Thu Mar 11 19:03:03 2021

Number of Points = 3626
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.218714	0.013038	0.000000	0.000017	0.724590

0.275215	-0.006326	0.005005	0.000007	0.724572
0.344272	-0.174961	0.010010	-0.000006	0.724266
0.101443	-0.134175	0.015014	0.000039	0.724262
0.244559	-0.154806	0.020019	0.000012	0.724272
0.308158	-0.171843	0.025024	-0.000000	0.724261
0.400651	-0.186372	0.030029	-0.000018	0.724265
0.381859	-0.184754	0.035034	-0.000015	0.724262
0.323515	-0.175777	0.040038	-0.000004	0.724260
0.514432	-0.207310	0.045043	-0.000040	0.724265
0.288183	-0.171269	0.050048	0.000002	0.724257
0.424604	-0.192263	0.055053	-0.000023	0.724264
0.342769	-0.180259	0.060058	-0.000008	0.724259
0.386539	-0.188903	0.065062	-0.000017	0.724258
0.504134	-0.205588	0.070067	-0.000039	0.724267
0.223612	-0.213732	0.075072	0.000013	0.724154
0.485788	-0.361003	0.080077	-0.000036	0.723957
0.520951	-0.370345	0.085082	-0.000043	0.723951
0.516780	-0.372127	0.090086	-0.000042	0.723947
0.466408	-0.358751	0.095091	-0.000033	0.723956
0.429879	-0.358000	0.100096	-0.000026	0.723945
0.464487	-0.385611	0.105101	-0.000033	0.723904
0.479915	-0.528625	0.110106	-0.000036	0.723629
0.445950	-0.521756	0.115110	-0.000030	0.723631
0.395128	-0.511925	0.120115	-0.000021	0.723633
0.379888	-0.514603	0.125120	-0.000018	0.723623
0.510575	-0.576832	0.130125	-0.000042	0.723547
0.331182	-0.651294	0.135130	-0.000009	0.723339
0.203016	-0.630201	0.140134	0.000014	0.723336
0.517850	-0.682887	0.145139	-0.000044	0.723343
0.422330	-0.687789	0.150144	-0.000027	0.723300
0.308435	-0.818126	0.155149	-0.000006	0.723005
0.282292	-0.814759	0.160154	-0.000001	0.723003
0.363234	-0.829066	0.165158	-0.000016	0.723004
0.370270	-0.887231	0.170163	-0.000018	0.722893
0.237949	-0.970135	0.175168	0.000007	0.722684
0.436112	-1.001376	0.180173	-0.000031	0.722693
0.522793	-1.024541	0.185178	-0.000047	0.722678
0.462698	-1.173949	0.190182	-0.000036	0.722364
0.593218	-1.192274	0.195187	-0.000060	0.722374
0.438901	-1.175466	0.200192	-0.000032	0.722354
0.433648	-1.316286	0.205197	-0.000031	0.722076
0.428578	-1.317386	0.210202	-0.000030	0.722072
0.209987	-1.313765	0.215206	0.000010	0.722003
0.090567	-1.422469	0.220211	0.000032	0.721748
0.183795	-1.445679	0.225216	0.000015	0.721736
0.310292	-1.526167	0.230221	-0.000009	0.721622
0.094747	-1.582628	0.235226	0.000031	0.721436
0.088190	-1.584652	0.240230	0.000032	0.721430
0.257241	-1.732991	0.245235	0.000000	0.721198
0.262350	-1.777654	0.250240	-0.000001	0.721113
0.313404	-1.823032	0.255245	-0.000011	0.721042
0.183530	-1.882809	0.260250	0.000013	0.720879
0.395812	-1.923642	0.265254	-0.000026	0.720874
0.375881	-2.084123	0.270259	-0.000023	0.720551
0.039618	-2.032902	0.275264	0.000040	0.720535
0.185258	-2.173755	0.280269	0.000012	0.720309
0.125341	-2.208489	0.285274	0.000023	0.720220
0.119835	-2.296698	0.290278	0.000024	0.720045
0.245713	-2.392237	0.295283	0.000001	0.719901
-0.089247	-2.402840	0.300288	0.000063	0.719763
-0.318112	-2.442699	0.305293	0.000105	0.719605
-0.282486	-2.497333	0.310298	0.000098	0.719510
-2.829326	-2.167967	0.315302	0.000572	0.719265
-3.395247	-2.063513	0.320307	0.000677	0.719273
-3.805680	-2.001318	0.325312	0.000753	0.719252
-4.187011	-2.080906	0.330317	0.000824	0.718961
-4.284637	-2.063574	0.335322	0.000842	0.718962
-4.501482	-2.028887	0.340326	0.000882	0.718954
-4.081849	-2.130028	0.345331	0.000804	0.718903
-5.415194	-2.027607	0.350336	0.001052	0.718637
-5.233102	-2.057286	0.355341	0.001018	0.718642
-5.094361	-2.083278	0.360346	0.000992	0.718640
-5.550573	-2.004928	0.365350	0.001077	0.718635
-5.569057	-2.096034	0.370355	0.001080	0.718449
-6.309325	-2.017531	0.375360	0.001217	0.718344
-6.145443	-2.042941	0.380365	0.001187	0.718352
-6.469681	-1.987066	0.385370	0.001247	0.718349
-6.575359	-1.967865	0.390374	0.001266	0.718350
-6.225553	-2.142310	0.395379	0.001201	0.718129
-7.639081	-1.949791	0.400384	0.001464	0.718012
-7.153803	-2.033792	0.405389	0.001373	0.718018
-7.153320	-2.034724	0.410394	0.001373	0.718016
-7.601989	-1.957632	0.415398	0.001456	0.718011
-7.145686	-2.052868	0.420403	0.001371	0.717984
-7.741701	-2.093703	0.425408	0.001482	0.717694
-8.114121	-2.021936	0.430413	0.001551	0.717705
-8.473322	-1.958249	0.435418	0.001618	0.717705
-8.149411	-2.020027	0.440422	0.001557	0.717697
-7.769262	-2.083528	0.445427	0.001486	0.717706
-8.321774	-2.024544	0.450432	0.001589	0.717629
-8.826430	-2.060376	0.455437	0.001683	0.717380
-8.788336	-2.067809	0.460442	0.001675	0.717380
-9.363613	-1.968160	0.465446	0.001782	0.717374
-9.207038	-1.992158	0.470451	0.001753	0.717383
-9.277563	-1.987388	0.475456	0.001766	0.717368
-9.252030	-1.989664	0.480461	0.001761	0.717373
-9.216717	-2.113854	0.485466	0.001754	0.717140
-10.270717	-1.959588	0.490470	0.001950	0.717074
-9.758326	-2.047481	0.495475	0.001854	0.717081
-9.889558	-2.029764	0.500480	0.001878	0.717070
-10.152624	-1.977280	0.505485	0.001927	0.717082
-9.601392	-2.077851	0.510490	0.001824	0.717078
-9.987482	-2.081726	0.515494	0.001896	0.716934
-11.227550	-1.952201	0.520499	0.002127	0.716754
-10.744992	-2.042828	0.525504	0.002037	0.716745
-10.922787	-2.009912	0.530509	0.002069	0.716748
-11.300050	-1.942018	0.535514	0.002139	0.716750
-11.065044	-1.985473	0.540518	0.002095	0.716747
-10.672368	-2.053110	0.545523	0.002022	0.716752
-10.978296	-2.055692	0.550528	0.002079	0.716639
-11.988572	-1.973796	0.555533	0.002267	0.716446
-11.418641	-2.076242	0.560538	0.002160	0.716444
-12.115472	-1.953945	0.565542	0.002290	0.716441
-11.963049	-1.978236	0.570547	0.002261	0.716447
-11.850944	-2.002873	0.575552	0.002240	0.716438
-11.928072	-1.986352	0.580557	0.002254	0.716444
-11.972350	-2.017898	0.585562	0.002262	0.716367
-13.146686	-1.931912	0.590566	0.002481	0.716123
-12.493155	-2.042790	0.595571	0.002359	0.716134
-12.761961	-1.999887	0.600576	0.002409	0.716125
-12.906894	-1.972235	0.605581	0.002436	0.716129
-12.554231	-2.036768	0.610586	0.002370	0.716126
-12.641641	-2.024326	0.615590	0.002386	0.716120
-12.625233	-2.045035	0.620595	0.002382	0.716086
-13.568689	-1.985118	0.625600	0.002558	0.715872
-13.372030	-2.016859	0.630605	0.002521	0.715879
-13.843603	-1.931492	0.635610	0.002609	0.715882
-14.077246	-1.894535	0.640614	0.002652	0.715873
-13.326396	-2.023936	0.645619	0.002512	0.715882
-13.767740	-1.950531	0.650624	0.002594	0.715872
-14.083044	-1.890284	0.655629	0.002652	0.715881
-13.816428	-2.074832	0.660634	0.002602	0.715609
-14.751508	-1.944451	0.665638	0.002776	0.715538
-14.745600	-1.941387	0.670643	0.002775	0.715547
-14.759383	-1.945759	0.675648	0.002777	0.715533
-14.327545	-2.018572	0.680653	0.002697	0.715542
-14.406941	-2.005469	0.685658	0.002711	0.715540
-14.811927	-1.934403	0.690662	0.002786	0.715539
-14.863484	-2.027848	0.695667	0.002796	0.715336
-15.699058	-1.936306	0.700672	0.002951	0.715222
-15.649320	-1.941721	0.705677	0.002942	0.715230
-15.455682	-1.977691	0.710682	0.002905	0.715227
-15.540122	-1.964554	0.715686	0.002921	0.715224
-15.331020	-1.997572	0.720691	0.002882	0.715233
-15.644747	-1.947169	0.725696	0.002940	0.715222
-15.340218	-2.075915	0.730701	0.002883	0.715075
-16.354562	-1.980899	0.735706	0.003072	0.714905
-16.366346	-1.980940	0.740710	0.003074	0.714901
-16.285339	-1.992439	0.745715	0.003058	0.714908
-16.423952	-1.972049	0.750720	0.003084	0.714899
-16.479094	-1.960159	0.755725	0.003094	0.714904
-16.416587	-1.971154	0.760730	0.003082	0.714905
-16.209521	-2.066657	0.765734	0.003043	0.714789
-17.159154	-1.989773	0.770739	0.003220	0.714606
-17.260562	-1.975930	0.775744	0.003239	0.714598
-17.065909	-2.008268	0.780749	0.003202	0.714603
-17.003820	-2.018560	0.785754	0.003190	0.714605
-17.554158	-1.923873	0.790758	0.003293	0.714599
-17.249170	-1.973980	0.795763	0.003236	0.714608
-17.282105	-2.041991	0.800768	0.003242	0.714461
-18.379337	-1.942456	0.805773	0.003446	0.714271
-18.154783	-1.979768	0.810778	0.003404	0.714277
-18.392917	-1.939717	0.815782	0.003448	0.714273
-18.146532	-1.982491	0.820787	0.003402	0.714275
-18.351290	-1.951491	0.825792	0.003439	0.714265
-18.334627	-1.951412	0.830797	0.003436	0.714271
-18.209942	-1.973761	0.835802	0.003413	0.714272
-18.957090	-1.990654	0.840806	0.003552	0.713974
-18.998939	-1.988204	0.845811	0.003559	0.713964
-19.190813	-1.958632	0.850816	0.003595	0.713956
-19.244797	-1.944672	0.855821	0.003604	0.713965
-19.353342	-1.927629	0.860826	0.003624	0.713961
-19.113516	-1.972299	0.865830	0.003580	0.713957
-18.747974	-2.031669	0.870835	0.003511	0.713969
-19.283620	-2.037335	0.875840	0.003611	0.713769
-20.299539	-1.918264	0.880845	0.003800	0.713646
-19.949059	-1.980176	0.885850	0.003734	0.713647
-20.222075	-1.934025	0.890854	0.003785	0.713643
-20.254897	-1.923483	0.895859	0.003791	0.713653
-20.049444	-1.965092	0.900864	0.003752	0.713643
-19.830255	-2.001453	0.905869	0.003711	0.713649
-20.154469	-1.982372	0.910874	0.003771	0.713572
-21.244363	-1.899428	0.915878	0.003974	0.713352
-20.710856	-1.989949	0.920883	0.003875	0.713361
-21.286863	-1.892951	0.925888	0.003982	0.713350
-20.766166	-1.982014	0.930893	0.003884	0.713358
-20.583973	-2.015199	0.935898	0.003850	0.713357
-21.336584	-1.883439	0.940902	0.003990	0.713353
-21.030620	-1.934635	0.945907	0.003933	0.713360
-21.249947	-2.047990	0.950912	0.003974	0.713057
-22.012304	-1.931199	0.955917	0.004115	0.713020
-22.359310	-1.869977	0.960922	0.004180	0.713019
-21.768089	-1.977218	0.965926	0.004069	0.713015
-21.747096	-1.975485	0.970931	0.004065	0.713027
-22.082285	-1.921311	0.975936	0.004127	0.713016
-22.049979	-1.925908	0.980941	0.004121	0.713019
-22.038318	-1.982242	0.985946	0.004119	0.712911
-23.226385	-1.876396	0.990950	0.004340	0.712701
-22.570885	-1.988820	0.995955	0.004218	0.712710
-23.073127	-1.904915	1.000960	0.004311	0.712699
-22.790825	-1.951862	1.005965	0.004258	0.712707
-22.630971	-1.981931	1.010970	0.004228	0.712704
-23.154696	-1.890514	1.015974	0.004325	0.712700
-22.955924	-1.921754	1.020979	0.004288	0.712709
-23.488068	-1.978322	1.025984	0.004387	0.712408
-23.889092	-1.919933	1.030989	0.004461	0.712383
-23.645170	-1.963296	1.035994	0.004416	0.712383
-23.618262	-1.971008	1.040998	0.004411	0.712378
-23.649965	-1.961381	1.046003	0.004416	0.712386
-23.921230	-1.918667	1.051008	0.004466	0.712375
-23.720136	-1.952518	1.056013	0.004429	0.712380
-24.186925	-1.954890	1.061018	0.004516	0.712210
-24.774234	-1.915790	1.066022	0.004625	0.712080
-23.988192	-2.053167	1.071027	0.004478	0.712085
-24.744346	-1.921191	1.076032	0.004619	0.712080
-24.897847	-1.893269	1.081037	0.004647	0.712082
-24.630330	-1.939349	1.086042	0.004597	0.712085
-24.552967	-1.957579	1.091046	0.004582	0.712077
-24.776713	-2.013594	1.096051	0.004624	0.711886
-25.880681	-1.885960	1.101056	0.004829	0.711749
-25.550160	-1.940763	1.106061	0.004767	0.711758
-25.546331	-1.941581	1.111066	0.004766	0.711758
-26.100645	-1.845723	1.116070	0.004869	0.711752
-25.427603	-1.963243	1.121075	0.004744	0.711758
-25.697947	-1.919865	1.126080	0.004794	0.711748
-25.525129	-1.948642	1.131085	0.004762	0.711753
-25.951618	-2.025971	1.136090	0.004841	0.711448
-26.723158	-1.892027	1.141094	0.004984	0.711441
-26.608777	-1.908201	1.146099	0.004963	0.711450
-26.349005	-1.959127	1.151104	0.004914	0.711441
-26.618634	-1.907303	1.156109	0.004964	0.711449
-26.758341	-1.883405	1.161114	0.004990	0.711447
-26.523435	-1.929351	1.166118	0.004946	0.711440
-26.387587	-2.051583	1.171123	0.004920	0.711244
-27.520097	-1.909129	1.176128	0.005131	0.711126
-27.477575	-1.914065	1.181133	0.005123	0.711132
-27.451654	-1.918624	1.186138	0.005118	0.711133
-27.568906	-1.901151	1.191142	0.005139	0.711126
-27.328271	-1.939201	1.196147	0.005094	0.711136
-27.799430	-1.861634	1.201152	0.005182	0.711124
-27.608758	-1.932432	1.206157	0.005146	0.711051
-28.022005	-1.953084	1.211162	0.005223	0.710863
-28.134733	-1.934265	1.216166	0.005244	0.710861
-28.348867	-1.894013	1.221171	0.005283	0.710866
-28.428788	-1.883387	1.226176	0.005298	0.710859
-28.336647	-1.897401	1.231181	0.005281	0.710864
-28.162604	-1.928903	1.236186	0.005248	0.710864
-28.523757	-1.912922	1.241190	0.005315	0.710767
-29.361173	-1.883618	1.246195	0.005471	0.710528
-28.985315	-1.953626	1.251200	0.005400	0.710523
-29.098357	-1.931858	1.256205	0.005421	0.710526
-29.234928	-1.906562	1.261210	0.005446	0.710529
-29.620845	-1.839762	1.266214	0.005518	0.710525
-28.813445	-1.978936	1.271219	0.005368	0.710535
-29.100177	-1.943761	1.276224	0.005421	0.710504
-30.147991	-1.902459	1.281229	0.005616	0.710214
-30.101876	-1.910227	1.286234	0.005607	0.710215
-30.338323	-1.872405	1.291238	0.005651	0.710207
-29.969154	-1.932433	1.296243	0.005582	0.710219
-30.118087	-1.909738	1.301248	0.005609	0.710211
-30.333002	-1.870050	1.306253	0.005649	0.710215
-29.940226	-1.941003	1.311258	0.005576	0.710213
-30.360899	-1.981999	1.316262	0.005654	0.709982
-31.039210	-1.904823	1.321267	0.005780	0.709895
-30.932874	-1.930703	1.326272	0.005760	0.709881
-30.885653	-1.935350	1.331277	0.005751	0.709889
-30.944793	-1.922604	1.336282	0.005762	0.709894
-30.893782	-1.937257	1.341286	0.005752	0.709884
-30.918566	-1.928291	1.346291	0.005756	0.709893
-31.301619	-1.982922	1.351296	0.005827	0.709648
-31.688403	-1.941756	1.356301	0.005899	0.709593
-31.696136	-1.940201	1.361306	0.005900	0.709593
-32.060218	-1.878807	1.366310	0.005968	0.709587
-31.853984	-1.909376	1.371315	0.005929	0.709600
-31.648948	-1.950462	1.376320	0.005891	0.709591
-31.940578	-1.896908	1.381325	0.005945	0.709595
-32.440003	-1.949778	1.386330	0.006038	0.709311
-32.886494	-1.898346	1.391334	0.006121	0.709255
-32.927219	-1.885880	1.396339	0.006128	0.709266
-32.973771	-1.882205	1.401344	0.006136	0.709257
-33.098488	-1.858514	1.406349	0.006159	0.709261
-32.633648	-1.941261	1.411354	0.006073	0.709261
-32.934503	-1.890391	1.416358	0.006128	0.709256
-32.785725	-1.960451	1.421363	0.006101	0.709170
-33.806269	-1.889751	1.426368	0.006290	0.708947
-33.462638	-1.948246	1.431373	0.006226	0.708953
-33.721411	-1.901600	1.436378	0.006274	0.708955
-33.648677	-1.919221	1.441382	0.006260	0.708946
-33.193217	-1.996087	1.446387	0.006175	0.708955
-33.951386	-1.863047	1.451392	0.006316	0.708951
-33.591384	-1.988197	1.456397	0.006249	0.708830
-34.497114	-1.922860	1.461402	0.006417	0.708638
-34.965651	-1.842372	1.466406	0.006504	0.708632
-34.537565	-1.913662	1.471411	0.006424	0.708642
-34.376646	-1.947505	1.476416	0.006394	0.708632
-34.619195	-1.902581	1.481421	0.006439	0.708636
-34.892136	-1.854499	1.486426	0.006490	0.708636
-34.555894	-1.922357	1.491430	0.006427	0.708620
-34.661781	-2.038031	1.496435	0.006447	0.708351
-35.390177	-1.912043	1.501440	0.006582	0.708344
-35.308705	-1.924402	1.506445	0.006566	0.708349
-34.947658	-1.989668	1.511450	0.006499	0.708347
-35.425364	-1.907349	1.516454	0.006588	0.708342
-35.240155	-1.936717	1.521459	0.006553	0.708350
-35.432132	-2.004207	1.526464	0.006589	0.708146
-36.570564	-1.870816	1.531469	0.006800	0.708007
-36.126237	-1.949253	1.536474	0.006717	0.708009
-36.303774	-1.921444	1.541478	0.006750	0.708002
-36.469177	-1.886376	1.546483	0.006781	0.708014
-36.587362	-1.869846	1.551488	0.006803	0.708005
-36.314667	-1.918159	1.556493	0.006752	0.708006
-36.300653	-1.964821	1.561498	0.006749	0.707918
-37.597512	-1.848580	1.566502	0.006990	0.707688
-37.135816	-1.925640	1.571507	0.006904	0.707699
-37.140520	-1.929568	1.576512	0.006904	0.707690
-37.177948	-1.920620	1.581517	0.006911	0.707695
-37.424392	-1.876363	1.586522	0.006957	0.707696
-37.715218	-1.828048	1.591526	0.007011	0.707689
-37.018732	-1.948279	1.596531	0.006881	0.707697
-37.527435	-1.994693	1.601536	0.006975	0.707423
-38.384757	-1.866482	1.606541	0.007135	0.707374
-37.955177	-1.941710	1.611546	0.007055	0.707377
-37.873907	-1.960922	1.616550	0.007039	0.707368
-38.226034	-1.894676	1.621555	0.007105	0.707375
-38.094684	-1.921764	1.626560	0.007080	0.707368
-38.138763	-1.914588	1.631565	0.007088	0.707367
-38.430112	-1.982451	1.636570	0.007142	0.707127
-39.158137	-1.880228	1.641574	0.007277	0.707073
-39.042713	-1.896817	1.646579	0.007255	0.707081
-38.959837	-1.914525	1.651584	0.007240	0.707076
-39.045072	-1.898458	1.656589	0.007255	0.707078
-38.649875	-1.968648	1.661594	0.007182	0.707079
-38.754841	-1.954623	1.666598	0.007201	0.707070
-39.505395	-1.972563	1.671603	0.007341	0.706765
-39.818453	-1.928709	1.676608	0.007399	0.706742
-40.091347	-1.878180	1.681613	0.007449	0.706746
-39.986623	-1.892476	1.686618	0.007429	0.706755
-39.999992	-1.895709	1.691622	0.007432	0.706744
-39.440203	-1.992403	1.696627	0.007327	0.706751
-39.787547	-1.933811	1.701632	0.007392	0.706745
-40.668020	-1.913250	1.706637	0.007555	0.706471
-40.688298	-1.923949	1.711642	0.007559	0.706443
-40.674469	-1.929930	1.716646	0.007556	0.706436
-40.539152	-1.947934	1.721651	0.007531	0.706449
-40.874316	-1.893568	1.726656	0.007593	0.706439
-40.621544	-1.939346	1.731661	0.007546	0.706438
-40.775036	-1.911033	1.736666	0.007574	0.706440
-41.168613	-1.969824	1.741670	0.007647	0.706181
-41.748330	-1.892633	1.746675	0.007755	0.706129
-41.601224	-1.921710	1.751680	0.007727	0.706124
-41.400988	-1.957735	1.756685	0.007690	0.706124
-41.434868	-1.951793	1.761690	0.007696	0.706124
-41.512429	-1.940898	1.766694	0.007710	0.706118
-41.408420	-1.956120	1.771699	0.007690	0.706125
-42.047204	-1.976183	1.776704	0.007809	0.705857
-42.102728	-1.964676	1.781709	0.007819	0.705860
-42.336783	-1.921497	1.786714	0.007863	0.705864
-42.519503	-1.894067	1.791718	0.007896	0.705854
-42.114524	-1.960653	1.796723	0.007821	0.705865
-42.409777	-1.913202	1.801728	0.007875	0.705855
-42.668337	-1.926112	1.806733	0.007923	0.705737
-43.321821	-1.914811	1.811738	0.008045	0.705526
-42.943013	-1.986239	1.816742	0.007974	0.705519
-43.238598	-1.930036	1.821747	0.008029	0.705526
-43.340209	-1.915356	1.826752	0.008048	0.705520
-43.198089	-1.940440	1.831757	0.008021	0.705520
-43.119334	-1.953064	1.836762	0.008006	0.705524
-43.533099	-1.958598	1.841766	0.008083	0.705365
-44.203503	-1.915724	1.846771	0.008207	0.705211
-43.984553	-1.958499	1.851776	0.008167	0.705204
-44.253631	-1.909193	1.856781	0.008216	0.705207
-44.206981	-1.917258	1.861786	0.008207	0.705208
-44.335429	-1.897132	1.866790	0.008231	0.705203
-44.388541	-1.884892	1.871795	0.008241	0.705209
-44.530108	-1.880688	1.876800	0.008267	0.705167
-44.844069	-1.967257	1.881805	0.008325	0.704880
-44.921059	-1.950839	1.886810	0.008339	0.704886
-45.756665	-1.805301	1.891814	0.008495	0.704879
-45.048970	-1.928348	1.896819	0.008363	0.704886
-44.791875	-1.977961	1.901824	0.008315	0.704879
-45.411146	-1.865603	1.906829	0.008430	0.704883
-45.088523	-1.923295	1.911834	0.008369	0.704883
-45.535321	-1.983333	1.916838	0.008452	0.704602
-45.957368	-1.914076	1.921843	0.008531	0.704591
-46.253655	-1.864993	1.926848	0.008586	0.704584
-46.091258	-1.891951	1.931853	0.008555	0.704588
-45.827408	-1.936376	1.936858	0.008506	0.704594
-46.253184	-1.865641	1.941862	0.008585	0.704584
-45.634470	-1.970272	1.946867	0.008469	0.704596
-46.201892	-2.019779	1.951872	0.008575	0.704292
-47.131786	-1.873296	1.956877	0.008748	0.704254
-46.867243	-1.915718	1.961882	0.008698	0.704264
-46.676337	-1.956046	1.966886	0.008663	0.704252
-47.089763	-1.876939	1.971891	0.008739	0.704263
-47.103675	-1.878428	1.976896	0.008742	0.704255
-46.562667	-1.974127	1.981901	0.008641	0.704257
-47.071416	-2.018498	1.986906	0.008735	0.703986
-48.290717	-1.821489	1.991910	0.008962	0.703945
-47.905254	-1.885511	1.996915	0.008890	0.703955
-47.671162	-1.929774	2.001920	0.008846	0.703950

-47.759008	-1.915392	2.011917	0.008862	0.703948
-47.769590	-1.911841	2.021914	0.008864	0.703953
-48.318897	-1.930362	2.031910	0.008966	0.703719
-48.503000	-1.939486	2.041907	0.008999	0.703635
-48.640519	-1.913033	2.051904	0.009024	0.703640
-48.219244	-1.905136	2.061901	0.008946	0.703808
-47.940379	-1.912201	2.071898	0.008893	0.703895
-47.446217	-1.971245	2.081894	0.008801	0.703954
-48.014456	-1.871060	2.091891	0.008906	0.703953
-47.773310	-1.915217	2.101888	0.008861	0.703951
-48.011293	-1.873022	2.111885	0.008905	0.703952
-47.780380	-1.913843	2.121882	0.008861	0.703953
-47.903938	-1.892668	2.131878	0.008884	0.703952
-47.814584	-1.909414	2.141875	0.008867	0.703952
-47.154960	-1.894900	2.151872	0.008743	0.704219
-47.031858	-1.896729	2.161869	0.008720	0.704260
-46.839455	-1.932079	2.171866	0.008684	0.704259
-46.886059	-1.924043	2.181862	0.008692	0.704259
-46.982181	-1.871474	2.191859	0.008709	0.704332
-45.774159	-1.959305	2.201856	0.008484	0.704590
-46.030863	-1.915829	2.211853	0.008531	0.704586
-45.908065	-1.934930	2.221850	0.008508	0.704592
-46.135969	-1.895269	2.231846	0.008550	0.704591
-45.406324	-1.879256	2.241843	0.008414	0.704886
-45.297467	-1.900681	2.251840	0.008393	0.704883
-45.047483	-1.944122	2.261837	0.008346	0.704886
-45.229200	-1.871720	2.271834	0.008379	0.704968
-44.227162	-1.930968	2.281830	0.008192	0.705209
-44.256729	-1.927212	2.291827	0.008198	0.705207
-43.973337	-1.978005	2.301824	0.008144	0.705207
-44.178005	-1.885303	2.311821	0.008182	0.705321
-43.002227	-1.993361	2.321818	0.007963	0.705526
-43.437015	-1.917211	2.331814	0.008043	0.705525
-43.340133	-1.935609	2.341811	0.008025	0.705523
-42.897657	-1.898652	2.351808	0.007942	0.705757
-42.582022	-1.905379	2.361805	0.007883	0.705858
-42.427035	-1.931725	2.371802	0.007853	0.705861
-42.542022	-1.887951	2.381798	0.007874	0.705909
-41.775270	-1.917594	2.391795	0.007731	0.706125
-41.813706	-1.911209	2.401792	0.007738	0.706125
-41.968183	-1.883166	2.411789	0.007766	0.706127
-41.031674	-1.913013	2.421786	0.007591	0.706403
-41.123190	-1.877799	2.431782	0.007608	0.706442
-40.928687	-1.912898	2.441779	0.007571	0.706442
-40.844921	-1.841285	2.451776	0.007555	0.706617
-40.188093	-1.893318	2.461773	0.007432	0.706748
-40.158118	-1.899011	2.471770	0.007426	0.706748
-40.100828	-1.850270	2.481766	0.007415	0.706867
-38.962917	-1.948636	2.491763	0.007203	0.707078
-39.186781	-1.910016	2.501760	0.007244	0.707076
-39.167160	-1.912968	2.511757	0.007240	0.707078
-38.793505	-1.873475	2.521754	0.007170	0.707292
-38.464560	-1.892736	2.531750	0.007108	0.707372
-38.334948	-1.916344	2.541747	0.007084	0.707372
-38.255683	-1.872361	2.551744	0.007068	0.707489
-37.574805	-1.891458	2.561741	0.006941	0.707695
-37.421164	-1.917128	2.571738	0.006912	0.707700
-37.623108	-1.882535	2.581734	0.006949	0.707698
-36.579134	-1.913928	2.591731	0.006755	0.708009
-36.789154	-1.877234	2.601728	0.006793	0.708008
-36.387716	-1.949213	2.611725	0.006718	0.708008
-36.442272	-1.867052	2.621722	0.006728	0.708154
-35.593981	-1.921185	2.631718	0.006569	0.708349
-35.660329	-1.911854	2.641715	0.006581	0.708345
-35.935947	-1.864327	2.651712	0.006632	0.708343
-35.201024	-1.855505	2.661709	0.006495	0.708624
-35.095616	-1.867383	2.671706	0.006475	0.708639
-34.886825	-1.904789	2.681702	0.006435	0.708639
-34.419628	-1.882651	2.691699	0.006348	0.708851
-34.352226	-1.844271	2.701696	0.006335	0.708953
-33.890183	-1.926656	2.711693	0.006249	0.708954
-34.082448	-1.846556	2.721690	0.006284	0.709046
-32.913311	-1.946798	2.731686	0.006066	0.709263
-32.960116	-1.938493	2.741683	0.006074	0.709264
-33.378027	-1.865260	2.751680	0.006151	0.709263
-32.748597	-1.866191	2.761677	0.006034	0.709486
-32.370788	-1.880973	2.771674	0.005963	0.709592
-32.107438	-1.929349	2.781670	0.005913	0.709590
-32.224735	-1.877925	2.791667	0.005935	0.709652
