Fri Apr 16 19:19:55 2021

Number of Points = 3638
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.545367	0.154226	0.000000	0.000146	0.311763

0.686780	0.127441	0.005005	0.000120	0.311758
0.939156	0.079989	0.010010	0.000073	0.311751
1.215150	0.025185	0.015014	0.000021	0.311730
1.019584	0.064873	0.020019	0.000058	0.311749
1.095396	0.047577	0.025024	0.000043	0.311733
1.122124	0.043697	0.030029	0.000038	0.311738
1.388148	-0.038971	0.035034	-0.000011	0.311578
1.140999	-0.031581	0.040038	0.000035	0.311404
1.006854	-0.004799	0.045043	0.000060	0.311416
1.006782	-0.007117	0.050048	0.000060	0.311405
0.867351	0.019975	0.055053	0.000086	0.311414
1.358362	-0.072544	0.060058	-0.000006	0.311398
1.160323	-0.035633	0.065062	0.000031	0.311403
1.427115	-0.083313	0.070067	-0.000019	0.311407
1.102691	-0.024524	0.075072	0.000042	0.311406
1.071447	-0.018578	0.080077	0.000048	0.311408
0.840088	0.028377	0.085082	0.000091	0.311431
0.676995	0.034389	0.090086	0.000121	0.311321
1.152394	-0.098256	0.095091	0.000032	0.311106
1.164834	-0.102798	0.100096	0.000030	0.311096
0.824676	-0.037936	0.105101	0.000093	0.311110
0.938461	-0.058516	0.110106	0.000072	0.311111
1.123454	-0.096497	0.115110	0.000038	0.311091
1.326716	-0.138519	0.120115	-0.000000	0.311067
1.058526	-0.150818	0.125120	0.000050	0.310784
1.212998	-0.181108	0.130125	0.000021	0.310773
1.039635	-0.147088	0.135130	0.000053	0.310785
1.063017	-0.153029	0.140134	0.000049	0.310778
1.287372	-0.212921	0.145139	0.000007	0.310689
1.275867	-0.247692	0.150144	0.000009	0.310517
0.970282	-0.187741	0.155149	0.000066	0.310538
0.670924	-0.130966	0.160154	0.000121	0.310549
0.398034	-0.084134	0.165158	0.000172	0.310537
0.986537	-0.261237	0.170163	0.000063	0.310210
1.111973	-0.289148	0.175168	0.000039	0.310186
1.315161	-0.328917	0.180173	0.000001	0.310173
1.085898	-0.308319	0.185178	0.000044	0.310075
0.459626	-0.235184	0.190182	0.000161	0.309885
0.774927	-0.291095	0.195187	0.000102	0.309892
0.573323	-0.257225	0.200192	0.000139	0.309879
0.960017	-0.382914	0.205197	0.000067	0.309621
0.497912	-0.310656	0.210202	0.000153	0.309566
0.678651	-0.347418	0.215206	0.000120	0.309548
1.118301	-0.460746	0.220211	0.000038	0.309392
0.999868	-0.467564	0.225216	0.000060	0.309260
0.892076	-0.447604	0.230221	0.000080	0.309261
0.779291	-0.475578	0.235226	0.000101	0.309035
0.652717	-0.474976	0.240230	0.000124	0.308930
0.934980	-0.526373	0.245235	0.000072	0.308930
0.733168	-0.551001	0.250240	0.000109	0.308643
0.760832	-0.560369	0.255245	0.000104	0.308623
0.774167	-0.583222	0.260250	0.000102	0.308527
1.033111	-0.682509	0.265254	0.000053	0.308282
1.157311	-0.703396	0.270259	0.000030	0.308290
1.486676	-0.823411	0.275264	-0.000031	0.308008
1.256530	-0.786168	0.280269	0.000012	0.307987
1.513247	-0.885716	0.285274	-0.000036	0.307738
1.644737	-0.931000	0.290278	-0.000060	0.307638
1.609488	-0.968828	0.295283	-0.000054	0.307430
1.334932	-0.938046	0.300288	-0.000003	0.307340
0.875542	-0.900326	0.305293	0.000083	0.307125
0.545197	-0.858572	0.310298	0.000144	0.307039
0.717310	-0.926918	0.315302	0.000112	0.306865
0.803286	-0.966577	0.320307	0.000096	0.306752
1.217889	-1.083216	0.325312	0.000019	0.306557
1.350667	-1.142820	0.330317	-0.000006	0.306390
0.920632	-1.103349	0.335322	0.000074	0.306207
1.082704	-1.158601	0.340326	0.000044	0.306085
0.946313	-1.186345	0.345331	0.000069	0.305837
0.776089	-1.169603	0.350336	0.000101	0.305770
0.752885	-1.216936	0.355341	0.000105	0.305526
1.029040	-1.280532	0.360346	0.000054	0.305463
0.519111	-1.247727	0.365350	0.000149	0.305180
0.358858	-1.237280	0.370355	0.000178	0.305091
0.400663	-1.291628	0.375360	0.000171	0.304870
0.676624	-1.381863	0.380365	0.000119	0.304680
0.680155	-1.412598	0.385370	0.000119	0.304537
0.534174	-1.437738	0.390374	0.000146	0.304292
0.784666	-1.504671	0.395379	0.000099	0.304190
0.227297	-1.460144	0.400384	0.000203	0.303920
0.079488	-1.462898	0.405389	0.000230	0.303779
0.339033	-1.545099	0.410394	0.000182	0.303613
0.514089	-1.636719	0.415398	0.000149	0.303328
0.841254	-1.723138	0.420403	0.000089	0.303199
0.717672	-1.746559	0.425408	0.000112	0.302980
0.539620	-1.765103	0.430413	0.000145	0.302737
0.689565	-1.826616	0.435418	0.000117	0.302574
0.875115	-1.913070	0.440422	0.000082	0.302322
0.808414	-1.952834	0.445427	0.000095	0.302074
0.528237	-1.938364	0.450432	0.000147	0.301899
0.361558	-1.946496	0.455437	0.000178	0.301715
0.209200	-1.976444	0.460442	0.000206	0.301439
0.415868	-2.054226	0.465446	0.000168	0.301246
0.298698	-2.066378	0.470451	0.000189	0.301086
-0.086147	-2.061419	0.475456	0.000261	0.300773
0.558592	-2.210875	0.480461	0.000141	0.300618
0.574218	-2.250130	0.485466	0.000138	0.300443
0.530509	-2.299984	0.490470	0.000146	0.300165
-0.132551	-2.231160	0.495475	0.000270	0.299916
-0.587421	-2.187843	0.500480	0.000354	0.299726
-0.493754	-2.244909	0.505485	0.000337	0.299533
-0.701906	-2.261952	0.510490	0.000375	0.299268
-0.755528	-2.297835	0.515494	0.000385	0.299048
-0.428723	-2.400938	0.520499	0.000325	0.298836
-0.689786	-2.404327	0.525504	0.000373	0.298590
-1.642266	-2.290357	0.530509	0.000550	0.298304
-2.703487	-2.124544	0.535514	0.000748	0.298173
-3.228286	-2.068560	0.540518	0.000846	0.297982
-4.015471	-1.966501	0.545523	0.000992	0.297783
-3.795996	-2.032067	0.550528	0.000951	0.297658
-3.407152	-2.160091	0.555533	0.000879	0.297379
-4.433129	-1.986907	0.560538	0.001070	0.297315
-4.602394	-2.017798	0.565542	0.001101	0.297015
-4.101664	-2.125212	0.570547	0.001008	0.296935
-4.927083	-2.014758	0.575552	0.001161	0.296743
-5.441557	-1.953977	0.580557	0.001257	0.296583
-5.589566	-1.963234	0.585562	0.001285	0.296407
-4.991865	-2.109219	0.590566	0.001173	0.296225
-5.781620	-1.989834	0.595571	0.001320	0.296107
-5.775100	-2.035882	0.600576	0.001319	0.295888
-6.117478	-1.995583	0.605581	0.001383	0.295781
-6.074886	-2.039010	0.610586	0.001375	0.295606
-6.383173	-1.998614	0.615590	0.001432	0.295530
-6.016203	-2.117606	0.620595	0.001364	0.295274
-6.759999	-2.000283	0.625600	0.001502	0.295187
-7.354979	-1.941849	0.630605	0.001613	0.294943
-6.929250	-2.031914	0.635610	0.001534	0.294881
-6.331100	-2.199426	0.640614	0.001422	0.294593
-7.111715	-2.069926	0.645619	0.001568	0.294532
-7.512683	-2.046989	0.650624	0.001642	0.294287
-7.530703	-2.050390	0.655629	0.001646	0.294254
-7.687916	-2.079663	0.660634	0.001675	0.293970
-8.288554	-1.982218	0.665638	0.001787	0.293912
-8.487240	-1.988706	0.670643	0.001824	0.293702
-9.160794	-1.880162	0.675648	0.001949	0.293634
-9.196439	-1.905909	0.680653	0.001955	0.293476
-9.078987	-1.962022	0.685658	0.001934	0.293304
-8.859965	-2.017791	0.690662	0.001893	0.293226
-9.210095	-1.998658	0.695667	0.001958	0.293006
-9.163592	-2.012391	0.700672	0.001949	0.292980
-9.601459	-1.997361	0.705677	0.002031	0.292661
-9.797858	-1.959181	0.710682	0.002067	0.292674
-9.868139	-1.999683	0.715686	0.002080	0.292411
-9.787879	-2.024694	0.720691	0.002065	0.292359
-10.240566	-1.978342	0.725696	0.002150	0.292181
-11.023695	-1.863823	0.730701	0.002295	0.292044
-10.374996	-1.992137	0.735706	0.002174	0.291992
-10.787236	-1.967246	0.740710	0.002251	0.291745
-11.253118	-1.880360	0.745715	0.002338	0.291756
-11.693092	-1.847276	0.750720	0.002420	0.291523
-11.803757	-1.844808	0.755725	0.002440	0.291436
-11.642942	-1.881639	0.760730	0.002410	0.291398
-11.834193	-1.905289	0.765734	0.002446	0.291108
-11.671750	-1.933784	0.770739	0.002416	0.291114
-11.369358	-2.036336	0.775744	0.002359	0.290877
-12.338845	-1.878201	0.780749	0.002540	0.290787
-11.791494	-1.993120	0.785754	0.002438	0.290711
-11.570563	-2.074237	0.790758	0.002397	0.290507
-12.015404	-1.990211	0.795763	0.002479	0.290523
-12.714908	-1.929991	0.800768	0.002610	0.290190
-12.482957	-1.972714	0.805773	0.002566	0.290187
-12.531471	-2.000887	0.810778	0.002575	0.290003
-13.207832	-1.907813	0.815782	0.002701	0.289854
-12.981635	-1.951335	0.820787	0.002659	0.289842
-13.180816	-1.975708	0.825792	0.002696	0.289539
-13.193821	-1.976649	0.830797	0.002699	0.289523
-13.003343	-2.048775	0.835802	0.002663	0.289336
-13.464741	-1.983704	0.840806	0.002749	0.289242
-13.692133	-1.956809	0.845811	0.002791	0.289170
-13.765230	-1.997468	0.850816	0.002805	0.288900
-13.817304	-1.986972	0.855821	0.002814	0.288905
-13.915674	-2.018663	0.860826	0.002833	0.288657
-14.796899	-1.869771	0.865830	0.002997	0.288601
-14.531927	-1.932276	0.870835	0.002947	0.288529
-14.607869	-1.968317	0.875840	0.002961	0.288279
-14.451269	-1.998277	0.880845	0.002932	0.288272
-14.137110	-2.101992	0.885850	0.002874	0.288038
-14.689457	-2.014069	0.890854	0.002977	0.287975
-14.604338	-2.057785	0.895859	0.002961	0.287834
-15.570418	-1.918434	0.900864	0.003140	0.287651
-15.829640	-1.867693	0.905869	0.003189	0.287670
-15.610672	-1.958391	0.910874	0.003148	0.287414
-15.770164	-1.946543	0.915878	0.003178	0.287328
-15.961136	-1.920957	0.920883	0.003213	0.287282
-15.890650	-1.988369	0.925888	0.003200	0.287007
-15.612555	-2.040988	0.930893	0.003148	0.286997
-15.978554	-2.012645	0.935898	0.003216	0.286804
-16.480861	-1.938327	0.940902	0.003310	0.286719
-16.074643	-2.026446	0.945907	0.003234	0.286647
-16.824441	-1.940080	0.950912	0.003374	0.286395
-17.011752	-1.905041	0.955917	0.003408	0.286400
-16.582227	-2.018632	0.960922	0.003328	0.286221
-17.282651	-1.920070	0.965926	0.003459	0.286075
-16.757918	-2.015850	0.970931	0.003361	0.286073
-16.864958	-2.059298	0.975936	0.003381	0.285755
-17.631468	-1.917538	0.980941	0.003524	0.285768
-17.477175	-1.965753	0.985946	0.003495	0.285666
-17.842911	-1.928609	0.990950	0.003563	0.285517
-17.221050	-2.042317	0.995955	0.003447	0.285514
-17.668787	-2.023615	1.000960	0.003530	0.285196
-17.843732	-1.999836	1.005965	0.003563	0.285156
-17.778774	-2.033695	1.010970	0.003551	0.285044
-18.479538	-1.944814	1.015974	0.003681	0.284848
-17.975469	-2.036731	1.020979	0.003587	0.284847
-18.441160	-2.008275	1.025984	0.003674	0.284562
-19.060559	-1.902344	1.030989	0.003789	0.284528
-19.141214	-1.894326	1.035994	0.003804	0.284494
-19.107199	-1.951509	1.040998	0.003798	0.284235
-19.259734	-1.919458	1.046003	0.003826	0.284257
-19.959874	-1.816050	1.051008	0.003956	0.284136
-19.950364	-1.861392	1.056013	0.003955	0.283914
-19.184977	-2.002785	1.061018	0.003812	0.283903
-19.478450	-1.990359	1.066022	0.003867	0.283694
-19.710178	-1.968817	1.071027	0.003910	0.283589
-19.360490	-2.039968	1.076032	0.003845	0.283551
-19.880465	-2.000172	1.081037	0.003941	0.283271
-20.784375	-1.831285	1.086042	0.004110	0.283295
-20.826313	-1.840743	1.091046	0.004117	0.283208
-20.493609	-1.943445	1.096051	0.004055	0.282992
-20.322399	-1.976592	1.101056	0.004024	0.282982
-20.656201	-1.955639	1.106061	0.004086	0.282779
-20.774223	-1.960201	1.111066	0.004108	0.282646
-20.941789	-1.929993	1.116070	0.004139	0.282645
-20.639236	-2.045162	1.121075	0.004082	0.282337
-21.106812	-1.962765	1.126080	0.004169	0.282323
-20.981091	-2.013897	1.131085	0.004146	0.282179
-21.894456	-1.879742	1.136090	0.004316	0.282015
-21.546164	-1.945001	1.141094	0.004251	0.282005
-21.374475	-2.016019	1.146099	0.004219	0.281801
-21.743989	-1.967640	1.151104	0.004288	0.281705
-21.433954	-2.034674	1.156109	0.004230	0.281650
-21.679918	-2.043931	1.161114	0.004276	0.281373
-21.757168	-2.031964	1.166118	0.004290	0.281362
-22.163845	-1.994553	1.171123	0.004366	0.281175
-22.375789	-1.978248	1.176128	0.004405	0.281060
-22.170491	-2.018362	1.181133	0.004367	0.281046
-22.685933	-1.982155	1.186138	0.004463	0.280750
-23.734800	-1.786783	1.191142	0.004658	0.280774
-23.328263	-1.866928	1.196147	0.004582	0.280742
-23.169102	-1.940133	1.201152	0.004553	0.280514
-23.013323	-1.969434	1.206157	0.004524	0.280509
-23.415205	-1.923275	1.211162	0.004598	0.280371
-23.752672	-1.899329	1.216166	0.004661	0.280178
-22.904299	-2.056339	1.221171	0.004503	0.280164
-23.616051	-1.977493	1.226176	0.004636	0.279902
-23.396305	-2.028511	1.231181	0.004595	0.279845
-23.627039	-2.005021	1.236186	0.004638	0.279750
-23.937849	-1.994105	1.241190	0.004696	0.279514
-23.448565	-2.081737	1.246195	0.004604	0.279521
-24.029502	-2.021492	1.251200	0.004713	0.279286
-24.694851	-1.910596	1.256205	0.004836	0.279234
-23.818436	-2.085592	1.261210	0.004673	0.279154
-23.980029	-2.109790	1.266214	0.004703	0.278876
-24.299428	-2.049562	1.271219	0.004763	0.278887
-24.966494	-1.975686	1.276224	0.004887	0.278641
-24.628042	-2.049721	1.281229	0.004824	0.278576
-24.934025	-2.006914	1.286234	0.004881	0.278510
-25.649221	-1.922890	1.291238	0.005014	0.278271
-25.237201	-1.995738	1.296243	0.004937	0.278282
-25.462932	-1.988779	1.301248	0.004979	0.278105
-26.160530	-1.883533	1.306253	0.005109	0.277992
-25.518469	-2.001550	1.311258	0.004989	0.277986
-25.872137	-1.995166	1.316262	0.005055	0.277684
-26.135635	-1.953670	1.321267	0.005104	0.277651
-26.076628	-1.978859	1.326272	0.005093	0.277576
-26.373664	-1.969961	1.331277	0.005148	0.277341
-26.439915	-1.958475	1.336282	0.005161	0.277338
-27.275080	-1.836930	1.341286	0.005316	0.277180
-27.108913	-1.896257	1.346291	0.005285	0.277028
-27.171055	-1.883632	1.351296	0.005297	0.277035
-27.605797	-1.837133	1.356301	0.005377	0.276865
-27.907650	-1.804832	1.361306	0.005434	0.276747
-27.510848	-1.878867	1.366310	0.005360	0.276738
-27.891603	-1.843182	1.371315	0.005431	0.276562
-27.976655	-1.860522	1.376320	0.005446	0.276391
-27.713105	-1.907954	1.381325	0.005397	0.276394
-27.592109	-1.971689	1.386330	0.005375	0.276175
-28.336671	-1.854431	1.391334	0.005513	0.276080
-27.579993	-1.996402	1.396339	0.005372	0.276058
-27.791442	-2.014652	1.401344	0.005412	0.275760
-28.851958	-1.818277	1.406349	0.005609	0.275779
-28.526356	-1.892403	1.411354	0.005548	0.275701
-28.819810	-1.872169	1.416358	0.005603	0.275527
-28.717562	-1.889850	1.421363	0.005584	0.275532
-29.020964	-1.868046	1.426368	0.005640	0.275357
-29.193280	-1.869225	1.431373	0.005672	0.275186
-29.155626	-1.871671	1.436378	0.005665	0.275209
-29.400771	-1.871826	1.441382	0.005711	0.274974
-29.366411	-1.898568	1.446387	0.005705	0.274866
-29.138170	-1.940406	1.451392	0.005662	0.274865
-29.635587	-1.908083	1.456397	0.005755	0.274559
-29.530092	-1.931003	1.461402	0.005735	0.274539
-29.496404	-1.953105	1.466406	0.005729	0.274455
-28.859742	-2.111493	1.471411	0.005610	0.274231
-29.810854	-1.935584	1.476416	0.005787	0.274246
-29.862331	-1.979660	1.481421	0.005797	0.273964
-30.224094	-1.921007	1.486426	0.005864	0.273927
-30.809101	-1.822714	1.491430	0.005973	0.273884
-31.333617	-1.774550	1.496435	0.006070	0.273635
-30.858813	-1.864046	1.501440	0.005982	0.273618
-30.742662	-1.900239	1.506445	0.005960	0.273539
-31.352480	-1.833290	1.511450	0.006074	0.273306
-31.680570	-1.773145	1.516454	0.006135	0.273309
-31.596122	-1.802852	1.521459	0.006119	0.273233
-32.164559	-1.738165	1.526464	0.006225	0.273028
-31.860972	-1.794813	1.531469	0.006168	0.273021
-31.610106	-1.857783	1.536474	0.006122	0.272929
-32.258543	-1.788432	1.541478	0.006242	0.272672
-32.213089	-1.792456	1.546483	0.006234	0.272694
-31.575755	-1.938882	1.551488	0.006115	0.272532
-31.964996	-1.903817	1.556493	0.006187	0.272343
-32.293702	-1.839717	1.561498	0.006249	0.272366
-32.590382	-1.831538	1.566502	0.006304	0.272123
-32.363958	-1.889373	1.571507	0.006262	0.272034
-32.798480	-1.810491	1.576512	0.006342	0.272034
-33.043978	-1.816358	1.581517	0.006388	0.271765
-32.740317	-1.875274	1.586522	0.006332	0.271746
-33.111106	-1.820206	1.591526	0.006401	0.271680
-33.840028	-1.734731	1.596531	0.006536	0.271429
-33.319070	-1.833544	1.601536	0.006439	0.271407
-32.945942	-1.921245	1.606541	0.006370	0.271302
-33.264674	-1.901984	1.611546	0.006429	0.271095
-33.494105	-1.861446	1.616550	0.006472	0.271089
-33.808696	-1.837041	1.621555	0.006530	0.270914
-33.433898	-1.934145	1.626560	0.006460	0.270760
-33.227048	-1.975733	1.631565	0.006422	0.270739
-33.285815	-2.006655	1.636570	0.006433	0.270516
-33.508902	-1.969021	1.641574	0.006474	0.270501
-33.689662	-1.975667	1.646579	0.006508	0.270289
-33.692343	-1.999547	1.651584	0.006508	0.270159
-33.779105	-1.998245	1.656589	0.006524	0.270082
-34.391407	-1.928956	1.661594	0.006638	0.269856
-34.702958	-1.871054	1.666598	0.006696	0.269863
-34.571094	-1.935443	1.671603	0.006672	0.269646
-35.286826	-1.825165	1.676608	0.006805	0.269540
-35.567645	-1.773288	1.681613	0.006857	0.269544
-35.271222	-1.873587	1.686618	0.006802	0.269295
-35.993938	-1.747591	1.691622	0.006936	0.269266
-35.925058	-1.760585	1.696627	0.006924	0.269264
-35.474715	-1.908856	1.701632	0.006840	0.268907
-35.412168	-1.919745	1.706637	0.006828	0.268910
-35.218777	-1.982356	1.711642	0.006792	0.268762
-35.772915	-1.914214	1.716646	0.006895	0.268587
-35.219854	-2.015968	1.721651	0.006792	0.268580
-35.818234	-1.966348	1.726656	0.006904	0.268261
-36.175260	-1.900816	1.731661	0.006970	0.268265
-36.041714	-1.949831	1.736666	0.006945	0.268131
-36.599511	-1.876569	1.741670	0.007049	0.267979
-35.712708	-2.040560	1.746675	0.006884	0.267965
-36.413082	-1.975089	1.751680	0.007014	0.267630
-36.052430	-2.042341	1.756685	0.006947	0.267622
-36.241927	-2.045132	1.761690	0.006982	0.267420
-36.735038	-1.976522	1.766694	0.007074	0.267306
-36.595665	-2.015329	1.771699	0.007048	0.267234
-37.127979	-1.962399	1.776704	0.007147	0.266996
-37.133228	-1.962054	1.781709	0.007148	0.266993
-36.896000	-2.045185	1.786714	0.007104	0.266776
-37.583977	-1.930657	1.791718	0.007232	0.266719
-37.630729	-1.941785	1.796723	0.007240	0.266612
-37.966743	-1.925155	1.801728	0.007303	0.266371
-37.763561	-1.961265	1.806733	0.007265	0.266376
-37.577027	-2.040731	1.811738	0.007230	0.266128
-37.970182	-1.983988	1.816742	0.007303	0.266048
-37.829622	-2.030837	1.821747	0.007277	0.265932
-38.306540	-1.977746	1.826752	0.007366	0.265749
-38.570100	-1.930055	1.831757	0.007415	0.265748
-38.676311	-1.951989	1.836762	0.007435	0.265524
-38.689001	-1.956670	1.841766	0.007437	0.265486
-38.547362	-2.010742	1.846771	0.007411	0.265331
-38.731337	-2.013639	1.851776	0.007445	0.265133
-38.702890	-2.020256	1.856781	0.007440	0.265125
-39.054963	-2.011253	1.861786	0.007505	0.264825
-39.419943	-1.946399	1.866790	0.007573	0.264817
-38.942156	-2.067030	1.871795	0.007484	0.264632
-39.094298	-2.066938	1.876800	0.007512	0.264482
-39.616719	-1.982825	1.881805	0.007609	0.264422
-39.550588	-2.033754	1.886810	0.007597	0.264209
-39.271169	-2.086510	1.891814	0.007545	0.264199
-39.635823	-2.074117	1.896819	0.007613	0.263903
-39.996402	-2.016714	1.901824	0.007680	0.263859
-39.900448	-2.064665	1.906829	0.007662	0.263691
-39.802040	-2.108118	1.911834	0.007644	0.263551
-40.131688	-2.061413	1.916838	0.007705	0.263479
-40.609905	-2.018829	1.921843	0.007794	0.263235
-40.530289	-2.033929	1.926848	0.007779	0.263232
-40.940455	-2.000995	1.931853	0.007856	0.263002
-40.765451	-2.042155	1.936858	0.007823	0.262951
-41.038226	-2.016967	1.941862	0.007874	0.262817
-41.316286	-2.003044	1.946867	0.007925	0.262615
-41.430154	-1.983491	1.951872	0.007947	0.262609
-41.237940	-2.070927	1.956877	0.007911	0.262320
-41.325136	-2.059585	1.961882	0.007927	0.262295
-41.864151	-1.993435	1.966886	0.008027	0.262119
-41.599012	-2.070084	1.971891	0.007978	0.261962
-41.728796	-2.052404	1.976896	0.008002	0.261929
-42.765317	-1.907567	1.981901	0.008195	0.261688
-42.489452	-1.957260	1.986906	0.008143	0.261691
-42.298278	-2.024551	1.991910	0.008108	0.261511
-42.414771	-2.031569	1.996915	0.008130	0.261355
-42.682728	-2.013959	2.001920	0.008179	0.261183

-42.972815	-1.994185	2.011917	0.008233	0.261000
-43.202372	-2.002169	2.021914	0.008276	0.260724
-43.487407	-1.973733	2.031910	0.008329	0.260595
-43.470766	-1.996544	2.041907	0.008326	0.260485
-43.795156	-1.973442	2.051904	0.008386	0.260286
-43.728080	-2.012427	2.061901	0.008373	0.260137
-43.800459	-2.011203	2.071898	0.008387	0.260071
-44.528588	-1.921265	2.081894	0.008522	0.259835
-44.236131	-1.975279	2.091891	0.008468	0.259831
-44.119387	-1.999479	2.101888	0.008446	0.259815
-44.050954	-2.043121	2.111885	0.008433	0.259641
-44.881127	-1.915997	2.121882	0.008588	0.259508
-44.804514	-1.930327	2.131878	0.008573	0.259507
-44.738846	-1.942483	2.141875	0.008561	0.259506
-45.086441	-1.878203	2.151872	0.008626	0.259512
-44.855928	-1.920055	2.161869	0.008583	0.259513
-44.821320	-1.926358	2.171866	0.008576	0.259514
-44.595059	-1.969032	2.181862	0.008534	0.259506
-44.356925	-2.005251	2.191859	0.008489	0.259546
-44.189446	-1.986182	2.201856	0.008458	0.259822
-43.932805	-2.032776	2.211853	0.008410	0.259823
-44.239475	-1.975296	2.221850	0.008467	0.259833
-44.061185	-2.009764	2.231846	0.008434	0.259822
-43.933188	-2.034791	2.241843	0.008410	0.259813
-44.313111	-1.963977	2.251840	0.008481	0.259823
-43.846624	-2.002181	2.261837	0.008394	0.260084
-43.752059	-2.009857	2.271834	0.008376	0.260137
-43.784382	-2.003808	2.281830	0.008382	0.260138
-43.869578	-1.973634	2.291827	0.008398	0.260221
-43.505618	-1.993324	2.301824	0.008330	0.260480
-43.394961	-2.012794	2.311821	0.008309	0.260484
-43.604383	-1.959727	2.321818	0.008348	0.260568
-43.526746	-1.943143	2.331814	0.008334	0.260739
-43.466213	-1.954834	2.341811	0.008322	0.260736
-43.164507	-1.952982	2.351808	0.008266	0.261051
-42.973656	-1.989161	2.361805	0.008230	0.261043
-42.882372	-1.960744	2.371802	0.008213	0.261293
-43.010921	-1.924487	2.381798	0.008237	0.261365
-42.673780	-1.937531	2.391795	0.008174	0.261633
-42.865377	-1.890165	2.401792	0.008210	0.261703
-42.478651	-1.911897	2.411789	0.008138	0.261972
-42.658731	-1.863974	2.421786	0.008171	0.262057
-42.199567	-1.900243	2.431782	0.008086	0.262318
-42.541279	-1.804135	2.441779	0.008149	0.262506
-42.084265	-1.864150	2.451776	0.008064	0.262634
-42.006073	-1.817110	2.461773	0.008049	0.262972
-42.034073	-1.786210	2.471770	0.008054	0.263114
-41.914129	-1.773847	2.481766	0.008032	0.263303
-41.515689	-1.793131	2.491763	0.007958	0.263596
-41.197792	-1.817450	2.501760	0.007898	0.263780
-40.635996	-1.896883	2.511757	0.007794	0.263906
-40.395000	-1.880498	2.521754	0.007749	0.264237
-40.303859	-1.871858	2.531750	0.007732	0.264375
-40.292609	-1.847552	2.541747	0.007730	0.264520
-40.044257	-1.833354	2.551744	0.007683	0.264845
-39.838109	-1.837802	2.561741	0.007645	0.265026
-39.733511	-1.822611	2.571738	0.007625	0.265214
-39.436577	-1.819847	2.581734	0.007570	0.265524
-39.262340	-1.818617	2.591731	0.007537	0.265704
-38.575788	-1.919706	2.601728	0.007409	0.265834
-38.273141	-1.932016	2.611725	0.007353	0.266067
-38.018283	-1.935897	2.621722	0.007305	0.266299
-38.089860	-1.889249	2.631718	0.007319	0.266482
-37.746759	-1.908722	2.641715	0.007255	0.266716
-37.692643	-1.874206	2.651712	0.007245	0.266957
-37.535691	-1.869608	2.661709	0.007215	0.267137
-36.998645	-1.932012	2.671706	0.007115	0.267329
-36.626800	-1.944169	2.681702	0.007046	0.267630
-36.678902	-1.900569	2.691699	0.007055	0.267815
-36.293564	-1.936973	2.701696	0.006984	0.267997
-36.105039	-1.923087	2.711693	0.006948	0.268258
-35.561065	-1.985325	2.721690	0.006847	0.268456
-35.599150	-1.945259	2.731686	0.006854	0.268635
-35.379128	-1.936895	2.741683	0.006813	0.268896
-35.128579	-1.935910	2.751680	0.006766	0.269147
-35.317452	-1.867769	2.761677	0.006801	0.269330
-34.857387	-1.914086	2.771674	0.006716	0.269531
-34.839968	-1.854438	2.781670	0.006712	0.269869
-34.050045	-1.963237	2.791667	0.006565	0.270056
-33.797785	-1.976979	2.801664	0.006518	0.270229
-33.943866	-1.897900	2.811661	0.006545	0.270510
-33.811177	-1.879083	2.821658	0.006520	0.270741
-33.783024	-1.843582	2.831654	0.006515	0.270958
