Fri Apr 16 19:41:25 2021

Number of Points = 3642
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
-0.443362	0.121860	0.000000	0.000058	0.311121

0.508266	-0.067328	0.005005	-0.000119	0.311045
0.010064	-0.025859	0.010010	-0.000026	0.310817
-0.735209	0.111221	0.015014	0.000113	0.310825
0.368175	-0.091591	0.020019	-0.000093	0.310815
0.304196	-0.081600	0.025024	-0.000081	0.310807
-0.441734	0.054507	0.030029	0.000058	0.310810
-0.067131	-0.012996	0.035034	-0.000012	0.310813
-0.169326	0.004270	0.040038	0.000007	0.310807
-0.645283	0.095536	0.045043	0.000096	0.310830
-0.498390	0.067497	0.050048	0.000068	0.310823
0.423941	-0.102727	0.055053	-0.000103	0.310811
-0.142367	0.001415	0.060058	0.000002	0.310817
-0.268967	0.020935	0.065062	0.000025	0.310801
0.045388	-0.029974	0.070067	-0.000033	0.310830
-0.069842	-0.019864	0.075072	-0.000012	0.310780
-0.757121	0.059936	0.080077	0.000116	0.310570
-1.183175	0.143318	0.085082	0.000195	0.310598
-0.364169	-0.010450	0.090086	0.000043	0.310575
-0.622553	0.037049	0.095091	0.000091	0.310578
-1.243906	0.151184	0.100096	0.000207	0.310584
-0.575428	0.029205	0.105101	0.000082	0.310582
-0.929593	0.097147	0.110106	0.000148	0.310599
-1.136050	0.130880	0.115110	0.000186	0.310581
-0.418652	-0.045875	0.120115	0.000053	0.310365
-0.675896	-0.022610	0.125120	0.000101	0.310256
-0.787308	-0.006721	0.130125	0.000121	0.310236
0.028344	-0.160323	0.135130	-0.000030	0.310211
-0.003042	-0.150916	0.140134	-0.000025	0.310228
-0.210376	-0.166017	0.145139	0.000014	0.309982
-0.959997	-0.045997	0.150144	0.000153	0.309907
-0.207132	-0.183535	0.155149	0.000013	0.309904
-0.391664	-0.147197	0.160154	0.000048	0.309917
-0.989373	-0.072297	0.165158	0.000159	0.309760
-1.133949	-0.081581	0.170163	0.000186	0.309594
-0.921116	-0.118498	0.175168	0.000146	0.309602
-0.938909	-0.119263	0.180173	0.000149	0.309584
-1.015371	-0.113038	0.185178	0.000163	0.309548
-0.230615	-0.312902	0.190182	0.000017	0.309281
-0.046036	-0.344521	0.195187	-0.000017	0.309290
-0.746104	-0.216637	0.200192	0.000113	0.309293
-0.555124	-0.310585	0.205197	0.000078	0.309016
-0.212514	-0.382179	0.210202	0.000014	0.308972
-1.229623	-0.197687	0.215206	0.000203	0.308971
-1.186153	-0.246360	0.220211	0.000195	0.308780
-0.904421	-0.323797	0.225216	0.000143	0.308658
-1.283877	-0.253003	0.230221	0.000213	0.308666
-1.300141	-0.275338	0.235226	0.000216	0.308548
-0.731566	-0.426574	0.240230	0.000110	0.308323
-0.981206	-0.379380	0.245235	0.000157	0.308332
-1.365888	-0.340443	0.250240	0.000228	0.308187
-0.323791	-0.562965	0.255245	0.000034	0.308031
-0.425754	-0.539252	0.260250	0.000053	0.308056
-1.249343	-0.457288	0.265254	0.000207	0.307738
-1.302011	-0.452871	0.270259	0.000216	0.307714
-0.326357	-0.652071	0.275264	0.000035	0.307611
-0.703306	-0.631341	0.280269	0.000105	0.307387
-1.298356	-0.522585	0.285274	0.000216	0.307390
-1.269387	-0.588465	0.290278	0.000210	0.307105
-0.805054	-0.680224	0.295283	0.000124	0.307070
-1.435840	-0.599206	0.300288	0.000241	0.306912
-1.444367	-0.625803	0.305293	0.000243	0.306779
-1.010760	-0.715216	0.310298	0.000162	0.306729
-1.099283	-0.764420	0.315302	0.000178	0.306421
-1.100490	-0.762215	0.320307	0.000179	0.306431
-0.281189	-0.977701	0.325312	0.000026	0.306116
-0.409611	-0.959653	0.330317	0.000050	0.306092
-1.130572	-0.889856	0.335322	0.000184	0.305802
-0.854807	-0.946532	0.340326	0.000133	0.305771
-0.821228	-0.997047	0.345331	0.000127	0.305561
-1.413290	-0.900082	0.350336	0.000237	0.305511
-1.790082	-0.896067	0.355341	0.000307	0.305206
-1.334276	-0.982491	0.360346	0.000222	0.305189
-1.010778	-1.108347	0.365350	0.000162	0.304871
-1.481886	-1.029080	0.370355	0.000249	0.304841
-0.484609	-1.273926	0.375360	0.000064	0.304539
-0.442441	-1.310110	0.380365	0.000056	0.304404
-0.657718	-1.302925	0.385370	0.000096	0.304253
-1.183817	-1.262933	0.390374	0.000194	0.303988
-0.754313	-1.359027	0.395379	0.000114	0.303902
-1.542221	-1.273028	0.400384	0.000261	0.303630
-1.895612	-1.233468	0.405389	0.000326	0.303513
-2.004424	-1.255058	0.410394	0.000347	0.303316
-1.910214	-1.307591	0.415398	0.000329	0.303147
-1.659460	-1.381601	0.420403	0.000282	0.303012
-1.829191	-1.406500	0.425408	0.000314	0.302745
-1.818714	-1.432348	0.430413	0.000312	0.302631
-2.212337	-1.415670	0.435418	0.000385	0.302369
-1.918398	-1.498185	0.440422	0.000330	0.302230
-1.665999	-1.581950	0.445427	0.000283	0.302049
-1.987159	-1.574106	0.450432	0.000343	0.301807
-2.305593	-1.538818	0.455437	0.000402	0.301699
-1.576802	-1.729781	0.460442	0.000267	0.301418
-1.929230	-1.708917	0.465446	0.000332	0.301211
-2.109869	-1.704627	0.470451	0.000366	0.301074
-2.571424	-1.682531	0.475456	0.000452	0.300777
-2.698642	-1.681290	0.480461	0.000476	0.300672
-2.953567	-1.656355	0.485466	0.000523	0.300569
-2.421245	-1.820657	0.490470	0.000424	0.300244
-2.671821	-1.803289	0.495475	0.000471	0.300108
-2.533758	-1.879714	0.500480	0.000445	0.299861
-2.691899	-1.903550	0.505485	0.000474	0.299607
-2.525753	-1.962732	0.510490	0.000443	0.299468
-2.622932	-1.988127	0.515494	0.000461	0.299260
-2.864662	-2.001826	0.520499	0.000506	0.298981
-3.463659	-1.924103	0.525504	0.000618	0.298831
-4.552304	-1.768795	0.530509	0.000820	0.298625
-4.511049	-1.817354	0.535514	0.000813	0.298426
-4.997278	-1.755463	0.540518	0.000903	0.298298
-5.203042	-1.771909	0.545523	0.000941	0.298037
-4.892278	-1.848677	0.550528	0.000884	0.297938
-5.411493	-1.810361	0.555533	0.000980	0.297666
-5.208238	-1.876345	0.560538	0.000942	0.297525
-6.169416	-1.732445	0.565542	0.001121	0.297376
-5.868860	-1.832191	0.570547	0.001065	0.297156
-6.985538	-1.650745	0.575552	0.001273	0.297052
-6.937692	-1.703662	0.580557	0.001264	0.296836
-6.410988	-1.815988	0.585562	0.001166	0.296755
-7.556504	-1.664352	0.590566	0.001379	0.296480
-7.571950	-1.669511	0.595571	0.001382	0.296441
-7.046465	-1.821124	0.600576	0.001284	0.296167
-7.402189	-1.767818	0.605581	0.001350	0.296112
-7.787768	-1.755343	0.610586	0.001422	0.295831
-7.805469	-1.760015	0.615590	0.001425	0.295792
-8.020059	-1.765910	0.620595	0.001465	0.295573
-8.551603	-1.672525	0.625600	0.001564	0.295557
-8.322820	-1.777402	0.630605	0.001522	0.295247
-8.206755	-1.805607	0.635610	0.001500	0.295212
-8.886266	-1.742634	0.640614	0.001626	0.294916
-8.858733	-1.753372	0.645619	0.001621	0.294888
-8.981223	-1.787493	0.650624	0.001644	0.294611
-9.326363	-1.732402	0.655629	0.001708	0.294574
-9.187849	-1.804560	0.660634	0.001682	0.294343
-9.263446	-1.808006	0.665638	0.001696	0.294259
-9.290452	-1.850560	0.670643	0.001702	0.294026
-10.327123	-1.677621	0.675648	0.001894	0.293949
-10.286734	-1.725867	0.680653	0.001887	0.293748
-9.988077	-1.805385	0.685658	0.001831	0.293624
-10.492547	-1.741333	0.690662	0.001925	0.293488
-11.071298	-1.667538	0.695667	0.002033	0.293333
-10.394231	-1.808964	0.700672	0.001907	0.293243
-10.658174	-1.806954	0.705677	0.001956	0.293016
-10.697539	-1.808431	0.710682	0.001963	0.292974
-11.266534	-1.767266	0.715686	0.002069	0.292666
-10.911203	-1.828241	0.720691	0.002003	0.292684
-11.579053	-1.767862	0.725696	0.002127	0.292383
-11.757590	-1.739406	0.730701	0.002160	0.292363
-11.387024	-1.851021	0.735706	0.002091	0.292144
-12.066828	-1.749256	0.740710	0.002218	0.292036
-11.739392	-1.838028	0.745715	0.002157	0.291891
-12.277994	-1.769830	0.750720	0.002257	0.291744
-11.960882	-1.846788	0.755725	0.002198	0.291649
-12.967448	-1.706545	0.760730	0.002385	0.291437
-12.751261	-1.751116	0.765734	0.002345	0.291411
-12.425824	-1.867743	0.770739	0.002285	0.291125
-12.748347	-1.815038	0.775744	0.002345	0.291096
-13.249536	-1.769751	0.780749	0.002438	0.290869
-12.900307	-1.849958	0.785754	0.002373	0.290785
-13.029290	-1.851484	0.790758	0.002397	0.290661
-13.770014	-1.739454	0.795763	0.002535	0.290549
-13.424477	-1.816543	0.800768	0.002470	0.290478
-13.534105	-1.857655	0.805773	0.002491	0.290174
-13.617244	-1.841129	0.810778	0.002506	0.290181
-14.300083	-1.774393	0.815782	0.002633	0.289895
-13.806296	-1.868104	0.820787	0.002541	0.289875
-13.952756	-1.881959	0.825792	0.002568	0.289673
-14.611037	-1.789862	0.830797	0.002691	0.289536
-14.128732	-1.896734	0.835802	0.002601	0.289440
-14.636143	-1.843877	0.840806	0.002696	0.289243
-14.562099	-1.857475	0.845811	0.002682	0.289243
-15.403319	-1.768195	0.850816	0.002838	0.288924
-15.208294	-1.803455	0.855821	0.002802	0.288926
-15.343635	-1.816460	0.860826	0.002827	0.288737
-15.833378	-1.753602	0.865830	0.002918	0.288606
-15.542644	-1.813132	0.870835	0.002864	0.288573
-16.342212	-1.721153	0.875840	0.003013	0.288305
-16.179940	-1.752919	0.880845	0.002983	0.288294
-16.232206	-1.775350	0.885850	0.002992	0.288134
-16.066447	-1.834230	0.890854	0.002961	0.287990
-16.392385	-1.782598	0.895859	0.003022	0.287952
-16.739871	-1.779385	0.900864	0.003087	0.287650
-16.609695	-1.801224	0.905869	0.003062	0.287660
-16.731015	-1.817464	0.910874	0.003085	0.287467
-17.435064	-1.714241	0.915878	0.003216	0.287343
-17.561064	-1.688298	0.920883	0.003239	0.287358
-17.903543	-1.688307	0.925888	0.003303	0.287044
-17.762491	-1.716539	0.930893	0.003277	0.287032
-17.471908	-1.788801	0.935898	0.003223	0.286934
-17.927427	-1.745291	0.940902	0.003307	0.286736
-17.961746	-1.736536	0.945907	0.003314	0.286749
-17.910949	-1.797792	0.950912	0.003304	0.286486
-18.044870	-1.790120	0.955917	0.003329	0.286402
-17.996973	-1.812618	0.960922	0.003320	0.286333
-18.565889	-1.758702	0.965926	0.003426	0.286082
-18.070335	-1.848504	0.970931	0.003334	0.286084
-18.397465	-1.834213	0.975936	0.003395	0.285855
-18.786578	-1.781187	0.980941	0.003467	0.285766
-18.983851	-1.753347	0.985946	0.003504	0.285726
-19.239575	-1.747250	0.990950	0.003551	0.285521
-19.235589	-1.744823	0.995955	0.003551	0.285537
-19.300586	-1.775306	1.000960	0.003563	0.285323
-19.658092	-1.736962	1.005965	0.003629	0.285188
-19.123495	-1.836271	1.010970	0.003530	0.285177
-19.666414	-1.799725	1.015974	0.003631	0.284862
-19.870369	-1.760333	1.020979	0.003669	0.284874
-19.996392	-1.767191	1.025984	0.003692	0.284723
-20.179646	-1.772063	1.030989	0.003726	0.284529
-19.810957	-1.839433	1.035994	0.003657	0.284527
-20.112842	-1.835430	1.040998	0.003714	0.284268
-20.061097	-1.849648	1.046003	0.003704	0.284244
-20.471250	-1.801369	1.051008	0.003780	0.284110
-21.177983	-1.709711	1.056013	0.003912	0.283923
-21.043985	-1.732383	1.061018	0.003887	0.283932
-20.883873	-1.811390	1.066022	0.003857	0.283677
-20.742017	-1.854139	1.071027	0.003831	0.283591
-20.523282	-1.911936	1.076032	0.003790	0.283499
-21.257786	-1.821987	1.081037	0.003927	0.283277
-21.552449	-1.766676	1.086042	0.003981	0.283286
-21.845085	-1.753659	1.091046	0.004036	0.283081
-21.434499	-1.847083	1.096051	0.003959	0.282985
-21.982071	-1.753560	1.101056	0.004061	0.282954
-22.229003	-1.766876	1.106061	0.004107	0.282656
-21.872564	-1.831818	1.111066	0.004041	0.282656
-22.038395	-1.834901	1.116070	0.004072	0.282486
-21.960254	-1.881273	1.121075	0.004057	0.282321
-22.002129	-1.878619	1.126080	0.004065	0.282296
-22.107222	-1.920264	1.131085	0.004084	0.281984
-22.777718	-1.792744	1.136090	0.004209	0.282013
-22.419250	-1.896619	1.141094	0.004142	0.281815
-22.395413	-1.921813	1.146099	0.004138	0.281708
-22.697795	-1.880556	1.151104	0.004194	0.281638
-23.584865	-1.768087	1.156109	0.004359	0.281387
-23.229659	-1.832629	1.161114	0.004293	0.281387
-23.896074	-1.744428	1.166118	0.004417	0.281218
-23.769411	-1.793347	1.171123	0.004393	0.281085
-23.432246	-1.855037	1.176128	0.004331	0.281083
-24.008926	-1.807665	1.181133	0.004438	0.280787
-24.055769	-1.805882	1.186138	0.004447	0.280752
-24.087069	-1.815502	1.191142	0.004452	0.280674
-24.071272	-1.847249	1.196147	0.004449	0.280525
-24.459216	-1.776329	1.201152	0.004522	0.280527
-25.017553	-1.717137	1.206157	0.004625	0.280309
-24.817659	-1.775674	1.211162	0.004588	0.280194
-24.946153	-1.755729	1.216166	0.004612	0.280177
-24.622478	-1.872361	1.221171	0.004552	0.279878
-24.827189	-1.839391	1.226176	0.004590	0.279856
-24.972630	-1.841222	1.231181	0.004617	0.279710
-25.387348	-1.798710	1.236186	0.004694	0.279540
-25.921719	-1.698610	1.241190	0.004794	0.279556
-25.860882	-1.747035	1.246195	0.004782	0.279362
-26.421864	-1.661780	1.251200	0.004887	0.279276
-26.072303	-1.728390	1.256205	0.004821	0.279260
-25.663054	-1.859024	1.261210	0.004745	0.278969
-26.522086	-1.710672	1.266214	0.004905	0.278928
-26.282739	-1.764846	1.271219	0.004861	0.278873
-26.691784	-1.739546	1.276224	0.004937	0.278618
-27.224935	-1.638169	1.281229	0.005036	0.278642
-26.753333	-1.746687	1.286234	0.004948	0.278523
-26.748437	-1.794593	1.291238	0.004947	0.278279
-26.445438	-1.847670	1.296243	0.004891	0.278290
-27.464022	-1.700277	1.301248	0.005080	0.278093
-28.004642	-1.614999	1.306253	0.005181	0.278026
-27.419084	-1.721405	1.311258	0.005072	0.278026
-28.141618	-1.641844	1.316262	0.005206	0.277756
-28.870292	-1.518539	1.321267	0.005342	0.277709
-28.045723	-1.672742	1.326272	0.005188	0.277687
-27.976694	-1.726248	1.331277	0.005175	0.277473
-28.512668	-1.647279	1.336282	0.005275	0.277377
-28.523198	-1.647811	1.341286	0.005277	0.277364
-28.153696	-1.762329	1.346291	0.005208	0.277117
-28.428425	-1.728740	1.351296	0.005259	0.277032
-28.858678	-1.650827	1.356301	0.005339	0.277031
-28.341869	-1.797380	1.361306	0.005243	0.276756
-28.963667	-1.685131	1.366310	0.005359	0.276752
-28.468846	-1.801322	1.371315	0.005267	0.276615
-28.905950	-1.762775	1.376320	0.005348	0.276401
-29.001790	-1.742212	1.381325	0.005366	0.276417
-29.045421	-1.776733	1.386330	0.005374	0.276195
-29.594776	-1.695636	1.391334	0.005476	0.276097
-28.925070	-1.822694	1.396339	0.005352	0.276069
-29.033699	-1.859002	1.401344	0.005372	0.275775
-29.342165	-1.802816	1.406349	0.005429	0.275776
-29.482220	-1.801558	1.411354	0.005455	0.275649
-29.703773	-1.782939	1.416358	0.005496	0.275535
-29.763256	-1.773695	1.421363	0.005507	0.275527
-30.165431	-1.761312	1.426368	0.005582	0.275208
-29.935791	-1.805994	1.431373	0.005540	0.275193
-30.194743	-1.783307	1.436378	0.005588	0.275065
-30.776739	-1.714342	1.441382	0.005696	0.274871
-30.332148	-1.792540	1.446387	0.005613	0.274885
-30.321811	-1.845769	1.451392	0.005611	0.274615
-31.012435	-1.732499	1.456397	0.005740	0.274550
-30.783698	-1.784935	1.461402	0.005697	0.274493
-30.457926	-1.892392	1.466406	0.005637	0.274239
-30.819633	-1.823303	1.471411	0.005704	0.274256
-31.491998	-1.749193	1.476416	0.005829	0.274002
-31.730585	-1.719844	1.481421	0.005873	0.273928
-31.608659	-1.742119	1.486426	0.005851	0.273928
-31.623870	-1.801371	1.491430	0.005853	0.273600
-31.406536	-1.838490	1.496435	0.005813	0.273613
-31.613659	-1.833289	1.501440	0.005851	0.273441
-32.357033	-1.726195	1.506445	0.005990	0.273293
-31.995510	-1.791565	1.511450	0.005922	0.273295
-32.112542	-1.822336	1.516454	0.005944	0.273019
-32.020293	-1.844215	1.521459	0.005927	0.272992
-31.883137	-1.900817	1.526464	0.005901	0.272825
-32.396001	-1.839513	1.531469	0.005997	0.272655
-32.207588	-1.873800	1.536474	0.005962	0.272655
-33.181754	-1.753901	1.541478	0.006143	0.272351
-33.420174	-1.708638	1.546483	0.006187	0.272361
-33.218583	-1.761450	1.551488	0.006150	0.272276
-34.034566	-1.655912	1.556493	0.006302	0.272048
-33.578038	-1.740853	1.561498	0.006217	0.272038
-33.714686	-1.745620	1.566502	0.006242	0.271881
-33.867482	-1.741833	1.571507	0.006270	0.271753
-34.353798	-1.651178	1.576512	0.006361	0.271765
-34.898345	-1.596726	1.581517	0.006462	0.271527
-34.507814	-1.684518	1.586522	0.006389	0.271438
-34.545590	-1.681293	1.591526	0.006396	0.271419
-34.139629	-1.804501	1.596531	0.006321	0.271156
-34.784809	-1.694058	1.601536	0.006441	0.271119
-35.273117	-1.609061	1.606541	0.006532	0.271099
-35.116184	-1.692764	1.611546	0.006503	0.270804
-34.885556	-1.737285	1.616550	0.006460	0.270791
-35.100880	-1.713198	1.621555	0.006500	0.270710
-35.847332	-1.605802	1.626560	0.006639	0.270559
-35.598562	-1.652042	1.631565	0.006592	0.270554
-35.293914	-1.738269	1.636570	0.006536	0.270389
-36.196024	-1.608353	1.641574	0.006703	0.270206
-36.349023	-1.576604	1.646579	0.006732	0.270227
-36.274941	-1.621427	1.651584	0.006718	0.270060
-36.652854	-1.581618	1.656589	0.006788	0.269905
-36.720904	-1.567044	1.661594	0.006801	0.269917
-36.741263	-1.601741	1.666598	0.006805	0.269711
-36.796958	-1.615925	1.671603	0.006815	0.269580
-36.633505	-1.646475	1.676608	0.006785	0.269576
-36.812731	-1.653020	1.681613	0.006818	0.269366
-36.717680	-1.685869	1.686618	0.006800	0.269283
-36.767269	-1.679824	1.691622	0.006809	0.269267
-36.900096	-1.715312	1.696627	0.006834	0.268946
-37.057096	-1.687358	1.701632	0.006863	0.268943
-37.205837	-1.681862	1.706637	0.006891	0.268827
-37.231419	-1.714056	1.711642	0.006896	0.268629
-37.182616	-1.724098	1.716646	0.006887	0.268623
-37.080877	-1.785303	1.721651	0.006868	0.268393
-37.754903	-1.680118	1.726656	0.006993	0.268299
-38.317727	-1.575864	1.731661	0.007098	0.268309
-38.064398	-1.672660	1.736666	0.007051	0.268036
-38.434456	-1.607222	1.741670	0.007119	0.268026
-38.390592	-1.630355	1.746675	0.007111	0.267944
-38.347706	-1.688112	1.751680	0.007103	0.267674
-38.208958	-1.713139	1.756685	0.007077	0.267675
-38.145458	-1.758650	1.761690	0.007065	0.267492
-38.826195	-1.659661	1.766694	0.007192	0.267358
-38.725159	-1.675477	1.771699	0.007173	0.267372
-38.962151	-1.691800	1.776704	0.007217	0.267050
-39.130867	-1.662482	1.781709	0.007249	0.267043
-39.082934	-1.684095	1.786714	0.007240	0.266973
-39.701064	-1.611341	1.791718	0.007355	0.266758
-39.797753	-1.591414	1.796723	0.007373	0.266771
-39.629573	-1.649710	1.801728	0.007341	0.266621
-39.926172	-1.630814	1.806733	0.007397	0.266430
-39.902306	-1.634261	1.811738	0.007392	0.266435
-40.043017	-1.655109	1.816742	0.007418	0.266183
-40.088399	-1.659072	1.821747	0.007427	0.266117
-40.438804	-1.594908	1.826752	0.007492	0.266119
-40.700871	-1.606724	1.831757	0.007541	0.265796
-40.778149	-1.590139	1.836762	0.007555	0.265810
-41.156928	-1.527504	1.841766	0.007625	0.265776
-40.728564	-1.647874	1.846771	0.007546	0.265544
-40.798030	-1.636437	1.851776	0.007559	0.265538
-41.271426	-1.575175	1.856781	0.007647	0.265403
-41.593659	-1.550978	1.861786	0.007707	0.265215
-41.813609	-1.511244	1.866790	0.007747	0.265214
-41.430648	-1.608923	1.871795	0.007676	0.265061
-42.105196	-1.515483	1.876800	0.007802	0.264901
-42.150843	-1.507248	1.881805	0.007810	0.264901
-41.377808	-1.685279	1.886810	0.007666	0.264697
-41.776075	-1.640525	1.891814	0.007740	0.264545
-41.642070	-1.665361	1.896819	0.007715	0.264543
-41.448818	-1.753223	1.901824	0.007679	0.264255
-41.809164	-1.685703	1.906829	0.007746	0.264266
-41.359738	-1.805844	1.911834	0.007663	0.264055
-42.065168	-1.704771	1.916838	0.007794	0.263906
-42.170253	-1.690595	1.921843	0.007814	0.263879
-42.572265	-1.665151	1.926848	0.007888	0.263618
-42.722585	-1.638774	1.931853	0.007916	0.263613
-42.095850	-1.784484	1.936858	0.007800	0.263439
-42.534653	-1.734028	1.941862	0.007881	0.263277
-42.621014	-1.727260	1.946867	0.007897	0.263228
-42.716186	-1.753412	1.951872	0.007915	0.262989
-42.786731	-1.740593	1.956877	0.007928	0.262989
-43.302163	-1.688726	1.961882	0.008024	0.262759
-44.018631	-1.573886	1.966886	0.008157	0.262674
-43.257606	-1.720708	1.971891	0.008016	0.262628
-43.621819	-1.703021	1.976896	0.008083	0.262360
-43.981274	-1.639138	1.981901	0.008150	0.262352
-43.978215	-1.671235	1.986906	0.008150	0.262178
-44.109697	-1.675549	1.991910	0.008174	0.262022
-44.173122	-1.662723	1.996915	0.008186	0.262029
-44.381023	-1.676534	2.001920	0.008225	0.261744

-44.808827	-1.634818	2.011917	0.008304	0.261545
-44.424513	-1.735230	2.021914	0.008233	0.261376
-44.486351	-1.778228	2.031910	0.008244	0.261076
-44.831052	-1.736712	2.041907	0.008308	0.260959
-44.974821	-1.746536	2.051904	0.008335	0.260759
-44.762862	-1.804295	2.061901	0.008295	0.260653
-44.926818	-1.799346	2.071898	0.008326	0.260515
-45.024121	-1.782785	2.081894	0.008344	0.260509
-45.376005	-1.778182	2.091891	0.008409	0.260179
-45.330910	-1.788251	2.101888	0.008401	0.260169
-45.997212	-1.662897	2.111885	0.008525	0.260193
-45.566643	-1.742951	2.121882	0.008444	0.260184
-45.748319	-1.755814	2.131878	0.008478	0.259928
-46.330793	-1.657935	2.141875	0.008586	0.259884
-46.595444	-1.609924	2.151872	0.008636	0.259883
-45.987017	-1.723543	2.161869	0.008522	0.259867
-46.121523	-1.698493	2.171866	0.008547	0.259871
-46.007853	-1.670591	2.181862	0.008526	0.260142
-45.829413	-1.694386	2.191859	0.008493	0.260191
-46.113237	-1.643280	2.201856	0.008545	0.260188
-45.967799	-1.667985	2.211853	0.008518	0.260199
-46.126077	-1.639645	2.221850	0.008548	0.260196
-45.827310	-1.695441	2.231846	0.008492	0.260189
-45.700112	-1.695142	2.241843	0.008468	0.260320
-45.426797	-1.707997	2.251840	0.008417	0.260525
-45.031774	-1.781867	2.261837	0.008344	0.260515
-45.253802	-1.740434	2.271834	0.008385	0.260521
-44.963574	-1.791473	2.281830	0.008331	0.260531
-44.859198	-1.770595	2.291827	0.008311	0.260753
-45.405600	-1.668772	2.301824	0.008413	0.260767
-45.551612	-1.626006	2.311821	0.008440	0.260857
-45.513544	-1.586349	2.321818	0.008433	0.261116
-45.113883	-1.660933	2.331814	0.008358	0.261106
-44.560793	-1.709748	2.341811	0.008255	0.261394
-44.374781	-1.744801	2.351808	0.008221	0.261388
-44.322541	-1.719120	2.361805	0.008211	0.261583
-44.139288	-1.726758	2.371802	0.008177	0.261726
-44.059674	-1.724009	2.381798	0.008162	0.261821
-43.554700	-1.783236	2.391795	0.008068	0.262002
-43.871859	-1.713919	2.401792	0.008127	0.262067
-43.364362	-1.758522	2.411789	0.008032	0.262331
-43.560398	-1.707468	2.421786	0.008068	0.262416
-43.133035	-1.742765	2.431782	0.007989	0.262651
-43.140739	-1.722646	2.441779	0.007990	0.262755
-43.372146	-1.635670	2.451776	0.008033	0.263002
-42.800411	-1.708342	2.461773	0.007927	0.263175
-43.219485	-1.609777	2.471770	0.008004	0.263298
-42.252944	-1.730949	2.481766	0.007824	0.263599
-42.358839	-1.697004	2.491763	0.007844	0.263680
-42.029658	-1.714051	2.501760	0.007783	0.263916
-41.860005	-1.708971	2.511757	0.007751	0.264114
-41.603645	-1.730981	2.521754	0.007703	0.264249
-41.481509	-1.705940	2.531750	0.007680	0.264508
-41.408963	-1.693973	2.541747	0.007667	0.264646
-40.590046	-1.806701	2.551744	0.007514	0.264845
-40.316997	-1.819256	2.561741	0.007463	0.265048
-40.327724	-1.796135	2.571738	0.007465	0.265164
-39.593601	-1.873345	2.581734	0.007329	0.265472
-39.567470	-1.869720	2.591731	0.007324	0.265518
-39.698612	-1.800515	2.601728	0.007348	0.265766
-39.335588	-1.840101	2.611725	0.007280	0.265911
-39.468502	-1.782973	2.621722	0.007305	0.266090
-39.099650	-1.800362	2.631718	0.007236	0.266361
-39.254681	-1.741186	2.641715	0.007265	0.266530
-38.578310	-1.828813	2.651712	0.007139	0.266723
-38.189557	-1.857741	2.661709	0.007066	0.266950
-38.120281	-1.847448	2.671706	0.007054	0.267074
-37.522289	-1.910285	2.681702	0.006942	0.267324
-37.758469	-1.833003	2.691699	0.006986	0.267510
-37.478309	-1.854749	2.701696	0.006934	0.267669
-37.173139	-1.852370	2.711693	0.006877	0.267982
-37.175299	-1.822511	2.721690	0.006877	0.268142
-36.378426	-1.946466	2.731686	0.006729	0.268255
-36.467024	-1.871486	2.741683	0.006745	0.268573
-35.887838	-1.951842	2.751680	0.006637	0.268708
-36.131930	-1.873737	2.761677	0.006683	0.268890
-35.688346	-1.898746	2.771674	0.006600	0.269190
-35.332636	-1.938748	2.781670	0.006534	0.269324
-35.036332	-1.959050	2.791667	0.006478	0.269505
-35.210970	-1.878422	2.801664	0.006511	0.269768
-34.899454	-1.904483	2.811661	0.006453	0.269932
-34.735628	-1.891661	2.821658	0.006422	0.270161