-31.503166	-1.889034	2.801664	0.005800	0.709888
-31.234599	-1.937597	2.811661	0.005750	0.709887
-31.673071	-1.857342	2.821658	0.005831	0.709892
-30.866645	-1.878054	2.831654	0.005680	0.710139
-30.643914	-1.881024	2.841651	0.005638	0.710213
-30.766465	-1.859024	2.851648	0.005661	0.710214
-30.313960	-1.887174	2.861645	0.005576	0.710320
-29.569006	-1.915983	2.871642	0.005437	0.710529
-29.781699	-1.878116	2.881638	0.005476	0.710529
-29.657549	-1.900355	2.891635	0.005452	0.710530
-28.989154	-1.874427	2.901632	0.005327	0.710820
-28.772416	-1.890812	2.911629	0.005287	0.710866
-28.936489	-1.861375	2.921626	0.005317	0.710867
-28.495806	-1.892688	2.931622	0.005234	0.710962
-28.079026	-1.880104	2.941619	0.005156	0.711136
-28.045151	-1.887821	2.951616	0.005149	0.711134
-27.958517	-1.903021	2.961613	0.005133	0.711135
-27.209689	-1.889293	2.971610	0.004993	0.711430
-27.011785	-1.913780	2.981606	0.004956	0.711452
-26.977949	-1.919727	2.991603	0.004949	0.711453
-27.142142	-1.831063	3.001600	0.004979	0.711572
-26.058445	-1.932612	3.011597	0.004777	0.711756
-26.404486	-1.870123	3.021594	0.004841	0.711758
-25.986364	-1.945017	3.031590	0.004763	0.711758
-25.776370	-1.827800	3.041587	0.004723	0.712067
-25.300946	-1.903726	3.051584	0.004634	0.712086
-25.240888	-1.915521	3.061581	0.004622	0.712084
-25.070652	-1.870625	3.071578	0.004590	0.712235
-24.299504	-1.933647	3.081574	0.004446	0.712384
-24.375724	-1.919512	3.091571	0.004460	0.712386
-24.437109	-1.911159	3.101568	0.004471	0.712382
-23.959457	-1.846397	3.111565	0.004382	0.712681
-23.753266	-1.871944	3.121562	0.004343	0.712704
-23.554366	-1.906555	3.131558	0.004305	0.712707
-23.303489	-1.852909	3.141555	0.004258	0.712903
-22.618633	-1.918031	3.151552	0.004130	0.713017
-22.970816	-1.854648	3.161549	0.004195	0.713020
-22.715152	-1.869917	3.171546	0.004147	0.713081
-21.644495	-1.922046	3.181542	0.003947	0.713357
-21.942230	-1.869465	3.191539	0.004002	0.713357
-21.735059	-1.907119	3.201536	0.003963	0.713357
-21.639987	-1.834459	3.211533	0.003945	0.713536
-20.993467	-1.894658	3.221530	0.003824	0.713646
-21.106449	-1.874366	3.231526	0.003845	0.713647
-21.024040	-1.856967	3.241523	0.003829	0.713712
-20.228281	-1.872095	3.251520	0.003681	0.713964
-20.225377	-1.873512	3.261517	0.003680	0.713963
-20.245807	-1.866681	3.271514	0.003683	0.713970
-19.411277	-1.881112	3.281510	0.003527	0.714238
-19.363454	-1.870349	3.291507	0.003518	0.714277
-19.098511	-1.918568	3.301504	0.003468	0.714276
-19.411478	-1.802959	3.311501	0.003526	0.714396
-18.209285	-1.910240	3.321498	0.003301	0.714609
-18.293976	-1.896642	3.331494	0.003317	0.714607
-18.177130	-1.918594	3.341491	0.003295	0.714605
-17.892395	-1.862981	3.351488	0.003241	0.714817
-17.701066	-1.854849	3.361485	0.003205	0.714902
-17.515365	-1.886350	3.371482	0.003170	0.714906
-17.490968	-1.834925	3.381478	0.003165	0.715017
-16.783720	-1.854516	3.391475	0.003033	0.715229
-16.458058	-1.913826	3.401472	0.002972	0.715228
-16.796302	-1.855060	3.411469	0.003034	0.715226
-15.892646	-1.873306	3.421466	0.002866	0.715510
-15.771218	-1.877983	3.431462	0.002843	0.715544
-15.341217	-1.953987	3.441459	0.002762	0.715546
-15.530932	-1.905402	3.451456	0.002797	0.715576
-14.648703	-1.910249	3.461453	0.002632	0.715879
-14.205091	-1.988755	3.471450	0.002549	0.715881
-14.289396	-1.975150	3.481446	0.002565	0.715879
-14.322399	-1.968396	3.491443	0.002570	0.715881
-13.735867	-1.965629	3.501440	0.002461	0.716095
-13.865249	-1.926952	3.511437	0.002484	0.716127
-13.475722	-1.994677	3.521434	0.002411	0.716131
-13.532397	-1.962402	3.531430	0.002421	0.716175
-12.725753	-1.970221	3.541427	0.002271	0.716445
-12.741680	-1.967456	3.551424	0.002273	0.716446
-12.877946	-1.945386	3.561421	0.002298	0.716443
-12.314577	-1.967733	3.571418	0.002193	0.716598
-11.656424	-2.005009	3.581414	0.002070	0.716757
-11.835847	-1.973437	3.591411	0.002103	0.716757
-12.002251	-1.945842	3.601408	0.002133	0.716754
-11.380494	-1.913022	3.611405	0.002017	0.717039
-10.901098	-1.977232	3.621402	0.001927	0.717082
-10.895157	-1.976505	3.631398	0.001926	0.717086
-10.639645	-1.990483	3.641395	0.001878	0.717149
-10.275288	-1.940383	3.651392	0.001809	0.717377
-9.951225	-1.999401	3.661389	0.001749	0.717376
-10.259452	-1.943307	3.671386	0.001806	0.717379
-9.323469	-1.993284	3.681382	0.001631	0.717611
-9.211363	-1.966509	3.691379	0.001610	0.717704
-9.229284	-1.965167	3.701376	0.001612	0.717701
-9.138846	-1.964146	3.711373	0.001595	0.717736
-8.340595	-1.963931	3.721370	0.001446	0.718018
-8.163983	-1.994510	3.731366	0.001413	0.718020
-8.056917	-2.014204	3.741363	0.001392	0.718020
-8.202349	-1.904099	3.751360	0.001419	0.718187
-6.825421	-2.065040	3.761357	0.001162	0.718355
-7.242399	-1.990171	3.771354	0.001239	0.718357
-7.019308	-2.030293	3.781350	0.001197	0.718357
-6.710396	-2.007283	3.791347	0.001139	0.718512
-6.233867	-2.027017	3.801344	0.001050	0.718641
-6.339284	-2.007679	3.811341	0.001069	0.718643
-6.227619	-2.027915	3.821338	0.001048	0.718643
-5.663062	-2.005646	3.831334	0.000943	0.718886
-5.312219	-2.030292	3.841331	0.000877	0.718962
-5.226730	-2.047450	3.851328	0.000861	0.718959
-5.343188	-2.020600	3.861325	0.000882	0.718972
-4.643612	-1.997031	3.871322	0.000751	0.719265
-4.195660	-2.076087	3.881318	0.000667	0.719267
-4.370177	-2.045513	3.891315	0.000699	0.719267
-4.224043	-2.023690	3.901312	0.000672	0.719362
-3.370039	-2.055491	3.911309	0.000512	0.719600
-3.485597	-2.035615	3.921306	0.000533	0.719599
-3.383744	-2.053825	3.931302	0.000514	0.719600
-3.467868	-1.946513	3.941299	0.000529	0.719783
-2.721023	-2.020764	3.951296	0.000390	0.719900
-2.747018	-2.017751	3.961293	0.000394	0.719897
-2.832766	-1.956294	3.971290	0.000409	0.719989
-2.057066	-1.976455	3.981286	0.000265	0.720222
-2.114613	-1.965999	3.991283	0.000275	0.720224
-2.005346	-1.971994	4.001280	0.000254	0.720251
-1.755962	-1.871382	4.011277	0.000207	0.720537
-1.724691	-1.876822	4.021274	0.000201	0.720538
-1.555591	-1.860745	4.031270	0.000169	0.720630
-1.148706	-1.806732	4.041267	0.000093	0.720880
-0.932421	-1.846508	4.051264	0.000052	0.720878
-1.040597	-1.762597	4.061261	0.000072	0.721006
-1.157645	-1.684248	4.071258	0.000093	0.721120
-1.032211	-1.661628	4.081254	0.000069	0.721209
-0.812011	-1.585477	4.091251	0.000028	0.721437
-0.775214	-1.557271	4.101248	0.000020	0.721506
-0.819841	-1.431488	4.111245	0.000028	0.721739
-0.821803	-1.362952	4.121242	0.000028	0.721873
-0.640267	-1.294013	4.131238	-0.000006	0.722073
-0.515894	-1.215185	4.141235	-0.000030	0.722272
-0.820958	-1.094221	4.151232	0.000026	0.722404
-0.729772	-0.966390	4.161229	0.000009	0.722688
-0.621469	-0.877562	4.171226	-0.000012	0.722900
-0.302703	-0.840958	4.181222	-0.000072	0.723084
-0.453405	-0.684470	4.191219	-0.000044	0.723340
-0.281660	-0.580721	4.201216	-0.000077	0.723604
-0.143835	-0.493340	4.211213	-0.000103	0.723824
-0.151026	-0.373922	4.221210	-0.000102	0.724056
-0.405183	-0.194611	4.231206	-0.000055	0.724319
-0.140846	-0.095142	4.241203	-0.000105	0.724607
-0.080101	0.036877	4.251200	-0.000117	0.724887
0.000000	0.200714	4.261197	-0.000132	0.725237

0.132469	0.817503	4.266202	-0.000158	0.726488
0.039684	2.104565	4.271206	-0.000142	0.728965
0.320304	3.910849	4.276211	-0.000195	0.732567
0.876620	6.236936	4.281216	-0.000300	0.737247
0.924736	9.151246	4.286221	-0.000312	0.742848
1.168404	12.521539	4.291226	-0.000359	0.749337
1.513699	16.320598	4.296230	-0.000426	0.756608
1.697860	20.552012	4.301235	-0.000464	0.764559
1.940227	25.185706	4.306240	-0.000512	0.773185
2.099812	30.181295	4.311245	-0.000545	0.782345
2.500531	35.488191	4.316250	-0.000623	0.792033
2.889812	41.110683	4.321254	-0.000700	0.802159
3.092613	47.068572	4.326259	-0.000742	0.812686
3.799615	53.223543	4.331264	-0.000878	0.823571
4.162126	59.711292	4.336269	-0.000950	0.834776
4.603294	66.402271	4.341274	-0.001036	0.846196
5.071548	73.320496	4.346278	-0.001128	0.857847
5.443086	80.451600	4.351283	-0.001202	0.869661
5.756235	87.778991	4.356288	-0.001266	0.881616
6.405637	95.225052	4.361293	-0.001392	0.893693
7.094362	102.830250	4.366298	-0.001525	0.905868
7.899287	110.561688	4.371302	-0.001680	0.918108
9.110346	118.341703	4.376307	-0.001911	0.930369
9.896090	126.321107	4.381312	-0.002063	0.942658
11.152308	134.326550	4.386317	-0.002302	0.954948
11.533028	142.567537	4.391322	-0.002378	0.967203
12.241033	150.847048	4.396326	-0.002516	0.979443
12.731357	159.244235	4.401331	-0.002613	0.991645
13.432936	167.646643	4.406336	-0.002749	1.003758
14.388511	176.047148	4.411341	-0.002933	1.015785
14.997888	184.556131	4.416346	-0.003052	1.027738
15.994349	193.034277	4.421350	-0.003243	1.039602
16.628466	201.600770	4.426355	-0.003367	1.051366
17.208353	210.214787	4.431360	-0.003481	1.063051
17.696777	218.860932	4.436365	-0.003578	1.074630
18.091300	227.517538	4.441370	-0.003657	1.086077
18.931970	236.114987	4.446374	-0.003820	1.097428
19.818577	244.708615	4.451379	-0.003990	1.108667
20.494585	253.356409	4.456384	-0.004122	1.119816
20.970028	262.023366	4.461389	-0.004217	1.130835
21.755927	270.637793	4.466394	-0.004369	1.141749
22.546959	279.278088	4.471398	-0.004522	1.152592
23.547105	287.837407	4.476403	-0.004714	1.163278
24.422604	296.429071	4.481408	-0.004883	1.173879
24.734619	305.088130	4.486413	-0.004947	1.184351
25.062520	313.749231	4.491418	-0.005014	1.194737
26.133427	322.255173	4.496422	-0.005219	1.204999
26.891530	330.816297	4.501427	-0.005366	1.215177
27.671288	339.375970	4.506432	-0.005517	1.225272
27.986895	348.007249	4.511437	-0.005581	1.235276
28.449672	356.564221	4.516442	-0.005673	1.245143
29.085143	365.090050	4.521446	-0.005798	1.254930
29.618914	373.604041	4.526451	-0.005903	1.264609
30.356248	382.100692	4.531456	-0.006046	1.274233
31.082027	390.556426	4.536461	-0.006187	1.283737
31.538922	399.076234	4.541466	-0.006277	1.293191
32.641349	407.468101	4.546470	-0.006488	1.302556
33.072044	416.047230	4.551475	-0.006574	1.311933
33.378671	424.580376	4.556480	-0.006637	1.321172
33.629990	433.031183	4.561485	-0.006690	1.330250
34.239779	441.430949	4.566490	-0.006809	1.339275
34.707549	449.838438	4.571494	-0.006902	1.348222
35.220549	458.223992	4.576499	-0.007003	1.357096
36.058229	466.541859	4.581504	-0.007165	1.365897
36.513490	474.945688	4.586509	-0.007255	1.374665
36.914257	483.330115	4.591514	-0.007335	1.383347
37.517249	491.697547	4.596518	-0.007453	1.391993
38.055455	500.036452	4.601523	-0.007559	1.400545
38.530563	508.389843	4.606528	-0.007653	1.409049
38.932299	516.746487	4.611533	-0.007734	1.417492
39.521809	525.051280	4.616538	-0.007849	1.425865
40.367186	533.346365	4.621542	-0.008012	1.434221
40.519237	541.702514	4.626547	-0.008046	1.442476
41.131180	550.009717	4.631552	-0.008166	1.450710
41.298160	558.369709	4.636557	-0.008203	1.458877
41.940617	566.632518	4.641562	-0.008328	1.466981
42.599607	574.957124	4.646566	-0.008456	1.475101
43.211845	583.197950	4.651571	-0.008576	1.483090
43.413601	591.528728	4.656576	-0.008619	1.491057
43.890918	599.800578	4.661581	-0.008714	1.498969
44.329757	608.062490	4.666586	-0.008801	1.506824
44.793996	616.347649	4.671590	-0.008893	1.514663
45.212516	624.585179	4.676595	-0.008976	1.522410
45.562072	632.871421	4.681600	-0.009047	1.530153
46.131971	641.113007	4.686605	-0.009159	1.537849
46.490136	649.371200	4.691610	-0.009231	1.545490
46.924309	657.646986	4.696614	-0.009318	1.553120
46.986054	665.912516	4.701619	-0.009335	1.560649
47.946577	674.055589	4.706624	-0.009519	1.568162
48.508554	682.265550	4.711629	-0.009629	1.575642
48.966673	690.492552	4.716634	-0.009720	1.583086
49.349684	698.738713	4.721638	-0.009797	1.590501
49.850481	706.954028	4.726643	-0.009896	1.597871
50.421277	715.140761	4.731648	-0.010008	1.605192
50.710644	723.397207	4.736653	-0.010067	1.612501
50.957857	731.636303	4.741658	-0.010119	1.619756
51.184859	739.880938	4.746662	-0.010167	1.626981
51.899266	748.082668	4.751667	-0.010305	1.634203
52.338866	756.273480	4.756672	-0.010393	1.641347
52.575275	764.481839	4.761677	-0.010442	1.648446
53.088152	772.664913	4.766682	-0.010543	1.655532
53.614198	780.829877	4.771686	-0.010647	1.662573
53.834596	789.044740	4.776691	-0.010694	1.669585
54.357313	797.221532	4.781696	-0.010796	1.676576
54.646043	805.399043	4.786701	-0.010856	1.683508
55.022868	813.583257	4.791706	-0.010931	1.690428
55.562658	821.758677	4.796710	-0.011038	1.697334
55.971122	829.917338	4.801715	-0.011119	1.704181
56.287557	838.145283	4.806720	-0.011184	1.711045
56.497017	846.345459	4.811725	-0.011228	1.717845
56.784797	854.502574	4.816730	-0.011287	1.724593
57.573388	862.628806	4.821734	-0.011440	1.731354
57.854758	870.815249	4.826739	-0.011498	1.738072
57.981097	879.017385	4.831744	-0.011527	1.744758
58.606257	887.146871	4.836749	-0.011649	1.751422
59.150213	895.288494	4.841754	-0.011755	1.758060
59.648593	903.423635	4.846758	-0.011854	1.764663
60.006100	911.590046	4.851763	-0.011926	1.771248
60.366317	919.771917	4.856768	-0.011999	1.777821
60.441137	927.958974	4.861773	-0.012018	1.784338
60.862666	936.131146	4.866778	-0.012102	1.790863
61.445762	944.266905	4.871782	-0.012216	1.797355
62.007426	952.358628	4.876787	-0.012326	1.803786
62.518549	960.487013	4.881792	-0.012427	1.810217
62.781291	968.658742	4.886797	-0.012481	1.816628
63.049685	976.802671	4.891802	-0.012537	1.822997
63.236195	984.984142	4.896806	-0.012577	1.829362
63.580384	993.115816	4.901811	-0.012647	1.835685
64.171249	1001.227015	4.906816	-0.012762	1.842000
64.354683	1009.381657	4.911821	-0.012802	1.848278
64.628558	1017.552004	4.916826	-0.012859	1.854558
65.230166	1025.640464	4.921830	-0.012976	1.860792
65.431122	1033.789042	4.926835	-0.013019	1.867005
66.071244	1041.927063	4.931840	-0.013144	1.873239
66.295253	1050.053655	4.936845	-0.013191	1.879397
66.601780	1058.172733	4.941850	-0.013254	1.885537
66.879463	1066.332772	4.946854	-0.013311	1.891686
67.276785	1074.435755	4.951859	-0.013390	1.897785
67.617589	1082.570607	4.956864	-0.013459	1.903882
67.647767	1090.733418	4.961869	-0.013470	1.909945
68.172627	1098.825632	4.966874	-0.013574	1.915992
68.668028	1106.926728	4.971878	-0.013671	1.922023
68.782141	1115.068515	4.976883	-0.013698	1.928022
69.162111	1123.203623	4.981888	-0.013774	1.934028
69.898373	1131.248716	4.986893	-0.013917	1.939988
70.243029	1139.376125	4.991898	-0.013987	1.945947
70.692073	1147.542377	4.996902	-0.014076	1.951927
70.889148	1155.680730	5.001907	-0.014118	1.957841
71.361620	1163.757398	5.006912	-0.014212	1.963723
71.766440	1171.845357	5.011917	-0.014292	1.969587
71.949832	1179.997162	5.016922	-0.014332	1.975457
72.496531	1188.075520	5.021926	-0.014439	1.981295
72.832181	1196.155915	5.026931	-0.014507	1.987094
73.270957	1204.299396	5.031936	-0.014595	1.992933
73.894850	1212.353241	5.036941	-0.014716	1.998710
74.431410	1220.433488	5.041946	-0.014822	2.004480
74.928358	1228.536252	5.046950	-0.014920	2.010245
75.348054	1236.659457	5.051955	-0.015003	2.016000
75.599780	1244.795371	5.056960	-0.015056	2.021729
75.659818	1252.924503	5.061965	-0.015072	2.027418
76.035948	1261.065852	5.066970	-0.015148	2.033132
76.529894	1269.148557	5.071974	-0.015245	2.038801
76.563802	1277.265617	5.076979	-0.015257	2.044431
76.876555	1285.381598	5.081984	-0.015321	2.050074
77.130169	1293.485338	5.086989	-0.015374	2.055686
77.583719	1301.550813	5.091994	-0.015464	2.061277
77.761583	1309.676344	5.096998	-0.015502	2.066866
77.961439	1317.794759	5.102003	-0.015545	2.072437
78.536334	1325.846843	5.107008	-0.015658	2.077985
78.790252	1333.927414	5.112013	-0.015710	2.083506
79.029642	1342.042118	5.117018	-0.015760	2.089034
79.563048	1350.128912	5.122022	-0.015865	2.094557
79.846389	1358.208871	5.127027	-0.015924	2.100037
80.305871	1366.293498	5.132032	-0.016015	2.105522
80.662142	1374.418228	5.137037	-0.016086	2.111010
81.085033	1382.547307	5.142042	-0.016171	2.116493
81.257997	1390.622652	5.147046	-0.016208	2.121902
81.442386	1398.704669	5.152051	-0.016248	2.127303
81.983105	1406.781088	5.157056	-0.016354	2.132720
82.221582	1414.875871	5.162061	-0.016404	2.138107
82.375619	1422.969322	5.167066	-0.016438	2.143471
82.762294	1431.054611	5.172070	-0.016516	2.148838
83.117406	1439.149251	5.177075	-0.016588	2.154195
83.579188	1447.213118	5.182080	-0.016679	2.159529
83.866079	1455.289022	5.187085	-0.016738	2.164841
84.328344	1463.351399	5.192090	-0.016829	2.170147
84.824913	1471.448431	5.197094	-0.016927	2.175466
84.674435	1479.571417	5.202099	-0.016905	2.180728
85.103338	1487.644791	5.207104	-0.016990	2.186000
85.490594	1495.732278	5.212109	-0.017068	2.191264
85.705509	1503.844741	5.217114	-0.017113	2.196515
85.829243	1511.930396	5.222118	-0.017142	2.201729
86.223352	1519.961154	5.227123	-0.017221	2.206919
86.503358	1528.062090	5.232128	-0.017278	2.212132
86.638490	1536.158201	5.237133	-0.017309	2.217316
86.951341	1544.220215	5.242138	-0.017373	2.222482
87.417587	1552.288564	5.247142	-0.017465	2.227654
87.402083	1560.409731	5.252147	-0.017468	2.232805
87.845104	1568.470713	5.257152	-0.017556	2.237946
88.084599	1576.528992	5.262157	-0.017606	2.243055
88.400993	1584.592874	5.267162	-0.017670	2.248164
88.648135	1592.708103	5.272166	-0.017722	2.253286
89.150610	1600.719513	5.277171	-0.017821	2.258355
89.605791	1608.796066	5.282176	-0.017911	2.263448
89.823810	1616.893749	5.287181	-0.017957	2.268522
90.089848	1625.061285	5.292186	-0.018012	2.273633
90.368194	1633.108664	5.297190	-0.018069	2.278659
90.366279	1641.175927	5.302195	-0.018075	2.283662
90.936699	1649.202428	5.307200	-0.018186	2.288677
91.409552	1657.263670	5.312205	-0.018280	2.293695
91.498395	1665.342187	5.317210	-0.018302	2.298679
92.031018	1673.381448	5.322214	-0.018406	2.303666
92.056315	1681.481065	5.327219	-0.018417	2.308637
92.372980	1689.570276	5.332224	-0.018481	2.313615
92.478294	1697.645397	5.337229	-0.018506	2.318556
92.695224	1705.704387	5.342234	-0.018552	2.323485
93.354193	1713.727328	5.347238	-0.018680	2.328419
93.366171	1721.859687	5.352243	-0.018688	2.333356
93.921488	1729.887694	5.357248	-0.018797	2.338263
94.165538	1737.949089	5.362253	-0.018848	2.343155
94.370688	1746.027598	5.367258	-0.018891	2.348044
94.682952	1754.158193	5.372262	-0.018955	2.352962
94.985918	1762.186804	5.377267	-0.019017	2.357808
95.417299	1770.225509	5.382272	-0.019103	2.362661
95.589507	1778.292452	5.387277	-0.019140	2.367499
95.756886	1786.393169	5.392282	-0.019177	2.372347
96.369307	1794.420088	5.397286	-0.019296	2.377178
96.496854	1802.488324	5.402291	-0.019326	2.381984
96.849778	1810.551450	5.407296	-0.019397	2.386795
97.123156	1818.650443	5.412301	-0.019453	2.391611
97.479368	1826.707811	5.417306	-0.019525	2.396400
97.759603	1834.756166	5.422310	-0.019583	2.401167
97.886717	1842.817475	5.427315	-0.019612	2.405921
98.113804	1850.910260	5.432320	-0.019660	2.410691
98.181060	1859.003674	5.437325	-0.019678	2.415440
98.882929	1866.998467	5.442330	-0.019814	2.420172
99.750886	1874.999694	5.447334	-0.019981	2.424910
99.973011	1883.080813	5.452339	-0.020028	2.429636
100.421224	1891.241213	5.457344	-0.020117	2.434416
100.661781	1899.273296	5.462349	-0.020167	2.439096
100.805818	1907.338262	5.467354	-0.020199	2.443779
101.159993	1915.388211	5.472358	-0.020271	2.448460
101.457873	1923.447925	5.477363	-0.020332	2.453134
101.724421	1931.514837	5.482368	-0.020387	2.457800
102.090903	1939.543958	5.487373	-0.020460	2.462443
102.213443	1947.630153	5.492378	-0.020489	2.467092
102.764060	1955.676119	5.497382	-0.020597	2.471741
102.893046	1963.737571	5.502387	-0.020626	2.476358
103.009212	1971.818569	5.507392	-0.020653	2.480978
103.467029	1979.839889	5.512397	-0.020744	2.485579
103.819020	1987.901916	5.517402	-0.020815	2.490188
104.064829	1995.993960	5.522406	-0.020866	2.494797
103.918067	2004.067736	5.527411	-0.020844	2.499359
104.445556	2012.089878	5.532416	-0.020948	2.503932
104.684881	2020.144506	5.537421	-0.020998	2.508494
104.938420	2028.254575	5.542426	-0.021051	2.513080
105.267947	2036.293990	5.547430	-0.021118	2.517624
105.572009	2044.329415	5.552435	-0.021180	2.522155
105.844981	2052.404114	5.557440	-0.021236	2.526697
106.102033	2060.450013	5.562445	-0.021289	2.531215
106.305114	2068.504190	5.567450	-0.021333	2.535725
106.516245	2076.578546	5.572454	-0.021377	2.540238
106.629936	2084.614354	5.577459	-0.021404	2.544715
107.212232	2092.640282	5.582464	-0.021518	2.549212
107.162791	2100.753325	5.587469	-0.021514	2.553705
107.460871	2108.787452	5.592474	-0.021575	2.558171
107.996742	2116.806285	5.597478	-0.021680	2.562637
108.447209	2124.839465	5.602483	-0.021770	2.567096
108.600404	2132.943423	5.607488	-0.021804	2.571567
108.533217	2141.029051	5.612493	-0.021797	2.576004
108.989756	2149.045349	5.617498	-0.021887	2.580432
109.164218	2157.113690	5.622502	-0.021925	2.584861
109.135981	2165.186235	5.627507	-0.021925	2.589271
109.697125	2173.390912	5.632512	-0.022036	2.593786
110.042786	2181.378993	5.637517	-0.022105	2.598160
110.156376	2189.387585	5.642522	-0.022132	2.602522
110.411795	2197.409579	5.647526	-0.022185	2.606894
110.493286	2205.464818	5.652531	-0.022206	2.611265
110.973693	2213.473094	5.657536	-0.022300	2.615629
111.173286	2221.502094	5.662541	-0.022343	2.619979
111.617922	2229.513069	5.667546	-0.022431	2.624328
111.707077	2237.605348	5.672550	-0.022453	2.628690
111.997380	2245.646187	5.677555	-0.022513	2.633031
112.521851	2253.673369	5.682560	-0.022616	2.637372
112.962142	2261.694703	5.687565	-0.022703	2.641697
112.913222	2269.778440	5.692570	-0.022700	2.646017
113.407955	2277.821574	5.697574	-0.022797	2.650343
113.564519	2285.876468	5.702579	-0.022832	2.654646
114.111748	2293.906174	5.707584	-0.022939	2.658955
114.534736	2301.930874	5.712589	-0.023024	2.663245
114.694610	2309.997887	5.717594	-0.023059	2.667534
114.911870	2318.106409	5.722598	-0.023105	2.671842
115.134868	2326.147671	5.727603	-0.023152	2.676108
115.389783	2334.205135	5.732608	-0.023205	2.680377
115.747235	2342.200343	5.737613	-0.023277	2.684613
116.017873	2350.234330	5.742618	-0.023333	2.688858
116.357314	2358.307967	5.747622	-0.023401	2.693120
116.693163	2366.322356	5.752627	-0.023469	2.697345
116.893152	2374.402850	5.757632	-0.023512	2.701589
117.031802	2382.440792	5.762637	-0.023543	2.705800
117.397836	2390.495209	5.767642	-0.023617	2.710028
117.989162	2398.538453	5.772646	-0.023733	2.714257
117.919024	2406.602791	5.777651	-0.023725	2.718449
118.305145	2414.621503	5.782656	-0.023802	2.722639
118.455215	2422.679108	5.787661	-0.023836	2.726829
118.236055	2430.790093	5.792666	-0.023800	2.731017
118.688111	2438.833118	5.797670	-0.023890	2.735204
118.849821	2446.854781	5.802675	-0.023926	2.739357
119.099419	2454.897100	5.807680	-0.023978	2.743519
119.152506	2462.953757	5.812685	-0.023993	2.747670
119.502503	2471.005245	5.817690	-0.024064	2.751830
120.182079	2479.082062	5.822694	-0.024196	2.756016
120.250637	2487.100720	5.827699	-0.024214	2.760130
120.591796	2495.091460	5.832704	-0.024283	2.764239
121.069692	2503.105788	5.837709	-0.024377	2.768363
121.203503	2511.183002	5.842714	-0.024408	2.772492
121.679953	2519.221291	5.847718	-0.024502	2.776615
121.825026	2527.250856	5.852723	-0.024534	2.780708
122.268877	2535.287711	5.857728	-0.024622	2.784816
122.084185	2543.382613	5.862733	-0.024593	2.788911
122.247061	2551.449002	5.867738	-0.024629	2.793005
122.844085	2559.454814	5.872742	-0.024746	2.797088
122.835637	2567.487588	5.877747	-0.024750	2.801144
