Fri Mar 12 13:49:10 2021

Number of Points = 3628
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.504862	-0.028659	0.000000	-0.000030	0.721136

0.429621	-0.018356	0.005005	-0.000016	0.721130
0.497190	-0.029794	0.010010	-0.000029	0.721131
0.368843	-0.007853	0.015014	-0.000005	0.721129
0.378170	-0.012411	0.020019	-0.000006	0.721124
0.477022	-0.025333	0.025024	-0.000025	0.721133
0.513013	-0.035037	0.030029	-0.000032	0.721127
0.508516	-0.032769	0.035034	-0.000031	0.721130
0.437873	-0.019119	0.040038	-0.000018	0.721132
0.319626	-0.002785	0.045043	0.000004	0.721123
0.401493	-0.013119	0.050048	-0.000011	0.721131
0.474669	-0.028294	0.055053	-0.000025	0.721127
0.294758	0.006480	0.060058	0.000009	0.721132
0.531324	-0.035290	0.065062	-0.000035	0.721133
0.459951	-0.027898	0.070067	-0.000022	0.721123
0.553061	-0.162940	0.075072	-0.000039	0.720890
0.413283	-0.142453	0.080077	-0.000013	0.720881
0.579456	-0.169428	0.085082	-0.000044	0.720886
0.527375	-0.160392	0.090086	-0.000035	0.720886
0.244173	-0.113174	0.095091	0.000018	0.720880
0.440034	-0.143810	0.100096	-0.000019	0.720888
0.511407	-0.251943	0.105101	-0.000032	0.720701
0.522870	-0.331979	0.110106	-0.000034	0.720547
0.595744	-0.343213	0.115110	-0.000048	0.720551
0.485035	-0.327622	0.120115	-0.000027	0.720543
0.289609	-0.288500	0.125120	0.000009	0.720551
0.421981	-0.413516	0.130125	-0.000015	0.720352
0.395872	-0.470773	0.135130	-0.000010	0.720230
0.507375	-0.490156	0.140134	-0.000031	0.720231
0.196293	-0.437810	0.145139	0.000027	0.720225
0.635557	-0.574485	0.150144	-0.000055	0.720110
0.431550	-0.641516	0.155149	-0.000017	0.719906
0.374501	-0.630763	0.160154	-0.000007	0.719907
0.374592	-0.627691	0.165158	-0.000007	0.719914
0.313088	-0.723951	0.170163	0.000005	0.719702
0.367165	-0.778328	0.175168	-0.000005	0.719614
0.210543	-0.753366	0.180173	0.000024	0.719609
0.316045	-0.813491	0.185178	0.000004	0.719527
0.281319	-0.931363	0.190182	0.000011	0.719283
0.109677	-0.904990	0.195187	0.000043	0.719274
0.095258	-0.898466	0.200192	0.000045	0.719282
0.165742	-1.069015	0.205197	0.000032	0.718971
-0.000058	-1.040674	0.210202	0.000063	0.718968
0.115833	-1.058269	0.215206	0.000041	0.718975
0.245976	-1.242461	0.220211	0.000017	0.718657
0.308285	-1.254430	0.225216	0.000006	0.718655
0.196978	-1.271103	0.230221	0.000026	0.718583
0.206245	-1.386923	0.235226	0.000025	0.718358
0.260301	-1.392283	0.240230	0.000014	0.718366
0.228273	-1.498659	0.245235	0.000020	0.718145
0.164674	-1.547626	0.250240	0.000032	0.718026
-0.100473	-1.519286	0.255245	0.000082	0.717989
-0.310260	-1.623006	0.260250	0.000121	0.717710
-0.230607	-1.633443	0.265254	0.000106	0.717718
-0.312948	-1.714884	0.270259	0.000121	0.717528
-0.145263	-1.813758	0.275264	0.000090	0.717391
-0.115400	-1.849352	0.280269	0.000084	0.717332
-0.124274	-1.971172	0.285274	0.000086	0.717088
-0.319751	-1.933395	0.290278	0.000122	0.717094
-0.287760	-2.090415	0.295283	0.000117	0.716794
-0.355213	-2.093546	0.300288	0.000129	0.716764
-0.350956	-2.195212	0.305293	0.000128	0.716565
-0.641857	-2.200480	0.310298	0.000182	0.716452
-0.660402	-2.263240	0.315302	0.000186	0.716321
-2.343012	-2.057536	0.320307	0.000499	0.716135
-1.859654	-2.138716	0.325312	0.000409	0.716145
-2.144991	-2.198118	0.330317	0.000462	0.715926
-2.639991	-2.129320	0.335322	0.000554	0.715888
-2.799193	-2.116519	0.340326	0.000584	0.715857
-3.492407	-2.150537	0.345331	0.000713	0.715545
-3.128698	-2.209661	0.350336	0.000645	0.715557
-3.687752	-2.123259	0.355341	0.000749	0.715531
-4.305118	-2.162802	0.360346	0.000864	0.715234
-4.084989	-2.198477	0.365350	0.000823	0.715241
-5.081676	-2.025093	0.370355	0.001008	0.715233
-4.896155	-2.153435	0.375360	0.000974	0.715044
-5.809644	-2.056309	0.380365	0.001144	0.714914
-5.575142	-2.098519	0.385370	0.001100	0.714913
-5.536506	-2.100606	0.390374	0.001093	0.714923
-6.019284	-2.097185	0.395379	0.001183	0.714759
-6.568192	-2.070719	0.400384	0.001285	0.714617
-6.400034	-2.103627	0.405389	0.001254	0.714612
-6.836153	-2.025342	0.410394	0.001335	0.714613
-6.396136	-2.103106	0.415398	0.001253	0.714614
-6.918209	-2.177886	0.420403	0.001350	0.714281
-7.522674	-2.066503	0.425408	0.001463	0.714289
-7.182402	-2.128542	0.430413	0.001399	0.714286
-7.162572	-2.131801	0.435418	0.001395	0.714286
-7.525025	-2.107739	0.440422	0.001463	0.714206
-8.673579	-2.019744	0.445427	0.001677	0.713974
-7.946876	-2.146114	0.450432	0.001541	0.713981
-8.348415	-2.075794	0.455437	0.001616	0.713978
-8.842498	-1.988122	0.460442	0.001708	0.713978
-7.873172	-2.159722	0.465446	0.001528	0.713980
-8.467374	-2.188474	0.470451	0.001638	0.713712
-9.293238	-2.066540	0.475456	0.001792	0.713662
-9.133748	-2.095624	0.480461	0.001762	0.713661
-9.155318	-2.093314	0.485466	0.001766	0.713658
-9.201596	-2.081301	0.490470	0.001775	0.713666
-9.456053	-2.055400	0.495475	0.001822	0.713627
-9.784035	-2.125153	0.500480	0.001883	0.713372
-9.990526	-2.090640	0.505485	0.001921	0.713368
-10.509051	-1.998570	0.510490	0.002018	0.713367
-9.770685	-2.126556	0.515494	0.001880	0.713375
-10.140982	-2.066664	0.520499	0.001949	0.713363
-10.295725	-2.034072	0.525504	0.001978	0.713373
-10.245828	-2.200092	0.530509	0.001969	0.713060
-11.062596	-2.068608	0.535514	0.002121	0.713032
-11.222383	-2.037669	0.540518	0.002150	0.713037
-11.102585	-2.064703	0.545523	0.002128	0.713026
-10.767691	-2.119903	0.550528	0.002066	0.713035
-10.774062	-2.120534	0.555533	0.002067	0.713032
-11.334245	-2.131588	0.560538	0.002171	0.712811
-12.153946	-2.030194	0.565542	0.002324	0.712722
-11.914894	-2.075534	0.570547	0.002279	0.712717
-11.887004	-2.077918	0.575552	0.002274	0.712722
-12.301692	-2.007442	0.580557	0.002351	0.712715
-12.116439	-2.041588	0.585562	0.002317	0.712713
-11.617302	-2.125507	0.590566	0.002224	0.712723
-12.335147	-2.117744	0.595571	0.002357	0.712484
-12.919456	-2.056661	0.600576	0.002466	0.712398
-12.799349	-2.079239	0.605581	0.002444	0.712396
-13.002174	-2.045452	0.610586	0.002481	0.712392
-12.586798	-2.116802	0.615590	0.002404	0.712397
-12.770594	-2.086445	0.620595	0.002438	0.712392
-13.067680	-2.030219	0.625600	0.002493	0.712399
-13.489990	-2.073409	0.630605	0.002572	0.712163
-13.937284	-2.026573	0.635610	0.002655	0.712098
-13.668497	-2.071022	0.640614	0.002605	0.712105
-14.198912	-1.983013	0.645619	0.002704	0.712092
-14.035596	-2.007925	0.650624	0.002673	0.712100
-13.614507	-2.085387	0.655629	0.002595	0.712095
-13.958836	-2.024386	0.660634	0.002659	0.712095
-13.933040	-2.087027	0.665638	0.002654	0.711979
-14.743161	-2.051603	0.670643	0.002805	0.711762
-14.399531	-2.109470	0.675648	0.002741	0.711769
-14.831051	-2.034301	0.680653	0.002821	0.711765
-14.548631	-2.084628	0.685658	0.002769	0.711766
-14.177488	-2.148297	0.690662	0.002699	0.711771
-15.023913	-2.001663	0.695667	0.002857	0.711762
-14.559624	-2.163155	0.700672	0.002771	0.711605
-15.481091	-2.071516	0.705677	0.002942	0.711461
-15.645529	-2.042098	0.710682	0.002973	0.711461
-15.443777	-2.073707	0.715686	0.002935	0.711470
-15.553643	-2.060628	0.720691	0.002955	0.711457
-15.436752	-2.076450	0.725696	0.002934	0.711467
-15.606510	-2.048628	0.730701	0.002965	0.711462
-15.717460	-2.129060	0.735706	0.002986	0.711262
-16.243134	-2.091365	0.740710	0.003084	0.711151
-16.642340	-2.026057	0.745715	0.003158	0.711139
-16.515278	-2.043694	0.750720	0.003134	0.711149
-16.271202	-2.089419	0.755725	0.003089	0.711145
-16.522196	-2.045046	0.760730	0.003135	0.711144
-16.286678	-2.082988	0.765734	0.003092	0.711152
-16.356354	-2.158295	0.770739	0.003104	0.710977
-17.185758	-2.057770	0.775744	0.003259	0.710883
-17.252292	-2.048456	0.780749	0.003271	0.710878
-17.418534	-2.020280	0.785754	0.003302	0.710875
-16.993454	-2.091066	0.790758	0.003223	0.710885
-17.250058	-2.049368	0.795763	0.003271	0.710877
-17.342407	-2.030724	0.800768	0.003288	0.710882
-17.355339	-2.172858	0.805773	0.003290	0.710593
-18.291531	-2.032405	0.810778	0.003464	0.710541
-18.148811	-2.052252	0.815782	0.003438	0.710552
-18.028582	-2.079736	0.820787	0.003415	0.710540
-17.808159	-2.115423	0.825792	0.003374	0.710547
-18.050798	-2.072420	0.830797	0.003419	0.710547
-18.184005	-2.070958	0.835802	0.003444	0.710503
-18.544758	-2.143333	0.840806	0.003511	0.710230
-19.007980	-2.064690	0.845811	0.003598	0.710222
-19.174428	-2.032021	0.850816	0.003628	0.710228
-18.779899	-2.103543	0.855821	0.003555	0.710226
-18.968692	-2.072204	0.860826	0.003590	0.710221
-19.081614	-2.047864	0.865830	0.003611	0.710230
-19.216914	-2.039651	0.870835	0.003636	0.710198
-19.571516	-2.125279	0.875840	0.003702	0.709901
-20.044607	-2.040696	0.880845	0.003790	0.709901
-20.449006	-1.972104	0.885850	0.003865	0.709894
-19.660344	-2.108712	0.890854	0.003719	0.709902
-19.702169	-2.104110	0.895859	0.003726	0.709897
-20.071761	-2.034186	0.900864	0.003795	0.709905
-19.844396	-2.076112	0.905869	0.003753	0.709902
-20.194539	-2.142918	0.910874	0.003818	0.709644
-20.972244	-2.021842	0.915878	0.003963	0.709609
-21.002739	-2.020936	0.920883	0.003968	0.709600
-20.749970	-2.063176	0.925888	0.003921	0.709606
-20.948686	-2.028192	0.930893	0.003958	0.709605
-20.884047	-2.041313	0.935898	0.003946	0.709602
-20.751844	-2.061988	0.940902	0.003921	0.709608
-20.999641	-2.119902	0.945907	0.003968	0.709403
-21.799108	-2.042685	0.950912	0.004116	0.709273
-21.410469	-2.112769	0.955917	0.004044	0.709271
-21.604421	-2.080935	0.960922	0.004080	0.709266
-21.877721	-2.026885	0.965926	0.004131	0.709277
-21.688881	-2.065964	0.970931	0.004096	0.709266
-21.618872	-2.075635	0.975936	0.004083	0.709272
-21.935677	-2.112502	0.980941	0.004142	0.709085
-22.968078	-1.992489	0.985946	0.004334	0.708957
-22.327555	-2.103061	0.990950	0.004214	0.708964
-22.455932	-2.083731	0.995955	0.004238	0.708957
-22.887940	-2.003853	1.000960	0.004319	0.708963
-22.716032	-2.032154	1.005965	0.004287	0.708968
-22.571930	-2.060645	1.010970	0.004260	0.708962
-22.536349	-2.125309	1.015974	0.004253	0.708846
-23.589413	-2.040364	1.020979	0.004449	0.708640
-23.259972	-2.094639	1.025984	0.004388	0.708649
-23.549770	-2.043497	1.030989	0.004442	0.708648
-23.646351	-2.028390	1.035994	0.004460	0.708644
-23.305966	-2.085278	1.040998	0.004396	0.708652
-23.654857	-2.029722	1.046003	0.004461	0.708638
-23.635113	-2.072755	1.051008	0.004457	0.708559
-24.207667	-2.069275	1.056013	0.004564	0.708362
-24.319820	-2.051235	1.061018	0.004585	0.708358
-24.556373	-2.005687	1.066022	0.004629	0.708365
-24.716847	-1.981566	1.071027	0.004659	0.708356
-24.251659	-2.061247	1.076032	0.004572	0.708363
-24.035028	-2.099587	1.081037	0.004532	0.708363
-24.562482	-2.033235	1.086042	0.004630	0.708308
-25.192099	-2.060700	1.091046	0.004747	0.708028
-25.027630	-2.095000	1.096051	0.004716	0.708018
-25.492375	-2.009987	1.101056	0.004803	0.708023
-25.338724	-2.036207	1.106061	0.004774	0.708025
-25.434742	-2.022949	1.111066	0.004792	0.708017
-25.348269	-2.031979	1.116070	0.004776	0.708030
-25.271127	-2.051765	1.121075	0.004761	0.708018
-25.594901	-2.131581	1.126080	0.004822	0.707742
-26.133186	-2.051984	1.131085	0.004922	0.707710
-26.559803	-1.977969	1.136090	0.005001	0.707706
-25.841898	-2.102000	1.141094	0.004867	0.707714
-26.273986	-2.030084	1.146099	0.004948	0.707704
-26.430458	-1.999394	1.151104	0.004977	0.707709
-26.013203	-2.072523	1.156109	0.004899	0.707712
-26.337863	-2.150251	1.161114	0.004960	0.707440
-27.136137	-2.030993	1.166118	0.005108	0.707394
-27.493981	-1.973668	1.171123	0.005175	0.707381
-26.946450	-2.067725	1.176128	0.005073	0.707388
-26.900923	-2.076503	1.181133	0.005064	0.707387
-27.439078	-1.984238	1.186138	0.005164	0.707380
-27.054319	-2.047920	1.191142	0.005093	0.707390
-27.294071	-2.086744	1.196147	0.005137	0.707226
-28.308101	-1.973188	1.201152	0.005326	0.707091
-28.034197	-2.021196	1.206157	0.005275	0.707093
-28.098414	-2.013095	1.211162	0.005287	0.707086
-27.940717	-2.038252	1.216166	0.005258	0.707092
-28.099695	-2.014659	1.221171	0.005287	0.707083
-27.870230	-2.052258	1.226176	0.005244	0.707089
-27.776275	-2.130199	1.231181	0.005227	0.706967
-29.177303	-1.986027	1.236186	0.005488	0.706755
-28.568999	-2.089370	1.241190	0.005374	0.706765
-28.748235	-2.061348	1.246195	0.005408	0.706757
-28.926518	-2.027627	1.251200	0.005441	0.706761
-28.735818	-2.062788	1.256205	0.005405	0.706759
-28.708093	-2.071423	1.261210	0.005400	0.706752
-28.727520	-2.150647	1.266214	0.005404	0.706586
-30.035845	-1.986075	1.271219	0.005647	0.706448
-29.584482	-2.063078	1.276224	0.005563	0.706455
-29.450365	-2.087920	1.281229	0.005538	0.706453
-30.111382	-1.974403	1.286234	0.005661	0.706444
-29.829745	-2.017850	1.291238	0.005609	0.706458
-29.796979	-2.029558	1.296243	0.005603	0.706446
-29.870574	-2.071476	1.301248	0.005616	0.706336
-30.801347	-2.004577	1.306253	0.005789	0.706137
-30.407567	-2.077181	1.311258	0.005716	0.706132
-30.278147	-2.096138	1.316262	0.005692	0.706141
-30.776391	-2.010701	1.321267	0.005785	0.706134
-30.537874	-2.051125	1.326272	0.005740	0.706138
-30.648489	-2.031680	1.331277	0.005761	0.706138
-30.863382	-2.039573	1.336282	0.005801	0.706045
-31.354827	-2.036701	1.341286	0.005892	0.705875
-31.070585	-2.091060	1.346291	0.005839	0.705867
-31.573760	-1.999230	1.351296	0.005933	0.705872
-31.569750	-1.998782	1.356301	0.005932	0.705874
-31.338659	-2.043239	1.361306	0.005889	0.705868
-31.029857	-2.094331	1.366310	0.005832	0.705876
-31.756214	-2.075128	1.371315	0.005967	0.705654
-32.661892	-1.973536	1.376320	0.006135	0.705533
-31.842769	-2.119406	1.381325	0.005983	0.705534
-32.367784	-2.028530	1.386330	0.006080	0.705528
-32.571309	-1.988332	1.391334	0.006118	0.705536
-32.207062	-2.054082	1.396339	0.006050	0.705535
-32.033984	-2.084784	1.401344	0.006018	0.705535
-32.497367	-2.110735	1.406349	0.006104	0.705317
-33.467143	-1.988532	1.411354	0.006285	0.705215
-32.756631	-2.110158	1.416358	0.006153	0.705225
-33.004472	-2.070553	1.421363	0.006199	0.705216
-33.452191	-1.988335	1.426368	0.006282	0.705221
-32.728894	-2.116660	1.431373	0.006147	0.705222
-33.288584	-2.022236	1.436378	0.006252	0.705212
-33.840842	-2.070735	1.441382	0.006354	0.704916
-34.096805	-2.037467	1.446387	0.006402	0.704891
-34.129982	-2.029075	1.451392	0.006408	0.704896
-34.054985	-2.042369	1.456397	0.006394	0.704896
-34.128585	-2.033203	1.461402	0.006408	0.704888
-33.767112	-2.091757	1.466406	0.006340	0.704900
-33.858832	-2.079670	1.471411	0.006357	0.704892
-34.544913	-2.096648	1.476416	0.006485	0.704611
-34.532379	-2.104463	1.481421	0.006483	0.704600
-34.844390	-2.053411	1.486426	0.006541	0.704591
-34.848560	-2.047479	1.491430	0.006542	0.704602
-34.826373	-2.052134	1.496435	0.006537	0.704600
-34.833859	-2.051344	1.501440	0.006539	0.704599
-34.774058	-2.101670	1.506445	0.006528	0.704519
-36.092990	-1.992307	1.511450	0.006773	0.704266
-35.411721	-2.110516	1.516454	0.006646	0.704273
-35.779076	-2.049013	1.521459	0.006715	0.704265
-35.893049	-2.027340	1.526464	0.006736	0.704267
-35.550895	-2.087181	1.531469	0.006672	0.704270
-35.855370	-2.036463	1.536474	0.006729	0.704263
-35.697907	-2.096555	1.541478	0.006699	0.704198
-36.496016	-2.073133	1.546483	0.006848	0.703959
-36.537461	-2.063231	1.551488	0.006855	0.703964
-36.941332	-1.990957	1.556493	0.006931	0.703964
-36.878626	-2.005776	1.561498	0.006919	0.703957
-36.277245	-2.108276	1.566502	0.006807	0.703967
-36.751567	-2.028240	1.571507	0.006895	0.703958
-36.875740	-2.022047	1.576512	0.006918	0.703926
-37.337124	-2.077485	1.581517	0.007004	0.703648
-37.318138	-2.086404	1.586522	0.007001	0.703637
-37.790177	-1.996327	1.591526	0.007088	0.703649
-37.489478	-2.053848	1.596531	0.007032	0.703641
-37.258750	-2.093672	1.601536	0.006989	0.703644
-37.319788	-2.081747	1.606541	0.007001	0.703646
-37.755571	-2.029388	1.611546	0.007082	0.703595
-38.051271	-2.096009	1.616550	0.007137	0.703354
-38.011733	-2.107585	1.621555	0.007129	0.703345
-38.587187	-2.002473	1.626560	0.007236	0.703350
-38.272179	-2.056320	1.631565	0.007178	0.703355
-38.131166	-2.084479	1.636570	0.007152	0.703349
-37.915429	-2.118461	1.641574	0.007111	0.703358
-38.292563	-2.160549	1.646579	0.007182	0.703138
-39.325708	-2.037988	1.651584	0.007374	0.703013
-39.329317	-2.032980	1.656589	0.007374	0.703022
-39.312718	-2.040154	1.661594	0.007371	0.703014
-39.042707	-2.085594	1.666598	0.007321	0.703019
-39.142799	-2.071189	1.671603	0.007340	0.703012
-39.482332	-2.010421	1.676608	0.007403	0.703013
-39.444499	-2.101752	1.681613	0.007396	0.702842
-40.306846	-2.019772	1.686618	0.007556	0.702697
-40.139330	-2.045896	1.691622	0.007525	0.702705
-40.368456	-2.008830	1.696627	0.007568	0.702697
-40.331688	-2.015967	1.701632	0.007561	0.702696
-39.815780	-2.105910	1.706637	0.007465	0.702700
-40.306864	-2.020900	1.711642	0.007556	0.702695
-40.320151	-2.068203	1.716646	0.007558	0.702595
-40.983640	-2.058872	1.721651	0.007682	0.702375
-41.084888	-2.038813	1.726656	0.007701	0.702379
-40.865488	-2.076006	1.731661	0.007660	0.702383
-41.017968	-2.052796	1.736666	0.007688	0.702375
-40.902921	-2.067907	1.741670	0.007667	0.702386
-41.191637	-2.019904	1.746675	0.007720	0.702379
-40.850924	-2.130420	1.751680	0.007657	0.702278
-41.577427	-2.095521	1.756685	0.007792	0.702087
-42.103945	-2.005731	1.761690	0.007890	0.702079
-41.864291	-2.045456	1.766694	0.007845	0.702085
-41.722650	-2.073338	1.771699	0.007819	0.702080
-41.804680	-2.057401	1.776704	0.007834	0.702083
-41.921695	-2.034802	1.781709	0.007856	0.702086
-41.696033	-2.151600	1.786714	0.007814	0.701931
-42.959355	-2.012633	1.791718	0.008049	0.701757
-43.067288	-1.997748	1.796723	0.008069	0.701748
-42.928028	-2.020847	1.801728	0.008043	0.701752
-42.315986	-2.128558	1.806733	0.007929	0.701755
-42.970565	-2.017934	1.811738	0.008051	0.701742
-42.752065	-2.050495	1.816742	0.008010	0.701755
-42.834903	-2.076070	1.821747	0.008026	0.701674
-43.702725	-2.035890	1.826752	0.008187	0.701442
-43.644143	-2.043293	1.831757	0.008176	0.701448
-43.985526	-1.987278	1.836762	0.008240	0.701439
-43.604488	-2.050754	1.841766	0.008169	0.701448
-43.689313	-2.039062	1.846771	0.008185	0.701441
-43.595398	-2.054192	1.851776	0.008167	0.701444
-43.324683	-2.141560	1.856781	0.008117	0.701365
-44.910954	-1.976331	1.861786	0.008412	0.701127
-44.324509	-2.076054	1.866790	0.008303	0.701137
-44.310834	-2.081616	1.871795	0.008300	0.701131
-44.381638	-2.069532	1.876800	0.008313	0.701130
-44.428877	-2.059107	1.881805	0.008322	0.701134
-44.606895	-2.032798	1.886810	0.008355	0.701123
-44.214557	-2.146538	1.891814	0.008282	0.701034
-45.322054	-2.024289	1.896819	0.008488	0.700882
-45.170787	-2.051729	1.901824	0.008460	0.700881
-44.552728	-2.160559	1.906829	0.008345	0.700884
-45.098425	-2.067141	1.911834	0.008446	0.700876
-45.172305	-2.050194	1.916838	0.008460	0.700884
-44.885259	-2.133664	1.921843	0.008407	0.700819
-45.777201	-2.112901	1.926848	0.008573	0.700538
-45.599191	-2.140566	1.931853	0.008540	0.700547
-46.069035	-2.060978	1.936858	0.008627	0.700538
-45.776606	-2.108894	1.941862	0.008573	0.700547
-45.975317	-2.077965	1.946867	0.008609	0.700538
-46.391455	-2.003835	1.951872	0.008687	0.700538
-46.019511	-2.189003	1.956877	0.008618	0.700297
-47.061827	-2.042228	1.961882	0.008812	0.700218
-47.494990	-1.959942	1.966886	0.008892	0.700228
-46.784244	-2.090427	1.971891	0.008760	0.700221
-46.958562	-2.058304	1.976896	0.008792	0.700223
-47.267103	-2.001243	1.981901	0.008850	0.700227
-47.065363	-2.042302	1.986906	0.008812	0.700217
-46.874449	-2.177126	1.991910	0.008777	0.700012
-48.301536	-1.979369	1.996915	0.009042	0.699897
-47.783988	-2.070751	2.001920	0.008946	0.699899

-47.897975	-2.052739	2.011917	0.008967	0.699895
-47.536347	-2.116503	2.021914	0.008900	0.699896
-47.827236	-2.064400	2.031910	0.008954	0.699897
-47.867469	-2.116615	2.041907	0.008961	0.699777
-48.236347	-2.084488	2.051904	0.009030	0.699709
-48.215827	-2.065627	2.061901	0.009026	0.699754
-47.891585	-2.056679	2.071898	0.008965	0.699890
-47.822590	-2.065098	2.081894	0.008952	0.699898
-47.414739	-2.135257	2.091891	0.008876	0.699903
-47.979970	-2.033882	2.101888	0.008981	0.699905
-47.762483	-2.074367	2.111885	0.008941	0.699902
-47.738943	-2.080419	2.121882	0.008936	0.699898
-47.818570	-2.065145	2.131878	0.008951	0.699900
-47.699221	-2.085393	2.141875	0.008929	0.699903
-47.552816	-2.007731	2.151872	0.008901	0.700113
-47.292328	-1.999515	2.161869	0.008853	0.700224
-47.105988	-2.033444	2.171866	0.008818	0.700223
-47.095166	-2.035109	2.181862	0.008816	0.700224
-46.479400	-2.058868	2.191859	0.008701	0.700398
-46.425599	-1.998271	2.201856	0.008691	0.700541
-46.295122	-2.020194	2.211853	0.008667	0.700544
-46.221332	-2.034900	2.221850	0.008653	0.700541
-45.687929	-2.024183	2.231846	0.008553	0.700755
-45.240259	-2.041886	2.241843	0.008470	0.700882
-45.361349	-2.021532	2.251840	0.008492	0.700879
-45.359154	-2.022506	2.261837	0.008492	0.700878
-45.021969	-1.975394	2.271834	0.008429	0.701096
-44.726739	-2.013421	2.281830	0.008374	0.701125
-44.440252	-2.063162	2.291827	0.008321	0.701128
-44.401256	-1.995256	2.301824	0.008313	0.701280
-43.679030	-2.044494	2.311821	0.008179	0.701441
-43.948799	-1.997166	2.321818	0.008229	0.701440
-43.777437	-2.011359	2.331814	0.008197	0.701473
-42.964129	-2.019776	2.341811	0.008045	0.701750
-42.995267	-2.013726	2.351808	0.008051	0.701751
-42.855628	-2.041294	2.361805	0.008025	0.701746
-42.425140	-2.002524	2.371802	0.007945	0.701980
-42.043123	-2.022427	2.381798	0.007874	0.702077
-42.050251	-2.020233	2.391795	0.007875	0.702079
-41.983520	-2.003271	2.401792	0.007862	0.702138
-41.065425	-2.049443	2.411789	0.007691	0.702376
-41.397082	-1.990619	2.421786	0.007753	0.702375
-41.141805	-2.037572	2.431782	0.007705	0.702372
-40.566094	-2.018474	2.441779	0.007598	0.702619
-40.352438	-2.015386	2.451776	0.007558	0.702702
-40.295617	-2.027030	2.461773	0.007547	0.702699
-40.477347	-1.939940	2.471770	0.007581	0.702810
-39.311785	-2.048335	2.481766	0.007364	0.703011
-39.485254	-2.016869	2.491763	0.007396	0.703012
-39.486670	-2.016504	2.501760	0.007396	0.703013
-38.510548	-2.035232	2.511757	0.007215	0.703326
-38.378469	-2.048255	2.521754	0.007190	0.703348
-38.204714	-2.080323	2.531750	0.007158	0.703346
-38.447427	-2.019167	2.541747	0.007203	0.703382
-37.593379	-2.042300	2.551744	0.007044	0.703643
-37.378346	-2.082386	2.561741	0.007003	0.703639
-37.806057	-2.006946	2.571738	0.007083	0.703638
-37.155228	-2.050592	2.581734	0.006962	0.703784
-36.642118	-2.056997	2.591731	0.006866	0.703956
-36.650655	-2.054355	2.601728	0.006868	0.703958
-36.854111	-2.016768	2.611725	0.006905	0.703961
-35.984898	-2.022136	2.621722	0.006743	0.704263
-35.798172	-2.055663	2.631718	0.006709	0.704263
-35.807318	-2.053145	2.641715	0.006710	0.704265
-35.400535	-2.043981	2.651712	0.006634	0.704429
-34.777385	-2.074028	2.661709	0.006518	0.704593
-35.030957	-2.030222	2.671706	0.006565	0.704590
-34.781588	-2.073520	2.681702	0.006519	0.704593
-34.383862	-2.018276	2.691699	0.006445	0.704847
-34.064492	-2.052634	2.701696	0.006385	0.704893
-34.189896	-2.030941	2.711693	0.006408	0.704891
-34.041179	-1.982211	2.721690	0.006381	0.705043
-33.238548	-2.038509	2.731686	0.006231	0.705218
-33.408127	-2.007156	2.741683	0.006263	0.705221
-33.011951	-2.057949	2.751680	0.006189	0.705261
-32.201510	-2.067256	2.761677	0.006038	0.705533
-32.214603	-2.065897	2.771674	0.006040	0.705531
-32.127710	-2.082323	2.781670	0.006024	0.705529
-32.176039	-2.009621	2.791667	0.006033	0.705658
-31.131555	-2.089673	2.801664	0.005838	0.705872
