Fri Mar 12 11:33:48 2021


Number of Points = 3626

Depth (nm)	Load (N)	Time (s)	Disp. Voltage(V)	Force Voltage(V)
0.286570	0.056043	0.000000	0.000008	0.719371
0.418988	-0.021453	0.005005	-0.000016	0.719265
0.558485	-0.040375	0.010010	-0.000042	0.719276
0.418842	-0.020306	0.015014	-0.000016	0.719267
0.417683	-0.017699	0.020019	-0.000016	0.719271
0.611005	-0.051193	0.025024	-0.000052	0.719273
0.508795	-0.036129	0.030029	-0.000033	0.719266
0.559795	-0.039646	0.035034	-0.000042	0.719277
0.558805	-0.043203	0.040038	-0.000042	0.719270
0.480798	-0.027107	0.045043	-0.000027	0.719274
0.276339	0.007513	0.050048	0.000011	0.719270
0.347114	-0.006847	0.055053	-0.000002	0.719266
0.393770	-0.010065	0.060058	-0.000010	0.719276
0.280897	0.003139	0.065062	0.000011	0.719262
0.499447	-0.050478	0.070067	-0.000030	0.719233
0.449058	-0.178044	0.075072	-0.000020	0.718963
0.216494	-0.139327	0.080077	0.000023	0.718958
0.323205	-0.153402	0.085082	0.000003	0.718967
0.467810	-0.184390	0.090086	-0.000023	0.718957
0.455515	-0.178496	0.095091	-0.000021	0.718964
0.539511	-0.193864	0.100096	-0.000037	0.718963
0.438373	-0.270110	0.105101	-0.000018	0.718777
0.544787	-0.354516	0.110106	-0.000037	0.718647
0.419326	-0.336770	0.115110	-0.000014	0.718638
0.335398	-0.317723	0.120115	0.000002	0.718646
0.462784	-0.340345	0.125120	-0.000022	0.718646
0.566102	-0.456047	0.130125	-0.000041	0.718454
0.579659	-0.507722	0.135130	-0.000043	0.718356
0.394226	-0.479569	0.140134	-0.000008	0.718346
0.281775	-0.458802	0.145139	0.000013	0.718348
0.271428	-0.524743	0.150144	0.000015	0.718213
0.411759	-0.651127	0.155149	-0.000011	0.718013
0.613424	-0.683149	0.160154	-0.000049	0.718020
0.431033	-0.654033	0.165158	-0.000015	0.718014
0.388791	-0.760705	0.170163	-0.000007	0.717788
0.314413	-0.789682	0.175168	0.000007	0.717704
0.155156	-0.764605	0.180173	0.000037	0.717697
0.331445	-0.837791	0.185178	0.000004	0.717614
0.490738	-0.988900	0.190182	-0.000025	0.717372
0.495266	-0.985970	0.195187	-0.000026	0.717379
0.213544	-0.966111	0.200192	0.000027	0.717319
0.084051	-1.066085	0.205197	0.000051	0.717075
0.111422	-1.065529	0.210202	0.000046	0.717086
0.187193	-1.113004	0.215206	0.000032	0.717018
0.373021	-1.278951	0.220211	-0.000002	0.716755
0.280887	-1.261961	0.225216	0.000015	0.716756
0.420436	-1.363165	0.230221	-0.000011	0.716605
0.341664	-1.426213	0.235226	0.000004	0.716452
0.332148	-1.428433	0.240230	0.000006	0.716444
0.328914	-1.570250	0.245235	0.000007	0.716162
0.317943	-1.582610	0.250240	0.000009	0.716133
0.301136	-1.641519	0.255245	0.000012	0.716010
0.236748	-1.692334	0.260250	0.000024	0.715887
0.069941	-1.682560	0.265254	0.000055	0.715847
0.130035	-1.845144	0.270259	0.000044	0.715546
0.189773	-1.855444	0.275264	0.000033	0.715546
0.059079	-1.961272	0.280269	0.000058	0.715290
-0.049607	-1.969153	0.285274	0.000078	0.715236
0.007898	-2.074228	0.290278	0.000068	0.715047
0.021748	-2.147667	0.295283	0.000065	0.714906
-0.004904	-2.203338	0.300288	0.000070	0.714786
-0.359855	-2.232829	0.305293	0.000137	0.714602
-0.456859	-2.248581	0.310298	0.000155	0.714536
-0.768089	-2.326263	0.315302	0.000213	0.714271
-2.909684	-1.941274	0.320307	0.000612	0.714278
-2.399230	-2.138462	0.325312	0.000517	0.714067
-4.059486	-1.895903	0.330317	0.000826	0.713961
-3.497342	-1.988645	0.335322	0.000721	0.713975
-3.337497	-2.081268	0.340326	0.000692	0.713848
-5.009655	-1.881125	0.345331	0.001003	0.713653
-4.463481	-1.976916	0.350336	0.000902	0.713656
-4.568112	-1.962801	0.355341	0.000921	0.713647
-4.618703	-2.029793	0.360346	0.000931	0.713495
-5.612699	-1.921854	0.365350	0.001116	0.713357
-5.090717	-2.012945	0.370355	0.001019	0.713361
-5.152879	-2.000116	0.375360	0.001031	0.713364
-5.712731	-1.982304	0.380365	0.001135	0.713201
-6.252149	-1.972975	0.385370	0.001235	0.713028
-6.142580	-1.996824	0.390374	0.001215	0.713019
-6.410318	-1.948975	0.395379	0.001265	0.713020
-6.388312	-1.951104	0.400384	0.001261	0.713023
-6.483966	-2.061479	0.405389	0.001279	0.712769
-7.316326	-1.940901	0.410394	0.001434	0.712714
-7.683148	-1.878572	0.415398	0.001502	0.712707
-6.823920	-2.030935	0.420403	0.001343	0.712709
-6.945156	-2.008483	0.425408	0.001365	0.712710
-7.672080	-2.012041	0.430413	0.001501	0.712445
-7.993114	-1.983339	0.435418	0.001561	0.712388
-8.094219	-1.968902	0.440422	0.001580	0.712381
-8.015291	-1.980979	0.445427	0.001565	0.712384
-8.146525	-1.954864	0.450432	0.001590	0.712390
-8.068938	-2.013330	0.455437	0.001575	0.712300
-8.690620	-2.008218	0.460442	0.001691	0.712090
-9.157204	-1.928303	0.465446	0.001778	0.712083
-9.073729	-1.941975	0.470451	0.001763	0.712085
-8.782726	-1.990197	0.475456	0.001709	0.712092
-9.233410	-1.914408	0.480461	0.001793	0.712083
-9.143017	-1.974469	0.485466	0.001776	0.711995
-9.897666	-1.959786	0.490470	0.001917	0.711756
-9.635216	-2.004371	0.495475	0.001868	0.711760
-10.125312	-1.915644	0.500480	0.001959	0.711763
-9.948464	-1.950300	0.505485	0.001926	0.711756
-9.460473	-2.031082	0.510490	0.001836	0.711769
-10.191858	-1.915605	0.515494	0.001972	0.711739
-10.437581	-2.013200	0.520499	0.002018	0.711457
-10.378484	-2.024721	0.525504	0.002007	0.711454
-11.240331	-1.875266	0.530509	0.002167	0.711446
-10.919325	-1.927157	0.535514	0.002108	0.711456
-10.759988	-1.958927	0.540518	0.002078	0.711449
-10.944440	-1.924702	0.545523	0.002113	0.711452
-10.687986	-2.051559	0.550528	0.002065	0.711290
-11.806503	-1.931427	0.555533	0.002273	0.711132
-11.192522	-2.035451	0.560538	0.002159	0.711142
-11.801001	-1.930162	0.565542	0.002273	0.711136
-12.064866	-1.883897	0.570547	0.002322	0.711134
-11.427741	-1.995683	0.575552	0.002203	0.711137
-11.698945	-1.949675	0.580557	0.002254	0.711132
-11.961618	-2.023010	0.585562	0.002303	0.710892
-12.414630	-1.953163	0.590566	0.002387	0.710870
-12.564186	-1.926368	0.595571	0.002415	0.710871
-12.556583	-1.926288	0.600576	0.002414	0.710873
-12.610838	-1.920384	0.605581	0.002424	0.710865
-12.091372	-2.006163	0.610586	0.002328	0.710879
-12.328020	-2.047232	0.615590	0.002372	0.710712
-13.634108	-1.902586	0.620595	0.002615	0.710536
-12.972133	-2.018494	0.625600	0.002492	0.710540
-13.452651	-1.937681	0.630605	0.002582	0.710530
-13.561366	-1.913161	0.635610	0.002602	0.710540
-13.333072	-1.958858	0.640614	0.002560	0.710530
-13.312675	-1.961137	0.645619	0.002556	0.710533
-13.610066	-2.009855	0.650624	0.002611	0.710329
-14.479907	-1.912627	0.655629	0.002773	0.710214
-13.880611	-2.015533	0.660634	0.002662	0.710221
-14.262794	-1.951733	0.665638	0.002733	0.710212
-14.652216	-1.880666	0.670643	0.002806	0.710215
-13.994453	-1.996491	0.675648	0.002683	0.710218
-14.073532	-1.985613	0.680653	0.002698	0.710211
-14.562313	-2.033051	0.685658	0.002789	0.709942
-15.310088	-1.925723	0.690662	0.002929	0.709890
-14.878798	-2.000878	0.695667	0.002849	0.709893
-14.906675	-1.994048	0.700672	0.002854	0.709897
-15.448151	-1.902636	0.705677	0.002955	0.709887
-14.956308	-1.983937	0.710682	0.002863	0.709899
-15.022577	-1.981274	0.715686	0.002876	0.709881
-15.778440	-1.987406	0.720691	0.003017	0.709599
-15.902004	-1.965475	0.725696	0.003040	0.709598
-16.171991	-1.922677	0.730701	0.003090	0.709587
-15.985231	-1.953280	0.735706	0.003055	0.709593
-15.920190	-1.967576	0.740710	0.003043	0.709587
-15.840803	-1.979940	0.745715	0.003029	0.709590
-15.704347	-2.032913	0.750720	0.003004	0.709533
-16.843047	-1.966021	0.755725	0.003216	0.709260
-16.274794	-2.063797	0.760730	0.003110	0.709267
-16.804920	-1.972605	0.765734	0.003209	0.709260
-17.155431	-1.909016	0.770739	0.003274	0.709262
-16.768286	-1.976426	0.775744	0.003202	0.709265
-17.072020	-1.925894	0.780749	0.003259	0.709258
-16.849598	-2.004197	0.785754	0.003218	0.709180
-17.871766	-1.934958	0.790758	0.003408	0.708954
-17.660869	-1.971737	0.795763	0.003369	0.708956
-17.809034	-1.943939	0.800768	0.003396	0.708958
-17.948678	-1.922532	0.805773	0.003423	0.708951
-17.527785	-1.992099	0.810778	0.003344	0.708962
-17.846256	-1.938665	0.815782	0.003404	0.708955
-17.968268	-1.916385	0.820787	0.003427	0.708956
-18.232292	-2.020340	0.825792	0.003476	0.708653
-18.831891	-1.922916	0.830797	0.003588	0.708634
-18.594862	-1.960536	0.835802	0.003544	0.708643
-18.636783	-1.955063	0.840806	0.003551	0.708639
-18.709087	-1.942188	0.845811	0.003565	0.708639
-18.601844	-1.957416	0.850816	0.003545	0.708646
-18.717303	-1.941759	0.855821	0.003567	0.708636
-18.802507	-2.049429	0.860826	0.003583	0.708390
-19.463753	-1.951334	0.865830	0.003706	0.708350
-19.578558	-1.930884	0.870835	0.003727	0.708350
-19.006915	-2.030872	0.875840	0.003621	0.708353
-19.567949	-1.933732	0.880845	0.003726	0.708347
-19.519941	-1.937548	0.885850	0.003717	0.708357
-19.329815	-2.013044	0.890854	0.003682	0.708273
-20.299316	-1.967629	0.895859	0.003862	0.708018
-20.037975	-2.012547	0.900864	0.003814	0.708021
-20.544518	-1.927335	0.905869	0.003908	0.708010
-20.207157	-1.983116	0.910874	0.003845	0.708019
-20.180425	-1.989955	0.915878	0.003841	0.708014
-20.851071	-1.869965	0.920883	0.003965	0.708015
-20.249043	-2.016210	0.925888	0.003854	0.707937
-21.095348	-1.984475	0.930893	0.004011	0.707698
-20.910812	-2.013098	0.935898	0.003977	0.707706
-21.441323	-1.921235	0.940902	0.004076	0.707700
-21.288956	-1.945019	0.945907	0.004048	0.707707
-20.872731	-2.018791	0.950912	0.003970	0.707708
-21.509047	-1.911066	0.955917	0.004089	0.707696
-21.203291	-2.023319	0.960922	0.004032	0.707580
-22.286068	-1.930931	0.965926	0.004234	0.707378
-22.321534	-1.924426	0.970931	0.004240	0.707378
-22.010073	-1.977815	0.975936	0.004183	0.707382
-22.277303	-1.933655	0.980941	0.004232	0.707375
-21.968418	-1.986507	0.985946	0.004175	0.707379
-22.363791	-1.917989	0.990950	0.004249	0.707375
-22.146534	-1.968977	0.995955	0.004208	0.707350
-22.473033	-2.042461	1.000960	0.004269	0.707086
-23.197384	-1.916546	1.005965	0.004404	0.707079
-22.934109	-1.960103	1.010970	0.004355	0.707086
-22.722284	-1.999271	1.015974	0.004316	0.707083
-23.106164	-1.931439	1.020979	0.004388	0.707081
-23.067045	-1.936791	1.025984	0.004380	0.707084
-22.924479	-2.001790	1.030989	0.004354	0.707004
-23.680190	-1.989565	1.035994	0.004495	0.706758
-23.783493	-1.974194	1.040998	0.004514	0.706752
-24.092911	-1.918273	1.046003	0.004572	0.706753
-23.882946	-1.953612	1.051008	0.004533	0.706757
-24.199961	-1.900806	1.056013	0.004592	0.706750
-24.041435	-1.925422	1.061018	0.004563	0.706757
-23.774147	-1.979840	1.066022	0.004513	0.706743
-24.396338	-2.017313	1.071027	0.004629	0.706445
-24.781489	-1.946493	1.076032	0.004701	0.706449
-24.906345	-1.928443	1.081037	0.004724	0.706440
-24.390157	-2.015612	1.086042	0.004628	0.706450
-25.035463	-1.902963	1.091046	0.004748	0.706445
-25.106654	-1.890827	1.096051	0.004762	0.706443
-24.514431	-1.996678	1.101056	0.004652	0.706443
-25.666413	-1.948611	1.106061	0.004866	0.706126
-25.731945	-1.934960	1.111066	0.004879	0.706130
-25.684902	-1.946501	1.116070	0.004870	0.706123
-25.843905	-1.915257	1.121075	0.004900	0.706129
-25.737104	-1.933297	1.126080	0.004880	0.706131
-25.852133	-1.915248	1.131085	0.004901	0.706126
-25.392165	-1.993216	1.136090	0.004816	0.706134
-26.025658	-1.979014	1.141094	0.004934	0.705935
-26.886121	-1.862739	1.146099	0.005094	0.705860
-26.010551	-2.015029	1.151104	0.004931	0.705867
-26.433966	-1.943945	1.156109	0.005010	0.705858
-26.469343	-1.933071	1.161114	0.005017	0.705867
-26.395741	-1.948569	1.166118	0.005003	0.705862
-26.233227	-1.996411	1.171123	0.004973	0.705824
-27.213526	-1.967509	1.176128	0.005156	0.705531
-27.254035	-1.963208	1.181133	0.005164	0.705524
-27.218549	-1.966247	1.186138	0.005157	0.705531
-27.376489	-1.939150	1.191142	0.005187	0.705528
-27.263078	-1.960658	1.196147	0.005166	0.705526
-26.868918	-2.028957	1.201152	0.005092	0.705529
-27.386971	-2.025121	1.206157	0.005189	0.705351
-28.381848	-1.915398	1.211162	0.005374	0.705215
-27.961897	-1.992910	1.216166	0.005296	0.705209
-28.200656	-1.951559	1.221171	0.005341	0.705207
-28.295694	-1.931177	1.226176	0.005358	0.705213
-28.559783	-1.887326	1.231181	0.005408	0.705207
-28.043400	-1.977842	1.236186	0.005312	0.705209
-28.381114	-1.989793	1.241190	0.005375	0.705064
-29.575162	-1.866463	1.246195	0.005597	0.704883
-28.683915	-2.020983	1.251200	0.005431	0.704892
-29.168656	-1.939653	1.256205	0.005522	0.704882
-29.270075	-1.915925	1.261210	0.005541	0.704893
-28.994752	-1.968158	1.266214	0.005490	0.704886
-29.096939	-1.951346	1.271219	0.005509	0.704883
-29.146851	-1.997908	1.276224	0.005518	0.704771
-30.350181	-1.875360	1.281229	0.005742	0.704586
-29.716810	-1.985112	1.286234	0.005624	0.704592
-30.004050	-1.936238	1.291238	0.005678	0.704587
-30.346714	-1.875778	1.296243	0.005742	0.704585
-29.794947	-1.969548	1.301248	0.005639	0.704594
-29.943788	-1.945967	1.306253	0.005667	0.704588
-29.929275	-2.003061	1.311258	0.005665	0.704478
-31.002974	-1.920925	1.316262	0.005865	0.704258
-30.771727	-1.961660	1.321267	0.005822	0.704259
-30.734034	-1.965564	1.326272	0.005815	0.704264
-30.992814	-1.922071	1.331277	0.005863	0.704258
-30.588169	-1.992946	1.336282	0.005788	0.704261
-30.876120	-1.942239	1.341286	0.005841	0.704259
-31.061647	-1.973048	1.346291	0.005876	0.704130
-31.727312	-1.940108	1.351296	0.006000	0.703957
-31.395649	-2.003739	1.356301	0.005939	0.703948
-31.793642	-1.928729	1.361306	0.006013	0.703956
-31.731843	-1.942002	1.366310	0.006001	0.703951
-31.650570	-1.955187	1.371315	0.005986	0.703954
-31.622734	-1.957258	1.376320	0.005981	0.703959
-32.180791	-1.936903	1.381325	0.006085	0.703799
-32.709224	-1.923395	1.386330	0.006184	0.703636
-32.507782	-1.961952	1.391334	0.006146	0.703631
-32.814483	-1.907783	1.396339	0.006204	0.703629
-32.460193	-1.966821	1.401344	0.006138	0.703638
-32.385913	-1.983324	1.406349	0.006124	0.703631
-32.463846	-1.967661	1.411354	0.006139	0.703634
-32.783378	-1.983683	1.416358	0.006198	0.703487
-33.513101	-1.926553	1.421363	0.006334	0.703339
-33.200550	-1.980395	1.426368	0.006276	0.703343
-33.702906	-1.895555	1.431373	0.006370	0.703333
-33.531807	-1.921471	1.436378	0.006338	0.703342
-33.389525	-1.947507	1.441382	0.006312	0.703340
-33.562955	-1.917678	1.446387	0.006344	0.703338
-33.111039	-2.082770	1.451392	0.006260	0.703167
-34.269757	-1.959935	1.456397	0.006476	0.702998
-34.041822	-1.995717	1.461402	0.006434	0.703007
-34.079559	-1.991588	1.466406	0.006441	0.703002
-34.110693	-1.985158	1.471411	0.006447	0.703003
-33.757191	-2.045686	1.476416	0.006381	0.703008
-34.550879	-1.939385	1.481421	0.006529	0.702937
-35.177963	-1.948506	1.486426	0.006646	0.702692
-34.879825	-2.003491	1.491430	0.006590	0.702689
-35.440400	-1.903549	1.496435	0.006695	0.702688
-35.348993	-1.917192	1.501440	0.006678	0.702693
-35.019527	-1.980737	1.506445	0.006617	0.702684
-35.157680	-1.952059	1.511450	0.006642	0.702692
-35.054061	-1.994723	1.516454	0.006623	0.702642
-35.804926	-1.997626	1.521459	0.006763	0.702366
-35.679773	-2.015589	1.526464	0.006740	0.702374
-36.305738	-1.909738	1.531469	0.006857	0.702362
-35.986533	-1.962495	1.536474	0.006797	0.702371
-35.757181	-2.004559	1.541478	0.006755	0.702368
-36.370228	-1.896339	1.546483	0.006869	0.702366
-35.938527	-2.003785	1.551488	0.006789	0.702304
-36.944761	-1.943368	1.556493	0.006976	0.702063
-36.820966	-1.959933	1.561498	0.006953	0.702074
-37.176691	-1.897132	1.566502	0.007020	0.702072
-37.259102	-1.883142	1.571507	0.007035	0.702071
-36.904466	-1.944844	1.576512	0.006969	0.702074
-37.202399	-1.897556	1.581517	0.007025	0.702062
-36.905963	-1.944173	1.586522	0.006970	0.702074
-37.190960	-2.028172	1.591526	0.007023	0.701801
-38.235979	-1.871966	1.596531	0.007217	0.701740
-37.790496	-1.948134	1.601536	0.007135	0.701746
-37.675955	-1.972965	1.606541	0.007113	0.701737
-37.715901	-1.961918	1.611546	0.007121	0.701745
-37.917004	-1.929038	1.616550	0.007159	0.701739
-37.839132	-1.942626	1.621555	0.007144	0.701739
-37.898565	-2.050662	1.626560	0.007155	0.701499
-39.088445	-1.871922	1.631565	0.007377	0.701431
-38.964924	-1.890566	1.636570	0.007354	0.701437
-38.590887	-1.958315	1.641574	0.007285	0.701435
-38.895695	-1.904087	1.646579	0.007341	0.701435
-38.605585	-1.952938	1.651584	0.007288	0.701440
-38.707523	-1.939050	1.656589	0.007307	0.701431
-38.539650	-2.079703	1.661594	0.007276	0.701207
-39.653566	-1.924086	1.666598	0.007483	0.701120
-39.426124	-1.966658	1.671603	0.007441	0.701115
-39.084108	-2.022917	1.676608	0.007377	0.701125
-39.769150	-1.905778	1.681613	0.007505	0.701114
-39.416262	-1.964092	1.686618	0.007439	0.701124
-39.090850	-2.053921	1.691622	0.007379	0.701059
-40.354038	-1.923218	1.696627	0.007614	0.700867
-40.153782	-1.955009	1.701632	0.007577	0.700875
-40.378898	-1.918535	1.706637	0.007619	0.700867
-39.865431	-2.005525	1.711642	0.007523	0.700876
-40.061342	-1.971254	1.716646	0.007560	0.700875
-40.195115	-1.950491	1.721651	0.007585	0.700868
-40.162627	-2.096289	1.726656	0.007579	0.700584
-41.129072	-1.953139	1.731661	0.007759	0.700525
-41.258347	-1.926246	1.736666	0.007783	0.700532
-40.808531	-2.007164	1.741670	0.007700	0.700531
-41.302759	-1.921387	1.746675	0.007792	0.700526
-41.224822	-1.932831	1.751680	0.007777	0.700531
-41.318731	-1.939156	1.756685	0.007795	0.700484
-41.846514	-1.974684	1.761690	0.007893	0.700220
-42.118518	-1.929073	1.766694	0.007944	0.700214
-42.385888	-1.882710	1.771699	0.007994	0.700211
-41.839505	-1.976387	1.776704	0.007892	0.700219
-42.027549	-1.947865	1.781709	0.007928	0.700209
-42.241152	-1.905588	1.786714	0.007967	0.700217
-41.767241	-2.004928	1.791718	0.007879	0.700187
-42.779544	-1.970568	1.796723	0.008068	0.699890
-43.000904	-1.927832	1.801728	0.008109	0.699896
-43.439485	-1.853549	1.806733	0.008191	0.699888
-42.556870	-2.008270	1.811738	0.008027	0.699893
-42.747807	-1.974729	1.816742	0.008062	0.699892
-43.375108	-1.864829	1.821747	0.008179	0.699888
-42.799836	-1.964162	1.826752	0.008072	0.699894
-43.448814	-1.995183	1.831757	0.008193	0.699596
-43.995872	-1.897938	1.836762	0.008295	0.699595
-43.722992	-1.945421	1.841766	0.008245	0.699597
-43.603702	-1.969666	1.846771	0.008222	0.699591
-43.540352	-1.977052	1.851776	0.008211	0.699599
-43.878716	-1.920331	1.856781	0.008274	0.699591
-43.616536	-2.004045	1.861786	0.008225	0.699516
-44.569550	-1.957317	1.866790	0.008403	0.699266
-44.865956	-1.906385	1.871795	0.008458	0.699261
-44.424845	-1.979685	1.876800	0.008376	0.699272
-44.687608	-1.937674	1.881805	0.008425	0.699262
-44.619409	-1.947541	1.886810	0.008412	0.699267
-44.817002	-1.913502	1.891814	0.008449	0.699264
-44.710698	-1.959177	1.896819	0.008430	0.699209
-45.123031	-2.007743	1.901824	0.008507	0.698961
-45.530859	-1.940010	1.906829	0.008583	0.698951
-45.557196	-1.931443	1.911834	0.008588	0.698958
-45.222058	-1.991224	1.916838	0.008525	0.698958
-45.575847	-1.932630	1.921843	0.008591	0.698949
-45.212006	-1.991192	1.926848	0.008524	0.698961
-45.494169	-2.029827	1.931853	0.008576	0.698780
-46.585964	-1.903805	1.936858	0.008780	0.698641
-46.047814	-1.999450	1.941862	0.008680	0.698641
-46.096021	-1.994471	1.946867	0.008689	0.698633
-46.208851	-1.969366	1.951872	0.008710	0.698643
-46.586782	-1.906654	1.956877	0.008780	0.698634
-46.097102	-1.990506	1.961882	0.008689	0.698640
-46.451445	-2.050344	1.966886	0.008755	0.698390
-47.337853	-1.912789	1.971891	0.008920	0.698348
-47.129361	-1.945417	1.976896	0.008882	0.698357
-47.020184	-1.969696	1.981901	0.008862	0.698347
-47.042114	-1.962686	1.986906	0.008866	0.698353
-47.167431	-1.940306	1.991910	0.008889	0.698353
-47.171975	-1.971701	1.996915	0.008890	0.698287
-47.916110	-1.974110	2.001920	0.009029	0.698012
-47.818849	-1.990248	2.011917	0.009011	0.698014
-47.896938	-1.977569	2.021914	0.009026	0.698011
-47.843526	-1.985464	2.031910	0.009016	0.698014
-47.831024	-1.987406	2.041907	0.009014	0.698014
-48.062487	-1.947601	2.051904	0.009057	0.698011
-47.724196	-2.006576	2.061901	0.008994	0.698013
-47.992755	-1.957965	2.071898	0.009045	0.698014
-48.082495	-1.944052	2.081894	0.009062	0.698010
-48.012462	-1.956947	2.091891	0.009049	0.698008
-47.863889	-1.981239	2.101888	0.009021	0.698012
-47.883475	-1.977726	2.111885	0.009025	0.698012
-48.146246	-1.930264	2.121882	0.009074	0.698013
-47.999299	-1.956608	2.131878	0.009047	0.698012
-47.415998	-1.898591	2.141875	0.008939	0.698341
-47.170424	-1.938644	2.151872	0.008893	0.698349
-47.056384	-1.957851	2.161869	0.008872	0.698350
-47.157179	-1.940585	2.171866	0.008891	0.698349
-47.117422	-1.910882	2.181862	0.008884	0.698423
-46.339492	-1.946911	2.191859	0.008739	0.698631
-46.201984	-1.968996	2.201856	0.008714	0.698636
-46.116554	-1.983099	2.211853	0.008698	0.698638
-46.335624	-1.926094	2.221850	0.008739	0.698674
-45.413867	-1.954006	2.231846	0.008568	0.698951
-45.568540	-1.924287	2.241843	0.008597	0.698955
-45.368719	-1.959368	2.251840	0.008560	0.698955
-45.225367	-1.936722	2.261837	0.008534	0.699053
-44.315874	-1.994380	2.271834	0.008364	0.699265
-44.563981	-1.951036	2.281830	0.008411	0.699263
-44.797224	-1.908496	2.291827	0.008454	0.699264
-44.109237	-1.942743	2.301824	0.008327	0.699443
-43.580868	-1.960739	2.311821	0.008228	0.699598
-43.746043	-1.930262	2.321818	0.008259	0.699599
-43.651639	-1.947311	2.331814	0.008242	0.699598
-43.015838	-1.923796	2.341811	0.008124	0.699876
-42.604219	-1.987402	2.351808	0.008048	0.699895
-42.679260	-1.974155	2.361805	0.008062	0.699895
-42.642711	-1.951498	2.371802	0.008055	0.699953
-41.815489	-1.969635	2.381798	0.007901	0.700215
-41.851407	-1.963482	2.391795	0.007908	0.700214
-41.718258	-1.987863	2.401792	0.007884	0.700213
-41.389579	-1.951694	2.411789	0.007823	0.700405
-41.067588	-1.945841	2.421786	0.007763	0.700532
-41.009779	-1.956864	2.431782	0.007752	0.700530
-41.203159	-1.902121	2.441779	0.007789	0.700571
-40.019876	-1.966118	2.451776	0.007568	0.700869
-39.983260	-1.971935	2.461773	0.007562	0.700870
-40.003459	-1.967274	2.471770	0.007566	0.700871
-39.800328	-1.937980	2.481766	0.007528	0.701004
-39.403809	-1.951879	2.491763	0.007455	0.701118
-39.415031	-1.949049	2.501760	0.007457	0.701120
-39.454145	-1.906557	2.511757	0.007464	0.701191
-38.399141	-1.974673	2.521754	0.007268	0.701434
-38.575269	-1.943905	2.531750	0.007301	0.701432
-38.765569	-1.909374	2.541747	0.007337	0.701433
-37.715440	-1.952206	2.551744	0.007142	0.701725
-37.876100	-1.915121	2.561741	0.007172	0.701741
-37.339816	-2.009920	2.571738	0.007072	0.701743
-37.392470	-1.921409	2.581734	0.007082	0.701902
-36.583599	-1.981978	2.591731	0.006932	0.702071
-36.711592	-1.958674	2.601728	0.006956	0.702072
-36.812828	-1.939987	2.611725	0.006975	0.702072
-35.913905	-1.958031	2.621722	0.006808	0.702360
-36.053204	-1.929929	2.631718	0.006834	0.702366
-35.977278	-1.942599	2.641715	0.006820	0.702367
-35.580132	-1.915425	2.651712	0.006746	0.702565
-35.188818	-1.923267	2.661709	0.006674	0.702689
-35.225487	-1.916015	2.671706	0.006681	0.702690
-35.002052	-1.905788	2.681702	0.006639	0.702791
-34.197940	-1.946237	2.691699	0.006490	0.702999
-34.288252	-1.928376	2.701696	0.006507	0.703002
-34.152039	-1.951213	2.711693	0.006482	0.703004
-33.453820	-1.925058	2.721690	0.006352	0.703308
-33.534670	-1.895451	2.731686	0.006367	0.703338
-33.322412	-1.934053	2.741683	0.006328	0.703336
-33.169442	-1.889916	2.751680	0.006299	0.703480
-32.438403	-1.944492	2.761677	0.006164	0.703633
-32.576684	-1.919549	2.771674	0.006190	0.703633
-32.708127	-1.877274	2.781670	0.006214	0.703670
-31.745978	-1.911118	2.791667	0.006035	0.703948