-34.693311	-1.841703	2.831654	0.006414	0.270470
-34.913590	-1.768381	2.841651	0.006455	0.270649
-34.254977	-1.857271	2.851648	0.006332	0.270814
-34.272664	-1.802822	2.861645	0.006336	0.271089
-33.980515	-1.806809	2.871642	0.006281	0.271351
-33.838399	-1.790476	2.881638	0.006254	0.271577
-33.574798	-1.799847	2.891635	0.006205	0.271783
-32.790799	-1.901135	2.901632	0.006059	0.272003
-32.793220	-1.851975	2.911629	0.006060	0.272263
-32.502428	-1.866615	2.921626	0.006005	0.272467
-32.044723	-1.915680	2.931622	0.005920	0.272648
-31.868839	-1.884423	2.941619	0.005887	0.272985
-31.760266	-1.870011	2.951616	0.005867	0.273166
-31.297899	-1.924507	2.961613	0.005781	0.273323
-31.318880	-1.868737	2.971610	0.005785	0.273599
-30.882400	-1.901869	2.981606	0.005703	0.273844
-31.079517	-1.824740	2.991603	0.005740	0.274062
-30.888927	-1.815759	3.001600	0.005704	0.274293
-30.636539	-1.814189	3.011597	0.005657	0.274544
-30.393209	-1.803018	3.021594	0.005612	0.274837
-29.668408	-1.897958	3.031590	0.005477	0.275031
-29.284992	-1.933691	3.041587	0.005405	0.275211
-29.020424	-1.926089	3.051584	0.005356	0.275504
-28.704317	-1.952368	3.061581	0.005297	0.275668
-28.585469	-1.945087	3.071578	0.005275	0.275820
-28.647046	-1.885591	3.081574	0.005286	0.276074
-28.612228	-1.838505	3.091571	0.005280	0.276355
-28.332019	-1.845850	3.101568	0.005227	0.276583
-27.998009	-1.869023	3.111565	0.005165	0.276780
-27.919477	-1.839158	3.121562	0.005150	0.277012
-28.094230	-1.743683	3.131558	0.005183	0.277345
-27.498884	-1.806561	3.141555	0.005072	0.277582
-27.576578	-1.741511	3.151552	0.005086	0.277848
-26.991354	-1.804160	3.161549	0.004977	0.278076
-27.228647	-1.712672	3.171546	0.005021	0.278328
-26.602923	-1.772935	3.181542	0.004905	0.278607
-25.858753	-1.858692	3.191539	0.004766	0.278865
-26.017483	-1.785337	3.201536	0.004796	0.279096
-25.721108	-1.794704	3.211533	0.004740	0.279327
-25.131424	-1.862610	3.221530	0.004631	0.279531
-24.898664	-1.844025	3.231526	0.004587	0.279847
-24.720512	-1.835903	3.241523	0.004554	0.280057
-24.459012	-1.840925	3.251520	0.004505	0.280277
-24.129198	-1.854089	3.261517	0.004444	0.280519
-24.094356	-1.815541	3.271514	0.004437	0.280751
-23.921691	-1.805357	3.281510	0.004405	0.280966
-23.609766	-1.817020	3.291507	0.004347	0.281198
-23.410162	-1.813831	3.301504	0.004309	0.281402
-23.155970	-1.798491	3.311501	0.004262	0.281719
-22.283363	-1.917481	3.321498	0.004099	0.281923
-22.552911	-1.828598	3.331494	0.004150	0.282128
-22.325303	-1.823981	3.341491	0.004107	0.282364
-22.461499	-1.742540	3.351488	0.004132	0.282655
-21.779475	-1.810305	3.361485	0.004005	0.282943
-21.685152	-1.785861	3.371482	0.003988	0.283156
-21.470947	-1.779865	3.381478	0.003948	0.283386
-21.396846	-1.746044	3.391475	0.003934	0.283628
-20.925794	-1.776598	3.401472	0.003846	0.283910
-20.654009	-1.771043	3.411469	0.003795	0.284190
-20.546217	-1.749849	3.421466	0.003775	0.284398
-20.092006	-1.790097	3.431462	0.003690	0.284614
-20.032957	-1.750018	3.441459	0.003679	0.284873
-19.740628	-1.743806	3.451456	0.003625	0.285175
-19.368902	-1.760626	3.461453	0.003556	0.285433
-19.400098	-1.713732	3.471450	0.003561	0.285642
-18.492051	-1.845229	3.481446	0.003392	0.285812
-18.297412	-1.829680	3.491443	0.003356	0.286071
-17.728975	-1.887534	3.501440	0.003250	0.286301
-17.416765	-1.910311	3.511437	0.003192	0.286473
-17.349869	-1.875166	3.521434	0.003179	0.286713
-16.908865	-1.905978	3.531430	0.003097	0.286962
-16.931731	-1.862589	3.541427	0.003101	0.287160
-16.735180	-1.861008	3.551424	0.003065	0.287349
-16.264422	-1.890472	3.561421	0.002977	0.287632
-16.193858	-1.858640	3.571418	0.002964	0.287857
-15.743006	-1.902110	3.581414	0.002880	0.288051
-15.842863	-1.839534	3.591411	0.002898	0.288274
-15.369454	-1.870141	3.601408	0.002810	0.288553
-15.411799	-1.823965	3.611405	0.002818	0.288746
-15.250667	-1.808915	3.621402	0.002787	0.288969
-14.617828	-1.868305	3.631398	0.002670	0.289248
-14.551893	-1.835656	3.641395	0.002657	0.289471
-14.450031	-1.811387	3.651392	0.002638	0.289685
-14.123660	-1.827618	3.661389	0.002577	0.289901
-13.764963	-1.837370	3.671386	0.002510	0.290178
-14.003787	-1.736621	3.681382	0.002555	0.290464
-13.847556	-1.722610	3.691379	0.002526	0.290676
-13.265393	-1.788774	3.701376	0.002417	0.290874
-13.167336	-1.760154	3.711373	0.002399	0.291105
-12.544886	-1.815650	3.721370	0.002283	0.291392
-11.949509	-1.881835	3.731366	0.002172	0.291601
-12.355621	-1.765557	3.741363	0.002247	0.291812
-11.920677	-1.800140	3.751360	0.002166	0.292033
-11.436805	-1.830707	3.761357	0.002076	0.292318
-11.440692	-1.788829	3.771354	0.002077	0.292522
-11.192831	-1.789575	3.781350	0.002031	0.292741
-10.963210	-1.774743	3.791347	0.001988	0.293021
-10.651480	-1.779262	3.801344	0.001930	0.293279
-10.135219	-1.833909	3.811341	0.001833	0.293473
-9.671764	-1.882808	3.821338	0.001747	0.293647
-9.601013	-1.839554	3.831334	0.001734	0.293924
-9.367967	-1.833600	3.841331	0.001690	0.294162
-9.050655	-1.854598	3.851328	0.001631	0.294343
-9.052328	-1.812965	3.861325	0.001631	0.294547
-8.579603	-1.836654	3.871322	0.001543	0.294853
-9.084812	-1.699013	3.881318	0.001637	0.295078
-8.273543	-1.801627	3.891315	0.001486	0.295298
-8.159979	-1.771663	3.901312	0.001465	0.295546
-8.212345	-1.715044	3.911309	0.001475	0.295777
-7.547978	-1.789637	3.921306	0.001351	0.296003
-8.013115	-1.655761	3.931302	0.001437	0.296245
-7.454751	-1.711630	3.941299	0.001333	0.296468
-7.006958	-1.733568	3.951296	0.001250	0.296758
-6.951056	-1.693826	3.961293	0.001239	0.297002
-6.776709	-1.675810	3.971290	0.001207	0.297244
-6.221179	-1.730543	3.981286	0.001103	0.297470
-5.821060	-1.760644	3.991283	0.001029	0.297677
-5.556678	-1.741122	4.001280	0.000979	0.298006
-5.492352	-1.712798	4.011277	0.000967	0.298201
-5.094125	-1.745687	4.021274	0.000893	0.298393
-5.133859	-1.689826	4.031270	0.000900	0.298629
-4.413602	-1.759488	4.041267	0.000766	0.298926
-4.251813	-1.746481	4.051264	0.000736	0.299131
-4.462229	-1.661994	4.061261	0.000775	0.299355
-4.225486	-1.662143	4.071258	0.000731	0.299563
-3.637522	-1.703983	4.081254	0.000621	0.299877
-3.916358	-1.604323	4.091251	0.000673	0.300114
-3.079202	-1.705079	4.101248	0.000517	0.300362
-3.507330	-1.581221	4.111245	0.000597	0.300584
-3.481669	-1.543680	4.121242	0.000592	0.300787
-3.935459	-1.396887	4.131238	0.000676	0.301097
-3.849628	-1.347446	4.141235	0.000660	0.301410
-2.776469	-1.477374	4.151232	0.000460	0.301722
-2.641700	-1.453017	4.161229	0.000435	0.301957
-1.864355	-1.539729	4.171226	0.000290	0.302219
-2.395880	-1.388419	4.181222	0.000389	0.302481
-2.691577	-1.268081	4.191219	0.000444	0.302800
-2.665137	-1.204841	4.201216	0.000439	0.303125
-2.585032	-1.155799	4.211213	0.000424	0.303429
-2.086819	-1.176624	4.221210	0.000331	0.303761
-1.878685	-1.145818	4.231206	0.000292	0.304088
-1.526019	-1.147917	4.241203	0.000227	0.304384
-2.060559	-0.979267	4.251200	0.000326	0.304724
-1.683237	-0.980056	4.261197	0.000256	0.305046
-2.158596	-0.812014	4.271194	0.000344	0.305433
-2.366739	-0.695803	4.281190	0.000382	0.305805
-2.116487	-0.655458	4.291187	0.000336	0.306211
-1.678904	-0.656137	4.301184	0.000254	0.306583
-2.485249	-0.431373	4.311181	0.000404	0.306953
-1.794307	-0.458702	4.321178	0.000275	0.307416
-2.019798	-0.330576	4.331174	0.000317	0.307826
-0.923634	-0.452156	4.341171	0.000113	0.308191
-0.821937	-0.387370	4.351168	0.000094	0.308582
-0.579213	-0.341566	4.361165	0.000049	0.309003
-0.656628	-0.243728	4.371162	0.000063	0.309396
-1.218173	-0.052705	4.381158	0.000167	0.309812
-0.403874	-0.098384	4.391155	0.000016	0.310290
-0.391440	-0.017746	4.401152	0.000013	0.310676
-0.504464	0.093034	4.411149	0.000034	0.311097
0.000000	0.096344	4.421146	-0.000060	0.311538

0.247371	0.326465	4.426150	-0.000106	0.312813
0.667610	0.820817	4.431155	-0.000185	0.315442
1.513836	1.526062	4.436160	-0.000343	0.319357
2.487051	2.503151	4.441165	-0.000525	0.324542
2.844613	3.896769	4.446170	-0.000592	0.330980
3.605770	5.499474	4.451174	-0.000735	0.338504
5.523873	7.208207	4.456179	-0.001093	0.347183
7.857883	9.165201	4.461184	-0.001529	0.356964
9.687151	11.533654	4.466189	-0.001871	0.367743
11.848802	14.182948	4.471194	-0.002276	0.379517
14.307121	17.121243	4.476198	-0.002735	0.392200
18.062898	20.181581	4.481203	-0.003437	0.405760
21.701130	23.636536	4.486208	-0.004116	0.420165
26.908509	27.189597	4.491213	-0.005088	0.435360
32.752404	31.024638	4.496218	-0.006179	0.451313
37.599424	35.446094	4.501222	-0.007085	0.467973
46.466891	39.548101	4.506227	-0.008738	0.485268
59.652575	43.341699	4.511232	-0.011196	0.503313
69.835474	48.137485	4.516237	-0.013095	0.521999
94.457015	50.850664	4.521242	-0.017682	0.541411
118.518479	54.277240	4.526246	-0.022164	0.561704
128.368894	60.796819	4.531251	-0.024003	0.582604
135.661842	68.141672	4.536256	-0.025365	0.603647
144.416063	75.592285	4.541261	-0.027000	0.624822
152.404082	83.523721	4.546266	-0.028493	0.646062
161.217101	91.626964	4.551270	-0.030139	0.667307
168.705963	100.246863	4.556275	-0.031539	0.688474
175.169613	109.295279	4.561280	-0.032749	0.709502
181.106411	118.647993	4.566285	-0.033860	0.730333
185.770187	128.406144	4.571290	-0.034735	0.750924
188.695209	138.564165	4.576294	-0.035286	0.771131
190.714495	148.967422	4.581299	-0.035669	0.790973
192.303825	159.472456	4.586304	-0.035972	0.810374
194.444752	169.901268	4.591309	-0.036378	0.829356
196.043552	180.425102	4.596314	-0.036682	0.847910
197.336372	190.959281	4.601318	-0.036930	0.865993
199.296273	201.341856	4.606323	-0.037301	0.883649
200.901530	211.742610	4.611328	-0.037607	0.900887
201.738436	222.238622	4.616333	-0.037770	0.917738
203.038715	232.557651	4.621338	-0.038019	0.934137
204.876700	242.690334	4.626342	-0.038368	0.950112
206.381916	252.822075	4.631347	-0.038655	0.965734
208.040338	262.846128	4.636352	-0.038970	0.980986
208.921502	272.961379	4.641357	-0.039141	0.995940
209.813666	282.935361	4.646362	-0.039313	1.010474
210.253219	292.897035	4.651366	-0.039402	1.024673
211.890841	302.538766	4.656371	-0.039713	1.038523
213.570559	312.114347	4.661376	-0.040032	1.052108
214.582994	321.738340	4.666381	-0.040227	1.065429
215.776919	331.234772	4.671386	-0.040455	1.078456
216.178495	340.792900	4.676390	-0.040536	1.091228
217.047633	350.185989	4.681395	-0.040704	1.103742
217.828010	359.516047	4.686400	-0.040856	1.116014
218.681737	368.746704	4.691405	-0.041021	1.128041
219.621555	377.923778	4.696410	-0.041202	1.139892
220.306205	387.077338	4.701414	-0.041335	1.151537
221.115907	396.138952	4.706419	-0.041492	1.162977
221.834043	405.156584	4.711424	-0.041632	1.174232
222.532574	414.112967	4.716429	-0.041768	1.185302
223.074582	423.066203	4.721434	-0.041874	1.196233
224.017813	431.866990	4.726438	-0.042056	1.206964
224.330051	440.774364	4.731443	-0.042120	1.217599
224.451629	449.652111	4.736448	-0.042148	1.228070
225.619219	458.285520	4.741453	-0.042371	1.238374
225.991985	467.044307	4.746458	-0.042447	1.248582
226.274064	475.769558	4.751462	-0.042505	1.258650
226.920462	484.418705	4.756467	-0.042631	1.268623
227.528465	493.019520	4.761472	-0.042750	1.278455
227.973478	501.623027	4.766477	-0.042838	1.288185
228.457987	510.215050	4.771482	-0.042934	1.297836
228.878548	518.791426	4.776486	-0.043018	1.307387
229.568392	527.370304	4.781491	-0.043152	1.316920
229.863319	535.867920	4.786496	-0.043213	1.326224
230.399547	544.339194	4.791501	-0.043318	1.335479
230.781586	552.828772	4.796506	-0.043395	1.344661
231.582655	561.224253	4.801510	-0.043549	1.353756
232.900179	569.505745	4.806515	-0.043800	1.362760
233.649101	577.912447	4.811520	-0.043945	1.371736
233.965946	586.375358	4.816525	-0.044010	1.380638
235.230885	594.673252	4.821530	-0.044251	1.389474
235.973649	603.042890	4.826534	-0.044394	1.398239
236.282824	611.489317	4.831539	-0.044457	1.406954
237.056168	619.819755	4.836544	-0.044607	1.415575
237.714038	628.177717	4.841549	-0.044735	1.424152
238.495269	636.530025	4.846554	-0.044886	1.432693
238.330329	644.992584	4.851558	-0.044861	1.441136
239.201054	653.269882	4.856563	-0.045028	1.449516
240.059174	661.563322	4.861568	-0.045194	1.457862
240.540826	669.908582	4.866573	-0.045289	1.466149
241.174907	678.244604	4.871578	-0.045412	1.474406
241.395991	686.596919	4.876582	-0.045459	1.482566
242.728320	694.757901	4.881587	-0.045712	1.490672
243.340047	703.057998	4.886592	-0.045832	1.498755
244.349102	711.267367	4.891597	-0.046025	1.506769
245.144697	719.557813	4.896602	-0.046179	1.514784
245.468745	727.886675	4.901606	-0.046244	1.522720
246.348087	736.112236	4.906611	-0.046413	1.530604
246.697976	744.446108	4.911616	-0.046484	1.538467
247.700129	752.636109	4.916621	-0.046676	1.546254
248.308538	760.926336	4.921626	-0.046795	1.554036
249.424013	769.067594	4.926630	-0.047008	1.561718
250.037399	777.358005	4.931635	-0.047127	1.569423
250.944400	785.570436	4.936640	-0.047302	1.577063
252.061300	793.753657	4.941645	-0.047515	1.584670
253.264684	801.943420	4.946650	-0.047745	1.592259
253.840487	810.215552	4.951654	-0.047857	1.599794
254.638443	818.460288	4.956659	-0.048011	1.607301
255.225706	826.714053	4.961664	-0.048126	1.614751
255.652861	834.993430	4.966669	-0.048211	1.622167
256.548986	843.206915	4.971674	-0.048383	1.629557
256.990413	851.473036	4.976678	-0.048471	1.636895
257.578347	859.684658	4.981683	-0.048586	1.644173
258.284225	867.874566	4.986688	-0.048722	1.651417
258.732933	876.111100	4.991693	-0.048811	1.658633
259.683441	884.251349	4.996698	-0.048994	1.665804
260.135527	892.503376	5.001702	-0.049083	1.672972
260.632204	900.717481	5.006707	-0.049181	1.680083
260.708888	908.993822	5.011712	-0.049201	1.687160
261.628216	917.119876	5.016717	-0.049377	1.694193
262.626328	925.229829	5.021722	-0.049569	1.701193
262.923571	933.477414	5.026726	-0.049629	1.708187
263.875452	941.607063	5.031731	-0.049812	1.715140
264.207150	949.816111	5.036736	-0.049879	1.722050
264.292793	958.085039	5.041741	-0.049901	1.728949
264.600679	966.308459	5.046746	-0.049963	1.735812
265.226176	974.431837	5.051750	-0.050085	1.742607
265.897693	982.595959	5.056755	-0.050215	1.749414
267.084781	990.636145	5.061760	-0.050442	1.756159
267.467672	998.852244	5.066765	-0.050518	1.762920
267.844239	1007.056316	5.071770	-0.050594	1.769643
268.495115	1015.196928	5.076774	-0.050720	1.776324
269.237018	1023.341133	5.081779	-0.050864	1.782995
269.781422	1031.527118	5.086784	-0.050971	1.789649
269.971348	1039.762350	5.091789	-0.051011	1.796273
270.430982	1047.908801	5.096794	-0.051102	1.802836
270.422052	1056.146838	5.101798	-0.051106	1.809390
270.645344	1064.317876	5.106803	-0.051153	1.815896
271.482376	1072.371122	5.111808	-0.051314	1.822360
271.718136	1080.572651	5.116813	-0.051364	1.828845
272.212829	1088.695039	5.121818	-0.051461	1.835276
272.759055	1096.794666	5.126822	-0.051568	1.841672
273.430534	1104.917183	5.131827	-0.051698	1.848080
273.700974	1113.105572	5.136832	-0.051754	1.854468
274.543818	1121.152597	5.141837	-0.051916	1.860793
275.052239	1129.320017	5.146842	-0.052016	1.867149
275.595054	1137.466138	5.151846	-0.052123	1.873472
276.110646	1145.590348	5.156851	-0.052224	1.879753
276.588569	1153.721138	5.161856	-0.052318	1.886013
276.676150	1161.938078	5.166861	-0.052340	1.892273
277.597087	1169.993817	5.171866	-0.052517	1.898486
277.929532	1178.124255	5.176870	-0.052584	1.904668
278.632882	1186.250033	5.181875	-0.052720	1.910868
279.223763	1194.353679	5.186880	-0.052836	1.917019
279.572869	1202.499198	5.191885	-0.052906	1.923154
279.787240	1210.703804	5.196890	-0.052951	1.929298
280.288714	1218.812566	5.201894	-0.053050	1.935383
280.559018	1226.972475	5.206899	-0.053106	1.941461
280.776680	1235.142449	5.211904	-0.053152	1.947522
281.916012	1243.121755	5.216909	-0.053369	1.953525
282.215513	1251.270664	5.221914	-0.053430	1.959542
282.794635	1259.320512	5.226918	-0.053543	1.965499
283.662057	1267.403939	5.231923	-0.053710	1.971493
284.179774	1275.550021	5.236928	-0.053812	1.977476
284.799866	1283.616069	5.241933	-0.053933	1.983394
285.184212	1291.790792	5.246938	-0.054010	1.989348
285.907724	1299.852426	5.251942	-0.054150	1.995239
285.829339	1308.083964	5.256947	-0.054140	2.001148
285.884791	1316.251197	5.261952	-0.054156	2.007008
286.966099	1324.244151	5.266957	-0.054363	2.012835
287.536748	1332.364529	5.271962	-0.054474	2.018682
288.228242	1340.412292	5.276966	-0.054608	2.024474
288.925449	1348.541754	5.281971	-0.054743	2.030306
288.957653	1356.726775	5.286976	-0.054755	2.036092
289.374124	1364.810119	5.291981	-0.054838	2.041830
289.940546	1372.902933	5.296986	-0.054949	2.047574
290.398278	1381.016414	5.301990	-0.055039	2.053305
290.934598	1389.124627	5.306995	-0.055144	2.059024
291.502446	1397.176936	5.312000	-0.055255	2.064691
292.006431	1405.301699	5.317005	-0.055354	2.070386
292.337355	1413.440049	5.322010	-0.055421	2.076058
292.627842	1421.551866	5.327014	-0.055481	2.081692
293.094129	1429.653909	5.332019	-0.055573	2.087321
293.558132	1437.749656	5.337024	-0.055665	2.092930
294.012961	1445.839189	5.342029	-0.055755	2.098520
294.133084	1454.002720	5.347034	-0.055782	2.104111
294.666994	1462.073014	5.352038	-0.055887	2.109665
294.913680	1470.229385	5.357043	-0.055938	2.115235
295.587967	1478.238175	5.362048	-0.056069	2.120731
296.267286	1486.268940	5.367053	-0.056201	2.126229
296.535209	1494.457785	5.372058	-0.056256	2.131779
296.860797	1502.541170	5.377062	-0.056322	2.137249
297.883615	1510.530995	5.382067	-0.056518	2.142710
298.904798	1518.546203	5.387072	-0.056713	2.148173
299.334810	1526.667677	5.392077	-0.056799	2.153636
299.529414	1534.823903	5.397082	-0.056840	2.159086
299.973283	1542.893465	5.402086	-0.056928	2.164489
300.572837	1550.974030	5.407091	-0.057045	2.169899
301.244734	1559.029673	5.412096	-0.057176	2.175287
301.442989	1567.175439	5.417101	-0.057218	2.180676
302.230610	1575.236734	5.422106	-0.057370	2.186051
302.380676	1583.378109	5.427110	-0.057403	2.191407
303.105130	1591.417650	5.432115	-0.057543	2.196735
303.879256	1599.427371	5.437120	-0.057693	2.202036
304.231111	1607.551055	5.442125	-0.057763	2.207359
304.668672	1615.663988	5.447130	-0.057850	2.212670
305.189939	1623.738880	5.452134	-0.057953	2.217951
305.551102	1631.853077	5.457139	-0.058025	2.223230
305.894938	1639.962385	5.462144	-0.058095	2.228492
306.061793	1648.104825	5.467149	-0.058131	2.233747
306.648316	1656.150960	5.472154	-0.058245	2.238966
307.200666	1664.177660	5.477158	-0.058354	2.244156
307.562390	1672.296012	5.482163	-0.058426	2.249376
308.347766	1680.332621	5.487168	-0.058578	2.254570
308.366602	1688.489655	5.492173	-0.058587	2.259759
308.844979	1696.550453	5.497178	-0.058681	2.264917
309.354792	1704.626841	5.502182	-0.058781	2.270075
309.947736	1712.709929	5.507187	-0.058897	2.275233
310.207642	1720.786594	5.512192	-0.058951	2.280346
311.098724	1728.741938	5.517197	-0.059122	2.285427
311.864778	1736.812377	5.522202	-0.059270	2.290557
311.878243	1744.969497	5.527206	-0.059278	2.295664
312.397490	1753.045253	5.532211	-0.059380	2.300753
312.815768	1761.106036	5.537216	-0.059463	2.305813
313.849887	1769.085531	5.542221	-0.059661	2.310864
314.126948	1777.208624	5.547226	-0.059718	2.315928
315.032945	1785.191491	5.552230	-0.059891	2.320947
315.748210	1793.274055	5.557235	-0.060030	2.326001
315.838421	1801.428261	5.562240	-0.060052	2.331035
316.428344	1809.476024	5.567245	-0.060167	2.336035
317.054260	1817.562253	5.572250	-0.060289	2.341050
317.358882	1825.655166	5.577254	-0.060351	2.346032
317.247801	1833.864480	5.582259	-0.060336	2.351040
317.811153	1841.891518	5.587264	-0.060446	2.355982
318.655845	1849.874802	5.592269	-0.060609	2.360910
319.029102	1857.954108	5.597274	-0.060683	2.365847
319.371462	1866.036168	5.602278	-0.060752	2.370773
320.347580	1874.044809	5.607283	-0.060939	2.375696
320.637274	1882.136599	5.612288	-0.060999	2.380603
320.940173	1890.205372	5.617293	-0.061060	2.385487
321.436649	1898.312196	5.622298	-0.061158	2.390399
321.657317	1906.401933	5.627302	-0.061205	2.395269
322.229339	1914.436924	5.632307	-0.061316	2.400124
323.185963	1922.393945	5.637312	-0.061500	2.404953
323.574228	1930.504367	5.642317	-0.061577	2.409819
324.014398	1938.612968	5.647322	-0.061665	2.414678
324.127085	1946.707616	5.652326	-0.061691	2.419492
324.679683	1954.753358	5.657331	-0.061799	2.424303
324.879074	1962.874002	5.662336	-0.061841	2.429121
325.446270	1970.925588	5.667341	-0.061952	2.433917
325.886293	1978.993834	5.672346	-0.062040	2.438704
326.320683	1987.017306	5.677350	-0.062126	2.443454
326.069537	1995.191688	5.682355	-0.062084	2.448230
325.863959	2003.318500	5.687360	-0.062051	2.452973
327.076150	2011.185226	5.692365	-0.062282	2.457664
327.481851	2019.269159	5.697370	-0.062363	2.462410
327.714405	2027.338549	5.702374	-0.062412	2.467126
328.201951	2035.399797	5.707379	-0.062508	2.471847
328.733226	2043.437111	5.712384	-0.062612	2.476548
329.066976	2051.493996	5.717389	-0.062679	2.481237
329.038978	2059.641131	5.722394	-0.062680	2.485942
329.673220	2067.638836	5.727398	-0.062803	2.490601
330.313017	2075.681343	5.732403	-0.062927	2.495278
330.316621	2083.811655	5.737408	-0.062933	2.499949
330.797074	2091.833214	5.742413	-0.063028	2.504584
331.312262	2099.900939	5.747418	-0.063129	2.509240
331.604132	2107.954601	5.752422	-0.063189	2.513862
332.066730	2116.010283	5.757427	-0.063280	2.518489
332.617675	2124.026593	5.762432	-0.063388	2.523092
333.200333	2132.054367	5.767437	-0.063502	2.527695
333.397471	2140.175074	5.772442	-0.063544	2.532315
333.557227	2148.250120	5.777446	-0.063579	2.536897
334.144450	2156.290918	5.782451	-0.063694	2.541483
334.380041	2164.375804	5.787456	-0.063743	2.546059
334.653832	2172.445260	5.792461	-0.063799	2.550622
335.167666	2180.480661	5.797466	-0.063900	2.555174
335.341913	2188.547221	5.802470	-0.063938	2.559712
335.876124	2196.576589	5.807475	-0.064043	2.564246
336.169337	2204.643273	5.812480	-0.064103	2.568775
336.745025	2212.656383	5.817485	-0.064215	2.573287
336.935709	2220.764619	5.822490	-0.064256	2.577817
336.941799	2228.858300	5.827494	-0.064262	2.582317
337.745863	2236.839831	5.832499	-0.064417	2.586803
338.177892	2244.954206	5.837504	-0.064503	2.591329
338.538194	2253.022289	5.842509	-0.064575	2.595817
338.660371	2261.107580	5.847514	-0.064603	2.600289
338.987221	2269.092495	5.852518	-0.064670	2.604713
339.638433	2277.092329	5.857523	-0.064796	2.609160
340.405678	2285.099109	5.862528	-0.064944	2.613611
340.929981	2293.137503	5.867533	-0.065047	2.618054
341.398873	2301.198783	5.872538	-0.065140	2.622499
341.620940	2309.270425	5.877542	-0.065186	2.626925
342.111331	2317.341976	5.882547	-0.065283	2.631362
342.559429	2325.393685	5.887552	-0.065372	2.635777
343.272074	2333.379014	5.892557	-0.065510	2.640167
343.574492	2341.450645	5.897562	-0.065571	2.644568
343.898430	2349.503851	5.902566	-0.065637	2.648954
344.066426	2357.634869	5.907571	-0.065673	2.653364
344.729853	2365.632671	5.912576	-0.065802	2.657728
344.888180	2373.689247	5.917581	-0.065837	2.662082
345.379497	2381.758339	5.922586	-0.065934	2.666458
345.603310	2389.840013	5.927590	-0.065981	2.670816
346.233850	2397.870179	5.932595	-0.066103	2.675166
346.234072	2405.948712	5.937600	-0.066109	2.679494
346.201739	2414.016820	5.942605	-0.066108	2.683806
346.941495	2422.003400	5.947610	-0.066251	2.688119
347.343678	2430.037209	5.952614	-0.066331	2.692428
347.557690	2438.149801	5.957619	-0.066376	2.696759
347.518621	2446.256223	5.962624	-0.066374	2.701064
348.015733	2454.218891	5.967629	-0.066472	2.705320