123.006044	2575.524380	5.882752	-0.024787	2.805206
123.249218	2583.571987	5.887757	-0.024838	2.809272
123.424136	2591.637383	5.892762	-0.024876	2.813336
123.734062	2599.670420	5.897766	-0.024939	2.817387
124.007534	2607.688213	5.902771	-0.024995	2.821422
124.317020	2615.727253	5.907776	-0.025058	2.825464
124.296419	2623.803815	5.912781	-0.025060	2.829499
124.496428	2631.886153	5.917786	-0.025103	2.833545
125.176747	2639.866557	5.922790	-0.025235	2.837561
125.102829	2647.921769	5.927795	-0.025227	2.841566
125.432422	2655.960764	5.932800	-0.025293	2.845580
125.821532	2663.960493	5.937805	-0.025371	2.849572
126.037725	2672.029668	5.942810	-0.025417	2.853583
126.275197	2680.082038	5.947814	-0.025467	2.857582
126.279958	2688.113252	5.952819	-0.025473	2.861551
126.589460	2696.144142	5.957824	-0.025536	2.865531
127.065054	2704.149977	5.962829	-0.025630	2.869503
127.029956	2712.263138	5.967834	-0.025629	2.873494
127.341648	2720.308080	5.972838	-0.025693	2.877465
127.266249	2728.341344	5.977843	-0.025684	2.881403
127.572799	2736.365927	5.982848	-0.025747	2.885353
128.077277	2744.364329	5.987853	-0.025846	2.889295
128.002677	2752.445949	5.992858	-0.025838	2.893241
128.202344	2760.502389	5.997862	-0.025880	2.897184
128.433971	2768.514464	6.002867	-0.025929	2.901102
128.766311	2776.554612	6.007872	-0.025996	2.905033
129.020177	2784.616426	6.012877	-0.026049	2.908966
129.231266	2792.721680	6.017882	-0.026094	2.912912
129.655713	2800.744990	6.022886	-0.026178	2.916824
129.801903	2808.739506	6.027891	-0.026211	2.920702
129.996386	2816.742674	6.032896	-0.026252	2.924582
130.382944	2824.782811	6.037901	-0.026330	2.928484
130.477752	2832.839171	6.042906	-0.026353	2.932374
130.585224	2840.915288	6.047910	-0.026378	2.936269
130.650242	2848.912616	6.052915	-0.026396	2.940118
131.017951	2856.933786	6.057920	-0.026470	2.943990
131.056970	2864.990269	6.062925	-0.026483	2.947856
131.396863	2873.013069	6.067930	-0.026551	2.951717
131.659415	2881.089525	6.072934	-0.026606	2.955594
131.829993	2889.077446	6.077939	-0.026643	2.959419
132.102686	2897.127014	6.082944	-0.026699	2.963274
132.386558	2905.163724	6.087949	-0.026758	2.967118
132.611466	2913.201582	6.092954	-0.026805	2.970955
132.746297	2921.264197	6.097958	-0.026835	2.974793
133.068671	2929.251456	6.102963	-0.026901	2.978601
133.545499	2937.271526	6.107968	-0.026995	2.982427
133.625996	2945.344996	6.112973	-0.027016	2.986253
133.739486	2953.378455	6.117978	-0.027042	2.990057
134.084499	2961.457864	6.122982	-0.027112	2.993890
134.295592	2969.468591	6.127987	-0.027157	2.997679
135.085339	2977.456955	6.132992	-0.027309	3.001481
135.291187	2985.480256	6.137997	-0.027353	3.005265
135.504716	2993.502337	6.143002	-0.027398	3.009045
135.841799	3001.579567	6.148006	-0.027466	3.012851
136.018094	3009.629394	6.153011	-0.027505	3.016632
136.267633	3017.662398	6.158016	-0.027557	3.020404
136.477655	3025.660925	6.163021	-0.027601	3.024153
136.639213	3033.722056	6.168026	-0.027637	3.027925
136.941240	3041.807518	6.173030	-0.027698	3.031710
136.905971	3049.849744	6.178035	-0.027697	3.035453
137.283139	3057.851731	6.183040	-0.027773	3.039193
137.479477	3065.893927	6.188045	-0.027815	3.042939
137.558988	3073.923199	6.193050	-0.027835	3.046668
137.790445	3081.961520	6.198054	-0.027884	3.050404
137.897335	3089.994296	6.203059	-0.027909	3.054127
138.226012	3098.040509	6.208064	-0.027976	3.057862
138.509002	3106.063532	6.213069	-0.028034	3.061580
138.752273	3114.061233	6.218074	-0.028085	3.065280
139.259380	3122.112998	6.223078	-0.028185	3.069012
139.411660	3130.208970	6.228083	-0.028219	3.072743
139.606802	3138.286031	6.233088	-0.028260	3.076464
139.682502	3146.274145	6.238093	-0.028280	3.080133
139.789487	3154.272068	6.243098	-0.028305	3.083804
140.116047	3162.298311	6.248102	-0.028372	3.087493
140.168878	3170.345572	6.253107	-0.028387	3.091175
140.689798	3178.362131	6.258112	-0.028489	3.094861
140.811482	3186.397172	6.263117	-0.028517	3.098531
141.216992	3194.381780	6.268122	-0.028598	3.102188
141.319516	3202.460608	6.273126	-0.028623	3.105869
141.632375	3210.464132	6.278131	-0.028687	3.109521
141.451523	3218.580862	6.283136	-0.028658	3.113198
141.777942	3226.602155	6.288141	-0.028725	3.116850
141.983280	3234.595407	6.293146	-0.028768	3.120480
142.142785	3242.633006	6.298150	-0.028803	3.124123
142.450659	3250.653633	6.303155	-0.028866	3.127761
142.748902	3258.701324	6.308160	-0.028927	3.131407
142.980061	3266.734679	6.313165	-0.028976	3.135039
142.985157	3274.767814	6.318170	-0.028982	3.138656
143.241443	3282.796663	6.323174	-0.029035	3.142279
143.499371	3290.813197	6.328179	-0.029089	3.145891
143.851048	3298.845225	6.333184	-0.029160	3.149511
143.877706	3306.933751	6.338189	-0.029170	3.153137
144.275405	3314.949396	6.343194	-0.029250	3.156743
144.405962	3322.968263	6.348198	-0.029279	3.160335
144.693554	3330.948910	6.353203	-0.029338	3.163912
145.129864	3338.981047	6.358208	-0.029425	3.167515
145.379617	3347.031477	6.363213	-0.029477	3.171113
145.136015	3355.119838	6.368218	-0.029437	3.174703
145.495401	3363.142318	6.373222	-0.029510	3.178286
145.618973	3371.158013	6.378227	-0.029538	3.181851
145.844683	3379.172972	6.383232	-0.029586	3.185416
146.074001	3387.212193	6.388237	-0.029634	3.188988
146.345585	3395.241694	6.393242	-0.029690	3.192554
146.600087	3403.308790	6.398246	-0.029743	3.196131
146.668597	3411.285337	6.403251	-0.029761	3.199657
146.990221	3419.292013	6.408256	-0.029826	3.203203
147.260353	3427.350885	6.413261	-0.029882	3.206765
147.470335	3435.386934	6.418266	-0.029926	3.210311
147.689003	3443.434002	6.423270	-0.029973	3.213859
147.946674	3451.456532	6.428275	-0.030026	3.217393
148.196538	3459.501567	6.433280	-0.030078	3.220932
148.078504	3467.507390	6.438285	-0.030062	3.224436
148.363663	3475.543374	6.443290	-0.030120	3.227965
148.655379	3483.636981	6.448294	-0.030180	3.231516
148.748522	3491.678760	6.453299	-0.030203	3.235033
149.011865	3499.667697	6.458304	-0.030257	3.238529
149.353798	3507.665278	6.463309	-0.030326	3.242028
149.523313	3515.676159	6.468314	-0.030363	3.245523
149.659533	3523.708897	6.473318	-0.030394	3.249022
149.792264	3531.746375	6.478323	-0.030424	3.252519
150.003017	3539.831467	6.483328	-0.030469	3.256036
150.171887	3547.809635	6.488333	-0.030506	3.259501
150.490525	3555.805024	6.493338	-0.030571	3.262975
150.819536	3563.883254	6.498342	-0.030637	3.266483
150.713299	3571.909553	6.503347	-0.030623	3.269947
150.931662	3579.961086	6.508352	-0.030669	3.273430
151.337098	3587.978237	6.513357	-0.030750	3.276903
151.311490	3595.980795	6.518362	-0.030751	3.280349
151.751663	3604.017154	6.523366	-0.030838	3.283824
152.137276	3612.009028	6.528371	-0.030915	3.287273
152.559275	3620.046958	6.533376	-0.030999	3.290741
152.372266	3628.130095	6.538381	-0.030970	3.294200
152.795824	3636.137736	6.543386	-0.031054	3.297647
153.068524	3644.170384	6.548390	-0.031111	3.301095
153.153655	3652.173519	6.553395	-0.031132	3.304520
153.415484	3660.213148	6.558400	-0.031186	3.307964
153.545850	3668.301528	6.563405	-0.031216	3.311420
153.790345	3676.338466	6.568410	-0.031267	3.314854
154.035295	3684.346407	6.573414	-0.031318	3.318273
154.250742	3692.322004	6.578419	-0.031364	3.321673
154.493482	3700.347591	6.583424	-0.031414	3.325092
154.578904	3708.379938	6.588429	-0.031436	3.328504
154.839689	3716.418454	6.593434	-0.031490	3.331922
155.167777	3724.475692	6.598438	-0.031556	3.335347
155.201949	3732.479930	6.603443	-0.031568	3.338735
155.483230	3740.504785	6.608448	-0.031626	3.342137
155.988953	3748.506611	6.613453	-0.031725	3.345535
155.924051	3756.572241	6.618458	-0.031719	3.348934
156.017529	3764.641974	6.623462	-0.031742	3.352338
156.145378	3772.682118	6.628467	-0.031771	3.355728
156.436417	3780.665890	6.633472	-0.031831	3.359096
156.714503	3788.671574	6.638477	-0.031888	3.362469
157.004959	3796.687354	6.643482	-0.031947	3.365844
157.318880	3804.727941	6.648486	-0.032011	3.369226
157.761190	3812.759839	6.653491	-0.032099	3.372606
157.721404	3820.838837	6.658496	-0.032097	3.375985
157.889807	3828.823035	6.663501	-0.032134	3.379328
158.043772	3836.845624	6.668506	-0.032168	3.382684
158.184658	3844.892341	6.673510	-0.032200	3.386045
158.336614	3852.912467	6.678515	-0.032233	3.389393
158.569107	3861.014098	6.683520	-0.032282	3.392774
158.725521	3869.085259	6.688525	-0.032317	3.396137
158.770657	3877.010698	6.693530	-0.032331	3.399431
159.334122	3884.997579	6.698534	-0.032441	3.402766
159.395502	3893.023911	6.703539	-0.032458	3.406097
159.333896	3901.057064	6.708544	-0.032452	3.409423
159.626805	3909.094259	6.713549	-0.032512	3.412759
160.048553	3917.125015	6.718554	-0.032596	3.416094
160.233096	3925.142595	6.723558	-0.032636	3.419412
160.357986	3933.141185	6.728563	-0.032664	3.422717
160.790325	3941.170013	6.733568	-0.032750	3.426042
161.030602	3949.177108	6.738573	-0.032801	3.429348
161.161573	3957.264767	6.743578	-0.032830	3.432680
161.483694	3965.316626	6.748582	-0.032896	3.436000
161.448446	3973.292979	6.753587	-0.032895	3.439275
161.698716	3981.319191	6.758592	-0.032947	3.442576
161.789996	3989.347072	6.763597	-0.032969	3.445869
161.987720	3997.371022	6.768602	-0.033011	3.449161
162.023126	4005.471576	6.773606	-0.033024	3.452476
162.150495	4013.473179	6.778611	-0.033053	3.455751
162.618983	4021.473402	6.783616	-0.033145	3.459033
162.687925	4029.513460	6.788621	-0.033164	3.462314
162.871015	4037.500709	6.793626	-0.033203	3.465575
163.115232	4045.579694	6.798630	-0.033254	3.468872
163.382308	4053.602468	6.803635	-0.033309	3.472144
163.443133	4061.660065	6.808640	-0.033326	3.475421
163.808299	4069.644281	6.813645	-0.033400	3.478674
163.949431	4077.639201	6.818650	-0.033431	3.481921
164.000570	4085.687287	6.823654	-0.033446	3.485184
163.836652	4093.711233	6.828659	-0.033421	3.488427
164.402943	4101.717789	6.833664	-0.033532	3.491683
164.615013	4109.767510	6.838669	-0.033577	3.494942
164.620763	4117.774398	6.843674	-0.033584	3.498175
164.742879	4125.824568	6.848678	-0.033612	3.501426
165.003267	4133.766909	6.853683	-0.033666	3.504634
165.191232	4141.839417	6.858688	-0.033706	3.507890
165.273854	4149.908236	6.863693	-0.033727	3.511138
165.479779	4157.924552	6.868698	-0.033771	3.514365
165.960116	4165.930374	6.873702	-0.033866	3.517594
165.807050	4173.975174	6.878707	-0.033843	3.520816
166.282456	4181.915337	6.883712	-0.033937	3.524012
166.332278	4189.995237	6.888717	-0.033951	3.527248
166.392471	4198.020109	6.893722	-0.033968	3.530460
166.740641	4206.088325	6.898726	-0.034038	3.533695
167.081215	4214.088788	6.903731	-0.034107	3.536899
167.141292	4222.098256	6.908736	-0.034124	3.540096
167.235264	4230.153987	6.913741	-0.034147	3.543309
167.563226	4238.183830	6.918746	-0.034213	3.546516
167.689451	4246.227563	6.923750	-0.034242	3.549719
167.861207	4254.287017	6.928755	-0.034280	3.552927
168.178196	4262.349320	6.933760	-0.034344	3.556138
168.259634	4270.318456	6.938765	-0.034365	3.559302
168.339517	4278.309028	6.943770	-0.034385	3.562471
168.513081	4286.334541	6.948774	-0.034423	3.565655
168.755071	4294.323587	6.953779	-0.034473	3.568822
168.930035	4302.372185	6.958784	-0.034511	3.572009
168.935740	4310.414367	6.963789	-0.034518	3.575185
169.334823	4318.382707	6.968794	-0.034598	3.578341
169.641219	4326.447425	6.973798	-0.034660	3.581529
169.606624	4334.420567	6.978803	-0.034659	3.584669
169.915967	4342.463051	6.983808	-0.034722	3.587843
170.040499	4350.519022	6.988813	-0.034751	3.591014
170.422104	4358.507183	6.993818	-0.034827	3.594163
170.666696	4366.564909	6.998822	-0.034878	3.597332
170.871971	4374.549844	7.003827	-0.034922	3.600469
170.706975	4382.593846	7.008832	-0.034897	3.603616
170.892201	4390.618227	7.013837	-0.034937	3.606762
171.111410	4398.604163	7.018842	-0.034983	3.609892
171.364128	4406.679483	7.023846	-0.035036	3.613054
171.356023	4414.722859	7.028851	-0.035039	3.616194
171.564666	4422.681066	7.033856	-0.035084	3.619305
171.872788	4430.724165	7.038861	-0.035147	3.622448
172.083587	4438.706634	7.043866	-0.035191	3.625562
172.463464	4446.765314	7.048870	-0.035267	3.628708
172.569182	4454.814949	7.053875	-0.035293	3.631840
173.054939	4462.870067	7.058880	-0.035389	3.634981
172.894856	4470.906375	7.063885	-0.035364	3.638096
173.174827	4478.908575	7.068890	-0.035422	3.641206
173.313585	4486.900889	7.073894	-0.035453	3.644306
173.417914	4494.924236	7.078899	-0.035478	3.647414
173.661863	4502.960243	7.083904	-0.035529	3.650528
174.028517	4511.009384	7.088909	-0.035603	3.653648
174.120642	4519.020395	7.093914	-0.035625	3.656743
174.344649	4527.068946	7.098918	-0.035672	3.659854
174.421897	4535.063903	7.103923	-0.035692	3.662937
174.551801	4543.085597	7.108928	-0.035722	3.666029
174.847035	4551.094859	7.113933	-0.035782	3.669118
174.964142	4559.123804	7.118938	-0.035809	3.672208
175.412460	4567.179642	7.123942	-0.035898	3.675314
175.302102	4575.189524	7.128947	-0.035883	3.678385
175.354740	4583.198449	7.133952	-0.035899	3.681457
175.990188	4591.165562	7.138957	-0.036022	3.684526
176.018414	4599.244319	7.143962	-0.036033	3.687619
175.955711	4607.313842	7.148966	-0.036027	3.690704
176.185479	4615.288275	7.153971	-0.036075	3.693757
176.585002	4623.317973	7.158976	-0.036155	3.696833
176.750796	4631.321557	7.163981	-0.036191	3.699891
176.838184	4639.323854	7.168986	-0.036213	3.702944
177.078534	4647.399921	7.173990	-0.036263	3.706026
177.353599	4655.377983	7.178995	-0.036320	3.709069
177.447945	4663.480384	7.184000	-0.036343	3.712152
177.611584	4671.538240	7.189005	-0.036379	3.715218
177.517365	4679.506709	7.194010	-0.036367	3.718240
177.942232	4687.544667	7.199014	-0.036451	3.721300
178.079405	4695.447136	7.204019	-0.036482	3.724298
178.619176	4703.511819	7.209024	-0.036588	3.727365
178.658248	4711.568168	7.214029	-0.036601	3.730414
178.637395	4719.559754	7.219034	-0.036602	3.733435
178.935128	4727.614575	7.224038	-0.036663	3.736485
179.164419	4735.601817	7.229043	-0.036711	3.739505
179.340025	4743.638746	7.234048	-0.036750	3.742540
179.728309	4751.649910	7.239053	-0.036827	3.745568
179.767319	4759.671280	7.244058	-0.036840	3.748590
180.070309	4767.740008	7.249062	-0.036902	3.751632
180.010512	4775.798872	7.254067	-0.036896	3.754660
180.263503	4783.807471	7.259072	-0.036949	3.757674
180.695267	4791.794959	7.264077	-0.037035	3.760682
180.430375	4799.779358	7.269082	-0.036991	3.763670
180.728176	4807.844734	7.274086	-0.037052	3.766699
180.897354	4815.836165	7.279091	-0.037089	3.769695
181.125236	4823.881390	7.284096	-0.037137	3.772710
181.229208	4831.958219	7.289101	-0.037161	3.775731
181.357309	4839.926387	7.294106	-0.037191	3.778710
181.404035	4847.985314	7.299110	-0.037205	3.781719
181.667165	4855.941371	7.304115	-0.037259	3.784692
182.020934	4863.985553	7.309120	-0.037331	3.787697
182.154929	4872.032623	7.314125	-0.037361	3.790696
182.051045	4880.090205	7.319130	-0.037347	3.793691
182.454072	4888.136671	7.324134	-0.037428	3.796691
182.418367	4896.075181	7.329139	-0.037426	3.799639
182.548019	4904.094262	7.334144	-0.037456	3.802618
182.974136	4912.093029	7.339149	-0.037541	3.805594
183.195736	4920.114429	7.344154	-0.037587	3.808571
183.397870	4928.158528	7.349158	-0.037631	3.811554
183.273561	4936.172278	7.354163	-0.037613	3.814516
183.519366	4944.186826	7.359168	-0.037664	3.817484
183.854533	4952.223705	7.364173	-0.037732	3.820460
183.967281	4960.207029	7.369178	-0.037758	3.823409
184.194172	4968.266243	7.374182	-0.037806	3.826386
184.561994	4976.228868	7.379187	-0.037880	3.829328
184.663363	4984.312191	7.384192	-0.037904	3.832307
184.896886	4992.340031	7.389197	-0.037953	3.835265
184.829606	5000.332576	7.394202	-0.037946	3.838203
185.281664	5008.371663	7.399206	-0.038036	3.841165
185.378988	5016.323078	7.404211	-0.038059	3.844086
185.646573	5024.372382	7.409216	-0.038115	3.847044
185.991191	5032.407518	7.414221	-0.038184	3.849997
185.968053	5040.464303	7.419226	-0.038185	3.852947
186.147460	5048.527137	7.424230	-0.038224	3.855901
186.329802	5056.488464	7.429235	-0.038264	3.858816
186.405876	5064.515589	7.434240	-0.038283	3.861751
186.602562	5072.529420	7.439245	-0.038325	3.864681
186.921823	5080.567557	7.444250	-0.038390	3.867620
187.069167	5088.606744	7.449254	-0.038423	3.870554
187.074382	5096.852713	7.454259	-0.038430	3.873558
187.366030	5104.827067	7.459264	-0.038490	3.876466
187.592020	5112.724351	7.464269	-0.038537	3.879343
187.673765	5120.714394	7.469274	-0.038558	3.882249
187.901440	5128.718146	7.474278	-0.038605	3.885160
188.028647	5136.717004	7.479283	-0.038635	3.888065
188.158542	5144.741573	7.484288	-0.038664	3.890978
188.307850	5152.788430	7.489293	-0.038697	3.893897
188.511670	5160.822138	7.494298	-0.038741	3.896809
188.663268	5168.802542	7.499302	-0.038775	3.899700
188.841624	5176.821230	7.504307	-0.038813	3.902602
189.089066	5184.820761	7.509312	-0.038865	3.905497
189.348077	5192.864672	7.514317	-0.038918	3.908406
189.331878	5200.903812	7.519322	-0.038921	3.911306
189.732889	5208.916171	7.524326	-0.039001	3.914201
189.810563	5216.939090	7.529331	-0.039021	3.917092
189.975739	5224.909707	7.534336	-0.039057	3.919964
190.247883	5232.947666	7.539341	-0.039113	3.922860
190.553683	5240.928282	7.544346	-0.039176	3.925734
190.697019	5249.016144	7.549350	-0.039208	3.928641
190.791067	5257.020295	7.554355	-0.039231	3.931516
190.914157	5265.031508	7.559360	-0.039259	3.934391
191.251200	5273.060618	7.564365	-0.039327	3.937274
191.238139	5281.059974	7.569370	-0.039330	3.940138
191.557667	5289.119376	7.574374	-0.039395	3.943027
191.788297	5297.101870	7.579379	-0.039444	3.945885
191.931948	5305.103274	7.584384	-0.039476	3.948747
192.040879	5313.177859	7.589389	-0.039502	3.951632
192.005924	5321.212890	7.594394	-0.039501	3.954498
192.192395	5329.233352	7.599398	-0.039541	3.957360
192.280898	5337.204832	7.604403	-0.039563	3.960201
192.641285	5345.199688	7.609408	-0.039635	3.963054
192.505364	5353.248865	7.614413	-0.039615	3.965915
192.850250	5361.211414	7.619418	-0.039685	3.968751
193.003711	5369.321689	7.624422	-0.039719	3.971635
193.119808	5377.313881	7.629427	-0.039746	3.974473
193.484668	5385.329157	7.634432	-0.039819	3.977322
193.559347	5393.350767	7.639437	-0.039839	3.980167
193.585380	5401.348689	7.644442	-0.039849	3.983000
194.148329	5409.400530	7.649446	-0.039959	3.985859
194.060637	5417.375579	7.654451	-0.039948	3.988678
194.159635	5425.477508	7.659456	-0.039972	3.991544
194.653805	5433.483105	7.664461	-0.040070	3.994379
194.805790	5441.483746	7.669466	-0.040104	3.997205
194.802975	5449.508700	7.674470	-0.040109	4.000035
194.960234	5457.510799	7.679475	-0.040143	4.002858
195.114701	5465.528501	7.684480	-0.040177	4.005684
195.207658	5473.578672	7.689485	-0.040200	4.008518
195.401087	5481.609653	7.694490	-0.040242	4.011345
195.827513	5489.643979	7.699494	-0.040327	4.014176
195.785195	5497.682779	7.704499	-0.040324	4.016998
196.066991	5505.605180	7.709504	-0.040382	4.019782
196.294927	5513.672728	7.714509	-0.040430	4.022615
196.333179	5521.656356	7.719514	-0.040442	4.025413
196.337459	5529.738911	7.724518	-0.040449	4.028244
196.740364	5537.764298	7.729523	-0.040529	4.031058
196.959894	5545.864148	7.734528	-0.040576	4.033894
196.911175	5553.860706	7.739533	-0.040572	4.036687
197.206402	5561.759485	7.744538	-0.040632	4.039450
197.497301	5569.817030	7.749542	-0.040692	4.042266
197.639034	5577.786359	7.754547	-0.040724	4.045047
197.652122	5585.833905	7.759552	-0.040732	4.047852
197.756960	5593.861653	7.764557	-0.040757	4.050649
197.960363	5601.883686	7.769562	-0.040800	4.053443
198.003809	5609.925213	7.774566	-0.040814	4.056240
198.327715	5617.860001	7.779571	-0.040879	4.059002
198.457649	5625.914484	7.784576	-0.040909	4.061801
198.746498	5633.917643	7.789581	-0.040968	4.064582
198.989215	5641.968830	7.794586	-0.041019	4.067378
199.199174	5649.973829	7.799590	-0.041063	4.070155
199.373320	5658.012899	7.804595	-0.041101	4.072941
199.391593	5666.019631	7.809600	-0.041110	4.075712
199.662134	5674.025298	7.814605	-0.041166	4.078485
199.900196	5682.051388	7.819610	-0.041216	4.081262
200.066940	5690.034344	7.824614	-0.041252	4.084021
200.111336	5698.062915	7.829619	-0.041266	4.086792
200.290795	5706.050888	7.834624	-0.041305	4.089550
200.340906	5714.175366	7.839629	-0.041320	4.092351
200.321146	5722.180309	7.844634	-0.041321	4.095107
200.633373	5730.192270	7.849638	-0.041385	4.097869
201.050139	5738.179401	7.854643	-0.041468	4.100622
200.954750	5746.175415	7.859648	-0.041456	4.103369
201.419025	5754.218995	7.864653	-0.041547	4.106138
201.622220	5762.244475	7.869658	-0.041591	4.108895
201.751584	5770.308281	7.874662	-0.041620	4.111663
201.805417	5778.327583	7.879667	-0.041636	4.114412
202.160446	5786.371079	7.884672	-0.041707	4.117172
202.469522	5794.355240	7.889677	-0.041770	4.119909
202.339557	5802.349259	7.894682	-0.041752	4.122642
202.748613	5810.376158	7.899686	-0.041833	4.125391
202.794951	5818.396301	7.904691	-0.041847	4.128132
203.038378	5826.416436	7.909696	-0.041898	4.130873
203.118215	5834.476323	7.914701	-0.041918	4.133624
203.335423	5842.472540	7.919706	-0.041964	4.136353
203.342413	5850.484435	7.924710	-0.041971	4.139083
203.483099	5858.464751	7.929715	-0.042003	4.141801
203.676185	5866.474214	7.934720	-0.042044	4.144529
203.645824	5874.543776	7.939725	-0.042044	4.147273
203.531271	5882.550870	7.944730	-0.042028	4.149992
204.018672	5890.589044	7.949734	-0.042124	4.152728
204.189498	5898.640968	7.954739	-0.042161	4.155462
204.172103	5906.591510	7.959744	-0.042164	4.158159
204.516173	5914.622333	7.964749	-0.042233	4.160884
204.892657	5922.561568	7.969754	-0.042309	4.163578
204.796487	5930.660565	7.974758	-0.042296	4.166318
204.949818	5938.665952	7.979763	-0.042330	4.169028
205.308407	5946.717768	7.984768	-0.042403	4.171753
205.578446	5954.777039	7.989773	-0.042458	4.174479
205.614294	5962.747705	7.994778	-0.042470	4.177170
205.892278	5970.752574	7.999782	-0.042528	4.179874
206.062088	5978.765368	8.004787	-0.042565	4.182577
206.198991	5986.718686	8.009792	-0.042596	4.185258
206.453789	5994.798562	8.014797	-0.042648	4.187982
206.427424	6002.834396	8.019802	-0.042649	4.190685
206.470393	6010.948424	8.024806	-0.042663	4.193414
206.729519	6018.981890	8.029811	-0.042716	4.196117
206.946800	6026.875042	8.034816	-0.042762	4.198770
207.247471	6034.925129	8.039821	-0.042823	4.201474
207.042071	6042.847364	8.044826	-0.042791	4.204129
207.244352	6050.894177	8.049830	-0.042834	4.206829
207.664886	6058.890102	8.054835	-0.042918	4.209511
207.650716	6066.944752	8.059840	-0.042920	4.212208
207.960357	6074.984431	8.064845	-0.042983	4.214900
208.070677	6082.957886	8.069850	-0.043009	4.217567
208.279564	6090.958714	8.074854	-0.043054	4.220242
208.474680	6098.994118	8.079859	-0.043096	4.222927
208.447725	6106.981417	8.084864	-0.043096	4.225592
208.700061	6115.061043	8.089869	-0.043148	4.228289
208.889704	6123.036258	8.094874	-0.043189	4.230949
208.975417	6131.161196	8.099878	-0.043211	4.233655
209.358436	6139.172062	8.104883	-0.043287	4.236325
209.460340	6147.132370	8.109888	-0.043312	4.238974
209.393982	6155.156995	8.114893	-0.043305	4.241641
209.639420	6163.074410	8.119898	-0.043356	4.244273
209.828678	6171.166811	8.124902	-0.043397	4.246962
209.875555	6179.167684	8.129907	-0.043411	4.249617
209.930764	6187.220451	8.134912	-0.043427	4.252287