-31.781891	-1.903652	2.801664	0.006042	0.703949
-31.739976	-1.909596	2.811661	0.006035	0.703952
-30.879738	-1.938777	2.821658	0.005875	0.704202
-30.870345	-1.912447	2.831654	0.005873	0.704258
-30.654734	-1.950676	2.841651	0.005833	0.704258
-30.886353	-1.864666	2.851648	0.005877	0.704348
-29.655616	-1.964127	2.861645	0.005648	0.704589
-29.748368	-1.947691	2.871642	0.005665	0.704589
-29.960676	-1.910638	2.881638	0.005705	0.704586
-29.417655	-1.905645	2.891635	0.005604	0.704791
-29.182768	-1.901488	2.901632	0.005560	0.704883
-28.891436	-1.951662	2.911629	0.005506	0.704887
-29.120047	-1.860095	2.921626	0.005549	0.704988
-28.155789	-1.921555	2.931622	0.005370	0.705210
-28.154161	-1.924157	2.941619	0.005370	0.705205
-28.211638	-1.913467	2.951616	0.005381	0.705206
-27.396573	-1.930000	2.961613	0.005229	0.705465
-27.384483	-1.901380	2.971610	0.005227	0.705526
-27.055786	-1.961241	2.981606	0.005166	0.705523
-27.237529	-1.893442	2.991603	0.005200	0.705594
-26.295618	-1.928547	3.001600	0.005025	0.705861
-26.190509	-1.945985	3.011597	0.005006	0.705863
-26.413740	-1.906719	3.021594	0.005048	0.705861
-25.966033	-1.897865	3.031590	0.004964	0.706039
-25.675893	-1.907473	3.041587	0.004911	0.706123
-25.804718	-1.881616	3.051584	0.004935	0.706129
-25.345262	-1.900133	3.061581	0.004849	0.706256
-24.459291	-1.964838	3.071578	0.004685	0.706443
-24.769344	-1.912119	3.081574	0.004743	0.706437
-24.737567	-1.916406	3.091571	0.004737	0.706440
-23.819757	-1.943497	3.101568	0.004566	0.706713
-23.723553	-1.943627	3.111565	0.004549	0.706747
-24.050505	-1.883696	3.121562	0.004610	0.706750
-23.643304	-1.887778	3.131558	0.004534	0.706887
-22.905022	-1.926064	3.141555	0.004397	0.707074
-22.994337	-1.909971	3.151552	0.004414	0.707074
-22.800386	-1.942892	3.161549	0.004378	0.707077
-22.393673	-1.880771	3.171546	0.004302	0.707347
-22.165848	-1.910420	3.181542	0.004260	0.707368
-22.278150	-1.890075	3.191539	0.004281	0.707369
-21.634087	-1.904095	3.201536	0.004162	0.707570
-21.109779	-1.934963	3.211533	0.004064	0.707695
-21.428459	-1.877561	3.221530	0.004124	0.707696
-21.033852	-1.933346	3.231526	0.004050	0.707725
-20.489509	-1.888334	3.241523	0.003949	0.708009
-20.288831	-1.924515	3.251520	0.003912	0.708008
-20.135517	-1.949799	3.261517	0.003884	0.708012
-19.891237	-1.901040	3.271514	0.003839	0.708196
-19.401226	-1.911615	3.281510	0.003748	0.708350
-19.504959	-1.894397	3.291507	0.003767	0.708347
-19.200862	-1.947334	3.301504	0.003711	0.708349
-18.697539	-1.899791	3.311501	0.003617	0.708623
-18.710402	-1.890655	3.321498	0.003620	0.708637
-18.262925	-1.970003	3.331494	0.003537	0.708637
-18.519783	-1.855490	3.341491	0.003585	0.708774
-17.530710	-1.941085	3.351488	0.003401	0.708956
-17.691090	-1.912720	3.361485	0.003431	0.708955
-17.879406	-1.872583	3.371482	0.003466	0.708967
-16.842771	-1.911526	3.381478	0.003273	0.709259
-16.654269	-1.944715	3.391475	0.003238	0.709259
-16.471245	-1.975170	3.401472	0.003205	0.709263
-16.541585	-1.911181	3.411469	0.003218	0.709366
-15.706454	-1.946122	3.421466	0.003063	0.709593
-15.544971	-1.975277	3.431462	0.003033	0.709592
-15.861249	-1.918504	3.441459	0.003092	0.709592
-15.329190	-1.934140	3.451456	0.002993	0.709750
-14.824087	-1.951831	3.461453	0.002899	0.709894
-14.956737	-1.927355	3.471450	0.002924	0.709896
-14.870952	-1.942589	3.481446	0.002908	0.709895
-14.158965	-1.909735	3.491443	0.002776	0.710214
-13.600647	-2.007888	3.501440	0.002672	0.710216
-14.074477	-1.923901	3.511437	0.002761	0.710215
-13.702767	-1.941551	3.521434	0.002692	0.710312
-12.936793	-1.968108	3.531430	0.002549	0.710531
-13.111090	-1.937737	3.541427	0.002582	0.710529
-12.859632	-1.981711	3.551424	0.002535	0.710530
-12.615037	-1.927530	3.561421	0.002490	0.710725
-12.103303	-1.944414	3.571418	0.002395	0.710873
-12.262569	-1.917035	3.581414	0.002425	0.710871
-11.970007	-1.969312	3.591411	0.002371	0.710870
-11.443054	-1.929448	3.601408	0.002273	0.711137
-11.365402	-1.941743	3.611405	0.002259	0.711139
-11.298511	-1.954196	3.621402	0.002246	0.711138
-11.064372	-1.894342	3.631398	0.002203	0.711340
-10.306841	-1.973253	3.641395	0.002062	0.711452
-10.389542	-1.956973	3.651392	0.002078	0.711454
-10.318562	-1.965218	3.661389	0.002065	0.711463
-9.290689	-1.998030	3.671386	0.001874	0.711762
-9.414896	-1.975216	3.681382	0.001897	0.711763
-9.470989	-1.967284	3.691379	0.001908	0.711758
-9.416890	-1.931553	3.701376	0.001898	0.711848
-8.541741	-1.965183	3.711373	0.001735	0.712092
-8.403988	-1.989753	3.721370	0.001710	0.712091
-8.981534	-1.886906	3.731366	0.001817	0.712091
-8.153232	-1.904766	3.741363	0.001663	0.712349
-7.837600	-1.943769	3.751360	0.001605	0.712383
-7.777577	-1.952841	3.761357	0.001594	0.712386
-7.286028	-1.955458	3.771354	0.001503	0.712554
-6.849803	-1.954398	3.781350	0.001422	0.712711
-6.875010	-1.951462	3.791347	0.001426	0.712707
-6.871137	-1.951667	3.801344	0.001426	0.712708
-5.925147	-1.980279	3.811341	0.001250	0.712986
-5.720740	-1.996736	3.821338	0.001212	0.713025
-5.815084	-1.980736	3.831334	0.001230	0.713023
-5.709719	-2.000242	3.841331	0.001211	0.713021
-4.918179	-1.971839	3.851328	0.001063	0.713358
-4.665519	-2.014287	3.861325	0.001017	0.713363
-4.622588	-2.022787	3.871322	0.001009	0.713361
-4.883534	-1.965592	3.881318	0.001058	0.713381
-4.128692	-1.962321	3.891315	0.000917	0.713655
-4.209013	-1.947918	3.901312	0.000932	0.713655
-3.917085	-1.997164	3.911309	0.000878	0.713660
-3.674825	-1.932906	3.921306	0.000833	0.713873
-3.229435	-1.961124	3.931302	0.000751	0.713974
-3.197996	-1.967851	3.941299	0.000745	0.713972
-3.125760	-1.952352	3.951296	0.000732	0.714027
-2.182682	-1.992237	3.961293	0.000556	0.714282
-2.153991	-1.995525	3.971290	0.000551	0.714285
-2.188923	-1.989012	3.981286	0.000558	0.714285
-2.014105	-1.934166	3.991283	0.000526	0.714455
-1.585433	-1.932829	4.001280	0.000446	0.714609
-1.609796	-1.926664	4.011277	0.000451	0.714612
-1.636262	-1.881586	4.021274	0.000456	0.714692
-1.511759	-1.793508	4.031270	0.000433	0.714911
-1.371381	-1.817439	4.041267	0.000407	0.714912
-1.495438	-1.686700	4.051264	0.000430	0.715127
-1.194693	-1.683771	4.061261	0.000375	0.715239
-1.122680	-1.638746	4.071258	0.000361	0.715353
-1.161196	-1.533347	4.081254	0.000369	0.715548
-0.899888	-1.532819	4.091251	0.000320	0.715641
-1.098120	-1.374796	4.101248	0.000357	0.715884
-0.930378	-1.347441	4.111245	0.000326	0.715997
-0.889403	-1.283571	4.121242	0.000319	0.716138
-0.685343	-1.206241	4.131238	0.000281	0.716363
-0.678488	-1.154134	4.141235	0.000280	0.716468
-0.543806	-1.032098	4.151232	0.000255	0.716756
-0.509077	-0.952190	4.161229	0.000249	0.716926
-0.290674	-0.909323	4.171226	0.000208	0.717088
-0.371245	-0.744905	4.181222	0.000223	0.717384
-0.363822	-0.649030	4.191219	0.000222	0.717576
-0.408941	-0.527915	4.201216	0.000231	0.717799
-0.204757	-0.447333	4.211213	0.000193	0.718030
-0.263659	-0.272095	4.221210	0.000204	0.718355
-0.264390	-0.149580	4.231206	0.000204	0.718596
-0.188408	-0.029204	4.241203	0.000190	0.718860
-0.067558	0.089173	4.251200	0.000168	0.719136
0.000000	0.239792	4.261197	0.000155	0.719456
-0.010363	0.862377	4.266202	0.000157	0.720679
0.094543	2.091975	4.271206	0.000137	0.723132
0.295778	3.911923	4.276211	0.000098	0.726763
0.451410	6.281576	4.281216	0.000068	0.731428
0.923936	9.117406	4.286221	-0.000022	0.737069
1.320104	12.430212	4.291226	-0.000098	0.743553
1.504203	16.243749	4.296230	-0.000135	0.750855
1.942531	20.420327	4.301235	-0.000219	0.758851
2.277403	24.998759	4.306240	-0.000284	0.767472
2.803229	29.934190	4.311245	-0.000385	0.776711
3.368139	35.190972	4.316250	-0.000494	0.786434
3.720825	40.817535	4.321254	-0.000563	0.796630
4.218306	46.711694	4.326259	-0.000659	0.807212
4.555641	52.921772	4.331264	-0.000726	0.818156
5.108990	59.367948	4.336269	-0.000833	0.829424
5.498558	66.068413	4.341274	-0.000910	0.840922
6.043963	72.962502	4.346278	-0.001016	0.852631
7.675926	79.879542	4.351283	-0.001324	0.864534
9.020115	87.054274	4.356288	-0.001579	0.876609
9.542047	94.560371	4.361293	-0.001681	0.888818
9.917059	102.230771	4.366298	-0.001756	0.901078
10.223383	110.069418	4.371302	-0.001818	0.913417
10.387730	118.036074	4.376307	-0.001853	0.925749
11.515169	125.943734	4.381312	-0.002068	0.938084
22.386162	132.387916	4.386317	-0.004096	0.950616
23.237255	140.755961	4.391322	-0.004260	0.963236
23.461497	149.301853	4.396326	-0.004307	0.975791
23.765066	157.881992	4.401331	-0.004369	0.988256
24.147659	166.485164	4.406336	-0.004446	1.000617
24.817737	175.060280	4.411341	-0.004576	1.012857
25.659688	183.620916	4.416346	-0.004739	1.024973
26.396970	192.244905	4.421350	-0.004882	1.037008
27.505863	200.815391	4.426355	-0.005093	1.048919
28.016018	209.514467	4.431360	-0.005194	1.060730
29.271753	218.123214	4.436365	-0.005433	1.072461
29.919201	226.813947	4.441370	-0.005559	1.084034
30.602209	235.523353	4.446374	-0.005692	1.095516
31.329055	244.213579	4.451379	-0.005833	1.106865
32.190767	252.871938	4.456384	-0.005999	1.118086
33.166948	261.514987	4.461389	-0.006186	1.129201
33.652744	270.236776	4.466394	-0.006282	1.140201
34.679439	278.882427	4.471398	-0.006479	1.151115
35.704623	287.504955	4.476403	-0.006675	1.161898
36.260370	296.181604	4.481408	-0.006784	1.172550
36.738545	304.859724	4.486413	-0.006879	1.183092
37.404532	313.491980	4.491418	-0.007009	1.193523
38.212511	322.073653	4.496422	-0.007165	1.203833
38.935094	330.672981	4.501427	-0.007305	1.214059
39.428318	339.274905	4.506432	-0.007402	1.224156
40.509930	347.808583	4.511437	-0.007609	1.234207
41.105389	356.363064	4.516442	-0.007725	1.244106
42.062365	364.865931	4.521446	-0.007909	1.253938
42.901450	373.372350	4.526451	-0.008070	1.263674
43.942014	381.846735	4.531456	-0.008270	1.273338
44.481556	390.387097	4.536461	-0.008375	1.282907
44.993485	398.913400	4.541466	-0.008476	1.292386
45.787832	407.371242	4.546470	-0.008630	1.301772
46.374450	415.931022	4.551475	-0.008744	1.311163
46.875959	424.446758	4.556480	-0.008843	1.320424
47.598074	432.859893	4.561485	-0.008983	1.329551
48.151442	441.288898	4.566490	-0.009091	1.338602
48.783537	449.690431	4.571494	-0.009214	1.347577
49.906862	458.033643	4.576499	-0.009429	1.356517
50.673861	466.396242	4.581504	-0.009577	1.365357
51.154441	474.835342	4.586509	-0.009672	1.374169
51.815863	483.187103	4.591514	-0.009800	1.382866
52.547356	491.554525	4.596518	-0.009942	1.391536
53.178114	499.923680	4.601523	-0.010065	1.400137
53.790943	508.259042	4.606528	-0.010184	1.408648
54.216687	516.652231	4.611533	-0.010269	1.417134
54.871614	524.959149	4.616538	-0.010396	1.425522
55.794801	533.253412	4.621542	-0.010573	1.433892
56.495155	541.568128	4.626547	-0.010709	1.442197
57.066196	549.889981	4.631552	-0.010821	1.450440
57.727448	558.209851	4.636557	-0.010949	1.458649
57.927628	566.570038	4.641562	-0.010992	1.466777
58.602241	574.905652	4.646566	-0.011123	1.474912
59.156080	583.187118	4.651571	-0.011231	1.482931
59.438886	591.496781	4.656576	-0.011289	1.490892
60.007614	599.775021	4.661581	-0.011400	1.498824
60.694456	608.002934	4.666586	-0.011533	1.506686
61.138171	616.302709	4.671590	-0.011621	1.514536
61.922096	624.525202	4.676595	-0.011772	1.522326
62.285171	632.802122	4.681600	-0.011845	1.530062
62.531346	641.124846	4.686605	-0.011896	1.537784
63.426004	649.290757	4.691610	-0.012068	1.545420
64.218504	657.545736	4.696614	-0.012221	1.553085
64.626142	665.798485	4.701619	-0.012302	1.560652
64.679818	674.083709	4.706624	-0.012318	1.568161
65.248481	682.317675	4.711629	-0.012429	1.575663
65.629548	690.543857	4.716634	-0.012505	1.583095
66.344028	698.730984	4.721638	-0.012643	1.590505
66.981001	706.947802	4.726643	-0.012767	1.597896
67.399295	715.160190	4.731648	-0.012850	1.605217
67.805240	723.410989	4.736653	-0.012931	1.612538
68.365683	731.603097	4.741658	-0.013041	1.619795
68.672469	739.838240	4.746662	-0.013103	1.627022
69.226985	748.103958	4.751667	-0.013211	1.634277
69.802384	756.260268	4.756672	-0.013324	1.641409
70.584076	764.410951	4.761677	-0.013475	1.648533
71.065823	772.611962	4.766682	-0.013569	1.655628
71.669441	780.776566	4.771686	-0.013687	1.662679
72.151671	788.989542	4.776691	-0.013782	1.669724
72.463260	797.196260	4.781696	-0.013845	1.676711
72.961454	805.380193	4.786701	-0.013943	1.683675
73.395355	813.562905	4.791706	-0.014029	1.690600
73.881625	821.762790	4.796710	-0.014125	1.697518
74.371500	829.939556	4.801715	-0.014222	1.704390
74.747861	838.139840	4.806720	-0.014297	1.711238
75.413355	846.315208	4.811725	-0.014426	1.718075
75.720325	854.469746	4.816730	-0.014488	1.724822
76.180774	862.661298	4.821734	-0.014579	1.731593
76.709980	870.820977	4.826739	-0.014683	1.738320
77.248762	878.943040	4.831744	-0.014789	1.744991
77.787171	887.117678	4.836749	-0.014894	1.751679
78.166697	895.294866	4.841754	-0.014970	1.758324
78.522619	903.445786	4.846758	-0.015041	1.764920
78.834294	911.637212	4.851763	-0.015105	1.771517
79.274576	919.781870	4.856768	-0.015192	1.778069
79.760737	927.925110	4.861773	-0.015288	1.784601
80.181510	936.112397	4.866778	-0.015371	1.791136
80.657729	944.287341	4.871782	-0.015465	1.797645
80.818398	952.454124	4.876787	-0.015500	1.804084
81.472072	960.535323	4.881792	-0.015627	1.810494
82.161554	968.662918	4.886797	-0.015761	1.816921
82.343379	976.827697	4.891802	-0.015800	1.823293
83.009368	984.938199	4.896806	-0.015929	1.829659
83.305187	993.112675	4.901811	-0.015989	1.836008
83.653290	1001.235196	4.906816	-0.016059	1.842301
83.994034	1009.400018	4.911821	-0.016128	1.848604
84.568272	1017.517389	4.916826	-0.016240	1.854877
84.849313	1025.666203	4.921830	-0.016297	1.861118
85.288910	1033.802982	4.926835	-0.016385	1.867348
85.800654	1041.946017	4.931840	-0.016485	1.873569
86.337218	1050.059969	4.936845	-0.016590	1.879751
86.646065	1058.183607	4.941850	-0.016653	1.885894
87.197573	1066.304026	4.946854	-0.016761	1.892042
87.513119	1074.459782	4.951859	-0.016825	1.898169
87.641230	1082.600479	4.956864	-0.016854	1.904244
87.907097	1090.761830	4.961869	-0.016908	1.910331
88.233510	1098.893184	4.966874	-0.016974	1.916383
88.761925	1106.968309	4.971878	-0.017078	1.922397
89.178150	1115.090807	4.976883	-0.017161	1.928414
89.739063	1123.188676	4.981888	-0.017270	1.934410
90.202724	1131.298778	4.986893	-0.017362	1.940386
90.529532	1139.421810	4.991898	-0.017428	1.946338
90.949280	1147.574365	4.996902	-0.017511	1.952303
91.350008	1155.708222	5.001907	-0.017591	1.958234
91.799433	1163.769046	5.006912	-0.017680	1.964100
92.330621	1171.863876	5.011917	-0.017784	1.969981
92.861533	1179.970550	5.016922	-0.017888	1.975853
93.073125	1188.099795	5.021926	-0.017932	1.981690
93.298843	1196.235319	5.026931	-0.017980	1.987516
93.653025	1204.351637	5.031936	-0.018051	1.993324
94.169569	1212.435202	5.036941	-0.018152	1.999109
94.517659	1220.525814	5.041946	-0.018222	2.004865
94.828767	1228.649007	5.046950	-0.018285	2.010623
95.245245	1236.772174	5.051955	-0.018368	2.016376
95.492929	1244.874239	5.056960	-0.018419	2.022080
95.913611	1252.975227	5.061965	-0.018503	2.027784
96.409811	1261.090958	5.066970	-0.018600	2.033491
96.994794	1269.147567	5.071974	-0.018714	2.039150
97.192172	1277.267972	5.076979	-0.018756	2.044797
97.513744	1285.367451	5.081984	-0.018821	2.050427
97.883491	1293.486945	5.086989	-0.018895	2.056060
98.449431	1301.551872	5.091994	-0.019006	2.061660
98.992731	1309.625854	5.096998	-0.019112	2.067249
99.351947	1317.756084	5.102003	-0.019184	2.072842
99.531245	1325.860735	5.107008	-0.019223	2.078385
99.922409	1333.970603	5.112013	-0.019301	2.083938
100.201082	1342.075668	5.117018	-0.019358	2.089461
100.621999	1350.175067	5.122022	-0.019441	2.094980
100.903187	1358.287456	5.127027	-0.019499	2.100480
100.994001	1366.386164	5.132032	-0.019521	2.105937
101.499696	1374.511687	5.137037	-0.019620	2.111438
101.635541	1382.643067	5.142042	-0.019651	2.116893
101.845722	1390.702174	5.147046	-0.019695	2.122293
102.301432	1398.757904	5.152051	-0.019785	2.127701
103.087512	1406.764405	5.157056	-0.019937	2.133093
103.885984	1414.810290	5.162061	-0.020090	2.138499
104.175728	1422.920048	5.167066	-0.020150	2.143885
104.372464	1431.044307	5.172070	-0.020191	2.149259
104.603955	1439.180763	5.177075	-0.020240	2.154630
105.018837	1447.220968	5.182080	-0.020322	2.159941
105.761436	1455.253199	5.187085	-0.020465	2.165265
106.124793	1463.356891	5.192090	-0.020538	2.170587
106.482666	1471.468812	5.197094	-0.020610	2.175901
107.024107	1479.538439	5.202099	-0.020716	2.181191
107.280365	1487.625564	5.207104	-0.020769	2.186454
107.657309	1495.750596	5.212109	-0.020844	2.191739
107.816831	1503.872943	5.217114	-0.020879	2.196990
108.189805	1511.919833	5.222118	-0.020954	2.202199
108.507389	1519.991192	5.227123	-0.021018	2.207407
108.631256	1528.092287	5.232128	-0.021046	2.212603
109.233067	1536.151934	5.237133	-0.021163	2.217804
109.774443	1544.189886	5.242138	-0.021269	2.222974
110.023666	1552.286441	5.247142	-0.021321	2.228142
110.380885	1560.399929	5.252147	-0.021393	2.233319
110.575947	1568.480093	5.257152	-0.021434	2.238448
111.028636	1576.528859	5.262157	-0.021524	2.243569
111.191480	1584.633784	5.267162	-0.021559	2.248687
111.885154	1592.682897	5.272166	-0.021693	2.253806
112.165971	1600.768331	5.277171	-0.021751	2.258899
112.621031	1608.828545	5.282176	-0.021841	2.263980
113.047765	1616.914383	5.287181	-0.021925	2.269063
113.358888	1625.085872	5.292186	-0.021988	2.274178
113.505281	1633.141555	5.297190	-0.022021	2.279195
113.807109	1641.193644	5.302195	-0.022082	2.284213
114.156533	1649.228549	5.307200	-0.022152	2.289212
114.563805	1657.315342	5.312205	-0.022233	2.294238
114.863488	1665.377604	5.317210	-0.022294	2.299228
115.132168	1673.442785	5.322214	-0.022349	2.304207
115.475968	1681.516584	5.327219	-0.022419	2.309186
115.642838	1689.616442	5.332224	-0.022455	2.314156
115.804703	1697.686659	5.337229	-0.022490	2.319097
116.341518	1705.712259	5.342234	-0.022595	2.324031
116.287111	1713.823020	5.347238	-0.022590	2.328957
116.834932	1721.885195	5.352243	-0.022697	2.333893
117.146860	1729.927700	5.357248	-0.022761	2.338787
117.656101	1737.981191	5.362253	-0.022861	2.343694
117.812037	1746.070501	5.367258	-0.022895	2.348583
118.002711	1754.199618	5.372262	-0.022935	2.353489
118.514314	1762.227766	5.377267	-0.023036	2.358349
118.655427	1770.274303	5.382272	-0.023067	2.363181
119.072774	1778.340187	5.387277	-0.023150	2.368037
119.123210	1786.446086	5.392282	-0.023165	2.372877
119.042095	1794.528777	5.397286	-0.023155	2.377683
119.358236	1802.589217	5.402291	-0.023219	2.382497
119.832529	1810.603363	5.407296	-0.023312	2.387287
120.199930	1818.689417	5.412301	-0.023386	2.392101
120.348686	1826.762480	5.417306	-0.023419	2.396881
120.863866	1834.767907	5.422310	-0.023520	2.401640
121.343344	1842.823801	5.427315	-0.023614	2.406416
121.648075	1850.899832	5.432320	-0.023676	2.411181
122.005486	1858.977054	5.437325	-0.023748	2.415942
122.420664	1867.024314	5.442330	-0.023830	2.420680
122.668809	1875.099558	5.447334	-0.023881	2.425411
122.876116	1883.225652	5.452339	-0.023925	2.430160
123.160033	1891.338592	5.457344	-0.023983	2.434898
123.259904	1899.392677	5.462349	-0.024007	2.439579
123.629373	1907.404432	5.467354	-0.024081	2.444246
124.064954	1915.434415	5.472358	-0.024167	2.448921
124.489071	1923.491556	5.477363	-0.024251	2.453600
124.581420	1931.572819	5.482368	-0.024274	2.458260
124.979490	1939.609100	5.487373	-0.024353	2.462908
125.423806	1947.658600	5.492378	-0.024441	2.467558
125.843380	1955.726259	5.497382	-0.024524	2.472208
126.001529	1963.825108	5.502387	-0.024559	2.476848
126.190173	1971.860498	5.507392	-0.024599	2.481445
126.412182	1979.910153	5.512397	-0.024645	2.486043
126.687840	1987.969008	5.517402	-0.024702	2.490643
126.841418	1996.052962	5.522406	-0.024736	2.495239
127.142405	2004.101964	5.527411	-0.024797	2.499818
127.405239	2012.130754	5.532416	-0.024851	2.504374
127.595132	2020.217255	5.537421	-0.024891	2.508949
127.728120	2028.319027	5.542426	-0.024921	2.513520
127.941256	2036.363071	5.547430	-0.024966	2.518056
128.435479	2044.367883	5.552435	-0.025063	2.522582
128.685449	2052.411973	5.557440	-0.025115	2.527105
129.252731	2060.433973	5.562445	-0.025226	2.531629
129.372544	2068.531460	5.567450	-0.025253	2.536156
129.520514	2076.589414	5.572454	-0.025286	2.540654
129.915398	2084.619080	5.577459	-0.025364	2.545147
130.198355	2092.692330	5.582464	-0.025422	2.549647
130.616690	2100.750723	5.587469	-0.025505	2.554141
130.967165	2108.781320	5.592474	-0.025576	2.558607
131.083722	2116.846991	5.597478	-0.025603	2.563068
131.561849	2124.892463	5.602483	-0.025697	2.567535
131.500192	2132.976873	5.607488	-0.025690	2.571978
131.787196	2141.046408	5.612493	-0.025749	2.576429
132.117304	2149.079922	5.617498	-0.025816	2.580856
132.314187	2157.122753	5.622502	-0.025857	2.585272
132.704519	2165.188101	5.627507	-0.025935	2.589705
132.971741	2173.426434	5.632512	-0.025990	2.594216
133.217215	2181.434074	5.637517	-0.026041	2.598593
133.515696	2189.413116	5.642522	-0.026102	2.602950
133.790324	2197.417898	5.647526	-0.026158	2.607312
134.197258	2205.459316	5.652531	-0.026239	2.611696
134.429012	2213.501871	5.657536	-0.026287	2.616061
135.006568	2221.507904	5.662541	-0.026400	2.620422
136.110535	2229.447982	5.667546	-0.026610	2.624775
136.518829	2237.508490	5.672550	-0.026692	2.629140
137.011218	2245.610659	5.677555	-0.026788	2.633525
137.300371	2253.661364	5.682560	-0.026847	2.637861
137.590767	2261.716006	5.687565	-0.026907	2.642193
137.751914	2269.804301	5.692570	-0.026942	2.646527
137.931737	2277.852145	5.697574	-0.026980	2.650834
138.209362	2285.936701	5.702579	-0.027037	2.655159
138.307344	2293.972859	5.707584	-0.027061	2.659440
138.834493	2302.009090	5.712589	-0.027164	2.663742
139.091291	2310.063275	5.717594	-0.027217	2.668028
139.139376	2318.148872	5.722598	-0.027231	2.672312
139.677863	2326.209217	5.727603	-0.027336	2.676606
139.942674	2334.215931	5.732608	-0.027391	2.680847
140.056525	2342.238930	5.737613	-0.027417	2.685081
140.254824	2350.296540	5.742618	-0.027459	2.689332
140.603188	2358.338803	5.747622	-0.027529	2.693577
140.913626	2366.415815	5.752627	-0.027592	2.697831
140.961878	2374.457312	5.757632	-0.027606	2.702044
141.317302	2382.499624	5.762637	-0.027678	2.706270
141.981130	2390.497997	5.767642	-0.027806	2.710485
142.061690	2398.594000	5.772646	-0.027826	2.714708
142.325277	2406.635752	5.777651	-0.027881	2.718908
142.503011	2414.659433	5.782656	-0.027919	2.723086
142.761117	2422.710679	5.787661	-0.027972	2.727278
143.046182	2430.768847	5.792666	-0.028030	2.731468
143.251983	2438.835069	5.797670	-0.028074	2.735650
143.428510	2446.896652	5.802675	-0.028112	2.739823
143.525824	2454.917566	5.807680	-0.028135	2.743963
143.853708	2462.984136	5.812685	-0.028201	2.748134
144.236951	2471.076088	5.817690	-0.028278	2.752315
144.305626	2479.146960	5.822694	-0.028296	2.756460
144.685503	2487.160526	5.827699	-0.028371	2.760589
144.947724	2495.132316	5.832704	-0.028425	2.764682
145.166344	2503.181128	5.837709	-0.028471	2.768806
145.203432	2511.257173	5.842714	-0.028483	2.772927
145.435783	2519.278907	5.847718	-0.028532	2.777026
145.944366	2527.316691	5.852723	-0.028631	2.781144
145.988620	2535.332708	5.857728	-0.028645	2.785216
146.262277	2543.390540	5.862733	-0.028701	2.789318
146.621216	2551.457910	5.867738	-0.028773	2.793423
146.766893	2559.482314	5.872742	-0.028805	2.797488