349.237826	2462.138192	5.972634	-0.066705	2.709593
349.452495	2470.242873	5.977638	-0.066750	2.713893
349.777251	2478.294634	5.982643	-0.066816	2.718164
349.782131	2486.397071	5.987648	-0.066822	2.722436
350.380268	2494.410860	5.992653	-0.066939	2.726692
350.891220	2502.468767	5.997658	-0.067039	2.730958
351.065667	2510.538097	6.002662	-0.067077	2.735203
351.359934	2518.595640	6.007667	-0.067137	2.739442
351.846721	2526.619025	6.012672	-0.067233	2.743669
352.231443	2534.663615	6.017677	-0.067310	2.747894
352.497900	2542.792377	6.022682	-0.067365	2.752149
352.934610	2550.811684	6.027686	-0.067452	2.756351
353.058680	2558.902709	6.032691	-0.067480	2.760564
353.616518	2566.828533	6.037696	-0.067589	2.764712
353.937883	2574.890927	6.042701	-0.067654	2.768910
353.896374	2583.021139	6.047706	-0.067652	2.773114
354.092028	2591.049331	6.052710	-0.067693	2.777274
354.719073	2599.052396	6.057715	-0.067815	2.781441
354.887841	2607.112398	6.062720	-0.067852	2.785603
355.400411	2615.104876	6.067725	-0.067953	2.789744
355.578283	2623.220993	6.072730	-0.067991	2.793923
356.143514	2631.190297	6.077734	-0.068102	2.798044
356.443547	2639.247068	6.082739	-0.068163	2.802187
356.932763	2647.272583	6.087744	-0.068259	2.806319
356.769842	2655.412746	6.092749	-0.068234	2.810465
357.746588	2663.361843	6.097754	-0.068421	2.814575
357.533431	2671.475947	6.102758	-0.068387	2.818693
357.833679	2679.508775	6.107763	-0.068448	2.822793
358.887494	2687.429748	6.112768	-0.068650	2.826875
359.183963	2695.524424	6.117773	-0.068710	2.830994
359.205592	2703.669397	6.122778	-0.068720	2.835117
359.880092	2711.595023	6.127782	-0.068850	2.839161
360.222838	2719.648908	6.132787	-0.068919	2.843245
360.294559	2727.711409	6.137792	-0.068938	2.847311
360.369155	2735.805649	6.142797	-0.068957	2.851388
360.456234	2743.911345	6.147802	-0.068979	2.855465
360.253781	2751.998673	6.152806	-0.068946	2.859511
361.103392	2759.916319	6.157811	-0.069110	2.863526
361.690458	2767.927105	6.162816	-0.069224	2.867567
362.044547	2775.981476	6.167821	-0.069296	2.871610
361.762482	2784.142335	6.172826	-0.069249	2.875665
361.918555	2792.146696	6.177830	-0.069283	2.879662
362.882812	2800.063884	6.182835	-0.069468	2.883654
362.937659	2808.156890	6.187840	-0.069483	2.887677
363.414726	2816.172988	6.192845	-0.069577	2.891680
363.797406	2824.254534	6.197850	-0.069654	2.895705
363.927466	2832.288585	6.202854	-0.069683	2.899686
363.872650	2840.403055	6.207859	-0.069678	2.903692
364.294251	2848.405417	6.212864	-0.069762	2.907663
364.840139	2856.444474	6.217869	-0.069869	2.911653
365.076821	2864.517071	6.222874	-0.069918	2.915637
365.696006	2872.460594	6.227878	-0.070039	2.919574
365.258479	2880.629319	6.232883	-0.069963	2.923558
365.250894	2888.632752	6.237888	-0.069967	2.927478
365.412548	2896.681924	6.242893	-0.070002	2.931426
365.952466	2904.682581	6.247898	-0.070108	2.935364
365.901149	2912.725830	6.252902	-0.070104	2.939286
366.249118	2920.724552	6.257907	-0.070174	2.943203
366.738270	2928.730891	6.262912	-0.070270	2.947125
367.087652	2936.782697	6.267917	-0.070340	2.951057
367.215450	2944.856691	6.272922	-0.070369	2.954983
367.166896	2952.896216	6.277926	-0.070366	2.958877
368.082449	2960.821060	6.282931	-0.070541	2.962761
368.184330	2968.926990	6.287936	-0.070566	2.966686
368.477106	2976.983608	6.292941	-0.070625	2.970591
368.968846	2984.999068	6.297946	-0.070722	2.974481
369.165557	2993.047338	6.302950	-0.070764	2.978366
369.516322	3001.070828	6.307955	-0.070835	2.982243
369.916985	3009.111956	6.312960	-0.070915	2.986126
369.724433	3017.214942	6.317965	-0.070884	2.990002
369.956976	3025.272460	6.322970	-0.070933	2.993874
369.843062	3033.318092	6.327974	-0.070917	2.997717
370.179072	3041.343063	6.332979	-0.070985	3.001568
370.631729	3049.312435	6.337984	-0.071074	3.005394
370.903110	3057.329149	6.342989	-0.071130	3.009228
370.919749	3065.462650	6.347994	-0.071138	3.013100
371.582395	3073.391750	6.352998	-0.071267	3.016902
371.818404	3081.447313	6.358003	-0.071316	3.020738
372.024935	3089.474183	6.363008	-0.071360	3.024554
372.677385	3097.464410	6.368013	-0.071487	3.028370
373.418514	3105.492750	6.373018	-0.071630	3.032204
373.489889	3113.579331	6.378022	-0.071649	3.036027
373.533927	3121.631988	6.383027	-0.071662	3.039827
374.294321	3129.590139	6.388032	-0.071809	3.043614
374.563978	3137.635626	6.393037	-0.071864	3.047413
374.800096	3145.764588	6.398042	-0.071914	3.051245
374.671492	3153.853231	6.403046	-0.071895	3.055035
375.187743	3161.841736	6.408051	-0.071996	3.058805
375.780881	3169.831754	6.413056	-0.072112	3.062574
376.104482	3177.869102	6.418061	-0.072178	3.066348
376.497576	3185.932112	6.423066	-0.072256	3.070132
376.351097	3194.082858	6.428070	-0.072234	3.073927
376.661823	3202.048497	6.433075	-0.072297	3.077653
376.880786	3210.071623	6.438080	-0.072343	3.081397
376.747040	3218.124549	6.443085	-0.072324	3.085133
377.077058	3226.139856	6.448090	-0.072390	3.088869
377.521958	3234.147282	6.453094	-0.072478	3.092602
377.775709	3242.178650	6.458099	-0.072531	3.096333
378.263059	3250.168451	6.463104	-0.072627	3.100051
378.082282	3258.245217	6.468109	-0.072599	3.103773
378.417158	3266.309953	6.473114	-0.072666	3.107510
379.347228	3274.218791	6.478118	-0.072845	3.111197
379.196001	3282.333896	6.483123	-0.072822	3.114925
380.208314	3290.256134	6.488128	-0.073016	3.118614
380.441070	3298.335157	6.493133	-0.073064	3.122334
380.640480	3306.412975	6.498138	-0.073107	3.126048
380.351068	3314.532281	6.503142	-0.073058	3.129754
380.589716	3322.559953	6.508147	-0.073108	3.133437
380.747196	3330.603908	6.513152	-0.073142	3.137120
380.711040	3338.656782	6.518157	-0.073141	3.140794
380.416142	3346.756364	6.523162	-0.073091	3.144474
381.186384	3354.648127	6.528166	-0.073240	3.148102
381.502787	3362.713690	6.533171	-0.073304	3.151785
382.033999	3370.701683	6.538176	-0.073408	3.155437
382.651473	3378.647357	6.543181	-0.073528	3.159071
382.646410	3386.753865	6.548186	-0.073533	3.162744
382.476252	3394.850780	6.553190	-0.073506	3.166403
382.781404	3402.889805	6.558195	-0.073569	3.170051
383.003286	3410.894503	6.563200	-0.073615	3.173676
382.941312	3418.965875	6.568205	-0.073609	3.177315
383.280221	3427.015853	6.573210	-0.073677	3.180958
383.644678	3434.937428	6.578214	-0.073750	3.184539
384.159966	3442.976494	6.583219	-0.073852	3.188176
384.263905	3451.055680	6.588224	-0.073876	3.191809
384.694766	3459.061792	6.593229	-0.073962	3.195419
385.050088	3467.055861	6.598234	-0.074033	3.199016
385.638959	3475.015062	6.603238	-0.074148	3.202603
386.037167	3483.098875	6.608243	-0.074227	3.206234
385.721641	3491.231592	6.613248	-0.074174	3.209852
385.188603	3499.360466	6.618253	-0.074080	3.213455
385.840410	3507.339852	6.623258	-0.074207	3.217038
385.878060	3515.368554	6.628262	-0.074219	3.220613
386.116430	3523.363284	6.633267	-0.074269	3.224177
386.536154	3531.370229	6.638272	-0.074352	3.227750
386.493353	3539.472886	6.643277	-0.074349	3.231342
386.934390	3547.445898	6.648282	-0.074437	3.234893
387.264225	3555.408706	6.653286	-0.074503	3.238431
387.778029	3563.430258	6.658291	-0.074604	3.241999
388.066104	3571.438183	6.663296	-0.074663	3.245547
388.565182	3579.430350	6.668301	-0.074761	3.249093
389.140819	3587.480370	6.673306	-0.074874	3.252663
389.063132	3595.587534	6.678310	-0.074865	3.256228
388.952527	3603.668240	6.683315	-0.074849	3.259777
388.924374	3611.702409	6.688320	-0.074850	3.263304
389.491704	3619.648203	6.693325	-0.074960	3.266813
390.027895	3627.703353	6.698330	-0.075066	3.270364
390.132175	3635.722372	6.703334	-0.075090	3.273879
390.825809	3643.690213	6.708339	-0.075225	3.277391
391.061818	3651.768252	6.713344	-0.075274	3.280929
391.199395	3659.787533	6.718349	-0.075305	3.284433
391.197413	3667.927095	6.723354	-0.075310	3.287981
391.319518	3675.935726	6.728358	-0.075338	3.291472
391.711924	3683.933390	6.733363	-0.075416	3.294966
392.095193	3691.929066	6.738368	-0.075493	3.298455
392.140179	3700.002879	6.743373	-0.075506	3.301961
392.371253	3708.046162	6.748378	-0.075555	3.305457
392.530128	3716.043276	6.753382	-0.075589	3.308926
393.083150	3724.050257	6.758387	-0.075698	3.312411
393.417872	3732.128900	6.763392	-0.075765	3.315916
393.615835	3740.073652	6.768397	-0.075807	3.319353
393.349910	3748.211594	6.773402	-0.075763	3.322852
393.901192	3756.176396	6.778406	-0.075871	3.326304
394.407053	3764.177013	6.783411	-0.075971	3.329767
395.009731	3772.195784	6.788416	-0.076088	3.333237
395.413091	3780.229946	6.793421	-0.076168	3.336702
395.176147	3788.373643	6.798426	-0.076130	3.340187
395.126982	3796.340806	6.803430	-0.076126	3.343599
395.929362	3804.317085	6.808435	-0.076280	3.347044
395.959237	3812.434040	6.813440	-0.076291	3.350516
395.039135	3820.573151	6.818445	-0.076125	3.353959
395.762516	3828.515132	6.823450	-0.076265	3.357375
395.986821	3836.523713	6.828454	-0.076312	3.360798
396.442808	3844.439745	6.833459	-0.076402	3.364186
396.959908	3852.484957	6.838464	-0.076504	3.367628
397.235159	3860.533872	6.843469	-0.076560	3.371059
397.658356	3868.551862	6.848474	-0.076644	3.374479
397.549194	3876.601985	6.853478	-0.076629	3.377890
398.212085	3884.610763	6.858483	-0.076758	3.381307
398.521728	3892.653849	6.863488	-0.076821	3.384723
398.115921	3900.794527	6.868493	-0.076751	3.388151
398.549838	3908.810913	6.873498	-0.076837	3.391553
398.792174	3916.840043	6.878502	-0.076887	3.394950
398.897205	3924.839369	6.883507	-0.076912	3.398326
399.200393	3932.825450	6.888512	-0.076974	3.401700
399.575053	3940.780896	6.893517	-0.077049	3.405061
399.365040	3948.969874	6.898522	-0.077015	3.408495
399.426570	3956.964868	6.903526	-0.077032	3.411854
399.753674	3964.967054	6.908531	-0.077098	3.415223
400.360422	3972.915842	6.913536	-0.077216	3.418575
399.957213	3981.025101	6.918541	-0.077146	3.421956
400.239085	3989.031253	6.923546	-0.077204	3.425314
400.550413	3997.057153	6.928550	-0.077267	3.428679
401.227487	4005.018058	6.933555	-0.077399	3.432025
401.453652	4013.101576	6.938560	-0.077446	3.435404
401.655324	4021.087222	6.943565	-0.077489	3.438737
402.547564	4029.071048	6.948570	-0.077660	3.442091
402.460888	4037.133863	6.953574	-0.077649	3.445440
402.580227	4045.169533	6.958579	-0.077677	3.448782
403.277276	4053.209412	6.963584	-0.077812	3.452142
403.078248	4061.283945	6.968589	-0.077780	3.455482
403.568283	4069.247452	6.973594	-0.077877	3.458797
403.722150	4077.305803	6.978598	-0.077911	3.462136
403.906290	4085.330265	6.983603	-0.077950	3.465459
403.895321	4093.417641	6.988608	-0.077953	3.468798
403.874805	4101.470426	6.993613	-0.077955	3.472120
404.140592	4109.498773	6.998618	-0.078010	3.475438
404.460963	4117.441028	7.003622	-0.078075	3.478719
404.676952	4125.422838	7.008627	-0.078120	3.482009
405.449308	4133.414195	7.013632	-0.078269	3.485319
405.923623	4141.385550	7.018637	-0.078363	3.488607
405.970665	4149.545606	7.023642	-0.078377	3.491956
406.064147	4157.573403	7.028646	-0.078399	3.495249
406.361248	4165.599571	7.033651	-0.078460	3.498544
406.718734	4173.634031	7.038656	-0.078532	3.501842
406.547698	4181.659769	7.043661	-0.078505	3.505116
407.419968	4189.653057	7.048666	-0.078673	3.508407
407.313224	4197.730983	7.053670	-0.078658	3.511699
407.252448	4205.774525	7.058675	-0.078652	3.514974
407.651188	4213.751355	7.063680	-0.078732	3.518234
407.852771	4221.754950	7.068685	-0.078775	3.521496
408.482149	4229.735181	7.073690	-0.078897	3.524758
408.691654	4237.795607	7.078694	-0.078941	3.528037
408.911672	4245.846651	7.083699	-0.078988	3.531309
409.040394	4253.888405	7.088704	-0.079017	3.534572
409.257621	4261.898453	7.093709	-0.079063	3.537821
409.205460	4270.025420	7.098714	-0.079058	3.541106
409.080553	4278.023246	7.103718	-0.079040	3.544334
409.435893	4286.042000	7.108723	-0.079112	3.547582
410.082075	4293.996601	7.113728	-0.079237	3.550810
410.078533	4302.102576	7.118733	-0.079242	3.554077
409.920895	4310.178014	7.123738	-0.079218	3.557323
410.001871	4318.141035	7.128742	-0.079238	3.560528
410.842876	4326.017561	7.133747	-0.079400	3.563719
411.182224	4334.076882	7.138752	-0.079468	3.566965
411.013964	4342.140431	7.143757	-0.079442	3.570194
411.548767	4350.180549	7.148762	-0.079547	3.573432
411.887219	4358.166382	7.153766	-0.079615	3.576640
411.888231	4366.206467	7.158771	-0.079621	3.579856
412.409685	4374.212899	7.163776	-0.079723	3.583072
412.715245	4382.247410	7.168781	-0.079785	3.586289
412.868487	4390.312249	7.173786	-0.079819	3.589511
412.659266	4398.394587	7.178790	-0.079786	3.592726
412.983961	4406.448873	7.183795	-0.079851	3.595943
413.000043	4414.427103	7.188800	-0.079860	3.599118
413.707155	4422.354163	7.193805	-0.079996	3.602289
414.119066	4430.377630	7.198810	-0.080078	3.605488
414.202854	4438.413315	7.203814	-0.080099	3.608679
414.591858	4446.469543	7.208819	-0.080177	3.611884
414.526580	4454.549309	7.213824	-0.080170	3.615082
414.572462	4462.569021	7.218829	-0.080184	3.618258
414.384323	4470.683683	7.223834	-0.080154	3.621461
414.715471	4478.585675	7.228838	-0.080221	3.624592
415.411660	4486.564366	7.233843	-0.080356	3.627761
415.934060	4494.614993	7.238848	-0.080459	3.630950
416.432031	4502.564486	7.243853	-0.080557	3.634096
416.692569	4510.640249	7.248858	-0.080610	3.637282
416.879114	4518.658554	7.253862	-0.080650	3.640441
417.271889	4526.625692	7.258867	-0.080729	3.643583
417.742095	4534.670828	7.263872	-0.080822	3.646755
417.442713	4542.786580	7.268877	-0.080771	3.649930
418.047017	4550.797619	7.273882	-0.080889	3.653086
418.030476	4558.837520	7.278886	-0.080891	3.656234
418.205259	4566.840742	7.283891	-0.080929	3.659370
418.593716	4574.851316	7.288896	-0.081006	3.662512
418.599201	4582.863380	7.293901	-0.081013	3.665642
419.117287	4590.903868	7.298906	-0.081115	3.668793
419.543905	4598.902511	7.303910	-0.081199	3.671923
419.673090	4606.931727	7.308915	-0.081229	3.675055
420.204090	4614.920394	7.313920	-0.081333	3.678178
420.280705	4622.991969	7.318925	-0.081352	3.681319
420.572555	4630.991582	7.323930	-0.081412	3.684436
420.264177	4639.087758	7.328934	-0.081360	3.687571
421.066613	4647.055423	7.333939	-0.081514	3.690682
421.263478	4655.089418	7.338944	-0.081556	3.693801
421.397702	4663.131270	7.343949	-0.081587	3.696919
421.606326	4671.181464	7.348954	-0.081631	3.700039
421.671450	4679.212567	7.353958	-0.081648	3.703145
421.510267	4687.297828	7.358963	-0.081623	3.706264
422.332442	4695.209780	7.363968	-0.081782	3.709339
422.767468	4703.268443	7.368973	-0.081868	3.712457
423.008412	4711.343622	7.373978	-0.081918	3.715575
422.827890	4719.317873	7.378982	-0.081890	3.718640
423.082639	4727.326167	7.383987	-0.081942	3.721727
423.534607	4735.327547	7.388992	-0.082032	3.724813
423.569170	4743.340155	7.393997	-0.082044	3.727891
424.130841	4751.368359	7.399002	-0.082153	3.730985
424.364144	4759.366061	7.404006	-0.082202	3.734057
423.826310	4767.525368	7.409011	-0.082107	3.737169
424.489671	4775.467133	7.414016	-0.082236	3.740224
424.195476	4783.493397	7.419021	-0.082187	3.743287
424.543096	4791.516981	7.424026	-0.082257	3.746361
424.871838	4799.492889	7.429030	-0.082323	3.749414
424.986152	4807.571763	7.434035	-0.082350	3.752498
425.401256	4815.551438	7.439040	-0.082432	3.755550
425.269947	4823.582121	7.444045	-0.082413	3.758605
425.826085	4831.574393	7.449050	-0.082522	3.761660
425.659107	4839.638484	7.454054	-0.082496	3.764722
426.236552	4847.591003	7.459059	-0.082609	3.767756
426.721142	4855.613579	7.464064	-0.082704	3.770813
427.351056	4863.575389	7.469069	-0.082827	3.773848
426.573690	4871.817316	7.474074	-0.082687	3.776953
426.733384	4879.782656	7.479078	-0.082722	3.779973
427.208604	4887.720162	7.484083	-0.082816	3.782987
427.560496	4895.765963	7.489088	-0.082887	3.786037
427.353408	4903.845159	7.494093	-0.082854	3.789084
427.441153	4911.947555	7.499098	-0.082875	3.792144
427.796200	4919.863074	7.504102	-0.082947	3.795138
428.358386	4927.826329	7.509107	-0.083056	3.798151
427.861548	4936.001945	7.514112	-0.082969	3.801218
428.613951	4943.825691	7.519117	-0.083115	3.804179
429.038008	4951.919819	7.524122	-0.083199	3.807231
429.313933	4959.925559	7.529126	-0.083255	3.810245
428.946953	4968.028503	7.534131	-0.083192	3.813278
429.567314	4976.024964	7.539136	-0.083313	3.816291
429.923019	4983.962013	7.544141	-0.083385	3.819273
429.757318	4992.088005	7.549146	-0.083359	3.822312
429.899493	5000.073734	7.554150	-0.083391	3.825302
430.617737	5008.038697	7.559155	-0.083530	3.828296
430.771695	5016.123449	7.564160	-0.083564	3.831319
430.660340	5024.148943	7.569165	-0.083548	3.834312
431.607161	5032.130146	7.574170	-0.083730	3.837309
431.581106	5040.186009	7.579174	-0.083730	3.840311
431.637792	5048.165396	7.584179	-0.083746	3.843283
432.189593	5056.214047	7.589184	-0.083854	3.846290
432.290291	5064.223662	7.594189	-0.083878	3.849270
432.082303	5072.358034	7.599194	-0.083845	3.852287
432.216488	5080.321065	7.604198	-0.083875	3.855246
432.351908	5088.320521	7.609203	-0.083905	3.858216
432.806437	5096.361277	7.614208	-0.083995	3.861206
433.439110	5104.253390	7.619213	-0.084118	3.864141
433.827642	5112.377321	7.624218	-0.084196	3.867156
433.330935	5120.485436	7.629222	-0.084109	3.870144
433.709741	5128.573680	7.634227	-0.084185	3.873140
434.116872	5136.608417	7.639232	-0.084266	3.876114
434.352414	5144.490518	7.644237	-0.084315	3.879027
434.509774	5152.538856	7.649242	-0.084349	3.881997
434.307882	5160.518189	7.654246	-0.084317	3.884932
434.695111	5168.520463	7.659251	-0.084394	3.887885
435.000365	5176.500345	7.664256	-0.084457	3.890826
435.313285	5184.505533	7.669261	-0.084520	3.893774
435.490532	5192.590615	7.674266	-0.084558	3.896746
435.470452	5200.586199	7.679270	-0.084560	3.899680
435.570303	5208.628207	7.684275	-0.084584	3.902630
435.876547	5216.669565	7.689280	-0.084646	3.905583
436.244988	5224.635343	7.694285	-0.084720	3.908506
436.880676	5232.639151	7.699290	-0.084844	3.911446
436.994435	5240.689714	7.704294	-0.084870	3.914391
437.319828	5248.724117	7.709299	-0.084936	3.917332
437.287202	5256.786087	7.714304	-0.084935	3.920274
437.635592	5264.702280	7.719309	-0.085005	3.923168
438.323284	5272.728465	7.724314	-0.085138	3.926106
438.439814	5280.735760	7.729318	-0.085165	3.929024
438.306817	5288.866695	7.734323	-0.085146	3.931980
438.414800	5296.920838	7.739328	-0.085171	3.934911
438.771609	5304.856510	7.744333	-0.085243	3.937801
438.844418	5312.945180	7.749338	-0.085262	3.940739
439.356028	5320.860014	7.754342	-0.085362	3.943620
439.783663	5328.874722	7.759347	-0.085447	3.946534
439.718731	5336.990300	7.764352	-0.085440	3.949472
440.195280	5344.967271	7.769357	-0.085534	3.952369
440.500806	5353.034010	7.774362	-0.085597	3.955292
440.560602	5361.037922	7.779366	-0.085613	3.958186
440.826758	5369.050415	7.784371	-0.085668	3.961085
441.459689	5376.973683	7.789376	-0.085791	3.963956
441.670482	5385.055465	7.794381	-0.085835	3.966874
441.748783	5393.116887	7.799386	-0.085855	3.969781
441.619518	5401.154543	7.804390	-0.085837	3.972673
441.733361	5409.166173	7.809395	-0.085863	3.975558
442.223473	5417.160165	7.814400	-0.085960	3.978441
442.588076	5425.144523	7.819405	-0.086033	3.981317
442.644414	5433.178393	7.824410	-0.086048	3.984202
442.768297	5441.195724	7.829414	-0.086077	3.987081
443.280882	5449.221211	7.834419	-0.086177	3.989968
443.293375	5457.281802	7.839424	-0.086185	3.992856
443.029476	5465.342171	7.844429	-0.086141	3.995737
443.518186	5473.302837	7.849434	-0.086237	3.998593
443.718483	5481.314437	7.854438	-0.086280	4.001461
443.956619	5489.278523	7.859443	-0.086330	4.004310
444.201881	5497.347789	7.864448	-0.086381	4.007195
444.220683	5505.357344	7.869453	-0.086389	4.010052
444.660476	5513.371534	7.874458	-0.086476	4.012916
444.979347	5521.398095	7.879462	-0.086541	4.015781
445.299192	5529.385738	7.884467	-0.086606	4.018629
445.534026	5537.470001	7.889472	-0.086655	4.021509
445.398489	5545.473342	7.894477	-0.086635	4.024351
445.683382	5553.552044	7.899482	-0.086693	4.027226
445.578610	5561.582957	7.904486	-0.086679	4.030074
446.193594	5569.559001	7.909491	-0.086799	4.032913
446.106881	5577.655150	7.914496	-0.086788	4.035781
446.351001	5585.586220	7.919501	-0.086839	4.038594
446.666760	5593.618580	7.924506	-0.086903	4.041442
446.367156	5601.655657	7.929510	-0.086852	4.044280
447.218011	5609.607046	7.934515	-0.087016	4.047104
447.447248	5617.658759	7.939520	-0.087064	4.049951
447.719789	5625.658608	7.944525	-0.087120	4.052778
447.839977	5633.743385	7.949530	-0.087148	4.055632
447.570929	5641.778054	7.954534	-0.087103	4.058459
448.877714	5649.691972	7.959539	-0.087351	4.061266
449.109306	5657.699624	7.964544	-0.087400	4.064088
449.380968	5665.770738	7.969549	-0.087456	4.066931
449.841162	5673.734769	7.974554	-0.087546	4.069736
449.890408	5681.818764	7.979558	-0.087561	4.072576
449.856730	5689.852289	7.984563	-0.087560	4.075395
449.880858	5697.896968	7.989568	-0.087570	4.078217
450.088712	5705.935137	7.994573	-0.087614	4.081037
450.211214	5713.897778	7.999578	-0.087642	4.083827
450.399261	5721.936396	8.004582	-0.087682	4.086643
451.116423	5729.881253	8.009587	-0.087821	4.089432
451.279909	5737.960782	8.014592	-0.087857	4.092258
451.314257	5745.960006	8.019597	-0.087868	4.095052
451.338699	5754.019702	8.024602	-0.087878	4.097866
451.574033	5762.036173	8.029606	-0.087927	4.100665
451.958911	5769.991306	8.034611	-0.088004	4.103443
452.327471	5778.072806	8.039616	-0.088078	4.106262
452.221701	5786.074739	8.044621	-0.088063	4.109046
452.940233	5794.107009	8.049626	-0.088203	4.111850
452.570414	5802.130286	8.054630	-0.088139	4.114633
452.759657	5810.141508	8.059635	-0.088179	4.117418
453.276895	5818.124797	8.064640	-0.088281	4.120196
453.463274	5826.085975	8.069645	-0.088321	4.122960
454.214418	5834.097523	8.074650	-0.088466	4.125747
453.681256	5842.201839	8.079654	-0.088372	4.128547
453.901932	5850.259276	8.084659	-0.088418	4.131339
454.358309	5858.205895	8.089664	-0.088509	4.134094
454.616105	5866.226931	8.094669	-0.088562	4.136870
455.143499	5874.227992	8.099674	-0.088665	4.139641
454.674618	5882.364983	8.104678	-0.088583	4.142444
455.386835	5890.240772	8.109683	-0.088721	4.145170
455.751822	5898.325102	8.114688	-0.088794	4.147962
455.569590	5906.376205	8.119693	-0.088766	4.150733
455.779386	5914.368412	8.124698	-0.088810	4.153487
455.839558	5922.429549	8.129702	-0.088827	4.156262
456.619201	5930.307518	8.134707	-0.088977	4.158980
456.589141	5938.400036	8.139712	-0.088977	4.161760
456.844025	5946.324968	8.144717	-0.089029	4.164484
457.296354	5954.440226	8.149722	-0.089119	4.167275
457.033698	5962.519903	8.154726	-0.089075	4.170042
457.745727	5970.463957	8.159731	-0.089213	4.172773
457.850140	5978.579759	8.164736	-0.089238	4.175553
457.404712	5986.573206	8.169741	-0.089160	4.178283
457.942744	5994.588852	8.174746	-0.089266	4.181031
457.852392	6002.586821	8.179750	-0.089254	4.183763
457.838304	6010.666934	8.184755	-0.089257	4.186523
458.020567	6018.696299	8.189760	-0.089296	4.189266
458.333290	6026.668003	8.194765	-0.089359	4.191988
459.189102	6034.655188	8.199770	-0.089524	4.194721
459.424237	6042.683336	8.204774	-0.089573	4.197458
459.186602	6050.680229	8.209779	-0.089534	4.200178
459.702435	6058.661022	8.214784	-0.089635	4.202898
460.132362	6066.664723	8.219789	-0.089721	4.205624
460.504038	6074.679377	8.224794	-0.089795	4.208351
460.696631	6082.796259	8.229798	-0.089836	4.211109
460.644661	6090.801248	8.234803	-0.089832	4.213825
460.970871	6098.841646	8.239808	-0.089898	4.216555