210.073434	6195.255167	8.139917	-0.043459	4.254951
210.414771	6203.258428	8.144922	-0.043528	4.257604
210.580996	6211.292345	8.149926	-0.043564	4.260265
210.691571	6219.290368	8.154931	-0.043590	4.262911
210.940182	6227.311450	8.159936	-0.043642	4.265564
210.885773	6235.373105	8.164941	-0.043637	4.268227
210.963197	6243.366295	8.169946	-0.043657	4.270866
211.283161	6251.435743	8.174950	-0.043722	4.273531
211.371959	6259.465222	8.179955	-0.043744	4.276179
211.422151	6267.402147	8.184960	-0.043759	4.278795
211.757318	6275.454262	8.189965	-0.043827	4.281449
211.856629	6283.361876	8.194970	-0.043851	4.284052
212.016295	6291.480781	8.199974	-0.043886	4.286724
212.060528	6299.466137	8.204979	-0.043899	4.289349
212.339973	6307.547548	8.209984	-0.043957	4.292005
212.525917	6315.568846	8.214989	-0.043997	4.294640
212.615159	6323.568957	8.219994	-0.044019	4.297265
212.821933	6331.567345	8.224998	-0.044063	4.299889
213.173260	6339.560564	8.230003	-0.044134	4.302511
213.582152	6347.566973	8.235008	-0.044215	4.305136
213.857128	6355.637912	8.240013	-0.044272	4.307780
213.874731	6363.641664	8.245018	-0.044281	4.310397
214.042200	6371.686940	8.250022	-0.044318	4.313028
214.243333	6379.687669	8.255027	-0.044360	4.315643
214.466952	6387.678477	8.260032	-0.044407	4.318254
214.215312	6395.720410	8.265037	-0.044366	4.320875
214.288857	6403.646806	8.270042	-0.044385	4.323461
214.524810	6411.743993	8.275046	-0.044435	4.326101
214.771342	6419.715579	8.280051	-0.044486	4.328699
214.729839	6427.779929	8.285056	-0.044484	4.331323
215.103371	6435.836313	8.290061	-0.044559	4.333946
215.303931	6443.798661	8.295066	-0.044601	4.336536
215.453421	6451.778481	8.300070	-0.044635	4.339129
215.587491	6459.815409	8.305075	-0.044665	4.341740
215.797427	6467.770953	8.310080	-0.044710	4.344322
215.761416	6475.890506	8.315085	-0.044708	4.346955
216.060742	6483.860657	8.320090	-0.044770	4.349540
216.286032	6491.935531	8.325094	-0.044817	4.352157
216.412196	6499.985522	8.330099	-0.044846	4.354764
216.639965	6507.995893	8.335104	-0.044894	4.357356
216.825191	6515.975269	8.340109	-0.044934	4.359937
216.761093	6523.945968	8.345114	-0.044927	4.362512
216.945970	6531.912668	8.350118	-0.044967	4.365086
217.093764	6539.980662	8.355123	-0.045000	4.367691
217.413035	6547.970889	8.360128	-0.045065	4.370270
217.445423	6556.016896	8.365133	-0.045076	4.372864
217.508103	6564.053565	8.370138	-0.045094	4.375453
218.157297	6572.071632	8.375142	-0.045220	4.378038
218.185756	6580.012828	8.380147	-0.045231	4.380594
217.879442	6588.054051	8.385152	-0.045179	4.383178
218.246086	6596.102496	8.390157	-0.045253	4.385767
218.396265	6604.065352	8.395162	-0.045286	4.388325
218.630417	6612.108316	8.400166	-0.045335	4.390908
218.616628	6620.136052	8.405171	-0.045338	4.393484
218.694454	6628.216616	8.410176	-0.045358	4.396075
218.949795	6636.223956	8.415181	-0.045411	4.398642
218.928874	6644.208500	8.420186	-0.045413	4.401199
219.240170	6652.201980	8.425190	-0.045476	4.403759
219.154455	6660.240867	8.430195	-0.045466	4.406330
219.337655	6668.275221	8.435200	-0.045505	4.408899
219.612058	6676.300188	8.440205	-0.045562	4.411465
219.712927	6684.286697	8.445210	-0.045586	4.414015
219.733867	6692.347611	8.450214	-0.045595	4.416588
219.908762	6700.329619	8.455219	-0.045633	4.419135
220.366981	6708.374738	8.460224	-0.045724	4.421701
220.250217	6716.332311	8.465229	-0.045708	4.424236
220.108979	6724.381085	8.470234	-0.045687	4.426798
220.583658	6732.408858	8.475238	-0.045781	4.429354
220.647258	6740.452257	8.480243	-0.045798	4.431912
220.808346	6748.494049	8.485248	-0.045833	4.434469
220.972051	6756.529702	8.490253	-0.045869	4.437022
221.202776	6764.436335	8.495258	-0.045918	4.439533
221.399883	6772.509421	8.500262	-0.045960	4.442095
221.255717	6780.481500	8.505267	-0.045939	4.444623
221.353512	6788.522882	8.510272	-0.045962	4.447171
221.648363	6796.551584	8.515277	-0.046023	4.449716
221.708587	6804.593917	8.520282	-0.046039	4.452262
221.861194	6812.618997	8.525286	-0.046073	4.454801
222.085110	6820.622162	8.530291	-0.046120	4.457332
222.134258	6828.595534	8.535296	-0.046135	4.459852
222.468990	6836.666929	8.540301	-0.046203	4.462402
222.434788	6844.651455	8.545306	-0.046202	4.464923
222.679742	6852.662003	8.550310	-0.046253	4.467450
222.665322	6860.668260	8.555315	-0.046255	4.469975
223.068541	6868.701130	8.560320	-0.046336	4.472507
223.027128	6876.754519	8.565325	-0.046334	4.475043
222.987811	6884.718185	8.570330	-0.046332	4.477549
223.298939	6892.722298	8.575335	-0.046395	4.480068
223.644831	6900.756512	8.580339	-0.046465	4.482595
223.542202	6908.717493	8.585344	-0.046451	4.485096
223.489552	6916.830560	8.590349	-0.046447	4.487644
223.750724	6924.795885	8.595354	-0.046501	4.490145
224.002912	6932.865407	8.600359	-0.046554	4.492677
223.980455	6940.862490	8.605363	-0.046555	4.495183
224.174450	6948.859044	8.610368	-0.046596	4.497690
224.304116	6956.866709	8.615373	-0.046626	4.500197
224.656704	6964.888900	8.620378	-0.046697	4.502709
224.756620	6972.885957	8.625383	-0.046721	4.505211
224.962725	6980.910582	8.630387	-0.046765	4.507720
225.030639	6988.933914	8.635392	-0.046783	4.510227
225.184102	6997.036061	8.640397	-0.046817	4.512757
225.278302	7005.019211	8.645402	-0.046840	4.515249
225.457595	7013.032193	8.650407	-0.046879	4.517749
225.137149	7021.009359	8.655411	-0.046825	4.520235
225.257162	7028.945487	8.660416	-0.046852	4.522708
225.631755	7036.968444	8.665421	-0.046928	4.525207
225.728575	7045.003933	8.670426	-0.046951	4.527708
225.714536	7053.028592	8.675431	-0.046954	4.530204
225.960269	7061.086120	8.680435	-0.047005	4.532709
226.062383	7069.083790	8.685440	-0.047030	4.535194
226.229859	7077.141810	8.690445	-0.047066	4.537697
226.191410	7085.074769	8.695450	-0.047065	4.540159
226.591868	7093.088032	8.700455	-0.047145	4.542645
226.589595	7101.081895	8.705459	-0.047150	4.545124
226.553404	7109.095428	8.710464	-0.047148	4.547607
227.080100	7117.187070	8.715469	-0.047252	4.550113
227.157295	7125.200867	8.720474	-0.047272	4.552594
227.143466	7133.247774	8.725479	-0.047275	4.555083
227.541649	7141.222453	8.730483	-0.047354	4.557549
227.580304	7149.214308	8.735488	-0.047367	4.560018
227.746304	7157.245377	8.740493	-0.047403	4.562499
227.703228	7165.220007	8.745498	-0.047400	4.564960
227.956617	7173.313209	8.750503	-0.047453	4.567457
227.941649	7181.296449	8.755507	-0.047456	4.569919
227.914818	7189.330652	8.760512	-0.047456	4.572394
228.154913	7197.389643	8.765517	-0.047506	4.574877
228.120751	7205.384954	8.770522	-0.047506	4.577338
228.332255	7213.371688	8.775527	-0.047550	4.579795
228.762555	7221.429257	8.780531	-0.047636	4.582273
229.102424	7229.387936	8.785536	-0.047705	4.584719
228.987005	7237.485215	8.790541	-0.047689	4.587206
229.066704	7245.434880	8.795546	-0.047709	4.589647
229.496954	7253.536768	8.800551	-0.047794	4.592133
229.581138	7261.529738	8.805555	-0.047816	4.594584
229.708231	7269.523897	8.810560	-0.047845	4.597034
229.800146	7277.493878	8.815565	-0.047867	4.599475
229.878719	7285.563013	8.820570	-0.047887	4.601946
230.140151	7293.513895	8.825575	-0.047941	4.604379
230.271935	7301.560060	8.830579	-0.047971	4.606839
230.535063	7309.543092	8.835584	-0.048026	4.609280
230.698280	7317.620450	8.840589	-0.048062	4.611747
230.632683	7325.644953	8.845594	-0.048055	4.614197
230.844990	7333.694197	8.850599	-0.048100	4.616654
230.802379	7341.625906	8.855603	-0.048097	4.619073
230.777253	7349.629384	8.860608	-0.048098	4.621513
231.003145	7357.637259	8.865613	-0.048146	4.623953
231.254620	7365.671018	8.870618	-0.048198	4.626399
231.242205	7373.695514	8.875623	-0.048201	4.628841
231.413257	7381.727564	8.880627	-0.048238	4.631285
231.732467	7389.787771	8.885632	-0.048303	4.633735
231.652332	7397.811637	8.890637	-0.048294	4.636173
231.879941	7405.740536	8.895642	-0.048342	4.638581
232.093446	7413.769297	8.900647	-0.048387	4.641018
232.238211	7421.751779	8.905651	-0.048419	4.643440
232.135421	7429.773935	8.910656	-0.048406	4.645873
232.235585	7437.812132	8.915661	-0.048430	4.648309
232.343211	7445.874201	8.920666	-0.048455	4.650751
232.539342	7453.889251	8.925671	-0.048497	4.653177
232.515815	7461.915088	8.930675	-0.048498	4.655606
232.765334	7469.848985	8.935680	-0.048550	4.658005
232.988101	7477.873760	8.940685	-0.048597	4.660431
233.047799	7485.893922	8.945690	-0.048614	4.662854
233.418495	7493.892639	8.950695	-0.048688	4.665269
233.346405	7501.938293	8.955699	-0.048680	4.667697
233.590221	7509.952230	8.960704	-0.048731	4.670114
233.696273	7518.097196	8.965709	-0.048756	4.672569
233.697759	7526.087436	8.970714	-0.048762	4.674977
233.801101	7534.070904	8.975719	-0.048787	4.677381
233.760558	7541.988279	8.980723	-0.048784	4.679765
234.118829	7550.025990	8.985728	-0.048857	4.682182
234.221416	7558.015699	8.990733	-0.048881	4.684585
234.272917	7566.035239	8.995738	-0.048896	4.686995
234.429437	7574.057479	9.000743	-0.048931	4.689405
234.567171	7582.087960	9.005747	-0.048962	4.691815
234.473985	7590.068099	9.010752	-0.048950	4.694210
234.740460	7598.164995	9.015757	-0.049005	4.696638
234.763351	7606.087465	9.020762	-0.049015	4.699013
234.980352	7614.165384	9.025767	-0.049061	4.701433
235.071232	7622.109014	9.030771	-0.049083	4.703812
235.240507	7630.177261	9.035776	-0.049120	4.706226
235.340918	7638.219982	9.040781	-0.049144	4.708632
235.416711	7646.192521	9.045786	-0.049164	4.711016
235.690941	7654.304451	9.050791	-0.049220	4.713439
235.809257	7662.313819	9.055795	-0.049248	4.715831
235.862683	7670.247273	9.060800	-0.049263	4.718200
236.152814	7678.307098	9.065805	-0.049322	4.720604
236.162357	7686.293333	9.070810	-0.049330	4.722986
236.323458	7694.301714	9.075815	-0.049365	4.725372
236.173833	7702.336559	9.080819	-0.049343	4.727767
236.305644	7710.322449	9.085824	-0.049373	4.730144
236.560781	7718.402762	9.090829	-0.049426	4.732549
236.528390	7726.416289	9.095834	-0.049425	4.734933
236.639658	7734.425809	9.100839	-0.049451	4.737314
236.844888	7742.430894	9.105843	-0.049495	4.739692
236.914884	7750.428192	9.110848	-0.049513	4.742067
237.254273	7758.441806	9.115853	-0.049582	4.744445
237.219101	7766.486127	9.120858	-0.049581	4.746833
237.655991	7774.464831	9.125863	-0.049668	4.749197
237.673528	7782.487324	9.130867	-0.049676	4.751575
237.683400	7790.559087	9.135872	-0.049684	4.753967
237.984160	7798.561257	9.140877	-0.049745	4.756336
237.947782	7806.508773	9.145882	-0.049744	4.758688
238.186752	7814.529959	9.150887	-0.049794	4.761060
238.176793	7822.549098	9.155891	-0.049797	4.763431
238.226574	7830.550775	9.160896	-0.049812	4.765796
238.570866	7838.570663	9.165901	-0.049882	4.768164
238.656809	7846.577685	9.170906	-0.049903	4.770527
238.741628	7854.628918	9.175911	-0.049924	4.772903
239.039860	7862.686966	9.180915	-0.049985	4.775278
239.074142	7870.625980	9.185920	-0.049997	4.777619
239.314320	7878.691413	9.190925	-0.050047	4.779994
239.343160	7886.680694	9.195930	-0.050058	4.782347
239.474088	7894.694425	9.200935	-0.050088	4.784705
239.491454	7902.736063	9.205939	-0.050097	4.787071
239.532519	7910.727869	9.210944	-0.050110	4.789421
239.719921	7918.782027	9.215949	-0.050150	4.791787
239.791871	7926.752472	9.220954	-0.050169	4.794129
240.031349	7934.808009	9.225959	-0.050219	4.796493
240.177988	7942.749194	9.230963	-0.050252	4.798823
240.233277	7950.771703	9.235968	-0.050267	4.801176
240.452541	7958.794291	9.240973	-0.050314	4.803527
240.438395	7966.797045	9.245978	-0.050317	4.805872
240.515449	7974.828594	9.250983	-0.050336	4.808225
240.568423	7982.883998	9.255987	-0.050352	4.810583
240.532963	7990.329408	9.260992	-0.050350	4.812761
240.925364	7995.023361	9.265997	-0.050426	4.814133

241.068903	7997.300634	9.271002	-0.050455	4.814798
241.203795	7998.687603	9.276007	-0.050481	4.815203
241.353631	7999.405441	9.281011	-0.050510	4.815412
241.179653	7999.727232	9.286016	-0.050478	4.815507
241.453591	7999.845962	9.291021	-0.050529	4.815540
241.406770	7999.736306	9.296026	-0.050521	4.815508
241.540895	7999.778016	9.301031	-0.050546	4.815520
241.596680	7999.724486	9.306035	-0.050556	4.815504
241.795627	7999.719201	9.311040	-0.050594	4.815502
241.552854	7999.808167	9.316045	-0.050549	4.815529
241.582944	7999.738202	9.321050	-0.050554	4.815508
241.763471	7999.733685	9.326055	-0.050588	4.815506
241.789698	7999.741606	9.331059	-0.050593	4.815508
241.752713	7999.755973	9.336064	-0.050587	4.815513
241.880869	7999.796519	9.341069	-0.050611	4.815524
241.864071	7999.881689	9.346074	-0.050608	4.815549
241.887659	7999.767838	9.351079	-0.050613	4.815515
241.943771	7999.980196	9.356083	-0.050623	4.815577
242.051942	7999.817534	9.361088	-0.050644	4.815529
241.946040	7999.925814	9.366093	-0.050624	4.815561
241.984120	7999.908300	9.371098	-0.050632	4.815556
242.369001	7999.924196	9.376103	-0.050703	4.815559
242.460275	7999.873379	9.381107	-0.050721	4.815543
242.389257	7999.925633	9.386112	-0.050708	4.815559
242.502158	7999.840998	9.391117	-0.050729	4.815534
242.233357	7999.918863	9.396122	-0.050679	4.815558
242.271875	7999.851169	9.401127	-0.050686	4.815538
242.260656	7999.943906	9.406131	-0.050685	4.815565
242.332069	7999.774238	9.411136	-0.050698	4.815515
242.310690	7999.895640	9.416141	-0.050694	4.815551
242.103642	7999.860254	9.421146	-0.050656	4.815541
242.254207	7999.763419	9.426151	-0.050684	4.815512
242.340104	7999.916466	9.431155	-0.050700	4.815557
242.347354	7999.874959	9.436160	-0.050702	4.815544
242.492919	7999.776974	9.441165	-0.050729	4.815515
242.424707	7999.947801	9.446170	-0.050717	4.815565
242.363242	7999.800529	9.451175	-0.050706	4.815523
242.618962	7999.802576	9.456179	-0.050753	4.815522
242.481632	7999.930634	9.461184	-0.050728	4.815560
242.643806	7999.817969	9.466189	-0.050759	4.815526
242.508527	7999.966349	9.471194	-0.050734	4.815570
242.850796	7999.769055	9.476199	-0.050797	4.815511
242.783422	7999.850200	9.481203	-0.050785	4.815535
242.416705	7999.827164	9.486208	-0.050717	4.815530
242.772163	7999.851124	9.491213	-0.050784	4.815535
242.737764	7999.934942	9.496218	-0.050777	4.815560
242.674780	7999.787644	9.501223	-0.050766	4.815517
242.798658	7999.919955	9.506227	-0.050789	4.815555
242.936589	7999.787674	9.511232	-0.050815	4.815516
243.073409	7999.875348	9.516237	-0.050841	4.815541
242.905446	7999.855547	9.521242	-0.050810	4.815536
243.115272	7999.803457	9.526247	-0.050849	4.815520
243.176413	7999.799133	9.531251	-0.050861	4.815518
243.039255	7999.848175	9.536256	-0.050835	4.815533
243.133006	7999.800601	9.541261	-0.050853	4.815519
243.122783	7999.855981	9.546266	-0.050851	4.815535
243.149352	7999.878858	9.551271	-0.050856	4.815542
243.206578	7999.892623	9.556275	-0.050867	4.815545
243.147010	7999.749651	9.561280	-0.050856	4.815504
243.250527	7999.921142	9.566285	-0.050876	4.815553
243.287827	7999.781882	9.571290	-0.050883	4.815513
243.268278	7999.784787	9.576295	-0.050880	4.815513
243.473558	7999.923766	9.581299	-0.050918	4.815553
243.176804	7999.806829	9.586304	-0.050863	4.815520
243.528849	7999.862771	9.591309	-0.050929	4.815535
243.288547	7999.882369	9.596314	-0.050884	4.815542
243.204632	7999.899175	9.601319	-0.050869	4.815547
243.183170	7999.857199	9.606323	-0.050865	4.815535
243.347039	7999.888719	9.611328	-0.050896	4.815543
243.568059	7999.864575	9.616333	-0.050937	4.815535
243.146238	7999.769094	9.621338	-0.050859	4.815509
243.300748	7999.869871	9.626343	-0.050888	4.815538
243.372243	7999.796306	9.631347	-0.050902	4.815516
243.280099	7999.858895	9.636352	-0.050885	4.815535
243.401552	7999.816043	9.641357	-0.050907	4.815522
243.368294	7999.843285	9.646362	-0.050901	4.815530
243.435396	7999.760038	9.651367	-0.050914	4.815505
243.375590	7999.887225	9.656371	-0.050903	4.815543
243.326131	7999.842657	9.661376	-0.050894	4.815530
243.469249	7999.755309	9.666381	-0.050921	4.815504
243.332634	7999.963469	9.671386	-0.050896	4.815565
243.609587	7999.804619	9.676391	-0.050948	4.815518
243.488080	7999.888087	9.681395	-0.050925	4.815542
243.516242	7999.777509	9.686400	-0.050931	4.815510
243.478575	7999.784390	9.691405	-0.050924	4.815512
243.674297	7999.877297	9.696410	-0.050961	4.815538
243.733723	7999.823824	9.701415	-0.050972	4.815523
243.632283	7999.900145	9.706419	-0.050953	4.815545
243.821023	7999.741993	9.711424	-0.050989	4.815498
243.896569	7999.828672	9.716429	-0.051003	4.815523
243.581156	7999.900438	9.721434	-0.050945	4.815546
243.619221	7999.804971	9.726439	-0.050952	4.815518
243.591232	7999.823756	9.731443	-0.050947	4.815523
243.753152	7999.791174	9.736448	-0.050977	4.815513
243.445295	7999.837436	9.741453	-0.050920	4.815528
243.517697	7999.871738	9.746458	-0.050934	4.815537
243.690114	7999.848938	9.751463	-0.050966	4.815530
243.601184	7999.801591	9.756467	-0.050950	4.815517
243.447039	7999.861035	9.761472	-0.050921	4.815535
243.674173	7999.773988	9.766477	-0.050964	4.815508
243.558549	7999.853280	9.771482	-0.050943	4.815532
243.785721	7999.785454	9.776487	-0.050985	4.815511
243.962776	7999.882329	9.781491	-0.051018	4.815538
243.849924	7999.843135	9.786496	-0.050997	4.815528
243.600464	7999.851905	9.791501	-0.050951	4.815531
243.569245	7999.812974	9.796506	-0.050946	4.815520
243.738380	7999.799731	9.801511	-0.050977	4.815515
243.810685	7999.891696	9.806515	-0.050991	4.815542
243.650974	7999.834653	9.811520	-0.050961	4.815526
243.792087	7999.893568	9.816525	-0.050988	4.815542
243.672091	7999.829697	9.821530	-0.050966	4.815524
243.628328	7999.819393	9.826535	-0.050958	4.815522
243.830239	7999.880366	9.831539	-0.050996	4.815538
243.937037	7999.840479	9.836544	-0.051016	4.815526
243.797468	7999.784832	9.841549	-0.050990	4.815511
243.647952	7999.809112	9.846554	-0.050962	4.815518
243.740080	7999.851211	9.851559	-0.050980	4.815530
243.648617	7999.831587	9.856563	-0.050963	4.815525
243.680810	7999.961341	9.861568	-0.050969	4.815563
244.058426	7999.762484	9.866573	-0.051040	4.815503
243.887998	7999.848360	9.871578	-0.051008	4.815529
243.809409	7999.848167	9.876583	-0.050994	4.815529
243.819997	7999.863309	9.881587	-0.050996	4.815533
243.887679	7999.846277	9.886592	-0.051009	4.815528
243.936833	7999.860980	9.891597	-0.051018	4.815532
243.695505	8000.001229	9.896602	-0.050974	4.815574
243.902449	7999.844441	9.901607	-0.051012	4.815528
243.746695	7999.854737	9.906611	-0.050984	4.815531
243.635434	7999.832655	9.911616	-0.050963	4.815525
243.942788	7999.902821	9.916621	-0.051021	4.815544
243.956369	7999.848601	9.921626	-0.051023	4.815528
243.668587	7999.848204	9.926631	-0.050970	4.815530
243.788026	7999.879001	9.931635	-0.050992	4.815538
243.819890	7999.908372	9.936640	-0.050999	4.815547
244.167658	7999.876683	9.941645	-0.051064	4.815536
244.004048	7999.960534	9.946650	-0.051033	4.815561
244.118072	7999.742432	9.951655	-0.051055	4.815497
244.308020	7999.965526	9.956659	-0.051090	4.815561
244.216844	7999.923481	9.961664	-0.051074	4.815549
244.231548	7999.788121	9.966669	-0.051076	4.815509
244.115482	7999.836439	9.971674	-0.051055	4.815524
244.007930	7999.877421	9.976679	-0.051035	4.815537
244.119451	7999.850425	9.981683	-0.051056	4.815528
244.337926	7999.864683	9.986688	-0.051097	4.815531
244.185786	7999.785338	9.991693	-0.051069	4.815509
244.154057	8000.034721	9.996698	-0.051064	4.815582
244.108695	7999.807614	10.001703	-0.051055	4.815516
244.157463	7999.865024	10.006707	-0.051065	4.815532
244.300461	7999.834270	10.011712	-0.051091	4.815523
244.505890	7999.848316	10.016717	-0.051130	4.815526
244.619278	7999.856591	10.021722	-0.051151	4.815528
244.428278	7999.854566	10.026727	-0.051116	4.815528
244.235387	7999.786302	10.031731	-0.051080	4.815509
244.441595	7999.854822	10.036736	-0.051119	4.815528
244.416088	7999.830932	10.041741	-0.051114	4.815521
244.374473	7999.970165	10.046746	-0.051107	4.815562
244.407437	7999.872478	10.051751	-0.051113	4.815533
244.390780	7999.782525	10.056755	-0.051110	4.815507
244.349330	7999.859823	10.061760	-0.051103	4.815530
244.507788	7999.783402	10.066765	-0.051132	4.815507
244.522422	7999.900059	10.071770	-0.051135	4.815541
244.338996	7999.814863	10.076775	-0.051101	4.815517
244.454312	7999.841323	10.081779	-0.051123	4.815524
244.490468	7999.856882	10.086784	-0.051130	4.815528
244.517129	7999.793263	10.091789	-0.051135	4.815509
244.426310	7999.874029	10.096794	-0.051119	4.815533
244.641592	7999.804941	10.101799	-0.051159	4.815512
244.673217	7999.842852	10.106803	-0.051165	4.815523
244.464384	7999.883251	10.111808	-0.051126	4.815536
244.728999	7999.813900	10.116813	-0.051176	4.815514
244.802950	7999.869586	10.121818	-0.051190	4.815530
244.539006	7999.779874	10.126823	-0.051141	4.815505
244.356190	7999.789730	10.131827	-0.051107	4.815509
244.500484	7999.890345	10.136832	-0.051134	4.815538
244.776816	7999.819048	10.141837	-0.051186	4.815516
244.663377	7999.857798	10.146842	-0.051165	4.815528
244.564893	7999.897860	10.151847	-0.051147	4.815540
244.566739	7999.865874	10.156851	-0.051147	4.815530
244.505001	7999.826444	10.161856	-0.051136	4.815519
244.628598	7999.844495	10.166861	-0.051159	4.815524
244.787955	7999.878081	10.171866	-0.051189	4.815533
244.600663	7999.774668	10.176871	-0.051155	4.815503
244.595911	7999.891008	10.181875	-0.051154	4.815537
244.738801	7999.861320	10.186880	-0.051181	4.815528
244.818930	7999.820998	10.191885	-0.051196	4.815516
244.729720	7999.846261	10.196890	-0.051180	4.815524
244.697281	7999.811580	10.201895	-0.051174	4.815514
244.684431	7999.869055	10.206899	-0.051172	4.815531
244.502023	7999.882120	10.211904	-0.051138	4.815535
244.608753	7999.824078	10.216909	-0.051158	4.815518
244.594664	7999.786492	10.221914	-0.051156	4.815507
244.798435	7999.907300	10.226919	-0.051194	4.815541
244.645604	7999.838620	10.231923	-0.051165	4.815522
244.562410	7999.768940	10.236928	-0.051150	4.815502
244.583466	7999.817357	10.241933	-0.051154	4.815516
244.634862	7999.850250	10.246938	-0.051164	4.815525
244.788114	7999.846360	10.251943	-0.051193	4.815523
244.844203	7999.908163	10.256947	-0.051204	4.815541
244.804406	7999.849868	10.261952	-0.051196	4.815524
244.811622	7999.817969	10.266957	-0.051198	4.815515
244.799038	7999.844480	10.271962	-0.051196	4.815523
244.787489	7999.769560	10.276967	-0.051194	4.815501
244.805626	7999.925786	10.281971	-0.051198	4.815547
244.909617	7999.782269	10.286976	-0.051217	4.815504
244.700331	7999.869647	10.291981	-0.051178	4.815531
244.674232	7999.827594	10.296986	-0.051174	4.815518
244.617783	7999.811743	10.301991	-0.051163	4.815514
244.795817	7999.793307	10.306995	-0.051197	4.815508
244.617590	7999.839544	10.312000	-0.051164	4.815522
244.686155	7999.794762	10.317005	-0.051177	4.815509
244.718857	7999.816672	10.322010	-0.051183	4.815515
244.734393	7999.900240	10.327015	-0.051186	4.815539
244.915043	7999.830588	10.332019	-0.051220	4.815518
244.608130	7999.869388	10.337024	-0.051163	4.815531
244.831975	7999.779083	10.342029	-0.051205	4.815503
244.697407	7999.911462	10.347034	-0.051180	4.815543
244.801233	7999.792503	10.352039	-0.051200	4.815508
244.689890	7999.853713	10.357043	-0.051179	4.815526
244.745140	7999.908027	10.362048	-0.051190	4.815542
244.942088	7999.770296	10.367053	-0.051227	4.815500
244.768381	7999.834761	10.372058	-0.051195	4.815520
244.899142	7999.872152	10.377063	-0.051219	4.815530
244.754214	7999.835637	10.382067	-0.051192	4.815520
244.878231	7999.808845	10.387072	-0.051216	4.815512
245.012446	7999.824935	10.392077	-0.051241	4.815516