147.075060	2567.512079	5.877747	-0.028868	2.801559
147.354836	2575.532185	5.882752	-0.028925	2.805617
147.707932	2583.581074	5.887757	-0.028996	2.809689
147.772806	2591.671252	5.892762	-0.029013	2.813758
147.991739	2599.705697	5.897766	-0.029059	2.817803
148.448276	2607.747657	5.902771	-0.029149	2.821859
148.596284	2615.768687	5.907776	-0.029182	2.825881
149.153091	2623.815826	5.912781	-0.029291	2.829934
149.546329	2631.904109	5.917786	-0.029369	2.833992
150.036019	2639.894159	5.922790	-0.029465	2.838000
150.552965	2647.926596	5.927795	-0.029567	2.842026
150.864879	2655.948690	5.932800	-0.029630	2.846029
151.125026	2663.981821	5.937805	-0.029683	2.850029
153.331773	2671.865672	5.942810	-0.030099	2.854058
154.613173	2679.849240	5.947814	-0.030343	2.858079
154.933649	2687.970061	5.952819	-0.030408	2.862108
155.105639	2696.059034	5.957824	-0.030445	2.866108
155.352618	2704.134502	5.962829	-0.030496	2.870099
155.774554	2712.223350	5.967834	-0.030580	2.874101
155.802200	2720.280034	5.972838	-0.030590	2.878060
156.166651	2728.321699	5.977843	-0.030663	2.882025
156.573203	2736.341252	5.982848	-0.030744	2.885975
156.844273	2744.389647	5.987853	-0.030800	2.889927
156.853634	2752.509614	5.992858	-0.030806	2.893894
157.292303	2760.499646	5.997862	-0.030893	2.897816
157.893123	2768.539235	6.002867	-0.031010	2.901765
158.234530	2776.537210	6.007872	-0.031079	2.905674
158.657457	2784.586028	6.012877	-0.031163	2.909607
158.861376	2792.737047	6.017882	-0.031206	2.913573
159.136919	2800.750211	6.022886	-0.031262	2.917470
159.647406	2808.745248	6.027891	-0.031363	2.921366
159.918087	2816.743875	6.032896	-0.031418	2.925245
160.194902	2824.794032	6.037901	-0.031475	2.929145
160.211070	2832.896473	6.042906	-0.031483	2.933050
160.242034	2840.933471	6.047910	-0.031494	2.936920
160.791309	2848.931899	6.052915	-0.031601	2.940793
160.960042	2856.948622	6.057920	-0.031638	2.944650
161.134847	2864.996800	6.062925	-0.031675	2.948517
161.494991	2873.064318	6.067930	-0.031748	2.952398
161.570670	2881.113891	6.072934	-0.031767	2.956251
161.814778	2889.133623	6.077939	-0.031817	2.960093
162.072945	2897.122437	6.082944	-0.031871	2.963916
162.413509	2905.169931	6.087949	-0.031939	2.967766
162.476425	2913.254529	6.092954	-0.031956	2.971614
162.751416	2921.290794	6.097958	-0.032012	2.975446
162.905369	2929.323492	6.102963	-0.032046	2.979264
163.290954	2937.333990	6.107968	-0.032123	2.983079
163.605326	2945.372428	6.112973	-0.032187	2.986898
163.853476	2953.423732	6.117978	-0.032238	2.990716
163.979520	2961.503696	6.122982	-0.032267	2.994535
164.293961	2969.522427	6.127987	-0.032330	2.998331
164.545036	2977.516373	6.132992	-0.032382	3.002107
164.940018	2985.540571	6.137997	-0.032461	3.005899
165.170968	2993.565760	6.143002	-0.032509	3.009679
165.221679	3001.638074	6.148006	-0.032524	3.013467
165.502118	3009.674495	6.153011	-0.032581	3.017245
165.737018	3017.697857	6.158016	-0.032630	3.021010
166.211498	3025.699656	6.163021	-0.032723	3.024771
166.556226	3033.755318	6.168026	-0.032793	3.028547
167.032307	3041.782756	6.173030	-0.032886	3.032311
167.368498	3049.859780	6.178035	-0.032954	3.036087
167.865342	3057.841690	6.183040	-0.033052	3.039822
168.234174	3065.867104	6.188045	-0.033125	3.043565
168.621214	3073.903414	6.193050	-0.033203	3.047311
169.123392	3081.937279	6.198054	-0.033301	3.051055
169.595029	3089.995228	6.203059	-0.033394	3.054805
169.721930	3098.025015	6.208064	-0.033423	3.058521
169.927305	3106.085709	6.213069	-0.033466	3.062250
170.410497	3114.094720	6.218074	-0.033561	3.065964
170.664611	3122.126220	6.223078	-0.033614	3.069673
171.120425	3130.247587	6.228083	-0.033704	3.073428
171.251196	3138.272033	6.233088	-0.033733	3.077119
171.610420	3146.265295	6.238093	-0.033805	3.080802
172.026567	3154.275505	6.243098	-0.033888	3.084491
172.117788	3162.304470	6.248102	-0.033910	3.088168
172.691865	3170.346298	6.253107	-0.034022	3.091870
172.768556	3178.398869	6.258112	-0.034042	3.095549
173.007374	3186.418049	6.263117	-0.034091	3.099215
173.058808	3194.474568	6.268122	-0.034106	3.102886
173.344302	3202.481513	6.273126	-0.034164	3.106541
174.051090	3210.507521	6.278131	-0.034301	3.110219
174.297246	3218.570740	6.283136	-0.034352	3.113889
174.585403	3226.595308	6.288141	-0.034411	3.117538
174.801193	3234.662845	6.293146	-0.034456	3.121200
175.113827	3242.617750	6.298150	-0.034519	3.124810
175.536309	3250.692896	6.303155	-0.034603	3.128476
175.852919	3258.724474	6.308160	-0.034667	3.132113
176.033552	3266.787967	6.313165	-0.034706	3.135754
176.194251	3274.798333	6.318170	-0.034741	3.139365
176.509371	3282.813974	6.323174	-0.034805	3.142982
176.658174	3290.862263	6.328179	-0.034838	3.146602
176.803670	3298.886094	6.333184	-0.034870	3.150207
177.222788	3306.934340	6.338189	-0.034953	3.153830
177.256968	3315.021862	6.343194	-0.034964	3.157450
177.288044	3323.007853	6.348198	-0.034975	3.161021
177.668666	3331.010281	6.353203	-0.035051	3.164609
178.030741	3339.023785	6.358208	-0.035124	3.168198
178.133731	3347.107359	6.363213	-0.035148	3.171803
178.430104	3355.130989	6.368218	-0.035208	3.175385
179.022703	3363.109326	6.373222	-0.035324	3.178955
179.380413	3371.161009	6.378227	-0.035396	3.182545
179.524376	3379.192422	6.383232	-0.035428	3.186111
179.905158	3387.213090	6.388237	-0.035504	3.189680
180.305635	3395.265067	6.393242	-0.035583	3.193258
180.467962	3403.304422	6.398246	-0.035619	3.196817
180.809636	3411.319502	6.403251	-0.035687	3.200369
181.154963	3419.331271	6.408256	-0.035757	3.203916
181.404115	3427.373256	6.413261	-0.035808	3.207468
181.820505	3435.418432	6.418266	-0.035891	3.211024
182.156539	3443.461831	6.423270	-0.035959	3.214572
182.387054	3451.502863	6.428275	-0.036007	3.218111
182.482243	3459.524956	6.433280	-0.036030	3.221632
182.693341	3467.537177	6.438285	-0.036074	3.225150
183.024023	3475.601346	6.443290	-0.036141	3.228691
183.223008	3483.646076	6.448294	-0.036183	3.232214
183.574936	3491.706923	6.453299	-0.036254	3.235747
184.080781	3499.658585	6.458304	-0.036353	3.239235
184.497177	3507.664654	6.463309	-0.036435	3.242739
184.945840	3515.677328	6.468314	-0.036524	3.246243
185.175814	3523.686007	6.473318	-0.036572	3.249733
185.512908	3531.789246	6.478323	-0.036640	3.253264
185.812571	3539.782448	6.483328	-0.036701	3.256742
186.064652	3547.814671	6.488333	-0.036753	3.260232
186.243022	3555.862376	6.493338	-0.036791	3.263721
186.420295	3563.894317	6.498342	-0.036829	3.267200
186.949794	3571.944051	6.503347	-0.036933	3.270696
186.930777	3580.005467	6.508352	-0.036935	3.274173
187.139318	3588.018553	6.513357	-0.036979	3.277634
187.336682	3596.055017	6.518362	-0.037021	3.281100
187.464216	3604.016305	6.523366	-0.037049	3.284528
187.728264	3612.098761	6.528371	-0.037104	3.288010
187.977016	3620.112667	6.533376	-0.037155	3.291458
188.154914	3628.153124	6.538381	-0.037193	3.294911
188.458281	3636.184304	6.543386	-0.037255	3.298361
188.636752	3644.188467	6.548390	-0.037293	3.301791
188.699859	3652.225956	6.553395	-0.037310	3.305227
188.998637	3660.239898	6.558400	-0.037371	3.308659
189.268451	3668.310306	6.563405	-0.037426	3.312110
189.491514	3676.388277	6.568410	-0.037473	3.315559
189.777176	3684.354710	6.573414	-0.037531	3.318959
190.344020	3692.348751	6.578419	-0.037642	3.322378
190.389863	3700.359636	6.583424	-0.037656	3.325781
190.617634	3708.395182	6.588429	-0.037703	3.329198
190.861236	3716.465727	6.593434	-0.037754	3.332626
191.025483	3724.499248	6.598438	-0.037789	3.336033
191.185758	3732.529592	6.603443	-0.037824	3.339434
191.340599	3740.533185	6.608448	-0.037858	3.342821
191.580560	3748.559050	6.613453	-0.037908	3.346216
191.883690	3756.583270	6.618458	-0.037970	3.349610
191.926042	3764.667249	6.623462	-0.037983	3.353016
192.467157	3772.714231	6.628467	-0.038089	3.356420
192.658360	3780.684554	6.633472	-0.038129	3.359777
192.727177	3788.726278	6.638477	-0.038147	3.363156
193.037960	3796.730822	6.643482	-0.038210	3.366524
193.300758	3804.732729	6.648486	-0.038264	3.369886
193.517431	3812.825049	6.653491	-0.038310	3.373281
193.888675	3820.845997	6.658496	-0.038384	3.376648
194.074008	3828.858013	6.663501	-0.038424	3.380001
194.499588	3836.889920	6.668506	-0.038508	3.383368
194.524798	3844.939138	6.673510	-0.038518	3.386724
194.883920	3852.942713	6.678515	-0.038590	3.390070
194.817688	3861.050955	6.683520	-0.038583	3.393441
194.964165	3869.097534	6.688525	-0.038615	3.396791
195.567581	3877.024364	6.693530	-0.038732	3.400103
195.698010	3885.015282	6.698534	-0.038762	3.403423
195.869308	3893.081513	6.703539	-0.038799	3.406771
196.062737	3901.059621	6.708544	-0.038840	3.410081
196.659335	3909.081619	6.713549	-0.038956	3.413419
196.947078	3917.164528	6.718554	-0.039015	3.416769
197.099480	3925.150150	6.723558	-0.039048	3.420071
197.523878	3933.168130	6.728563	-0.039132	3.423391
197.802961	3941.191634	6.733568	-0.039190	3.426706
197.842887	3949.250235	6.738573	-0.039202	3.430024
198.031579	3957.320454	6.743578	-0.039242	3.433349
198.276757	3965.322507	6.748582	-0.039293	3.436644
198.491984	3973.337843	6.753587	-0.039338	3.439941
198.647891	3981.355125	6.758592	-0.039373	3.443233
199.013325	3989.392932	6.763597	-0.039446	3.446537
199.215450	3997.416711	6.768602	-0.039488	3.449827
199.363585	4005.476287	6.773606	-0.039521	3.453127
199.841792	4013.524761	6.778611	-0.039615	3.456430
200.082261	4021.483869	6.783616	-0.039665	3.459685
200.362007	4029.534802	6.788621	-0.039722	3.462976
200.480541	4037.571115	6.793626	-0.039750	3.466252
200.860851	4045.580434	6.798630	-0.039826	3.469523
201.156171	4053.661879	6.803635	-0.039886	3.472818
201.262188	4061.673838	6.808640	-0.039911	3.476075
201.400659	4069.653846	6.813645	-0.039941	3.479317
201.713727	4077.664593	6.818650	-0.040005	3.482573
201.781741	4085.688377	6.823654	-0.040023	3.485825
202.028327	4093.718807	6.828659	-0.040074	3.489081
202.290753	4101.778033	6.833664	-0.040128	3.492347
202.327109	4109.823901	6.838669	-0.040140	3.495597
202.680276	4117.803835	6.843674	-0.040210	3.498827
202.975328	4125.822951	6.848678	-0.040270	3.502068
203.193707	4133.828430	6.853683	-0.040316	3.505299
203.329172	4141.847808	6.858688	-0.040347	3.508529
203.662977	4149.921528	6.863693	-0.040414	3.511784
203.853205	4157.961046	6.868698	-0.040454	3.515018
203.779603	4165.936424	6.873702	-0.040446	3.518216
204.233337	4174.001038	6.878707	-0.040535	3.521462
204.430628	4181.946235	6.883712	-0.040577	3.524650
204.597137	4190.018171	6.888717	-0.040613	3.527884
204.886795	4198.070277	6.893722	-0.040672	3.531111
205.328862	4206.077678	6.898726	-0.040760	3.534322
205.642359	4214.122635	6.903731	-0.040823	3.537541
205.743389	4222.148760	6.908736	-0.040847	3.540743
205.949150	4230.166492	6.913741	-0.040891	3.543943
206.187339	4238.226822	6.918746	-0.040940	3.547157
206.232959	4246.215468	6.923750	-0.040954	3.550334
206.662331	4254.358068	6.928755	-0.041039	3.553580
206.927312	4262.383573	6.933760	-0.041093	3.556772
207.014144	4270.315385	6.938765	-0.041115	3.559919
207.322558	4278.330924	6.943770	-0.041177	3.563103
207.654932	4286.315705	6.948774	-0.041244	3.566273
207.811079	4294.361792	6.953779	-0.041278	3.569458
208.044879	4302.369912	6.958784	-0.041327	3.572628
208.409434	4310.397057	6.963789	-0.041400	3.575807
208.761738	4318.395182	6.968794	-0.041471	3.578971
208.733304	4326.448878	6.973798	-0.041471	3.582143
209.182315	4334.478221	6.978803	-0.041559	3.585316
209.629791	4342.474493	6.983808	-0.041648	3.588473
209.812216	4350.542467	6.988813	-0.041687	3.591648
210.016716	4358.587436	6.993818	-0.041730	3.594812
210.220885	4366.569536	6.998822	-0.041773	3.597949
210.537800	4374.573740	7.003827	-0.041837	3.601094
210.641249	4382.585979	7.008832	-0.041862	3.604234
210.690090	4390.642683	7.013837	-0.041876	3.607387
211.016901	4398.656351	7.018842	-0.041942	3.610528
211.169226	4406.708709	7.023846	-0.041975	3.613676
211.440816	4414.773350	7.028851	-0.042031	3.616830
211.569772	4422.743832	7.033856	-0.042060	3.619941
211.644114	4430.752338	7.038861	-0.042079	3.623062
211.832685	4438.797510	7.043866	-0.042119	3.626197
212.216335	4446.780678	7.048870	-0.042196	3.629312
212.508463	4454.913144	7.053875	-0.042255	3.632479
212.217792	4462.949283	7.058880	-0.042206	3.635590
212.469455	4470.906284	7.063885	-0.042258	3.638682
212.804299	4478.949069	7.068890	-0.042326	3.641807
212.955599	4486.897802	7.073894	-0.042359	3.644888
213.245948	4494.969755	7.078899	-0.042418	3.648018
213.324687	4502.994574	7.083904	-0.042438	3.651121
213.503751	4511.046105	7.088909	-0.042477	3.654235
213.644689	4519.088565	7.093914	-0.042508	3.657341
213.848819	4527.055854	7.098918	-0.042551	3.660418
214.281004	4535.079377	7.103923	-0.042637	3.663519
214.424606	4543.101789	7.108928	-0.042669	3.666610
214.742839	4551.103848	7.113933	-0.042733	3.669695
215.207394	4559.168010	7.118938	-0.042825	3.672805
215.250285	4567.191770	7.123942	-0.042838	3.675885
215.491350	4575.197658	7.128947	-0.042888	3.678962
215.860379	4583.218963	7.133952	-0.042961	3.682045
216.263735	4591.193488	7.138957	-0.043042	3.685108
216.369624	4599.260651	7.143962	-0.043067	3.688197
216.553955	4607.300855	7.148966	-0.043106	3.691274
216.893051	4615.326229	7.153971	-0.043174	3.694348
217.193552	4623.330688	7.158976	-0.043235	3.697409
217.237172	4631.359537	7.163981	-0.043249	3.700471
217.598315	4639.388302	7.168986	-0.043321	3.703539
217.740576	4647.382315	7.173990	-0.043352	3.706585
217.966620	4655.409575	7.178995	-0.043400	3.709643
218.096912	4663.522085	7.184000	-0.043429	3.712729
218.343095	4671.547567	7.189005	-0.043480	3.715782
218.545821	4679.519159	7.194010	-0.043523	3.718811
218.877904	4687.516259	7.199014	-0.043590	3.721850
219.187599	4695.502509	7.204019	-0.043653	3.724882
219.730154	4703.523513	7.209024	-0.043759	3.727931
220.058079	4711.521989	7.214029	-0.043825	3.730963
220.419669	4719.587826	7.219034	-0.043897	3.734019
220.865027	4727.598065	7.224038	-0.043985	3.737053
221.212675	4735.627783	7.229043	-0.044055	3.740090
221.520370	4743.642657	7.234048	-0.044118	3.743117
221.986687	4751.674992	7.239053	-0.044210	3.746153
222.108788	4759.758728	7.244058	-0.044238	3.749197
222.381714	4767.759978	7.249062	-0.044293	3.752211
222.618085	4775.815781	7.254067	-0.044343	3.755243
222.954351	4783.803808	7.259072	-0.044410	3.758249
222.973321	4791.817056	7.264077	-0.044419	3.761254
223.558642	4799.846200	7.269082	-0.044533	3.764276
223.786292	4807.856359	7.274086	-0.044581	3.767281
223.990835	4815.911160	7.279091	-0.044624	3.770299
224.220652	4823.945911	7.284096	-0.044672	3.773307
224.401069	4831.955052	7.289101	-0.044710	3.776303
224.598593	4839.979649	7.294106	-0.044752	3.779302
224.843538	4847.958449	7.299110	-0.044803	3.782283
225.179201	4855.976779	7.304115	-0.044871	3.785278
225.479408	4863.997860	7.309120	-0.044932	3.788271
225.590256	4872.025778	7.314125	-0.044957	3.791260
225.995734	4880.119907	7.319130	-0.045038	3.794278
226.099645	4888.086298	7.324134	-0.045062	3.797239
226.190019	4896.125397	7.329139	-0.045084	3.800225
226.526758	4904.090701	7.334144	-0.045152	3.803186
226.712808	4912.115016	7.339149	-0.045192	3.806164
226.927301	4920.133921	7.344154	-0.045237	3.809137
226.949613	4928.210046	7.349158	-0.045246	3.812126
227.078320	4936.217925	7.354163	-0.045275	3.815089
227.234953	4944.255844	7.359168	-0.045310	3.818061
227.494870	4952.216309	7.364173	-0.045363	3.821005
227.920651	4960.258197	7.369178	-0.045448	3.823980
228.174453	4968.236710	7.374182	-0.045500	3.826926
228.427356	4976.299568	7.379187	-0.045552	3.829900
228.617346	4984.335885	7.384192	-0.045593	3.832861
228.807218	4992.330940	7.389197	-0.045633	3.835804
229.090840	5000.352443	7.394202	-0.045691	3.838757
229.025764	5008.403253	7.399206	-0.045684	3.841711
229.228218	5016.389059	7.404211	-0.045727	3.844645
229.523609	5024.401433	7.409216	-0.045787	3.847587
229.552444	5032.440019	7.414221	-0.045797	3.850532
229.907944	5040.509343	7.419226	-0.045869	3.853492
230.166823	5048.519481	7.424230	-0.045922	3.856427
230.424755	5056.515377	7.429235	-0.045975	3.859354
230.653144	5064.568693	7.434240	-0.046023	3.862299
230.890948	5072.537007	7.439245	-0.046072	3.865210
230.977610	5080.611335	7.444250	-0.046094	3.868156
231.167309	5088.640831	7.449254	-0.046134	3.871084
231.341695	5096.898693	7.454259	-0.046172	3.874094
231.657624	5104.873788	7.459264	-0.046236	3.877001
231.707308	5112.734386	7.464269	-0.046250	3.879859
231.917725	5120.772803	7.469274	-0.046294	3.882782
232.327370	5128.709510	7.474278	-0.046376	3.885670
232.565615	5136.738918	7.479283	-0.046425	3.888586
232.836776	5144.772721	7.484288	-0.046481	3.891503
233.132509	5152.829494	7.489293	-0.046541	3.894426
233.356595	5160.832336	7.494298	-0.046588	3.897325
233.569796	5168.778749	7.499302	-0.046633	3.900202
233.815654	5176.848727	7.504307	-0.046683	3.903122
233.808089	5184.875726	7.509312	-0.046687	3.906020
233.894491	5192.874391	7.514317	-0.046708	3.908907
234.333281	5200.919775	7.519322	-0.046795	3.911815
234.560285	5208.957066	7.524326	-0.046843	3.914714
234.921926	5216.970974	7.529331	-0.046915	3.917605
234.850674	5224.960042	7.534336	-0.046907	3.920477
235.230402	5232.948570	7.539341	-0.046983	3.923355
235.471485	5240.997974	7.544346	-0.047033	3.926250
235.520973	5248.996933	7.549350	-0.047047	3.929121
235.918443	5257.043540	7.554355	-0.047126	3.932013
235.910308	5265.091240	7.559360	-0.047130	3.934897
236.059902	5273.096872	7.564365	-0.047163	3.937766
236.294130	5281.128659	7.569370	-0.047211	3.940644
236.606505	5289.071717	7.574374	-0.047275	3.943489
236.686845	5297.125601	7.579379	-0.047295	3.946368
236.910131	5305.125040	7.584384	-0.047341	3.949228
237.106937	5313.167565	7.589389	-0.047383	3.952100
237.555536	5321.239714	7.594394	-0.047472	3.954986
237.734070	5329.217930	7.599398	-0.047510	3.957831
237.863515	5337.239431	7.604403	-0.047539	3.960688
238.031910	5345.225406	7.609408	-0.047576	3.963532
238.174517	5353.228970	7.614413	-0.047608	3.966379
238.447913	5361.275209	7.619418	-0.047664	3.969242
238.645594	5369.307213	7.624422	-0.047706	3.972096
238.703118	5377.345542	7.629427	-0.047721	3.974948
238.867669	5385.367016	7.634432	-0.047757	3.977794
239.255724	5393.371495	7.639437	-0.047835	3.980635
239.457883	5401.411715	7.644442	-0.047877	3.983484
239.574155	5409.386711	7.649446	-0.047904	3.986306
239.984864	5417.438631	7.654451	-0.047986	3.989158
240.184405	5425.492957	7.659456	-0.048028	3.992006
240.407176	5433.527281	7.664461	-0.048075	3.994845
240.461977	5441.572435	7.669466	-0.048090	3.997683
240.428474	5449.517456	7.674470	-0.048089	4.000482
240.775603	5457.560770	7.679475	-0.048158	4.003320
240.937430	5465.581912	7.684480	-0.048194	4.006145
241.104894	5473.594328	7.689485	-0.048230	4.008965
241.452181	5481.652420	7.694490	-0.048300	4.011802
241.505717	5489.632495	7.699494	-0.048315	4.014605
241.584814	5497.690029	7.704499	-0.048335	4.017433
241.831056	5505.679997	7.709504	-0.048386	4.020239
242.154226	5513.674951	7.714509	-0.048451	4.023045
242.320856	5521.686044	7.719514	-0.048487	4.025853
242.562856	5529.690599	7.724518	-0.048537	4.028657
242.861573	5537.770731	7.729523	-0.048598	4.031487
242.857923	5545.906365	7.734528	-0.048603	4.034330
243.035930	5553.870890	7.739533	-0.048641	4.037113
243.501348	5561.823334	7.744538	-0.048733	4.039895
243.644735	5569.805914	7.749542	-0.048764	4.042680
243.711363	5577.795526	7.754547	-0.048782	4.045465
243.953159	5585.843385	7.759552	-0.048832	4.048271
244.075625	5593.867838	7.764557	-0.048860	4.051065
244.225945	5601.928162	7.769562	-0.048893	4.053870
244.396996	5609.941145	7.774566	-0.048930	4.056656
244.705064	5617.924363	7.779571	-0.048992	4.059433
244.805322	5625.961346	7.784576	-0.049016	4.062223
245.201869	5633.912495	7.789581	-0.049095	4.064986
245.445244	5641.988139	7.794586	-0.049146	4.067787
245.729689	5649.976697	7.799590	-0.049204	4.070557
245.751293	5658.068090	7.804595	-0.049213	4.073357
245.906823	5666.046783	7.809600	-0.049247	4.076119
246.181006	5674.018074	7.814605	-0.049303	4.078877
246.375263	5682.070419	7.819610	-0.049344	4.081660
246.627835	5690.040963	7.824614	-0.049396	4.084414
246.843237	5698.114464	7.829619	-0.049442	4.087201
247.083214	5706.105606	7.834624	-0.049491	4.089958
246.949045	5714.151319	7.839629	-0.049472	4.092727
247.279189	5722.197095	7.844634	-0.049538	4.095500
247.305061	5730.199390	7.849638	-0.049548	4.098253
247.575395	5738.214944	7.854643	-0.049604	4.101011
247.921838	5746.222188	7.859648	-0.049673	4.103765
248.174712	5754.248536	7.864653	-0.049725	4.106523
248.338483	5762.275573	7.869658	-0.049761	4.109279
248.527119	5770.317157	7.874662	-0.049801	4.112037
249.138039	5778.360251	7.879667	-0.049920	4.114800
249.267648	5786.364914	7.884672	-0.049949	4.117541
249.577626	5794.326281	7.889677	-0.050012	4.120268
249.893717	5802.375062	7.894682	-0.050076	4.123024
249.991459	5810.345037	7.899686	-0.050100	4.125747
250.200020	5818.374833	7.904691	-0.050143	4.128491
250.139731	5826.442716	7.909696	-0.050137	4.131242
250.371593	5834.477006	7.914701	-0.050186	4.133984
250.500212	5842.539694	7.919706	-0.050215	4.136732
250.551345	5850.472973	7.924710	-0.050229	4.139434
251.157581	5858.529425	7.929715	-0.050347	4.142182
251.106468	5866.528374	7.934720	-0.050343	4.144901
251.160353	5874.558284	7.939725	-0.050358	4.147630
251.495084	5882.528509	7.944730	-0.050426	4.150340
251.628844	5890.619679	7.949734	-0.050456	4.153087
251.729689	5898.668594	7.954739	-0.050480	4.155818
251.990239	5906.650085	7.959744	-0.050533	4.158525
252.461362	5914.634307	7.964749	-0.050626	4.161235
252.745526	5922.657971	7.969754	-0.050684	4.163953
252.988260	5930.662547	7.974758	-0.050734	4.166663
253.291182	5938.686127	7.979763	-0.050796	4.169378
253.525408	5946.756200	7.984768	-0.050845	4.172107
253.865864	5954.744859	7.989773	-0.050913	4.174807
254.226963	5962.786301	7.994778	-0.050985	4.177523
254.551470	5970.736127	7.999782	-0.051051	4.180207
254.407185	5978.752842	8.004787	-0.051029	4.182906
254.671267	5986.803191	8.009792	-0.051083	4.185619
254.850184	5994.821707	8.014797	-0.051122	4.188318
255.098851	6002.822807	8.019802	-0.051173	4.191011
255.290824	6010.936000	8.024806	-0.051214	4.193739
255.575778	6018.966051	8.029811	-0.051272	4.196438
255.424010	6026.920196	8.034816	-0.051249	4.199106
255.581465	6034.925558	8.039821	-0.051284	4.201792
255.716133	6042.899547	8.044826	-0.051314	4.204466
255.992325	6050.940513	8.049830	-0.051370	4.207162
256.148703	6058.924182	8.054835	-0.051405	4.209835
256.268267	6066.991614	8.059840	-0.051432	4.212535
256.739068	6074.955544	8.064845	-0.051525	4.215202
256.970311	6083.002040	8.069850	-0.051573	4.217892
256.884001	6091.026779	8.074854	-0.051562	4.220570
257.108130	6099.032393	8.079859	-0.051609	4.223243
257.298624	6107.059157	8.084864	-0.051649	4.225921
257.452423	6115.038748	8.089869	-0.051683	4.228581
257.698048	6123.092977	8.094874	-0.051734	4.231266
257.862454	6131.125684	8.099878	-0.051770	4.233940
258.054105	6139.174032	8.104883	-0.051811	4.236619
258.317247	6147.148465	8.109888	-0.051865	4.239271
258.654022	6155.148488	8.114893	-0.051932	4.241932
258.909352	6163.184195	8.119898	-0.051985	4.244601
258.906817	6171.166372	8.124902	-0.051990	4.247249
259.175287	6179.197832	8.129907	-0.052045	4.249914
259.507906	6187.240225	8.134912	-0.052112	4.252581