461.236940	6106.759360	8.244813	-0.089953	4.219241
461.680465	6114.860145	8.249818	-0.090041	4.221989
461.836796	6122.798242	8.254822	-0.090075	4.224677
462.082690	6130.911350	8.259827	-0.090126	4.227423
462.219310	6138.972248	8.264832	-0.090157	4.230149
462.483211	6146.910583	8.269837	-0.090211	4.232833
463.018774	6154.942894	8.274842	-0.090316	4.235550
463.545622	6162.860498	8.279846	-0.090419	4.238226
463.790446	6170.919708	8.284851	-0.090470	4.240945
464.010443	6178.961770	8.289856	-0.090517	4.243656
464.159474	6186.994495	8.294861	-0.090550	4.246362
464.924054	6194.969596	8.299866	-0.090697	4.249053
464.760573	6203.067520	8.304870	-0.090672	4.251774
464.947884	6211.046914	8.309875	-0.090712	4.254457
465.457220	6219.057405	8.314880	-0.090812	4.257152
465.626512	6227.080217	8.319885	-0.090849	4.259846
465.780991	6235.098367	8.324890	-0.090883	4.262537
465.914685	6243.097087	8.329894	-0.090913	4.265219
465.948718	6251.126101	8.334899	-0.090925	4.267909
466.365913	6259.174625	8.339904	-0.091008	4.270607
466.588037	6267.162908	8.344909	-0.091054	4.273281
467.003105	6275.205129	8.349914	-0.091137	4.275973
467.291913	6283.183159	8.354918	-0.091196	4.278641
467.460628	6291.191087	8.359923	-0.091233	4.281317
467.544391	6299.218571	8.364928	-0.091254	4.283996
467.760199	6307.214788	8.369933	-0.091299	4.286664
468.018532	6315.276797	8.374938	-0.091352	4.289353
468.159056	6323.315222	8.379942	-0.091384	4.292032
468.324577	6331.322418	8.384947	-0.091420	4.294698
468.902100	6339.327650	8.389952	-0.091533	4.297366
468.691527	6347.332243	8.394957	-0.091499	4.300025
469.161715	6355.344862	8.399962	-0.091592	4.302691
469.111658	6363.387234	8.404966	-0.091588	4.305360
469.777806	6371.356180	8.409971	-0.091717	4.308010
469.822363	6379.447672	8.414976	-0.091730	4.310693
470.287710	6387.391418	8.419981	-0.091822	4.313330
470.370194	6395.440235	8.424986	-0.091843	4.315996
470.471244	6403.438884	8.429990	-0.091867	4.318644
470.692988	6411.505641	8.434995	-0.091914	4.321314
470.942855	6419.426586	8.440000	-0.091965	4.323934
471.218912	6427.454858	8.445005	-0.092022	4.326588
471.547513	6435.470848	8.450010	-0.092088	4.329237
471.632210	6443.561064	8.455014	-0.092109	4.331907
471.883347	6451.508455	8.460019	-0.092161	4.334530
472.236188	6459.574975	8.465024	-0.092232	4.337191
472.367931	6467.532204	8.470029	-0.092262	4.339812
472.549858	6475.612716	8.475034	-0.092301	4.342473
472.795591	6483.562000	8.480038	-0.092352	4.345090
472.799547	6491.636559	8.485043	-0.092358	4.347744
473.832135	6499.581972	8.490048	-0.092556	4.350362
473.784568	6507.676247	8.495053	-0.092552	4.353019
473.830001	6515.786751	8.500058	-0.092566	4.355681
474.397426	6523.668092	8.505062	-0.092677	4.358269
474.689020	6531.718457	8.510067	-0.092737	4.360909
475.038753	6539.684866	8.515072	-0.092807	4.363521
475.265392	6547.730346	8.520077	-0.092854	4.366156
475.589617	6555.709057	8.525082	-0.092920	4.368768
475.814341	6563.777846	8.530086	-0.092967	4.371407
475.950617	6571.772173	8.535091	-0.092998	4.374020
475.870485	6579.919194	8.540096	-0.092988	4.376680
476.439790	6587.787274	8.545101	-0.093099	4.379251
476.553819	6595.850247	8.550106	-0.093126	4.381881
476.865858	6603.807865	8.555110	-0.093189	4.384477
476.973632	6611.906618	8.560115	-0.093215	4.387116
477.162046	6619.930079	8.565120	-0.093255	4.389729
477.355187	6627.935276	8.570125	-0.093296	4.392334
477.481347	6635.975392	8.575130	-0.093325	4.394949
477.689409	6643.984225	8.580135	-0.093369	4.397553
478.270195	6651.985227	8.585139	-0.093482	4.400155
478.133093	6660.076518	8.590144	-0.093462	4.402780
478.426217	6668.004013	8.595149	-0.093522	4.405353
478.806664	6676.042597	8.600154	-0.093598	4.407962
479.220344	6684.062380	8.605159	-0.093680	4.410562
479.204440	6692.122571	8.610163	-0.093683	4.413172
479.576205	6700.186606	8.615168	-0.093757	4.415783
479.886697	6708.136880	8.620173	-0.093820	4.418356
479.816777	6716.240399	8.625178	-0.093813	4.420975
479.671570	6724.192377	8.630183	-0.093791	4.423543
480.293445	6732.220387	8.635187	-0.093912	4.426138
480.451203	6740.289996	8.640192	-0.093946	4.428742
480.045034	6748.384192	8.645197	-0.093876	4.431350
481.219365	6756.236820	8.650202	-0.094100	4.433887
481.501291	6764.294665	8.655207	-0.094158	4.436483
481.799850	6772.226111	8.660211	-0.094219	4.439038
481.933636	6780.348266	8.665216	-0.094249	4.441651
481.982584	6788.262852	8.670221	-0.094263	4.444196
482.323679	6796.376870	8.675226	-0.094332	4.446805
482.308830	6804.390195	8.680231	-0.094334	4.449378
482.468761	6812.407556	8.685235	-0.094369	4.451952
482.723155	6820.427295	8.690240	-0.094422	4.454525
482.702397	6828.481991	8.695245	-0.094424	4.457107
483.216251	6836.429569	8.700250	-0.094524	4.459655
483.265263	6844.505366	8.705255	-0.094539	4.462241
483.814807	6852.390708	8.710259	-0.094646	4.464767
483.971705	6860.481306	8.715264	-0.094681	4.467355
484.243565	6868.496005	8.720269	-0.094737	4.469918
484.520094	6876.524157	8.725274	-0.094794	4.472484
484.335017	6884.534593	8.730279	-0.094764	4.475040
484.436017	6892.547886	8.735283	-0.094788	4.477598
484.790355	6900.605746	8.740288	-0.094860	4.480169
484.961481	6908.583419	8.745293	-0.094897	4.482712
485.601003	6916.569857	8.750298	-0.095021	4.485258
485.680831	6924.613837	8.755303	-0.095041	4.487819
486.338836	6932.588965	8.760307	-0.095169	4.490359
486.308203	6940.635698	8.765312	-0.095169	4.492917
486.689486	6948.645030	8.770317	-0.095245	4.495464
487.146346	6956.708374	8.775322	-0.095335	4.498026
487.291487	6964.729719	8.780327	-0.095368	4.500573
487.133473	6972.688033	8.785331	-0.095343	4.503097
487.806216	6980.733650	8.790336	-0.095474	4.505650
487.780925	6988.721312	8.795341	-0.095474	4.508181
487.568838	6996.799163	8.800346	-0.095440	4.510739
488.164945	7004.749209	8.805351	-0.095556	4.513257
488.338167	7012.801823	8.810355	-0.095594	4.515805
488.365633	7020.806121	8.815360	-0.095604	4.518336
488.773550	7028.780745	8.820365	-0.095686	4.520857
489.248387	7036.737624	8.825370	-0.095779	4.523371
489.696082	7044.769617	8.830375	-0.095868	4.525907
490.105481	7052.770005	8.835379	-0.095949	4.528432
490.462043	7060.881471	8.840384	-0.096021	4.530990
490.539134	7068.869166	8.845389	-0.096041	4.533507
490.938948	7076.883507	8.850394	-0.096120	4.536032
491.349066	7084.813094	8.855399	-0.096202	4.538528
491.447005	7092.937274	8.860403	-0.096225	4.541084
491.760627	7100.876703	8.865408	-0.096289	4.543581
491.746635	7108.959204	8.870413	-0.096292	4.546120
492.182838	7116.981350	8.875418	-0.096378	4.548640
492.482706	7125.032955	8.880423	-0.096439	4.551168
492.547664	7132.999153	8.885427	-0.096457	4.553667
492.861969	7141.072721	8.890432	-0.096521	4.556198
493.461252	7148.938789	8.895437	-0.096637	4.558664
493.746632	7157.057623	8.900442	-0.096696	4.561207
493.936996	7164.988094	8.905447	-0.096736	4.563689
495.587106	7173.075282	8.910451	-0.097049	4.566222
496.122365	7181.089925	8.915456	-0.097154	4.568728
496.594502	7189.144512	8.920461	-0.097247	4.571245
496.779105	7197.134213	8.925466	-0.097287	4.573741
496.829441	7205.206077	8.930471	-0.097301	4.576260
497.353245	7213.094926	8.935475	-0.097404	4.578721
497.531473	7221.229241	8.940480	-0.097443	4.581257
497.931002	7229.115585	8.945485	-0.097522	4.583715
498.421651	7237.225574	8.950490	-0.097619	4.586241
498.454675	7245.213625	8.955495	-0.097630	4.588727
498.373652	7253.315896	8.960499	-0.097621	4.591247
498.276338	7261.282020	8.965504	-0.097608	4.593723
498.251526	7269.297392	8.970509	-0.097608	4.596214
498.549752	7277.293946	8.975514	-0.097669	4.598697
499.409470	7285.273127	8.980519	-0.097834	4.601175
499.464695	7293.190770	8.985523	-0.097850	4.603631
499.684780	7301.387223	8.990528	-0.097896	4.606172
499.690798	7309.321742	8.995533	-0.097903	4.608630
500.005387	7317.388888	9.000538	-0.097966	4.611129
499.942213	7325.361430	9.005543	-0.097960	4.613597
500.300766	7333.398011	9.010547	-0.098032	4.616083
500.757018	7341.380332	9.015552	-0.098122	4.618551
500.930319	7349.440282	9.020557	-0.098160	4.621042
501.458561	7357.363663	9.025562	-0.098263	4.623489
501.364198	7365.429705	9.030567	-0.098251	4.625979
501.812736	7373.415579	9.035571	-0.098340	4.628443
501.984065	7381.544827	9.040576	-0.098377	4.630950
502.360533	7389.477820	9.045581	-0.098452	4.633395
502.369495	7397.559229	9.050586	-0.098459	4.635884
502.714483	7405.444110	9.055591	-0.098529	4.638311
503.302633	7413.527147	9.060595	-0.098644	4.640798
503.680753	7421.496895	9.065600	-0.098719	4.643249
503.772795	7429.569421	9.070605	-0.098742	4.645730
503.600297	7437.639005	9.075610	-0.098715	4.648209
504.027367	7445.650313	9.080615	-0.098800	4.650668
504.478311	7453.577522	9.085619	-0.098889	4.653101
504.843458	7461.675943	9.090624	-0.098962	4.655584
504.548998	7469.665793	9.095629	-0.098912	4.658033
504.879099	7477.687293	9.100634	-0.098979	4.660491
505.039465	7485.640434	9.105639	-0.099014	4.662926
504.963254	7493.729965	9.110643	-0.099005	4.665402
505.852422	7501.693236	9.115648	-0.099176	4.667837
505.747800	7509.741314	9.120653	-0.099162	4.670297
505.818377	7517.823708	9.125658	-0.099180	4.672767
506.769316	7525.788172	9.130663	-0.099363	4.675198
506.557033	7533.787373	9.135667	-0.099328	4.677640
506.553351	7541.843563	9.140672	-0.099333	4.680098
506.885656	7549.789415	9.145677	-0.099400	4.682520
506.853862	7557.823249	9.150682	-0.099400	4.684968
506.950079	7565.855619	9.155687	-0.099423	4.687415
507.684140	7573.807604	9.160691	-0.099565	4.689834
507.958863	7581.902662	9.165696	-0.099621	4.692297
508.136167	7589.851728	9.170701	-0.099659	4.694714
509.003477	7597.892405	9.175706	-0.099826	4.697157
509.218447	7605.858399	9.180711	-0.099871	4.699576
509.364403	7613.916698	9.185715	-0.099904	4.702023
509.605130	7621.889193	9.190720	-0.099954	4.704442
509.429032	7630.013964	9.195725	-0.099926	4.706906
509.899651	7637.978639	9.200730	-0.100019	4.709320
510.083463	7646.029414	9.205735	-0.100059	4.711759
509.881542	7654.047066	9.210739	-0.100026	4.714187
510.308321	7662.111879	9.215744	-0.100111	4.716627
510.608567	7669.995452	9.220749	-0.100172	4.719011
510.963397	7678.107620	9.225754	-0.100244	4.721463
511.589947	7685.967646	9.230759	-0.100366	4.723837
511.113121	7694.189156	9.235763	-0.100282	4.726322
511.630103	7702.096082	9.240768	-0.100384	4.728707
511.927699	7710.138072	9.245773	-0.100444	4.731133
512.393233	7718.088242	9.250778	-0.100536	4.733530
512.790289	7726.157101	9.255783	-0.100615	4.735961
513.038612	7734.145121	9.260787	-0.100667	4.738367
513.245815	7742.234460	9.265792	-0.100711	4.740802
513.221306	7750.237911	9.270797	-0.100712	4.743210
513.537286	7758.267023	9.275802	-0.100776	4.745625
514.167612	7766.276095	9.280807	-0.100898	4.748031
514.460879	7774.312452	9.285811	-0.100958	4.750445
514.872821	7782.364500	9.290816	-0.101040	4.752862
515.101167	7790.326510	9.295821	-0.101088	4.755251
515.297890	7798.296481	9.300826	-0.101130	4.757642
515.168852	7806.389225	9.305831	-0.101111	4.760069
515.544972	7814.331647	9.310835	-0.101186	4.762448
515.679557	7822.360193	9.315840	-0.101217	4.764852
515.963134	7830.395432	9.320845	-0.101275	4.767257
516.395698	7838.409279	9.325850	-0.101360	4.769654
516.462860	7846.419246	9.330855	-0.101378	4.772050
516.640868	7854.466863	9.335859	-0.101417	4.774455
516.936968	7862.502156	9.340864	-0.101477	4.776855
517.436063	7870.399600	9.345869	-0.101575	4.779211
517.594639	7878.534721	9.350874	-0.101610	4.781639
517.682329	7886.458634	9.355879	-0.101632	4.784003
517.888269	7894.534529	9.360883	-0.101675	4.786410
517.943717	7902.553037	9.365888	-0.101691	4.788800
518.210751	7910.539386	9.370893	-0.101746	4.791178
518.491311	7918.523689	9.375898	-0.101803	4.793554
518.650383	7926.607074	9.380903	-0.101838	4.795959
518.776339	7934.540874	9.385907	-0.101867	4.798318
518.846471	7942.660681	9.390912	-0.101885	4.800732
519.172970	7950.573608	9.395917	-0.101951	4.803082
519.545937	7958.623655	9.400922	-0.102026	4.805471
519.421103	7966.667916	9.405927	-0.102008	4.807859
519.670843	7974.655008	9.410931	-0.102060	4.810228
519.951243	7982.729762	9.415936	-0.102117	4.812621
519.699584	7990.182636	9.420941	-0.102075	4.814831
520.181258	7994.883807	9.425946	-0.102168	4.816222

520.063144	7997.534925	9.430951	-0.102148	4.817008
520.259826	7998.914402	9.435955	-0.102185	4.817416
521.071834	7999.311946	9.440960	-0.102337	4.817530
520.802240	8000.121901	9.445965	-0.102287	4.817771
521.317294	8000.151489	9.450970	-0.102383	4.817778
521.936188	8000.094025	9.455975	-0.102499	4.817758
521.951252	8000.099517	9.460979	-0.102501	4.817759
522.288456	8000.103344	9.465984	-0.102564	4.817759
522.006635	8000.140386	9.470989	-0.102512	4.817771
521.999272	8000.161368	9.475994	-0.102511	4.817778
522.344937	8000.143178	9.480999	-0.102575	4.817771
522.524628	8000.119424	9.486003	-0.102608	4.817763
522.812387	8000.103559	9.491008	-0.102662	4.817757
522.709860	8000.097862	9.496013	-0.102643	4.817756
523.015977	8000.121271	9.501018	-0.102700	4.817761
522.945290	8000.120252	9.506023	-0.102687	4.817761
523.120679	8000.113304	9.511027	-0.102720	4.817758
523.357830	8000.125174	9.516032	-0.102764	4.817761
523.130590	8000.121888	9.521037	-0.102721	4.817761
523.328344	8000.117373	9.526042	-0.102758	4.817759
522.988061	8000.120886	9.531047	-0.102695	4.817761
522.859631	8000.165419	9.536051	-0.102671	4.817775
523.487411	8000.129174	9.541056	-0.102788	4.817762
523.586562	8000.107417	9.546061	-0.102807	4.817755
523.619836	8000.179595	9.551066	-0.102813	4.817776
523.621884	8000.116369	9.556071	-0.102813	4.817757
523.283751	8000.149433	9.561075	-0.102750	4.817768
523.881993	8000.153879	9.566080	-0.102862	4.817767
524.017408	8000.115779	9.571085	-0.102887	4.817755
523.901822	8000.158389	9.576090	-0.102866	4.817768
523.883144	8000.163394	9.581095	-0.102862	4.817770
523.969003	8000.166748	9.586099	-0.102878	4.817771
523.867429	8000.217996	9.591104	-0.102859	4.817786
524.091579	8000.156932	9.596109	-0.102901	4.817767
524.381914	8000.168519	9.601114	-0.102955	4.817769
524.416897	8000.141617	9.606119	-0.102962	4.817761
524.026584	8000.202390	9.611123	-0.102889	4.817781
524.294250	8000.178857	9.616128	-0.102939	4.817773
524.656324	8000.128224	9.621133	-0.103006	4.817756
524.922954	8000.145796	9.626138	-0.103056	4.817760
524.602442	8000.144320	9.631143	-0.102996	4.817761
524.846826	8000.140482	9.636147	-0.103042	4.817759
525.041399	8000.146466	9.641152	-0.103078	4.817760
524.736530	8000.136782	9.646157	-0.103022	4.817758
524.621192	8000.198374	9.651162	-0.103000	4.817777
525.041836	8000.165460	9.656167	-0.103078	4.817766
525.001725	8000.171208	9.661171	-0.103071	4.817768
524.975399	8000.205623	9.666176	-0.103066	4.817778
525.204948	8000.174159	9.671181	-0.103109	4.817768
525.425440	8000.169976	9.676186	-0.103150	4.817765
525.052148	8000.158245	9.681191	-0.103081	4.817763
525.141709	8000.166926	9.686195	-0.103097	4.817766
525.360189	8000.169040	9.691200	-0.103138	4.817765
524.757707	8000.159261	9.696205	-0.103026	4.817765
525.028930	8000.196932	9.701210	-0.103076	4.817775
525.539863	8000.146348	9.706215	-0.103172	4.817758
525.690381	8000.164347	9.711219	-0.103200	4.817763
525.345757	8000.180444	9.716224	-0.103136	4.817769
525.528649	8000.155684	9.721229	-0.103170	4.817761
525.523444	8000.173536	9.726234	-0.103169	4.817766
525.311108	8000.193658	9.731239	-0.103129	4.817773
525.406271	8000.188714	9.736243	-0.103147	4.817771
525.969486	8000.155759	9.741248	-0.103252	4.817759
525.881921	8000.156601	9.746253	-0.103236	4.817759
525.574995	8000.180625	9.751258	-0.103179	4.817768
526.039055	8000.153613	9.756263	-0.103265	4.817758
526.044365	8000.206411	9.761267	-0.103266	4.817773
526.026300	8000.186120	9.766272	-0.103263	4.817768
525.847759	8000.161394	9.771277	-0.103229	4.817761
526.026884	8000.179808	9.776282	-0.103263	4.817766
525.673061	8000.189445	9.781287	-0.103197	4.817770
525.558132	8000.208870	9.786291	-0.103176	4.817776
525.740057	8000.220998	9.791296	-0.103210	4.817779
525.769943	8000.198239	9.796301	-0.103215	4.817772
525.932567	8000.200599	9.801306	-0.103246	4.817772
525.971806	8000.185355	9.806311	-0.103253	4.817768
526.028133	8000.168250	9.811315	-0.103263	4.817762
526.243256	8000.171371	9.816320	-0.103303	4.817762
525.900384	8000.135829	9.821325	-0.103240	4.817753
526.330190	8000.119919	9.826330	-0.103320	4.817747
526.121425	8000.152745	9.831335	-0.103281	4.817757
526.185007	8000.173703	9.836339	-0.103293	4.817763
526.280050	8000.187736	9.841344	-0.103311	4.817767
525.508342	8000.233490	9.846349	-0.103167	4.817784
525.517781	8000.229413	9.851354	-0.103169	4.817783
525.523073	8000.227384	9.856359	-0.103170	4.817782
525.855640	8000.209011	9.861363	-0.103232	4.817775
525.833052	8000.238208	9.866368	-0.103228	4.817784
525.776743	8000.216308	9.871373	-0.103217	4.817778
525.581425	8000.254601	9.876378	-0.103181	4.817790
525.608174	8000.214926	9.881383	-0.103186	4.817778
525.316168	8000.227568	9.886387	-0.103131	4.817783
525.684387	8000.247668	9.891392	-0.103200	4.817787
525.753542	8000.218097	9.896397	-0.103213	4.817778
526.014752	8000.197635	9.901402	-0.103262	4.817771
526.179913	8000.193706	9.906407	-0.103292	4.817769
526.129787	8000.186656	9.911411	-0.103283	4.817767
526.219577	8000.219592	9.916416	-0.103300	4.817777
525.856963	8000.211176	9.921421	-0.103232	4.817776
526.365918	8000.216448	9.926426	-0.103327	4.817775
525.985370	8000.286849	9.931431	-0.103256	4.817798
526.221693	8000.205928	9.936435	-0.103300	4.817773
526.344408	8000.218254	9.941440	-0.103323	4.817776
526.409099	8000.191781	9.946445	-0.103335	4.817768
526.307594	8000.208237	9.951450	-0.103317	4.817773
525.729056	8000.273660	9.956455	-0.103209	4.817795
525.624138	8000.277415	9.961459	-0.103189	4.817796
525.588868	8000.322244	9.966464	-0.103183	4.817810
525.753782	8000.224473	9.971469	-0.103214	4.817780
525.964129	8000.229634	9.976474	-0.103253	4.817781
525.935336	8000.250307	9.981479	-0.103248	4.817787
525.964602	8000.240190	9.986483	-0.103253	4.817784
526.140237	8000.282805	9.991488	-0.103286	4.817796
526.418741	8000.216203	9.996493	-0.103338	4.817775
526.449973	8000.228257	10.001498	-0.103344	4.817778
526.408667	8000.201302	10.006503	-0.103336	4.817770
526.700920	8000.188672	10.011507	-0.103390	4.817765
526.637303	8000.188807	10.016512	-0.103378	4.817766
526.693997	8000.171708	10.021517	-0.103389	4.817760
526.781221	8000.219368	10.026522	-0.103405	4.817774
526.649825	8000.228010	10.031527	-0.103381	4.817777
526.376104	8000.211392	10.036531	-0.103330	4.817773
526.587523	8000.254527	10.041536	-0.103369	4.817785
526.816018	8000.194580	10.046541	-0.103412	4.817767
526.503774	8000.211144	10.051546	-0.103354	4.817773
526.414654	8000.237269	10.056551	-0.103337	4.817781
526.380729	8000.227291	10.061555	-0.103331	4.817778
526.526734	8000.262096	10.066560	-0.103358	4.817788
526.640482	8000.186779	10.071565	-0.103380	4.817765
526.958422	8000.230404	10.076570	-0.103439	4.817777
527.018189	8000.233383	10.081575	-0.103450	4.817777
526.802824	8000.220774	10.086579	-0.103410	4.817774
526.626425	8000.227709	10.091584	-0.103377	4.817777
526.980940	8000.195948	10.096589	-0.103443	4.817766
526.718536	8000.254355	10.101594	-0.103394	4.817785
526.844266	8000.228768	10.106599	-0.103418	4.817777
527.031990	8000.230439	10.111603	-0.103453	4.817776
526.824744	8000.248524	10.116608	-0.103414	4.817783
526.850503	8000.237303	10.121613	-0.103419	4.817779
527.305349	8000.222814	10.126618	-0.103504	4.817773
527.192750	8000.205368	10.131623	-0.103483	4.817768
527.207379	8000.185550	10.136627	-0.103486	4.817762
526.920541	8000.263636	10.141632	-0.103432	4.817787
527.603865	8000.211340	10.146637	-0.103560	4.817768
527.501266	8000.196148	10.151642	-0.103540	4.817764
527.387856	8000.186071	10.156647	-0.103519	4.817762
527.145343	8000.189938	10.161651	-0.103474	4.817764
527.307418	8000.199672	10.166656	-0.103504	4.817766
526.900619	8000.180070	10.171661	-0.103429	4.817762
527.313444	8000.210310	10.176666	-0.103506	4.817769
527.389546	8000.187166	10.181671	-0.103520	4.817762
527.161779	8000.199682	10.186675	-0.103478	4.817767
527.239418	8000.246150	10.191680	-0.103492	4.817780
527.147768	8000.201594	10.196685	-0.103475	4.817767
527.148766	8000.229025	10.201690	-0.103475	4.817775
526.575470	8000.278707	10.206695	-0.103369	4.817793
526.757131	8000.261310	10.211699	-0.103402	4.817787
526.836766	8000.246653	10.216704	-0.103417	4.817782
527.158425	8000.185948	10.221709	-0.103477	4.817763
527.193785	8000.215987	10.226714	-0.103484	4.817771
527.219951	8000.193173	10.231719	-0.103489	4.817764
526.949398	8000.214558	10.236723	-0.103438	4.817772
526.846501	8000.299529	10.241728	-0.103419	4.817798
526.818068	8000.262216	10.246733	-0.103414	4.817787
526.797069	8000.241881	10.251738	-0.103410	4.817781
526.843095	8000.263640	10.256743	-0.103419	4.817787
526.928269	8000.253280	10.261747	-0.103435	4.817783
527.147913	8000.281773	10.266752	-0.103476	4.817791
526.992429	8000.241564	10.271757	-0.103447	4.817780
526.886064	8000.269547	10.276762	-0.103427	4.817788
527.166232	8000.251471	10.281767	-0.103479	4.817782
527.252904	8000.187359	10.286771	-0.103495	4.817763
527.063354	8000.239442	10.291776	-0.103460	4.817779
527.404392	8000.210650	10.296781	-0.103524	4.817769
527.571668	8000.216242	10.301786	-0.103555	4.817770
527.263091	8000.218097	10.306791	-0.103497	4.817772
527.283807	8000.180442	10.311795	-0.103501	4.817760
527.495456	8000.233071	10.316800	-0.103541	4.817775
527.286707	8000.216340	10.321805	-0.103502	4.817771
527.511013	8000.215378	10.326810	-0.103544	4.817770
527.586873	8000.231243	10.331815	-0.103558	4.817774
527.791377	8000.184656	10.336819	-0.103596	4.817759
527.321942	8000.261148	10.341824	-0.103509	4.817784
527.548016	8000.204329	10.346829	-0.103551	4.817766
527.905942	8000.201089	10.351834	-0.103617	4.817764
527.401523	8000.197993	10.356839	-0.103524	4.817765
527.478660	8000.223366	10.361843	-0.103538	4.817772
527.722300	8000.237448	10.366848	-0.103583	4.817775
527.536380	8000.210503	10.371853	-0.103549	4.817768
527.537975	8000.216855	10.376858	-0.103549	4.817770
527.306675	8000.235646	10.381863	-0.103506	4.817777
527.302297	8000.227151	10.386867	-0.103505	4.817774
527.099012	8000.295904	10.391872	-0.103468	4.817795
527.672702	8000.189299	10.396877	-0.103574	4.817761
527.557030	8000.226637	10.401882	-0.103553	4.817773
527.240357	8000.220993	10.406887	-0.103494	4.817773
527.831873	8000.186345	10.411891	-0.103604	4.817760
528.005060	8000.224710	10.416896	-0.103636	4.817770
527.528813	8000.211479	10.421901	-0.103548	4.817768
527.499706	8000.232148	10.426906	-0.103542	4.817775
528.004708	8000.199409	10.431911	-0.103636	4.817763
527.823171	8000.207323	10.436915	-0.103603	4.817766
527.896371	8000.234748	10.441920	-0.103616	4.817774
527.868500	8000.201660	10.446925	-0.103611	4.817764
528.178853	8000.212492	10.451930	-0.103669	4.817766
527.664171	8000.252477	10.456935	-0.103573	4.817780
527.425231	8000.223709	10.461939	-0.103529	4.817773
527.708866	8000.233098	10.466944	-0.103582	4.817774
527.785909	8000.240545	10.471949	-0.103596	4.817776
527.669793	8000.239918	10.476954	-0.103574	4.817776
527.613673	8000.253869	10.481959	-0.103564	4.817781
527.698127	8000.224519	10.486963	-0.103580	4.817772
527.817627	8000.227310	10.491968	-0.103602	4.817772
527.962185	8000.196724	10.496973	-0.103629	4.817762
527.914789	8000.232944	10.501978	-0.103620	4.817773