-31.343678	-2.053068	2.811661	0.005878	0.705870
-31.264931	-2.069169	2.821658	0.005863	0.705866
-30.978536	-2.018945	2.831654	0.005809	0.706070
-30.661146	-2.043885	2.841651	0.005750	0.706133
-30.584698	-2.055418	2.851648	0.005736	0.706138
-30.420598	-2.024841	2.861645	0.005705	0.706258
-29.926674	-2.018279	2.871642	0.005613	0.706448
-29.830486	-2.035196	2.881638	0.005595	0.706449
-29.977568	-1.978722	2.891635	0.005623	0.706510
-28.819837	-2.060840	2.901632	0.005407	0.706760
-29.166532	-2.000095	2.911629	0.005471	0.706758
-28.801252	-2.067429	2.921626	0.005403	0.706754
-28.404788	-2.001890	2.931622	0.005329	0.707027
-27.914204	-2.060145	2.941619	0.005238	0.707086
-27.802131	-2.080553	2.951616	0.005217	0.707085
-28.044807	-2.004871	2.961613	0.005262	0.707151
-27.262812	-2.029781	2.971610	0.005116	0.707380
-27.102123	-2.057220	2.981606	0.005086	0.707383
-27.102438	-2.056700	2.991603	0.005086	0.707384
-26.459001	-2.038013	3.001600	0.004967	0.707652
-26.628933	-1.981817	3.011597	0.004998	0.707704
-26.107184	-2.076143	3.021594	0.004901	0.707702
-26.333899	-1.971868	3.031590	0.004943	0.707830
-25.195339	-2.081573	3.041587	0.004731	0.708017
-25.527235	-2.022030	3.051584	0.004793	0.708018
-25.588514	-2.010995	3.061581	0.004804	0.708018
-24.641657	-2.012718	3.071578	0.004627	0.708353
-24.495351	-2.038603	3.081574	0.004600	0.708354
-24.354106	-2.062572	3.091571	0.004574	0.708356
-24.319246	-2.002401	3.101568	0.004567	0.708489
-23.476001	-2.075759	3.111565	0.004410	0.708644
-23.633311	-2.047999	3.121562	0.004439	0.708643
-23.867562	-2.005316	3.131558	0.004483	0.708645
-22.924906	-2.026622	3.141555	0.004307	0.708939
-23.018084	-1.997176	3.151552	0.004324	0.708965
-22.639289	-2.067306	3.161549	0.004254	0.708960
-22.600421	-1.997247	3.171546	0.004247	0.709114
-22.014404	-2.025036	3.181542	0.004137	0.709268
-21.956122	-2.033474	3.191539	0.004126	0.709272
-22.173296	-1.971885	3.201536	0.004167	0.709318
-21.205117	-2.003331	3.211533	0.003986	0.709600
-21.093435	-2.023512	3.221530	0.003966	0.709600
-21.161277	-2.011854	3.231526	0.003978	0.709599
-20.452038	-2.032348	3.241523	0.003846	0.709811
-20.210260	-2.031778	3.251520	0.003801	0.709899
-20.199304	-2.036118	3.261517	0.003799	0.709894
-20.214091	-2.009992	3.271514	0.003801	0.709941
-19.528567	-1.992571	3.281510	0.003674	0.710220
-19.223065	-2.046235	3.291507	0.003617	0.710222
-19.381407	-2.017982	3.301504	0.003646	0.710222
-18.705019	-2.020117	3.311501	0.003520	0.710459
-18.356549	-2.043837	3.321498	0.003455	0.710536
-18.450169	-2.027861	3.331494	0.003472	0.710535
-18.265761	-2.043823	3.341491	0.003438	0.710568
-17.735109	-1.984418	3.351488	0.003339	0.710876
-17.288950	-2.063928	3.361485	0.003256	0.710876
-17.371429	-2.050603	3.371482	0.003271	0.710874
-17.395024	-2.001614	3.381478	0.003276	0.710963
-16.604796	-2.053900	3.391475	0.003128	0.711140
-16.891562	-2.002293	3.401472	0.003182	0.711141
-16.850300	-1.989949	3.411469	0.003174	0.711181
-16.135155	-1.979813	3.421466	0.003041	0.711455
-15.876993	-2.024095	3.431462	0.002992	0.711459
-16.020057	-1.996450	3.441459	0.003019	0.711463
-15.512251	-1.953659	3.451456	0.002924	0.711729
-15.044477	-2.017769	3.461453	0.002837	0.711768
-14.973385	-2.032988	3.471450	0.002824	0.711763
-14.680403	-2.008555	3.481446	0.002769	0.711916
-13.929670	-2.051551	3.491443	0.002629	0.712097
-14.260135	-1.992553	3.501440	0.002691	0.712097
-13.950573	-2.047637	3.511437	0.002633	0.712098
-13.853716	-1.934944	3.521434	0.002615	0.712357
-13.131162	-2.045843	3.531430	0.002480	0.712392
-13.483115	-1.982624	3.541427	0.002546	0.712394
-12.876143	-2.000722	3.551424	0.002433	0.712573
-12.435743	-2.007211	3.561421	0.002351	0.712717
-12.720169	-1.957124	3.571418	0.002403	0.712716
-12.422234	-1.978730	3.581414	0.002348	0.712778
-11.558704	-2.006122	3.591411	0.002187	0.713030
-11.494151	-2.018020	3.601408	0.002175	0.713030
-11.578728	-2.003778	3.611405	0.002191	0.713028
-11.125209	-1.973743	3.621402	0.002106	0.713249
-10.493643	-2.027970	3.631398	0.001988	0.713365
-10.825645	-1.968819	3.641395	0.002050	0.713365
-10.533252	-2.002019	3.651392	0.001996	0.713403
-9.895764	-1.989211	3.661389	0.001877	0.713654
-9.778706	-2.009991	3.671386	0.001855	0.713655
-9.627667	-2.036354	3.681382	0.001827	0.713656
-9.531687	-1.966064	3.691379	0.001809	0.713830
-8.792379	-2.024331	3.701376	0.001671	0.713976
-9.140482	-1.962629	3.711373	0.001736	0.713975
-8.996369	-1.963728	3.721370	0.001709	0.714024
-8.081576	-1.998080	3.731366	0.001538	0.714280
-7.935439	-2.023253	3.741363	0.001511	0.714282
-7.819172	-2.043143	3.751360	0.001489	0.714284
-7.567468	-1.982215	3.761357	0.001442	0.714494
-6.571183	-2.102049	3.771354	0.001257	0.714609
-6.603922	-2.094684	3.781350	0.001263	0.714612
-6.587052	-2.097929	3.791347	0.001260	0.714612
-6.531673	-2.062093	3.801344	0.001249	0.714703
-5.856039	-2.076425	3.811341	0.001123	0.714913
-5.800682	-2.087117	3.821338	0.001113	0.714912
-5.671133	-2.110514	3.831334	0.001089	0.714911
-5.917922	-2.000503	3.841331	0.001135	0.715042
-4.528173	-2.149286	3.851328	0.000876	0.715239
-4.872867	-2.088710	3.861325	0.000940	0.715237
-4.861109	-2.092581	3.871322	0.000938	0.715234
-4.536187	-2.070792	3.881318	0.000877	0.715392
-4.017180	-2.083322	3.891315	0.000780	0.715551
-4.085154	-2.069639	3.901312	0.000793	0.715554
-4.199316	-2.051315	3.911309	0.000814	0.715550
-3.409672	-2.027930	3.921306	0.000667	0.715875
-3.054660	-2.085731	3.931302	0.000601	0.715886
-2.878311	-2.117109	3.941299	0.000568	0.715886
-2.532175	-2.175735	3.951296	0.000503	0.715893
-2.422991	-2.071567	3.961293	0.000483	0.716138
-2.035300	-2.141775	3.971290	0.000411	0.716136
-2.462659	-2.063954	3.981286	0.000490	0.716139
-2.019959	-2.064180	3.991283	0.000408	0.716295
-1.535392	-2.070030	4.001280	0.000317	0.716455
-1.541971	-2.068466	4.011277	0.000318	0.716456
-1.477734	-2.047386	4.021274	0.000306	0.716520
-1.280990	-1.961664	4.031270	0.000270	0.716759
-1.201083	-1.975623	4.041267	0.000255	0.716760
-1.063683	-1.929767	4.051264	0.000229	0.716899
-0.875377	-1.867089	4.061261	0.000194	0.717090
-0.991398	-1.847689	4.071258	0.000215	0.717088
-0.790585	-1.737775	4.081254	0.000178	0.717376
-0.749448	-1.738781	4.091251	0.000170	0.717388
-0.709312	-1.616988	4.101248	0.000162	0.717644
-0.693960	-1.586117	4.111245	0.000159	0.717710
-0.808569	-1.434252	4.121242	0.000180	0.717970
-0.648646	-1.416813	4.131238	0.000151	0.718061
-0.437594	-1.305196	4.141235	0.000111	0.718356
-0.408234	-1.243459	4.151232	0.000106	0.718488
-0.387785	-1.166741	4.161229	0.000102	0.718647
-0.168850	-1.058820	4.171226	0.000061	0.718937
-0.139464	-0.987366	4.181222	0.000055	0.719089
-0.056312	-0.907997	4.191219	0.000039	0.719274
-0.010888	-0.751680	4.201216	0.000031	0.719599
-0.089566	-0.640171	4.211213	0.000045	0.719791
-0.093173	-0.522569	4.221210	0.000046	0.720022
-0.100919	-0.391335	4.231206	0.000047	0.720278
-0.178804	-0.237005	4.241203	0.000061	0.720554
-0.079263	-0.089198	4.251200	0.000043	0.720880
0.001534	0.010651	4.261197	0.000027	0.721105
-0.184753	0.189055	4.271194	0.000062	0.721391
0.000000	0.315912	4.281190	0.000027	0.721705

0.014573	0.939878	4.286195	0.000024	0.722936
0.349243	2.145365	4.291200	-0.000039	0.725414
0.347702	3.995510	4.296205	-0.000040	0.729022
0.552208	6.361318	4.301210	-0.000080	0.733682
1.052327	9.186327	4.306214	-0.000175	0.739294
1.181732	12.558975	4.311219	-0.000201	0.745781
1.575010	16.340505	4.316224	-0.000277	0.753071
2.117518	20.493931	4.321229	-0.000380	0.761033
2.252619	25.128579	4.326234	-0.000409	0.769667
2.788153	30.055410	4.331238	-0.000512	0.778867
3.259793	35.337892	4.336243	-0.000603	0.788579
3.930981	40.916321	4.341248	-0.000732	0.798761
4.211506	46.854838	4.346253	-0.000788	0.809324
4.819985	53.025609	4.351258	-0.000905	0.820253
5.250915	59.501227	4.356262	-0.000990	0.831505
5.441778	66.235703	4.361267	-0.001030	0.842971
5.972155	73.138475	4.366272	-0.001133	0.854661
6.233433	80.277972	4.371277	-0.001186	0.866503
6.800462	87.564221	4.376282	-0.001297	0.878510
7.354656	95.023926	4.381286	-0.001405	0.890626
7.745400	102.670363	4.386291	-0.001482	0.902828
8.175215	110.459252	4.391296	-0.001568	0.915099
8.562264	118.351100	4.396301	-0.001645	0.927352
9.088348	126.361787	4.401306	-0.001748	0.939662
9.464356	134.492833	4.406310	-0.001823	0.951953
9.999730	142.675560	4.411315	-0.001928	0.964203
10.432862	150.971584	4.416320	-0.002015	0.976439
18.270806	158.102665	4.421325	-0.003479	0.988701
23.359496	165.952489	4.426330	-0.004431	1.001150
23.580763	174.660754	4.431334	-0.004478	1.013460
23.863933	183.373173	4.436339	-0.004537	1.025643
24.199433	192.108101	4.441344	-0.004605	1.037725
24.108275	200.901846	4.446349	-0.004594	1.049649
24.542712	209.622263	4.451354	-0.004680	1.061461
24.882653	218.367462	4.456358	-0.004749	1.073155
25.085379	227.109256	4.461363	-0.004793	1.084687
26.386439	235.683248	4.466368	-0.005041	1.096125
26.965084	244.368245	4.471373	-0.005154	1.107427
27.459068	253.090843	4.476378	-0.005252	1.118644
28.075598	261.765001	4.481382	-0.005372	1.129715
28.788652	270.421542	4.486387	-0.005511	1.140677
29.522354	279.107766	4.491392	-0.005653	1.151575
30.009211	287.781297	4.496397	-0.005749	1.162304
30.494771	296.445466	4.501402	-0.005846	1.172923
31.356983	305.030520	4.506406	-0.006012	1.183428
31.697084	313.693362	4.511411	-0.006081	1.193827
32.706468	322.218831	4.516416	-0.006274	1.204108
33.374425	330.803189	4.521421	-0.006404	1.214303
33.726502	339.422889	4.526426	-0.006476	1.224392
34.473251	347.986599	4.531430	-0.006620	1.234410
35.213883	356.494066	4.536435	-0.006764	1.244282
35.649839	365.073390	4.541440	-0.006851	1.254099
36.022414	373.619067	4.546445	-0.006926	1.263790
36.589026	382.142685	4.551450	-0.007037	1.273419
37.088510	390.637435	4.556454	-0.007135	1.282931
37.365469	399.169851	4.561459	-0.007192	1.292373
38.259635	407.586772	4.566464	-0.007364	1.301733
38.863339	416.103188	4.571469	-0.007482	1.311081
39.314116	424.614308	4.576474	-0.007572	1.320330
39.941845	433.008944	4.581478	-0.007694	1.329421
40.331457	441.439193	4.586483	-0.007772	1.338446
41.075978	449.808648	4.591488	-0.007917	1.347408
41.805985	458.177837	4.596493	-0.008058	1.356309
42.420562	466.551040	4.601498	-0.008178	1.365135
42.839419	474.964080	4.606502	-0.008261	1.373911
43.161320	483.362180	4.611507	-0.008327	1.382600
43.636622	491.760796	4.616512	-0.008421	1.391261
43.945706	500.134174	4.621517	-0.008484	1.399815
44.459443	508.464140	4.626522	-0.008585	1.408307
44.918126	516.812344	4.631526	-0.008676	1.416757
45.084130	525.172043	4.636531	-0.008712	1.425120
45.696296	533.487498	4.641536	-0.008832	1.433463
45.886710	541.819085	4.646541	-0.008873	1.441705
46.200434	550.146620	4.651546	-0.008937	1.449916
46.817507	558.424130	4.656550	-0.009057	1.458081
47.247867	566.713380	4.661555	-0.009143	1.466182
47.647940	575.072945	4.666560	-0.009223	1.474300
48.093285	583.328389	4.671565	-0.009311	1.482282
48.380758	591.621490	4.676570	-0.009370	1.490232
48.812656	599.896772	4.681574	-0.009456	1.498145
49.005836	608.171767	4.686579	-0.009497	1.505980
49.472170	616.449319	4.691584	-0.009589	1.513818
49.497994	624.740552	4.696589	-0.009600	1.521561
49.825569	632.998438	4.701594	-0.009666	1.529280
50.368303	641.224963	4.706598	-0.009772	1.536963
50.879495	649.434336	4.711603	-0.009873	1.544587
51.474972	657.679686	4.716608	-0.009989	1.552219
51.830284	665.912276	4.721613	-0.010061	1.559766
52.180134	674.140348	4.726618	-0.010131	1.567273
52.599652	682.377490	4.731622	-0.010215	1.574761
52.988080	690.587401	4.736627	-0.010293	1.582185
53.597349	698.797675	4.741632	-0.010412	1.589606
53.926022	707.034836	4.746637	-0.010478	1.596976
54.335114	715.240112	4.751642	-0.010560	1.604296
54.929577	723.438198	4.756646	-0.010676	1.611602
55.299408	731.661144	4.761651	-0.010750	1.618865
55.533960	739.900129	4.766656	-0.010799	1.626090
56.103548	748.135674	4.771661	-0.010911	1.633327
56.633068	756.304183	4.776666	-0.011015	1.640469
56.936362	764.512119	4.781670	-0.011076	1.647582
57.038703	772.748332	4.786675	-0.011101	1.654661
57.874674	780.858267	4.791680	-0.011262	1.661702
58.482127	789.019243	4.796685	-0.011380	1.668726
58.566975	797.269569	4.801690	-0.011402	1.675725
59.236139	805.395011	4.806694	-0.011532	1.682668
59.427946	813.604594	4.811699	-0.011573	1.689589
59.665598	821.836357	4.816704	-0.011622	1.696507
59.994557	830.002931	4.821709	-0.011689	1.703354
60.477680	838.175057	4.826714	-0.011784	1.710198
60.883508	846.371814	4.831718	-0.011865	1.717025
61.187877	854.511017	4.836723	-0.011927	1.723765
61.541221	862.696860	4.841728	-0.011998	1.730523
61.746585	870.888906	4.846733	-0.012042	1.737240
62.020086	879.054370	4.851738	-0.012098	1.743919
62.456825	887.211441	4.856742	-0.012185	1.750586
62.996825	895.338624	4.861747	-0.012291	1.757216
63.282019	903.507283	4.866752	-0.012349	1.763823
63.651651	911.653137	4.871757	-0.012423	1.770397
64.202826	919.796908	4.876762	-0.012531	1.776967
64.574021	927.958282	4.881766	-0.012606	1.783505
64.904042	936.119099	4.886771	-0.012673	1.790014
65.257283	944.325978	4.891776	-0.012744	1.796538
65.585243	952.450507	4.896781	-0.012810	1.802970
65.799290	960.609448	4.901786	-0.012856	1.809393
66.435897	968.713932	4.906790	-0.012979	1.815801
66.762706	976.849066	4.911795	-0.013046	1.822173
67.274739	984.983877	4.916800	-0.013146	1.828545
67.437296	993.162505	4.921805	-0.013182	1.834886
68.076856	1001.259574	4.926810	-0.013306	1.841200
68.571657	1009.392610	4.931814	-0.013404	1.847502
68.505416	1017.590435	4.936819	-0.013397	1.853767
69.235166	1025.679354	4.941824	-0.013538	1.860020
69.329981	1033.843051	4.946829	-0.013561	1.866235
69.575181	1042.017930	4.951834	-0.013612	1.872455
69.811541	1050.171677	4.956838	-0.013661	1.878638
70.190064	1058.237992	4.961843	-0.013737	1.884751
70.541427	1066.373556	4.966848	-0.013808	1.890892
70.898963	1074.496491	4.971853	-0.013880	1.897006
71.679159	1082.547867	4.976858	-0.014030	1.903093
72.374458	1090.646600	4.981862	-0.014165	1.909187
72.548058	1098.810232	4.986867	-0.014203	1.915251
72.915163	1106.935087	4.991872	-0.014277	1.921288
73.286948	1115.047951	4.996877	-0.014351	1.927298
73.523915	1123.211495	5.001882	-0.014401	1.933312
73.816263	1131.347876	5.006886	-0.014460	1.939293
74.228250	1139.432256	5.011891	-0.014542	1.945231
74.581072	1147.601801	5.016896	-0.014614	1.951206
74.714421	1155.759049	5.021901	-0.014644	1.957130
74.979886	1163.849508	5.026906	-0.014698	1.963002
75.239357	1171.964685	5.031910	-0.014752	1.968874
75.508887	1180.068858	5.036915	-0.014808	1.974721
75.704274	1188.192197	5.041920	-0.014849	1.980557
76.277720	1196.243294	5.046925	-0.014961	1.986364
76.386574	1204.393042	5.051930	-0.014987	1.992175
76.955116	1212.468015	5.056934	-0.015098	1.997965
77.160444	1220.556262	5.061939	-0.015142	2.003709
77.446913	1228.684472	5.066944	-0.015200	2.009473
77.700917	1236.797080	5.071949	-0.015253	2.015206
77.999418	1244.891235	5.076954	-0.015314	2.020915
78.626412	1252.963421	5.081958	-0.015436	2.026626
78.848443	1261.103564	5.086963	-0.015483	2.032326
78.928059	1269.249737	5.091968	-0.015503	2.038000
79.376773	1277.301350	5.096973	-0.015592	2.043631
79.538604	1285.423753	5.101978	-0.015627	2.049265
79.693397	1293.552695	5.106982	-0.015661	2.054888
80.115732	1301.605577	5.111987	-0.015745	2.060470
80.599319	1309.695621	5.116992	-0.015841	2.066069
81.049553	1317.786377	5.121997	-0.015930	2.071649
81.566318	1325.867860	5.127002	-0.016031	2.077215
81.927704	1333.944448	5.132006	-0.016104	2.082747
82.070436	1342.055715	5.137011	-0.016136	2.088266
82.566585	1350.158962	5.142016	-0.016234	2.093800
83.030464	1358.230385	5.147021	-0.016325	2.099294
83.235007	1366.336971	5.152026	-0.016369	2.104772
83.511493	1374.476795	5.157030	-0.016425	2.110266
84.015756	1382.584167	5.162035	-0.016525	2.115745
84.672447	1390.607224	5.167040	-0.016652	2.121168
84.828191	1398.709635	5.172045	-0.016687	2.126583
84.949253	1406.829353	5.177050	-0.016714	2.131991
85.726164	1414.855568	5.182054	-0.016864	2.137386
86.039863	1422.934124	5.187059	-0.016928	2.142759
86.218150	1431.062789	5.192064	-0.016967	2.148138
86.412937	1439.176128	5.197069	-0.017008	2.153494
86.494422	1447.284104	5.202074	-0.017029	2.158824
86.813286	1455.342767	5.207078	-0.017093	2.164130
87.158936	1463.420516	5.212083	-0.017163	2.169438
87.801439	1471.494567	5.217088	-0.017288	2.174758
87.952626	1479.592783	5.222093	-0.017321	2.180035
88.237513	1487.664062	5.227098	-0.017380	2.185295
88.786794	1495.755495	5.232102	-0.017487	2.190579
89.105012	1503.845069	5.237107	-0.017552	2.195827
89.287429	1511.929728	5.242112	-0.017591	2.201048
89.497377	1520.005994	5.247117	-0.017636	2.206253
89.703849	1528.111749	5.252122	-0.017679	2.211465
90.087894	1536.181733	5.257126	-0.017756	2.216657
90.318709	1544.244908	5.262131	-0.017804	2.221819
90.825977	1552.300026	5.267136	-0.017904	2.226989
90.965570	1560.421068	5.272141	-0.017936	2.232155
91.197002	1568.504507	5.277146	-0.017984	2.237294
91.596243	1576.574364	5.282150	-0.018064	2.242428
91.937754	1584.629410	5.287155	-0.018132	2.247535
92.084909	1592.743776	5.292160	-0.018165	2.252651
92.275148	1600.827873	5.297165	-0.018206	2.257739
92.707955	1608.873445	5.302170	-0.018292	2.262814
92.882098	1616.981033	5.307174	-0.018330	2.267893
93.187274	1625.101320	5.312179	-0.018392	2.272980
93.661464	1633.155327	5.317184	-0.018485	2.278029
93.927300	1641.192348	5.322189	-0.018540	2.283038
94.198857	1649.245168	5.327194	-0.018596	2.288047
94.597938	1657.324833	5.332198	-0.018676	2.293071
94.748858	1665.387173	5.337203	-0.018709	2.298053
95.028883	1673.462607	5.342208	-0.018766	2.303044
95.331036	1681.506891	5.347213	-0.018828	2.308006
95.783759	1689.575393	5.352218	-0.018918	2.312985
96.083043	1697.664941	5.357222	-0.018979	2.317953
96.055545	1705.745952	5.362227	-0.018979	2.322878
96.775076	1713.766381	5.367232	-0.019118	2.327817
97.056463	1721.851141	5.372237	-0.019176	2.332749
96.950951	1729.972292	5.377242	-0.019161	2.337661
97.470957	1738.008991	5.382246	-0.019264	2.342562
97.640838	1746.073059	5.387251	-0.019300	2.347441
97.846268	1754.195937	5.392256	-0.019344	2.352348
98.190350	1762.240716	5.397261	-0.019413	2.357210
98.530749	1770.271307	5.402266	-0.019482	2.362052
98.734103	1778.362161	5.407270	-0.019525	2.366909
98.982465	1786.421330	5.412275	-0.019577	2.371742
99.315870	1794.492762	5.417280	-0.019644	2.376578
99.595551	1802.557861	5.422285	-0.019702	2.381396
99.791524	1810.611214	5.427290	-0.019743	2.386191
100.174177	1818.684156	5.432294	-0.019820	2.391003
100.347968	1826.755798	5.437299	-0.019858	2.395787
100.688874	1834.800477	5.442304	-0.019926	2.400560
100.865916	1842.869430	5.447309	-0.019965	2.405324
101.098786	1850.935114	5.452314	-0.020013	2.410081
101.720609	1858.989478	5.457318	-0.020134	2.414852
101.765317	1867.060378	5.462323	-0.020148	2.419579
102.061700	1875.119653	5.467328	-0.020208	2.424309
102.275605	1883.203099	5.472333	-0.020254	2.429038
102.418350	1891.346221	5.477338	-0.020285	2.433786
102.909226	1899.367146	5.482342	-0.020382	2.438481
103.338843	1907.367976	5.487347	-0.020467	2.443151
103.581798	1915.424337	5.492352	-0.020518	2.447829
103.854441	1923.492652	5.497357	-0.020574	2.452508
104.236894	1931.532609	5.502362	-0.020651	2.457170
104.313586	1939.627293	5.507366	-0.020670	2.461831
104.313929	1947.684479	5.512371	-0.020675	2.466456
104.526698	1955.766712	5.517376	-0.020720	2.471103
104.784584	1963.838754	5.522381	-0.020774	2.475738
104.989561	1971.868381	5.527386	-0.020817	2.480336
105.439468	1979.891652	5.532390	-0.020906	2.484941
105.724061	1987.947421	5.537395	-0.020964	2.489543
105.958551	1996.047898	5.542400	-0.021013	2.494158
106.034785	2004.116164	5.547405	-0.021033	2.498735
106.366725	2012.136424	5.552410	-0.021100	2.503295
106.796207	2020.201852	5.557414	-0.021185	2.507879
106.936093	2028.293532	5.562419	-0.021217	2.512449
107.285575	2036.348654	5.567424	-0.021287	2.517005
107.692269	2044.349196	5.572429	-0.021368	2.521526
107.813928	2052.401442	5.577434	-0.021396	2.526047
108.154718	2060.466136	5.582438	-0.021465	2.530583
108.683731	2068.487619	5.587443	-0.021568	2.535100
108.898085	2076.551270	5.592448	-0.021614	2.539610
109.062656	2084.624224	5.597453	-0.021650	2.544113
109.514970	2092.657843	5.602458	-0.021739	2.548607
109.982933	2100.726488	5.607462	-0.021832	2.553113
110.063843	2108.794673	5.612467	-0.021852	2.557585
110.359405	2116.834312	5.617472	-0.021912	2.562047
110.712552	2124.878896	5.622477	-0.021983	2.566508
111.227716	2132.931165	5.627482	-0.022085	2.570977
111.621538	2141.012772	5.632486	-0.022163	2.575446
111.941109	2149.026596	5.637491	-0.022228	2.579865
112.156810	2157.094793	5.642496	-0.022273	2.584299
112.417522	2165.164198	5.647501	-0.022327	2.588728
112.952108	2173.346693	5.652506	-0.022432	2.593231
113.769348	2181.347547	5.657510	-0.022590	2.597646
114.082726	2189.338086	5.662515	-0.022653	2.602013
114.442396	2197.373594	5.667520	-0.022725	2.606401
114.862121	2205.414243	5.672525	-0.022809	2.610788
115.076471	2213.467919	5.677530	-0.022854	2.615161
115.196081	2221.531060	5.682534	-0.022882	2.619525
115.523842	2229.562543	5.687539	-0.022948	2.623879
116.080531	2237.592322	5.692544	-0.023057	2.628240
116.136206	2245.699661	5.697549	-0.023073	2.632602
116.312449	2253.746243	5.702554	-0.023111	2.636932
116.604573	2261.802402	5.707558	-0.023170	2.641267
116.777806	2269.833139	5.712563	-0.023208	2.645575
117.123981	2277.873413	5.717568	-0.023278	2.649891
117.520457	2285.946930	5.722573	-0.023357	2.654221
117.719534	2293.996669	5.727578	-0.023399	2.658519
117.871563	2302.037671	5.732582	-0.023433	2.662802
117.979958	2310.086435	5.737587	-0.023458	2.667080
118.355263	2318.175877	5.742592	-0.023533	2.671389
118.497544	2326.254931	5.747597	-0.023565	2.675671
118.829903	2334.241710	5.752602	-0.023632	2.679909
119.041367	2342.277904	5.757606	-0.023677	2.684159
119.405996	2350.288858	5.762611	-0.023750	2.688399
119.621569	2358.374670	5.767616	-0.023796	2.692662
119.866431	2366.412135	5.772621	-0.023846	2.696894
120.152024	2374.440775	5.777626	-0.023905	2.701118
120.384121	2382.498737	5.782630	-0.023953	2.705347
120.747482	2390.505244	5.787635	-0.024026	2.709551
121.073878	2398.593550	5.792640	-0.024092	2.713788
121.089401	2406.668236	5.797645	-0.024101	2.717993
121.366638	2414.655078	5.802650	-0.024157	2.722161
121.771606	2422.708948	5.807654	-0.024238	2.726366
121.896206	2430.764826	5.812659	-0.024267	2.730548
122.180178	2438.837156	5.817664	-0.024325	2.734742
122.406039	2446.880551	5.822669	-0.024372	2.738910
122.667040	2454.906737	5.827674	-0.024426	2.743066
123.041721	2462.953657	5.832678	-0.024501	2.747233
123.035878	2471.058519	5.837683	-0.024505	2.751400
123.302968	2479.159957	5.842688	-0.024560	2.755576
123.542068	2487.152198	5.847693	-0.024610	2.759688
123.539212	2495.174529	5.852698	-0.024615	2.763794
123.902357	2503.197689	5.857702	-0.024688	2.767917
124.124169	2511.241602	5.862707	-0.024734	2.772035
124.584150	2519.281439	5.867712	-0.024825	2.776160
124.991517	2527.286218	5.872717	-0.024906	2.780257
124.882912	2535.334825	5.877722	-0.024891	2.784340
125.389384	2543.392678	5.882726	-0.024991	2.788458
125.642115	2551.412618	5.887731	-0.025043	2.792536
126.191427	2559.439104	5.892736	-0.025151	2.796628