-33.064026	-1.938224	2.841651	0.006381	0.271152
-33.098679	-1.887517	2.851648	0.006387	0.271389
-32.666690	-1.910230	2.861645	0.006307	0.271687
-32.428860	-1.916476	2.871642	0.006263	0.271885
-32.370411	-1.887307	2.881638	0.006252	0.272097
-31.640524	-1.975982	2.891635	0.006116	0.272332
-31.717723	-1.912046	2.901632	0.006130	0.272598
-31.570822	-1.897043	2.911629	0.006102	0.272820
-31.174584	-1.926098	2.921626	0.006029	0.273048
-30.826885	-1.946646	2.931622	0.005964	0.273275
-30.543227	-1.950611	2.941619	0.005911	0.273528
-30.871363	-1.848204	2.951616	0.005972	0.273754
-30.806137	-1.812944	2.961613	0.005960	0.274004
-30.100094	-1.894420	2.971610	0.005828	0.274252
-29.846410	-1.887885	2.981606	0.005781	0.274530
-29.155909	-1.974072	2.991603	0.005652	0.274738
-29.313791	-1.906375	3.001600	0.005681	0.274944
-28.782022	-1.960823	3.011597	0.005582	0.275167
-28.817664	-1.893027	3.021594	0.005589	0.275490
-28.688362	-1.881503	3.031590	0.005565	0.275675
-28.480618	-1.881927	3.041587	0.005526	0.275871
-27.934865	-1.942782	3.051584	0.005424	0.276073
-27.798064	-1.907928	3.061581	0.005399	0.276386
-27.514250	-1.915211	3.071578	0.005346	0.276619
-27.190972	-1.937923	3.081574	0.005285	0.276808
-26.901268	-1.951887	3.091571	0.005231	0.277011
-26.866217	-1.898442	3.101568	0.005225	0.277324
-26.275334	-1.968126	3.111565	0.005115	0.277521
-25.927105	-1.994037	3.121562	0.005050	0.277717
-25.193941	-2.081122	3.131558	0.004913	0.277958
-25.225279	-2.032560	3.141555	0.004919	0.278182
-25.312101	-1.982816	3.151552	0.004935	0.278359
-24.961753	-2.005053	3.161549	0.004870	0.278575
-25.151153	-1.911054	3.171546	0.004905	0.278885
-24.636478	-1.961503	3.181542	0.004809	0.279109
-24.442345	-1.956332	3.191539	0.004773	0.279319
-24.043718	-1.992521	3.201536	0.004698	0.279508
-23.559878	-2.020940	3.211533	0.004608	0.279816
-23.633015	-1.971772	3.221530	0.004622	0.280002
-23.110726	-2.030624	3.231526	0.004525	0.280190
-22.655743	-2.056476	3.241523	0.004440	0.280484
-22.555553	-2.044783	3.251520	0.004421	0.280638
-22.188914	-2.084295	3.261517	0.004353	0.280779
-22.019851	-2.065502	3.271514	0.004321	0.281035
-21.691324	-2.080502	3.281510	0.004260	0.281265
-21.581072	-2.065593	3.291507	0.004239	0.281446
-21.292251	-2.073614	3.301504	0.004185	0.281675
-20.864529	-2.102566	3.311501	0.004106	0.281926
-20.891653	-2.065269	3.321498	0.004111	0.282093
-20.250451	-2.145061	3.331494	0.003991	0.282282
-20.161232	-2.103644	3.341491	0.003974	0.282578
-20.045944	-2.090275	3.351488	0.003953	0.282754
-19.788709	-2.099760	3.361485	0.003905	0.282945
-19.694798	-2.061694	3.371482	0.003887	0.283227
-19.351296	-2.084034	3.381478	0.003823	0.283433
-19.436348	-2.028784	3.391475	0.003839	0.283636
-18.937671	-2.075520	3.401472	0.003746	0.283861
-18.675852	-2.066021	3.411469	0.003697	0.284152
-18.645482	-2.035554	3.421466	0.003691	0.284336
-18.082211	-2.104216	3.431462	0.003587	0.284508
-18.042196	-2.051526	3.441459	0.003579	0.284813
-17.657967	-2.079241	3.451456	0.003507	0.285028
-17.671472	-2.035853	3.461453	0.003510	0.285236
-17.444571	-2.028123	3.471450	0.003467	0.285485
-16.766430	-2.105523	3.481446	0.003341	0.285718
-16.765572	-2.069046	3.491443	0.003341	0.285904
-16.693231	-2.042200	3.501440	0.003327	0.286107
-16.345209	-2.056675	3.511437	0.003262	0.286354
-16.065951	-2.052260	3.521434	0.003210	0.286633
-15.744327	-2.073628	3.531430	0.003150	0.286821
-15.732624	-2.037271	3.541427	0.003148	0.287015
-15.229371	-2.073541	3.551424	0.003054	0.287294
-14.952516	-2.076758	3.561421	0.003003	0.287532
-14.858969	-2.053945	3.571418	0.002985	0.287733
-14.222225	-2.126713	3.581414	0.002867	0.287949
-14.125116	-2.090000	3.591411	0.002848	0.288223
-13.702831	-2.130695	3.601408	0.002770	0.288404
-13.777906	-2.079571	3.611405	0.002784	0.288593
-13.500639	-2.075054	3.621402	0.002732	0.288868
-13.135567	-2.090240	3.631398	0.002664	0.289125
-13.151614	-2.047639	3.641395	0.002667	0.289324
-12.769029	-2.081507	3.651392	0.002595	0.289503
-13.120064	-1.950505	3.661389	0.002661	0.289839
-12.617374	-1.994606	3.671386	0.002567	0.290075
-12.518766	-1.964584	3.681382	0.002548	0.290315
-11.806167	-2.053051	3.691379	0.002416	0.290520
-11.533235	-2.059640	3.701376	0.002365	0.290735
-11.292866	-2.054143	3.711373	0.002320	0.290980
-10.935747	-2.081985	3.721370	0.002253	0.291165
-11.131210	-2.001819	3.731366	0.002290	0.291387
-11.032847	-1.954247	3.741363	0.002271	0.291712
-10.564089	-1.994149	3.751360	0.002184	0.291937
-10.061139	-2.046001	3.761357	0.002090	0.292134
-9.967255	-2.019162	3.771354	0.002073	0.292352
-9.981105	-1.958588	3.781350	0.002075	0.292639
-9.189124	-2.045516	3.791347	0.001928	0.292921
-9.104256	-2.024552	3.801344	0.001912	0.293102
-8.732988	-2.056159	3.811341	0.001842	0.293279
-8.483071	-2.042253	3.821338	0.001796	0.293572
-8.537276	-1.985461	3.831334	0.001806	0.293804
-8.066591	-2.026957	3.841331	0.001718	0.294021
-8.126131	-1.968153	3.851328	0.001729	0.294258
-7.603201	-2.011521	3.861325	0.001632	0.294512
-7.466554	-1.987190	3.871322	0.001606	0.294754
-7.095280	-2.012167	3.881318	0.001537	0.294963
-6.922813	-2.000990	3.891315	0.001505	0.295172
-6.958163	-1.929217	3.901312	0.001511	0.295493
-6.926640	-1.892589	3.911309	0.001505	0.295700
-6.139347	-1.992833	3.921306	0.001359	0.295910
-6.534430	-1.874640	3.931302	0.001432	0.296137
-5.694697	-1.979188	3.941299	0.001276	0.296373
-6.033812	-1.853348	3.951296	0.001339	0.296686
-5.068324	-1.982339	3.961293	0.001159	0.296913
-5.478405	-1.864224	3.971290	0.001235	0.297126
-4.962451	-1.907126	3.981286	0.001139	0.297374
-4.485350	-1.940832	3.991283	0.001050	0.297632
-5.187124	-1.749467	4.001280	0.001180	0.297943
-4.116226	-1.894304	4.011277	0.000981	0.298185
-4.427287	-1.792356	4.021274	0.001039	0.298406
-3.889962	-1.836962	4.031270	0.000939	0.298663
-3.470892	-1.866252	4.041267	0.000861	0.298891
-3.860362	-1.727180	4.051264	0.000933	0.299221
-3.082978	-1.815386	4.061261	0.000788	0.299478
-3.625680	-1.665463	4.071258	0.000889	0.299727
-2.845047	-1.747014	4.081254	0.000744	0.300018
-3.390197	-1.589231	4.091251	0.000845	0.300301
-3.152148	-1.574774	4.101248	0.000800	0.300580
-3.016651	-1.548589	4.111245	0.000775	0.300825
-2.679828	-1.545930	4.121242	0.000712	0.301132
-1.951003	-1.622403	4.131238	0.000577	0.301401
-3.068756	-1.344626	4.141235	0.000784	0.301760
-1.871743	-1.508836	4.151232	0.000562	0.302016
-2.694221	-1.285972	4.161229	0.000715	0.302368
-1.837821	-1.375868	4.171226	0.000555	0.302682
-1.935107	-1.286590	4.181222	0.000573	0.303025
-2.086032	-1.188309	4.191219	0.000601	0.303363
-1.450198	-1.236446	4.201216	0.000483	0.303685
-1.775524	-1.104951	4.211213	0.000543	0.304030
-2.131179	-0.961867	4.221210	0.000609	0.304404
-1.518446	-0.998437	4.231206	0.000495	0.304759
-1.615937	-0.901343	4.241203	0.000513	0.305136
-1.167573	-0.896541	4.251200	0.000429	0.305545
-1.340135	-0.795197	4.261197	0.000461	0.305877
-0.793266	-0.820580	4.271194	0.000359	0.306227
-0.633879	-0.767033	4.281190	0.000330	0.306617
-1.469320	-0.528163	4.291187	0.000485	0.307028
-0.951098	-0.531563	4.301184	0.000388	0.307456
-1.201588	-0.398393	4.311181	0.000435	0.307869
-0.971286	-0.346975	4.321178	0.000392	0.308307
-0.931201	-0.259930	4.331174	0.000384	0.308750
-0.680973	-0.213981	4.341171	0.000337	0.309178
-0.681412	-0.113891	4.351168	0.000337	0.309646
-0.459847	-0.066579	4.361165	0.000296	0.310055
-0.548159	0.061235	4.371162	0.000312	0.310577
0.000000	0.037214	4.381158	0.000210	0.310929

0.093925	0.297845	4.386163	0.000192	0.312219
0.181679	0.852507	4.391168	0.000176	0.314852
0.304244	1.685912	4.396173	0.000152	0.318760
0.569435	2.777159	4.401178	0.000102	0.323890
1.040020	4.132416	4.406182	0.000014	0.330263
1.015209	5.867178	4.411187	0.000017	0.337758
1.539228	7.801762	4.416192	-0.000082	0.346343
2.174030	10.031009	4.421197	-0.000202	0.356001
2.686178	12.582274	4.426202	-0.000299	0.366589
3.649085	15.385014	4.431206	-0.000480	0.378157
4.426924	18.548139	4.436211	-0.000627	0.390592
5.386973	22.015988	4.441216	-0.000808	0.403855
5.883263	25.918508	4.446221	-0.000903	0.417911
6.335190	30.175669	4.451226	-0.000990	0.432669
7.670868	34.615584	4.456230	-0.001241	0.448048
8.695605	39.468723	4.461235	-0.001435	0.464029
9.788335	44.663789	4.466240	-0.001642	0.480544
10.685353	50.241745	4.471245	-0.001813	0.497521
12.889326	55.938111	4.476250	-0.002227	0.514932
14.078423	62.157987	4.481254	-0.002453	0.532698
14.684980	68.804381	4.486259	-0.002570	0.550734
15.627552	75.706896	4.491264	-0.002750	0.569003
16.411269	82.942715	4.496269	-0.002901	0.587452
17.289319	90.437010	4.501274	-0.003069	0.605997
18.245191	98.197268	4.506278	-0.003252	0.624639
18.657815	106.295906	4.511283	-0.003334	0.643281
19.673124	114.524030	4.516288	-0.003529	0.661916
20.328263	123.018284	4.521293	-0.003656	0.680469
21.301786	131.644804	4.526298	-0.003843	0.698920
22.437062	140.425358	4.531302	-0.004060	0.717265
22.991095	149.456997	4.536307	-0.004170	0.735440
24.111298	158.539487	4.541312	-0.004384	0.753468
25.160097	167.730820	4.546317	-0.004585	0.771254
25.859486	177.094993	4.551322	-0.004722	0.788841
26.693928	186.524329	4.556326	-0.004883	0.806203
27.500790	196.015513	4.561331	-0.005040	0.823299
28.392847	205.554160	4.566336	-0.005212	0.840154
29.720919	215.032011	4.571341	-0.005466	0.856704
30.879668	224.574554	4.576346	-0.005688	0.872996
31.657573	234.198909	4.581350	-0.005839	0.889014
32.587433	243.803429	4.586355	-0.006018	0.904758
33.786138	253.355854	4.591360	-0.006248	0.920224
34.584034	262.961097	4.596365	-0.006403	0.935407
35.302689	272.558346	4.601370	-0.006543	0.950314
36.246980	282.087284	4.606374	-0.006725	0.964946
37.076731	291.605136	4.611379	-0.006886	0.979314
37.846374	301.120067	4.616384	-0.007035	0.993453
38.774094	310.536681	4.621389	-0.007214	1.007292
40.233072	319.816538	4.626394	-0.007492	1.020880
40.973033	329.205627	4.631398	-0.007636	1.034267
41.553308	338.546487	4.636403	-0.007750	1.047377
42.538304	347.789372	4.641408	-0.007939	1.060287
43.298645	357.038811	4.646413	-0.008087	1.072998
43.964300	366.218991	4.651418	-0.008217	1.085445
44.988446	375.324035	4.656422	-0.008414	1.097733
45.309945	384.502611	4.661427	-0.008480	1.109823
46.278276	393.501215	4.666432	-0.008666	1.121693
47.285871	402.466197	4.671437	-0.008859	1.133405
48.403094	411.385846	4.676442	-0.009073	1.144962
49.269161	420.327854	4.681446	-0.009240	1.156378
49.598388	429.283843	4.686451	-0.009307	1.167585
50.207835	438.162504	4.691456	-0.009427	1.178650
50.627594	447.031375	4.696461	-0.009511	1.189560
51.236755	455.817536	4.701466	-0.009630	1.200309
51.816525	464.599202	4.706470	-0.009744	1.210952
51.919287	473.411046	4.711475	-0.009769	1.221442
52.980204	482.025631	4.716480	-0.009972	1.231801
54.117137	490.600340	4.721485	-0.010189	1.242042
54.263252	499.338818	4.726490	-0.010222	1.252195
55.268846	507.895053	4.731494	-0.010415	1.262223
55.442378	516.571782	4.736499	-0.010453	1.272149
56.098069	525.129162	4.741504	-0.010581	1.281955
56.436112	533.746507	4.746509	-0.010649	1.291694
57.239495	542.234872	4.751514	-0.010804	1.301303
57.843335	550.808807	4.756518	-0.010922	1.310899
58.367336	559.337451	4.761523	-0.011026	1.320361
58.972241	567.793881	4.766528	-0.011144	1.329691
59.386235	576.277712	4.771533	-0.011226	1.338951
59.698953	584.757762	4.776538	-0.011290	1.348125
60.184629	593.210621	4.781542	-0.011386	1.357239
60.516973	601.639006	4.786547	-0.011454	1.366239
61.559100	609.963214	4.791552	-0.011653	1.375194
62.599636	618.279931	4.796557	-0.011852	1.384083
63.003706	626.730397	4.801562	-0.011933	1.392944
62.697513	635.257641	4.806566	-0.011882	1.401706
62.744896	643.692231	4.811571	-0.011896	1.410380
63.926153	651.905161	4.816576	-0.012121	1.418965
64.577564	660.229384	4.821581	-0.012248	1.427523
65.131614	668.559838	4.826586	-0.012357	1.436019
65.420262	676.942798	4.831590	-0.012416	1.444474
65.701887	685.316710	4.836595	-0.012474	1.452869
66.396879	693.601663	4.841600	-0.012609	1.461195
67.214475	701.871225	4.846605	-0.012767	1.469478
67.617400	710.205335	4.851610	-0.012847	1.477712
67.962480	718.522329	4.856614	-0.012917	1.485873
68.596436	726.783351	4.861619	-0.013040	1.493982
69.368316	735.033983	4.866624	-0.013189	1.502058
69.529206	743.400604	4.871629	-0.013225	1.510106
69.649150	751.719563	4.876634	-0.013253	1.518059
70.563749	759.909415	4.881638	-0.013428	1.525972
70.914899	768.204432	4.886643	-0.013499	1.533856
71.230394	776.484283	4.891648	-0.013563	1.541680
71.751428	784.739769	4.896653	-0.013666	1.549473
72.119943	793.002350	4.901658	-0.013740	1.557210
72.377195	801.283302	4.906662	-0.013793	1.564909
72.397473	809.597197	4.911667	-0.013802	1.572565
73.047699	817.782900	4.916672	-0.013929	1.580160
73.436428	826.039203	4.921677	-0.014007	1.587744
73.254713	834.357833	4.926682	-0.013978	1.595266
74.109925	842.482892	4.931686	-0.014143	1.602728
74.344219	850.732479	4.936691	-0.014192	1.610177
74.771379	858.957611	4.941696	-0.014277	1.617598
75.338880	867.125814	4.946701	-0.014388	1.624954
75.471757	875.426798	4.951706	-0.014418	1.632332
75.632966	883.657320	4.956710	-0.014454	1.639619
75.708821	891.885818	4.961715	-0.014473	1.646861
76.248015	900.040924	4.966720	-0.014579	1.654070
76.416758	908.265115	4.971725	-0.014616	1.661258
76.559335	916.470705	4.976730	-0.014648	1.668394
77.254807	924.605386	4.981734	-0.014782	1.675515
77.292797	932.832636	4.986739	-0.014795	1.682595
77.534453	941.033631	4.991744	-0.014845	1.689650
77.404455	949.310503	4.996749	-0.014827	1.696691
77.427005	957.514266	5.001754	-0.014836	1.703661
77.798421	965.679715	5.006758	-0.014911	1.710617
78.274391	973.795476	5.011763	-0.015005	1.717516
78.862925	981.908759	5.016768	-0.015119	1.724401
78.883776	990.139281	5.021773	-0.015129	1.731281
78.957878	998.338985	5.026778	-0.015148	1.738116
79.410235	1006.483736	5.031782	-0.015238	1.744927
79.947665	1014.603712	5.036787	-0.015343	1.751702
80.345698	1022.754166	5.041792	-0.015422	1.758458
80.320920	1030.969366	5.046797	-0.015423	1.765187
80.794833	1039.100238	5.051802	-0.015517	1.771885
80.708164	1047.348166	5.056806	-0.015506	1.778582
81.089196	1055.457122	5.061811	-0.015582	1.785200
81.151680	1063.703528	5.066816	-0.015599	1.791864
81.531269	1071.828161	5.071821	-0.015675	1.798446
81.926873	1079.901819	5.076826	-0.015754	1.804965
81.719419	1088.173251	5.081830	-0.015721	1.811543
81.739297	1096.343237	5.086835	-0.015730	1.818044
82.451202	1104.369360	5.091840	-0.015868	1.824494
82.702875	1112.526393	5.096845	-0.015920	1.830967
83.244482	1120.615171	5.101850	-0.016026	1.837400
83.557623	1128.757281	5.106854	-0.016090	1.843823
83.982329	1136.863921	5.111859	-0.016175	1.850211
83.755338	1145.129907	5.116864	-0.016138	1.856622
84.333496	1153.198527	5.121869	-0.016251	1.862954
84.546360	1161.352590	5.126874	-0.016296	1.869287
84.861596	1169.491270	5.131878	-0.016360	1.875598
85.157723	1177.580427	5.136883	-0.016420	1.881849
85.812667	1185.651356	5.141888	-0.016547	1.888106
86.026317	1193.833800	5.146893	-0.016593	1.894376
86.168430	1201.980894	5.151898	-0.016624	1.900591
86.924951	1210.044619	5.156902	-0.016771	1.906792
86.817180	1218.262500	5.161907	-0.016756	1.912991
87.065574	1226.405803	5.166912	-0.016807	1.919154
87.244248	1234.537792	5.171917	-0.016846	1.925281
87.721739	1242.621396	5.176922	-0.016940	1.931386
87.974895	1250.777926	5.181926	-0.016993	1.937501
88.330593	1258.898117	5.186931	-0.017064	1.943581
88.610748	1267.040911	5.191936	-0.017122	1.949650
89.029315	1275.123783	5.196941	-0.017205	1.955671
89.085602	1283.263732	5.201946	-0.017221	1.961676
89.554397	1291.348653	5.206950	-0.017314	1.967667
89.946703	1299.434680	5.211955	-0.017392	1.973633
89.661766	1307.661536	5.216960	-0.017344	1.979609
90.386494	1315.658269	5.221965	-0.017484	1.985510
90.973173	1323.732786	5.226970	-0.017599	1.991434
90.958581	1331.921144	5.231974	-0.017602	1.997358
91.088498	1340.034942	5.236979	-0.017631	2.003227
91.376772	1348.156052	5.241984	-0.017690	2.009100
91.685954	1356.254059	5.246989	-0.017753	2.014942
91.341304	1364.458898	5.251994	-0.017694	2.020774
92.033499	1372.480230	5.256998	-0.017828	2.026568
91.722023	1380.697856	5.262003	-0.017776	2.032379
92.038660	1388.771184	5.267008	-0.017840	2.038137
93.252827	1396.679406	5.272013	-0.018071	2.043856
93.697476	1404.773004	5.277018	-0.018159	2.049610
94.088678	1412.897372	5.282022	-0.018238	2.055363
93.938559	1421.086760	5.287027	-0.018215	2.061089
94.370326	1429.170901	5.292032	-0.018301	2.066786
94.839802	1437.248421	5.297037	-0.018394	2.072467
95.058845	1445.360446	5.302042	-0.018440	2.078130
95.699547	1453.415542	5.307046	-0.018564	2.083781
95.207902	1461.651189	5.312051	-0.018478	2.089427
95.433705	1469.764889	5.317056	-0.018525	2.095047
95.682247	1477.865899	5.322061	-0.018577	2.100644
96.263799	1485.889481	5.327066	-0.018691	2.106207
96.559825	1494.044985	5.332070	-0.018751	2.111817
97.145583	1502.058768	5.337075	-0.018865	2.117344
97.421686	1510.135148	5.342080	-0.018922	2.122868
97.489047	1518.269907	5.347085	-0.018940	2.128397
98.096214	1526.316037	5.352090	-0.019058	2.133905
98.695827	1534.356986	5.357094	-0.019175	2.139393
98.507455	1542.530517	5.362099	-0.019146	2.144881
98.877524	1550.641007	5.367104	-0.019220	2.150366
99.162174	1558.719478	5.372109	-0.019278	2.155808
99.436165	1566.772660	5.377114	-0.019334	2.161218
99.852386	1574.856095	5.382118	-0.019417	2.166647
99.730488	1583.021407	5.387123	-0.019400	2.172067
100.218886	1591.063280	5.392128	-0.019496	2.177449
100.627307	1599.127871	5.397133	-0.019578	2.182825
100.974247	1607.225925	5.402138	-0.019647	2.188204
101.539917	1615.292165	5.407142	-0.019758	2.193569
101.502581	1623.423615	5.412147	-0.019756	2.198908
101.870217	1631.463916	5.417152	-0.019830	2.204212
102.398142	1639.535811	5.422157	-0.019934	2.209538
102.268909	1647.706465	5.427162	-0.019915	2.214855
103.193494	1655.657405	5.432166	-0.020092	2.220113
103.458730	1663.749361	5.437171	-0.020147	2.225390
103.681600	1671.883356	5.442176	-0.020194	2.230678
104.054259	1679.948250	5.447181	-0.020269	2.235922
103.989202	1688.067457	5.452186	-0.020262	2.241149
104.108431	1696.184824	5.457190	-0.020289	2.246379
103.876684	1704.346288	5.462195	-0.020252	2.251594
104.477225	1712.348733	5.467200	-0.020369	2.256770
104.855237	1720.395957	5.472205	-0.020444	2.261942
105.200763	1728.467890	5.477210	-0.020514	2.267115
105.817620	1736.535453	5.482214	-0.020634	2.272298
105.722969	1744.672377	5.487219	-0.020622	2.277450
106.246109	1752.674131	5.492224	-0.020725	2.282559
106.101222	1760.807708	5.497229	-0.020703	2.287681
106.549631	1768.835764	5.502234	-0.020792	2.292778
106.649805	1776.963027	5.507238	-0.020816	2.297894
107.392782	1784.903024	5.512243	-0.020959	2.302938
107.627260	1793.021544	5.517248	-0.021008	2.308038
107.609955	1801.178633	5.522253	-0.021010	2.313130
107.705931	1809.249556	5.527258	-0.021034	2.318166
108.198754	1817.249131	5.532262	-0.021131	2.323181
108.190835	1825.372348	5.537267	-0.021134	2.328219
108.565176	1833.432001	5.542272	-0.021209	2.333239
108.529196	1841.561636	5.547277	-0.021208	2.338257
109.053781	1849.543374	5.552282	-0.021311	2.343220
109.072400	1857.696824	5.557286	-0.021320	2.348236
109.656306	1865.710240	5.562291	-0.021434	2.353202
109.879314	1873.788056	5.567296	-0.021481	2.358167
110.217946	1881.836407	5.572301	-0.021549	2.363113
110.428709	1889.909728	5.577306	-0.021594	2.368054
110.543311	1898.041082	5.582310	-0.021620	2.373011
110.737700	1906.084295	5.587315	-0.021662	2.377911
111.175521	1914.098722	5.592320	-0.021749	2.382804
111.424093	1922.187493	5.597325	-0.021800	2.387716
111.287103	1930.300754	5.602330	-0.021780	2.392601
111.764457	1938.333621	5.607334	-0.021874	2.397477
111.747087	1946.415815	5.612339	-0.021876	2.402334
112.228403	1954.441496	5.617344	-0.021971	2.407186
112.144577	1962.599580	5.622349	-0.021961	2.412063
112.289135	1970.654398	5.627354	-0.021993	2.416887
113.154445	1978.613195	5.632358	-0.022159	2.421701
113.475519	1986.668843	5.637363	-0.022224	2.426519
113.706235	1994.786175	5.642368	-0.022273	2.431358
114.037588	2002.853993	5.647373	-0.022340	2.436165
114.220470	2010.897186	5.652378	-0.022379	2.440937
114.353230	2018.994124	5.657382	-0.022409	2.445727
114.691353	2027.032647	5.662387	-0.022477	2.450489
114.917124	2035.112515	5.667392	-0.022525	2.455258
115.029721	2043.191763	5.672397	-0.022551	2.460008
115.301574	2051.219578	5.677402	-0.022607	2.464731
115.397937	2059.337115	5.682406	-0.022630	2.469484
115.868147	2067.317351	5.687411	-0.022723	2.474176
116.082159	2075.396288	5.692416	-0.022768	2.478898
116.086448	2083.480073	5.697421	-0.022774	2.483597
116.385522	2091.500230	5.702426	-0.022835	2.488272
116.602146	2099.592312	5.707430	-0.022881	2.492974
116.636995	2107.684053	5.712435	-0.022893	2.497654
116.959590	2115.712911	5.717440	-0.022958	2.502310
116.991947	2123.820447	5.722445	-0.022969	2.506981
117.235318	2131.868170	5.727450	-0.023020	2.511624
117.581457	2139.921987	5.732454	-0.023090	2.516270
117.791498	2147.941407	5.737459	-0.023134	2.520878
117.876312	2156.009317	5.742464	-0.023155	2.525495
118.119454	2164.088609	5.747469	-0.023206	2.530123
118.265799	2172.129201	5.752474	-0.023238	2.534712
118.736053	2180.152974	5.757478	-0.023331	2.539308
118.698114	2188.232072	5.762483	-0.023329	2.543889
118.841263	2196.317395	5.767488	-0.023361	2.548479
119.168657	2204.363679	5.772493	-0.023428	2.553052
119.502257	2212.392246	5.777498	-0.023495	2.557607
119.821499	2220.428578	5.782502	-0.023560	2.562157
120.104635	2228.469835	5.787507	-0.023618	2.566699
120.384761	2236.555407	5.792512	-0.023675	2.571258
120.877938	2244.598047	5.797517	-0.023772	2.575800
121.253265	2252.617356	5.802522	-0.023847	2.580312
121.706546	2260.669887	5.807526	-0.023937	2.584840
121.767067	2268.788466	5.812531	-0.023954	2.589370
122.242690	2276.898652	5.817536	-0.024048	2.593916
122.495974	2284.928476	5.822541	-0.024100	2.598393
122.941295	2292.908973	5.827546	-0.024188	2.602849
123.071138	2301.000942	5.832550	-0.024218	2.607337
123.004887	2309.096492	5.837555	-0.024211	2.611806
123.180097	2317.157209	5.842560	-0.024249	2.616265
123.482999	2325.168719	5.847565	-0.024310	2.620697
123.428039	2333.230730	5.852570	-0.024305	2.625125
123.665549	2341.283802	5.857574	-0.024355	2.629561
123.594134	2349.372841	5.862579	-0.024347	2.633988
123.927555	2357.369992	5.867584	-0.024414	2.638385
124.452786	2365.360027	5.872589	-0.024517	2.642784
124.705947	2373.410315	5.877594	-0.024570	2.647189
124.828044	2381.522258	5.882598	-0.024598	2.651612
124.818967	2389.596173	5.887603	-0.024601	2.655998
125.313477	2397.587329	5.892608	-0.024699	2.660366
125.326461	2405.668537	5.897613	-0.024706	2.664743
125.680423	2413.676616	5.902618	-0.024778	2.669096
125.828374	2421.785800	5.907622	-0.024810	2.673483
126.028334	2429.807510	5.912627	-0.024853	2.677819
126.229729	2437.834622	5.917632	-0.024896	2.682151
126.726644	2445.827094	5.922637	-0.024994	2.686476
126.814713	2453.911758	5.927642	-0.025015	2.690817
127.220124	2461.984894	5.932646	-0.025096	2.695166
127.431427	2470.006652	5.937651	-0.025141	2.699467
127.250989	2478.117586	5.942656	-0.025112	2.703784
127.357170	2486.188465	5.947661	-0.025137	2.708091
127.924556	2494.159477	5.952666	-0.025248	2.712368
128.043176	2502.254104	5.957670	-0.025276	2.716675
127.929455	2510.323099	5.962675	-0.025260	2.720946
