234.762741	1092.311731	18.594957	-0.044489	1.929199
234.839705	1084.379773	18.599962	-0.044499	1.923400
234.629656	1076.495815	18.604967	-0.044454	1.917586
234.566854	1068.585964	18.609971	-0.044438	1.911752
234.522533	1060.643064	18.614976	-0.044424	1.905878
234.720209	1052.714103	18.619981	-0.044456	1.900023
234.358322	1044.865460	18.624986	-0.044384	1.894147
234.552507	1036.893542	18.629991	-0.044415	1.888223
234.619390	1028.990152	18.634995	-0.044422	1.882318
234.286808	1021.137144	18.640000	-0.044355	1.876386
234.417976	1013.182902	18.645005	-0.044374	1.870412
234.298299	1005.280002	18.650010	-0.044347	1.864429
234.114997	997.411429	18.655015	-0.044308	1.858446
234.049275	989.497658	18.660019	-0.044291	1.852422
234.015180	981.574359	18.665024	-0.044279	1.846375
234.160636	973.670056	18.670029	-0.044301	1.840344
233.819356	965.824582	18.675034	-0.044233	1.834280
233.673100	957.903117	18.680039	-0.044200	1.828161
233.898639	949.977676	18.685043	-0.044237	1.822063
233.703793	942.106307	18.690048	-0.044196	1.815936
233.598822	934.215931	18.695053	-0.044171	1.809784
233.508235	926.317679	18.700058	-0.044149	1.803607
233.453728	918.440550	18.705063	-0.044134	1.797429
233.362526	910.516105	18.710067	-0.044112	1.791188
233.188014	902.606157	18.715072	-0.044074	1.784927
233.195882	894.730023	18.720077	-0.044071	1.778693
233.107472	886.831094	18.725082	-0.044049	1.772407
233.130430	878.917488	18.730087	-0.044048	1.766100
233.276340	871.032789	18.735091	-0.044071	1.759810
233.024503	863.171965	18.740096	-0.044019	1.753466
232.911752	855.296209	18.745101	-0.043993	1.747105
232.933493	847.401005	18.750106	-0.043992	1.740721
232.762728	839.550816	18.755111	-0.043955	1.734326
232.500420	831.694900	18.760115	-0.043901	1.727891
232.491441	823.796691	18.765120	-0.043894	1.721430
232.546460	815.922019	18.770125	-0.043899	1.714972
232.597086	808.000266	18.775130	-0.043904	1.708451
232.309714	800.157185	18.780135	-0.043845	1.701925
232.462824	792.266505	18.785139	-0.043869	1.695393
232.438057	784.372816	18.790144	-0.043859	1.688809
232.314999	776.530441	18.795149	-0.043831	1.682229
232.136365	768.690338	18.800154	-0.043793	1.675618
232.080421	760.804601	18.805159	-0.043777	1.668959
232.157804	752.932675	18.810163	-0.043787	1.662302
231.876551	745.093048	18.815168	-0.043729	1.655598
231.915680	737.214922	18.820173	-0.043731	1.648877
231.782350	729.372833	18.825178	-0.043701	1.642136
231.661915	721.529474	18.830183	-0.043674	1.635368
231.722663	713.590068	18.835187	-0.043680	1.628513
231.678448	705.728903	18.840192	-0.043667	1.621683
231.669229	697.884334	18.845197	-0.043660	1.614844
231.635757	690.022733	18.850202	-0.043649	1.607957
231.535854	682.188779	18.855207	-0.043625	1.601055
231.235138	674.400597	18.860211	-0.043564	1.594136
231.199114	666.519628	18.865216	-0.043553	1.587141
231.196680	658.675300	18.870221	-0.043547	1.580153
231.171806	650.834574	18.875226	-0.043537	1.573134
231.074705	642.986030	18.880231	-0.043514	1.566066
231.037302	635.184867	18.885235	-0.043502	1.559018
230.845785	627.343067	18.890240	-0.043462	1.551877
230.677313	619.511367	18.895245	-0.043425	1.544717
230.712281	611.669499	18.900250	-0.043427	1.537544
230.853415	603.794715	18.905255	-0.043448	1.530322
230.642708	596.008964	18.910259	-0.043404	1.523097
230.559415	588.189939	18.915264	-0.043383	1.515824
230.612659	580.343640	18.920269	-0.043388	1.508513
230.324331	572.563849	18.925274	-0.043329	1.501175