528.310901	8000.202844	10.506983	-0.103694	4.817763
528.113059	8000.213684	10.511987	-0.103657	4.817767
527.608704	8000.282288	10.516992	-0.103563	4.817789
527.932002	8000.217390	10.521997	-0.103624	4.817768
527.874171	8000.226044	10.527002	-0.103613	4.817771
528.104742	8000.231501	10.532007	-0.103656	4.817772
528.293071	8000.195223	10.537011	-0.103691	4.817760
528.260921	8000.202141	10.542016	-0.103685	4.817763
528.239342	8000.197613	10.547021	-0.103681	4.817761
528.032489	8000.223084	10.552026	-0.103643	4.817770
528.209981	8000.228826	10.557031	-0.103676	4.817771
527.956075	8000.194567	10.562035	-0.103628	4.817762
528.047209	8000.232797	10.567040	-0.103645	4.817773
527.987535	8000.184486	10.572045	-0.103634	4.817758
528.078512	8000.237475	10.577050	-0.103651	4.817774
528.016878	8000.224986	10.582055	-0.103640	4.817770
528.121483	8000.231778	10.587059	-0.103659	4.817772
528.253169	8000.241073	10.592064	-0.103684	4.817774
528.000106	8000.220534	10.597069	-0.103637	4.817769
528.096594	8000.226155	10.602074	-0.103655	4.817770
527.678931	8000.286526	10.607079	-0.103577	4.817790
527.604519	8000.256981	10.612083	-0.103563	4.817782
527.544461	8000.258222	10.617088	-0.103552	4.817782
527.566898	8000.268040	10.622093	-0.103557	4.817785
527.506904	8000.280880	10.627098	-0.103545	4.817789
527.867624	8000.228124	10.632103	-0.103613	4.817772
527.950313	8000.238816	10.637107	-0.103628	4.817775
527.799248	8000.253498	10.642112	-0.103600	4.817780
527.754259	8000.230706	10.647117	-0.103592	4.817773
527.682321	8000.272897	10.652122	-0.103578	4.817786
527.802683	8000.284136	10.657127	-0.103601	4.817789
527.673681	8000.282267	10.662131	-0.103577	4.817789
527.500205	8000.352508	10.667136	-0.103545	4.817810
527.385582	8000.344522	10.672141	-0.103523	4.817808
527.344298	8000.386102	10.677146	-0.103516	4.817821
526.969793	8000.436556	10.682151	-0.103446	4.817837
527.021459	8000.388806	10.687155	-0.103456	4.817823
527.475623	8000.344786	10.692160	-0.103540	4.817808
527.245323	8000.362537	10.697165	-0.103497	4.817814
527.334822	8000.403906	10.702170	-0.103514	4.817826
527.701313	8000.378648	10.707175	-0.103582	4.817817
527.752925	8000.361475	10.712179	-0.103592	4.817812
527.557172	8000.403978	10.717184	-0.103556	4.817825
528.052353	8000.273037	10.722189	-0.103648	4.817784
527.444136	8000.389691	10.727194	-0.103535	4.817822
527.628088	8000.316445	10.732199	-0.103569	4.817799
528.084930	8000.240832	10.737203	-0.103654	4.817775
527.986640	8000.252062	10.742208	-0.103636	4.817778
527.772271	8000.254227	10.747213	-0.103596	4.817780
528.006947	8000.254472	10.752218	-0.103639	4.817779
527.823856	8000.302431	10.757223	-0.103605	4.817794
528.093110	8000.258892	10.762227	-0.103656	4.817780
527.671103	8000.318146	10.767232	-0.103577	4.817799
527.923913	8000.272259	10.772237	-0.103624	4.817785
527.985824	8000.261562	10.777242	-0.103636	4.817781
528.353053	8000.235261	10.782247	-0.103704	4.817772
528.101996	8000.225295	10.787251	-0.103657	4.817770
528.318044	8000.248467	10.792256	-0.103698	4.817776
528.222304	8000.219666	10.797261	-0.103680	4.817768
528.475522	8000.237051	10.802266	-0.103727	4.817772
528.491310	8000.200378	10.807271	-0.103730	4.817761
528.338089	8000.231899	10.812275	-0.103702	4.817771
528.004241	8000.268181	10.817280	-0.103640	4.817783
527.847051	8000.251142	10.822285	-0.103610	4.817779
528.134342	8000.248986	10.827290	-0.103664	4.817777
528.264104	8000.254036	10.832295	-0.103688	4.817778
528.125417	8000.235156	10.837299	-0.103662	4.817773
528.255760	8000.268683	10.842304	-0.103687	4.817782
527.989335	8000.293290	10.847309	-0.103637	4.817791
527.898574	8000.294085	10.852314	-0.103620	4.817791
527.735089	8000.339164	10.857319	-0.103590	4.817805
528.043592	8000.249801	10.862323	-0.103647	4.817778
528.060015	8000.271130	10.867328	-0.103650	4.817784
527.921003	8000.270171	10.872333	-0.103624	4.817784
528.198924	8000.280533	10.877338	-0.103676	4.817786
528.082089	8000.275678	10.882343	-0.103655	4.817785
528.095075	8000.246346	10.887347	-0.103657	4.817776
528.245779	8000.241154	10.892352	-0.103685	4.817774
528.244377	8000.265389	10.897357	-0.103685	4.817781
527.855244	8000.273454	10.902362	-0.103612	4.817785
528.211987	8000.263871	10.907367	-0.103679	4.817781
528.202803	8000.251088	10.912371	-0.103677	4.817777
528.321820	8000.257035	10.917376	-0.103699	4.817778
527.711148	8000.281920	10.922381	-0.103586	4.817788
527.732997	8000.294893	10.927386	-0.103590	4.817792
527.889082	8000.279235	10.932391	-0.103619	4.817787
528.083704	8000.211416	10.937395	-0.103655	4.817766
528.234649	8000.227317	10.942400	-0.103683	4.817770
527.821803	8000.288813	10.947405	-0.103607	4.817790
527.818978	8000.285612	10.952410	-0.103606	4.817789
527.767290	8000.335477	10.957415	-0.103597	4.817804
527.713596	8000.299905	10.962419	-0.103587	4.817794
527.876078	8000.312810	10.967424	-0.103617	4.817797
528.027354	8000.279158	10.972429	-0.103645	4.817786
528.237352	8000.264283	10.977434	-0.103684	4.817781
528.504197	8000.235471	10.982439	-0.103734	4.817771
528.328094	8000.232919	10.987443	-0.103701	4.817771
528.791193	8000.225935	10.992448	-0.103787	4.817767
528.598324	8000.223139	10.997453	-0.103752	4.817767
528.536841	8000.242284	11.002458	-0.103740	4.817773
528.652335	8000.207058	11.007463	-0.103762	4.817762
528.571438	8000.189016	11.012467	-0.103747	4.817757
528.770104	8000.238298	11.017472	-0.103784	4.817771
528.485807	8000.234175	11.022477	-0.103731	4.817771
528.778360	8000.225771	11.027482	-0.103785	4.817767
528.670762	8000.231593	11.032487	-0.103765	4.817769
528.637049	8000.205801	11.037491	-0.103759	4.817762
528.354605	8000.271297	11.042496	-0.103707	4.817783
528.786890	8000.220635	11.047501	-0.103787	4.817766
528.790473	8000.228071	11.052506	-0.103788	4.817768
528.593320	8000.266336	11.057511	-0.103751	4.817780
528.517008	8000.240979	11.062515	-0.103737	4.817773
528.768783	8000.236201	11.067520	-0.103784	4.817770
528.418291	8000.237444	11.072525	-0.103719	4.817772
528.629170	8000.255270	11.077530	-0.103758	4.817777
528.667356	8000.286406	11.082535	-0.103765	4.817786
528.588966	8000.255747	11.087539	-0.103751	4.817777
529.030798	8000.262163	11.092544	-0.103833	4.817777
528.741754	8000.236882	11.097549	-0.103779	4.817771
528.767705	8000.245697	11.102554	-0.103784	4.817773
528.988104	8000.238355	11.107559	-0.103825	4.817770
528.803772	8000.236737	11.112563	-0.103791	4.817770
528.758931	8000.261396	11.117568	-0.103782	4.817778
528.720013	8000.226038	11.122573	-0.103775	4.817768
528.724861	8000.246146	11.127578	-0.103776	4.817773
528.638679	8000.286021	11.132583	-0.103760	4.817786
528.743888	8000.240101	11.137587	-0.103780	4.817772
528.906537	8000.235084	11.142592	-0.103810	4.817769
528.847975	8000.213149	11.147597	-0.103799	4.817763
528.891603	8000.246473	11.152602	-0.103807	4.817773
528.925632	8000.222718	11.157607	-0.103814	4.817766
528.680699	8000.229710	11.162611	-0.103768	4.817769
528.509018	8000.280998	11.167616	-0.103736	4.817785
528.750701	8000.210698	11.172621	-0.103781	4.817763
528.626777	8000.255298	11.177626	-0.103758	4.817777
529.009735	8000.240825	11.182631	-0.103830	4.817771
528.927340	8000.201672	11.187635	-0.103814	4.817759
529.210475	8000.219493	11.192640	-0.103867	4.817763
529.308344	8000.159759	11.197645	-0.103885	4.817745
528.992252	8000.227931	11.202650	-0.103827	4.817767
529.022778	8000.216778	11.207655	-0.103832	4.817763
529.088817	8000.194542	11.212659	-0.103845	4.817757
529.245533	8000.237943	11.217664	-0.103874	4.817769
529.069188	8000.184773	11.222669	-0.103841	4.817754
528.937921	8000.231375	11.227674	-0.103817	4.817768
529.415612	8000.217224	11.232679	-0.103906	4.817762
529.398254	8000.204322	11.237683	-0.103902	4.817758
529.472842	8000.224388	11.242688	-0.103916	4.817764
529.304828	8000.171338	11.247693	-0.103885	4.817749
529.542794	8000.174796	11.252698	-0.103929	4.817749
529.145754	8000.196451	11.257703	-0.103856	4.817757
529.038138	8000.207546	11.262707	-0.103836	4.817761
529.471846	8000.229661	11.267712	-0.103916	4.817765
529.328453	8000.192786	11.272717	-0.103890	4.817755
529.094685	8000.228410	11.277722	-0.103846	4.817767
529.242384	8000.228448	11.282727	-0.103874	4.817766
529.085427	8000.234609	11.287731	-0.103845	4.817768
529.470751	8000.218062	11.292736	-0.103916	4.817762
529.283401	8000.195311	11.297741	-0.103882	4.817756
529.432474	8000.206968	11.302746	-0.103909	4.817759
529.192743	8000.224580	11.307751	-0.103865	4.817765
529.189228	8000.208716	11.312755	-0.103864	4.817760
529.258330	8000.224484	11.317760	-0.103877	4.817765
529.228524	8000.190312	11.322765	-0.103871	4.817755
529.172524	8000.214809	11.327770	-0.103861	4.817762
529.340743	8000.220418	11.332775	-0.103892	4.817763
529.222797	8000.218709	11.337779	-0.103871	4.817763
529.140433	8000.275511	11.342784	-0.103855	4.817780
528.956246	8000.277058	11.347789	-0.103821	4.817782
529.115418	8000.247738	11.352794	-0.103851	4.817772
528.892087	8000.205485	11.357799	-0.103809	4.817761
528.713920	8000.238754	11.362803	-0.103776	4.817771
528.938745	8000.284197	11.367808	-0.103818	4.817784
529.024912	8000.229566	11.372813	-0.103834	4.817767
529.094949	8000.247457	11.377818	-0.103847	4.817772
529.098135	8000.263323	11.382823	-0.103848	4.817777
529.152999	8000.245142	11.387827	-0.103858	4.817771
529.269756	8000.253167	11.392832	-0.103880	4.817773
529.364046	8000.228178	11.397837	-0.103897	4.817765
529.335020	8000.225651	11.402842	-0.103892	4.817765
529.501044	8000.199594	11.407847	-0.103923	4.817756
528.964999	8000.220286	11.412851	-0.103823	4.817765
529.447040	8000.235722	11.417856	-0.103913	4.817767
529.337041	8000.208822	11.422861	-0.103893	4.817760
529.245338	8000.224365	11.427866	-0.103875	4.817765
529.358470	8000.250262	11.432871	-0.103897	4.817772
529.250392	8000.243424	11.437875	-0.103877	4.817770
529.189699	8000.261526	11.442880	-0.103865	4.817776
529.281010	8000.249147	11.447885	-0.103882	4.817772
529.248983	8000.236032	11.452890	-0.103876	4.817768
529.262830	8000.229910	11.457895	-0.103879	4.817766
529.205455	8000.228025	11.462899	-0.103868	4.817766
529.349383	8000.257534	11.467904	-0.103895	4.817774
529.422238	8000.189001	11.472909	-0.103909	4.817753
529.557644	8000.213113	11.477914	-0.103934	4.817760
529.274581	8000.260675	11.482919	-0.103881	4.817775
529.057745	8000.249095	11.487923	-0.103841	4.817773
529.439854	8000.237774	11.492928	-0.103912	4.817768
529.244914	8000.227566	11.497933	-0.103876	4.817766
529.317901	8000.256044	11.502938	-0.103890	4.817774
528.814453	8000.349965	11.507943	-0.103796	4.817804
528.957716	8000.255040	11.512947	-0.103823	4.817775
529.366234	8000.288389	11.517952	-0.103899	4.817783
529.102458	8000.244494	11.522957	-0.103850	4.817771
528.708144	8000.295713	11.527962	-0.103776	4.817788
529.250710	8000.279340	11.532967	-0.103877	4.817781
529.163439	8000.241170	11.537971	-0.103861	4.817770
528.994938	8000.267198	11.542976	-0.103830	4.817778
529.014491	8000.232688	11.547981	-0.103833	4.817768
529.083420	8000.252672	11.552986	-0.103846	4.817774
529.144000	8000.263044	11.557991	-0.103858	4.817777
528.937260	8000.241066	11.562995	-0.103819	4.817771
529.416344	8000.248024	11.568000	-0.103908	4.817771
529.483500	8000.220532	11.573005	-0.103921	4.817763
529.113367	8000.279483	11.578010	-0.103852	4.817782
529.040877	8000.299523	11.583015	-0.103839	4.817788
529.239725	8000.251799	11.588019	-0.103876	4.817773
529.521893	8000.246409	11.593024	-0.103928	4.817770
529.384458	8000.184313	11.598029	-0.103903	4.817752
529.166160	8000.290810	11.603034	-0.103862	4.817785
529.338238	8000.226881	11.608039	-0.103894	4.817765
529.166997	8000.242324	11.613043	-0.103862	4.817770
529.446677	8000.259041	11.618048	-0.103915	4.817774
529.250416	8000.222452	11.623053	-0.103878	4.817764
529.233101	8000.242238	11.628058	-0.103875	4.817770
529.316704	8000.261381	11.633063	-0.103890	4.817775
529.314103	8000.239203	11.638067	-0.103890	4.817769
529.469007	8000.261489	11.643072	-0.103919	4.817775
529.528454	8000.221232	11.648077	-0.103930	4.817763
529.424704	8000.250308	11.653082	-0.103911	4.817772
529.331083	8000.304838	11.658087	-0.103893	4.817788
528.962693	8000.269968	11.663091	-0.103825	4.817779
529.330592	8000.261604	11.668096	-0.103893	4.817775
529.283838	8000.249330	11.673101	-0.103885	4.817772
529.146366	8000.302169	11.678106	-0.103859	4.817788
529.659840	8000.259013	11.683111	-0.103955	4.817773
529.448879	8000.230646	11.688115	-0.103915	4.817766
529.229913	8000.288629	11.693120	-0.103875	4.817784
529.027999	8000.295191	11.698125	-0.103837	4.817787
529.120770	8000.299704	11.703130	-0.103855	4.817788
529.160873	8000.277091	11.708135	-0.103862	4.817781
529.052229	8000.297661	11.713139	-0.103842	4.817787
529.209908	8000.290463	11.718144	-0.103871	4.817784
529.051795	8000.282898	11.723149	-0.103842	4.817783
528.985877	8000.296707	11.728154	-0.103830	4.817787
529.081864	8000.325519	11.733159	-0.103848	4.817795
529.396787	8000.258392	11.738163	-0.103906	4.817774
528.930761	8000.319114	11.743168	-0.103820	4.817794
528.542650	8000.334572	11.748173	-0.103747	4.817800
528.931774	8000.280121	11.753178	-0.103820	4.817783
529.010575	8000.368787	11.758183	-0.103835	4.817808
528.754222	8000.330272	11.763187	-0.103787	4.817798
529.027951	8000.340575	11.768192	-0.103838	4.817800
528.666519	8000.338495	11.773197	-0.103771	4.817801
528.977437	8000.277636	11.778202	-0.103828	4.817782
529.147552	8000.325450	11.783207	-0.103860	4.817795
529.183267	8000.254269	11.788211	-0.103867	4.817774
528.910577	8000.287219	11.793216	-0.103816	4.817785
528.709213	8000.376036	11.798221	-0.103779	4.817812
528.756377	8000.327165	11.803226	-0.103788	4.817797
528.652135	8000.392084	11.808231	-0.103768	4.817817
528.526949	8000.422958	11.813235	-0.103745	4.817827
528.405939	8000.443348	11.818240	-0.103722	4.817833
528.848006	8000.367522	11.823245	-0.103805	4.817809
528.871976	8000.343621	11.828250	-0.103809	4.817802
528.793212	8000.315065	11.833255	-0.103795	4.817793
529.169380	8000.264643	11.838259	-0.103865	4.817777
529.113440	8000.301794	11.843264	-0.103854	4.817788
529.349231	8000.268315	11.848269	-0.103898	4.817777
529.293148	8000.286484	11.853274	-0.103888	4.817783
529.275588	8000.271470	11.858279	-0.103885	4.817778
529.362353	8000.270624	11.863283	-0.103901	4.817778
529.192636	8000.299796	11.868288	-0.103869	4.817787
528.908684	8000.316766	11.873293	-0.103816	4.817793
528.960266	8000.293266	11.878298	-0.103826	4.817786
528.618462	8000.356846	11.883303	-0.103763	4.817807
528.853287	8000.329679	11.888307	-0.103806	4.817798
528.811845	8000.356496	11.893312	-0.103799	4.817806
528.766400	8000.329479	11.898317	-0.103790	4.817798
529.348165	8000.266225	11.903322	-0.103898	4.817777
529.445090	8000.251819	11.908327	-0.103917	4.817772
529.286489	8000.218940	11.913331	-0.103887	4.817763
529.114502	8000.282877	11.918336	-0.103855	4.817783
529.360108	8000.244268	11.923341	-0.103901	4.817770
529.576076	8000.230535	11.928346	-0.103941	4.817765
529.677230	8000.235170	11.933351	-0.103960	4.817766
529.619086	8000.183715	11.938355	-0.103949	4.817751
529.658063	8000.243334	11.943360	-0.103957	4.817768
529.433956	8000.243247	11.948365	-0.103915	4.817769
529.324771	8000.253264	11.953370	-0.103895	4.817773
529.352946	8000.270547	11.958375	-0.103900	4.817778
529.500772	8000.204157	11.963379	-0.103927	4.817758
529.523911	8000.253001	11.968384	-0.103932	4.817772
529.412925	8000.238739	11.973389	-0.103911	4.817768
529.081529	8000.292980	11.978394	-0.103849	4.817786
529.233815	8000.269888	11.983399	-0.103878	4.817778
529.693262	8000.198532	11.988403	-0.103963	4.817755
530.009711	8000.189422	11.993408	-0.104022	4.817751
529.869667	8000.213753	11.998413	-0.103996	4.817759
529.661766	8000.239208	12.003418	-0.103958	4.817767
529.771225	8000.236582	12.008423	-0.103978	4.817766
529.677240	8000.215186	12.013427	-0.103961	4.817760
529.858540	8000.226257	12.018432	-0.103994	4.817763
529.747019	8000.215151	12.023437	-0.103974	4.817760
529.790345	8000.214729	12.028442	-0.103982	4.817759
529.657080	8000.263411	12.033447	-0.103957	4.817774
529.485837	8000.234566	12.038451	-0.103925	4.817767
529.642242	8000.247385	12.043456	-0.103954	4.817770
529.809311	8000.237161	12.048461	-0.103986	4.817766
529.429490	8000.249575	12.053466	-0.103915	4.817771
529.155395	8000.339444	12.058471	-0.103864	4.817799
529.005686	8000.296151	12.063475	-0.103836	4.817787
529.155528	8000.282512	12.068480	-0.103864	4.817782
529.416330	8000.258886	12.073485	-0.103913	4.817774
529.336629	8000.273549	12.078490	-0.103898	4.817779
529.387786	8000.311201	12.083495	-0.103907	4.817790
529.323362	8000.257546	12.088499	-0.103895	4.817774
529.623336	8000.254523	12.093504	-0.103951	4.817772
529.441599	8000.229744	12.098509	-0.103917	4.817765
529.081173	8000.269856	12.103514	-0.103850	4.817779
529.441665	8000.251895	12.108519	-0.103918	4.817772
529.404903	8000.243983	12.113523	-0.103911	4.817770
529.240657	8000.252146	12.118528	-0.103880	4.817773
529.503608	8000.258076	12.123533	-0.103929	4.817773
529.759053	8000.222773	12.128538	-0.103977	4.817762
529.836639	8000.239720	12.133543	-0.103991	4.817767
529.396425	8000.245985	12.138547	-0.103909	4.817770
529.277172	8000.303306	12.143552	-0.103887	4.817788
529.288066	8000.272888	12.148557	-0.103889	4.817779
529.502445	8000.233825	12.153562	-0.103929	4.817766
529.832824	8000.256551	12.158567	-0.103991	4.817772
529.887675	8000.197247	12.163571	-0.104001	4.817754
529.857368	8000.246370	12.168576	-0.103995	4.817768
529.518963	8000.237241	12.173581	-0.103932	4.817767
529.395288	8000.255483	12.178586	-0.103909	4.817773
529.605081	8000.239552	12.183591	-0.103949	4.817768
529.446869	8000.229877	12.188595	-0.103919	4.817765
529.432363	8000.285556	12.193600	-0.103917	4.817782
529.750777	8000.223751	12.198605	-0.103976	4.817762
529.331833	8000.246142	12.203610	-0.103898	4.817771
529.637644	8000.282219	12.208615	-0.103955	4.817780
529.539894	8000.243897	12.213619	-0.103937	4.817769
529.440022	8000.273029	12.218624	-0.103918	4.817778
529.416422	8000.262145	12.223629	-0.103914	4.817775
530.012697	8000.214920	12.228634	-0.104025	4.817758
530.246271	8000.230969	12.233639	-0.104068	4.817762
530.122279	8000.190156	12.238643	-0.104045	4.817751
530.116956	8000.241751	12.243648	-0.104044	4.817766
529.922664	8000.226279	12.248653	-0.104008	4.817762
530.071075	8000.247418	12.253658	-0.104036	4.817768
530.237841	8000.234026	12.258663	-0.104067	4.817763
530.267503	8000.200717	12.263667	-0.104073	4.817753
530.219969	8000.246426	12.268672	-0.104064	4.817767
530.067600	8000.229454	12.273677	-0.104035	4.817763
529.943921	8000.233988	12.278682	-0.104012	4.817764
530.171468	8000.235186	12.283687	-0.104055	4.817764
529.966282	8000.233264	12.288691	-0.104017	4.817764
530.062913	8000.243106	12.293696	-0.104035	4.817767
530.141773	8000.225274	12.298701	-0.104049	4.817761
530.422414	8000.221972	12.303706	-0.104102	4.817759
530.350504	8000.226203	12.308711	-0.104088	4.817760
530.238981	8000.170809	12.313715	-0.104068	4.817744
530.234729	8000.216092	12.318720	-0.104067	4.817758
529.908258	8000.210300	12.323725	-0.104006	4.817758
530.163505	8000.246698	12.328730	-0.104054	4.817767
530.286402	8000.222125	12.333735	-0.104077	4.817759
530.060214	8000.217788	12.338739	-0.104035	4.817759
529.899748	8000.253422	12.343744	-0.104005	4.817770
530.043308	8000.253401	12.348749	-0.104032	4.817770
529.953188	8000.265803	12.353754	-0.104015	4.817774
529.967971	8000.261803	12.358759	-0.104018	4.817773
529.922199	8000.223181	12.363763	-0.104009	4.817761
530.223618	8000.211744	12.368768	-0.104065	4.817757
529.962559	8000.230100	12.373773	-0.104017	4.817763
530.148965	8000.219102	12.378778	-0.104051	4.817759
530.270188	8000.253555	12.383783	-0.104074	4.817769
529.806891	8000.253156	12.388787	-0.103988	4.817771
529.890817	8000.270195	12.393792	-0.104003	4.817775
529.735545	8000.289033	12.398797	-0.103975	4.817782
530.023052	8000.255250	12.403802	-0.104028	4.817770
530.180219	8000.259645	12.408807	-0.104057	4.817771
529.936328	8000.238180	12.413811	-0.104012	4.817766
529.904168	8000.277786	12.418816	-0.104006	4.817778
529.741817	8000.253288	12.423821	-0.103976	4.817771
529.638805	8000.281320	12.428826	-0.103957	4.817780
530.100809	8000.302795	12.433831	-0.104043	4.817784
529.746643	8000.260748	12.438835	-0.103977	4.817773
529.612545	8000.263022	12.443840	-0.103952	4.817774
529.864014	8000.256132	12.448845	-0.103999	4.817771
529.449441	8000.287022	12.453850	-0.103922	4.817782
529.305322	8000.308130	12.458855	-0.103895	4.817789
529.418777	8000.301345	12.463859	-0.103916	4.817787
528.384223	8000.488782	12.468864	-0.103724	4.817847
528.704833	8000.398540	12.473869	-0.103783	4.817818
528.896104	8000.389721	12.478874	-0.103819	4.817815
529.069839	8000.376430	12.483879	-0.103851	4.817810
529.166432	8000.321949	12.488883	-0.103869	4.817794
529.287959	8000.359569	12.493888	-0.103892	4.817804
529.159161	8000.374573	12.498893	-0.103868	4.817809
528.852720	8000.379617	12.503898	-0.103811	4.817812
529.048335	8000.417257	12.508903	-0.103848	4.817822
529.357588	8000.278345	12.513907	-0.103905	4.817780
529.848599	8000.275987	12.518912	-0.103997	4.817777
529.701128	8000.266468	12.523917	-0.103969	4.817775
529.450683	8000.291305	12.528922	-0.103923	4.817783
529.457968	8000.333592	12.533927	-0.103924	4.817796
529.486626	8000.287615	12.538931	-0.103929	4.817782
529.456965	8000.316712	12.543936	-0.103924	4.817791
529.919927	8000.259116	12.548941	-0.104010	4.817772
529.793819	8000.254125	12.553946	-0.103987	4.817771
529.766292	8000.287471	12.558951	-0.103982	4.817781
529.582445	8000.266879	12.563955	-0.103947	4.817776
529.430057	8000.330045	12.568960	-0.103919	4.817795
529.274207	8000.319350	12.573965	-0.103890	4.817793
528.960101	8000.313738	12.578970	-0.103832	4.817792
528.665562	8000.391712	12.583975	-0.103777	4.817817
529.160113	8000.320866	12.588979	-0.103869	4.817793
528.852022	8000.393371	12.593984	-0.103812	4.817816
528.991845	8000.367989	12.598989	-0.103838	4.817808
529.148590	8000.373431	12.603994	-0.103867	4.817809
528.975977	8000.421541	12.608999	-0.103835	4.817824
528.805645	8000.416963	12.614003	-0.103803	4.817823
529.166386	8000.357882	12.619008	-0.103870	4.817804
528.806189	8000.437011	12.624013	-0.103804	4.817829
528.626399	8000.335287	12.629018	-0.103770	4.817800
529.115114	8000.389835	12.634023	-0.103861	4.817814
529.545592	8000.331767	12.639027	-0.103941	4.817795
529.742188	8000.298773	12.644032	-0.103978	4.817784
529.167959	8000.315746	12.649037	-0.103871	4.817792
529.370469	8000.314471	12.654042	-0.103909	4.817791
529.066955	8000.381770	12.659047	-0.103852	4.817812
528.959885	8000.401308	12.664051	-0.103832	4.817818
528.918350	8000.439723	12.669056	-0.103825	4.817830
529.216830	8000.414535	12.674061	-0.103880	4.817821
528.913853	8000.433337	12.679066	-0.103824	4.817828
529.083995	8000.428429	12.684071	-0.103856	4.817826
529.053961	8000.399526	12.689075	-0.103850	4.817817
529.119130	8000.356189	12.694080	-0.103862	4.817804
529.293496	8000.341852	12.699085	-0.103895	4.817799
528.656538	8000.466522	12.704090	-0.103776	4.817839
528.298279	8000.441290	12.709095	-0.103710	4.817833
528.233624	8000.348619	12.714099	-0.103698	4.817806
528.392590	8000.243378	12.719104	-0.103727	4.817774
528.658384	8000.515066	12.724109	-0.103777	4.817853
528.375293	8000.375991	12.729114	-0.103724	4.817813