127.962064	2518.373521	5.967680	-0.025271	2.725211
128.264963	2526.412355	5.972685	-0.025333	2.729479
128.366537	2534.470958	5.977690	-0.025357	2.733739
128.999534	2542.472577	5.982694	-0.025480	2.737996
128.833593	2550.554707	5.987699	-0.025455	2.742238
129.506170	2558.538985	5.992704	-0.025585	2.746474
129.528357	2566.662996	5.997709	-0.025595	2.750737
130.223244	2574.643167	6.002714	-0.025729	2.754959
130.599684	2582.651136	6.007718	-0.025805	2.759170
130.935707	2590.672168	6.012723	-0.025872	2.763378
131.176506	2598.747478	6.017728	-0.025923	2.767603
131.095010	2606.868593	6.022733	-0.025913	2.771824
131.028890	2614.945526	6.027738	-0.025906	2.776018
131.706855	2622.932469	6.032742	-0.026037	2.780204
131.713047	2630.955433	6.037747	-0.026044	2.784361
131.958368	2639.026315	6.042752	-0.026095	2.788552
132.360632	2647.055389	6.047757	-0.026175	2.792723
132.625942	2655.062468	6.052762	-0.026229	2.796869
132.960369	2663.120216	6.057766	-0.026297	2.801040
132.750525	2671.204487	6.062771	-0.026263	2.805184
133.204108	2679.219646	6.067776	-0.026353	2.809327
133.384689	2687.291455	6.072781	-0.026392	2.813477
133.626138	2695.315739	6.077786	-0.026442	2.817599
133.692374	2703.410737	6.082790	-0.026460	2.821742
133.769268	2711.450953	6.087795	-0.026479	2.825850
133.986173	2719.500228	6.092800	-0.026525	2.829966
133.581544	2727.622000	6.097805	-0.026455	2.834076
134.354727	2735.504138	6.102810	-0.026604	2.838128
134.794362	2743.533585	6.107814	-0.026691	2.842228
135.015627	2751.561106	6.112819	-0.026738	2.846310
134.923773	2759.696042	6.117824	-0.026726	2.850421
135.205550	2767.714003	6.122829	-0.026784	2.854489
135.563884	2775.711915	6.127834	-0.026856	2.858545
135.895805	2783.763467	6.132838	-0.026923	2.862621
136.043063	2791.816033	6.137843	-0.026956	2.866682
136.110646	2799.900349	6.142848	-0.026973	2.870747
136.239570	2807.955589	6.147853	-0.027003	2.874796
136.444188	2815.963810	6.152858	-0.027046	2.878820
136.713751	2823.994748	6.157862	-0.027102	2.882853
136.923861	2832.013157	6.162867	-0.027146	2.886872
137.256159	2840.061658	6.167872	-0.027213	2.890906
137.675018	2848.109979	6.172877	-0.027296	2.894939
137.566356	2856.170572	6.177882	-0.027281	2.898943
137.662626	2864.236274	6.182886	-0.027305	2.902956
137.575075	2872.298495	6.187891	-0.027294	2.906951
137.986951	2880.339334	6.192896	-0.027376	2.910958
138.217303	2888.409191	6.197901	-0.027424	2.914964
138.279569	2896.388216	6.202906	-0.027441	2.918910
138.638464	2904.409079	6.207910	-0.027513	2.922887
138.918628	2912.397810	6.212915	-0.027570	2.926839
139.117669	2920.472503	6.217920	-0.027613	2.930823
139.242520	2928.572217	6.222925	-0.027641	2.934810
139.147753	2936.588836	6.227930	-0.027629	2.938739
138.967956	2944.703909	6.232934	-0.027601	2.942707
138.998627	2952.716712	6.237939	-0.027612	2.946630
139.174553	2960.748570	6.242944	-0.027650	2.950565
139.902123	2968.698838	6.247949	-0.027790	2.954485
139.842451	2976.740996	6.252954	-0.027785	2.958402
140.256528	2984.755566	6.257958	-0.027867	2.962326
140.691222	2992.763324	6.262963	-0.027953	2.966242
140.679522	3000.864545	6.267968	-0.027956	2.970175
140.786332	3008.939159	6.272973	-0.027981	2.974096
140.643989	3016.985685	6.277978	-0.027960	2.977985
141.177175	3024.956035	6.282982	-0.028065	2.981868
141.394234	3033.010002	6.287987	-0.028110	2.985769
141.690148	3041.042164	6.292992	-0.028171	2.989658
141.975482	3049.102950	6.297997	-0.028229	2.993556
141.825105	3057.147158	6.303002	-0.028207	2.997419
141.935989	3065.202926	6.308006	-0.028232	3.001295
142.045255	3073.193176	6.313011	-0.028258	3.005135
142.351823	3081.220227	6.318016	-0.028320	3.008997
142.789796	3089.279002	6.323021	-0.028407	3.012876
142.909434	3097.292735	6.328026	-0.028435	3.016713
143.428844	3105.325325	6.333030	-0.028537	3.020574
142.904986	3113.439755	6.338035	-0.028445	3.024416
143.072704	3121.489090	6.343040	-0.028481	3.028258
143.367906	3129.492577	6.348045	-0.028541	3.032079
142.746388	3137.627304	6.353050	-0.028431	3.035911
143.619541	3145.529093	6.358054	-0.028599	3.039703
143.996206	3153.528968	6.363059	-0.028674	3.043512
144.408826	3161.533318	6.368064	-0.028756	3.047320
144.661211	3169.629453	6.373069	-0.028808	3.051158
144.903458	3177.627771	6.378074	-0.028859	3.054945
144.996638	3185.708018	6.383078	-0.028882	3.058759
145.138973	3193.748832	6.388083	-0.028913	3.062552
145.410108	3201.779674	6.393088	-0.028969	3.066341
145.679100	3209.850089	6.398093	-0.029024	3.070144
145.910913	3217.906533	6.403098	-0.029073	3.073934
146.326070	3225.912101	6.408102	-0.029155	3.077705
146.100193	3233.959071	6.413107	-0.029119	3.081459
146.062205	3241.999755	6.418112	-0.029117	3.085215
146.077725	3250.067486	6.423117	-0.029125	3.088981
146.281547	3258.056087	6.428122	-0.029168	3.092715
146.420325	3266.102704	6.433126	-0.029199	3.096468
146.383356	3274.136806	6.438131	-0.029198	3.100203
146.102240	3282.202106	6.443136	-0.029151	3.103936
146.936870	3290.137215	6.448141	-0.029311	3.107657
147.064450	3298.187091	6.453146	-0.029340	3.111393
147.640311	3306.195213	6.458150	-0.029453	3.115126
148.387556	3314.122925	6.463155	-0.029597	3.118826
148.541422	3322.207618	6.468160	-0.029631	3.122566
148.643498	3330.305954	6.473165	-0.029656	3.126305
148.872301	3338.328052	6.478170	-0.029703	3.130010
149.202272	3346.382901	6.483174	-0.029770	3.133731
149.401903	3354.416363	6.488179	-0.029813	3.137432
149.781719	3362.451616	6.493184	-0.029889	3.141137
149.670059	3370.530601	6.498189	-0.029873	3.144835
149.906353	3378.560518	6.503194	-0.029922	3.148523
150.299583	3386.584379	6.508198	-0.030001	3.152210
150.153229	3394.646743	6.513203	-0.029979	3.155886
150.328348	3402.640061	6.518208	-0.030017	3.159541
150.989495	3410.630353	6.523213	-0.030145	3.163212
151.505926	3418.604735	6.528218	-0.030247	3.166865
151.674444	3426.694972	6.533222	-0.030283	3.170551
151.887089	3434.737416	6.538227	-0.030328	3.174213
152.169053	3442.803127	6.543232	-0.030386	3.177884
152.363717	3450.855828	6.548237	-0.030427	3.181541
152.725553	3458.803562	6.553242	-0.030500	3.185154
153.647505	3466.801300	6.558246	-0.030677	3.188810
153.840713	3474.854640	6.563251	-0.030718	3.192454
153.711234	3482.942367	6.568256	-0.030699	3.196096
153.949127	3490.979412	6.573261	-0.030749	3.199727
153.713361	3499.048583	6.578266	-0.030710	3.203348
153.797195	3507.115405	6.583270	-0.030731	3.206977
153.810253	3515.153001	6.588275	-0.030739	3.210586
153.683463	3523.220752	6.593280	-0.030721	3.214199
154.158839	3531.195857	6.598285	-0.030815	3.217791
154.641956	3539.148659	6.603290	-0.030910	3.221370
155.077407	3547.157039	6.608294	-0.030996	3.224968
155.588163	3555.166011	6.613299	-0.031096	3.228565
155.914556	3563.232530	6.618304	-0.031162	3.232176
156.070665	3571.308970	6.623309	-0.031197	3.235780
156.106016	3579.294305	6.628314	-0.031209	3.239335
156.093563	3587.378701	6.633318	-0.031212	3.242927
156.593719	3595.328726	6.638323	-0.031310	3.246478
156.833636	3603.393911	6.643328	-0.031360	3.250064
157.107493	3611.425453	6.648333	-0.031416	3.253633
157.094783	3619.482226	6.653338	-0.031419	3.257198
157.469138	3627.528584	6.658342	-0.031494	3.260769
157.957015	3635.472184	6.663347	-0.031590	3.264297
157.938458	3643.571663	6.668352	-0.031592	3.267868
158.056438	3651.654546	6.673357	-0.031619	3.271434
158.101807	3659.652250	6.678362	-0.031633	3.274955
158.364419	3667.670461	6.683366	-0.031687	3.278490
158.475206	3675.668091	6.688371	-0.031713	3.282007
158.940747	3683.687238	6.693376	-0.031805	3.285543
158.865992	3691.783490	6.698381	-0.031796	3.289087
158.942594	3699.817459	6.703386	-0.031816	3.292607
159.721644	3707.793591	6.708390	-0.031966	3.296125
159.848242	3715.809652	6.713395	-0.031995	3.299631
159.907518	3723.868371	6.718400	-0.032012	3.303149
160.000494	3731.931933	6.723405	-0.032034	3.306667
160.204917	3739.966033	6.728410	-0.032077	3.310173
160.793944	3747.958822	6.733414	-0.032192	3.313672
160.801186	3755.977722	6.738419	-0.032199	3.317156
161.093864	3763.995147	6.743424	-0.032259	3.320647
161.142206	3772.026580	6.748429	-0.032273	3.324130
161.135385	3780.069981	6.753434	-0.032277	3.327613
161.264934	3788.170966	6.758438	-0.032307	3.331123
161.484780	3796.151051	6.763443	-0.032353	3.334580
162.055177	3804.129951	6.768448	-0.032464	3.338046
162.441936	3812.161306	6.773453	-0.032541	3.341524
162.664129	3820.178140	6.778458	-0.032588	3.344986
162.993582	3828.261391	6.783462	-0.032655	3.348477
163.198423	3836.303230	6.788467	-0.032698	3.351942
163.354376	3844.315623	6.793472	-0.032732	3.355389
163.616425	3852.329904	6.798477	-0.032787	3.358837
163.759578	3860.354255	6.803482	-0.032818	3.362281
163.960296	3868.417614	6.808486	-0.032861	3.365740
164.424605	3876.384507	6.813491	-0.032953	3.369165
164.359390	3884.457140	6.818496	-0.032946	3.372611
164.557262	3892.532657	6.823501	-0.032988	3.376065
164.925848	3900.475695	6.828506	-0.033062	3.379465
165.310382	3908.517938	6.833510	-0.033139	3.382905
165.429091	3916.546039	6.838515	-0.033166	3.386325
165.543199	3924.623871	6.843520	-0.033193	3.389762
166.066818	3932.666603	6.848525	-0.033296	3.393197
165.958515	3940.714604	6.853530	-0.033281	3.396607
166.054086	3948.751695	6.858534	-0.033304	3.400016
166.515890	3956.674819	6.863539	-0.033395	3.403387
166.681170	3964.720702	6.868544	-0.033431	3.406795
166.890841	3972.759858	6.873549	-0.033475	3.410199
167.094802	3980.757312	6.878554	-0.033519	3.413582
167.264326	3988.829433	6.883558	-0.033555	3.416991
167.322989	3996.861237	6.888563	-0.033572	3.420377
167.404226	4004.858302	6.893568	-0.033592	3.423745
167.615991	4012.965240	6.898573	-0.033637	3.427160
168.094589	4020.947884	6.903578	-0.033731	3.430529
168.286381	4028.971575	6.908582	-0.033772	3.433902
168.178052	4037.026850	6.913587	-0.033757	3.437275
168.355301	4045.028876	6.918592	-0.033796	3.440631
168.662601	4053.007824	6.923597	-0.033858	3.443980
168.807166	4061.062761	6.928602	-0.033890	3.447351
169.281681	4069.130505	6.933606	-0.033984	3.450736
169.423485	4077.105824	6.938611	-0.034015	3.454067
169.488267	4085.140993	6.943616	-0.034033	3.457417
169.591939	4093.247579	6.948621	-0.034057	3.460795
169.887648	4101.173631	6.953626	-0.034118	3.464101
169.947108	4109.265825	6.958630	-0.034134	3.467465
170.050714	4117.323927	6.963635	-0.034159	3.470813
170.361740	4125.263743	6.968640	-0.034222	3.474116
170.520125	4133.318675	6.973645	-0.034257	3.477458
170.669044	4141.345977	6.978650	-0.034290	3.480785
170.902816	4149.295606	6.983654	-0.034338	3.484080
170.979960	4157.384233	6.988659	-0.034358	3.487423
171.174479	4165.418235	6.993664	-0.034400	3.490745
171.340186	4173.443360	6.998669	-0.034436	3.494059
171.466076	4181.463451	7.003674	-0.034464	3.497367
171.337944	4189.588922	7.008678	-0.034446	3.500706
171.492033	4197.520293	7.013683	-0.034480	3.503972
171.855546	4205.539074	7.018688	-0.034553	3.507277
172.011456	4213.649812	7.023693	-0.034587	3.510610
172.324743	4221.576063	7.028698	-0.034651	3.513869
172.756831	4229.617138	7.033702	-0.034736	3.517176
172.288653	4237.729232	7.038707	-0.034655	3.520480
172.548289	4245.673142	7.043712	-0.034708	3.523736
172.535502	4253.740704	7.048717	-0.034711	3.527030
172.832046	4261.746470	7.053722	-0.034771	3.530306
173.308820	4269.741169	7.058726	-0.034865	3.533580
173.377508	4277.820493	7.063731	-0.034884	3.536873
173.747311	4285.797282	7.068736	-0.034958	3.540130
174.057397	4293.800045	7.073741	-0.035021	3.543393
174.328793	4301.861005	7.078746	-0.035077	3.546675
174.689276	4309.929636	7.083750	-0.035149	3.549960
174.384070	4318.040075	7.088755	-0.035097	3.553238
174.522926	4326.015886	7.093760	-0.035129	3.556472
175.554031	4333.890724	7.098765	-0.035326	3.559691
175.419982	4341.925308	7.103770	-0.035306	3.562934
175.845258	4349.970278	7.108774	-0.035390	3.566197
175.934006	4358.014269	7.113779	-0.035412	3.569445
176.187809	4366.012091	7.118784	-0.035465	3.572677
176.382017	4374.097773	7.123789	-0.035506	3.575939
176.440578	4382.061420	7.128794	-0.035522	3.579146
176.966288	4390.090422	7.133798	-0.035626	3.582389
176.971785	4398.154991	7.138803	-0.035632	3.585629
177.233968	4406.146217	7.143808	-0.035686	3.588844
177.688543	4414.214548	7.148813	-0.035776	3.592092
177.353145	4422.283553	7.153818	-0.035719	3.595314
177.658419	4430.276307	7.158822	-0.035781	3.598522
177.970568	4438.265676	7.163827	-0.035844	3.601726
178.360276	4446.233139	7.168832	-0.035922	3.604920
178.462559	4454.317398	7.173837	-0.035946	3.608150
178.296794	4462.375334	7.178842	-0.035921	3.611359
178.282102	4470.448143	7.183846	-0.035923	3.614574
178.364138	4478.478721	7.188851	-0.035944	3.617774
178.866946	4486.441887	7.193856	-0.036043	3.620955
178.920063	4494.467687	7.198861	-0.036058	3.624146
179.099330	4502.518218	7.203866	-0.036097	3.627347
179.511105	4510.539500	7.208870	-0.036179	3.630541
179.676541	4518.529795	7.213875	-0.036215	3.633712
179.894896	4526.580153	7.218880	-0.036261	3.636906
179.933909	4534.619729	7.223885	-0.036273	3.640087
180.052706	4542.581652	7.228890	-0.036300	3.643238
180.416895	4550.620861	7.233894	-0.036374	3.646423
180.870283	4558.605531	7.238899	-0.036463	3.649586
181.183823	4566.657940	7.243904	-0.036527	3.652769
181.400589	4574.713247	7.248909	-0.036573	3.655948
181.558669	4582.698052	7.253914	-0.036607	3.659095
181.785719	4590.738190	7.258918	-0.036655	3.662262
181.834745	4598.761282	7.263923	-0.036669	3.665416
182.134850	4606.778568	7.268928	-0.036730	3.668571
182.494262	4614.820277	7.273933	-0.036803	3.671734
182.248699	4622.855263	7.278938	-0.036762	3.674876
182.740460	4630.853191	7.283942	-0.036859	3.678020
182.797495	4638.900959	7.288947	-0.036875	3.681170
183.044196	4646.861887	7.293952	-0.036926	3.684288
183.109849	4654.932480	7.298957	-0.036944	3.687441
183.217060	4662.971150	7.303962	-0.036969	3.690580
183.474776	4670.996038	7.308966	-0.037022	3.693715
183.579899	4679.039848	7.313971	-0.037047	3.696851
183.467264	4687.082840	7.318976	-0.037031	3.699978
184.005609	4695.042780	7.323981	-0.037137	3.703087
183.832634	4703.087371	7.328986	-0.037110	3.706208
184.203403	4711.128664	7.333990	-0.037184	3.709339
184.660460	4719.165503	7.338995	-0.037274	3.712468
184.601774	4727.236555	7.344000	-0.037269	3.715594
184.653476	4735.228780	7.349005	-0.037284	3.718690
184.630925	4743.264117	7.354010	-0.037285	3.721798
184.997852	4751.231876	7.359014	-0.037358	3.724887
185.284230	4759.230342	7.364019	-0.037417	3.727983
185.661423	4767.244178	7.369024	-0.037492	3.731085
185.672486	4775.275135	7.374029	-0.037500	3.734182
185.650441	4783.334397	7.379034	-0.037501	3.737286
186.208852	4791.328378	7.384038	-0.037610	3.740377
186.116577	4799.366712	7.389043	-0.037598	3.743467
186.501168	4807.370136	7.394048	-0.037675	3.746552
186.602286	4815.435283	7.399053	-0.037699	3.749651
187.120156	4823.391530	7.404058	-0.037801	3.752716
186.911130	4831.515341	7.409062	-0.037767	3.755825
187.316371	4839.431084	7.414067	-0.037848	3.758867
187.634460	4847.467540	7.419072	-0.037913	3.761950
187.660870	4855.518710	7.424077	-0.037923	3.765029
187.574294	4863.523175	7.429082	-0.037912	3.768086
187.529292	4871.644378	7.434086	-0.037909	3.771185
188.004625	4879.556793	7.439091	-0.038003	3.774214
188.069218	4887.619645	7.444096	-0.038020	3.777289
188.358636	4895.643826	7.449101	-0.038079	3.780352
188.654051	4903.586447	7.454106	-0.038139	3.783381
188.956376	4911.658360	7.459110	-0.038201	3.786457
189.097035	4919.702634	7.464115	-0.038232	3.789516
189.223891	4927.738700	7.469120	-0.038261	3.792570
189.828536	4935.730372	7.474125	-0.038379	3.795615
189.722470	4943.723061	7.479130	-0.038365	3.798641
190.066422	4951.743117	7.484134	-0.038434	3.801686
190.093212	4959.764409	7.489139	-0.038444	3.804722
190.387910	4967.807174	7.494144	-0.038504	3.807769
190.377779	4975.920531	7.499149	-0.038508	3.810834
190.483059	4983.874551	7.504154	-0.038533	3.813838
190.821248	4991.924339	7.509158	-0.038601	3.816882
190.700298	4999.955318	7.514163	-0.038584	3.819905
190.831179	5007.930218	7.519168	-0.038613	3.822911
190.841740	5016.029892	7.524173	-0.038620	3.825959
190.956765	5024.006853	7.529178	-0.038647	3.828961
191.280639	5032.063349	7.534182	-0.038713	3.831994
191.560453	5040.035796	7.539187	-0.038770	3.834993
191.983308	5048.005330	7.544192	-0.038854	3.837991
192.117152	5056.114145	7.549197	-0.038884	3.841033
192.278971	5064.030138	7.554202	-0.038920	3.844001
192.539936	5072.103454	7.559206	-0.038974	3.847027
192.695600	5080.130909	7.564211	-0.039008	3.850032
192.730657	5088.189273	7.569216	-0.039020	3.853043
192.923463	5096.249014	7.574221	-0.039061	3.856056
193.101917	5104.206285	7.579226	-0.039099	3.859028
193.543034	5112.220034	7.584230	-0.039187	3.862024
193.661894	5120.212547	7.589235	-0.039214	3.865003
194.020791	5128.232826	7.594240	-0.039286	3.867995
194.017827	5136.345592	7.599245	-0.039291	3.871011
194.085594	5144.485900	7.604250	-0.039309	3.874037
194.281836	5152.454567	7.609254	-0.039351	3.877000
194.456189	5160.412131	7.614259	-0.039388	3.879955
194.261899	5168.394014	7.619264	-0.039357	3.882910
194.744253	5176.422461	7.624269	-0.039453	3.885894
195.043775	5184.344284	7.629274	-0.039513	3.888832
194.950568	5192.491669	7.634278	-0.039501	3.891843
195.149421	5200.444070	7.639283	-0.039544	3.894786
195.554785	5208.418250	7.644288	-0.039624	3.897739
195.694382	5216.492837	7.649293	-0.039656	3.900721
195.345820	5224.524172	7.654298	-0.039596	3.903675
195.968662	5232.567766	7.659302	-0.039717	3.906651
195.925607	5240.547938	7.664307	-0.039715	3.909588
196.263565	5248.544014	7.669312	-0.039783	3.912536
196.676826	5256.563450	7.674317	-0.039865	3.915492
196.653581	5264.572652	7.679322	-0.039866	3.918433
196.835386	5272.638997	7.684326	-0.039905	3.921397
197.059893	5280.601094	7.689331	-0.039952	3.924321
197.284945	5288.654430	7.694336	-0.039999	3.927277
197.665983	5296.707372	7.699341	-0.040076	3.930233
196.978107	5304.826435	7.704346	-0.039953	3.933190
197.588229	5312.780495	7.709350	-0.040072	3.936110
197.931646	5320.751296	7.714355	-0.040141	3.939029
197.790468	5328.816789	7.719360	-0.040120	3.941971
197.866195	5336.827308	7.724365	-0.040139	3.944895
198.239032	5344.809552	7.729370	-0.040214	3.947812
198.512711	5352.843287	7.734374	-0.040270	3.950743
198.940826	5360.866585	7.739379	-0.040355	3.953672
199.029977	5368.922848	7.744384	-0.040377	3.956604
199.132413	5376.926019	7.749389	-0.040401	3.959514
199.191735	5384.930445	7.754394	-0.040418	3.962422
199.320628	5392.968238	7.759398	-0.040447	3.965342
199.650435	5400.961394	7.764403	-0.040514	3.968247
199.764054	5409.017970	7.769408	-0.040540	3.971168
199.907532	5417.065238	7.774413	-0.040572	3.974085
199.660780	5425.118112	7.779418	-0.040531	3.976994
200.170382	5433.078717	7.784422	-0.040631	3.979882
199.559124	5441.152701	7.789427	-0.040523	3.982788
199.730248	5449.149619	7.794432	-0.040560	3.985678
200.135354	5457.126208	7.799437	-0.040641	3.988563
200.627772	5465.097547	7.804442	-0.040738	3.991446
200.947173	5473.137049	7.809446	-0.040802	3.994348
200.979414	5481.173058	7.814451	-0.040814	3.997241
201.164029	5489.170211	7.819456	-0.040853	4.000121
201.355445	5497.207638	7.824461	-0.040894	4.003014
201.254573	5505.243251	7.829466	-0.040881	4.005898
201.871680	5513.196376	7.834470	-0.041001	4.008764
202.122474	5521.267795	7.839475	-0.041053	4.011663
202.065368	5529.303120	7.844480	-0.041048	4.014542
202.583493	5537.362395	7.849485	-0.041149	4.017438
202.562303	5545.323037	7.854490	-0.041151	4.020287
202.545096	5553.392177	7.859494	-0.041153	4.023172
202.980002	5561.383998	7.864499	-0.041239	4.026036
202.938201	5569.391580	7.869504	-0.041236	4.028895
203.186507	5577.481568	7.874509	-0.041288	4.031786
203.445290	5585.459646	7.879514	-0.041341	4.034636
203.800454	5593.498655	7.884518	-0.041413	4.037506
203.682542	5601.473923	7.889523	-0.041396	4.040344
203.559019	5609.469053	7.894528	-0.041378	4.043188
203.901296	5617.514559	7.899533	-0.041447	4.046054
203.945467	5625.491467	7.904538	-0.041461	4.048890
204.090652	5633.586431	7.909542	-0.041493	4.051767
204.167067	5641.568834	7.914547	-0.041513	4.054600
204.248194	5649.597165	7.919552	-0.041533	4.057449
204.832612	5657.615948	7.924557	-0.041647	4.060299
204.677119	5665.609731	7.929562	-0.041623	4.063128
205.315748	5673.622720	7.934566	-0.041748	4.065973
204.978605	5681.688641	7.939571	-0.041690	4.068820
205.179379	5689.735800	7.944576	-0.041733	4.071667
205.773570	5697.683203	7.949581	-0.041849	4.074482
205.895319	5705.722217	7.954586	-0.041877	4.077321
205.953992	5713.781112	7.959590	-0.041893	4.080163
206.316689	5721.744929	7.964595	-0.041966	4.082975
206.116788	5729.825233	7.969600	-0.041934	4.085817
206.272723	5737.842776	7.974605	-0.041968	4.088641
206.336298	5745.885810	7.979610	-0.041985	4.091470
206.548993	5753.906862	7.984614	-0.042030	4.094291
206.192121	5761.976884	7.989619	-0.041969	4.097120
206.867766	5769.863484	7.994624	-0.042100	4.099897
207.126576	5777.916345	7.999629	-0.042153	4.102725
207.453398	5785.927517	8.004634	-0.042219	4.105537
207.435900	5794.001238	8.009638	-0.042221	4.108364
207.498918	5802.001377	8.014643	-0.042238	4.111164
207.798010	5809.971528	8.019648	-0.042299	4.113956
208.005333	5818.015275	8.024653	-0.042343	4.116770
207.863053	5826.047366	8.029658	-0.042322	4.119572
208.257460	5834.057150	8.034662	-0.042401	4.122373
208.131152	5842.058349	8.039667	-0.042382	4.125162
208.277971	5850.053204	8.044672	-0.042415	4.127950
208.756329	5858.122971	8.049677	-0.042509	4.130767
208.721991	5866.086642	8.054682	-0.042508	4.133538
209.025041	5874.168204	8.059686	-0.042570	4.136353
208.593752	5882.227300	8.064691	-0.042495	4.139148
208.978831	5890.181010	8.069696	-0.042572	4.141916
209.444320	5898.151513	8.074701	-0.042664	4.144688
209.398524	5906.181319	8.079706	-0.042661	4.147473
209.819218	5914.229399	8.084710	-0.042744	4.150268
210.022378	5922.249844	8.089715	-0.042787	4.153049
209.946966	5930.316921	8.094720	-0.042779	4.155840
210.052558	5938.301363	8.099725	-0.042803	4.158603
210.094938	5946.329659	8.104730	-0.042817	4.161379
210.022374	5954.279006	8.109734	-0.042808	4.164124
210.362056	5962.321502	8.114739	-0.042877	4.166905
210.840037	5970.289309	8.119744	-0.042971	4.169660
210.905749	5978.418044	8.124749	-0.042989	4.172463
211.076687	5986.370791	8.129754	-0.043026	4.175205
211.202626	5994.440224	8.134758	-0.043055	4.177985
211.492126	6002.433881	8.139763	-0.043114	4.180739
211.090317	6010.468521	8.144768	-0.043044	4.183497
211.600246	6018.500464	8.149773	-0.043144	4.186263
211.352287	6026.523778	8.154778	-0.043103	4.189015
211.700436	6034.616885	8.159782	-0.043174	4.191796
212.087607	6042.579372	8.164787	-0.043251	4.194531
212.825619	6050.521367	8.169792	-0.043394	4.197262
212.864146	6058.520361	8.174797	-0.043406	4.200002
212.992363	6066.537947	8.179802	-0.043435	4.202747
213.034804	6074.645944	8.184806	-0.043448	4.205521
212.847387	6082.677580	8.189811	-0.043419	4.208264
212.688960	6090.712494	8.194816	-0.043395	4.211007
213.296874	6098.698503	8.199821	-0.043513	4.213740
213.822538	6106.680798	8.204826	-0.043616	4.216469
213.744384	6114.700429	8.209830	-0.043607	4.219202
213.758670	6122.776272	8.214835	-0.043615	4.221953
214.002577	6130.719611	8.219840	-0.043665	4.224660
214.312790	6138.798168	8.224845	-0.043728	4.227412
214.352597	6146.760458	8.229850	-0.043741	4.230120