244.950484	7999.909376	10.397082	-0.051230	4.815541
244.945155	7999.868728	10.402087	-0.051229	4.815529
244.941545	7999.823838	10.407091	-0.051228	4.815516
244.732820	7999.825795	10.412096	-0.051190	4.815518
244.745403	7999.847377	10.417101	-0.051192	4.815524
244.838276	7999.893762	10.422106	-0.051210	4.815537
245.048678	7999.789354	10.427111	-0.051249	4.815505
245.038945	7999.861832	10.432115	-0.051248	4.815527
244.815715	7999.883842	10.437120	-0.051206	4.815534
245.073047	7999.821847	10.442125	-0.051254	4.815515
245.045673	7999.837439	10.447130	-0.051250	4.815519
244.884249	7999.910647	10.452135	-0.051220	4.815542
244.866057	7999.832414	10.457139	-0.051217	4.815519
244.850785	7999.795877	10.462144	-0.051214	4.815508
245.257758	7999.847381	10.467149	-0.051290	4.815521
245.101611	7999.947373	10.472154	-0.051261	4.815551
245.033122	7999.823469	10.477159	-0.051249	4.815515
245.038470	7999.793675	10.482163	-0.051250	4.815507
245.016975	7999.880911	10.487168	-0.051246	4.815532
245.309415	7999.848321	10.492173	-0.051301	4.815521
245.134454	7999.821995	10.497178	-0.051268	4.815514
245.048369	7999.815272	10.502183	-0.051253	4.815513
245.060458	7999.843254	10.507187	-0.051255	4.815521
245.165223	7999.874882	10.512192	-0.051275	4.815530
245.011348	7999.827542	10.517197	-0.051246	4.815517
244.926968	7999.812304	10.522202	-0.051231	4.815513
245.111440	7999.923187	10.527207	-0.051265	4.815544
245.066042	7999.856257	10.532211	-0.051257	4.815525
244.922607	7999.849667	10.537216	-0.051231	4.815523
244.988598	7999.784554	10.542221	-0.051243	4.815504
245.200180	7999.889472	10.547226	-0.051283	4.815534
245.140859	7999.832994	10.552231	-0.051272	4.815518
245.111827	7999.970298	10.557235	-0.051267	4.815558
245.069841	7999.774209	10.562240	-0.051259	4.815501
245.051318	7999.888191	10.567245	-0.051256	4.815534
244.888015	7999.862055	10.572250	-0.051226	4.815527
244.957026	7999.862132	10.577255	-0.051239	4.815527
245.175538	7999.798436	10.582259	-0.051280	4.815507
245.149694	7999.922978	10.587264	-0.051275	4.815544
245.162741	7999.857001	10.592269	-0.051278	4.815524
245.004386	7999.974043	10.597274	-0.051249	4.815559
245.059309	7999.784873	10.602279	-0.051259	4.815504
245.146149	7999.818345	10.607283	-0.051275	4.815513
245.014739	7999.879228	10.612288	-0.051251	4.815532
245.135354	7999.776560	10.617293	-0.051274	4.815501
244.864334	7999.882155	10.622298	-0.051224	4.815533
245.161878	7999.858191	10.627303	-0.051279	4.815525
245.087263	7999.837773	10.632307	-0.051266	4.815519
244.949023	7999.829132	10.637312	-0.051240	4.815517
244.939832	7999.843952	10.642317	-0.051239	4.815522
245.040179	7999.888323	10.647322	-0.051258	4.815534
245.150868	7999.776950	10.652327	-0.051278	4.815501
244.977342	7999.909763	10.657331	-0.051246	4.815541
245.116765	7999.792452	10.662336	-0.051272	4.815506
245.273042	7999.912487	10.667341	-0.051302	4.815540
244.964967	7999.766523	10.672346	-0.051245	4.815499
245.058933	7999.882338	10.677351	-0.051262	4.815532
245.181786	7999.881157	10.682355	-0.051285	4.815531
245.037865	7999.886306	10.687360	-0.051259	4.815533
245.162663	7999.800793	10.692365	-0.051282	4.815508
245.354384	7999.898980	10.697370	-0.051318	4.815536
245.326706	7999.851561	10.702375	-0.051313	4.815522
245.110807	7999.822432	10.707379	-0.051273	4.815514
245.015171	7999.894577	10.712384	-0.051256	4.815536
245.240929	7999.789351	10.717389	-0.051298	4.815504
245.011360	7999.938337	10.722394	-0.051256	4.815549
245.133490	7999.799386	10.727399	-0.051278	4.815508
245.255115	7999.856919	10.732403	-0.051301	4.815524
244.907155	7999.893982	10.737408	-0.051237	4.815536
244.893840	7999.807285	10.742413	-0.051234	4.815511
245.000031	7999.820782	10.747418	-0.051254	4.815514
244.986556	7999.907081	10.752423	-0.051252	4.815540
244.963624	7999.881098	10.757427	-0.051248	4.815532
244.999042	7999.808010	10.762432	-0.051255	4.815511
245.321657	7999.836783	10.767437	-0.051315	4.815518
245.045843	7999.792794	10.772442	-0.051264	4.815506
245.146335	7999.885223	10.777447	-0.051283	4.815532
245.259682	7999.845442	10.782451	-0.051304	4.815520
245.347248	7999.903488	10.787456	-0.051321	4.815537
245.338251	7999.825404	10.792461	-0.051319	4.815514
245.293392	7999.843914	10.797466	-0.051311	4.815520
245.298310	7999.862168	10.802471	-0.051313	4.815525
245.248553	7999.947877	10.807475	-0.051304	4.815550
245.176373	7999.822843	10.812480	-0.051290	4.815514
245.353641	7999.858858	10.817485	-0.051323	4.815524
245.088945	7999.879124	10.822490	-0.051274	4.815531
245.026960	7999.827942	10.827495	-0.051263	4.815516
245.250615	7999.926650	10.832499	-0.051305	4.815544
245.272149	7999.853336	10.837504	-0.051309	4.815523
245.159440	7999.758611	10.842509	-0.051288	4.815495
245.155762	7999.874971	10.847514	-0.051288	4.815529
245.459250	7999.934402	10.852519	-0.051345	4.815545
245.467102	7999.810673	10.857523	-0.051346	4.815509
245.066594	7999.853286	10.862528	-0.051272	4.815523
245.394763	7999.904576	10.867533	-0.051333	4.815537
245.371875	7999.813451	10.872538	-0.051329	4.815510
245.377134	7999.876562	10.877543	-0.051331	4.815529
245.379295	7999.911858	10.882547	-0.051331	4.815539
245.205052	7999.777685	10.887552	-0.051299	4.815501
245.261452	7999.907840	10.892557	-0.051310	4.815538
244.983508	7999.888377	10.897562	-0.051258	4.815534
245.197551	7999.754128	10.902567	-0.051298	4.815494
245.206729	7999.887784	10.907571	-0.051300	4.815533
245.008364	7999.864280	10.912576	-0.051263	4.815527
245.478897	7999.854884	10.917581	-0.051351	4.815522
245.098542	7999.903165	10.922586	-0.051281	4.815538
245.202425	7999.835465	10.927591	-0.051300	4.815518
245.289373	7999.837970	10.932595	-0.051317	4.815518
245.418539	7999.934071	10.937600	-0.051341	4.815545
245.186780	7999.840608	10.942605	-0.051298	4.815519
245.171313	7999.814746	10.947610	-0.051295	4.815512
245.444255	7999.806401	10.952615	-0.051346	4.815508
245.421466	7999.979049	10.957619	-0.051342	4.815558
245.278364	7999.869945	10.962624	-0.051316	4.815527
245.473101	7999.847510	10.967629	-0.051352	4.815520
245.424248	7999.846733	10.972634	-0.051344	4.815520
245.082298	7999.903116	10.977639	-0.051280	4.815538
245.481048	7999.848766	10.982643	-0.051355	4.815520
245.437937	7999.802163	10.987648	-0.051347	4.815507
245.448023	7999.863217	10.992653	-0.051349	4.815524
245.352739	7999.939640	10.997658	-0.051331	4.815547
245.606460	7999.801766	11.002663	-0.051379	4.815506
245.634723	7999.909037	11.007667	-0.051384	4.815537
245.565097	7999.952773	11.012672	-0.051372	4.815550
245.559151	7999.879010	11.017677	-0.051371	4.815528
245.354813	7999.870358	11.022682	-0.051333	4.815527
245.284999	7999.810505	11.027687	-0.051320	4.815510
245.490985	7999.882229	11.032691	-0.051359	4.815530
245.483310	7999.808438	11.037696	-0.051357	4.815508
245.236025	7999.899469	11.042701	-0.051312	4.815536
245.321648	7999.816520	11.047706	-0.051328	4.815511
245.460279	7999.918115	11.052711	-0.051354	4.815540
245.599063	7999.901175	11.057715	-0.051380	4.815535
245.253789	7999.829356	11.062720	-0.051316	4.815515
245.274257	7999.843591	11.067725	-0.051320	4.815519
245.332977	7999.902235	11.072730	-0.051331	4.815536
245.203759	7999.815784	11.077735	-0.051307	4.815512
245.389081	7999.945905	11.082739	-0.051342	4.815549
245.502330	7999.814283	11.087744	-0.051363	4.815510
245.470274	7999.887465	11.092749	-0.051358	4.815531
245.279045	7999.943102	11.097754	-0.051322	4.815548
245.437855	7999.848532	11.102759	-0.051352	4.815520
245.342724	7999.896124	11.107763	-0.051334	4.815534
245.352444	7999.830092	11.112768	-0.051336	4.815515
245.424927	7999.870805	11.117773	-0.051350	4.815527
245.441848	7999.850811	11.122778	-0.051354	4.815521
245.159551	7999.832345	11.127783	-0.051301	4.815517
245.368169	7999.983137	11.132787	-0.051340	4.815560
245.435016	7999.793091	11.137792	-0.051353	4.815504
245.187884	7999.832866	11.142797	-0.051307	4.815517
245.228426	7999.897620	11.147802	-0.051315	4.815535
245.381491	7999.812568	11.152807	-0.051344	4.815510
245.513622	7999.855322	11.157811	-0.051368	4.815522
245.526620	7999.885455	11.162816	-0.051371	4.815530
245.512220	7999.861745	11.167821	-0.051369	4.815523
245.418979	7999.908300	11.172826	-0.051352	4.815537
245.391955	7999.808564	11.177831	-0.051347	4.815508
245.421193	7999.952160	11.182835	-0.051352	4.815550
245.429684	7999.840188	11.187840	-0.051354	4.815518
245.657078	7999.866341	11.192845	-0.051397	4.815524
245.546617	7999.795146	11.197850	-0.051376	4.815504
245.479891	7999.893392	11.202855	-0.051364	4.815533
245.396976	8000.006326	11.207859	-0.051349	4.815566
245.424378	7999.828452	11.212864	-0.051354	4.815514
245.597053	7999.844102	11.217869	-0.051387	4.815518
245.381080	7999.828853	11.222874	-0.051347	4.815514
245.250920	7999.876942	11.227879	-0.051323	4.815529
245.636067	7999.899260	11.232883	-0.051395	4.815534
245.588741	7999.829094	11.237888	-0.051386	4.815513
245.487315	7999.863769	11.242893	-0.051367	4.815524
245.429407	7999.972839	11.247898	-0.051357	4.815556
245.743421	7999.876527	11.252903	-0.051416	4.815527
245.612651	7999.874414	11.257907	-0.051391	4.815527
245.320621	7999.889963	11.262912	-0.051337	4.815532
245.435113	7999.837386	11.267917	-0.051359	4.815517
245.564815	7999.900391	11.272922	-0.051383	4.815534
245.693176	7999.852312	11.277927	-0.051407	4.815520
245.690228	7999.887524	11.282931	-0.051407	4.815530
245.604779	7999.916052	11.287936	-0.051391	4.815539
245.532693	7999.868976	11.292941	-0.051378	4.815525
245.472662	7999.858406	11.297946	-0.051367	4.815523
245.514319	7999.814252	11.302951	-0.051375	4.815509
245.458772	7999.937243	11.307955	-0.051365	4.815546
245.404732	7999.861628	11.312960	-0.051355	4.815524
245.549893	7999.871490	11.317965	-0.051382	4.815526
245.595858	7999.831679	11.322970	-0.051391	4.815514
245.458165	7999.921293	11.327975	-0.051366	4.815541
245.575588	7999.862357	11.332979	-0.051388	4.815523
245.892215	7999.887830	11.337984	-0.051447	4.815529
245.856610	7999.874454	11.342989	-0.051441	4.815525
245.679053	7999.901479	11.347994	-0.051408	4.815534
245.655877	7999.862676	11.352999	-0.051404	4.815523
246.023651	7999.915682	11.358003	-0.051472	4.815537
245.875973	7999.886595	11.363008	-0.051445	4.815529
245.639316	7999.935083	11.368013	-0.051401	4.815544
245.790180	7999.879895	11.373018	-0.051430	4.815527
245.838092	7999.980013	11.378023	-0.051439	4.815556
245.648468	7999.913933	11.383027	-0.051404	4.815538
245.411919	7999.811848	11.388032	-0.051360	4.815509
245.640195	7999.877528	11.393037	-0.051403	4.815527
245.666812	7999.901476	11.398042	-0.051408	4.815534
245.519126	7999.896951	11.403047	-0.051380	4.815533
245.520089	7999.907665	11.408051	-0.051381	4.815537
245.443737	7999.829551	11.413056	-0.051367	4.815514
245.641476	7999.937450	11.418061	-0.051404	4.815545
245.756443	7999.891288	11.423066	-0.051426	4.815531
245.762260	7999.892470	11.428071	-0.051427	4.815531
245.585522	7999.850095	11.433075	-0.051394	4.815519
245.625899	7999.819804	11.438080	-0.051402	4.815510
245.951998	7999.908439	11.443085	-0.051463	4.815535
245.689881	7999.933017	11.448090	-0.051414	4.815543
245.626609	7999.845504	11.453095	-0.051403	4.815518
245.638997	7999.855337	11.458099	-0.051405	4.815521
245.582424	7999.927052	11.463104	-0.051395	4.815542
245.548343	7999.807978	11.468109	-0.051389	4.815507
245.672158	7999.928554	11.473114	-0.051412	4.815542
245.651216	7999.805423	11.478119	-0.051408	4.815506
245.631307	7999.828612	11.483123	-0.051405	4.815513
245.681370	7999.905269	11.488128	-0.051414	4.815535
245.966288	7999.866151	11.493133	-0.051468	4.815522
245.713732	7999.838558	11.498138	-0.051421	4.815515
245.807537	7999.910589	11.503143	-0.051439	4.815536
245.813682	7999.832751	11.508147	-0.051440	4.815513
245.697897	7999.905637	11.513152	-0.051419	4.815535
245.790750	7999.815330	11.518157	-0.051436	4.815508
245.928932	7999.858184	11.523162	-0.051462	4.815520
245.730361	7999.908361	11.528167	-0.051425	4.815536
245.644088	7999.887751	11.533171	-0.051410	4.815530
245.402767	7999.831508	11.538176	-0.051365	4.815515
245.718234	7999.814245	11.543181	-0.051424	4.815508
245.627026	7999.953742	11.548186	-0.051407	4.815549
245.431803	7999.825633	11.553191	-0.051371	4.815513
245.728218	7999.899900	11.558195	-0.051426	4.815533
245.815346	7999.896001	11.563200	-0.051443	4.815532
245.665980	7999.885041	11.568205	-0.051415	4.815529
245.674996	7999.817929	11.573210	-0.051417	4.815509
245.905514	7999.812097	11.578215	-0.051460	4.815507
245.830469	7999.966808	11.583219	-0.051447	4.815552
245.512941	7999.864469	11.588224	-0.051388	4.815524
245.884080	7999.861998	11.593229	-0.051457	4.815521
246.011540	7999.914288	11.598234	-0.051481	4.815536
245.969038	7999.873034	11.603239	-0.051473	4.815524
245.944698	7999.882268	11.608243	-0.051469	4.815527
245.901556	7999.821780	11.613248	-0.051461	4.815509
245.970522	7999.879524	11.618253	-0.051474	4.815526
245.789058	7999.989784	11.623258	-0.051441	4.815559
245.774879	7999.858218	11.628263	-0.051438	4.815521
245.837965	7999.829365	11.633267	-0.051450	4.815512
245.602202	7999.921652	11.638272	-0.051406	4.815540
245.780401	7999.886133	11.643277	-0.051440	4.815529
245.732117	7999.850124	11.648282	-0.051431	4.815518
245.580947	7999.830592	11.653287	-0.051403	4.815513
245.642953	7999.975791	11.658291	-0.051415	4.815556
245.737647	7999.816100	11.663296	-0.051433	4.815508
245.705157	7999.833744	11.668301	-0.051427	4.815514
245.573074	7999.989661	11.673306	-0.051403	4.815560
245.873054	7999.876034	11.678311	-0.051459	4.815525
245.949093	7999.903992	11.683315	-0.051473	4.815533
245.698723	7999.865755	11.688320	-0.051427	4.815523
245.955213	7999.857142	11.693325	-0.051475	4.815519
245.852523	7999.931309	11.698330	-0.051456	4.815542
245.888641	7999.822990	11.703335	-0.051463	4.815510
245.781022	7999.890669	11.708339	-0.051443	4.815530
245.790914	7999.872695	11.713344	-0.051445	4.815525
245.880898	7999.973499	11.718349	-0.051462	4.815554
245.940776	7999.835666	11.723354	-0.051473	4.815513
246.049329	7999.810758	11.728359	-0.051494	4.815505
246.060741	7999.934842	11.733363	-0.051496	4.815542
245.785949	7999.920769	11.738368	-0.051445	4.815539
245.703377	7999.868182	11.743373	-0.051430	4.815524
246.163495	7999.877841	11.748378	-0.051516	4.815524
246.065217	7999.866646	11.753383	-0.051498	4.815522
245.873666	7999.857134	11.758387	-0.051462	4.815520
246.173486	7999.931459	11.763392	-0.051518	4.815540
245.966592	7999.852282	11.768397	-0.051480	4.815518
245.697109	7999.840431	11.773402	-0.051430	4.815516
245.857442	7999.834522	11.778407	-0.051460	4.815513
246.146454	7999.905466	11.783411	-0.051514	4.815532
246.069321	7999.930926	11.788416	-0.051500	4.815540
245.834500	7999.821392	11.793421	-0.051457	4.815509
246.005772	7999.923521	11.798426	-0.051489	4.815538
245.902407	7999.778754	11.803431	-0.051470	4.815497
246.010164	7999.906545	11.808435	-0.051490	4.815533
245.979761	7999.829178	11.813440	-0.051485	4.815511
246.027295	7999.895116	11.818445	-0.051494	4.815530
246.034885	7999.965743	11.823450	-0.051495	4.815551
245.975782	7999.794999	11.828455	-0.051484	4.815501
245.897196	7999.965672	11.833459	-0.051470	4.815551
245.772967	7999.808817	11.838464	-0.051447	4.815506
245.821773	7999.855553	11.843469	-0.051456	4.815519
246.073436	7999.931228	11.848474	-0.051504	4.815540
245.963803	7999.818396	11.853479	-0.051483	4.815508
245.941491	7999.831934	11.858483	-0.051479	4.815512
245.776815	7999.898683	11.863488	-0.051449	4.815532
246.016465	7999.836400	11.868493	-0.051494	4.815513
245.841100	7999.858122	11.873498	-0.051461	4.815520
245.909666	7999.962848	11.878503	-0.051474	4.815550
246.052241	7999.850925	11.883507	-0.051501	4.815517
246.061186	7999.931185	11.888512	-0.051503	4.815540
245.935217	7999.829833	11.893517	-0.051480	4.815511
246.018472	7999.862180	11.898522	-0.051496	4.815520
246.147047	7999.872840	11.903527	-0.051520	4.815523
246.029963	7999.890173	11.908531	-0.051498	4.815528
245.876016	7999.870595	11.913536	-0.051470	4.815523
246.079106	7999.946546	11.918541	-0.051508	4.815545
246.098564	7999.867856	11.923546	-0.051512	4.815522
245.903892	7999.851886	11.928551	-0.051476	4.815518
246.000552	7999.961342	11.933555	-0.051494	4.815549
246.008531	7999.808779	11.938560	-0.051495	4.815505
245.974499	7999.929986	11.943565	-0.051489	4.815540
246.150943	7999.849586	11.948570	-0.051522	4.815516
246.056942	7999.851276	11.953575	-0.051505	4.815517
245.986368	7999.903541	11.958579	-0.051492	4.815532
245.941345	7999.931660	11.963584	-0.051484	4.815541
246.145269	7999.851707	11.968589	-0.051522	4.815517
245.929995	7999.846080	11.973594	-0.051482	4.815516
246.030154	7999.913944	11.978599	-0.051501	4.815535
246.039612	7999.900235	11.983603	-0.051503	4.815531
246.107582	7999.823405	11.988608	-0.051516	4.815508
246.123526	7999.902711	11.993613	-0.051519	4.815532
246.020120	7999.919199	11.998618	-0.051500	4.815537
246.029077	7999.861696	12.003623	-0.051502	4.815520
246.117017	7999.902664	12.008627	-0.051519	4.815532
245.934355	7999.950964	12.013632	-0.051485	4.815547
246.209276	7999.908479	12.018637	-0.051536	4.815533
246.162025	7999.906660	12.023642	-0.051528	4.815532
246.041367	7999.837433	12.028647	-0.051506	4.815513
246.020710	7999.879832	12.033651	-0.051502	4.815525
245.914984	7999.908029	12.038656	-0.051483	4.815534
245.980795	7999.864269	12.043661	-0.051495	4.815521
246.048077	7999.894220	12.048666	-0.051508	4.815529
245.792045	7999.924237	12.053671	-0.051460	4.815539
245.804635	7999.824078	12.058675	-0.051463	4.815510
245.833954	7999.921756	12.063680	-0.051469	4.815538
246.220373	7999.872547	12.068685	-0.051541	4.815522
246.110493	7999.882521	12.073690	-0.051521	4.815526
245.894045	7999.913184	12.078695	-0.051480	4.815536
246.134274	7999.902171	12.083699	-0.051525	4.815531
246.259376	7999.864718	12.088704	-0.051549	4.815520
246.215860	7999.873639	12.093709	-0.051541	4.815523
246.009969	7999.904474	12.098714	-0.051503	4.815532
246.375079	7999.850645	12.103719	-0.051571	4.815515
246.193847	8000.006830	12.108723	-0.051538	4.815562
246.117513	7999.900947	12.113728	-0.051524	4.815531
245.987507	7999.890303	12.118733	-0.051500	4.815528
245.969918	7999.849454	12.123738	-0.051497	4.815517
245.952123	7999.815010	12.128743	-0.051493	4.815507
246.253639	7999.943827	12.133747	-0.051550	4.815543
246.240631	7999.844317	12.138752	-0.051548	4.815514
246.132589	7999.905582	12.143757	-0.051528	4.815532
246.080675	7999.941065	12.148762	-0.051518	4.815543
246.179565	7999.825225	12.153767	-0.051537	4.815508
246.175824	7999.884988	12.158771	-0.051536	4.815526
246.119961	7999.850990	12.163776	-0.051526	4.815516
246.438636	7999.912809	12.168781	-0.051586	4.815533
246.257909	7999.954733	12.173786	-0.051552	4.815546
246.130169	7999.835197	12.178791	-0.051529	4.815512
246.187687	7999.847902	12.183795	-0.051540	4.815515
246.283681	7999.923174	12.188800	-0.051558	4.815537
246.465664	7999.906940	12.193805	-0.051592	4.815531
246.251187	7999.883170	12.198810	-0.051552	4.815525
246.114306	7999.830764	12.203815	-0.051527	4.815510
246.328549	7999.953887	12.208819	-0.051567	4.815545
245.930129	7999.849158	12.213824	-0.051493	4.815517
246.193086	7999.894048	12.218829	-0.051542	4.815528
246.235331	7999.884077	12.223834	-0.051550	4.815525
246.127745	7999.904768	12.228839	-0.051531	4.815532
246.298943	7999.908648	12.233843	-0.051563	4.815532
246.149378	7999.939334	12.238848	-0.051535	4.815542
246.337319	7999.934944	12.243853	-0.051570	4.815540
246.139923	7999.874075	12.248858	-0.051534	4.815523
246.193391	7999.816231	12.253863	-0.051544	4.815506
246.308580	7999.908904	12.258867	-0.051566	4.815532
245.991532	7999.931517	12.263872	-0.051507	4.815540
246.124567	7999.895262	12.268877	-0.051532	4.815529
246.325243	7999.897487	12.273882	-0.051569	4.815529
246.053063	7999.893066	12.278887	-0.051519	4.815529
245.991913	7999.865391	12.283891	-0.051508	4.815521
246.125345	7999.932730	12.288896	-0.051533	4.815540
246.231095	7999.900301	12.293901	-0.051553	4.815530
246.189353	7999.926338	12.298906	-0.051545	4.815538
246.133589	7999.887002	12.303911	-0.051535	4.815527
246.332693	7999.911629	12.308915	-0.051572	4.815533
246.366619	7999.950647	12.313920	-0.051579	4.815544
246.351608	7999.869259	12.318925	-0.051576	4.815520
246.300136	7999.890865	12.323930	-0.051567	4.815527
246.371614	7999.927293	12.328935	-0.051581	4.815537
246.390203	7999.864608	12.333939	-0.051584	4.815519
246.409181	7999.862801	12.338944	-0.051588	4.815518
246.287034	7999.859760	12.343949	-0.051565	4.815518
246.421151	7999.911093	12.348954	-0.051591	4.815532
246.380768	7999.938220	12.353959	-0.051583	4.815540
246.338461	7999.878813	12.358963	-0.051576	4.815523
246.172890	7999.834482	12.363968	-0.051545	4.815511
246.094929	7999.931479	12.368973	-0.051531	4.815540
246.317255	7999.893476	12.373978	-0.051572	4.815528
246.503972	7999.886931	12.378983	-0.051607	4.815525
246.341332	7999.903520	12.383987	-0.051577	4.815530
246.369808	7999.867694	12.388992	-0.051583	4.815520
246.345472	7999.890811	12.393997	-0.051579	4.815527
246.190029	7999.939556	12.399002	-0.051550	4.815542
246.215489	7999.859896	12.404007	-0.051555	4.815518
246.417898	7999.928361	12.409011	-0.051593	4.815537
246.345539	7999.884483	12.414016	-0.051579	4.815525
246.354140	7999.898526	12.419021	-0.051581	4.815529
246.305100	7999.891338	12.424026	-0.051572	4.815527
246.280656	7999.930473	12.429031	-0.051568	4.815538
246.284029	7999.858996	12.434035	-0.051569	4.815518
246.320869	7999.813695	12.439040	-0.051576	4.815504
246.228781	7999.942500	12.444045	-0.051559	4.815542
246.216395	7999.882513	12.449050	-0.051557	4.815525
246.240526	7999.830598	12.454055	-0.051562	4.815509
246.405874	7999.896323	12.459059	-0.051593	4.815528
246.129727	7999.917468	12.464064	-0.051542	4.815535
246.198285	7999.874821	12.469069	-0.051555	4.815523
246.320112	7999.964399	12.474074	-0.051577	4.815548
246.300330	7999.824196	12.479079	-0.051574	4.815507
246.242979	7999.901239	12.484083	-0.051564	4.815530
246.340268	7999.958379	12.489088	-0.051582	4.815546
246.484598	7999.883861	12.494093	-0.051609	4.815524
246.355733	7999.891390	12.499098	-0.051585	4.815527
246.129875	7999.833261	12.504103	-0.051543	4.815511
246.567783	7999.893821	12.509107	-0.051625	4.815526
246.408623	7999.956388	12.514112	-0.051596	4.815545
246.436909	7999.885317	12.519117	-0.051601	4.815524
246.257731	7999.881346	12.524122	-0.051568	4.815524
246.295589	7999.807228	12.529127	-0.051575	4.815502
246.352509	7999.953415	12.534131	-0.051586	4.815545
246.375967	7999.861975	12.539136	-0.051591	4.815518
246.441202	7999.892961	12.544141	-0.051603	4.815527
246.494431	7999.963265	12.549146	-0.051613	4.815547
246.361535	7999.857526	12.554151	-0.051589	4.815517
246.547597	7999.895823	12.559155	-0.051624	4.815527
246.314446	7999.825827	12.564160	-0.051580	4.815508
246.353263	7999.889488	12.569165	-0.051588	4.815526
246.383080	8000.002128	12.574170	-0.051594	4.815559
246.447293	7999.868634	12.579175	-0.051606	4.815519
246.454865	7999.922175	12.584179	-0.051607	4.815535
246.253984	7999.876199	12.589184	-0.051570	4.815523
246.371785	7999.881345	12.594189	-0.051592	4.815523
246.221019	7999.881041	12.599194	-0.051565	4.815524
246.298600	7999.932519	12.604199	-0.051579	4.815539
246.307508	7999.866472	12.609203	-0.051581	4.815519
