Number of Data Points = 30
        
File	hc(nm)	Pmax(N)	S(N/nm)	A(nm^2)	hmax(nm)	heff(nm)	Er(GPa)	H(GPa)	A	hf(nm)	m	X(mm)	Y(mm)	Drift(nm/s)
KGT3461_Position 6_00000 LC.hys	186.352427	7999.345128	195.569521	2135167.198090	217.286948	217.029542	118.582351	3.746472	60.606281	166.193071	1.242860	-128.664993	-57.460498	0.845302
KGT3461_Position 6_00001 LC.hys	216.181648	7999.335048	189.506428	2944021.355574	248.013131	247.840211	97.856189	2.717146	54.236742	194.766179	1.257338	-128.657997	-57.460498	0.370209
KGT3461_Position 6_00002 LC.hys	239.228699	7999.537519	191.102703	3649288.803715	270.707161	270.623615	88.633427	2.192081	57.716654	218.427524	1.246924	-128.650993	-57.460498	0.276946
KGT3461_Position 6_00003 LC.hys	215.663917	7999.185504	202.991019	2928966.240246	245.307858	245.218865	105.088325	2.731061	73.942604	197.474547	1.211582	-128.643493	-57.460498	0.169288
KGT3461_Position 6_00004 LC.hys	204.957960	7999.414096	211.826411	2625589.843466	233.600085	233.280965	115.824783	3.046711	79.372515	187.677543	1.207590	-128.636993	-57.460498	0.166233
KGT3461_Position 6_00005 LC.hys	186.624855	7999.512054	199.766232	2142004.078776	216.583293	216.658129	120.933538	3.734592	96.520243	170.497935	1.152726	-128.629997	-57.459999	0.181617
KGT3461_Position 6_00006 LC.hys	211.841768	7999.302011	205.344409	2818913.117213	241.091230	241.058421	108.361964	2.837726	64.608251	192.668691	1.242178	-128.664993	-57.453499	0.212232
KGT3461_Position 6_00007 LC.hys	224.588991	7999.248381	200.459023	3193392.754052	254.911560	254.517483	99.388073	2.504937	46.928756	202.601456	1.301002	-128.657997	-57.453499	0.187316
KGT3461_Position 6_00008 LC.hys	221.088674	7999.284005	205.681786	3088453.168217	250.423935	250.257339	103.695558	2.590062	61.921917	201.592477	1.251296	-128.650993	-57.453499	0.210648
KGT3461_Position 6_00009 LC.hys	211.187040	7999.663196	204.999746	2800254.688715	240.664924	240.454137	108.539892	2.856763	67.451659	192.342237	1.232918	-128.643997	-57.453499	0.260726
KGT3461_Position 6_00010 LC.hys	212.103648	7999.704681	211.577530	2826392.053800	240.613753	240.461000	111.503415	2.830359	75.925349	194.465510	1.216496	-128.636993	-57.453499	0.249663
KGT3461_Position 6_00011 LC.hys	226.617429	7999.287512	190.575558	3254929.131602	258.260673	258.098201	93.590390	2.457592	63.222675	206.561147	1.227822	-128.629493	-57.453499	0.263920
KGT3461_Position 6_00012 LC.hys	218.374017	7999.186083	199.587255	3008162.458443	248.504792	248.432998	101.956986	2.659160	86.262128	201.311908	1.175716	-128.664993	-57.446499	0.303255
KGT3461_Position 6_00013 LC.hys	216.476518	7999.314426	197.139439	2952611.606149	246.995558	246.909220	101.649485	2.709234	59.579327	196.254997	1.248350	-128.657997	-57.446499	0.289102
KGT3461_Position 6_00014 LC.hys	232.429113	7999.295550	201.177553	3434155.692825	262.425646	262.250888	96.184338	2.329334	77.973212	214.597740	1.198448	-128.650993	-57.446499	0.338037
KGT3461_Position 6_00015 LC.hys	211.898243	7999.637778	206.193302	2820525.200479	241.176364	240.995833	108.778832	2.836223	69.054457	193.292741	1.229563	-128.643493	-57.446499	0.249521
KGT3461_Position 6_00016 LC.hys	193.261007	7999.539772	217.100502	2311729.985657	221.175477	220.896386	126.510655	3.460413	54.019321	173.238018	1.293406	-128.636993	-57.446499	0.289942
KGT3461_Position 6_00017 LC.hys	219.198629	7999.716532	203.754419	3032450.307674	248.731154	248.644800	103.668071	2.638037	51.047717	198.066794	1.288232	-128.629493	-57.446499	0.285955
KGT3461_Position 6_00018 LC.hys	222.354560	7999.697965	218.024987	3126221.418578	250.299289	249.873303	109.252461	2.558903	55.162159	202.532721	1.290227	-128.664993	-57.439499	0.299355
KGT3461_Position 6_00019 LC.hys	221.880398	7999.728956	215.210851	3112050.235890	249.848412	249.759088	108.087555	2.570565	55.517055	201.976238	1.285467	-128.657997	-57.439499	0.260378
KGT3461_Position 6_00020 LC.hys	219.424135	7999.662785	216.999484	3039107.704040	247.351412	247.072804	110.286025	2.632241	73.846769	201.777956	1.228672	-128.650993	-57.439499	0.239865
KGT3461_Position 6_00021 LC.hys	214.501490	7999.583004	208.015114	2895292.268826	243.640099	243.344045	108.313731	2.762962	49.413099	193.338842	1.300298	-128.643493	-57.439499	0.274417
KGT3461_Position 6_00022 LC.hys	220.171925	7999.662698	209.514757	3061231.441439	249.004838	248.808318	106.096575	2.613217	47.104463	198.715796	1.311946	-128.636993	-57.439499	0.261828
KGT3461_Position 6_00023 LC.hys	220.581918	7999.778890	209.433475	3073392.187061	249.372991	249.229842	105.845387	2.602915	72.266360	202.471160	1.224138	-128.629493	-57.439499	0.225130
KGT3461_Position 6_00024 LC.hys	226.803704	7999.177881	210.295728	3260606.625533	255.476804	255.332022	103.184883	2.453279	63.160367	207.673255	1.252933	-128.664993	-57.432499	0.266948
KGT3461_Position 6_00025 LC.hys	230.585908	7999.139969	216.293964	3376846.380938	258.593844	258.322951	104.285415	2.368820	52.472796	210.305112	1.298386	-128.657997	-57.432499	0.225289
KGT3461_Position 6_00026 LC.hys	230.015633	7999.202616	209.506137	3359202.882720	258.818721	258.651557	101.277614	2.381280	58.006862	210.183236	1.269428	-128.650993	-57.432499	0.238424
KGT3461_Position 6_00027 LC.hys	217.167725	7999.599558	212.057216	2972792.721634	245.734592	245.460559	108.969653	2.690938	53.950323	196.893283	1.287445	-128.643493	-57.432499	0.223150
KGT3461_Position 6_00028 LC.hys	217.918352	7999.578696	216.041033	2994779.544184	246.100847	245.689392	110.608536	2.671174	54.031604	197.846937	1.292060	-128.636993	-57.432499	0.234243
KGT3461_Position 6_00029 LC.hys	227.239048	7999.174941	207.990877	3273892.934739	256.222420	256.083492	101.846680	2.443322	60.947077	207.724198	1.257416	-128.629997	-57.432499	0.234111