214.550341	6154.816534	8.234854	-0.043783	4.232859
214.652351	6162.844195	8.239859	-0.043808	4.235586
214.929653	6170.789597	8.244864	-0.043864	4.238286
215.078126	6178.865814	8.249869	-0.043897	4.241026
215.660141	6186.751246	8.254874	-0.044011	4.243705
215.674845	6194.879998	8.259878	-0.044019	4.246458
215.756263	6202.929850	8.264883	-0.044039	4.249184
216.077953	6210.940572	8.269888	-0.044105	4.251897
216.357527	6218.925504	8.274893	-0.044162	4.254599
216.243383	6226.965524	8.279898	-0.044146	4.257314
216.632093	6234.982474	8.284902	-0.044224	4.260024
216.584476	6243.012258	8.289907	-0.044220	4.262733
216.554132	6251.062368	8.294912	-0.044220	4.265447
217.121922	6258.984926	8.299917	-0.044331	4.268122
217.280291	6267.048108	8.304922	-0.044365	4.270839
217.375746	6275.099778	8.309926	-0.044388	4.273549
217.035859	6283.159983	8.314931	-0.044330	4.276257
217.311563	6291.068001	8.319936	-0.044387	4.278917
217.382817	6299.140340	8.324941	-0.044405	4.281629
217.773042	6307.023599	8.329946	-0.044483	4.284279
217.834557	6315.183738	8.334950	-0.044500	4.287017
218.136512	6323.151399	8.339955	-0.044562	4.289691
217.738714	6331.267673	8.344960	-0.044493	4.292407
217.738666	6339.262247	8.349965	-0.044498	4.295084
218.032649	6347.194923	8.354970	-0.044558	4.297741
218.341094	6355.232164	8.359974	-0.044621	4.300431
218.338782	6363.207314	8.364979	-0.044626	4.303097
218.757130	6371.221896	8.369984	-0.044709	4.305777
218.794291	6379.281789	8.374989	-0.044721	4.308468
218.704566	6387.366030	8.379994	-0.044710	4.311164
219.344012	6395.295554	8.384998	-0.044834	4.313813
219.439717	6403.350375	8.390003	-0.044857	4.316497
219.719597	6411.270401	8.395008	-0.044914	4.319136
219.773824	6419.394556	8.400013	-0.044930	4.321840
219.927818	6427.293059	8.405018	-0.044964	4.324468
220.227661	6435.332753	8.410022	-0.045025	4.327142
220.171098	6443.433546	8.415027	-0.045019	4.329832
220.284025	6451.433505	8.420032	-0.045046	4.332488
220.528489	6459.494479	8.425037	-0.045097	4.335164
220.316923	6467.471903	8.430042	-0.045062	4.337807
220.707547	6475.450721	8.435046	-0.045140	4.340453
220.736037	6483.420710	8.440051	-0.045151	4.343092
220.831899	6491.527966	8.445056	-0.045174	4.345776
220.973470	6499.540029	8.450061	-0.045206	4.348426
220.840645	6507.603222	8.455066	-0.045186	4.351090
220.585291	6515.688366	8.460070	-0.045144	4.353758
221.037803	6523.642702	8.465075	-0.045234	4.356387
221.119085	6531.544324	8.470080	-0.045254	4.358995
221.614915	6539.577645	8.475085	-0.045351	4.361647
221.532221	6547.561880	8.480090	-0.045341	4.364277
222.163514	6555.589868	8.485094	-0.045464	4.366925
222.608401	6563.611960	8.490099	-0.045552	4.369568
222.560313	6571.649034	8.495104	-0.045549	4.372211
222.820037	6579.684221	8.500109	-0.045602	4.374853
222.926008	6587.687783	8.505114	-0.045627	4.377483
223.296727	6595.732374	8.510118	-0.045702	4.380126
223.601500	6603.711041	8.515123	-0.045764	4.382746
223.159011	6611.758964	8.520128	-0.045686	4.385382
223.172983	6619.857288	8.525133	-0.045694	4.388035
223.355817	6627.809215	8.530138	-0.045734	4.390641
223.401718	6635.826963	8.535142	-0.045747	4.393265
223.396007	6643.912642	8.540147	-0.045752	4.395910
223.698301	6651.813564	8.545152	-0.045813	4.398494
223.981081	6659.907969	8.550157	-0.045871	4.401141
224.046658	6667.843310	8.555162	-0.045889	4.403732
224.443990	6675.896506	8.560167	-0.045968	4.406362
224.519558	6683.889086	8.565171	-0.045987	4.408969
224.642811	6691.977510	8.570176	-0.046015	4.411606
224.625770	6700.021717	8.575181	-0.046018	4.414226
224.412931	6708.085893	8.580186	-0.045983	4.416850
224.838506	6716.026771	8.585191	-0.046068	4.419436
224.741247	6724.107917	8.590195	-0.046055	4.422062
224.977508	6732.042646	8.595200	-0.046104	4.424642
224.923842	6740.131573	8.600205	-0.046099	4.427269
225.027265	6748.144553	8.605210	-0.046124	4.429870
225.139906	6756.211232	8.610215	-0.046150	4.432487
225.496360	6764.139762	8.615219	-0.046222	4.435059
225.911985	6772.116366	8.620224	-0.046304	4.437646
225.786003	6780.222757	8.625229	-0.046286	4.440270
226.010670	6788.176484	8.630234	-0.046333	4.442845
226.340319	6796.203667	8.635239	-0.046400	4.445443
226.589215	6804.210924	8.640243	-0.046452	4.448032
226.856439	6812.273897	8.645248	-0.046507	4.450638
226.773878	6820.317335	8.650253	-0.046497	4.453234
227.014380	6828.335155	8.655258	-0.046547	4.455823
227.243240	6836.355985	8.660263	-0.046594	4.458410
227.077387	6844.386709	8.665267	-0.046569	4.460997
227.273101	6852.281740	8.670272	-0.046610	4.463541
227.614706	6860.433344	8.675277	-0.046679	4.466167
227.716015	6868.391550	8.680282	-0.046704	4.468727
227.131139	6876.544139	8.685287	-0.046600	4.471346
227.420936	6884.430088	8.690291	-0.046659	4.473881
227.283092	6892.490114	8.695296	-0.046639	4.476469
227.709304	6900.413501	8.700301	-0.046723	4.479014
227.968772	6908.461690	8.705306	-0.046777	4.481597
228.038123	6916.418855	8.710311	-0.046795	4.484148
228.008391	6924.548595	8.715315	-0.046795	4.486753
228.213768	6932.489751	8.720320	-0.046838	4.489297
228.497803	6940.562296	8.725325	-0.046897	4.491881
228.821475	6948.508266	8.730330	-0.046962	4.494424
229.103718	6956.591284	8.735335	-0.047020	4.497009
229.012676	6964.587963	8.740339	-0.047008	4.499564
229.161819	6972.599884	8.745344	-0.047041	4.502122
229.447301	6980.573669	8.750349	-0.047100	4.504668
229.164261	6988.649952	8.755354	-0.047052	4.507243
229.393325	6996.679652	8.760359	-0.047100	4.509803
229.715140	7004.684512	8.765363	-0.047165	4.512354
229.579373	7012.674724	8.770368	-0.047145	4.514898
230.018579	7020.680629	8.775373	-0.047232	4.517447
230.234996	7028.633786	8.780378	-0.047278	4.519977
230.027835	7036.692354	8.785383	-0.047245	4.522538
230.021567	7044.727724	8.790387	-0.047249	4.525090
230.143468	7052.730892	8.795392	-0.047277	4.527632
230.333416	7060.791062	8.800397	-0.047317	4.530190
229.914979	7068.860985	8.805402	-0.047245	4.532748
230.587538	7076.790586	8.810407	-0.047375	4.535263
230.870663	7084.764103	8.815411	-0.047433	4.537790
230.686794	7092.799858	8.820416	-0.047404	4.540333
231.252294	7100.785751	8.825421	-0.047515	4.542862
231.548899	7108.777771	8.830426	-0.047575	4.545390
231.774659	7116.838230	8.835431	-0.047623	4.547938
231.292598	7124.927230	8.840435	-0.047538	4.550492
231.844514	7132.864451	8.845440	-0.047646	4.552999
232.021646	7140.955853	8.850445	-0.047684	4.555553
231.755230	7148.930678	8.855450	-0.047640	4.558067
231.767285	7156.992826	8.860455	-0.047648	4.560608
231.671444	7164.938371	8.865459	-0.047635	4.563110
231.962608	7172.942879	8.870464	-0.047694	4.565631
232.453756	7180.966353	8.875469	-0.047791	4.568157
232.261593	7189.029116	8.880474	-0.047761	4.570692
232.284222	7197.019289	8.885479	-0.047770	4.573203
232.782349	7204.994770	8.890483	-0.047868	4.575710
233.001062	7213.010470	8.895488	-0.047914	4.578227
233.253094	7221.139943	8.900493	-0.047966	4.580778
233.349797	7229.037007	8.905498	-0.047990	4.583255
233.886993	7237.070281	8.910503	-0.048095	4.585773
234.061040	7245.130215	8.915507	-0.048133	4.588298
234.088759	7253.155577	8.920512	-0.048143	4.590811
234.181780	7261.184007	8.925517	-0.048166	4.593323
234.715893	7269.147699	8.930522	-0.048270	4.595815
234.942560	7277.121449	8.935527	-0.048318	4.598307
234.972465	7285.158541	8.940531	-0.048329	4.600818
235.090376	7293.126624	8.945536	-0.048356	4.603306
234.677534	7301.304552	8.950541	-0.048284	4.605857
234.980654	7309.216513	8.955546	-0.048346	4.608325
235.415969	7317.248529	8.960551	-0.048432	4.610829
235.785352	7325.248251	8.965555	-0.048506	4.613322
235.997729	7333.285111	8.970560	-0.048551	4.615825
235.733520	7341.302958	8.975565	-0.048507	4.618319
235.947724	7349.319494	8.980570	-0.048552	4.620813
235.520185	7357.362478	8.985575	-0.048478	4.623313
235.232858	7365.406246	8.990579	-0.048430	4.625812
235.105730	7373.383442	8.995584	-0.048411	4.628289
235.783446	7381.404163	9.000589	-0.048543	4.630778
235.772134	7389.338395	9.005594	-0.048546	4.633239
236.384873	7397.368243	9.010599	-0.048665	4.635729
236.956961	7405.365441	9.015603	-0.048777	4.638207
236.716129	7413.463283	9.020608	-0.048738	4.640715
236.723341	7421.404633	9.025613	-0.048744	4.643173
237.497856	7429.366391	9.030618	-0.048894	4.645636
237.755100	7437.451413	9.035623	-0.048947	4.648136
237.891751	7445.499568	9.040627	-0.048977	4.650623
237.881396	7453.504668	9.045632	-0.048981	4.653095
238.246535	7461.571514	9.050637	-0.049054	4.655585
238.180662	7469.525534	9.055642	-0.049047	4.658039
238.283326	7477.575877	9.060647	-0.049071	4.660522
238.724991	7485.552569	9.065651	-0.049159	4.662980
238.541118	7493.582129	9.070656	-0.049130	4.665453
239.197876	7501.587897	9.075661	-0.049258	4.667918
239.517868	7509.596913	9.080666	-0.049322	4.670382
239.729170	7517.686357	9.085671	-0.049367	4.672869
239.564336	7525.755411	9.090675	-0.049342	4.675350
239.737217	7533.669523	9.095680	-0.049379	4.677781
240.146959	7541.672592	9.100685	-0.049461	4.680238
240.334182	7549.658294	9.105690	-0.049501	4.682688
240.305836	7557.698768	9.110695	-0.049501	4.685154
240.251021	7565.734253	9.115699	-0.049496	4.687617
240.448966	7573.710305	9.120704	-0.049538	4.690061
240.449268	7581.792099	9.125709	-0.049543	4.692536
240.150721	7589.792693	9.130714	-0.049493	4.694985
240.302659	7597.844569	9.135719	-0.049526	4.697448
240.531283	7605.797808	9.140723	-0.049574	4.699879
241.021205	7613.767342	9.145728	-0.049671	4.702314
240.858182	7621.850428	9.150733	-0.049646	4.704783
241.074520	7629.840863	9.155738	-0.049691	4.707222
241.039680	7637.903156	9.160743	-0.049690	4.709682
241.450482	7645.925356	9.165747	-0.049772	4.712127
241.466049	7653.844699	9.170752	-0.049780	4.714541
241.567678	7661.943791	9.175757	-0.049804	4.717008
242.146980	7669.848322	9.180762	-0.049917	4.719414
242.455742	7677.937469	9.185767	-0.049980	4.721875
242.413485	7685.925516	9.190771	-0.049977	4.724304
242.714892	7693.922522	9.195776	-0.050039	4.726735
242.979026	7701.962627	9.200781	-0.050093	4.729177
242.870945	7710.006988	9.205786	-0.050078	4.731620
243.033858	7718.051886	9.210791	-0.050114	4.734062
243.084968	7726.138433	9.215795	-0.050129	4.736515
243.043328	7734.077223	9.220800	-0.050126	4.738922
243.443094	7742.153712	9.225805	-0.050206	4.741368
243.493919	7750.014707	9.230810	-0.050221	4.743749
243.807047	7758.076406	9.235815	-0.050284	4.746189
243.737638	7766.097420	9.240819	-0.050277	4.748616
243.942660	7774.169907	9.245824	-0.050320	4.751057
244.252969	7782.206075	9.250829	-0.050383	4.753485
244.464789	7790.237472	9.255834	-0.050428	4.755911
244.532991	7798.156119	9.260839	-0.050446	4.758302
244.638141	7806.244635	9.265843	-0.050471	4.760743
245.088991	7814.179676	9.270848	-0.050560	4.763135
245.110194	7822.285205	9.275853	-0.050569	4.765579
245.048885	7830.237720	9.280858	-0.050563	4.767975
245.239057	7838.331196	9.285863	-0.050604	4.770412
245.283875	7846.329049	9.290867	-0.050617	4.772819
245.335714	7854.319611	9.295872	-0.050632	4.775223
245.626453	7862.363170	9.300877	-0.050692	4.777641
245.427872	7870.403182	9.305882	-0.050660	4.780058
245.444556	7878.407691	9.310887	-0.050668	4.782463
245.497986	7886.355242	9.315891	-0.050683	4.784849
246.084610	7894.428680	9.320896	-0.050798	4.787270
246.120539	7902.443547	9.325901	-0.050810	4.789674
246.265047	7910.425053	9.330906	-0.050842	4.792067
246.479040	7918.426981	9.335911	-0.050887	4.794464
246.783450	7926.509055	9.340915	-0.050949	4.796883
246.510856	7934.482576	9.345920	-0.050904	4.799271
246.702107	7942.574759	9.350925	-0.050945	4.801691
246.898269	7950.446645	9.355930	-0.050986	4.804045
247.130006	7958.536022	9.360935	-0.051035	4.806462
247.568371	7966.512837	9.365939	-0.051122	4.808843
247.479319	7974.592048	9.370944	-0.051110	4.811256
247.133352	7982.585312	9.375949	-0.051051	4.813643
247.084950	7990.038593	9.380954	-0.051047	4.815866
247.389426	7994.696267	9.385959	-0.051107	4.817254

247.688578	7997.087695	9.390963	-0.051164	4.817966
247.423829	7998.583147	9.395968	-0.051116	4.818413
247.820233	7999.640814	9.400973	-0.051190	4.818726
248.030526	7999.575378	9.405978	-0.051230	4.818706
248.067542	8000.011606	9.410983	-0.051237	4.818836
247.966841	8000.408399	9.415987	-0.051218	4.818955
247.805734	8000.256574	9.420992	-0.051188	4.818910
247.874598	7999.954714	9.425997	-0.051201	4.818820
247.366830	8000.043643	9.431002	-0.051106	4.818848
247.954064	7999.993431	9.436007	-0.051216	4.818831
248.426659	8000.368119	9.441011	-0.051304	4.818941
248.059807	8000.256648	9.446016	-0.051236	4.818909
248.515958	8000.329445	9.451021	-0.051321	4.818929
248.650704	8000.493517	9.456026	-0.051346	4.818977
248.376875	8000.241798	9.461031	-0.051295	4.818903
248.342765	8000.250799	9.466035	-0.051289	4.818906
248.805040	8000.490235	9.471040	-0.051375	4.818976
248.923720	8000.192135	9.476045	-0.051397	4.818886
249.082244	8000.501071	9.481050	-0.051427	4.818978
248.827552	8000.013894	9.486055	-0.051379	4.818834
249.203733	8000.524609	9.491059	-0.051449	4.818984
249.361501	8000.420798	9.496064	-0.051479	4.818953
249.188826	8000.422813	9.501069	-0.051447	4.818954
249.211186	8000.428335	9.506074	-0.051451	4.818956
248.972195	8000.275523	9.511079	-0.051406	4.818911
249.085600	8000.114586	9.516083	-0.051427	4.818863
249.016608	8000.299135	9.521088	-0.051415	4.818918
249.432355	7999.939833	9.526093	-0.051492	4.818809
248.970730	8000.206377	9.531098	-0.051406	4.818891
248.993514	8000.038013	9.536103	-0.051410	4.818840
249.107799	7999.977652	9.541107	-0.051432	4.818822
249.312774	8000.069280	9.546112	-0.051470	4.818848
249.177438	7999.822454	9.551117	-0.051444	4.818775
249.295221	8000.064875	9.556122	-0.051467	4.818847
249.740879	8000.291533	9.561127	-0.051550	4.818913
249.639056	8000.290252	9.566131	-0.051531	4.818913
249.487255	8000.174155	9.571136	-0.051503	4.818879
249.241761	7999.828516	9.576141	-0.051457	4.818777
249.356027	7999.975567	9.581146	-0.051478	4.818820
249.163634	8000.042282	9.586151	-0.051442	4.818841
249.788595	8000.305771	9.591155	-0.051559	4.818917
249.789541	8000.373879	9.596160	-0.051559	4.818937
249.642453	8000.258888	9.601165	-0.051532	4.818904
249.628453	8000.398041	9.606170	-0.051529	4.818945
249.609636	7999.967259	9.611175	-0.051526	4.818817
249.403680	7999.867244	9.616179	-0.051487	4.818788
249.617620	8000.249158	9.621184	-0.051527	4.818901
250.142871	8000.243217	9.626189	-0.051625	4.818897
249.923064	8000.357775	9.631194	-0.051584	4.818932
250.189964	8000.376860	9.636199	-0.051634	4.818937
249.772207	8000.325498	9.641203	-0.051556	4.818923
249.828030	8000.201544	9.646208	-0.051567	4.818886
249.775860	8000.070991	9.651213	-0.051557	4.818847
249.789508	8000.147638	9.656218	-0.051560	4.818870
249.969277	8000.030486	9.661223	-0.051593	4.818834
249.852654	8000.096062	9.666227	-0.051571	4.818854
249.620815	8000.048096	9.671232	-0.051528	4.818841
250.030612	7999.951654	9.676237	-0.051604	4.818811
249.897538	8000.286247	9.681242	-0.051580	4.818911
250.100736	8000.136916	9.686247	-0.051618	4.818866
250.005316	8000.072861	9.691251	-0.051600	4.818847
250.543729	8000.288125	9.696256	-0.051700	4.818909
250.140806	8000.055719	9.701261	-0.051625	4.818841
249.875836	8000.386555	9.706266	-0.051576	4.818941
250.130007	8000.194916	9.711271	-0.051623	4.818883
250.597093	8000.549663	9.716275	-0.051711	4.818987
250.315144	8000.215067	9.721280	-0.051658	4.818888
250.893872	8000.282087	9.726285	-0.051766	4.818906
250.706761	8000.426392	9.731290	-0.051731	4.818950
250.507318	8000.232167	9.736295	-0.051694	4.818892
250.294806	8000.358341	9.741299	-0.051655	4.818931
250.345003	8000.277265	9.746304	-0.051664	4.818906
250.311407	7999.885052	9.751309	-0.051657	4.818790
249.608270	7999.848954	9.756314	-0.051526	4.818782
249.574937	7999.883105	9.761319	-0.051520	4.818792
249.641706	7999.753007	9.766323	-0.051533	4.818753
249.556143	7999.844115	9.771328	-0.051517	4.818780
249.739905	7999.768916	9.776333	-0.051551	4.818757
249.705393	7999.967517	9.781338	-0.051545	4.818817
250.158909	7999.970097	9.786343	-0.051629	4.818816
249.952410	8000.025111	9.791347	-0.051591	4.818833
249.654420	7999.827560	9.796352	-0.051535	4.818775
249.572861	7999.867389	9.801357	-0.051520	4.818787
249.884404	8000.080830	9.806362	-0.051578	4.818850
250.152695	7999.836993	9.811367	-0.051628	4.818776
249.718519	7999.873424	9.816371	-0.051548	4.818788
249.954084	7999.997913	9.821376	-0.051592	4.818825
250.633271	7999.970866	9.826381	-0.051718	4.818814
250.471622	8000.093491	9.831386	-0.051688	4.818851
250.104838	7999.887735	9.836391	-0.051620	4.818791
250.825926	8000.074921	9.841395	-0.051754	4.818844
250.350041	7999.917022	9.846400	-0.051665	4.818799
250.404930	7999.917717	9.851405	-0.051676	4.818799
250.503644	8000.091814	9.856410	-0.051694	4.818851
250.208514	7999.907912	9.861415	-0.051639	4.818797
250.439674	7999.943305	9.866419	-0.051682	4.818807
249.809687	7999.846322	9.871424	-0.051565	4.818780
250.540032	7999.956100	9.876429	-0.051701	4.818810
250.590430	8000.311869	9.881434	-0.051711	4.818916
250.854821	8000.209403	9.886439	-0.051760	4.818884
250.937842	8000.383308	9.891443	-0.051776	4.818936
251.269501	8000.500642	9.896448	-0.051837	4.818970
251.251561	8000.440704	9.901453	-0.051834	4.818952
250.676823	8000.284689	9.906458	-0.051727	4.818907
251.121184	8000.223256	9.911463	-0.051810	4.818887
251.100195	8000.226137	9.916467	-0.051806	4.818888
250.869300	8000.454745	9.921472	-0.051763	4.818957
250.921671	7999.954659	9.926477	-0.051773	4.818808
250.835103	8000.482604	9.931482	-0.051757	4.818966
251.069537	8000.091669	9.936487	-0.051800	4.818848
250.855807	8000.289065	9.941491	-0.051761	4.818908
250.478757	8000.029746	9.946496	-0.051690	4.818832
250.631934	8000.032729	9.951501	-0.051719	4.818832
251.033409	8000.270363	9.956506	-0.051794	4.818902
250.889527	7999.987796	9.961511	-0.051767	4.818818
250.962644	8000.289380	9.966515	-0.051781	4.818908
250.764375	8000.148598	9.971520	-0.051744	4.818866
250.680093	7999.993543	9.976525	-0.051728	4.818821
250.936498	7999.942307	9.981530	-0.051776	4.818804
250.502955	7999.939983	9.986535	-0.051695	4.818805
250.161128	7999.826729	9.991539	-0.051631	4.818773
250.583016	7999.928428	9.996544	-0.051710	4.818802
250.896964	8000.068577	10.001549	-0.051769	4.818842
250.791871	8000.230677	10.006554	-0.051749	4.818891
250.888066	8000.046471	10.011559	-0.051767	4.818836
250.880104	8000.054754	10.016563	-0.051766	4.818838
250.574914	7999.915769	10.021568	-0.051709	4.818798
250.699973	7999.756025	10.026573	-0.051732	4.818750
250.467374	7999.850517	10.031578	-0.051689	4.818779
250.410388	7999.838278	10.036583	-0.051678	4.818775
251.168958	8000.244887	10.041587	-0.051820	4.818894
251.009184	8000.153827	10.046592	-0.051790	4.818867
251.248684	8000.052093	10.051597	-0.051835	4.818836
251.172330	8000.333985	10.056602	-0.051821	4.818920
251.258161	8000.229263	10.061607	-0.051837	4.818889
251.087616	8000.229208	10.066611	-0.051805	4.818889
251.235967	8000.368320	10.071616	-0.051833	4.818930
251.574497	8000.438600	10.076621	-0.051896	4.818950
251.550908	8000.458209	10.081626	-0.051891	4.818956
251.198158	8000.052523	10.086631	-0.051825	4.818836
251.215375	8000.202550	10.091635	-0.051829	4.818881
251.237860	8000.232170	10.096640	-0.051833	4.818890
251.524510	7999.915226	10.101645	-0.051886	4.818794
251.333845	8000.229197	10.106650	-0.051851	4.818888
251.414207	8000.407262	10.111655	-0.051866	4.818941
251.463124	8000.325120	10.116659	-0.051875	4.818916
251.601708	8000.425350	10.121664	-0.051901	4.818946
251.248694	7999.982996	10.126669	-0.051835	4.818815
251.090089	8000.014520	10.131674	-0.051806	4.818825
250.915448	7999.889752	10.136679	-0.051773	4.818789
250.886305	7999.909292	10.141683	-0.051768	4.818795
251.072554	8000.380967	10.146688	-0.051803	4.818935
251.311813	8000.003711	10.151693	-0.051847	4.818821
251.115911	8000.197142	10.156698	-0.051811	4.818880
251.213348	7999.897716	10.161703	-0.051829	4.818790
251.029050	8000.002247	10.166707	-0.051795	4.818822
251.159971	8000.068852	10.171712	-0.051819	4.818841
251.181441	8000.193790	10.176717	-0.051823	4.818878
251.526432	8000.236911	10.181722	-0.051888	4.818890
251.402300	8000.224870	10.186727	-0.051864	4.818887
251.569922	8000.479466	10.191731	-0.051896	4.818962
251.284103	8000.299859	10.196736	-0.051843	4.818910
251.358133	8000.078704	10.201741	-0.051856	4.818843
251.321371	8000.471097	10.206746	-0.051850	4.818960
251.284027	8000.101869	10.211751	-0.051843	4.818851
251.325862	8000.104495	10.216755	-0.051850	4.818851
250.905645	8000.089766	10.221760	-0.051772	4.818848
251.070033	8000.018512	10.226765	-0.051803	4.818827
251.416502	8000.477551	10.231770	-0.051868	4.818962
251.645898	8000.073976	10.236775	-0.051910	4.818841
251.854115	8000.429657	10.241779	-0.051949	4.818946
251.607064	8000.453777	10.246784	-0.051903	4.818954
251.831778	8000.467095	10.251789	-0.051945	4.818957
251.560792	8000.451103	10.256794	-0.051895	4.818954
251.490394	8000.296216	10.261799	-0.051882	4.818908
251.376559	8000.044404	10.266803	-0.051860	4.818833
251.543990	8000.248708	10.271808	-0.051892	4.818893
251.379432	8000.087397	10.276813	-0.051861	4.818846
251.388208	8000.223700	10.281818	-0.051863	4.818886
251.555956	8000.045632	10.286823	-0.051894	4.818833
251.810115	8000.201795	10.291827	-0.051941	4.818878
251.440575	8000.087133	10.296832	-0.051872	4.818846
251.395695	7999.849814	10.301837	-0.051864	4.818775
251.331665	7999.964243	10.306842	-0.051852	4.818809
251.797199	8000.350406	10.311847	-0.051939	4.818923
251.811819	8000.456404	10.316851	-0.051942	4.818954
251.441855	8000.111259	10.321856	-0.051873	4.818853
251.874668	8000.018251	10.326861	-0.051953	4.818823
251.840409	8000.399155	10.331866	-0.051947	4.818937
252.074553	8000.555072	10.336871	-0.051991	4.818983
251.922435	8000.342577	10.341875	-0.051963	4.818920
251.910200	8000.508999	10.346880	-0.051961	4.818970
252.099299	8000.293483	10.351885	-0.051996	4.818905
251.989120	8000.194665	10.356890	-0.051975	4.818876
251.870695	8000.183744	10.361895	-0.051953	4.818873
251.707668	8000.295878	10.366899	-0.051923	4.818907
251.855165	8000.409841	10.371904	-0.051950	4.818940
252.196779	8000.541973	10.376909	-0.052014	4.818978
251.869406	8000.430979	10.381914	-0.051953	4.818946
251.891173	8000.373637	10.386919	-0.051957	4.818929
251.812166	8000.141118	10.391923	-0.051942	4.818860
251.646479	7999.838367	10.396928	-0.051911	4.818771
251.558892	7999.879169	10.401933	-0.051895	4.818783
251.825892	8000.206252	10.406938	-0.051945	4.818880
251.798327	7999.849721	10.411943	-0.051940	4.818773
251.806021	8000.115912	10.416947	-0.051942	4.818853
251.534594	8000.075822	10.421952	-0.051891	4.818842
252.055211	8000.420781	10.426957	-0.051988	4.818943
251.494366	8000.277508	10.431962	-0.051884	4.818902
251.314915	7999.880301	10.436967	-0.051850	4.818784
251.594875	7999.940406	10.441971	-0.051902	4.818801
251.660911	8000.341430	10.446976	-0.051915	4.818920
251.814983	8000.088808	10.451981	-0.051943	4.818845
252.032021	8000.513746	10.456986	-0.051984	4.818970
251.871911	8000.481344	10.461991	-0.051954	4.818961
251.453864	7999.891500	10.466995	-0.051876	4.818787
251.156763	7999.971560	10.472000	-0.051821	4.818812
251.976751	7999.978771	10.477005	-0.051974	4.818811
252.033868	8000.315780	10.482010	-0.051985	4.818911
251.920142	8000.077584	10.487015	-0.051963	4.818841