126.165734	2567.534260	5.897741	-0.025152	2.800715
126.317479	2575.521638	5.902746	-0.025185	2.804753
126.729011	2583.575044	5.907750	-0.025267	2.808832
126.817613	2591.657671	5.912755	-0.025289	2.812902
126.790122	2599.738643	5.917760	-0.025289	2.816959
127.183424	2607.749985	5.922765	-0.025367	2.820998
127.437454	2615.746550	5.927770	-0.025420	2.825017
127.514952	2623.857927	5.932774	-0.025440	2.829077
127.763072	2631.907730	5.937779	-0.025491	2.833111
128.140911	2639.928058	5.942784	-0.025567	2.837131
128.518094	2647.937462	5.947789	-0.025642	2.841140
128.756100	2655.938998	5.952794	-0.025692	2.845131
129.088156	2664.004814	5.957798	-0.025759	2.849154
129.339978	2672.071128	5.962803	-0.025811	2.853167
129.269560	2680.152513	5.967808	-0.025803	2.857164
129.734431	2688.150091	5.972813	-0.025895	2.861144
129.951647	2696.148328	5.977818	-0.025941	2.865104
130.072099	2704.247842	5.982822	-0.025969	2.869104
130.263140	2712.295607	5.987827	-0.026010	2.873076
130.709218	2720.307010	5.992832	-0.026098	2.877039
130.945349	2728.361442	5.997837	-0.026147	2.881007
131.187705	2736.358868	6.002842	-0.026198	2.884941
131.646619	2744.389182	6.007846	-0.026288	2.888897
131.776708	2752.471145	6.012851	-0.026318	2.892855
131.847050	2760.531213	6.017856	-0.026336	2.896794
132.112633	2768.565295	6.022861	-0.026391	2.900726
132.604740	2776.535976	6.027866	-0.026488	2.904634
132.715980	2784.647722	6.032870	-0.026514	2.908584
132.936932	2792.742392	6.037875	-0.026560	2.912526
133.552300	2800.769992	6.042880	-0.026680	2.916452
133.658185	2808.783393	6.047885	-0.026705	2.920338
134.079521	2816.734205	6.052890	-0.026789	2.924206
134.308181	2824.808704	6.057894	-0.026837	2.928118
134.415238	2832.854298	6.062899	-0.026862	2.932004
134.493932	2840.934477	6.067904	-0.026882	2.935900
134.628734	2848.945949	6.072909	-0.026912	2.939761
135.018236	2856.935167	6.077914	-0.026990	2.943620
135.314425	2865.005104	6.082918	-0.027050	2.947507
135.384921	2873.047040	6.087923	-0.027069	2.951364
135.635672	2881.104878	6.092928	-0.027121	2.955232
135.885920	2889.123133	6.097933	-0.027173	2.959077
136.041300	2897.153659	6.102938	-0.027207	2.962918
136.323845	2905.203316	6.107942	-0.027265	2.966769
136.460391	2913.229372	6.112947	-0.027295	2.970597
136.677089	2921.289477	6.117952	-0.027341	2.974440
136.939841	2929.313096	6.122957	-0.027395	2.978263
137.232586	2937.330135	6.127962	-0.027455	2.982079
137.510813	2945.393455	6.132966	-0.027512	2.985911
137.895059	2953.376099	6.137971	-0.027589	2.989706
138.253293	2961.455187	6.142976	-0.027661	2.993540
138.466343	2969.494640	6.147981	-0.027706	2.997344
138.744799	2977.503696	6.152986	-0.027763	3.001131
138.959505	2985.534393	6.157990	-0.027808	3.004920
139.326927	2993.551955	6.162995	-0.027882	3.008706
139.435943	3001.628939	6.168000	-0.027908	3.012503
139.820131	3009.680645	6.173005	-0.027984	3.016296
140.228905	3017.668722	6.178010	-0.028066	3.020056
140.505713	3025.703482	6.183014	-0.028123	3.023826
140.578779	3033.752284	6.188019	-0.028142	3.027589
140.945779	3041.807998	6.193024	-0.028215	3.031364
141.242448	3049.871874	6.198029	-0.028276	3.035134
141.331938	3057.880141	6.203034	-0.028298	3.038865
141.659406	3065.928117	6.208038	-0.028364	3.042620
141.985085	3073.937260	6.213043	-0.028430	3.046353
142.272845	3081.967727	6.218048	-0.028489	3.050089
142.445460	3090.040295	6.223053	-0.028526	3.053834
142.509226	3098.059062	6.228058	-0.028543	3.057545
142.792289	3106.102999	6.233062	-0.028601	3.061273
142.835831	3114.110303	6.238067	-0.028615	3.064969
142.971849	3122.189728	6.243072	-0.028645	3.068698
143.377284	3130.286206	6.248077	-0.028726	3.072442
143.454015	3138.328353	6.253082	-0.028746	3.076142
143.626352	3146.311989	6.258086	-0.028783	3.079814
144.025614	3154.282240	6.263091	-0.028863	3.083487
144.327524	3162.315716	6.268096	-0.028924	3.087180
144.511631	3170.349698	6.273101	-0.028964	3.090863
144.792344	3178.395250	6.278106	-0.029021	3.094551
145.185821	3186.420035	6.283110	-0.029100	3.098231
145.318758	3194.447830	6.288115	-0.029130	3.101895
145.511357	3202.484703	6.293120	-0.029171	3.105563
145.918310	3210.495311	6.298125	-0.029252	3.109223
145.931730	3218.579625	6.303130	-0.029260	3.112895
146.185868	3226.657779	6.308134	-0.029312	3.116570
146.441626	3234.632361	6.313139	-0.029365	3.120195
146.687097	3242.619444	6.318144	-0.029416	3.123820
146.843084	3250.682164	6.323149	-0.029450	3.127471
146.927233	3258.734508	6.328154	-0.029471	3.131110
147.294147	3266.784997	6.333158	-0.029545	3.134757
147.380061	3274.808221	6.338163	-0.029566	3.138374
147.669922	3282.837374	6.343168	-0.029626	3.141999
148.084556	3290.842859	6.348173	-0.029708	3.145615
148.153798	3298.872789	6.353178	-0.029726	3.149222
148.378297	3306.960903	6.358182	-0.029773	3.152858
148.695228	3314.988075	6.363187	-0.029838	3.156466
148.833638	3322.979114	6.368192	-0.029869	3.160046
149.062878	3331.015219	6.373197	-0.029917	3.163647
149.200129	3339.026816	6.378202	-0.029947	3.167228
149.544720	3347.077960	6.383206	-0.030017	3.170832
149.564028	3355.134058	6.388211	-0.030026	3.174420
149.910873	3363.147368	6.393216	-0.030096	3.177998
150.308505	3371.182588	6.398221	-0.030175	3.181585
150.647647	3379.132729	6.403226	-0.030243	3.185127
150.833755	3387.242564	6.408230	-0.030283	3.188730
151.140007	3395.259175	6.413235	-0.030346	3.192292
151.528701	3403.314475	6.418240	-0.030423	3.195870
151.605302	3411.330209	6.423245	-0.030443	3.199415
151.766766	3419.329119	6.428250	-0.030478	3.202951
152.220694	3427.387908	6.433254	-0.030568	3.206522
152.198680	3435.434938	6.438259	-0.030569	3.210064
152.291912	3443.497023	6.443264	-0.030592	3.213613
152.692112	3451.502188	6.448269	-0.030671	3.217146
152.916779	3459.508651	6.453274	-0.030719	3.220669
153.110252	3467.527636	6.458278	-0.030760	3.224192
153.166861	3475.588993	6.463283	-0.030776	3.227724
153.500359	3483.658352	6.468288	-0.030843	3.231267
154.016278	3491.711871	6.473293	-0.030944	3.234806
154.321168	3499.675993	6.478298	-0.031006	3.238294
154.681739	3507.693850	6.483302	-0.031079	3.241804
154.889262	3515.703191	6.488307	-0.031123	3.245300
154.768774	3523.752313	6.493312	-0.031106	3.248796
155.055729	3531.791884	6.498317	-0.031164	3.252301
155.400034	3539.823483	6.503322	-0.031234	3.255800
155.648540	3547.845320	6.508326	-0.031285	3.259288
155.664646	3555.873376	6.513331	-0.031294	3.262766
156.013360	3563.902698	6.518336	-0.031364	3.266254
156.126527	3571.942760	6.523341	-0.031390	3.269733
156.081309	3579.991399	6.528346	-0.031387	3.273206
156.519071	3588.016998	6.533350	-0.031474	3.276684
156.795120	3596.006549	6.538355	-0.031530	3.280136
156.913613	3604.014559	6.543360	-0.031558	3.283587
157.177591	3612.065880	6.548365	-0.031612	3.287059
157.234496	3620.098676	6.553370	-0.031628	3.290510
157.719247	3628.157551	6.558374	-0.031724	3.293986
157.895678	3636.169006	6.563379	-0.031762	3.297426
158.211150	3644.197637	6.568384	-0.031826	3.300875
158.490466	3652.185458	6.573389	-0.031883	3.304301
158.447042	3660.256541	6.578394	-0.031880	3.307747
158.782159	3668.323596	6.583398	-0.031948	3.311202
158.911167	3676.362575	6.588403	-0.031977	3.314634
159.331075	3684.328452	6.593408	-0.032061	3.318042
159.430933	3692.372120	6.598413	-0.032085	3.321467
159.623242	3700.357193	6.603418	-0.032126	3.324868
159.958714	3708.397551	6.608422	-0.032193	3.328294
160.016612	3716.457459	6.613427	-0.032209	3.331714
160.224378	3724.505927	6.618432	-0.032253	3.335131
160.414950	3732.530306	6.623437	-0.032294	3.338534
160.514504	3740.541351	6.628442	-0.032318	3.341925
160.938639	3748.541972	6.633446	-0.032402	3.345319
161.288142	3756.578135	6.638451	-0.032473	3.348723
161.366429	3764.662434	6.643456	-0.032492	3.352133
161.593450	3772.707294	6.648461	-0.032540	3.355528
161.871372	3780.681769	6.653466	-0.032597	3.358892
162.005259	3788.707986	6.658470	-0.032627	3.362270
162.227664	3796.713169	6.663475	-0.032674	3.365638
162.464656	3804.723745	6.668480	-0.032723	3.369006
162.846905	3812.794174	6.673485	-0.032800	3.372400
162.858099	3820.832891	6.678490	-0.032807	3.375765
163.217889	3828.856727	6.683494	-0.032879	3.379132
163.193437	3836.892918	6.688499	-0.032880	3.382488
163.291677	3844.927450	6.693504	-0.032904	3.385844
163.616947	3852.952337	6.698509	-0.032969	3.389200
163.845621	3861.030232	6.703514	-0.033017	3.392572
164.193184	3869.096527	6.708518	-0.033087	3.395940
164.103712	3877.045299	6.713523	-0.033076	3.399240
164.412767	3885.028607	6.718528	-0.033139	3.402565
164.806788	3893.085082	6.723533	-0.033217	3.405920
164.821418	3901.085549	6.728538	-0.033225	3.409236
165.063798	3909.117154	6.733542	-0.033276	3.412569
165.468310	3917.174264	6.738547	-0.033356	3.415915
165.516703	3925.165337	6.743552	-0.033371	3.419218
165.717680	3933.177310	6.748557	-0.033413	3.422532
165.856737	3941.204518	6.753562	-0.033444	3.425846
166.282973	3949.256183	6.758566	-0.033529	3.429177
166.566619	3957.320733	6.763571	-0.033587	3.432506
166.891469	3965.342021	6.768576	-0.033653	3.435815
167.085537	3973.333190	6.773581	-0.033694	3.439103
167.289798	3981.335083	6.778586	-0.033738	3.442394
167.607151	3989.365275	6.783590	-0.033802	3.445696
167.915777	3997.381153	6.788595	-0.033865	3.448989
168.161105	4005.431328	6.793600	-0.033916	3.452291
168.183156	4013.523362	6.798605	-0.033925	3.455599
168.480054	4021.487884	6.803610	-0.033986	3.458861
168.810985	4029.534669	6.808614	-0.034053	3.462155
169.119760	4037.519013	6.813619	-0.034115	3.465420
169.380129	4045.568592	6.818624	-0.034169	3.468706
169.976389	4053.606120	6.823629	-0.034285	3.471995
169.989417	4061.678629	6.828634	-0.034293	3.475276
170.089577	4069.684957	6.833638	-0.034317	3.478530
170.191258	4077.709494	6.838643	-0.034341	3.481789
170.407842	4085.682454	6.843648	-0.034387	3.485027
170.759723	4093.701675	6.848653	-0.034458	3.488285
170.837461	4101.759321	6.853658	-0.034477	3.491547
171.086240	4109.777936	6.858662	-0.034529	3.494795
171.317743	4117.792330	6.863667	-0.034577	3.498038
171.287570	4125.827667	6.868672	-0.034577	3.501279
171.416558	4133.834836	6.873677	-0.034606	3.504510
171.487961	4141.868659	6.878682	-0.034625	3.507746
171.733196	4149.922919	6.883686	-0.034676	3.510994
172.086266	4157.939145	6.888691	-0.034747	3.514226
172.185954	4165.983167	6.893696	-0.034771	3.517459
172.260727	4174.023315	6.898701	-0.034790	3.520687
172.574129	4181.958339	6.903706	-0.034853	3.523877
172.797814	4190.024553	6.908710	-0.034900	3.527113
172.728808	4198.054181	6.913715	-0.034893	3.530323
172.916186	4206.115407	6.918720	-0.034933	3.533551
173.302485	4214.144014	6.923725	-0.035010	3.536768
173.796185	4222.108592	6.928730	-0.035107	3.539960
174.119563	4230.138866	6.933734	-0.035173	3.543171
174.217123	4238.191964	6.938739	-0.035196	3.546381
174.630363	4246.213853	6.943744	-0.035279	3.549584
174.903440	4254.322807	6.948749	-0.035335	3.552816
175.021163	4262.367476	6.953754	-0.035362	3.556014
175.339558	4270.324242	6.958758	-0.035426	3.559180
175.518655	4278.345056	6.963763	-0.035465	3.562365
175.478589	4286.328609	6.968768	-0.035463	3.565526
175.755422	4294.374809	6.973773	-0.035520	3.568718
176.012867	4302.395008	6.978778	-0.035573	3.571896
176.137161	4310.440937	6.983782	-0.035601	3.575077
176.377169	4318.435773	6.988787	-0.035651	3.578239
176.598227	4326.447891	6.993792	-0.035698	3.581405
176.693260	4334.455759	6.998797	-0.035721	3.584562
176.753107	4342.493922	7.003802	-0.035737	3.587727
177.285845	4350.513740	7.008806	-0.035842	3.590896
177.183905	4358.566814	7.013811	-0.035828	3.594057
177.191094	4366.593624	7.018816	-0.035834	3.597208
177.570252	4374.592822	7.023821	-0.035910	3.600356
178.010951	4382.576461	7.028826	-0.035998	3.603497
178.173679	4390.622216	7.033830	-0.036033	3.606651
178.260313	4398.649371	7.038835	-0.036055	3.609794
178.637442	4406.678130	7.043840	-0.036130	3.612942
178.741983	4414.761363	7.048845	-0.036155	3.616101
178.760538	4422.721689	7.053850	-0.036164	3.619207
178.978766	4430.767759	7.058854	-0.036209	3.622350
179.321852	4438.769649	7.063859	-0.036279	3.625475
179.459673	4446.783347	7.068864	-0.036310	3.628597
179.583313	4454.870079	7.073869	-0.036338	3.631745
179.771464	4462.901504	7.078874	-0.036378	3.634869
179.944193	4470.885473	7.083878	-0.036416	3.637973
180.101035	4478.932215	7.088883	-0.036450	3.641097
180.223969	4486.902835	7.093888	-0.036478	3.644189
180.426540	4494.979692	7.098893	-0.036521	3.647321
180.341619	4503.001766	7.103898	-0.036511	3.650421
180.709019	4511.048157	7.108902	-0.036584	3.653540
181.025506	4519.048447	7.113907	-0.036649	3.656638
181.220848	4527.038817	7.118912	-0.036690	3.659725
181.592873	4535.077517	7.123917	-0.036765	3.662833
181.488021	4543.105212	7.128922	-0.036750	3.665922
181.646310	4551.124316	7.133926	-0.036785	3.669012
181.928246	4559.190679	7.138931	-0.036843	3.672121
181.934059	4567.228874	7.143936	-0.036849	3.675209
182.306764	4575.189078	7.148941	-0.036924	3.678274
182.293106	4583.210371	7.153946	-0.036927	3.681349
182.563356	4591.202373	7.158950	-0.036982	3.684419
182.914752	4599.274102	7.163955	-0.037053	3.687518
183.071351	4607.274218	7.168960	-0.037087	3.690582
183.253148	4615.335784	7.173965	-0.037127	3.693668
183.541994	4623.348072	7.178970	-0.037186	3.696735
183.738786	4631.346989	7.183974	-0.037228	3.699792
183.659017	4639.382975	7.188979	-0.037218	3.702854
183.995267	4647.373064	7.193984	-0.037286	3.705906
184.179016	4655.415908	7.198989	-0.037325	3.708972
184.292733	4663.508629	7.203994	-0.037352	3.712052
184.415657	4671.582878	7.208998	-0.037380	3.715123
184.634429	4679.529370	7.214003	-0.037426	3.718146
184.802044	4687.544992	7.219008	-0.037462	3.721191
185.082486	4695.503186	7.224013	-0.037520	3.724214
185.321339	4703.520935	7.229018	-0.037570	3.727256
185.597738	4711.541309	7.234022	-0.037626	3.730298
185.918602	4719.601058	7.239027	-0.037691	3.733353
186.036556	4727.650622	7.244032	-0.037719	3.736397
186.364541	4735.610839	7.249037	-0.037785	3.739410
186.383165	4743.656677	7.254042	-0.037794	3.742445
186.448734	4751.665515	7.259046	-0.037811	3.745465
186.739085	4759.704144	7.264051	-0.037871	3.748499
187.022170	4767.753194	7.269056	-0.037929	3.751534
187.217115	4775.789440	7.274061	-0.037970	3.754560
187.458703	4783.781986	7.279066	-0.038020	3.757568
187.629746	4791.809528	7.284070	-0.038057	3.760585
187.848710	4799.817338	7.289075	-0.038104	3.763594
188.087763	4807.830427	7.294080	-0.038153	3.766602
188.287462	4815.885802	7.299085	-0.038196	3.769623
188.312181	4823.911636	7.304090	-0.038206	3.772626
188.772555	4831.929149	7.309094	-0.038297	3.775634
189.030005	4839.970553	7.314099	-0.038350	3.778644
188.988601	4847.992152	7.319104	-0.038347	3.781637
189.314202	4856.004744	7.324109	-0.038413	3.784632
189.347555	4864.026249	7.329114	-0.038425	3.787622
189.680312	4872.030371	7.334118	-0.038492	3.790610
189.913981	4880.125765	7.339123	-0.038541	3.793627
190.040929	4888.102143	7.344128	-0.038570	3.796595
190.183384	4896.120061	7.349133	-0.038602	3.799577
190.331924	4904.095184	7.354138	-0.038634	3.802540
190.383821	4912.121854	7.359142	-0.038649	3.805518
190.561998	4920.132280	7.364147	-0.038688	3.808491
190.687808	4928.179094	7.369152	-0.038716	3.811473
190.882668	4936.232479	7.374157	-0.038758	3.814457
191.098671	4944.240351	7.379162	-0.038804	3.817422
191.484656	4952.212609	7.384166	-0.038881	3.820376
191.460418	4960.258816	7.389171	-0.038881	3.823345
191.516214	4968.256727	7.394176	-0.038897	3.826297
191.603690	4976.316657	7.399181	-0.038919	3.829269
191.768981	4984.325881	7.404186	-0.038955	3.832222
192.022492	4992.373698	7.409190	-0.039007	3.835189
192.415004	5000.337609	7.414195	-0.039086	3.838125
192.624683	5008.359756	7.419200	-0.039130	3.841077
192.872715	5016.367302	7.424205	-0.039181	3.844022
193.083677	5024.393396	7.429210	-0.039226	3.846971
193.274678	5032.433676	7.434214	-0.039267	3.849922
193.363249	5040.457773	7.439219	-0.039288	3.852863
193.417476	5048.552242	7.444224	-0.039304	3.855827
193.725283	5056.528805	7.449229	-0.039366	3.858750
193.827839	5064.520285	7.454234	-0.039391	3.861673
193.886099	5072.544248	7.459238	-0.039407	3.864604
194.117698	5080.594822	7.464243	-0.039455	3.867546
194.308549	5088.614449	7.469248	-0.039496	3.870474
194.665554	5096.898690	7.474253	-0.039568	3.873499
194.819517	5104.840216	7.479258	-0.039602	3.876393
194.984020	5112.700467	7.484262	-0.039638	3.879256
195.164940	5120.780520	7.489267	-0.039677	3.882197
195.181180	5128.702757	7.494272	-0.039685	3.885074
195.488157	5136.747911	7.499277	-0.039747	3.888000
195.694428	5144.785665	7.504282	-0.039791	3.890919
195.844278	5152.828225	7.509286	-0.039824	3.893837
196.255053	5160.843306	7.514291	-0.039906	3.896747
196.367210	5168.801694	7.519296	-0.039932	3.899629
196.452424	5176.867627	7.524301	-0.039953	3.902547
196.674583	5184.823594	7.529306	-0.040000	3.905426
196.895226	5192.853083	7.534310	-0.040046	3.908329
197.143964	5200.909700	7.539315	-0.040098	3.911241
197.122578	5208.934369	7.544320	-0.040099	3.914133
197.394441	5216.955992	7.549325	-0.040155	3.917028
197.514976	5224.930675	7.554330	-0.040183	3.919901
197.833691	5232.953269	7.559334	-0.040247	3.922792
197.825542	5240.987214	7.564339	-0.040251	3.925680
197.998608	5248.979659	7.569344	-0.040289	3.928554
198.128512	5257.039383	7.574349	-0.040318	3.931449
198.146119	5265.057622	7.579354	-0.040327	3.934325
198.633876	5273.080913	7.584358	-0.040423	3.937209
198.945305	5281.078088	7.589363	-0.040486	3.940078
199.232282	5289.066734	7.594368	-0.040545	3.942942
199.400779	5297.110838	7.599373	-0.040581	3.945821
199.574859	5305.109053	7.604378	-0.040619	3.948682
199.665928	5313.209059	7.609382	-0.040641	3.951576
199.833372	5321.239545	7.614387	-0.040678	3.954444
200.021193	5329.226772	7.619392	-0.040718	3.957295
200.275549	5337.220132	7.624397	-0.040770	3.960148
200.105741	5345.224903	7.629402	-0.040744	3.962995
200.668265	5353.211618	7.634406	-0.040854	3.965846
200.677483	5361.238690	7.639411	-0.040861	3.968700
201.008465	5369.293151	7.644416	-0.040928	3.971566
201.259673	5377.344168	7.649421	-0.040980	3.974429
201.709605	5385.328326	7.654426	-0.041069	3.977268
201.697081	5393.343664	7.659430	-0.041072	3.980110
201.858532	5401.375979	7.664435	-0.041107	3.982957
202.155890	5409.392779	7.669440	-0.041168	3.985800
202.280828	5417.460529	7.674445	-0.041197	3.988656
202.067096	5425.484401	7.679450	-0.041162	3.991488
202.446646	5433.498941	7.684454	-0.041238	3.994325
202.762367	5441.549705	7.689459	-0.041302	3.997172
202.854272	5449.497030	7.694464	-0.041324	3.999976
202.908486	5457.546506	7.699469	-0.041340	4.002814
203.057939	5465.545094	7.704474	-0.041373	4.005634
203.350998	5473.562436	7.709478	-0.041433	4.008460
203.210892	5481.617445	7.714483	-0.041412	4.011291
203.530050	5489.640679	7.719488	-0.041477	4.014116
203.710488	5497.690109	7.724493	-0.041515	4.016945
203.853378	5505.655303	7.729498	-0.041547	4.019743
204.153239	5513.675291	7.734502	-0.041608	4.022560
204.224902	5521.702145	7.739507	-0.041627	4.025374
204.214151	5529.715964	7.744512	-0.041630	4.028181
204.411263	5537.765591	7.749517	-0.041672	4.031001
204.539042	5545.871281	7.754522	-0.041701	4.033838
205.033847	5553.875751	7.759526	-0.041799	4.036642
205.139307	5561.793621	7.764531	-0.041824	4.039409
205.125152	5569.825892	7.769536	-0.041826	4.042212
205.537098	5577.790979	7.774541	-0.041908	4.044996
205.536898	5585.832961	7.779546	-0.041913	4.047799
205.687854	5593.843660	7.784550	-0.041947	4.050591
205.963815	5601.918425	7.789555	-0.042004	4.053405
206.208263	5609.909541	7.794560	-0.042054	4.056187
206.525221	5617.921211	7.799565	-0.042119	4.058976
206.667874	5625.953839	7.804570	-0.042150	4.061768
206.992632	5633.911668	7.809574	-0.042216	4.064534
207.147303	5641.983792	7.814579	-0.042250	4.067336
207.510786	5649.943995	7.819584	-0.042323	4.070100
207.672924	5658.023451	7.824589	-0.042359	4.072900
207.696201	5666.060914	7.829594	-0.042368	4.075682
207.760771	5674.037208	7.834598	-0.042386	4.078442
208.154454	5682.055465	7.839603	-0.042464	4.081219
208.294277	5690.039732	7.844608	-0.042495	4.083978
208.555742	5698.094318	7.849613	-0.042549	4.086762
208.715480	5706.069787	7.854618	-0.042584	4.089515
208.867464	5714.146148	7.859622	-0.042618	4.092301
208.920142	5722.166677	7.864627	-0.042633	4.095064
208.994799	5730.150062	7.869632	-0.042652	4.097813
209.594660	5738.199348	7.874637	-0.042769	4.100589
209.547660	5746.206544	7.879642	-0.042766	4.103341
209.607752	5754.242280	7.884646	-0.042782	4.106102
209.859283	5762.264340	7.889651	-0.042834	4.108859
210.169972	5770.296942	7.894656	-0.042897	4.111619
210.208573	5778.349887	7.899661	-0.042910	4.114380
210.527903	5786.384065	7.904666	-0.042975	4.117136
210.733699	5794.340425	7.909670	-0.043018	4.119863
211.001630	5802.373785	7.914675	-0.043073	4.122615
211.124821	5810.360422	7.919680	-0.043101	4.125347
211.342022	5818.419347	7.924685	-0.043147	4.128103
211.441160	5826.436842	7.929690	-0.043171	4.130841
211.544311	5834.460476	7.934694	-0.043195	4.133580
212.154098	5842.510564	7.939699	-0.043314	4.136333
212.198176	5850.458284	7.944704	-0.043328	4.139041
212.396034	5858.571745	7.949709	-0.043370	4.141806
212.413340	5866.481459	7.954714	-0.043378	4.144498
212.670143	5874.550415	7.959718	-0.043431	4.147245
212.844952	5882.579929	7.964723	-0.043469	4.149976
212.686312	5890.623710	7.969728	-0.043445	4.152706
213.108428	5898.684744	7.974733	-0.043529	4.155447
213.148034	5906.630067	7.979738	-0.043541	4.158142
213.472213	5914.678591	7.984742	-0.043607	4.160874
213.587636	5922.639180	7.989747	-0.043634	4.163572
213.718098	5930.636768	7.994752	-0.043663	4.166280
213.952218	5938.704437	7.999757	-0.043712	4.169012
214.057681	5946.726394	8.004762	-0.043737	4.171725
214.222084	5954.720225	8.009766	-0.043773	4.174427
214.596284	5962.773397	8.014771	-0.043848	4.177150
214.806651	5970.718909	8.019776	-0.043892	4.179833
215.105677	5978.752853	8.024781	-0.043953	4.182545
215.133887	5986.773170	8.029786	-0.043964	4.185248
215.266553	5994.814780	8.034790	-0.043994	4.187957
215.472515	6002.828671	8.039795	-0.044037	4.190656
215.728119	6010.948384	8.044800	-0.044090	4.193390
215.817978	6018.967272	8.049805	-0.044112	4.196086
215.948691	6026.900799	8.054810	-0.044142	4.198751
216.251247	6034.891713	8.059814	-0.044204	4.201437
216.549278	6042.843320	8.064819	-0.044264	4.204107
216.692896	6050.922300	8.069824	-0.044296	4.206817
216.781825	6058.900098	8.074829	-0.044318	4.209490
217.170013	6066.954059	8.079834	-0.044396	4.212190
217.158287	6074.984471	8.084838	-0.044399	4.214877
217.286421	6083.026049	8.089843	-0.044428	4.217567
217.588374	6090.987207	8.094848	-0.044489	4.220230
217.882931	6099.033245	8.099853	-0.044549	4.222919
217.882406	6107.007202	8.104858	-0.044555	4.225580
218.231172	6115.044250	8.109862	-0.044625	4.228264
218.269936	6123.088144	8.114867	-0.044637	4.230945
218.331804	6131.095233	8.119872	-0.044654	4.233612
218.826940	6139.139911	8.124877	-0.044752	4.236295
218.917234	6147.102008	8.129882	-0.044774	4.238944
219.030697	6155.128593	8.134886	-0.044800	4.241613
219.297562	6163.137141	8.139891	-0.044855	4.244277
219.610307	6171.128849	8.144896	-0.044919	4.246933
219.706443	6179.218344	8.149901	-0.044942	4.249618