259.595709	6195.265264	8.139917	-0.052133	4.255239
259.731946	6203.307262	8.144922	-0.052164	4.257901
260.074957	6211.277004	8.149926	-0.052233	4.260540
260.383608	6219.333080	8.154931	-0.052295	4.263205
260.556700	6227.361997	8.159936	-0.052333	4.265858
260.613074	6235.354595	8.164941	-0.052348	4.268496
260.903532	6243.399063	8.169946	-0.052408	4.271152
260.948514	6251.442725	8.174950	-0.052421	4.273804
261.389247	6259.471723	8.179955	-0.052508	4.276453
261.540098	6267.455439	8.184960	-0.052541	4.279082
261.570378	6275.448146	8.189965	-0.052552	4.281712
261.825719	6283.465758	8.194970	-0.052605	4.284351
262.249115	6291.455709	8.199974	-0.052689	4.286980
262.300990	6299.483736	8.204979	-0.052704	4.289616
262.350157	6307.544392	8.209984	-0.052718	4.292262
262.490019	6315.553563	8.214989	-0.052749	4.294890
262.905906	6323.615321	8.219994	-0.052832	4.297536
263.006992	6331.542978	8.224998	-0.052856	4.300134
263.008502	6339.581825	8.230003	-0.052861	4.302766
263.353168	6347.595535	8.235008	-0.052930	4.305391
263.503468	6355.646537	8.240013	-0.052963	4.308024
263.709007	6363.656333	8.245018	-0.053007	4.310643
263.578023	6371.653032	8.250022	-0.052987	4.313254
263.822904	6379.710043	8.255027	-0.053038	4.315886
263.970108	6387.702486	8.260032	-0.053071	4.318494
264.175362	6395.696607	8.265037	-0.053114	4.321101
264.445072	6403.718175	8.270042	-0.053169	4.323717
264.437175	6411.720153	8.275046	-0.053173	4.326322
264.717633	6419.747519	8.280051	-0.053230	4.328936
265.215095	6427.796278	8.285056	-0.053328	4.331557
265.276163	6435.795120	8.290061	-0.053345	4.334157
265.482521	6443.825508	8.295066	-0.053388	4.336766
265.516582	6451.800963	8.300070	-0.053400	4.339356
265.657215	6459.836733	8.305075	-0.053431	4.341963
265.882150	6467.851569	8.310080	-0.053478	4.344563
265.882171	6475.881705	8.315085	-0.053483	4.347165
266.511030	6483.897123	8.320090	-0.053605	4.349765
266.533127	6492.027278	8.325094	-0.053614	4.352396
266.641367	6500.051542	8.330099	-0.053640	4.354992
266.942842	6508.024656	8.335104	-0.053701	4.357571
266.952121	6515.939696	8.340109	-0.053708	4.360128
267.045994	6523.967060	8.345114	-0.053730	4.362720
267.250386	6531.938085	8.350118	-0.053773	4.365293
267.400935	6539.947851	8.355123	-0.053807	4.367877
267.727520	6547.977534	8.360128	-0.053873	4.370467
267.988716	6556.036604	8.365133	-0.053926	4.373064
268.139053	6564.091944	8.370138	-0.053959	4.375658
268.360426	6572.061526	8.375142	-0.054006	4.378223
268.547835	6580.079228	8.380147	-0.054046	4.380802
268.928241	6588.106079	8.385152	-0.054122	4.383383
269.142852	6596.076552	8.390157	-0.054167	4.385944
269.327164	6604.133069	8.395162	-0.054206	4.388530
269.519649	6612.160203	8.400166	-0.054247	4.391106
269.697576	6620.214789	8.405171	-0.054285	4.393689
269.785777	6628.230860	8.410176	-0.054307	4.396257
270.002048	6636.191009	8.415181	-0.054352	4.398807
270.393412	6644.268158	8.420186	-0.054430	4.401394
270.504678	6652.236606	8.425190	-0.054456	4.403942
270.571171	6660.279816	8.430195	-0.054474	4.406513
270.782777	6668.307859	8.435200	-0.054518	4.409079
270.975520	6676.291073	8.440205	-0.054559	4.411628
271.259287	6684.338271	8.445210	-0.054617	4.414197
271.208222	6692.375797	8.450214	-0.054613	4.416759
271.461531	6700.375174	8.455219	-0.054665	4.419310
271.738628	6708.412265	8.460224	-0.054722	4.421871
271.893447	6716.332305	8.465229	-0.054756	4.424392
272.119867	6724.454199	8.470234	-0.054803	4.426977
272.242680	6732.446862	8.475238	-0.054831	4.429519
272.151763	6740.485515	8.480243	-0.054819	4.432072
272.449835	6748.525337	8.485248	-0.054880	4.434627
272.619463	6756.548065	8.490253	-0.054916	4.437174
272.900920	6764.507017	8.495258	-0.054974	4.439700
272.976447	6772.536409	8.500262	-0.054993	4.442245
273.231734	6780.487259	8.505267	-0.055046	4.444765
273.264001	6788.556073	8.510272	-0.055057	4.447320
273.341014	6796.497730	8.515277	-0.055076	4.449834
273.636502	6804.602121	8.520282	-0.055137	4.452398
273.716080	6812.589490	8.525286	-0.055156	4.454923
273.810600	6820.641548	8.530291	-0.055179	4.457467
274.165219	6828.603158	8.535296	-0.055250	4.459983
274.343264	6836.646699	8.540301	-0.055289	4.462521
274.512221	6844.636581	8.545306	-0.055325	4.465042
274.517926	6852.674519	8.550310	-0.055331	4.467575
274.749922	6860.662951	8.555315	-0.055380	4.470093
275.002602	6868.759911	8.560320	-0.055432	4.472643
275.090525	6876.743284	8.565325	-0.055453	4.475155
275.423961	6884.799094	8.570330	-0.055520	4.477689
275.545705	6892.722699	8.575335	-0.055548	4.480180
275.609336	6900.767680	8.580339	-0.055565	4.482707
275.801352	6908.794066	8.585344	-0.055606	4.485228
275.880208	6916.785351	8.590349	-0.055626	4.487735
276.279952	6924.848768	8.595354	-0.055705	4.490265
276.422834	6932.833622	8.600359	-0.055737	4.492768
276.741526	6940.880195	8.605363	-0.055802	4.495289
276.804788	6948.880852	8.610368	-0.055818	4.497794
276.769922	6956.870899	8.615373	-0.055817	4.500294
276.919058	6964.887760	8.620378	-0.055850	4.502801
277.130155	6972.896643	8.625383	-0.055894	4.505305
277.368341	6980.927844	8.630387	-0.055944	4.507814
277.592083	6988.976743	8.635392	-0.055991	4.510327
277.681933	6996.963215	8.640397	-0.056012	4.512819
278.033316	7005.011229	8.645402	-0.056083	4.515329
278.054812	7013.021238	8.650407	-0.056092	4.517826
278.428098	7020.994034	8.655411	-0.056167	4.520310
278.758704	7029.034871	8.660416	-0.056233	4.522814
278.636857	7037.003116	8.665421	-0.056216	4.525293
278.871457	7045.033563	8.670426	-0.056265	4.527790
279.023482	7053.056018	8.675431	-0.056298	4.530284
279.292317	7061.073175	8.680435	-0.056353	4.532775
279.377322	7069.119114	8.685440	-0.056374	4.535272
279.484015	7077.114044	8.690445	-0.056399	4.537753
279.943061	7085.120449	8.695450	-0.056490	4.540237
279.965794	7093.166076	8.700455	-0.056499	4.542730
280.208047	7101.143392	8.705459	-0.056549	4.545202
280.284023	7109.164335	8.710464	-0.056569	4.547685
280.379255	7117.177494	8.715469	-0.056591	4.550164
280.563342	7125.246149	8.720474	-0.056631	4.552660
280.797647	7133.263512	8.725479	-0.056680	4.555138
281.091794	7141.271937	8.730483	-0.056739	4.557612
281.281000	7149.270100	8.735488	-0.056780	4.560082
281.285514	7157.281506	8.740493	-0.056786	4.562554
281.522720	7165.271076	8.745498	-0.056835	4.565018
281.542163	7173.313459	8.750503	-0.056844	4.567497
281.770599	7181.293629	8.755507	-0.056891	4.569955
281.963837	7189.389876	8.760512	-0.056933	4.572448
282.048713	7197.390479	8.765517	-0.056953	4.574910
282.156612	7205.445122	8.770522	-0.056979	4.577388
282.241050	7213.376231	8.775527	-0.056999	4.579826
282.522770	7221.432095	8.780531	-0.057057	4.582301
282.793419	7229.410076	8.785536	-0.057113	4.584751
283.021865	7237.454596	8.790541	-0.057160	4.587219
283.326706	7245.484063	8.795546	-0.057222	4.589682
283.458057	7253.499913	8.800551	-0.057252	4.592140
283.448363	7261.566183	8.805555	-0.057255	4.594611
283.885910	7269.592401	8.810560	-0.057342	4.597069
284.009928	7277.487707	8.815565	-0.057370	4.599486
284.044815	7285.608830	8.820570	-0.057381	4.601970
284.123689	7293.535152	8.825575	-0.057401	4.604393
284.426587	7301.565742	8.830579	-0.057463	4.606847
284.646265	7309.555768	8.835584	-0.057509	4.609287
284.693635	7317.598217	8.840589	-0.057523	4.611742
285.099576	7325.627625	8.845594	-0.057603	4.614191
285.312512	7333.657304	8.850599	-0.057648	4.616640
285.344006	7341.640003	8.855603	-0.057659	4.619072
285.683801	7349.697898	8.860608	-0.057727	4.621527
285.800011	7357.653323	8.865613	-0.057754	4.623948
286.004679	7365.724946	8.870618	-0.057797	4.626404
286.113226	7373.721745	8.875623	-0.057823	4.628836
286.330247	7381.721934	8.880627	-0.057868	4.631267
286.407436	7389.763191	8.885632	-0.057888	4.633710
286.426323	7397.784961	8.890637	-0.057896	4.636145
286.777039	7405.783871	8.895642	-0.057967	4.638572
286.927637	7413.802102	8.900647	-0.058000	4.641004
287.243008	7421.779684	8.905651	-0.058064	4.643422
287.328991	7429.838247	8.910656	-0.058085	4.645864
287.388724	7437.814385	8.915661	-0.058101	4.648279
287.533831	7445.874416	8.920666	-0.058133	4.650718
287.587372	7453.868241	8.925671	-0.058148	4.653136
287.879402	7461.882571	8.930675	-0.058208	4.655559
288.043225	7469.947233	8.935680	-0.058243	4.657995
288.060016	7477.909123	8.940685	-0.058252	4.660400
288.349003	7485.954862	8.945690	-0.058311	4.662828
288.421437	7493.909806	8.950695	-0.058329	4.665228
288.626088	7501.993742	8.955699	-0.058372	4.667665
288.972225	7509.968666	8.960704	-0.058442	4.670068
289.297881	7518.031714	8.965709	-0.058508	4.672497
289.456519	7526.148042	8.970714	-0.058543	4.674940
289.565647	7534.121058	8.975719	-0.058568	4.677339
289.819269	7542.008662	8.980723	-0.058620	4.679711
289.974601	7550.044226	8.985728	-0.058654	4.682126
289.853724	7557.989898	8.990733	-0.058637	4.684513
290.281007	7566.059340	8.995738	-0.058721	4.686936
290.540614	7574.025964	9.000743	-0.058775	4.689326
290.617357	7582.081999	9.005747	-0.058794	4.691743
290.745579	7590.175894	9.010752	-0.058823	4.694169
290.909970	7598.153394	9.015757	-0.058859	4.696559
291.128711	7606.156259	9.020762	-0.058905	4.698956
291.095364	7614.161498	9.025767	-0.058904	4.701352
291.357073	7622.163592	9.030771	-0.058958	4.703746
291.447665	7630.222880	9.035776	-0.058980	4.706156
291.633797	7638.216035	9.040781	-0.059019	4.708544
292.029348	7646.189903	9.045786	-0.059098	4.710925
292.215769	7654.280265	9.050791	-0.059138	4.713341
292.448329	7662.294666	9.055795	-0.059186	4.715732
292.665652	7670.291117	9.060800	-0.059232	4.718116
292.731002	7678.264191	9.065805	-0.059249	4.720493
292.953860	7686.310842	9.070810	-0.059296	4.722890
292.956232	7694.283121	9.075815	-0.059301	4.725264
293.249530	7702.354445	9.080819	-0.059361	4.727666
293.542670	7710.351271	9.085824	-0.059421	4.730045
293.596554	7718.426585	9.090829	-0.059436	4.732446
293.967976	7726.437721	9.095834	-0.059510	4.734826
293.968805	7734.469274	9.100839	-0.059516	4.737211
294.227710	7742.419189	9.105843	-0.059569	4.739571
294.485144	7750.482596	9.110848	-0.059622	4.741963
294.509140	7758.377130	9.115853	-0.059631	4.744305
294.704034	7766.516552	9.120858	-0.059673	4.746717
294.714523	7774.512718	9.125863	-0.059680	4.749086
294.971529	7782.518827	9.130867	-0.059733	4.751457
295.348203	7790.578940	9.135872	-0.059808	4.753841
295.401214	7798.566652	9.140877	-0.059823	4.756204
295.687803	7806.586476	9.145882	-0.059882	4.758575
295.901976	7814.554603	9.150887	-0.059927	4.760929
295.834626	7822.559261	9.155891	-0.059919	4.763294
296.077869	7830.545298	9.160896	-0.059970	4.765651
296.172645	7838.591714	9.165901	-0.059992	4.768025
296.218395	7846.633087	9.170906	-0.060006	4.770397
296.377563	7854.628062	9.175911	-0.060041	4.772754
296.441193	7862.680901	9.180915	-0.060058	4.775126
296.684284	7870.717918	9.185920	-0.060108	4.777492
296.761656	7878.616741	9.190925	-0.060128	4.779817
296.999230	7886.703141	9.195930	-0.060177	4.782196
297.028408	7894.673948	9.200935	-0.060187	4.784540
297.187638	7902.725954	9.205939	-0.060222	4.786906
297.409753	7910.738276	9.210944	-0.060269	4.789259
297.767617	7918.768306	9.215949	-0.060340	4.791615
298.020983	7926.818978	9.220954	-0.060393	4.793977
298.031629	7934.814741	9.225959	-0.060400	4.796323
298.291170	7942.777729	9.230963	-0.060453	4.798657
298.319825	7950.823204	9.235968	-0.060464	4.801014
298.300221	7958.786617	9.240973	-0.060465	4.803347
298.362009	7966.811712	9.245978	-0.060482	4.805696
298.646408	7974.850714	9.250983	-0.060540	4.808047
298.958853	7982.863258	9.255987	-0.060603	4.810390
298.912221	7990.262989	9.260992	-0.060599	4.812553
299.176159	7994.769042	9.265997	-0.060651	4.813869
299.445818	7997.348601	9.271002	-0.060703	4.814621
299.375232	7998.627667	9.276007	-0.060691	4.814995
299.403481	7999.064155	9.281011	-0.060696	4.815123
299.670141	8000.112728	9.286016	-0.060746	4.815428
299.896471	8000.086538	9.291021	-0.060788	4.815419
299.976679	8000.124195	9.296026	-0.060803	4.815429
300.158792	8000.058797	9.301031	-0.060837	4.815409
300.232736	8000.074974	9.306035	-0.060851	4.815414
300.387597	8000.086078	9.311040	-0.060879	4.815416
300.441911	8000.059179	9.316045	-0.060889	4.815408
300.307163	8000.111447	9.321050	-0.060864	4.815424
300.304982	8000.102851	9.326055	-0.060864	4.815422
300.329753	8000.065843	9.331059	-0.060868	4.815411
300.527518	8000.087277	9.336064	-0.060905	4.815416
300.438820	8000.081524	9.341069	-0.060888	4.815415
300.490608	8000.140087	9.346074	-0.060898	4.815432
300.739478	8000.111065	9.351079	-0.060944	4.815422
300.800981	8000.051151	9.356083	-0.060955	4.815404
300.881579	8000.134774	9.361088	-0.060970	4.815428
300.772410	8000.116925	9.366093	-0.060950	4.815424
300.904169	8000.156505	9.371098	-0.060974	4.815434
300.891232	8000.137043	9.376103	-0.060972	4.815429
300.764972	8000.107153	9.381107	-0.060948	4.815421
300.947130	8000.126192	9.386112	-0.060982	4.815425
300.996553	8000.089591	9.391117	-0.060991	4.815414
301.084530	8000.130585	9.396122	-0.061007	4.815426
301.128456	8000.107788	9.401127	-0.061015	4.815419
301.215737	8000.063264	9.406131	-0.061031	4.815406
301.278954	8000.142326	9.411136	-0.061043	4.815429
301.161103	8000.112575	9.416141	-0.061021	4.815420
301.334590	8000.109025	9.421146	-0.061053	4.815419
301.413159	8000.143451	9.426151	-0.061068	4.815428
301.334745	8000.148555	9.431155	-0.061053	4.815430
301.647378	8000.157999	9.436160	-0.061111	4.815431
301.706127	8000.091626	9.441165	-0.061122	4.815412
301.578448	8000.122635	9.446170	-0.061098	4.815421
301.621760	8000.132962	9.451175	-0.061106	4.815424
301.612217	8000.079352	9.456179	-0.061104	4.815409
301.652516	8000.097111	9.461184	-0.061111	4.815414
301.685458	8000.068789	9.466189	-0.061117	4.815405
301.879685	8000.127576	9.471194	-0.061154	4.815421
301.679520	8000.119975	9.476199	-0.061116	4.815420
301.650476	8000.129104	9.481203	-0.061111	4.815423
301.739407	8000.159426	9.486208	-0.061127	4.815431
301.766589	8000.137420	9.491213	-0.061132	4.815425
301.911193	8000.160114	9.496218	-0.061159	4.815431
301.845813	8000.168641	9.501223	-0.061147	4.815434
301.872786	8000.086777	9.506227	-0.061151	4.815409
301.958173	8000.126660	9.511232	-0.061167	4.815421
301.881522	8000.084764	9.516237	-0.061153	4.815409
302.098657	8000.125761	9.521242	-0.061193	4.815420
301.998705	8000.109132	9.526247	-0.061175	4.815415
301.868437	8000.049246	9.531251	-0.061150	4.815399
302.082316	8000.107291	9.536256	-0.061190	4.815414
302.239093	8000.079950	9.541261	-0.061219	4.815406
302.183972	8000.121781	9.546266	-0.061209	4.815418
302.138001	8000.109253	9.551271	-0.061200	4.815415
302.326596	8000.040754	9.556275	-0.061235	4.815394
302.418769	8000.140606	9.561280	-0.061252	4.815423
302.154937	8000.044304	9.566285	-0.061203	4.815396
302.459008	8000.119876	9.571290	-0.061259	4.815416
302.473096	8000.111549	9.576295	-0.061262	4.815414
302.409917	8000.082702	9.581299	-0.061250	4.815406
302.621667	8000.127886	9.586304	-0.061289	4.815418
302.397355	8000.087819	9.591309	-0.061247	4.815407
302.546741	8000.113799	9.596314	-0.061275	4.815414
302.560847	8000.130056	9.601319	-0.061278	4.815419
302.532069	8000.115674	9.606323	-0.061272	4.815415
302.481674	8000.116967	9.611328	-0.061263	4.815415
302.386843	8000.112179	9.616333	-0.061245	4.815414
302.460086	8000.126209	9.621338	-0.061258	4.815418
302.484408	8000.097743	9.626343	-0.061263	4.815410
302.586262	8000.096214	9.631347	-0.061282	4.815409
302.494163	8000.134226	9.636352	-0.061264	4.815420
302.459423	8000.116539	9.641357	-0.061258	4.815415
302.513303	8000.153764	9.646362	-0.061268	4.815426
302.480172	8000.132896	9.651367	-0.061261	4.815420
302.476045	8000.036621	9.656371	-0.061260	4.815392
302.751797	8000.141653	9.661376	-0.061312	4.815421
302.795026	8000.160531	9.666381	-0.061320	4.815427
302.696403	8000.138578	9.671386	-0.061301	4.815421
302.609225	8000.125366	9.676391	-0.061285	4.815417
302.550234	8000.120103	9.681395	-0.061274	4.815416
302.806559	8000.154269	9.686400	-0.061321	4.815425
302.540819	8000.086793	9.691405	-0.061272	4.815406
302.828532	8000.105446	9.696410	-0.061325	4.815410
302.738300	8000.118905	9.701415	-0.061308	4.815415
302.699634	8000.070155	9.706419	-0.061301	4.815401
302.893809	8000.143909	9.711424	-0.061337	4.815421
302.807428	8000.127503	9.716429	-0.061321	4.815417
302.901281	8000.151495	9.721434	-0.061338	4.815424
302.810820	8000.132884	9.726439	-0.061321	4.815419
302.824054	8000.039033	9.731443	-0.061324	4.815391
302.829717	8000.109663	9.736448	-0.061325	4.815412
302.825848	8000.149137	9.741453	-0.061324	4.815423
303.031939	8000.179265	9.746458	-0.061362	4.815431
302.920004	8000.158160	9.751463	-0.061341	4.815425
302.899407	8000.096883	9.756467	-0.061337	4.815408
303.036990	8000.156872	9.761472	-0.061363	4.815424
302.785501	8000.127042	9.766477	-0.061316	4.815417
302.812686	8000.163824	9.771482	-0.061321	4.815428
302.989422	8000.137884	9.776487	-0.061353	4.815419
303.041753	8000.138741	9.781491	-0.061363	4.815419
302.943680	8000.176654	9.786496	-0.061345	4.815431
302.827880	8000.152279	9.791501	-0.061323	4.815424
303.046931	8000.184759	9.796506	-0.061364	4.815433
302.895922	8000.107426	9.801511	-0.061336	4.815411
302.814256	8000.135991	9.806515	-0.061320	4.815419
303.100030	8000.162095	9.811520	-0.061373	4.815426
302.974795	8000.131150	9.816525	-0.061350	4.815417
303.144783	8000.169230	9.821530	-0.061381	4.815428
303.235926	8000.151491	9.826535	-0.061398	4.815422
303.250110	8000.085446	9.831539	-0.061401	4.815403
303.115250	8000.154816	9.836544	-0.061376	4.815424
302.921035	8000.101350	9.841549	-0.061339	4.815409
303.246138	8000.148415	9.846554	-0.061400	4.815421
303.160329	8000.163016	9.851559	-0.061384	4.815426
303.140836	8000.160545	9.856563	-0.061380	4.815425
303.224363	8000.185435	9.861568	-0.061395	4.815432
303.128349	8000.114357	9.866573	-0.061377	4.815412
303.241333	8000.084153	9.871578	-0.061398	4.815402
303.109777	8000.107616	9.876583	-0.061374	4.815410
303.185322	8000.070379	9.881587	-0.061388	4.815399
303.233974	8000.134239	9.886592	-0.061397	4.815417
303.267933	8000.107001	9.891597	-0.061403	4.815409
303.484192	8000.113783	9.896602	-0.061443	4.815410
303.212307	8000.132782	9.901607	-0.061392	4.815417
303.222761	8000.114774	9.906611	-0.061394	4.815411
303.393186	8000.132554	9.911616	-0.061426	4.815416
303.118798	8000.095929	9.916621	-0.061374	4.815406
303.060784	8000.103509	9.921626	-0.061364	4.815409
303.132186	8000.104683	9.926631	-0.061377	4.815409
303.175408	8000.095769	9.931635	-0.061385	4.815406
303.137150	8000.095125	9.936640	-0.061377	4.815406
303.158097	8000.095463	9.941645	-0.061381	4.815406
303.257170	8000.124886	9.946650	-0.061400	4.815414
303.212865	8000.130555	9.951655	-0.061391	4.815416
303.233856	8000.133031	9.956659	-0.061395	4.815417
303.325475	8000.166606	9.961664	-0.061412	4.815426
303.526027	8000.117545	9.966669	-0.061449	4.815411
303.553362	8000.111575	9.971674	-0.061454	4.815409
303.361026	8000.142582	9.976679	-0.061418	4.815419
303.459059	8000.109993	9.981683	-0.061436	4.815409
303.597012	8000.176403	9.986688	-0.061462	4.815428
303.359483	8000.155353	9.991693	-0.061418	4.815423
303.640568	8000.143970	9.996698	-0.061470	4.815418
303.426305	8000.144684	10.001703	-0.061430	4.815419
303.367823	8000.136222	10.006707	-0.061419	4.815417
303.657998	8000.192329	10.011712	-0.061473	4.815432
303.339846	8000.129326	10.016717	-0.061413	4.815415
303.433328	8000.176827	10.021722	-0.061431	4.815429
303.367017	8000.159685	10.026727	-0.061418	4.815424
303.265543	8000.166544	10.031731	-0.061399	4.815426
303.522669	8000.188968	10.036736	-0.061447	4.815432
303.551606	8000.122098	10.041741	-0.061452	4.815412
303.581531	8000.169615	10.046746	-0.061458	4.815426
303.399116	8000.143066	10.051751	-0.061424	4.815419
303.286178	8000.101635	10.056755	-0.061403	4.815407
303.465365	8000.131318	10.061760	-0.061436	4.815415
303.471537	8000.138893	10.066765	-0.061437	4.815417
303.527895	8000.119508	10.071770	-0.061447	4.815411
303.630119	8000.154328	10.076775	-0.061466	4.815421
303.716352	8000.132233	10.081779	-0.061482	4.815414
303.630087	8000.157515	10.086784	-0.061466	4.815422
303.448996	8000.119230	10.091789	-0.061432	4.815412
303.394549	8000.118318	10.096794	-0.061422	4.815412
303.469289	8000.138787	10.101799	-0.061436	4.815417
303.377055	8000.155419	10.106803	-0.061418	4.815423
303.465039	8000.141903	10.111808	-0.061435	4.815418
303.574793	8000.098819	10.116813	-0.061455	4.815405
303.411805	8000.098246	10.121818	-0.061424	4.815406
303.488031	8000.158288	10.126823	-0.061439	4.815423
303.601617	8000.128095	10.131827	-0.061460	4.815414
303.748342	8000.143344	10.136832	-0.061487	4.815417
303.526430	8000.061627	10.141837	-0.061445	4.815395
303.744452	8000.096229	10.146842	-0.061486	4.815404
303.791611	8000.145101	10.151847	-0.061495	4.815418
303.563201	8000.108169	10.156851	-0.061452	4.815408
303.705514	8000.134034	10.161856	-0.061478	4.815415
303.725271	8000.025325	10.166861	-0.061482	4.815383
303.730766	8000.046784	10.171866	-0.061483	4.815389
303.684420	8000.088761	10.176871	-0.061474	4.815402
303.560791	8000.130526	10.181875	-0.061451	4.815414
303.600615	8000.119419	10.186880	-0.061458	4.815411
303.479844	8000.107787	10.191885	-0.061436	4.815408
303.597293	8000.164238	10.196890	-0.061457	4.815424
303.725658	8000.118256	10.201895	-0.061481	4.815410
303.577384	8000.082653	10.206899	-0.061453	4.815400
303.676604	8000.115285	10.211904	-0.061472	4.815409
303.664790	8000.066980	10.216909	-0.061469	4.815395
303.797305	8000.152540	10.221914	-0.061494	4.815420
303.690011	8000.152889	10.226919	-0.061474	4.815420
303.714835	8000.108397	10.231923	-0.061479	4.815407
303.930571	8000.167547	10.236928	-0.061519	4.815424
303.707127	8000.126421	10.241933	-0.061477	4.815413
303.823128	8000.110163	10.246938	-0.061498	4.815407
303.561183	8000.133602	10.251943	-0.061449	4.815415
303.494801	8000.091874	10.256947	-0.061437	4.815404
303.579395	8000.163813	10.261952	-0.061453	4.815424
303.590956	8000.121240	10.266957	-0.061455	4.815412
303.624256	8000.095060	10.271962	-0.061461	4.815404
303.576799	8000.065403	10.276967	-0.061452	4.815395
303.505268	8000.035348	10.281971	-0.061438	4.815387
303.936573	8000.151515	10.286976	-0.061519	4.815419
303.609016	8000.080872	10.291981	-0.061457	4.815400
303.711450	8000.078285	10.296986	-0.061476	4.815399
304.000286	8000.120475	10.301991	-0.061530	4.815409
303.973783	8000.054823	10.306995	-0.061525	4.815390
303.862286	8000.133132	10.312000	-0.061504	4.815414
303.979323	8000.090169	10.317005	-0.061526	4.815401
304.102868	8000.066554	10.322010	-0.061549	4.815393
303.941171	8000.123721	10.327015	-0.061519	4.815411
303.834299	8000.055668	10.332019	-0.061499	4.815391
304.104793	8000.106105	10.337024	-0.061549	4.815405
303.789115	8000.099793	10.342029	-0.061490	4.815404
303.747238	8000.085193	10.347034	-0.061482	4.815400
303.884297	8000.115247	10.352039	-0.061507	4.815409
303.813106	8000.100161	10.357043	-0.061494	4.815404
303.687489	8000.148307	10.362048	-0.061471	4.815419
303.706718	8000.093033	10.367053	-0.061474	4.815403
303.935575	8000.131022	10.372058	-0.061517	4.815413
303.643065	8000.151816	10.377063	-0.061462	4.815420
303.589800	8000.104961	10.382067	-0.061452	4.815407
303.797504	8000.108395	10.387072	-0.061490	4.815407