252.334584	8000.360444	10.492019	-0.052041	4.818924
252.209801	8000.249916	10.497024	-0.052017	4.818891
252.232200	8000.131820	10.502029	-0.052022	4.818856
252.412094	8000.450482	10.507034	-0.052055	4.818950
252.444475	8000.332510	10.512039	-0.052061	4.818915
252.265985	8000.551310	10.517043	-0.052028	4.818981
252.382046	8000.372585	10.522048	-0.052050	4.818927
252.341128	8000.275688	10.527053	-0.052042	4.818898
251.685297	8000.040074	10.532058	-0.051920	4.818831
251.770418	8000.003438	10.537063	-0.051936	4.818819
251.892498	8000.051077	10.542067	-0.051959	4.818833
252.065352	8000.248120	10.547072	-0.051991	4.818891
251.863562	8000.013004	10.552077	-0.051953	4.818822
252.054917	8000.245899	10.557082	-0.051989	4.818891
252.383924	8000.334917	10.562087	-0.052051	4.818916
252.152079	8000.198941	10.567091	-0.052007	4.818876
251.805145	7999.853043	10.572096	-0.051943	4.818774
252.071219	7999.786215	10.577101	-0.051992	4.818753
252.009627	7999.982389	10.582106	-0.051981	4.818812
252.180156	8000.012831	10.587111	-0.052013	4.818821
252.314355	8000.378056	10.592115	-0.052038	4.818929
252.022048	8000.158554	10.597120	-0.051983	4.818865
252.030204	7999.903043	10.602125	-0.051985	4.818788
251.785542	8000.045574	10.607130	-0.051939	4.818832
252.016377	8000.084110	10.612135	-0.051982	4.818842
252.015834	8000.158487	10.617139	-0.051982	4.818865
252.110387	8000.338829	10.622144	-0.052000	4.818918
252.170700	8000.002259	10.627149	-0.052011	4.818817
252.280797	8000.457276	10.632154	-0.052032	4.818953
252.429455	8000.336583	10.637159	-0.052060	4.818916
252.279991	8000.346222	10.642163	-0.052032	4.818920
252.016592	8000.093562	10.647168	-0.051983	4.818845
252.151861	7999.988416	10.652173	-0.052008	4.818813
252.330069	8000.332196	10.657178	-0.052041	4.818915
252.184195	8000.192069	10.662183	-0.052014	4.818874
252.064319	8000.296368	10.667187	-0.051992	4.818906
252.073064	8000.254576	10.672192	-0.051994	4.818893
251.863545	7999.959648	10.677197	-0.051954	4.818806
251.687364	7999.915523	10.682202	-0.051922	4.818793
251.053444	7999.819530	10.687207	-0.051804	4.818767
251.531254	7999.849656	10.692211	-0.051893	4.818774
251.183327	7999.787652	10.697216	-0.051828	4.818757
251.354406	7999.765719	10.702221	-0.051860	4.818750
251.499684	8000.056690	10.707226	-0.051887	4.818836
251.883842	7999.755644	10.712231	-0.051958	4.818745
252.084128	7999.959314	10.717235	-0.051996	4.818805
252.094575	8000.224496	10.722240	-0.051998	4.818884
252.303071	8000.148560	10.727245	-0.052037	4.818861
251.863667	8000.136728	10.732250	-0.051955	4.818859
252.117393	7999.997459	10.737255	-0.052002	4.818816
251.559907	7999.875189	10.742259	-0.051898	4.818782
251.897787	7999.966407	10.747264	-0.051961	4.818808
252.452104	8000.039409	10.752269	-0.052065	4.818827
252.405880	8000.530170	10.757274	-0.052056	4.818974
252.324768	7999.956092	10.762279	-0.052041	4.818803
252.292387	8000.219687	10.767283	-0.052035	4.818882
252.063556	7999.963276	10.772288	-0.051992	4.818806
252.560136	8000.267077	10.777293	-0.052085	4.818895
252.160417	8000.211743	10.782298	-0.052011	4.818880
251.892402	8000.028171	10.787303	-0.051961	4.818826
252.287106	8000.201825	10.792307	-0.052034	4.818876
252.366768	8000.340075	10.797312	-0.052049	4.818917
252.238789	7999.974935	10.802317	-0.052025	4.818809
252.090276	7999.930111	10.807322	-0.051998	4.818796
252.340942	7999.961564	10.812327	-0.052044	4.818805
252.168854	8000.065203	10.817331	-0.052012	4.818836
252.253050	8000.061031	10.822336	-0.052028	4.818835
252.512196	8000.094688	10.827341	-0.052077	4.818844
252.752402	8000.435067	10.832346	-0.052122	4.818944
252.289490	8000.141119	10.837351	-0.052035	4.818858
252.930982	8000.464570	10.842355	-0.052155	4.818952
252.498563	8000.365865	10.847360	-0.052074	4.818925
252.880400	8000.533082	10.852365	-0.052146	4.818973
252.291489	8000.264776	10.857370	-0.052036	4.818895
252.267730	8000.115716	10.862375	-0.052031	4.818851
252.120457	8000.031097	10.867379	-0.052004	4.818826
252.340574	8000.280072	10.872384	-0.052045	4.818900
252.358367	8000.280300	10.877389	-0.052048	4.818900
252.232883	8000.205383	10.882394	-0.052025	4.818878
252.189867	8000.131509	10.887399	-0.052017	4.818856
252.047319	8000.081521	10.892403	-0.051991	4.818842
252.522472	8000.421722	10.897408	-0.052079	4.818941
252.427726	8000.060141	10.902413	-0.052061	4.818834
252.153631	8000.161444	10.907418	-0.052010	4.818865
252.532284	8000.137944	10.912423	-0.052081	4.818856
252.233105	8000.055596	10.917427	-0.052025	4.818833
251.964788	7999.845833	10.922432	-0.051975	4.818772
252.340868	8000.048582	10.927437	-0.052045	4.818831
252.848457	8000.447864	10.932442	-0.052140	4.818948
252.943481	8000.471069	10.937447	-0.052158	4.818954
253.030411	8000.351690	10.942451	-0.052174	4.818918
252.795447	8000.455584	10.947456	-0.052131	4.818950
252.804812	8000.027218	10.952461	-0.052132	4.818822
252.482951	8000.182395	10.957466	-0.052072	4.818870
252.584376	8000.165870	10.962471	-0.052091	4.818865
252.436613	8000.348390	10.967475	-0.052064	4.818920
252.305813	8000.100547	10.972480	-0.052039	4.818846
252.302254	8000.026123	10.977485	-0.052039	4.818824
252.178668	8000.329425	10.982490	-0.052016	4.818915
252.706371	8000.446100	10.987495	-0.052114	4.818948
252.582200	8000.160622	10.992499	-0.052091	4.818863
252.752561	8000.448785	10.997504	-0.052123	4.818948
252.932954	8000.220584	11.002509	-0.052156	4.818880
252.479083	8000.217995	11.007514	-0.052072	4.818881
252.797873	8000.044975	11.012519	-0.052131	4.818828
252.954814	8000.454496	11.017523	-0.052161	4.818949
252.722623	8000.409658	11.022528	-0.052118	4.818937
252.628526	8000.124560	11.027533	-0.052100	4.818852
252.712225	8000.442009	11.032538	-0.052116	4.818946
253.168936	7999.973200	11.037543	-0.052201	4.818805
252.934285	8000.114812	11.042547	-0.052157	4.818848
252.873632	8000.207289	11.047552	-0.052146	4.818876
253.019095	8000.101223	11.052557	-0.052173	4.818844
252.572051	8000.266343	11.057562	-0.052090	4.818895
252.644106	8000.010586	11.062567	-0.052103	4.818818
252.474857	8000.134166	11.067571	-0.052072	4.818856
252.345904	8000.062349	11.072576	-0.052048	4.818835
252.554761	8000.122610	11.077581	-0.052087	4.818852
252.746882	8000.383808	11.082586	-0.052123	4.818929
252.744211	8000.122914	11.087591	-0.052122	4.818851
252.984711	8000.027477	11.092595	-0.052167	4.818822
252.936114	8000.245823	11.097600	-0.052158	4.818887
253.193350	8000.046881	11.102605	-0.052206	4.818827
252.792160	8000.030292	11.107610	-0.052131	4.818823
253.083344	8000.251883	11.112615	-0.052185	4.818888
253.315202	8000.574356	11.117619	-0.052229	4.818984
253.130645	8000.318489	11.122624	-0.052194	4.818908
253.065926	8000.075667	11.127629	-0.052182	4.818836
252.971701	8000.448491	11.132634	-0.052165	4.818947
252.761288	8000.094872	11.137639	-0.052126	4.818843
252.876820	8000.419010	11.142643	-0.052147	4.818939
252.733826	8000.354346	11.147648	-0.052121	4.818920
253.049564	8000.057665	11.152653	-0.052179	4.818831
252.840341	8000.426939	11.157658	-0.052141	4.818941
252.977789	8000.387821	11.162663	-0.052166	4.818929
253.282823	8000.544640	11.167667	-0.052223	4.818975
253.185271	8000.460644	11.172672	-0.052205	4.818950
253.222187	8000.379395	11.177677	-0.052212	4.818926
253.334119	8000.407005	11.182682	-0.052233	4.818934
253.323880	8000.542028	11.187687	-0.052231	4.818974
253.254437	8000.481436	11.192691	-0.052218	4.818956
253.187180	8000.499446	11.197696	-0.052206	4.818962
253.249824	8000.462525	11.202701	-0.052217	4.818950
253.186043	8000.460674	11.207706	-0.052205	4.818950
253.083025	8000.389180	11.212711	-0.052186	4.818929
252.950663	8000.423130	11.217715	-0.052162	4.818940
252.871969	8000.378137	11.222720	-0.052147	4.818927
253.017512	8000.249023	11.227725	-0.052174	4.818888
253.009492	8000.266734	11.232730	-0.052173	4.818893
253.026490	8000.404195	11.237735	-0.052176	4.818934
252.857374	8000.197768	11.242739	-0.052144	4.818873
253.238926	8000.499082	11.247744	-0.052216	4.818961
253.219215	8000.488359	11.252749	-0.052212	4.818958
253.083362	8000.539027	11.257754	-0.052187	4.818974
252.770504	8000.457547	11.262759	-0.052129	4.818951
253.062048	8000.433997	11.267763	-0.052183	4.818943
253.070353	8000.562968	11.272768	-0.052185	4.818981
253.296434	8000.380392	11.277773	-0.052227	4.818926
253.206991	8000.539558	11.282778	-0.052210	4.818974
253.195017	8000.279588	11.287783	-0.052208	4.818896
253.168896	8000.423838	11.292787	-0.052203	4.818939
252.999448	8000.387126	11.297792	-0.052171	4.818929
253.331025	8000.460467	11.302797	-0.052233	4.818950
253.132810	8000.394056	11.307802	-0.052196	4.818930
253.248822	8000.416479	11.312807	-0.052218	4.818937
252.912885	8000.035082	11.317811	-0.052155	4.818824
253.194021	8000.260738	11.322816	-0.052208	4.818891
253.292932	8000.356281	11.327821	-0.052226	4.818919
252.596981	8000.161006	11.332826	-0.052097	4.818863
253.082358	8000.199619	11.337831	-0.052187	4.818873
253.317697	8000.411081	11.342835	-0.052231	4.818935
253.256299	8000.289827	11.347840	-0.052220	4.818899
252.597204	7999.946257	11.352845	-0.052097	4.818799
253.048623	8000.143679	11.357850	-0.052181	4.818856
252.881920	8000.026336	11.362855	-0.052150	4.818822
253.297081	8000.051489	11.367859	-0.052227	4.818828
253.293923	8000.558520	11.372864	-0.052227	4.818979
252.943898	8000.048080	11.377869	-0.052162	4.818828
252.409574	7999.977429	11.382874	-0.052062	4.818809
252.674425	7999.930490	11.387879	-0.052111	4.818794
252.477378	8000.009719	11.392883	-0.052075	4.818818
252.248187	7999.998447	11.397888	-0.052032	4.818816
251.972520	7999.897542	11.402893	-0.051981	4.818787
252.169509	7999.726130	11.407898	-0.052017	4.818735
252.532199	7999.989471	11.412903	-0.052085	4.818812
252.628585	7999.960310	11.417907	-0.052103	4.818803
252.568668	8000.186892	11.422912	-0.052092	4.818871
252.736157	7999.948055	11.427917	-0.052123	4.818799
252.478975	7999.910239	11.432922	-0.052075	4.818789
252.417654	8000.028896	11.437927	-0.052064	4.818824
252.546223	7999.959284	11.442931	-0.052088	4.818803
252.551771	8000.321838	11.447936	-0.052089	4.818911
252.607906	7999.913974	11.452941	-0.052100	4.818789
252.981447	8000.512711	11.457946	-0.052170	4.818966
252.968939	8000.270546	11.462951	-0.052167	4.818894
253.123871	8000.116408	11.467955	-0.052196	4.818848
252.771807	8000.083676	11.472960	-0.052130	4.818839
252.623333	8000.012660	11.477965	-0.052103	4.818819
252.610220	8000.093165	11.482970	-0.052100	4.818843
253.023451	8000.138199	11.487975	-0.052177	4.818855
252.465457	8000.033722	11.492979	-0.052073	4.818826
252.400317	8000.173284	11.497984	-0.052061	4.818867
252.559648	7999.847394	11.502989	-0.052091	4.818770
252.619285	7999.891102	11.507994	-0.052102	4.818783
252.681688	8000.042751	11.512999	-0.052114	4.818827
252.755725	8000.014355	11.518003	-0.052128	4.818819
252.766804	8000.114023	11.523008	-0.052130	4.818848
252.481837	7999.855854	11.528013	-0.052077	4.818773
252.784282	8000.026249	11.533018	-0.052133	4.818822
252.691337	7999.831267	11.538023	-0.052116	4.818764
252.387729	7999.838961	11.543027	-0.052059	4.818768
251.610944	7999.827064	11.548032	-0.051915	4.818767
252.152281	7999.903041	11.553037	-0.052016	4.818788
252.428619	7999.912819	11.558042	-0.052067	4.818790
252.290089	7999.897454	11.563047	-0.052041	4.818786
253.066449	7999.929261	11.568051	-0.052186	4.818792
252.963781	8000.094541	11.573056	-0.052167	4.818842
252.885084	7999.953166	11.578061	-0.052152	4.818800
252.607399	8000.054425	11.583066	-0.052101	4.818831
252.571166	8000.048732	11.588071	-0.052094	4.818830
252.544313	7999.855633	11.593075	-0.052089	4.818772
252.398825	7999.874752	11.598080	-0.052062	4.818778
252.160233	7999.802601	11.603085	-0.052017	4.818758
252.613886	7999.840806	11.608090	-0.052102	4.818768
252.679438	7999.863637	11.613095	-0.052114	4.818774
252.276688	7999.903602	11.618099	-0.052039	4.818787
251.966748	7999.804360	11.623104	-0.051982	4.818759
252.189153	7999.818694	11.628109	-0.052023	4.818763
251.568750	7999.865342	11.633114	-0.051908	4.818779
252.142765	7999.871542	11.638119	-0.052015	4.818778
252.333202	7999.775474	11.643123	-0.052050	4.818749
252.591943	7999.842648	11.648128	-0.052098	4.818768
252.626013	7999.862986	11.653133	-0.052105	4.818774
252.255642	7999.843646	11.658138	-0.052036	4.818770
252.621699	7999.818937	11.663143	-0.052104	4.818761
252.870879	7999.848277	11.668147	-0.052150	4.818769
252.465579	7999.928019	11.673152	-0.052075	4.818794
252.284890	7999.861836	11.678157	-0.052041	4.818775
252.425628	7999.825902	11.683162	-0.052068	4.818764
252.779589	7999.911041	11.688167	-0.052134	4.818788
252.617661	8000.046237	11.693171	-0.052104	4.818829
252.281320	7999.870183	11.698176	-0.052041	4.818778
252.453698	7999.806363	11.703181	-0.052073	4.818758
252.429391	7999.941201	11.708186	-0.052069	4.818798
252.806780	7999.874732	11.713191	-0.052139	4.818777
252.219843	7999.828562	11.718195	-0.052030	4.818765
252.245454	7999.780699	11.723200	-0.052034	4.818751
251.856662	7999.852269	11.728205	-0.051962	4.818774
252.159018	7999.875993	11.733210	-0.052018	4.818780
252.007465	7999.816465	11.738215	-0.051990	4.818763
252.204418	7999.789621	11.743219	-0.052027	4.818754
252.325728	7999.840393	11.748224	-0.052050	4.818768
251.959512	7999.936342	11.753229	-0.051981	4.818798
252.345403	7999.813409	11.758234	-0.052053	4.818760
252.754889	7999.865725	11.763239	-0.052130	4.818774
252.597345	7999.871071	11.768243	-0.052100	4.818777
252.029906	7999.830387	11.773248	-0.051995	4.818767
252.520492	7999.840774	11.778253	-0.052086	4.818768
252.165158	7999.828957	11.783258	-0.052020	4.818766
252.070630	7999.839291	11.788263	-0.052002	4.818769
252.398942	7999.842391	11.793267	-0.052064	4.818769
252.592882	7999.853223	11.798272	-0.052100	4.818771
252.614110	7999.890161	11.803277	-0.052104	4.818782
252.418231	7999.934833	11.808282	-0.052067	4.818796
252.601811	7999.769536	11.813287	-0.052101	4.818746
252.333618	7999.876152	11.818291	-0.052052	4.818779
252.042827	7999.874579	11.823296	-0.051998	4.818780
252.312772	7999.772181	11.828301	-0.052048	4.818748
252.475251	7999.856996	11.833306	-0.052078	4.818773
252.503684	7999.856311	11.838311	-0.052083	4.818773
252.644090	7999.795229	11.843315	-0.052110	4.818754
252.450587	7999.879741	11.848320	-0.052074	4.818780
252.352343	7999.784219	11.853325	-0.052055	4.818752
252.492586	7999.844658	11.858330	-0.052082	4.818769
252.233870	7999.765968	11.863335	-0.052033	4.818747
252.103523	7999.882704	11.868339	-0.052009	4.818782
251.858803	7999.787430	11.873344	-0.051964	4.818754
252.215008	7999.800309	11.878349	-0.052030	4.818757
251.962351	7999.817027	11.883354	-0.051983	4.818763
251.944114	7999.894322	11.888359	-0.051980	4.818786
252.213815	7999.794017	11.893363	-0.052030	4.818755
252.401535	7999.852961	11.898368	-0.052065	4.818772
252.158952	7999.813235	11.903373	-0.052020	4.818761
251.823492	7999.819480	11.908378	-0.051957	4.818764
252.039700	7999.830592	11.913383	-0.051998	4.818767
252.246813	7999.790258	11.918387	-0.052036	4.818754
252.602540	8000.059799	11.923392	-0.052103	4.818833
252.503393	7999.810264	11.928397	-0.052084	4.818759
252.269762	7999.825127	11.933402	-0.052041	4.818764
252.469635	7999.899939	11.938407	-0.052078	4.818786
252.054476	7999.854891	11.943411	-0.052001	4.818774
251.919252	7999.912900	11.948416	-0.051976	4.818792
252.381360	7999.796167	11.953421	-0.052062	4.818755
252.316982	7999.777548	11.958426	-0.052050	4.818750
252.818353	7999.939976	11.963431	-0.052143	4.818796
252.604434	7999.951944	11.968435	-0.052103	4.818801
252.897586	7999.970316	11.973440	-0.052158	4.818805
252.983146	7999.988162	11.978445	-0.052174	4.818810
252.669091	8000.076389	11.983450	-0.052116	4.818837
252.346223	7999.800982	11.988455	-0.052055	4.818757
252.654200	7999.925349	11.993459	-0.052113	4.818792
252.967744	7999.978551	11.998464	-0.052171	4.818807
252.820817	8000.072032	12.003469	-0.052144	4.818836
252.774228	7999.858778	12.008474	-0.052135	4.818772
252.981275	7999.934730	12.013479	-0.052174	4.818794
252.920975	7999.888923	12.018483	-0.052163	4.818781
252.401442	7999.776557	12.023488	-0.052066	4.818749
252.430103	7999.823016	12.028493	-0.052071	4.818763
252.770239	7999.905885	12.033498	-0.052135	4.818786
252.761784	7999.860734	12.038503	-0.052133	4.818773
253.076243	7999.891946	12.043507	-0.052192	4.818781
253.037272	8000.002506	12.048512	-0.052185	4.818814
252.894900	7999.849852	12.053517	-0.052158	4.818769
252.498254	7999.852180	12.058522	-0.052084	4.818771
252.656886	7999.786090	12.063527	-0.052114	4.818751
252.960744	7999.927169	12.068531	-0.052171	4.818792
252.681943	7999.853460	12.073536	-0.052119	4.818771
252.693506	7999.919609	12.078541	-0.052121	4.818791
252.859240	7999.785514	12.083546	-0.052152	4.818750
252.350706	7999.786430	12.088551	-0.052057	4.818752
252.165849	7999.773624	12.093555	-0.052023	4.818749
252.858072	7999.966747	12.098560	-0.052152	4.818804
252.811992	7999.952549	12.103565	-0.052143	4.818800
252.456146	7999.892534	12.108570	-0.052077	4.818783
252.561499	7999.868724	12.113575	-0.052097	4.818776
252.896585	7999.920102	12.118579	-0.052159	4.818790
252.743466	7999.941219	12.123584	-0.052131	4.818797
252.849146	7999.824175	12.128589	-0.052150	4.818762
252.703636	7999.954341	12.133594	-0.052123	4.818801
252.796990	7999.863332	12.138599	-0.052141	4.818773
252.878774	7999.837129	12.143603	-0.052156	4.818765
252.912918	7999.843849	12.148608	-0.052162	4.818767
253.271441	7999.875618	12.153613	-0.052229	4.818775
253.234524	7999.975728	12.158618	-0.052222	4.818805
252.886495	7999.965049	12.163623	-0.052158	4.818803
253.079397	7999.853296	12.168627	-0.052193	4.818769
253.406468	8000.083722	12.173632	-0.052255	4.818837
253.438616	8000.009748	12.178637	-0.052261	4.818815
253.239922	7999.878381	12.183642	-0.052224	4.818776
253.339042	7999.981257	12.188647	-0.052242	4.818807
253.288369	7999.947095	12.193651	-0.052233	4.818797
253.564256	8000.309930	12.198656	-0.052284	4.818904
253.625144	8000.310703	12.203661	-0.052296	4.818904
253.294508	8000.211188	12.208666	-0.052234	4.818875
253.269542	8000.032775	12.213671	-0.052229	4.818822
253.398970	7999.934887	12.218675	-0.052253	4.818792
253.164596	8000.132029	12.223680	-0.052210	4.818852
253.288623	7999.825593	12.228685	-0.052233	4.818760
253.306738	8000.183071	12.233690	-0.052237	4.818867
253.729747	7999.956888	12.238695	-0.052315	4.818798
253.693754	7999.957484	12.243699	-0.052309	4.818798
253.531437	7999.994199	12.248704	-0.052278	4.818810
253.727621	8000.089923	12.253709	-0.052315	4.818837
253.384791	8000.121213	12.258714	-0.052251	4.818848
253.294700	8000.016360	12.263719	-0.052234	4.818817
253.621591	8000.133640	12.268723	-0.052295	4.818851
253.528610	8000.165993	12.273728	-0.052278	4.818861
253.522651	8000.021344	12.278733	-0.052277	4.818818
253.352270	8000.078910	12.283738	-0.052245	4.818836
253.471943	8000.110807	12.288743	-0.052268	4.818845
253.426669	7999.911185	12.293747	-0.052259	4.818785
253.284687	7999.924061	12.298752	-0.052233	4.818790
253.477527	7999.994597	12.303757	-0.052269	4.818810
253.163899	8000.133117	12.308762	-0.052211	4.818852
253.060388	7999.760950	12.313767	-0.052191	4.818742
253.329523	8000.054547	12.318771	-0.052241	4.818828
253.008969	7999.799068	12.323776	-0.052182	4.818753
253.049931	7999.841493	12.328781	-0.052189	4.818766
253.583002	8000.018996	12.333786	-0.052289	4.818817
253.512413	7999.866198	12.338791	-0.052276	4.818772
253.594218	8000.021239	12.343795	-0.052291	4.818817
253.445534	7999.995267	12.348800	-0.052263	4.818810
253.538850	7999.952448	12.353805	-0.052281	4.818797
253.948830	8000.424893	12.358810	-0.052357	4.818936
254.112074	8000.321145	12.363815	-0.052388	4.818905
254.216230	8000.452379	12.368819	-0.052407	4.818944
253.967691	8000.542482	12.373824	-0.052361	4.818971
253.851792	8000.266525	12.378829	-0.052339	4.818890
253.912149	8000.381489	12.383834	-0.052351	4.818924
253.951618	8000.476283	12.388839	-0.052358	4.818952
253.846262	8000.481239	12.393843	-0.052339	4.818954
253.326459	8000.258847	12.398848	-0.052242	4.818889
253.369936	7999.994344	12.403853	-0.052250	4.818810
253.718238	8000.319333	12.408858	-0.052315	4.818906
253.366866	8000.081266	12.413863	-0.052249	4.818836
253.182349	8000.016078	12.418867	-0.052215	4.818817
253.485782	7999.926675	12.423872	-0.052271	4.818790
253.705175	8000.045739	12.428877	-0.052312	4.818824
253.768019	8000.288547	12.433882	-0.052324	4.818896
253.852600	8000.189043	12.438887	-0.052340	4.818866
254.063259	8000.370863	12.443891	-0.052379	4.818920
253.230298	7999.933938	12.448896	-0.052224	4.818793
253.322521	7999.874343	12.453901	-0.052241	4.818775
253.599404	8000.237189	12.458906	-0.052293	4.818882
253.529584	7999.947157	12.463911	-0.052280	4.818796
253.394990	7999.862695	12.468915	-0.052255	4.818771
253.372319	7999.896984	12.473920	-0.052251	4.818781
253.995950	7999.979250	12.478925	-0.052367	4.818803
253.878227	8000.418834	12.483930	-0.052345	4.818935
253.622920	8000.181978	12.488935	-0.052298	4.818865
253.683462	8000.057027	12.493939	-0.052309	4.818828
253.772473	8000.301213	12.498944	-0.052326	4.818900
253.616982	8000.026858	12.503949	-0.052297	4.818819
253.437505	7999.943924	12.508954	-0.052263	4.818795
253.344225	7999.927034	12.513959	-0.052246	4.818790
253.759181	8000.213052	12.518963	-0.052323	4.818874
253.625771	8000.052124	12.523968	-0.052298	4.818827
253.876438	7999.888718	12.528973	-0.052345	4.818777
253.377699	7999.845753	12.533978	-0.052252	4.818766
253.437987	8000.047665	12.538983	-0.052264	4.818826
253.467310	7999.882510	12.543987	-0.052269	4.818777
253.554374	7999.956948	12.548992	-0.052285	4.818798
253.368527	7999.920031	12.553997	-0.052251	4.818788
253.467639	8000.010336	12.559002	-0.052269	4.818815
253.662958	8000.151098	12.564007	-0.052306	4.818856
253.762679	8000.172267	12.569011	-0.052324	4.818862
253.691592	8000.109559	12.574016	-0.052311	4.818843
253.601442	8000.208998	12.579021	-0.052294	4.818873
253.181848	8000.113599	12.584026	-0.052216	4.818847
253.701201	8000.228075	12.589031	-0.052313	4.818879
253.831718	8000.387927	12.594035	-0.052338	4.818926
253.685428	8000.194356	12.599040	-0.052310	4.818869
253.521528	7999.964946	12.604045	-0.052280	4.818801
253.671388	8000.174279	12.609050	-0.052308	4.818863
253.658983	8000.059930	12.614055	-0.052305	4.818829
253.826167	7999.953090	12.619059	-0.052336	4.818796
253.688530	8000.169266	12.624064	-0.052311	4.818861
254.038498	8000.309892	12.629069	-0.052376	4.818902
253.645633	8000.212731	12.634074	-0.052303	4.818874
253.642612	8000.276604	12.639079	-0.052303	4.818893
253.668535	7999.989876	12.644083	-0.052307	4.818808
253.627759	7999.987268	12.649088	-0.052300	4.818807
253.747390	8000.016022	12.654093	-0.052322	4.818815
253.347253	7999.968015	12.659098	-0.052248	4.818802
253.563388	7999.902651	12.664103	-0.052288	4.818782
253.609125	8000.040474	12.669107	-0.052297	4.818823
253.590365	8000.132434	12.674112	-0.052293	4.818851
253.677801	7999.973251	12.679117	-0.052309	4.818803
253.479070	8000.054554	12.684122	-0.052272	4.818828
253.305383	7999.874263	12.689127	-0.052240	4.818775
253.779995	7999.979789	12.694131	-0.052329	4.818804
253.128659	7999.904513	12.699136	-0.052207	4.818784
253.501735	7999.872562	12.704141	-0.052277	4.818773
253.491684	8000.275784	12.709146	-0.052275	4.818894