219.590803	6187.229403	8.154906	-0.044925	4.252273
219.977947	6195.252308	8.159910	-0.045003	4.254935
220.135170	6203.298954	8.164915	-0.045037	4.257601
220.171601	6211.290773	8.169920	-0.045049	4.260247
220.514818	6219.311411	8.174925	-0.045119	4.262902
220.791622	6227.309687	8.179930	-0.045175	4.265549
220.855000	6235.312105	8.184934	-0.045192	4.268193
221.086179	6243.419150	8.189939	-0.045241	4.270871
221.093666	6251.417027	8.194944	-0.045247	4.273510
221.377922	6259.494121	8.199949	-0.045306	4.276175
221.356819	6267.411762	8.204954	-0.045307	4.278784
221.710637	6275.472576	8.209958	-0.045378	4.281441
221.867240	6283.426841	8.214963	-0.045413	4.284061
221.894328	6291.475717	8.219968	-0.045423	4.286708
222.176694	6299.471893	8.224973	-0.045481	4.289339
222.482242	6307.536221	8.229978	-0.045543	4.291990
222.497156	6315.545285	8.234982	-0.045551	4.294619
222.495205	6323.619652	8.239987	-0.045556	4.297268
223.066984	6331.570801	8.244992	-0.045668	4.299880
223.136618	6339.604860	8.249997	-0.045686	4.302513
223.172617	6347.562664	8.255002	-0.045698	4.305119
223.723283	6355.610468	8.260006	-0.045806	4.307757
224.135653	6363.634217	8.265011	-0.045888	4.310385
223.993180	6371.684544	8.270016	-0.045866	4.313015
224.140861	6379.717745	8.275021	-0.045899	4.315641
224.466828	6387.674342	8.280026	-0.045965	4.318241
224.697279	6395.697385	8.285030	-0.046013	4.320860
224.772785	6403.707810	8.290035	-0.046033	4.323472
224.822974	6411.728474	8.295040	-0.046047	4.326086
225.092214	6419.747258	8.300045	-0.046103	4.328700
225.172668	6427.751152	8.305050	-0.046123	4.331305
225.273949	6435.815139	8.310054	-0.046147	4.333929
225.571695	6443.848132	8.315059	-0.046208	4.336543
225.800599	6451.774137	8.320064	-0.046256	4.339119
226.009848	6459.866957	8.325069	-0.046300	4.341748
226.259649	6467.795500	8.330074	-0.046352	4.344323
226.467461	6475.834692	8.335078	-0.046396	4.346931
226.744473	6483.915926	8.340083	-0.046452	4.349552
226.688200	6491.919266	8.345088	-0.046447	4.352144
227.285759	6499.997157	8.350093	-0.046564	4.354763
227.242596	6507.975171	8.355098	-0.046561	4.357343
227.372051	6515.961256	8.360102	-0.046590	4.359926
227.885196	6524.002619	8.365107	-0.046691	4.362528
227.901071	6531.924203	8.370112	-0.046699	4.365086
227.879025	6539.961487	8.375117	-0.046700	4.367680
228.145445	6548.000008	8.380122	-0.046755	4.370274
228.375156	6556.002452	8.385126	-0.046803	4.372855
228.688669	6564.074084	8.390131	-0.046867	4.375457
228.733404	6572.036292	8.395136	-0.046881	4.378021
229.044019	6580.082791	8.400141	-0.046944	4.380612
228.761704	6588.064260	8.405146	-0.046896	4.383177
229.094438	6596.085983	8.410150	-0.046964	4.385757
229.536298	6604.112593	8.415155	-0.047051	4.388338
229.649176	6612.126496	8.420160	-0.047077	4.390911
229.699746	6620.210473	8.425165	-0.047092	4.393505
229.862015	6628.230145	8.430170	-0.047128	4.396077
230.117441	6636.220858	8.435174	-0.047181	4.398639
230.304259	6644.247710	8.440179	-0.047221	4.401210
230.210394	6652.167845	8.445184	-0.047208	4.403745
230.572546	6660.257903	8.450189	-0.047281	4.406334
230.803837	6668.250450	8.455194	-0.047329	4.408891
230.991866	6676.312933	8.460198	-0.047370	4.411468
230.990604	6684.325476	8.465203	-0.047375	4.414026
231.005658	6692.399180	8.470208	-0.047383	4.416603
231.178216	6700.345957	8.475213	-0.047420	4.419138
231.353201	6708.377675	8.480218	-0.047458	4.421699
231.664706	6716.349354	8.485222	-0.047521	4.424240
231.740594	6724.430240	8.490227	-0.047541	4.426813
231.758611	6732.391080	8.495232	-0.047549	4.429346
232.119614	6740.494959	8.500237	-0.047622	4.431925
232.358356	6748.507176	8.505242	-0.047672	4.434473
232.314788	6756.518200	8.510246	-0.047669	4.437017
232.816291	6764.502725	8.515251	-0.047767	4.439554
232.764150	6772.523135	8.520256	-0.047763	4.442098
232.946318	6780.471142	8.525261	-0.047802	4.444620
233.219483	6788.521089	8.530266	-0.047858	4.447172
233.550993	6796.548399	8.535270	-0.047925	4.449716
233.785437	6804.613250	8.540275	-0.047974	4.452269
233.913463	6812.603223	8.545280	-0.048003	4.454798
234.209711	6820.577935	8.550285	-0.048064	4.457320
234.211604	6828.594471	8.555290	-0.048069	4.459853
234.087885	6836.616088	8.560295	-0.048051	4.462386
234.371260	6844.653259	8.565299	-0.048110	4.464924
234.490088	6852.666338	8.570304	-0.048137	4.467452
234.756722	6860.696197	8.575309	-0.048192	4.469985
234.931013	6868.746623	8.580314	-0.048230	4.472522
235.326711	6876.735796	8.585319	-0.048308	4.475039
235.616546	6884.783364	8.590323	-0.048368	4.477573
235.425031	6892.728530	8.595328	-0.048337	4.480072
235.575432	6900.785760	8.600333	-0.048371	4.482605
235.690105	6908.743619	8.605338	-0.048397	4.485106
235.906149	6916.773575	8.610343	-0.048443	4.487628
236.204863	6924.814295	8.615347	-0.048504	4.490153
236.477417	6932.866888	8.620352	-0.048560	4.492679
236.703619	6940.868780	8.625357	-0.048607	4.495188
236.607390	6948.888187	8.630362	-0.048594	4.497701
236.905816	6956.861605	8.635367	-0.048655	4.500198
237.011531	6964.901155	8.640371	-0.048680	4.502715
237.201197	6972.877630	8.645376	-0.048721	4.505210
237.446126	6980.911089	8.650381	-0.048772	4.507722
237.604562	6988.947849	8.655386	-0.048806	4.510233
237.812375	6997.016763	8.660391	-0.048850	4.512753
237.991049	7005.042475	8.665395	-0.048889	4.515259
238.169688	7012.995628	8.670400	-0.048927	4.517740
238.179721	7020.984546	8.675405	-0.048934	4.520230
238.536415	7028.957311	8.680410	-0.049006	4.522715
238.710174	7036.980034	8.685415	-0.049044	4.525213
239.103279	7045.028834	8.690419	-0.049122	4.527719
238.922420	7053.035903	8.695424	-0.049094	4.530209
239.202744	7061.061388	8.700429	-0.049151	4.532705
239.232354	7069.085963	8.705434	-0.049162	4.535198
239.405442	7077.075878	8.710439	-0.049200	4.537679
239.575770	7085.135664	8.715443	-0.049237	4.540181
239.961512	7093.095035	8.720448	-0.049314	4.542650
239.841364	7101.129190	8.725453	-0.049297	4.545141
239.988994	7109.162250	8.730458	-0.049329	4.547630
240.110480	7117.149488	8.735463	-0.049357	4.550104
240.471576	7125.226717	8.740467	-0.049430	4.552604
240.295651	7133.231335	8.745472	-0.049402	4.555080
240.657868	7141.280215	8.750477	-0.049475	4.557569
240.743930	7149.223677	8.755482	-0.049496	4.560023
240.992607	7157.241567	8.760487	-0.049548	4.562499
241.436717	7165.238857	8.765491	-0.049636	4.564968
241.350247	7173.277087	8.770496	-0.049625	4.567448
241.681724	7181.283719	8.775501	-0.049692	4.569917
241.618039	7189.376223	8.780506	-0.049685	4.572410
241.874406	7197.330143	8.785511	-0.049738	4.574860
242.287475	7205.386374	8.790515	-0.049821	4.577340
242.223696	7213.340883	8.795520	-0.049814	4.579787
242.558768	7221.473280	8.800525	-0.049882	4.582288
242.974837	7229.390558	8.805530	-0.049964	4.584721
243.065725	7237.429864	8.810535	-0.049986	4.587190
243.151448	7245.470504	8.815539	-0.050008	4.589659
243.357226	7253.514275	8.820544	-0.050051	4.592127
243.471210	7261.526968	8.825549	-0.050078	4.594584
243.592487	7269.566408	8.830554	-0.050106	4.597048
243.697620	7277.465465	8.835559	-0.050130	4.599467
243.857384	7285.564524	8.840563	-0.050166	4.601947
243.781172	7293.493699	8.845568	-0.050157	4.604373
244.111720	7301.586064	8.850573	-0.050223	4.606848
244.259925	7309.559375	8.855578	-0.050256	4.609285
244.340323	7317.564592	8.860583	-0.050276	4.611730
244.734770	7325.664078	8.865587	-0.050355	4.614203
244.849762	7333.672867	8.870592	-0.050382	4.616647
244.788443	7341.628560	8.875597	-0.050376	4.619073
244.924011	7349.664327	8.880602	-0.050406	4.621523
244.873447	7357.623314	8.885607	-0.050402	4.623948
245.227257	7365.708866	8.890611	-0.050473	4.626410
245.104690	7373.678302	8.895616	-0.050456	4.628835
245.173190	7381.774291	8.900621	-0.050474	4.631298
245.445906	7389.757826	8.905626	-0.050530	4.633725
245.699264	7397.808320	8.910631	-0.050582	4.636171
245.921004	7405.737664	8.915635	-0.050629	4.638579
245.812546	7413.770337	8.920640	-0.050614	4.641017
246.049294	7421.783272	8.925645	-0.050663	4.643448
246.092295	7429.791793	8.930650	-0.050676	4.645876
246.407826	7437.773305	8.935655	-0.050740	4.648295
246.704390	7445.874520	8.940659	-0.050801	4.650749
246.802943	7453.872258	8.945664	-0.050825	4.653170
246.842748	7461.902915	8.950669	-0.050837	4.655599
247.083570	7469.897174	8.955674	-0.050887	4.658017
247.032052	7477.866734	8.960679	-0.050883	4.660426
246.979722	7485.926200	8.965683	-0.050879	4.662861
247.194701	7493.893718	8.970688	-0.050924	4.665266
247.314647	7501.946787	8.975693	-0.050951	4.667696
247.490213	7509.984681	8.980698	-0.050989	4.670121
247.467712	7518.024882	8.985703	-0.050990	4.672544
247.896193	7526.138782	8.990707	-0.051076	4.674989
248.032671	7534.042037	8.995712	-0.051106	4.677369
248.133552	7541.973055	9.000717	-0.051130	4.679756
248.336206	7550.048847	9.005722	-0.051173	4.682185
248.442343	7557.982985	9.010727	-0.051198	4.684570
248.591972	7566.140715	9.015731	-0.051231	4.687022
248.855660	7574.016520	9.020736	-0.051286	4.689387
249.021433	7582.083038	9.025741	-0.051322	4.691808
249.074902	7590.102089	9.030746	-0.051337	4.694215
249.108150	7598.157430	9.035751	-0.051349	4.696630
249.527928	7606.108068	9.040755	-0.051432	4.699013
249.625989	7614.119054	9.045760	-0.051455	4.701413
249.489841	7622.151282	9.050765	-0.051435	4.703818
249.731184	7630.161123	9.055770	-0.051486	4.706215
249.972979	7638.146966	9.060775	-0.051536	4.708603
250.052203	7646.195246	9.065779	-0.051556	4.711009
250.224853	7654.257823	9.070784	-0.051593	4.713418
250.415222	7662.243190	9.075789	-0.051634	4.715803
250.757717	7670.290430	9.080794	-0.051703	4.718204
250.848623	7678.242439	9.085799	-0.051725	4.720577
251.124030	7686.295383	9.090803	-0.051782	4.722978
251.305857	7694.303514	9.095808	-0.051821	4.725364
251.201262	7702.340429	9.100813	-0.051807	4.727759
251.368982	7710.322031	9.105818	-0.051843	4.730135
251.610215	7718.393407	9.110823	-0.051893	4.732536
251.652069	7726.437664	9.115827	-0.051907	4.734929
251.607815	7734.420044	9.120832	-0.051904	4.737302
251.947693	7742.429190	9.125837	-0.051972	4.739681
252.115660	7750.430226	9.130842	-0.052009	4.742057
252.024197	7758.405289	9.135847	-0.051997	4.744425
252.227123	7766.485318	9.140851	-0.052040	4.746822
252.448425	7774.472838	9.145856	-0.052086	4.749190
252.511562	7782.521693	9.150861	-0.052103	4.751575
252.745969	7790.559681	9.155866	-0.052152	4.753956
252.749271	7798.578068	9.160871	-0.052158	4.756330
252.989355	7806.528301	9.165875	-0.052208	4.758682
253.038781	7814.557384	9.170880	-0.052223	4.761057
253.331117	7822.526873	9.175885	-0.052282	4.763412
253.707011	7830.575416	9.180890	-0.052358	4.765789
253.579961	7838.560582	9.185895	-0.052339	4.768148
253.734361	7846.590223	9.190899	-0.052373	4.770518
253.885361	7854.625998	9.195904	-0.052407	4.772889
253.941001	7862.608478	9.200909	-0.052422	4.775243
253.908174	7870.672156	9.205914	-0.052421	4.777620
254.267284	7878.658166	9.210919	-0.052494	4.779971
254.417179	7886.702684	9.215923	-0.052527	4.782340
254.485352	7894.659950	9.220928	-0.052545	4.784681
254.766713	7902.718591	9.225933	-0.052602	4.787051
254.951181	7910.720499	9.230938	-0.052642	4.789403
254.831103	7918.749682	9.235943	-0.052625	4.791763
255.288959	7926.801809	9.240947	-0.052715	4.794127
255.298763	7934.744075	9.245952	-0.052722	4.796459
255.495121	7942.769616	9.250957	-0.052764	4.798813
255.561655	7950.783380	9.255962	-0.052782	4.801163
255.903536	7958.796795	9.260967	-0.052851	4.803511
256.028727	7966.803451	9.265971	-0.052879	4.805856
256.094976	7974.831276	9.270976	-0.052897	4.808207
256.339571	7982.862696	9.275981	-0.052948	4.810557
256.580956	7990.351648	9.280986	-0.052998	4.812747
256.706317	7994.889089	9.285991	-0.053024	4.814074

256.583478	7997.412065	9.290995	-0.053003	4.814812
256.819454	7998.751678	9.296000	-0.053048	4.815203
256.949875	7999.186275	9.301005	-0.053072	4.815329
256.858795	8000.097824	9.306010	-0.053056	4.815596
256.861979	8000.073318	9.311015	-0.053057	4.815589
257.127225	8000.116092	9.316019	-0.053106	4.815600
257.097132	8000.108129	9.321024	-0.053101	4.815598
257.069628	8000.093802	9.326029	-0.053095	4.815594
257.244105	8000.081700	9.331034	-0.053128	4.815590
257.281936	8000.053487	9.336039	-0.053135	4.815581
257.391832	8000.147123	9.341043	-0.053156	4.815608
257.415584	8000.121885	9.346048	-0.053160	4.815601
257.586327	8000.113994	9.351053	-0.053192	4.815597
257.432869	8000.157415	9.356058	-0.053163	4.815611
257.623659	8000.117814	9.361063	-0.053199	4.815598
257.766352	8000.122281	9.366067	-0.053226	4.815599
257.737475	8000.088708	9.371072	-0.053220	4.815589
257.945006	8000.101709	9.376077	-0.053259	4.815592
258.042794	8000.106511	9.381082	-0.053277	4.815593
257.985557	8000.114125	9.386087	-0.053267	4.815596
257.990238	8000.223134	9.391091	-0.053267	4.815627
258.024809	8000.138267	9.396096	-0.053274	4.815602
258.202116	8000.178541	9.401101	-0.053307	4.815613
258.061760	8000.168779	9.406106	-0.053281	4.815611
258.053885	8000.130209	9.411111	-0.053279	4.815600
257.922623	8000.186808	9.416115	-0.053255	4.815617
257.926515	8000.154837	9.421120	-0.053256	4.815608
258.128779	8000.152801	9.426125	-0.053294	4.815606
258.215079	8000.176639	9.431130	-0.053310	4.815613
258.351563	8000.113726	9.436135	-0.053335	4.815594
258.319041	8000.163392	9.441139	-0.053329	4.815608
258.380801	8000.124890	9.446144	-0.053341	4.815597
258.381328	8000.155872	9.451149	-0.053341	4.815606
258.132345	8000.133659	9.456154	-0.053294	4.815601
258.338966	8000.166936	9.461159	-0.053333	4.815609
258.304621	8000.183466	9.466163	-0.053327	4.815614
258.293760	8000.144847	9.471168	-0.053325	4.815603
258.442916	8000.136605	9.476173	-0.053352	4.815600
258.471560	8000.165911	9.481178	-0.053358	4.815608
258.313891	8000.132371	9.486183	-0.053329	4.815599
258.457423	8000.166755	9.491187	-0.053355	4.815609
258.596632	8000.186118	9.496192	-0.053381	4.815614
258.667950	8000.193693	9.501197	-0.053395	4.815616
258.593696	8000.197825	9.506202	-0.053381	4.815617
258.467722	8000.143444	9.511207	-0.053357	4.815602
258.667495	8000.187289	9.516211	-0.053395	4.815614
258.654564	8000.163587	9.521216	-0.053392	4.815607
258.720853	8000.200983	9.526221	-0.053405	4.815617
258.790304	8000.255518	9.531226	-0.053418	4.815633
258.725390	8000.203200	9.536231	-0.053406	4.815618
258.755976	8000.231470	9.541235	-0.053411	4.815626
258.646880	8000.175228	9.546240	-0.053391	4.815610
258.738247	8000.173519	9.551245	-0.053408	4.815609
258.680538	8000.211027	9.556250	-0.053397	4.815621
258.681185	8000.192886	9.561255	-0.053398	4.815615
258.864203	8000.233255	9.566259	-0.053432	4.815626
258.824199	8000.212315	9.571264	-0.053424	4.815620
258.755095	8000.159929	9.576269	-0.053411	4.815605
259.101918	8000.278797	9.581274	-0.053476	4.815638
259.042802	8000.209486	9.586279	-0.053465	4.815618
258.887484	8000.245402	9.591283	-0.053436	4.815630
258.834404	8000.217840	9.596288	-0.053426	4.815622
259.021587	8000.190996	9.601293	-0.053461	4.815613
259.195672	8000.223744	9.606298	-0.053494	4.815622
258.845962	8000.199885	9.611303	-0.053429	4.815616
259.180001	8000.266215	9.616307	-0.053491	4.815634
259.123770	8000.233262	9.621312	-0.053481	4.815625
258.978609	8000.204197	9.626317	-0.053454	4.815617
259.082685	8000.231530	9.631322	-0.053473	4.815625
258.931457	8000.191687	9.636327	-0.053445	4.815614
259.039507	8000.243649	9.641331	-0.053465	4.815628
259.132954	8000.201391	9.646336	-0.053482	4.815616
259.068019	8000.252665	9.651341	-0.053470	4.815631
259.001583	8000.253720	9.656346	-0.053458	4.815631
259.129149	8000.178913	9.661351	-0.053482	4.815609
259.334165	8000.244206	9.666355	-0.053520	4.815627
259.156392	8000.221016	9.671360	-0.053487	4.815621
259.159280	8000.213591	9.676365	-0.053488	4.815619
259.317007	8000.241801	9.681370	-0.053517	4.815626
259.366364	8000.146493	9.686375	-0.053526	4.815598
259.405528	8000.238982	9.691379	-0.053534	4.815625
259.139902	8000.226105	9.696384	-0.053484	4.815623
259.264389	8000.230277	9.701389	-0.053507	4.815623
259.395986	8000.291168	9.706394	-0.053532	4.815641
259.228314	8000.263871	9.711399	-0.053501	4.815633
259.522646	8000.230233	9.716403	-0.053556	4.815622
259.445548	8000.208686	9.721408	-0.053541	4.815616
259.355471	8000.182656	9.726413	-0.053525	4.815609
259.368621	8000.244817	9.731418	-0.053527	4.815627
259.468711	8000.190920	9.736423	-0.053546	4.815611
259.319407	8000.267516	9.741427	-0.053518	4.815634
259.141462	8000.263547	9.746432	-0.053485	4.815634
259.313582	8000.251409	9.751437	-0.053517	4.815629
259.346668	8000.306420	9.756442	-0.053523	4.815645
259.111939	8000.178707	9.761447	-0.053479	4.815609
259.207688	8000.212313	9.766451	-0.053497	4.815618
259.143483	8000.234763	9.771456	-0.053485	4.815625
259.146506	8000.211321	9.776461	-0.053486	4.815618
259.442638	8000.284510	9.781466	-0.053541	4.815638
259.390475	8000.234535	9.786471	-0.053532	4.815624
259.195824	8000.235633	9.791475	-0.053495	4.815625
259.201430	8000.207961	9.796480	-0.053496	4.815617
259.256595	8000.212069	9.801485	-0.053507	4.815618
259.305104	8000.261991	9.806490	-0.053516	4.815632
259.213223	8000.190009	9.811495	-0.053499	4.815612
259.264778	8000.215418	9.816499	-0.053508	4.815619
259.454502	8000.188616	9.821504	-0.053544	4.815610
259.306152	8000.164838	9.826509	-0.053516	4.815604
259.155224	8000.181602	9.831514	-0.053488	4.815610
259.451689	8000.182173	9.836519	-0.053543	4.815608
259.491481	8000.297100	9.841523	-0.053551	4.815642
259.301733	8000.229927	9.846528	-0.053516	4.815623
259.498515	8000.214988	9.851533	-0.053552	4.815618
259.390718	8000.311485	9.856538	-0.053532	4.815646
259.319312	8000.265468	9.861543	-0.053519	4.815633
259.375230	8000.271725	9.866547	-0.053529	4.815635
259.515461	8000.276154	9.871552	-0.053556	4.815636
259.401115	8000.282835	9.876557	-0.053534	4.815638
259.269363	8000.284959	9.881562	-0.053510	4.815639
259.363240	8000.239505	9.886567	-0.053527	4.815626
259.505948	8000.292034	9.891571	-0.053554	4.815640
259.383795	8000.261208	9.896576	-0.053531	4.815632
259.347493	8000.312949	9.901581	-0.053525	4.815647
259.569630	8000.299492	9.906586	-0.053566	4.815642
259.397995	8000.214460	9.911591	-0.053534	4.815618
259.488029	8000.271468	9.916595	-0.053551	4.815634
259.594934	8000.328752	9.921600	-0.053571	4.815651
259.625426	8000.286535	9.926605	-0.053577	4.815638
259.446295	8000.262254	9.931610	-0.053543	4.815632
259.438495	8000.217276	9.936615	-0.053542	4.815619
259.739455	8000.251029	9.941619	-0.053598	4.815627
259.738215	8000.270236	9.946624	-0.053598	4.815633
259.371956	8000.273871	9.951629	-0.053530	4.815636
259.678377	8000.341889	9.956634	-0.053587	4.815654
259.584411	8000.259192	9.961639	-0.053569	4.815630
259.685527	8000.331333	9.966643	-0.053588	4.815651
259.638162	8000.317748	9.971648	-0.053579	4.815647
259.493726	8000.298305	9.976653	-0.053552	4.815642
259.510496	8000.329554	9.981658	-0.053556	4.815651
259.511258	8000.240928	9.986663	-0.053556	4.815625
259.661361	8000.276490	9.991667	-0.053584	4.815635
259.643819	8000.230285	9.996672	-0.053581	4.815621
259.533852	8000.221017	10.001677	-0.053560	4.815619
259.707626	8000.252693	10.006682	-0.053593	4.815628
259.621625	8000.259837	10.011687	-0.053577	4.815630
259.685757	8000.224576	10.016691	-0.053589	4.815620
259.618663	8000.234164	10.021696	-0.053576	4.815623
259.751416	8000.264103	10.026701	-0.053601	4.815631
259.861120	8000.255219	10.031706	-0.053621	4.815628
259.717036	8000.187723	10.036711	-0.053594	4.815609
259.958485	8000.263224	10.041715	-0.053640	4.815630
259.667067	8000.284101	10.046720	-0.053585	4.815637
259.782115	8000.275303	10.051725	-0.053607	4.815634
259.896680	8000.336985	10.056730	-0.053628	4.815651
259.674728	8000.263945	10.061735	-0.053587	4.815631
259.828309	8000.354032	10.066739	-0.053616	4.815657
259.866417	8000.306598	10.071744	-0.053623	4.815643
259.845911	8000.246460	10.076749	-0.053619	4.815625
259.639535	8000.251638	10.081754	-0.053580	4.815628
259.787341	8000.240171	10.086759	-0.053608	4.815624
259.751417	8000.303667	10.091763	-0.053601	4.815642
259.828117	8000.308128	10.096768	-0.053616	4.815643
259.830043	8000.306027	10.101773	-0.053616	4.815643
259.871860	8000.344093	10.106778	-0.053624	4.815654
259.778598	8000.307330	10.111783	-0.053607	4.815643
259.721750	8000.271162	10.116787	-0.053596	4.815633
259.719975	8000.248709	10.121792	-0.053596	4.815626
259.862699	8000.267063	10.126797	-0.053622	4.815631
259.751406	8000.336805	10.131802	-0.053602	4.815652
259.609886	8000.233039	10.136807	-0.053575	4.815622
259.865293	8000.264981	10.141811	-0.053623	4.815631
259.978916	8000.296744	10.146816	-0.053644	4.815639
259.856141	8000.218916	10.151821	-0.053621	4.815617
259.833896	8000.236712	10.156826	-0.053617	4.815622
259.730395	8000.206190	10.161831	-0.053598	4.815614
259.701914	8000.246312	10.166835	-0.053593	4.815626
259.787312	8000.303245	10.171840	-0.053609	4.815642
259.889388	8000.235497	10.176845	-0.053628	4.815622
259.735354	8000.271433	10.181850	-0.053599	4.815633
259.552088	8000.246017	10.186855	-0.053565	4.815626
260.005161	8000.330314	10.191859	-0.053650	4.815649
259.957003	8000.281472	10.196864	-0.053641	4.815635
259.747431	8000.264169	10.201869	-0.053602	4.815631
260.034899	8000.260323	10.206874	-0.053655	4.815628
260.043446	8000.185708	10.211879	-0.053657	4.815606
259.844507	8000.251882	10.216883	-0.053620	4.815627
259.599756	8000.240413	10.221888	-0.053574	4.815625
259.844778	8000.260438	10.226893	-0.053620	4.815629
259.890465	8000.323131	10.231898	-0.053629	4.815647
259.832905	8000.213260	10.236903	-0.053618	4.815616
259.825506	8000.255862	10.241907	-0.053616	4.815628
259.830715	8000.281583	10.246912	-0.053618	4.815636
259.981731	8000.198614	10.251917	-0.053646	4.815611
260.026744	8000.281587	10.256922	-0.053654	4.815635
260.121209	8000.232938	10.261927	-0.053672	4.815620
260.154845	8000.258055	10.266931	-0.053678	4.815627
259.936871	8000.238479	10.271936	-0.053637	4.815622
259.929756	8000.274679	10.276941	-0.053636	4.815633
260.109724	8000.288301	10.281946	-0.053670	4.815636
259.857455	8000.239330	10.286951	-0.053623	4.815623
259.913695	8000.221028	10.291955	-0.053633	4.815617
260.216492	8000.276172	10.296960	-0.053690	4.815632
259.888099	8000.194986	10.301965	-0.053629	4.815610
260.048947	8000.259560	10.306970	-0.053659	4.815628
260.254898	8000.237295	10.311975	-0.053697	4.815621
260.090418	8000.211117	10.316979	-0.053666	4.815614
259.949044	8000.207744	10.321984	-0.053640	4.815613
260.159782	8000.254977	10.326989	-0.053679	4.815626
260.246328	8000.305522	10.331994	-0.053696	4.815641
259.941082	8000.242869	10.336999	-0.053639	4.815624
260.011891	8000.253641	10.342003	-0.053652	4.815626
260.020213	8000.310384	10.347008	-0.053654	4.815643
259.919370	8000.276701	10.352013	-0.053635	4.815634
260.050529	8000.290595	10.357018	-0.053659	4.815637
260.136476	8000.272778	10.362023	-0.053675	4.815631
260.227375	8000.292422	10.367027	-0.053692	4.815637
260.000008	8000.306869	10.372032	-0.053650	4.815642
260.061554	8000.261954	10.377037	-0.053662	4.815629
260.104453	8000.297902	10.382042	-0.053670	4.815639
259.764675	8000.228278	10.387047	-0.053606	4.815620
260.104818	8000.317139	10.392051	-0.053670	4.815645
260.195881	8000.289795	10.397056	-0.053687	4.815636
260.014160	8000.286830	10.402061	-0.053653	4.815636
259.788062	8000.290618	10.407066	-0.053611	4.815638