303.843769	8000.068534	10.392077	-0.061499	4.815395
303.718885	8000.071799	10.397082	-0.061476	4.815397
303.816395	8000.151434	10.402087	-0.061494	4.815419
303.970706	8000.110158	10.407091	-0.061522	4.815407
303.995081	8000.141550	10.412096	-0.061527	4.815416
304.010740	8000.118284	10.417101	-0.061530	4.815409
304.006096	8000.117129	10.422106	-0.061529	4.815409
303.722239	8000.143411	10.427111	-0.061476	4.815418
303.797429	8000.065550	10.432115	-0.061489	4.815395
303.938862	8000.140569	10.437120	-0.061516	4.815416
303.965228	8000.127101	10.442125	-0.061521	4.815412
303.981512	8000.134843	10.447130	-0.061523	4.815414
304.072932	8000.157727	10.452135	-0.061540	4.815420
304.015614	8000.108667	10.457139	-0.061530	4.815406
304.100863	8000.150688	10.462144	-0.061545	4.815418
303.989707	8000.146698	10.467149	-0.061525	4.815417
304.081644	8000.156764	10.472154	-0.061542	4.815420
304.116426	8000.126332	10.477159	-0.061548	4.815411
304.109099	8000.090927	10.482163	-0.061546	4.815400
304.085788	8000.116185	10.487168	-0.061542	4.815408
304.063694	8000.138255	10.492173	-0.061538	4.815414
304.127282	8000.089062	10.497178	-0.061549	4.815400
304.071461	8000.158674	10.502183	-0.061539	4.815420
304.085623	8000.061629	10.507187	-0.061541	4.815392
304.040681	8000.136766	10.512192	-0.061533	4.815414
303.855418	8000.115513	10.517197	-0.061498	4.815409
304.021690	8000.159947	10.522202	-0.061529	4.815421
303.976714	8000.177363	10.527207	-0.061521	4.815426
303.990049	8000.129474	10.532211	-0.061523	4.815412
304.290236	8000.162233	10.537216	-0.061579	4.815420
303.966578	8000.107687	10.542221	-0.061519	4.815406
304.001069	8000.078320	10.547226	-0.061525	4.815397
303.892368	8000.091472	10.552231	-0.061504	4.815402
304.035800	8000.112012	10.557235	-0.061531	4.815407
304.108736	8000.183759	10.562240	-0.061545	4.815428
304.052051	8000.141122	10.567245	-0.061534	4.815415
304.148838	8000.090341	10.572250	-0.061552	4.815400
304.155537	8000.111820	10.577255	-0.061553	4.815406
303.959159	8000.010216	10.582259	-0.061516	4.815378
304.120989	8000.148639	10.587264	-0.061546	4.815417
304.048581	8000.114293	10.592269	-0.061533	4.815408
303.897868	8000.079717	10.597274	-0.061505	4.815398
304.182868	8000.147498	10.602279	-0.061558	4.815417
304.047977	8000.090738	10.607283	-0.061532	4.815401
303.892698	8000.185423	10.612288	-0.061503	4.815429
303.814341	8000.084707	10.617293	-0.061489	4.815400
304.179188	8000.176258	10.622298	-0.061556	4.815425
304.103124	8000.116197	10.627303	-0.061542	4.815408
303.964836	8000.102137	10.632307	-0.061516	4.815404
304.140381	8000.109313	10.637312	-0.061549	4.815406
304.006573	8000.132738	10.642317	-0.061524	4.815413
304.072967	8000.104969	10.647322	-0.061536	4.815405
304.025084	8000.129819	10.652327	-0.061527	4.815412
304.120935	8000.114296	10.657331	-0.061545	4.815407
304.149771	8000.151107	10.662336	-0.061550	4.815418
303.993729	8000.134614	10.667341	-0.061521	4.815414
303.933986	8000.127200	10.672346	-0.061510	4.815412
303.997158	8000.144271	10.677351	-0.061521	4.815417
304.011829	8000.088922	10.682355	-0.061524	4.815400
303.896631	8000.116932	10.687360	-0.061502	4.815409
303.992845	8000.102483	10.692365	-0.061520	4.815404
304.022067	8000.111509	10.697370	-0.061525	4.815407
304.022434	8000.130746	10.702375	-0.061525	4.815413
303.987683	8000.056406	10.707379	-0.061519	4.815391
304.314111	8000.129149	10.712384	-0.061580	4.815411
303.978998	8000.098998	10.717389	-0.061517	4.815404
304.075994	8000.070667	10.722394	-0.061535	4.815395
304.133482	8000.154985	10.727399	-0.061546	4.815419
304.231837	8000.112781	10.732403	-0.061564	4.815406
304.306117	8000.174930	10.737408	-0.061578	4.815424
304.220641	8000.109369	10.742413	-0.061561	4.815405
304.208322	8000.078157	10.747418	-0.061559	4.815396
304.209610	8000.126269	10.752423	-0.061559	4.815410
304.055042	8000.032840	10.757427	-0.061530	4.815384
304.253008	8000.116280	10.762432	-0.061567	4.815407
304.005000	8000.072609	10.767437	-0.061521	4.815396
304.185444	8000.079866	10.772442	-0.061554	4.815397
304.199041	8000.151698	10.777447	-0.061557	4.815418
304.201605	8000.074770	10.782451	-0.061557	4.815395
304.277857	8000.089920	10.787456	-0.061571	4.815399
304.153038	8000.089978	10.792461	-0.061548	4.815400
304.405205	8000.114459	10.797466	-0.061595	4.815406
304.274147	8000.160377	10.802471	-0.061570	4.815420
304.427279	8000.074187	10.807475	-0.061598	4.815394
304.385575	8000.137620	10.812480	-0.061591	4.815413
304.307561	8000.140592	10.817485	-0.061576	4.815414
304.285542	8000.088910	10.822490	-0.061572	4.815399
304.275026	8000.118655	10.827495	-0.061570	4.815408
304.207249	8000.101488	10.832499	-0.061557	4.815403
304.260039	8000.075631	10.837504	-0.061567	4.815395
304.260340	8000.061730	10.842509	-0.061567	4.815391
304.146867	8000.038461	10.847514	-0.061545	4.815385
304.311649	8000.096766	10.852519	-0.061576	4.815401
304.161520	8000.037616	10.857523	-0.061548	4.815385
304.304095	8000.123344	10.862528	-0.061574	4.815409
304.248383	8000.161960	10.867533	-0.061564	4.815421
304.365715	8000.131828	10.872538	-0.061586	4.815411
304.362029	8000.156342	10.877543	-0.061585	4.815419
304.174633	8000.085884	10.882547	-0.061550	4.815399
304.267457	8000.141927	10.887552	-0.061567	4.815415
304.182613	8000.120202	10.892557	-0.061551	4.815409
304.287368	8000.090931	10.897562	-0.061570	4.815400
304.221779	8000.099453	10.902567	-0.061558	4.815403
304.223688	8000.082373	10.907571	-0.061558	4.815398
304.490440	8000.124198	10.912576	-0.061608	4.815409
304.426745	8000.093202	10.917581	-0.061596	4.815400
304.380437	8000.057151	10.922586	-0.061587	4.815390
304.493679	8000.132773	10.927591	-0.061608	4.815411
304.435815	8000.052705	10.932595	-0.061597	4.815388
304.425109	8000.114514	10.937600	-0.061595	4.815406
304.254033	8000.066774	10.942605	-0.061563	4.815393
304.434702	8000.062277	10.947610	-0.061597	4.815391
304.416889	8000.096177	10.952615	-0.061593	4.815401
304.531594	8000.172893	10.957619	-0.061615	4.815423
304.468408	8000.191076	10.962624	-0.061603	4.815428
304.340351	8000.128014	10.967629	-0.061579	4.815410
304.221621	8000.147414	10.972634	-0.061557	4.815417
304.399322	8000.174936	10.977639	-0.061590	4.815424
304.430542	8000.151928	10.982643	-0.061595	4.815417
304.446010	8000.168208	10.987648	-0.061598	4.815422
304.318671	8000.094470	10.992653	-0.061574	4.815401
304.308867	8000.093229	10.997658	-0.061572	4.815400
304.416907	8000.128146	11.002663	-0.061592	4.815410
304.181458	8000.096441	11.007667	-0.061548	4.815402
304.363082	8000.171059	11.012672	-0.061582	4.815423
304.215613	8000.182500	11.017677	-0.061554	4.815427
304.260601	8000.162927	11.022682	-0.061563	4.815421
304.272548	8000.144944	11.027687	-0.061565	4.815416
304.250696	8000.112504	11.032691	-0.061561	4.815406
304.307211	8000.152981	11.037696	-0.061571	4.815418
304.418810	8000.151615	11.042701	-0.061592	4.815417
304.539092	8000.147187	11.047706	-0.061614	4.815415
304.452527	8000.198118	11.052711	-0.061598	4.815430
304.130748	8000.115811	11.057715	-0.061538	4.815408
304.422862	8000.149505	11.062720	-0.061592	4.815416
304.254552	8000.119982	11.067725	-0.061561	4.815409
304.424664	8000.167687	11.072730	-0.061592	4.815422
304.319544	8000.190519	11.077735	-0.061573	4.815429
304.160414	8000.128012	11.082739	-0.061543	4.815411
304.213815	8000.189815	11.087744	-0.061553	4.815429
304.261060	8000.146763	11.092749	-0.061561	4.815416
304.256596	8000.071857	11.097754	-0.061560	4.815395
304.303242	8000.147443	11.102759	-0.061569	4.815416
304.130078	8000.119977	11.107763	-0.061537	4.815409
304.374046	8000.136840	11.112768	-0.061582	4.815413
304.439677	8000.117609	11.117773	-0.061594	4.815407
304.477267	8000.175944	11.122778	-0.061601	4.815424
304.547748	8000.163207	11.127783	-0.061614	4.815420
304.549257	8000.140775	11.132787	-0.061614	4.815413
304.651287	8000.163835	11.137792	-0.061633	4.815419
304.419131	8000.149286	11.142797	-0.061590	4.815416
304.567694	8000.148533	11.147802	-0.061617	4.815415
304.506825	8000.193477	11.152807	-0.061606	4.815429
304.339233	8000.160759	11.157811	-0.061574	4.815420
304.451431	8000.227813	11.162816	-0.061595	4.815439
304.588497	8000.173424	11.167821	-0.061621	4.815423
304.561744	8000.149455	11.172826	-0.061616	4.815416
304.561404	8000.183644	11.177831	-0.061615	4.815426
304.644433	8000.133704	11.182835	-0.061631	4.815411
304.439268	8000.177324	11.187840	-0.061592	4.815424
304.316398	8000.159243	11.192845	-0.061569	4.815420
304.458760	8000.171214	11.197850	-0.061596	4.815423
304.660835	8000.143557	11.202855	-0.061633	4.815414
304.369554	8000.083134	11.207859	-0.061579	4.815397
304.486684	8000.163096	11.212864	-0.061601	4.815420
304.653544	8000.151958	11.217869	-0.061632	4.815416
304.435946	8000.214612	11.222874	-0.061591	4.815435
304.653583	8000.224625	11.227879	-0.061631	4.815437
304.841725	8000.188186	11.232883	-0.061666	4.815426
304.610382	8000.203579	11.237888	-0.061623	4.815431
304.542259	8000.172510	11.242893	-0.061610	4.815423
304.544775	8000.131923	11.247898	-0.061611	4.815411
304.479942	8000.178939	11.252903	-0.061599	4.815425
304.403531	8000.158422	11.257907	-0.061584	4.815419
304.565997	8000.197449	11.262912	-0.061614	4.815430
304.676638	8000.155449	11.267917	-0.061635	4.815417
304.600896	8000.123185	11.272922	-0.061621	4.815408
304.747666	8000.155539	11.277927	-0.061648	4.815417
304.668788	8000.076190	11.282931	-0.061633	4.815394
304.631470	8000.121525	11.287936	-0.061626	4.815407
304.660100	8000.104887	11.292941	-0.061631	4.815402
304.742205	8000.086998	11.297946	-0.061646	4.815397
304.965316	8000.141997	11.302951	-0.061688	4.815412
304.846451	8000.095121	11.307955	-0.061666	4.815399
304.630582	8000.165286	11.312960	-0.061625	4.815420
304.632095	8000.171715	11.317965	-0.061625	4.815422
304.775303	8000.204010	11.322970	-0.061652	4.815431
304.755016	8000.211146	11.327975	-0.061648	4.815433
304.839819	8000.170855	11.332979	-0.061664	4.815421
304.594637	8000.173192	11.337984	-0.061618	4.815423
304.685200	8000.163995	11.342989	-0.061635	4.815419
304.621014	8000.130854	11.347994	-0.061623	4.815410
304.769746	8000.171791	11.352999	-0.061650	4.815421
304.624975	8000.108452	11.358003	-0.061623	4.815404
304.802265	8000.141312	11.363008	-0.061656	4.815412
304.843353	8000.113123	11.368013	-0.061664	4.815404
304.657158	8000.103612	11.373018	-0.061629	4.815402
304.591712	8000.138860	11.378023	-0.061617	4.815413
304.658039	8000.130330	11.383027	-0.061629	4.815410
304.706482	8000.171742	11.388032	-0.061638	4.815422
304.464951	8000.133522	11.393037	-0.061593	4.815412
304.499277	8000.098807	11.398042	-0.061599	4.815401
304.665998	8000.164628	11.403047	-0.061630	4.815420
304.530520	8000.118546	11.408051	-0.061604	4.815407
304.622435	8000.149990	11.413056	-0.061622	4.815416
304.708772	8000.127896	11.418061	-0.061637	4.815409
304.652618	8000.135506	11.423066	-0.061627	4.815411
304.695571	8000.121244	11.428071	-0.061635	4.815407
304.693109	8000.110504	11.433075	-0.061634	4.815404
304.639836	8000.125644	11.438080	-0.061624	4.815409
304.573537	8000.090330	11.443085	-0.061612	4.815399
304.406196	8000.075788	11.448090	-0.061580	4.815395
304.876482	8000.147711	11.453095	-0.061668	4.815414
304.547136	8000.101621	11.458099	-0.061606	4.815402
304.459947	8000.181402	11.463104	-0.061590	4.815426
304.574802	8000.155505	11.468109	-0.061611	4.815418
304.535005	8000.085357	11.473114	-0.061604	4.815397
304.564425	8000.172416	11.478119	-0.061609	4.815423
304.554714	8000.092077	11.483123	-0.061607	4.815399
304.816717	8000.158409	11.488128	-0.061656	4.815417
304.551535	8000.126210	11.493133	-0.061607	4.815409
304.587706	8000.125731	11.498138	-0.061613	4.815409
304.949571	8000.171272	11.503143	-0.061680	4.815420
304.735240	8000.108918	11.508147	-0.061640	4.815403
304.703135	8000.131891	11.513152	-0.061634	4.815410
304.801201	8000.074718	11.518157	-0.061652	4.815393
304.911693	8000.097919	11.523162	-0.061673	4.815399
304.924010	8000.138732	11.528167	-0.061675	4.815411
304.655261	8000.144954	11.533171	-0.061625	4.815414
304.850784	8000.178117	11.538176	-0.061661	4.815423
304.803125	8000.101423	11.543181	-0.061652	4.815401
304.743468	8000.054461	11.548186	-0.061641	4.815387
304.747260	8000.128269	11.553191	-0.061642	4.815409
304.749221	8000.088742	11.558195	-0.061642	4.815397
304.818318	8000.089878	11.563200	-0.061655	4.815397
304.748927	8000.129336	11.568205	-0.061642	4.815409
304.800880	8000.058571	11.573210	-0.061651	4.815388
304.698414	8000.169097	11.578215	-0.061632	4.815421
304.711498	8000.147926	11.583219	-0.061634	4.815415
304.923663	8000.164262	11.588224	-0.061674	4.815419
304.698887	8000.114561	11.593229	-0.061632	4.815405
304.647830	8000.020710	11.598234	-0.061622	4.815378
304.774381	8000.126483	11.603239	-0.061646	4.815408
304.746283	8000.089664	11.608243	-0.061640	4.815398
304.757736	8000.122980	11.613248	-0.061642	4.815407
304.897066	8000.125281	11.618253	-0.061668	4.815407
304.910057	8000.093419	11.623258	-0.061670	4.815398
304.748015	8000.136686	11.628263	-0.061640	4.815411
304.741616	8000.150465	11.633267	-0.061639	4.815415
304.961644	8000.173345	11.638272	-0.061680	4.815421
304.900307	8000.134906	11.643277	-0.061668	4.815410
304.774267	8000.131737	11.648282	-0.061645	4.815410
305.015058	8000.165651	11.653287	-0.061689	4.815419
305.044840	8000.089173	11.658291	-0.061695	4.815396
304.942711	8000.073573	11.663296	-0.061676	4.815392
304.798798	8000.117140	11.668301	-0.061649	4.815405
304.888496	8000.092964	11.673306	-0.061665	4.815398
305.072268	8000.145172	11.678311	-0.061699	4.815412
304.882776	8000.134537	11.683315	-0.061664	4.815410
304.964735	8000.143369	11.688320	-0.061679	4.815412
305.026279	8000.161482	11.693325	-0.061691	4.815417
304.743961	8000.137550	11.698330	-0.061638	4.815412
304.984052	8000.139384	11.703335	-0.061682	4.815411
305.108401	8000.110438	11.708339	-0.061705	4.815402
305.110872	8000.164984	11.713344	-0.061706	4.815418
304.959245	8000.159253	11.718349	-0.061678	4.815417
304.971952	8000.111352	11.723354	-0.061680	4.815403
305.029241	8000.170014	11.728359	-0.061690	4.815420
304.860209	8000.129789	11.733363	-0.061659	4.815409
304.884707	8000.193251	11.738368	-0.061663	4.815427
304.867627	8000.137374	11.743373	-0.061660	4.815411
304.833269	8000.152829	11.748378	-0.061653	4.815416
304.925722	8000.172524	11.753383	-0.061671	4.815421
304.960134	8000.113225	11.758387	-0.061677	4.815404
304.817374	8000.171776	11.763392	-0.061650	4.815421
304.844963	8000.138018	11.768397	-0.061655	4.815411
304.782675	8000.139113	11.773402	-0.061643	4.815412
305.227824	8000.192451	11.778407	-0.061726	4.815425
304.993475	8000.153279	11.783411	-0.061682	4.815415
305.124404	8000.190715	11.788416	-0.061707	4.815425
305.110221	8000.190470	11.793421	-0.061704	4.815425
304.981749	8000.148779	11.798426	-0.061680	4.815414
305.184472	8000.198096	11.803431	-0.061718	4.815427
305.039593	8000.135823	11.808435	-0.061690	4.815410
304.953383	8000.175003	11.813440	-0.061674	4.815422
304.874172	8000.145887	11.818445	-0.061659	4.815414
304.940032	8000.076421	11.823450	-0.061672	4.815393
304.887197	8000.176013	11.828455	-0.061662	4.815422
304.960564	8000.124843	11.833459	-0.061675	4.815407
304.910484	8000.163553	11.838464	-0.061666	4.815419
304.876979	8000.174745	11.843469	-0.061659	4.815422
304.893050	8000.131176	11.848474	-0.061662	4.815409
304.980566	8000.146514	11.853479	-0.061678	4.815413
304.962637	8000.108795	11.858483	-0.061675	4.815402
304.917677	8000.129418	11.863488	-0.061667	4.815409
305.017517	8000.186648	11.868493	-0.061685	4.815425
304.970517	8000.198685	11.873498	-0.061676	4.815429
305.029562	8000.227447	11.878503	-0.061687	4.815437
305.063338	8000.162793	11.883507	-0.061693	4.815418
305.012966	8000.157672	11.888512	-0.061684	4.815416
304.975396	8000.177348	11.893517	-0.061677	4.815422
304.959567	8000.123630	11.898522	-0.061674	4.815407
305.020542	8000.177009	11.903527	-0.061685	4.815422
304.994844	8000.173366	11.908531	-0.061680	4.815421
304.935333	8000.144577	11.913536	-0.061669	4.815413
304.815042	8000.190673	11.918541	-0.061646	4.815427
304.878469	8000.179957	11.923546	-0.061658	4.815424
304.988432	8000.196736	11.928551	-0.061678	4.815428
304.944729	8000.165003	11.933555	-0.061670	4.815419
304.827320	8000.136323	11.938560	-0.061648	4.815411
304.946231	8000.148975	11.943565	-0.061670	4.815414
304.910717	8000.150514	11.948570	-0.061663	4.815415
305.140007	8000.161789	11.953575	-0.061706	4.815417
305.009203	8000.157472	11.958579	-0.061682	4.815416
305.154368	8000.184455	11.963584	-0.061708	4.815424
305.084816	8000.187567	11.968589	-0.061695	4.815425
305.082755	8000.189661	11.973594	-0.061695	4.815425
305.107235	8000.206091	11.978599	-0.061699	4.815430
304.992826	8000.128290	11.983603	-0.061678	4.815408
305.023313	8000.180094	11.988608	-0.061683	4.815423
305.105560	8000.196414	11.993613	-0.061699	4.815427
304.973495	8000.170697	11.998618	-0.061674	4.815420
305.021818	8000.186454	12.003623	-0.061683	4.815425
304.974593	8000.120457	12.008627	-0.061674	4.815406
304.980361	8000.161161	12.013632	-0.061675	4.815418
305.095605	8000.188717	12.018637	-0.061696	4.815425
304.952710	8000.195957	12.023642	-0.061670	4.815428
305.222863	8000.216463	12.028647	-0.061720	4.815433
305.079766	8000.131772	12.033651	-0.061693	4.815409
305.041687	8000.162129	12.038656	-0.061686	4.815418
305.053626	8000.168731	12.043661	-0.061688	4.815419
305.195771	8000.197802	12.048666	-0.061714	4.815427
305.223398	8000.175803	12.053671	-0.061719	4.815421
305.222066	8000.156531	12.058675	-0.061719	4.815415
305.130266	8000.176377	12.063680	-0.061702	4.815421
305.108303	8000.176002	12.068685	-0.061698	4.815421
305.025810	8000.163935	12.073690	-0.061682	4.815418
305.168759	8000.142780	12.078695	-0.061709	4.815411
305.085005	8000.124278	12.083699	-0.061693	4.815406
305.033577	8000.151207	12.088704	-0.061683	4.815414
304.965953	8000.180006	12.093709	-0.061671	4.815423
304.860350	8000.146177	12.098714	-0.061651	4.815414
305.003236	8000.203052	12.103719	-0.061677	4.815430
304.894550	8000.099692	12.108723	-0.061657	4.815400
305.254165	8000.144128	12.113728	-0.061724	4.815411
305.302439	8000.158815	12.118733	-0.061733	4.815415
305.176819	8000.170617	12.123738	-0.061709	4.815419
305.178493	8000.198427	12.128743	-0.061709	4.815428
305.040601	8000.175821	12.133747	-0.061684	4.815422
305.121505	8000.186773	12.138752	-0.061698	4.815424
304.889884	8000.176508	12.143757	-0.061655	4.815423
305.064251	8000.168701	12.148762	-0.061688	4.815419
305.078405	8000.156099	12.153767	-0.061690	4.815416
305.039242	8000.137268	12.158771	-0.061683	4.815410
305.114510	8000.141713	12.163776	-0.061697	4.815411
305.037496	8000.188528	12.168781	-0.061682	4.815425
304.988722	8000.175951	12.173786	-0.061673	4.815422
304.960849	8000.149824	12.178791	-0.061668	4.815414
305.063983	8000.104493	12.183795	-0.061687	4.815401
305.038715	8000.157510	12.188800	-0.061682	4.815416
304.952348	8000.121862	12.193805	-0.061666	4.815406
305.222086	8000.148774	12.198810	-0.061716	4.815413
305.398837	8000.155971	12.203815	-0.061749	4.815414
305.086905	8000.134754	12.208819	-0.061690	4.815409
305.335592	8000.143144	12.213824	-0.061737	4.815411
305.295444	8000.165985	12.218829	-0.061729	4.815418
305.061425	8000.159956	12.223834	-0.061685	4.815417
305.116574	8000.186515	12.228839	-0.061696	4.815424
305.096811	8000.141282	12.233843	-0.061692	4.815411
305.259935	8000.209183	12.238848	-0.061722	4.815430
305.268588	8000.189007	12.243853	-0.061724	4.815424
305.150644	8000.148559	12.248858	-0.061701	4.815413
305.093416	8000.193564	12.253863	-0.061691	4.815427
304.962065	8000.150756	12.258867	-0.061666	4.815415
305.082781	8000.119612	12.263872	-0.061688	4.815405
305.122706	8000.161953	12.268877	-0.061696	4.815417
305.011407	8000.138718	12.273882	-0.061675	4.815411
305.119825	8000.177919	12.278887	-0.061695	4.815422
305.177901	8000.176735	12.283891	-0.061706	4.815421
305.171296	8000.189442	12.288896	-0.061704	4.815425
305.349592	8000.181701	12.293901	-0.061738	4.815422
305.213931	8000.187992	12.298906	-0.061712	4.815424
305.047249	8000.187355	12.303911	-0.061681	4.815425
305.111492	8000.160619	12.308915	-0.061693	4.815417
305.121369	8000.202461	12.313920	-0.061695	4.815429
305.153228	8000.183739	12.318925	-0.061700	4.815424
305.071072	8000.120369	12.323930	-0.061685	4.815405
305.034839	8000.214892	12.328935	-0.061678	4.815433
305.007999	8000.208024	12.333939	-0.061673	4.815431
305.251514	8000.212053	12.338944	-0.061718	4.815431
305.198856	8000.209032	12.343949	-0.061708	4.815431
305.079459	8000.164285	12.348954	-0.061686	4.815418
305.179344	8000.231136	12.353959	-0.061705	4.815437
305.037373	8000.176394	12.358963	-0.061678	4.815422
305.207447	8000.197377	12.363968	-0.061710	4.815427
305.047992	8000.175482	12.368973	-0.061680	4.815422
304.993451	8000.171361	12.373978	-0.061669	4.815421
305.060777	8000.214155	12.378983	-0.061682	4.815433
305.145558	8000.187760	12.383987	-0.061698	4.815425
305.152643	8000.188937	12.388992	-0.061699	4.815425
305.035234	8000.122844	12.393997	-0.061677	4.815406
305.077718	8000.152400	12.399002	-0.061685	4.815415
305.251804	8000.209793	12.404007	-0.061717	4.815431
305.027216	8000.159025	12.409011	-0.061675	4.815417
305.238655	8000.180694	12.414016	-0.061714	4.815422
305.184668	8000.205443	12.419021	-0.061704	4.815430
305.170668	8000.220166	12.424026	-0.061701	4.815434
305.226363	8000.240320	12.429031	-0.061712	4.815440
305.123635	8000.178747	12.434035	-0.061692	4.815422
304.946833	8000.150150	12.439040	-0.061659	4.815415
305.075662	8000.166173	12.444045	-0.061683	4.815419
305.154313	8000.169606	12.449050	-0.061698	4.815419
305.297255	8000.202966	12.454055	-0.061724	4.815429
305.059684	8000.171223	12.459059	-0.061680	4.815420
305.085732	8000.166301	12.464064	-0.061685	4.815419
305.185094	8000.173284	12.469069	-0.061703	4.815420
305.091890	8000.174935	12.474074	-0.061686	4.815421
305.239566	8000.210511	12.479079	-0.061713	4.815431
305.196615	8000.180928	12.484083	-0.061705	4.815423
305.322405	8000.189418	12.489088	-0.061728	4.815424
305.134227	8000.200183	12.494093	-0.061693	4.815429
305.214603	8000.182266	12.499098	-0.061708	4.815423
305.437277	8000.235121	12.504103	-0.061749	4.815437
305.298558	8000.201811	12.509107	-0.061723	4.815428
305.267755	8000.189532	12.514112	-0.061717	4.815425
305.308132	8000.207294	12.519117	-0.061725	4.815430
305.285574	8000.152395	12.524122	-0.061721	4.815414
305.357444	8000.214506	12.529127	-0.061734	4.815432
305.405983	8000.205681	12.534131	-0.061743	4.815429
305.559857	8000.244568	12.539136	-0.061771	4.815439
305.483763	8000.208021	12.544141	-0.061757	4.815429
305.357926	8000.177063	12.549146	-0.061733	4.815421
305.280133	8000.191796	12.554151	-0.061719	4.815425
305.260306	8000.172217	12.559155	-0.061715	4.815420
305.422885	8000.201627	12.564160	-0.061745	4.815428
305.334580	8000.195877	12.569165	-0.061729	4.815426
305.205160	8000.087897	12.574170	-0.061704	4.815395
305.487271	8000.195183	12.579175	-0.061757	4.815425
305.439496	8000.159106	12.584179	-0.061748	4.815415
305.570515	8000.208303	12.589184	-0.061772	4.815429
305.276943	8000.188458	12.594189	-0.061717	4.815424
305.306935	8000.126948	12.599194	-0.061723	4.815406
305.540338	8000.183187	12.604199	-0.061766	4.815422