528.413308	8000.440867	12.734119	-0.103731	4.817832
528.515093	8000.475035	12.739123	-0.103750	4.817842
528.367025	8000.486597	12.744128	-0.103723	4.817846
528.646145	8000.453746	12.749133	-0.103775	4.817835
528.501662	8000.459033	12.754138	-0.103748	4.817837
528.713154	8000.436800	12.759143	-0.103787	4.817830
528.609869	8000.333023	12.764147	-0.103768	4.817799
528.837378	8000.390105	12.769152	-0.103810	4.817815
529.247650	8000.311709	12.774157	-0.103887	4.817790
528.953980	8000.350681	12.779162	-0.103832	4.817803
529.252049	8000.338140	12.784167	-0.103888	4.817798
529.248943	8000.340207	12.789171	-0.103887	4.817799
529.273741	8000.409110	12.794176	-0.103892	4.817819
529.487352	8000.350002	12.799181	-0.103932	4.817801
529.778118	8000.223475	12.804186	-0.103986	4.817762
529.729872	8000.308189	12.809191	-0.103977	4.817787
529.487179	8000.288851	12.814195	-0.103932	4.817783
529.228275	8000.379995	12.819200	-0.103884	4.817811
529.373191	8000.336761	12.824205	-0.103911	4.817797
529.339051	8000.283546	12.829210	-0.103904	4.817782
529.218219	8000.342953	12.834215	-0.103882	4.817800
529.312107	8000.297923	12.839219	-0.103899	4.817786
529.441079	8000.304017	12.844224	-0.103923	4.817787
529.532812	8000.275827	12.849229	-0.103941	4.817778
529.818989	8000.277877	12.854234	-0.103994	4.817778
529.868404	8000.349247	12.859239	-0.104003	4.817799
529.527786	8000.313724	12.864243	-0.103940	4.817790
529.540219	8000.397210	12.869248	-0.103942	4.817814
529.341487	8000.422798	12.874253	-0.103905	4.817823
528.658973	8000.404456	12.879258	-0.103778	4.817820
528.825334	8000.461705	12.884263	-0.103809	4.817837
528.734027	8000.468818	12.889267	-0.103792	4.817839
529.124257	8000.382750	12.894272	-0.103865	4.817812
529.381234	8000.359069	12.899277	-0.103913	4.817804
529.252216	8000.391996	12.904282	-0.103889	4.817814
529.417461	8000.423923	12.909287	-0.103920	4.817823
529.360954	8000.338749	12.914291	-0.103909	4.817798
529.381021	8000.411801	12.919296	-0.103913	4.817819
529.161524	8000.397018	12.924301	-0.103872	4.817816
528.998359	8000.410469	12.929306	-0.103842	4.817821
528.682252	8000.482857	12.934311	-0.103783	4.817843
528.418381	8000.481138	12.939315	-0.103734	4.817844
529.005178	8000.387379	12.944320	-0.103843	4.817814
529.176173	8000.378266	12.949325	-0.103875	4.817810
528.889077	8000.380428	12.954330	-0.103822	4.817812
529.192243	8000.423848	12.959335	-0.103878	4.817824
528.825844	8000.418531	12.964339	-0.103810	4.817824
528.869553	8000.428658	12.969344	-0.103818	4.817827
529.018051	8000.394966	12.974349	-0.103846	4.817816
529.137248	8000.319725	12.979354	-0.103868	4.817793
529.090081	8000.440306	12.984359	-0.103859	4.817829
529.426853	8000.328154	12.989363	-0.103922	4.817794
529.283814	8000.399892	12.994368	-0.103895	4.817816
529.104113	8000.362489	12.999373	-0.103862	4.817806
528.957603	8000.393053	13.004378	-0.103835	4.817816
528.993482	8000.469498	13.009383	-0.103842	4.817838
528.940532	8000.430772	13.014387	-0.103832	4.817827
529.168242	8000.370814	13.019392	-0.103874	4.817808
528.932297	8000.444366	13.024397	-0.103830	4.817831
528.935625	8000.389586	13.029402	-0.103831	4.817815
529.487887	8000.357539	13.034407	-0.103934	4.817803
529.066144	8000.400978	13.039411	-0.103855	4.817817
529.436372	8000.340980	13.044416	-0.103924	4.817798
529.394420	8000.348810	13.049421	-0.103916	4.817801
529.451826	8000.277944	13.054426	-0.103927	4.817779
529.484391	8000.388083	13.059431	-0.103933	4.817812
529.616056	8000.268736	13.064435	-0.103958	4.817776
529.838836	8000.284627	13.069440	-0.103999	4.817780
529.780735	8000.280623	13.074445	-0.103988	4.817779
529.485430	8000.307972	13.079450	-0.103934	4.817788
529.551519	8000.345841	13.084455	-0.103946	4.817799
529.301529	8000.345377	13.089459	-0.103899	4.817800
529.580394	8000.355757	13.094464	-0.103951	4.817802
529.304768	8000.359139	13.099469	-0.103900	4.817804
529.307979	8000.338099	13.104474	-0.103901	4.817798
529.687919	8000.362600	13.109479	-0.103972	4.817803
529.147257	8000.325228	13.114483	-0.103871	4.817795
529.406365	8000.336374	13.119488	-0.103919	4.817797
529.368118	8000.348475	13.124493	-0.103912	4.817801
529.677768	8000.305524	13.129498	-0.103970	4.817787
529.587720	8000.327418	13.134503	-0.103953	4.817793
529.478656	8000.287877	13.139507	-0.103933	4.817782
529.586133	8000.312639	13.144512	-0.103953	4.817789
529.780270	8000.278555	13.149517	-0.103989	4.817778
529.484284	8000.320656	13.154522	-0.103934	4.817792
529.730489	8000.350596	13.159527	-0.103980	4.817800
529.669372	8000.280117	13.164531	-0.103968	4.817779
530.381458	8000.258828	13.169536	-0.104101	4.817770
530.038243	8000.231703	13.174541	-0.104037	4.817763
529.893937	8000.261244	13.179546	-0.104010	4.817773
529.674778	8000.284426	13.184551	-0.103970	4.817780
529.503362	8000.305138	13.189555	-0.103938	4.817787
529.759024	8000.342597	13.194560	-0.103985	4.817797
529.792532	8000.288255	13.199565	-0.103992	4.817781
529.927341	8000.273344	13.204570	-0.104017	4.817776
530.278294	8000.256300	13.209575	-0.104082	4.817769
529.934309	8000.254471	13.214579	-0.104018	4.817770
529.965973	8000.307658	13.219584	-0.104024	4.817786
529.681590	8000.298258	13.224589	-0.103971	4.817784
529.771701	8000.374437	13.229594	-0.103988	4.817807
529.643683	8000.346219	13.234599	-0.103964	4.817799
529.726176	8000.308405	13.239603	-0.103980	4.817787
530.037459	8000.292894	13.244608	-0.104038	4.817781
529.930857	8000.298731	13.249613	-0.104018	4.817783
529.488608	8000.317618	13.254618	-0.103936	4.817791
529.967949	8000.296112	13.259623	-0.104025	4.817783
530.225556	8000.241861	13.264627	-0.104073	4.817765
530.093736	8000.296891	13.269632	-0.104048	4.817782
530.325925	8000.229617	13.274637	-0.104092	4.817761
530.099776	8000.259024	13.279642	-0.104050	4.817771
529.991634	8000.315452	13.284647	-0.104029	4.817788
529.993366	8000.282792	13.289651	-0.104030	4.817778
530.047623	8000.273039	13.294656	-0.104040	4.817775
529.637229	8000.337731	13.299661	-0.103964	4.817796
529.669828	8000.303410	13.304666	-0.103970	4.817786
530.072097	8000.280785	13.309671	-0.104045	4.817778
529.918887	8000.294380	13.314675	-0.104016	4.817782
529.842680	8000.298549	13.319680	-0.104002	4.817784
529.719780	8000.305203	13.324685	-0.103979	4.817786
529.962419	8000.276041	13.329690	-0.104024	4.817777
530.164054	8000.285300	13.334695	-0.104062	4.817778
529.794622	8000.233541	13.339699	-0.103993	4.817765
529.921864	8000.284952	13.344704	-0.104017	4.817779
529.639109	8000.349389	13.349709	-0.103964	4.817800
529.928266	8000.308249	13.354714	-0.104018	4.817786
530.392413	8000.301286	13.359719	-0.104105	4.817782
530.076971	8000.288271	13.364723	-0.104046	4.817780
529.894597	8000.310933	13.369728	-0.104012	4.817787
530.325382	8000.269742	13.374733	-0.104092	4.817773
530.138257	8000.272300	13.379738	-0.104058	4.817775
529.948530	8000.314889	13.384743	-0.104022	4.817788
529.973176	8000.262527	13.389747	-0.104027	4.817773
530.282373	8000.289165	13.394752	-0.104084	4.817779
530.504469	8000.231234	13.399757	-0.104126	4.817761
530.205039	8000.254305	13.404762	-0.104070	4.817769
530.269369	8000.285822	13.409767	-0.104082	4.817778
529.958233	8000.300287	13.414771	-0.104024	4.817784
530.291110	8000.297743	13.419776	-0.104086	4.817782
529.963974	8000.302485	13.424781	-0.104025	4.817784
529.309860	8000.403708	13.429786	-0.103904	4.817817
529.809392	8000.331880	13.434791	-0.103997	4.817794
529.647460	8000.292626	13.439795	-0.103967	4.817783
529.587285	8000.357132	13.444800	-0.103956	4.817802
529.800718	8000.319110	13.449805	-0.103995	4.817790
529.438234	8000.318067	13.454810	-0.103928	4.817791
529.611498	8000.319532	13.459815	-0.103960	4.817791
529.028220	8000.421783	13.464819	-0.103852	4.817824
529.253551	8000.322776	13.469824	-0.103894	4.817793
529.195951	8000.385210	13.474829	-0.103883	4.817812
529.685374	8000.282657	13.479834	-0.103974	4.817780
529.234644	8000.374180	13.484839	-0.103890	4.817809
529.246799	8000.342725	13.489843	-0.103892	4.817799
529.435054	8000.327536	13.494848	-0.103928	4.817794
529.600522	8000.325725	13.499853	-0.103958	4.817793
529.264371	8000.346153	13.504858	-0.103896	4.817800
529.347226	8000.369503	13.509863	-0.103911	4.817807
529.341044	8000.292441	13.514867	-0.103910	4.817784
529.254720	8000.342859	13.519872	-0.103894	4.817799
528.834922	8000.414797	13.524877	-0.103816	4.817822
528.811717	8000.380721	13.529882	-0.103812	4.817812
529.241238	8000.356381	13.534887	-0.103892	4.817803
529.114421	8000.389340	13.539891	-0.103868	4.817814
529.046356	8000.343013	13.544896	-0.103856	4.817800
529.140388	8000.406594	13.549901	-0.103873	4.817819
529.064401	8000.392841	13.554906	-0.103859	4.817815
529.053701	8000.453847	13.559911	-0.103857	4.817833
529.472996	8000.387181	13.564915	-0.103935	4.817812
529.601428	8000.367960	13.569920	-0.103959	4.817805
529.536232	8000.370180	13.574925	-0.103947	4.817806
529.305668	8000.343637	13.579930	-0.103904	4.817799
529.260771	8000.429454	13.584935	-0.103896	4.817825
529.336007	8000.384153	13.589939	-0.103910	4.817811
529.418618	8000.387465	13.594944	-0.103925	4.817812
529.299017	8000.379404	13.599949	-0.103903	4.817810
529.313799	8000.360642	13.604954	-0.103906	4.817804
528.845949	8000.388649	13.609959	-0.103819	4.817815
529.019099	8000.422800	13.614963	-0.103851	4.817824
529.419775	8000.361136	13.619968	-0.103926	4.817804
529.371988	8000.359391	13.624973	-0.103917	4.817804
529.054990	8000.356900	13.629978	-0.103858	4.817804
529.621683	8000.333498	13.634983	-0.103963	4.817795
530.060015	8000.261836	13.639987	-0.104045	4.817772
530.076180	8000.282109	13.644992	-0.104048	4.817778
530.587084	8000.254736	13.649997	-0.104143	4.817768
530.166531	8000.287646	13.655002	-0.104065	4.817779
529.983390	8000.319787	13.660007	-0.104031	4.817789
529.615865	8000.307071	13.665011	-0.103963	4.817787
529.903535	8000.331287	13.670016	-0.104016	4.817793
529.960599	8000.313138	13.675021	-0.104027	4.817788
529.868008	8000.298088	13.680026	-0.104010	4.817783
529.427152	8000.398190	13.685031	-0.103928	4.817815
529.360479	8000.358210	13.690035	-0.103915	4.817803
529.624839	8000.335691	13.695040	-0.103964	4.817796
529.805180	8000.336204	13.700045	-0.103998	4.817795
529.880712	8000.310942	13.705050	-0.104012	4.817787
530.042859	8000.344935	13.710055	-0.104042	4.817797
529.697622	8000.296690	13.715059	-0.103978	4.817784
529.903706	8000.352410	13.720064	-0.104017	4.817799
529.643724	8000.362345	13.725069	-0.103968	4.817803
529.282955	8000.365545	13.730074	-0.103901	4.817806
529.758469	8000.389325	13.735079	-0.103990	4.817811
530.160246	8000.252810	13.740083	-0.104065	4.817769
529.696702	8000.323058	13.745088	-0.103978	4.817792
529.715091	8000.306456	13.750093	-0.103982	4.817787
530.371622	8000.229528	13.755098	-0.104104	4.817761
530.424570	8000.294624	13.760103	-0.104114	4.817780
530.178257	8000.261524	13.765107	-0.104068	4.817771
530.156729	8000.287576	13.770112	-0.104064	4.817779
529.971200	8000.328118	13.775117	-0.104030	4.817792
529.732862	8000.366838	13.780122	-0.103985	4.817804
530.066393	8000.327398	13.785127	-0.104047	4.817791
530.179749	8000.274215	13.790131	-0.104069	4.817775
529.877577	8000.317280	13.795136	-0.104012	4.817789
530.018430	8000.297185	13.800141	-0.104039	4.817783
530.174707	8000.286804	13.805146	-0.104068	4.817779
530.022510	8000.280379	13.810151	-0.104039	4.817778
529.805581	8000.295158	13.815155	-0.103999	4.817783
529.922638	8000.307406	13.820160	-0.104021	4.817786
530.383586	8000.316213	13.825165	-0.104107	4.817787
529.970991	8000.306005	13.830170	-0.104030	4.817785
530.178262	8000.306910	13.835175	-0.104069	4.817785
530.226699	8000.268601	13.840179	-0.104078	4.817773
530.468756	8000.285829	13.845184	-0.104123	4.817777
529.975871	8000.280781	13.850189	-0.104031	4.817778
529.962905	8000.285869	13.855194	-0.104029	4.817779
529.989834	8000.329496	13.860199	-0.104034	4.817792
529.891556	8000.277457	13.865203	-0.104015	4.817777
529.911841	8000.288300	13.870208	-0.104019	4.817780
529.734542	8000.327907	13.875213	-0.103986	4.817793
529.838203	8000.305163	13.880218	-0.104006	4.817786
529.981646	8000.293541	13.885223	-0.104032	4.817782
529.441429	8000.398526	13.890227	-0.103932	4.817815
529.626059	8000.341106	13.895232	-0.103966	4.817797
530.014306	8000.327768	13.900237	-0.104039	4.817792
530.076374	8000.317073	13.905242	-0.104050	4.817788
530.246902	8000.336425	13.910247	-0.104082	4.817793
530.302616	8000.254988	13.915251	-0.104092	4.817769
530.426193	8000.290530	13.920256	-0.104115	4.817779
530.212537	8000.343317	13.925261	-0.104076	4.817795
530.017371	8000.278271	13.930266	-0.104039	4.817777
530.053028	8000.328352	13.935271	-0.104046	4.817792
529.729723	8000.316279	13.940275	-0.103986	4.817789
530.114916	8000.307114	13.945280	-0.104058	4.817785
530.229290	8000.262381	13.950285	-0.104079	4.817771
530.048657	8000.296667	13.955290	-0.104045	4.817782
530.367157	8000.300242	13.960295	-0.104105	4.817782
530.218623	8000.280162	13.965299	-0.104077	4.817777
530.265449	8000.282954	13.970304	-0.104086	4.817777
530.083421	8000.341473	13.975309	-0.104052	4.817795
530.192161	8000.274514	13.980314	-0.104072	4.817775
530.583033	8000.289686	13.985319	-0.104145	4.817778
530.049326	8000.286154	13.990323	-0.104046	4.817779
530.381695	8000.294149	13.995328	-0.104108	4.817780
529.977138	8000.337836	14.000333	-0.104033	4.817795
530.157630	8000.295118	14.005338	-0.104066	4.817781
530.070429	8000.326543	14.010343	-0.104050	4.817791
529.936251	8000.291909	14.015347	-0.104025	4.817781
529.826275	8000.348311	14.020352	-0.104005	4.817798
529.623743	8000.411804	14.025357	-0.103967	4.817818
529.652925	8000.380597	14.030362	-0.103972	4.817809
529.986109	8000.365404	14.035367	-0.104035	4.817803
530.135224	8000.245254	14.040371	-0.104062	4.817767
530.169459	8000.282661	14.045376	-0.104069	4.817778
530.008767	8000.367852	14.050381	-0.104039	4.817803
529.759191	8000.338923	14.055386	-0.103992	4.817796
530.011517	8000.326774	14.060391	-0.104039	4.817791
529.578025	8000.343679	14.065395	-0.103959	4.817798
529.735544	8000.322772	14.070400	-0.103988	4.817791
529.884223	8000.312281	14.075405	-0.104016	4.817788
529.765531	8000.284198	14.080410	-0.103994	4.817780
529.789546	8000.352036	14.085415	-0.103998	4.817800
530.025593	8000.290090	14.090419	-0.104042	4.817780
530.204051	8000.289522	14.095424	-0.104076	4.817779
530.283256	8000.278022	14.100429	-0.104090	4.817776
529.681061	8000.320948	14.105434	-0.103978	4.817791
530.105136	8000.355581	14.110439	-0.104057	4.817799
529.892363	8000.335622	14.115443	-0.104018	4.817794
530.153048	8000.285634	14.120448	-0.104066	4.817778
530.230207	8000.319446	14.125453	-0.104081	4.817788
530.432944	8000.268616	14.130458	-0.104118	4.817772
530.251485	8000.344015	14.135463	-0.104085	4.817795
530.403578	8000.271359	14.140467	-0.104113	4.817773
530.544711	8000.245996	14.145472	-0.104139	4.817765
530.566770	8000.258973	14.150477	-0.104144	4.817769
530.390031	8000.258518	14.155482	-0.104111	4.817769
530.735728	8000.276197	14.160487	-0.104175	4.817773
530.684969	8000.270190	14.165491	-0.104166	4.817772
530.682404	8000.297573	14.170496	-0.104165	4.817780
531.020804	8000.259259	14.175501	-0.104228	4.817767
530.349317	8000.279032	14.180506	-0.104103	4.817776
530.197118	8000.392817	14.185511	-0.104075	4.817810
530.278208	8000.291714	14.190515	-0.104090	4.817780
530.173507	8000.293359	14.195520	-0.104071	4.817781
530.024801	8000.352362	14.200525	-0.104043	4.817799
530.319337	8000.256468	14.205530	-0.104098	4.817769
530.310600	8000.280597	14.210535	-0.104096	4.817776
529.868267	8000.323736	14.215539	-0.104014	4.817791
530.265412	8000.297873	14.220544	-0.104088	4.817782
530.160160	8000.292130	14.225549	-0.104068	4.817780
530.024251	8000.288050	14.230554	-0.104043	4.817780
530.026965	8000.303910	14.235559	-0.104044	4.817784
530.222152	8000.299367	14.240563	-0.104080	4.817782
530.410586	8000.277854	14.245568	-0.104115	4.817775
530.201143	8000.309613	14.250573	-0.104076	4.817785
530.189137	8000.294679	14.255578	-0.104074	4.817781
529.889186	8000.376792	14.260583	-0.104018	4.817807
529.536418	8000.384325	14.265587	-0.103953	4.817810
529.667706	8000.372527	14.270592	-0.103977	4.817806
530.120634	8000.307404	14.275597	-0.104061	4.817785
529.718405	8000.359561	14.280602	-0.103987	4.817802
529.950761	8000.349231	14.285607	-0.104030	4.817798
529.612257	8000.383333	14.290611	-0.103967	4.817810
530.038461	8000.333640	14.295616	-0.104046	4.817793
530.484059	8000.296882	14.300621	-0.104129	4.817780
530.376122	8000.249975	14.305626	-0.104109	4.817767
530.579413	8000.280347	14.310631	-0.104147	4.817775
530.611182	8000.273431	14.315635	-0.104153	4.817773
530.425881	8000.279178	14.320640	-0.104119	4.817775
530.191737	8000.362247	14.325645	-0.104075	4.817801
530.072741	8000.330996	14.330650	-0.104053	4.817792
530.378206	8000.331219	14.335655	-0.104110	4.817791
530.255214	8000.304128	14.340659	-0.104087	4.817783
530.661348	8000.269961	14.345664	-0.104163	4.817772
530.305846	8000.295379	14.350669	-0.104097	4.817781
530.382896	8000.240614	14.355674	-0.104111	4.817764
530.317471	8000.293445	14.360679	-0.104099	4.817780
530.367095	8000.275189	14.365683	-0.104108	4.817774
530.472569	8000.288323	14.370688	-0.104128	4.817778
530.328190	8000.278848	14.375693	-0.104101	4.817776
530.777522	8000.237927	14.380698	-0.104185	4.817762
530.494897	8000.280221	14.385703	-0.104132	4.817775
530.467559	8000.289318	14.390707	-0.104127	4.817778
530.615378	8000.285141	14.395712	-0.104155	4.817776
530.870376	8000.287795	14.400717	-0.104202	4.817776
530.504692	8000.272995	14.405722	-0.104134	4.817773
530.375887	8000.304870	14.410727	-0.104110	4.817783
529.922809	8000.409012	14.415731	-0.104026	4.817816
529.873388	8000.350301	14.420736	-0.104017	4.817799
529.429921	8000.402914	14.425741	-0.103934	4.817816
529.894502	7999.418487	14.430746	-0.104020	4.817523

529.834805	7996.217804	14.435751	-0.104007	4.816575
529.573132	7990.633026	14.440755	-0.103955	4.814922
529.880590	7984.000638	14.445760	-0.104008	4.812956
529.612715	7976.759493	14.450765	-0.103953	4.810810
529.601270	7969.098969	14.455770	-0.103946	4.808538
529.989016	7961.324422	14.460775	-0.104013	4.806230
530.141449	7953.354759	14.465779	-0.104036	4.803863
530.083984	7945.549094	14.470784	-0.104021	4.801545
529.924636	7937.555783	14.475789	-0.103986	4.799171
529.836714	7929.589460	14.480794	-0.103964	4.796803
530.321256	7921.539893	14.485799	-0.104049	4.794407
529.982901	7913.552126	14.490803	-0.103981	4.792031
529.950922	7905.500920	14.495808	-0.103970	4.789634
529.870308	7897.587296	14.500813	-0.103950	4.787276
529.389947	7889.497986	14.505818	-0.103855	4.784867
529.705924	7881.539446	14.510823	-0.103909	4.782493
529.494520	7873.508613	14.515827	-0.103864	4.780098
529.635902	7865.507824	14.520832	-0.103885	4.777709
529.670966	7857.568344	14.525837	-0.103887	4.775338
529.844480	7849.489103	14.530842	-0.103914	4.772923
529.959817	7841.489491	14.535847	-0.103930	4.770532
529.589692	7833.491900	14.540851	-0.103856	4.768141
529.581103	7825.509490	14.545856	-0.103849	4.765752
529.767262	7817.485102	14.550861	-0.103879	4.763349
529.947787	7809.513619	14.555866	-0.103907	4.760961
530.049216	7801.520313	14.560871	-0.103921	4.758565
529.558717	7793.618018	14.565875	-0.103824	4.756197
529.529857	7785.513990	14.570880	-0.103814	4.753766
529.121991	7777.565615	14.575885	-0.103733	4.751381
529.104555	7769.446110	14.580890	-0.103724	4.748943
529.512101	7761.463312	14.585895	-0.103795	4.746543
529.534058	7753.436466	14.590899	-0.103794	4.744130
529.506206	7745.523293	14.595904	-0.103784	4.741751
529.590733	7737.479147	14.600909	-0.103794	4.739330
529.606135	7729.438539	14.605914	-0.103792	4.736909
529.474078	7721.447527	14.610919	-0.103762	4.734502
529.722515	7713.429339	14.615923	-0.103803	4.732085
529.291509	7705.445349	14.620928	-0.103718	4.729679
529.734184	7697.396339	14.625933	-0.103795	4.727249
529.455896	7689.357647	14.630938	-0.103738	4.724824
529.390778	7681.493111	14.635943	-0.103721	4.722449
528.807751	7673.544443	14.640947	-0.103607	4.720048
529.018342	7665.530791	14.645952	-0.103641	4.717625
528.802997	7657.503063	14.650957	-0.103596	4.715198
529.217222	7649.453432	14.655962	-0.103668	4.712761
529.185874	7641.416563	14.660967	-0.103657	4.710328
529.145284	7633.430180	14.665971	-0.103644	4.707908
529.165336	7625.393676	14.670976	-0.103642	4.705473
529.254043	7617.397718	14.675981	-0.103654	4.703048
528.624670	7609.456764	14.680986	-0.103531	4.700639
529.696405	7601.426578	14.685991	-0.103726	4.698200
529.382213	7593.466677	14.690995	-0.103662	4.695783
529.253724	7585.444040	14.696000	-0.103633	4.693345
529.208680	7577.487582	14.701005	-0.103620	4.690926
529.148184	7569.380253	14.706010	-0.103603	4.688460
529.050699	7561.496543	14.711015	-0.103580	4.686061
529.318070	7553.368158	14.716019	-0.103624	4.683586
529.016938	7545.539089	14.721024	-0.103563	4.681201
529.298818	7537.456996	14.726029	-0.103610	4.678737
529.125957	7529.476920	14.731034	-0.103573	4.676303
529.100902	7521.453428	14.736039	-0.103563	4.673855
529.120322	7513.417922	14.741043	-0.103562	4.671402
529.007819	7505.363827	14.746048	-0.103536	4.668942
528.787988	7497.435309	14.751053	-0.103489	4.666519
528.545561	7489.390510	14.756058	-0.103439	4.664059
528.660346	7481.503773	14.761063	-0.103455	4.661646
528.613382	7473.392403	14.766067	-0.103441	4.659163
528.453894	7465.439093	14.771072	-0.103407	4.656727
528.588482	7457.373277	14.776077	-0.103426	4.654255
528.648487	7449.388985	14.781082	-0.103432	4.651807
528.480400	7441.437152	14.786087	-0.103396	4.649368
528.429490	7433.465248	14.791091	-0.103381	4.646922
528.487578	7425.384813	14.796096	-0.103387	4.644440
528.545542	7417.444807	14.801101	-0.103393	4.642001
528.288050	7409.377926	14.806106	-0.103339	4.639521
528.464295	7401.446368	14.811111	-0.103367	4.637081
528.421638	7393.392189	14.816115	-0.103354	4.634603
528.598104	7385.427407	14.821120	-0.103382	4.632150
528.553539	7377.349386	14.826125	-0.103368	4.629662
528.139286	7369.399566	14.831130	-0.103286	4.627211
528.418725	7361.341104	14.836135	-0.103333	4.624726
528.830809	7353.349433	14.841139	-0.103404	4.622261
528.432971	7345.395335	14.846144	-0.103325	4.619805
528.510184	7337.434782	14.851149	-0.103334	4.617346
528.379552	7329.350555	14.856154	-0.103305	4.614847
528.281917	7321.404946	14.861159	-0.103281	4.612390
528.151925	7313.347673	14.866163	-0.103252	4.609897
528.027859	7305.393613	14.871168	-0.103224	4.607435
528.390426	7297.342863	14.876173	-0.103286	4.604942
527.851623	7289.423692	14.881178	-0.103181	4.602487
527.800112	7281.413921	14.886183	-0.103166	4.600004
528.026005	7273.384498	14.891187	-0.103203	4.597513
527.492398	7265.403092	14.896192	-0.103098	4.595035
527.496889	7257.396179	14.901197	-0.103094	4.592548
527.711148	7249.322522	14.906202	-0.103128	4.590040
527.393318	7241.398834	14.911207	-0.103064	4.587576
527.328576	7233.306927	14.916211	-0.103047	4.585059
527.173316	7225.358272	14.921216	-0.103013	4.582585
527.309332	7217.333494	14.926221	-0.103033	4.580086
527.607477	7209.275230	14.931226	-0.103083	4.577575
527.716465	7201.263247	14.936231	-0.103098	4.575078
527.566840	7193.350972	14.941235	-0.103065	4.572609
527.478441	7185.296704	14.946240	-0.103044	4.570096
527.558602	7177.316957	14.951245	-0.103054	4.567604
527.597253	7169.265854	14.956250	-0.103056	4.565089
527.899334	7161.325473	14.961255	-0.103107	4.562607