246.383711	7999.899772	12.614208	-0.051596	4.815529
246.365827	7999.831152	12.619213	-0.051592	4.815509
246.462169	7999.986527	12.624218	-0.051611	4.815554
246.413698	7999.824497	12.629223	-0.051602	4.815507
246.426476	7999.977440	12.634227	-0.051604	4.815551
246.406428	7999.845776	12.639232	-0.051601	4.815513
246.391560	7999.858368	12.644237	-0.051598	4.815517
246.515821	7999.941579	12.649242	-0.051622	4.815540
246.395155	7999.844583	12.654247	-0.051599	4.815513
246.486092	7999.889872	12.659251	-0.051617	4.815525
246.395920	7999.950361	12.664256	-0.051600	4.815543
246.467764	7999.889612	12.669261	-0.051614	4.815525
246.652606	7999.909734	12.674266	-0.051648	4.815530
246.353128	7999.845063	12.679271	-0.051593	4.815513
246.503802	7999.978898	12.684275	-0.051621	4.815551
246.340836	7999.849174	12.689280	-0.051591	4.815514
246.470178	7999.887613	12.694285	-0.051615	4.815525
246.461680	7999.876815	12.699290	-0.051614	4.815522
246.205281	7999.914301	12.704295	-0.051566	4.815534
246.458134	7999.897087	12.709299	-0.051614	4.815528
246.412578	7999.904907	12.714304	-0.051605	4.815530
246.321901	7999.877817	12.719309	-0.051589	4.815523
246.580543	7999.920502	12.724314	-0.051637	4.815534
246.385538	7999.879962	12.729319	-0.051601	4.815523
246.612205	7999.926397	12.734323	-0.051643	4.815535
246.591380	7999.949572	12.739328	-0.051640	4.815542
246.457881	7999.851299	12.744333	-0.051615	4.815514
246.559088	7999.874328	12.749338	-0.051634	4.815520
246.526328	7999.871677	12.754343	-0.051628	4.815520
246.791258	7999.959320	12.759347	-0.051678	4.815544
246.681299	7999.999195	12.764352	-0.051658	4.815556
246.584315	7999.910060	12.769357	-0.051640	4.815531
246.739035	7999.906197	12.774362	-0.051669	4.815529
246.434699	7999.844650	12.779367	-0.051612	4.815512
246.439248	8000.020954	12.784371	-0.051614	4.815564
246.426352	7999.911833	12.789376	-0.051611	4.815532
246.437449	7999.886403	12.794381	-0.051614	4.815524
246.441230	7999.922794	12.799386	-0.051615	4.815535
246.439999	7999.886484	12.804391	-0.051615	4.815524
246.655589	7999.954098	12.809395	-0.051655	4.815543
246.623255	7999.956794	12.814400	-0.051649	4.815544
246.719140	7999.898573	12.819405	-0.051667	4.815527
246.666639	7999.929774	12.824410	-0.051658	4.815536
246.551516	7999.880926	12.829415	-0.051636	4.815522
246.724633	7999.949983	12.834419	-0.051669	4.815542
246.661278	7999.885959	12.839424	-0.051657	4.815523
246.609058	7999.896874	12.844429	-0.051648	4.815527
246.557971	7999.913148	12.849434	-0.051639	4.815532
246.477813	7999.904384	12.854439	-0.051624	4.815529
246.378760	7999.867545	12.859443	-0.051606	4.815519
246.418194	7999.837238	12.864448	-0.051613	4.815510
246.326967	7999.952175	12.869453	-0.051596	4.815544
246.295438	7999.874788	12.874458	-0.051591	4.815522
246.443862	7999.865482	12.879463	-0.051619	4.815518
246.685705	7999.872651	12.884467	-0.051664	4.815519
246.428723	7999.964593	12.889472	-0.051616	4.815547
246.628092	7999.846120	12.894477	-0.051654	4.815512
246.560415	7999.901636	12.899482	-0.051641	4.815528
246.322070	7999.893495	12.904487	-0.051597	4.815527
246.400265	7999.874500	12.909491	-0.051612	4.815521
246.332318	7999.857392	12.914496	-0.051599	4.815516
246.637505	7999.977728	12.919501	-0.051656	4.815550
246.516053	7999.895670	12.924506	-0.051634	4.815527
246.673737	7999.883311	12.929511	-0.051664	4.815522
246.850495	7999.930001	12.934515	-0.051697	4.815535
246.720331	7999.889451	12.939520	-0.051673	4.815524
246.578862	7999.897841	12.944525	-0.051647	4.815527
246.592474	7999.887404	12.949530	-0.051649	4.815524
246.534400	7999.961232	12.954535	-0.051639	4.815546
246.434407	7999.885932	12.959539	-0.051620	4.815524
246.429951	7999.858112	12.964544	-0.051620	4.815516
246.694271	7999.903026	12.969549	-0.051669	4.815528
246.450679	8000.001594	12.974554	-0.051624	4.815558
246.477575	7999.848269	12.979559	-0.051629	4.815513
246.749814	7999.950981	12.984563	-0.051680	4.815542
246.445662	7999.874486	12.989568	-0.051624	4.815521
246.676045	7999.914574	12.994573	-0.051667	4.815531
246.756561	7999.973577	12.999578	-0.051682	4.815548
246.508129	7999.853137	13.004583	-0.051636	4.815514
246.402979	7999.858916	13.009587	-0.051617	4.815516
246.374314	7999.936428	13.014592	-0.051612	4.815539
246.687295	7999.895633	13.019597	-0.051670	4.815526
246.514434	7999.860794	13.024602	-0.051638	4.815516
246.526699	7999.913342	13.029607	-0.051641	4.815532
246.729864	7999.960463	13.034611	-0.051679	4.815544
246.487170	7999.899921	13.039616	-0.051634	4.815528
246.447707	7999.888618	13.044621	-0.051627	4.815525
246.535583	7999.902886	13.049626	-0.051643	4.815528
246.599523	7999.854824	13.054631	-0.051655	4.815514
246.814548	7999.919225	13.059635	-0.051696	4.815532
246.582104	7999.901568	13.064640	-0.051653	4.815528
246.660969	7999.968020	13.069645	-0.051668	4.815547
246.458999	7999.941249	13.074650	-0.051630	4.815540
246.513557	7999.841772	13.079655	-0.051640	4.815511
246.577557	7999.926135	13.084659	-0.051653	4.815535
246.455648	7999.847274	13.089664	-0.051630	4.815513
246.615563	7999.983396	13.094669	-0.051660	4.815552
246.770720	7999.899443	13.099674	-0.051689	4.815526
246.596197	7999.935061	13.104679	-0.051657	4.815537
246.566023	7999.957015	13.109683	-0.051652	4.815544
246.684153	7999.913041	13.114688	-0.051674	4.815531
246.719621	7999.930726	13.119693	-0.051681	4.815536
246.831864	7999.959276	13.124698	-0.051702	4.815543
246.680454	7999.925855	13.129703	-0.051674	4.815534
246.875614	7999.902360	13.134707	-0.051710	4.815527
246.557185	7999.915339	13.139712	-0.051651	4.815532
246.763134	7999.930466	13.144717	-0.051690	4.815535
246.827837	7999.896299	13.149722	-0.051702	4.815525
246.996837	7999.906553	13.154727	-0.051734	4.815527
246.843662	7999.951062	13.159731	-0.051706	4.815541
246.750192	7999.920722	13.164736	-0.051688	4.815532
246.869804	7999.917354	13.169741	-0.051711	4.815531
246.747039	7999.896147	13.174746	-0.051688	4.815525
246.716652	7999.956544	13.179751	-0.051683	4.815543
246.953910	7999.926261	13.184755	-0.051727	4.815533
246.657781	7999.907565	13.189760	-0.051672	4.815529
246.747372	7999.933609	13.194765	-0.051689	4.815536
246.834646	7999.955344	13.199770	-0.051706	4.815542
246.804037	7999.929233	13.204775	-0.051700	4.815535
246.862599	7999.928072	13.209779	-0.051711	4.815534
246.651809	7999.876595	13.214784	-0.051672	4.815520
246.807367	7999.962453	13.219789	-0.051702	4.815544
246.910815	7999.928918	13.224794	-0.051721	4.815534
246.735360	7999.871609	13.229799	-0.051688	4.815518
246.723094	7999.926962	13.234803	-0.051686	4.815534
246.725089	7999.904587	13.239808	-0.051687	4.815528
246.654920	7999.878899	13.244813	-0.051674	4.815521
246.732074	7999.925031	13.249818	-0.051689	4.815534
246.680726	7999.993630	13.254823	-0.051680	4.815554
246.676093	7999.926293	13.259827	-0.051679	4.815534
246.604831	7999.861073	13.264832	-0.051666	4.815516
246.754375	7999.868872	13.269837	-0.051694	4.815517
246.752527	7999.926531	13.274842	-0.051694	4.815534
246.386809	7999.850099	13.279847	-0.051626	4.815513
246.501226	7999.931013	13.284851	-0.051647	4.815537
246.550672	7999.922228	13.289856	-0.051657	4.815534
246.517960	7999.890743	13.294861	-0.051651	4.815525
246.642018	7999.986767	13.299866	-0.051674	4.815552
246.885750	7999.888240	13.304871	-0.051720	4.815522
246.904052	7999.922733	13.309875	-0.051724	4.815532
246.553666	7999.874317	13.314880	-0.051658	4.815520
246.636101	7999.848983	13.319885	-0.051674	4.815512
246.729947	7999.991503	13.324890	-0.051692	4.815553
246.537591	7999.860230	13.329895	-0.051656	4.815516
246.457370	7999.892047	13.334899	-0.051641	4.815525
246.639330	7999.859793	13.339904	-0.051676	4.815515
246.540023	7999.917998	13.344909	-0.051657	4.815532
246.535143	7999.898715	13.349914	-0.051657	4.815527
246.750748	7999.894777	13.354919	-0.051697	4.815525
246.723455	7999.946681	13.359923	-0.051692	4.815540
246.721128	7999.909284	13.364928	-0.051692	4.815529
246.878662	7999.932165	13.369933	-0.051721	4.815535
246.919388	7999.914694	13.374938	-0.051729	4.815530
246.868050	7999.972614	13.379943	-0.051720	4.815547
246.880401	7999.933320	13.384947	-0.051722	4.815535
246.862090	7999.919158	13.389952	-0.051719	4.815531
246.799428	7999.941650	13.394957	-0.051708	4.815538
246.628450	7999.907909	13.399962	-0.051676	4.815529
246.684833	7999.885353	13.404967	-0.051687	4.815522
246.887478	7999.938874	13.409971	-0.051725	4.815537
246.726324	7999.927720	13.414976	-0.051695	4.815534
246.781772	7999.880586	13.419981	-0.051706	4.815520
246.853429	7999.933037	13.424986	-0.051719	4.815535
246.748066	7999.880075	13.429991	-0.051700	4.815520
246.628463	7999.883483	13.434995	-0.051678	4.815522
246.684338	7999.968783	13.440000	-0.051688	4.815547
246.963556	7999.918893	13.445005	-0.051741	4.815531
246.802607	7999.886384	13.450010	-0.051711	4.815522
246.642871	7999.904088	13.455015	-0.051681	4.815528
247.050816	7999.954551	13.460019	-0.051758	4.815541
246.826497	7999.906055	13.465024	-0.051716	4.815528
246.978234	7999.901075	13.470029	-0.051744	4.815525
247.053139	7999.961055	13.475034	-0.051759	4.815542
246.602536	7999.900324	13.480039	-0.051675	4.815527
246.704970	7999.954344	13.485043	-0.051694	4.815542
246.807703	7999.907983	13.490048	-0.051714	4.815528
246.870539	7999.883397	13.495053	-0.051726	4.815521
246.799195	7999.923902	13.500058	-0.051712	4.815533
246.883179	7999.905001	13.505063	-0.051728	4.815527
246.887716	7999.949949	13.510067	-0.051729	4.815540
246.577434	7999.940633	13.515072	-0.051672	4.815539
246.681750	7999.920996	13.520077	-0.051692	4.815532
246.724490	7999.956956	13.525082	-0.051700	4.815543
246.722264	7999.913153	13.530087	-0.051699	4.815530
246.781372	7999.935496	13.535091	-0.051711	4.815536
246.925444	7999.979517	13.540096	-0.051738	4.815548
247.093644	7999.949175	13.545101	-0.051769	4.815539
247.101335	7999.968544	13.550106	-0.051771	4.815544
246.724932	7999.898343	13.555111	-0.051701	4.815526
246.996385	7999.956190	13.560115	-0.051752	4.815541
246.790205	7999.889836	13.565120	-0.051714	4.815523
246.725511	7999.871712	13.570125	-0.051702	4.815518
246.795117	7999.948692	13.575130	-0.051715	4.815540
246.689747	7999.942721	13.580135	-0.051696	4.815539
246.795848	7999.869715	13.585139	-0.051716	4.815517
246.875263	7999.868895	13.590144	-0.051731	4.815516
246.879676	7999.911704	13.595149	-0.051732	4.815529
246.831437	7999.907733	13.600154	-0.051723	4.815528
246.610591	7999.922304	13.605159	-0.051682	4.815533
246.748141	7999.936315	13.610163	-0.051708	4.815537
246.698712	7999.905626	13.615168	-0.051699	4.815528
246.668646	7999.851757	13.620173	-0.051693	4.815512
246.830038	7999.924895	13.625178	-0.051724	4.815533
246.784374	7999.933781	13.630183	-0.051716	4.815536
246.742318	7999.900008	13.635187	-0.051708	4.815526
246.650903	7999.873973	13.640192	-0.051691	4.815519
246.905751	7999.982811	13.645197	-0.051739	4.815549
246.850053	7999.909301	13.650202	-0.051729	4.815528
246.531856	7999.893448	13.655207	-0.051670	4.815525
246.503470	7999.883393	13.660211	-0.051665	4.815522
246.639650	7999.906994	13.665216	-0.051690	4.815528
246.628319	7999.889741	13.670221	-0.051688	4.815523
246.670010	7999.925684	13.675226	-0.051696	4.815534
246.689509	7999.954856	13.680231	-0.051700	4.815542
246.659660	7999.876428	13.685235	-0.051695	4.815519
246.670323	7999.862738	13.690240	-0.051697	4.815515
246.681106	7999.897108	13.695245	-0.051699	4.815525
246.704276	7999.880419	13.700250	-0.051704	4.815520
246.838779	7999.903992	13.705255	-0.051729	4.815527
246.884632	7999.911168	13.710259	-0.051738	4.815528
246.894228	8000.014936	13.715264	-0.051740	4.815559
246.769461	7999.907192	13.720269	-0.051717	4.815528
246.645401	7999.851789	13.725274	-0.051694	4.815512
246.564872	7999.859038	13.730279	-0.051679	4.815515
246.752900	7999.957174	13.735283	-0.051714	4.815542
246.464274	7999.845689	13.740288	-0.051661	4.815511
246.599006	7999.946158	13.745293	-0.051686	4.815540
246.708558	7999.875345	13.750298	-0.051707	4.815519
246.661479	7999.869256	13.755303	-0.051698	4.815517
246.777274	7999.930971	13.760307	-0.051720	4.815535
246.499884	7999.888018	13.765312	-0.051669	4.815523
246.609216	7999.917588	13.770317	-0.051689	4.815532
246.817803	7999.927419	13.775322	-0.051728	4.815533
246.814331	8000.000003	13.780327	-0.051728	4.815555
246.862133	7999.906823	13.785331	-0.051737	4.815527
246.916635	7999.875693	13.790336	-0.051747	4.815518
247.114628	7999.918459	13.795341	-0.051784	4.815529
246.754205	7999.923275	13.800346	-0.051718	4.815532
246.747892	7999.864455	13.805351	-0.051717	4.815515
246.737722	7999.972172	13.810355	-0.051715	4.815547
246.678963	7999.890068	13.815360	-0.051704	4.815523
246.813421	7999.881602	13.820365	-0.051729	4.815520
246.717680	7999.953748	13.825370	-0.051712	4.815542
246.585383	7999.916366	13.830375	-0.051687	4.815531
246.727337	7999.929382	13.835379	-0.051714	4.815534
246.567256	7999.985527	13.840384	-0.051685	4.815552
246.848281	7999.875861	13.845389	-0.051737	4.815518
246.852867	7999.944305	13.850394	-0.051738	4.815538
246.647372	7999.869418	13.855399	-0.051700	4.815517
246.701032	7999.958953	13.860403	-0.051710	4.815543
246.782512	7999.936808	13.865408	-0.051726	4.815536
246.754415	7999.919281	13.870413	-0.051721	4.815531
247.005427	7999.926601	13.875418	-0.051768	4.815532
246.984174	7999.929478	13.880423	-0.051764	4.815533
246.931418	7999.936112	13.885427	-0.051754	4.815535
246.706280	8000.039253	13.890432	-0.051713	4.815567
246.818145	7999.891585	13.895437	-0.051734	4.815523
246.742216	7999.909588	13.900442	-0.051720	4.815528
246.853067	7999.856951	13.905447	-0.051741	4.815513
246.780087	7999.915585	13.910451	-0.051727	4.815530
246.682756	7999.970618	13.915456	-0.051709	4.815547
246.755576	7999.952603	13.920461	-0.051723	4.815541
246.626026	7999.908858	13.925466	-0.051699	4.815529
246.662968	7999.924432	13.930471	-0.051706	4.815533
246.918602	7999.921148	13.935475	-0.051754	4.815531
246.811468	7999.917283	13.940480	-0.051734	4.815530
246.869615	7999.952426	13.945485	-0.051746	4.815540
247.142449	7999.990006	13.950490	-0.051797	4.815550
247.082979	7999.886530	13.955495	-0.051786	4.815520
247.018902	7999.976281	13.960499	-0.051774	4.815547
246.964144	7999.963659	13.965504	-0.051764	4.815543
246.983138	7999.980008	13.970509	-0.051768	4.815548
247.029672	7999.957292	13.975514	-0.051777	4.815541
246.968754	7999.938162	13.980519	-0.051766	4.815536
247.177955	7999.989655	13.985523	-0.051805	4.815550
246.871431	8000.051953	13.990528	-0.051748	4.815569
247.010263	7999.923947	13.995533	-0.051774	4.815531
247.138557	7999.947420	14.000538	-0.051798	4.815537
246.915526	7999.897877	14.005543	-0.051757	4.815524
247.144315	7999.936873	14.010547	-0.051800	4.815534
247.035524	7999.927641	14.015552	-0.051780	4.815532
247.062559	7999.846937	14.020557	-0.051785	4.815508
247.095295	7999.926520	14.025562	-0.051791	4.815532
247.066686	7999.980539	14.030567	-0.051786	4.815547
247.351412	7999.906177	14.035571	-0.051839	4.815524
247.067645	7999.918652	14.040576	-0.051787	4.815529
247.004916	7999.908036	14.045581	-0.051775	4.815527
246.935413	7999.886630	14.050586	-0.051762	4.815521
246.929396	7999.892959	14.055591	-0.051762	4.815523
247.043795	7999.911933	14.060595	-0.051783	4.815528
247.003160	7999.913425	14.065600	-0.051776	4.815528
246.996556	7999.900522	14.070605	-0.051775	4.815524
246.995588	8000.036157	14.075610	-0.051775	4.815564
247.063333	7999.896311	14.080615	-0.051788	4.815523
247.166359	7999.931119	14.085619	-0.051807	4.815532
246.876413	7999.882620	14.090624	-0.051753	4.815520
246.901372	7999.908678	14.095629	-0.051758	4.815527
246.978441	8000.031703	14.100634	-0.051773	4.815563
246.911515	7999.872572	14.105639	-0.051760	4.815517
246.875896	7999.938224	14.110643	-0.051754	4.815536
246.992245	7999.939074	14.115648	-0.051776	4.815536
247.155261	7999.930007	14.120653	-0.051807	4.815532
246.892545	7999.923603	14.125658	-0.051758	4.815532
246.931908	7999.906109	14.130663	-0.051765	4.815526
247.162168	7999.959014	14.135667	-0.051808	4.815541
247.056457	7999.878278	14.140672	-0.051789	4.815518
246.991000	7999.913540	14.145677	-0.051777	4.815528
247.046912	7999.935832	14.150682	-0.051788	4.815534
247.024522	7999.859661	14.155687	-0.051784	4.815512
247.086355	7999.926903	14.160691	-0.051795	4.815532
247.062685	7999.887022	14.165696	-0.051791	4.815520
246.902705	7999.891906	14.170701	-0.051762	4.815522
246.931796	8000.017352	14.175706	-0.051767	4.815559
246.956411	7999.894958	14.180711	-0.051772	4.815523
247.039743	7999.882454	14.185715	-0.051788	4.815519
246.979125	7999.912455	14.190720	-0.051777	4.815528
247.006221	7999.956703	14.195725	-0.051782	4.815541
247.113345	7999.980899	14.200730	-0.051802	4.815547
247.105699	7999.928463	14.205735	-0.051801	4.815532
247.002676	7999.963112	14.210739	-0.051782	4.815542
246.960896	7999.910120	14.215744	-0.051775	4.815527
247.113460	7999.885930	14.220749	-0.051803	4.815519
247.298770	8000.004316	14.225754	-0.051838	4.815553
247.098870	7999.940197	14.230759	-0.051801	4.815535
247.002242	7999.973883	14.235763	-0.051783	4.815546
246.893964	7999.975339	14.240768	-0.051763	4.815547
247.044350	7999.967133	14.245773	-0.051791	4.815543
247.182198	7999.962995	14.250778	-0.051817	4.815542
247.213874	7999.911202	14.255783	-0.051823	4.815526
247.097894	7999.934959	14.260787	-0.051802	4.815534
247.064442	7999.920549	14.265792	-0.051796	4.815530
247.039543	7999.662785	14.270797	-0.051791	4.815454

246.966971	7996.408977	14.275802	-0.051776	4.814503
246.814473	7990.788013	14.280807	-0.051744	4.812860
247.161684	7984.028929	14.285811	-0.051805	4.810881
246.941085	7976.674873	14.290816	-0.051759	4.808730
246.798474	7969.067445	14.295821	-0.051728	4.806503
246.898185	7961.224409	14.300826	-0.051741	4.804205
246.906997	7953.370935	14.305831	-0.051738	4.801903
246.953839	7945.363205	14.310835	-0.051742	4.799555
246.872933	7937.461754	14.315840	-0.051722	4.797237
246.912824	7929.434068	14.320845	-0.051724	4.794880
246.959195	7921.448677	14.325850	-0.051728	4.792535
246.642799	7913.343045	14.330855	-0.051664	4.790155
246.722459	7905.442497	14.335859	-0.051674	4.787832
246.450069	7897.361534	14.340864	-0.051618	4.785457
246.406844	7889.405565	14.345869	-0.051605	4.783116
246.371092	7881.424990	14.350874	-0.051594	4.780766
246.316774	7873.397249	14.355879	-0.051578	4.778402
246.329755	7865.437938	14.360883	-0.051576	4.776057
246.369234	7857.363256	14.365888	-0.051578	4.773676
246.337583	7849.348831	14.370893	-0.051567	4.771312
246.456299	7841.360370	14.375898	-0.051584	4.768954
246.443420	7833.394290	14.380903	-0.051577	4.766602
246.384566	7825.344962	14.385907	-0.051561	4.764224
246.300103	7817.434549	14.390912	-0.051540	4.761886
246.234306	7809.340401	14.395917	-0.051523	4.759493
246.288378	7801.422642	14.400922	-0.051528	4.757150
246.250541	7793.356946	14.405927	-0.051516	4.754763
246.168245	7785.335931	14.410931	-0.051496	4.752387
246.208426	7777.300290	14.415936	-0.051498	4.750006
246.235361	7769.306433	14.420941	-0.051498	4.747636
246.182522	7761.365182	14.425946	-0.051484	4.745281
245.893604	7753.298191	14.430951	-0.051425	4.742888
246.051868	7745.350315	14.435955	-0.051449	4.740528
246.128124	7737.351941	14.440960	-0.051458	4.738152
245.736690	7729.307828	14.445965	-0.051381	4.735762
245.971651	7721.355808	14.450970	-0.051419	4.733397
245.792649	7713.299931	14.455975	-0.051381	4.731001
245.852751	7705.305986	14.460979	-0.051387	4.728621
245.734848	7697.331217	14.465984	-0.051360	4.726247
245.668774	7689.248879	14.470989	-0.051343	4.723839
245.768121	7681.382569	14.475994	-0.051356	4.721493
245.516969	7673.296378	14.480999	-0.051305	4.719082
245.527584	7665.361964	14.486003	-0.051302	4.716715
245.369821	7657.338189	14.491008	-0.051267	4.714319
245.425838	7649.261721	14.496013	-0.051273	4.711907
245.389484	7641.303550	14.501018	-0.051261	4.709528
245.486278	7633.260644	14.506023	-0.051274	4.707123
245.536911	7625.285125	14.511027	-0.051278	4.704737
245.646575	7617.300502	14.516032	-0.051294	4.702347
245.598942	7609.338628	14.521037	-0.051280	4.699963
245.431647	7601.336269	14.526042	-0.051244	4.697565
245.144095	7593.290437	14.531047	-0.051185	4.695154
245.216746	7585.304193	14.536051	-0.051194	4.692758
245.266001	7577.258420	14.541056	-0.051198	4.690344
245.109203	7569.288332	14.546061	-0.051164	4.687951
244.985993	7561.310104	14.551066	-0.051136	4.685554
244.876520	7553.314282	14.556071	-0.051111	4.683151
245.022933	7545.286608	14.561075	-0.051133	4.680737
244.912147	7537.284533	14.566080	-0.051107	4.678330
244.796552	7529.331189	14.571085	-0.051081	4.675936
245.079880	7521.242918	14.576090	-0.051128	4.673499
244.930347	7513.113295	14.581095	-0.051096	4.671050
244.848548	7505.227440	14.586099	-0.051075	4.668673
244.630226	7497.200213	14.591104	-0.051030	4.666251
244.594880	7489.186242	14.596109	-0.051018	4.663833
244.863682	7481.280960	14.601114	-0.051063	4.661445
244.810035	7473.233845	14.606119	-0.051048	4.659014
244.746857	7465.297281	14.611123	-0.051032	4.656615
244.695009	7457.222454	14.616128	-0.051017	4.654173
244.528735	7449.235102	14.621133	-0.050981	4.651757
244.821091	7441.187276	14.626138	-0.051030	4.649320
244.631833	7433.202073	14.631143	-0.050990	4.646901
244.609575	7425.206064	14.636147	-0.050981	4.644478
244.636342	7417.267878	14.641152	-0.050981	4.642071
244.479607	7409.175001	14.646157	-0.050947	4.639616
244.432907	7401.275876	14.651162	-0.050933	4.637218
244.344889	7393.235887	14.656167	-0.050912	4.634776
244.180774	7385.215475	14.661171	-0.050876	4.632339
244.206463	7377.135941	14.666176	-0.050876	4.629883
244.081268	7369.178534	14.671181	-0.050848	4.627462
244.264877	7361.182539	14.676186	-0.050877	4.625029
244.105161	7353.185335	14.681191	-0.050842	4.622594
244.179148	7345.191502	14.686195	-0.050851	4.620158
243.970451	7337.221238	14.691200	-0.050807	4.617729
244.168843	7329.208219	14.696205	-0.050839	4.615285
244.087014	7321.173833	14.701210	-0.050819	4.612833
243.879293	7313.119263	14.706215	-0.050775	4.610374
243.883811	7305.168081	14.711219	-0.050771	4.607945
243.748366	7297.159923	14.716224	-0.050741	4.605497
243.692703	7289.179488	14.721229	-0.050725	4.603057
243.826455	7281.199029	14.726234	-0.050745	4.600615
243.527093	7273.151945	14.731239	-0.050685	4.598151
243.521991	7265.194464	14.736243	-0.050679	4.595714
243.544944	7257.133210	14.741248	-0.050678	4.593244
243.446468	7249.079571	14.746253	-0.050655	4.590774
243.332907	7241.151409	14.751258	-0.050628	4.588342
243.411022	7233.100988	14.756263	-0.050638	4.585871
243.512437	7225.145275	14.761267	-0.050652	4.583428
243.497090	7217.083366	14.766272	-0.050644	4.580950
243.230216	7209.155468	14.771277	-0.050589	4.578513
243.238189	7201.197592	14.776282	-0.050586	4.576065
243.227119	7193.148717	14.781287	-0.050579	4.573587
243.377837	7185.118867	14.786291	-0.050602	4.571115
243.243816	7177.115608	14.791296	-0.050572	4.568649
243.195009	7169.122482	14.796301	-0.050558	4.566184
243.215008	7161.134435	14.801306	-0.050557	4.563720
243.105713	7153.140118	14.806311	-0.050531	4.561253
243.074853	7145.146802	14.811315	-0.050521	4.558785
242.813482	7137.165958	14.816320	-0.050467	4.556319
242.712171	7129.098922	14.821325	-0.050443	4.553825
242.990856	7121.117219	14.826330	-0.050490	4.551357
