Fri Apr 16 19:16:51 2021

Number of Points = 3635
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
1.614194	0.045519	0.000000	0.000049	0.311095

1.656602	0.038680	0.005005	0.000041	0.311099
1.561002	0.058249	0.010010	0.000059	0.311110
1.615709	0.043931	0.015014	0.000048	0.311089
1.850447	0.004668	0.020019	0.000005	0.311105
1.627082	0.045619	0.025024	0.000046	0.311107
1.117177	0.139628	0.030029	0.000141	0.311114
1.384703	0.090598	0.035034	0.000091	0.311112
1.463700	0.073507	0.040038	0.000076	0.311099
1.065387	0.148681	0.045043	0.000151	0.311113
1.715906	0.026733	0.050048	0.000029	0.311095
1.672087	0.035292	0.055053	0.000038	0.311098
1.446825	0.077499	0.060058	0.000079	0.311104
1.421914	0.080394	0.065062	0.000084	0.311097
1.695232	0.032842	0.070067	0.000033	0.311107
1.509745	0.067415	0.075072	0.000068	0.311111
1.478511	0.069408	0.080077	0.000073	0.311094
1.720968	0.027126	0.085082	0.000028	0.311103
1.419132	0.045669	0.090086	0.000084	0.310934
1.275640	0.041386	0.095091	0.000111	0.310793
1.433180	0.012778	0.100096	0.000082	0.310793
1.565215	-0.011698	0.105101	0.000057	0.310791
1.402315	0.018138	0.110106	0.000087	0.310793
0.733782	0.139188	0.115110	0.000212	0.310791
1.260211	0.044193	0.120115	0.000114	0.310794
1.663794	-0.057675	0.125120	0.000039	0.310661
1.089037	0.020605	0.130125	0.000146	0.310540
1.757017	-0.102738	0.135130	0.000021	0.310531
2.165319	-0.179723	0.140134	-0.000055	0.310518
1.529096	-0.060610	0.145139	0.000064	0.310534
1.588434	-0.127356	0.150144	0.000052	0.310274
1.874960	-0.200470	0.155149	-0.000001	0.310176
1.789601	-0.181956	0.160154	0.000015	0.310190
1.239003	-0.082208	0.165158	0.000117	0.310189
1.438445	-0.162517	0.170163	0.000080	0.309983
1.925370	-0.277366	0.175168	-0.000010	0.309860
1.621122	-0.222626	0.180173	0.000046	0.309858
1.614640	-0.226620	0.185178	0.000047	0.309834
1.376665	-0.246358	0.190182	0.000092	0.309540
0.825200	-0.142051	0.195187	0.000194	0.309559
1.488891	-0.267739	0.200192	0.000071	0.309536
1.878685	-0.376737	0.205197	-0.000002	0.309357
1.794334	-0.384145	0.210202	0.000014	0.309251
1.679268	-0.366165	0.215206	0.000035	0.309238
1.654734	-0.407376	0.220211	0.000040	0.309024
1.500597	-0.403538	0.225216	0.000068	0.308911
1.034073	-0.318036	0.230221	0.000155	0.308915
1.296591	-0.412606	0.235226	0.000106	0.308696
1.132578	-0.401591	0.240230	0.000137	0.308608
0.877773	-0.354249	0.245235	0.000184	0.308613
0.503020	-0.341271	0.250240	0.000254	0.308354
0.834008	-0.413625	0.255245	0.000192	0.308297
0.821043	-0.408503	0.260250	0.000195	0.308311
0.126158	-0.338882	0.265254	0.000324	0.308045
0.667380	-0.442510	0.270259	0.000223	0.308020
0.441407	-0.405061	0.275264	0.000265	0.308003
0.217609	-0.435066	0.280269	0.000307	0.307671
0.997719	-0.579596	0.285274	0.000162	0.307659
1.204963	-0.650863	0.290278	0.000123	0.307501
0.970499	-0.640887	0.295283	0.000167	0.307347
0.732882	-0.609154	0.300288	0.000211	0.307294
0.636219	-0.648988	0.305293	0.000229	0.307023
0.469434	-0.615072	0.310298	0.000260	0.307041
-0.032391	-0.572886	0.315302	0.000353	0.306810
-0.118087	-0.568286	0.320307	0.000369	0.306758
-0.055233	-0.597414	0.325312	0.000357	0.306675
0.493324	-0.755303	0.330317	0.000255	0.306400
0.296517	-0.716166	0.335322	0.000292	0.306417
0.757800	-0.869795	0.340326	0.000206	0.306087
1.072605	-0.929344	0.345331	0.000147	0.306076
-0.136031	-0.772977	0.350336	0.000372	0.305777
-0.129763	-0.776590	0.355341	0.000371	0.305766
0.350291	-0.904225	0.360346	0.000282	0.305574
-0.701784	-0.723657	0.365350	0.000478	0.305524
-1.070585	-0.695201	0.370355	0.000546	0.305342
-0.321241	-0.865046	0.375360	0.000407	0.305183
-0.312770	-0.893471	0.380365	0.000405	0.305055
-0.713467	-0.861261	0.385370	0.000480	0.304863
-0.454252	-0.928949	0.390374	0.000431	0.304765
0.134936	-1.086208	0.395379	0.000322	0.304527
-0.480196	-0.993673	0.400384	0.000436	0.304436
-1.021688	-0.933935	0.405389	0.000537	0.304252
-0.493940	-1.052163	0.410394	0.000439	0.304146
-1.181246	-0.977298	0.415398	0.000567	0.303908
-0.892180	-1.053687	0.420403	0.000513	0.303795
-0.805825	-1.111154	0.425408	0.000497	0.303596
-1.137448	-1.079480	0.430413	0.000558	0.303460
-1.641271	-1.026006	0.435418	0.000652	0.303279
-1.393813	-1.093587	0.440422	0.000606	0.303171
-0.934290	-1.216120	0.445427	0.000520	0.302985
-1.616235	-1.127106	0.450432	0.000647	0.302818
-1.754417	-1.138615	0.455437	0.000673	0.302643
-1.663993	-1.185209	0.460442	0.000656	0.302499
-1.926360	-1.170712	0.465446	0.000705	0.302341
-2.492249	-1.107299	0.470451	0.000810	0.302152
-2.373146	-1.157067	0.475456	0.000788	0.302018
-1.858908	-1.289031	0.480461	0.000692	0.301833
-2.401891	-1.213122	0.485466	0.000793	0.301724
-3.378331	-1.081089	0.490470	0.000975	0.301507
-2.685802	-1.227555	0.495475	0.000846	0.301408
-2.533024	-1.300960	0.500480	0.000818	0.301189
-2.985934	-1.240773	0.505485	0.000902	0.301083
-2.438834	-1.388447	0.510490	0.000800	0.300851
-2.647844	-1.367703	0.515494	0.000839	0.300768
-2.865172	-1.376731	0.520499	0.000879	0.300535
-3.587033	-1.247591	0.525504	0.001014	0.300525
-2.580776	-1.503562	0.530509	0.000827	0.300173
-2.695207	-1.504107	0.535514	0.000848	0.300071
-3.422705	-1.416908	0.540518	0.000983	0.299854
-3.230849	-1.481929	0.545523	0.000947	0.299708
-3.179998	-1.524679	0.550528	0.000938	0.299547
-3.686318	-1.478234	0.555533	0.001032	0.299327
-3.578574	-1.510549	0.560538	0.001012	0.299265
-3.426015	-1.605763	0.565542	0.000984	0.298939
-4.198224	-1.478166	0.570547	0.001127	0.298878
-4.728030	-1.433799	0.575552	0.001226	0.298626
-4.253240	-1.539439	0.580557	0.001138	0.298533
-4.456144	-1.547139	0.585562	0.001175	0.298317
-4.923700	-1.490498	0.590566	0.001262	0.298180
-4.397288	-1.621942	0.595571	0.001164	0.298006
-3.964857	-1.749160	0.600576	0.001084	0.297770
-4.649573	-1.647081	0.605581	0.001211	0.297662
-4.392058	-1.756754	0.610586	0.001163	0.297356
-4.445189	-1.767637	0.615590	0.001173	0.297256
-4.618964	-1.785414	0.620595	0.001205	0.297016
-5.351378	-1.680455	0.625600	0.001342	0.296879
-4.911658	-1.792489	0.630605	0.001260	0.296723
-4.896897	-1.847782	0.635610	0.001257	0.296466
-5.624820	-1.732872	0.640614	0.001393	0.296381
-5.498377	-1.813996	0.645619	0.001369	0.296098
-5.829889	-1.774884	0.650624	0.001431	0.295995
-6.614212	-1.672440	0.655629	0.001577	0.295799
-6.211992	-1.770447	0.660634	0.001502	0.295677
-6.182165	-1.805823	0.665638	0.001496	0.295530
-6.738573	-1.749096	0.670643	0.001600	0.295313
-6.165796	-1.880467	0.675648	0.001493	0.295180
-6.381867	-1.900679	0.680653	0.001533	0.294888
-6.565548	-1.882374	0.685658	0.001567	0.294814
-6.900626	-1.879811	0.690662	0.001630	0.294528
-6.842645	-1.912412	0.695667	0.001619	0.294420
-7.445700	-1.834884	0.700672	0.001731	0.294262
-7.672724	-1.833911	0.705677	0.001773	0.294064
-7.622159	-1.871775	0.710682	0.001764	0.293923
-7.918007	-1.864879	0.715686	0.001819	0.293693
-8.543238	-1.765108	0.720691	0.001935	0.293624
-8.569741	-1.808675	0.725696	0.001940	0.293386
-8.226151	-1.890404	0.730701	0.001876	0.293291
-8.491162	-1.889623	0.735706	0.001926	0.293057
-8.729761	-1.858281	0.740710	0.001970	0.292998
-8.729192	-1.923282	0.745715	0.001970	0.292678
-8.506679	-1.976384	0.750720	0.001928	0.292615
-9.301722	-1.887603	0.755725	0.002076	0.292340
-9.612847	-1.836781	0.760730	0.002134	0.292312
-9.623046	-1.894069	0.765734	0.002136	0.292019
-10.061364	-1.816895	0.770739	0.002218	0.292007
-10.857263	-1.721257	0.775744	0.002366	0.291764
-10.793079	-1.735442	0.780749	0.002354	0.291751
-10.192038	-1.906995	0.785754	0.002242	0.291442
-10.557120	-1.850030	0.790758	0.002310	0.291396
-10.751844	-1.865287	0.795763	0.002346	0.291145
-11.036513	-1.820564	0.800768	0.002399	0.291110
-11.477901	-1.787120	0.805773	0.002481	0.290877
-11.587301	-1.782264	0.810778	0.002501	0.290803
-11.033022	-1.915282	0.815782	0.002398	0.290642
-11.458356	-1.861237	0.820787	0.002477	0.290527
-11.490730	-1.889214	0.825792	0.002483	0.290358
-12.026825	-1.825850	0.830797	0.002583	0.290188
-11.875620	-1.874481	0.835802	0.002555	0.290083
-12.783650	-1.752085	0.840806	0.002724	0.289870
-12.536088	-1.798828	0.845811	0.002678	0.289862
-13.040764	-1.767117	0.850816	0.002772	0.289562
-13.342507	-1.713362	0.855821	0.002828	0.289557
-13.178720	-1.781164	0.860826	0.002797	0.289367
-13.841098	-1.680089	0.865830	0.002921	0.289270
-13.335406	-1.787936	0.870835	0.002826	0.289191
-13.794302	-1.755863	0.875840	0.002912	0.288934
-13.894579	-1.737974	0.880845	0.002930	0.288933
-13.637106	-1.835738	0.885850	0.002882	0.288677
-13.988378	-1.785233	0.890854	0.002948	0.288611
-14.079560	-1.800326	0.895859	0.002965	0.288452
-14.807542	-1.696413	0.900864	0.003100	0.288309
-14.808445	-1.696612	0.905869	0.003100	0.288308
-15.194961	-1.679774	0.910874	0.003172	0.288040
-15.238597	-1.674957	0.915878	0.003180	0.288024
-15.111375	-1.725886	0.920883	0.003157	0.287885
-15.633142	-1.671009	0.925888	0.003254	0.287684
-15.502153	-1.696306	0.930893	0.003229	0.287677
-15.248112	-1.792181	0.935898	0.003182	0.287427
-15.741854	-1.716470	0.940902	0.003274	0.287356
-15.901374	-1.705362	0.945907	0.003304	0.287266
-16.242272	-1.686758	0.950912	0.003367	0.287048
-15.912845	-1.748886	0.955917	0.003306	0.287037
-16.086791	-1.759268	0.960922	0.003338	0.286825
-16.563451	-1.687579	0.965926	0.003427	0.286750
-16.617586	-1.684724	0.970931	0.003437	0.286715
-16.899470	-1.691064	0.975936	0.003489	0.286424
-16.783145	-1.714434	0.980941	0.003467	0.286413
-16.639718	-1.769774	0.985946	0.003441	0.286265
-17.269226	-1.686711	0.990950	0.003558	0.286107
-17.192950	-1.701259	0.995955	0.003544	0.286103
-17.376380	-1.726522	1.000960	0.003578	0.285807
-17.735831	-1.663381	1.005965	0.003645	0.285796
-16.989719	-1.821344	1.010970	0.003506	0.285683
-17.647557	-1.733646	1.015974	0.003628	0.285522
-17.419476	-1.774133	1.020979	0.003586	0.285527
-17.128519	-1.891287	1.025984	0.003531	0.285201
-17.401831	-1.850284	1.030989	0.003582	0.285157
-17.044316	-1.952718	1.035994	0.003516	0.284967
-17.753942	-1.850135	1.040998	0.003648	0.284833
-17.471525	-1.922663	1.046003	0.003595	0.284726
-17.971248	-1.872722	1.051008	0.003688	0.284518
-17.970627	-1.875817	1.056013	0.003688	0.284503
-18.503491	-1.829931	1.061018	0.003787	0.284244
-18.799426	-1.777512	1.066022	0.003842	0.284237
-18.673154	-1.835887	1.071027	0.003819	0.284057
-19.280056	-1.753898	1.076032	0.003932	0.283912
-19.396301	-1.732206	1.081037	0.003953	0.283915
-18.842893	-1.893072	1.086042	0.003850	0.283608
-19.418618	-1.789060	1.091046	0.003957	0.283605
-19.947362	-1.722475	1.096051	0.004056	0.283454
-20.146200	-1.718511	1.101056	0.004093	0.283290
-20.130548	-1.719832	1.106061	0.004090	0.283298
-20.275215	-1.738128	1.111066	0.004117	0.283070
-20.721416	-1.669452	1.116070	0.004200	0.283007
-20.305948	-1.752100	1.121075	0.004122	0.282971
-20.301009	-1.815586	1.126080	0.004121	0.282651
-21.002062	-1.686442	1.131085	0.004252	0.282659
-20.658387	-1.775516	1.136090	0.004188	0.282523
-21.364717	-1.680786	1.141094	0.004319	0.282351
-21.329884	-1.686874	1.146099	0.004313	0.282352
-21.483479	-1.703198	1.151104	0.004341	0.282126
-21.394145	-1.741625	1.156109	0.004325	0.282012
-21.312474	-1.757405	1.161114	0.004309	0.282007
-21.677551	-1.746958	1.166118	0.004377	0.281720
-21.473172	-1.783722	1.171123	0.004339	0.281723
-21.843464	-1.741112	1.176128	0.004408	0.281596
-22.531746	-1.652910	1.181133	0.004536	0.281406
-22.084242	-1.734151	1.186138	0.004453	0.281407
-21.794848	-1.831415	1.191142	0.004399	0.281177
-22.360696	-1.747785	1.196147	0.004504	0.281078
-22.428066	-1.739837	1.201152	0.004517	0.281056
-22.486778	-1.785805	1.206157	0.004528	0.280765
-22.780637	-1.727917	1.211162	0.004582	0.280788
-23.737632	-1.567818	1.216166	0.004760	0.280716
-23.511994	-1.638084	1.221171	0.004718	0.280566
-23.386182	-1.662585	1.226176	0.004695	0.280558
-23.470985	-1.679377	1.231181	0.004711	0.280392
-23.613874	-1.689188	1.236186	0.004737	0.280207
-23.697416	-1.673603	1.241190	0.004753	0.280209
-23.792963	-1.698833	1.246195	0.004770	0.279989
-24.083497	-1.664609	1.251200	0.004824	0.279893
-23.858025	-1.706380	1.256205	0.004782	0.279889
-23.751429	-1.788624	1.261210	0.004763	0.279564
-24.056279	-1.737991	1.266214	0.004819	0.279540
-24.162317	-1.737830	1.271219	0.004839	0.279441
-24.603455	-1.689518	1.276224	0.004921	0.279276
-24.671262	-1.678339	1.281229	0.004934	0.279270
-24.150408	-1.817962	1.286234	0.004837	0.279037
-24.632043	-1.752653	1.291238	0.004926	0.278922
-24.437120	-1.797562	1.296243	0.004890	0.278873
-25.244543	-1.700633	1.301248	0.005040	0.278614
-25.054779	-1.736923	1.306253	0.005005	0.278605
-24.882919	-1.794339	1.311258	0.004973	0.278469
-25.755468	-1.668516	1.316262	0.005135	0.278299
-25.478089	-1.718095	1.321267	0.005084	0.278303
-25.177021	-1.819749	1.326272	0.005028	0.278059
-26.445205	-1.596503	1.331277	0.005264	0.278021
-26.150180	-1.653942	1.336282	0.005209	0.278002
-26.475909	-1.655939	1.341286	0.005269	0.277683
-26.592854	-1.632540	1.346291	0.005291	0.277694
-26.825164	-1.599535	1.351296	0.005334	0.277646
-26.466432	-1.720371	1.356301	0.005267	0.277356
-26.198829	-1.768725	1.361306	0.005218	0.277358
-26.508733	-1.746747	1.366310	0.005275	0.277179
-26.650188	-1.750990	1.371315	0.005301	0.277023
-26.143169	-1.845242	1.376320	0.005207	0.277012
-27.067577	-1.730924	1.381325	0.005379	0.276731
-27.072791	-1.730438	1.386330	0.005380	0.276729
-26.666531	-1.831750	1.391334	0.005304	0.276585
-26.803443	-1.844653	1.396339	0.005330	0.276388
-26.456307	-1.912289	1.401344	0.005265	0.276364
-27.086295	-1.854821	1.406349	0.005382	0.276065
-26.935255	-1.878942	1.411354	0.005354	0.276083
-27.446397	-1.828417	1.416358	0.005449	0.275861
-27.878181	-1.767508	1.421363	0.005530	0.275768
-27.764445	-1.792305	1.426368	0.005509	0.275747
-28.226221	-1.749583	1.431373	0.005594	0.275531
-28.360008	-1.723340	1.436378	0.005619	0.275541
-28.446130	-1.741449	1.441382	0.005635	0.275363
-28.303497	-1.801666	1.446387	0.005609	0.275183
-29.006156	-1.670610	1.451392	0.005739	0.275201
-29.199101	-1.686730	1.456397	0.005775	0.274932
-29.324463	-1.668986	1.461402	0.005799	0.274905
-29.755279	-1.592524	1.466406	0.005879	0.274895
-30.071456	-1.593567	1.471411	0.005938	0.274587
-29.709382	-1.662524	1.476416	0.005870	0.274571
-29.711586	-1.670381	1.481421	0.005871	0.274528
-30.249495	-1.618248	1.486426	0.005971	0.274287
-30.432198	-1.585676	1.491430	0.006005	0.274283
-29.900009	-1.696455	1.496435	0.005906	0.274210
-30.230842	-1.688402	1.501440	0.005967	0.273935
-30.218013	-1.693263	1.506445	0.005965	0.273922
-29.511098	-1.853848	1.511450	0.005833	0.273752
-30.176498	-1.761208	1.516454	0.005957	0.273603
-30.013739	-1.795088	1.521459	0.005927	0.273580
-30.720909	-1.720512	1.526464	0.006058	0.273294
-30.875281	-1.692769	1.531469	0.006087	0.273293
-31.269370	-1.636031	1.536474	0.006160	0.273214
-31.609659	-1.609868	1.541478	0.006223	0.273025
-31.049374	-1.714715	1.546483	0.006119	0.273009
-31.051720	-1.751500	1.551488	0.006120	0.272812
-31.549072	-1.688560	1.556493	0.006212	0.272666
-31.002288	-1.787185	1.561498	0.006110	0.272671
-32.227543	-1.620655	1.566502	0.006338	0.272372
-32.251899	-1.617261	1.571507	0.006343	0.272366
-32.260910	-1.619182	1.576512	0.006344	0.272348
-32.414690	-1.648224	1.581517	0.006373	0.272045
-32.430730	-1.644251	1.586522	0.006376	0.272051
-32.435101	-1.661845	1.591526	0.006377	0.271953
-32.182371	-1.747912	1.596531	0.006330	0.271739
-31.836836	-1.812941	1.601536	0.006265	0.271728
-32.707190	-1.702189	1.606541	0.006427	0.271475
-32.925913	-1.672071	1.611546	0.006468	0.271423
-32.931055	-1.675353	1.616550	0.006469	0.271401
-33.536674	-1.615646	1.621555	0.006582	0.271132
-33.749664	-1.576781	1.626560	0.006621	0.271133
-33.534963	-1.628641	1.631565	0.006581	0.271065
-33.998558	-1.590204	1.636570	0.006667	0.270820
-33.952518	-1.600067	1.641574	0.006659	0.270812
-33.704466	-1.661542	1.646579	0.006613	0.270725
-34.290547	-1.587017	1.651584	0.006722	0.270553
-34.424496	-1.563293	1.656589	0.006747	0.270550
-33.749500	-1.715271	1.661594	0.006621	0.270394
-34.256851	-1.660650	1.666598	0.006715	0.270193
-34.161845	-1.678301	1.671603	0.006698	0.270191
-34.115782	-1.737858	1.676608	0.006689	0.269917
-34.280475	-1.717695	1.681613	0.006720	0.269864
-34.833114	-1.626348	1.686618	0.006822	0.269815
-34.891524	-1.668729	1.691622	0.006833	0.269531
-34.759329	-1.690470	1.696627	0.006809	0.269544
-34.887115	-1.696596	1.701632	0.006832	0.269386
-35.403315	-1.626749	1.706637	0.006928	0.269257
-34.818899	-1.732264	1.711642	0.006820	0.269261
-35.016791	-1.759182	1.716646	0.006856	0.268923
-35.689331	-1.634671	1.721651	0.006982	0.268935
-35.923326	-1.608789	1.726656	0.007025	0.268845
-35.896493	-1.656916	1.731661	0.007020	0.268613
-35.381316	-1.751976	1.736666	0.006924	0.268605
-35.756987	-1.727388	1.741670	0.006994	0.268370
-36.225002	-1.655685	1.746675	0.007081	0.268298
-35.699734	-1.763333	1.751680	0.006983	0.268232
-36.478008	-1.665790	1.756685	0.007128	0.267995
-36.677403	-1.624385	1.761690	0.007165	0.268023
-36.580224	-1.675456	1.766694	0.007147	0.267843
-36.638863	-1.699382	1.771699	0.007158	0.267656
-36.967401	-1.637988	1.776704	0.007219	0.267665
-37.299104	-1.624706	1.781709	0.007281	0.267410
-37.233156	-1.644946	1.786714	0.007269	0.267366
-37.425279	-1.619197	1.791718	0.007304	0.267316
-37.278620	-1.697703	1.796723	0.007277	0.267036
-37.642892	-1.628967	1.801728	0.007345	0.267049
-38.094831	-1.571283	1.806733	0.007429	0.266916
-38.053383	-1.608959	1.811738	0.007421	0.266753
-37.606440	-1.692735	1.816742	0.007338	0.266740
-37.726431	-1.714358	1.821747	0.007360	0.266504
-38.409899	-1.605669	1.826752	0.007487	0.266419
-38.236049	-1.642228	1.831757	0.007455	0.266393
-38.300107	-1.682262	1.836762	0.007467	0.266112
-38.658715	-1.618701	1.841766	0.007533	0.266103
-38.623130	-1.648585	1.846771	0.007527	0.265976
-38.951045	-1.623001	1.851776	0.007588	0.265790
-38.977419	-1.621184	1.856781	0.007593	0.265774
-39.014145	-1.644526	1.861786	0.007600	0.265611
-38.915016	-1.680066	1.866790	0.007581	0.265516
-39.124601	-1.648440	1.871795	0.007620	0.265481
-39.445828	-1.645468	1.876800	0.007680	0.265178
-39.454915	-1.644466	1.881805	0.007681	0.265175
-39.496376	-1.662450	1.886810	0.007689	0.265036
-40.180447	-1.568505	1.891814	0.007816	0.264869
-39.948085	-1.610116	1.896819	0.007773	0.264873
-40.086178	-1.627950	1.901824	0.007799	0.264638
-40.060060	-1.653367	1.906829	0.007794	0.264525
-40.088660	-1.653668	1.911834	0.007799	0.264495
-40.249132	-1.668367	1.916838	0.007829	0.264255
-40.368461	-1.646868	1.921843	0.007851	0.264254
-40.587862	-1.638255	1.926848	0.007892	0.264083
-40.675941	-1.656489	1.931853	0.007908	0.263895
-40.690043	-1.648482	1.936858	0.007911	0.263925
-40.730795	-1.698790	1.941862	0.007919	0.263609
-41.127642	-1.627061	1.946867	0.007992	0.263606
-40.545564	-1.758486	1.951872	0.007884	0.263466
-41.263148	-1.663384	1.956877	0.008018	0.263271
-40.804696	-1.747590	1.961882	0.007932	0.263267
-41.034533	-1.756693	1.966886	0.007975	0.262987
-41.183053	-1.731669	1.971891	0.008003	0.262976
-41.806285	-1.647293	1.976896	0.008118	0.262817
-42.059385	-1.632777	1.981901	0.008166	0.262643
-41.410466	-1.750017	1.986906	0.008045	0.262648
-42.063538	-1.688127	1.991910	0.008166	0.262334
-42.457693	-1.616335	1.996915	0.008240	0.262335
-42.429913	-1.662680	2.001920	0.008234	0.262107

-42.643401	-1.652315	2.011917	0.008274	0.261950
-42.852036	-1.655206	2.021914	0.008313	0.261725
-43.418305	-1.579045	2.031910	0.008418	0.261577
-43.240682	-1.645755	2.041907	0.008385	0.261386
-43.368525	-1.646144	2.051904	0.008409	0.261256
-43.700163	-1.616587	2.061901	0.008470	0.261086
-43.884899	-1.580719	2.071898	0.008505	0.261099
-43.919158	-1.606001	2.081894	0.008511	0.260924
-44.294927	-1.564651	2.091891	0.008581	0.260775
-43.855803	-1.645049	2.101888	0.008499	0.260772
-44.283361	-1.566107	2.111885	0.008579	0.260779
-44.177945	-1.584742	2.121882	0.008559	0.260783
-44.053803	-1.608279	2.131878	0.008536	0.260778
-44.294212	-1.563970	2.141875	0.008580	0.260781
-43.998832	-1.620090	2.151872	0.008525	0.260769
-44.247365	-1.572668	2.161869	0.008571	0.260781
-44.425065	-1.538261	2.171866	0.008604	0.260793
-44.398980	-1.544273	2.181862	0.008599	0.260787
-44.218850	-1.579623	2.191859	0.008566	0.260773
-43.996326	-1.621547	2.201856	0.008524	0.260765
-44.432467	-1.539013	2.211853	0.008605	0.260784
-44.332757	-1.548442	2.221850	0.008587	0.260832
-43.990595	-1.564329	2.231846	0.008523	0.261090
-43.806283	-1.597136	2.241843	0.008489	0.261095
-43.665134	-1.625089	2.251840	0.008462	0.261082
-43.620209	-1.624832	2.261837	0.008454	0.261130
-43.525835	-1.591707	2.271834	0.008436	0.261409
-43.477305	-1.602312	2.281830	0.008427	0.261399
-43.864384	-1.522325	2.291827	0.008499	0.261453
-43.386790	-1.556019	2.301824	0.008410	0.261748
-43.131685	-1.603852	2.311821	0.008362	0.261740
-42.850072	-1.627731	2.321818	0.008310	0.261892
-43.022908	-1.572196	2.331814	0.008342	0.262026
-42.725559	-1.619411	2.341811	0.008287	0.262064
-42.146719	-1.676730	2.351808	0.008179	0.262330
-42.349983	-1.638595	2.361805	0.008217	0.262337
-41.875821	-1.684709	2.371802	0.008128	0.262558
-41.684254	-1.705099	2.381798	0.008092	0.262639
-41.462066	-1.727937	2.391795	0.008051	0.262736
-41.452933	-1.685098	2.401792	0.008049	0.262982
-41.828063	-1.605160	2.411789	0.008119	0.263047
-41.201989	-1.676683	2.421786	0.008002	0.263280
-41.057828	-1.691838	2.431782	0.007975	0.263341
-40.717637	-1.708652	2.441779	0.007912	0.263590
-41.147232	-1.611694	2.451776	0.007992	0.263693
-40.716070	-1.650517	2.461773	0.007911	0.263911
-40.599029	-1.638809	2.471770	0.007890	0.264093
-40.547412	-1.618874	2.481766	0.007880	0.264254
-40.826982	-1.521367	2.491763	0.007932	0.264510
-41.027100	-1.450831	2.501760	0.007969	0.264697
-40.111933	-1.583596	2.511757	0.007799	0.264882
-40.099239	-1.535260	2.521754	0.007796	0.265159
-39.792298	-1.561058	2.531750	0.007739	0.265324
-39.638778	-1.548359	2.541747	0.007710	0.265546
-39.340295	-1.561503	2.551744	0.007655	0.265770
-38.707950	-1.654062	2.561741	0.007537	0.265893
-37.898519	-1.765988	2.571738	0.007386	0.266086
-37.847554	-1.741601	2.581734	0.007376	0.266270
-37.835286	-1.721384	2.591731	0.007374	0.266392
-37.774054	-1.677357	2.601728	0.007363	0.266692
-37.323465	-1.739365	2.611725	0.007279	0.266801
-37.275033	-1.709015	2.621722	0.007269	0.267014
-36.997954	-1.718888	2.631718	0.007218	0.267234
-36.876172	-1.718036	2.641715	0.007195	0.267359
-36.825787	-1.672296	2.651712	0.007186	0.267657
-36.212453	-1.749957	2.661709	0.007071	0.267840
-36.180860	-1.727759	2.671706	0.007065	0.267992
-35.940912	-1.718781	2.681702	0.007021	0.268277
-35.787695	-1.716830	2.691699	0.006992	0.268438
-35.649551	-1.712326	2.701696	0.006966	0.268598
-35.232950	-1.731955	2.711693	0.006889	0.268901
-35.693684	-1.611804	2.721690	0.006974	0.269097
-35.647240	-1.575651	2.731686	0.006965	0.269337
-35.648694	-1.532063	2.741683	0.006966	0.269571
-34.897456	-1.614542	2.751680	0.006826	0.269862
-34.400308	-1.668284	2.761677	0.006733	0.270059
-34.450837	-1.618865	2.771674	0.006742	0.270275
-33.748851	-1.698903	2.781670	0.006612	0.270531
-33.484659	-1.710540	2.791667	0.006562	0.270726
-33.392897	-1.698996	2.801664	0.006545	0.270877
-32.801849	-1.766989	2.811661	0.006435	0.271089
-32.937460	-1.689501	2.821658	0.006460	0.271371
-32.648055	-1.706144	2.831654	0.006406	0.271564