253.558998	8000.079678	12.714151	-0.052288	4.818835
253.268965	7999.996394	12.719155	-0.052234	4.818811
253.716196	8000.335206	12.724160	-0.052317	4.818911
253.861469	7999.931599	12.729165	-0.052344	4.818790
253.606329	8000.245818	12.734170	-0.052297	4.818884
253.951648	7999.948460	12.739175	-0.052361	4.818794
253.678608	8000.047682	12.744179	-0.052310	4.818825
253.883425	7999.982176	12.749184	-0.052348	4.818805
253.589439	8000.085324	12.754189	-0.052294	4.818837
253.323885	7999.849394	12.759194	-0.052244	4.818767
253.567649	7999.861905	12.764199	-0.052289	4.818770
253.543194	7999.866838	12.769203	-0.052285	4.818772
253.650391	7999.975055	12.774208	-0.052305	4.818803
254.014562	7999.860227	12.779213	-0.052373	4.818768
254.110127	8000.267933	12.784218	-0.052391	4.818889
253.962774	8000.221022	12.789223	-0.052364	4.818876
254.006428	8000.123096	12.794227	-0.052372	4.818846
253.696669	8000.458629	12.799232	-0.052314	4.818947
254.117599	8000.354997	12.804237	-0.052393	4.818915
253.807831	8000.363654	12.809242	-0.052335	4.818919
253.701622	7999.946391	12.814247	-0.052315	4.818795
253.639944	7999.949805	12.819251	-0.052303	4.818796
253.744235	7999.975222	12.824256	-0.052323	4.818803
253.798722	7999.903626	12.829261	-0.052333	4.818782
253.278689	7999.919059	12.834266	-0.052236	4.818788
252.862750	7999.804855	12.839271	-0.052159	4.818756
253.296712	7999.862720	12.844275	-0.052240	4.818771
253.356911	7999.865578	12.849280	-0.052251	4.818772
253.185090	7999.765982	12.854285	-0.052219	4.818743
253.293456	7999.892021	12.859290	-0.052239	4.818780
253.316578	7999.896507	12.864295	-0.052244	4.818781
253.224813	7999.761254	12.869299	-0.052226	4.818741
252.772707	7999.852976	12.874304	-0.052142	4.818770
253.463481	7999.778941	12.879309	-0.052271	4.818746
253.541465	7999.999934	12.884314	-0.052286	4.818811
253.049431	7999.777908	12.889319	-0.052194	4.818747
252.895140	7999.789581	12.894323	-0.052165	4.818751
252.702790	7999.874108	12.899328	-0.052130	4.818777
253.072142	7999.783441	12.904333	-0.052198	4.818748
253.132679	7999.847067	12.909338	-0.052210	4.818767
253.295079	7999.827120	12.914343	-0.052240	4.818761
253.522158	7999.778658	12.919347	-0.052282	4.818745
254.052374	8000.225377	12.924352	-0.052381	4.818876
253.755692	7999.848663	12.929357	-0.052326	4.818765
253.615797	7999.953758	12.934362	-0.052300	4.818797
253.971834	8000.119600	12.939367	-0.052366	4.818845
253.910723	7999.938633	12.944371	-0.052355	4.818792
253.899982	8000.119745	12.949376	-0.052353	4.818846
253.494172	8000.023473	12.954381	-0.052278	4.818818
253.282169	7999.944319	12.959386	-0.052238	4.818796
253.344065	7999.859197	12.964391	-0.052250	4.818770
253.670314	7999.897894	12.969395	-0.052310	4.818780
253.370918	7999.974783	12.974400	-0.052255	4.818804
253.671490	7999.916772	12.979405	-0.052311	4.818786
253.270356	7999.854087	12.984410	-0.052236	4.818769
253.202305	7999.949613	12.989415	-0.052223	4.818797
253.566528	7999.827453	12.994419	-0.052291	4.818760
253.392819	7999.975074	12.999424	-0.052259	4.818804
253.408819	7999.799276	13.004429	-0.052262	4.818752
253.292602	7999.943432	13.009434	-0.052240	4.818795
253.578187	7999.751134	13.014439	-0.052294	4.818737
253.138360	7999.897489	13.019443	-0.052212	4.818782
253.044764	7999.798880	13.024448	-0.052194	4.818753
253.135820	7999.810509	13.029453	-0.052211	4.818756
253.002513	7999.874829	13.034458	-0.052187	4.818776
252.814901	7999.810653	13.039463	-0.052152	4.818758
253.506241	7999.956628	13.044467	-0.052281	4.818798
252.943257	7999.780851	13.049472	-0.052176	4.818748
252.751963	7999.877962	13.054477	-0.052140	4.818778
253.184041	7999.860374	13.059482	-0.052221	4.818771
252.917338	7999.877961	13.064487	-0.052171	4.818777
252.986707	7999.843221	13.069491	-0.052184	4.818767
253.145631	7999.880850	13.074496	-0.052214	4.818777
253.587144	7999.877002	13.079501	-0.052296	4.818774
253.617960	8000.116259	13.084506	-0.052302	4.818846
253.055453	7999.811624	13.089511	-0.052197	4.818757
252.913692	7999.873742	13.094515	-0.052171	4.818776
252.820098	7999.811801	13.099520	-0.052153	4.818758
253.136962	7999.814758	13.104525	-0.052212	4.818758
253.198155	7999.848010	13.109530	-0.052224	4.818767
252.799408	7999.881739	13.114535	-0.052149	4.818779
253.276222	7999.792430	13.119539	-0.052238	4.818750
253.692808	8000.016653	13.124544	-0.052316	4.818816
253.707629	7999.952936	13.129549	-0.052319	4.818797
253.609524	7999.922366	13.134554	-0.052301	4.818788
253.866448	7999.909900	13.139559	-0.052348	4.818783
253.547180	7999.953013	13.144563	-0.052289	4.818797
253.791634	7999.940390	13.149568	-0.052335	4.818792
253.652401	7999.766820	13.154573	-0.052309	4.818741
253.659990	7999.897874	13.159578	-0.052310	4.818780
253.584811	7999.866546	13.164583	-0.052296	4.818771
254.058380	7999.985679	13.169587	-0.052384	4.818805
253.798192	8000.192974	13.174592	-0.052336	4.818868
253.604605	7999.942235	13.179597	-0.052300	4.818794
253.926914	8000.058410	13.184602	-0.052360	4.818827
253.332974	7999.849759	13.189607	-0.052249	4.818767
253.629545	7999.984465	13.194611	-0.052305	4.818806
253.601750	7999.963163	13.199616	-0.052300	4.818800
253.445622	7999.781000	13.204621	-0.052270	4.818746
253.007776	7999.878140	13.209626	-0.052189	4.818777
253.158567	7999.814047	13.214631	-0.052217	4.818757
252.897942	7999.831711	13.219635	-0.052169	4.818763
252.807791	7999.766670	13.224640	-0.052152	4.818744
252.960124	7999.950884	13.229645	-0.052180	4.818799
253.338761	7999.961956	13.234650	-0.052251	4.818801
253.175382	7999.845703	13.239655	-0.052221	4.818767
253.322604	7999.850708	13.244659	-0.052248	4.818768
253.224432	7999.869376	13.249664	-0.052230	4.818773
253.361250	7999.867964	13.254669	-0.052255	4.818773
253.471003	7999.867258	13.259674	-0.052276	4.818772
253.648024	7999.951214	13.264679	-0.052309	4.818796
253.436313	7999.908732	13.269683	-0.052269	4.818784
253.155641	7999.793092	13.274688	-0.052217	4.818751
253.398572	7999.841212	13.279693	-0.052262	4.818764
253.262256	7999.844731	13.284698	-0.052237	4.818766
252.961427	7999.829410	13.289703	-0.052181	4.818763
252.944199	7999.835481	13.294707	-0.052178	4.818764
252.996985	7999.897961	13.299712	-0.052188	4.818783
253.154988	7999.824530	13.304717	-0.052217	4.818760
253.208239	7999.851397	13.309722	-0.052227	4.818768
253.394082	7999.780413	13.314727	-0.052262	4.818746
253.447997	7999.886908	13.319731	-0.052272	4.818778
253.275115	7999.768439	13.324736	-0.052240	4.818743
252.903757	7999.866420	13.329741	-0.052171	4.818774
253.417563	7999.859293	13.334746	-0.052266	4.818770
253.477909	7999.767867	13.339751	-0.052278	4.818742
253.489022	7999.872774	13.344755	-0.052280	4.818773
253.008251	7999.778703	13.349760	-0.052190	4.818747
253.160427	7999.813104	13.354765	-0.052219	4.818757
252.964202	7999.881867	13.359770	-0.052182	4.818778
253.772792	7999.814560	13.364775	-0.052333	4.818755
253.773660	7999.890004	13.369779	-0.052333	4.818778
253.960239	8000.102944	13.374784	-0.052368	4.818840
254.083812	7999.993457	13.379789	-0.052391	4.818807
254.197880	8000.466358	13.384794	-0.052413	4.818948
254.289253	8000.297791	13.389799	-0.052430	4.818897
254.114660	8000.166721	13.394803	-0.052397	4.818859
254.016564	8000.051288	13.399808	-0.052379	4.818825
254.084425	7999.975669	13.404813	-0.052391	4.818802
253.973587	8000.282285	13.409818	-0.052371	4.818894
253.957355	7999.943686	13.414823	-0.052368	4.818793
254.210774	8000.214049	13.419827	-0.052415	4.818872
254.099212	8000.398081	13.424832	-0.052394	4.818928
254.024250	8000.214839	13.429837	-0.052380	4.818873
254.065945	8000.197558	13.434842	-0.052388	4.818868
254.201595	8000.178323	13.439847	-0.052414	4.818862
254.222405	8000.080108	13.444851	-0.052417	4.818832
253.721887	8000.126166	13.449856	-0.052324	4.818848
254.196056	7999.901677	13.454861	-0.052412	4.818779
254.160393	8000.272105	13.459866	-0.052406	4.818890
254.008955	8000.097326	13.464871	-0.052378	4.818838
253.894386	7999.950256	13.469875	-0.052356	4.818795
254.084200	8000.144381	13.474880	-0.052392	4.818852
253.982229	8000.275102	13.479885	-0.052373	4.818891
253.936294	8000.144612	13.484890	-0.052364	4.818853
253.838229	8000.042800	13.489895	-0.052346	4.818823
253.967952	8000.099969	13.494899	-0.052370	4.818839
254.036972	8000.471723	13.499904	-0.052384	4.818950
253.949714	7999.991835	13.504909	-0.052367	4.818807
253.895663	8000.241547	13.509914	-0.052357	4.818882
254.029543	8000.136380	13.514919	-0.052382	4.818850
254.027527	8000.077688	13.519923	-0.052382	4.818832
253.682775	7999.976948	13.524928	-0.052318	4.818804
253.836311	7999.989368	13.529933	-0.052346	4.818807
254.374074	8000.413147	13.534938	-0.052447	4.818931
254.611307	8000.435010	13.539943	-0.052491	4.818937
254.227356	8000.014225	13.544947	-0.052419	4.818813
254.134675	8000.110490	13.549952	-0.052402	4.818842
254.295341	8000.226721	13.554957	-0.052432	4.818876
254.219945	8000.399687	13.559962	-0.052418	4.818928
253.730140	8000.207008	13.564967	-0.052327	4.818872
254.038026	8000.057944	13.569971	-0.052384	4.818827
253.886907	8000.256141	13.574976	-0.052356	4.818886
253.930225	8000.074397	13.579981	-0.052364	4.818832
253.837504	8000.227235	13.584986	-0.052347	4.818878
253.585849	7999.920236	13.589991	-0.052300	4.818787
253.575696	7999.805918	13.594995	-0.052298	4.818753
253.505769	8000.093140	13.600000	-0.052285	4.818839
253.431866	7999.749630	13.605005	-0.052271	4.818737
253.671915	8000.052292	13.610010	-0.052316	4.818826
253.520665	8000.093337	13.615015	-0.052288	4.818839
253.943119	7999.950959	13.620019	-0.052367	4.818795
253.759314	8000.199030	13.625024	-0.052333	4.818870
254.104110	8000.140532	13.630029	-0.052397	4.818851
253.779648	8000.171006	13.635034	-0.052337	4.818861
253.121309	7999.933253	13.640039	-0.052214	4.818793
253.299641	7999.815031	13.645043	-0.052247	4.818757
252.716754	7999.779387	13.650048	-0.052139	4.818748
253.155665	7999.860362	13.655053	-0.052220	4.818771
253.499414	7999.906613	13.660058	-0.052284	4.818783
253.427923	7999.847045	13.665063	-0.052271	4.818766
253.241567	7999.865646	13.670067	-0.052237	4.818772
253.356329	7999.840908	13.675072	-0.052258	4.818764
253.582145	7999.921289	13.680077	-0.052300	4.818787
253.229319	7999.866548	13.685082	-0.052234	4.818773
253.500700	7999.847979	13.690087	-0.052285	4.818766
253.683869	7999.859724	13.695091	-0.052319	4.818769
253.768175	7999.981272	13.700096	-0.052335	4.818805
254.536536	8000.247670	13.705101	-0.052478	4.818881
254.162610	8000.188464	13.710106	-0.052409	4.818865
254.320824	8000.451343	13.715111	-0.052438	4.818943
254.143138	8000.141078	13.720115	-0.052405	4.818851
254.087902	8000.257723	13.725120	-0.052395	4.818886
254.291554	8000.068576	13.730125	-0.052433	4.818829
254.090475	8000.289191	13.735130	-0.052395	4.818895
254.070203	8000.229220	13.740135	-0.052392	4.818877
254.193508	8000.076774	13.745139	-0.052415	4.818832
253.940375	8000.356449	13.750144	-0.052368	4.818916
253.936834	7999.910100	13.755149	-0.052367	4.818783
254.032219	8000.204655	13.760154	-0.052385	4.818870
253.852042	7999.819984	13.765159	-0.052351	4.818756
254.166501	8000.255600	13.770163	-0.052410	4.818885
254.282489	8000.307359	13.775168	-0.052432	4.818900
254.062218	8000.053134	13.780173	-0.052390	4.818825
253.824319	7999.940125	13.785178	-0.052346	4.818792
254.049189	8000.088595	13.790183	-0.052388	4.818836
254.192955	7999.958410	13.795187	-0.052415	4.818796
254.243127	8000.303732	13.800192	-0.052424	4.818899
254.616483	8000.094730	13.805197	-0.052494	4.818835
254.487179	8000.407404	13.810202	-0.052470	4.818929
254.592581	8000.317591	13.815207	-0.052490	4.818902
254.320159	8000.539403	13.820211	-0.052439	4.818969
254.269457	8000.206645	13.825216	-0.052429	4.818870
254.390182	8000.102359	13.830221	-0.052452	4.818838
254.191192	8000.377482	13.835226	-0.052415	4.818921
254.134332	8000.142085	13.840231	-0.052404	4.818851
254.169435	7999.890044	13.845235	-0.052411	4.818776
254.065502	8000.259608	13.850240	-0.052392	4.818886
253.987714	7999.970518	13.855245	-0.052377	4.818801
254.273577	8000.043280	13.860250	-0.052430	4.818821
254.115981	8000.198442	13.865255	-0.052401	4.818868
253.835490	7999.948697	13.870259	-0.052349	4.818795
253.964126	8000.181860	13.875264	-0.052373	4.818864
254.062896	8000.055296	13.880269	-0.052391	4.818826
253.719171	7999.923140	13.885274	-0.052327	4.818787
253.856355	7999.959449	13.890279	-0.052353	4.818798
253.943844	7999.859983	13.895283	-0.052369	4.818768
253.892802	8000.058395	13.900288	-0.052360	4.818827
253.848155	7999.844112	13.905293	-0.052351	4.818763
253.642275	7999.857229	13.910298	-0.052313	4.818768
254.275259	8000.156482	13.915303	-0.052431	4.818855
253.963826	8000.019494	13.920307	-0.052373	4.818815
253.916685	7999.926707	13.925312	-0.052364	4.818788
254.128649	7999.945104	13.930317	-0.052404	4.818792
254.074973	8000.259777	13.935322	-0.052394	4.818886
253.801907	8000.097081	13.940327	-0.052343	4.818839
253.920944	7999.988584	13.945331	-0.052365	4.818806
254.315683	8000.331978	13.950336	-0.052439	4.818907
253.823895	7999.844883	13.955341	-0.052347	4.818764
254.039377	7999.913611	13.960346	-0.052388	4.818783
253.827015	8000.079603	13.965351	-0.052348	4.818834
254.265189	7999.914375	13.970355	-0.052430	4.818783
253.639366	7999.945232	13.975360	-0.052313	4.818794
253.748003	7999.784223	13.980365	-0.052333	4.818746
254.167518	7999.987534	13.985370	-0.052412	4.818805
254.303742	8000.253273	13.990375	-0.052437	4.818884
254.184723	7999.947946	13.995379	-0.052415	4.818793
253.755211	7999.954044	14.000384	-0.052335	4.818797
253.651486	7999.882544	14.005389	-0.052316	4.818776
253.816963	7999.919210	14.010394	-0.052347	4.818786
253.555743	7999.897055	14.015399	-0.052298	4.818780
253.595432	7999.771842	14.020403	-0.052305	4.818743
253.532013	7999.861141	14.025408	-0.052294	4.818770
253.831827	7999.862837	14.030413	-0.052350	4.818769
253.898470	8000.015592	14.035418	-0.052362	4.818814
253.771244	7999.862077	14.040423	-0.052338	4.818769
253.950336	7999.855962	14.045427	-0.052372	4.818767
253.949192	7999.899951	14.050432	-0.052372	4.818780
253.639689	7999.847852	14.055437	-0.052314	4.818765
253.429149	7999.852528	14.060442	-0.052275	4.818768
253.537690	7999.868569	14.065447	-0.052295	4.818772
253.905595	7999.794647	14.070451	-0.052364	4.818748
254.355530	8000.371319	14.075456	-0.052448	4.818919
254.221073	8000.008172	14.080461	-0.052423	4.818811
253.838982	7999.961438	14.085466	-0.052351	4.818798
253.805787	8000.000833	14.090471	-0.052345	4.818810
254.252216	7999.917427	14.095475	-0.052428	4.818784
254.492213	8000.272484	14.100480	-0.052473	4.818889
253.956586	8000.035225	14.105485	-0.052374	4.818820
254.005873	8000.154237	14.110490	-0.052383	4.818855
253.951445	8000.062405	14.115495	-0.052373	4.818828
253.778154	7999.873735	14.120499	-0.052340	4.818773
254.036589	7999.946149	14.125504	-0.052389	4.818793
254.152680	7999.983240	14.130509	-0.052410	4.818804
253.973963	8000.005080	14.135514	-0.052377	4.818811
254.324403	8000.302863	14.140519	-0.052442	4.818898
254.623297	8000.275217	14.145523	-0.052498	4.818889
254.455068	8000.429198	14.150528	-0.052467	4.818935
254.594116	8000.464487	14.155533	-0.052493	4.818945
254.458804	8000.442871	14.160538	-0.052468	4.818940
254.587876	8000.453937	14.165543	-0.052492	4.818942
254.797158	8000.385344	14.170547	-0.052531	4.818921
254.729624	8000.445259	14.175552	-0.052518	4.818939
255.021594	8000.569446	14.180557	-0.052573	4.818975
255.022429	8000.437446	14.185562	-0.052573	4.818936
254.813458	8000.465188	14.190567	-0.052534	4.818945
254.834234	8000.571273	14.195571	-0.052538	4.818976
254.734890	8000.483058	14.200576	-0.052520	4.818950
254.684136	8000.322120	14.205581	-0.052510	4.818903
254.581389	8000.532459	14.210586	-0.052491	4.818966
254.581870	8000.426650	14.215591	-0.052491	4.818934
254.840841	8000.315730	14.220595	-0.052539	4.818900
254.429202	8000.357671	14.225600	-0.052463	4.818914
254.470548	8000.110942	14.230605	-0.052470	4.818841
254.521068	8000.304359	14.235610	-0.052480	4.818898
254.323671	8000.213859	14.240615	-0.052443	4.818872
254.167225	7999.980348	14.245619	-0.052414	4.818803
254.419226	8000.094590	14.250624	-0.052461	4.818836
254.333724	8000.093511	14.255629	-0.052445	4.818836
254.364744	8000.116956	14.260634	-0.052451	4.818843
254.597846	8000.286489	14.265639	-0.052494	4.818892
254.873801	8000.442949	14.270643	-0.052546	4.818938
254.304139	8000.094197	14.275648	-0.052440	4.818836
254.313632	8000.003172	14.280653	-0.052441	4.818809
254.532978	8000.300348	14.285658	-0.052483	4.818897
254.604352	8000.142005	14.290663	-0.052496	4.818849
254.502881	8000.189965	14.295667	-0.052477	4.818864
254.171483	8000.016054	14.300672	-0.052415	4.818813
254.163284	7999.785468	14.305677	-0.052414	4.818745
254.129522	7999.852094	14.310682	-0.052407	4.818765
254.380582	8000.257578	14.315687	-0.052454	4.818885
254.199110	8000.018510	14.320691	-0.052421	4.818814
254.423305	8000.404801	14.325696	-0.052463	4.818928
254.745362	8000.346017	14.330701	-0.052523	4.818910
254.792836	8000.227183	14.335706	-0.052531	4.818874
254.609436	8000.239533	14.340711	-0.052497	4.818878
254.637896	8000.201132	14.345715	-0.052503	4.818867
254.742966	8000.445530	14.350720	-0.052522	4.818939
254.994187	8000.340799	14.355725	-0.052569	4.818907
254.425260	8000.321030	14.360730	-0.052463	4.818903
254.325254	8000.294624	14.365735	-0.052445	4.818896
254.523333	8000.343231	14.370739	-0.052482	4.818910
254.245106	8000.449722	14.375744	-0.052430	4.818942
254.270225	8000.325367	14.380749	-0.052434	4.818905
254.345059	8000.136685	14.385754	-0.052448	4.818849
254.586802	7999.438859	14.390759	-0.052493	4.818640

254.770522	7996.419010	14.395763	-0.052525	4.817739
254.401781	7990.798992	14.400768	-0.052453	4.816065
254.734901	7984.099012	14.405773	-0.052511	4.814066
254.403841	7976.874771	14.410778	-0.052444	4.811912
254.278843	7969.198332	14.415783	-0.052416	4.809621
254.497561	7961.433475	14.420787	-0.052452	4.807301
254.167471	7953.483156	14.425792	-0.052385	4.804927
254.078883	7945.621077	14.430797	-0.052364	4.802577
254.418666	7937.578764	14.435802	-0.052422	4.800170
254.451351	7929.596460	14.440807	-0.052423	4.797782
254.000289	7921.657758	14.445811	-0.052333	4.795407
253.794138	7913.596541	14.450816	-0.052290	4.792993
253.911803	7905.661560	14.455821	-0.052307	4.790614
254.126799	7897.575323	14.460826	-0.052341	4.788189
254.128184	7889.538841	14.465831	-0.052337	4.785778
254.505431	7881.541290	14.470835	-0.052402	4.783377
254.326010	7873.590098	14.475840	-0.052363	4.780990
254.279629	7865.570441	14.480845	-0.052349	4.778580
254.464485	7857.585018	14.485850	-0.052379	4.776180
254.484899	7849.515925	14.490855	-0.052377	4.773753
254.413166	7841.591201	14.495859	-0.052359	4.771369
254.192282	7833.510557	14.500864	-0.052312	4.768937
254.448770	7825.583229	14.505869	-0.052355	4.766548
254.334824	7817.533480	14.510874	-0.052328	4.764123
254.184606	7809.622170	14.515879	-0.052295	4.761738
254.300269	7801.555562	14.520883	-0.052312	4.759304
253.810502	7793.656981	14.525888	-0.052215	4.756922
254.365284	7785.542942	14.530893	-0.052313	4.754470
254.059479	7777.570234	14.535898	-0.052251	4.752062
254.066815	7769.502714	14.540903	-0.052248	4.749624
254.016751	7761.584468	14.545907	-0.052233	4.747229
253.853252	7753.463182	14.550912	-0.052197	4.744772
253.802423	7745.584032	14.555917	-0.052183	4.742387
253.817601	7737.558841	14.560922	-0.052180	4.739956
253.900308	7729.551570	14.565927	-0.052191	4.737529
253.729744	7721.555118	14.570931	-0.052154	4.735105
253.607476	7713.525043	14.575936	-0.052126	4.732669
253.992184	7705.521494	14.580941	-0.052192	4.730239
253.768762	7697.514568	14.585946	-0.052146	4.727808
253.732362	7689.502542	14.590951	-0.052134	4.725374
253.880694	7681.540756	14.595955	-0.052156	4.722954
253.595923	7673.606604	14.600960	-0.052098	4.720541
253.788465	7665.618283	14.605965	-0.052129	4.718110
253.842225	7657.595477	14.610970	-0.052133	4.715667
253.521181	7649.568081	14.615975	-0.052068	4.713222
253.407162	7641.599058	14.620979	-0.052042	4.710794
253.709000	7633.499635	14.625984	-0.052093	4.708324
253.711701	7625.520930	14.630989	-0.052088	4.705889
253.559314	7617.511069	14.635994	-0.052055	4.703444
253.463602	7609.565919	14.640999	-0.052032	4.701018
253.684863	7601.523723	14.646003	-0.052068	4.698560
253.697430	7593.525909	14.651008	-0.052065	4.696115
253.463923	7585.578556	14.656013	-0.052016	4.693684
253.561375	7577.602566	14.661018	-0.052029	4.691243
253.313637	7569.499457	14.666023	-0.051978	4.688762
253.193744	7561.606792	14.671027	-0.051951	4.686344
253.077523	7553.503415	14.676032	-0.051924	4.683860
253.422151	7545.558821	14.681037	-0.051983	4.681424
253.669757	7537.474678	14.686042	-0.052024	4.678943
253.332570	7529.575972	14.691047	-0.051956	4.676518
253.304850	7521.509096	14.696051	-0.051945	4.674040
252.996568	7513.480801	14.701056	-0.051883	4.671573
253.350916	7505.446161	14.706061	-0.051944	4.669102
253.352089	7497.492574	14.711066	-0.051939	4.666655
253.316781	7489.393092	14.716071	-0.051927	4.664162
253.331390	7481.522943	14.721075	-0.051924	4.661738
253.201601	7473.478637	14.726080	-0.051895	4.659259
253.339509	7465.493260	14.731085	-0.051916	4.656797
253.285882	7457.455493	14.736090	-0.051900	4.654318
253.214922	7449.534299	14.741095	-0.051882	4.651873
253.235870	7441.484821	14.746099	-0.051881	4.649387
253.061821	7433.503496	14.751104	-0.051843	4.646921
252.950596	7425.469865	14.756109	-0.051817	4.644437
253.206566	7417.525825	14.761114	-0.051860	4.641980
252.906348	7409.461751	14.766119	-0.051799	4.639485
253.002937	7401.552615	14.771123	-0.051812	4.637036
252.873876	7393.427449	14.776128	-0.051782	4.634518
252.784728	7385.523155	14.781133	-0.051761	4.632068
252.233710	7377.497398	14.786138	-0.051653	4.629579
252.405457	7369.477311	14.791143	-0.051680	4.627090
252.506077	7361.419458	14.796147	-0.051693	4.624589
252.405743	7353.470026	14.801152	-0.051669	4.622119
252.497267	7345.413813	14.806157	-0.051681	4.619615
252.852316	7337.478480	14.811162	-0.051742	4.617148
252.805774	7329.422299	14.816167	-0.051728	4.614641
252.854250	7321.464408	14.821171	-0.051732	4.612164
252.781501	7313.350935	14.826176	-0.051713	4.609637
252.778602	7305.467996	14.831181	-0.051708	4.607180
252.410568	7297.452726	14.836186	-0.051634	4.604680
252.036358	7289.473002	14.841191	-0.051559	4.602190
252.329669	7281.459592	14.846195	-0.051609	4.599689
252.254879	7273.435262	14.851200	-0.051590	4.597183
251.981628	7265.443330	14.856205	-0.051533	4.594685
251.893204	7257.466854	14.861210	-0.051512	4.592191
252.193156	7249.359922	14.866215	-0.051562	4.589655
251.779106	7241.437928	14.871219	-0.051480	4.587175
251.931934	7233.336662	14.876224	-0.051503	4.584638
252.051297	7225.425294	14.881229	-0.051521	4.582159
251.852235	7217.419627	14.886234	-0.051478	4.579648
252.055295	7209.382995	14.891239	-0.051511	4.577128
252.267337	7201.407341	14.896243	-0.051545	4.574625
251.906324	7193.407115	14.901248	-0.051473	4.572111
251.902670	7185.388055	14.906253	-0.051467	4.569592
251.802333	7177.424760	14.911258	-0.051443	4.567088
251.449932	7169.336788	14.916263	-0.051372	4.564543
251.403818	7161.465325	14.921267	-0.051359	4.562065
251.465502	7153.326751	14.926272	-0.051365	4.559502
251.844651	7145.421972	14.931277	-0.051430	4.557013