260.135966	8000.235428	10.412071	-0.053676	4.815621
260.196884	8000.250310	10.417075	-0.053687	4.815625
259.969630	8000.262622	10.422080	-0.053645	4.815629
259.939364	8000.243976	10.427085	-0.053639	4.815624
260.077623	8000.302841	10.432090	-0.053665	4.815641
259.921170	8000.191355	10.437095	-0.053636	4.815609
260.184204	8000.252258	10.442099	-0.053685	4.815625
260.267985	8000.277126	10.447104	-0.053701	4.815632
260.216155	8000.169484	10.452109	-0.053691	4.815601
259.989144	8000.269375	10.457114	-0.053649	4.815631
260.165834	8000.298964	10.462119	-0.053682	4.815639
260.066674	8000.278125	10.467123	-0.053663	4.815633
260.227391	8000.275413	10.472128	-0.053693	4.815632
260.273661	8000.238793	10.477133	-0.053702	4.815621
260.330433	8000.315552	10.482138	-0.053713	4.815643
260.100064	8000.229557	10.487143	-0.053670	4.815619
260.307778	8000.257517	10.492147	-0.053708	4.815626
260.187369	8000.304682	10.497152	-0.053686	4.815641
260.175617	8000.206239	10.502157	-0.053684	4.815612
260.199182	8000.256823	10.507162	-0.053688	4.815626
260.145537	8000.255951	10.512167	-0.053678	4.815626
260.277172	8000.246356	10.517171	-0.053703	4.815623
260.151250	8000.229352	10.522176	-0.053680	4.815619
260.006534	8000.200292	10.527181	-0.053653	4.815611
260.252272	8000.322857	10.532186	-0.053698	4.815646
260.241882	8000.276767	10.537191	-0.053697	4.815632
260.285891	8000.249721	10.542195	-0.053705	4.815624
260.195788	8000.283497	10.547200	-0.053688	4.815634
260.324508	8000.261040	10.552205	-0.053712	4.815627
260.161241	8000.307504	10.557210	-0.053682	4.815641
259.961957	8000.247650	10.562215	-0.053645	4.815625
260.270308	8000.310361	10.567219	-0.053702	4.815642
260.211779	8000.252805	10.572224	-0.053691	4.815625
260.112268	8000.212736	10.577229	-0.053673	4.815614
260.193477	8000.253582	10.582234	-0.053688	4.815626
260.303619	8000.194509	10.587239	-0.053708	4.815608
260.276089	8000.269891	10.592243	-0.053703	4.815630
260.291429	8000.327817	10.597248	-0.053706	4.815647
260.317449	8000.298342	10.602253	-0.053711	4.815638
260.282165	8000.328741	10.607258	-0.053705	4.815647
260.119361	8000.235306	10.612263	-0.053674	4.815621
260.272930	8000.231410	10.617267	-0.053703	4.815619
260.188688	8000.289845	10.622272	-0.053687	4.815636
260.225752	8000.286183	10.627277	-0.053694	4.815635
260.432557	8000.371801	10.632282	-0.053733	4.815659
260.401231	8000.281580	10.637287	-0.053727	4.815633
260.239682	8000.256517	10.642291	-0.053697	4.815626
260.362425	8000.302314	10.647296	-0.053720	4.815639
260.298286	8000.223306	10.652301	-0.053708	4.815616
260.175587	8000.221306	10.657306	-0.053685	4.815616
260.079470	8000.199448	10.662311	-0.053667	4.815610
260.399067	8000.237779	10.667315	-0.053727	4.815620
260.227990	8000.285185	10.672320	-0.053695	4.815635
260.311897	8000.228887	10.677325	-0.053711	4.815618
260.423087	8000.341779	10.682330	-0.053732	4.815650
260.287514	8000.215681	10.687335	-0.053706	4.815614
260.396454	8000.237755	10.692339	-0.053727	4.815620
260.319420	8000.220481	10.697344	-0.053712	4.815615
260.542938	8000.224136	10.702349	-0.053754	4.815615
260.739121	8000.260452	10.707354	-0.053791	4.815625
260.627256	8000.261832	10.712359	-0.053770	4.815626
260.551910	8000.316142	10.717363	-0.053756	4.815642
260.363759	8000.271420	10.722368	-0.053721	4.815630
260.415348	8000.249838	10.727373	-0.053730	4.815623
260.462846	8000.296542	10.732378	-0.053739	4.815637
260.545862	8000.292562	10.737383	-0.053755	4.815635
260.485721	8000.261679	10.742387	-0.053744	4.815626
260.348049	8000.330990	10.747392	-0.053718	4.815647
260.493249	8000.285305	10.752397	-0.053745	4.815633
260.392802	8000.258036	10.757402	-0.053727	4.815626
260.393793	8000.231356	10.762407	-0.053727	4.815618
260.492120	8000.239374	10.767411	-0.053745	4.815620
260.410441	8000.306396	10.772416	-0.053730	4.815640
260.242174	8000.239571	10.777421	-0.053699	4.815621
260.364273	8000.237297	10.782426	-0.053721	4.815620
260.245780	8000.208666	10.787431	-0.053699	4.815612
260.394035	8000.285851	10.792435	-0.053727	4.815634
260.372732	8000.296187	10.797440	-0.053723	4.815637
260.394812	8000.269851	10.802445	-0.053727	4.815629
260.379501	8000.342229	10.807450	-0.053725	4.815651
260.315321	8000.245064	10.812455	-0.053713	4.815622
260.322450	8000.238776	10.817459	-0.053714	4.815621
260.580244	8000.262215	10.822464	-0.053762	4.815626
260.446333	8000.252555	10.827469	-0.053737	4.815624
260.548912	8000.325791	10.832474	-0.053756	4.815645
260.558839	8000.208476	10.837479	-0.053758	4.815611
260.701211	8000.252458	10.842483	-0.053785	4.815623
260.545039	8000.285155	10.847488	-0.053756	4.815633
260.692265	8000.289699	10.852493	-0.053783	4.815634
260.602226	8000.335225	10.857498	-0.053766	4.815647
260.319479	8000.326337	10.862503	-0.053714	4.815646
260.440619	8000.268512	10.867507	-0.053736	4.815629
260.361504	8000.306739	10.872512	-0.053722	4.815640
260.336608	8000.243324	10.877517	-0.053717	4.815622
260.451799	8000.313562	10.882522	-0.053739	4.815642
260.409124	8000.322480	10.887527	-0.053731	4.815645
260.443456	8000.335861	10.892531	-0.053737	4.815648
260.409930	8000.350269	10.897536	-0.053731	4.815653
260.450010	8000.270827	10.902541	-0.053738	4.815629
260.461046	8000.323344	10.907546	-0.053741	4.815645
260.466842	8000.248682	10.912551	-0.053742	4.815623
260.456093	8000.245306	10.917555	-0.053740	4.815622
260.483012	8000.310898	10.922560	-0.053745	4.815641
260.337895	8000.298919	10.927565	-0.053718	4.815638
260.292286	8000.337694	10.932570	-0.053709	4.815650
260.484618	8000.231903	10.937575	-0.053745	4.815618
260.301191	8000.282311	10.942579	-0.053711	4.815633
260.232349	8000.334590	10.947584	-0.053698	4.815649
260.337591	8000.223105	10.952589	-0.053718	4.815616
260.459496	8000.298792	10.957594	-0.053741	4.815637
260.331901	8000.273215	10.962599	-0.053717	4.815631
260.244459	8000.228003	10.967603	-0.053701	4.815618
260.426313	8000.286513	10.972608	-0.053735	4.815634
260.498578	8000.263133	10.977613	-0.053748	4.815627
260.459170	8000.326573	10.982618	-0.053741	4.815646
260.468282	8000.270121	10.987623	-0.053743	4.815629
260.530599	8000.259395	10.992627	-0.053754	4.815626
260.515146	8000.349927	10.997632	-0.053751	4.815652
260.436473	8000.299517	11.002637	-0.053737	4.815638
260.585753	8000.390604	11.007642	-0.053765	4.815664
260.587952	8000.295591	11.012647	-0.053765	4.815636
260.698457	8000.297400	11.017651	-0.053786	4.815636
260.816694	8000.305744	11.022656	-0.053808	4.815638
260.670926	8000.255306	11.027661	-0.053781	4.815624
260.637431	8000.313503	11.032666	-0.053774	4.815641
260.676673	8000.323759	11.037671	-0.053782	4.815644
260.671624	8000.301252	11.042675	-0.053781	4.815637
260.479821	8000.289579	11.047680	-0.053745	4.815635
260.465876	8000.256247	11.052685	-0.053743	4.815625
260.620911	8000.289755	11.057690	-0.053772	4.815634
260.371378	8000.319859	11.062695	-0.053725	4.815644
260.387488	8000.284882	11.067699	-0.053728	4.815634
260.539036	8000.274545	11.072704	-0.053756	4.815630
260.678376	8000.241581	11.077709	-0.053782	4.815620
260.664465	8000.273397	11.082714	-0.053780	4.815629
260.471745	8000.269185	11.087719	-0.053744	4.815629
260.683542	8000.335661	11.092723	-0.053784	4.815647
260.715348	8000.337252	11.097728	-0.053790	4.815647
260.461335	8000.277570	11.102733	-0.053742	4.815631
260.617599	8000.349547	11.107738	-0.053771	4.815651
260.570593	8000.293246	11.112743	-0.053763	4.815635
260.685454	8000.330371	11.117747	-0.053784	4.815646
260.664496	8000.354596	11.122752	-0.053780	4.815653
260.591144	8000.258349	11.127757	-0.053767	4.815625
260.482138	8000.296088	11.132762	-0.053746	4.815636
260.663610	8000.239248	11.137767	-0.053780	4.815619
260.855288	8000.253063	11.142771	-0.053816	4.815622
260.714599	8000.308441	11.147776	-0.053790	4.815639
260.325324	8000.248686	11.152781	-0.053717	4.815623
260.535168	8000.326878	11.157786	-0.053756	4.815645
260.573593	8000.255953	11.162791	-0.053764	4.815624
260.425420	8000.271692	11.167795	-0.053736	4.815630
260.483565	8000.322842	11.172800	-0.053747	4.815644
260.540976	8000.314171	11.177805	-0.053758	4.815641
260.572659	8000.358481	11.182810	-0.053764	4.815654
260.628992	8000.320957	11.187815	-0.053774	4.815643
260.698667	8000.251610	11.192819	-0.053787	4.815622
260.402174	8000.262791	11.197824	-0.053732	4.815627
260.484053	8000.261996	11.202829	-0.053747	4.815626
260.862810	8000.329064	11.207834	-0.053818	4.815644
260.430652	8000.283559	11.212839	-0.053737	4.815633
260.420075	8000.313294	11.217843	-0.053736	4.815642
260.479006	8000.312125	11.222848	-0.053747	4.815641
260.514067	8000.236873	11.227853	-0.053753	4.815619
260.456564	8000.297882	11.232858	-0.053742	4.815637
260.348651	8000.225635	11.237863	-0.053722	4.815616
260.547454	8000.276946	11.242867	-0.053759	4.815631
260.622025	8000.350792	11.247872	-0.053773	4.815652
260.376245	8000.296585	11.252877	-0.053728	4.815637
260.523093	8000.319279	11.257882	-0.053755	4.815643
260.805718	8000.239527	11.262887	-0.053808	4.815618
260.691151	8000.241931	11.267891	-0.053786	4.815620
260.471725	8000.255439	11.272896	-0.053746	4.815625
260.561037	8000.197094	11.277901	-0.053762	4.815607
260.493590	8000.209880	11.282906	-0.053750	4.815611
260.314793	8000.262499	11.287911	-0.053717	4.815627
260.453758	8000.231665	11.292915	-0.053742	4.815618
260.476762	8000.233112	11.297920	-0.053747	4.815618
260.583027	8000.211355	11.302925	-0.053767	4.815611
260.824337	8000.296470	11.307930	-0.053812	4.815635
260.619435	8000.307010	11.312935	-0.053773	4.815639
260.490175	8000.240822	11.317939	-0.053749	4.815620
260.567976	8000.320061	11.322944	-0.053764	4.815643
260.380462	8000.273213	11.327949	-0.053729	4.815630
260.574789	8000.278528	11.332954	-0.053765	4.815631
260.605928	8000.208552	11.337959	-0.053771	4.815610
260.717185	8000.234937	11.342963	-0.053792	4.815617
260.943567	8000.251455	11.347968	-0.053834	4.815621
260.671474	8000.207498	11.352973	-0.053783	4.815610
260.815122	8000.238684	11.357978	-0.053810	4.815618
260.825023	8000.255938	11.362983	-0.053812	4.815623
260.730325	8000.225558	11.367987	-0.053795	4.815615
260.674319	8000.278047	11.372992	-0.053784	4.815630
260.706435	8000.280712	11.377997	-0.053790	4.815631
260.886957	8000.338134	11.383002	-0.053824	4.815647
260.635160	8000.281691	11.388007	-0.053777	4.815631
260.730238	8000.244800	11.393011	-0.053795	4.815620
260.721305	8000.329030	11.398016	-0.053793	4.815645
260.676993	8000.296270	11.403021	-0.053785	4.815636
260.656754	8000.362159	11.408026	-0.053781	4.815655
260.737802	8000.299407	11.413031	-0.053796	4.815636
260.674386	8000.305850	11.418035	-0.053785	4.815638
260.790834	8000.368633	11.423040	-0.053806	4.815656
260.704380	8000.318096	11.428045	-0.053790	4.815642
260.839428	8000.336326	11.433050	-0.053815	4.815646
260.905574	8000.309642	11.438055	-0.053828	4.815638
260.835440	8000.281800	11.443059	-0.053815	4.815631
260.791212	8000.292829	11.448064	-0.053807	4.815634
260.774546	8000.265860	11.453069	-0.053804	4.815626
260.719435	8000.369629	11.458074	-0.053793	4.815657
260.881708	8000.341312	11.463079	-0.053824	4.815648
260.904079	8000.276532	11.468083	-0.053828	4.815629
260.804605	8000.330447	11.473088	-0.053809	4.815645
260.904904	8000.254125	11.478093	-0.053828	4.815622
260.924121	8000.334544	11.483098	-0.053832	4.815646
260.764196	8000.272126	11.488103	-0.053802	4.815628
260.742126	8000.247205	11.493107	-0.053798	4.815621
261.041241	8000.328992	11.498112	-0.053854	4.815643
260.930555	8000.315439	11.503117	-0.053833	4.815640
261.018369	8000.302994	11.508122	-0.053849	4.815636
260.856439	8000.342004	11.513127	-0.053819	4.815648
260.992002	8000.310046	11.518131	-0.053845	4.815638
260.801158	8000.331496	11.523136	-0.053809	4.815645
260.788373	8000.273619	11.528141	-0.053807	4.815628
260.917444	8000.330200	11.533146	-0.053831	4.815644
260.973624	8000.351414	11.538151	-0.053841	4.815650
261.036911	8000.295847	11.543155	-0.053853	4.815634
261.117612	8000.384747	11.548160	-0.053868	4.815659
260.944232	8000.311428	11.553165	-0.053836	4.815639
260.826668	8000.369320	11.558170	-0.053814	4.815656
260.896111	8000.261521	11.563175	-0.053827	4.815624
260.981130	8000.291750	11.568179	-0.053843	4.815633
260.861862	8000.304757	11.573184	-0.053821	4.815637
260.779742	8000.228659	11.578189	-0.053806	4.815615
260.904318	8000.281962	11.583194	-0.053829	4.815630
260.735022	8000.269588	11.588199	-0.053797	4.815627
260.748367	8000.268742	11.593203	-0.053800	4.815627
260.869624	8000.319855	11.598208	-0.053823	4.815641
260.828393	8000.305301	11.603213	-0.053815	4.815637
260.649980	8000.345110	11.608218	-0.053782	4.815650
260.846927	8000.357944	11.613223	-0.053818	4.815653
260.930292	8000.299501	11.618227	-0.053834	4.815635
260.762033	8000.297824	11.623232	-0.053803	4.815636
260.903259	8000.242462	11.628237	-0.053829	4.815619
260.981280	8000.266169	11.633242	-0.053844	4.815625
260.735261	8000.242929	11.638247	-0.053798	4.815620
260.517766	8000.213748	11.643251	-0.053757	4.815612
260.872800	8000.239843	11.648256	-0.053823	4.815618
260.778468	8000.291707	11.653261	-0.053806	4.815634
260.713469	8000.263948	11.658266	-0.053794	4.815626
260.669634	8000.297412	11.663271	-0.053786	4.815636
260.842023	8000.238287	11.668275	-0.053818	4.815618
260.863066	8000.313396	11.673280	-0.053822	4.815640
260.710374	8000.220124	11.678285	-0.053793	4.815613
260.878348	8000.262388	11.683290	-0.053825	4.815625
260.861319	8000.249298	11.688295	-0.053822	4.815621
260.688643	8000.236869	11.693299	-0.053790	4.815618
260.919302	8000.348510	11.698304	-0.053833	4.815650
260.876241	8000.288001	11.703309	-0.053825	4.815632
260.831627	8000.319317	11.708314	-0.053816	4.815641
260.988029	8000.306923	11.713319	-0.053846	4.815637
261.112171	8000.237398	11.718323	-0.053869	4.815616
260.839001	8000.291680	11.723328	-0.053818	4.815633
260.683267	8000.229331	11.728333	-0.053789	4.815616
261.117023	8000.353903	11.733338	-0.053870	4.815650
260.971394	8000.338711	11.738343	-0.053843	4.815646
260.748196	8000.277395	11.743347	-0.053801	4.815630
260.742626	8000.351001	11.748352	-0.053800	4.815651
260.920169	8000.264192	11.753357	-0.053833	4.815625
260.825818	8000.351300	11.758362	-0.053816	4.815651
260.818991	8000.327695	11.763367	-0.053814	4.815644
261.122844	8000.343344	11.768371	-0.053871	4.815647
261.260672	8000.285791	11.773376	-0.053897	4.815630
260.812810	8000.258185	11.778381	-0.053813	4.815624
260.942113	8000.285933	11.783386	-0.053838	4.815631
260.947131	8000.291359	11.788391	-0.053839	4.815633
260.947010	8000.282817	11.793395	-0.053839	4.815630
261.101971	8000.352638	11.798400	-0.053867	4.815650
261.042357	8000.305743	11.803405	-0.053856	4.815636
261.079141	8000.314891	11.808410	-0.053863	4.815639
261.057303	8000.328423	11.813415	-0.053859	4.815643
261.255680	8000.322056	11.818419	-0.053896	4.815640
261.024795	8000.353531	11.823424	-0.053853	4.815651
260.999248	8000.289037	11.828429	-0.053849	4.815632
261.097912	8000.342985	11.833434	-0.053867	4.815647
260.976598	8000.312170	11.838439	-0.053844	4.815639
260.862494	8000.279337	11.843443	-0.053823	4.815630
261.007213	8000.319086	11.848448	-0.053850	4.815641
261.261227	8000.262363	11.853453	-0.053898	4.815623
261.123420	8000.295360	11.858458	-0.053872	4.815633
260.835411	8000.300270	11.863463	-0.053818	4.815636
261.227060	8000.291721	11.868467	-0.053891	4.815631
261.162582	8000.317372	11.873472	-0.053879	4.815639
260.850183	8000.269550	11.878477	-0.053821	4.815627
261.171943	8000.258791	11.883482	-0.053881	4.815622
261.093053	8000.307703	11.888487	-0.053867	4.815637
260.907447	8000.247001	11.893491	-0.053832	4.815620
261.032428	8000.356916	11.898496	-0.053855	4.815651
261.110362	8000.255664	11.903501	-0.053870	4.815621
261.145099	8000.318180	11.908506	-0.053876	4.815640
261.222412	8000.304495	11.913511	-0.053891	4.815635
261.263840	8000.281679	11.918515	-0.053899	4.815628
261.264587	8000.294511	11.923520	-0.053899	4.815632
260.919784	8000.216256	11.928525	-0.053835	4.815611
260.796126	8000.240940	11.933530	-0.053812	4.815619
261.125674	8000.280504	11.938535	-0.053873	4.815629
261.010340	8000.240175	11.943539	-0.053852	4.815617
261.066386	8000.329740	11.948544	-0.053862	4.815643
261.170259	8000.272700	11.953549	-0.053881	4.815626
261.183053	8000.331654	11.958554	-0.053884	4.815643
260.933240	8000.344664	11.963559	-0.053837	4.815648
261.320851	8000.254879	11.968563	-0.053910	4.815620
261.221818	8000.294918	11.973568	-0.053891	4.815632
261.235945	8000.310105	11.978573	-0.053894	4.815637
261.186511	8000.341342	11.983578	-0.053885	4.815646
261.277540	8000.278751	11.988583	-0.053902	4.815627
261.268602	8000.259385	11.993587	-0.053900	4.815622
260.996881	8000.341458	11.998592	-0.053850	4.815647
261.154742	8000.263940	12.003597	-0.053879	4.815624
261.071896	8000.290358	12.008602	-0.053864	4.815632
261.149565	8000.302311	12.013607	-0.053878	4.815635
261.158276	8000.218084	12.018611	-0.053880	4.815610
261.139297	8000.275451	12.023616	-0.053876	4.815627
261.064127	8000.264614	12.028621	-0.053862	4.815624
261.126568	8000.285930	12.033626	-0.053874	4.815630
261.223072	8000.268287	12.038631	-0.053892	4.815625
261.046246	8000.236565	12.043635	-0.053859	4.815616
261.179423	8000.287873	12.048640	-0.053884	4.815631
261.119667	8000.214275	12.053645	-0.053873	4.815609
261.235123	8000.275975	12.058650	-0.053894	4.815627
260.958926	8000.304574	12.063655	-0.053843	4.815636
261.036247	8000.311181	12.068659	-0.053858	4.815638
261.060175	8000.400222	12.073664	-0.053862	4.815664
261.003682	8000.322405	12.078669	-0.053852	4.815641
261.025519	8000.335582	12.083674	-0.053856	4.815645
261.157673	8000.319588	12.088679	-0.053880	4.815640
261.331256	8000.278640	12.093683	-0.053913	4.815627
261.280415	8000.315193	12.098688	-0.053903	4.815638
261.240205	8000.248323	12.103693	-0.053896	4.815619
261.211422	8000.307665	12.108698	-0.053890	4.815636
261.198147	8000.337357	12.113703	-0.053888	4.815645
261.280782	8000.277834	12.118707	-0.053903	4.815627
261.340813	8000.314063	12.123712	-0.053915	4.815637
261.267131	8000.237033	12.128717	-0.053901	4.815615
261.145278	8000.315147	12.133722	-0.053878	4.815639
261.369242	8000.303859	12.138727	-0.053920	4.815634
261.277001	8000.252158	12.143731	-0.053903	4.815620
261.028034	8000.330331	12.148736	-0.053857	4.815644
261.224954	8000.328213	12.153741	-0.053893	4.815642
261.368991	8000.323094	12.158746	-0.053920	4.815640
261.443936	8000.290146	12.163751	-0.053934	4.815630
261.245834	8000.229239	12.168755	-0.053897	4.815613
261.473061	8000.281017	12.173760	-0.053940	4.815627
261.484336	8000.295089	12.178765	-0.053942	4.815631
261.399450	8000.283025	12.183770	-0.053926	4.815628
261.453871	8000.305279	12.188775	-0.053936	4.815634
261.413497	8000.248018	12.193779	-0.053929	4.815618
261.338095	8000.325823	12.198784	-0.053915	4.815641
261.355792	8000.286599	12.203789	-0.053918	4.815629
261.391149	8000.246596	12.208794	-0.053925	4.815617
261.229252	8000.268519	12.213799	-0.053895	4.815625
261.181382	8000.227155	12.218803	-0.053886	4.815613
261.358610	8000.319769	12.223808	-0.053919	4.815639
261.315433	8000.232557	12.228813	-0.053911	4.815614
261.119405	8000.267807	12.233818	-0.053874	4.815625
261.262038	8000.274413	12.238823	-0.053901	4.815626
261.224292	8000.244963	12.243827	-0.053894	4.815618
261.264686	8000.285144	12.248832	-0.053902	4.815629
261.164228	8000.223697	12.253837	-0.053883	4.815612
261.316053	8000.276379	12.258842	-0.053911	4.815626
261.177703	8000.284802	12.263847	-0.053886	4.815630
261.196092	8000.242385	12.268851	-0.053889	4.815617
261.377662	8000.277397	12.273856	-0.053923	4.815626
261.205854	8000.234008	12.278861	-0.053891	4.815615
261.125246	8000.249783	12.283866	-0.053876	4.815620
261.302605	8000.312494	12.288871	-0.053909	4.815637
261.439778	8000.254930	12.293875	-0.053935	4.815620
261.289367	8000.273837	12.298880	-0.053907	4.815626
261.091232	8000.244970	12.303885	-0.053870	4.815618
261.353645	8000.318684	12.308890	-0.053919	4.815639
261.332170	8000.340765	12.313895	-0.053915	4.815645
261.300179	8000.306069	12.318899	-0.053909	4.815635
261.371894	8000.290156	12.323904	-0.053922	4.815630
261.207377	8000.274655	12.328909	-0.053892	4.815626
261.154189	8000.225729	12.333914	-0.053882	4.815612
261.222161	8000.298401	12.338919	-0.053894	4.815633
261.281582	8000.202186	12.343923	-0.053905	4.815605
261.477788	8000.239572	12.348928	-0.053942	4.815615
261.119063	8000.164293	12.353933	-0.053875	4.815595
261.360836	8000.199220	12.358938	-0.053920	4.815604
261.379192	8000.233700	12.363943	-0.053924	4.815614
261.298516	8000.186461	12.368947	-0.053909	4.815600
261.322104	8000.238115	12.373952	-0.053913	4.815615
261.160670	8000.209848	12.378957	-0.053883	4.815608
261.328165	8000.276670	12.383962	-0.053915	4.815626
261.117848	8000.270033	12.388967	-0.053875	4.815626
261.329335	8000.253200	12.393971	-0.053915	4.815620
261.529197	8000.286375	12.398976	-0.053952	4.815628
261.315617	8000.283956	12.403981	-0.053912	4.815629
261.513803	8000.317104	12.408986	-0.053949	4.815637
261.394056	8000.272429	12.413991	-0.053927	4.815625
261.330539	8000.240422	12.418995	-0.053915	4.815616
261.350399	8000.219390	12.424000	-0.053919	4.815610
261.177739	8000.202689	12.429005	-0.053887	4.815606
261.379019	8000.249770	12.434010	-0.053924	4.815618
261.399609	8000.214865	12.439015	-0.053928	4.815608
261.387902	8000.215746	12.444019	-0.053926	4.815608
261.441687	8000.262554	12.449024	-0.053936	4.815622
261.327004	8000.208350	12.454029	-0.053915	4.815606
261.539894	8000.269506	12.459034	-0.053955	4.815623
261.390455	8000.242503	12.464039	-0.053927	4.815616
261.256824	8000.182650	12.469043	-0.053902	4.815599
261.192241	8000.260632	12.474048	-0.053890	4.815622
261.247676	8000.202801	12.479053	-0.053900	4.815605
261.443459	8000.203867	12.484058	-0.053937	4.815605
261.417445	8000.272868	12.489063	-0.053932	4.815625
261.483411	8000.245113	12.494067	-0.053944	4.815616
261.530382	8000.307830	12.499072	-0.053953	4.815635
261.271818	8000.290792	12.504077	-0.053905	4.815631
261.530923	8000.321730	12.509082	-0.053953	4.815639
261.424877	8000.322137	12.514087	-0.053934	4.815639
261.324078	8000.230780	12.519091	-0.053915	4.815613
261.444033	8000.317118	12.524096	-0.053937	4.815638
261.531349	8000.237378	12.529101	-0.053954	4.815614
261.521154	8000.255372	12.534106	-0.053952	4.815619
261.323461	8000.332247	12.539111	-0.053915	4.815643
261.386250	8000.254243	12.544115	-0.053927	4.815620
261.373005	8000.267914	12.549120	-0.053924	4.815624
261.276046	8000.217205	12.554125	-0.053906	4.815609
261.323199	8000.242543	12.559130	-0.053915	4.815616
261.497733	8000.236855	12.564135	-0.053948	4.815614
261.193070	8000.201976	12.569139	-0.053891	4.815605
261.131945	8000.302443	12.574144	-0.053880	4.815635
261.170454	8000.275307	12.579149	-0.053887	4.815627
261.336458	8000.288704	12.584154	-0.053918	4.815630
261.394113	8000.277901	12.589159	-0.053929	4.815626
261.462059	8000.275811	12.594163	-0.053941	4.815626
261.581561	8000.289516	12.599168	-0.053964	4.815629
261.420273	8000.242027	12.604173	-0.053934	4.815616
261.275262	8000.259954	12.609178	-0.053907	4.815622
261.297862	8000.287028	12.614183	-0.053911	4.815630
261.256649	8000.267133	12.619187	-0.053903	4.815624
261.236836	8000.248657	12.624192	-0.053900	4.815619