-32.050536	-1.784569	2.841651	0.006295	0.271725
-31.933499	-1.752887	2.851648	0.006273	0.272008
-31.620786	-1.775401	2.861645	0.006215	0.272191
-31.949387	-1.676880	2.871642	0.006276	0.272398
-31.580365	-1.694168	2.881638	0.006207	0.272663
-31.179427	-1.718611	2.891635	0.006132	0.272921
-30.732753	-1.765861	2.901632	0.006049	0.273101
-30.157076	-1.837629	2.911629	0.005942	0.273276
-30.489398	-1.723340	2.921626	0.006004	0.273562
-30.314148	-1.717249	2.931622	0.005971	0.273763
-30.525613	-1.634876	2.941619	0.006010	0.273996
-30.255106	-1.633189	2.951616	0.005960	0.274265
-30.056336	-1.618453	2.961613	0.005922	0.274534
-29.714822	-1.633134	2.971610	0.005859	0.274784
-29.191379	-1.688070	2.981606	0.005761	0.274997
-28.920960	-1.698676	2.991603	0.005711	0.275200
-28.960660	-1.627293	3.001600	0.005718	0.275538
-28.400898	-1.695555	3.011597	0.005614	0.275714
-28.404008	-1.656957	3.021594	0.005614	0.275914
-27.730353	-1.740575	3.031590	0.005489	0.276119
-27.656957	-1.701833	3.041587	0.005475	0.276392
-26.960322	-1.783829	3.051584	0.005345	0.276627
-26.932319	-1.756825	3.061581	0.005340	0.276795
-26.136243	-1.863854	3.071578	0.005192	0.276993
-26.227874	-1.796657	3.081574	0.005209	0.277257
-25.724442	-1.858488	3.091571	0.005115	0.277413
-25.631440	-1.834021	3.101568	0.005098	0.277629
-25.712584	-1.761530	3.111565	0.005113	0.277930
-25.720368	-1.723196	3.121562	0.005114	0.278123
-25.479684	-1.727723	3.131558	0.005069	0.278327
-25.121170	-1.742763	3.141555	0.005002	0.278589
-24.895919	-1.733791	3.151552	0.004960	0.278848
-24.658715	-1.737197	3.161549	0.004916	0.279055
-24.091784	-1.800314	3.171546	0.004810	0.279263
-23.846902	-1.794140	3.181542	0.004765	0.279526
-23.509804	-1.813523	3.191539	0.004702	0.279743
-23.401729	-1.797702	3.201536	0.004682	0.279927
-23.381456	-1.754217	3.211533	0.004678	0.280171
-22.818883	-1.797711	3.221530	0.004573	0.280475
-22.960116	-1.742203	3.231526	0.004599	0.280630
-22.899232	-1.715125	3.241523	0.004588	0.280827
-22.165374	-1.804552	3.251520	0.004451	0.281054
-22.213314	-1.743312	3.261517	0.004460	0.281325
-21.953452	-1.747056	3.271514	0.004411	0.281549
-21.508624	-1.787540	3.281510	0.004328	0.281757
-21.122101	-1.813792	3.291507	0.004256	0.281984
-21.492802	-1.693255	3.301504	0.004325	0.282257
-21.327812	-1.678561	3.311501	0.004294	0.282486
-21.045219	-1.680596	3.321498	0.004242	0.282739
-21.094071	-1.617450	3.331494	0.004251	0.283018
-20.082836	-1.752414	3.341491	0.004062	0.283268
-19.815647	-1.756204	3.351488	0.004013	0.283497
-19.615962	-1.753888	3.361485	0.003975	0.283695
-19.535125	-1.722184	3.371482	0.003960	0.283932
-19.002793	-1.759306	3.381478	0.003861	0.284236
-18.493665	-1.814591	3.391475	0.003766	0.284426
-18.292670	-1.819360	3.401472	0.003729	0.284588
-18.276149	-1.771947	3.411469	0.003725	0.284845
-17.657751	-1.831421	3.421466	0.003610	0.285115
-17.830366	-1.760581	3.431462	0.003642	0.285315
-17.011084	-1.874371	3.441459	0.003490	0.285494
-17.048854	-1.818418	3.451456	0.003497	0.285743
-16.887911	-1.809230	3.461453	0.003467	0.285938
-16.746885	-1.796038	3.471450	0.003440	0.286135
-16.270192	-1.834920	3.481446	0.003351	0.286377
-15.941705	-1.845292	3.491443	0.003290	0.286627
-16.038270	-1.791181	3.501440	0.003308	0.286812
-15.669348	-1.821210	3.511437	0.003239	0.286999
-15.008410	-1.881217	3.521434	0.003116	0.287303
-15.106528	-1.828436	3.531430	0.003134	0.287479
-14.803803	-1.848013	3.541427	0.003078	0.287658
-14.343923	-1.872271	3.551424	0.002992	0.287957
-13.719771	-1.952006	3.561421	0.002876	0.288127
-13.677074	-1.932869	3.571418	0.002868	0.288262
-13.593860	-1.885081	3.581414	0.002852	0.288578
-13.331073	-1.898919	3.591411	0.002803	0.288749
-13.141913	-1.901322	3.601408	0.002768	0.288909
-12.650058	-1.929794	3.611405	0.002676	0.289215
-12.321385	-1.958189	3.621402	0.002615	0.289372
-12.245572	-1.944813	3.631398	0.002601	0.289508
-12.055083	-1.914855	3.641395	0.002565	0.289831
-12.021468	-1.885642	3.651392	0.002559	0.290008
-11.949988	-1.857014	3.661389	0.002545	0.290216
-11.576618	-1.867800	3.671386	0.002476	0.290501
-11.131591	-1.911848	3.681382	0.002393	0.290685
-10.887988	-1.925385	3.691379	0.002348	0.290839
-10.784670	-1.898294	3.701376	0.002328	0.291067
-10.630041	-1.873580	3.711373	0.002299	0.291330
-10.392606	-1.876585	3.721370	0.002255	0.291530
-10.293675	-1.852568	3.731366	0.002236	0.291739
-9.938307	-1.865025	3.741363	0.002170	0.291998
-10.029154	-1.800542	3.751360	0.002187	0.292236
-9.849115	-1.787435	3.761357	0.002153	0.292463
-9.297201	-1.845409	3.771354	0.002051	0.292673
-8.972177	-1.842937	3.781350	0.001990	0.292977
-8.626791	-1.864659	3.791347	0.001926	0.293180
-8.541154	-1.843139	3.801344	0.001910	0.293364
-8.290110	-1.845593	3.811341	0.001863	0.293577
-8.169282	-1.805422	3.821338	0.001840	0.293884
-8.100871	-1.769413	3.831334	0.001827	0.294123
-7.857897	-1.768971	3.841331	0.001782	0.294342
-7.711878	-1.751775	3.851328	0.001755	0.294558
-7.342487	-1.759449	3.861325	0.001686	0.294850
-7.462956	-1.681912	3.871322	0.001708	0.295123
-7.454665	-1.625289	3.881318	0.001706	0.295409
-7.673434	-1.533081	3.891315	0.001747	0.295666
-7.072826	-1.594956	3.901312	0.001635	0.295898
-6.555794	-1.637571	3.911309	0.001539	0.296149
-6.395078	-1.615260	3.921306	0.001509	0.296401
-6.167541	-1.589523	3.931302	0.001466	0.296729
-5.689450	-1.629252	3.941299	0.001377	0.296959
-5.499030	-1.613449	3.951296	0.001342	0.297205
-5.733348	-1.513561	3.961293	0.001385	0.297484
-5.721803	-1.453479	3.971290	0.001383	0.297787
-5.249961	-1.481522	3.981286	0.001295	0.298068
-5.196241	-1.436689	3.991283	0.001285	0.298333
-4.784424	-1.454514	4.001280	0.001208	0.298610
-4.867115	-1.377202	4.011277	0.001223	0.298912
-4.641330	-1.348338	4.021274	0.001181	0.299251
-4.804789	-1.260036	4.031270	0.001212	0.299534
-4.385349	-1.270961	4.041267	0.001133	0.299850
-4.268476	-1.228900	4.051264	0.001112	0.300156
-4.303804	-1.148196	4.061261	0.001118	0.300514
-3.861884	-1.179593	4.071258	0.001036	0.300750
-3.660886	-1.150494	4.081254	0.000998	0.301066
-3.436391	-1.127920	4.091251	0.000956	0.301370
-3.226000	-1.092728	4.101248	0.000917	0.301723
-3.067697	-1.059033	4.111245	0.000887	0.302023
-2.969204	-1.005376	4.121242	0.000869	0.302366
-2.781288	-0.970017	4.131238	0.000834	0.302699
-2.798206	-0.891847	4.141235	0.000837	0.303058
-2.589848	-0.861415	4.151232	0.000798	0.303384
-2.359228	-0.831361	4.161229	0.000755	0.303727
-1.740525	-0.873832	4.171226	0.000640	0.304061
-1.825795	-0.787603	4.181222	0.000655	0.304398
-1.358230	-0.802280	4.191219	0.000568	0.304732
-1.487717	-0.705660	4.201216	0.000592	0.305079
-1.565922	-0.608988	4.211213	0.000607	0.305470
-1.509379	-0.544578	4.221210	0.000596	0.305824
-1.186566	-0.525723	4.231206	0.000536	0.306191
-1.246123	-0.434879	4.241203	0.000547	0.306570
-1.361937	-0.333635	4.251200	0.000568	0.306948
-1.203948	-0.272870	4.261197	0.000539	0.307370
-0.480334	-0.321162	4.271194	0.000404	0.307762
-0.805233	-0.178649	4.281190	0.000464	0.308154
-0.499340	-0.153099	4.291187	0.000407	0.308535
-0.750304	-0.005086	4.301184	0.000454	0.309016
-0.275198	-0.007219	4.311181	0.000365	0.309410
0.060992	0.012625	4.321178	0.000302	0.309789
0.144835	0.098838	4.331174	0.000287	0.310262
0.353384	0.144102	4.341171	0.000248	0.310650
0.000000	0.283572	4.351168	0.000313	0.311001

1.009590	0.376160	4.356173	0.000125	0.312283
1.457911	0.869992	4.361178	0.000041	0.314937
1.753687	1.675718	4.366182	-0.000014	0.318861
3.721018	2.469311	4.371187	-0.000381	0.324041
6.519296	3.416311	4.376192	-0.000903	0.330473
8.909694	4.760954	4.381197	-0.001349	0.338169
12.822397	6.139897	4.386202	-0.002078	0.346990
17.065763	7.806995	4.391206	-0.002870	0.357004
22.735380	9.550227	4.396211	-0.003926	0.368060
28.051693	11.731514	4.401216	-0.004918	0.380216
34.862897	14.021172	4.406221	-0.006188	0.393388
43.325956	16.408536	4.411226	-0.007765	0.407539
53.893985	18.844856	4.416230	-0.009734	0.422681
65.045704	21.631910	4.421235	-0.011813	0.438798
75.047789	25.079898	4.426240	-0.013677	0.455772
83.335184	29.287320	4.431245	-0.015223	0.473503
90.512097	34.127612	4.436250	-0.016563	0.491857
94.483085	39.958322	4.441254	-0.017306	0.510711
97.341762	46.360138	4.446259	-0.017843	0.529901
99.689688	53.200453	4.451264	-0.018284	0.549329
102.629391	60.266508	4.456269	-0.018836	0.568933
105.506052	67.675747	4.461274	-0.019377	0.588696
109.213939	75.236664	4.466278	-0.020072	0.608528
112.240280	83.230849	4.471283	-0.020641	0.628445
114.493384	91.612281	4.476288	-0.021066	0.648301
117.286699	100.146750	4.481293	-0.021592	0.668103
120.458488	108.816078	4.486298	-0.022188	0.687758
122.225169	117.949354	4.491302	-0.022523	0.707299
124.300006	127.184049	4.496307	-0.022915	0.726623
126.325384	136.567700	4.501312	-0.023299	0.745715
127.991980	146.137389	4.506317	-0.023615	0.764560
129.007108	155.914730	4.511322	-0.023811	0.783119
131.502247	165.493375	4.516326	-0.024281	0.801362
132.722709	175.377927	4.521331	-0.024515	0.819338
133.866271	185.313400	4.526336	-0.024735	0.836992
134.894487	195.262442	4.531341	-0.024933	0.854268
136.053796	205.193796	4.536346	-0.025155	0.871210
137.240413	215.107444	4.541350	-0.025382	0.887807
138.362629	225.030351	4.546355	-0.025598	0.904094
139.087433	234.981781	4.551360	-0.025739	0.920029
139.861517	244.884638	4.556365	-0.025890	0.935629
141.068696	254.664491	4.561370	-0.026121	0.950902
141.517049	264.528220	4.566374	-0.026211	0.965860
142.117507	274.313994	4.571379	-0.026329	0.980513
143.074991	283.985025	4.576384	-0.026514	0.994874
143.808995	293.609899	4.581389	-0.026657	1.008909
144.713591	303.144329	4.586394	-0.026832	1.022665
145.455451	312.650348	4.591398	-0.026976	1.036158
146.165233	322.107159	4.596403	-0.027114	1.049403
146.503612	331.557097	4.601408	-0.027184	1.062385
147.273763	340.884518	4.606413	-0.027333	1.075147
147.874546	350.146903	4.611418	-0.027451	1.087633
148.457396	359.379305	4.616422	-0.027566	1.099933
149.274949	368.513360	4.621427	-0.027724	1.112023
149.370765	377.706697	4.626432	-0.027748	1.123898
150.315838	386.713256	4.631437	-0.027930	1.135597
151.023807	395.714918	4.636442	-0.028067	1.147120
151.447199	404.727200	4.641446	-0.028152	1.158479
152.199643	413.612171	4.646451	-0.028298	1.169641
152.993118	422.446926	4.651456	-0.028452	1.180644
153.924479	431.243205	4.656461	-0.028631	1.191527
154.679902	440.021510	4.661466	-0.028777	1.202254
154.899610	448.874271	4.666470	-0.028824	1.212865
155.560479	457.609172	4.671475	-0.028953	1.223333
156.460150	466.263950	4.676480	-0.029126	1.233667
156.970486	474.953054	4.681485	-0.029227	1.243877
157.601451	483.605055	4.686490	-0.029350	1.253984
158.011177	492.262821	4.691494	-0.029432	1.263975
158.818969	500.831926	4.696499	-0.029588	1.273862
159.012157	509.458755	4.701504	-0.029629	1.283622
159.509299	518.047597	4.706509	-0.029728	1.293322
160.037264	526.583791	4.711514	-0.029832	1.302898
160.360224	535.206996	4.716518	-0.029897	1.312461
161.247288	543.650263	4.721523	-0.030068	1.321862
161.451239	552.162271	4.726528	-0.030112	1.331146
162.273449	560.564232	4.731533	-0.030270	1.340359
162.072766	569.132353	4.736538	-0.030239	1.349504
162.549175	577.544514	4.741542	-0.030333	1.358541
162.974310	585.965379	4.746547	-0.030417	1.367519
163.727477	594.310314	4.751552	-0.030563	1.376416
164.456930	602.671826	4.756557	-0.030704	1.385268
164.867337	611.086399	4.761562	-0.030786	1.394064
165.266428	619.455360	4.766566	-0.030866	1.402756
165.601382	627.851781	4.771571	-0.030934	1.411411
165.723466	636.257909	4.776576	-0.030962	1.419988
166.125632	644.616816	4.781581	-0.031043	1.428512
166.443218	652.971645	4.786586	-0.031107	1.436967
167.243644	661.212781	4.791590	-0.031262	1.445339
167.691339	669.554097	4.796595	-0.031351	1.453703
167.686685	677.946242	4.801600	-0.031355	1.461997
168.203715	686.264845	4.806605	-0.031457	1.470256
168.952373	694.509679	4.811610	-0.031602	1.478433
169.189887	702.825958	4.816614	-0.031652	1.486553
169.334014	711.173124	4.821619	-0.031684	1.494644
169.954040	719.391395	4.826624	-0.031805	1.502643
170.396707	727.675782	4.831629	-0.031893	1.510634
170.713029	735.965082	4.836634	-0.031957	1.518568
170.883045	744.265994	4.841638	-0.031994	1.526449
171.080057	752.571126	4.846643	-0.032036	1.534298
171.781537	760.750866	4.851648	-0.032172	1.542066
172.304008	769.000345	4.856653	-0.032275	1.549833
172.655962	777.255272	4.861658	-0.032346	1.557540
173.127635	785.471306	4.866662	-0.032439	1.565191
173.526846	793.731209	4.871667	-0.032519	1.572835
173.870977	801.971893	4.876672	-0.032588	1.580415
174.091958	810.258897	4.881677	-0.032635	1.587983
174.624721	818.449753	4.886682	-0.032739	1.595474
174.886470	826.687113	4.891686	-0.032794	1.602932
175.522165	834.874806	4.896691	-0.032917	1.610365
175.485148	843.171982	4.901696	-0.032916	1.617765
175.951336	851.372041	4.906701	-0.033008	1.625116
176.406179	859.594651	4.911706	-0.033098	1.632453
176.925006	867.758757	4.916710	-0.033200	1.639714
177.045360	876.023178	4.921715	-0.033228	1.646975
177.658517	884.160462	4.926720	-0.033347	1.654162
177.659911	892.426688	4.931725	-0.033353	1.661345
178.044789	900.604953	4.936730	-0.033430	1.668473
178.567132	908.764121	4.941734	-0.033533	1.675574
178.956473	916.951001	4.946739	-0.033611	1.682650
179.113590	925.157083	4.951744	-0.033645	1.689681
179.651438	933.328613	4.956749	-0.033751	1.696705
179.954083	941.517176	4.961754	-0.033813	1.703683
179.933106	949.764108	4.966758	-0.033814	1.710638
180.325947	957.935398	4.971763	-0.033893	1.717556
180.432149	966.114990	4.976768	-0.033918	1.724416
181.178429	974.216048	4.981773	-0.034062	1.731267
181.721704	982.375132	4.986778	-0.034169	1.738112
182.489964	990.468678	4.991782	-0.034317	1.744905
182.557241	998.732790	4.996787	-0.034335	1.751722
182.861075	1006.895905	5.001792	-0.034397	1.758460
183.248707	1015.062071	5.006797	-0.034474	1.765185
183.447148	1023.258246	5.011802	-0.034517	1.771885
183.833899	1031.410612	5.016806	-0.034594	1.778548
183.888406	1039.629289	5.021811	-0.034610	1.785197
184.087806	1047.817116	5.026816	-0.034652	1.791815
184.933210	1055.887485	5.031821	-0.034815	1.798395
185.412701	1063.991650	5.036826	-0.034909	1.804933
185.819979	1072.151025	5.041830	-0.034991	1.811482
186.111768	1080.335177	5.046835	-0.035050	1.818012
186.431123	1088.457590	5.051840	-0.035115	1.824474
186.696489	1096.645854	5.056845	-0.035170	1.830958
187.036682	1104.769031	5.061850	-0.035239	1.837377
187.387867	1112.903086	5.066854	-0.035309	1.843783
187.620861	1121.062712	5.071859	-0.035358	1.850173
188.050157	1129.181393	5.076864	-0.035443	1.856532
188.450183	1137.317079	5.081869	-0.035523	1.862879
188.532539	1145.517231	5.086874	-0.035544	1.869217
188.983987	1153.605678	5.091878	-0.035633	1.875491
189.525504	1161.709515	5.096883	-0.035739	1.881766
189.572344	1169.876726	5.101888	-0.035753	1.888011
189.941018	1178.017880	5.106893	-0.035827	1.894252
190.338852	1186.124943	5.111898	-0.035907	1.900451
190.821612	1194.227136	5.116902	-0.036002	1.906635
191.021492	1202.412529	5.121907	-0.036045	1.912830
191.521693	1210.486746	5.126912	-0.036143	1.918955
191.931857	1218.585004	5.131917	-0.036225	1.925068
192.095958	1226.764617	5.136922	-0.036261	1.931195
192.264565	1234.921598	5.141926	-0.036297	1.937286
192.751567	1243.013198	5.146931	-0.036393	1.943345
192.576705	1251.224937	5.151936	-0.036366	1.949400
193.049213	1259.292169	5.156941	-0.036460	1.955402
193.576470	1267.349594	5.161946	-0.036563	1.961384
193.902704	1275.452662	5.166950	-0.036629	1.967359
194.103154	1283.610218	5.171955	-0.036672	1.973342
194.442581	1291.712908	5.176960	-0.036740	1.979282
194.738582	1299.827369	5.181965	-0.036801	1.985208
194.847279	1307.975098	5.186970	-0.036826	1.991120
195.231273	1316.072984	5.191974	-0.036903	1.997008
195.686394	1324.160201	5.196979	-0.036993	2.002878
195.779923	1332.281538	5.201984	-0.037016	2.008718
195.960593	1340.431577	5.206989	-0.037055	2.014570
196.277844	1348.515349	5.211994	-0.037119	2.020372
196.616342	1356.606312	5.216998	-0.037188	2.026165
196.395101	1364.820707	5.222003	-0.037152	2.031970
196.207481	1372.957354	5.227008	-0.037122	2.037707
196.964848	1380.952138	5.232013	-0.037269	2.043426
197.103106	1389.078715	5.237018	-0.037300	2.049158
197.182422	1397.192733	5.242022	-0.037320	2.054859
197.614069	1405.268885	5.247027	-0.037405	2.060554
197.989794	1413.330245	5.252032	-0.037481	2.066216
198.225766	1421.465972	5.257037	-0.037530	2.071901
198.595553	1429.543392	5.262042	-0.037604	2.077543
198.612254	1437.661704	5.267046	-0.037613	2.083163
199.092705	1445.749689	5.272051	-0.037707	2.088793
199.378908	1453.823024	5.277056	-0.037766	2.094378
199.748251	1461.915161	5.282061	-0.037840	2.099970
199.874781	1470.035470	5.287066	-0.037869	2.105541
200.158322	1478.154614	5.292070	-0.037927	2.111113
200.604007	1486.254268	5.297075	-0.038015	2.116673
200.888713	1494.305911	5.302080	-0.038074	2.122169
201.114103	1502.403622	5.307085	-0.038121	2.127677
201.426006	1510.488272	5.312090	-0.038184	2.133170
201.824605	1518.560180	5.317094	-0.038264	2.138649
202.002876	1526.673205	5.322099	-0.038302	2.144119
201.849523	1534.832641	5.327104	-0.038279	2.149575
202.165264	1542.895107	5.332109	-0.038343	2.154998
202.853871	1550.882964	5.337114	-0.038477	2.160393
203.140951	1558.971365	5.342118	-0.038536	2.165802
203.511365	1567.083141	5.347123	-0.038610	2.171222
203.634487	1575.196499	5.352128	-0.038638	2.176605
203.664318	1583.309754	5.357133	-0.038649	2.181967
203.966599	1591.407525	5.362138	-0.038711	2.187330
204.143473	1599.508052	5.367142	-0.038749	2.192671
204.392880	1607.592668	5.372147	-0.038801	2.197995
204.355148	1615.675200	5.377152	-0.038799	2.203277
204.878792	1623.728273	5.382157	-0.038902	2.208580
205.047563	1631.815755	5.387162	-0.038938	2.213860
205.185728	1639.909194	5.392166	-0.038969	2.219128
205.102584	1648.046922	5.397171	-0.038959	2.224392
205.841594	1656.031744	5.402176	-0.039102	2.229620
206.071207	1664.128103	5.407181	-0.039150	2.234861
206.118425	1672.217517	5.412186	-0.039164	2.240069
206.394291	1680.280098	5.417190	-0.039221	2.245268
206.696364	1688.392569	5.422195	-0.039283	2.250489
206.799435	1696.467539	5.427200	-0.039307	2.255657
207.104583	1704.535832	5.432205	-0.039369	2.260826
207.139267	1712.654646	5.437210	-0.039381	2.265992
207.357688	1720.748699	5.442214	-0.039427	2.271146
207.843512	1728.813749	5.447219	-0.039523	2.276294
208.033795	1736.840714	5.452224	-0.039563	2.281380
208.338375	1744.906839	5.457229	-0.039625	2.286489
208.248886	1753.046058	5.462234	-0.039614	2.291598
208.819802	1761.043556	5.467238	-0.039726	2.296665
209.258610	1769.075872	5.472243	-0.039813	2.301731
209.115320	1777.223238	5.477248	-0.039791	2.306807
209.279316	1785.327843	5.482253	-0.039827	2.311871
209.914316	1793.317473	5.487258	-0.039951	2.316894
210.134725	1801.378544	5.492262	-0.039997	2.321914
210.407854	1809.474483	5.497267	-0.040053	2.326950
210.205996	1817.618793	5.502272	-0.040021	2.331964
210.596927	1825.650785	5.507277	-0.040099	2.336948
210.938870	1833.697240	5.512282	-0.040168	2.341926
211.242384	1841.757137	5.517286	-0.040230	2.346899
211.570411	1849.842235	5.522291	-0.040296	2.351879
211.516569	1857.927844	5.527296	-0.040291	2.356816
212.115630	1865.915880	5.532301	-0.040408	2.361738
212.340921	1874.015561	5.537306	-0.040455	2.366687
212.466852	1882.108504	5.542310	-0.040484	2.371613
212.859345	1890.154756	5.547315	-0.040563	2.376522
212.849931	1898.263898	5.552320	-0.040566	2.381426
213.023781	1906.337881	5.557325	-0.040604	2.386314
212.901539	1914.474618	5.562330	-0.040586	2.391205
213.785598	1922.399148	5.567334	-0.040756	2.396041
213.942683	1930.487316	5.572339	-0.040791	2.400906
214.043341	1938.570596	5.577344	-0.040815	2.405753
214.354166	1946.656262	5.582349	-0.040878	2.410610
214.806954	1954.694938	5.587354	-0.040968	2.415439
214.976924	1962.758332	5.592358	-0.041005	2.420251
215.393013	1970.803272	5.597363	-0.041087	2.425062
215.620456	1978.901954	5.602368	-0.041135	2.429881
215.909718	1986.999416	5.607373	-0.041194	2.434693
216.064778	1995.033769	5.612378	-0.041228	2.439449
216.187764	2003.081263	5.617382	-0.041257	2.444201
216.656455	2011.145826	5.622387	-0.041349	2.448980
216.775099	2019.217567	5.627392	-0.041376	2.453727
217.009792	2027.288394	5.632397	-0.041425	2.458473
217.386187	2035.308223	5.637402	-0.041501	2.463191
217.383000	2043.412316	5.642406	-0.041506	2.467919
217.729683	2051.466460	5.647411	-0.041575	2.472637
217.860102	2059.527467	5.652416	-0.041605	2.477333
217.975892	2067.602277	5.657421	-0.041632	2.482027
218.278500	2075.629467	5.662426	-0.041693	2.486698
218.419854	2083.705967	5.667430	-0.041725	2.491378
218.785212	2091.765321	5.672435	-0.041798	2.496055
218.969738	2099.816344	5.677440	-0.041838	2.500705
219.296060	2107.864609	5.682445	-0.041904	2.505355
219.665857	2115.924313	5.687450	-0.041978	2.510007
219.899296	2124.001588	5.692454	-0.042027	2.514649
220.055354	2132.061310	5.697459	-0.042061	2.519268
220.292171	2140.097845	5.702464	-0.042111	2.523870
220.464467	2148.181395	5.707469	-0.042148	2.528487
220.601403	2156.240134	5.712474	-0.042179	2.533078
220.869394	2164.281052	5.717478	-0.042234	2.537660
221.158095	2172.340645	5.722483	-0.042293	2.542246
221.220336	2180.400329	5.727488	-0.042310	2.546807
221.399659	2188.489710	5.732493	-0.042349	2.551385
221.649109	2196.532368	5.737498	-0.042400	2.555934
221.386883	2204.648658	5.742502	-0.042357	2.560479
221.658174	2212.678440	5.747507	-0.042413	2.565006
222.105617	2220.679835	5.752512	-0.042501	2.569522
222.860507	2228.652372	5.757517	-0.042647	2.574035
222.996575	2236.749706	5.762522	-0.042678	2.578566
223.175345	2244.802715	5.767526	-0.042716	2.583067
223.515239	2252.891650	5.772531	-0.042785	2.587592
223.558202	2261.047611	5.777536	-0.042798	2.592125
223.998968	2269.074510	5.782541	-0.042886	2.596607
224.354883	2277.062152	5.787546	-0.042957	2.601053
224.547782	2285.112430	5.792550	-0.042998	2.605514
224.615876	2293.191998	5.797555	-0.043016	2.609976
224.748041	2301.221528	5.802560	-0.043046	2.614407
224.956355	2309.276566	5.807565	-0.043090	2.618849
225.233204	2317.294162	5.812570	-0.043147	2.623268
225.473599	2325.337693	5.817574	-0.043197	2.627691
225.935721	2333.385630	5.822579	-0.043289	2.632125
226.119474	2341.414185	5.827584	-0.043328	2.636521
226.112922	2349.517978	5.832589	-0.043332	2.640938
226.220934	2357.569770	5.837594	-0.043358	2.645327
226.595550	2365.581346	5.842598	-0.043433	2.649705
226.861798	2373.671050	5.847603	-0.043487	2.654110
226.837119	2381.714138	5.852608	-0.043488	2.658464
227.307115	2389.743066	5.857613	-0.043581	2.662836
227.527387	2397.802258	5.862618	-0.043627	2.667200
227.693824	2405.860515	5.867622	-0.043664	2.671553
228.350798	2413.859181	5.872627	-0.043791	2.675899
228.462440	2421.929187	5.877632	-0.043817	2.680241
228.710835	2429.954871	5.882637	-0.043869	2.684560
228.852117	2438.014859	5.887642	-0.043900	2.688884
228.973447	2446.093849	5.892646	-0.043928	2.693210
229.264085	2454.153631	5.897651	-0.043988	2.697530
229.320977	2462.185067	5.902656	-0.044003	2.701812
229.928350	2470.200818	5.907661	-0.044122	2.706115
229.938043	2478.288995	5.912666	-0.044129	2.710411
229.917804	2486.373595	5.917670	-0.044130	2.714696
230.392384	2494.357635	5.922675	-0.044224	2.718953
230.508097	2502.402371	5.927680	-0.044251	2.723212