230.263477	564.748676	18.930279	-0.043313	1.493803
230.410915	556.899199	18.935283	-0.043335	1.486395
230.152172	549.132626	18.940288	-0.043282	1.478965
229.968743	541.315127	18.945293	-0.043243	1.471460
229.896121	533.478800	18.950298	-0.043225	1.463916
229.734161	525.695424	18.955303	-0.043189	1.456370
229.764187	517.873309	18.960307	-0.043190	1.448778
229.657235	510.077440	18.965312	-0.043165	1.441149
229.710384	502.280472	18.970317	-0.043170	1.433505
229.445815	494.509173	18.975322	-0.043116	1.425793
229.439783	486.719554	18.980327	-0.043110	1.418064
229.387946	478.932902	18.985331	-0.043095	1.410287
229.456687	471.127442	18.990336	-0.043103	1.402468
229.334415	463.381983	18.995341	-0.043075	1.394635
229.150044	455.594482	19.000346	-0.043036	1.386703
229.119682	447.817525	19.005351	-0.043025	1.378763
229.134309	440.038664	19.010355	-0.043023	1.370783
228.846791	432.304584	19.015360	-0.042964	1.362750
228.962105	424.531084	19.020365	-0.042981	1.354699
228.913330	416.752808	19.025370	-0.042967	1.346565
228.750148	409.026640	19.030375	-0.042931	1.338417
228.539048	401.308222	19.035379	-0.042887	1.330219
228.481623	393.553884	19.040384	-0.042871	1.321959
228.377111	385.801689	19.045389	-0.042847	1.313640
228.200026	377.968374	19.050394	-0.042809	1.305168
228.194968	370.244632	19.055399	-0.042803	1.296791
228.222069	362.509567	19.060403	-0.042803	1.288353
227.981365	354.821130	19.065408	-0.042753	1.279861
228.048953	347.098184	19.070413	-0.042761	1.271332
227.974468	339.389914	19.075418	-0.042742	1.262734
227.767694	331.715485	19.080423	-0.042699	1.254091
227.772078	323.996311	19.085427	-0.042695	1.245377
227.484868	316.354058	19.090432	-0.042636	1.236633
227.440030	308.648414	19.095437	-0.042623	1.227802
227.211147	300.988512	19.100442	-0.042575	1.218923
227.134510	293.303564	19.105447	-0.042556	1.209979
227.232136	285.613952	19.110451	-0.042569	1.200999
226.930862	277.992676	19.115456	-0.042508	1.191951
226.929629	270.321283	19.120461	-0.042503	1.182835
226.852052	262.673193	19.125466	-0.042484	1.173661
226.691164	255.039956	19.130471	-0.042449	1.164415
226.692892	247.406216	19.135475	-0.042445	1.155128
226.493052	239.749208	19.140480	-0.042402	1.145695
226.384243	232.139437	19.145485	-0.042377	1.136262
226.186698	224.537886	19.150490	-0.042336	1.126741
226.010398	216.951721	19.155495	-0.042298	1.117162
225.901031	209.359108	19.160499	-0.042273	1.107507
225.579582	201.805954	19.165504	-0.042208	1.097771
225.355248	194.242172	19.170509	-0.042161	1.087956
225.134173	186.697896	19.175514	-0.042115	1.078077
224.823800	179.153742	19.180519	-0.042053	1.068086
224.304501	171.667862	19.185523	-0.041951	1.058031
223.977543	164.139179	19.190528	-0.041886	1.047866
223.789316	156.622458	19.195533	-0.041846	1.037650
223.314329	149.148516	19.200538	-0.041752	1.027323
222.746808	141.701372	19.205543	-0.041642	1.016906
222.336705	134.233799	19.210547	-0.041561	1.006391
221.641541	126.829172	19.215552	-0.041427	0.995783
221.564136	119.285237	19.220557	-0.041407	0.985015
221.042020	111.874349	19.225562	-0.041305	0.974208
220.733121	104.429506	19.230567	-0.041243	0.963285
220.256619	97.047996	19.235571	-0.041150	0.952286
219.692756	89.674637	19.240576	-0.041040	0.941148
219.227201	82.309080	19.245581	-0.040949	0.929915
218.787928	74.956933	19.250586	-0.040862	0.918571
218.386569	67.599878	19.255591	-0.040783	0.907088
218.141163	60.483948	19.260595	-0.040732	0.895880