261.296927	8000.200514	12.629197	-0.053911	4.815604
261.682533	8000.309349	12.634202	-0.053983	4.815634
261.393917	8000.277936	12.639207	-0.053929	4.815626
261.480718	8000.218480	12.644211	-0.053945	4.815609
261.644537	8000.309808	12.649216	-0.053976	4.815635
261.449194	8000.276714	12.654221	-0.053939	4.815626
261.366621	8000.284981	12.659226	-0.053924	4.815629
261.486714	8000.271995	12.664231	-0.053946	4.815624
261.508464	8000.279830	12.669235	-0.053951	4.815626
261.440632	8000.342807	12.674240	-0.053938	4.815645
261.244413	8000.312903	12.679245	-0.053902	4.815637
261.381186	8000.242516	12.684250	-0.053927	4.815616
261.351287	8000.291161	12.689255	-0.053921	4.815631
261.316164	8000.275638	12.694259	-0.053915	4.815626
261.510719	8000.215808	12.699264	-0.053951	4.815608
261.518880	8000.206333	12.704269	-0.053953	4.815605
261.449080	8000.262869	12.709274	-0.053940	4.815622
261.454015	8000.276838	12.714279	-0.053941	4.815626
261.350514	8000.223885	12.719283	-0.053922	4.815611
261.363713	8000.294594	12.724288	-0.053924	4.815631
261.365509	8000.225206	12.729293	-0.053924	4.815611
261.649197	8000.268294	12.734298	-0.053977	4.815622
261.294697	8000.288137	12.739303	-0.053911	4.815630
261.434089	8000.225269	12.744307	-0.053937	4.815611
261.490562	8000.335135	12.749312	-0.053948	4.815643
261.510639	8000.237208	12.754317	-0.053952	4.815614
261.666082	8000.273929	12.759322	-0.053981	4.815624
261.653608	8000.232076	12.764327	-0.053978	4.815612
261.449631	8000.218066	12.769331	-0.053940	4.815609
261.639382	8000.310885	12.774336	-0.053976	4.815635
261.412632	8000.291163	12.779341	-0.053934	4.815630
261.735085	8000.314593	12.784346	-0.053994	4.815636
261.604627	8000.306056	12.789351	-0.053970	4.815634
261.408393	8000.272948	12.794355	-0.053933	4.815625
261.642570	8000.255418	12.799360	-0.053977	4.815619
261.582196	8000.238415	12.804365	-0.053965	4.815614
261.503455	8000.289465	12.809370	-0.053951	4.815629
261.553296	8000.288148	12.814375	-0.053960	4.815629
261.620695	8000.202742	12.819379	-0.053973	4.815603
261.713185	8000.276884	12.824384	-0.053990	4.815625
261.701826	8000.260681	12.829389	-0.053988	4.815620
261.773664	8000.336622	12.834394	-0.054001	4.815642
261.713478	8000.303601	12.839399	-0.053990	4.815632
261.474045	8000.247358	12.844403	-0.053946	4.815617
261.673193	8000.320038	12.849408	-0.053983	4.815637
261.620073	8000.326650	12.854413	-0.053973	4.815640
261.742291	8000.327583	12.859418	-0.053996	4.815639
261.679433	8000.294519	12.864423	-0.053984	4.815630
261.829929	8000.232900	12.869427	-0.054012	4.815611
261.756873	8000.276567	12.874432	-0.053999	4.815624
261.637538	8000.263940	12.879437	-0.053976	4.815621
261.866063	8000.318945	12.884442	-0.054019	4.815636
261.783116	8000.299436	12.889447	-0.054004	4.815631
261.654750	8000.277049	12.894451	-0.053980	4.815625
261.836237	8000.283223	12.899456	-0.054014	4.815626
261.769379	8000.300291	12.904461	-0.054001	4.815631
261.663752	8000.263323	12.909466	-0.053982	4.815621
261.796734	8000.287929	12.914471	-0.054006	4.815627
261.851619	8000.282422	12.919475	-0.054017	4.815626
261.799805	8000.342457	12.924480	-0.054007	4.815643
261.754502	8000.286182	12.929485	-0.053999	4.815627
261.598316	8000.323150	12.934490	-0.053970	4.815639
261.745549	8000.347989	12.939495	-0.053997	4.815645
261.695905	8000.319413	12.944499	-0.053988	4.815637
262.062398	8000.357448	12.949504	-0.054056	4.815646
262.079275	8000.290441	12.954509	-0.054059	4.815627
261.989898	8000.281508	12.959514	-0.054043	4.815625
262.081268	8000.346020	12.964519	-0.054060	4.815643
262.104204	8000.254546	12.969523	-0.054064	4.815616
261.851696	8000.326254	12.974528	-0.054017	4.815638
261.654560	8000.251477	12.979533	-0.053980	4.815617
261.761989	8000.278869	12.984538	-0.054000	4.815625
261.848520	8000.318737	12.989543	-0.054017	4.815636
261.579216	8000.271617	12.994547	-0.053967	4.815624
261.794216	8000.350966	12.999552	-0.054007	4.815646
261.804346	8000.325502	13.004557	-0.054009	4.815638
261.769076	8000.224534	13.009562	-0.054002	4.815609
261.661972	8000.317842	13.014567	-0.053982	4.815637
261.607758	8000.247538	13.019571	-0.053972	4.815616
261.759557	8000.315173	13.024576	-0.054000	4.815636
261.572821	8000.270471	13.029581	-0.053966	4.815623
261.568625	8000.273610	13.034586	-0.053965	4.815624
261.803169	8000.300944	13.039591	-0.054009	4.815631
261.857582	8000.228143	13.044595	-0.054019	4.815610
261.849438	8000.333749	13.049600	-0.054017	4.815641
261.852760	8000.299630	13.054605	-0.054018	4.815631
261.739964	8000.305266	13.059610	-0.053997	4.815633
261.795171	8000.357438	13.064615	-0.054007	4.815648
261.756425	8000.299135	13.069619	-0.054000	4.815631
261.748688	8000.295808	13.074624	-0.053999	4.815630
261.647448	8000.300565	13.079629	-0.053980	4.815632
261.699725	8000.291811	13.084634	-0.053990	4.815629
261.897675	8000.295050	13.089639	-0.054027	4.815629
261.700909	8000.249116	13.094643	-0.053990	4.815616
261.592952	8000.316778	13.099648	-0.053970	4.815637
261.692592	8000.308798	13.104653	-0.053989	4.815634
261.678527	8000.227401	13.109658	-0.053986	4.815610
261.745153	8000.303256	13.114663	-0.053998	4.815632
261.864074	8000.228305	13.119667	-0.054021	4.815610
261.870349	8000.308514	13.124672	-0.054022	4.815633
261.695144	8000.285362	13.129677	-0.053989	4.815627
261.818358	8000.278835	13.134682	-0.054012	4.815625
261.752779	8000.296991	13.139687	-0.054000	4.815630
261.656419	8000.254835	13.144691	-0.053982	4.815618
261.529607	8000.342481	13.149696	-0.053959	4.815645
261.775923	8000.269612	13.154701	-0.054004	4.815622
261.891346	8000.243733	13.159706	-0.054026	4.815614
261.952002	8000.281042	13.164711	-0.054037	4.815625
261.654083	8000.258020	13.169715	-0.053982	4.815619
262.155778	8000.275836	13.174720	-0.054075	4.815622
261.642802	8000.258911	13.179725	-0.053980	4.815620
261.608700	8000.228452	13.184730	-0.053974	4.815611
261.772418	8000.296282	13.189735	-0.054004	4.815630
261.729312	8000.248587	13.194739	-0.053996	4.815616
261.635931	8000.275902	13.199744	-0.053979	4.815625
261.625882	8000.214864	13.204749	-0.053977	4.815607
261.622857	8000.242587	13.209754	-0.053976	4.815615
261.552043	8000.296971	13.214759	-0.053963	4.815631
261.643592	8000.250409	13.219763	-0.053980	4.815617
261.695528	8000.271554	13.224768	-0.053990	4.815623
261.739434	8000.281888	13.229773	-0.053998	4.815626
261.698917	8000.257733	13.234778	-0.053991	4.815619
261.922364	8000.236824	13.239783	-0.054032	4.815612
261.699656	8000.207555	13.244787	-0.053991	4.815604
261.711759	8000.344465	13.249792	-0.053993	4.815644
261.833076	8000.318683	13.254797	-0.054016	4.815636
261.949456	8000.228737	13.259802	-0.054038	4.815609
261.829448	8000.303678	13.264807	-0.054015	4.815632
261.658553	8000.223990	13.269811	-0.053984	4.815609
261.840654	8000.271828	13.274816	-0.054018	4.815622
261.982169	8000.298710	13.279821	-0.054044	4.815630
261.930265	8000.279708	13.284826	-0.054034	4.815624
261.862669	8000.335213	13.289831	-0.054022	4.815641
261.788201	8000.295550	13.294835	-0.054008	4.815630
261.696508	8000.297260	13.299840	-0.053991	4.815631
261.787619	8000.293412	13.304845	-0.054008	4.815629
261.760175	8000.247042	13.309850	-0.054003	4.815616
261.663194	8000.284978	13.314855	-0.053985	4.815627
261.695325	8000.245989	13.319859	-0.053991	4.815616
261.879413	8000.242594	13.324864	-0.054025	4.815614
261.626067	8000.254477	13.329869	-0.053978	4.815618
261.622383	8000.245877	13.334874	-0.053977	4.815616
261.785091	8000.347867	13.339879	-0.054008	4.815645
261.961062	8000.268508	13.344883	-0.054041	4.815621
261.924913	8000.291418	13.349888	-0.054034	4.815628
261.872500	8000.298041	13.354893	-0.054024	4.815630
262.048272	8000.245380	13.359898	-0.054057	4.815614
261.894818	8000.302686	13.364903	-0.054028	4.815631
261.708381	8000.202451	13.369907	-0.053994	4.815603
261.755565	8000.249151	13.374912	-0.054003	4.815616
261.833518	8000.232272	13.379917	-0.054017	4.815611
261.720104	8000.204790	13.384922	-0.053996	4.815603
261.986944	8000.233719	13.389927	-0.054046	4.815611
262.012754	8000.181811	13.394931	-0.054051	4.815595
261.932206	8000.307595	13.399936	-0.054036	4.815632
261.779837	8000.286952	13.404941	-0.054007	4.815627
261.825916	8000.215082	13.409946	-0.054016	4.815606
261.938528	8000.266056	13.414951	-0.054037	4.815620
261.631093	8000.230062	13.419955	-0.053980	4.815611
262.025190	8000.285637	13.424960	-0.054053	4.815626
262.056726	8000.281884	13.429965	-0.054059	4.815624
261.870645	8000.237193	13.434970	-0.054025	4.815612
261.960687	8000.314499	13.439975	-0.054041	4.815634
262.074825	8000.258694	13.444979	-0.054063	4.815617
261.842388	8000.314709	13.449984	-0.054019	4.815635
261.946643	8000.305736	13.454989	-0.054039	4.815632
261.824400	8000.240728	13.459994	-0.054016	4.815613
261.836139	8000.324230	13.464999	-0.054018	4.815638
261.960517	8000.284613	13.470003	-0.054042	4.815626
261.983633	8000.254022	13.475008	-0.054046	4.815616
261.874002	8000.230873	13.480013	-0.054026	4.815610
262.048255	8000.237997	13.485018	-0.054058	4.815611
262.039681	8000.361754	13.490023	-0.054057	4.815648
261.996728	8000.262795	13.495027	-0.054049	4.815619
262.070584	8000.271482	13.500032	-0.054062	4.815621
261.927035	8000.275548	13.505037	-0.054036	4.815623
261.836577	8000.193970	13.510042	-0.054019	4.815600
262.067771	8000.302421	13.515047	-0.054062	4.815630
261.758370	8000.236489	13.520051	-0.054004	4.815612
261.945089	8000.274790	13.525056	-0.054039	4.815623
261.836966	8000.262346	13.530061	-0.054019	4.815620
261.946435	8000.253459	13.535066	-0.054039	4.815616
261.926435	8000.333239	13.540071	-0.054036	4.815640
261.897782	8000.205677	13.545075	-0.054030	4.815603
262.107939	8000.231545	13.550080	-0.054070	4.815609
262.167910	8000.217576	13.555085	-0.054081	4.815605
262.086842	8000.215187	13.560090	-0.054066	4.815605
262.183126	8000.268031	13.565095	-0.054084	4.815620
262.096477	8000.228168	13.570099	-0.054068	4.815608
262.111539	8000.327747	13.575104	-0.054071	4.815637
262.069241	8000.213846	13.580109	-0.054063	4.815604
262.136050	8000.237371	13.585114	-0.054075	4.815611
262.080703	8000.288804	13.590119	-0.054065	4.815626
262.014548	8000.314427	13.595123	-0.054053	4.815634
262.158274	8000.255902	13.600128	-0.054079	4.815616
262.064455	8000.273597	13.605133	-0.054062	4.815622
261.905372	8000.262456	13.610138	-0.054032	4.815619
262.171172	8000.304186	13.615143	-0.054082	4.815630
262.036193	8000.262466	13.620147	-0.054057	4.815619
262.040579	8000.306331	13.625152	-0.054058	4.815631
261.935891	8000.277923	13.630157	-0.054038	4.815624
261.958581	8000.271889	13.635162	-0.054043	4.815622
261.987236	8000.335376	13.640167	-0.054048	4.815640
262.150441	8000.257944	13.645171	-0.054078	4.815617
262.130531	8000.304616	13.650176	-0.054075	4.815631
261.906977	8000.314850	13.655181	-0.054033	4.815635
261.986151	8000.278766	13.660186	-0.054048	4.815624
262.043922	8000.384383	13.665191	-0.054059	4.815654
261.977261	8000.322419	13.670195	-0.054046	4.815636
262.046057	8000.406855	13.675200	-0.054059	4.815661
262.058421	8000.334433	13.680205	-0.054062	4.815640
262.021512	8000.282567	13.685210	-0.054055	4.815625
261.831805	8000.315784	13.690215	-0.054019	4.815635
261.757016	8000.293204	13.695219	-0.054006	4.815629
261.850332	8000.348135	13.700224	-0.054023	4.815645
261.853774	8000.294793	13.705229	-0.054024	4.815629
261.931421	8000.253344	13.710234	-0.054038	4.815616
261.891242	8000.312502	13.715239	-0.054031	4.815634
261.795169	8000.232968	13.720243	-0.054013	4.815611
261.982955	8000.250994	13.725248	-0.054048	4.815616
261.793581	8000.234018	13.730253	-0.054013	4.815611
261.855307	8000.212602	13.735258	-0.054024	4.815605
262.082336	8000.276126	13.740263	-0.054067	4.815622
262.042182	8000.230616	13.745267	-0.054059	4.815609
262.193180	8000.257653	13.750272	-0.054087	4.815616
261.912335	8000.266951	13.755277	-0.054035	4.815621
261.837003	8000.272131	13.760282	-0.054021	4.815622
261.904227	8000.274302	13.765287	-0.054034	4.815623
261.834404	8000.262484	13.770291	-0.054021	4.815620
261.909233	8000.285072	13.775296	-0.054035	4.815626
261.762530	8000.307242	13.780301	-0.054007	4.815633
262.107339	8000.268025	13.785306	-0.054072	4.815620
262.114699	8000.292714	13.790311	-0.054073	4.815627
262.194269	8000.248092	13.795315	-0.054088	4.815614
262.113526	8000.332220	13.800320	-0.054073	4.815639
261.713174	8000.308591	13.805325	-0.053998	4.815634
261.581283	8000.215656	13.810330	-0.053974	4.815607
261.845732	8000.328921	13.815335	-0.054023	4.815639
261.775404	8000.229516	13.820339	-0.054010	4.815610
261.596681	8000.245824	13.825344	-0.053977	4.815616
261.830109	8000.269935	13.830349	-0.054020	4.815622
261.982824	8000.277775	13.835354	-0.054049	4.815623
261.800961	8000.255582	13.840359	-0.054015	4.815618
261.833313	8000.228345	13.845363	-0.054021	4.815610
262.280335	8000.252744	13.850368	-0.054104	4.815615
262.155432	8000.319061	13.855373	-0.054081	4.815635
262.091919	8000.263556	13.860378	-0.054069	4.815619
262.191780	8000.349569	13.865383	-0.054088	4.815643
261.808146	8000.317668	13.870387	-0.054017	4.815636
261.973020	8000.317163	13.875392	-0.054047	4.815635
261.967428	8000.277557	13.880397	-0.054046	4.815623
262.140203	8000.243004	13.885402	-0.054079	4.815612
262.042222	8000.274515	13.890407	-0.054060	4.815622
262.013430	8000.164040	13.895411	-0.054055	4.815590
262.195805	8000.268489	13.900416	-0.054089	4.815620
262.064641	8000.334703	13.905421	-0.054065	4.815640
261.812843	8000.293210	13.910426	-0.054018	4.815629
262.110940	8000.284201	13.915431	-0.054073	4.815625
261.922220	8000.252283	13.920435	-0.054038	4.815616
262.130840	8000.290943	13.925440	-0.054077	4.815626
261.996042	8000.317580	13.930445	-0.054052	4.815635
261.992998	8000.245975	13.935450	-0.054052	4.815614
262.009093	8000.260126	13.940455	-0.054055	4.815618
261.901985	8000.204978	13.945459	-0.054035	4.815602
262.286003	8000.235823	13.950464	-0.054106	4.815610
262.250285	8000.255536	13.955469	-0.054100	4.815616
262.018689	8000.243210	13.960474	-0.054057	4.815613
262.199889	8000.361525	13.965479	-0.054090	4.815647
262.200015	8000.297447	13.970483	-0.054090	4.815628
262.340740	8000.370243	13.975488	-0.054117	4.815649
262.181050	8000.300349	13.980493	-0.054087	4.815629
262.044295	8000.309866	13.985498	-0.054062	4.815632
262.085689	8000.348996	13.990503	-0.054069	4.815644
262.100489	8000.284091	13.995507	-0.054072	4.815625
262.181795	8000.259790	14.000512	-0.054087	4.815617
262.098792	8000.346017	14.005517	-0.054072	4.815643
261.932423	8000.343301	14.010522	-0.054041	4.815643
262.159837	8000.371588	14.015527	-0.054083	4.815650
261.942664	8000.287938	14.020531	-0.054043	4.815626
261.988661	8000.291897	14.025536	-0.054052	4.815627
261.956666	8000.340508	14.030541	-0.054046	4.815642
261.933002	8000.284587	14.035546	-0.054041	4.815626
261.874852	8000.291116	14.040551	-0.054030	4.815628
261.664704	8000.296230	14.045555	-0.053991	4.815630
261.716988	8000.307768	14.050560	-0.054001	4.815633
261.683702	8000.306160	14.055565	-0.053995	4.815633
261.634058	8000.277583	14.060570	-0.053986	4.815625
261.763938	8000.357677	14.065575	-0.054010	4.815648
261.840907	8000.255339	14.070579	-0.054024	4.815617
261.796412	8000.274908	14.075584	-0.054016	4.815623
261.861590	8000.337924	14.080589	-0.054028	4.815641
261.660868	8000.262020	14.085594	-0.053991	4.815620
261.762485	8000.318154	14.090599	-0.054010	4.815636
261.749023	8000.244243	14.095603	-0.054007	4.815615
261.930955	8000.205567	14.100608	-0.054041	4.815602
261.991181	8000.290931	14.105613	-0.054053	4.815627
261.744765	8000.186511	14.110618	-0.054007	4.815598
261.878091	8000.239960	14.115623	-0.054032	4.815613
261.792221	8000.217199	14.120627	-0.054016	4.815606
261.742801	8000.229212	14.125632	-0.054007	4.815610
261.672084	8000.270781	14.130637	-0.053993	4.815623
261.706989	8000.210477	14.135642	-0.054000	4.815605
261.921424	8000.286612	14.140647	-0.054040	4.815626
261.876144	8000.268787	14.145651	-0.054032	4.815621
261.934670	8000.248387	14.150656	-0.054043	4.815615
262.066488	8000.291131	14.155661	-0.054067	4.815627
261.943085	8000.258144	14.160666	-0.054044	4.815618
261.748540	8000.296622	14.165671	-0.054008	4.815630
261.801535	8000.269723	14.170675	-0.054018	4.815622
261.969796	8000.259660	14.175680	-0.054049	4.815618
261.936967	8000.262331	14.180685	-0.054043	4.815619
262.114869	8000.259903	14.185690	-0.054076	4.815617
262.017610	8000.294630	14.190695	-0.054058	4.815628
261.951912	8000.317057	14.195699	-0.054046	4.815635
261.718553	8000.329267	14.200704	-0.054003	4.815640
261.973912	8000.270430	14.205709	-0.054050	4.815621
261.923609	8000.235435	14.210714	-0.054041	4.815611
262.025735	8000.280897	14.215719	-0.054060	4.815624
262.093209	8000.248895	14.220723	-0.054073	4.815614
261.671410	8000.260161	14.225728	-0.053994	4.815620
261.858679	8000.328376	14.230733	-0.054029	4.815639
261.831482	8000.256376	14.235738	-0.054024	4.815618
261.976649	8000.250208	14.240743	-0.054051	4.815615
261.859159	8000.211979	14.245747	-0.054029	4.815605
261.950222	8000.214539	14.250752	-0.054046	4.815605
261.898842	8000.337596	14.255757	-0.054037	4.815641
262.051303	8000.283485	14.260762	-0.054065	4.815625
262.140929	8000.322336	14.265767	-0.054082	4.815636
262.039909	8000.256605	14.270771	-0.054063	4.815617
262.280837	8000.256275	14.275776	-0.054108	4.815616
262.025114	8000.303365	14.280781	-0.054061	4.815631
261.728146	8000.255793	14.285786	-0.054005	4.815618
262.059890	7999.301075	14.290791	-0.054066	4.815337

261.949761	7996.066825	14.295795	-0.054044	4.814392
261.989882	7990.616351	14.300800	-0.054048	4.812798
262.067482	7983.941198	14.305805	-0.054058	4.810845
262.170796	7976.618560	14.310810	-0.054072	4.808702
261.846341	7969.027049	14.315815	-0.054007	4.806480
261.660385	7961.162145	14.320819	-0.053967	4.804177
261.871637	7953.397655	14.325824	-0.054002	4.801901
261.874902	7945.378179	14.330829	-0.053997	4.799549
261.831745	7937.440685	14.335834	-0.053984	4.797221
261.896552	7929.427828	14.340839	-0.053991	4.794869
261.769462	7921.458633	14.345843	-0.053962	4.792529
261.766694	7913.411229	14.350848	-0.053956	4.790165
261.828014	7905.399502	14.355853	-0.053963	4.787809
261.760414	7897.342157	14.360858	-0.053945	4.785440
261.794838	7889.432378	14.365863	-0.053946	4.783113
261.516144	7881.401354	14.370867	-0.053889	4.780750
261.531005	7873.362417	14.375872	-0.053887	4.778382
261.503000	7865.422237	14.380877	-0.053876	4.776042
261.380147	7857.365110	14.385882	-0.053848	4.773667
261.604847	7849.381010	14.390887	-0.053885	4.771312
261.400886	7841.330900	14.395891	-0.053842	4.768937
261.373609	7833.362118	14.400896	-0.053831	4.766584
261.564592	7825.348158	14.405901	-0.053862	4.764216
261.445926	7817.427363	14.410906	-0.053835	4.761875
261.193287	7809.415001	14.415911	-0.053782	4.759507
261.196598	7801.374868	14.420915	-0.053778	4.757128
261.324413	7793.391845	14.425920	-0.053796	4.754765
261.229541	7785.341762	14.430925	-0.053774	4.752381
260.893934	7777.261525	14.435930	-0.053706	4.749988
261.020461	7769.354718	14.440935	-0.053724	4.747644
261.074065	7761.294203	14.445939	-0.053729	4.745253
260.947892	7753.340007	14.450944	-0.053700	4.742893
260.848744	7745.329125	14.455949	-0.053677	4.740515
260.985643	7737.340427	14.460954	-0.053697	4.738142
261.055212	7729.337174	14.465959	-0.053705	4.735763
260.879006	7721.298826	14.470963	-0.053667	4.733374
261.089751	7713.304973	14.475968	-0.053701	4.730995
260.965984	7705.306745	14.480973	-0.053673	4.728615
260.731735	7697.294834	14.485978	-0.053624	4.726229
260.984573	7689.340599	14.490983	-0.053666	4.723859
260.919613	7681.292243	14.495987	-0.053649	4.721460
260.911883	7673.322798	14.500992	-0.053642	4.719083
260.693816	7665.380751	14.505997	-0.053596	4.716714
260.692138	7657.268886	14.511002	-0.053591	4.714292
260.746926	7649.319429	14.516007	-0.053596	4.711918
260.657993	7641.264247	14.521011	-0.053574	4.709511
260.914273	7633.329585	14.526016	-0.053617	4.707137
260.754432	7625.286257	14.531021	-0.053582	4.704732
260.583088	7617.303344	14.536026	-0.053545	4.702343
260.620420	7609.311406	14.541031	-0.053546	4.699949
260.769714	7601.374287	14.546035	-0.053569	4.697571
260.606483	7593.333944	14.551040	-0.053533	4.695161
260.506052	7585.300278	14.556045	-0.053510	4.692752
260.432501	7577.229344	14.561050	-0.053491	4.690330
260.450793	7569.295188	14.566055	-0.053489	4.687948
260.442054	7561.217362	14.571059	-0.053482	4.685522
260.333800	7553.285463	14.576064	-0.053457	4.683138
260.400015	7545.297339	14.581069	-0.053464	4.680736
260.358519	7537.274360	14.586074	-0.053451	4.678322
260.603633	7529.296366	14.591079	-0.053492	4.675921
260.590102	7521.240317	14.596083	-0.053484	4.673494
260.333705	7513.149031	14.601088	-0.053431	4.671057
260.247841	7505.160140	14.606093	-0.053410	4.668649
260.204370	7497.184903	14.611098	-0.053396	4.666243
260.194701	7489.260480	14.616103	-0.053390	4.663852
260.019935	7481.259912	14.621107	-0.053352	4.661436
260.184317	7473.241021	14.626112	-0.053377	4.659013
260.122487	7465.271947	14.631117	-0.053361	4.656605
260.170031	7457.206233	14.636122	-0.053364	4.654166
259.959092	7449.203790	14.641127	-0.053320	4.651744
259.923374	7441.191662	14.646131	-0.053308	4.649319
259.878895	7433.235238	14.651136	-0.053294	4.646909
259.890080	7425.205857	14.656141	-0.053291	4.644476
259.733237	7417.196783	14.661146	-0.053257	4.642047
259.866622	7409.231657	14.666151	-0.053277	4.639631
259.694610	7401.252592	14.671155	-0.053240	4.637209
259.660546	7393.224554	14.676160	-0.053228	4.634771
259.640637	7385.231600	14.681165	-0.053219	4.632343
259.506209	7377.135933	14.686170	-0.053189	4.629882
259.580626	7369.206985	14.691175	-0.053198	4.627470
259.614989	7361.149812	14.696179	-0.053199	4.625018
259.683365	7353.217887	14.701184	-0.053206	4.622603
259.551314	7345.198809	14.706189	-0.053177	4.620160
259.404797	7337.173787	14.711194	-0.053144	4.617714
259.643201	7329.211459	14.716199	-0.053183	4.615285
259.114682	7321.172498	14.721203	-0.053080	4.612832
259.604794	7313.152049	14.726208	-0.053166	4.610384
259.596378	7305.206423	14.731213	-0.053159	4.607957
259.428065	7297.143571	14.736218	-0.053123	4.605493
259.277764	7289.173895	14.741223	-0.053089	4.603056
259.292076	7281.142021	14.746227	-0.053087	4.600598
259.419911	7273.190771	14.751232	-0.053106	4.598164
259.432248	7265.199017	14.756237	-0.053103	4.595717
259.074685	7257.141851	14.761242	-0.053031	4.593247
259.181231	7249.112746	14.766247	-0.053046	4.590786
259.167944	7241.099349	14.771251	-0.053038	4.588327
259.265995	7233.124588	14.776256	-0.053051	4.585880
259.315981	7225.184661	14.781261	-0.053055	4.583442
259.215558	7217.126428	14.786266	-0.053031	4.580965
259.130322	7209.152761	14.791271	-0.053010	4.578514
259.070093	7201.137670	14.796275	-0.052994	4.576049
258.963880	7193.139246	14.801280	-0.052969	4.573587
258.773500	7185.078566	14.806285	-0.052928	4.571105
258.863950	7177.075033	14.811290	-0.052940	4.568639
258.936050	7169.119402	14.816295	-0.052948	4.566187
258.855737	7161.108923	14.821299	-0.052928	4.563716
258.837216	7153.161227	14.826304	-0.052919	4.561263
258.893668	7145.178071	14.831309	-0.052925	4.558798
258.981440	7137.175840	14.836314	-0.052936	4.556326
258.711845	7129.172549	14.841319	-0.052881	4.553852