230.698809	2510.463794	5.932685	-0.044292	2.727478
231.010198	2518.538314	5.937690	-0.044355	2.731752
231.329227	2526.577834	5.942694	-0.044420	2.736002
231.675531	2534.624405	5.947699	-0.044489	2.740250
231.639027	2542.670365	5.952704	-0.044488	2.744467
231.969610	2550.724938	5.957709	-0.044555	2.748705
232.054719	2558.845838	5.962714	-0.044576	2.752956
232.080443	2566.867287	5.967718	-0.044586	2.757145
232.282472	2574.906435	5.972723	-0.044629	2.761347
232.608101	2582.871882	5.977728	-0.044695	2.765513
232.710056	2590.947510	5.982733	-0.044719	2.769715
232.870646	2599.007477	5.987738	-0.044754	2.773907
233.079376	2607.025817	5.992742	-0.044798	2.778073
233.011803	2615.115986	5.997747	-0.044791	2.782254
233.309687	2623.134265	6.002752	-0.044852	2.786414
233.765793	2631.141922	6.007757	-0.044942	2.790571
234.052006	2639.193795	6.012762	-0.045001	2.794734
234.142326	2647.232718	6.017766	-0.045023	2.798873
234.240984	2655.314881	6.022771	-0.045046	2.803029
234.053857	2663.385685	6.027776	-0.045017	2.807155
234.586062	2671.373086	6.032781	-0.045121	2.811275
234.937364	2679.413669	6.037786	-0.045192	2.815406
235.270516	2687.423069	6.042790	-0.045259	2.819514
235.525271	2695.480381	6.047795	-0.045312	2.823635
235.531391	2703.541476	6.052800	-0.045318	2.827738
235.835096	2711.610742	6.057805	-0.045380	2.831856
236.036839	2719.656867	6.062810	-0.045423	2.835950
236.267266	2727.659033	6.067814	-0.045471	2.840018
236.234533	2735.727677	6.072819	-0.045470	2.844099
236.433420	2743.759129	6.077824	-0.045513	2.848168
236.663832	2751.795487	6.082829	-0.045561	2.852236
236.873253	2759.826002	6.087834	-0.045605	2.856293
237.286097	2767.836204	6.092838	-0.045687	2.860347
237.107323	2775.953234	6.097843	-0.045659	2.864414
237.248930	2783.987438	6.102848	-0.045691	2.868452
237.668987	2792.002757	6.107853	-0.045775	2.872491
237.896487	2800.055116	6.112858	-0.045822	2.876532
238.055447	2808.071629	6.117862	-0.045857	2.880545
238.283185	2816.108577	6.122867	-0.045905	2.884567
238.487691	2824.136281	6.127872	-0.045948	2.888577
238.389962	2832.272007	6.132877	-0.045935	2.892619
238.396317	2840.325634	6.137882	-0.045942	2.896620
238.603601	2848.330763	6.142886	-0.045986	2.900602
239.104084	2856.331920	6.147891	-0.046084	2.904593
239.384116	2864.353156	6.152896	-0.046141	2.908577
239.532103	2872.488156	6.157901	-0.046174	2.912603
239.792173	2880.494120	6.162906	-0.046228	2.916567
239.749860	2888.523104	6.167910	-0.046225	2.920520
239.982979	2896.541978	6.172915	-0.046274	2.924478
240.301788	2904.524857	6.177920	-0.046339	2.928417
240.621639	2912.591777	6.182925	-0.046404	2.932392
240.433536	2920.694531	6.187930	-0.046374	2.936352
240.275252	2928.765905	6.192934	-0.046350	2.940293
240.988205	2936.669290	6.197939	-0.046488	2.944194
241.019614	2944.758086	6.202944	-0.046499	2.948143
241.353049	2952.791385	6.207949	-0.046566	2.952075
241.875826	2960.822616	6.212954	-0.046669	2.956012
241.881968	2968.854938	6.217958	-0.046675	2.959916
242.114569	2976.902204	6.222963	-0.046724	2.963835
242.372264	2984.913058	6.227968	-0.046777	2.967732
242.679803	2992.979519	6.232973	-0.046840	2.971653
242.822679	3001.040375	6.237978	-0.046871	2.975558
242.888184	3009.065910	6.242982	-0.046889	2.979436
243.481317	3017.056076	6.247987	-0.047005	2.983320
243.559603	3025.135085	6.252992	-0.047024	2.987215
243.649297	3033.218266	6.257997	-0.047046	2.991107
243.399072	3041.315306	6.263002	-0.047005	2.994983
243.648466	3049.280018	6.268006	-0.047057	2.998817
243.620319	3057.333617	6.273011	-0.047057	3.002673
243.981975	3065.312903	6.278016	-0.047130	3.006510
243.701302	3073.448747	6.283021	-0.047083	3.010383
243.889185	3081.450229	6.288026	-0.047123	3.014211
244.095198	3089.466620	6.293030	-0.047166	3.018043
244.225921	3097.534098	6.298035	-0.047196	3.021890
244.551528	3105.490802	6.303040	-0.047262	3.025689
245.032410	3113.493284	6.308045	-0.047357	3.029513
245.520373	3121.531082	6.313050	-0.047453	3.033349
245.540918	3129.587539	6.318054	-0.047462	3.037165
245.271359	3137.714295	6.323059	-0.047417	3.040996
246.152104	3145.605099	6.328064	-0.047586	3.044767
245.843216	3153.748315	6.333069	-0.047534	3.048594
245.846223	3161.830629	6.338074	-0.047540	3.052403
246.357455	3169.777213	6.343078	-0.047640	3.056168
246.653313	3177.820047	6.348083	-0.047701	3.059963
246.456316	3185.874239	6.353088	-0.047669	3.063735
247.099803	3193.863912	6.358093	-0.047794	3.067513
247.128723	3201.975303	6.363098	-0.047805	3.071313
247.356759	3210.016786	6.368102	-0.047853	3.075085
247.558002	3218.018868	6.373107	-0.047896	3.078833
247.398095	3226.074612	6.378112	-0.047871	3.082584
247.777355	3234.084133	6.383117	-0.047947	3.086335
247.921799	3242.116225	6.388122	-0.047979	3.090080
248.139156	3250.132551	6.393126	-0.048025	3.093818
248.217951	3258.215875	6.398131	-0.048045	3.097575
248.577018	3266.178826	6.403136	-0.048117	3.101284
248.665723	3274.245054	6.408141	-0.048139	3.105025
248.601840	3282.329104	6.413146	-0.048132	3.108762
248.911532	3290.319481	6.418150	-0.048195	3.112469
249.133305	3298.376484	6.423155	-0.048242	3.116198
249.247941	3306.354441	6.428160	-0.048268	3.119881
249.483223	3314.384030	6.433165	-0.048317	3.123589
249.437853	3322.448070	6.438170	-0.048314	3.127295
249.408965	3330.518649	6.443174	-0.048314	3.131001
249.888027	3338.539811	6.448179	-0.048409	3.134703
249.950272	3346.553686	6.453184	-0.048426	3.138378
249.838713	3354.628433	6.458189	-0.048410	3.142069
250.083806	3362.647099	6.463194	-0.048461	3.145746
250.114412	3370.680828	6.468198	-0.048472	3.149416
250.517481	3378.706925	6.473203	-0.048552	3.153095
250.891902	3386.684412	6.478208	-0.048627	3.156746
251.160629	3394.731871	6.483213	-0.048683	3.160420
251.351506	3402.738769	6.488218	-0.048723	3.164068
251.064554	3410.834990	6.493222	-0.048675	3.167731
251.515708	3418.857729	6.498227	-0.048765	3.171389
251.906873	3426.856524	6.503232	-0.048843	3.175029
251.794476	3434.916650	6.508237	-0.048827	3.178670
251.953325	3442.942246	6.513242	-0.048862	3.182304
252.076477	3450.979884	6.518246	-0.048890	3.185938
252.671839	3458.969140	6.523251	-0.049006	3.189566
252.603099	3467.041163	6.528256	-0.048999	3.193198
252.830878	3475.081177	6.533261	-0.049046	3.196824
252.861196	3483.130031	6.538266	-0.049057	3.200442
253.134288	3491.075543	6.543270	-0.049113	3.204020
253.334348	3499.153463	6.548275	-0.049156	3.207650
253.445432	3507.233132	6.553280	-0.049182	3.211273
253.415030	3515.257312	6.558285	-0.049181	3.214860
253.911974	3523.266638	6.563290	-0.049279	3.218460
253.995680	3531.279085	6.568294	-0.049300	3.222039
254.246100	3539.339987	6.573299	-0.049352	3.225643
254.019145	3547.397836	6.578304	-0.049315	3.229222
253.942427	3555.481183	6.583309	-0.049306	3.232814
254.335293	3563.443314	6.588314	-0.049384	3.236368
254.651056	3571.405484	6.593318	-0.049449	3.239915
254.771840	3579.453387	6.598323	-0.049476	3.243488
255.110439	3587.455902	6.603328	-0.049545	3.247046
255.114738	3595.543208	6.608333	-0.049551	3.250623
255.366064	3603.539963	6.613338	-0.049603	3.254167
255.537971	3611.569968	6.618342	-0.049640	3.257718
255.339303	3619.697209	6.623347	-0.049608	3.261293
255.571764	3627.642106	6.628352	-0.049657	3.264802
255.804103	3635.674495	6.633357	-0.049705	3.268345
256.058566	3643.732866	6.638362	-0.049758	3.271897
255.851766	3651.765900	6.643366	-0.049725	3.275414
256.301916	3659.731219	6.648371	-0.049814	3.278925
256.537356	3667.745743	6.653376	-0.049863	3.282446
256.609023	3675.814728	6.658381	-0.049882	3.285979
256.938580	3683.833076	6.663386	-0.049948	3.289497
257.090736	3691.884983	6.668390	-0.049982	3.293018
257.359268	3699.935687	6.673395	-0.050037	3.296540
257.084123	3707.989435	6.678400	-0.049991	3.300038
257.215299	3715.972338	6.683405	-0.050021	3.303518
257.096447	3724.072615	6.688410	-0.050004	3.307035
257.358361	3732.098108	6.693414	-0.050058	3.310530
257.515095	3740.129472	6.698419	-0.050093	3.314021
257.761324	3748.092852	6.703424	-0.050144	3.317482
258.110474	3756.119638	6.708429	-0.050214	3.320970
258.397221	3764.108631	6.713434	-0.050273	3.324436
258.341040	3772.170059	6.718438	-0.050267	3.327917
258.896459	3780.186738	6.723443	-0.050376	3.331398
258.915700	3788.226522	6.728448	-0.050385	3.334864
258.851609	3796.295154	6.733453	-0.050378	3.338337
259.403446	3804.279765	6.738458	-0.050486	3.341793
258.950306	3812.379318	6.743462	-0.050407	3.345256
259.328351	3820.399089	6.748467	-0.050483	3.348713
259.683697	3828.369612	6.753472	-0.050554	3.352145
260.036202	3836.426015	6.758477	-0.050625	3.355610
259.856658	3844.448561	6.763482	-0.050597	3.359037
259.853793	3852.464483	6.768486	-0.050602	3.362464
260.460184	3860.469012	6.773491	-0.050720	3.365905
260.147704	3868.553331	6.778496	-0.050667	3.369343
260.435344	3876.571590	6.783501	-0.050726	3.372771
260.437643	3884.646386	6.788506	-0.050732	3.376209
260.386710	3892.660596	6.793510	-0.050728	3.379616
260.880242	3900.634375	6.798515	-0.050825	3.383023
260.771385	3908.708084	6.803520	-0.050810	3.386446
260.870347	3916.770574	6.808525	-0.050833	3.389869
260.896954	3924.839365	6.813530	-0.050844	3.393288
261.766961	3932.721601	6.818534	-0.051011	3.396655
261.617855	3940.805502	6.823539	-0.050988	3.400068
262.057902	3948.715619	6.828544	-0.051076	3.403424
262.195998	3956.794903	6.833549	-0.051107	3.406838
262.194531	3964.883086	6.838554	-0.051112	3.410248
262.500335	3972.853969	6.843558	-0.051174	3.413615
262.643216	3980.913456	6.848563	-0.051206	3.417010
262.548759	3988.982445	6.853568	-0.051193	3.420398
262.715346	3996.968267	6.858573	-0.051230	3.423757
262.787323	4005.053357	6.863578	-0.051248	3.427150
263.055575	4013.042120	6.868582	-0.051304	3.430507
263.366734	4021.032275	6.873587	-0.051367	3.433863
263.641639	4029.051344	6.878592	-0.051423	3.437226
263.843121	4037.104690	6.883597	-0.051466	3.440597
264.343774	4045.064907	6.888602	-0.051564	3.443937
264.206119	4053.163027	6.893606	-0.051544	3.447308
264.378067	4061.203738	6.898611	-0.051581	3.450664
264.317411	4069.241480	6.903616	-0.051575	3.454006
264.642957	4077.238002	6.908621	-0.051641	3.457342
264.481864	4085.348441	6.913626	-0.051617	3.460705
264.252891	4093.346532	6.918630	-0.051579	3.464016
264.470770	4101.385829	6.923635	-0.051625	3.467356
264.749454	4109.365440	6.928640	-0.051682	3.470670
265.303610	4117.331224	6.933645	-0.051791	3.473984
265.037643	4125.449841	6.938650	-0.051746	3.477331
265.127647	4133.436989	6.943654	-0.051768	3.480632
265.648607	4141.366017	6.948659	-0.051871	3.483921
265.701139	4149.430605	6.953664	-0.051886	3.487246
266.086299	4157.513436	6.958669	-0.051963	3.490587
266.110901	4165.533554	6.963674	-0.051973	3.493887
265.914579	4173.581933	6.968678	-0.051941	3.497188
266.277555	4181.632893	6.973683	-0.052014	3.500506
266.494916	4189.588241	6.978688	-0.052060	3.503776
266.629922	4197.652161	6.983693	-0.052090	3.507085
267.181419	4205.636707	6.988698	-0.052198	3.510372
267.098619	4213.683552	6.993702	-0.052188	3.513660
267.478725	4221.698469	6.998707	-0.052264	3.516948
267.277627	4229.778872	7.003712	-0.052232	3.520240
267.119880	4237.808993	7.008717	-0.052208	3.523511
267.486876	4245.819374	7.013722	-0.052282	3.526787
267.025373	4253.905681	7.018726	-0.052201	3.530064
267.396137	4261.924717	7.023731	-0.052275	3.533337
267.483745	4269.907957	7.028736	-0.052297	3.536584
267.711932	4277.906188	7.033741	-0.052345	3.539839
267.785723	4285.922244	7.038746	-0.052364	3.543092
268.128281	4293.908873	7.043750	-0.052433	3.546340
268.518457	4301.965684	7.048755	-0.052510	3.549614
268.556762	4310.067831	7.053760	-0.052523	3.552892
268.863706	4318.065027	7.058765	-0.052585	3.556133
269.089235	4326.029442	7.063770	-0.052633	3.559356
269.203672	4334.011935	7.068774	-0.052659	3.562579
269.285369	4342.111924	7.073779	-0.052680	3.565846
269.082805	4350.132237	7.078784	-0.052647	3.569069
269.333681	4358.130238	7.083789	-0.052699	3.572294
269.311474	4366.230698	7.088794	-0.052700	3.575549
270.113747	4374.086218	7.093798	-0.052855	3.578728
269.846490	4382.243863	7.098803	-0.052810	3.581993
269.996845	4390.203948	7.103808	-0.052844	3.585188
270.171215	4398.263799	7.108813	-0.052881	3.588421
270.439904	4406.299814	7.113818	-0.052937	3.591644
270.263803	4414.326830	7.118822	-0.052909	3.594847
270.286892	4422.390043	7.123827	-0.052919	3.598068
270.309004	4430.418302	7.128832	-0.052928	3.601272
270.474470	4438.379754	7.133837	-0.052964	3.604451
270.704166	4446.411057	7.138842	-0.053012	3.607657
271.157975	4454.423848	7.143846	-0.053102	3.610859
271.052959	4462.478335	7.148851	-0.053088	3.614058
271.014234	4470.507591	7.153856	-0.053086	3.617247
271.310063	4478.529155	7.158861	-0.053146	3.620439
271.933162	4486.468160	7.163866	-0.053267	3.623605
271.751490	4494.559824	7.168870	-0.053239	3.626806
272.168645	4502.595853	7.173875	-0.053322	3.629998
272.206579	4510.609437	7.178880	-0.053334	3.633169
271.920702	4518.727462	7.183885	-0.053286	3.636369
272.003488	4526.703644	7.188890	-0.053307	3.639520
272.106664	4534.677418	7.193894	-0.053331	3.642668
272.501899	4542.726225	7.198899	-0.053410	3.645851
272.331660	4550.732548	7.203904	-0.053384	3.648999
272.610009	4558.770494	7.208909	-0.053441	3.652169
272.635086	4566.819833	7.213914	-0.053451	3.655334
273.245228	4574.725451	7.218918	-0.053570	3.658456
273.357433	4582.821716	7.223923	-0.053596	3.661636
273.436154	4590.821454	7.228928	-0.053616	3.664774
273.877436	4598.835607	7.233933	-0.053703	3.667926
273.505039	4607.009763	7.238938	-0.053639	3.671115
274.121458	4614.881376	7.243942	-0.053759	3.674210
274.181029	4622.955730	7.248947	-0.053776	3.677366
274.241870	4630.966561	7.253952	-0.053792	3.680495
274.133531	4638.982213	7.258957	-0.053777	3.683619
274.292427	4647.032065	7.263962	-0.053812	3.686760
274.640737	4654.991743	7.268966	-0.053882	3.689868
274.982054	4663.026206	7.273971	-0.053951	3.693003
275.205672	4671.049911	7.278976	-0.053998	3.696128
275.117701	4679.129690	7.283981	-0.053987	3.699264
275.293372	4687.139794	7.288986	-0.054025	3.702377
274.934324	4695.212746	7.293990	-0.053963	3.705498
275.697732	4703.176936	7.298995	-0.054111	3.708603
275.589032	4711.273304	7.304000	-0.054096	3.711734
276.005176	4719.268873	7.309005	-0.054179	3.714837
276.172625	4727.270031	7.314010	-0.054215	3.717933
276.085258	4735.297217	7.319014	-0.054204	3.721030
276.340035	4743.251017	7.324019	-0.054257	3.724105
276.590266	4751.298511	7.329024	-0.054309	3.727213
276.929234	4759.352703	7.334029	-0.054377	3.730323
276.928008	4767.409221	7.339034	-0.054382	3.733424
276.886432	4775.422270	7.344038	-0.054380	3.736503
276.761805	4783.473331	7.349043	-0.054362	3.739593
276.517658	4791.502942	7.354048	-0.054321	3.742669
276.948045	4799.426282	7.359053	-0.054407	3.745719
276.889023	4807.513295	7.364058	-0.054401	3.748817
277.156501	4815.498743	7.369062	-0.054456	3.751881
277.847438	4823.464564	7.374067	-0.054590	3.754945
277.475891	4831.545838	7.379072	-0.054526	3.758026
277.688371	4839.585811	7.384077	-0.054571	3.761102
277.363147	4847.620732	7.389082	-0.054516	3.764160
277.316108	4855.645287	7.394086	-0.054512	3.767219
277.456447	4863.689953	7.399091	-0.054544	3.770288
278.091735	4871.574785	7.404096	-0.054667	3.773305
278.476019	4879.615763	7.409101	-0.054744	3.776373
279.023865	4887.603121	7.414106	-0.054851	3.779422
278.935719	4895.672945	7.419110	-0.054840	3.782485
279.166964	4903.688310	7.424115	-0.054888	3.785532
279.097287	4911.765920	7.429120	-0.054881	3.788593
279.174379	4919.841816	7.434125	-0.054900	3.791654
278.915133	4927.881422	7.439130	-0.054857	3.794692
279.079962	4935.845235	7.444134	-0.054893	3.797708
279.702763	4943.854424	7.449139	-0.055015	3.800749
279.679073	4951.787264	7.454144	-0.055015	3.803744
279.571133	4959.906108	7.459149	-0.055001	3.806806
279.848206	4967.926980	7.464154	-0.055058	3.809836
279.844892	4975.951375	7.469158	-0.055062	3.812859
280.611437	4983.969896	7.474163	-0.055210	3.815895
280.417669	4991.984580	7.479168	-0.055179	3.818905
280.524923	5000.020779	7.484173	-0.055205	3.821928
280.726150	5008.049483	7.489178	-0.055247	3.824948
280.725610	5016.082447	7.494182	-0.055253	3.827962
280.631808	5024.181407	7.499187	-0.055240	3.830996
280.916629	5032.099382	7.504192	-0.055299	3.833969
280.661138	5040.181347	7.509197	-0.055256	3.836989
280.749485	5048.207698	7.514202	-0.055278	3.839993
280.661592	5056.198022	7.519206	-0.055267	3.842978
280.878616	5064.226969	7.524211	-0.055313	3.845981
281.067957	5072.178533	7.529216	-0.055353	3.848953
281.143627	5080.249268	7.534221	-0.055373	3.851964
280.690394	5088.367705	7.539226	-0.055293	3.854979
281.105821	5096.261272	7.544230	-0.055376	3.857927
281.365420	5104.326962	7.549235	-0.055430	3.860933
281.705912	5112.252460	7.554240	-0.055498	3.863887
281.216477	5120.422176	7.559245	-0.055412	3.866911
281.398959	5128.447296	7.564250	-0.055452	3.869893
281.581162	5136.507340	7.569254	-0.055491	3.872886
281.446709	5144.588977	7.574259	-0.055471	3.875879
281.899775	5152.439788	7.579264	-0.055561	3.878795
282.090566	5160.441337	7.584269	-0.055601	3.881760
282.248051	5168.437429	7.589274	-0.055636	3.884720
282.417503	5176.420432	7.594278	-0.055673	3.887672
282.569668	5184.514600	7.599283	-0.055707	3.890663
282.244771	5192.576136	7.604288	-0.055651	3.893631
282.965848	5200.515991	7.609293	-0.055791	3.896572
282.920427	5208.542213	7.614298	-0.055788	3.899527
283.051969	5216.547902	7.619302	-0.055817	3.902476
283.561911	5224.518795	7.624307	-0.055918	3.905418
283.780787	5232.557556	7.629312	-0.055964	3.908376
284.057249	5240.633429	7.634317	-0.056020	3.911347
284.001536	5248.658495	7.639322	-0.056015	3.914291
283.942361	5256.676992	7.644326	-0.056010	3.917229
283.971131	5264.718970	7.649331	-0.056020	3.920176
283.884168	5272.727949	7.654336	-0.056009	3.923106
284.601747	5280.656781	7.659341	-0.056148	3.926021
284.562026	5288.716321	7.664346	-0.056146	3.928966
284.748991	5296.785386	7.669350	-0.056186	3.931917
284.975896	5304.820861	7.674355	-0.056234	3.934854
285.012330	5312.828699	7.679360	-0.056246	3.937775
285.000778	5320.893845	7.684365	-0.056249	3.940715
285.661698	5328.798154	7.689370	-0.056377	3.943605
285.780706	5336.866935	7.694374	-0.056404	3.946544
285.616436	5344.949461	7.699379	-0.056379	3.949480
285.689453	5352.984544	7.704384	-0.056398	3.952401
286.111238	5360.977733	7.709389	-0.056482	3.955311
286.064774	5369.002484	7.714394	-0.056478	3.958221
286.401641	5376.968090	7.719398	-0.056546	3.961116
286.649542	5384.977775	7.724403	-0.056598	3.964022
286.600529	5393.004898	7.729408	-0.056594	3.966927
286.699109	5401.064185	7.734413	-0.056618	3.969844
286.894389	5409.085756	7.739418	-0.056659	3.972747
286.757807	5417.139253	7.744422	-0.056639	3.975654
286.899139	5425.162369	7.749427	-0.056671	3.978552
286.772984	5433.170794	7.754432	-0.056653	3.981439
287.155043	5441.091623	7.759437	-0.056729	3.984300
287.647035	5449.138685	7.764442	-0.056826	3.987207
287.836908	5457.177888	7.769446	-0.056866	3.990104
287.822688	5465.226825	7.774451	-0.056869	3.992998
288.082316	5473.231896	7.779456	-0.056923	3.995879
288.205655	5481.208534	7.784461	-0.056951	3.998746
288.450297	5489.266091	7.789466	-0.057002	4.001642
288.338786	5497.252501	7.794470	-0.056986	4.004504
288.324182	5505.366365	7.799475	-0.056989	4.007411
288.756536	5513.341148	7.804480	-0.057075	4.010274
288.921423	5521.348372	7.809485	-0.057110	4.013142
288.815304	5529.433498	7.814490	-0.057096	4.016031
289.096856	5537.349852	7.819494	-0.057154	4.018864
289.180228	5545.442951	7.824499	-0.057174	4.021755
289.001829	5553.445489	7.829504	-0.057147	4.024607
289.213587	5561.482081	7.834509	-0.057191	4.027476
289.711314	5569.477189	7.839514	-0.057289	4.030333
289.434792	5577.572341	7.844518	-0.057243	4.033210
290.109057	5585.518416	7.849523	-0.057374	4.036048
290.332103	5593.466220	7.854528	-0.057421	4.038877
290.387309	5601.530124	7.859533	-0.057436	4.041743
290.407354	5609.527465	7.864538	-0.057445	4.044582
290.742909	5617.531296	7.869542	-0.057513	4.047427
290.787919	5625.648990	7.874547	-0.057527	4.050306
290.887108	5633.616685	7.879552	-0.057550	4.053130
291.215557	5641.667206	7.884557	-0.057617	4.055985
290.889713	5649.737289	7.889562	-0.057561	4.058835
291.192897	5657.685564	7.894566	-0.057623	4.061649
291.318626	5665.675505	7.899571	-0.057652	4.064474
291.352392	5673.727249	7.904576	-0.057663	4.067316
291.711705	5681.724558	7.909581	-0.057735	4.070143
292.255759	5689.724963	7.914586	-0.057842	4.072972
292.111441	5697.773022	7.919590	-0.057820	4.075805
292.593657	5705.775996	7.924595	-0.057915	4.078629
292.477418	5713.848267	7.929600	-0.057899	4.081467
292.561239	5721.790631	7.934605	-0.057920	4.084260
292.951884	5729.900729	7.939610	-0.057998	4.087115
292.763345	5737.910988	7.944614	-0.057968	4.089924
293.183453	5745.919166	7.949619	-0.058052	4.092740
293.464562	5753.939687	7.954624	-0.058109	4.095555
293.317480	5761.954082	7.959629	-0.058087	4.098361
293.346898	5770.035367	7.964634	-0.058098	4.101190
293.729360	5777.908759	7.969638	-0.058174	4.103950
293.890837	5786.059240	7.974643	-0.058210	4.106802
293.598881	5794.088079	7.979648	-0.058161	4.109602
293.764172	5802.092251	7.984653	-0.058197	4.112399
294.034628	5810.102211	7.989658	-0.058252	4.115197
294.178138	5818.049348	7.994662	-0.058284	4.117970
294.379700	5826.132273	7.999667	-0.058327	4.120789
294.399314	5834.043219	8.004672	-0.058336	4.123543
294.463184	5842.154311	8.009677	-0.058353	4.126366
294.604494	5850.138619	8.014682	-0.058385	4.129144
294.411047	5858.218687	8.019686	-0.058354	4.131949
294.740074	5866.246182	8.024691	-0.058420	4.134741
294.377581	5874.248261	8.029696	-0.058358	4.137512
294.706627	5882.247991	8.034701	-0.058425	4.140291
294.893246	5890.206391	8.039706	-0.058465	4.143051
295.222482	5898.234221	8.044710	-0.058531	4.145835
295.625229	5906.232330	8.049715	-0.058612	4.148608
295.131819	5914.362609	8.054720	-0.058525	4.151413
295.756956	5922.265754	8.059725	-0.058647	4.154152
295.712600	5930.332176	8.064730	-0.058644	4.156938
295.504317	5938.332229	8.069734	-0.058610	4.159696
295.538318	5946.436368	8.074739	-0.058622	4.162491
296.155120	5954.310827	8.079744	-0.058742	4.165213
296.467432	5962.345939	8.084749	-0.058805	4.167984
296.302931	5970.524455	8.089754	-0.058780	4.170797
296.173831	5978.483800	8.094758	-0.058761	4.173534
296.334451	5986.512460	8.099763	-0.058796	4.176295
296.780609	5994.428161	8.104768	-0.058885	4.179020
296.838953	6002.501222	8.109773	-0.058901	4.181792
297.056462	6010.496691	8.114778	-0.058947	4.184537
296.689287	6018.593577	8.119782	-0.058883	4.187309
297.165952	6026.603422	8.124787	-0.058977	4.190059
297.377302	6034.614231	8.129792	-0.059022	4.192804
297.271989	6042.686006	8.134797	-0.059008	4.195564
297.133234	6050.709402	8.139802	-0.058987	4.198306
297.719711	6058.654829	8.144806	-0.059102	4.201028
297.466861	6066.663311	8.149811	-0.059060	4.203759
297.737355	6074.677611	8.154816	-0.059115	4.206497
298.032773	6082.629565	8.159821	-0.059176	4.209213
297.931809	6090.768571	8.164826	-0.059162	4.211985
297.999789	6098.701005	8.169830	-0.059180	4.214688
297.989075	6106.848519	8.174835	-0.059183	4.217461
298.342254	6114.757219	8.179840	-0.059254	4.220155
298.765396	6122.729490	8.184845	-0.059338	4.222869
298.565133	6130.810849	8.189850	-0.059306	4.225612
298.539810	6138.820938	8.194854	-0.059307	4.228331