251.856870	7137.336292	14.936282	-0.051427	4.554463
251.569318	7129.440712	14.941287	-0.051369	4.551972
251.685448	7121.330520	14.946291	-0.051385	4.549413
251.667557	7113.321904	14.951296	-0.051377	4.546884
251.368824	7105.335103	14.956301	-0.051316	4.544359
251.496495	7097.400281	14.961306	-0.051335	4.541851
252.057350	7089.295038	14.966311	-0.051434	4.539289
251.603833	7081.413923	14.971315	-0.051344	4.536793
251.377899	7073.338974	14.976320	-0.051297	4.534235
251.770999	7065.377758	14.981325	-0.051365	4.531714
251.087053	7057.358918	14.986330	-0.051232	4.529169
251.360219	7049.344789	14.991335	-0.051278	4.526628
251.891176	7041.286125	14.996339	-0.051372	4.524072
251.866087	7033.328206	15.001344	-0.051362	4.521545
251.544346	7025.305311	15.006349	-0.051297	4.518994
251.632035	7017.371859	15.011354	-0.051308	4.516472
251.749125	7009.286474	15.016359	-0.051325	4.513901
251.504565	7001.383390	15.021363	-0.051274	4.511384
251.382189	6993.294240	15.026368	-0.051246	4.508808
251.505171	6985.314592	15.031373	-0.051264	4.506266
251.355789	6977.269283	15.036378	-0.051231	4.503700
251.476503	6969.316294	15.041383	-0.051248	4.501163
251.426242	6961.334681	15.046387	-0.051234	4.498615
251.456145	6953.294057	15.051392	-0.051234	4.496048
251.035182	6945.303871	15.056397	-0.051150	4.493493
251.168131	6937.290669	15.061402	-0.051170	4.490931
251.207408	6929.244212	15.066407	-0.051172	4.488357
251.025373	6921.321369	15.071411	-0.051133	4.485820
250.904784	6913.305777	15.076416	-0.051105	4.483252
251.033152	6905.299179	15.081421	-0.051124	4.480687
251.063667	6897.285844	15.086426	-0.051125	4.478117
250.949448	6889.284026	15.091431	-0.051098	4.475550
251.341523	6881.286360	15.096435	-0.051166	4.472984
250.659524	6873.287453	15.101440	-0.051034	4.470411
250.836516	6865.288479	15.106445	-0.051062	4.467841
250.471338	6857.273063	15.111450	-0.050988	4.465262
250.449829	6849.302797	15.116455	-0.050979	4.462697
250.703034	6841.266013	15.121459	-0.051021	4.460111
250.796303	6833.227571	15.126464	-0.051033	4.457522
250.750772	6825.226946	15.131469	-0.051020	4.454943
250.810556	6817.264135	15.136474	-0.051026	4.452375
250.950087	6809.189522	15.141479	-0.051047	4.449770
250.708025	6801.268887	15.146483	-0.050996	4.447211
250.661767	6793.198972	15.151488	-0.050982	4.444604
250.614550	6785.305690	15.156493	-0.050969	4.442052
250.690809	6777.179440	15.161498	-0.050978	4.439424
249.905535	6769.375540	15.166503	-0.050826	4.436893
250.031876	6761.304252	15.171507	-0.050845	4.434280
249.487352	6753.316857	15.176512	-0.050738	4.431689
249.914123	6745.234366	15.181517	-0.050812	4.429071
250.347889	6737.189078	15.186522	-0.050888	4.426464
250.172768	6729.124773	15.191527	-0.050850	4.423845
249.917750	6721.282992	15.196531	-0.050797	4.421296
250.062938	6713.201231	15.201536	-0.050819	4.418671
250.266324	6705.228714	15.206541	-0.050852	4.416079
250.057906	6697.209103	15.211546	-0.050808	4.413469
250.392596	6689.214651	15.216551	-0.050865	4.410868
250.417264	6681.187644	15.221555	-0.050865	4.408253
250.289382	6673.197091	15.226560	-0.050836	4.405648
250.382150	6665.219430	15.231565	-0.050848	4.403047
250.585285	6657.221311	15.236570	-0.050880	4.400438
250.415238	6649.226735	15.241575	-0.050844	4.397827
250.473202	6641.275359	15.246579	-0.050849	4.395229
250.183426	6633.244117	15.251584	-0.050790	4.392602
250.044438	6625.268127	15.256589	-0.050759	4.389992
249.825050	6617.313873	15.261594	-0.050713	4.387387
249.977538	6609.249896	15.266599	-0.050736	4.384747
250.080538	6601.320346	15.271603	-0.050750	4.382149
250.040055	6593.247191	15.276608	-0.050737	4.379501
249.596554	6585.371233	15.281613	-0.050650	4.376914
249.925157	6577.304574	15.286618	-0.050706	4.374268
250.216171	6569.258701	15.291623	-0.050755	4.371627
249.357768	6561.375037	15.296627	-0.050590	4.369030
249.764648	6553.279284	15.301632	-0.050660	4.366370
249.643143	6545.308339	15.306637	-0.050633	4.363746
249.820504	6537.353458	15.311642	-0.050660	4.361128
250.012755	6529.239074	15.316647	-0.050691	4.358456
250.322869	6521.304847	15.321651	-0.050744	4.355843
249.732204	6513.266653	15.326656	-0.050628	4.353186
249.797555	6505.285318	15.331661	-0.050635	4.350552
249.810280	6497.279807	15.336666	-0.050633	4.347908
249.432369	6489.257341	15.341671	-0.050557	4.345254
250.073506	6481.238979	15.346675	-0.050671	4.342607
249.796876	6473.261693	15.351680	-0.050615	4.339966
249.526869	6465.368403	15.356685	-0.050559	4.337350
249.644212	6457.270715	15.361690	-0.050576	4.334668
249.541106	6449.282336	15.366695	-0.050552	4.332019
249.764635	6441.228608	15.371699	-0.050588	4.329350
249.538614	6433.260702	15.376704	-0.050541	4.326703
249.543931	6425.215763	15.381709	-0.050537	4.324031
249.347988	6417.374431	15.386714	-0.050495	4.321424
249.125752	6409.313335	15.391719	-0.050448	4.318741
248.950900	6401.366795	15.396723	-0.050411	4.316096
249.331979	6393.210020	15.401728	-0.050476	4.313383
249.610748	6385.211762	15.406733	-0.050523	4.310721
249.436889	6377.265963	15.411738	-0.050486	4.308071
249.128783	6369.217383	15.416743	-0.050423	4.305383
249.290066	6361.320255	15.421747	-0.050448	4.302749
248.942122	6353.276341	15.426752	-0.050378	4.300060
248.853483	6345.301487	15.431757	-0.050356	4.297394
249.479651	6337.196178	15.436762	-0.050468	4.294689
249.322708	6329.267651	15.441767	-0.050433	4.292035
248.967491	6321.273204	15.446771	-0.050362	4.289355
248.379874	6313.314672	15.451776	-0.050247	4.286683
248.116952	6305.283247	15.456781	-0.050193	4.283988
248.238480	6297.314865	15.461786	-0.050211	4.281316
248.690538	6289.163389	15.466791	-0.050290	4.278585
249.036046	6281.229106	15.471795	-0.050349	4.275923
248.695776	6273.178448	15.476800	-0.050280	4.273214
248.943824	6265.207671	15.481805	-0.050321	4.270536
248.828084	6257.206162	15.486810	-0.050295	4.267842
248.826893	6249.179477	15.491815	-0.050289	4.265140
249.019719	6241.215076	15.496819	-0.050320	4.262458
249.323058	6233.120838	15.501824	-0.050371	4.259732
249.127483	6225.249380	15.506829	-0.050330	4.257075
249.065540	6217.192090	15.511834	-0.050313	4.254354
248.761406	6209.243508	15.516839	-0.050251	4.251666
248.745907	6201.240388	15.521843	-0.050243	4.248961
248.532214	6193.245767	15.526848	-0.050198	4.246255
248.585955	6185.183426	15.531853	-0.050203	4.243527
248.753286	6177.227745	15.536858	-0.050229	4.240835
248.791015	6169.189055	15.541863	-0.050231	4.238111
248.178468	6161.309686	15.546867	-0.050112	4.235433
248.431314	6153.225716	15.551872	-0.050154	4.232692
248.361339	6145.232663	15.556877	-0.050135	4.229978
248.497076	6137.179316	15.561882	-0.050155	4.227243
248.406838	6129.152273	15.566887	-0.050133	4.224513
248.553185	6121.248393	15.571891	-0.050156	4.221826
248.317640	6113.179637	15.576896	-0.050106	4.219077
248.156290	6105.267714	15.581901	-0.050071	4.216380
248.158626	6097.229099	15.586906	-0.050067	4.213640
248.530816	6089.156763	15.591911	-0.050131	4.210891
248.947775	6081.152972	15.596915	-0.050203	4.208165
248.916130	6073.152076	15.601920	-0.050192	4.205432
248.571697	6065.250194	15.606925	-0.050123	4.202728
248.474473	6057.228229	15.611930	-0.050100	4.199983
248.388785	6049.248552	15.616935	-0.050078	4.197252
248.913053	6041.177270	15.621939	-0.050171	4.194495
248.611625	6033.144483	15.626944	-0.050110	4.191739
248.193383	6025.177651	15.631949	-0.050026	4.189002
248.313814	6017.140778	15.636954	-0.050044	4.186247
248.487117	6009.132734	15.641959	-0.050071	4.183500
248.506762	6001.216229	15.646963	-0.050069	4.180780
248.113004	5993.222566	15.651968	-0.049991	4.178028
248.174331	5985.193419	15.656973	-0.049997	4.175267
248.241387	5977.256403	15.661978	-0.050004	4.172535
248.165627	5969.194760	15.666983	-0.049985	4.169758
248.056044	5961.245713	15.671987	-0.049960	4.167017
248.344579	5953.129818	15.676992	-0.050008	4.164221
248.452258	5945.225817	15.681997	-0.050023	4.161495
248.507691	5937.181598	15.687002	-0.050028	4.158717
248.561336	5929.198797	15.692007	-0.050033	4.155959
248.697392	5921.248865	15.697011	-0.050053	4.153212
248.462187	5913.202743	15.702016	-0.050004	4.150425
248.364503	5905.282184	15.707021	-0.049981	4.147681
248.441278	5897.233247	15.712026	-0.049990	4.144893
248.123542	5889.278661	15.717031	-0.049926	4.142131
248.361429	5881.224420	15.722035	-0.049965	4.139339
248.089589	5873.270801	15.727040	-0.049909	4.136574
247.963881	5865.243264	15.732045	-0.049880	4.133783
247.718246	5857.287846	15.737050	-0.049829	4.131014
247.822422	5849.202096	15.742055	-0.049844	4.128202
247.771358	5841.255259	15.747059	-0.049829	4.125435
247.532064	5833.239744	15.752064	-0.049779	4.122639
247.793612	5825.236618	15.757069	-0.049823	4.119853
247.530967	5817.298320	15.762074	-0.049769	4.117080
247.267981	5809.240338	15.767079	-0.049715	4.114263
247.466579	5801.243432	15.772083	-0.049746	4.111472
247.266306	5793.239557	15.777088	-0.049704	4.108672
247.374732	5785.241979	15.782093	-0.049719	4.105876
247.608692	5777.186697	15.787098	-0.049757	4.103059
247.657965	5769.181016	15.792103	-0.049761	4.100256
247.650479	5761.231232	15.797107	-0.049755	4.097469
247.422867	5753.208850	15.802112	-0.049707	4.094652
247.704175	5745.196556	15.807117	-0.049754	4.091843
248.036108	5737.128881	15.812122	-0.049811	4.089015
247.845219	5729.190871	15.817127	-0.049770	4.086222
247.868107	5721.193395	15.822131	-0.049769	4.083409
247.907986	5713.244150	15.827136	-0.049772	4.080612
248.065523	5705.204924	15.832141	-0.049796	4.077783
247.767278	5697.243082	15.837146	-0.049735	4.074972
247.556680	5689.284844	15.842151	-0.049691	4.072162
247.637206	5681.271801	15.847155	-0.049701	4.069335
247.603530	5673.192407	15.852160	-0.049689	4.066481
247.677492	5665.213768	15.857165	-0.049698	4.063662
247.449721	5657.259218	15.862170	-0.049650	4.060845
246.996165	5649.307044	15.867175	-0.049561	4.058023
246.862097	5641.317334	15.872179	-0.049530	4.055191
247.074704	5633.240320	15.877184	-0.049565	4.052332
247.012070	5625.238449	15.882189	-0.049548	4.049493
247.266179	5617.190164	15.887194	-0.049590	4.046640
247.159750	5609.200648	15.892199	-0.049565	4.043801
247.436057	5601.269674	15.897203	-0.049611	4.040986
246.964337	5593.282559	15.902208	-0.049518	4.038138
247.279236	5585.253893	15.907213	-0.049572	4.035285
247.328166	5577.226352	15.912218	-0.049576	4.032426
247.118802	5569.199774	15.917223	-0.049532	4.029562
247.232280	5561.203410	15.922227	-0.049548	4.026712
247.328828	5553.186352	15.927232	-0.049560	4.023852
247.553825	5545.251962	15.932237	-0.049597	4.021021
247.214761	5537.298021	15.937242	-0.049529	4.018172
247.296410	5529.226227	15.942247	-0.049539	4.015286
247.202670	5521.279230	15.947251	-0.049516	4.012440
247.076358	5513.244502	15.952256	-0.049488	4.009560
247.238237	5505.259323	15.957261	-0.049513	4.006700
247.355335	5497.254089	15.962266	-0.049529	4.003830
247.069968	5489.318238	15.967271	-0.049471	4.000976
247.218158	5481.322075	15.972275	-0.049493	3.998106
247.109143	5473.315416	15.977280	-0.049468	3.995226
246.885350	5465.332313	15.982285	-0.049421	3.992350
246.771778	5457.280333	15.987290	-0.049395	3.989449
246.823434	5449.297190	15.992295	-0.049399	3.986574
247.140520	5441.257385	15.997299	-0.049453	3.983680
246.947196	5433.266687	16.002304	-0.049412	3.980794
246.897881	5425.284235	16.007309	-0.049398	3.977911
247.130972	5417.275392	16.012314	-0.049436	3.975021
246.879112	5409.331919	16.017319	-0.049384	3.972144
246.940285	5401.279419	16.022323	-0.049390	3.969231
246.840249	5393.282303	16.027328	-0.049366	3.966333
247.007577	5385.274970	16.032333	-0.049392	3.963435
246.929438	5377.331505	16.037338	-0.049372	3.960552
246.768008	5369.285461	16.042343	-0.049337	3.957629
247.079234	5361.310616	16.047347	-0.049390	3.954739
246.973444	5353.288193	16.052352	-0.049365	3.951821
246.919591	5345.225311	16.057357	-0.049350	3.948887
246.896296	5337.263752	16.062362	-0.049340	3.945989
246.853469	5329.276518	16.067367	-0.049327	3.943078
246.777217	5321.302941	16.072371	-0.049308	3.940170
246.706609	5313.318741	16.077376	-0.049290	3.937256
246.632398	5305.293662	16.082381	-0.049271	3.934325
246.733624	5297.309772	16.087386	-0.049284	3.931410
246.577150	5289.277118	16.092391	-0.049250	3.928470
246.817621	5281.307940	16.097395	-0.049290	3.925558
246.503967	5273.332348	16.102400	-0.049226	3.922632
246.337099	5265.372882	16.107405	-0.049190	3.919712
246.296544	5257.380306	16.112410	-0.049177	3.916780
246.433922	5249.306770	16.117415	-0.049197	3.913820
246.350986	5241.371862	16.122419	-0.049177	3.910904
246.042019	5233.329515	16.127424	-0.049114	3.907942
246.324197	5225.330785	16.132429	-0.049161	3.905005
246.516318	5217.350509	16.137434	-0.049192	3.902071
246.229693	5209.339726	16.142439	-0.049134	3.899114
246.302847	5201.419469	16.147443	-0.049142	3.896196
246.169499	5193.351581	16.152448	-0.049112	3.893217
246.123909	5185.360293	16.157453	-0.049098	3.890265
246.193515	5177.368690	16.162458	-0.049106	3.887314
246.074890	5169.405454	16.167463	-0.049079	3.884366
246.109221	5161.424573	16.172467	-0.049080	3.881414
246.019435	5153.373310	16.177472	-0.049058	3.878430
246.075696	5145.406778	16.182477	-0.049064	3.875478
246.254429	5137.284558	16.187482	-0.049092	3.872469
246.211888	5129.208047	16.192487	-0.049078	3.869470
246.323321	5121.302101	16.197491	-0.049094	3.866536
245.994297	5113.339155	16.202496	-0.049028	3.863568
245.903298	5105.387275	16.207501	-0.049006	3.860608
245.972111	5097.352722	16.212506	-0.049013	3.857617
246.196783	5089.331288	16.217511	-0.049050	3.854633
246.004380	5081.369428	16.222515	-0.049009	3.851660
245.661631	5073.353144	16.227520	-0.048940	3.848660
245.982770	5065.368042	16.232525	-0.048994	3.845685
245.965583	5057.405446	16.237530	-0.048986	3.842708
245.633031	5049.425004	16.242535	-0.048919	3.839715
245.743710	5041.434830	16.247539	-0.048935	3.836726
245.672357	5033.401628	16.252544	-0.048916	3.833715
245.511172	5025.420050	16.257549	-0.048881	3.830718
245.657115	5017.369976	16.262554	-0.048903	3.827701
245.586021	5009.367398	16.267559	-0.048884	3.824693
245.433909	5001.443254	16.272563	-0.048851	3.821712
245.578359	4993.415465	16.277568	-0.048873	3.818695
245.630820	4985.404480	16.282573	-0.048877	3.815680
245.482560	4977.420226	16.287578	-0.048845	3.812669
245.574186	4969.394697	16.292583	-0.048856	3.809645
245.644672	4961.390851	16.297587	-0.048864	3.806626
245.522494	4953.395173	16.302592	-0.048836	3.803604
245.448443	4945.473973	16.307597	-0.048818	3.800608
245.397741	4937.468517	16.312602	-0.048803	3.797579
245.605106	4929.437091	16.317607	-0.048836	3.794544
245.327114	4921.497193	16.322611	-0.048779	3.791529
245.123235	4913.445560	16.327616	-0.048736	3.788471
245.475245	4905.405427	16.332621	-0.048797	3.785429
245.231828	4897.490107	16.337626	-0.048746	3.782417
245.267111	4889.424182	16.342631	-0.048748	3.779352
245.702249	4881.451268	16.347635	-0.048823	3.776330
245.348078	4873.442436	16.352640	-0.048752	3.773272
245.444132	4865.469159	16.357645	-0.048765	3.770237
245.186931	4857.517280	16.362650	-0.048712	3.767198
244.942519	4849.489346	16.367655	-0.048661	3.764129
244.935834	4841.587743	16.372659	-0.048655	3.761111
244.934280	4833.514997	16.377664	-0.048649	3.758025
245.055685	4825.514423	16.382669	-0.048667	3.754967
245.090180	4817.531613	16.387674	-0.048668	3.751912
245.042661	4809.477517	16.392679	-0.048654	3.748824
245.272794	4801.482915	16.397683	-0.048692	3.745764
245.005220	4793.515666	16.402688	-0.048637	3.742700
244.920644	4785.525282	16.407693	-0.048616	3.739628
245.090309	4777.538709	16.412698	-0.048642	3.736562
245.190442	4769.485311	16.417703	-0.048656	3.733466
245.216990	4761.497685	16.422707	-0.048656	3.730391
245.018331	4753.526614	16.427712	-0.048613	3.727314
244.954281	4745.525010	16.432717	-0.048596	3.724226
244.912121	4737.616742	16.437722	-0.048583	3.721172
244.867052	4729.521329	16.442727	-0.048570	3.718043
244.812354	4721.557683	16.447731	-0.048554	3.714962
244.753375	4713.529192	16.452736	-0.048538	3.711854
244.907553	4705.491561	16.457741	-0.048562	3.708744
244.778594	4697.531966	16.462746	-0.048533	3.705655
244.704417	4689.534355	16.467751	-0.048514	3.702551
244.691623	4681.559435	16.472755	-0.048506	3.699454
244.822327	4673.536508	16.477760	-0.048525	3.696339
244.788317	4665.545129	16.482765	-0.048514	3.693230
244.521542	4657.566750	16.487770	-0.048459	3.690117
244.677588	4649.556707	16.492775	-0.048483	3.687000
244.577969	4641.590111	16.497779	-0.048459	3.683891
244.615688	4633.636839	16.502784	-0.048461	3.680788
244.512500	4625.634467	16.507789	-0.048437	3.677660
244.097342	4617.677290	16.512794	-0.048354	3.674538
244.325696	4609.636985	16.517799	-0.048391	3.671398
244.454388	4601.590470	16.522803	-0.048410	3.668250
244.224313	4593.620413	16.527808	-0.048362	3.665120
244.474867	4585.652305	16.532813	-0.048404	3.662001
244.352271	4577.648687	16.537818	-0.048376	3.658855
244.372038	4569.689652	16.542823	-0.048374	3.655728
244.109659	4561.682729	16.547827	-0.048320	3.652572
244.006708	4553.665237	16.552832	-0.048296	3.649413
244.054085	4545.699530	16.557837	-0.048299	3.646276
243.748277	4537.727778	16.562842	-0.048237	3.643124
243.583585	4529.745104	16.567847	-0.048202	3.639969
244.126273	4521.703077	16.572851	-0.048297	3.636808
243.996597	4513.663889	16.577856	-0.048268	3.633626
243.973916	4505.661974	16.582861	-0.048259	3.630459
243.803775	4497.724170	16.587866	-0.048222	3.627310
243.873043	4489.649296	16.592871	-0.048230	3.624112
243.523963	4481.795098	16.597875	-0.048159	3.620986
243.639903	4473.694025	16.602880	-0.048176	3.617772
243.863687	4465.687256	16.607885	-0.048212	3.614596
243.805381	4457.698611	16.612890	-0.048196	3.611417
243.726559	4449.680913	16.617895	-0.048176	3.608222
243.985757	4441.683134	16.622899	-0.048220	3.605043
243.905255	4433.718864	16.627904	-0.048199	3.601864
243.710737	4425.784932	16.632909	-0.048158	3.598691
243.817233	4417.777245	16.637914	-0.048173	3.595495
243.687468	4409.778552	16.642919	-0.048143	3.592292
243.702849	4401.755212	16.647923	-0.048141	3.589081
243.563813	4393.740438	16.652928	-0.048110	3.585866
243.687481	4385.744413	16.657933	-0.048128	3.582664
243.531360	4377.790451	16.662938	-0.048094	3.579467
243.636877	4369.778179	16.667943	-0.048108	3.576252
243.681702	4361.793164	16.672947	-0.048111	3.573042
243.563513	4353.780318	16.677952	-0.048084	3.569814
243.505551	4345.828324	16.682957	-0.048068	3.566610
243.441159	4337.819751	16.687962	-0.048051	3.563379
243.295642	4329.837797	16.692967	-0.048019	3.560154
243.370573	4321.896549	16.697971	-0.048028	3.556949
243.095032	4313.862640	16.702976	-0.047971	3.553692
243.449868	4305.770920	16.707981	-0.048032	3.550429
243.165312	4297.842738	16.712986	-0.047974	3.547209
243.079318	4289.815747	16.717991	-0.047953	3.543953
243.319164	4281.867913	16.722995	-0.047992	3.540736
243.210891	4273.866562	16.728000	-0.047967	3.537483
243.098434	4265.862971	16.733005	-0.047941	3.534226
243.202454	4257.889079	16.738010	-0.047955	3.530985
243.182895	4249.863144	16.743015	-0.047946	3.527716
243.204334	4241.860595	16.748019	-0.047945	3.524455
243.003531	4233.925709	16.753024	-0.047902	3.521211
242.862332	4225.937762	16.758029	-0.047871	3.517944
242.796854	4217.947521	16.763034	-0.047854	3.514676
243.010496	4209.911424	16.768039	-0.047888	3.511395
242.719591	4201.978328	16.773043	-0.047829	3.508137
242.646203	4193.927369	16.778048	-0.047810	3.504835
242.566232	4185.953773	16.783053	-0.047790	3.501561
242.537341	4177.966885	16.788058	-0.047779	3.498280
242.558126	4169.926599	16.793063	-0.047778	3.494976
242.746157	4161.939664	16.798067	-0.047808	3.491696
242.599610	4153.937784	16.803072	-0.047775	3.488395
242.312784	4145.976802	16.808077	-0.047717	3.485104
242.283994	4138.051046	16.813082	-0.047706	3.481833
242.094509	4130.003715	16.818087	-0.047666	3.478503
242.701798	4121.962950	16.823091	-0.047774	3.475199
242.518102	4113.998402	16.828096	-0.047734	3.471897
242.472296	4105.971516	16.833101	-0.047721	3.468571
241.965086	4098.093924	16.838106	-0.047621	3.465288
242.072138	4090.047401	16.843111	-0.047636	3.461953
242.227663	4082.058697	16.848115	-0.047660	3.458639
242.035749	4074.061889	16.853120	-0.047619	3.455308
242.412074	4066.043266	16.858125	-0.047684	3.451984
242.229762	4058.102349	16.863130	-0.047645	3.448669
242.099350	4050.063829	16.868135	-0.047615	3.445313
242.362988	4042.055055	16.873139	-0.047659	3.441979
242.118389	4034.117893	16.878144	-0.047608	3.438655
242.024547	4026.140129	16.883149	-0.047586	3.435315
241.949931	4018.148438	16.888154	-0.047567	3.431967
242.053327	4010.105724	16.893159	-0.047581	3.428601
241.940345	4002.132196	16.898163	-0.047555	3.425252
241.698347	3994.155834	16.903168	-0.047504	3.421895
241.754496	3986.176360	16.908173	-0.047510	3.418543
241.579354	3978.200520	16.913178	-0.047472	3.415182
241.458298	3970.190981	16.918183	-0.047444	3.411805
242.039991	3962.105277	16.923187	-0.047547	3.408417
241.573507	3954.171357	16.928192	-0.047455	3.405053
241.783226	3946.223235	16.933197	-0.047489	3.401704
241.783009	3938.187880	16.938202	-0.047484	3.398307
242.032570	3930.173799	16.943207	-0.047525	3.394924
242.164830	3922.155575	16.948211	-0.047545	3.391533
242.161849	3914.123850	16.953216	-0.047539	3.388127
242.160882	3906.145611	16.958221	-0.047534	3.384740
242.143245	3898.214261	16.963226	-0.047525	3.381370
242.076179	3890.206341	16.968231	-0.047508	3.377962
242.005473	3882.250100	16.973235	-0.047489	3.374572
242.056608	3874.243684	16.978240	-0.047494	3.371162
242.018250	3866.244385	16.983245	-0.047481	3.367748
241.906885	3858.258146	16.988250	-0.047455	3.364333
241.860045	3850.332082	16.993255	-0.047442	3.360943
241.982017	3842.318988	16.998259	-0.047459	3.357519
241.818079	3834.315886	17.003264	-0.047423	3.354085
241.885887	3826.336266	17.008269	-0.047431	3.350666
241.980897	3818.339092	17.013274	-0.047443	3.347237
241.985656	3810.304330	17.018279	-0.047439	3.343785
241.982077	3802.368570	17.023283	-0.047433	3.340372
241.922287	3794.369832	17.028288	-0.047417	3.336926
241.921366	3786.378481	17.033293	-0.047412	3.333482
241.732316	3778.394135	17.038298	-0.047371	3.330030
241.549335	3770.419787	17.043303	-0.047332	3.326578
241.577172	3762.430540	17.048307	-0.047332	3.323126
241.453881	3754.430746	17.053312	-0.047304	3.319659
241.627185	3746.445030	17.058317	-0.047331	3.316206
241.468792	3738.466597	17.063322	-0.047296	3.312739
241.494643	3730.446125	17.068327	-0.047296	3.309258
241.389867	3722.455993	17.073331	-0.047271	3.305782
241.519033	3714.430804	17.078336	-0.047290	3.302295
241.519043	3706.443002	17.083341	-0.047285	3.298816
241.464878	3698.491482	17.088346	-0.047270	3.295347
241.315590	3690.494157	17.093351	-0.047237	3.291851
241.378119	3682.488114	17.098355	-0.047243	3.288356
241.164456	3674.492407	17.103360	-0.047198	3.284850
241.255807	3666.545657	17.108365	-0.047210	3.281374
241.538766	3658.540475	17.113370	-0.047258	3.277877
241.143322	3650.602199	17.118375	-0.047179	3.274378
241.140451	3642.591455	17.123379	-0.047173	3.270859
240.998463	3634.596583	17.128384	-0.047142	3.267338
241.023400	3626.575016	17.133389	-0.047141	3.263808
240.953820	3618.633955	17.138394	-0.047123	3.260306
241.072078	3610.596905	17.143399	-0.047140	3.256765
240.947487	3602.654172	17.148403	-0.047112	3.253252
241.077096	3594.629878	17.153408	-0.047130	3.249710