258.686224	7121.135178	14.846323	-0.052871	4.551366
258.738680	7113.110894	14.851328	-0.052875	4.548883
258.804805	7105.111069	14.856333	-0.052882	4.546407
258.529611	7097.083210	14.861338	-0.052826	4.543919
258.764083	7089.136507	14.866343	-0.052864	4.541457
258.831758	7081.068203	14.871347	-0.052872	4.538955
258.727027	7073.140169	14.876352	-0.052847	4.536495
258.627445	7065.088774	14.881357	-0.052824	4.533995
258.475238	7057.087422	14.886362	-0.052790	4.531509
258.595381	7049.095741	14.891367	-0.052807	4.529026
258.492929	7041.122982	14.896371	-0.052783	4.526546
258.370363	7033.118668	14.901376	-0.052755	4.524055
258.436335	7025.147528	14.906381	-0.052762	4.521574
258.295282	7017.103128	14.911386	-0.052731	4.519068
258.368604	7009.157757	14.916391	-0.052739	4.516592
258.206206	7001.081444	14.921395	-0.052704	4.514073
258.150290	6993.046869	14.926400	-0.052688	4.511566
258.302352	6985.045074	14.931405	-0.052711	4.509069
258.138472	6977.055316	14.936410	-0.052676	4.506573
258.188407	6969.085194	14.941415	-0.052680	4.504082
257.966811	6961.095908	14.946419	-0.052633	4.501583
258.052718	6953.050528	14.951424	-0.052644	4.499066
257.929286	6945.106265	14.956429	-0.052616	4.496579
257.855778	6937.030468	14.961434	-0.052597	4.494049
257.970724	6929.049071	14.966439	-0.052613	4.491548
257.929088	6921.028824	14.971443	-0.052600	4.489033
257.827705	6913.072383	14.976448	-0.052576	4.486536
257.894923	6905.052093	14.981453	-0.052584	4.484019
257.772349	6897.079988	14.986458	-0.052556	4.481514
257.992153	6889.050192	14.991463	-0.052591	4.478991
257.798118	6881.075936	14.996467	-0.052550	4.476483
257.896651	6873.015740	15.001472	-0.052563	4.473947
257.939896	6865.055876	15.006477	-0.052566	4.471442
257.644339	6857.015121	15.011482	-0.052506	4.468908
257.764490	6849.043586	15.016487	-0.052523	4.466396
257.662732	6841.014762	15.021491	-0.052499	4.463864
257.640833	6833.029158	15.026496	-0.052490	4.461344
257.752812	6825.072167	15.031501	-0.052506	4.458832
257.760751	6817.012216	15.036506	-0.052502	4.456286
257.680717	6809.056723	15.041511	-0.052482	4.453771
257.520686	6800.985386	15.046515	-0.052447	4.451218
257.799035	6793.025554	15.051520	-0.052493	4.448701
257.634816	6784.998028	15.056525	-0.052458	4.446158
257.538021	6777.010727	15.061530	-0.052434	4.443628
257.614844	6769.015841	15.066535	-0.052444	4.441094
257.595737	6761.025820	15.071539	-0.052435	4.438560
257.404768	6753.021118	15.076544	-0.052394	4.436019
257.322674	6745.025456	15.081549	-0.052374	4.433480
257.272564	6736.933755	15.086554	-0.052359	4.430909
257.215673	6728.975496	15.091559	-0.052343	4.428379
257.218311	6720.963051	15.096563	-0.052339	4.425830
257.190576	6712.983138	15.101568	-0.052328	4.423290
257.254460	6705.017234	15.106573	-0.052335	4.420754
257.023600	6696.980037	15.111578	-0.052287	4.418192
257.279284	6688.991024	15.116583	-0.052329	4.415646
257.039922	6680.987819	15.121587	-0.052280	4.413092
256.973464	6672.948487	15.126592	-0.052262	4.410526
256.824329	6664.982622	15.131597	-0.052229	4.407981
257.014353	6656.935851	15.136602	-0.052259	4.405411
257.214002	6648.983358	15.141607	-0.052291	4.402869
257.058330	6640.991510	15.146611	-0.052257	4.400312
256.961943	6633.037512	15.151616	-0.052234	4.397765
256.829955	6625.007890	15.156621	-0.052204	4.395193
256.772241	6616.977863	15.161626	-0.052188	4.392619
256.755995	6608.971320	15.166631	-0.052180	4.390051
256.925433	6600.982760	15.171635	-0.052207	4.387489
256.882417	6592.967572	15.176640	-0.052193	4.384916
256.942250	6584.991222	15.181645	-0.052199	4.382354
256.639335	6576.927040	15.186650	-0.052138	4.379760
256.781234	6569.051778	15.191655	-0.052159	4.377228
256.741434	6561.001073	15.196659	-0.052147	4.374637
256.841735	6552.997133	15.201664	-0.052160	4.372060
256.947327	6544.963875	15.206669	-0.052174	4.369473
256.694475	6536.997358	15.211674	-0.052122	4.366903
256.759542	6528.992750	15.216679	-0.052129	4.364322
256.882963	6521.052646	15.221683	-0.052147	4.361760
256.675328	6512.989334	15.226688	-0.052103	4.359154
256.453242	6505.050020	15.231693	-0.052057	4.356587
256.264811	6496.956502	15.236698	-0.052016	4.353969
256.242257	6488.888697	15.241703	-0.052007	4.351359
256.193068	6480.900532	15.246707	-0.051993	4.348773
256.172604	6472.916555	15.251712	-0.051984	4.346187
256.382298	6464.938334	15.256717	-0.052018	4.343602
256.178830	6456.949403	15.261722	-0.051974	4.341010
256.208476	6448.982514	15.266727	-0.051975	4.338425
256.240596	6440.967449	15.271731	-0.051976	4.335823
256.218491	6432.928579	15.276736	-0.051966	4.333211
256.335647	6424.952027	15.281741	-0.051983	4.330619
256.224305	6416.959324	15.286746	-0.051957	4.328018
256.252857	6408.923307	15.291751	-0.051957	4.325403
256.032584	6400.975336	15.296755	-0.051911	4.322813
255.976616	6392.977758	15.301760	-0.051895	4.320206
256.115227	6384.956682	15.306765	-0.051916	4.317592
256.028022	6376.954205	15.311770	-0.051895	4.314980
256.073449	6368.924867	15.316775	-0.051898	4.312359
256.099219	6360.882705	15.321779	-0.051898	4.309732
255.899153	6352.947196	15.326784	-0.051855	4.307137
255.743388	6344.966839	15.331789	-0.051821	4.304526
255.709695	6336.930301	15.336794	-0.051810	4.301896
255.899724	6328.941918	15.341799	-0.051840	4.299281
255.798456	6320.937777	15.346803	-0.051816	4.296658
255.819629	6312.944143	15.351808	-0.051815	4.294037
255.857394	6304.925487	15.356813	-0.051816	4.291407
255.498547	6296.913047	15.361818	-0.051744	4.288774
255.516922	6288.962737	15.366823	-0.051743	4.286163
255.421605	6280.905243	15.371827	-0.051720	4.283514
255.372003	6272.922791	15.376832	-0.051705	4.280888
255.534878	6264.953094	15.381837	-0.051730	4.278267
255.274429	6256.889211	15.386842	-0.051677	4.275609
255.306598	6248.890092	15.391847	-0.051678	4.272974
255.080849	6240.912134	15.396851	-0.051630	4.270342
255.226276	6232.912356	15.401856	-0.051652	4.267704
255.256430	6224.867594	15.406861	-0.051653	4.265049
255.108264	6216.924274	15.411866	-0.051620	4.262424
255.241900	6208.880096	15.416871	-0.051640	4.259766
255.235053	6200.935310	15.421875	-0.051633	4.257139
254.980692	6192.906018	15.426880	-0.051581	4.254480
254.966652	6184.905389	15.431885	-0.051573	4.251830
255.040772	6176.844200	15.436890	-0.051582	4.249160
255.075820	6168.913410	15.441895	-0.051583	4.246531
255.076998	6160.876526	15.446899	-0.051578	4.243865
254.855565	6152.990160	15.451904	-0.051532	4.241245
254.975651	6144.925186	15.456909	-0.051549	4.238567
254.957809	6136.925573	15.461914	-0.051540	4.235908
254.852907	6128.926949	15.466919	-0.051516	4.233247
254.886266	6120.902179	15.471923	-0.051517	4.230577
255.047744	6112.867467	15.476928	-0.051541	4.227903
254.793000	6104.939983	15.481933	-0.051489	4.225259
254.940746	6096.898904	15.486938	-0.051511	4.222579
254.996495	6088.959174	15.491943	-0.051516	4.219931
254.931499	6080.951388	15.496947	-0.051499	4.217257
254.679271	6072.926358	15.501952	-0.051447	4.214573
254.973148	6064.908575	15.506957	-0.051497	4.211896
254.897748	6056.901508	15.511962	-0.051477	4.209217
254.697139	6048.978974	15.516967	-0.051435	4.206563
254.692964	6040.937075	15.521971	-0.051429	4.203870
254.657444	6032.958128	15.526976	-0.051417	4.201196
254.464542	6024.966896	15.531981	-0.051376	4.198514
254.356274	6016.927023	15.536986	-0.051351	4.195815
254.625592	6008.852468	15.541991	-0.051396	4.193107
254.697104	6000.840453	15.546995	-0.051404	4.190415
254.576317	5992.859256	15.552000	-0.051376	4.187731
254.376832	5984.884856	15.557005	-0.051334	4.185046
254.326196	5976.928424	15.562010	-0.051319	4.182367
254.172224	5968.892489	15.567015	-0.051285	4.179658
254.248445	5960.927384	15.572019	-0.051294	4.176974
254.189679	5952.920964	15.577024	-0.051278	4.174273
254.407112	5944.887418	15.582029	-0.051314	4.171564
254.338055	5936.894505	15.587034	-0.051296	4.168864
254.363643	5928.911922	15.592039	-0.051295	4.166167
254.060477	5920.904142	15.597043	-0.051234	4.163455
254.029802	5912.903468	15.602048	-0.051223	4.160747
254.281028	5904.923225	15.607053	-0.051264	4.158048
254.191109	5896.895376	15.612058	-0.051242	4.155327
254.200815	5888.914474	15.617063	-0.051239	4.152621
254.110693	5880.876953	15.622067	-0.051217	4.149893
254.131308	5872.900625	15.627072	-0.051216	4.147185
254.115854	5864.877495	15.632077	-0.051208	4.144460
254.024476	5856.922029	15.637082	-0.051186	4.141754
254.078105	5848.914332	15.642087	-0.051190	4.139031
254.092681	5840.896789	15.647091	-0.051188	4.136302
253.845098	5832.892169	15.652096	-0.051137	4.133572
253.635371	5824.865018	15.657101	-0.051092	4.130834
253.656632	5816.876034	15.662106	-0.051091	4.128109
253.659010	5808.900331	15.667111	-0.051086	4.125387
253.599824	5800.916633	15.672115	-0.051070	4.122660
253.670284	5792.875912	15.677120	-0.051078	4.119912
253.823093	5784.945152	15.682125	-0.051101	4.117202
253.486460	5776.888320	15.687130	-0.051034	4.114441
253.501852	5768.884854	15.692135	-0.051031	4.111700
253.642496	5760.859216	15.697139	-0.051052	4.108952
253.629327	5752.842016	15.702144	-0.051045	4.106203
253.569924	5744.882902	15.707149	-0.051028	4.103471
253.365720	5736.901960	15.712154	-0.050985	4.100728
253.536172	5728.952859	15.717159	-0.051012	4.097999
253.304341	5720.923841	15.722163	-0.050964	4.095236
253.270309	5712.871769	15.727168	-0.050952	4.092465
253.110469	5704.895371	15.732173	-0.050917	4.089716
253.084063	5696.910094	15.737178	-0.050907	4.086965
253.328404	5688.876042	15.742183	-0.050947	4.084199
253.187808	5680.970306	15.747187	-0.050916	4.081469
252.943901	5672.948387	15.752192	-0.050865	4.078697
253.048590	5664.985791	15.757197	-0.050880	4.075947
253.130952	5656.897618	15.762202	-0.050890	4.073153
253.061641	5648.917657	15.767207	-0.050872	4.070391
253.122409	5640.936043	15.772211	-0.050878	4.067629
253.143295	5632.904704	15.777216	-0.050877	4.064848
253.246128	5624.970930	15.782221	-0.050891	4.062099
253.114625	5616.922609	15.787226	-0.050861	4.059305
253.204859	5608.973186	15.792231	-0.050873	4.056547
253.161022	5600.952965	15.797235	-0.050859	4.053761
252.919623	5592.917829	15.802240	-0.050809	4.050965
253.086198	5584.953725	15.807245	-0.050835	4.048197
252.886876	5576.940539	15.812250	-0.050793	4.045405
252.842895	5568.938921	15.817255	-0.050779	4.042617
252.624816	5560.962813	15.822259	-0.050734	4.039834
252.599629	5552.950923	15.827264	-0.050724	4.037039
252.635009	5544.940203	15.832269	-0.050725	4.034244
252.550903	5536.838332	15.837274	-0.050704	4.031413
252.688434	5528.863823	15.842279	-0.050725	4.028628
252.707542	5520.868716	15.847283	-0.050723	4.025832
252.399574	5512.915794	15.852288	-0.050661	4.023043
252.527082	5504.930633	15.857293	-0.050679	4.020248
252.247331	5496.917345	15.862298	-0.050622	4.017436
252.500512	5488.895020	15.867303	-0.050664	4.014626
252.245598	5480.896433	15.872307	-0.050611	4.011814
252.241167	5472.882570	15.877312	-0.050605	4.009000
252.234676	5464.941032	15.882317	-0.050599	4.006208
252.090250	5456.917217	15.887322	-0.050567	4.003384
251.980161	5448.925948	15.892327	-0.050541	4.000569
252.196974	5440.942291	15.897331	-0.050576	3.997761
252.002745	5432.933390	15.902336	-0.050535	3.994935
252.225374	5424.904891	15.907341	-0.050571	3.992106
252.030130	5416.864148	15.912346	-0.050530	3.989265
252.199928	5408.929814	15.917351	-0.050556	3.986465
251.990051	5400.908296	15.922355	-0.050512	3.983626
251.904535	5392.924718	15.927360	-0.050491	3.980801
252.026605	5384.966203	15.932365	-0.050508	3.977986
251.893639	5376.961861	15.937370	-0.050479	3.975148
251.835502	5368.925421	15.942375	-0.050463	3.972299
251.922595	5360.915153	15.947379	-0.050474	3.969458
251.928960	5352.938175	15.952384	-0.050470	3.966627
251.725404	5344.959383	15.957389	-0.050427	3.963789
251.587225	5336.977109	15.962394	-0.050396	3.960949
251.812173	5328.982213	15.967399	-0.050432	3.958108
251.775982	5320.970564	15.972403	-0.050420	3.955256
251.491864	5312.939994	15.977408	-0.050362	3.952390
251.577933	5304.930549	15.982413	-0.050373	3.949535
251.390696	5296.937649	15.987418	-0.050333	3.946680
251.436770	5288.947868	15.992423	-0.050337	3.943828
251.216961	5281.009318	15.997427	-0.050291	3.940988
251.466779	5272.974726	16.002432	-0.050332	3.938120
251.365373	5265.017466	16.007437	-0.050308	3.935270
251.357294	5256.968096	16.012442	-0.050301	3.932388
251.355046	5248.967020	16.017447	-0.050296	3.929521
251.184454	5241.023790	16.022451	-0.050259	3.926669
251.164894	5232.976152	16.027456	-0.050250	3.923780
251.280660	5225.022299	16.032461	-0.050266	3.920926
251.212040	5217.001974	16.037466	-0.050248	3.918042
251.112589	5209.017802	16.042471	-0.050225	3.915169
251.307802	5200.985382	16.047475	-0.050256	3.912281
251.275815	5192.962737	16.052480	-0.050245	3.909391
251.146696	5185.011678	16.057485	-0.050215	3.906522
251.129731	5176.963798	16.062490	-0.050207	3.903619
251.240163	5168.992215	16.067495	-0.050222	3.900743
251.201989	5161.000559	16.072499	-0.050210	3.897855
250.915360	5153.028766	16.077504	-0.050152	3.894968
250.830064	5145.004955	16.082509	-0.050131	3.892063
251.040327	5136.968948	16.087514	-0.050165	3.889157
250.836863	5129.001321	16.092519	-0.050121	3.886266
250.951037	5120.993520	16.097523	-0.050138	3.883365
250.824696	5112.989913	16.102528	-0.050109	3.880458
250.932791	5105.057114	16.107533	-0.050124	3.877579
250.672426	5097.006622	16.112538	-0.050070	3.874648
250.886606	5088.757342	16.117543	-0.050105	3.871652
250.714672	5080.845694	16.122547	-0.050068	3.868769
250.454534	5072.895138	16.127552	-0.050014	3.865868
250.529843	5064.973421	16.132557	-0.050023	3.862981
250.746900	5056.927492	16.137562	-0.050058	3.860050
250.734046	5049.022483	16.142567	-0.050051	3.857164
250.448976	5041.001777	16.147571	-0.049992	3.854228
250.559166	5032.972225	16.152576	-0.050008	3.851294
250.468114	5024.998327	16.157581	-0.049986	3.848374
250.124520	5017.029285	16.162586	-0.049916	3.845449
250.373744	5009.029843	16.167591	-0.049958	3.842523
250.366659	5001.003153	16.172595	-0.049951	3.839578
250.216307	4993.070635	16.177600	-0.049918	3.836664
250.208242	4985.062246	16.182605	-0.049911	3.833722
250.264301	4977.026659	16.187610	-0.049917	3.830769
250.211193	4969.065398	16.192615	-0.049902	3.827839
249.995917	4961.059352	16.197619	-0.049856	3.824887
250.261115	4953.061663	16.202624	-0.049901	3.821946
250.177341	4945.104501	16.207629	-0.049880	3.819010
250.045636	4937.098762	16.212634	-0.049850	3.816053
250.112020	4929.047252	16.217639	-0.049857	3.813080
250.158763	4921.038602	16.222643	-0.049861	3.810121
249.993634	4913.076364	16.227648	-0.049825	3.807173
250.029615	4905.088367	16.232653	-0.049826	3.804216
249.884132	4897.112172	16.237658	-0.049794	3.801258
249.835479	4889.120558	16.242663	-0.049780	3.798294
249.927513	4881.121005	16.247667	-0.049792	3.795328
249.759264	4873.054867	16.252672	-0.049755	3.792329
249.816776	4865.045575	16.257677	-0.049761	3.789354
249.636631	4857.107088	16.262682	-0.049722	3.786397
249.642537	4849.089124	16.267687	-0.049718	3.783413
249.796323	4841.111330	16.272691	-0.049742	3.780445
249.535829	4833.082677	16.277696	-0.049688	3.777446
249.493505	4825.101696	16.282701	-0.049675	3.774467
249.522158	4817.089303	16.287706	-0.049675	3.771476
249.598532	4809.065324	16.292711	-0.049684	3.768479
249.454881	4801.112035	16.297715	-0.049652	3.765501
249.375023	4793.121177	16.302720	-0.049632	3.762508
249.562380	4785.110304	16.307725	-0.049662	3.759512
249.511613	4777.108764	16.312730	-0.049647	3.756511
249.437290	4769.093477	16.317735	-0.049628	3.753502
249.627518	4761.078222	16.322739	-0.049658	3.750497
249.599327	4753.048855	16.327744	-0.049648	3.747479
249.582088	4745.086695	16.332749	-0.049640	3.744484
249.379840	4737.160739	16.337754	-0.049597	3.741496
249.354222	4729.129878	16.342759	-0.049587	3.738470
249.224948	4721.163387	16.347763	-0.049558	3.735463
249.139009	4713.158452	16.352768	-0.049537	3.732441
249.272172	4705.144507	16.357773	-0.049556	3.729418
249.189965	4697.188683	16.362778	-0.049536	3.726409
249.048468	4689.173799	16.367783	-0.049504	3.723374
249.154307	4681.159594	16.372787	-0.049519	3.720343
249.100279	4673.184376	16.377792	-0.049504	3.717321
249.016524	4665.214294	16.382797	-0.049483	3.714297
248.954884	4657.085665	16.387802	-0.049466	3.711210
248.878408	4649.124200	16.392807	-0.049447	3.708185
248.704609	4641.154244	16.397811	-0.049409	3.705151
248.716265	4633.155032	16.402816	-0.049406	3.702109
248.711621	4625.194610	16.407821	-0.049400	3.699078
248.580144	4617.213810	16.412826	-0.049370	3.696033
248.584214	4609.211105	16.417831	-0.049366	3.692982
248.557279	4601.204798	16.422835	-0.049356	3.689925
248.521067	4593.206572	16.427840	-0.049344	3.686869
248.758835	4585.209088	16.432845	-0.049383	3.683818
248.660532	4577.248624	16.437850	-0.049360	3.680769
248.783465	4569.275982	16.442855	-0.049377	3.677719
248.648869	4561.257910	16.447859	-0.049347	3.674643
248.539825	4553.200158	16.452864	-0.049322	3.671549
248.677039	4545.218860	16.457869	-0.049342	3.668489
248.364707	4537.240369	16.462874	-0.049279	3.665415
248.276477	4529.283585	16.467879	-0.049257	3.662353
248.429482	4521.229570	16.472883	-0.049280	3.659258
248.251046	4513.281816	16.477888	-0.049242	3.656191
248.231805	4505.262769	16.482893	-0.049233	3.653099
248.126156	4497.230556	16.487898	-0.049208	3.649997
248.298550	4489.258072	16.492903	-0.049235	3.646923
248.387906	4481.230130	16.497907	-0.049247	3.643823
248.184459	4473.272746	16.502912	-0.049204	3.640739
248.346710	4465.308995	16.507917	-0.049229	3.637660
248.230646	4457.310824	16.512922	-0.049202	3.634558
248.196738	4449.260717	16.517927	-0.049191	3.631435
248.187033	4441.264106	16.522931	-0.049184	3.628331
248.093920	4433.227970	16.527936	-0.049161	3.625206
248.012983	4425.313527	16.532941	-0.049141	3.622127
247.959501	4417.286849	16.537946	-0.049126	3.619001
248.014368	4409.314775	16.542951	-0.049131	3.615898
247.778725	4401.326843	16.547955	-0.049082	3.612777
247.614520	4393.295270	16.552960	-0.049046	3.609639
247.897812	4385.367599	16.557965	-0.049094	3.606551
247.731774	4377.350883	16.562970	-0.049057	3.603413
247.740336	4369.359860	16.567975	-0.049054	3.600288
247.864288	4361.395404	16.572979	-0.049072	3.597173
247.649420	4353.362606	16.577984	-0.049027	3.594019
247.400764	4345.379975	16.582989	-0.048975	3.590881
247.459505	4337.363941	16.587994	-0.048981	3.587736
247.565919	4329.342724	16.592999	-0.048996	3.584587
247.576115	4321.401368	16.598003	-0.048992	3.581465
247.450837	4313.400693	16.603008	-0.048964	3.578312
247.455570	4305.448333	16.608013	-0.048960	3.575179
247.367193	4297.413998	16.613018	-0.048938	3.572009
247.518680	4289.381882	16.618023	-0.048961	3.568844
247.570690	4281.402865	16.623027	-0.048965	3.565694
247.459547	4273.420822	16.628032	-0.048940	3.562535
247.471834	4265.435991	16.633037	-0.048937	3.559376
247.355542	4257.480396	16.638042	-0.048910	3.556221
247.323773	4249.387863	16.643047	-0.048899	3.553013
247.242388	4241.354339	16.648051	-0.048878	3.549823
247.028867	4233.385894	16.653056	-0.048834	3.546652
247.138125	4225.405188	16.658061	-0.048849	3.543483
247.008820	4217.455000	16.663066	-0.048820	3.540317
247.141895	4209.466354	16.668071	-0.048839	3.537140
246.992685	4201.469355	16.673075	-0.048806	3.533948
246.991484	4193.416031	16.678080	-0.048801	3.530736
247.189728	4185.438525	16.683085	-0.048832	3.527556
246.862382	4177.460507	16.688090	-0.048766	3.524358
247.037091	4169.485112	16.693095	-0.048794	3.521174
246.882504	4161.497627	16.698099	-0.048760	3.517971
246.622542	4153.519344	16.703104	-0.048706	3.514766
246.775251	4145.497276	16.708109	-0.048730	3.511553
246.721229	4137.482878	16.713114	-0.048714	3.508334
246.638348	4129.487415	16.718119	-0.048694	3.505119
246.608029	4121.527070	16.723123	-0.048683	3.501916
246.571505	4113.521021	16.728128	-0.048671	3.498692
246.568463	4105.559264	16.733133	-0.048665	3.495484
246.663451	4097.516701	16.738138	-0.048678	3.492243
246.609843	4089.541121	16.743143	-0.048663	3.489022
246.721295	4081.570028	16.748147	-0.048678	3.485805
246.573051	4073.574202	16.753152	-0.048645	3.482566
246.597816	4065.594603	16.758157	-0.048645	3.479337
246.432761	4057.641258	16.763162	-0.048609	3.476109
246.544606	4049.602657	16.768167	-0.048625	3.472852
246.482391	4041.563849	16.773171	-0.048608	3.469587
246.289616	4033.573755	16.778176	-0.048567	3.466334
246.547340	4025.608246	16.783181	-0.048610	3.463103
246.271983	4017.604549	16.788186	-0.048553	3.459836
246.255480	4009.641394	16.793191	-0.048545	3.456591
246.224686	4001.644798	16.798195	-0.048534	3.453328
246.129380	3993.599063	16.803200	-0.048511	3.450040
246.041805	3985.649768	16.808205	-0.048490	3.446789
245.909268	3977.649862	16.813210	-0.048460	3.443512
245.974612	3969.656060	16.818215	-0.048467	3.440242
246.046813	3961.679175	16.823219	-0.048475	3.436975
245.774631	3953.681632	16.828224	-0.048419	3.433686
245.904817	3945.649878	16.833229	-0.048438	3.430392
245.869666	3937.670456	16.838234	-0.048427	3.427112
245.922733	3929.658835	16.843239	-0.048431	3.423818
245.849924	3921.727406	16.848243	-0.048413	3.420549
245.730978	3913.721851	16.853248	-0.048385	3.417245
245.839148	3905.722713	16.858253	-0.048400	3.413949
245.914323	3897.696965	16.863258	-0.048409	3.410637
245.895774	3889.727532	16.868263	-0.048400	3.407342
245.772740	3881.751899	16.873267	-0.048372	3.404038
245.806391	3873.763459	16.878272	-0.048373	3.400730
245.703099	3865.821333	16.883277	-0.048349	3.397434
245.525479	3857.782664	16.888282	-0.048311	3.394092
245.488931	3849.686058	16.893287	-0.048299	3.390727
245.725690	3841.722325	16.898291	-0.048338	3.387424
245.554577	3833.710726	16.903296	-0.048301	3.384084
245.264466	3825.820554	16.908301	-0.048242	3.380786
245.400814	3817.832459	16.913306	-0.048262	3.377460
245.428892	3809.804568	16.918311	-0.048262	3.374110
245.249154	3801.817285	16.923315	-0.048223	3.370766
244.978085	3793.845817	16.928320	-0.048168	3.367422
245.243434	3785.820087	16.933325	-0.048212	3.364071
245.216953	3777.878643	16.938330	-0.048202	3.360742
245.182625	3769.881049	16.943335	-0.048190	3.357385
245.161291	3761.876236	16.948339	-0.048181	3.354023
245.014292	3753.853945	16.953344	-0.048148	3.350645
245.049528	3745.876693	16.958349	-0.048150	3.347290
245.042112	3737.892608	16.963354	-0.048143	3.343926
244.727981	3729.918811	16.968359	-0.048080	3.340553
244.763463	3721.946413	16.973363	-0.048081	3.337189
244.765531	3713.924397	16.978368	-0.048076	3.333800
244.766282	3705.912133	16.983373	-0.048071	3.330411
244.825202	3697.912507	16.988378	-0.048077	3.327026
244.720550	3689.947159	16.993383	-0.048052	3.323647
244.648479	3681.969442	16.998387	-0.048034	3.320260
244.487828	3674.000378	17.003392	-0.047999	3.316870
244.540001	3665.997219	17.008397	-0.048003	3.313469
244.636161	3657.956556	17.013402	-0.048016	3.310052
244.552356	3649.978243	17.018407	-0.047995	3.306650
244.496095	3642.026952	17.023411	-0.047980	3.303257
244.613236	3634.009900	17.028416	-0.047996	3.299839
244.344047	3626.085321	17.033421	-0.047941	3.296443
244.328972	3618.066014	17.038426	-0.047933	3.293012
244.260945	3610.040887	17.043431	-0.047915	3.289573
244.417322	3602.056396	17.048435	-0.047939	3.286157
244.190990	3594.087764	17.053440	-0.047892	3.282729
244.220999	3586.092038	17.058445	-0.047892	3.279296