298.791560	6146.868771	8.199859	-0.059359	4.231064
299.157958	6154.810512	8.204864	-0.059433	4.233761
299.355726	6162.884454	8.209869	-0.059475	4.236498
299.696890	6170.865140	8.214874	-0.059543	4.239204
299.209710	6178.922057	8.219878	-0.059458	4.241925
299.840215	6186.870913	8.224883	-0.059581	4.244620
299.941744	6194.948530	8.229888	-0.059605	4.247351
299.682630	6202.995238	8.234893	-0.059562	4.250066
299.724451	6211.028615	8.239898	-0.059575	4.252777
299.841436	6219.024141	8.244902	-0.059602	4.255475
300.246935	6226.992071	8.249907	-0.059683	4.258165
300.162534	6235.069708	8.254912	-0.059672	4.260886
300.345975	6243.030463	8.259917	-0.059712	4.263567
300.579225	6251.064471	8.264922	-0.059760	4.266273
300.572435	6259.108820	8.269926	-0.059764	4.268977
301.297483	6267.097118	8.274931	-0.059905	4.271668
301.424143	6275.060535	8.279936	-0.059934	4.274344
301.665308	6283.123445	8.284941	-0.059984	4.277052
301.662467	6291.117478	8.289946	-0.059988	4.279732
301.672228	6299.171151	8.294950	-0.059996	4.282432
302.307920	6307.112634	8.299955	-0.060119	4.285098
302.467373	6315.115480	8.304960	-0.060154	4.287778
302.638776	6323.184693	8.309965	-0.060191	4.290479
302.858102	6331.237203	8.314970	-0.060237	4.293173
302.681100	6339.304714	8.319974	-0.060210	4.295866
302.785683	6347.273278	8.324979	-0.060234	4.298528
302.785039	6355.350733	8.329984	-0.060240	4.301223
303.399133	6363.235212	8.334989	-0.060359	4.303858
303.524548	6371.322302	8.339994	-0.060388	4.306554
303.214043	6379.373441	8.344998	-0.060335	4.309233
303.726415	6387.376146	8.350003	-0.060436	4.311901
303.561650	6395.390254	8.355008	-0.060411	4.314565
303.827478	6403.368151	8.360013	-0.060465	4.317219
304.331939	6411.347820	8.365018	-0.060564	4.319875
304.249265	6419.358726	8.370022	-0.060554	4.322534
304.497212	6427.415196	8.375027	-0.060606	4.325209
304.703234	6435.451434	8.380032	-0.060649	4.327875
304.788438	6443.455178	8.385037	-0.060671	4.330528
304.745516	6451.508499	8.390042	-0.060668	4.333195
304.729365	6459.502904	8.395046	-0.060670	4.335841
305.190322	6467.479371	8.400051	-0.060761	4.338483
305.063945	6475.551448	8.405056	-0.060743	4.341151
305.205783	6483.497314	8.410061	-0.060775	4.343777
305.641218	6491.572627	8.415066	-0.060861	4.346447
305.541059	6499.556730	8.420070	-0.060848	4.349080
305.914022	6507.658766	8.425075	-0.060922	4.351755
306.163497	6515.615261	8.430080	-0.060974	4.354379
306.254060	6523.644752	8.435085	-0.060996	4.357024
306.425600	6531.645084	8.440090	-0.061033	4.359659
306.351278	6539.634938	8.445094	-0.061025	4.362287
306.509935	6547.663375	8.450099	-0.061060	4.364927
306.446270	6555.655051	8.455104	-0.061053	4.367553
306.456930	6563.721230	8.460109	-0.061060	4.370201
306.272740	6571.768917	8.465114	-0.061031	4.372841
306.355127	6579.769048	8.470118	-0.061052	4.375465
306.462533	6587.762059	8.475123	-0.061077	4.378086
306.962614	6595.750721	8.480128	-0.061175	4.380706
307.367389	6603.768295	8.485133	-0.061256	4.383334
307.052197	6611.856260	8.490138	-0.061203	4.385978
307.213799	6619.814147	8.495142	-0.061238	4.388581
307.506043	6627.879317	8.500147	-0.061298	4.391218
307.672569	6635.844875	8.505152	-0.061334	4.393821
307.667265	6643.899006	8.510157	-0.061338	4.396450
307.852340	6651.834556	8.515162	-0.061378	4.399039
308.108886	6659.881725	8.520166	-0.061431	4.401664
308.148163	6667.878555	8.525171	-0.061444	4.404270
308.102052	6675.959457	8.530176	-0.061440	4.406901
308.351478	6684.005063	8.535181	-0.061492	4.409520
308.246984	6692.090005	8.540186	-0.061478	4.412149
308.548731	6700.059825	8.545190	-0.061539	4.414741
309.422784	6708.066319	8.550195	-0.061707	4.417347
309.241772	6716.089245	8.555200	-0.061679	4.419951
309.290033	6724.108894	8.560205	-0.061693	4.422553
309.700567	6732.127858	8.565210	-0.061775	4.425155
309.867042	6740.115502	8.570215	-0.061811	4.427745
310.039885	6748.214819	8.575219	-0.061849	4.430369
309.812561	6756.228399	8.580224	-0.061812	4.432961
310.171321	6764.211593	8.585229	-0.061884	4.435546
310.295186	6772.210276	8.590234	-0.061912	4.438132
310.240516	6780.259153	8.595239	-0.061907	4.440733
310.759958	6788.232780	8.600243	-0.062009	4.443310
310.844234	6796.269544	8.605248	-0.062030	4.445904
310.924178	6804.279160	8.610253	-0.062050	4.448488
311.179637	6812.375003	8.615258	-0.062103	4.451099
311.303965	6820.315856	8.620263	-0.062131	4.453658
311.441586	6828.433780	8.625267	-0.062162	4.456272
311.346984	6836.379529	8.630272	-0.062150	4.458828
311.270493	6844.457720	8.635277	-0.062141	4.461426
311.316223	6852.392077	8.640282	-0.062155	4.463976
311.425016	6860.430217	8.645287	-0.062180	4.466559
311.558430	6868.477570	8.650291	-0.062210	4.469143
311.443963	6876.552617	8.655296	-0.062194	4.471733
311.590578	6884.458232	8.660301	-0.062227	4.474269
311.588750	6892.567280	8.665306	-0.062232	4.476868
311.964424	6900.440944	8.670311	-0.062307	4.479391
311.959054	6908.521367	8.675315	-0.062311	4.481978
312.007115	6916.493504	8.680320	-0.062325	4.484528
312.262057	6924.534910	8.685325	-0.062378	4.487101
312.065565	6932.609293	8.690330	-0.062347	4.489680
312.203638	6940.597985	8.695335	-0.062378	4.492232
312.774965	6948.582972	8.700339	-0.062489	4.494783
313.043952	6956.608727	8.705344	-0.062545	4.497344
312.707714	6964.654279	8.710349	-0.062488	4.499908
313.272673	6972.602495	8.715354	-0.062598	4.502443
313.179480	6980.624852	8.720359	-0.062586	4.504997
313.181503	6988.703629	8.725363	-0.062592	4.507568
313.062026	6996.698072	8.730368	-0.062575	4.510111
313.548007	7004.665743	8.735373	-0.062670	4.512646
314.129348	7012.671460	8.740378	-0.062784	4.515191
314.356344	7020.628667	8.745383	-0.062831	4.517719
314.699512	7028.710246	8.750387	-0.062900	4.520285
314.240179	7036.715199	8.755392	-0.062820	4.522823
314.403061	7044.756630	8.760397	-0.062856	4.525372
314.542091	7052.786147	8.765402	-0.062887	4.527917
314.731441	7060.832578	8.770407	-0.062927	4.530465
315.201164	7068.849388	8.775411	-0.063020	4.533004
315.084678	7076.857568	8.780416	-0.063004	4.535536
315.137661	7084.852839	8.785421	-0.063019	4.538064
315.536669	7092.841610	8.790426	-0.063098	4.540589
315.610574	7100.824965	8.795431	-0.063117	4.543110
315.501749	7108.927155	8.800435	-0.063103	4.545667
315.375124	7116.942929	8.805440	-0.063084	4.548194
315.325416	7124.981319	8.810445	-0.063080	4.550728
315.762552	7132.944987	8.815450	-0.063167	4.553238
316.047197	7140.928292	8.820455	-0.063225	4.555753
316.176936	7148.955002	8.825459	-0.063255	4.558279
315.916853	7156.979158	8.830464	-0.063211	4.560802
316.057455	7164.941220	8.835469	-0.063243	4.563306
316.392265	7173.015703	8.840474	-0.063310	4.565843
316.127367	7180.993451	8.845479	-0.063266	4.568348
316.291044	7189.121930	8.850483	-0.063302	4.570899
316.368599	7197.050469	8.855488	-0.063322	4.573386
316.299417	7205.113772	8.860493	-0.063314	4.575913
316.521115	7213.095052	8.865498	-0.063361	4.578415
316.412886	7221.116607	8.870503	-0.063346	4.580926
316.984974	7229.048920	8.875507	-0.063458	4.583410
317.037456	7237.120359	8.880512	-0.063473	4.585934
316.943306	7245.139098	8.885517	-0.063460	4.588441
317.657312	7253.183135	8.890522	-0.063599	4.590956
317.796299	7261.142632	8.895527	-0.063630	4.593441
317.915887	7269.217658	8.900531	-0.063657	4.595962
317.534395	7277.206282	8.905536	-0.063592	4.598453
317.932210	7285.228856	8.910541	-0.063671	4.600955
318.204623	7293.181299	8.915546	-0.063727	4.603433
318.079523	7301.247967	8.920551	-0.063709	4.605945
317.625824	7309.357319	8.925555	-0.063630	4.608468
317.973347	7317.302543	8.930560	-0.063700	4.610940
317.996032	7325.316510	8.935565	-0.063709	4.613432
318.247045	7333.313022	8.940570	-0.063761	4.615917
318.601651	7341.285498	8.945575	-0.063832	4.618394
319.052131	7349.343635	8.950579	-0.063922	4.620895
319.003110	7357.290793	8.955584	-0.063918	4.623361
319.402799	7365.331800	8.960589	-0.063997	4.625854
319.483178	7373.404177	8.965594	-0.064018	4.628356
319.797779	7381.376669	8.970599	-0.064081	4.630825
319.614957	7389.460314	8.975603	-0.064053	4.633328
319.946852	7397.461698	8.980608	-0.064120	4.635803
319.685348	7405.427878	8.985613	-0.064076	4.638267
320.132816	7413.456013	8.990618	-0.064165	4.640748
320.175964	7421.386891	8.995623	-0.064178	4.643198
320.163428	7429.493978	9.000627	-0.064181	4.645701
319.851820	7437.545888	9.005632	-0.064128	4.648185
320.003842	7445.583610	9.010637	-0.064162	4.650664
320.053272	7453.591256	9.015642	-0.064176	4.653132
320.269803	7461.588999	9.020647	-0.064222	4.655596
320.350249	7469.612334	9.025651	-0.064242	4.658067
320.237281	7477.625677	9.030656	-0.064226	4.660533
320.443684	7485.575406	9.035661	-0.064270	4.662978
320.561588	7493.645127	9.040666	-0.064297	4.665459
320.856166	7501.635020	9.045671	-0.064357	4.667914
320.775954	7509.750812	9.050675	-0.064348	4.670406
321.434891	7517.660333	9.055680	-0.064476	4.672833
321.711078	7525.694754	9.060685	-0.064532	4.675298
322.015897	7533.699970	9.065690	-0.064594	4.677752
321.772770	7541.722685	9.070695	-0.064554	4.680211
321.869641	7549.746202	9.075699	-0.064578	4.682668
322.201518	7557.685786	9.080704	-0.064645	4.685098
321.906638	7565.786216	9.085709	-0.064595	4.687577
322.060468	7573.794036	9.090714	-0.064629	4.690025
322.313830	7581.777795	9.095719	-0.064682	4.692465
322.577341	7589.781182	9.100723	-0.064736	4.694910
323.015466	7597.768981	9.105728	-0.064823	4.697348
323.093499	7605.778246	9.110733	-0.064842	4.699792
323.266211	7613.840199	9.115738	-0.064880	4.702250
323.181412	7621.807081	9.120743	-0.064869	4.704679
323.732529	7629.862689	9.125747	-0.064977	4.707132
323.401714	7637.915818	9.130752	-0.064921	4.709585
323.545837	7645.942344	9.135757	-0.064953	4.712028
323.490026	7653.980366	9.140762	-0.064948	4.714473
323.656587	7661.995910	9.145767	-0.064984	4.716910
324.112309	7669.963712	9.150771	-0.065074	4.719330
323.936306	7678.000294	9.155776	-0.065047	4.721771
324.506373	7685.918548	9.160781	-0.065158	4.724174
324.617163	7694.029887	9.165786	-0.065184	4.726635
324.210880	7702.005489	9.170791	-0.065114	4.729054
324.776057	7710.078524	9.175795	-0.065224	4.731500
324.846046	7718.028113	9.180800	-0.065243	4.733908
324.993995	7726.121530	9.185805	-0.065275	4.736358
325.351356	7734.085416	9.190810	-0.065347	4.738767
325.558801	7742.126809	9.195815	-0.065391	4.741199
325.336758	7750.143557	9.200819	-0.065355	4.743623
325.393145	7758.176685	9.205824	-0.065371	4.746050
325.391628	7766.204217	9.210829	-0.065376	4.748474
325.594813	7774.272602	9.215834	-0.065419	4.750909
325.698210	7782.175702	9.220839	-0.065443	4.753293
325.929996	7790.283732	9.225843	-0.065492	4.755737
326.201025	7798.227453	9.230848	-0.065547	4.758130
326.229959	7806.237522	9.235853	-0.065558	4.760543
326.440579	7814.232495	9.240858	-0.065603	4.762950
326.132933	7822.252974	9.245863	-0.065551	4.765364
326.105542	7830.359886	9.250867	-0.065551	4.767802
326.696040	7838.241857	9.255872	-0.065666	4.770170
326.678717	7846.316625	9.260877	-0.065668	4.772596
327.170351	7854.353593	9.265882	-0.065765	4.775008
326.800997	7862.377025	9.270887	-0.065701	4.777417
326.695854	7870.415340	9.275891	-0.065687	4.779829
326.861630	7878.460442	9.280896	-0.065723	4.782241
326.702380	7886.388557	9.285901	-0.065699	4.784617
326.973357	7894.466892	9.290906	-0.065755	4.787036
327.041188	7902.441889	9.295911	-0.065772	4.789423
327.178399	7910.527061	9.300915	-0.065803	4.791842
327.481088	7918.407315	9.305920	-0.065865	4.794198
327.103858	7926.555457	9.310925	-0.065800	4.796635
327.913892	7934.446433	9.315930	-0.065956	4.798990
327.596745	7942.509274	9.320935	-0.065902	4.801399
327.436010	7950.502591	9.325939	-0.065877	4.803786
327.833562	7958.532767	9.330944	-0.065957	4.806180
327.958472	7966.546993	9.335949	-0.065985	4.808569
328.469286	7974.605716	9.340954	-0.066086	4.810969
328.012778	7982.627017	9.345959	-0.066006	4.813360
328.771781	7990.060555	9.350963	-0.066152	4.815571
329.084238	7994.873099	9.355968	-0.066214	4.817002

328.950236	7997.398909	9.360973	-0.066190	4.817754
328.903667	7998.896763	9.365978	-0.066183	4.818200
328.743668	7999.396283	9.370983	-0.066153	4.818349
329.285061	8000.304879	9.375987	-0.066255	4.818617
329.053808	8000.495997	9.380992	-0.066212	4.818675
329.226378	8000.372330	9.385997	-0.066244	4.818637
329.529412	8000.451882	9.391002	-0.066300	4.818660
329.696315	8000.420496	9.396007	-0.066331	4.818650
329.508768	8000.407537	9.401011	-0.066297	4.818647
329.556496	8000.487930	9.406016	-0.066306	4.818670
329.512682	8000.539832	9.411021	-0.066297	4.818686
329.573663	8000.351726	9.416026	-0.066309	4.818630
329.186898	8000.452643	9.421031	-0.066237	4.818661
329.775372	8000.410009	9.426035	-0.066346	4.818646
329.648384	8000.445074	9.431040	-0.066323	4.818657
329.662356	8000.364449	9.436045	-0.066325	4.818633
329.850470	8000.440392	9.441050	-0.066361	4.818655
329.967488	8000.499658	9.446055	-0.066382	4.818672
330.020761	8000.440539	9.451059	-0.066392	4.818654
330.128392	8000.479740	9.456064	-0.066412	4.818666
329.979278	8000.377028	9.461069	-0.066385	4.818636
330.225581	8000.422252	9.466074	-0.066431	4.818648
329.746787	8000.371877	9.471079	-0.066341	4.818635
330.057462	8000.311946	9.476083	-0.066399	4.818616
330.201960	8000.543695	9.481088	-0.066426	4.818684
330.129003	8000.351725	9.486093	-0.066413	4.818628
330.111476	8000.460647	9.491098	-0.066410	4.818660
329.935911	8000.534955	9.496103	-0.066377	4.818683
330.200939	8000.320145	9.501107	-0.066426	4.818618
330.086935	8000.530651	9.506112	-0.066405	4.818681
330.042616	8000.412524	9.511117	-0.066397	4.818646
330.134208	8000.415831	9.516122	-0.066414	4.818647
330.131896	8000.444141	9.521127	-0.066414	4.818655
330.244006	8000.318627	9.526131	-0.066434	4.818617
330.504884	8000.443807	9.531136	-0.066483	4.818654
330.369527	8000.445177	9.536141	-0.066458	4.818654
330.643077	8000.460325	9.541146	-0.066509	4.818658
330.413421	8000.449959	9.546151	-0.066466	4.818656
330.343713	8000.332547	9.551155	-0.066453	4.818621
330.695427	8000.343475	9.556160	-0.066519	4.818623
330.878892	8000.445598	9.561165	-0.066553	4.818653
330.905775	8000.418666	9.566170	-0.066558	4.818645
330.831163	8000.452322	9.571175	-0.066544	4.818655
330.639831	8000.420420	9.576179	-0.066509	4.818646
331.137286	8000.454258	9.581184	-0.066601	4.818654
330.997162	8000.477606	9.586189	-0.066575	4.818662
331.115739	8000.465526	9.591194	-0.066597	4.818658
330.907881	8000.379879	9.596199	-0.066559	4.818633
331.222554	8000.457492	9.601203	-0.066617	4.818655
331.004868	8000.425242	9.606208	-0.066577	4.818646
331.065546	8000.413449	9.611213	-0.066588	4.818642
331.127905	8000.512930	9.616218	-0.066600	4.818672
331.005174	8000.402165	9.621223	-0.066577	4.818639
331.179066	8000.402357	9.626227	-0.066609	4.818639
330.835665	8000.449268	9.631232	-0.066546	4.818654
331.324476	8000.385385	9.636237	-0.066637	4.818633
331.158987	8000.439885	9.641242	-0.066606	4.818650
330.847699	8000.511358	9.646247	-0.066548	4.818672
331.503574	8000.373058	9.651251	-0.066670	4.818629
331.406197	8000.466239	9.656256	-0.066652	4.818657
331.401450	8000.456733	9.661261	-0.066651	4.818654
331.455548	8000.483687	9.666266	-0.066661	4.818662
331.692095	8000.352461	9.671271	-0.066705	4.818622
331.578407	8000.480063	9.676275	-0.066684	4.818660
331.461536	8000.409256	9.681280	-0.066662	4.818640
331.278382	8000.496060	9.686285	-0.066628	4.818666
331.208559	8000.389139	9.691290	-0.066615	4.818635
331.241362	8000.414763	9.696295	-0.066622	4.818642
331.719972	8000.488239	9.701299	-0.066711	4.818662
331.405698	8000.349761	9.706304	-0.066652	4.818622
331.221907	8000.423962	9.711309	-0.066618	4.818645
331.008383	8000.347686	9.716314	-0.066578	4.818623
331.360559	8000.488766	9.721319	-0.066644	4.818664
331.465096	8000.431370	9.726323	-0.066664	4.818646
331.225392	8000.439762	9.731328	-0.066619	4.818650
331.565171	8000.380216	9.736333	-0.066682	4.818630
331.664944	8000.441357	9.741338	-0.066701	4.818648
331.528334	8000.516179	9.746343	-0.066676	4.818671
331.824268	8000.416172	9.751347	-0.066731	4.818640
331.502891	8000.458124	9.756352	-0.066671	4.818654
331.153853	8000.431491	9.761357	-0.066606	4.818647
330.941594	8000.405611	9.766362	-0.066566	4.818640
331.457105	8000.370417	9.771367	-0.066662	4.818628
331.453103	8000.424944	9.776371	-0.066662	4.818644
331.458737	8000.451260	9.781376	-0.066663	4.818652
331.545960	8000.385240	9.786381	-0.066679	4.818632
331.734361	8000.484283	9.791386	-0.066714	4.818661
331.426966	8000.311260	9.796391	-0.066657	4.818610
331.351086	8000.348048	9.801395	-0.066643	4.818622
331.834690	8000.506604	9.806400	-0.066733	4.818667
331.970006	8000.405532	9.811405	-0.066758	4.818636
331.721069	8000.469428	9.816410	-0.066712	4.818656
332.039115	8000.451579	9.821415	-0.066771	4.818650
331.619459	8000.443956	9.826419	-0.066693	4.818649
331.716833	8000.449440	9.831424	-0.066711	4.818650
331.766778	8000.330451	9.836429	-0.066721	4.818615
331.860370	8000.525855	9.841434	-0.066738	4.818673
331.658446	8000.421391	9.846439	-0.066701	4.818642
331.619010	8000.457609	9.851443	-0.066693	4.818653
331.643558	8000.379219	9.856448	-0.066698	4.818630
331.092362	8000.318440	9.861453	-0.066595	4.818614
331.098095	8000.158989	9.866458	-0.066596	4.818566
330.618205	8000.160026	9.871463	-0.066507	4.818569
331.284051	8000.144649	9.876467	-0.066631	4.818561
330.653078	8000.039796	9.881472	-0.066513	4.818533
331.004387	8000.189254	9.886477	-0.066579	4.818576
331.556824	8000.315124	9.891482	-0.066682	4.818611
331.528010	8000.437545	9.896487	-0.066677	4.818648
331.435587	8000.342922	9.901491	-0.066659	4.818620
331.637012	8000.448433	9.906496	-0.066697	4.818650
331.757110	8000.458413	9.911501	-0.066719	4.818653
332.082324	8000.458501	9.916506	-0.066780	4.818652
331.705152	8000.341234	9.921511	-0.066710	4.818618
331.247832	8000.121112	9.926515	-0.066625	4.818555
330.978744	8000.149061	9.931520	-0.066574	4.818564
330.896917	8000.178423	9.936525	-0.066559	4.818573
331.175241	8000.064541	9.941530	-0.066611	4.818538
331.259250	8000.220979	9.946535	-0.066627	4.818584
331.647744	8000.330000	9.951539	-0.066699	4.818615
331.648066	8000.234499	9.956544	-0.066699	4.818587
331.803497	8000.299520	9.961549	-0.066728	4.818605
331.964083	8000.448576	9.966554	-0.066758	4.818649
332.184730	8000.413701	9.971559	-0.066800	4.818638
332.118206	8000.389737	9.976563	-0.066787	4.818631
331.504568	8000.392156	9.981568	-0.066673	4.818634
331.366218	8000.305324	9.986573	-0.066647	4.818609
331.968486	8000.370981	9.991578	-0.066759	4.818626
331.562973	8000.379289	9.996583	-0.066684	4.818630
331.912830	8000.314627	10.001587	-0.066749	4.818610
331.816009	8000.428807	10.006592	-0.066731	4.818644
331.855059	8000.420928	10.011597	-0.066738	4.818641
331.939623	8000.373764	10.016602	-0.066754	4.818627
331.832003	8000.347161	10.021607	-0.066734	4.818620
331.929651	8000.416671	10.026611	-0.066752	4.818640
331.332531	8000.295461	10.031616	-0.066641	4.818606
331.560838	8000.235496	10.036621	-0.066684	4.818587
332.035016	8000.242790	10.041626	-0.066772	4.818588
332.220029	8000.389020	10.046631	-0.066807	4.818630
332.188451	8000.350822	10.051635	-0.066801	4.818619
332.105550	8000.387518	10.056640	-0.066785	4.818630
332.125243	8000.356293	10.061645	-0.066789	4.818621
332.096109	8000.330723	10.066650	-0.066784	4.818614
331.773677	8000.419891	10.071655	-0.066724	4.818641
332.113175	8000.358242	10.076659	-0.066787	4.818622
332.440732	8000.422384	10.081664	-0.066848	4.818640
332.070488	8000.264275	10.086669	-0.066779	4.818594
331.977981	8000.313439	10.091674	-0.066762	4.818609
331.750120	8000.396505	10.096679	-0.066720	4.818635
331.366738	8000.159512	10.101683	-0.066648	4.818566
331.621054	8000.251023	10.106688	-0.066696	4.818592
331.437101	8000.311578	10.111693	-0.066661	4.818610
331.672247	8000.333568	10.116698	-0.066705	4.818616
331.577019	8000.329169	10.121703	-0.066688	4.818615
332.181333	8000.326632	10.126707	-0.066800	4.818612
332.217885	8000.389041	10.131712	-0.066807	4.818630
332.015357	8000.442004	10.136717	-0.066769	4.818647
332.433227	8000.399230	10.141722	-0.066847	4.818633
332.620921	8000.460482	10.146727	-0.066882	4.818650
332.163818	8000.448166	10.151731	-0.066797	4.818648
331.710631	8000.297362	10.156736	-0.066713	4.818605
331.848880	8000.308631	10.161741	-0.066738	4.818608
331.970707	8000.311288	10.166746	-0.066761	4.818608
331.896059	8000.422611	10.171751	-0.066747	4.818642
332.476145	8000.433402	10.176755	-0.066856	4.818643
332.499654	8000.420070	10.181760	-0.066860	4.818639
332.200497	8000.311176	10.186765	-0.066804	4.818607
332.453880	8000.452010	10.191770	-0.066851	4.818648
331.666251	8000.321991	10.196775	-0.066705	4.818613
331.703912	8000.232228	10.201779	-0.066712	4.818586
331.891340	8000.287176	10.206784	-0.066747	4.818601
331.865043	8000.319369	10.211789	-0.066742	4.818611
331.626793	8000.189240	10.216794	-0.066698	4.818573
331.677238	8000.376727	10.221799	-0.066707	4.818629
331.754196	8000.302175	10.226803	-0.066721	4.818606
331.608411	8000.176412	10.231808	-0.066694	4.818570
331.412150	8000.190625	10.236813	-0.066658	4.818575
331.551816	8000.006698	10.241818	-0.066684	4.818519
331.922272	8000.291805	10.246823	-0.066753	4.818603
331.719558	8000.128558	10.251827	-0.066715	4.818555
331.893177	8000.244197	10.256832	-0.066747	4.818589
331.918624	8000.343194	10.261837	-0.066752	4.818618
332.363360	8000.349053	10.266842	-0.066835	4.818618
332.222012	8000.362938	10.271847	-0.066809	4.818623
332.299823	8000.351371	10.276851	-0.066823	4.818619
331.911562	8000.348360	10.281856	-0.066751	4.818620
332.826556	8000.355165	10.286861	-0.066922	4.818618
332.837787	8000.428787	10.291866	-0.066924	4.818640
332.750791	8000.520008	10.296871	-0.066908	4.818667
332.433397	8000.337401	10.301875	-0.066849	4.818614
332.457562	8000.473117	10.306880	-0.066853	4.818654
332.378457	8000.353476	10.311885	-0.066838	4.818619
332.034004	8000.169469	10.316890	-0.066774	4.818566
332.469481	8000.380920	10.321895	-0.066855	4.818627
332.408915	8000.368580	10.326899	-0.066844	4.818624
332.700743	8000.438551	10.331904	-0.066899	4.818643
332.494675	8000.544996	10.336909	-0.066860	4.818676
332.403436	8000.291898	10.341914	-0.066843	4.818601
332.271534	8000.316403	10.346919	-0.066819	4.818609
332.781636	8000.381901	10.351923	-0.066914	4.818626
332.906657	8000.467518	10.356928	-0.066937	4.818651
332.679463	8000.390007	10.361933	-0.066895	4.818629
332.741328	8000.443304	10.366938	-0.066906	4.818645
332.800871	8000.411554	10.371943	-0.066918	4.818635
332.517619	8000.346950	10.376947	-0.066865	4.818617
332.668492	8000.471742	10.381952	-0.066893	4.818653
332.578648	8000.283736	10.386957	-0.066876	4.818598
332.770409	8000.433206	10.391962	-0.066912	4.818641
332.816135	8000.456902	10.396967	-0.066921	4.818648
332.530383	8000.342935	10.401971	-0.066867	4.818615
332.103081	8000.162034	10.406976	-0.066788	4.818563
332.609966	8000.368129	10.411981	-0.066882	4.818623
332.373377	8000.272654	10.416986	-0.066838	4.818595
332.382159	8000.439654	10.421991	-0.066840	4.818645
332.242801	8000.214264	10.426995	-0.066814	4.818578
332.439823	8000.462461	10.432000	-0.066851	4.818651
332.623080	8000.384060	10.437005	-0.066885	4.818627
332.428229	8000.272341	10.442010	-0.066849	4.818595
332.671466	8000.520100	10.447015	-0.066894	4.818668
332.630058	8000.333781	10.452019	-0.066886	4.818612