242.806403	7113.076571	14.831335	-0.050451	4.548868
242.771928	7105.098067	14.836339	-0.050439	4.546398
242.737668	7097.080599	14.841344	-0.050428	4.543914
242.858724	7089.127062	14.846349	-0.050445	4.541449
242.701867	7081.136174	14.851354	-0.050411	4.538970
242.612958	7073.126172	14.856359	-0.050390	4.536484
242.743914	7065.158421	14.861363	-0.050409	4.534011
242.748194	7057.095327	14.866368	-0.050405	4.531506
242.533514	7049.053225	14.871373	-0.050360	4.529006
242.707003	7041.156498	14.876378	-0.050387	4.526551
242.498353	7033.083142	14.881383	-0.050343	4.524038
242.426444	7025.133666	14.886387	-0.050325	4.521563
242.319963	7017.113690	14.891392	-0.050300	4.519064
242.399707	7009.136828	14.896397	-0.050310	4.516578
242.419598	7001.104755	14.901402	-0.050309	4.514073
242.290373	6992.966311	14.906407	-0.050280	4.511534
242.201259	6985.052113	14.911411	-0.050258	4.509063
242.227927	6977.067381	14.916416	-0.050258	4.506568
242.137133	6969.049135	14.921421	-0.050236	4.504062
242.107442	6961.088751	14.926426	-0.050226	4.501573
242.015028	6953.069516	14.931431	-0.050203	4.499063
242.157065	6945.094511	14.936435	-0.050225	4.496567
241.989607	6937.041109	14.941440	-0.050189	4.494044
242.038719	6929.021095	14.946445	-0.050193	4.491530
242.196137	6921.030375	14.951450	-0.050217	4.489025
242.081875	6913.055728	14.956455	-0.050191	4.486522
242.000019	6905.066364	14.961459	-0.050171	4.484014
242.008388	6897.077594	14.966464	-0.050167	4.481504
241.886661	6889.049992	14.971469	-0.050140	4.478981
241.786441	6881.105143	14.976474	-0.050116	4.476482
242.006974	6873.046203	14.981479	-0.050152	4.473947
241.818034	6865.030022	14.986483	-0.050112	4.471422
241.705052	6857.011644	14.991488	-0.050086	4.468896
241.643660	6849.043797	14.996493	-0.050069	4.466384
241.635270	6841.030360	15.001498	-0.050063	4.463857
241.571353	6833.005319	15.006503	-0.050046	4.461324
241.566654	6825.037532	15.011507	-0.050040	4.458809
241.666323	6817.064074	15.016512	-0.050054	4.456290
241.384867	6809.020865	15.021517	-0.049996	4.453747
241.491329	6801.008036	15.026522	-0.050011	4.451213
241.352670	6792.990074	15.031527	-0.049980	4.448675
241.441290	6785.007290	15.036531	-0.049992	4.446148
241.352685	6776.999846	15.041536	-0.049970	4.443610
241.239146	6769.013108	15.046541	-0.049944	4.441078
241.467974	6761.009570	15.051546	-0.049982	4.438541
241.351480	6753.021213	15.056551	-0.049955	4.436005
241.464210	6744.998873	15.061555	-0.049971	4.433458
241.178093	6736.947494	15.066560	-0.049913	4.430899
241.020912	6728.966768	15.071565	-0.049878	4.428361
241.181363	6720.970340	15.076570	-0.049903	4.425818
240.928497	6712.969870	15.081575	-0.049851	4.423270
240.934806	6704.985905	15.086579	-0.049847	4.420728
240.953333	6696.991660	15.091584	-0.049846	4.418181
240.883939	6688.967161	15.096589	-0.049828	4.415622
240.867333	6681.003269	15.101594	-0.049820	4.413081
240.900799	6672.924875	15.106599	-0.049821	4.410503
240.865948	6664.971511	15.111603	-0.049810	4.407962
240.927929	6656.994817	15.116608	-0.049816	4.405413
240.957268	6648.980310	15.121613	-0.049817	4.402851
240.842052	6641.001150	15.126618	-0.049790	4.400297
240.686883	6632.969822	15.131623	-0.049756	4.397725
240.734196	6624.984650	15.136627	-0.049760	4.395168
240.617956	6617.013736	15.141632	-0.049734	4.392613
240.546965	6608.906585	15.146637	-0.049715	4.390012
240.728976	6600.977831	15.151642	-0.049744	4.387469
240.303239	6592.951624	15.156647	-0.049660	4.384890
240.255256	6585.014866	15.161651	-0.049646	4.382340
240.210851	6576.999190	15.166656	-0.049633	4.379763
240.412326	6568.988605	15.171661	-0.049665	4.377187
240.260556	6561.011505	15.176666	-0.049632	4.374619
240.322007	6552.969263	15.181671	-0.049639	4.372030
240.338209	6544.965557	15.186675	-0.049637	4.369451
240.191492	6536.974527	15.191680	-0.049604	4.366874
240.154508	6528.949400	15.196685	-0.049592	4.364285
240.126254	6521.049754	15.201690	-0.049582	4.361735
240.239373	6512.976088	15.206695	-0.049598	4.359128
239.977194	6505.031527	15.211699	-0.049544	4.356559
239.978984	6496.968717	15.216704	-0.049540	4.353952
239.958168	6488.867793	15.221709	-0.049531	4.351330
240.015490	6480.889709	15.226714	-0.049537	4.348748
239.785957	6472.914561	15.231719	-0.049489	4.346163
240.051365	6464.908912	15.236723	-0.049533	4.343570
239.897789	6456.968719	15.241728	-0.049500	4.340993
239.558725	6448.962228	15.246733	-0.049432	4.338393
239.703069	6441.016651	15.251738	-0.049453	4.335814
239.780725	6432.955198	15.256743	-0.049463	4.333195
239.333566	6424.934036	15.261747	-0.049375	4.330584
239.340645	6416.984660	15.266752	-0.049371	4.327998
239.481048	6408.945034	15.271757	-0.049392	4.325382
239.519793	6400.952744	15.276762	-0.049394	4.322779
239.305343	6392.942246	15.281767	-0.049349	4.320167
239.334261	6384.973257	15.286771	-0.049350	4.317569
239.237078	6376.931609	15.291776	-0.049327	4.314944
239.266743	6368.906303	15.296781	-0.049327	4.312324
239.381926	6360.931640	15.301786	-0.049344	4.309720
239.339031	6352.911059	15.306791	-0.049331	4.307097
239.324276	6344.934795	15.311795	-0.049323	4.304488
239.108048	6336.960571	15.316800	-0.049278	4.301877
239.095029	6328.907282	15.321805	-0.049270	4.299239
238.846526	6320.955155	15.326810	-0.049219	4.296632
238.863513	6312.891993	15.331815	-0.049217	4.293988
239.234943	6304.894484	15.336819	-0.049281	4.291367
239.148482	6296.888400	15.341824	-0.049260	4.288738
238.894257	6288.894328	15.346829	-0.049208	4.286110
238.980465	6280.934642	15.351834	-0.049219	4.283494
238.785352	6272.908195	15.356839	-0.049178	4.280853
238.865683	6264.943258	15.361843	-0.049188	4.278232
238.789689	6256.948360	15.366848	-0.049169	4.275599
238.900196	6248.887265	15.371853	-0.049184	4.272943
238.851202	6240.842903	15.376858	-0.049170	4.270291
238.575980	6232.889959	15.381863	-0.049114	4.267664
238.616271	6224.882571	15.386867	-0.049116	4.265021
238.581057	6216.890668	15.391872	-0.049105	4.262381
238.560709	6208.865567	15.396877	-0.049096	4.259728
238.422086	6200.934572	15.401882	-0.049065	4.257104
238.348110	6192.871901	15.406887	-0.049046	4.254435
238.428264	6184.890181	15.411891	-0.049056	4.251792
238.492111	6176.881828	15.416896	-0.049063	4.249139
238.391527	6168.876472	15.421901	-0.049040	4.246484
238.345933	6160.946114	15.426906	-0.049026	4.243853
238.205449	6152.933143	15.431911	-0.048995	4.241191
238.360605	6144.967553	15.436915	-0.049019	4.238546
238.323841	6136.961697	15.441920	-0.049007	4.235885
238.241402	6128.884336	15.446925	-0.048987	4.233197
238.357604	6120.895440	15.451930	-0.049003	4.230540
238.396407	6112.894115	15.456935	-0.049006	4.227875
238.302324	6104.917673	15.461939	-0.048983	4.225216
238.069999	6096.976614	15.466944	-0.048935	4.222566
238.068383	6088.928976	15.471949	-0.048929	4.219881
238.081461	6080.972025	15.476954	-0.048927	4.217224
237.970865	6072.930421	15.481959	-0.048901	4.214537
237.999542	6064.887883	15.486963	-0.048902	4.211848
238.058324	6056.926988	15.491968	-0.048908	4.209186
237.910858	6048.925272	15.496973	-0.048875	4.206506
237.895661	6040.940451	15.501978	-0.048867	4.203831
237.554968	6032.920623	15.506983	-0.048799	4.201140
237.954395	6024.933036	15.511987	-0.048868	4.198465
237.842452	6016.954489	15.516992	-0.048843	4.195787
237.788690	6008.835177	15.521997	-0.048827	4.193059
237.808921	6000.833048	15.527002	-0.048826	4.190371
237.693411	5992.833005	15.532007	-0.048800	4.187680
237.704830	5984.878567	15.537011	-0.048797	4.185003
237.761992	5976.938850	15.542016	-0.048803	4.182331
237.536592	5968.868021	15.547021	-0.048756	4.179610
237.435904	5960.937301	15.552026	-0.048732	4.176935
237.290814	5952.892906	15.557031	-0.048700	4.174220
237.349683	5944.892303	15.562035	-0.048706	4.171520
237.377962	5936.881258	15.567040	-0.048706	4.168814
237.278926	5928.860321	15.572045	-0.048683	4.166102
237.329661	5920.915234	15.577050	-0.048687	4.163416
237.174701	5912.914050	15.582055	-0.048653	4.160706
237.176307	5904.933962	15.587059	-0.048649	4.158004
237.286386	5896.920321	15.592064	-0.048664	4.155289
237.268869	5888.864771	15.597069	-0.048656	4.152558
237.113947	5880.845095	15.602074	-0.048622	4.149835
237.240573	5872.841997	15.607079	-0.048641	4.147119
237.212596	5864.863340	15.612083	-0.048630	4.144408
237.053466	5856.915698	15.617088	-0.048596	4.141704
236.876896	5848.868443	15.622093	-0.048558	4.138964
236.869521	5840.916777	15.627098	-0.048552	4.136257
236.569403	5832.891118	15.632103	-0.048491	4.133519
236.808801	5824.861385	15.637107	-0.048530	4.130785
236.736385	5816.861985	15.642112	-0.048512	4.128055
236.562939	5808.850591	15.647117	-0.048474	4.125319
236.586354	5800.934183	15.652122	-0.048474	4.122615
236.515573	5792.879447	15.657127	-0.048456	4.119861
236.549694	5784.935723	15.662131	-0.048457	4.117145
236.465114	5776.931466	15.667136	-0.048436	4.114404
236.374114	5768.859922	15.672141	-0.048414	4.111639
236.519187	5760.855948	15.677146	-0.048436	4.108897
236.501655	5752.857079	15.682151	-0.048428	4.106154
236.294221	5744.855374	15.687155	-0.048385	4.103406
236.305060	5736.894356	15.692160	-0.048382	4.100672
236.016574	5728.891179	15.697165	-0.048323	4.097918
236.126764	5720.920685	15.702170	-0.048338	4.095179
236.154615	5712.859834	15.707175	-0.048339	4.092405
236.292969	5704.851773	15.712179	-0.048359	4.089650
236.164307	5696.919365	15.717184	-0.048330	4.086915
236.109744	5688.871719	15.722189	-0.048315	4.084140
236.158444	5680.969288	15.727194	-0.048319	4.081414
235.904905	5672.944097	15.732199	-0.048267	4.078640
235.817043	5664.956664	15.737203	-0.048246	4.075879
236.192305	5656.874741	15.742208	-0.048311	4.073090
236.027712	5648.856192	15.747213	-0.048275	4.070314
235.766562	5640.954402	15.752218	-0.048221	4.067574
235.675104	5632.924076	15.757223	-0.048199	4.064791
235.771459	5624.939279	15.762227	-0.048212	4.062024
235.862768	5616.914216	15.767232	-0.048224	4.059242
235.828097	5608.961891	15.772237	-0.048213	4.056481
236.030687	5600.939517	15.777242	-0.048246	4.053697
235.525961	5592.898363	15.782247	-0.048147	4.050894
235.468733	5584.908739	15.787251	-0.048131	4.048114
235.599336	5576.899651	15.792256	-0.048150	4.045328
235.556304	5568.925813	15.797261	-0.048137	4.042550
235.462310	5560.946228	15.802266	-0.048115	4.039767
235.501676	5552.986150	15.807271	-0.048117	4.036991
235.580812	5544.913594	15.812275	-0.048127	4.034174
235.359864	5536.790844	15.817280	-0.048081	4.031333
235.418229	5528.836767	15.822285	-0.048087	4.028554
235.379410	5520.871884	15.827290	-0.048074	4.025767
235.284965	5512.886449	15.832295	-0.048052	4.022970
235.283812	5504.878447	15.837299	-0.048047	4.020165
235.195089	5496.957376	15.842304	-0.048025	4.017387
235.105047	5488.934230	15.847309	-0.048003	4.014571
235.012842	5480.899962	15.852314	-0.047981	4.011750
234.930062	5472.860308	15.857319	-0.047961	4.008924
235.115981	5464.900384	15.862323	-0.047991	4.006129
235.097423	5456.925025	15.867328	-0.047982	4.003323
234.922352	5448.876382	15.872333	-0.047944	4.000487
235.120955	5440.960009	15.877338	-0.047977	3.997702
234.894158	5432.936644	15.882343	-0.047929	3.994870
234.529525	5424.892676	15.887347	-0.047856	3.992026
234.612792	5416.867508	15.892352	-0.047867	3.989195
234.596806	5408.883533	15.897357	-0.047859	3.986374
234.642435	5400.885579	15.902362	-0.047862	3.983547
234.440349	5392.897817	15.907367	-0.047820	3.980718
234.547235	5384.920710	15.912371	-0.047835	3.977896
234.660925	5376.923359	15.917376	-0.047851	3.975065
234.395769	5368.901185	15.922381	-0.047797	3.972216
234.573736	5360.877893	15.927386	-0.047825	3.969373
234.446165	5352.940793	15.932391	-0.047796	3.966553
234.639240	5344.927272	15.937395	-0.047827	3.963709
234.644037	5336.978520	15.942400	-0.047823	3.960883
234.494451	5328.991152	15.947405	-0.047790	3.958038
234.519076	5320.983616	15.952410	-0.047790	3.955187
234.209492	5312.893020	15.957415	-0.047727	3.952299
234.469026	5304.881301	15.962419	-0.047770	3.949447
234.314771	5296.933186	15.967424	-0.047737	3.946608
234.091715	5288.963663	15.972429	-0.047690	3.943758
234.075919	5281.000227	15.977434	-0.047682	3.940912
233.899062	5272.967650	15.982439	-0.047644	3.938037
233.995434	5265.015477	15.987443	-0.047657	3.935193
233.982662	5256.951610	15.992448	-0.047650	3.932304
233.893488	5248.912323	15.997453	-0.047628	3.929422
234.022671	5240.987174	16.002458	-0.047647	3.926582
233.719801	5232.999159	16.007463	-0.047586	3.923709
233.734149	5225.023595	16.012467	-0.047584	3.920845
233.812724	5216.991543	16.017472	-0.047593	3.917959
233.682703	5208.968257	16.022477	-0.047564	3.915070
233.910976	5200.958543	16.027482	-0.047602	3.912191
233.608513	5192.943904	16.032487	-0.047540	3.909298
233.541543	5184.990657	16.037491	-0.047523	3.906430
233.472021	5177.002763	16.042496	-0.047505	3.903547
233.377839	5168.971960	16.047501	-0.047482	3.900645
233.629054	5161.031872	16.052506	-0.047524	3.897781
233.375101	5152.982527	16.057511	-0.047472	3.894866
233.287435	5144.961599	16.062515	-0.047450	3.891962
233.367161	5136.952487	16.067520	-0.047460	3.889063
233.090542	5129.001844	16.072525	-0.047404	3.886177
233.250383	5120.992645	16.077530	-0.047429	3.883275
233.072534	5112.973915	16.082535	-0.047391	3.880361
233.095113	5105.026991	16.087539	-0.047390	3.877475
233.070681	5097.000941	16.092544	-0.047380	3.874557
233.163445	5088.724955	16.097549	-0.047392	3.871549
233.295747	5080.844133	16.102554	-0.047412	3.868682
233.075375	5072.886384	16.107559	-0.047366	3.865779
232.718182	5064.939631	16.112563	-0.047295	3.862875
232.935940	5056.902446	16.117568	-0.047330	3.859946
232.786702	5048.958155	16.122573	-0.047297	3.857043
232.643612	5040.978583	16.127578	-0.047266	3.854124
232.657015	5032.951213	16.132583	-0.047263	3.851189
232.622766	5024.953082	16.137587	-0.047252	3.848261
232.626907	5016.989589	16.142592	-0.047248	3.845344
232.564118	5009.009499	16.147597	-0.047231	3.842418
232.627112	5001.027596	16.152602	-0.047238	3.839491
232.192869	4993.073870	16.157607	-0.047152	3.836563
232.409424	4985.043682	16.162611	-0.047187	3.833617
232.465965	4977.011696	16.167616	-0.047193	3.830665
232.560888	4968.994720	16.172621	-0.047205	3.827717
232.681042	4960.999393	16.177626	-0.047223	3.824776
232.548143	4953.034859	16.182631	-0.047193	3.821838
232.352312	4945.056444	16.187635	-0.047152	3.818891
232.516613	4937.075302	16.192640	-0.047177	3.815949
232.317886	4929.048639	16.197645	-0.047135	3.812980
232.357347	4921.038946	16.202650	-0.047138	3.810020
232.345833	4913.072185	16.207655	-0.047131	3.807073
232.125308	4905.060626	16.212659	-0.047084	3.804102
232.360522	4897.111191	16.217664	-0.047123	3.801162
232.062123	4889.095750	16.222669	-0.047063	3.798183
232.146636	4881.103609	16.227674	-0.047073	3.795219
231.976771	4873.049588	16.232679	-0.047037	3.792224
231.990040	4865.023012	16.237683	-0.047034	3.789241
232.055353	4857.060054	16.242688	-0.047041	3.786280
231.926061	4849.075562	16.247693	-0.047012	3.783305
232.062297	4841.051296	16.252698	-0.047033	3.780318
231.825434	4833.081765	16.257703	-0.046984	3.777342
231.886532	4825.057946	16.262707	-0.046990	3.774349
231.798309	4817.083796	16.267712	-0.046969	3.771369
231.680294	4809.066037	16.272717	-0.046942	3.768370
231.571070	4801.081714	16.277722	-0.046916	3.765381
231.396024	4793.107818	16.282727	-0.046879	3.762392
231.477666	4785.067919	16.287731	-0.046889	3.759381
231.503231	4777.143593	16.292736	-0.046889	3.756411
231.583969	4769.062439	16.297741	-0.046899	3.753380
231.644533	4761.071301	16.302746	-0.046905	3.750381
231.390577	4753.112755	16.307751	-0.046853	3.747384
231.539791	4745.055874	16.312755	-0.046876	3.744356
231.274444	4737.133377	16.317760	-0.046821	3.741368
231.263831	4729.111042	16.322765	-0.046814	3.738345
231.278589	4721.115955	16.327770	-0.046812	3.735331
231.035020	4713.108916	16.332775	-0.046762	3.732303
230.976785	4705.100041	16.337779	-0.046746	3.729277
231.162172	4697.157336	16.342784	-0.046775	3.726279
230.991442	4689.140544	16.347789	-0.046739	3.723243
231.147332	4681.167176	16.352794	-0.046763	3.720228
230.992923	4673.173176	16.357799	-0.046729	3.717195
231.005104	4665.180811	16.362803	-0.046726	3.714164
230.929708	4657.074818	16.367808	-0.046707	3.711086
230.762105	4649.062896	16.372813	-0.046671	3.708039
230.845604	4641.120959	16.377818	-0.046682	3.705022
230.609177	4633.184154	16.382823	-0.046633	3.701996
230.685746	4625.163836	16.387827	-0.046642	3.698944
230.587617	4617.220515	16.392832	-0.046619	3.695915
230.364982	4609.183119	16.397837	-0.046572	3.692843
230.458269	4601.169294	16.402842	-0.046584	3.689787
230.586936	4593.174439	16.407847	-0.046603	3.686736
230.535742	4585.197260	16.412851	-0.046589	3.683684
230.548434	4577.230626	16.417856	-0.046586	3.680636
230.402197	4569.237191	16.422861	-0.046554	3.677571
230.302856	4561.235956	16.427866	-0.046531	3.674501
230.249830	4553.213134	16.432871	-0.046516	3.671422
230.338997	4545.194008	16.437875	-0.046527	3.668345
230.163744	4537.227025	16.442880	-0.046490	3.665279
230.105123	4529.215897	16.447885	-0.046474	3.662196
230.347844	4521.232446	16.452890	-0.046514	3.659130
230.184280	4513.249210	16.457895	-0.046479	3.656050
230.085671	4505.240828	16.462899	-0.046455	3.652959
230.088825	4497.192686	16.467904	-0.046451	3.649853
230.088847	4489.200899	16.472909	-0.046446	3.646767
229.903641	4481.233474	16.477914	-0.046406	3.643682
229.781148	4473.252424	16.482919	-0.046379	3.640591
230.156371	4465.256665	16.487923	-0.046444	3.637505
230.112477	4457.259574	16.492928	-0.046430	3.634404
229.758387	4449.227361	16.497933	-0.046359	3.631279
230.081288	4441.217683	16.502938	-0.046415	3.628178
229.922543	4433.234763	16.507943	-0.046380	3.625072
229.839738	4425.291951	16.512947	-0.046360	3.621981
229.713694	4417.285242	16.517952	-0.046331	3.618861
229.696282	4409.274629	16.522957	-0.046323	3.615740
229.818964	4401.275443	16.527962	-0.046341	3.612625
229.500584	4393.272812	16.532967	-0.046276	3.609493
229.608922	4385.307644	16.537971	-0.046292	3.606385
229.593885	4377.307008	16.542976	-0.046284	3.603257
229.359828	4369.344150	16.547981	-0.046235	3.600135
229.301222	4361.396446	16.552986	-0.046219	3.597021
229.381433	4353.353313	16.557991	-0.046229	3.593871
229.118561	4345.330006	16.562995	-0.046175	3.590716
229.337651	4337.331488	16.568000	-0.046211	3.587582
229.328345	4329.332598	16.573005	-0.046205	3.584439
229.067044	4321.421730	16.578010	-0.046151	3.581320
228.927205	4313.374262	16.583015	-0.046120	3.578148
229.150464	4305.374788	16.588019	-0.046156	3.575002
229.051284	4297.394803	16.593024	-0.046133	3.571853
228.985251	4289.360967	16.598029	-0.046116	3.568680
229.139893	4281.392310	16.603034	-0.046140	3.565536
229.206604	4273.403962	16.608039	-0.046147	3.562380
229.065813	4265.404124	16.613043	-0.046116	3.559210
228.915291	4257.474443	16.618048	-0.046083	3.556064
228.626319	4249.348061	16.623053	-0.046024	3.552834
228.679415	4241.320069	16.628058	-0.046029	3.549650
228.654505	4233.348309	16.633063	-0.046019	3.546483
228.520817	4225.384779	16.638067	-0.045989	3.543313
228.601174	4217.397445	16.643072	-0.045999	3.540137
228.477338	4209.403648	16.648077	-0.045971	3.536950
228.395475	4201.431168	16.653082	-0.045951	3.533770
228.288178	4193.420124	16.658087	-0.045926	3.530570
228.398035	4185.424904	16.663091	-0.045942	3.527381
228.545269	4177.409822	16.668096	-0.045964	3.524182
228.198588	4169.476328	16.673101	-0.045894	3.520997
228.331170	4161.493226	16.678106	-0.045914	3.517805
228.409396	4153.456085	16.683111	-0.045924	3.514586
228.623232	4145.453958	16.688115	-0.045959	3.511382
228.547343	4137.466621	16.693120	-0.045939	3.508173
228.212016	4129.447681	16.698125	-0.045872	3.504940
228.158912	4121.522251	16.703130	-0.045857	3.501750
228.083020	4113.520588	16.708135	-0.045838	3.498526
227.979386	4105.533147	16.713139	-0.045814	3.495304
228.020962	4097.547973	16.718144	-0.045817	3.492084
227.997127	4089.508802	16.723149	-0.045807	3.488837
228.217800	4081.522031	16.728154	-0.045843	3.485617
227.920367	4073.582534	16.733159	-0.045783	3.482396
227.999442	4065.572273	16.738163	-0.045793	3.479155
227.908965	4057.620580	16.743168	-0.045771	3.475930
227.682893	4049.562434	16.748173	-0.045724	3.472654
227.700832	4041.556406	16.753178	-0.045722	3.469404
227.692371	4033.563050	16.758183	-0.045715	3.466155
227.676003	4025.560951	16.763187	-0.045707	3.462899
227.544202	4017.604750	16.768192	-0.045678	3.459656
227.497908	4009.604808	16.773197	-0.045664	3.456394
227.499738	4001.605514	16.778202	-0.045660	3.453131
227.354583	3993.587422	16.783207	-0.045628	3.449852
227.454705	3985.589273	16.788211	-0.045641	3.446586
227.516209	3977.621622	16.793216	-0.045648	3.443329
227.314869	3969.630244	16.798221	-0.045605	3.440050
227.018821	3961.706822	16.803226	-0.045545	3.436792
227.034894	3953.657590	16.808231	-0.045543	3.433491
227.212212	3945.632547	16.813235	-0.045571	3.430201
227.340469	3937.627496	16.818240	-0.045590	3.426915
227.111490	3929.651073	16.823245	-0.045542	3.423625
227.141608	3921.676246	16.828250	-0.045543	3.420342
227.062785	3913.696108	16.833255	-0.045523	3.417049
227.086039	3905.691058	16.838259	-0.045523	3.413747
227.164969	3897.699708	16.843264	-0.045532	3.410449
227.120516	3889.697630	16.848269	-0.045519	3.407139
227.081340	3881.737598	16.853274	-0.045507	3.403843
227.040530	3873.772629	16.858279	-0.045494	3.400542
226.882935	3865.790574	16.863283	-0.045460	3.397227
226.755775	3857.780756	16.868288	-0.045431	3.393898
226.786089	3849.659721	16.873293	-0.045432	3.390525
226.592064	3841.734484	16.878298	-0.045391	3.387222
226.470976	3833.748696	16.883303	-0.045363	3.383893
226.372508	3825.774902	16.888307	-0.045340	3.380567
226.553105	3817.793554	16.893312	-0.045369	3.377245
226.440567	3809.790354	16.898317	-0.045343	3.373899
226.284184	3801.791421	16.903322	-0.045309	3.370550
226.372934	3793.763908	16.908327	-0.045320	3.367195
226.620784	3785.782149	16.913331	-0.045361	3.363861
226.538657	3777.847675	16.918336	-0.045341	3.360532
226.461240	3769.877569	16.923341	-0.045322	3.357185
226.526940	3761.871168	16.928346	-0.045329	3.353825
226.361610	3753.831128	16.933351	-0.045293	3.350438
226.309281	3745.841412	16.938355	-0.045278	3.347074
226.339386	3737.832606	16.943360	-0.045279	3.343701
226.093018	3729.869238	16.948365	-0.045228	3.340333
226.010189	3721.910851	16.953370	-0.045208	3.336971
225.912476	3713.916048	16.958375	-0.045185	3.333589
225.962397	3705.874435	16.963379	-0.045189	3.330189
226.108428	3697.888585	16.968384	-0.045211	3.326813
225.908693	3689.902906	16.973389	-0.045169	3.323420
225.933726	3681.965970	16.978394	-0.045169	3.320053
225.743182	3673.989266	16.983399	-0.045128	3.316658
225.650590	3665.960781	16.988403	-0.045106	3.313241
225.952315	3657.923237	16.993408	-0.045157	3.309832
225.740709	3649.946069	16.998413	-0.045113	3.306425
225.556973	3641.984986	17.003418	-0.045074	3.303023
225.390429	3633.999965	17.008423	-0.045038	3.299607
225.504331	3626.031783	17.013427	-0.045054	3.296206
225.505501	3618.019160	17.018432	-0.045049	3.292778
225.376647	3610.014184	17.023437	-0.045020	3.289345
225.444875	3602.056651	17.028442	-0.045028	3.285936
225.443990	3594.061962	17.033447	-0.045023	3.282505
225.402723	3586.070573	17.038451	-0.045010	3.279070
225.438594	3578.105982	17.043456	-0.045012	3.275646