241.035910	3586.630338	17.158413	-0.047118	3.246168
240.951248	3578.679567	17.163418	-0.047097	3.242641
240.930907	3570.652626	17.168423	-0.047088	3.239080
241.002862	3562.738223	17.173427	-0.047096	3.235569
240.913740	3554.714288	17.178432	-0.047074	3.231998
240.828807	3546.736030	17.183437	-0.047053	3.228444
240.931496	3538.693408	17.188442	-0.047067	3.224865
240.531759	3530.753777	17.193447	-0.046988	3.221307
240.670275	3522.752091	17.198451	-0.047008	3.217740
240.487447	3514.764170	17.203456	-0.046969	3.214162
240.616174	3506.737202	17.208461	-0.046988	3.210575
240.593955	3498.745502	17.213466	-0.046979	3.206994
240.666542	3490.732735	17.218471	-0.046987	3.203403
240.545213	3482.808799	17.223475	-0.046959	3.199840
240.572005	3474.825970	17.228480	-0.046959	3.196253
240.634819	3466.806305	17.233485	-0.046966	3.192647
240.615147	3458.850089	17.238490	-0.046957	3.189061
240.716343	3450.814970	17.243495	-0.046970	3.185442
240.674887	3442.877479	17.248499	-0.046958	3.181856
240.595103	3434.887823	17.253504	-0.046937	3.178241
240.471146	3426.906111	17.258509	-0.046909	3.174623
240.559570	3418.919611	17.263514	-0.046921	3.171008
240.480043	3410.886461	17.268519	-0.046901	3.167361
240.506968	3402.925638	17.273523	-0.046900	3.163747
240.450716	3394.956718	17.278528	-0.046885	3.160121
240.522244	3386.991878	17.283533	-0.046893	3.156499
240.380278	3378.998415	17.288538	-0.046861	3.152850
240.314180	3370.968450	17.293543	-0.046844	3.149183
240.397244	3362.993833	17.298547	-0.046854	3.145545
240.387537	3354.997392	17.303552	-0.046847	3.141888
239.926996	3347.064827	17.308557	-0.046756	3.138235
240.087969	3339.061854	17.313562	-0.046781	3.134574
240.034081	3331.068611	17.318567	-0.046766	3.130903
240.202690	3323.046806	17.323571	-0.046792	3.127226
240.071310	3315.067932	17.328576	-0.046763	3.123550
239.713753	3307.135550	17.333581	-0.046691	3.119880
239.792168	3299.179475	17.338586	-0.046700	3.116215
239.768304	3291.141007	17.343591	-0.046691	3.112504
239.991510	3283.119496	17.348595	-0.046727	3.108807
239.864163	3275.141005	17.353600	-0.046698	3.105109
239.941420	3267.178874	17.358605	-0.046707	3.101424
239.745310	3259.213008	17.363610	-0.046666	3.097720
239.790698	3251.194474	17.368615	-0.046669	3.093999
239.809262	3243.241998	17.373619	-0.046667	3.090302
239.774443	3235.220049	17.378624	-0.046656	3.086567
239.772965	3227.245243	17.383629	-0.046650	3.082850
239.636201	3219.292647	17.388634	-0.046620	3.079133
239.325149	3211.367032	17.393639	-0.046557	3.075415
239.578487	3203.292124	17.398643	-0.046598	3.071650
239.617263	3195.261190	17.403648	-0.046601	3.067891
239.541712	3187.267243	17.408653	-0.046581	3.064139
239.509548	3179.317166	17.413658	-0.046570	3.060405
239.572890	3171.333679	17.418663	-0.046577	3.056655
239.611984	3163.346575	17.423667	-0.046579	3.052898
239.448748	3155.359966	17.428672	-0.046543	3.049127
239.261515	3147.440064	17.433677	-0.046503	3.045381
239.202455	3139.465043	17.438682	-0.046487	3.041611
239.132873	3131.472023	17.443687	-0.046469	3.037827
239.444019	3123.452879	17.448691	-0.046522	3.034045
239.151596	3115.489451	17.453696	-0.046462	3.030255
239.224079	3107.476562	17.458701	-0.046471	3.026454
239.021498	3099.533005	17.463706	-0.046428	3.022668
239.161024	3091.504891	17.468711	-0.046449	3.018854
239.180236	3083.554628	17.473715	-0.046447	3.015067
239.028746	3075.580199	17.478720	-0.046414	3.011254
239.062670	3067.573326	17.483725	-0.046415	3.007431
239.109521	3059.585674	17.488730	-0.046418	3.003612
238.751235	3051.637170	17.493735	-0.046346	2.999787
238.873397	3043.674824	17.498739	-0.046364	2.995975
238.847536	3035.645530	17.503744	-0.046354	2.992118
239.080080	3027.620870	17.508749	-0.046392	2.988271
238.977942	3019.655448	17.513754	-0.046368	2.984431
238.947330	3011.688728	17.518759	-0.046357	2.980589
238.907863	3003.737133	17.523763	-0.046345	2.976749
238.906233	2995.731038	17.528768	-0.046339	2.972880
239.188716	2987.674877	17.533773	-0.046387	2.968996
238.969979	2979.758936	17.538778	-0.046341	2.965149
238.874115	2971.797562	17.543783	-0.046318	2.961281
238.575930	2963.886055	17.548787	-0.046257	2.957422
238.663361	2955.883881	17.553792	-0.046268	2.953533
238.462793	2947.889145	17.558797	-0.046226	2.949628
238.163318	2939.942179	17.563802	-0.046165	2.945736
238.164673	2931.914051	17.568807	-0.046160	2.941815
238.383116	2923.905903	17.573811	-0.046195	2.937911
238.331876	2915.897249	17.578816	-0.046181	2.933986
238.245650	2907.951558	17.583821	-0.046159	2.930085
238.336648	2899.963208	17.588826	-0.046171	2.926168
238.367731	2891.952173	17.593831	-0.046172	2.922230
238.473343	2883.994972	17.598835	-0.046186	2.918319
238.400490	2876.038491	17.603840	-0.046168	2.914392
238.422870	2868.013907	17.608845	-0.046167	2.910432
238.173960	2860.051340	17.613850	-0.046115	2.906482
238.245183	2852.053854	17.618855	-0.046123	2.902527
238.207665	2844.084445	17.623859	-0.046111	2.898574
238.044043	2836.095448	17.628864	-0.046075	2.894600
238.145319	2828.112221	17.633869	-0.046089	2.890637
237.997863	2820.160366	17.638874	-0.046057	2.886671
237.694847	2812.199505	17.643879	-0.045995	2.882686
237.825018	2804.216508	17.648883	-0.046014	2.878709
237.922861	2796.211303	17.653888	-0.046027	2.874713
238.193218	2788.206346	17.658893	-0.046072	2.870722
238.129801	2780.233466	17.663898	-0.046055	2.866723
238.273401	2772.231418	17.668903	-0.046077	2.862715
238.092622	2764.324008	17.673907	-0.046038	2.858730
238.016557	2756.327132	17.678912	-0.046019	2.854701
237.817671	2748.390908	17.683917	-0.045977	2.850689
237.706918	2740.416932	17.688922	-0.045951	2.846658
237.485326	2732.455913	17.693927	-0.045904	2.842621
237.623955	2724.459390	17.698931	-0.045925	2.838582
237.273880	2716.492873	17.703936	-0.045855	2.834523
237.205875	2708.536170	17.708941	-0.045837	2.830480
237.254422	2700.505611	17.713946	-0.045841	2.826401
237.190030	2692.511937	17.718951	-0.045824	2.822328
237.452935	2684.510277	17.723955	-0.045867	2.818264
237.374951	2676.537574	17.728960	-0.045848	2.814188
237.842403	2668.501467	17.733965	-0.045930	2.810107
237.902136	2660.523637	17.738970	-0.045936	2.806026
237.666169	2652.605250	17.743975	-0.045887	2.801951
237.488230	2644.680190	17.748979	-0.045848	2.797871
237.317103	2636.709577	17.753984	-0.045811	2.793762
237.436322	2628.697373	17.758989	-0.045828	2.789642
237.640722	2620.682099	17.763994	-0.045861	2.785520
237.456434	2612.744207	17.768999	-0.045822	2.781408
237.401838	2604.796246	17.774003	-0.045806	2.777293
237.431353	2596.783937	17.779008	-0.045807	2.773144
237.423432	2588.794038	17.784013	-0.045800	2.768997
237.451635	2580.842450	17.789018	-0.045800	2.764867
237.201889	2572.908703	17.794023	-0.045749	2.760723
237.303819	2564.933280	17.799027	-0.045762	2.756572
237.369995	2556.903543	17.804032	-0.045770	2.752384
237.566091	2548.872897	17.809037	-0.045801	2.748198
237.203823	2540.939469	17.814042	-0.045728	2.744021
237.026624	2532.997394	17.819047	-0.045690	2.739845
237.053970	2525.021063	17.824051	-0.045690	2.735658
237.206691	2517.002752	17.829056	-0.045713	2.731450
237.324511	2509.023403	17.834061	-0.045730	2.727253
236.983967	2501.103121	17.839066	-0.045662	2.723053
236.861016	2493.156051	17.844071	-0.045634	2.718845
237.040802	2485.167138	17.849075	-0.045662	2.714628
236.986543	2477.167621	17.854080	-0.045647	2.710384
236.829867	2469.215389	17.859085	-0.045612	2.706152
237.064911	2461.224668	17.864090	-0.045651	2.701918
236.842730	2453.274918	17.869095	-0.045604	2.697670
236.879043	2445.304035	17.874099	-0.045606	2.693420
237.027374	2437.260247	17.879104	-0.045628	2.689132
237.059168	2429.308125	17.884109	-0.045629	2.684879
237.011571	2421.373630	17.889114	-0.045615	2.680623
236.931206	2413.415094	17.894119	-0.045595	2.676345
237.032298	2405.431997	17.899123	-0.045609	2.672059
236.772670	2397.470027	17.904128	-0.045555	2.667754
236.761230	2389.497474	17.909133	-0.045548	2.663452
236.728394	2381.530047	17.914138	-0.045537	2.659145
236.468805	2373.601789	17.919143	-0.045483	2.654837
236.309380	2365.633890	17.924147	-0.045448	2.650507
236.371415	2357.634459	17.929152	-0.045455	2.646168
236.319436	2349.649622	17.934157	-0.045440	2.641822
236.330997	2341.699841	17.939162	-0.045437	2.637492
236.430530	2333.682993	17.944167	-0.045450	2.633124
236.332406	2325.731105	17.949171	-0.045427	2.628771
236.016047	2317.779775	17.954176	-0.045363	2.624397
236.040075	2309.823260	17.959181	-0.045362	2.620035
236.412999	2301.825823	17.964186	-0.045426	2.615668
235.720226	2293.933655	17.969191	-0.045292	2.611277
235.950988	2285.916355	17.974195	-0.045330	2.606875
236.026822	2277.919217	17.979200	-0.045339	2.602465
236.026641	2269.955585	17.984205	-0.045334	2.598061
235.540073	2262.071554	17.989210	-0.045238	2.593659
235.724818	2253.908167	17.994215	-0.045267	2.589142
236.003709	2245.920117	17.999219	-0.045314	2.584722
235.634232	2238.040276	18.004224	-0.045240	2.580308
235.522763	2230.091358	18.009229	-0.045214	2.575866
235.028058	2222.218851	18.014234	-0.045117	2.571432
235.324257	2214.128634	18.019239	-0.045167	2.566925
235.389378	2206.175900	18.024243	-0.045174	2.562471
235.135544	2198.272373	18.029248	-0.045122	2.558013
235.320037	2190.271039	18.034253	-0.045151	2.553524
235.245124	2182.304130	18.039258	-0.045132	2.549028
235.154593	2174.316031	18.044263	-0.045110	2.544511
235.123856	2166.377502	18.049267	-0.045099	2.540019
234.805581	2158.464953	18.054272	-0.045034	2.535512
234.896052	2150.447546	18.059277	-0.045046	2.530967
235.249394	2142.438278	18.064282	-0.045107	2.526438
234.830823	2134.520663	18.069287	-0.045024	2.521896
235.056973	2126.563687	18.074291	-0.045061	2.517372
234.890153	2118.605218	18.079296	-0.045024	2.512809
235.033571	2110.602816	18.084301	-0.045046	2.508236
234.837108	2102.655534	18.089306	-0.045004	2.503660
234.889501	2094.671257	18.094311	-0.045009	2.499074
234.881174	2086.729817	18.099315	-0.045002	2.494499
234.741316	2078.762810	18.104320	-0.044971	2.489892
234.801921	2070.782815	18.109325	-0.044977	2.485283
234.665990	2062.876418	18.114330	-0.044947	2.480693
234.605809	2054.907342	18.119335	-0.044930	2.476065
235.257067	2046.841573	18.124339	-0.045046	2.471425
234.849719	2038.943340	18.129344	-0.044965	2.466794
234.887114	2030.977857	18.134349	-0.044967	2.462149
234.958367	2023.024512	18.139354	-0.044975	2.457504
234.785702	2015.074154	18.144359	-0.044938	2.452834
234.783453	2007.117837	18.149363	-0.044933	2.448165
234.594463	1999.191341	18.154368	-0.044892	2.443490
234.672150	1991.218558	18.159373	-0.044902	2.438799
234.770114	1983.260741	18.164378	-0.044915	2.434109
234.421881	1975.292089	18.169383	-0.044845	2.429369
234.416208	1967.310689	18.174387	-0.044838	2.424639
234.389492	1959.361323	18.179392	-0.044828	2.419918
234.393218	1951.404277	18.184397	-0.044824	2.415185
234.322676	1943.438738	18.189402	-0.044806	2.410431
234.266516	1935.465872	18.194407	-0.044790	2.405665
234.146781	1927.558014	18.199411	-0.044763	2.400923
234.125647	1919.600584	18.204416	-0.044754	2.396151
234.299953	1911.605467	18.209421	-0.044781	2.391361
234.437300	1903.623192	18.214426	-0.044801	2.386567
234.015813	1895.722683	18.219431	-0.044718	2.381767
233.832271	1887.826344	18.224435	-0.044678	2.376979
233.782466	1879.834209	18.229440	-0.044664	2.372135
233.951761	1871.818717	18.234445	-0.044690	2.367284
233.618907	1863.954588	18.239450	-0.044623	2.362474
233.802486	1855.944904	18.244455	-0.044652	2.357609
233.949313	1847.971434	18.249459	-0.044674	2.352752
233.772430	1840.006440	18.254464	-0.044636	2.347863
233.761335	1832.054848	18.259469	-0.044629	2.342986
233.697840	1824.134072	18.264474	-0.044612	2.338114
233.758656	1816.138881	18.269479	-0.044618	2.333196
233.592909	1808.218073	18.274483	-0.044582	2.328295
233.111571	1800.329105	18.279488	-0.044488	2.323376
233.428686	1792.326053	18.284493	-0.044541	2.318443
233.044877	1784.454081	18.289498	-0.044465	2.313522
233.331547	1776.414260	18.294503	-0.044513	2.308543
233.198135	1768.484293	18.299507	-0.044483	2.303586
233.532429	1760.468427	18.304512	-0.044540	2.298605
233.232624	1752.577848	18.309517	-0.044479	2.293637
233.108709	1744.644168	18.314522	-0.044451	2.288646
232.965194	1736.681757	18.319527	-0.044419	2.283624
233.003909	1728.773207	18.324531	-0.044421	2.278641
233.236852	1720.754210	18.329536	-0.044459	2.273594
233.304731	1712.754173	18.334541	-0.044467	2.268534
233.232499	1704.822182	18.339546	-0.044448	2.263493
232.817770	1696.937118	18.344551	-0.044366	2.258441
233.597922	1688.864406	18.349555	-0.044506	2.253364
233.417399	1680.943917	18.354560	-0.044467	2.248286
233.604146	1672.986985	18.359565	-0.044497	2.243207
233.485805	1665.092730	18.364570	-0.044470	2.238130
233.408157	1657.158625	18.369575	-0.044450	2.233018
233.409637	1649.222392	18.374579	-0.044445	2.227901
233.038382	1641.318834	18.379584	-0.044371	2.222759
233.108801	1633.364448	18.384589	-0.044379	2.217613
232.876873	1625.467381	18.389594	-0.044331	2.212464
232.695341	1617.505768	18.394599	-0.044292	2.207265
232.601023	1609.588895	18.399603	-0.044269	2.202092
232.969094	1601.570888	18.404608	-0.044333	2.196883
232.667268	1593.681387	18.409613	-0.044271	2.191683
232.799740	1585.700082	18.414618	-0.044291	2.186452
232.834579	1577.738666	18.419623	-0.044292	2.181212
232.767661	1569.815592	18.424627	-0.044275	2.175975
232.383783	1561.925840	18.429632	-0.044198	2.170717
232.602751	1553.932496	18.434637	-0.044234	2.165435
231.971147	1546.123549	18.439642	-0.044111	2.160182
232.173531	1538.107912	18.444647	-0.044143	2.154858
232.330026	1530.134377	18.449651	-0.044167	2.149544
232.375025	1522.181810	18.454656	-0.044171	2.144221
231.849281	1514.345125	18.459661	-0.044068	2.138906
231.985099	1506.380713	18.464666	-0.044088	2.133557
232.386113	1498.336855	18.469671	-0.044157	2.128167
232.427529	1490.419920	18.474675	-0.044160	2.122813
232.452004	1482.478020	18.479680	-0.044159	2.117428
232.443566	1474.560831	18.484685	-0.044153	2.112042
232.434504	1466.597380	18.489690	-0.044146	2.106611
232.241093	1458.676478	18.494695	-0.044105	2.101177
232.277516	1450.756363	18.499699	-0.044106	2.095752
232.246947	1442.822239	18.504704	-0.044096	2.090297
232.300522	1434.859886	18.509709	-0.044100	2.084816
232.317902	1426.969059	18.514714	-0.044099	2.079367
231.585925	1419.177091	18.519719	-0.043957	2.073896
231.875700	1411.163266	18.524723	-0.044006	2.068360
231.885521	1403.209059	18.529728	-0.044003	2.062822
232.049775	1395.249014	18.534733	-0.044028	2.057281
232.134145	1387.320460	18.539738	-0.044039	2.051739
231.654580	1379.456379	18.544743	-0.043944	2.046169
231.587948	1371.556226	18.549747	-0.043927	2.040601
231.444719	1363.646798	18.554752	-0.043895	2.035003
231.354983	1355.708358	18.559757	-0.043873	2.029375
231.446057	1347.750705	18.564762	-0.043885	2.023736
231.298301	1339.847054	18.569767	-0.043852	2.018095
231.047499	1331.960804	18.574771	-0.043801	2.012440
231.246293	1323.960343	18.579776	-0.043832	2.006735
231.556127	1315.986541	18.584781	-0.043885	2.001044
231.288650	1308.141143	18.589786	-0.043830	1.995368
231.323791	1300.183470	18.594791	-0.043831	1.989627
231.461417	1292.248888	18.599795	-0.043852	1.983898
231.225705	1284.377724	18.604800	-0.043803	1.978157
230.887601	1276.531218	18.609805	-0.043735	1.972406
230.802634	1268.592813	18.614810	-0.043714	1.966599
230.985329	1260.640870	18.619815	-0.043743	1.960794
230.903371	1252.763139	18.624819	-0.043723	1.954998
230.763335	1244.832102	18.629824	-0.043691	1.949138
230.881672	1236.869581	18.634829	-0.043708	1.943266
231.320169	1228.887693	18.639834	-0.043785	1.937398
231.188719	1220.995853	18.644839	-0.043755	1.931515
231.368025	1213.046815	18.649843	-0.043783	1.925607
231.282740	1205.161681	18.654848	-0.043762	1.919698
231.119850	1197.300596	18.659853	-0.043727	1.913780
230.899545	1189.421103	18.664858	-0.043681	1.907823
231.033580	1181.464573	18.669863	-0.043701	1.901830
230.910797	1173.589175	18.674867	-0.043673	1.895850
230.797111	1165.689521	18.679872	-0.043646	1.889834
230.629854	1157.811206	18.684877	-0.043610	1.883808
230.732519	1149.910001	18.689882	-0.043624	1.877777
230.470712	1142.031766	18.694887	-0.043570	1.871701
230.666169	1134.071546	18.699891	-0.043602	1.865597
230.718488	1126.146024	18.704896	-0.043606	1.859482
230.385035	1118.310801	18.709901	-0.043539	1.853371
230.770253	1110.333557	18.714906	-0.043606	1.847216
230.787419	1102.421442	18.719911	-0.043604	1.841046
230.843298	1094.549335	18.724915	-0.043609	1.834892
230.748613	1086.670044	18.729920	-0.043586	1.828693
230.415390	1078.813856	18.734925	-0.043519	1.822462
230.500116	1070.918312	18.739930	-0.043530	1.816230
230.374942	1063.015113	18.744935	-0.043502	1.809944
230.253138	1055.152029	18.749939	-0.043474	1.803669
230.426615	1047.228945	18.754944	-0.043501	1.797360
230.259090	1039.352321	18.759949	-0.043465	1.791024
230.157265	1031.447157	18.764954	-0.043441	1.784651
229.868775	1023.610008	18.769959	-0.043382	1.778286
229.819418	1015.729378	18.774963	-0.043368	1.771894
229.714954	1007.814917	18.779968	-0.043343	1.765443
229.946967	999.904433	18.784973	-0.043381	1.759016
230.246770	991.989526	18.789978	-0.043432	1.752570
229.894576	984.142052	18.794983	-0.043361	1.746071
230.010583	976.253727	18.799987	-0.043378	1.739575
229.795335	968.418978	18.804992	-0.043332	1.733056
229.664467	960.548303	18.809997	-0.043303	1.726493
229.711411	952.676416	18.815002	-0.043307	1.719928
229.098624	944.910565	18.820007	-0.043188	1.713339
229.317262	936.966674	18.825011	-0.043223	1.706685
229.192669	929.084375	18.830016	-0.043195	1.700012
229.407403	921.177859	18.835021	-0.043230	1.693337
229.231821	913.320236	18.840026	-0.043192	1.686625
229.290389	905.428019	18.845031	-0.043198	1.679888
229.363635	897.578986	18.850035	-0.043206	1.673163
229.256089	889.714030	18.855040	-0.043181	1.666372
229.252326	881.853472	18.860045	-0.043175	1.659572
229.053744	874.047374	18.865050	-0.043133	1.652764
229.310604	866.104012	18.870055	-0.043176	1.645871
229.396450	858.262738	18.875059	-0.043187	1.639015
229.027221	850.461646	18.880064	-0.043113	1.632102
229.052568	842.555187	18.885069	-0.043113	1.625121
228.894312	834.754564	18.890074	-0.043078	1.618179
229.137998	826.840046	18.895079	-0.043119	1.611162
229.126936	818.998919	18.900083	-0.043111	1.604144
228.830820	811.214571	18.905088	-0.043051	1.597105
228.802350	803.361923	18.910093	-0.043041	1.590012
228.500018	795.572520	18.915098	-0.042980	1.582904
228.400774	787.730812	18.920103	-0.042956	1.575746
228.147682	779.937410	18.925107	-0.042904	1.568578
228.319938	772.041449	18.930112	-0.042931	1.561345
228.794194	764.127068	18.935117	-0.043014	1.554106
228.806091	756.298356	18.940122	-0.043011	1.546844
228.307001	748.555991	18.945127	-0.042913	1.539551
228.587743	740.682775	18.950131	-0.042960	1.532219
228.626615	732.834298	18.955136	-0.042963	1.524838
228.496162	725.061853	18.960141	-0.042933	1.517467
227.996303	717.337280	18.965146	-0.042835	1.510049
227.815226	709.522559	18.970151	-0.042796	1.502557
227.732167	701.719850	18.975155	-0.042776	1.495054
227.709832	693.888412	18.980160	-0.042767	1.487495
227.958395	686.025107	18.985165	-0.042808	1.479910
227.692510	678.271223	18.990170	-0.042753	1.472310
227.866530	670.387811	18.995175	-0.042781	1.464615
227.840125	662.604125	19.000179	-0.042771	1.456945
227.278861	654.893243	19.005184	-0.042661	1.449219
227.555755	647.034107	19.010189	-0.042708	1.441441
227.984906	639.177296	19.015194	-0.042783	1.433649
227.868774	631.392723	19.020199	-0.042756	1.425797
227.760188	623.667816	19.025203	-0.042731	1.417962
227.747944	615.872494	19.030208	-0.042723	1.410029
227.855826	608.075131	19.035213	-0.042738	1.402069
227.768480	600.344696	19.040218	-0.042717	1.394099
227.422656	592.615585	19.045223	-0.042648	1.386040
227.391235	584.865334	19.050227	-0.042637	1.377966
227.335933	577.088890	19.055232	-0.042622	1.369813
226.654406	569.449040	19.060237	-0.042490	1.361645
226.703020	561.683722	19.065242	-0.042494	1.353424
227.078369	553.816860	19.070247	-0.042559	1.345103
227.057007	546.096650	19.075251	-0.042550	1.336816
227.298989	538.294410	19.080256	-0.042590	1.328436
226.844286	530.654917	19.085261	-0.042500	1.320053
227.044354	522.848028	19.090266	-0.042532	1.311554
227.070721	515.054348	19.095271	-0.042532	1.302981
226.862789	507.382320	19.100275	-0.042488	1.294443
226.735885	499.677627	19.105280	-0.042460	1.285827
226.455107	492.020909	19.110285	-0.042403	1.277178
226.378999	484.324531	19.115290	-0.042384	1.268464
226.379776	476.603796	19.120295	-0.042379	1.259676
226.445584	468.888950	19.125299	-0.042386	1.250846
226.494792	461.189591	19.130304	-0.042390	1.241968
226.367968	453.536957	19.135309	-0.042362	1.233046
226.106889	445.892202	19.140314	-0.042308	1.224041
226.484258	438.140401	19.145319	-0.042373	1.214971
226.099821	430.545156	19.150323	-0.042297	1.205865
226.006292	422.904800	19.155328	-0.042274	1.196695
226.136350	415.216235	19.160333	-0.042294	1.187442
226.279128	407.553713	19.165338	-0.042315	1.178151
225.978914	399.956092	19.170343	-0.042255	1.168773
226.012122	392.333640	19.175347	-0.042256	1.159358
225.837431	384.719097	19.180352	-0.042218	1.149832
225.921261	377.068226	19.185357	-0.042229	1.140236
225.937756	369.456527	19.190362	-0.042227	1.130594
225.545212	361.920618	19.195367	-0.042149	1.120876
225.207188	354.403262	19.200371	-0.042081	1.111109
225.584897	346.726550	19.205376	-0.042147	1.101209
225.677240	339.136104	19.210381	-0.042159	1.091267
225.373057	331.632240	19.215386	-0.042098	1.081258
225.386423	324.072161	19.220391	-0.042095	1.071154
225.483352	316.500038	19.225395	-0.042108	1.060956
225.468608	308.966270	19.230400	-0.042101	1.050686
225.257268	301.489406	19.235405	-0.042057	1.040346
224.871616	294.054230	19.240410	-0.041980	1.029918
224.715787	286.567249	19.245415	-0.041946	1.019366
225.094504	279.006777	19.250419	-0.042012	1.008732
224.732263	271.604480	19.255424	-0.041939	0.998027
224.718629	264.116404	19.260429	-0.041932	0.987168
224.795265	256.653328	19.265434	-0.041942	0.976250
224.317214	249.296155	19.270439	-0.041848	0.965221
224.245354	241.890462	19.275443	-0.041830	0.954098
224.308770	234.462102	19.280448	-0.041837	0.942845
223.725736	227.177588	19.285453	-0.041723	0.931504
223.693774	219.806222	19.290458	-0.041713	0.920038
223.728970	212.435310	19.295463	-0.041714	0.908447
223.395101	205.156667	19.300467	-0.041648	0.896750
222.584675	197.970621	19.305472	-0.041492	0.884912
222.255180	190.718531	19.310477	-0.041426	0.872944
221.985688	183.471615	19.315482	-0.041371	0.860836
221.081141	176.350224	19.320487	-0.041198	0.848578
220.516865	169.196738	19.325491	-0.041088	0.836187
219.830651	162.057688	19.330496	-0.040956	0.823598
219.582416	154.875028	19.335501	-0.040905	0.810872
218.909935	147.809502	19.340506	-0.040775	0.798020
217.905405	140.821996	19.345511	-0.040584	0.784991
217.650447	133.726144	19.350515	-0.040532	0.771788
216.969759	126.733772	19.355520	-0.040401	0.758408
216.137944	119.809082	19.360525	-0.040241	0.744866
216.140881	112.755140	19.365530	-0.040237	0.731111
215.553905	105.848314	19.370535	-0.040123	0.717176
214.948323	98.999245	19.375539	-0.040006	0.703076
214.001393	92.246798	19.380544	-0.039826	0.688761
213.264142	85.497826	19.385549	-0.039684	0.674230
212.405974	78.976473	19.390554	-0.039520	0.659827