305.329578	8000.186095	12.609203	-0.061727	4.815424
305.431630	8000.217708	12.614208	-0.061746	4.815432
305.469126	8000.220458	12.619213	-0.061753	4.815433
305.323394	8000.169929	12.624218	-0.061725	4.815419
305.397374	8000.175422	12.629223	-0.061739	4.815420
305.421173	8000.161911	12.634227	-0.061743	4.815416
305.499409	8000.216646	12.639232	-0.061758	4.815432
305.457764	8000.203118	12.644237	-0.061750	4.815428
305.228382	8000.144787	12.649242	-0.061707	4.815412
305.456938	8000.193464	12.654247	-0.061750	4.815425
305.466808	8000.170101	12.659251	-0.061751	4.815418
305.341573	8000.228943	12.664256	-0.061728	4.815436
305.340600	8000.226779	12.669261	-0.061728	4.815435
305.265109	8000.152830	12.674266	-0.061713	4.815414
305.516117	8000.231809	12.679271	-0.061760	4.815436
305.144901	8000.172195	12.684275	-0.061691	4.815420
305.440432	8000.187777	12.689280	-0.061746	4.815424
305.333228	8000.192402	12.694285	-0.061726	4.815425
305.356083	8000.193840	12.699290	-0.061730	4.815426
305.596728	8000.187133	12.704295	-0.061775	4.815423
305.462586	8000.178485	12.709299	-0.061749	4.815421
305.421169	8000.152133	12.714304	-0.061742	4.815413
305.480835	8000.190526	12.719309	-0.061753	4.815424
305.665437	8000.192510	12.724314	-0.061787	4.815424
305.661797	8000.219163	12.729319	-0.061786	4.815432
305.503928	8000.200500	12.734323	-0.061757	4.815427
305.579589	8000.182504	12.739328	-0.061771	4.815421
305.417364	8000.180872	12.744333	-0.061740	4.815422
305.225499	8000.196920	12.749338	-0.061704	4.815427
305.307904	8000.220725	12.754343	-0.061720	4.815434
305.306625	8000.179006	12.759347	-0.061719	4.815422
305.355030	8000.201178	12.764352	-0.061728	4.815428
305.457269	8000.201795	12.769357	-0.061747	4.815428
305.485637	8000.185153	12.774362	-0.061752	4.815423
305.477113	8000.229897	12.779367	-0.061751	4.815436
305.498217	8000.185342	12.784371	-0.061754	4.815423
305.628505	8000.173597	12.789376	-0.061779	4.815419
305.495711	8000.161764	12.794381	-0.061754	4.815416
305.330548	8000.153670	12.799386	-0.061723	4.815414
305.570369	8000.210016	12.804391	-0.061767	4.815429
305.585134	8000.150391	12.809395	-0.061770	4.815412
305.515552	8000.177019	12.814400	-0.061757	4.815420
305.438826	8000.178943	12.819405	-0.061743	4.815421
305.556420	8000.126369	12.824410	-0.061764	4.815405
305.613381	8000.196784	12.829415	-0.061775	4.815425
305.441470	8000.185371	12.834419	-0.061743	4.815423
305.338884	8000.158005	12.839424	-0.061724	4.815415
305.297487	8000.193652	12.844429	-0.061716	4.815426
305.441682	8000.205655	12.849434	-0.061742	4.815429
305.354256	8000.203126	12.854439	-0.061726	4.815429
305.333083	8000.164283	12.859443	-0.061722	4.815417
305.311082	8000.219493	12.864448	-0.061718	4.815434
305.347388	8000.240395	12.869453	-0.061724	4.815439
305.648116	8000.140619	12.874458	-0.061780	4.815409
305.638484	8000.217412	12.879463	-0.061778	4.815431
305.555265	8000.165782	12.884467	-0.061763	4.815417
305.582421	8000.166223	12.889472	-0.061768	4.815417
305.575105	8000.142575	12.894477	-0.061766	4.815410
305.500303	8000.156289	12.899482	-0.061752	4.815414
305.561559	8000.181881	12.904487	-0.061764	4.815421
305.487610	8000.168886	12.909491	-0.061750	4.815418
305.628755	8000.154115	12.914496	-0.061776	4.815413
305.574027	8000.158542	12.919501	-0.061766	4.815414
305.738364	8000.142018	12.924506	-0.061796	4.815409
305.725659	8000.213416	12.929511	-0.061794	4.815430
305.472771	8000.201728	12.934515	-0.061746	4.815428
305.469520	8000.207009	12.939520	-0.061746	4.815429
305.686441	8000.204184	12.944525	-0.061786	4.815427
305.567220	8000.176542	12.949530	-0.061764	4.815420
305.718346	8000.176902	12.954535	-0.061792	4.815419
305.615274	8000.161286	12.959539	-0.061772	4.815415
305.736772	8000.153671	12.964544	-0.061795	4.815412
305.532138	8000.172714	12.969549	-0.061757	4.815419
305.579675	8000.158528	12.974554	-0.061765	4.815414
305.887933	8000.182873	12.979559	-0.061823	4.815420
305.521616	8000.183199	12.984563	-0.061754	4.815422
305.583614	8000.206666	12.989568	-0.061766	4.815429
305.612513	8000.165447	12.994573	-0.061771	4.815416
305.492001	8000.117474	12.999578	-0.061748	4.815403
305.580420	8000.167033	13.004583	-0.061765	4.815417
305.715461	8000.137195	13.009587	-0.061790	4.815408
305.613171	8000.152591	13.014592	-0.061771	4.815413
305.559622	8000.179485	13.019597	-0.061761	4.815421
305.487937	8000.170804	13.024602	-0.061747	4.815419
305.593533	8000.207821	13.029607	-0.061767	4.815429
305.500325	8000.143198	13.034611	-0.061749	4.815410
305.656100	8000.162875	13.039616	-0.061778	4.815415
305.732154	8000.189781	13.044621	-0.061792	4.815423
305.425884	8000.167587	13.049626	-0.061735	4.815418
305.526166	8000.218412	13.054631	-0.061754	4.815432
305.503622	8000.136790	13.059635	-0.061749	4.815409
305.520726	8000.164856	13.064640	-0.061752	4.815417
305.336810	8000.132934	13.069645	-0.061718	4.815408
305.408975	8000.065710	13.074650	-0.061731	4.815388
305.572732	8000.155000	13.079655	-0.061762	4.815414
305.454496	8000.138063	13.084659	-0.061740	4.815409
305.417420	8000.121405	13.089664	-0.061733	4.815404
305.645678	8000.128388	13.094669	-0.061775	4.815405
305.751581	8000.100205	13.099674	-0.061795	4.815397
305.526521	8000.161666	13.104679	-0.061753	4.815416
305.700263	8000.145298	13.109683	-0.061785	4.815410
305.643749	8000.165729	13.114688	-0.061774	4.815416
305.493306	8000.211326	13.119693	-0.061746	4.815430
305.639017	8000.164562	13.124698	-0.061773	4.815416
305.769818	8000.185963	13.129703	-0.061797	4.815422
305.610636	8000.168348	13.134707	-0.061768	4.815417
305.651956	8000.148714	13.139712	-0.061775	4.815411
305.891433	8000.183676	13.144717	-0.061820	4.815420
305.718614	8000.155144	13.149722	-0.061787	4.815413
305.707230	8000.178462	13.154727	-0.061785	4.815420
305.529381	8000.142365	13.159731	-0.061752	4.815410
305.685713	8000.189844	13.164736	-0.061781	4.815423
305.516609	8000.184891	13.169741	-0.061749	4.815423
305.559363	8000.167418	13.174746	-0.061757	4.815417
305.808076	8000.235671	13.179751	-0.061803	4.815436
305.639415	8000.186899	13.184755	-0.061772	4.815423
305.625014	8000.188788	13.189760	-0.061769	4.815423
305.664838	8000.192645	13.194765	-0.061776	4.815424
305.682709	8000.158726	13.199770	-0.061780	4.815414
305.599651	8000.180855	13.204775	-0.061764	4.815421
305.547392	8000.153255	13.209779	-0.061754	4.815413
305.584682	8000.162415	13.214784	-0.061761	4.815416
305.956341	8000.209191	13.219789	-0.061830	4.815428
305.565560	8000.133217	13.224794	-0.061757	4.815407
305.662440	8000.220329	13.229799	-0.061775	4.815432
305.605781	8000.192656	13.234803	-0.061765	4.815424
305.831370	8000.183562	13.239808	-0.061806	4.815421
305.783375	8000.180618	13.244813	-0.061797	4.815420
305.835716	8000.140857	13.249818	-0.061807	4.815408
305.870297	8000.190592	13.254823	-0.061813	4.815423
305.792407	8000.195703	13.259827	-0.061799	4.815424
305.776611	8000.199707	13.264832	-0.061796	4.815426
305.701958	8000.208079	13.269837	-0.061782	4.815429
305.595428	8000.192406	13.274842	-0.061762	4.815424
305.607932	8000.217189	13.279847	-0.061764	4.815432
305.602877	8000.198923	13.284851	-0.061763	4.815426
305.509957	8000.179200	13.289856	-0.061745	4.815421
305.658558	8000.182724	13.294861	-0.061773	4.815421
305.650587	8000.166548	13.299866	-0.061771	4.815417
305.816466	8000.196014	13.304871	-0.061802	4.815424
305.730964	8000.137932	13.309875	-0.061786	4.815408
305.803178	8000.139120	13.314880	-0.061799	4.815408
305.795301	8000.171048	13.319885	-0.061798	4.815417
305.526676	8000.171926	13.324890	-0.061748	4.815419
305.616625	8000.173409	13.329895	-0.061764	4.815419
305.494538	8000.141443	13.334899	-0.061742	4.815410
305.782378	8000.153691	13.339904	-0.061795	4.815412
305.729581	8000.205183	13.344909	-0.061785	4.815428
305.912514	8000.197519	13.349914	-0.061819	4.815424
305.861281	8000.213762	13.354919	-0.061809	4.815429
305.470848	8000.180552	13.359923	-0.061737	4.815422
305.825823	8000.218499	13.364928	-0.061803	4.815431
305.934982	8000.233128	13.369933	-0.061823	4.815435
305.779868	8000.205959	13.374938	-0.061794	4.815428
305.831746	8000.253843	13.379943	-0.061803	4.815441
305.820104	8000.171332	13.384947	-0.061801	4.815417
305.667497	8000.138860	13.389952	-0.061773	4.815409
305.500017	8000.156381	13.394957	-0.061741	4.815414
305.438171	8000.128623	13.399962	-0.061730	4.815407
305.652376	8000.131097	13.404967	-0.061769	4.815406
305.522223	8000.135342	13.409971	-0.061745	4.815408
305.768826	8000.215317	13.414976	-0.061791	4.815430
305.720669	8000.228405	13.419981	-0.061782	4.815434
305.473559	8000.145194	13.424986	-0.061736	4.815411
305.539714	8000.200797	13.429991	-0.061748	4.815427
305.627867	8000.191561	13.434995	-0.061764	4.815424
305.501925	8000.175565	13.440000	-0.061741	4.815420
305.831036	8000.170326	13.445005	-0.061802	4.815417
305.666128	8000.104514	13.450010	-0.061771	4.815399
305.701060	8000.098670	13.455015	-0.061777	4.815397
305.637942	8000.142508	13.460019	-0.061766	4.815410
305.694419	8000.171227	13.465024	-0.061776	4.815418
305.961661	8000.192754	13.470029	-0.061826	4.815423
305.871170	8000.167726	13.475034	-0.061809	4.815416
305.919594	8000.147141	13.480039	-0.061818	4.815410
305.787630	8000.167390	13.485043	-0.061793	4.815416
305.853714	8000.220854	13.490048	-0.061805	4.815432
305.787471	8000.191953	13.495053	-0.061793	4.815424
305.648804	8000.158643	13.500058	-0.061767	4.815414
305.852672	8000.195153	13.505063	-0.061805	4.815424
305.760078	8000.187193	13.510067	-0.061787	4.815422
305.602486	8000.126847	13.515072	-0.061758	4.815405
305.623209	8000.176351	13.520077	-0.061761	4.815420
305.598334	8000.132103	13.525082	-0.061757	4.815407
305.885051	8000.143263	13.530087	-0.061810	4.815409
305.911492	8000.168277	13.535091	-0.061815	4.815416
305.861232	8000.190950	13.540096	-0.061805	4.815423
305.838266	8000.162767	13.545101	-0.061801	4.815415
305.804446	8000.121577	13.550106	-0.061795	4.815403
305.775818	8000.161711	13.555111	-0.061789	4.815415
305.717145	8000.147901	13.560115	-0.061778	4.815411
305.789894	8000.160856	13.565120	-0.061791	4.815414
305.864788	8000.144986	13.570125	-0.061805	4.815409
305.794873	8000.087163	13.575130	-0.061792	4.815393
305.752746	8000.166624	13.580135	-0.061784	4.815416
305.724065	8000.176828	13.585139	-0.061779	4.815419
305.588953	8000.160681	13.590144	-0.061754	4.815415
305.657706	8000.185328	13.595149	-0.061766	4.815422
305.646266	8000.112441	13.600154	-0.061764	4.815401
305.736058	8000.143851	13.605159	-0.061781	4.815410
305.753285	8000.151609	13.610163	-0.061784	4.815412
305.709354	8000.125216	13.615168	-0.061775	4.815404
305.857569	8000.216387	13.620173	-0.061803	4.815430
305.583947	8000.170149	13.625178	-0.061752	4.815418
305.722574	8000.208783	13.630183	-0.061778	4.815429
305.753057	8000.209279	13.635187	-0.061783	4.815429
305.762791	8000.179500	13.640192	-0.061785	4.815420
305.745566	8000.210204	13.645197	-0.061782	4.815429
305.781441	8000.122068	13.650202	-0.061788	4.815403
305.893695	8000.180574	13.655207	-0.061809	4.815420
305.766050	8000.179515	13.660211	-0.061785	4.815420
305.655684	8000.166985	13.665216	-0.061764	4.815417
305.828827	8000.179468	13.670221	-0.061796	4.815420
305.625226	8000.098049	13.675226	-0.061758	4.815397
305.778294	8000.112336	13.680231	-0.061787	4.815400
305.715838	8000.124117	13.685235	-0.061775	4.815404
305.797337	8000.114770	13.690240	-0.061790	4.815401
305.884083	8000.170715	13.695245	-0.061806	4.815417
305.808281	8000.088209	13.700250	-0.061792	4.815393
306.125151	8000.144765	13.705255	-0.061851	4.815408
306.004205	8000.183368	13.710259	-0.061828	4.815420
305.893618	8000.181523	13.715264	-0.061808	4.815420
305.978567	8000.226750	13.720269	-0.061823	4.815433
305.824385	8000.202803	13.725274	-0.061794	4.815427
305.850953	8000.198958	13.730279	-0.061799	4.815425
305.710988	8000.184868	13.735283	-0.061773	4.815422
306.048048	8000.154106	13.740288	-0.061836	4.815411
305.890860	8000.172867	13.745293	-0.061806	4.815418
305.857063	8000.117781	13.750298	-0.061800	4.815402
305.929648	8000.170284	13.755303	-0.061813	4.815417
305.994691	8000.124320	13.760307	-0.061825	4.815403
305.879542	8000.093539	13.765312	-0.061804	4.815395
305.913790	8000.186026	13.770317	-0.061810	4.815421
305.828325	8000.132220	13.775322	-0.061794	4.815406
305.810553	8000.109468	13.780327	-0.061791	4.815399
305.868512	8000.089041	13.785331	-0.061801	4.815393
305.867757	8000.167051	13.790336	-0.061801	4.815416
305.834372	8000.166487	13.795341	-0.061795	4.815416
305.737654	8000.161666	13.800346	-0.061777	4.815415
305.796729	8000.204325	13.805351	-0.061788	4.815427
305.907003	8000.117423	13.810355	-0.061808	4.815401
305.721204	8000.091883	13.815360	-0.061773	4.815395
305.771746	8000.147227	13.820365	-0.061782	4.815411
305.798217	8000.111313	13.825370	-0.061787	4.815400
305.800744	8000.202204	13.830375	-0.061788	4.815427
305.696474	8000.147018	13.835379	-0.061768	4.815411
305.718993	8000.139899	13.840384	-0.061772	4.815409
305.594360	8000.176303	13.845389	-0.061749	4.815420
305.680219	8000.156339	13.850394	-0.061765	4.815414
305.884181	8000.203540	13.855399	-0.061803	4.815427
305.913293	8000.116360	13.860403	-0.061808	4.815401
305.885260	8000.128712	13.865408	-0.061803	4.815405
305.855246	8000.130342	13.870413	-0.061797	4.815405
305.832250	8000.103228	13.875418	-0.061793	4.815398
305.843085	8000.170740	13.880423	-0.061794	4.815417
305.694868	8000.163996	13.885427	-0.061767	4.815416
305.827065	8000.115939	13.890432	-0.061791	4.815401
305.977570	8000.196459	13.895437	-0.061819	4.815424
305.750980	8000.141381	13.900442	-0.061777	4.815409
305.911268	8000.173960	13.905447	-0.061807	4.815418
305.874597	8000.146619	13.910451	-0.061800	4.815410
305.914304	8000.153681	13.915456	-0.061807	4.815412
305.769478	8000.188682	13.920461	-0.061780	4.815423
305.768363	8000.144827	13.925466	-0.061780	4.815410
305.634285	8000.185350	13.930471	-0.061754	4.815423
305.838329	8000.141692	13.935475	-0.061792	4.815409
305.800969	8000.094030	13.940480	-0.061785	4.815395
305.955812	8000.155380	13.945485	-0.061814	4.815412
305.921495	8000.144112	13.950490	-0.061808	4.815409
305.834353	8000.142656	13.955495	-0.061791	4.815409
306.008245	8000.120946	13.960499	-0.061823	4.815402
305.986330	8000.136606	13.965504	-0.061819	4.815407
305.866346	8000.192328	13.970509	-0.061797	4.815424
305.922935	8000.144086	13.975514	-0.061807	4.815409
305.882570	8000.116683	13.980519	-0.061800	4.815401
305.809519	8000.138978	13.985523	-0.061786	4.815408
306.085406	8000.123236	13.990528	-0.061837	4.815402
305.872543	8000.150694	13.995533	-0.061797	4.815411
305.706014	8000.128680	14.000538	-0.061766	4.815406
305.829784	8000.160654	14.005543	-0.061789	4.815414
305.757369	8000.180821	14.010547	-0.061776	4.815421
305.902870	8000.111607	14.015552	-0.061803	4.815400
305.792388	8000.154659	14.020557	-0.061782	4.815413
305.784268	8000.151308	14.025562	-0.061780	4.815412
305.988562	8000.163239	14.030567	-0.061818	4.815414
305.857246	8000.178154	14.035571	-0.061794	4.815419
306.073138	8000.155002	14.040576	-0.061834	4.815412
306.009357	8000.178520	14.045581	-0.061822	4.815419
305.882558	8000.115477	14.050586	-0.061798	4.815401
305.771271	8000.126448	14.055591	-0.061777	4.815405
305.908947	8000.107344	14.060595	-0.061803	4.815399
306.010513	8000.060917	14.065600	-0.061821	4.815385
306.077981	8000.175333	14.070605	-0.061834	4.815418
306.015125	8000.129385	14.075610	-0.061822	4.815404
306.159504	8000.186287	14.080615	-0.061849	4.815420
305.848754	8000.149053	14.085619	-0.061791	4.815411
305.963287	8000.125289	14.090624	-0.061812	4.815404
306.164210	8000.179922	14.095629	-0.061850	4.815419
306.049790	8000.172669	14.100634	-0.061828	4.815417
305.929518	8000.213421	14.105639	-0.061806	4.815429
305.917543	8000.188627	14.110643	-0.061803	4.815422
305.971633	8000.136068	14.115648	-0.061813	4.815407
305.954519	8000.164635	14.120653	-0.061810	4.815415
305.921954	8000.191878	14.125658	-0.061804	4.815423
306.050764	8000.190798	14.130663	-0.061828	4.815422
306.095539	8000.202221	14.135667	-0.061836	4.815425
306.171716	8000.133994	14.140672	-0.061850	4.815405
306.198213	8000.180388	14.145677	-0.061855	4.815419
305.875132	8000.155777	14.150682	-0.061794	4.815413
305.838046	8000.127359	14.155687	-0.061787	4.815405
305.820158	8000.152707	14.160691	-0.061784	4.815412
305.804665	8000.085098	14.165696	-0.061781	4.815393
305.982785	8000.187454	14.170701	-0.061814	4.815422
305.757740	8000.169814	14.175706	-0.061772	4.815418
305.883759	8000.150516	14.180711	-0.061795	4.815411
305.784485	8000.172376	14.185715	-0.061777	4.815418
305.872354	8000.169548	14.190720	-0.061793	4.815417
306.008065	8000.187824	14.195725	-0.061818	4.815422
305.837577	8000.174296	14.200730	-0.061786	4.815419
305.902276	8000.151843	14.205735	-0.061798	4.815412
305.978693	8000.157377	14.210739	-0.061812	4.815413
306.213350	8000.139882	14.215744	-0.061856	4.815407
306.093934	8000.212716	14.220749	-0.061834	4.815429
305.827210	8000.142007	14.225754	-0.061784	4.815409
306.054461	8000.204559	14.230759	-0.061826	4.815426
306.016701	8000.181475	14.235763	-0.061819	4.815420
306.069009	8000.128886	14.240768	-0.061829	4.815404
306.261949	8000.233627	14.245773	-0.061864	4.815434
306.091326	8000.161305	14.250778	-0.061833	4.815414
306.047163	8000.208665	14.255783	-0.061824	4.815428
306.088558	8000.197583	14.260787	-0.061832	4.815424
306.021398	8000.138737	14.265792	-0.061819	4.815407
305.990635	7999.164445	14.270797	-0.061813	4.815123
305.773866	7996.011194	14.275802	-0.061770	4.814203
306.055056	7990.610312	14.280807	-0.061819	4.812623
305.788215	7983.941030	14.285811	-0.061765	4.810675
305.988825	7976.644782	14.290816	-0.061797	4.808541
305.984573	7968.994248	14.295821	-0.061791	4.806303
305.795569	7961.171639	14.300826	-0.061751	4.804014
305.801847	7953.356921	14.305831	-0.061747	4.801725
305.928435	7945.367724	14.310835	-0.061765	4.799384
305.804766	7937.433986	14.315840	-0.061737	4.797059
305.719577	7929.404676	14.320845	-0.061716	4.794705
305.491940	7921.377260	14.325850	-0.061668	4.792351
305.571053	7913.351949	14.330855	-0.061677	4.789995
305.571394	7905.444217	14.335859	-0.061672	4.787672
305.616010	7897.349753	14.340864	-0.061675	4.785293
305.730649	7889.473683	14.345869	-0.061691	4.782977
305.633772	7881.370336	14.350874	-0.061668	4.780594
305.464117	7873.431310	14.355879	-0.061631	4.778259
305.264746	7865.389831	14.360883	-0.061588	4.775892
305.436461	7857.359416	14.365888	-0.061615	4.773526
305.515472	7849.422807	14.370893	-0.061624	4.771187
305.381134	7841.333859	14.375898	-0.061594	4.768802
305.465518	7833.396712	14.380903	-0.061604	4.766460
305.518803	7825.362596	14.385907	-0.061609	4.764089
305.286821	7817.424126	14.390912	-0.061561	4.761745
305.351611	7809.366440	14.395917	-0.061567	4.759365
305.407345	7801.381298	14.400922	-0.061572	4.757004
305.247265	7793.356447	14.405927	-0.061537	4.754631
305.089755	7785.286123	14.410931	-0.061502	4.752244
305.103570	7777.271395	14.415936	-0.061500	4.749871
305.103129	7769.302671	14.420941	-0.061494	4.747511
304.796427	7761.319863	14.425946	-0.061432	4.745146
304.986889	7753.360122	14.430951	-0.061462	4.742786
304.914563	7745.345774	14.435955	-0.061443	4.740409
304.770417	7737.304250	14.440960	-0.061411	4.738023
304.986717	7729.305145	14.445965	-0.061446	4.735647
305.016163	7721.300787	14.450970	-0.061446	4.733269
304.910865	7713.305451	14.455975	-0.061421	4.730893
304.986329	7705.349475	14.460979	-0.061430	4.728526
304.989288	7697.300279	14.465984	-0.061425	4.726131
304.814550	7689.309131	14.470989	-0.061387	4.723753
304.633685	7681.302117	14.475994	-0.061348	4.721369
304.708986	7673.340204	14.480999	-0.061357	4.718996
304.743122	7665.343190	14.486003	-0.061358	4.716612
304.537679	7657.322071	14.491008	-0.061315	4.714220
304.688071	7649.298578	14.496013	-0.061337	4.711825
304.675119	7641.251692	14.501018	-0.061329	4.709422
304.458192	7633.330639	14.506023	-0.061284	4.707056
304.458913	7625.284764	14.511027	-0.061279	4.704651
304.378475	7617.305040	14.516032	-0.061258	4.702265
304.501639	7609.298519	14.521037	-0.061276	4.699869
304.438467	7601.281195	14.526042	-0.061259	4.697470
304.525928	7593.265891	14.531047	-0.061270	4.695069
304.537862	7585.302080	14.536051	-0.061267	4.692682
304.219408	7577.248614	14.541056	-0.061202	4.690268
304.207898	7569.306406	14.546061	-0.061195	4.687886
304.180082	7561.247515	14.551066	-0.061184	4.685467
304.327365	7553.318547	14.556071	-0.061206	4.683086
304.186653	7545.276639	14.561075	-0.061175	4.680670
304.130246	7537.310009	14.566080	-0.061159	4.678276
304.211868	7529.308767	14.571085	-0.061169	4.675869
303.982414	7521.149288	14.576090	-0.061121	4.673415
303.982693	7513.132146	14.581095	-0.061115	4.671001
304.201152	7505.212384	14.586099	-0.061151	4.668615
304.135352	7497.189702	14.591104	-0.061133	4.666197
303.966432	7489.250482	14.596109	-0.061096	4.663804
303.957213	7481.237425	14.601114	-0.061089	4.661386
303.995664	7473.234924	14.606119	-0.061091	4.658971
303.775809	7465.244930	14.611123	-0.061045	4.656558
303.904051	7457.209752	14.616128	-0.061063	4.654130
303.972230	7449.179563	14.621133	-0.061071	4.651703
303.594886	7441.162508	14.626138	-0.060995	4.649278
303.886084	7433.216678	14.631143	-0.061044	4.646873
303.776695	7425.215031	14.636147	-0.061018	4.644450
303.496682	7417.241915	14.641152	-0.060961	4.642035
303.535936	7409.212008	14.646157	-0.060963	4.639601
303.382855	7401.238397	14.651162	-0.060929	4.637183
303.547061	7393.197607	14.656167	-0.060954	4.634744
303.402533	7385.183090	14.661171	-0.060922	4.632311
303.352490	7377.142164	14.666176	-0.060907	4.629868
303.448306	7369.202241	14.671181	-0.060920	4.627455
303.196090	7361.131571	14.676186	-0.060868	4.625001
303.300538	7353.203098	14.681191	-0.060882	4.622589
303.490888	7345.185481	14.686195	-0.060912	4.620149
303.389942	7337.189302	14.691200	-0.060888	4.617714
303.225328	7329.209659	14.696205	-0.060852	4.615282
303.442548	7321.135043	14.701210	-0.060887	4.612821
303.465979	7313.097415	14.706215	-0.060886	4.610369
303.355533	7305.180681	14.711219	-0.060860	4.607953
303.204770	7297.158797	14.716224	-0.060827	4.605503
303.371944	7289.198259	14.721229	-0.060852	4.603071
303.264679	7281.128759	14.726234	-0.060827	4.600604
303.147965	7273.184067	14.731239	-0.060800	4.598175
303.089114	7265.167061	14.736243	-0.060784	4.595721
302.929805	7257.079071	14.741248	-0.060749	4.593245
302.829245	7249.092212	14.746253	-0.060725	4.590798
302.791202	7241.125841	14.751258	-0.060712	4.588357
302.939247	7233.121635	14.756263	-0.060735	4.585902
302.874195	7225.154681	14.761267	-0.060717	4.583457
302.697974	7217.123140	14.766272	-0.060679	4.580992
302.730240	7209.151353	14.771277	-0.060680	4.578543
302.688550	7201.096690	14.776282	-0.060667	4.576068
302.597764	7193.131819	14.781287	-0.060644	4.573618
302.739968	7185.097482	14.786291	-0.060666	4.571147
302.770213	7177.089110	14.791296	-0.060666	4.568682
302.730411	7169.123814	14.796301	-0.060653	4.566228
302.513274	7161.128034	14.801306	-0.060607	4.563764
302.652732	7153.159563	14.806311	-0.060628	4.561307
302.510623	7145.075087	14.811315	-0.060596	4.558813
302.405711	7137.119317	14.816320	-0.060571	4.556358
302.575311	7129.101968	14.821325	-0.060598	4.553882