527.142651	7153.350786	14.966259	-0.102961	4.560111
526.953577	7145.377234	14.971264	-0.102920	4.557615
526.878711	7137.363540	14.976269	-0.102901	4.555106
526.816138	7129.295443	14.981274	-0.102884	4.552578
527.065207	7121.291467	14.986279	-0.102925	4.550070
527.109416	7113.299222	14.991283	-0.102928	4.547563
526.717123	7105.287665	14.996288	-0.102850	4.545048
526.761479	7097.328169	15.001293	-0.102853	4.542549
526.332466	7089.328953	15.006298	-0.102768	4.540034
526.508498	7081.338569	15.011303	-0.102796	4.537523
526.648250	7073.264519	15.016307	-0.102817	4.534984
526.889756	7065.235768	15.021312	-0.102857	4.532458
526.937719	7057.248710	15.026317	-0.102860	4.529943
526.779646	7049.235149	15.031322	-0.102826	4.527418
527.157745	7041.207572	15.036327	-0.102891	4.524889
527.189602	7033.286400	15.041331	-0.102892	4.522390
527.560985	7025.171658	15.046336	-0.102956	4.519831
527.684609	7017.259407	15.051341	-0.102973	4.517333
527.759724	7009.224510	15.056346	-0.102982	4.514795
527.739524	7001.280939	15.061351	-0.102973	4.512284
527.684855	6993.260240	15.066355	-0.102958	4.509747
527.775976	6985.203160	15.071360	-0.102970	4.507197
527.546990	6977.255438	15.076365	-0.102922	4.504680
526.908320	6969.261389	15.081370	-0.102798	4.502145
527.394933	6961.218716	15.086375	-0.102883	4.499597
527.426416	6953.239492	15.091379	-0.102884	4.497067
527.244632	6945.218928	15.096384	-0.102845	4.494521
526.880856	6937.278760	15.101389	-0.102772	4.491998
526.847051	6929.240201	15.106394	-0.102761	4.489444
527.312675	6921.280920	15.111399	-0.102842	4.486915
526.436375	6913.215283	15.116403	-0.102674	4.484347
526.568580	6905.291528	15.121408	-0.102693	4.481825
526.435629	6897.300947	15.126413	-0.102663	4.479280
526.036228	6889.254613	15.131418	-0.102584	4.476715
526.382733	6881.151744	15.136423	-0.102643	4.474133
526.339494	6873.218886	15.141427	-0.102630	4.471602
526.167915	6865.171939	15.146432	-0.102593	4.469033
525.739813	6857.241568	15.151437	-0.102508	4.466499
525.750638	6849.116592	15.156442	-0.102505	4.463903
525.762595	6841.252088	15.161447	-0.102502	4.461388
526.061819	6833.110004	15.166451	-0.102552	4.458785
526.184818	6825.181742	15.171456	-0.102570	4.456247
525.857385	6817.232189	15.176461	-0.102504	4.453700
525.611740	6809.223815	15.181466	-0.102453	4.451132
525.908718	6801.124651	15.186471	-0.102503	4.448537
525.574588	6793.187296	15.191475	-0.102436	4.445989
525.897821	6785.146594	15.196480	-0.102491	4.443409
526.184768	6777.188726	15.201485	-0.102539	4.440854
525.905495	6769.132350	15.206490	-0.102482	4.438263
526.470539	6761.136574	15.211495	-0.102582	4.435695
525.859593	6753.245209	15.216499	-0.102463	4.433153
525.810042	6745.229464	15.221504	-0.102449	4.430572
525.829724	6737.208581	15.226509	-0.102447	4.427988
525.325711	6729.125406	15.231514	-0.102348	4.425380
525.448423	6721.144264	15.236519	-0.102366	4.422806
525.401860	6713.157984	15.241523	-0.102352	4.420229
525.531601	6705.129911	15.246528	-0.102371	4.417637
525.555650	6697.118939	15.251533	-0.102370	4.415049
525.240403	6689.131085	15.256538	-0.102306	4.412465
525.697661	6681.092073	15.261543	-0.102386	4.409867
525.680796	6673.123870	15.266547	-0.102378	4.407288
524.813595	6665.197720	15.271552	-0.102211	4.404716
525.310152	6657.188328	15.276557	-0.102299	4.402124
525.461535	6649.114689	15.281562	-0.102321	4.399507
525.694992	6641.154919	15.286567	-0.102360	4.396926
525.764129	6633.091274	15.291571	-0.102367	4.394309
525.576801	6625.172735	15.296576	-0.102327	4.391736
525.459724	6617.123135	15.301581	-0.102300	4.389119
525.535533	6609.129385	15.306586	-0.102309	4.386520
525.194177	6601.160928	15.311591	-0.102241	4.383925
525.132805	6593.213885	15.316595	-0.102224	4.381337
525.338215	6585.123533	15.321600	-0.102257	4.378702
525.566780	6577.109322	15.326605	-0.102295	4.376092
525.529258	6569.069784	15.331610	-0.102282	4.373469
525.226770	6561.208810	15.336615	-0.102221	4.370902
525.415136	6553.093021	15.341619	-0.102251	4.368253
525.381017	6545.129033	15.346624	-0.102239	4.365650
525.632805	6537.171453	15.351629	-0.102281	4.363050
525.630212	6529.122784	15.356634	-0.102275	4.360417
525.948043	6521.188459	15.361639	-0.102329	4.357822
525.806851	6513.172399	15.366643	-0.102298	4.355195
525.874354	6505.141460	15.371648	-0.102305	4.352564
525.634570	6497.164934	15.376653	-0.102255	4.349946
525.335738	6489.172744	15.381658	-0.102195	4.347322
525.339133	6481.164497	15.386663	-0.102190	4.344692
525.610385	6473.214918	15.391667	-0.102235	4.342083
525.419597	6465.177032	15.396672	-0.102195	4.339439
525.414805	6457.277449	15.401677	-0.102189	4.336840
524.671337	6449.254601	15.406682	-0.102045	4.334194
525.098041	6441.247585	15.411687	-0.102119	4.331561
525.196527	6433.122291	15.416691	-0.102132	4.328884
525.144003	6425.207180	15.421696	-0.102118	4.326273
524.977268	6417.213522	15.426701	-0.102081	4.323635
525.029553	6409.204417	15.431706	-0.102086	4.320991
525.453213	6401.183623	15.436711	-0.102160	4.318345
524.970558	6393.240756	15.441715	-0.102065	4.315715
524.700803	6385.234455	15.446720	-0.102009	4.313065
524.676425	6377.212002	15.451725	-0.101999	4.310410
524.881458	6369.124672	15.456730	-0.102032	4.307733
524.796803	6361.138147	15.461735	-0.102011	4.305086
524.710398	6353.187683	15.466739	-0.101990	4.302449
524.626166	6345.110381	15.471744	-0.101969	4.299769
524.364001	6337.211038	15.476749	-0.101915	4.297144
523.902799	6329.186522	15.481754	-0.101824	4.294475
524.302156	6321.178420	15.486759	-0.101894	4.291816
524.271378	6313.098285	15.491763	-0.101883	4.289128
524.313509	6305.146019	15.496768	-0.101885	4.286482
524.207673	6297.148265	15.501773	-0.101860	4.283818
523.933803	6289.194730	15.506778	-0.101804	4.281165
523.780299	6281.193359	15.511783	-0.101771	4.278496
523.225242	6273.247342	15.516787	-0.101662	4.275840
523.582567	6265.167269	15.521792	-0.101723	4.273145
523.821403	6257.122540	15.526797	-0.101763	4.270460
523.726822	6249.112652	15.531802	-0.101740	4.267782
523.553468	6241.153913	15.536807	-0.101702	4.265118
523.675458	6233.154546	15.541811	-0.101720	4.262442
523.902050	6225.060253	15.546816	-0.101757	4.259733
524.568118	6217.078529	15.551821	-0.101876	4.257065
524.076881	6209.102473	15.556826	-0.101779	4.254386
524.104758	6201.180702	15.561831	-0.101779	4.251728
523.870014	6193.141444	15.566835	-0.101730	4.249026
523.942817	6185.123403	15.571840	-0.101739	4.246333
524.002200	6177.121966	15.576845	-0.101745	4.243644
523.702911	6169.185489	15.581850	-0.101684	4.240971
523.885803	6161.166374	15.586855	-0.101713	4.238274
523.628368	6153.173056	15.591859	-0.101659	4.235579
523.534807	6145.126231	15.596864	-0.101637	4.232866
523.545771	6137.156361	15.601869	-0.101634	4.230178
523.429163	6129.122439	15.606874	-0.101607	4.227466
523.222152	6121.153841	15.611879	-0.101563	4.224773
523.185402	6113.208182	15.616883	-0.101551	4.222088
523.105487	6105.124962	15.621888	-0.101531	4.219354
522.940633	6097.207451	15.626893	-0.101495	4.216673
523.201901	6089.131209	15.631898	-0.101539	4.213942
523.027323	6081.207658	15.636903	-0.101501	4.211255
523.348462	6073.046770	15.641907	-0.101556	4.208492
523.108642	6065.125533	15.646912	-0.101506	4.205803
523.759510	6057.100404	15.651917	-0.101622	4.203086
523.057089	6049.161391	15.656922	-0.101486	4.200382
523.026920	6041.191809	15.661927	-0.101475	4.197673
523.092120	6033.130619	15.666931	-0.101482	4.194932
523.297396	6025.063578	15.671936	-0.101515	4.192189
523.078203	6017.057249	15.676941	-0.101469	4.189460
523.597648	6009.005620	15.681946	-0.101560	4.186722
523.731149	6000.995971	15.686951	-0.101580	4.183993
523.653769	5993.116709	15.691955	-0.101561	4.181304
523.605109	5985.100794	15.696960	-0.101546	4.178566
523.827263	5977.121903	15.701965	-0.101583	4.175843
523.564262	5969.102012	15.706970	-0.101528	4.173098
523.176948	5961.120141	15.711975	-0.101451	4.170363
523.469599	5953.104267	15.716979	-0.101501	4.167622
523.096842	5945.125277	15.721984	-0.101426	4.164885
523.258259	5937.163663	15.726989	-0.101451	4.162158
522.997604	5929.132213	15.731994	-0.101397	4.159400
523.365172	5921.134550	15.736999	-0.101460	4.156659
522.900588	5913.148457	15.742003	-0.101369	4.153910
523.240327	5905.122287	15.747008	-0.101427	4.151156
522.872227	5897.129882	15.752013	-0.101353	4.148403
523.214711	5889.023446	15.757018	-0.101412	4.145617
523.323805	5881.085912	15.762023	-0.101427	4.142885
522.812822	5873.167524	15.767027	-0.101327	4.140150
522.736234	5865.166886	15.772032	-0.101307	4.137390
522.700258	5857.164675	15.777037	-0.101295	4.134629
522.785241	5849.139776	15.782042	-0.101306	4.131859
522.998696	5841.116266	15.787047	-0.101340	4.129089
522.685905	5833.174961	15.792051	-0.101277	4.126339
522.525421	5825.146662	15.797056	-0.101242	4.123560
522.927074	5817.186065	15.802061	-0.101312	4.120809
522.477407	5809.219389	15.807066	-0.101223	4.118043
522.393223	5801.188248	15.812071	-0.101202	4.115257
522.270743	5793.170380	15.817075	-0.101174	4.112474
522.190095	5785.132084	15.822080	-0.101154	4.109682
521.922571	5777.176734	15.827085	-0.101099	4.106915
522.532200	5769.002676	15.832090	-0.101207	4.104082
522.624254	5761.173117	15.837095	-0.101219	4.101359
522.406104	5753.168377	15.842099	-0.101173	4.098570
522.254452	5745.146800	15.847104	-0.101140	4.095773
522.497438	5737.129153	15.852109	-0.101180	4.092982
522.248836	5729.126996	15.857114	-0.101128	4.090187
522.100992	5721.185320	15.862119	-0.101096	4.087413
521.564425	5713.181049	15.867123	-0.100991	4.084609
521.627477	5705.209598	15.872128	-0.100997	4.081824
521.620017	5697.159046	15.877133	-0.100991	4.079008
521.775593	5689.159893	15.882138	-0.101014	4.076210
522.032659	5681.101347	15.887143	-0.101057	4.073392
522.256905	5673.108424	15.892147	-0.101094	4.070593
522.043077	5665.096664	15.897152	-0.101049	4.067780
521.596562	5657.172419	15.902157	-0.100960	4.064992
521.654704	5649.166583	15.907162	-0.100966	4.062181
521.627764	5641.157477	15.912167	-0.100956	4.059366
521.746787	5633.122835	15.917171	-0.100973	4.056541
521.538193	5625.127380	15.922176	-0.100929	4.053724
521.790539	5617.145081	15.927181	-0.100971	4.050917
521.983962	5609.066296	15.932186	-0.101001	4.048072
521.635603	5601.167217	15.937191	-0.100931	4.045281
521.587699	5593.204847	15.942195	-0.100917	4.042470
521.469881	5585.157462	15.947200	-0.100890	4.039625
521.111670	5577.258895	15.952205	-0.100818	4.036828
521.317590	5569.157335	15.957210	-0.100852	4.033966
521.106952	5561.162056	15.962215	-0.100807	4.031133
521.004723	5553.136791	15.967219	-0.100783	4.028289
521.311300	5545.064482	15.972224	-0.100835	4.025432
521.299846	5537.152075	15.977229	-0.100828	4.022626
520.802699	5529.218037	15.982234	-0.100730	4.019801
520.895932	5521.216276	15.987239	-0.100742	4.016961
520.756232	5513.163214	15.992243	-0.100711	4.014096
520.827393	5505.150129	15.997248	-0.100719	4.011247
520.861967	5497.125995	16.002253	-0.100720	4.008391
520.913859	5489.124289	16.007258	-0.100725	4.005542
520.689474	5481.209431	16.012263	-0.100678	4.002717
520.381043	5473.249953	16.017267	-0.100615	3.999872
520.367275	5465.220352	16.022272	-0.100607	3.997005
520.383186	5457.229194	16.027277	-0.100605	3.994151
520.433478	5449.220296	16.032282	-0.100609	3.991289
520.388139	5441.213827	16.037287	-0.100596	3.988424
520.475033	5433.166720	16.042291	-0.100607	3.985544
520.193566	5425.243248	16.047296	-0.100549	3.982701
520.360550	5417.188184	16.052301	-0.100575	3.979816
520.509818	5409.164981	16.057306	-0.100598	3.976940
521.134277	5401.080122	16.062311	-0.100709	3.974048
520.756560	5393.215648	16.067315	-0.100633	3.971216
520.477152	5385.197639	16.072320	-0.100576	3.968328
520.148288	5377.267818	16.077325	-0.100510	3.965469
520.164858	5369.208082	16.082330	-0.100508	3.962567
520.055503	5361.257487	16.087335	-0.100482	3.959700
520.013831	5353.266065	16.092339	-0.100469	3.956817
519.853951	5345.230181	16.097344	-0.100434	3.953914
520.268509	5337.205190	16.102349	-0.100506	3.951024
520.146784	5329.166249	16.107354	-0.100478	3.948116
520.104127	5321.171578	16.112359	-0.100465	3.945224
520.313111	5313.182973	16.117363	-0.100499	3.942336
520.202543	5305.189688	16.122368	-0.100473	3.939439
520.680976	5297.223913	16.127373	-0.100557	3.936561
520.718176	5289.153033	16.132378	-0.100559	3.933634
520.717585	5281.176069	16.137383	-0.100554	3.930738
520.883348	5273.170624	16.142387	-0.100579	3.927833
520.829769	5265.167816	16.147392	-0.100564	3.924923
521.096374	5257.183477	16.152397	-0.100609	3.922023
520.591048	5249.235830	16.157402	-0.100509	3.919120
520.987043	5241.259886	16.162407	-0.100578	3.916221
520.517344	5233.283029	16.167411	-0.100485	3.913304
520.301788	5225.240748	16.172416	-0.100440	3.910365
520.691391	5217.234917	16.177421	-0.100507	3.907449
519.968242	5209.259950	16.182426	-0.100368	3.904521
519.898070	5201.327240	16.187431	-0.100349	3.901618
520.376051	5193.191171	16.192435	-0.100433	3.898650
520.326813	5185.250497	16.197440	-0.100419	3.895740
520.301566	5177.266808	16.202445	-0.100409	3.892814
520.099309	5169.227266	16.207450	-0.100366	3.889861
519.536554	5161.340193	16.212455	-0.100256	3.886954
519.603533	5153.264353	16.217459	-0.100263	3.883988
519.344671	5145.364442	16.222464	-0.100210	3.881079
519.709620	5137.306518	16.227469	-0.100273	3.878121
519.230594	5129.314697	16.232474	-0.100178	3.875169
519.503196	5121.174099	16.237479	-0.100224	3.872174
519.606520	5113.118479	16.242483	-0.100238	3.869206
519.236395	5105.225610	16.247488	-0.100164	3.866285
518.634515	5097.334089	16.252493	-0.100047	3.863358
518.958145	5089.239834	16.257498	-0.100102	3.860373
519.249175	5081.268278	16.262503	-0.100151	3.857430
519.247732	5073.250088	16.267507	-0.100145	3.854461
519.315273	5065.238383	16.272512	-0.100153	3.851495
519.431897	5057.245186	16.277517	-0.100169	3.848533
519.241432	5049.294974	16.282522	-0.100129	3.845579
519.148798	5041.327706	16.287527	-0.100106	3.842619
519.793914	5033.224291	16.292531	-0.100221	3.839621
519.458849	5025.314359	16.297536	-0.100154	3.836672
519.647571	5017.291476	16.302541	-0.100184	3.833690
519.364467	5009.326449	16.307546	-0.100126	3.830717
518.878924	5001.355251	16.312551	-0.100030	3.827735
519.084722	4993.273956	16.317555	-0.100063	3.824724
519.130132	4985.297778	16.322560	-0.100067	3.821747
519.012056	4977.324059	16.327565	-0.100040	3.818765
518.558526	4969.398125	16.332570	-0.099950	3.815791
519.052334	4961.305728	16.337575	-0.100037	3.812773
518.714943	4953.312245	16.342579	-0.099969	3.809771
518.394869	4945.385790	16.347584	-0.099904	3.806793
518.948499	4937.267850	16.352589	-0.100002	3.803760
518.425104	4929.377874	16.357594	-0.099899	3.800786
519.422801	4921.243277	16.362599	-0.100080	3.797752
519.335943	4913.242488	16.367603	-0.100058	3.794742
518.963850	4905.373176	16.372608	-0.099984	3.791772
518.746719	4897.376489	16.377613	-0.099938	3.788755
518.878198	4889.331074	16.382618	-0.099958	3.785725
518.705954	4881.399141	16.387623	-0.099920	3.782729
518.365236	4873.412824	16.392627	-0.099852	3.779706
518.777541	4865.328060	16.397632	-0.099923	3.776661
518.195464	4857.422453	16.402637	-0.099810	3.773658
518.066265	4849.393097	16.407642	-0.099781	3.770616
518.381350	4841.345150	16.412647	-0.099834	3.767575
517.878819	4833.422037	16.417651	-0.099735	3.764560
517.451571	4825.517244	16.422656	-0.099651	3.761551
517.690453	4817.459654	16.427661	-0.099690	3.758497
517.598791	4809.439163	16.432666	-0.099668	3.755447
517.497794	4801.466033	16.437671	-0.099644	3.752413
517.664164	4793.361949	16.442675	-0.099670	3.749332
518.302125	4785.296777	16.447680	-0.099783	3.746276
517.963080	4777.416380	16.452685	-0.099715	3.743263
517.642497	4769.425972	16.457690	-0.099650	3.740207
517.643915	4761.488626	16.462695	-0.099645	3.737176
517.689885	4753.427472	16.467699	-0.099649	3.734096
517.300293	4745.482625	16.472704	-0.099571	3.731048
517.978930	4737.367765	16.477709	-0.099692	3.727958
518.146796	4729.345411	16.482714	-0.099718	3.724889
518.480807	4721.414023	16.487719	-0.099775	3.721856
517.877349	4713.449272	16.492723	-0.099658	3.718785
518.048848	4705.466671	16.497728	-0.099684	3.715724
518.224127	4697.422132	16.502733	-0.099712	3.712636
517.853710	4689.403094	16.507738	-0.099638	3.709542
517.972489	4681.438058	16.512743	-0.099655	3.706478
518.225866	4673.415578	16.517747	-0.099697	3.703393
517.776841	4665.460072	16.522752	-0.099608	3.700314
518.087248	4657.446267	16.527757	-0.099660	3.697229
517.433368	4649.516348	16.532762	-0.099534	3.694148
517.823201	4641.489527	16.537767	-0.099601	3.691055
517.622938	4633.449229	16.542771	-0.099558	3.687939
518.103429	4625.389298	16.547776	-0.099643	3.684830
518.108421	4617.493689	16.552781	-0.099639	3.681770
517.432364	4609.537365	16.557786	-0.099508	3.678665
517.894348	4601.495461	16.562791	-0.099588	3.675555
517.836697	4593.548578	16.567795	-0.099572	3.672466
517.472396	4585.518638	16.572800	-0.099499	3.669333
517.812273	4577.513205	16.577805	-0.099558	3.666226
517.765205	4569.491342	16.582810	-0.099544	3.663100
517.852808	4561.526300	16.587815	-0.099555	3.659996
517.505992	4553.575612	16.592819	-0.099485	3.656884
517.138516	4545.599728	16.597824	-0.099411	3.653759
517.181011	4537.603142	16.602829	-0.099414	3.650635
517.064828	4529.597330	16.607834	-0.099387	3.647499
516.782809	4521.606863	16.612839	-0.099330	3.644362
517.447650	4513.526789	16.617843	-0.099448	3.641214
517.285804	4505.528217	16.622848	-0.099413	3.638072
517.521513	4497.538821	16.627853	-0.099452	3.634942
517.665824	4489.539636	16.632858	-0.099473	3.631803
517.251867	4481.594800	16.637863	-0.099391	3.628667
516.962683	4473.615654	16.642867	-0.099332	3.625518
517.077867	4465.629815	16.647872	-0.099348	3.622375
517.232966	4457.617144	16.652877	-0.099372	3.619220
516.753143	4449.673484	16.657882	-0.099278	3.616071
517.189204	4441.582694	16.662887	-0.099354	3.612888
516.680090	4433.639537	16.667891	-0.099254	3.609733
517.296974	4425.563095	16.672896	-0.099363	3.606555
517.186443	4417.619451	16.677901	-0.099338	3.603406
517.031551	4409.625409	16.682906	-0.099304	3.600232
517.427245	4401.615713	16.687911	-0.099372	3.597066
517.029636	4393.640938	16.692915	-0.099293	3.593888
516.974500	4385.678960	16.697920	-0.099278	3.590722
517.171486	4377.660035	16.702925	-0.099309	3.587538
516.743779	4369.661970	16.707930	-0.099224	3.584341
516.939604	4361.705119	16.712935	-0.099256	3.581176
517.214840	4353.635118	16.717939	-0.099302	3.577965
516.766747	4345.697794	16.722944	-0.099213	3.574783
517.033716	4337.669284	16.727949	-0.099258	3.571583
517.059007	4329.647923	16.732954	-0.099257	3.568376
517.162468	4321.687954	16.737959	-0.099271	3.565193
516.766654	4313.769346	16.742963	-0.099192	3.562008
516.828095	4305.734164	16.747968	-0.099199	3.558788
516.843652	4297.754004	16.752973	-0.099196	3.555585
517.113420	4289.644544	16.757978	-0.099241	3.552335
516.962900	4281.658795	16.762983	-0.099208	3.549120
516.593398	4273.767536	16.767987	-0.099134	3.545933
516.775260	4265.698279	16.772992	-0.099163	3.542688
516.637651	4257.781445	16.777997	-0.099132	3.539491
516.264386	4249.812528	16.783002	-0.099057	3.536264
516.258079	4241.792025	16.788007	-0.099051	3.533024
516.433201	4233.747190	16.793011	-0.099078	3.529777
516.154037	4225.779391	16.798016	-0.099021	3.526543
516.657449	4217.727757	16.803021	-0.099110	3.523298
516.520007	4209.762969	16.808026	-0.099079	3.520064
516.292751	4201.844839	16.813031	-0.099032	3.516844
516.556241	4193.777557	16.818035	-0.099076	3.513576
516.161209	4185.845040	16.823040	-0.098997	3.510338
516.386961	4177.810885	16.828045	-0.099034	3.507076
516.038493	4169.808451	16.833050	-0.098964	3.503805
516.407766	4161.847551	16.838055	-0.099027	3.500571
516.357101	4153.850465	16.843059	-0.099013	3.497306
515.954047	4145.859682	16.848064	-0.098932	3.494030
516.366444	4137.823457	16.853069	-0.099004	3.490757
516.040533	4129.873021	16.858074	-0.098938	3.487493
515.775575	4121.873529	16.863079	-0.098884	3.484208
515.705394	4113.958265	16.868083	-0.098866	3.480961
516.089550	4105.817149	16.873088	-0.098932	3.477632
516.347523	4097.828989	16.878093	-0.098975	3.474359
516.217771	4089.837656	16.883098	-0.098945	3.471069
515.914954	4081.936147	16.888103	-0.098884	3.467808
516.231243	4073.828603	16.893107	-0.098937	3.464478
515.652329	4065.962363	16.898112	-0.098825	3.461215
515.820830	4057.922958	16.903117	-0.098851	3.457903
515.558824	4049.948100	16.908122	-0.098797	3.454600
515.485517	4041.982970	16.913127	-0.098778	3.451303
515.365908	4033.983285	16.918131	-0.098751	3.447988
515.711188	4025.901307	16.923136	-0.098810	3.444651
515.375400	4018.018360	16.928141	-0.098742	3.441371
515.469387	4009.980682	16.933146	-0.098754	3.438037
515.498252	4002.016210	16.938151	-0.098755	3.434729
515.604764	3994.022973	16.943155	-0.098769	3.431408
515.235401	3986.031896	16.948160	-0.098695	3.428069
515.428223	3978.005078	16.953165	-0.098726	3.424730
515.448347	3970.022822	16.958170	-0.098725	3.421401
515.350561	3962.045467	16.963175	-0.098701	3.418067
515.717841	3953.980300	16.968179	-0.098764	3.414709
515.591790	3946.039596	16.973184	-0.098736	3.411382
514.909679	3938.151195	16.978189	-0.098604	3.408055
514.776476	3930.083151	16.983194	-0.098574	3.404668
514.973039	3922.140374	16.988199	-0.098605	3.401342
514.954550	3914.112036	16.993203	-0.098596	3.397970
514.770826	3906.122025	16.998208	-0.098557	3.394604
515.125854	3898.039364	17.003213	-0.098618	3.391215
514.632927	3890.096865	17.008218	-0.098521	3.387851
514.655879	3882.085137	17.013223	-0.098520	3.384474
514.825372	3874.091775	17.018227	-0.098547	3.381105
515.118305	3866.040325	17.023232	-0.098596	3.377714
514.771999	3858.138844	17.028237	-0.098526	3.374359
514.070390	3850.252420	17.033242	-0.098391	3.370995
514.340887	3842.173918	17.038247	-0.098436	3.367581
514.749464	3834.106242	17.043251	-0.098507	3.364173
514.447169	3826.205213	17.048256	-0.098445	3.360807
514.489865	3818.211049	17.053261	-0.098448	3.357410
514.458779	3810.174192	17.058266	-0.098437	3.353989
514.627188	3802.191131	17.063271	-0.098463	3.350595
514.259160	3794.238154	17.068275	-0.098389	3.347190
514.152532	3786.242008	17.073280	-0.098364	3.343773
514.157367	3778.286649	17.078285	-0.098360	3.340374
514.272030	3770.239976	17.083290	-0.098376	3.336937
514.202634	3762.265169	17.088295	-0.098358	3.333520
514.647432	3754.223222	17.093299	-0.098436	3.330090
514.340519	3746.249474	17.098304	-0.098374	3.326657
514.480415	3738.269097	17.103309	-0.098394	3.323235
514.521927	3730.283866	17.108314	-0.098397	3.319804
514.704295	3722.309528	17.113319	-0.098426	3.316379
514.656849	3714.321169	17.118323	-0.098412	3.312936
514.685668	3706.294509	17.123328	-0.098412	3.309475
514.508335	3698.349690	17.128333	-0.098374	3.306038
514.215347	3690.379590	17.133338	-0.098314	3.302583
514.068888	3682.401149	17.138343	-0.098282	3.299125
514.217754	3674.402998	17.143347	-0.098304	3.295668
514.098534	3666.351817	17.148352	-0.098277	3.292172
513.744537	3658.431949	17.153357	-0.098206	3.288721
513.776591	3650.409299	17.158362	-0.098207	3.285237
514.086581	3642.394909	17.163367	-0.098259	3.281764
514.161435	3634.404616	17.168371	-0.098268	3.278288
513.785236	3626.465511	17.173376	-0.098193	3.274813
513.728416	3618.520722	17.178381	-0.098177	3.271345
512.972267	3610.557986	17.183386	-0.098031	3.267836
513.616293	3602.436570	17.188391	-0.098146	3.264311