332.403763	8000.336051	10.457024	-0.066844	4.818614
332.517144	8000.416266	10.462029	-0.066865	4.818637
332.840000	8000.416324	10.467034	-0.066926	4.818636
332.350056	8000.288122	10.472039	-0.066834	4.818600
332.643246	8000.455721	10.477043	-0.066889	4.818649
332.131237	8000.336675	10.482048	-0.066794	4.818615
332.290322	8000.248511	10.487053	-0.066823	4.818588
332.721311	8000.469353	10.492058	-0.066904	4.818652
332.351879	8000.356383	10.497063	-0.066835	4.818620
332.609222	8000.451089	10.502067	-0.066883	4.818647
332.168577	8000.145112	10.507072	-0.066801	4.818558
332.476331	8000.403163	10.512077	-0.066858	4.818634
332.734148	8000.362479	10.517082	-0.066906	4.818620
332.924047	8000.489885	10.522087	-0.066942	4.818658
332.809631	8000.301554	10.527091	-0.066920	4.818602
332.633450	8000.461921	10.532096	-0.066888	4.818650
332.619181	8000.313746	10.537101	-0.066885	4.818606
332.793920	8000.453545	10.542106	-0.066918	4.818647
332.954114	8000.452510	10.547111	-0.066948	4.818646
332.815948	8000.373023	10.552115	-0.066922	4.818623
332.720133	8000.371764	10.557120	-0.066904	4.818623
332.076935	8000.226853	10.562125	-0.066784	4.818583
332.571529	8000.239665	10.567130	-0.066876	4.818585
333.154986	8000.522346	10.572135	-0.066985	4.818666
332.960669	8000.228003	10.577139	-0.066949	4.818580
333.173732	8000.429185	10.582144	-0.066989	4.818639
332.896262	8000.306929	10.587149	-0.066937	4.818603
333.155760	8000.504525	10.592154	-0.066986	4.818661
332.637282	8000.407431	10.597159	-0.066889	4.818634
333.152351	8000.431014	10.602163	-0.066985	4.818639
333.244437	8000.435379	10.607168	-0.067002	4.818640
333.080228	8000.423772	10.612173	-0.066972	4.818637
332.788283	8000.470308	10.617178	-0.066917	4.818652
333.147830	8000.428867	10.622183	-0.066984	4.818639
333.348968	8000.391636	10.627187	-0.067022	4.818627
333.137786	8000.409848	10.632192	-0.066982	4.818633
333.212050	8000.408730	10.637197	-0.066996	4.818632
333.292390	8000.423436	10.642202	-0.067011	4.818636
333.068353	8000.506554	10.647207	-0.066970	4.818662
333.399615	8000.410161	10.652211	-0.067031	4.818632
333.354754	8000.529227	10.657216	-0.067023	4.818668
333.359736	8000.382352	10.662221	-0.067024	4.818624
333.243576	8000.482635	10.667226	-0.067002	4.818654
333.439804	8000.381313	10.672231	-0.067039	4.818623
333.396179	8000.521388	10.677235	-0.067031	4.818665
333.057357	8000.427710	10.682240	-0.066968	4.818639
333.376316	8000.410924	10.687245	-0.067027	4.818632
333.127886	8000.375116	10.692250	-0.066981	4.818623
333.123319	8000.426488	10.697255	-0.066980	4.818638
333.036263	8000.392807	10.702259	-0.066964	4.818628
332.657356	8000.366827	10.707264	-0.066894	4.818622
332.949822	8000.396922	10.712269	-0.066948	4.818630
333.251515	8000.462826	10.717274	-0.067004	4.818648
333.406602	8000.476419	10.722279	-0.067033	4.818652
333.373417	8000.425603	10.727283	-0.067027	4.818637
333.108890	8000.557519	10.732288	-0.066978	4.818677
333.448393	8000.330034	10.737293	-0.067041	4.818608
333.488556	8000.513197	10.742298	-0.067049	4.818662
333.012033	8000.435547	10.747303	-0.066960	4.818641
333.413420	8000.371566	10.752307	-0.067035	4.818620
333.146600	8000.417384	10.757312	-0.066985	4.818635
332.826729	8000.478247	10.762317	-0.066926	4.818654
333.380119	8000.346995	10.767322	-0.067029	4.818613
333.349099	8000.441053	10.772327	-0.067023	4.818641
333.349342	8000.390679	10.777331	-0.067023	4.818626
332.856244	8000.437713	10.782336	-0.066931	4.818642
332.968153	8000.324786	10.787341	-0.066952	4.818608
333.256755	8000.395765	10.792346	-0.067006	4.818628
332.692072	8000.341097	10.797351	-0.066901	4.818614
333.426655	8000.432646	10.802355	-0.067038	4.818639
333.492627	8000.450312	10.807360	-0.067050	4.818644
333.204700	8000.419231	10.812365	-0.066996	4.818635
333.572670	8000.516449	10.817370	-0.067065	4.818663
333.546264	8000.377556	10.822375	-0.067060	4.818622
333.454255	8000.479207	10.827379	-0.067043	4.818652
333.391895	8000.500430	10.832384	-0.067031	4.818659
333.317415	8000.383995	10.837389	-0.067018	4.818625
333.669635	8000.512494	10.842394	-0.067083	4.818661
333.501874	8000.482996	10.847399	-0.067052	4.818653
333.661897	8000.388544	10.852403	-0.067082	4.818625
333.285296	8000.467552	10.857408	-0.067012	4.818650
333.077276	8000.428077	10.862413	-0.066973	4.818639
333.223500	8000.369131	10.867418	-0.067000	4.818620
333.118101	8000.374042	10.872423	-0.066981	4.818622
333.093200	8000.351676	10.877427	-0.066976	4.818616
332.981599	8000.347060	10.882432	-0.066955	4.818615
333.322877	8000.428180	10.887437	-0.067019	4.818638
333.074301	8000.344088	10.892442	-0.066973	4.818614
333.157503	8000.521520	10.897447	-0.066988	4.818666
332.965572	8000.196770	10.902451	-0.066952	4.818570
333.240158	8000.484829	10.907456	-0.067004	4.818655
333.026460	8000.316181	10.912461	-0.066964	4.818605
333.314358	8000.431234	10.917466	-0.067018	4.818639
333.358791	8000.427624	10.922471	-0.067026	4.818637
333.231737	8000.361927	10.927475	-0.067002	4.818618
332.850919	8000.343268	10.932480	-0.066931	4.818614
332.987369	8000.486763	10.937485	-0.066957	4.818656
333.167981	8000.355848	10.942490	-0.066991	4.818617
333.077000	8000.380892	10.947495	-0.066974	4.818625
333.260587	8000.253164	10.952499	-0.067008	4.818586
333.397439	8000.528916	10.957504	-0.067034	4.818667
333.311530	8000.399735	10.962509	-0.067018	4.818629
333.455153	8000.529682	10.967514	-0.067044	4.818667
333.350441	8000.330980	10.972519	-0.067025	4.818609
333.557100	8000.422922	10.977523	-0.067063	4.818635
333.683382	8000.507509	10.982528	-0.067087	4.818660
333.713902	8000.459632	10.987533	-0.067093	4.818645
333.828283	8000.426505	10.992538	-0.067114	4.818635
333.636657	8000.485909	10.997543	-0.067078	4.818654
333.371963	8000.463531	11.002547	-0.067029	4.818648
333.735650	8000.467278	11.007552	-0.067097	4.818648
333.454970	8000.363869	11.012557	-0.067045	4.818618
333.675205	8000.544158	11.017562	-0.067086	4.818671
333.553917	8000.402964	11.022567	-0.067063	4.818629
333.839703	8000.492802	11.027571	-0.067116	4.818655
333.665521	8000.501005	11.032576	-0.067084	4.818658
333.547052	8000.415478	11.037581	-0.067062	4.818633
333.463397	8000.368196	11.042586	-0.067046	4.818619
333.344716	8000.440107	11.047591	-0.067024	4.818641
333.512757	8000.412935	11.052595	-0.067056	4.818632
333.196519	8000.356291	11.057600	-0.066997	4.818617
333.146873	8000.270623	11.062605	-0.066988	4.818591
333.476736	8000.349493	11.067610	-0.067049	4.818614
333.436571	8000.392000	11.072615	-0.067042	4.818626
333.601921	8000.317561	11.077619	-0.067072	4.818604
333.093040	8000.293017	11.082624	-0.066978	4.818598
333.262414	8000.348780	11.087629	-0.067009	4.818614
333.099154	8000.253219	11.092634	-0.066979	4.818586
332.916954	8000.336887	11.097639	-0.066945	4.818612
333.193401	8000.467533	11.102643	-0.066997	4.818650
333.250075	8000.342332	11.107648	-0.067007	4.818612
333.591456	8000.453893	11.112653	-0.067071	4.818644
333.187708	8000.384549	11.117658	-0.066996	4.818625
332.988848	8000.363039	11.122663	-0.066959	4.818620
332.938394	8000.013918	11.127667	-0.066949	4.818516
333.054059	8000.212764	11.132672	-0.066971	4.818575
333.293030	8000.234807	11.137677	-0.067015	4.818580
333.501308	8000.305778	11.142682	-0.067054	4.818600
333.030040	8000.358348	11.147687	-0.066967	4.818618
333.013700	8000.255277	11.152691	-0.066964	4.818587
333.140488	8000.292636	11.157696	-0.066987	4.818598
332.833880	8000.119618	11.162701	-0.066930	4.818548
333.008256	8000.318189	11.167706	-0.066963	4.818606
332.717643	8000.193663	11.172711	-0.066909	4.818570
332.855560	8000.217523	11.177715	-0.066934	4.818577
333.106754	8000.250223	11.182720	-0.066981	4.818586
333.189982	8000.375173	11.187725	-0.066997	4.818622
333.320826	8000.121850	11.192730	-0.067021	4.818546
332.905815	8000.291667	11.197735	-0.066944	4.818599
333.145765	8000.303227	11.202739	-0.066989	4.818601
333.282392	8000.396345	11.207744	-0.067014	4.818628
333.724558	8000.305612	11.212749	-0.067096	4.818600
333.550257	8000.363145	11.217754	-0.067064	4.818617
333.031522	8000.346866	11.222759	-0.066967	4.818615
333.031736	8000.132758	11.227763	-0.066967	4.818551
333.130267	8000.316685	11.232768	-0.066986	4.818605
332.992915	8000.273945	11.237773	-0.066960	4.818593
332.975443	8000.127827	11.242778	-0.066957	4.818550
332.951735	8000.273409	11.247783	-0.066953	4.818593
332.683012	8000.107189	11.252787	-0.066903	4.818545
332.781941	8000.080156	11.257792	-0.066921	4.818536
333.064243	8000.177288	11.262797	-0.066974	4.818564
333.093140	8000.278432	11.267802	-0.066979	4.818594
333.284599	8000.394313	11.272807	-0.067015	4.818628
333.019916	8000.196655	11.277811	-0.066966	4.818570
333.337237	8000.258565	11.282816	-0.067025	4.818587
333.251482	8000.317265	11.287821	-0.067009	4.818605
333.518421	8000.305041	11.292826	-0.067059	4.818600
333.334251	8000.465305	11.297831	-0.067025	4.818649
333.699179	8000.293784	11.302835	-0.067092	4.818596
333.364132	8000.461506	11.307840	-0.067030	4.818647
333.664193	8000.357355	11.312845	-0.067086	4.818615
333.709732	8000.329618	11.317850	-0.067095	4.818607
333.771705	8000.486830	11.322855	-0.067106	4.818653
333.522184	8000.470948	11.327859	-0.067060	4.818650
333.903483	8000.487524	11.332864	-0.067131	4.818653
333.687675	8000.397564	11.337869	-0.067091	4.818627
333.800679	8000.473579	11.342874	-0.067112	4.818649
333.650603	8000.435917	11.347879	-0.067084	4.818639
333.589913	8000.354300	11.352883	-0.067073	4.818615
333.017948	8000.306882	11.357888	-0.066966	4.818603
332.983844	8000.054538	11.362893	-0.066960	4.818528
333.272898	8000.325991	11.367898	-0.067014	4.818607
332.763661	8000.185989	11.372903	-0.066919	4.818568
333.112889	8000.233624	11.377907	-0.066984	4.818581
333.054828	8000.119508	11.382912	-0.066973	4.818547
332.685631	8000.171326	11.387917	-0.066904	4.818564
332.819187	8000.176236	11.392922	-0.066929	4.818565
332.404602	8000.119352	11.397927	-0.066852	4.818549
332.750848	8000.060939	11.402931	-0.066917	4.818531
333.139645	8000.383035	11.407936	-0.066989	4.818625
333.102605	8000.153741	11.412941	-0.066982	4.818557
333.418502	8000.135863	11.417946	-0.067041	4.818550
332.679223	8000.301409	11.422951	-0.066904	4.818602
333.186629	8000.231476	11.427955	-0.066998	4.818580
333.004279	8000.253217	11.432960	-0.066964	4.818587
332.856572	8000.205093	11.437965	-0.066937	4.818573
332.706738	8000.090819	11.442970	-0.066909	4.818540
332.829015	8000.212083	11.447975	-0.066932	4.818575
332.539197	8000.017249	11.452979	-0.066877	4.818518
333.221823	8000.200469	11.457984	-0.067005	4.818570
333.317632	8000.248966	11.462989	-0.067023	4.818584
333.251659	8000.022440	11.467994	-0.067010	4.818517
333.194963	8000.184381	11.472999	-0.067000	4.818566
333.043899	8000.129915	11.478003	-0.066972	4.818550
333.094355	8000.089649	11.483008	-0.066981	4.818538
332.670668	8000.148097	11.488013	-0.066902	4.818557
332.759797	8000.144025	11.493018	-0.066919	4.818555
333.488163	8000.387681	11.498023	-0.067055	4.818625
333.418940	8000.258721	11.503027	-0.067042	4.818587
333.186255	8000.350121	11.508032	-0.066999	4.818615
333.028210	8000.097192	11.513037	-0.066969	4.818540
333.031604	8000.119281	11.518042	-0.066970	4.818547
332.571588	7999.980982	11.523047	-0.066884	4.818507
333.117254	8000.200182	11.528051	-0.066986	4.818571
333.421331	8000.385771	11.533056	-0.067043	4.818625
333.095978	8000.171569	11.538061	-0.066982	4.818562
332.569916	8000.040796	11.543066	-0.066884	4.818525
332.934566	8000.240821	11.548071	-0.066952	4.818583
333.264471	8000.105575	11.553075	-0.067013	4.818542
332.891234	8000.136348	11.558080	-0.066944	4.818552
332.843501	8000.342489	11.563085	-0.066935	4.818614
333.546615	8000.345458	11.568090	-0.067066	4.818612
333.423153	8000.369025	11.573095	-0.067043	4.818620
333.743750	8000.333368	11.578099	-0.067103	4.818608
333.677181	8000.367130	11.583104	-0.067091	4.818618
333.410894	8000.200937	11.588109	-0.067041	4.818570
333.244992	8000.283771	11.593114	-0.067010	4.818595
333.270379	8000.272563	11.598119	-0.067015	4.818591
333.210004	8000.026169	11.603123	-0.067004	4.818518
333.289254	8000.209842	11.608128	-0.067019	4.818573
333.020000	8000.053060	11.613133	-0.066968	4.818527
333.259013	8000.152772	11.618138	-0.067013	4.818556
333.190391	8000.316656	11.623143	-0.067000	4.818605
332.794030	8000.015458	11.628147	-0.066926	4.818517
333.032715	8000.298841	11.633152	-0.066971	4.818600
333.270984	8000.296735	11.638157	-0.067015	4.818599
333.284849	8000.186713	11.643162	-0.067018	4.818566
333.778332	8000.322319	11.648167	-0.067110	4.818604
333.522443	8000.284313	11.653171	-0.067062	4.818594
333.695257	8000.345370	11.658176	-0.067095	4.818611
333.648300	8000.411929	11.663181	-0.067086	4.818631
333.807866	8000.358406	11.668186	-0.067116	4.818615
333.825871	8000.435268	11.673191	-0.067119	4.818638
333.859011	8000.394773	11.678195	-0.067125	4.818625
333.704603	8000.374897	11.683200	-0.067097	4.818620
334.010330	8000.440857	11.688205	-0.067154	4.818639
333.800683	8000.357276	11.693210	-0.067115	4.818615
333.490178	8000.332195	11.698215	-0.067057	4.818608
333.782480	8000.326604	11.703219	-0.067111	4.818605
333.653708	8000.250388	11.708224	-0.067087	4.818583
333.180782	8000.305036	11.713229	-0.066999	4.818601
333.604553	8000.245548	11.718234	-0.067078	4.818582
333.778928	8000.436778	11.723239	-0.067111	4.818638
333.768146	8000.280247	11.728243	-0.067109	4.818592
333.561789	8000.357300	11.733248	-0.067070	4.818615
333.723224	8000.331091	11.738253	-0.067101	4.818607
333.881788	8000.466485	11.743258	-0.067130	4.818647
334.037512	8000.447548	11.748263	-0.067159	4.818640
334.039940	8000.334225	11.753267	-0.067160	4.818607
333.775777	8000.474543	11.758272	-0.067111	4.818650
334.042310	8000.428727	11.763277	-0.067160	4.818635
334.033304	8000.363535	11.768282	-0.067159	4.818615
333.959403	8000.448633	11.773287	-0.067145	4.818641
333.757548	8000.302178	11.778291	-0.067107	4.818598
334.036973	8000.367791	11.783296	-0.067159	4.818617
334.035299	8000.535711	11.788301	-0.067159	4.818667
333.737064	8000.260982	11.793306	-0.067104	4.818586
333.440726	8000.222444	11.798311	-0.067048	4.818576
334.033660	8000.342568	11.803315	-0.067159	4.818609
333.671530	8000.246483	11.808320	-0.067091	4.818582
333.608849	8000.389455	11.813325	-0.067080	4.818625
333.490200	8000.145438	11.818330	-0.067058	4.818553
333.528721	8000.326479	11.823335	-0.067065	4.818606
333.325426	8000.149571	11.828339	-0.067027	4.818555
333.747668	8000.339866	11.833344	-0.067106	4.818610
333.962085	8000.430862	11.838349	-0.067146	4.818636
334.107393	8000.326770	11.843354	-0.067173	4.818604
333.785204	8000.368709	11.848359	-0.067113	4.818618
333.788467	8000.263794	11.853363	-0.067114	4.818587
333.839744	8000.415616	11.858368	-0.067123	4.818632
333.435831	8000.341022	11.863373	-0.067048	4.818611
333.660472	8000.370225	11.868378	-0.067090	4.818619
333.705487	8000.387615	11.873383	-0.067098	4.818624
333.564198	8000.174787	11.878387	-0.067072	4.818561
333.765315	8000.330681	11.883392	-0.067110	4.818607
333.993212	8000.417657	11.888397	-0.067152	4.818632
334.108020	8000.382437	11.893402	-0.067173	4.818621
334.121877	8000.439302	11.898407	-0.067176	4.818638
333.757179	8000.149005	11.903411	-0.067108	4.818553
333.254239	8000.103548	11.908416	-0.067014	4.818541
333.801209	8000.354263	11.913421	-0.067117	4.818614
333.825806	8000.396575	11.918426	-0.067121	4.818626
333.556073	8000.346840	11.923431	-0.067071	4.818612
332.967908	7999.972791	11.928435	-0.066961	4.818503
333.388815	8000.139971	11.933440	-0.067040	4.818551
333.421137	8000.190780	11.938445	-0.067046	4.818566
333.564137	8000.162229	11.943450	-0.067072	4.818557
333.563575	8000.454013	11.948455	-0.067073	4.818644
333.658487	8000.347157	11.953459	-0.067090	4.818612
333.443853	8000.176397	11.958464	-0.067050	4.818562
333.604461	8000.199508	11.963469	-0.067080	4.818568
333.775289	8000.334011	11.968474	-0.067112	4.818608
333.994600	8000.351599	11.973479	-0.067153	4.818612
333.298393	8000.134608	11.978483	-0.067023	4.818550
333.725907	8000.255698	11.983488	-0.067103	4.818585
333.496240	8000.255824	11.988493	-0.067060	4.818586
333.767352	8000.136596	11.993498	-0.067111	4.818549
333.379498	8000.331962	11.998503	-0.067039	4.818609
333.573665	8000.257903	12.003507	-0.067075	4.818586
333.716020	8000.278674	12.008512	-0.067101	4.818591
333.718329	8000.341684	12.013517	-0.067102	4.818610
333.798709	8000.187405	12.018522	-0.067117	4.818564
333.487731	8000.207451	12.023527	-0.067059	4.818571
333.587738	8000.239210	12.028531	-0.067078	4.818580
333.296356	8000.094730	12.033536	-0.067023	4.818538
333.743719	8000.323140	12.038541	-0.067107	4.818605
333.688965	8000.192271	12.043546	-0.067097	4.818566
333.922355	8000.431511	12.048551	-0.067140	4.818636
333.939687	8000.401304	12.053555	-0.067143	4.818627
333.936240	8000.342483	12.058560	-0.067143	4.818610
333.718318	8000.250397	12.063565	-0.067102	4.818583
333.843133	8000.275136	12.068570	-0.067126	4.818590
333.620072	8000.184034	12.073575	-0.067084	4.818564
333.794336	8000.317533	12.078579	-0.067117	4.818603
333.293895	8000.029653	12.083584	-0.067023	4.818519
333.426708	8000.291702	12.088589	-0.067048	4.818596
333.709069	8000.087606	12.093594	-0.067101	4.818535
333.518173	8000.312855	12.098599	-0.067065	4.818602
334.114232	8000.325962	12.103603	-0.067176	4.818604
334.484455	8000.528176	12.108608	-0.067245	4.818663
334.102835	8000.386695	12.113613	-0.067174	4.818622
334.164310	8000.259456	12.118618	-0.067186	4.818584
333.919820	8000.377991	12.123623	-0.067140	4.818620
333.965134	8000.294622	12.128627	-0.067149	4.818595
333.879262	8000.454084	12.133632	-0.067133	4.818643
333.829894	8000.333781	12.138637	-0.067124	4.818607
333.757651	8000.304492	12.143642	-0.067110	4.818599
334.005116	8000.422164	12.148647	-0.067156	4.818633
333.999825	8000.163894	12.153651	-0.067155	4.818556
334.148903	8000.322253	12.158656	-0.067183	4.818603
334.275149	8000.424684	12.163661	-0.067207	4.818633
334.409841	8000.337244	12.168666	-0.067232	4.818606
334.139443	8000.365171	12.173671	-0.067182	4.818615
334.002905	8000.119866	12.178675	-0.067156	4.818543
333.917190	8000.271981	12.183680	-0.067140	4.818589
334.029466	8000.159057	12.188685	-0.067161	4.818555
334.400772	8000.455747	12.193690	-0.067231	4.818641
334.344622	8000.372089	12.198695	-0.067220	4.818617
334.183163	8000.121206	12.203699	-0.067190	4.818543
334.307797	8000.302335	12.208704	-0.067213	4.818596
334.255651	8000.219780	12.213709	-0.067204	4.818572
334.261012	8000.256590	12.218714	-0.067205	4.818583
334.268142	8000.386840	12.223719	-0.067206	4.818621
334.260927	8000.191519	12.228723	-0.067205	4.818563
334.552489	8000.472466	12.233728	-0.067259	4.818646
334.116303	8000.367003	12.238733	-0.067178	4.818616
334.479668	8000.387541	12.243738	-0.067246	4.818621
334.246570	8000.394967	12.248743	-0.067202	4.818624
334.715295	8000.395902	12.253747	-0.067290	4.818622
334.260227	8000.206222	12.258752	-0.067205	4.818568
334.105313	8000.458190	12.263757	-0.067176	4.818643
333.928663	8000.265884	12.268762	-0.067143	4.818587
333.970920	8000.352512	12.273767	-0.067151	4.818612
334.033958	8000.243137	12.278771	-0.067163	4.818580
333.926345	8000.393915	12.283776	-0.067143	4.818625
333.778903	8000.337395	12.288781	-0.067115	4.818609
334.181303	8000.365793	12.293786	-0.067190	4.818615
334.069738	8000.455642	12.298791	-0.067170	4.818643
333.956003	8000.259967	12.303795	-0.067148	4.818585
333.802521	8000.319874	12.308800	-0.067120	4.818603
334.137117	8000.326387	12.313805	-0.067182	4.818604
334.124259	8000.403892	12.318810	-0.067180	4.818627
334.291343	8000.410296	12.323815	-0.067211	4.818628
334.403716	8000.292124	12.328819	-0.067232	4.818593
334.345258	8000.456147	12.333824	-0.067221	4.818642
334.253618	8000.310093	12.338829	-0.067204	4.818599
334.340041	8000.360568	12.343834	-0.067220	4.818613
334.277129	8000.531880	12.348839	-0.067209	4.818664
334.297589	8000.431388	12.353843	-0.067213	4.818635
334.195439	8000.383861	12.358848	-0.067194	4.818621
334.325991	8000.408677	12.363853	-0.067218	4.818628
334.144805	8000.367455	12.368858	-0.067184	4.818616
333.977016	8000.323262	12.373863	-0.067153	4.818604
334.395826	8000.288900	12.378867	-0.067231	4.818592
334.463465	8000.444089	12.383872	-0.067244	4.818638
334.005249	8000.367726	12.388877	-0.067158	4.818617
334.317337	8000.360298	12.393882	-0.067217	4.818613
334.105439	8000.358557	12.398887	-0.067177	4.818614
333.922750	8000.335159	12.403891	-0.067143	4.818607
334.193204	8000.389109	12.408896	-0.067194	4.818622
333.953417	8000.391199	12.413901	-0.067149	4.818624
334.057412	8000.234081	12.418906	-0.067168	4.818577
334.121247	8000.368226	12.423911	-0.067180	4.818616
333.864842	8000.335460	12.428915	-0.067133	4.818608
334.076916	8000.414881	12.433920	-0.067172	4.818630
333.390284	8000.111947	12.438925	-0.067044	4.818543
334.078701	8000.324643	12.443930	-0.067173	4.818604
333.594886	8000.121995	12.448935	-0.067082	4.818545
333.671994	8000.176543	12.453939	-0.067097	4.818561
333.597153	8000.253230	12.458944	-0.067083	4.818584
333.708063	8000.365952	12.463949	-0.067104	4.818617
333.571546	7999.972658	12.468954	-0.067078	4.818501
332.958819	8000.066401	12.473959	-0.066964	4.818531
332.775719	7999.883469	12.478963	-0.066930	4.818477
333.432863	8000.078947	12.483968	-0.067052	4.818533
333.708734	8000.216932	12.488973	-0.067104	4.818573
333.818413	8000.164851	12.493978	-0.067124	4.818557
334.045187	8000.303241	12.498983	-0.067167	4.818597
334.016581	8000.224146	12.503987	-0.067161	4.818574
333.908195	8000.221671	12.508992	-0.067141	4.818574
334.108035	8000.360757	12.513997	-0.067179	4.818614
333.902610	8000.231050	12.519002	-0.067140	4.818576
333.862188	8000.294546	12.524007	-0.067133	4.818595
333.884141	8000.313731	12.529011	-0.067137	4.818601
334.088350	8000.357361	12.534016	-0.067175	4.818613
333.913266	8000.354006	12.539021	-0.067143	4.818613
333.939455	8000.188516	12.544026	-0.067147	4.818564
333.985568	8000.356015	12.549031	-0.067156	4.818613
334.178033	8000.341761	12.554035	-0.067192	4.818608
334.118398	8000.370367	12.559040	-0.067181	4.818617
334.085489	8000.248181	12.564045	-0.067175	4.818581
334.272170	8000.322018	12.569050	-0.067210	4.818602
333.944879	8000.234788	12.574055	-0.067149	4.818577
334.086731	8000.287042	12.579059	-0.067175	4.818592
333.970823	8000.165862	12.584064	-0.067153	4.818557
334.161557	8000.361507	12.589069	-0.067189	4.818614
334.219160	8000.360170	12.594074	-0.067200	4.818614
333.886611	8000.278118	12.599079	-0.067138	4.818590
333.856836	8000.278778	12.604083	-0.067133	4.818591
333.546912	8000.222217	12.609088	-0.067075	4.818575
333.533081	8000.255625	12.614093	-0.067072	4.818585
334.211995	8000.166961	12.619098	-0.067199	4.818556
334.043241	8000.248709	12.624103	-0.067167	4.818581
333.532409	8000.145418	12.629107	-0.067072	4.818552
333.751530	8000.172448	12.634112	-0.067113	4.818560
333.713188	8000.299997	12.639117	-0.067106	4.818598
333.966762	8000.206778	12.644122	-0.067153	4.818569
334.164669	8000.374178	12.649127	-0.067190	4.818618
334.040610	8000.328462	12.654131	-0.067167	4.818605
333.449061	8000.180023	12.659136	-0.067057	4.818563
333.466188	8000.096285	12.664141	-0.067060	4.818538
333.667098	8000.183951	12.669146	-0.067098	4.818563
334.047390	8000.301273	12.674151	-0.067169	4.818597
333.928091	8000.190545	12.679155	-0.067146	4.818564