302.373962	7121.071471	14.826330	-0.060555	4.551400
302.359938	7113.083898	14.831335	-0.060547	4.548931
302.374682	7105.125755	14.836339	-0.060544	4.546469
302.242173	7097.082951	14.841344	-0.060514	4.543979
302.555662	7089.168162	14.846349	-0.060567	4.541529
302.307997	7081.084422	14.851354	-0.060516	4.539024
302.337519	7073.140551	14.856359	-0.060516	4.536561
302.392475	7065.108262	14.861363	-0.060521	4.534070
302.386220	7057.086792	14.866368	-0.060514	4.531580
302.513125	7049.081950	14.871373	-0.060533	4.529095
302.386815	7041.109259	14.876378	-0.060504	4.526618
302.165284	7033.126580	14.881383	-0.060457	4.524136
302.140732	7025.122911	14.886387	-0.060447	4.521646
302.251356	7017.076560	14.891392	-0.060463	4.519142
302.268221	7009.163629	14.896397	-0.060461	4.516678
301.889741	7001.044638	14.901402	-0.060385	4.514148
302.079821	6993.059089	14.906407	-0.060415	4.511659
302.157961	6985.034745	14.911411	-0.060424	4.509157
301.779047	6977.039577	14.916416	-0.060348	4.506661
301.751417	6969.092033	14.921421	-0.060338	4.504179
301.926586	6961.055240	14.926426	-0.060365	4.501668
301.856943	6953.037996	14.931431	-0.060347	4.499162
301.746332	6945.078511	14.936435	-0.060321	4.496672
301.787193	6937.061262	14.941440	-0.060323	4.494164
301.977202	6929.066028	14.946445	-0.060353	4.491661
301.739040	6921.044400	14.951450	-0.060303	4.489147
301.653450	6913.069692	14.956455	-0.060282	4.486647
301.670075	6905.075569	14.961459	-0.060280	4.484139
301.529245	6897.044747	14.966464	-0.060248	4.481619
301.511874	6889.077867	14.971469	-0.060240	4.479117
301.554602	6881.051242	14.976474	-0.060242	4.476595
301.413192	6873.044010	14.981479	-0.060211	4.474078
301.284661	6865.002508	14.986483	-0.060182	4.471548
301.304640	6857.015540	14.991488	-0.060180	4.469035
301.325072	6849.019184	14.996493	-0.060178	4.466517
301.317814	6841.044496	15.001498	-0.060172	4.464004
301.212358	6833.012092	15.006503	-0.060147	4.461471
301.232443	6825.069885	15.011507	-0.060145	4.458966
301.101512	6817.062758	15.016512	-0.060116	4.456439
301.354454	6809.028846	15.021517	-0.060157	4.453903
301.230794	6800.928044	15.026522	-0.060129	4.451343
301.077208	6792.986347	15.031527	-0.060095	4.448831
301.148361	6785.019678	15.036531	-0.060103	4.446312
301.093080	6776.978292	15.041536	-0.060087	4.443766
301.078070	6769.055335	15.046541	-0.060079	4.441257
300.783785	6761.020446	15.051546	-0.060019	4.438710
300.943453	6753.003806	15.056551	-0.060043	4.436169
300.787514	6744.963593	15.061555	-0.060009	4.433618
300.755501	6736.913561	15.066560	-0.059998	4.431062
300.944807	6728.977084	15.071565	-0.060028	4.428542
300.670902	6720.920110	15.076570	-0.059971	4.425981
300.641660	6712.984105	15.081575	-0.059961	4.423457
300.848195	6704.975589	15.086579	-0.059994	4.420910
300.754300	6696.963364	15.091584	-0.059971	4.418359
300.725001	6688.976391	15.096589	-0.059960	4.415815
300.592174	6680.949602	15.101594	-0.059930	4.413256
300.528743	6672.931344	15.106599	-0.059913	4.410699
300.605204	6664.944914	15.111603	-0.059922	4.408151
300.606996	6656.944716	15.116608	-0.059917	4.405597
300.626737	6648.995774	15.121613	-0.059915	4.403058
300.625107	6640.962907	15.126618	-0.059910	4.400491
300.481119	6633.025896	15.131623	-0.059878	4.397951
300.422958	6624.991640	15.136627	-0.059861	4.395380
300.536565	6616.961163	15.141632	-0.059877	4.392810
300.621995	6608.957264	15.146637	-0.059888	4.390246
300.339011	6600.941990	15.151642	-0.059830	4.387675
300.437034	6592.918064	15.156647	-0.059843	4.385102
300.495415	6585.007463	15.161651	-0.059848	4.382563
300.384753	6576.935337	15.166656	-0.059822	4.379970
300.104357	6569.004183	15.171661	-0.059765	4.377420
300.109947	6560.936641	15.176666	-0.059760	4.374827
300.193572	6552.969470	15.181671	-0.059771	4.372264
300.313559	6544.957785	15.186675	-0.059788	4.369686
300.244674	6536.963069	15.191680	-0.059770	4.367110
300.277277	6528.984731	15.196685	-0.059770	4.364540
300.064876	6520.998377	15.201690	-0.059725	4.361963
299.978110	6513.007624	15.206695	-0.059704	4.359384
299.830159	6505.035410	15.211699	-0.059671	4.356809
299.833446	6496.907495	15.216704	-0.059666	4.354184
299.864308	6488.872773	15.221709	-0.059667	4.351587
299.725087	6480.883912	15.226714	-0.059636	4.349002
299.858213	6472.890454	15.231719	-0.059655	4.346416
299.807328	6464.918026	15.236723	-0.059640	4.343834
299.604937	6456.945807	15.241728	-0.059597	4.341250
299.833590	6448.987678	15.246733	-0.059634	4.338672
299.617681	6440.932960	15.251738	-0.059589	4.336057
299.534894	6432.928428	15.256743	-0.059568	4.333458
299.637822	6424.940113	15.261747	-0.059582	4.330865
299.561160	6416.914357	15.266752	-0.059562	4.328256
299.433951	6408.974251	15.271757	-0.059533	4.325673
299.371168	6400.995314	15.276762	-0.059516	4.323077
299.441513	6392.930037	15.281767	-0.059524	4.320451
299.315076	6384.993832	15.286771	-0.059495	4.317865
299.325752	6376.925278	15.291776	-0.059492	4.315235
299.390721	6368.906334	15.296781	-0.059499	4.312620
299.330767	6360.890340	15.301786	-0.059482	4.310003
299.284806	6352.918106	15.306791	-0.059468	4.307400
299.274444	6344.902124	15.311795	-0.059461	4.304780
299.269800	6336.951992	15.316800	-0.059455	4.302181
299.268788	6328.929313	15.321805	-0.059449	4.299556
299.273349	6320.931430	15.326810	-0.059445	4.296938
299.225090	6312.912077	15.331815	-0.059431	4.294311
299.173867	6304.901540	15.336819	-0.059416	4.291685
299.083662	6296.905461	15.341824	-0.059394	4.289062
299.001372	6288.908414	15.346829	-0.059373	4.286437
299.073790	6280.901980	15.351834	-0.059381	4.283809
298.998685	6272.910809	15.356839	-0.059362	4.281182
299.010630	6264.921417	15.361843	-0.059359	4.278556
298.878350	6256.925450	15.366848	-0.059329	4.275924
298.797797	6248.896153	15.371853	-0.059308	4.273281
298.941987	6240.855599	15.376858	-0.059330	4.270633
298.989514	6232.849975	15.381863	-0.059333	4.267995
298.861282	6224.850142	15.386867	-0.059304	4.265356
298.667851	6216.877862	15.391872	-0.059263	4.262724
298.916362	6208.875128	15.396877	-0.059304	4.260083
298.689744	6200.960924	15.401882	-0.059256	4.257466
298.763748	6192.883033	15.406887	-0.059265	4.254796
298.696441	6184.901797	15.411891	-0.059247	4.252156
298.779151	6176.836564	15.416896	-0.059257	4.249487
298.641648	6168.925707	15.421901	-0.059226	4.246865
298.257945	6160.824217	15.426906	-0.059149	4.244176
298.322409	6152.927157	15.431911	-0.059156	4.241558
298.412683	6144.909139	15.436915	-0.059168	4.238898
298.232862	6136.932965	15.441920	-0.059129	4.236248
298.229413	6128.903259	15.446925	-0.059123	4.233580
298.305649	6120.883830	15.451930	-0.059132	4.230914
298.408151	6112.875235	15.456935	-0.059145	4.228251
298.204777	6104.906863	15.461939	-0.059102	4.225596
298.363651	6096.885124	15.466944	-0.059126	4.222925
298.308834	6088.943098	15.471949	-0.059111	4.220278
297.969053	6080.957519	15.476954	-0.059042	4.217611
298.149083	6072.916619	15.481959	-0.059071	4.214929
298.162782	6064.927860	15.486963	-0.059068	4.212261
298.198746	6056.865034	15.491968	-0.059069	4.209567
298.043542	6048.951360	15.496973	-0.059035	4.206920
298.142861	6040.879115	15.501978	-0.059048	4.204220
297.912035	6032.947181	15.506983	-0.059000	4.201562
297.874856	6024.958426	15.511987	-0.058988	4.198885
298.045493	6016.944052	15.516992	-0.059014	4.196200
297.855611	6008.848454	15.521997	-0.058973	4.193482
297.774221	6000.804017	15.527002	-0.058953	4.190781
297.728019	5992.848237	15.532007	-0.058939	4.188108
297.908353	5984.825267	15.537011	-0.058967	4.185414
297.641993	5976.910954	15.542016	-0.058912	4.182749
297.596360	5968.889813	15.547021	-0.058898	4.180049
297.659994	5960.930541	15.552026	-0.058905	4.177370
297.454677	5952.903721	15.557031	-0.058861	4.174662
297.426226	5944.883737	15.562035	-0.058851	4.171958
297.425498	5936.862499	15.567040	-0.058845	4.169251
297.601093	5928.906193	15.572045	-0.058873	4.166567
297.162046	5920.883315	15.577050	-0.058786	4.163852
297.386186	5912.919971	15.582055	-0.058822	4.161162
297.453489	5904.922763	15.587059	-0.058829	4.158457
297.293840	5896.879522	15.592064	-0.058794	4.155733
297.481227	5888.877560	15.597069	-0.058824	4.153024
297.262669	5880.838675	15.602074	-0.058778	4.150297
297.322388	5872.845145	15.607079	-0.058784	4.147587
297.217177	5864.869971	15.612083	-0.058759	4.144879
297.156435	5856.899409	15.617088	-0.058742	4.142171
297.291674	5848.863769	15.622093	-0.058762	4.139442
296.920795	5840.870715	15.627098	-0.058687	4.136719
296.881792	5832.886768	15.632103	-0.058675	4.134001
296.975383	5824.856567	15.637107	-0.058687	4.131268
296.995981	5816.835214	15.642112	-0.058685	4.128535
297.012335	5808.866007	15.647117	-0.058683	4.125818
297.051147	5800.880190	15.652122	-0.058685	4.123094
296.963275	5792.868660	15.657127	-0.058663	4.120357
296.730771	5784.937279	15.662131	-0.058615	4.117645
296.775488	5776.895924	15.667136	-0.058618	4.114896
296.784398	5768.920569	15.672141	-0.058614	4.112168
296.630685	5760.865462	15.677146	-0.058580	4.109408
297.019274	5752.826306	15.682151	-0.058647	4.106659
296.803651	5744.884540	15.687155	-0.058602	4.103934
296.615408	5736.889779	15.692160	-0.058561	4.101189
296.551022	5728.912066	15.697165	-0.058544	4.098450
296.589872	5720.863049	15.702170	-0.058546	4.095686
296.624518	5712.855032	15.707175	-0.058547	4.092934
296.538477	5704.874339	15.712179	-0.058526	4.090188
296.614287	5696.871853	15.717184	-0.058535	4.087434
296.685761	5688.865845	15.722189	-0.058543	4.084678
296.393097	5680.943917	15.727194	-0.058483	4.081944
296.410467	5672.909223	15.732199	-0.058481	4.079173
296.538469	5664.957864	15.737203	-0.058499	4.076430
296.333602	5656.899555	15.742208	-0.058456	4.073645
296.316898	5648.914218	15.747213	-0.058447	4.070885
296.447210	5640.894059	15.752218	-0.058466	4.068113
296.329109	5632.874103	15.757223	-0.058439	4.065336
296.332096	5624.943953	15.762227	-0.058434	4.062590
296.222557	5616.910316	15.767232	-0.058408	4.059805
296.488015	5608.968462	15.772237	-0.058453	4.057054
296.316476	5600.924105	15.777242	-0.058415	4.054261
296.026393	5592.923568	15.782247	-0.058356	4.051478
296.080140	5584.922340	15.787251	-0.058361	4.048699
296.137130	5576.885169	15.792256	-0.058366	4.045905
296.018734	5568.934493	15.797261	-0.058339	4.043136
296.009421	5560.918362	15.802266	-0.058331	4.040345
295.942624	5552.955913	15.807271	-0.058314	4.037570
295.887588	5544.926866	15.812275	-0.058298	4.034769
295.700467	5536.813405	15.817280	-0.058258	4.031935
296.142533	5528.825114	15.822285	-0.058335	4.029153
295.887196	5520.875132	15.827290	-0.058282	4.026371
295.695962	5512.888689	15.832295	-0.058241	4.023576
295.551080	5504.900501	15.837299	-0.058209	4.020778
295.692243	5496.908916	15.842304	-0.058230	4.017982
295.519289	5488.917133	15.847309	-0.058192	4.015179
295.419269	5480.895729	15.852314	-0.058168	4.012365
295.643050	5472.832654	15.857319	-0.058205	4.009539
295.328722	5464.947709	15.862323	-0.058141	4.006766
295.325000	5456.883858	15.867328	-0.058135	4.003932
295.474861	5448.914643	15.872333	-0.058157	4.001132
295.367021	5440.897008	15.877338	-0.058132	3.998310
295.382143	5432.913166	15.882343	-0.058129	3.995498
295.447988	5424.890996	15.887347	-0.058136	3.992673
295.381422	5416.847822	15.892352	-0.058119	3.989835
295.290173	5408.895564	15.897357	-0.058096	3.987028
295.113197	5400.899896	15.902362	-0.058058	3.984202
295.213599	5392.914742	15.907367	-0.058071	3.981381
295.136792	5384.938195	15.912371	-0.058052	3.978559
294.969210	5376.916045	15.917376	-0.058015	3.975718
295.182335	5368.880893	15.922381	-0.058050	3.972876
295.059289	5360.866428	15.927386	-0.058021	3.970034
294.968780	5352.927499	15.932391	-0.057999	3.967217
294.904405	5344.939364	15.937395	-0.057982	3.964381
295.065569	5336.959363	15.942400	-0.058007	3.961549
294.910651	5328.964198	15.947405	-0.057972	3.958705
294.851605	5320.957939	15.952410	-0.057956	3.955857
294.909196	5312.921136	15.957415	-0.057962	3.952997
294.936759	5304.908241	15.962419	-0.057961	3.950144
295.003677	5296.908841	15.967424	-0.057968	3.947294
294.996288	5288.934591	15.972429	-0.057962	3.944449
294.977523	5280.984150	15.977434	-0.057953	3.941611
294.619790	5273.000288	15.982439	-0.057881	3.938753
294.547484	5264.980280	15.987443	-0.057862	3.935884
294.617788	5256.941603	15.992448	-0.057870	3.933010
294.626075	5248.949368	15.997453	-0.057866	3.930149
294.459334	5240.963903	16.002458	-0.057830	3.927285
294.533975	5232.966082	16.007463	-0.057838	3.924419
294.720456	5225.028443	16.012467	-0.057868	3.921575
294.411447	5216.986053	16.017472	-0.057805	3.918682
294.503746	5209.003113	16.022477	-0.057817	3.915815
294.455282	5200.960282	16.027482	-0.057803	3.912922
294.478035	5192.929310	16.032487	-0.057801	3.910033
294.496305	5185.004169	16.037491	-0.057800	3.907179
294.435447	5176.946883	16.042496	-0.057783	3.904274
294.530352	5169.005228	16.047501	-0.057795	3.901412
294.184550	5161.011058	16.052506	-0.057726	3.898521
294.243738	5152.989683	16.057511	-0.057731	3.895625
294.505643	5144.947202	16.062515	-0.057775	3.892723
294.270717	5136.914372	16.067520	-0.057726	3.889813
294.315689	5129.009935	16.072525	-0.057729	3.886952
294.344796	5120.967410	16.077530	-0.057729	3.884040
294.164168	5112.982553	16.082535	-0.057690	3.881141
294.094677	5105.033929	16.087539	-0.057672	3.878256
294.202152	5096.988921	16.092544	-0.057686	3.875338
294.166180	5088.790172	16.097549	-0.057674	3.872358
294.090099	5080.800761	16.102554	-0.057655	3.869451
294.164306	5072.874416	16.107559	-0.057663	3.866569
294.183338	5064.926111	16.112563	-0.057661	3.863674
293.977396	5056.950669	16.117568	-0.057618	3.860764
294.120663	5048.971597	16.122573	-0.057639	3.857857
294.110588	5040.971013	16.127578	-0.057632	3.854936
293.987499	5032.961385	16.132583	-0.057604	3.852008
293.852601	5024.957708	16.137587	-0.057573	3.849080
293.763181	5016.961923	16.142592	-0.057551	3.846153
293.818358	5009.008526	16.147597	-0.057556	3.843242
293.550640	5001.025559	16.152602	-0.057501	3.840312
293.669921	4993.035569	16.157607	-0.057518	3.837385
293.650973	4985.025407	16.162611	-0.057509	3.834445
293.354902	4977.014139	16.167616	-0.057449	3.831497
293.436965	4969.014025	16.172621	-0.057459	3.828558
293.484600	4960.999925	16.177626	-0.057462	3.825612
293.673254	4953.017838	16.182631	-0.057492	3.822678
293.453708	4945.051665	16.187635	-0.057446	3.819739
293.428192	4937.083943	16.192640	-0.057436	3.816801
293.552736	4929.050265	16.197645	-0.057454	3.813840
293.547969	4921.022665	16.202650	-0.057447	3.810876
293.335569	4913.065754	16.207655	-0.057402	3.807931
293.295828	4905.075489	16.212659	-0.057390	3.804975
293.223414	4897.108546	16.217664	-0.057371	3.802025
293.148190	4889.076368	16.222669	-0.057352	3.799049
292.977301	4881.108361	16.227674	-0.057314	3.796092
292.943567	4873.056090	16.232679	-0.057303	3.793104
292.952409	4865.010183	16.237683	-0.057299	3.790117
292.782371	4857.030821	16.242688	-0.057262	3.787149
293.019378	4849.051126	16.247693	-0.057301	3.784187
292.711276	4841.094289	16.252698	-0.057238	3.781219
292.788817	4833.076260	16.257703	-0.057247	3.778235
292.789046	4825.080920	16.262707	-0.057242	3.775255
292.661314	4817.087923	16.267712	-0.057213	3.772271
292.724107	4809.062171	16.272717	-0.057219	3.769276
292.889211	4801.056598	16.277722	-0.057245	3.766289
292.632463	4793.075549	16.282727	-0.057192	3.763299
292.601175	4785.118014	16.287731	-0.057181	3.760320
292.632768	4777.121274	16.292736	-0.057181	3.757326
292.702914	4769.097717	16.297741	-0.057189	3.754321
292.581263	4761.066625	16.302746	-0.057161	3.751306
292.488204	4753.085169	16.307751	-0.057138	3.748307
292.670349	4745.083891	16.312755	-0.057167	3.745306
292.633091	4737.110115	16.317760	-0.057155	3.742307
292.377772	4729.117422	16.322765	-0.057102	3.739293
292.318321	4721.122309	16.327770	-0.057085	3.736280
292.443073	4713.088958	16.332775	-0.057103	3.733256
292.317745	4705.105168	16.337779	-0.057075	3.730241
292.206987	4697.098038	16.342784	-0.057049	3.727215
292.245122	4689.118562	16.347789	-0.057050	3.724201
292.205670	4681.157909	16.352794	-0.057038	3.721190
292.200947	4673.147903	16.357799	-0.057032	3.718159
292.358193	4665.164537	16.362803	-0.057055	3.715139
292.163845	4657.094957	16.367808	-0.057014	3.712075
292.026961	4649.074489	16.372813	-0.056983	3.709029
292.135573	4641.094105	16.377818	-0.056998	3.706002
291.987358	4633.152474	16.382823	-0.056965	3.702980
292.054125	4625.128729	16.387827	-0.056972	3.699930
291.697351	4617.177767	16.392832	-0.056900	3.696895
291.772468	4609.186373	16.397837	-0.056909	3.693853
291.644363	4601.195238	16.402842	-0.056880	3.690803
291.768214	4593.172092	16.407847	-0.056898	3.687745
291.739129	4585.176282	16.412851	-0.056887	3.684690
291.722126	4577.216530	16.417856	-0.056879	3.681648
291.626960	4569.253065	16.422861	-0.056855	3.678599
291.736363	4561.226372	16.427866	-0.056871	3.675529
291.655319	4553.202784	16.432871	-0.056850	3.672452
291.519619	4545.203460	16.437875	-0.056820	3.669381
291.451048	4537.201508	16.442880	-0.056801	3.666308
291.676331	4529.218173	16.447885	-0.056838	3.663247
291.561887	4521.223801	16.452890	-0.056811	3.660171
291.444190	4513.238050	16.457895	-0.056784	3.657095
291.740422	4505.223635	16.462899	-0.056834	3.654017
291.533438	4497.208872	16.467904	-0.056790	3.650922
291.367815	4489.248332	16.472909	-0.056754	3.647847
291.259399	4481.208214	16.477914	-0.056728	3.644740
291.428112	4473.256898	16.482919	-0.056755	3.641672
291.320273	4465.299010	16.487923	-0.056729	3.638591
291.023182	4457.294893	16.492928	-0.056669	3.635485
291.212837	4449.251108	16.497933	-0.056699	3.632374
291.140287	4441.225933	16.502938	-0.056680	3.629261
291.067262	4433.216563	16.507943	-0.056661	3.626151
291.144931	4425.267038	16.512947	-0.056670	3.623065
291.118158	4417.239261	16.517952	-0.056660	3.619944
291.059375	4409.300084	16.522957	-0.056643	3.616853
290.776837	4401.284931	16.527962	-0.056585	3.613724
290.903473	4393.267136	16.532967	-0.056604	3.610603
290.814964	4385.295480	16.537971	-0.056582	3.607491
290.506206	4377.293652	16.542976	-0.056519	3.604358
290.599756	4369.350106	16.547981	-0.056531	3.601257
290.627917	4361.353409	16.552986	-0.056531	3.598130
290.472596	4353.353688	16.557991	-0.056497	3.594995
290.394654	4345.357054	16.562995	-0.056477	3.591859
290.435594	4337.324656	16.568000	-0.056479	3.588711
290.645953	4329.323628	16.573005	-0.056513	3.585577
290.413220	4321.390210	16.578010	-0.056465	3.582454
290.382635	4313.373730	16.583015	-0.056454	3.579301
290.517547	4305.416515	16.588019	-0.056473	3.576174
290.282803	4297.383857	16.593024	-0.056424	3.573003
290.348005	4289.350727	16.598029	-0.056431	3.569839
290.423791	4281.392732	16.603034	-0.056440	3.566701
290.266487	4273.383006	16.608039	-0.056405	3.563533
290.293005	4265.414284	16.613043	-0.056405	3.560385
290.318442	4257.425077	16.618048	-0.056404	3.557225
290.328385	4249.393671	16.623053	-0.056401	3.554045
290.185756	4241.308361	16.628058	-0.056369	3.550837
290.116154	4233.339056	16.633063	-0.056351	3.547673
290.248660	4225.350780	16.638067	-0.056370	3.544506
289.946104	4217.410843	16.643072	-0.056308	3.541342
289.999299	4209.432578	16.648077	-0.056313	3.538170
289.978749	4201.408212	16.653082	-0.056304	3.534975
289.794501	4193.424630	16.658087	-0.056264	3.531788
289.864122	4185.431461	16.663091	-0.056272	3.528603
289.724150	4177.380098	16.668096	-0.056240	3.525384
289.791665	4169.442203	16.673101	-0.056248	3.522215
289.790314	4161.441772	16.678106	-0.056242	3.519016
289.938373	4153.455902	16.683111	-0.056264	3.515824
289.977356	4145.473905	16.688115	-0.056266	3.512627
289.615388	4137.449839	16.693120	-0.056194	3.509398
289.861712	4129.465739	16.698125	-0.056234	3.506201
289.866636	4121.491158	16.703130	-0.056230	3.502998
289.609052	4113.494545	16.708135	-0.056176	3.499774
289.538728	4105.566863	16.713139	-0.056158	3.496582
289.469300	4097.517800	16.718144	-0.056140	3.493337
289.552887	4089.501456	16.723149	-0.056150	3.490107
289.395807	4081.570096	16.728154	-0.056116	3.486901
289.491117	4073.542880	16.733159	-0.056128	3.483661
289.539965	4065.571510	16.738163	-0.056132	3.480440
289.368939	4057.590138	16.743168	-0.056095	3.477204
289.416873	4049.558150	16.748173	-0.056098	3.473952
289.349561	4041.525864	16.753178	-0.056080	3.470693
289.456972	4033.544182	16.758183	-0.056095	3.467457
289.240693	4025.572629	16.763187	-0.056049	3.464212
289.248983	4017.564638	16.768192	-0.056046	3.460956
289.355853	4009.595401	16.773197	-0.056060	3.457716
289.235233	4001.598978	16.778202	-0.056032	3.454454
289.075591	3993.598764	16.783207	-0.055997	3.451187
289.328476	3985.603549	16.788211	-0.056039	3.447932
289.181262	3977.585454	16.793216	-0.056006	3.444651
289.132555	3969.679270	16.798221	-0.055992	3.441416
288.874170	3961.679395	16.803226	-0.055939	3.438133
288.716971	3953.654684	16.808231	-0.055904	3.434840
288.888905	3945.629172	16.813235	-0.055931	3.431555
288.690574	3937.634692	16.818240	-0.055888	3.428266
288.839741	3929.631662	16.823245	-0.055911	3.424983
288.763278	3921.669186	16.828250	-0.055891	3.421705
288.702308	3913.681270	16.833255	-0.055875	3.418415
288.758317	3905.699757	16.838259	-0.055880	3.415128
288.396590	3897.704472	16.843264	-0.055807	3.411817
288.585914	3889.688069	16.848269	-0.055837	3.408514
288.600556	3881.699153	16.853274	-0.055834	3.405213
288.562462	3873.717095	16.858279	-0.055822	3.401909
288.532292	3865.776815	16.863283	-0.055811	3.398620
288.504786	3857.741632	16.868288	-0.055801	3.395289
288.517803	3849.670340	16.873293	-0.055798	3.391940
288.549556	3841.680579	16.878298	-0.055798	3.388623
288.275032	3833.710923	16.883303	-0.055742	3.385301
288.375960	3825.762515	16.888307	-0.055755	3.381997
288.451953	3817.752773	16.893312	-0.055764	3.378663
288.286316	3809.781131	16.898317	-0.055728	3.375333
288.201859	3801.797078	16.903322	-0.055707	3.371998
288.111729	3793.809502	16.908327	-0.055685	3.368658
288.220688	3785.819608	16.913331	-0.055700	3.365320
288.137038	3777.836935	16.918336	-0.055679	3.361976
288.178857	3769.860422	16.923341	-0.055681	3.358635
288.197108	3761.843269	16.928346	-0.055680	3.355273
287.984514	3753.836947	16.933351	-0.055635	3.351904
288.060592	3745.862851	16.938355	-0.055643	3.348555
287.775713	3737.857483	16.943360	-0.055585	3.345177
287.764276	3729.894413	16.948365	-0.055578	3.341823
287.800700	3721.872268	16.953370	-0.055579	3.338442
287.723115	3713.885919	16.958375	-0.055559	3.335069
287.710312	3705.901294	16.963379	-0.055552	3.331696
287.658672	3697.882412	16.968384	-0.055537	3.328303
287.776091	3689.878284	16.973389	-0.055553	3.324919
287.610838	3681.961602	16.978394	-0.055517	3.321559
287.563563	3673.968314	16.983399	-0.055503	3.318167
287.588680	3665.973159	16.988403	-0.055502	3.314773
287.575795	3657.952103	16.993408	-0.055495	3.311364
287.663027	3649.942175	16.998413	-0.055506	3.307959
287.573751	3641.957610	17.003418	-0.055484	3.304555
287.590736	3633.987956	17.008423	-0.055482	3.301158
287.469405	3626.030075	17.013427	-0.055454	3.297757
287.409393	3618.007782	17.018432	-0.055437	3.294328
287.495991	3609.999703	17.023437	-0.055448	3.290906
287.266787	3602.023186	17.028442	-0.055400	3.287483
287.260312	3594.019747	17.033447	-0.055393	3.284053
287.381714	3586.067692	17.038451	-0.055411	3.280646