513.617340	3594.485664	17.193395	-0.098141	3.260831
512.680833	3586.630035	17.198400	-0.097961	3.257351
512.608031	3578.610668	17.203405	-0.097943	3.253830
512.252395	3570.604994	17.208410	-0.097871	3.250300
512.701524	3562.523293	17.213415	-0.097950	3.246766
513.029056	3554.467199	17.218419	-0.098005	3.243234
513.049106	3546.505853	17.223424	-0.098004	3.239727
513.430083	3538.524245	17.228429	-0.098070	3.236223
513.164080	3530.553913	17.233434	-0.098015	3.232693
513.054036	3522.575626	17.238439	-0.097989	3.229162
513.053115	3514.588074	17.243443	-0.097984	3.225628
512.885796	3506.626415	17.248448	-0.097948	3.222094
512.967953	3498.615473	17.253453	-0.097958	3.218545
513.170209	3490.573118	17.258458	-0.097990	3.214983
512.937192	3482.639238	17.263463	-0.097942	3.211447
512.838431	3474.641112	17.268467	-0.097918	3.207884
512.673218	3466.631649	17.273472	-0.097882	3.204309
512.905048	3458.687687	17.278477	-0.097920	3.200777
513.075589	3450.679279	17.283482	-0.097947	3.197209
513.157781	3442.658193	17.288487	-0.097957	3.193628
512.970714	3434.724983	17.293491	-0.097917	3.190070
512.821264	3426.703049	17.298496	-0.097884	3.186470
513.055234	3418.716526	17.303501	-0.097922	3.182899
512.883539	3410.717664	17.308506	-0.097885	3.179301
512.810891	3402.803729	17.313511	-0.097867	3.175741
512.356328	3394.843603	17.318515	-0.097777	3.172139
512.439495	3386.798809	17.323520	-0.097787	3.168519
512.732108	3378.748954	17.328525	-0.097836	3.164901
513.025359	3370.756475	17.333530	-0.097886	3.161306
512.713886	3362.812872	17.338535	-0.097823	3.157702
512.847561	3354.828586	17.343539	-0.097842	3.154094
512.758246	3346.856023	17.348544	-0.097821	3.150478
512.699238	3338.892425	17.353549	-0.097805	3.146864
512.343923	3330.915050	17.358554	-0.097733	3.143225
512.046659	3322.968803	17.363559	-0.097673	3.139600
512.038704	3314.999774	17.368563	-0.097666	3.135972
512.007554	3306.936143	17.373568	-0.097655	3.132296
512.469688	3298.866408	17.378573	-0.097736	3.128636
511.847809	3290.970014	17.383578	-0.097615	3.125001
512.459390	3282.912106	17.388583	-0.097724	3.121344
512.470044	3274.955531	17.393587	-0.097721	3.117702
512.098270	3266.994877	17.398592	-0.097646	3.114036
511.815254	3259.094701	17.403597	-0.097588	3.110398
511.682776	3251.073982	17.408602	-0.097559	3.106706
511.940427	3243.028251	17.413607	-0.097601	3.103017
511.958324	3235.053459	17.418611	-0.097599	3.099346
511.915528	3227.068543	17.423616	-0.097586	3.095662
512.059153	3219.070859	17.428621	-0.097608	3.091977
511.621922	3211.128866	17.433626	-0.097521	3.088286
511.683491	3203.101957	17.438631	-0.097528	3.084574
511.594468	3195.195680	17.443635	-0.097506	3.080907
511.199791	3187.236617	17.448640	-0.097427	3.077197
511.403518	3179.193134	17.453645	-0.097460	3.073471
511.249965	3171.145647	17.458650	-0.097426	3.069722
511.192500	3163.175264	17.463655	-0.097410	3.066008
511.184912	3155.191357	17.468659	-0.097404	3.062287
510.947697	3147.229497	17.473664	-0.097354	3.058560
511.811241	3139.114888	17.478669	-0.097510	3.054810
511.374692	3131.217861	17.483674	-0.097424	3.051094
511.266438	3123.237316	17.488679	-0.097398	3.047351
511.189234	3115.292680	17.493683	-0.097379	3.043621
510.797146	3107.357405	17.498688	-0.097301	3.039876
510.907966	3099.361038	17.503693	-0.097316	3.036122
511.044579	3091.285638	17.508698	-0.097336	3.032328
511.533016	3083.245647	17.513703	-0.097422	3.028563
511.458962	3075.299567	17.518707	-0.097403	3.024809
511.118788	3067.397316	17.523712	-0.097335	3.021059
511.331338	3059.392746	17.528717	-0.097369	3.017283
510.681361	3051.500315	17.533722	-0.097243	3.013512
510.870464	3043.428070	17.538727	-0.097273	3.009693
510.754003	3035.471930	17.543731	-0.097246	3.005909
511.048761	3027.438264	17.548736	-0.097296	3.002105
511.400855	3019.430164	17.553741	-0.097356	2.998310
510.833271	3011.530624	17.558746	-0.097245	2.994516
510.720892	3003.560791	17.563751	-0.097219	2.990707
510.588257	2995.570041	17.568755	-0.097189	2.986881
509.935001	2987.641439	17.573760	-0.097063	2.983054
510.135130	2979.637664	17.578765	-0.097095	2.979229
510.167445	2971.600314	17.583770	-0.097096	2.975375
510.493302	2963.558644	17.588775	-0.097151	2.971529
510.066808	2955.647935	17.593779	-0.097067	2.967702
509.705028	2947.706328	17.598784	-0.096994	2.963859
509.766765	2939.706076	17.603789	-0.097000	2.960004
509.538848	2931.752148	17.608794	-0.096953	2.956152
509.816554	2923.695058	17.613799	-0.096999	2.952271
509.196210	2915.809310	17.618803	-0.096879	2.948420
509.192598	2907.767193	17.623808	-0.096873	2.944521
509.247263	2899.811637	17.628813	-0.096878	2.940663
509.010171	2891.844498	17.633818	-0.096829	2.936778
509.400303	2883.762226	17.638823	-0.096896	2.932865
509.375580	2875.763613	17.643827	-0.096886	2.928965
509.570563	2867.763006	17.648832	-0.096917	2.925072
509.259275	2859.901523	17.653837	-0.096854	2.921214
508.835578	2851.955237	17.658842	-0.096770	2.917303
509.234130	2843.877336	17.663847	-0.096839	2.913366
509.065721	2835.867852	17.668851	-0.096803	2.909428
508.998349	2827.868890	17.673856	-0.096785	2.905494
509.194828	2819.874933	17.678861	-0.096816	2.901572
509.004169	2811.949986	17.683866	-0.096776	2.897658
508.913037	2803.972886	17.688871	-0.096754	2.893718
509.177479	2795.932862	17.693875	-0.096798	2.889761
508.831518	2788.007352	17.698880	-0.096728	2.885822
509.118311	2780.018754	17.703885	-0.096776	2.881881
509.319437	2771.999601	17.708890	-0.096809	2.877915
509.306778	2764.027380	17.713895	-0.096801	2.873955
509.180155	2756.100327	17.718899	-0.096772	2.870005
508.613509	2748.186950	17.723904	-0.096662	2.866032
508.184169	2740.266198	17.728909	-0.096577	2.862057
508.718015	2732.156993	17.733914	-0.096671	2.858037
508.757293	2724.181149	17.738919	-0.096673	2.854051
508.487125	2716.247864	17.743923	-0.096618	2.850062
508.682573	2708.204392	17.748928	-0.096649	2.846039
508.678444	2700.265139	17.753933	-0.096643	2.842051
508.256469	2692.320880	17.758938	-0.096559	2.838031
508.405740	2684.326449	17.763943	-0.096582	2.834013
508.389795	2676.349842	17.768947	-0.096574	2.829989
508.296613	2668.329842	17.773952	-0.096551	2.825933
508.298816	2660.377663	17.778957	-0.096546	2.821910
508.247062	2652.392535	17.783962	-0.096532	2.817862
508.087009	2644.435713	17.788967	-0.096497	2.813816
508.126141	2636.426865	17.793971	-0.096499	2.809750
508.058927	2628.442517	17.798976	-0.096481	2.805684
509.183075	2620.332818	17.803981	-0.096685	2.801618
508.962561	2612.419842	17.808986	-0.096639	2.797568
508.323386	2604.584875	17.813991	-0.096515	2.793526
508.150351	2596.609717	17.818995	-0.096478	2.789435
508.143209	2588.588025	17.824000	-0.096471	2.785324
508.563145	2580.568348	17.829005	-0.096544	2.781233
507.972530	2572.691973	17.834010	-0.096429	2.777149
507.785258	2564.727456	17.839015	-0.096389	2.773038
507.602447	2556.745886	17.844019	-0.096350	2.768912
507.773417	2548.689949	17.849024	-0.096376	2.764763
507.939066	2540.746789	17.854029	-0.096402	2.760666
508.034860	2532.747066	17.859034	-0.096415	2.756530
507.859927	2524.775083	17.864039	-0.096377	2.752385
508.045918	2516.723785	17.869043	-0.096406	2.748214
508.000054	2508.732512	17.874048	-0.096393	2.744055
507.786146	2500.848211	17.879053	-0.096348	2.739934
507.870087	2492.836384	17.884058	-0.096358	2.735759
507.844241	2484.874310	17.889063	-0.096348	2.731597
508.111648	2476.840472	17.894067	-0.096393	2.727409
507.477884	2468.956412	17.899072	-0.096270	2.723236
507.570605	2461.011388	17.904077	-0.096282	2.719071
507.255236	2453.058053	17.909082	-0.096218	2.714870
507.333624	2445.060976	17.914087	-0.096228	2.710663
507.165312	2437.098879	17.919091	-0.096191	2.706453
507.220574	2429.092176	17.924096	-0.096196	2.702228
507.465505	2421.102761	17.929101	-0.096237	2.698016
507.739256	2413.052721	17.934106	-0.096282	2.693768
507.744708	2405.100639	17.939111	-0.096278	2.689548
507.475014	2397.181524	17.944115	-0.096223	2.685321
507.394103	2389.233326	17.949120	-0.096203	2.681084
508.039855	2381.187592	17.954125	-0.096318	2.676836
507.727679	2373.265262	17.959130	-0.096254	2.672584
507.694015	2365.291365	17.964135	-0.096243	2.668317
507.433503	2357.338788	17.969139	-0.096189	2.664039
507.458465	2349.366471	17.974144	-0.096189	2.659762
507.635531	2341.380164	17.979149	-0.096217	2.655481
507.059942	2333.462083	17.984154	-0.096104	2.651179
507.053502	2325.479582	17.989159	-0.096098	2.646874
507.112047	2317.493101	17.994163	-0.096104	2.642564
506.933184	2309.551246	17.999168	-0.096065	2.638255
507.182607	2301.550771	18.004173	-0.096107	2.633936
506.836132	2293.622453	18.009178	-0.096037	2.629609
506.583720	2285.661001	18.014183	-0.095985	2.625263
507.001905	2277.617781	18.019187	-0.096057	2.620911
506.724073	2269.688614	18.024192	-0.096001	2.616567
506.658016	2261.732956	18.029197	-0.095983	2.612215
506.459342	2253.762698	18.034202	-0.095941	2.607839
506.635708	2245.751630	18.039207	-0.095969	2.603459
507.211441	2237.695955	18.044211	-0.096071	2.599074
507.094195	2229.754641	18.049216	-0.096044	2.594697
506.946604	2221.755317	18.054221	-0.096011	2.590279
506.746976	2213.788141	18.059226	-0.095969	2.585868
506.953865	2205.799236	18.064231	-0.096002	2.581465
507.127853	2197.824043	18.069235	-0.096029	2.577059
507.298535	2189.850145	18.074240	-0.096056	2.572647
507.368476	2181.901451	18.079245	-0.096064	2.568234
507.255152	2173.947310	18.084250	-0.096038	2.563798
507.003537	2166.057562	18.089255	-0.095986	2.559380
506.607959	2158.176165	18.094259	-0.095907	2.554949
506.818163	2150.138428	18.099264	-0.095941	2.550466
507.428117	2142.065916	18.104269	-0.096049	2.545983
506.794571	2134.209725	18.109274	-0.095926	2.541526
506.634706	2126.289064	18.114279	-0.095891	2.537058
506.771313	2118.275271	18.119283	-0.095911	2.532551
507.119435	2110.234418	18.124288	-0.095971	2.528037
506.799209	2102.336635	18.129293	-0.095906	2.523546
506.760715	2094.380223	18.134298	-0.095894	2.519035
507.064597	2086.359595	18.139303	-0.095945	2.514504
507.103934	2078.396987	18.144307	-0.095948	2.509979
506.325098	2070.553688	18.149312	-0.095798	2.505454
506.590049	2062.533020	18.154317	-0.095842	2.500895
506.615293	2054.539891	18.159322	-0.095841	2.496327
506.488433	2046.590931	18.164327	-0.095812	2.491764
506.574418	2038.608803	18.169331	-0.095823	2.487190
506.341888	2030.670861	18.174336	-0.095775	2.482609
506.139933	2022.769442	18.179341	-0.095732	2.478042
506.526633	2014.709849	18.184346	-0.095799	2.473420
506.511139	2006.754117	18.189351	-0.095791	2.468820
506.809752	1998.741627	18.194355	-0.095841	2.464201
506.315022	1990.880334	18.199360	-0.095744	2.459602
506.022652	1982.972850	18.204365	-0.095685	2.454982
506.290239	1974.917567	18.209370	-0.095729	2.450310
506.235716	1966.960013	18.214375	-0.095714	2.445662
506.143332	1959.026079	18.219379	-0.095692	2.441015
506.117409	1951.071097	18.224384	-0.095682	2.436353
506.465643	1943.028142	18.229389	-0.095741	2.431659
505.948692	1935.123427	18.234394	-0.095640	2.426970
506.054848	1927.142041	18.239399	-0.095654	2.422275
506.139324	1919.187124	18.244403	-0.095665	2.417585
505.445924	1911.335619	18.249408	-0.095531	2.412886
505.581557	1903.330607	18.254413	-0.095551	2.408152
505.542945	1895.347967	18.259418	-0.095539	2.403409
505.034560	1887.480890	18.264423	-0.095439	2.398687
505.502598	1879.430830	18.269427	-0.095521	2.393925
505.540747	1871.448397	18.274432	-0.095523	2.389159
504.736805	1863.637441	18.279437	-0.095368	2.384419
504.347089	1855.713231	18.284442	-0.095290	2.379634
504.529665	1847.679585	18.289447	-0.095319	2.374821
505.084996	1839.614655	18.294451	-0.095417	2.370009
504.847688	1831.664292	18.299456	-0.095368	2.365192
505.275172	1823.673850	18.304461	-0.095442	2.360395
505.653468	1815.664846	18.309466	-0.095508	2.355573
505.121091	1807.825848	18.314471	-0.095403	2.350770
505.009989	1799.880616	18.319475	-0.095378	2.345926
504.904314	1791.926817	18.324480	-0.095353	2.341068
504.655330	1784.048932	18.329485	-0.095301	2.336235
504.992570	1775.958508	18.334490	-0.095359	2.331310
505.514252	1767.941326	18.339495	-0.095451	2.326435
505.290613	1760.067687	18.344499	-0.095404	2.321576
504.923334	1752.170114	18.349504	-0.095331	2.316679
504.901800	1744.218541	18.354509	-0.095322	2.311768
504.644447	1736.276451	18.359514	-0.095268	2.306832
505.052420	1728.246890	18.364519	-0.095339	2.301888
504.864646	1720.350763	18.369523	-0.095299	2.296966
504.826204	1712.394729	18.374528	-0.095287	2.292008
504.808620	1704.467032	18.379533	-0.095278	2.287060
504.730117	1696.504587	18.384538	-0.095259	2.282073
504.716282	1688.568786	18.389543	-0.095251	2.277098
504.778501	1680.595586	18.394547	-0.095257	2.272095
504.616429	1672.616816	18.399552	-0.095222	2.267057
504.724621	1664.667696	18.404557	-0.095237	2.262051
504.312224	1656.786185	18.409562	-0.095155	2.257031
503.995182	1648.876946	18.414567	-0.095091	2.251991
504.013417	1640.895325	18.419571	-0.095089	2.246922
503.962056	1632.917666	18.424576	-0.095075	2.241839
504.297742	1624.942013	18.429581	-0.095132	2.236780
504.095804	1617.005947	18.434586	-0.095089	2.231687
504.187327	1609.043733	18.439591	-0.095101	2.226591
503.975211	1601.156218	18.444595	-0.095056	2.221505
504.207077	1593.142026	18.449600	-0.095094	2.216365
503.651005	1585.321419	18.454605	-0.094986	2.211267
503.760116	1577.304268	18.459610	-0.095001	2.206090
503.761824	1569.373932	18.464615	-0.094996	2.200948
503.610532	1561.458837	18.469619	-0.094963	2.195789
503.464083	1553.507661	18.474624	-0.094930	2.190596
503.524872	1545.538832	18.479629	-0.094937	2.185397
503.207740	1537.640274	18.484634	-0.094872	2.180197
503.185669	1529.677404	18.489639	-0.094863	2.174970
502.934904	1521.769373	18.494643	-0.094811	2.169745
503.473581	1513.702079	18.499648	-0.094907	2.164476
503.393878	1505.812739	18.504653	-0.094887	2.159254
503.311148	1497.890247	18.509658	-0.094866	2.153997
503.299557	1489.956985	18.514663	-0.094859	2.148727
502.703444	1482.109539	18.519667	-0.094743	2.143445
502.602569	1474.161372	18.524672	-0.094719	2.138130
502.278039	1466.280599	18.529677	-0.094653	2.132826
502.440383	1458.249066	18.534682	-0.094678	2.127454
502.101247	1450.364543	18.539687	-0.094610	2.122118
502.120950	1442.427635	18.544691	-0.094609	2.116769
502.403723	1434.374883	18.549696	-0.094656	2.111354
502.527493	1426.391136	18.554701	-0.094674	2.105956
502.217155	1418.512543	18.559706	-0.094611	2.100572
503.145146	1410.413303	18.564711	-0.094779	2.095147
502.763863	1402.594446	18.569715	-0.094703	2.089770
502.634925	1394.655387	18.574720	-0.094673	2.084321
502.643479	1386.790003	18.579725	-0.094670	2.078923
502.284199	1378.912453	18.584730	-0.094598	2.073465
502.541510	1370.918720	18.589735	-0.094641	2.067975
502.930196	1362.920217	18.594739	-0.094708	2.062480
502.236961	1355.126318	18.599744	-0.094574	2.057002
502.787189	1347.097138	18.604749	-0.094671	2.051473
502.450820	1339.215717	18.609754	-0.094603	2.045942
502.273522	1331.335772	18.614759	-0.094565	2.040412
502.318728	1323.402932	18.619763	-0.094568	2.034854
502.124696	1315.483573	18.624768	-0.094527	2.029265
502.045453	1307.567647	18.629773	-0.094507	2.023674
501.844981	1299.662032	18.634778	-0.094465	2.018063
501.307250	1291.810711	18.639783	-0.094360	2.012439
501.298360	1283.854382	18.644787	-0.094353	2.006781
501.422706	1275.870732	18.649792	-0.094371	2.001101
501.370426	1267.976004	18.654797	-0.094356	1.995449
501.391406	1260.003411	18.659802	-0.094355	1.989734
501.577697	1252.061316	18.664807	-0.094384	1.984042
501.905901	1244.097299	18.669811	-0.094440	1.978333
501.806590	1236.181549	18.674816	-0.094417	1.972596
501.939118	1228.255240	18.679821	-0.094436	1.966860
501.875481	1220.356688	18.684826	-0.094419	1.961106
501.663899	1212.496500	18.689831	-0.094375	1.955347
501.151659	1204.667747	18.694835	-0.094274	1.949560
501.353360	1196.679175	18.699840	-0.094307	1.943718
501.690463	1188.702695	18.704845	-0.094364	1.937882
501.352979	1180.825329	18.709850	-0.094296	1.932027
501.620614	1172.861111	18.714855	-0.094341	1.926157
501.425905	1164.985603	18.719859	-0.094300	1.920283
501.083368	1157.129736	18.724864	-0.094231	1.914389
501.267498	1149.190933	18.729869	-0.094260	1.908475
501.266001	1141.263170	18.734874	-0.094255	1.902529
501.293597	1133.346825	18.739879	-0.094255	1.896577
501.391238	1125.417763	18.744883	-0.094268	1.890604
501.037796	1117.563860	18.749888	-0.094197	1.884617
501.164341	1109.670553	18.754893	-0.094215	1.878637
501.406166	1101.699936	18.759898	-0.094255	1.872592
501.100602	1093.849763	18.764903	-0.094193	1.866556
501.091217	1085.930055	18.769907	-0.094186	1.860482
500.836140	1078.071433	18.774912	-0.094134	1.854405
500.817919	1070.161197	18.779917	-0.094125	1.848297
500.660412	1062.270531	18.784922	-0.094091	1.842167
500.396986	1054.416920	18.789927	-0.094037	1.836033
500.372144	1046.497412	18.794931	-0.094027	1.829855
500.111770	1038.625240	18.799936	-0.093973	1.823665
500.502628	1030.664870	18.804941	-0.094041	1.817464
499.772705	1022.874001	18.809946	-0.093900	1.811238
499.976826	1014.912231	18.814951	-0.093933	1.804970
499.753994	1007.077699	18.819955	-0.093886	1.798729
499.670837	999.157399	18.824960	-0.093866	1.792415
499.613994	991.233636	18.829965	-0.093850	1.786079
499.539483	983.343274	18.834970	-0.093831	1.779745
499.491955	975.467907	18.839975	-0.093817	1.773403
499.409147	967.552677	18.844979	-0.093797	1.767003
499.645255	959.613828	18.849984	-0.093835	1.760600
499.659705	951.770447	18.854989	-0.093833	1.754223
499.295675	943.932521	18.859994	-0.093760	1.747779
498.823951	936.115010	18.864999	-0.093667	1.741315
498.860985	928.211622	18.870003	-0.093669	1.734820
498.661216	920.344760	18.875008	-0.093627	1.728301
498.486088	912.488421	18.880013	-0.093589	1.721770
499.158422	904.467773	18.885018	-0.093709	1.715187
498.868186	896.639323	18.890023	-0.093650	1.708613
498.930808	888.745712	18.895027	-0.093657	1.702006
498.663990	880.918254	18.900032	-0.093602	1.695385
499.027434	872.976042	18.905037	-0.093664	1.688725
498.707307	865.154549	18.910042	-0.093600	1.682049
498.687543	857.296017	18.915047	-0.093591	1.675356
498.839593	849.421133	18.920051	-0.093614	1.668645
498.551496	841.580217	18.925056	-0.093555	1.661877
498.732021	833.698456	18.930061	-0.093584	1.655109
498.841764	825.800200	18.935066	-0.093599	1.648290
498.612119	817.995811	18.940071	-0.093551	1.641477
498.539794	810.169210	18.945075	-0.093533	1.634638
498.812848	802.198667	18.950080	-0.093579	1.627693
498.692440	794.382011	18.955085	-0.093551	1.620797
498.640412	786.535177	18.960090	-0.093536	1.613856
498.562955	778.692827	18.965095	-0.093517	1.606885
498.443470	770.867164	18.970099	-0.093490	1.599892
498.567652	763.004875	18.975104	-0.093508	1.592870
498.338492	755.196934	18.980109	-0.093460	1.585816
498.374370	747.339238	18.985114	-0.093462	1.578723
498.347913	739.506724	18.990119	-0.093452	1.571612
498.347154	731.667347	18.995123	-0.093446	1.564467
498.163157	723.875183	19.000128	-0.093407	1.557304
498.256301	716.018523	19.005133	-0.093419	1.550091
497.928784	708.227777	19.010138	-0.093353	1.542841
498.117993	700.349873	19.015143	-0.093383	1.535555
498.340772	692.491743	19.020147	-0.093420	1.528257
497.926947	684.733809	19.025152	-0.093338	1.520921
497.839672	676.942090	19.030157	-0.093316	1.513567
497.925327	669.084505	19.035162	-0.093327	1.506142
497.709578	661.307048	19.040167	-0.093282	1.498710
497.450420	653.536511	19.045171	-0.093229	1.491240
497.329810	645.717925	19.050176	-0.093201	1.483708
497.468626	637.896366	19.055181	-0.093222	1.476176
496.931497	630.142704	19.060186	-0.093117	1.468564
496.854035	622.316728	19.065191	-0.093098	1.460915
496.877032	614.501701	19.070195	-0.093097	1.453252
496.837128	606.678600	19.075200	-0.093084	1.445531
496.745506	598.916289	19.080205	-0.093062	1.437820
496.851987	591.081530	19.085210	-0.093077	1.430028
496.604575	583.338267	19.090215	-0.093026	1.422226
496.636415	575.541722	19.095219	-0.093027	1.414374
496.635477	567.723699	19.100224	-0.093022	1.406451
496.320804	560.035724	19.105229	-0.092958	1.398562
495.943868	552.307139	19.110234	-0.092883	1.390577
496.007859	544.501374	19.115239	-0.092890	1.382541
496.042817	536.712133	19.120243	-0.092891	1.374470
495.826837	528.955671	19.125248	-0.092846	1.366342
496.133893	521.135692	19.130253	-0.092898	1.358191
496.242919	513.352423	19.135258	-0.092913	1.349994
496.351866	505.591669	19.140263	-0.092929	1.341771
496.159801	497.888830	19.145267	-0.092888	1.333506
495.675872	490.219909	19.150272	-0.092793	1.325172
496.077392	482.416952	19.155277	-0.092863	1.316802
495.586022	474.688566	19.160282	-0.092766	1.308296
495.480258	466.954658	19.165287	-0.092741	1.299799
495.355391	459.259507	19.170291	-0.092713	1.291285
495.131771	451.560184	19.175296	-0.092667	1.282692
495.486518	443.782181	19.180301	-0.092728	1.274062
495.161081	436.115652	19.185306	-0.092662	1.265369
495.031075	428.436611	19.190311	-0.092633	1.256639
495.027332	420.731376	19.195315	-0.092627	1.247843
494.894735	413.044143	19.200320	-0.092597	1.238980
494.958533	405.353347	19.205325	-0.092604	1.230087
494.747366	397.688953	19.210330	-0.092560	1.221106
494.598958	390.028046	19.215335	-0.092528	1.212075
494.553157	382.362848	19.220339	-0.092514	1.202992
494.228781	374.752415	19.225344	-0.092449	1.193848
494.425492	367.051543	19.230349	-0.092480	1.184632
493.840037	359.497215	19.235354	-0.092366	1.175359
493.599842	351.877892	19.240359	-0.092317	1.166005
493.850562	344.195306	19.245363	-0.092359	1.156601
493.828461	336.525421	19.250368	-0.092349	1.147078
493.838370	328.901896	19.255373	-0.092346	1.137540
493.583379	321.318160	19.260378	-0.092294	1.127914
493.663033	313.692915	19.265383	-0.092304	1.118225
493.109425	306.201254	19.270387	-0.092196	1.108484
492.731775	298.661956	19.275392	-0.092121	1.098633
492.609211	291.087191	19.280397	-0.092093	1.088704
492.178624	283.582375	19.285402	-0.092008	1.078706
491.876390	276.053235	19.290407	-0.091947	1.068612
491.951200	268.464618	19.295411	-0.091956	1.058428
491.261378	261.013244	19.300416	-0.091823	1.048153
490.291662	253.633804	19.305421	-0.091637	1.037807
489.037088	246.292987	19.310426	-0.091399	1.027342
488.271548	238.857630	19.315431	-0.091252	1.016755
487.785529	231.381656	19.320435	-0.091156	1.006068
487.224860	223.931489	19.325440	-0.091047	0.995284
487.334827	216.358398	19.330445	-0.091063	0.984372
486.721929	208.949920	19.335450	-0.090944	0.973395
485.491974	201.671044	19.340455	-0.090710	0.962325
485.365322	194.201586	19.345459	-0.090682	0.951129
484.593804	186.857449	19.350464	-0.090533	0.939818
483.990423	179.514369	19.355469	-0.090416	0.928416
483.025220	172.252813	19.360474	-0.090232	0.916900
482.962387	164.813181	19.365479	-0.090215	0.905206
482.122449	157.556277	19.370483	-0.090054	0.893433
481.457738	150.280523	19.375488	-0.089926	0.881522
480.604296	143.079093	19.380493	-0.089762	0.869514
479.781040	135.861119	19.385498	-0.089604	0.857319
479.366525	128.600049	19.390503	-0.089522	0.844997
478.766454	121.404286	19.395507	-0.089406	0.832548
477.446014	114.333800	19.400512	-0.089155	0.819906
476.401151	107.256726	19.405517	-0.088956	0.807139
474.740046	100.315761	19.410522	-0.088643	0.794216
472.603514	93.458765	19.415527	-0.088240	0.781077
470.215319	86.662305	19.420531	-0.087791	0.767741
467.732185	79.894906	19.425536	-0.087325	0.754191
463.358600	73.660338	19.430541	-0.086506	0.740771