334.263200	8000.297826	12.684160	-0.067209	4.818595
334.243112	8000.397278	12.689165	-0.067205	4.818625
334.350295	8000.175125	12.694170	-0.067225	4.818558
334.233231	8000.406600	12.699175	-0.067203	4.818627
334.103448	8000.274740	12.704179	-0.067179	4.818589
333.778853	8000.090984	12.709184	-0.067119	4.818535
334.127930	8000.339095	12.714189	-0.067184	4.818608
333.971519	8000.195339	12.719194	-0.067155	4.818566
333.538346	8000.142403	12.724199	-0.067074	4.818551
333.487151	8000.019979	12.729203	-0.067065	4.818515
334.410271	8000.339680	12.734208	-0.067237	4.818607
334.132987	8000.186982	12.739213	-0.067185	4.818562
334.151270	8000.281691	12.744218	-0.067188	4.818590
333.606473	8000.264018	12.749223	-0.067087	4.818587
333.728030	8000.089291	12.754227	-0.067110	4.818535
333.504447	8000.125183	12.759232	-0.067068	4.818546
333.102821	8000.048525	12.764237	-0.066993	4.818525
333.728367	8000.124990	12.769242	-0.067110	4.818546
334.151846	8000.298510	12.774247	-0.067189	4.818595
334.147477	8000.285860	12.779251	-0.067188	4.818592
334.321524	8000.436154	12.784256	-0.067221	4.818636
334.038938	8000.368404	12.789261	-0.067168	4.818617
334.035237	8000.262348	12.794266	-0.067167	4.818585
333.867353	8000.365099	12.799271	-0.067136	4.818616
334.315209	8000.295433	12.804275	-0.067220	4.818594
334.359151	8000.342198	12.809280	-0.067228	4.818608
334.299820	8000.441133	12.814285	-0.067217	4.818637
334.359512	8000.336961	12.819290	-0.067228	4.818606
334.312724	8000.340545	12.824295	-0.067219	4.818607
334.512858	8000.522674	12.829299	-0.067257	4.818661
334.173595	8000.315626	12.834304	-0.067193	4.818600
334.152588	8000.430810	12.839309	-0.067190	4.818635
334.679188	8000.408367	12.844314	-0.067288	4.818626
334.579045	8000.378709	12.849319	-0.067269	4.818618
334.359504	8000.360073	12.854323	-0.067228	4.818613
334.408578	8000.370169	12.859328	-0.067237	4.818616
334.332913	8000.435301	12.864333	-0.067223	4.818635
334.299029	8000.337242	12.869338	-0.067217	4.818606
334.435152	8000.447151	12.874343	-0.067243	4.818639
334.081941	8000.250417	12.879347	-0.067177	4.818581
334.175081	8000.342964	12.884352	-0.067194	4.818609
334.355533	8000.227789	12.889357	-0.067228	4.818574
334.080938	8000.234669	12.894362	-0.067177	4.818577
334.045219	8000.346509	12.899367	-0.067170	4.818610
334.388746	8000.414019	12.904371	-0.067234	4.818629
333.863412	8000.097462	12.909376	-0.067136	4.818537
333.953822	8000.116500	12.914381	-0.067153	4.818542
333.869930	8000.271788	12.919386	-0.067138	4.818589
334.117857	8000.302348	12.924391	-0.067184	4.818597
334.047977	8000.241602	12.929395	-0.067171	4.818579
334.276006	8000.343275	12.934400	-0.067213	4.818608
334.371449	8000.466292	12.939405	-0.067231	4.818645
334.751665	8000.290773	12.944410	-0.067302	4.818591
334.364206	8000.358091	12.949415	-0.067230	4.818612
334.582355	8000.341027	12.954419	-0.067271	4.818606
334.363569	8000.323451	12.959424	-0.067230	4.818602
334.612823	8000.446398	12.964429	-0.067276	4.818638
334.573844	8000.434341	12.969434	-0.067269	4.818634
334.241784	8000.332351	12.974439	-0.067207	4.818605
334.277896	8000.363269	12.979443	-0.067214	4.818614
334.483444	8000.286210	12.984448	-0.067252	4.818590
334.620236	8000.437064	12.989453	-0.067278	4.818635
334.286772	8000.264730	12.994458	-0.067216	4.818585
334.307205	8000.388858	12.999463	-0.067220	4.818622
334.432609	8000.320189	13.004467	-0.067243	4.818601
334.331166	8000.325152	13.009472	-0.067224	4.818603
334.242749	8000.313494	13.014477	-0.067208	4.818600
334.399698	8000.304020	13.019482	-0.067237	4.818596
334.241174	8000.404796	13.024487	-0.067208	4.818627
334.543665	8000.422432	13.029491	-0.067264	4.818631
334.635184	8000.341771	13.034496	-0.067281	4.818606
334.424262	8000.450253	13.039501	-0.067242	4.818640
334.137425	8000.159929	13.044506	-0.067188	4.818554
334.240933	8000.456239	13.049511	-0.067208	4.818642
334.099503	8000.306381	13.054515	-0.067181	4.818598
334.697127	8000.501097	13.059520	-0.067293	4.818654
334.189465	8000.285530	13.064525	-0.067198	4.818591
334.307314	8000.241953	13.069530	-0.067220	4.818578
334.564048	8000.398586	13.074535	-0.067268	4.818624
334.352674	8000.284542	13.079539	-0.067229	4.818590
334.400895	8000.298825	13.084544	-0.067238	4.818595
334.571655	8000.363008	13.089549	-0.067270	4.818613
334.653734	8000.374589	13.094554	-0.067285	4.818616
334.166598	8000.379715	13.099559	-0.067194	4.818620
334.273642	8000.369583	13.104563	-0.067214	4.818616
333.892752	8000.176686	13.109568	-0.067143	4.818560
334.199199	8000.366508	13.114573	-0.067201	4.818615
334.267611	8000.390505	13.119578	-0.067213	4.818622
334.501944	8000.397796	13.124583	-0.067257	4.818624
334.515841	8000.323459	13.129587	-0.067260	4.818601
334.521582	8000.386515	13.134592	-0.067261	4.818620
334.562729	8000.445840	13.139597	-0.067268	4.818638
334.690479	8000.373004	13.144602	-0.067292	4.818615
334.181509	8000.306467	13.149607	-0.067197	4.818598
334.141477	8000.266057	13.154611	-0.067190	4.818586
334.398922	8000.271553	13.159616	-0.067238	4.818586
333.876129	8000.284608	13.164621	-0.067141	4.818592
333.815325	8000.220833	13.169626	-0.067129	4.818574
334.096282	8000.365187	13.174631	-0.067182	4.818615
334.007803	8000.311543	13.179635	-0.067165	4.818600
334.234016	8000.295634	13.184640	-0.067208	4.818594
334.339257	8000.306471	13.189645	-0.067227	4.818597
334.309370	8000.204267	13.194650	-0.067222	4.818567
333.947429	8000.353793	13.199655	-0.067154	4.818613
333.725122	8000.167185	13.204659	-0.067113	4.818558
334.077663	8000.233760	13.209664	-0.067179	4.818576
334.279748	8000.420110	13.214669	-0.067216	4.818631
334.517000	8000.379157	13.219674	-0.067261	4.818618
334.237441	8000.472039	13.224679	-0.067209	4.818647
334.631511	8000.402715	13.229683	-0.067282	4.818625
334.697886	8000.447678	13.234688	-0.067294	4.818638
334.479869	8000.390225	13.239693	-0.067254	4.818621
334.471922	8000.381726	13.244698	-0.067252	4.818619
334.555465	8000.349242	13.249703	-0.067268	4.818609
334.367825	8000.333126	13.254707	-0.067233	4.818605
334.491849	8000.344211	13.259712	-0.067256	4.818608
334.500901	8000.336986	13.264717	-0.067258	4.818605
334.954131	8000.438483	13.269722	-0.067342	4.818634
334.887246	8000.442851	13.274727	-0.067330	4.818635
334.529074	8000.323721	13.279731	-0.067263	4.818601
334.710550	8000.357606	13.284736	-0.067297	4.818611
334.428799	8000.470402	13.289741	-0.067245	4.818645
334.313580	8000.354477	13.294746	-0.067223	4.818611
334.038120	8000.353997	13.299751	-0.067172	4.818612
334.233772	8000.260014	13.304755	-0.067208	4.818584
334.427256	8000.381175	13.309760	-0.067245	4.818619
334.356882	8000.334067	13.314765	-0.067232	4.818605
334.043500	8000.270110	13.319770	-0.067173	4.818587
334.232061	8000.255805	13.324775	-0.067208	4.818582
334.211442	8000.177865	13.329779	-0.067204	4.818559
334.084150	8000.247564	13.334784	-0.067181	4.818581
334.438378	8000.341453	13.339789	-0.067247	4.818607
334.607999	8000.229284	13.344794	-0.067278	4.818573
334.375400	8000.363721	13.349799	-0.067235	4.818614
334.489981	8000.303307	13.354803	-0.067257	4.818595
334.355532	8000.239609	13.359808	-0.067232	4.818577
334.625273	8000.430002	13.364813	-0.067282	4.818633
334.746434	8000.375972	13.369818	-0.067305	4.818616
334.304826	8000.225305	13.374823	-0.067222	4.818573
334.762551	8000.270178	13.379827	-0.067308	4.818585
334.286210	8000.237661	13.384832	-0.067219	4.818577
333.559572	8000.002426	13.389837	-0.067083	4.818510
334.361886	8000.271202	13.394842	-0.067233	4.818586
334.407207	8000.388311	13.399847	-0.067242	4.818621
334.450715	8000.386788	13.404851	-0.067250	4.818620
334.578308	8000.246774	13.409856	-0.067273	4.818578
334.374870	8000.395240	13.414861	-0.067236	4.818623
334.178463	8000.189029	13.419866	-0.067199	4.818563
334.119029	8000.310003	13.424871	-0.067188	4.818599
334.210226	8000.231437	13.429875	-0.067205	4.818575
334.424465	8000.163940	13.434880	-0.067245	4.818554
334.181915	8000.154449	13.439885	-0.067200	4.818552
334.653378	8000.234139	13.444890	-0.067288	4.818574
334.559150	8000.348358	13.449895	-0.067270	4.818609
334.467128	8000.213846	13.454899	-0.067253	4.818569
334.447204	8000.289159	13.459904	-0.067249	4.818591
334.419088	8000.271997	13.464909	-0.067244	4.818586
334.463484	8000.211708	13.469914	-0.067253	4.818568
334.102310	8000.314010	13.474919	-0.067185	4.818600
334.339646	8000.339184	13.479923	-0.067230	4.818607
334.122694	8000.156843	13.484928	-0.067189	4.818553
333.821800	8000.080459	13.489933	-0.067133	4.818532
334.000307	8000.101707	13.494938	-0.067166	4.818537
334.358005	8000.371976	13.499943	-0.067233	4.818616
334.680534	8000.360487	13.504947	-0.067293	4.818612
333.930305	8000.136480	13.509952	-0.067154	4.818548
333.944134	8000.171302	13.514957	-0.067156	4.818558
334.280353	8000.208273	13.519962	-0.067219	4.818568
334.023063	8000.211183	13.524967	-0.067171	4.818570
334.254995	8000.193250	13.529971	-0.067214	4.818564
334.132155	8000.233619	13.534976	-0.067191	4.818576
334.458174	8000.348129	13.539981	-0.067252	4.818609
334.416779	8000.255220	13.544986	-0.067245	4.818581
334.148411	8000.316761	13.549991	-0.067195	4.818601
334.522531	8000.318547	13.554995	-0.067264	4.818600
334.503545	8000.140914	13.560000	-0.067261	4.818547
334.977552	8000.511390	13.565005	-0.067349	4.818655
335.124975	8000.416770	13.570010	-0.067377	4.818627
334.791589	8000.454361	13.575015	-0.067315	4.818639
334.540144	8000.276809	13.580019	-0.067268	4.818587
334.291829	8000.230504	13.585024	-0.067222	4.818575
334.030501	8000.129450	13.590029	-0.067173	4.818546
334.010900	8000.164881	13.595034	-0.067169	4.818556
334.349030	8000.299492	13.600039	-0.067232	4.818595
334.755658	8000.377281	13.605043	-0.067308	4.818616
334.574994	8000.306676	13.610048	-0.067275	4.818596
334.455907	8000.225337	13.615053	-0.067252	4.818572
334.821020	8000.360308	13.620058	-0.067320	4.818611
334.517786	8000.390950	13.625063	-0.067264	4.818621
334.616211	8000.335571	13.630067	-0.067282	4.818605
334.801341	8000.381050	13.635072	-0.067317	4.818617
334.357490	8000.444475	13.640077	-0.067234	4.818638
334.564940	8000.377938	13.645082	-0.067273	4.818617
334.715574	8000.353687	13.650087	-0.067301	4.818610
334.905204	8000.423367	13.655091	-0.067336	4.818630
334.780515	8000.295770	13.660096	-0.067313	4.818592
334.668757	8000.463290	13.665101	-0.067293	4.818642
334.879874	8000.389454	13.670106	-0.067332	4.818620
334.741488	8000.432766	13.675111	-0.067306	4.818633
334.713573	8000.328487	13.680115	-0.067301	4.818602
334.337664	8000.187083	13.685120	-0.067231	4.818561
334.754897	8000.408810	13.690125	-0.067309	4.818626
334.774150	8000.338741	13.695130	-0.067312	4.818605
334.705471	8000.451199	13.700135	-0.067300	4.818639
335.016459	8000.331446	13.705139	-0.067358	4.818602
334.638652	8000.343261	13.710144	-0.067287	4.818607
334.510268	8000.305884	13.715149	-0.067263	4.818596
334.610483	8000.210643	13.720154	-0.067282	4.818567
334.531740	8000.294627	13.725159	-0.067267	4.818593
334.626953	8000.393501	13.730163	-0.067285	4.818622
334.770820	8000.296735	13.735168	-0.067312	4.818592
334.616517	8000.329341	13.740173	-0.067283	4.818603
334.862720	8000.388222	13.745178	-0.067329	4.818619
334.870168	8000.345288	13.750183	-0.067331	4.818606
334.799417	8000.368499	13.755187	-0.067318	4.818614
335.155796	8000.446678	13.760192	-0.067384	4.818635
335.180299	8000.485841	13.765197	-0.067389	4.818647
335.267935	8000.429269	13.770202	-0.067405	4.818630
334.780100	8000.439631	13.775207	-0.067314	4.818635
334.990970	8000.376288	13.780211	-0.067353	4.818615
335.119132	8000.477698	13.785216	-0.067377	4.818645
334.827484	8000.439215	13.790221	-0.067323	4.818635
334.653980	8000.209161	13.795226	-0.067291	4.818567
334.976792	8000.341475	13.800231	-0.067351	4.818605
334.999194	8000.412099	13.805235	-0.067355	4.818626
334.970022	8000.322498	13.810240	-0.067350	4.818599
334.909894	8000.469707	13.815245	-0.067339	4.818643
334.873876	8000.247762	13.820250	-0.067332	4.818577
334.870025	8000.424052	13.825255	-0.067331	4.818630
335.099740	8000.448078	13.830259	-0.067374	4.818636
335.004753	8000.449977	13.835264	-0.067357	4.818637
334.909066	8000.464463	13.840269	-0.067339	4.818642
334.522584	8000.252591	13.845274	-0.067267	4.818580
334.658285	8000.385587	13.850279	-0.067292	4.818619
334.901841	8000.310079	13.855283	-0.067337	4.818596
335.040876	8000.426326	13.860288	-0.067363	4.818630
334.311453	8000.343236	13.865293	-0.067228	4.818608
334.963843	8000.362338	13.870298	-0.067349	4.818611
334.667992	8000.326950	13.875303	-0.067294	4.818602
334.250019	8000.130413	13.880307	-0.067216	4.818545
334.609046	8000.192876	13.885312	-0.067283	4.818562
334.613371	8000.248566	13.890317	-0.067284	4.818579
334.481316	8000.272019	13.895322	-0.067259	4.818586
333.984156	8000.139516	13.900327	-0.067167	4.818549
334.211230	8000.169801	13.905331	-0.067209	4.818557
334.693844	8000.237044	13.910336	-0.067299	4.818575
334.413561	8000.409688	13.915341	-0.067247	4.818627
334.579326	8000.276475	13.920346	-0.067278	4.818587
334.235735	8000.272998	13.925351	-0.067214	4.818587
334.542778	8000.202525	13.930355	-0.067271	4.818565
334.691312	8000.329392	13.935360	-0.067299	4.818602
334.814246	8000.375101	13.940365	-0.067322	4.818615
334.750842	8000.118159	13.945370	-0.067310	4.818539
334.733655	8000.496851	13.950375	-0.067307	4.818652
335.012943	8000.407120	13.955379	-0.067359	4.818624
335.027602	8000.362182	13.960384	-0.067362	4.818611
335.062360	8000.517991	13.965389	-0.067368	4.818657
335.070505	8000.380597	13.970394	-0.067370	4.818616
335.085904	8000.386052	13.975399	-0.067373	4.818618
335.320538	8000.359759	13.980403	-0.067416	4.818609
335.122146	8000.473656	13.985408	-0.067380	4.818644
334.690267	8000.343056	13.990413	-0.067299	4.818606
334.648170	8000.383439	13.995418	-0.067291	4.818619
334.813081	8000.352028	14.000423	-0.067322	4.818609
335.054655	8000.468579	14.005427	-0.067367	4.818642
335.113548	8000.338153	14.010432	-0.067378	4.818603
335.188540	8000.533330	14.015437	-0.067392	4.818661
335.135526	8000.406676	14.020442	-0.067382	4.818624
335.365217	8000.505227	14.025447	-0.067425	4.818652
335.076612	8000.315635	14.030451	-0.067371	4.818597
335.132876	8000.494820	14.035456	-0.067382	4.818650
334.812425	8000.324753	14.040461	-0.067322	4.818600
335.099484	8000.432456	14.045466	-0.067376	4.818631
334.861532	8000.336952	14.050471	-0.067332	4.818604
334.915039	8000.480412	14.055475	-0.067342	4.818646
335.093393	8000.275988	14.060480	-0.067375	4.818585
334.954729	8000.526076	14.065485	-0.067349	4.818660
334.845864	8000.293722	14.070490	-0.067329	4.818591
334.944199	8000.458766	14.075495	-0.067347	4.818640
334.928840	8000.419729	14.080499	-0.067344	4.818628
335.307752	8000.511852	14.085504	-0.067415	4.818654
334.780781	8000.438775	14.090509	-0.067317	4.818635
334.701877	8000.186876	14.095514	-0.067302	4.818560
334.542697	8000.445087	14.100519	-0.067273	4.818637
334.606019	8000.231801	14.105523	-0.067284	4.818574
335.069775	8000.469889	14.110528	-0.067371	4.818643
334.995970	8000.370252	14.115533	-0.067357	4.818613
334.859263	8000.390495	14.120538	-0.067332	4.818620
334.946720	8000.467225	14.125543	-0.067348	4.818642
334.992879	8000.367071	14.130547	-0.067357	4.818612
335.096763	8000.331707	14.135552	-0.067376	4.818601
335.078231	8000.360855	14.140557	-0.067373	4.818610
335.045485	8000.326838	14.145562	-0.067367	4.818600
335.201689	8000.418121	14.150567	-0.067396	4.818627
335.205192	8000.439163	14.155571	-0.067396	4.818633
335.410609	8000.526898	14.160576	-0.067435	4.818658
335.263571	8000.407400	14.165581	-0.067407	4.818623
335.291487	8000.444509	14.170586	-0.067413	4.818634
335.413763	8000.505956	14.175591	-0.067436	4.818652
335.465431	8000.403774	14.180595	-0.067445	4.818621
335.253538	8000.423024	14.185600	-0.067406	4.818628
335.046768	8000.483278	14.190605	-0.067367	4.818647
335.304114	8000.449938	14.195610	-0.067415	4.818636
335.188351	8000.444215	14.200615	-0.067394	4.818635
335.102847	8000.386410	14.205619	-0.067378	4.818618
335.239755	8000.436502	14.210624	-0.067403	4.818632
335.167575	8000.516376	14.215629	-0.067390	4.818656
335.404635	8000.395648	14.220634	-0.067434	4.818619
335.177912	8000.490277	14.225639	-0.067392	4.818648
335.372649	8000.320706	14.230643	-0.067428	4.818597
335.412391	8000.467135	14.235648	-0.067436	4.818640
334.981265	8000.465649	14.240653	-0.067355	4.818642
335.544112	8000.454184	14.245658	-0.067460	4.818636
335.245578	8000.421907	14.250663	-0.067405	4.818628
335.196242	8000.397118	14.255667	-0.067396	4.818620
335.622611	8000.463626	14.260672	-0.067475	4.818639
335.502314	8000.421105	14.265677	-0.067453	4.818626
335.293355	8000.440393	14.270682	-0.067414	4.818633
335.479752	8000.468047	14.275687	-0.067449	4.818640
335.439649	8000.500061	14.280691	-0.067441	4.818650
335.326233	8000.497517	14.285696	-0.067420	4.818650
335.130749	8000.372132	14.290701	-0.067384	4.818613
335.391131	8000.414407	14.295706	-0.067432	4.818625
335.217628	8000.371185	14.300711	-0.067400	4.818613
335.447757	8000.426706	14.305715	-0.067443	4.818628
335.283752	8000.386758	14.310720	-0.067412	4.818617
335.272592	8000.503125	14.315725	-0.067410	4.818652
334.889338	8000.326980	14.320730	-0.067339	4.818601
335.096108	8000.447270	14.325735	-0.067378	4.818636
335.386326	8000.513032	14.330739	-0.067432	4.818654
335.007953	8000.342199	14.335744	-0.067361	4.818605
335.074626	8000.548812	14.340749	-0.067374	4.818666
335.074630	8000.327339	14.345754	-0.067374	4.818600
334.754549	8000.380851	14.350759	-0.067314	4.818617
335.022413	8000.381238	14.355763	-0.067364	4.818616
335.314413	7999.421543	14.360768	-0.067418	4.818330

335.331292	7996.279608	14.365773	-0.067419	4.817395
335.203865	7990.759146	14.370778	-0.067392	4.815753
335.278271	7983.973311	14.375783	-0.067401	4.813733
335.215834	7976.800771	14.380787	-0.067385	4.811597
334.905785	7969.219788	14.385792	-0.067322	4.809339
334.930628	7961.377480	14.390797	-0.067322	4.807002
335.314276	7953.439699	14.395802	-0.067388	4.804633
335.413799	7945.510694	14.400807	-0.067402	4.802267
335.153267	7937.524905	14.405811	-0.067348	4.799884
335.208047	7929.602196	14.410816	-0.067353	4.797517
335.199498	7921.584484	14.415821	-0.067346	4.795121
335.002307	7913.660570	14.420826	-0.067304	4.792753
335.198959	7905.556080	14.425831	-0.067336	4.790328
335.339850	7897.559325	14.430835	-0.067357	4.787935
335.096584	7889.595843	14.435840	-0.067306	4.785551
334.710737	7881.559944	14.440845	-0.067229	4.783145
335.169387	7873.571156	14.445850	-0.067310	4.780749
335.089607	7865.552758	14.450855	-0.067289	4.778345
334.905931	7857.569674	14.455859	-0.067250	4.775950
335.269848	7849.528310	14.460864	-0.067313	4.773535
335.035842	7841.523749	14.465869	-0.067264	4.771132
334.875857	7833.531268	14.470874	-0.067229	4.768731
334.632220	7825.546286	14.475879	-0.067178	4.766331
334.944317	7817.474830	14.480883	-0.067231	4.763902
334.883263	7809.660361	14.485888	-0.067215	4.761551
334.850308	7801.512072	14.490893	-0.067204	4.759098
334.827757	7793.625046	14.495898	-0.067194	4.756722
334.650625	7785.561585	14.500903	-0.067156	4.754292
334.571775	7777.569333	14.505907	-0.067136	4.751882
334.534896	7769.501834	14.510912	-0.067124	4.749448
334.098624	7761.568922	14.515917	-0.067038	4.747054
333.921492	7753.512872	14.520922	-0.067000	4.744622
333.915959	7745.524210	14.525927	-0.066993	4.742208
334.115374	7737.446044	14.530931	-0.067025	4.739765
333.965797	7729.533728	14.535936	-0.066992	4.737372
334.030703	7721.464935	14.540941	-0.066999	4.734930
334.140475	7713.541790	14.545946	-0.067014	4.732531
333.870144	7705.474029	14.550951	-0.066959	4.730087
334.018203	7697.465516	14.555955	-0.066981	4.727660
334.135819	7689.509269	14.560960	-0.066998	4.725247
334.122852	7681.503873	14.565965	-0.066990	4.722818
334.015717	7673.546323	14.570970	-0.066965	4.720402
334.278593	7665.480707	14.575975	-0.067009	4.717952
334.221243	7657.505955	14.580979	-0.066993	4.715529
334.193648	7649.563191	14.585984	-0.066983	4.713114
333.553989	7641.587901	14.590989	-0.066859	4.710689
333.888365	7633.513489	14.595994	-0.066916	4.708231
334.126332	7625.483776	14.600999	-0.066955	4.705785
334.306332	7617.443585	14.606003	-0.066983	4.703336
333.921021	7609.569242	14.611008	-0.066906	4.700936
333.996066	7601.515469	14.616013	-0.066915	4.698479
334.044422	7593.556833	14.621018	-0.066919	4.696051
334.015560	7585.496761	14.626023	-0.066908	4.693590
333.771579	7577.557806	14.631027	-0.066858	4.691165
333.809236	7569.512519	14.636032	-0.066860	4.688706
333.172821	7561.568728	14.641037	-0.066736	4.686278
333.192843	7553.516604	14.646042	-0.066735	4.683814
333.318956	7545.528087	14.651047	-0.066753	4.681368
333.283587	7537.493448	14.656051	-0.066741	4.678908
333.587152	7529.539037	14.661056	-0.066792	4.676470
333.722211	7521.434674	14.666061	-0.066812	4.673985
333.813579	7513.500367	14.671066	-0.066824	4.671551
333.382077	7505.476994	14.676071	-0.066739	4.669089
333.679781	7497.460799	14.681075	-0.066789	4.666627
333.616968	7489.430147	14.686080	-0.066772	4.664160
333.418738	7481.473751	14.691085	-0.066730	4.661714
333.327922	7473.487158	14.696090	-0.066708	4.659258
333.391373	7465.504857	14.701095	-0.066715	4.656801
333.572116	7457.417275	14.706099	-0.066743	4.654311
333.131613	7449.525544	14.711104	-0.066656	4.651880
333.484641	7441.436328	14.716109	-0.066716	4.649387
333.291730	7433.487237	14.721114	-0.066675	4.646936
333.137191	7425.405835	14.726119	-0.066641	4.644442
333.150916	7417.476294	14.731123	-0.066639	4.641994
333.272513	7409.408340	14.736128	-0.066656	4.639502
333.271600	7401.431698	14.741133	-0.066651	4.637037
333.488450	7393.439799	14.746138	-0.066686	4.634566
333.498930	7385.501873	14.751143	-0.066683	4.632110
333.563565	7377.420841	14.756147	-0.066690	4.629609
333.483773	7369.428108	14.761152	-0.066670	4.627133
333.271656	7361.382580	14.766157	-0.066625	4.624640
333.441512	7353.478455	14.771162	-0.066652	4.622190
333.175069	7345.437758	14.776167	-0.066597	4.619695
333.192223	7337.479143	14.781171	-0.066595	4.617225
333.251953	7329.422140	14.786176	-0.066601	4.614723
332.797500	7321.466593	14.791181	-0.066511	4.612251
332.777579	7313.404567	14.796186	-0.066502	4.609744
332.544664	7305.440033	14.801191	-0.066453	4.607267
332.815070	7297.341559	14.806195	-0.066499	4.604747
332.507253	7289.437188	14.811200	-0.066436	4.602285
332.813300	7281.320198	14.816205	-0.066488	4.599757
333.231127	7273.445365	14.821210	-0.066561	4.597302
333.083713	7265.364033	14.826215	-0.066528	4.594782
333.080041	7257.427536	14.831219	-0.066522	4.592305
333.171251	7249.410887	14.836224	-0.066534	4.589802
333.022373	7241.358867	14.841229	-0.066501	4.587286
332.659593	7233.379384	14.846234	-0.066428	4.584792
332.927755	7225.382912	14.851239	-0.066473	4.582291
332.907762	7217.326540	14.856243	-0.066464	4.579770
332.832758	7209.410524	14.861248	-0.066445	4.577292
332.298278	7201.429926	14.866253	-0.066340	4.574790
332.613247	7193.428599	14.871258	-0.066394	4.572283
332.246566	7185.381269	14.876263	-0.066320	4.569759
332.450625	7177.338669	14.881267	-0.066353	4.567236
332.548844	7169.303165	14.886272	-0.066366	4.564713
332.324087	7161.380689	14.891277	-0.066319	4.562224
332.060817	7153.436102	14.896282	-0.066265	4.559726
332.202026	7145.408577	14.901287	-0.066286	4.557202