287.197085	3578.095567	17.043456	-0.055371	3.277215
287.094644	3570.092498	17.048461	-0.055347	3.273771
286.843204	3562.069383	17.053466	-0.055294	3.270308
286.949005	3554.091188	17.058471	-0.055309	3.266875
286.863341	3546.114917	17.063475	-0.055288	3.263432
286.637050	3538.099973	17.068480	-0.055240	3.259963
286.914169	3530.164532	17.073485	-0.055286	3.256544
286.780381	3522.150232	17.078490	-0.055256	3.253072
286.754321	3514.098628	17.083495	-0.055246	3.249583
286.808483	3506.158405	17.088499	-0.055251	3.246143
286.813841	3498.149846	17.093504	-0.055246	3.242667
286.861481	3490.171816	17.098509	-0.055250	3.239203
286.744653	3482.214686	17.103514	-0.055223	3.235737
286.655646	3474.153198	17.108519	-0.055201	3.232223
286.603528	3466.188714	17.113523	-0.055186	3.228749
286.504393	3458.176439	17.118528	-0.055162	3.225249
286.542143	3450.217256	17.123533	-0.055164	3.221773
286.601875	3442.212500	17.128538	-0.055170	3.218275
286.463088	3434.234352	17.133543	-0.055139	3.214777
286.434015	3426.257484	17.138547	-0.055128	3.211279
286.382466	3418.250195	17.143552	-0.055113	3.207764
286.235862	3410.274902	17.148557	-0.055080	3.204255
286.165893	3402.343033	17.153562	-0.055062	3.200764
286.178507	3394.334756	17.158567	-0.055059	3.197239
286.312954	3386.315938	17.163571	-0.055079	3.193711
286.275037	3378.298290	17.168576	-0.055066	3.190173
286.354150	3370.317953	17.173581	-0.055076	3.186651
286.286755	3362.361826	17.178586	-0.055058	3.183131
285.971661	3354.388932	17.183591	-0.054994	3.179588
286.020127	3346.421856	17.188595	-0.054998	3.176060
286.035054	3338.366263	17.193600	-0.054995	3.172486
286.044601	3330.388407	17.198605	-0.054992	3.168944
285.837541	3322.395486	17.203610	-0.054948	3.165381
286.028511	3314.425010	17.208615	-0.054978	3.161841
286.135557	3306.450504	17.213619	-0.054993	3.158292
285.890591	3298.471565	17.218624	-0.054942	3.154722
285.751601	3290.461424	17.223629	-0.054910	3.151138
285.824493	3282.454447	17.228634	-0.054919	3.147561
285.699044	3274.482902	17.233639	-0.054890	3.143987
285.923340	3266.482047	17.238643	-0.054926	3.140411
285.819328	3258.523814	17.243648	-0.054902	3.136835
285.582505	3250.538452	17.248653	-0.054852	3.133238
285.461306	3242.557927	17.253658	-0.054825	3.129643
285.544369	3234.541518	17.258663	-0.054835	3.126038
285.790832	3226.592222	17.263667	-0.054875	3.122466
285.582946	3218.580779	17.268672	-0.054831	3.118841
285.730382	3210.608386	17.273677	-0.054853	3.115246
285.649922	3202.605029	17.278682	-0.054833	3.111622
285.504313	3194.629937	17.283687	-0.054801	3.108004
285.503446	3186.625661	17.288691	-0.054795	3.104375
285.498501	3178.656591	17.293696	-0.054789	3.100757
285.411179	3170.705086	17.298701	-0.054767	3.097140
285.169438	3162.710539	17.303706	-0.054717	3.093492
285.180957	3154.678135	17.308711	-0.054714	3.089833
285.382573	3146.712694	17.313715	-0.054746	3.086210
285.026998	3138.726028	17.318720	-0.054675	3.082547
284.933549	3130.781197	17.323725	-0.054652	3.078911
285.077117	3122.791081	17.328730	-0.054673	3.075260
285.016769	3114.677899	17.333735	-0.054657	3.071540
284.877268	3106.724101	17.338739	-0.054625	3.067884
284.745941	3098.732830	17.343744	-0.054596	3.064208
284.914997	3090.788364	17.348749	-0.054622	3.060562
284.766249	3082.826869	17.353754	-0.054589	3.056889
284.797225	3074.811910	17.358759	-0.054589	3.053196
284.930158	3066.813732	17.363763	-0.054609	3.049511
284.613392	3058.854588	17.368768	-0.054544	3.045818
284.623591	3050.877596	17.373773	-0.054541	3.042127
284.727594	3042.903951	17.378778	-0.054555	3.038439
284.457031	3034.940384	17.383783	-0.054499	3.034732
284.563430	3026.926073	17.388787	-0.054514	3.031016
284.582603	3018.929935	17.393792	-0.054512	3.027299
284.701800	3010.949279	17.398797	-0.054529	3.023590
284.744468	3002.969606	17.403802	-0.054532	3.019873
284.595082	2994.995743	17.408807	-0.054498	3.016145
284.738291	2986.995836	17.413811	-0.054520	3.012414
284.372883	2979.019110	17.418816	-0.054446	3.008664
284.367804	2971.035963	17.423821	-0.054440	3.004925
284.388647	2963.086639	17.428826	-0.054439	3.001198
284.272686	2955.099154	17.433831	-0.054412	2.997441
284.512816	2947.095392	17.438835	-0.054451	2.993690
284.146461	2939.074951	17.443840	-0.054378	2.989896
284.091551	2931.114589	17.448845	-0.054362	2.986142
284.111289	2923.144438	17.453850	-0.054361	2.982381
284.096528	2915.150368	17.458855	-0.054353	2.978603
284.190512	2907.157490	17.463859	-0.054365	2.974826
283.974344	2899.161753	17.468864	-0.054319	2.971027
284.081341	2891.193728	17.473869	-0.054334	2.967253
284.029864	2883.233073	17.478874	-0.054319	2.963469
283.929833	2875.230094	17.483879	-0.054295	2.959658
283.795644	2867.323056	17.488883	-0.054265	2.955886
283.626607	2859.289903	17.493888	-0.054228	2.952047
283.629992	2851.298334	17.498893	-0.054223	2.948232
283.766604	2843.289642	17.503898	-0.054243	2.944411
283.496282	2835.332123	17.508903	-0.054188	2.940588
283.588352	2827.369834	17.513907	-0.054199	2.936777
283.495522	2819.352779	17.518912	-0.054177	2.932924
283.486543	2811.368335	17.523917	-0.054170	2.929087
283.554248	2803.391177	17.528922	-0.054177	2.925252
283.487405	2795.434625	17.533927	-0.054159	2.921416
283.363725	2787.488969	17.538931	-0.054131	2.917576
283.233869	2779.451824	17.543936	-0.054102	2.913686
283.251881	2771.390521	17.548941	-0.054100	2.909788
283.306267	2763.431339	17.553946	-0.054104	2.905936
283.112173	2755.483720	17.558951	-0.054063	2.902071
283.151002	2747.522980	17.563955	-0.054065	2.898207
283.046443	2739.541236	17.568960	-0.054040	2.894319
283.003535	2731.549979	17.573965	-0.054027	2.890426
282.868429	2723.590634	17.578970	-0.053996	2.886537
282.777066	2715.603355	17.583975	-0.053974	2.882632
282.859862	2707.656028	17.588979	-0.053984	2.878751
282.590866	2699.671360	17.593984	-0.053929	2.874827
282.787662	2691.645635	17.598989	-0.053960	2.870903
282.905482	2683.661868	17.603994	-0.053977	2.866990
282.890885	2675.665726	17.608999	-0.053969	2.863058
282.972497	2667.712219	17.614003	-0.053979	2.859147
282.891579	2659.749884	17.619008	-0.053958	2.855217
282.656380	2651.772355	17.624013	-0.053909	2.851266
282.583377	2643.816711	17.629018	-0.053890	2.847329
282.425650	2635.838216	17.634023	-0.053856	2.843371
282.415484	2627.878727	17.639027	-0.053848	2.839425
282.201223	2619.914528	17.644032	-0.053803	2.835459
282.312485	2611.873083	17.649037	-0.053819	2.831468
282.182597	2603.882310	17.654042	-0.053789	2.827483
282.065221	2595.917091	17.659047	-0.053762	2.823505
281.998426	2587.961750	17.664051	-0.053744	2.819530
282.167124	2579.962602	17.669056	-0.053770	2.815541
282.116737	2571.974914	17.674061	-0.053756	2.811539
282.002968	2563.997199	17.679066	-0.053729	2.807533
281.922828	2556.029547	17.684071	-0.053709	2.803528
282.103731	2548.046318	17.689075	-0.053737	2.799524
281.908531	2540.100511	17.694080	-0.053696	2.795512
281.871413	2532.086670	17.699085	-0.053683	2.791469
281.970167	2524.093423	17.704090	-0.053696	2.787439
281.990035	2516.108503	17.709095	-0.053695	2.783402
281.986862	2508.164324	17.714099	-0.053689	2.779379
281.873952	2500.195837	17.719104	-0.053663	2.775331
282.032105	2492.192666	17.724109	-0.053687	2.771275
281.613465	2484.275283	17.729114	-0.053603	2.767223
281.650415	2476.267398	17.734119	-0.053605	2.763146
281.709489	2468.308466	17.739123	-0.053611	2.759089
281.484325	2460.345740	17.744128	-0.053563	2.755008
281.563635	2452.271320	17.749133	-0.053573	2.750881
281.687319	2444.296279	17.754138	-0.053591	2.746802
281.353860	2436.338341	17.759143	-0.053523	2.742698
281.451456	2428.391311	17.764147	-0.053536	2.738619
281.566213	2420.384333	17.769152	-0.053552	2.734505
281.605554	2412.397075	17.774157	-0.053554	2.730390
281.411779	2404.455573	17.779162	-0.053513	2.726278
281.402424	2396.496371	17.784167	-0.053506	2.722162
281.347280	2388.543223	17.789171	-0.053490	2.718040
281.274045	2380.571245	17.794176	-0.053471	2.713900
281.322736	2372.547643	17.799181	-0.053475	2.709736
281.378884	2364.593621	17.804186	-0.053480	2.705601
281.184576	2356.624887	17.809191	-0.053439	2.701437
281.317916	2348.660268	17.814195	-0.053458	2.697289
281.231845	2340.688267	17.819200	-0.053437	2.693117
281.095356	2332.704945	17.824205	-0.053406	2.688930
281.038573	2324.748314	17.829210	-0.053390	2.684755
281.068369	2316.771045	17.834215	-0.053390	2.680568
281.184388	2308.807640	17.839219	-0.053407	2.676387
280.939128	2300.822852	17.844224	-0.053356	2.672165
280.836751	2292.838783	17.849229	-0.053331	2.667947
280.955992	2284.852826	17.854234	-0.053348	2.663734
280.773310	2276.878508	17.859239	-0.053309	2.659502
280.565817	2268.964152	17.864243	-0.053265	2.655294
280.642062	2260.919659	17.869248	-0.053274	2.651027
280.683090	2252.966879	17.874253	-0.053276	2.646801
280.442908	2245.028471	17.879258	-0.053226	2.642557
280.620740	2237.031719	17.884263	-0.053254	2.638302
280.617209	2229.077664	17.889267	-0.053248	2.634051
280.371852	2221.075913	17.894272	-0.053197	2.629752
280.311893	2213.128508	17.899277	-0.053181	2.625488
280.274625	2205.172653	17.904282	-0.053168	2.621213
280.197302	2197.193576	17.909287	-0.053149	2.616916
280.402505	2189.198690	17.914291	-0.053182	2.612623
280.194880	2181.239771	17.919296	-0.053138	2.608314
280.222162	2173.269807	17.924301	-0.053137	2.604008
280.287807	2165.312260	17.929306	-0.053144	2.599704
280.079085	2157.367572	17.934311	-0.053100	2.595381
280.191708	2149.206587	17.939315	-0.053116	2.590955
279.910236	2141.260997	17.944320	-0.053058	2.586612
279.901417	2133.328214	17.949325	-0.053051	2.582288
280.084006	2125.372121	17.954330	-0.053080	2.577956
279.955065	2117.417697	17.959335	-0.053050	2.573597
279.888580	2109.456146	17.964339	-0.053033	2.569231
279.965241	2101.472489	17.969344	-0.053042	2.564855
279.771180	2093.575476	17.974349	-0.053000	2.560500
279.662581	2085.625114	17.979354	-0.052975	2.556115
279.707742	2077.621755	17.984359	-0.052978	2.551703
279.645620	2069.655980	17.989363	-0.052961	2.547297
279.517837	2061.692641	17.994368	-0.052932	2.542880
279.611810	2053.718078	17.999373	-0.052944	2.538465
279.512881	2045.781918	18.004378	-0.052920	2.534050
279.493544	2037.777727	18.009383	-0.052912	2.529595
279.539623	2029.826565	18.014387	-0.052915	2.525166
279.512618	2021.872702	18.019392	-0.052905	2.520723
279.424975	2013.930613	18.024397	-0.052883	2.516274
279.220852	2005.951616	18.029402	-0.052840	2.511788
279.089099	1997.954902	18.034407	-0.052810	2.507290
279.173070	1990.008609	18.039411	-0.052820	2.502827
279.181206	1982.036941	18.044416	-0.052816	2.498337
278.993640	1974.095762	18.049421	-0.052776	2.493841
279.144045	1966.083352	18.054426	-0.052799	2.489321
279.132278	1958.117148	18.059431	-0.052791	2.484808
278.961273	1950.204774	18.064435	-0.052754	2.480305
278.917082	1942.250882	18.069440	-0.052741	2.475780
278.928727	1934.249793	18.074445	-0.052737	2.471224
278.948649	1926.279314	18.079450	-0.052736	2.466677
278.834195	1918.332597	18.084455	-0.052709	2.462126
278.951937	1910.378450	18.089459	-0.052726	2.457579
278.808593	1902.414691	18.094464	-0.052694	2.452999
278.600120	1894.458425	18.099469	-0.052650	2.448409
278.653524	1886.495265	18.104474	-0.052654	2.443827
278.640861	1878.530554	18.109479	-0.052647	2.439230
278.603008	1870.592269	18.114483	-0.052634	2.434638
278.437348	1862.545019	18.119488	-0.052598	2.429964
278.566953	1854.569475	18.124493	-0.052617	2.425346
278.428905	1846.657316	18.129498	-0.052586	2.420735
278.348686	1838.704731	18.134503	-0.052566	2.416096
278.483717	1830.721270	18.139507	-0.052586	2.411447
278.327455	1822.773148	18.144512	-0.052551	2.406786
278.240691	1814.841911	18.149517	-0.052530	2.402132
278.167349	1806.908099	18.154522	-0.052511	2.397469
278.329627	1798.887004	18.159527	-0.052536	2.392763
278.342456	1790.929328	18.164531	-0.052533	2.388074
277.967302	1783.012781	18.169536	-0.052458	2.383370
278.079674	1775.050977	18.174541	-0.052473	2.378667
278.179450	1767.087324	18.179546	-0.052487	2.373954
277.990521	1759.116267	18.184551	-0.052446	2.369203
277.832192	1751.197536	18.189555	-0.052411	2.364477
277.823563	1743.232984	18.194560	-0.052405	2.359726
277.866728	1735.298351	18.199565	-0.052407	2.354987
277.696997	1727.306354	18.204570	-0.052370	2.350187
277.800532	1719.309387	18.209575	-0.052384	2.345396
277.685261	1711.393869	18.214579	-0.052358	2.340627
277.727852	1703.428607	18.219584	-0.052360	2.335831
277.667563	1695.470923	18.224589	-0.052344	2.331022
277.532783	1687.538030	18.229594	-0.052313	2.326211
277.218255	1679.612954	18.234599	-0.052250	2.321380
277.287099	1671.677131	18.239603	-0.052257	2.316564
277.357146	1663.659494	18.244608	-0.052265	2.311688
277.298151	1655.713695	18.249613	-0.052248	2.306835
277.183599	1647.779763	18.254618	-0.052222	2.301975
277.220290	1639.816186	18.259623	-0.052223	2.297099
277.252638	1631.873380	18.264627	-0.052224	2.292224
277.309269	1623.878963	18.269632	-0.052229	2.287310
277.247935	1615.950055	18.274637	-0.052213	2.282416
277.263058	1608.018292	18.279642	-0.052210	2.277515
277.167350	1600.022718	18.284647	-0.052187	2.272555
277.123669	1592.050263	18.289651	-0.052174	2.267603
277.000198	1584.112318	18.294656	-0.052145	2.262655
276.839892	1576.196924	18.299661	-0.052110	2.257707
276.831783	1568.241132	18.304666	-0.052103	2.252736
276.696034	1560.285799	18.309671	-0.052073	2.247743
276.799927	1552.336184	18.314675	-0.052087	2.242763
276.522710	1544.424864	18.319680	-0.052030	2.237763
276.612385	1536.450433	18.324685	-0.052041	2.232744
276.754061	1528.476950	18.329690	-0.052062	2.227719
276.469630	1520.560881	18.334695	-0.052004	2.222682
276.461659	1512.632983	18.339699	-0.051997	2.217650
276.426428	1504.671502	18.344704	-0.051986	2.212582
276.499358	1496.705953	18.349709	-0.051994	2.207511
276.317517	1488.790648	18.354714	-0.051955	2.202436
276.331245	1480.838102	18.359719	-0.051952	2.197344
276.354220	1472.893672	18.364723	-0.051951	2.192246
276.256565	1464.922731	18.369728	-0.051928	2.187108
276.126676	1456.999799	18.374733	-0.051898	2.181986
276.149380	1449.072690	18.379738	-0.051897	2.176863
276.344107	1441.069510	18.384743	-0.051928	2.171694
276.384122	1433.136762	18.389747	-0.051930	2.166545
276.175527	1425.230232	18.394752	-0.051886	2.161378
276.018747	1417.325559	18.399757	-0.051852	2.156204
275.932983	1409.378098	18.404762	-0.051830	2.150996
276.004058	1401.396114	18.409767	-0.051838	2.145767
276.151565	1393.455766	18.414771	-0.051860	2.140561
275.907526	1385.548665	18.419776	-0.051810	2.135326
275.761717	1377.615619	18.424781	-0.051777	2.130071
275.771069	1369.671214	18.429786	-0.051774	2.124810
275.675333	1361.750791	18.434791	-0.051751	2.119542
275.547218	1353.837449	18.439795	-0.051722	2.114263
275.522768	1345.812161	18.444800	-0.051712	2.108905
275.618212	1337.858677	18.449805	-0.051724	2.103593
275.623495	1329.961490	18.454810	-0.051720	2.098297
275.399630	1322.031646	18.459815	-0.051673	2.092944
275.482578	1314.085566	18.464819	-0.051683	2.087595
275.421773	1306.155287	18.469824	-0.051666	2.082230
275.315654	1298.252529	18.474829	-0.051641	2.076864
275.523854	1290.277171	18.479834	-0.051675	2.071467
275.196563	1282.368291	18.484839	-0.051609	2.066047
275.080247	1274.467140	18.489843	-0.051582	2.060640
275.095362	1266.530227	18.494848	-0.051579	2.055207
275.006360	1258.594552	18.499853	-0.051557	2.049750
275.120014	1250.648062	18.504858	-0.051573	2.044291
274.764871	1242.777543	18.509863	-0.051502	2.038823
274.899706	1234.827494	18.514867	-0.051522	2.033334
274.952992	1226.845644	18.519872	-0.051526	2.027801
274.805702	1218.946681	18.524877	-0.051494	2.022289
274.976467	1211.007858	18.529882	-0.051520	2.016767
274.864259	1203.070739	18.534887	-0.051494	2.011202
274.770875	1195.159530	18.539891	-0.051471	2.005642
274.655744	1187.256693	18.544896	-0.051445	2.000070
274.649737	1179.343840	18.549901	-0.051438	1.994487
274.510312	1171.413243	18.554906	-0.051407	1.988861
274.282843	1163.502673	18.559911	-0.051359	1.983224
274.460395	1155.571052	18.564915	-0.051387	1.977599
274.257454	1147.658737	18.569920	-0.051344	1.971932
274.195069	1139.738292	18.574925	-0.051327	1.966257
274.161020	1131.835627	18.579930	-0.051316	1.960581
274.124235	1123.914026	18.584935	-0.051304	1.954875
274.093572	1115.942305	18.589939	-0.051293	1.949117
274.134859	1108.005506	18.594944	-0.051295	1.943375
274.145666	1100.094322	18.599949	-0.051292	1.937631
274.004366	1092.197995	18.604954	-0.051260	1.931864
273.970328	1084.262227	18.609959	-0.051248	1.926063
274.141856	1076.345294	18.614963	-0.051275	1.920281
274.050094	1068.457246	18.619968	-0.051253	1.914473
273.947984	1060.531739	18.624973	-0.051229	1.908619
273.766788	1052.649115	18.629978	-0.051190	1.902770
273.818529	1044.726731	18.634983	-0.051194	1.896900
273.693896	1036.836519	18.639987	-0.051165	1.891015
273.650086	1028.908534	18.644992	-0.051152	1.885092
273.752405	1021.004450	18.649997	-0.051166	1.879186
273.547273	1013.126724	18.655002	-0.051122	1.873246
273.338658	1005.203506	18.660007	-0.051078	1.867252
273.388503	997.291737	18.665011	-0.051082	1.861277
273.321038	989.392826	18.670016	-0.051064	1.855279
273.270359	981.473892	18.675021	-0.051050	1.849248
273.103027	973.604816	18.680026	-0.051013	1.843222
273.135146	965.689842	18.685031	-0.051014	1.837164
273.117239	957.778986	18.690035	-0.051005	1.831084
273.043170	949.880590	18.695040	-0.050986	1.824986
272.957172	942.000182	18.700045	-0.050965	1.818880
272.929089	934.099582	18.705050	-0.050955	1.812745
272.834615	926.193148	18.710055	-0.050932	1.806577
272.868326	918.309881	18.715059	-0.050933	1.800421
273.098576	910.381914	18.720064	-0.050970	1.794233
272.754228	902.488770	18.725069	-0.050901	1.787980
272.613610	894.614565	18.730074	-0.050870	1.781746
272.652888	886.705223	18.735079	-0.050872	1.775484
272.894821	878.777651	18.740083	-0.050911	1.769210
272.682140	870.923598	18.745088	-0.050867	1.762916
272.675720	863.054075	18.750093	-0.050860	1.756613
272.840114	855.124220	18.755098	-0.050886	1.750260
272.624938	847.271902	18.760103	-0.050840	1.743899
272.614996	839.412970	18.765107	-0.050833	1.737535
272.562310	831.513369	18.770112	-0.050818	1.731109
272.463941	823.649125	18.775117	-0.050795	1.724683
272.372880	815.800528	18.780122	-0.050772	1.718245
272.106916	807.930032	18.785127	-0.050718	1.711743
272.096242	800.033172	18.790131	-0.050710	1.705228
271.925991	792.182218	18.795136	-0.050673	1.698705
271.993804	784.278945	18.800141	-0.050681	1.692144
272.049164	776.393233	18.805146	-0.050686	1.685571
271.792733	768.561132	18.810151	-0.050633	1.678975
271.801200	760.689853	18.815155	-0.050629	1.672356
271.829920	752.787967	18.820160	-0.050629	1.665688
271.831168	744.928066	18.825165	-0.050624	1.659024
271.836034	737.067626	18.830170	-0.050620	1.652334
271.664882	729.204475	18.835175	-0.050583	1.645590
271.732598	721.366431	18.840179	-0.050590	1.638873
271.649938	713.482625	18.845184	-0.050570	1.632068
271.441350	705.604149	18.850189	-0.050526	1.625221
271.522347	697.751571	18.855194	-0.050535	1.618408
271.450486	689.888749	18.860199	-0.050517	1.611536
271.512513	682.036746	18.865203	-0.050523	1.604664
271.267893	674.228394	18.870208	-0.050472	1.597756
271.189254	666.370923	18.875213	-0.050452	1.590799
271.263089	658.513815	18.880218	-0.050461	1.583833
271.309724	650.658128	18.885223	-0.050464	1.576834
271.393194	642.802386	18.890227	-0.050475	1.569809
271.138341	635.006187	18.895232	-0.050422	1.562756
270.801519	627.223149	18.900237	-0.050354	1.555672
270.930028	619.336351	18.905242	-0.050373	1.548529
270.972855	611.475878	18.910247	-0.050376	1.541364
270.730001	603.694287	18.915251	-0.050325	1.534196
270.705734	595.841344	18.920256	-0.050315	1.526961
270.785317	588.003614	18.925261	-0.050325	1.519722
270.661542	580.204852	18.930266	-0.050297	1.512453
270.524777	572.375073	18.935271	-0.050266	1.505118
270.444332	564.576987	18.940275	-0.050246	1.497786
270.427334	556.743165	18.945280	-0.050238	1.490393
270.413216	548.932224	18.950285	-0.050230	1.482986
270.499110	541.117531	18.955290	-0.050241	1.475553
270.194534	533.290942	18.960295	-0.050179	1.468010
270.182949	525.482127	18.965299	-0.050171	1.460492
270.382498	517.650719	18.970304	-0.050203	1.452946
270.143873	509.873657	18.975309	-0.050154	1.445344
270.023762	502.121036	18.980314	-0.050126	1.437745
269.931230	494.303212	18.985319	-0.050104	1.430045
270.166137	486.482077	18.990323	-0.050142	1.422354
269.890233	478.741861	18.995328	-0.050086	1.414618
269.905615	470.930875	19.000333	-0.050083	1.406816
269.852632	463.175800	19.005338	-0.050068	1.399016
269.764018	455.383861	19.010343	-0.050047	1.391129
269.764205	447.602663	19.015347	-0.050041	1.383222
269.827100	439.817013	19.020352	-0.050048	1.375277
269.885509	432.025858	19.025357	-0.050054	1.367278
269.676042	424.316144	19.030362	-0.050010	1.359271
269.457464	416.574961	19.035367	-0.049964	1.351182
269.328115	408.827014	19.040371	-0.049934	1.343053
269.199761	401.101453	19.045376	-0.049905	1.334898
269.286049	393.316452	19.050381	-0.049916	1.326667
269.135086	385.613557	19.055386	-0.049883	1.318431
268.912767	377.795924	19.060391	-0.049836	1.310006
268.825711	370.037946	19.065395	-0.049815	1.301616
268.811746	362.303123	19.070400	-0.049807	1.293211
268.814705	354.568143	19.075405	-0.049803	1.284753
268.733126	346.877183	19.080410	-0.049782	1.276272
268.684105	339.150439	19.085415	-0.049768	1.267700
268.916182	331.411844	19.090419	-0.049806	1.259110
268.589219	323.760990	19.095424	-0.049740	1.250453
268.565506	316.056608	19.100429	-0.049731	1.241734
268.530863	308.383801	19.105434	-0.049719	1.232987
268.380256	300.683837	19.110439	-0.049686	1.224123
268.434409	293.000662	19.115443	-0.049691	1.215254
268.247392	285.336798	19.120448	-0.049651	1.206295
268.027285	277.710529	19.125453	-0.049605	1.197306
268.072523	270.029478	19.130458	-0.049608	1.188238
267.969071	262.374992	19.135463	-0.049584	1.179102
268.124612	254.699140	19.140467	-0.049608	1.169921
267.937509	247.082029	19.145472	-0.049568	1.160669
267.830546	239.442846	19.150477	-0.049543	1.151331
267.990524	231.764315	19.155482	-0.049567	1.141925
267.916663	224.151042	19.160487	-0.049549	1.132473
267.812621	216.560239	19.165491	-0.049524	1.122962
267.682268	208.979421	19.170496	-0.049495	1.113377
267.595028	201.378742	19.175501	-0.049474	1.103693
267.722998	193.780915	19.180506	-0.049492	1.093974
267.335437	186.250337	19.185511	-0.049415	1.084141
267.444212	178.672386	19.190515	-0.049430	1.074267
267.082372	171.150945	19.195520	-0.049358	1.064269
267.008543	163.603402	19.200525	-0.049339	1.054208
267.104187	156.041883	19.205530	-0.049352	1.044070
266.903336	148.542927	19.210535	-0.049310	1.033848
266.856944	141.023308	19.215539	-0.049296	1.023533
266.728768	133.538768	19.220544	-0.049267	1.013141
266.684524	126.041789	19.225549	-0.049254	1.002645
266.568295	118.572184	19.230554	-0.049227	0.992059
266.378548	111.096916	19.235559	-0.049187	0.981332
266.451437	103.629600	19.240563	-0.049196	0.970564
266.311123	96.207347	19.245568	-0.049164	0.959687
266.242732	88.782756	19.250573	-0.049147	0.948701
266.308522	81.367860	19.255578	-0.049154	0.937635
266.143855	73.987270	19.260583	-0.049118	0.926429
266.065627	66.633612	19.265587	-0.049099	0.915149
265.921284	59.509318	19.270592	-0.049067	0.904069