244.166209	3578.147193	17.063450	-0.047877	3.275877
244.142418	3570.103465	17.068455	-0.047867	3.272414
244.062743	3562.105217	17.073459	-0.047847	3.268965
244.003229	3554.095530	17.078464	-0.047831	3.265507
244.177801	3546.122103	17.083469	-0.047858	3.262071
243.943051	3538.148285	17.088474	-0.047810	3.258615
243.889413	3530.166422	17.093479	-0.047794	3.255159
243.931779	3522.165507	17.098483	-0.047797	3.251695
243.947179	3514.159757	17.103488	-0.047795	3.248224
243.940516	3506.184723	17.108493	-0.047788	3.244762
243.915254	3498.224239	17.113498	-0.047779	3.241301
244.083723	3490.220593	17.118503	-0.047805	3.237826
244.042570	3482.227031	17.123507	-0.047792	3.234343
243.900472	3474.174208	17.128512	-0.047760	3.230827
243.867369	3466.200840	17.133517	-0.047749	3.227345
243.800174	3458.200005	17.138522	-0.047731	3.223847
243.539788	3450.275218	17.143527	-0.047678	3.220370
243.687112	3442.302307	17.148531	-0.047700	3.216885
243.685239	3434.253776	17.153536	-0.047694	3.213357
243.635392	3426.259140	17.158541	-0.047680	3.209846
243.760480	3418.299366	17.163546	-0.047698	3.206354
243.625048	3410.318238	17.168551	-0.047668	3.202839
243.602107	3402.375668	17.173555	-0.047658	3.199341
243.480557	3394.380379	17.178560	-0.047631	3.195812
243.489870	3386.354649	17.183565	-0.047627	3.192271
243.347491	3378.352301	17.188570	-0.047595	3.188730
243.263327	3370.349114	17.193575	-0.047575	3.185187
243.343943	3362.408153	17.198579	-0.047584	3.181675
243.313656	3354.401390	17.203584	-0.047574	3.178125
243.303898	3346.427635	17.208589	-0.047567	3.174586
243.100359	3338.436505	17.213594	-0.047524	3.171028
243.220772	3330.435082	17.218599	-0.047541	3.167475
243.159585	3322.461560	17.223603	-0.047524	3.163922
243.199952	3314.478077	17.228608	-0.047527	3.160366
243.187482	3306.507999	17.233613	-0.047519	3.156809
243.130169	3298.498196	17.238618	-0.047503	3.153228
243.098460	3290.463628	17.243623	-0.047492	3.149633
243.160274	3282.482769	17.248627	-0.047499	3.146063
243.033477	3274.512015	17.253632	-0.047470	3.142484
242.982312	3266.556889	17.258637	-0.047455	3.138912
242.819332	3258.587119	17.263642	-0.047420	3.135324
242.940118	3250.554197	17.268647	-0.047437	3.131716
242.951763	3242.565501	17.273651	-0.047434	3.128120
242.649733	3234.592796	17.278656	-0.047373	3.124512
242.819215	3226.658762	17.283661	-0.047399	3.120938
242.906640	3218.636235	17.288666	-0.047410	3.117317
242.568835	3210.674955	17.293671	-0.047342	3.113700
242.513748	3202.650135	17.298675	-0.047327	3.110063
242.670923	3194.639677	17.303680	-0.047351	3.106438
242.605096	3186.682117	17.308685	-0.047333	3.102822
242.525124	3178.686547	17.313690	-0.047313	3.099185
242.548702	3170.716745	17.318695	-0.047312	3.095559
242.361783	3162.745270	17.323699	-0.047273	3.091919
242.417225	3154.698640	17.328704	-0.047278	3.088251
242.573239	3146.727905	17.333709	-0.047302	3.084618
242.526876	3138.778100	17.338714	-0.047288	3.080981
242.287269	3130.807549	17.343719	-0.047238	3.077322
242.116783	3122.811666	17.348723	-0.047201	3.073649
242.115785	3114.715012	17.353728	-0.047196	3.069934
242.106168	3106.753329	17.358733	-0.047189	3.066276
242.156636	3098.795691	17.363738	-0.047193	3.062618
242.229086	3090.814796	17.368743	-0.047201	3.058947
242.267555	3082.857086	17.373747	-0.047203	3.055280
241.988539	3074.858407	17.378752	-0.047146	3.051574
242.007734	3066.883435	17.383757	-0.047145	3.047889
242.025786	3058.883156	17.388762	-0.047143	3.044188
241.953403	3050.927537	17.393767	-0.047124	3.040499
242.173459	3042.975546	17.398771	-0.047160	3.036821
241.915124	3034.973874	17.403776	-0.047107	3.033092
241.880332	3026.951560	17.408781	-0.047095	3.029360
241.761914	3018.974667	17.413786	-0.047068	3.025640
241.803692	3010.992271	17.418791	-0.047071	3.021922
241.796945	3003.041467	17.423795	-0.047064	3.018210
241.507217	2995.056633	17.428800	-0.047005	3.014465
241.681094	2987.049911	17.433805	-0.047032	3.010727
241.883750	2979.054015	17.438810	-0.047065	3.006992
241.593522	2971.092576	17.443815	-0.047006	3.003243
241.462749	2963.142347	17.448819	-0.046976	2.999503
241.576007	2955.141811	17.453824	-0.046992	2.995746
241.723266	2947.127773	17.458829	-0.047014	2.991981
241.472234	2939.127604	17.463834	-0.046962	2.988197
241.560753	2931.129385	17.468839	-0.046974	2.984426
241.557960	2923.193862	17.473843	-0.046968	2.980676
241.296049	2915.210906	17.478848	-0.046914	2.976885
241.275890	2907.229549	17.483853	-0.046905	2.973102
241.358838	2899.213787	17.488858	-0.046915	2.969304
241.230302	2891.253246	17.493863	-0.046886	2.965516
241.188813	2883.310650	17.498867	-0.046873	2.961736
241.072398	2875.315524	17.503872	-0.046847	2.957922
241.207191	2867.314814	17.508877	-0.046867	2.954114
241.013974	2859.323834	17.513882	-0.046825	2.950289
240.974505	2851.343003	17.518887	-0.046813	2.946471
241.071463	2843.366223	17.523891	-0.046826	2.942658
241.081586	2835.363599	17.528896	-0.046823	2.938822
240.930255	2827.418880	17.533901	-0.046789	2.935001
240.977121	2819.397423	17.538906	-0.046793	2.931149
240.985766	2811.427616	17.543911	-0.046789	2.927314
240.904989	2803.459897	17.548915	-0.046769	2.923470
240.678868	2795.475941	17.553920	-0.046722	2.919606
240.818155	2787.538782	17.558925	-0.046743	2.915779
240.778554	2779.468469	17.563930	-0.046730	2.911873
240.624129	2771.457073	17.568935	-0.046696	2.907984
240.485172	2763.502368	17.573939	-0.046665	2.904118
240.232143	2755.571576	17.578944	-0.046613	2.900252
240.250124	2747.599043	17.583949	-0.046611	2.896376
240.310549	2739.595954	17.588954	-0.046617	2.892481
240.400510	2731.574739	17.593959	-0.046629	2.888574
240.288647	2723.626397	17.598963	-0.046603	2.884687
240.203892	2715.650079	17.603968	-0.046582	2.880782
240.345016	2707.689347	17.608973	-0.046603	2.876891
240.326321	2699.686555	17.613978	-0.046594	2.872966
240.476272	2691.681533	17.618983	-0.046617	2.869044
240.436782	2683.706736	17.623987	-0.046604	2.865121
240.372884	2675.759567	17.628992	-0.046587	2.861205
240.350446	2667.785738	17.633997	-0.046578	2.857272
240.293052	2659.799037	17.639002	-0.046562	2.853326
240.219390	2651.804429	17.644007	-0.046543	2.849370
240.143379	2643.852110	17.649011	-0.046524	2.845428
240.043084	2635.892208	17.654016	-0.046500	2.841477
239.978340	2627.931853	17.659021	-0.046483	2.837521
239.863040	2619.932535	17.664026	-0.046456	2.833538
239.750526	2611.907864	17.669031	-0.046430	2.829536
239.865558	2603.939340	17.674035	-0.046447	2.825570
239.811372	2595.964424	17.679040	-0.046431	2.821585
239.689160	2588.001107	17.684045	-0.046403	2.817597
239.753253	2580.005322	17.689050	-0.046410	2.813597
239.842945	2571.986195	17.694055	-0.046422	2.809582
239.661888	2564.053768	17.699059	-0.046383	2.805589
239.467447	2556.120627	17.704064	-0.046341	2.801588
239.486299	2548.146404	17.709069	-0.046340	2.797574
239.605009	2540.129992	17.714074	-0.046357	2.793539
239.690445	2532.106714	17.719079	-0.046367	2.789492
239.656282	2524.159498	17.724083	-0.046356	2.785471
239.481386	2516.195790	17.729088	-0.046318	2.781427
239.500505	2508.242689	17.734093	-0.046317	2.777394
239.506312	2500.252930	17.739098	-0.046313	2.773336
239.331738	2492.257304	17.744103	-0.046275	2.769259
239.393896	2484.297893	17.749107	-0.046281	2.765208
239.194199	2476.339230	17.754112	-0.046239	2.761135
239.380034	2468.344089	17.759117	-0.046268	2.757061
239.239583	2460.344781	17.764122	-0.046237	2.752960
239.182390	2452.315398	17.769127	-0.046221	2.748842
239.198084	2444.352693	17.774131	-0.046219	2.744756
239.253467	2436.390465	17.779136	-0.046224	2.740667
239.086927	2428.457274	17.784141	-0.046188	2.736573
239.043465	2420.464568	17.789146	-0.046175	2.732449
238.859827	2412.483682	17.794151	-0.046136	2.728317
238.717942	2404.534756	17.799155	-0.046104	2.724198
238.734766	2396.571186	17.804160	-0.046102	2.720075
238.710531	2388.616761	17.809165	-0.046092	2.715948
238.783295	2380.598585	17.814170	-0.046101	2.711787
238.834368	2372.595268	17.819175	-0.046105	2.707626
238.752594	2364.657874	17.824179	-0.046085	2.703485
238.510204	2356.681445	17.829184	-0.046034	2.699308
238.602261	2348.720229	17.834189	-0.046046	2.695152
238.478666	2340.732868	17.839194	-0.046018	2.690963
238.436217	2332.757737	17.844199	-0.046005	2.686779
238.593994	2324.792228	17.849203	-0.046029	2.682606
238.336077	2316.828269	17.854208	-0.045976	2.678401
238.440878	2308.856062	17.859213	-0.045991	2.674208
238.289512	2300.854099	17.864218	-0.045957	2.669977
238.132889	2292.886798	17.869223	-0.045923	2.665756
238.112304	2284.937429	17.874227	-0.045914	2.661548
238.124823	2276.953646	17.879232	-0.045911	2.657316
238.167998	2268.968833	17.884237	-0.045914	2.653079
238.164380	2260.992213	17.889242	-0.045908	2.648837
238.132523	2252.999916	17.894247	-0.045897	2.644577
238.216204	2245.066541	17.899251	-0.045907	2.640350
237.946570	2237.119237	17.904256	-0.045852	2.636086
237.965714	2229.113813	17.909261	-0.045851	2.631802
238.024781	2221.131901	17.914266	-0.045856	2.627526
237.839332	2213.174577	17.919271	-0.045817	2.623241
237.679551	2205.241391	17.924275	-0.045782	2.618963
237.630708	2197.251629	17.929280	-0.045768	2.614655
237.721154	2189.256607	17.934285	-0.045779	2.610347
237.758968	2181.291371	17.939290	-0.045781	2.606044
237.625144	2173.344803	17.944295	-0.045751	2.601732
237.874193	2165.365440	17.949299	-0.045792	2.597421
237.710197	2157.319003	17.954304	-0.045757	2.593039
237.659127	2149.254646	17.959309	-0.045742	2.588647
237.537358	2141.321878	17.964314	-0.045714	2.584315
237.364850	2133.401994	17.969319	-0.045677	2.579979
237.399913	2125.466859	17.974323	-0.045678	2.575641
237.286793	2117.495685	17.979328	-0.045652	2.571266
237.312414	2109.526042	17.984333	-0.045652	2.566894
237.222915	2101.595279	17.989338	-0.045630	2.562528
237.204507	2093.637649	17.994343	-0.045621	2.558145
237.493547	2085.632094	17.999347	-0.045670	2.553749
237.069405	2077.682085	18.004352	-0.045586	2.549327
237.220540	2069.698098	18.009357	-0.045609	2.544918
237.218316	2061.749898	18.014362	-0.045603	2.540511
237.248230	2053.781346	18.019367	-0.045604	2.536087
237.314662	2045.813605	18.024371	-0.045611	2.531658
237.185164	2037.850952	18.029376	-0.045582	2.527210
237.035739	2029.915554	18.034381	-0.045549	2.522769
236.823640	2021.982458	18.039386	-0.045504	2.518316
236.873444	2013.989804	18.044391	-0.045508	2.513841
236.793253	2005.996950	18.049395	-0.045488	2.509348
236.815133	1997.995877	18.054400	-0.045487	2.504850
236.724899	1990.080368	18.059405	-0.045465	2.500384
237.034348	1982.082097	18.064410	-0.045517	2.495892
236.734393	1974.137705	18.069415	-0.045456	2.491378
236.686662	1966.182090	18.074419	-0.045442	2.486868
236.640400	1958.203362	18.079424	-0.045429	2.482337
236.543082	1950.283443	18.084429	-0.045405	2.477828
236.614406	1942.295257	18.089434	-0.045414	2.473283
236.380230	1934.314784	18.094439	-0.045365	2.468712
236.593731	1926.349175	18.099443	-0.045399	2.464174
236.571383	1918.379642	18.104448	-0.045390	2.459609
236.374221	1910.467642	18.109453	-0.045348	2.455054
236.470619	1902.471182	18.114458	-0.045361	2.450465
236.468388	1894.495002	18.119463	-0.045355	2.445871
236.409703	1886.577712	18.124467	-0.045339	2.441298
236.287769	1878.617521	18.129472	-0.045312	2.436687
236.314261	1870.600927	18.134477	-0.045311	2.432046
236.017380	1862.646619	18.139482	-0.045251	2.427407
235.732826	1854.710627	18.144487	-0.045193	2.422771
236.116011	1846.716004	18.149491	-0.045259	2.418143
235.864222	1838.774973	18.154496	-0.045207	2.413489
235.869014	1830.813461	18.159501	-0.045203	2.408834
235.882466	1822.854997	18.164506	-0.045200	2.404172
235.702530	1814.909293	18.169511	-0.045161	2.399493
235.688910	1806.975827	18.174515	-0.045154	2.394826
235.585655	1798.993069	18.179520	-0.045129	2.390113
235.665954	1791.015548	18.184525	-0.045139	2.385408
235.726269	1783.066133	18.189530	-0.045145	2.380709
235.693460	1775.106194	18.194535	-0.045134	2.375988
235.837674	1767.131212	18.199539	-0.045156	2.371262
235.766945	1759.166893	18.204544	-0.045137	2.366516
235.478373	1751.271215	18.209549	-0.045079	2.361783
235.638750	1743.311382	18.214554	-0.045103	2.357039
235.176594	1735.376335	18.219559	-0.045012	2.352250
235.272624	1727.372841	18.224563	-0.045025	2.347455
235.119583	1719.430276	18.229568	-0.044991	2.342667
235.113258	1711.478432	18.234573	-0.044985	2.337875
235.176003	1703.508701	18.239578	-0.044991	2.333069
235.296566	1695.524275	18.244583	-0.045009	2.328248
235.404544	1687.572670	18.249587	-0.045024	2.323436
235.146598	1679.669434	18.254592	-0.044970	2.318614
234.904525	1671.737088	18.259597	-0.044920	2.313764
235.061046	1663.741146	18.264602	-0.044944	2.308899
235.083483	1655.760680	18.269607	-0.044943	2.304022
234.890432	1647.871713	18.274611	-0.044902	2.299173
234.671219	1639.920306	18.279616	-0.044856	2.294273
234.852725	1631.911603	18.284621	-0.044885	2.289360
235.124383	1623.947231	18.289626	-0.044930	2.284473
234.871889	1616.043036	18.294631	-0.044878	2.279567
234.979187	1608.106282	18.299635	-0.044893	2.274662
234.708291	1600.077855	18.304640	-0.044837	2.269656
234.566444	1592.148202	18.309645	-0.044806	2.264712
234.492131	1584.227326	18.314650	-0.044787	2.259768
234.573880	1576.246966	18.319655	-0.044797	2.254790
234.756894	1568.271809	18.324659	-0.044826	2.249813
234.380598	1560.357076	18.329664	-0.044751	2.244814
234.503529	1552.429471	18.334669	-0.044768	2.239839
234.520676	1544.493342	18.339674	-0.044767	2.234839
234.314026	1536.522839	18.344679	-0.044723	2.229786
234.462690	1528.563837	18.349683	-0.044745	2.224760
234.194535	1520.650480	18.354688	-0.044690	2.219714
234.127654	1512.724552	18.359693	-0.044673	2.214668
234.073311	1504.771909	18.364698	-0.044658	2.209593
234.128322	1496.788715	18.369703	-0.044663	2.204498
234.155788	1488.883079	18.374707	-0.044663	2.199437
233.990004	1480.943476	18.379712	-0.044627	2.194326
233.974170	1472.961515	18.384717	-0.044619	2.189189
233.993055	1465.015365	18.389722	-0.044617	2.184066
233.833390	1457.093864	18.394727	-0.044582	2.178931
233.890176	1449.149797	18.399731	-0.044588	2.173789
233.682218	1441.208837	18.404736	-0.044544	2.168612
233.566568	1433.279331	18.409741	-0.044517	2.163439
233.368601	1425.380360	18.414746	-0.044475	2.158266
233.559520	1417.392237	18.419751	-0.044505	2.153058
233.456204	1409.441828	18.424755	-0.044481	2.147835
233.269591	1401.517528	18.429760	-0.044441	2.142608
233.460212	1393.562133	18.434765	-0.044472	2.137384
233.552504	1385.616076	18.439770	-0.044484	2.132143
233.540360	1377.657633	18.444775	-0.044476	2.126872
233.463825	1369.765287	18.449779	-0.044457	2.121625
233.503206	1361.816520	18.454784	-0.044459	2.116339
233.279491	1353.848666	18.459789	-0.044412	2.111002
233.205950	1345.916928	18.464794	-0.044393	2.105689
233.156890	1337.981936	18.469799	-0.044379	2.100363
233.079417	1330.080480	18.474803	-0.044360	2.095044
233.113418	1322.111937	18.479808	-0.044361	2.089677
232.971450	1314.194238	18.484813	-0.044329	2.084313
233.214491	1306.247195	18.489818	-0.044369	2.078953
232.909095	1298.352841	18.494823	-0.044307	2.073561
232.990156	1290.396749	18.499827	-0.044317	2.068151
232.902951	1282.469306	18.504832	-0.044296	2.062729
232.903524	1274.545353	18.509837	-0.044291	2.057305
232.945058	1266.610157	18.514842	-0.044294	2.051862
232.946677	1258.649261	18.519847	-0.044289	2.046384
232.912347	1250.764638	18.524851	-0.044277	2.040939
232.764838	1242.850559	18.529856	-0.044245	2.035449
232.554418	1234.916632	18.534861	-0.044200	2.029923
232.713747	1226.957107	18.539866	-0.044225	2.024402
232.534170	1219.050852	18.544871	-0.044186	2.018868
232.447960	1211.145903	18.549875	-0.044165	2.013329
232.421354	1203.187700	18.554880	-0.044155	2.007745
232.338231	1195.283946	18.559885	-0.044134	2.002176
232.574862	1187.334217	18.564890	-0.044173	1.996594
232.430740	1179.410849	18.569895	-0.044141	1.990974
232.420285	1171.486319	18.574899	-0.044134	1.985352
232.251678	1163.589807	18.579904	-0.044098	1.979717
232.181836	1155.686515	18.584909	-0.044080	1.974071
232.087231	1147.762279	18.589914	-0.044057	1.968392
231.989930	1139.844853	18.594919	-0.044034	1.962701
232.213112	1131.920436	18.599923	-0.044070	1.957022
232.049643	1123.970510	18.604928	-0.044035	1.951267
231.983569	1116.031030	18.609933	-0.044017	1.945513
231.669294	1108.173623	18.614938	-0.043954	1.939775
231.626719	1100.241866	18.619943	-0.043941	1.933995
231.768866	1092.295745	18.624947	-0.043962	1.928207
231.740349	1084.374611	18.629952	-0.043951	1.922402
231.441429	1076.531186	18.634957	-0.043891	1.916606
231.368580	1068.596297	18.639962	-0.043872	1.910750
231.509504	1060.632934	18.644967	-0.043893	1.904879
231.274943	1052.792525	18.649971	-0.043844	1.899038
231.317281	1044.859552	18.654976	-0.043847	1.893143
231.400027	1036.916251	18.659981	-0.043857	1.887225
231.405239	1029.029133	18.664986	-0.043853	1.881322
231.148808	1021.164674	18.669991	-0.043800	1.875388
231.253212	1013.201330	18.674995	-0.043815	1.869402
231.166638	1005.295432	18.680000	-0.043794	1.863418
231.055569	997.419537	18.685005	-0.043768	1.857434
231.162690	989.488119	18.690010	-0.043783	1.851414
231.008251	981.585508	18.695015	-0.043749	1.845367
230.905684	973.728215	18.700019	-0.043725	1.839339
230.918831	965.811978	18.705024	-0.043722	1.833261
230.970449	957.877396	18.710029	-0.043726	1.827153
230.774205	950.017741	18.715034	-0.043685	1.821052
230.814740	942.105834	18.720039	-0.043687	1.814919
230.875843	934.200800	18.725043	-0.043693	1.808773
230.804290	926.307544	18.730048	-0.043675	1.802599
230.527762	918.466141	18.735053	-0.043618	1.796420
230.609714	910.495287	18.740058	-0.043629	1.790161
230.349418	902.619741	18.745063	-0.043575	1.783913
230.274644	894.748056	18.750067	-0.043556	1.777669
230.168874	886.855353	18.755072	-0.043531	1.771383
230.192474	878.946725	18.760077	-0.043530	1.765078
230.202655	871.084341	18.765082	-0.043527	1.758785
230.184368	863.182140	18.770087	-0.043519	1.752434
230.094131	855.304926	18.775091	-0.043497	1.746072
229.884933	847.448520	18.780096	-0.043453	1.739687
229.881271	839.559334	18.785101	-0.043447	1.733279
230.105154	831.644061	18.790106	-0.043484	1.726855
230.008230	823.768602	18.795111	-0.043461	1.720398
229.900928	815.931781	18.800115	-0.043435	1.713947
229.820120	808.017919	18.805120	-0.043415	1.707411
229.733796	800.152945	18.810125	-0.043394	1.700891
229.694914	792.296230	18.815130	-0.043382	1.694358
229.558370	784.415752	18.820135	-0.043351	1.687767
229.382750	776.569345	18.825139	-0.043314	1.681174
229.411117	768.705749	18.830144	-0.043314	1.674567
229.226616	760.836919	18.835149	-0.043274	1.667901
229.476763	752.932818	18.840154	-0.043316	1.661237
229.409237	745.078789	18.845159	-0.043298	1.654546
229.394365	737.211313	18.850163	-0.043290	1.647823
229.193036	729.382196	18.855168	-0.043248	1.641081
229.185936	721.524729	18.860173	-0.043241	1.634312
229.052592	713.620507	18.865178	-0.043211	1.627458
228.748348	705.786332	18.870183	-0.043150	1.620611
228.925186	697.913973	18.875187	-0.043178	1.613770
228.771738	690.065124	18.880192	-0.043144	1.606873
228.613074	682.239214	18.885197	-0.043109	1.599967
228.841823	674.370977	18.890202	-0.043147	1.593047
228.831240	666.498073	18.895207	-0.043140	1.586060
228.568299	658.704490	18.900211	-0.043086	1.579076
228.398041	650.875492	18.905216	-0.043049	1.572042
228.539930	642.995712	18.910221	-0.043070	1.564977
228.641618	635.164507	18.915226	-0.043084	1.557917
228.232394	627.361229	18.920231	-0.043003	1.550776
228.337295	619.502729	18.925235	-0.043017	1.543627
228.380517	611.661535	18.930240	-0.043020	1.536451
228.077339	603.859475	18.935245	-0.042959	1.529226
228.232128	596.006739	18.940250	-0.042983	1.521989
228.159141	588.193486	18.945255	-0.042964	1.514720
228.176266	580.368343	18.950259	-0.042962	1.507418
227.851174	572.584910	18.955264	-0.042897	1.500067
227.819359	564.767538	18.960269	-0.042886	1.492693
227.803183	556.943114	18.965274	-0.042877	1.485278
227.698352	549.148819	18.970279	-0.042853	1.477840
227.934352	541.267109	18.975283	-0.042892	1.470335
227.697884	533.477573	18.980288	-0.042843	1.462806
227.440543	525.708245	18.985293	-0.042790	1.455254
227.359196	517.907082	18.990298	-0.042770	1.447659
227.495492	510.083421	18.995303	-0.042790	1.440037
227.380498	502.314608	19.000307	-0.042763	1.432388
226.994286	494.560690	19.005312	-0.042687	1.424669
227.099567	486.750830	19.010317	-0.042701	1.416932
227.131787	478.950709	19.015322	-0.042702	1.409151
226.713799	471.225929	19.020327	-0.042619	1.401327
226.686288	463.455264	19.025331	-0.042609	1.393478
226.737875	455.626685	19.030336	-0.042614	1.385539
226.505941	447.885188	19.035341	-0.042565	1.377595
226.541407	440.096880	19.040346	-0.042567	1.369603
226.489677	432.322124	19.045351	-0.042552	1.361563
226.304815	424.608694	19.050355	-0.042513	1.353515
226.241070	416.834522	19.055360	-0.042496	1.345377
225.973228	409.123772	19.060365	-0.042441	1.337221
225.969352	401.355815	19.065370	-0.042435	1.329000
225.791508	393.620715	19.070375	-0.042397	1.320732
225.545356	385.876917	19.075379	-0.042347	1.312391
225.410749	378.052924	19.080384	-0.042316	1.303929
225.262555	370.346110	19.085389	-0.042284	1.295537
225.082265	362.636148	19.090394	-0.042245	1.287081
224.893295	354.940000	19.095399	-0.042205	1.278583
224.692556	347.245326	19.100403	-0.042163	1.270027
224.405467	339.554679	19.105408	-0.042104	1.261401
224.380272	331.844543	19.110413	-0.042095	1.252743
224.129418	324.164286	19.115418	-0.042043	1.244016
223.878380	316.495438	19.120423	-0.041991	1.235240
223.643215	308.808706	19.125427	-0.041943	1.226384
223.311503	301.153785	19.130432	-0.041876	1.217481
222.877059	293.516214	19.135437	-0.041790	1.208512
222.504531	285.875856	19.140442	-0.041716	1.199485
222.147535	278.236427	19.145447	-0.041644	1.190394
221.893525	270.585946	19.150451	-0.041592	1.181240
221.288417	263.002907	19.155456	-0.041474	1.172023
221.197319	255.323106	19.160461	-0.041453	1.162723
220.855887	247.713357	19.165466	-0.041384	1.153381
220.268610	240.095769	19.170471	-0.041270	1.143900
219.953555	232.487207	19.175475	-0.041206	1.134410
219.323552	224.924681	19.180480	-0.041084	1.124829
218.764431	217.365429	19.185485	-0.040975	1.115185
218.361992	209.779370	19.190490	-0.040895	1.105457
217.906845	202.207069	19.195495	-0.040806	1.095648
217.685885	194.608762	19.200499	-0.040760	1.085769
216.995397	187.111650	19.205504	-0.040626	1.075826
216.454351	179.564133	19.210509	-0.040520	1.065757
215.995684	172.043186	19.215514	-0.040430	1.055646
215.433248	164.521809	19.220519	-0.040321	1.045413
214.767190	157.058584	19.225523	-0.040192	1.035133
214.217032	149.558004	19.230528	-0.040085	1.024725
213.665486	142.087733	19.235533	-0.039977	1.014252
213.100721	134.621471	19.240538	-0.039867	1.003673
212.532567	127.158056	19.245543	-0.039756	0.992983
212.274504	119.639986	19.250547	-0.039703	0.982176
211.206223	112.296357	19.255552	-0.039500	0.971296
210.735126	104.857410	19.260557	-0.039407	0.960306
210.507751	97.411492	19.265562	-0.039360	0.949241
209.772743	90.051789	19.270567	-0.039219	0.938042
209.220463	82.682442	19.275571	-0.039111	0.926741
208.528807	75.362115	19.280576	-0.038977	0.915338
208.045205	67.996691	19.285581	-0.038883	0.903778
207.363387	60.938070	19.290586	-0.038751	0.892497