332.471482	7137.356691	14.906291	-0.066331	4.554669
332.411515	7129.396057	14.911296	-0.066315	4.552163
332.338698	7121.341850	14.916301	-0.066296	4.549626
332.212342	7113.337179	14.921306	-0.066267	4.547102
331.786113	7105.311842	14.926311	-0.066183	4.544570
332.052800	7097.332619	14.931315	-0.066227	4.542053
331.992689	7089.345792	14.936320	-0.066211	4.539532
332.461027	7081.283552	14.941325	-0.066293	4.536986
332.600812	7073.281040	14.946330	-0.066314	4.534458
332.621948	7065.322561	14.951335	-0.066313	4.531941
332.580754	7057.290188	14.956339	-0.066300	4.529399
332.375878	7049.338885	14.961344	-0.066256	4.526881
331.986009	7041.322022	14.966349	-0.066179	4.524341
332.132236	7033.417589	14.971354	-0.066201	4.521836
332.295190	7025.285039	14.976359	-0.066226	4.519258
332.020038	7017.382061	14.981363	-0.066170	4.516749
331.803593	7009.330575	14.986368	-0.066124	4.514192
331.883139	7001.330597	14.991373	-0.066134	4.511651
331.985163	6993.285752	14.996378	-0.066147	4.509094
331.980187	6985.280025	15.001383	-0.066141	4.506548
332.073432	6977.206091	15.006387	-0.066154	4.503980
331.732689	6969.375160	15.011392	-0.066085	4.501485
331.196917	6961.292390	15.016397	-0.065980	4.498908
331.564870	6953.310207	15.021402	-0.066043	4.496365
331.884729	6945.229262	15.026407	-0.066098	4.493789
331.840374	6937.299226	15.031411	-0.066084	4.491259
332.051311	6929.259971	15.036416	-0.066118	4.488693
331.809294	6921.261384	15.041421	-0.066068	4.486137
331.609446	6913.288388	15.046426	-0.066026	4.483587
331.581031	6905.295283	15.051431	-0.066015	4.481030
331.505031	6897.237183	15.056435	-0.065996	4.478451
331.614028	6889.288446	15.061440	-0.066011	4.475907
331.300636	6881.277980	15.066445	-0.065948	4.473339
331.466598	6873.296641	15.071450	-0.065973	4.470781
331.526754	6865.237643	15.076455	-0.065979	4.468196
331.178216	6857.231032	15.081459	-0.065909	4.465625
331.399487	6849.255799	15.086464	-0.065945	4.463065
331.289471	6841.260851	15.091469	-0.065920	4.460496
331.536340	6833.247709	15.096474	-0.065960	4.457920
330.946609	6825.251878	15.101479	-0.065845	4.455345
331.102149	6817.268783	15.106483	-0.065869	4.452777
331.106552	6809.278070	15.111488	-0.065865	4.450203
330.922687	6801.184556	15.116493	-0.065825	4.447594
331.148322	6793.197716	15.121498	-0.065862	4.445020
331.292563	6785.224482	15.126503	-0.065884	4.442448
330.777044	6777.290825	15.131507	-0.065783	4.439885
331.029334	6769.285426	15.136512	-0.065825	4.437300
330.667029	6761.200294	15.141517	-0.065752	4.434685
330.632266	6753.254457	15.146522	-0.065740	4.432116
330.675649	6745.167219	15.151527	-0.065743	4.429499
330.435032	6737.217904	15.156531	-0.065693	4.426924
330.745122	6729.188481	15.161536	-0.065746	4.424325
330.523971	6721.238586	15.166541	-0.065700	4.421746
330.789469	6713.187480	15.171546	-0.065744	4.419137
330.363130	6705.283441	15.176551	-0.065659	4.416569
330.455985	6697.178559	15.181555	-0.065671	4.413938
330.331197	6689.257350	15.186560	-0.065643	4.411364
330.443953	6681.170280	15.191565	-0.065659	4.408735
330.541119	6673.211104	15.196570	-0.065672	4.406147
330.350451	6665.137426	15.201575	-0.065631	4.403518
330.755275	6657.182681	15.206579	-0.065701	4.400930
331.041838	6649.190716	15.211584	-0.065749	4.398327
330.485065	6641.269779	15.216589	-0.065641	4.395741
330.658067	6633.192836	15.221594	-0.065668	4.393107
330.133367	6625.300104	15.226599	-0.065565	4.390527
330.159220	6617.221418	15.231603	-0.065564	4.387888
330.102247	6609.281066	15.236608	-0.065549	4.385292
330.407969	6601.219602	15.241613	-0.065600	4.382658
330.485705	6593.235350	15.246618	-0.065610	4.380046
330.363568	6585.267676	15.251623	-0.065582	4.377436
330.481367	6577.236832	15.256627	-0.065598	4.374806
330.416693	6569.326088	15.261632	-0.065581	4.372212
330.537599	6561.201015	15.266637	-0.065599	4.369548
330.454389	6553.279303	15.271642	-0.065578	4.366947
330.477486	6545.254519	15.276647	-0.065577	4.364312
329.831735	6537.395718	15.281651	-0.065452	4.361725
330.248521	6529.249390	15.286656	-0.065524	4.359049
329.977197	6521.353036	15.291661	-0.065468	4.356449
330.077271	6513.281443	15.296666	-0.065482	4.353793
330.278603	6505.194411	15.301671	-0.065514	4.351130
329.915959	6497.236130	15.306675	-0.065441	4.348504
330.010680	6489.264536	15.311680	-0.065454	4.345876
329.807130	6481.211144	15.316685	-0.065411	4.343217
330.051123	6473.271218	15.321690	-0.065451	4.340597
330.045509	6465.245634	15.326695	-0.065445	4.337945
329.951584	6457.263918	15.331699	-0.065422	4.335305
329.833517	6449.323548	15.336704	-0.065395	4.332677
329.761013	6441.247390	15.341709	-0.065376	4.330003
329.746731	6433.325578	15.346714	-0.065369	4.327379
329.981550	6425.199907	15.351719	-0.065407	4.324688
329.636700	6417.307412	15.356723	-0.065338	4.322068
329.557002	6409.280517	15.361728	-0.065318	4.319403
329.556621	6401.324266	15.366733	-0.065313	4.316762
329.428873	6393.268142	15.371738	-0.065284	4.314084
329.599122	6385.296662	15.376743	-0.065310	4.311435
329.400925	6377.226119	15.381747	-0.065268	4.308749
329.370990	6369.263159	15.386752	-0.065257	4.306098
329.479522	6361.200253	15.391757	-0.065272	4.303413
329.477060	6353.232395	15.396762	-0.065267	4.300758
329.455516	6345.214764	15.401767	-0.065257	4.298084
329.013114	6337.244401	15.406771	-0.065170	4.295420
329.269860	6329.261033	15.411776	-0.065213	4.292757
329.446954	6321.145528	15.416781	-0.065240	4.290047
329.143439	6313.277097	15.421786	-0.065179	4.287413
329.384889	6305.135358	15.426791	-0.065218	4.284692
328.966226	6297.306248	15.431795	-0.065135	4.282067
328.808926	6289.272536	15.436800	-0.065101	4.279375
328.712953	6281.307390	15.441805	-0.065078	4.276704
328.901686	6273.264667	15.446810	-0.065108	4.274009
328.874008	6265.225746	15.451815	-0.065097	4.271311
328.775113	6257.167038	15.456819	-0.065074	4.268603
328.571946	6249.251216	15.461824	-0.065031	4.265942
328.629920	6241.172159	15.466829	-0.065036	4.263226
328.553989	6233.251550	15.471834	-0.065017	4.260560
328.750121	6225.175790	15.476839	-0.065048	4.257844
328.868168	6217.178794	15.481843	-0.065065	4.255151
328.874439	6209.230932	15.486848	-0.065061	4.252472
328.426481	6201.186217	15.491853	-0.064973	4.249754
328.715742	6193.209376	15.496858	-0.065021	4.247064
328.791988	6185.179342	15.501863	-0.065030	4.244353
328.888242	6177.203668	15.506867	-0.065043	4.241659
328.739287	6169.225899	15.511872	-0.065010	4.238960
328.003993	6161.328845	15.516877	-0.064868	4.236280
328.257992	6153.209559	15.521882	-0.064910	4.233533
327.917239	6145.254335	15.526887	-0.064842	4.230834
328.025892	6137.194247	15.531891	-0.064857	4.228103
328.786175	6129.097241	15.536896	-0.064993	4.225364
329.013717	6121.104222	15.541901	-0.065030	4.222654
329.113683	6113.153475	15.546906	-0.065044	4.219954
329.066766	6105.207075	15.551911	-0.065030	4.217252
329.237121	6097.160462	15.556915	-0.065056	4.214518
329.109908	6089.191213	15.561920	-0.065028	4.211804
328.795215	6081.155500	15.566925	-0.064964	4.209064
328.659552	6073.257456	15.571930	-0.064933	4.206371
328.802720	6065.186741	15.576935	-0.064955	4.203620
329.027552	6057.204469	15.581939	-0.064992	4.200899
328.930646	6049.243724	15.586944	-0.064968	4.198180
328.409325	6041.238776	15.591949	-0.064866	4.195439
328.715717	6033.195257	15.596954	-0.064918	4.192692
329.041080	6025.098761	15.601959	-0.064973	4.189926
328.974286	6017.097722	15.606963	-0.064956	4.187186
328.421555	6009.181836	15.611968	-0.064848	4.184468
328.513320	6001.201288	15.616973	-0.064860	4.181733
328.777949	5993.128824	15.621978	-0.064904	4.178968
328.657932	5985.184407	15.626983	-0.064876	4.176239
328.663270	5977.173510	15.631987	-0.064872	4.173488
328.739456	5969.205307	15.636992	-0.064881	4.170750
328.581602	5961.165478	15.641997	-0.064846	4.167983
328.888367	5953.157689	15.647002	-0.064898	4.165231
328.629735	5945.235562	15.652007	-0.064845	4.162500
328.772852	5937.201640	15.657011	-0.064867	4.159733
329.183719	5929.189366	15.662016	-0.064938	4.156975
328.944526	5921.184685	15.667021	-0.064888	4.154210
328.965247	5913.239910	15.672026	-0.064887	4.151467
328.658135	5905.224169	15.677031	-0.064825	4.148694
328.450772	5897.220089	15.682035	-0.064781	4.145923
328.194385	5889.277433	15.687040	-0.064728	4.143172
328.380780	5881.214215	15.692045	-0.064757	4.140383
328.553597	5873.235254	15.697050	-0.064784	4.137621
328.556267	5865.215894	15.702055	-0.064780	4.134841
328.407244	5857.272577	15.707059	-0.064747	4.132083
328.279831	5849.217818	15.712064	-0.064718	4.129285
328.490317	5841.210174	15.717069	-0.064752	4.126506
328.395104	5833.244991	15.722074	-0.064729	4.123736
328.127333	5825.261512	15.727079	-0.064674	4.120955
328.692258	5817.208373	15.732083	-0.064774	4.118160
328.681232	5809.284678	15.737088	-0.064767	4.115400
328.177512	5801.250840	15.742093	-0.064668	4.112592
328.009100	5793.255737	15.747098	-0.064631	4.109801
328.176629	5785.215898	15.752103	-0.064657	4.106997
328.031064	5777.197784	15.757107	-0.064625	4.104195
327.966157	5769.286393	15.762112	-0.064608	4.101429
328.111921	5761.177206	15.767117	-0.064630	4.098595
328.107863	5753.231339	15.772122	-0.064624	4.095813
327.915676	5745.202429	15.777127	-0.064583	4.092999
328.012854	5737.172435	15.782131	-0.064596	4.090186
327.917867	5729.254738	15.787136	-0.064573	4.087407
327.790442	5721.181099	15.792141	-0.064544	4.084572
328.110178	5713.240001	15.797146	-0.064598	4.081788
328.139021	5705.190422	15.802151	-0.064599	4.078959
328.101170	5697.273498	15.807155	-0.064586	4.076174
327.855919	5689.270667	15.812160	-0.064536	4.073354
327.751888	5681.249698	15.817165	-0.064511	4.070528
328.087229	5673.206537	15.822170	-0.064568	4.067699
327.945799	5665.189504	15.827175	-0.064537	4.064869
327.881079	5657.217227	15.832179	-0.064519	4.062055
327.939298	5649.232762	15.837184	-0.064525	4.059236
327.865139	5641.225199	15.842189	-0.064506	4.056405
327.767980	5633.224279	15.847194	-0.064483	4.053574
327.105362	5625.304319	15.852199	-0.064354	4.050760
327.439500	5617.230341	15.857203	-0.064411	4.047906
327.623065	5609.204761	15.862208	-0.064440	4.045065
327.562738	5601.227380	15.867213	-0.064424	4.042235
327.662673	5593.225528	15.872218	-0.064437	4.039397
327.602428	5585.276941	15.877223	-0.064421	4.036573
327.754722	5577.240860	15.882227	-0.064444	4.033719
327.586304	5569.210135	15.887232	-0.064408	4.030860
327.282953	5561.197513	15.892237	-0.064346	4.028004
327.220477	5553.227811	15.897242	-0.064329	4.025164
327.419054	5545.239434	15.902247	-0.064361	4.022321
327.479889	5537.203525	15.907251	-0.064367	4.019455
327.586621	5529.235893	15.912256	-0.064382	4.016614
327.044202	5521.278046	15.917261	-0.064276	4.013762
326.894158	5513.349551	15.922266	-0.064243	4.010926
326.918154	5505.285018	15.927271	-0.064242	4.008042
326.968258	5497.253822	15.932275	-0.064246	4.005168
327.063965	5489.307236	15.937280	-0.064259	4.002323
327.225996	5481.243814	15.942285	-0.064284	3.999436
326.870681	5473.354538	15.947290	-0.064212	3.996600
326.864289	5465.296842	15.952295	-0.064206	3.993707
327.117085	5457.236798	15.957299	-0.064248	3.990816
326.981480	5449.269944	15.962304	-0.064218	3.987950
326.690508	5441.260937	15.967309	-0.064158	3.985063
326.719231	5433.342770	15.972314	-0.064158	3.982213
326.475113	5425.300742	15.977319	-0.064108	3.979312
326.988375	5417.285316	15.982323	-0.064198	3.976431
326.909319	5409.269364	15.987328	-0.064178	3.973538
326.940005	5401.232224	15.992333	-0.064179	3.970636
326.588607	5393.316768	15.997338	-0.064108	3.967770
326.530496	5385.297545	16.002343	-0.064092	3.964869
326.533716	5377.330297	16.007347	-0.064088	3.961987
326.511097	5369.283113	16.012352	-0.064078	3.959072
325.827262	5361.421799	16.017357	-0.063946	3.956211
326.004787	5353.347934	16.022362	-0.063974	3.953286
325.532668	5345.394858	16.027367	-0.063881	3.950391
325.740855	5337.280599	16.032371	-0.063914	3.947448
325.973766	5329.243165	16.037376	-0.063952	3.944531
325.624880	5321.336029	16.042381	-0.063882	3.941649
326.159484	5313.270689	16.047386	-0.063977	3.938723
326.291582	5305.263775	16.052391	-0.063996	3.935809
326.000967	5297.272843	16.057395	-0.063937	3.932890
325.848159	5289.332930	16.062400	-0.063903	3.929991
325.581375	5281.299801	16.067405	-0.063848	3.927053
325.861124	5273.271265	16.072410	-0.063895	3.924125
326.206693	5265.299747	16.077415	-0.063954	3.921218
326.235314	5257.253633	16.082419	-0.063954	3.918274
325.979641	5249.354033	16.087424	-0.063902	3.915377
325.963268	5241.311301	16.092429	-0.063893	3.912429
326.081792	5233.290365	16.097434	-0.063910	3.909490
325.661995	5225.381015	16.102439	-0.063827	3.906579
326.001885	5217.295526	16.107443	-0.063885	3.903616
325.958666	5209.340459	16.112448	-0.063872	3.900692
325.784314	5201.343389	16.117453	-0.063834	3.897747
325.499468	5193.425474	16.122458	-0.063776	3.894826
325.718814	5185.371547	16.127463	-0.063812	3.891864
325.613456	5177.333108	16.132467	-0.063787	3.888898
325.355258	5169.451420	16.137472	-0.063734	3.885985
324.568204	5161.469893	16.142477	-0.063582	3.883022
325.188157	5153.391047	16.147482	-0.063692	3.880050
325.507226	5145.356059	16.152487	-0.063747	3.877085
324.949518	5137.425203	16.157491	-0.063638	3.874138
325.034925	5129.292510	16.162496	-0.063648	3.871128
325.541611	5121.209665	16.167501	-0.063737	3.868143
325.660115	5113.261712	16.172506	-0.063754	3.865197
325.425960	5105.352447	16.177511	-0.063706	3.862256
325.461896	5097.319646	16.182515	-0.063707	3.859273
325.404110	5089.357175	16.187520	-0.063691	3.856311
325.254006	5081.355832	16.192525	-0.063658	3.853331
325.259814	5073.382770	16.197530	-0.063654	3.850362
325.528405	5065.323609	16.202535	-0.063699	3.847365
325.469918	5057.299649	16.207539	-0.063683	3.844371
325.420874	5049.421897	16.212544	-0.063668	3.841430
324.896094	5041.446831	16.217549	-0.063566	3.838440
325.355618	5033.387940	16.222554	-0.063646	3.835437
325.425834	5025.373918	16.227559	-0.063654	3.832441
325.243305	5017.362720	16.232563	-0.063615	3.829438
325.209661	5009.411544	16.237568	-0.063603	3.826458
325.535706	5001.337021	16.242573	-0.063659	3.823437
326.016777	4993.371771	16.247578	-0.063743	3.820459
325.383044	4985.425176	16.252583	-0.063620	3.817460
325.295850	4977.399183	16.257587	-0.063599	3.814441
325.168898	4969.467432	16.262592	-0.063570	3.811455
325.039390	4961.412793	16.267597	-0.063540	3.808420
325.147237	4953.403274	16.272602	-0.063555	3.805404
325.260892	4945.455991	16.277607	-0.063571	3.802410
325.259422	4937.429317	16.282611	-0.063566	3.799381
325.297086	4929.494251	16.287616	-0.063568	3.796386
324.802968	4921.508884	16.292621	-0.063471	3.793356
325.076497	4913.423479	16.297626	-0.063516	3.790304
324.867860	4905.483877	16.302631	-0.063472	3.787293
324.972022	4897.397053	16.307635	-0.063487	3.784232
324.870295	4889.511413	16.312640	-0.063463	3.781239
324.635006	4881.476736	16.317645	-0.063414	3.778185
324.738243	4873.504746	16.322650	-0.063428	3.775160
324.358771	4865.563624	16.327655	-0.063352	3.772132
324.650296	4857.449027	16.332659	-0.063401	3.769052
324.850629	4849.460633	16.337664	-0.063433	3.766016
324.338486	4841.520409	16.342669	-0.063332	3.762978
324.346572	4833.562808	16.347674	-0.063329	3.759944
324.443337	4825.516039	16.352679	-0.063342	3.756875
324.390819	4817.477988	16.357683	-0.063327	3.753804
324.447664	4809.579142	16.362688	-0.063332	3.750786
324.273424	4801.527731	16.367693	-0.063294	3.747701
324.200187	4793.526241	16.372698	-0.063276	3.744636
324.166169	4785.532065	16.377703	-0.063264	3.741572
324.211336	4777.511659	16.382707	-0.063267	3.738497
324.633883	4769.485496	16.387712	-0.063341	3.735427
324.312128	4761.521602	16.392717	-0.063276	3.732359
324.738166	4753.478966	16.397722	-0.063350	3.729278
324.591645	4745.546859	16.402727	-0.063318	3.726222
324.447319	4737.526372	16.407731	-0.063285	3.723130
324.303500	4729.600842	16.412736	-0.063254	3.720071
324.063357	4721.583101	16.417741	-0.063204	3.716972
324.453151	4713.528731	16.422746	-0.063271	3.713873
324.446444	4705.516196	16.427751	-0.063265	3.710777
324.054507	4697.558672	16.432755	-0.063187	3.707689
324.390105	4689.479418	16.437760	-0.063244	3.704571
324.239429	4681.536959	16.442765	-0.063211	3.701491
324.662708	4673.503771	16.447770	-0.063284	3.698387
324.604867	4665.527330	16.452775	-0.063268	3.695291
323.946179	4657.629640	16.457779	-0.063141	3.692207
324.071841	4649.582798	16.462784	-0.063159	3.689083
324.047303	4641.574615	16.467789	-0.063149	3.685967
323.815625	4633.638669	16.472794	-0.063101	3.682871
323.680705	4625.655624	16.477799	-0.063070	3.679757
323.914836	4617.636447	16.482803	-0.063109	3.676636
323.976602	4609.619065	16.487808	-0.063115	3.673508
323.920464	4601.597461	16.492813	-0.063100	3.670373
323.645873	4593.646563	16.497818	-0.063043	3.667257
323.662953	4585.581807	16.502823	-0.063041	3.664102
323.860122	4577.658858	16.507827	-0.063073	3.661004
324.211623	4569.609150	16.512832	-0.063133	3.657858
324.140159	4561.610160	16.517837	-0.063115	3.654718
323.953569	4553.673854	16.522842	-0.063075	3.651597
323.967736	4545.640553	16.527847	-0.063072	3.648440
323.959779	4537.633221	16.532851	-0.063065	3.645290
323.875673	4529.705591	16.537856	-0.063045	3.642167
324.064950	4521.634709	16.542861	-0.063075	3.638992
323.934627	4513.745482	16.547866	-0.063045	3.635877
323.920897	4505.710858	16.552871	-0.063038	3.632706
323.639443	4497.752197	16.557875	-0.062980	3.629554
323.258766	4489.788762	16.562880	-0.062904	3.626394
323.537051	4481.661996	16.567885	-0.062951	3.623186
323.635136	4473.724704	16.572890	-0.062964	3.620045
323.469281	4465.725199	16.577895	-0.062928	3.616869
323.543462	4457.701228	16.582899	-0.062936	3.613688
323.050165	4449.780587	16.587904	-0.062839	3.610528
322.956301	4441.736692	16.592909	-0.062817	3.607328
323.259823	4433.697587	16.597914	-0.062868	3.604138
323.214331	4425.763162	16.602919	-0.062854	3.600978
323.212032	4417.726064	16.607923	-0.062849	3.597774
323.102951	4409.778322	16.612928	-0.062823	3.594601
322.866143	4401.788474	16.617933	-0.062774	3.591404
322.991651	4393.778220	16.622938	-0.062792	3.588207
322.909420	4385.778787	16.627943	-0.062772	3.585005
323.204334	4377.766242	16.632947	-0.062821	3.581806
323.139402	4369.742432	16.637952	-0.062804	3.578589
322.919559	4361.785716	16.642957	-0.062758	3.575391
322.979630	4353.818318	16.647962	-0.062764	3.572195
323.074846	4345.742758	16.652967	-0.062777	3.568954
323.212327	4337.784606	16.657971	-0.062797	3.565758
323.346974	4329.820567	16.662976	-0.062817	3.562556
323.225674	4321.823397	16.667981	-0.062789	3.559331
323.276349	4313.868442	16.672986	-0.062794	3.556125
322.882229	4305.860992	16.677991	-0.062715	3.552881
323.135932	4297.781400	16.682995	-0.062757	3.549625
323.233231	4289.799047	16.688000	-0.062770	3.546401
322.962146	4281.812115	16.693005	-0.062714	3.543160
323.014936	4273.881636	16.698010	-0.062719	3.539950
322.965217	4265.882349	16.703015	-0.062705	3.536705
322.760158	4257.878616	16.708019	-0.062661	3.533450
322.755722	4249.898289	16.713024	-0.062655	3.530209
322.837021	4241.854154	16.718029	-0.062665	3.526941
322.610266	4233.933486	16.723034	-0.062618	3.523711
322.418371	4225.948512	16.728039	-0.062577	3.520452
322.628168	4217.935720	16.733043	-0.062611	3.517192
322.842690	4209.897775	16.738048	-0.062646	3.513919
322.654036	4201.907380	16.743053	-0.062605	3.510650
322.790010	4193.923320	16.748058	-0.062625	3.507390
322.658257	4185.896128	16.753063	-0.062596	3.504101
322.586651	4177.952525	16.758067	-0.062577	3.500845
322.507810	4169.972779	16.763072	-0.062557	3.497571
322.402661	4161.957016	16.768077	-0.062533	3.494278
322.517626	4153.987493	16.773082	-0.062549	3.491008
322.524254	4145.959683	16.778087	-0.062545	3.487708
321.830073	4138.023046	16.783091	-0.062411	3.484419
322.084494	4130.060298	16.788096	-0.062453	3.481148
322.380595	4121.963056	16.793101	-0.062503	3.477819
322.256117	4113.998185	16.798106	-0.062474	3.474528
322.535825	4106.011177	16.803111	-0.062521	3.471238
322.272709	4098.000259	16.808115	-0.062467	3.467917
322.341294	4090.003297	16.813120	-0.062475	3.464609
322.234820	4082.028992	16.818125	-0.062450	3.461302
322.360169	4074.034359	16.823130	-0.062468	3.457991
322.299013	4066.039323	16.828135	-0.062451	3.454670
322.345464	4058.070949	16.833139	-0.062455	3.451361
322.470384	4050.063963	16.838144	-0.062473	3.448036
322.472684	4042.015559	16.843149	-0.062468	3.444686
322.076793	4034.177213	16.848154	-0.062389	3.441406
322.383399	4026.110152	16.853159	-0.062441	3.438052
322.401841	4018.112918	16.858163	-0.062439	3.434714
322.362892	4010.150642	16.863168	-0.062427	3.431385
322.076702	4002.160083	16.868173	-0.062369	3.428033
322.137235	3994.135763	16.873178	-0.062375	3.424675
322.039550	3986.150444	16.878183	-0.062351	3.421325
322.102876	3978.121512	16.883187	-0.062358	3.417959
322.435415	3970.130513	16.888192	-0.062415	3.414615
322.403744	3962.131958	16.893197	-0.062404	3.411252
322.248056	3954.154045	16.898202	-0.062370	3.407889
322.323304	3946.162247	16.903207	-0.062378	3.404526
322.420923	3938.208237	16.908211	-0.062391	3.401176
322.256367	3930.234111	16.913216	-0.062356	3.397805
321.908444	3922.254113	16.918221	-0.062286	3.394421
321.978499	3914.233873	16.923226	-0.062294	3.391032
321.664178	3906.226627	16.928231	-0.062230	3.387631
321.508526	3898.216124	16.933235	-0.062196	3.384232
321.469665	3890.280920	16.938240	-0.062183	3.380864
321.203371	3882.294671	16.943245	-0.062129	3.377464
321.382474	3874.264041	16.948250	-0.062157	3.374058
321.212825	3866.293006	16.953255	-0.062120	3.370660
321.462853	3858.237867	16.958259	-0.062161	3.367239
321.693968	3850.219533	16.963264	-0.062199	3.363830
321.294441	3842.319947	16.968269	-0.062120	3.360444
321.494292	3834.334347	16.973274	-0.062152	3.357040
321.144288	3826.364914	16.978279	-0.062081	3.353619
321.310808	3818.313844	16.983283	-0.062107	3.350180
321.402382	3810.343124	16.988288	-0.062119	3.346768
321.403144	3802.322317	16.993293	-0.062114	3.343328
321.434358	3794.381202	16.998298	-0.062115	3.339919
321.469207	3786.381790	17.003303	-0.062116	3.336483
321.319888	3778.380887	17.008307	-0.062083	3.333035
321.474336	3770.365594	17.013312	-0.062107	3.329589
321.488208	3762.371817	17.018317	-0.062104	3.326143
321.440392	3754.435229	17.023322	-0.062090	3.322716
321.041781	3746.468284	17.028327	-0.062011	3.319259
321.373171	3738.431177	17.033331	-0.062067	3.315796
321.548931	3730.442290	17.038336	-0.062095	3.312344
321.391119	3722.412583	17.043341	-0.062060	3.308858
321.168255	3714.458446	17.048346	-0.062013	3.305398
321.138598	3706.490906	17.053351	-0.062003	3.301937
321.168567	3698.486123	17.058355	-0.062003	3.298458
321.113893	3690.510393	17.063360	-0.061988	3.294985
321.024820	3682.504702	17.068365	-0.061966	3.291494
321.057899	3674.494944	17.073370	-0.061967	3.288002
321.127932	3666.488151	17.078375	-0.061975	3.284509
321.023111	3658.550890	17.083379	-0.061950	3.281036
320.915904	3650.591641	17.088384	-0.061925	3.277549
320.902193	3642.596668	17.093389	-0.061917	3.274047
320.735521	3634.650736	17.098394	-0.061881	3.270556
320.698722	3626.605366	17.103399	-0.061869	3.267023
320.783924	3618.583667	17.108403	-0.061880	3.263502
320.968129	3610.599680	17.113408	-0.061909	3.259997
320.712574	3602.651734	17.118413	-0.061856	3.256487
320.925703	3594.637549	17.123418	-0.061891	3.252963