225.285111	3570.071961	17.048461	-0.044978	3.272181
225.372842	3562.081039	17.053466	-0.044989	3.268741
225.218318	3554.097449	17.058471	-0.044956	3.265290
225.355538	3546.091367	17.063475	-0.044976	3.261838
225.303468	3538.139910	17.068480	-0.044962	3.258398
225.054281	3530.136392	17.073485	-0.044910	3.254924
225.199468	3522.129744	17.078490	-0.044932	3.251461
225.072281	3514.135089	17.083495	-0.044904	3.247989
224.957732	3506.145007	17.088499	-0.044877	3.244515
224.964616	3498.206138	17.093504	-0.044874	3.241064
224.874974	3490.210818	17.098509	-0.044852	3.237582
225.221609	3482.186452	17.103514	-0.044911	3.234100
225.074477	3474.134272	17.108519	-0.044879	3.230583
224.847627	3466.178434	17.113523	-0.044832	3.227101
225.063494	3458.172744	17.118528	-0.044867	3.223611
224.503242	3450.254795	17.123533	-0.044758	3.220124
224.630786	3442.259005	17.128538	-0.044777	3.216627
224.599608	3434.244090	17.133543	-0.044766	3.213112
224.590374	3426.247269	17.138547	-0.044759	3.209602
224.702500	3418.262647	17.143552	-0.044775	3.206098
224.471217	3410.285886	17.148557	-0.044727	3.202579
224.556332	3402.316322	17.153562	-0.044738	3.199073
224.568353	3394.331973	17.158567	-0.044735	3.195554
224.422693	3386.323367	17.163571	-0.044703	3.192013
224.182141	3378.360324	17.168576	-0.044653	3.188485
224.334952	3370.323435	17.173581	-0.044677	3.184936
224.463023	3362.364038	17.178586	-0.044695	3.181417
224.250299	3354.391927	17.183591	-0.044651	3.177874
224.216231	3346.401775	17.188595	-0.044640	3.174326
224.162613	3338.398584	17.193600	-0.044625	3.170768
223.926222	3330.406636	17.198605	-0.044576	3.167203
223.847225	3322.438694	17.203610	-0.044556	3.163652
223.578843	3314.470121	17.208615	-0.044501	3.160088
223.554172	3306.519838	17.213619	-0.044491	3.156538
223.887907	3298.438853	17.218624	-0.044549	3.152942
223.565910	3290.436506	17.223629	-0.044484	3.149348
223.463711	3282.488148	17.228634	-0.044460	3.145784
223.707668	3274.480831	17.233639	-0.044500	3.142205
223.795859	3266.485995	17.238643	-0.044511	3.138620
223.559903	3258.541861	17.243648	-0.044463	3.135040
223.612832	3250.509092	17.248653	-0.044467	3.131428
223.651526	3242.531307	17.253658	-0.044470	3.127837
223.543631	3234.556416	17.258663	-0.044445	3.124236
223.652331	3226.577594	17.263667	-0.044460	3.120639
223.420331	3218.641075	17.268672	-0.044412	3.117041
223.402876	3210.620080	17.273677	-0.044403	3.113411
223.440963	3202.598779	17.278682	-0.044406	3.109779
223.430412	3194.604076	17.283687	-0.044399	3.106152
223.176248	3186.637609	17.288691	-0.044346	3.102523
223.267941	3178.682275	17.293696	-0.044358	3.098911
223.236038	3170.695126	17.298701	-0.044347	3.095274
223.056089	3162.700107	17.303706	-0.044309	3.091622
222.783751	3154.708902	17.308711	-0.044253	3.087964
222.730961	3146.716045	17.313715	-0.044238	3.084311
222.972509	3138.753365	17.318720	-0.044278	3.080680
222.793871	3130.788069	17.323725	-0.044240	3.077025
222.693105	3122.782213	17.328730	-0.044217	3.073351
222.734820	3114.682416	17.333735	-0.044219	3.069635
222.795531	3106.709293	17.338739	-0.044226	3.065974
222.817652	3098.750966	17.343744	-0.044225	3.062314
222.490562	3090.796594	17.348749	-0.044159	3.058635
222.579891	3082.835612	17.353754	-0.044171	3.054968
222.604126	3074.819885	17.358759	-0.044170	3.051268
222.489838	3066.845012	17.363763	-0.044144	3.047576
222.463306	3058.880243	17.368768	-0.044134	3.043888
222.469100	3050.900928	17.373773	-0.044130	3.040191
222.449347	3042.952793	17.378778	-0.044121	3.036502
222.563891	3034.921136	17.383783	-0.044138	3.032776
222.315304	3026.925643	17.388787	-0.044086	3.029046
222.356087	3018.957556	17.393792	-0.044089	3.025337
222.270689	3010.962201	17.398797	-0.044068	3.021605
222.420004	3003.011043	17.403802	-0.044091	3.017900
222.087642	2995.028576	17.408807	-0.044024	3.014153
221.933519	2987.027505	17.413811	-0.043990	3.010401
222.261135	2979.033118	17.418816	-0.044046	3.006671
222.118645	2971.046791	17.423821	-0.044015	3.002917
222.024054	2963.110636	17.428826	-0.043992	2.999185
221.885066	2955.126748	17.433831	-0.043961	2.995423
221.889466	2947.089414	17.438835	-0.043957	2.991638
221.824917	2939.095371	17.443840	-0.043940	2.987865
221.545023	2931.122452	17.448845	-0.043883	2.984087
221.738796	2923.141681	17.453850	-0.043914	2.980324
221.753169	2915.159045	17.458855	-0.043912	2.976546
221.489866	2907.191195	17.463859	-0.043858	2.972757
221.550183	2899.203599	17.468864	-0.043864	2.968970
221.526213	2891.195149	17.473869	-0.043855	2.965163
221.448765	2883.263730	17.478874	-0.043835	2.961386
221.549229	2875.272890	17.483879	-0.043849	2.957585
221.400420	2867.295603	17.488883	-0.043816	2.953772
221.446192	2859.271745	17.493888	-0.043820	2.949942
221.407499	2851.270686	17.498893	-0.043808	2.946114
221.367844	2843.342702	17.503898	-0.043795	2.942316
221.273235	2835.381489	17.508903	-0.043773	2.938494
221.214130	2827.389130	17.513907	-0.043757	2.934654
221.493122	2819.349645	17.518912	-0.043804	2.930804
221.347243	2811.358539	17.523917	-0.043772	2.926950
221.128960	2803.447450	17.528922	-0.043726	2.923125
220.874071	2795.471326	17.533927	-0.043674	2.919262
220.966844	2787.499369	17.538931	-0.043686	2.915415
220.870661	2779.449058	17.543936	-0.043663	2.911514
220.676792	2771.426785	17.548941	-0.043622	2.907617
220.768703	2763.461642	17.553946	-0.043634	2.903757
220.707371	2755.529117	17.558951	-0.043618	2.899900
220.777666	2747.534887	17.563955	-0.043626	2.896014
220.735605	2739.552923	17.568960	-0.043613	2.892124
220.759250	2731.533489	17.573965	-0.043612	2.888213
220.546796	2723.596530	17.578970	-0.043568	2.884325
220.567746	2715.636071	17.583975	-0.043567	2.880432
220.663104	2707.644292	17.588979	-0.043580	2.876523
220.537719	2699.658760	17.593984	-0.043551	2.872600
220.172779	2691.687551	17.598989	-0.043478	2.868665
220.307139	2683.682837	17.603994	-0.043498	2.864735
220.306365	2675.731471	17.608999	-0.043493	2.860819
220.200309	2667.769956	17.614003	-0.043469	2.856887
220.357185	2659.746828	17.619008	-0.043493	2.852934
220.403881	2651.743406	17.624013	-0.043496	2.848979
220.182416	2643.813566	17.629018	-0.043450	2.845039
220.014708	2635.861680	17.634023	-0.043414	2.841086
220.107672	2627.880024	17.639027	-0.043426	2.837128
220.278378	2619.873005	17.644032	-0.043453	2.833156
220.188302	2611.851721	17.649037	-0.043431	2.829156
219.941556	2603.906639	17.654042	-0.043381	2.825180
220.076065	2595.934262	17.659047	-0.043401	2.821206
219.994415	2587.961004	17.664051	-0.043380	2.817214
220.158603	2579.974614	17.669056	-0.043406	2.813224
219.944201	2571.987627	17.674061	-0.043361	2.809206
219.782433	2564.030347	17.679066	-0.043326	2.805200
219.604600	2556.082032	17.684071	-0.043288	2.801192
219.759431	2548.067112	17.689075	-0.043312	2.797164
219.602492	2540.114577	17.694080	-0.043278	2.793144
219.453249	2532.104134	17.699085	-0.043245	2.789089
219.685039	2524.107425	17.704090	-0.043283	2.785057
219.457895	2516.198333	17.709095	-0.043236	2.781037
219.248577	2508.210794	17.714099	-0.043192	2.776972
219.295041	2500.243896	17.719104	-0.043196	2.772927
219.239691	2492.218956	17.724109	-0.043180	2.768840
219.457439	2484.229625	17.729114	-0.043216	2.764782
219.181319	2476.308600	17.734119	-0.043159	2.760723
219.131077	2468.336218	17.739123	-0.043145	2.756645
219.236631	2460.298207	17.744128	-0.043160	2.752537
219.001533	2452.288550	17.749133	-0.043111	2.748417
219.013061	2444.310531	17.754138	-0.043108	2.744322
218.933537	2436.373379	17.759143	-0.043088	2.740236
218.876777	2428.407245	17.764147	-0.043073	2.736131
219.071974	2420.408687	17.769152	-0.043104	2.732018
218.986448	2412.434882	17.774157	-0.043083	2.727894
218.998688	2404.477828	17.779162	-0.043081	2.723779
218.713837	2396.536290	17.784167	-0.043023	2.719647
218.645871	2388.575671	17.789171	-0.043005	2.715513
218.784066	2380.560531	17.794176	-0.043026	2.711357
218.573615	2372.582580	17.799181	-0.042982	2.707192
218.568634	2364.605538	17.804186	-0.042976	2.703033
218.458322	2356.662393	17.809191	-0.042950	2.698880
218.525259	2348.684544	17.814195	-0.042958	2.694713
218.638118	2340.669970	17.819200	-0.042974	2.690523
218.437240	2332.726515	17.824205	-0.042931	2.686344
218.467773	2324.752697	17.829210	-0.042932	2.682158
218.352084	2316.811392	17.834215	-0.042906	2.677972
218.330958	2308.813668	17.839219	-0.042897	2.673757
218.162621	2300.824586	17.844224	-0.042860	2.669530
218.097690	2292.849828	17.849229	-0.042843	2.665310
217.932738	2284.904052	17.854234	-0.042808	2.661092
218.023263	2276.923299	17.859239	-0.042819	2.656866
217.909273	2268.953183	17.864243	-0.042793	2.652625
217.788580	2260.959460	17.869248	-0.042766	2.648365
218.026790	2252.962152	17.874253	-0.042805	2.644119
217.965274	2245.029864	17.879258	-0.042789	2.639882
217.735800	2237.105046	17.884263	-0.042741	2.635630
217.667302	2229.094360	17.889267	-0.042723	2.631337
217.882303	2221.088834	17.894272	-0.042758	2.627057
217.773871	2213.132437	17.899277	-0.042733	2.622776
217.732835	2205.187122	17.904282	-0.042721	2.618499
217.819606	2197.201337	17.909287	-0.042732	2.614200
217.484839	2189.232165	17.914291	-0.042664	2.609876
217.524365	2181.278574	17.919296	-0.042667	2.605578
217.467833	2173.307142	17.924301	-0.042651	2.601257
217.416876	2165.374450	17.929306	-0.042637	2.596950
217.129636	2157.314571	17.934311	-0.042578	2.592550
217.032218	2149.235324	17.939315	-0.042555	2.588145
217.254902	2141.258174	17.944320	-0.042592	2.583811
217.156441	2133.342309	17.949325	-0.042568	2.579480
217.152110	2125.419115	17.954330	-0.042563	2.575145
217.124330	2117.436514	17.959335	-0.042553	2.570768
217.126502	2109.474253	17.964339	-0.042548	2.566397
217.090732	2101.543672	17.969344	-0.042536	2.562034
217.068494	2093.579606	17.974349	-0.042527	2.557645
216.994246	2085.624502	17.979354	-0.042509	2.553250
216.957879	2077.632617	17.984359	-0.042497	2.548830
216.907684	2069.662003	17.989363	-0.042482	2.544413
216.904230	2061.742886	17.994368	-0.042477	2.540020
216.671569	2053.785568	17.999373	-0.042429	2.535582
216.790539	2045.783969	18.004378	-0.042446	2.531137
216.741673	2037.822846	18.009383	-0.042432	2.526694
216.692535	2029.864615	18.014387	-0.042418	2.522246
216.437747	2021.956580	18.019392	-0.042365	2.517802
216.416718	2013.946381	18.024397	-0.042356	2.513310
216.467437	2005.946275	18.029402	-0.042361	2.508821
216.226820	1997.994106	18.034407	-0.042311	2.504330
216.195786	1990.035387	18.039411	-0.042300	2.499843
216.231976	1982.084495	18.044416	-0.042302	2.495356
216.348460	1974.067447	18.049421	-0.042319	2.490830
216.326452	1966.119722	18.054426	-0.042310	2.486325
216.006852	1958.196190	18.059431	-0.042245	2.481803
215.823823	1950.257745	18.064435	-0.042206	2.477275
216.170165	1942.242285	18.069440	-0.042266	2.472734
215.963934	1934.278673	18.074445	-0.042222	2.468173
215.981706	1926.312926	18.079450	-0.042221	2.463618
216.012833	1918.364226	18.084455	-0.042221	2.459067
215.671677	1910.431422	18.089459	-0.042153	2.454488
215.767116	1902.446335	18.094464	-0.042166	2.449903
215.691343	1894.485622	18.099469	-0.042147	2.445311
215.635313	1886.542709	18.104474	-0.042131	2.440721
215.683116	1878.574928	18.109479	-0.042135	2.436117
215.589156	1870.555555	18.114483	-0.042113	2.431463
215.502315	1862.583418	18.119488	-0.042092	2.426828
215.308099	1854.652560	18.124493	-0.042051	2.422201
215.484951	1846.685667	18.129498	-0.042078	2.417571
215.393331	1838.731609	18.134503	-0.042056	2.412920
215.395101	1830.749339	18.139507	-0.042052	2.408251
215.332867	1822.812608	18.144512	-0.042035	2.403594
215.527154	1814.834534	18.149517	-0.042066	2.398923
215.357149	1806.917828	18.154522	-0.042030	2.394252
215.312748	1798.930853	18.159527	-0.042017	2.389539
215.235504	1790.978567	18.164531	-0.041997	2.384835
215.329869	1783.030864	18.169536	-0.042010	2.380138
214.977186	1775.113297	18.174541	-0.041939	2.375414
215.073372	1767.124335	18.179546	-0.041952	2.370674
214.881938	1759.177162	18.184551	-0.041912	2.365927
214.809410	1751.232379	18.189555	-0.041893	2.361181
214.955219	1743.279871	18.194560	-0.041915	2.356438
214.886537	1735.276734	18.199565	-0.041898	2.351638
214.610173	1727.343025	18.204570	-0.041841	2.346853
214.561702	1719.388810	18.209575	-0.041827	2.342064
214.568111	1711.428428	18.214579	-0.041823	2.337266
214.693396	1703.456853	18.219584	-0.041842	2.332462
214.432344	1695.512214	18.224589	-0.041788	2.327632
214.552488	1687.557194	18.229594	-0.041806	2.322817
214.560075	1679.612136	18.234599	-0.041802	2.317988
214.223228	1671.691022	18.239603	-0.041734	2.313136
214.414008	1663.696873	18.244608	-0.041765	2.308273
214.549714	1655.711939	18.249613	-0.041785	2.303401
214.363525	1647.823102	18.254618	-0.041746	2.298550
214.161657	1639.870424	18.259623	-0.041703	2.293648
214.030618	1631.906120	18.264627	-0.041674	2.288735
214.243367	1623.952795	18.269632	-0.041708	2.283847
213.992836	1616.018759	18.274637	-0.041657	2.278921
214.136358	1608.053592	18.279642	-0.041679	2.273998
214.044284	1600.019390	18.284647	-0.041656	2.269002
213.881907	1592.086352	18.289651	-0.041621	2.264052
213.782764	1584.178235	18.294656	-0.041598	2.259112
213.720447	1576.220227	18.299661	-0.041581	2.254133
213.616502	1568.269195	18.304666	-0.041557	2.249144
213.518504	1560.325845	18.309671	-0.041534	2.244149
213.547447	1552.387220	18.314675	-0.041534	2.239156
213.572682	1544.452439	18.319680	-0.041534	2.234155
213.402336	1536.490731	18.324685	-0.041497	2.229109
213.593477	1528.513468	18.329690	-0.041528	2.224073
213.444128	1520.608059	18.334695	-0.041495	2.219041
213.134943	1512.687759	18.339699	-0.041433	2.213973
213.356468	1504.697402	18.344704	-0.041469	2.208897
213.295319	1496.757276	18.349709	-0.041453	2.203816
213.159073	1488.843412	18.354714	-0.041422	2.198733
212.928635	1480.924821	18.359719	-0.041374	2.193627
212.802433	1472.933039	18.364723	-0.041346	2.188471
213.095711	1464.966200	18.369728	-0.041396	2.183358
212.875028	1457.044931	18.374733	-0.041350	2.178215
212.791267	1449.120648	18.379738	-0.041329	2.173070
212.901386	1441.147997	18.384743	-0.041345	2.167899
212.754615	1433.217468	18.389747	-0.041312	2.162720
212.919917	1425.287048	18.394752	-0.041338	2.157558
212.614993	1417.369520	18.399757	-0.041276	2.152347
212.843668	1409.386951	18.404762	-0.041314	2.147131
212.491063	1401.484343	18.409767	-0.041243	2.141901
212.509289	1393.546192	18.414771	-0.041242	2.136669
212.599148	1385.590977	18.419776	-0.041254	2.131420
212.088500	1377.685170	18.424781	-0.041154	2.126133
212.402299	1369.723366	18.429786	-0.041207	2.120875
212.480061	1361.788871	18.434791	-0.041217	2.115599
212.156368	1353.814585	18.439795	-0.041151	2.110245
212.041891	1345.886183	18.444800	-0.041125	2.104928
212.060931	1337.947392	18.449805	-0.041124	2.099604
212.081924	1330.027030	18.454810	-0.041123	2.094278
212.037827	1322.065714	18.459815	-0.041109	2.088905
211.774625	1314.158818	18.464819	-0.041056	2.083534
212.060359	1306.214207	18.469824	-0.041104	2.078177
211.921927	1298.288579	18.474829	-0.041073	2.072777
211.913460	1290.349619	18.479834	-0.041067	2.067367
211.734478	1282.441279	18.484839	-0.041028	2.061946
211.751908	1274.524654	18.489843	-0.041027	2.056526
211.780695	1266.577944	18.494848	-0.041027	2.051071
211.630133	1258.645132	18.499853	-0.040994	2.045593
211.498216	1250.748082	18.504858	-0.040965	2.040128
211.516674	1242.826060	18.509863	-0.040963	2.034645
211.412262	1234.855196	18.514867	-0.040939	2.029101
211.515378	1226.922148	18.519872	-0.040953	2.023590
211.295177	1219.020380	18.524877	-0.040907	2.018052
210.944222	1211.140183	18.529882	-0.040837	2.012500
211.101492	1203.158101	18.534887	-0.040861	2.006914
211.072638	1195.227895	18.539891	-0.040851	2.001330
211.148955	1187.313263	18.544896	-0.040860	1.995752
210.874058	1179.402169	18.549901	-0.040804	1.990124
211.033158	1171.458506	18.554906	-0.040829	1.984502
210.965203	1163.550879	18.559911	-0.040811	1.978867
211.061691	1155.617905	18.564915	-0.040824	1.973214
211.102670	1147.691025	18.569920	-0.040827	1.967544
210.808554	1139.806659	18.574925	-0.040767	1.961852
210.937145	1131.882293	18.579930	-0.040786	1.956160
210.714289	1123.956717	18.584935	-0.040740	1.950413
210.449659	1116.038762	18.589939	-0.040685	1.944649
210.663408	1108.106664	18.594944	-0.040720	1.938911
210.569016	1100.184754	18.599949	-0.040698	1.933129
210.460394	1092.271460	18.604954	-0.040672	1.927334
210.406406	1084.370162	18.609959	-0.040658	1.921536
210.115950	1076.499198	18.614963	-0.040599	1.915717
210.096126	1068.567664	18.619968	-0.040590	1.909866
210.058940	1060.633972	18.624973	-0.040578	1.903993
209.914989	1052.758383	18.629978	-0.040546	1.898134
210.094520	1044.800698	18.634983	-0.040575	1.892231
210.077381	1036.876686	18.639987	-0.040567	1.886313
209.995674	1029.002126	18.644992	-0.040547	1.880406
209.903484	1021.109758	18.649997	-0.040524	1.874465
209.881486	1013.170328	18.655002	-0.040515	1.868478
209.853784	1005.259051	18.660007	-0.040505	1.862493
209.751436	997.372081	18.665011	-0.040481	1.856498
209.660229	989.472071	18.670016	-0.040459	1.850475
209.527636	981.570085	18.675021	-0.040430	1.844426
209.488901	973.696975	18.680026	-0.040418	1.838390
209.378517	965.797066	18.685031	-0.040392	1.832306
209.421338	957.867735	18.690035	-0.040395	1.826196
209.601580	949.942868	18.695040	-0.040424	1.820086
209.350674	942.089881	18.700045	-0.040372	1.813959
209.383252	934.171586	18.705050	-0.040373	1.807795
209.375868	926.286010	18.710055	-0.040367	1.801630
209.074588	918.442717	18.715059	-0.040306	1.795442
209.026337	910.489246	18.720064	-0.040292	1.789176
208.907897	902.592882	18.725069	-0.040265	1.782925
208.953808	894.701273	18.730074	-0.040269	1.776676
209.079174	886.781283	18.735079	-0.040287	1.770392
209.013597	878.897734	18.740083	-0.040270	1.764091
208.859904	871.062146	18.745088	-0.040237	1.757795
208.853331	863.158284	18.750093	-0.040230	1.751440
208.856656	855.255643	18.755098	-0.040226	1.745063
208.967550	847.372291	18.760103	-0.040242	1.738693
208.506339	839.544908	18.765107	-0.040151	1.732272
208.625417	831.643597	18.770112	-0.040168	1.725841
208.690560	823.747896	18.775117	-0.040176	1.719383
208.444421	815.917468	18.780122	-0.040125	1.712915
208.384209	808.016695	18.785127	-0.040109	1.706388
208.336925	800.138659	18.790131	-0.040095	1.699856
208.223267	792.290697	18.795136	-0.040069	1.693316
208.176662	784.387103	18.800141	-0.040055	1.686712
208.193710	776.515893	18.805146	-0.040054	1.680118
208.175801	768.669753	18.810151	-0.040045	1.673515
208.007982	760.794598	18.815155	-0.040009	1.666841
208.092419	752.921473	18.820160	-0.040020	1.660176
208.119533	745.056006	18.825165	-0.040020	1.653482
207.875642	737.215905	18.830170	-0.039970	1.646746
207.572024	729.396726	18.835175	-0.039908	1.639992
207.696588	721.496272	18.840179	-0.039927	1.633199
207.755406	713.581236	18.845184	-0.039933	1.626356
207.474799	705.759443	18.850189	-0.039876	1.619518
207.464817	697.905239	18.855194	-0.039869	1.612661
207.431492	690.039800	18.860199	-0.039858	1.605760
207.128097	682.239307	18.865203	-0.039796	1.598850
207.073566	674.392080	18.870208	-0.039781	1.591903
207.010655	666.525025	18.875213	-0.039765	1.584906
207.242625	658.660353	18.880218	-0.039803	1.577924
206.912063	650.852294	18.885223	-0.039737	1.570879
206.822886	643.015969	18.890227	-0.039715	1.563813
207.021778	635.155564	18.895232	-0.039747	1.556735
206.815512	627.321640	18.900237	-0.039704	1.549589
206.665796	619.502543	18.905242	-0.039671	1.542431
206.776142	611.644821	18.910247	-0.039687	1.535244
206.479770	603.847519	18.915251	-0.039627	1.528017
206.487301	596.023266	18.920256	-0.039623	1.520777
206.304121	588.221524	18.925261	-0.039584	1.513494
206.303039	580.380594	18.930266	-0.039579	1.506168
206.205403	572.573424	18.935271	-0.039556	1.498822
206.105271	564.749345	18.940275	-0.039533	1.491423
206.313475	556.904616	18.945280	-0.039567	1.484017
205.994120	549.146589	18.950285	-0.039502	1.476573
205.879391	541.298012	18.955290	-0.039476	1.469036
205.971228	533.458894	18.960295	-0.039488	1.461503
205.919353	525.661083	18.965299	-0.039474	1.453948
205.803904	517.875818	18.970304	-0.039447	1.446355
205.804658	510.079048	18.975309	-0.039443	1.438730
205.822268	502.275910	18.980314	-0.039441	1.431060
205.735547	494.489966	18.985319	-0.039420	1.423349
205.625656	486.722315	18.990323	-0.039395	1.415611
205.710410	478.915716	18.995328	-0.039406	1.407823
205.697532	471.132792	19.000333	-0.039399	1.399999
205.529474	463.385743	19.005338	-0.039362	1.392142
205.536384	455.585614	19.010343	-0.039359	1.384216
205.206653	447.857987	19.015347	-0.039293	1.376260
205.037768	440.103912	19.020352	-0.039256	1.368259
205.249893	432.295211	19.025357	-0.039291	1.360220
205.046901	424.577575	19.030362	-0.039248	1.352156
204.939382	416.820724	19.035367	-0.039224	1.344019
204.847227	409.068080	19.040371	-0.039202	1.335839
205.184550	401.264264	19.045376	-0.039259	1.327632
204.600513	393.611194	19.050381	-0.039146	1.319369
204.568346	385.796726	19.055386	-0.039135	1.310980
204.856788	377.953804	19.060391	-0.039184	1.302564
204.686220	370.254136	19.065395	-0.039147	1.294166
204.626216	362.540822	19.070400	-0.039131	1.285718
204.313018	354.880237	19.075405	-0.039068	1.277225
204.418299	347.137264	19.080410	-0.039083	1.268663
204.266248	339.457419	19.085415	-0.039050	1.260064
203.963705	331.787859	19.090419	-0.038989	1.251389
204.058210	324.073402	19.095424	-0.039002	1.242679
204.101848	316.363704	19.100429	-0.039005	1.233902
204.016739	308.667339	19.105434	-0.038984	1.225053
203.613802	301.050756	19.110439	-0.038905	1.216170
203.694479	293.335043	19.115443	-0.038915	1.207201
203.711297	285.675587	19.120448	-0.038913	1.198219
203.698013	277.997339	19.125453	-0.038906	1.189140
203.840737	270.312525	19.130458	-0.038928	1.180016
203.666808	262.693533	19.135463	-0.038891	1.170834
203.260764	255.111261	19.140467	-0.038810	1.161577
203.679586	247.398178	19.145472	-0.038883	1.152257
203.483638	239.764018	19.150477	-0.038842	1.142829
203.138435	232.201793	19.155482	-0.038773	1.133380
203.047655	224.591285	19.160487	-0.038752	1.123846
203.079058	216.975241	19.165491	-0.038753	1.114250
202.811256	209.417159	19.170496	-0.038698	1.104578
202.420189	201.885779	19.175501	-0.038621	1.094829
202.505415	194.273776	19.180506	-0.038632	1.084993
202.676468	186.676604	19.185511	-0.038659	1.075106
202.422251	179.133109	19.190515	-0.038607	1.065101
202.559073	171.559106	19.195520	-0.038628	1.055051
202.308514	164.040951	19.200525	-0.038576	1.044890
202.249384	156.534792	19.205530	-0.038561	1.034689
202.231976	149.009426	19.210535	-0.038553	1.024371
202.156400	141.512363	19.215539	-0.038534	1.013973
202.005665	134.040636	19.220544	-0.038501	1.003485
201.811252	126.577918	19.225549	-0.038460	0.992887
201.700938	119.095732	19.230554	-0.038435	0.982169
201.530317	111.661633	19.235559	-0.038399	0.971386
201.253948	104.253335	19.240563	-0.038343	0.960493
201.217364	96.828654	19.245568	-0.038331	0.949513
201.129304	89.418136	19.250573	-0.038310	0.938413
200.830148	82.064306	19.255578	-0.038250	0.927209
200.800228	74.693219	19.260583	-0.038240	0.915914
200.737507	67.310848	19.265587	-0.038224	0.904452
200.781213	60.191819	19.270592	-0.038227	0.893288