320.838145	3586.633234	17.128423	-0.061869	3.249427
320.604368	3578.683179	17.133427	-0.061821	3.245905
320.529730	3570.700099	17.138432	-0.061802	3.242371
320.523201	3562.703841	17.143437	-0.061795	3.238831
320.425422	3554.753107	17.148442	-0.061772	3.235302
320.371934	3546.737994	17.153447	-0.061757	3.231744
320.558442	3538.709692	17.158451	-0.061786	3.228185
320.751973	3530.695802	17.163456	-0.061817	3.224629
320.530049	3522.735107	17.168461	-0.061771	3.221076
320.504113	3514.759716	17.173466	-0.061761	3.217520
320.296873	3506.765028	17.178471	-0.061717	3.213944
320.545418	3498.737096	17.183475	-0.061758	3.210369
320.489309	3490.782107	17.188480	-0.061742	3.206809
320.208780	3482.805981	17.193485	-0.061685	3.203227
320.086681	3474.850114	17.198490	-0.061657	3.199656
320.078580	3466.853939	17.203495	-0.061650	3.196067
320.107429	3458.854842	17.208499	-0.061651	3.192476
320.217191	3450.829834	17.213504	-0.061666	3.188872
319.969130	3442.858990	17.218509	-0.061615	3.185272
319.953610	3434.901655	17.223514	-0.061607	3.181685
320.027732	3426.887170	17.228519	-0.061615	3.178072
319.806391	3418.916845	17.233523	-0.061569	3.174462
320.095436	3410.911952	17.238528	-0.061617	3.170854
320.114463	3402.912188	17.243533	-0.061616	3.167233
319.697407	3394.960978	17.248538	-0.061533	3.163610
319.740954	3386.999174	17.253543	-0.061536	3.159999
319.890238	3378.999623	17.258547	-0.061559	3.156371
319.975784	3370.992174	17.263552	-0.061569	3.152733
319.486405	3363.022776	17.268557	-0.061473	3.149082
319.617177	3355.028021	17.273562	-0.061492	3.145443
319.702473	3347.039456	17.278567	-0.061503	3.141800
319.632377	3339.023704	17.283571	-0.061485	3.138134
319.443706	3331.053061	17.288576	-0.061444	3.134479
319.462386	3323.055410	17.293581	-0.061443	3.130816
319.608787	3315.041385	17.298586	-0.061465	3.127148
319.378357	3307.092873	17.303591	-0.061417	3.123488
319.271225	3299.112205	17.308595	-0.061392	3.119815
319.277063	3291.190627	17.313600	-0.061388	3.116170
319.104092	3283.158225	17.318605	-0.061350	3.112461
319.293573	3275.133991	17.323610	-0.061380	3.108768
319.300940	3267.149817	17.328615	-0.061377	3.105081
319.198604	3259.198412	17.333619	-0.061352	3.101399
319.226834	3251.211541	17.338624	-0.061352	3.097703
319.099559	3243.222442	17.343629	-0.061324	3.093994
318.873481	3235.273252	17.348634	-0.061276	3.090295
319.287799	3227.203029	17.353639	-0.061348	3.086565
319.397078	3219.211186	17.358643	-0.061363	3.082852
319.232921	3211.287816	17.363648	-0.061328	3.079154
318.929335	3203.372340	17.368653	-0.061266	3.075449
319.094636	3195.280547	17.373658	-0.061292	3.071679
319.080474	3187.294571	17.378663	-0.061284	3.067945
319.233744	3179.241665	17.383667	-0.061307	3.064184
319.086886	3171.353536	17.388672	-0.061275	3.060481
318.749318	3163.393752	17.393677	-0.061207	3.056730
319.042624	3155.354352	17.398682	-0.061256	3.052968
318.777276	3147.382290	17.403687	-0.061202	3.049206
318.461149	3139.464603	17.408691	-0.061138	3.045462
318.573424	3131.484855	17.413696	-0.061153	3.041705
318.423481	3123.490184	17.418701	-0.061120	3.037924
318.320894	3115.528298	17.423706	-0.061096	3.034155
318.430487	3107.506562	17.428711	-0.061111	3.030365
318.622229	3099.465077	17.433715	-0.061142	3.026564
318.431695	3091.525263	17.438720	-0.061101	3.022788
318.604920	3083.497215	17.443725	-0.061128	3.018983
318.509902	3075.566015	17.448730	-0.061105	3.015206
318.394429	3067.572940	17.453735	-0.061079	3.011394
318.307016	3059.564817	17.458739	-0.061057	3.007571
318.911674	3051.521921	17.463744	-0.061165	3.003761
318.955572	3043.542257	17.468749	-0.061168	2.999949
318.696241	3035.647517	17.473754	-0.061114	2.996157
318.712289	3027.653326	17.478759	-0.061112	2.992327
318.798014	3019.631975	17.483763	-0.061123	2.988482
318.676958	3011.684698	17.488768	-0.061095	2.984657
318.602254	3003.705714	17.493773	-0.061076	2.980815
318.685029	2995.733665	17.498778	-0.061086	2.976979
318.763107	2987.726431	17.503783	-0.061096	2.973121
318.729237	2979.712605	17.508787	-0.061084	2.969248
318.816908	2971.771549	17.513792	-0.061095	2.965413
318.604414	2963.818580	17.518797	-0.061051	2.961550
318.916033	2955.786213	17.523802	-0.061104	2.957672
318.715811	2947.867603	17.528807	-0.061061	2.953817
318.333459	2939.903607	17.533811	-0.060985	2.949925
318.210517	2931.934107	17.538816	-0.060957	2.946039
318.365724	2923.889000	17.543821	-0.060981	2.942126
318.508537	2915.919799	17.548826	-0.061002	2.938244
318.301309	2907.951694	17.553831	-0.060958	2.934339
318.212457	2899.943007	17.558835	-0.060937	2.930415
318.337985	2891.971719	17.563840	-0.060955	2.926516
318.266649	2884.003519	17.568845	-0.060936	2.922602
317.835330	2876.107510	17.573850	-0.060851	2.918699
317.744426	2868.123631	17.578855	-0.060829	2.914766
318.051415	2860.006909	17.583859	-0.060881	2.910784
317.533781	2852.116305	17.588864	-0.060779	2.906862
317.292061	2844.122475	17.593869	-0.060729	2.902900
317.597573	2836.091132	17.598874	-0.060781	2.898944
317.657564	2828.116974	17.603879	-0.060787	2.894997
317.596896	2820.124425	17.608883	-0.060770	2.891029
317.486995	2812.164116	17.613888	-0.060745	2.887069
317.521534	2804.163407	17.618893	-0.060746	2.883091
317.552816	2796.187868	17.623898	-0.060747	2.879120
317.239216	2788.289161	17.628903	-0.060683	2.875162
316.997261	2780.325311	17.633907	-0.060633	2.871171
317.296272	2772.280174	17.638912	-0.060683	2.867164
317.217317	2764.272832	17.643917	-0.060663	2.863149
317.106592	2756.345688	17.648922	-0.060638	2.859166
317.261886	2748.343445	17.653927	-0.060661	2.855156
316.889817	2740.405710	17.658931	-0.060587	2.851142
317.148907	2732.366341	17.663936	-0.060630	2.847107
316.944939	2724.402372	17.668941	-0.060587	2.843078
317.288554	2716.412947	17.673946	-0.060646	2.839062
317.016157	2708.486279	17.678951	-0.060590	2.835037
317.232182	2700.460624	17.683955	-0.060625	2.830984
317.407568	2692.443647	17.688960	-0.060652	2.826927
317.196945	2684.480187	17.693965	-0.060608	2.822869
316.835348	2676.581932	17.698970	-0.060536	2.818830
317.141838	2668.540658	17.703975	-0.060588	2.814751
317.126516	2660.564105	17.708979	-0.060580	2.810680
317.241164	2652.580347	17.713984	-0.060596	2.806607
317.276408	2644.588092	17.718989	-0.060597	2.802520
317.121217	2636.670471	17.723994	-0.060563	2.798453
316.910978	2628.709476	17.728999	-0.060519	2.794355
316.739869	2620.751450	17.734003	-0.060482	2.790254
317.148488	2612.707584	17.739008	-0.060553	2.786139
316.942594	2604.755370	17.744013	-0.060509	2.782027
316.975560	2596.807489	17.749018	-0.060510	2.777926
316.724445	2588.855904	17.754023	-0.060458	2.773799
316.829397	2580.827898	17.759027	-0.060473	2.769649
316.639362	2572.880406	17.764032	-0.060432	2.765516
316.901091	2564.865608	17.769037	-0.060476	2.761370
316.873147	2556.902432	17.774042	-0.060465	2.757226
316.757470	2548.930515	17.779047	-0.060439	2.753067
316.649873	2540.910549	17.784051	-0.060413	2.748876
316.779693	2532.933106	17.789056	-0.060432	2.744716
316.535243	2524.986102	17.794061	-0.060382	2.740542
316.538809	2517.032419	17.799066	-0.060377	2.736374
316.533997	2509.047278	17.804071	-0.060371	2.732182
316.307389	2501.092080	17.809075	-0.060324	2.727986
316.646748	2493.061145	17.814080	-0.060382	2.723779
316.667843	2485.106728	17.819085	-0.060381	2.719586
316.649668	2477.174611	17.824090	-0.060372	2.715396
316.536674	2469.199544	17.829095	-0.060346	2.711170
316.506621	2461.202806	17.834099	-0.060335	2.706931
316.707295	2453.214197	17.839104	-0.060367	2.702705
316.455711	2445.261682	17.844109	-0.060315	2.698463
316.232634	2437.345899	17.849114	-0.060269	2.694235
316.432310	2429.328057	17.854119	-0.060301	2.689974
316.396042	2421.340442	17.859123	-0.060289	2.685706
316.465137	2413.384768	17.864128	-0.060297	2.681456
316.341682	2405.434327	17.869133	-0.060268	2.677189
316.324903	2397.477760	17.874138	-0.060260	2.672919
316.132270	2389.493937	17.879143	-0.060219	2.668616
315.969524	2381.504362	17.884147	-0.060184	2.664305
315.817718	2373.607472	17.889152	-0.060150	2.660037
315.908879	2365.582501	17.894157	-0.060162	2.655710
315.904753	2357.596148	17.899162	-0.060156	2.651390
315.801818	2349.621198	17.904167	-0.060132	2.647063
315.572145	2341.681351	17.909171	-0.060084	2.642739
315.461374	2333.744773	17.914176	-0.060058	2.638417
315.411274	2325.742108	17.919181	-0.060044	2.634057
315.439604	2317.756698	17.924186	-0.060044	2.629704
315.044710	2309.835756	17.929191	-0.059965	2.625351
315.487209	2301.767887	17.934195	-0.060042	2.620966
315.457235	2293.838567	17.939200	-0.060032	2.616618
315.146725	2285.895312	17.944205	-0.059969	2.612236
315.610830	2277.844698	17.949210	-0.060050	2.607841
315.191304	2269.955338	17.954215	-0.059967	2.603467
315.139290	2261.982986	17.959219	-0.059952	2.599064
315.237228	2254.020251	17.964224	-0.059965	2.594670
314.925275	2245.980348	17.969229	-0.059902	2.590197
315.217955	2237.925147	17.974234	-0.059951	2.585750
315.194309	2229.999136	17.979239	-0.059941	2.581345
315.059752	2222.062033	17.984243	-0.059911	2.576918
315.293428	2214.090545	17.989248	-0.059950	2.572491
315.253548	2206.116827	17.994253	-0.059937	2.568035
314.488957	2198.281775	17.999258	-0.059790	2.563598
314.180675	2190.353349	18.004263	-0.059727	2.559133
314.682828	2182.248020	18.009267	-0.059815	2.554619
314.615729	2174.319027	18.014272	-0.059798	2.550155
314.476391	2166.333187	18.019277	-0.059767	2.545647
315.045902	2158.294763	18.024282	-0.059867	2.541151
314.352530	2150.463767	18.029287	-0.059733	2.536674
314.742957	2142.393127	18.034291	-0.059801	2.532132
314.776264	2134.460220	18.039296	-0.059802	2.527633
314.852609	2126.461771	18.044301	-0.059811	2.523093
314.848925	2118.550998	18.049306	-0.059805	2.518588
314.456167	2110.633604	18.054311	-0.059727	2.514043
314.447155	2102.650769	18.059315	-0.059720	2.509481
314.688275	2094.625760	18.064320	-0.059760	2.504904
314.845886	2086.635082	18.069325	-0.059784	2.500333
314.728225	2078.728380	18.074330	-0.059757	2.495781
315.002963	2070.701869	18.079335	-0.059803	2.491181
314.456073	2062.838856	18.084339	-0.059696	2.486605
314.723779	2054.838048	18.089344	-0.059741	2.482003
314.347876	2046.925354	18.094349	-0.059665	2.477394
314.386714	2038.954165	18.099354	-0.059667	2.472775
314.354811	2030.984578	18.104359	-0.059656	2.468142
314.484433	2022.973908	18.109363	-0.059675	2.463488
314.319017	2015.081031	18.114368	-0.059639	2.458873
314.199876	2007.103021	18.119373	-0.059612	2.454202
314.115512	1999.166844	18.124378	-0.059591	2.449549
314.447254	1991.133877	18.129383	-0.059648	2.444863
314.010138	1983.255044	18.134387	-0.059561	2.440199
314.185058	1975.266688	18.139392	-0.059589	2.435509
313.904903	1967.303536	18.144397	-0.059531	2.430790
313.643813	1959.364832	18.149402	-0.059478	2.426077
313.628940	1951.394967	18.154407	-0.059470	2.421355
314.016714	1943.348841	18.159411	-0.059537	2.416611
314.025926	1935.413666	18.164416	-0.059533	2.411894
313.926046	1927.449430	18.169421	-0.059510	2.407142
314.072724	1919.476052	18.174426	-0.059532	2.402394
314.051011	1911.544307	18.179431	-0.059523	2.397649
313.734847	1903.637118	18.184435	-0.059459	2.392884
313.866610	1895.673410	18.189440	-0.059478	2.388113
313.836281	1887.688266	18.194445	-0.059467	2.383306
313.807044	1879.742889	18.199450	-0.059457	2.378514
313.621376	1871.805243	18.204455	-0.059417	2.373703
313.682183	1863.829844	18.209459	-0.059423	2.368880
313.720511	1855.862113	18.214464	-0.059425	2.364050
313.627891	1847.934296	18.219469	-0.059403	2.359224
313.820977	1839.972670	18.224474	-0.059434	2.354391
313.885876	1832.010967	18.229479	-0.059440	2.349537
313.599350	1824.056686	18.234483	-0.059382	2.344649
313.407287	1816.157173	18.239488	-0.059341	2.339791
313.331571	1808.197599	18.244493	-0.059322	2.334897
313.390299	1800.202407	18.249498	-0.059328	2.329981
313.323561	1792.237688	18.254503	-0.059310	2.325063
313.015600	1784.367104	18.259507	-0.059248	2.320173
312.925559	1776.451141	18.264512	-0.059226	2.315262
313.001786	1768.418851	18.269517	-0.059235	2.310283
313.199254	1760.432982	18.274522	-0.059266	2.305333
313.152022	1752.509140	18.279527	-0.059252	2.300390
313.243993	1744.529450	18.284531	-0.059264	2.295413
313.273672	1736.600268	18.289536	-0.059265	2.290451
313.364543	1728.613149	18.294541	-0.059277	2.285448
313.268736	1720.712742	18.299546	-0.059254	2.280472
312.863310	1712.844195	18.304551	-0.059173	2.275478
312.997884	1704.796090	18.309555	-0.059193	2.270407
313.042270	1696.834097	18.314560	-0.059196	2.265371
312.519165	1688.957140	18.319565	-0.059093	2.260328
312.601745	1680.980875	18.324570	-0.059104	2.255264
312.632245	1673.019218	18.329575	-0.059104	2.250193
312.532705	1665.062440	18.334579	-0.059081	2.245102
312.365320	1657.170793	18.339584	-0.059044	2.240035
312.200689	1649.233044	18.344589	-0.059009	2.234928
311.885129	1641.340592	18.349594	-0.058945	2.229824
311.500229	1633.415950	18.354599	-0.058868	2.224681
311.606476	1625.407303	18.359603	-0.058882	2.219517
312.113512	1617.374076	18.364608	-0.058972	2.214361
311.884914	1609.448577	18.369613	-0.058924	2.209196
311.807823	1601.515267	18.374618	-0.058905	2.204028
312.215521	1593.525154	18.379623	-0.058975	2.198855
311.928863	1585.631154	18.384627	-0.058917	2.193669
311.873215	1577.709120	18.389632	-0.058901	2.188473
312.023784	1569.694178	18.394637	-0.058924	2.183224
312.341355	1561.728096	18.399642	-0.058978	2.178009
312.289094	1553.803883	18.404647	-0.058963	2.172775
312.247853	1545.874818	18.409651	-0.058950	2.167526
312.146053	1537.972466	18.414656	-0.058926	2.162276
312.242205	1530.026036	18.419661	-0.058939	2.157003
312.026464	1522.132724	18.424666	-0.058894	2.151723
312.209506	1514.143957	18.429671	-0.058923	2.146404
312.077339	1506.235108	18.434675	-0.058893	2.141095
311.793728	1498.368709	18.439680	-0.058835	2.135786
311.779514	1490.397466	18.444685	-0.058827	2.130420
311.639316	1482.477906	18.449690	-0.058796	2.125063
311.732197	1474.530152	18.454695	-0.058808	2.119696
311.676769	1466.590360	18.459699	-0.058793	2.114307
311.787322	1458.616255	18.464704	-0.058808	2.108896
311.661092	1450.665115	18.469709	-0.058780	2.103464
311.149083	1442.844091	18.474714	-0.058679	2.098068
311.366717	1434.845117	18.479719	-0.058715	2.092610
311.175466	1426.915572	18.484723	-0.058674	2.087143
311.249672	1418.989204	18.489728	-0.058683	2.081692
311.127063	1411.066477	18.494733	-0.058655	2.076208
311.032070	1403.158230	18.499738	-0.058632	2.070723
310.924678	1395.221832	18.504743	-0.058607	2.065202
311.174472	1387.233672	18.509747	-0.058648	2.059667
311.422956	1379.290187	18.514752	-0.058689	2.054148
311.146940	1371.387122	18.519757	-0.058633	2.048589
310.984664	1363.495379	18.524762	-0.058597	2.043034
310.928192	1355.598953	18.529767	-0.058582	2.037472
310.927861	1347.651083	18.534771	-0.058577	2.031864
310.998729	1339.705341	18.539776	-0.058585	2.026249
310.671042	1331.811807	18.544781	-0.058518	2.020614
310.354446	1323.938224	18.549786	-0.058454	2.014979
310.787701	1315.914341	18.554791	-0.058530	2.009299
310.551955	1308.025340	18.559795	-0.058481	2.003630
310.529769	1300.131372	18.564800	-0.058472	1.997963
310.199407	1292.238809	18.569805	-0.058405	1.992248
310.204065	1284.309825	18.574810	-0.058401	1.986526
309.903831	1276.424896	18.579815	-0.058340	1.980787
309.802773	1268.490274	18.584819	-0.058316	1.975016
310.080653	1260.524026	18.589824	-0.058362	1.969247
309.755998	1252.647592	18.594829	-0.058297	1.963461
309.669978	1244.765354	18.599834	-0.058276	1.957679
309.664764	1236.827648	18.604839	-0.058270	1.951848
309.602216	1228.878474	18.609843	-0.058253	1.945985
309.246049	1221.030683	18.614848	-0.058182	1.940147
309.689068	1212.994179	18.619853	-0.058259	1.934240
309.855008	1205.041327	18.624858	-0.058285	1.928347
309.931876	1197.132789	18.629863	-0.058294	1.922458
309.828999	1189.238959	18.634867	-0.058270	1.916542
309.701951	1181.364501	18.639872	-0.058241	1.910619
309.625092	1173.439603	18.644877	-0.058221	1.904646
309.682750	1165.548027	18.649882	-0.058227	1.898695
309.343063	1157.692468	18.654887	-0.058159	1.892706
309.157985	1149.795572	18.659891	-0.058119	1.886685
309.175937	1141.893611	18.664896	-0.058117	1.880664
309.201352	1133.969903	18.669901	-0.058117	1.874608
309.369555	1126.021840	18.674906	-0.058143	1.868530
309.543000	1118.073133	18.679911	-0.058170	1.862433
309.423815	1110.212744	18.684915	-0.058143	1.856349
309.452827	1102.309344	18.689920	-0.058143	1.850229
309.196032	1094.438718	18.694925	-0.058090	1.844081
309.042976	1086.592133	18.699930	-0.058057	1.837943
309.199823	1078.647571	18.704935	-0.058081	1.831745
309.014415	1070.755389	18.709939	-0.058041	1.825526
309.000396	1062.885676	18.714944	-0.058034	1.819324
309.196395	1054.937707	18.719949	-0.058065	1.813065
309.270397	1047.024874	18.724954	-0.058074	1.806797
308.894028	1039.215366	18.729959	-0.057998	1.800534
308.630098	1031.369430	18.734963	-0.057944	1.794233
308.578931	1023.454777	18.739968	-0.057930	1.787882
308.050905	1015.613684	18.744973	-0.057826	1.781508
308.368549	1007.656448	18.749978	-0.057880	1.775123
308.593481	999.713129	18.754983	-0.057917	1.768715
308.519041	991.823500	18.759987	-0.057898	1.762289
308.462813	983.977187	18.764992	-0.057882	1.755877
308.543083	976.077278	18.769997	-0.057892	1.749415
308.650463	968.171286	18.775002	-0.057907	1.742928
308.486103	960.321038	18.780007	-0.057871	1.736428
308.525597	952.424399	18.785011	-0.057874	1.729891
308.247089	944.626904	18.790016	-0.057817	1.723370
307.990356	936.783473	18.795021	-0.057764	1.716789
307.538046	928.994130	18.800026	-0.057675	1.710202
308.199521	920.953363	18.805031	-0.057793	1.703526
308.471534	913.031787	18.810035	-0.057838	1.696872
308.373110	905.190466	18.815040	-0.057815	1.690211
308.380773	897.323548	18.820045	-0.057811	1.683515
308.376286	889.477756	18.825050	-0.057805	1.676810
308.159093	881.639746	18.830055	-0.057760	1.670055
307.976541	873.807296	18.835059	-0.057721	1.663282
307.829474	865.986269	18.840064	-0.057688	1.656496
307.842005	858.098374	18.845069	-0.057685	1.649646
307.554258	850.290966	18.850074	-0.057627	1.642796
307.549321	842.438741	18.855079	-0.057621	1.635918
307.447639	834.532794	18.860083	-0.057597	1.628950
307.279933	826.702688	18.865088	-0.057561	1.622009
307.035336	818.872374	18.870093	-0.057510	1.615027
306.917477	811.037207	18.875098	-0.057483	1.608029
307.188396	803.106279	18.880103	-0.057528	1.600970
307.146527	795.274564	18.885107	-0.057515	1.593924
307.308449	787.406795	18.890112	-0.057540	1.586844
307.065397	779.599275	18.895117	-0.057490	1.579728
307.073891	771.757048	18.900122	-0.057487	1.572584
307.413017	763.844936	18.905127	-0.057545	1.565394
307.299531	756.055286	18.910131	-0.057518	1.558215
307.226461	748.245618	18.915136	-0.057500	1.550990
306.986673	740.441185	18.920141	-0.057450	1.543712
306.996504	732.613608	18.925146	-0.057447	1.536415
306.832262	724.796939	18.930151	-0.057411	1.529067
306.869373	716.967255	18.935155	-0.057413	1.521702
306.882279	709.159702	18.940160	-0.057410	1.514318
306.463083	701.407977	18.945165	-0.057327	1.506884
305.865456	693.684483	18.950170	-0.057211	1.499413
306.351537	685.754990	18.955175	-0.057297	1.491876
306.266783	677.937501	18.960179	-0.057276	1.484319
306.047265	670.187405	18.965184	-0.057230	1.476767
306.070683	662.333063	18.970189	-0.057229	1.469113
306.154775	654.493805	18.975194	-0.057240	1.461444
306.314852	646.659420	18.980199	-0.057264	1.453752
306.385447	638.836461	18.985203	-0.057273	1.446016
306.516649	631.055635	18.990208	-0.057292	1.438289
306.199697	623.313903	18.995213	-0.057228	1.430487
306.035652	615.560631	19.000218	-0.057192	1.422655
306.049607	607.782516	19.005223	-0.057190	1.414784
305.937525	600.003450	19.010227	-0.057164	1.406847
306.231974	592.183623	19.015232	-0.057214	1.398893
306.290676	584.390396	19.020237	-0.057220	1.390880
306.269216	576.633413	19.025242	-0.057211	1.382844
306.057746	568.911671	19.030247	-0.057166	1.374765
306.176808	561.118690	19.035251	-0.057183	1.366622
305.908787	553.438850	19.040256	-0.057129	1.358481
305.373346	545.762934	19.045261	-0.057024	1.350247
305.603487	537.948262	19.050266	-0.057062	1.341951
305.788571	530.169632	19.055271	-0.057091	1.333635
305.647381	522.443337	19.060275	-0.057060	1.325263
305.441259	514.773372	19.065280	-0.057017	1.316888
305.233611	506.977727	19.070285	-0.056973	1.308321
305.217150	499.229292	19.075290	-0.056965	1.299785
305.102436	491.513704	19.080295	-0.056938	1.291211
305.299905	483.759624	19.085299	-0.056970	1.282596
305.318395	476.063018	19.090304	-0.056969	1.273952
304.934195	468.409895	19.095309	-0.056892	1.265222
304.681179	460.762053	19.100314	-0.056840	1.256463
304.781088	453.036895	19.105319	-0.056854	1.247621
304.883887	445.317179	19.110323	-0.056868	1.238724
304.696343	437.675986	19.115328	-0.056828	1.229796
304.412572	430.019876	19.120333	-0.056770	1.220766
304.457291	422.344683	19.125338	-0.056774	1.211712
304.370891	414.675756	19.130343	-0.056753	1.202571
304.416146	407.004210	19.135347	-0.056756	1.193384
304.233537	399.390232	19.140352	-0.056717	1.184148
304.361408	391.700241	19.145357	-0.056736	1.174811
304.306123	384.078683	19.150362	-0.056721	1.165446
304.105172	376.488078	19.155367	-0.056678	1.156012
304.148240	368.827908	19.160371	-0.056681	1.146465
303.914791	361.255478	19.165376	-0.056633	1.136889
303.916250	353.619519	19.170381	-0.056628	1.127202
303.979304	346.019973	19.175386	-0.056635	1.117492
303.608679	338.493070	19.180391	-0.056561	1.107694
303.537422	330.913725	19.185395	-0.056543	1.097807
303.234955	323.397261	19.190400	-0.056482	1.087860
303.427025	315.785834	19.195405	-0.056513	1.077809
303.280518	308.246598	19.200410	-0.056481	1.067682
303.552500	300.648185	19.205415	-0.056526	1.057475
302.917185	293.228427	19.210419	-0.056403	1.047199
303.136056	285.669367	19.215424	-0.056439	1.036833
302.921258	278.187674	19.220429	-0.056394	1.026365
303.007561	270.674934	19.225434	-0.056406	1.015819
303.100841	263.167268	19.230439	-0.056418	1.005172
302.750990	255.767865	19.235443	-0.056348	0.994455
302.788505	248.279348	19.240448	-0.056350	0.983590
302.457566	240.880925	19.245453	-0.056284	0.972642
301.877739	233.550989	19.250458	-0.056171	0.961606
302.011655	226.095287	19.255463	-0.056191	0.950441
301.687670	218.745827	19.260467	-0.056126	0.939182
301.851645	211.324553	19.265472	-0.056152	0.927808
302.006436	203.922705	19.270477	-0.056176	0.916321
301.854074	196.603787	19.275482	-0.056143	0.904734
301.785910	189.278627	19.280487	-0.056126	0.893011
301.698985	181.976738	19.285491	-0.056105	0.881163
301.688517	174.701937	19.290496	-0.056098	0.869222
301.353470	167.489332	19.295501	-0.056031	0.857122
301.102358	160.292891	19.300506	-0.055980	0.844902
300.856241	153.106210	19.305511	-0.055929	0.832520
301.069945	145.840905	19.310515	-0.055964	0.819956
300.655513	138.741564	19.315520	-0.055882	0.807294
299.984098	131.710673	19.320525	-0.055753	0.794472
299.783052	124.618828	19.325530	-0.055711	0.781479
298.868872	117.680819	19.330535	-0.055536	0.768318
297.139825	110.913536	19.335539	-0.055210	0.754977
294.238776	104.346272	19.340544	-0.054665	0.741377
292.026716	97.652103	19.345549	-0.054249	0.727514
290.579339	90.858834	19.350554	-0.053975	0.713454
289.472483	84.029520	19.355559	-0.053765	0.699161
288.509202	77.392656	19.360563	-0.053581	0.685026