Fri Apr 16 19:50:58 2021

Number of Points = 3644
Depth (nm)	Load (N)	Time (s)	Depth (V)	Load (V)
0.743011	-0.018412	0.000000	-0.000081	0.313600

0.826342	-0.035746	0.005005	-0.000096	0.313590
0.717451	-0.014458	0.010010	-0.000076	0.313597
0.282334	0.032276	0.015014	0.000005	0.313449
0.990555	-0.136895	0.020019	-0.000127	0.313262
1.170737	-0.168145	0.025024	-0.000160	0.313269
0.872215	-0.116516	0.030029	-0.000105	0.313257
0.675431	-0.077290	0.035034	-0.000068	0.313274
0.719309	-0.085721	0.040038	-0.000077	0.313272
0.505129	-0.046347	0.045043	-0.000037	0.313274
0.935117	-0.123845	0.050048	-0.000117	0.313277
0.579182	-0.059386	0.055053	-0.000051	0.313277
0.716409	-0.084261	0.060058	-0.000076	0.313277
0.540735	-0.069335	0.065062	-0.000044	0.313199
0.479094	-0.104394	0.070067	-0.000032	0.312986
0.785308	-0.159708	0.075072	-0.000089	0.312987
0.569091	-0.121964	0.080077	-0.000049	0.312981
0.861983	-0.175300	0.085082	-0.000104	0.312980
0.873681	-0.177506	0.090086	-0.000106	0.312980
0.887879	-0.194382	0.095091	-0.000109	0.312914
1.234722	-0.317467	0.100096	-0.000173	0.312637
1.136069	-0.302155	0.105101	-0.000155	0.312625
1.084778	-0.292664	0.110106	-0.000145	0.312626
1.212038	-0.316130	0.115110	-0.000169	0.312625
1.251393	-0.383623	0.120115	-0.000177	0.312346
1.059003	-0.353289	0.125120	-0.000141	0.312325
1.074774	-0.359276	0.130125	-0.000144	0.312311
0.989903	-0.347968	0.135130	-0.000128	0.312292
1.160161	-0.444267	0.140134	-0.000160	0.311989
1.042838	-0.424219	0.145139	-0.000138	0.311984
1.146087	-0.441651	0.150144	-0.000157	0.311990
1.089563	-0.473707	0.155149	-0.000147	0.311794
1.051716	-0.486267	0.160154	-0.000140	0.311704
0.892161	-0.456565	0.165158	-0.000110	0.311708
0.751563	-0.463102	0.170163	-0.000084	0.311559
0.933401	-0.535203	0.175168	-0.000118	0.311378
0.609283	-0.476050	0.180173	-0.000058	0.311379
0.614690	-0.498176	0.185178	-0.000059	0.311281
0.313040	-0.484707	0.190182	-0.000003	0.311090
0.487120	-0.518688	0.195187	-0.000035	0.311079
0.534283	-0.545032	0.200192	-0.000044	0.310997
0.661054	-0.621471	0.205197	-0.000068	0.310748
1.228701	-0.725113	0.210202	-0.000173	0.310746
1.012110	-0.721032	0.215206	-0.000133	0.310582
0.783052	-0.699300	0.220211	-0.000090	0.310490
0.747349	-0.701223	0.225216	-0.000084	0.310451
0.753538	-0.767061	0.230221	-0.000085	0.310150
0.761742	-0.768397	0.235226	-0.000087	0.310151
0.966237	-0.854177	0.240230	-0.000125	0.309924
0.572191	-0.801223	0.245235	-0.000051	0.309837
0.593246	-0.831167	0.250240	-0.000055	0.309716
0.695145	-0.895408	0.255245	-0.000074	0.309502
0.848108	-0.932617	0.260250	-0.000103	0.309459
0.748121	-0.964483	0.265254	-0.000084	0.309225
0.480452	-0.916198	0.270259	-0.000035	0.309224
0.824378	-1.049630	0.275264	-0.000099	0.308892
0.616027	-1.013942	0.280269	-0.000060	0.308882
0.729474	-1.095274	0.285274	-0.000081	0.308598
0.730217	-1.100159	0.290278	-0.000081	0.308576
0.511934	-1.125462	0.295283	-0.000041	0.308271
0.514497	-1.128445	0.300288	-0.000041	0.308260
0.592388	-1.202858	0.305293	-0.000056	0.307977
0.669942	-1.222022	0.310298	-0.000070	0.307954
0.592981	-1.277576	0.315302	-0.000056	0.307627
0.451246	-1.266171	0.320307	-0.000030	0.307560
0.593761	-1.344070	0.325312	-0.000056	0.307316
0.365703	-1.327453	0.330317	-0.000014	0.307199
0.367412	-1.372441	0.335322	-0.000014	0.306989
0.482181	-1.425630	0.340326	-0.000036	0.306837
0.312658	-1.424156	0.345331	-0.000004	0.306699
0.268724	-1.469516	0.350336	0.000004	0.306447
0.340132	-1.504908	0.355341	-0.000009	0.306342
0.410638	-1.578307	0.360346	-0.000022	0.306056
0.451680	-1.611198	0.365350	-0.000030	0.305936
0.252195	-1.617959	0.370355	0.000007	0.305733
0.485725	-1.700172	0.375360	-0.000036	0.305545
0.401582	-1.711686	0.380365	-0.000021	0.305418
0.264428	-1.746149	0.385370	0.000005	0.305137
0.435831	-1.815774	0.390374	-0.000027	0.304955
0.159750	-1.794847	0.395379	0.000024	0.304816
0.160674	-1.860915	0.400384	0.000024	0.304504
-0.149333	-1.834645	0.405389	0.000082	0.304361
0.019870	-1.897077	0.410394	0.000050	0.304211
-0.093677	-1.941353	0.415398	0.000071	0.303902
-0.643724	-1.868990	0.420403	0.000173	0.303771
-0.443903	-1.944136	0.425408	0.000136	0.303586
-0.572495	-1.979084	0.430413	0.000160	0.303309
-0.403070	-2.041358	0.435418	0.000129	0.303159
-0.135374	-2.133823	0.440422	0.000079	0.302950
-0.336459	-2.158525	0.445427	0.000116	0.302658
0.091642	-2.275336	0.450432	0.000036	0.302471
-0.297156	-2.243555	0.455437	0.000109	0.302286
-0.487818	-2.272745	0.460442	0.000144	0.301980
-0.577267	-2.291449	0.465446	0.000161	0.301813
-0.447222	-2.356596	0.470451	0.000136	0.301614
-0.306611	-2.436655	0.475456	0.000110	0.301353
-0.597665	-2.438096	0.480461	0.000164	0.301092
-0.770654	-2.447420	0.485466	0.000197	0.300897
-1.152856	-2.414004	0.490470	0.000268	0.300724
-1.412969	-2.411777	0.495475	0.000316	0.300507
-0.814358	-2.570906	0.500480	0.000205	0.300265
-1.258795	-2.535165	0.505485	0.000287	0.300048
-1.512251	-2.533722	0.510490	0.000334	0.299834
-1.855954	-2.533910	0.515494	0.000398	0.299531
-3.452567	-2.277571	0.520499	0.000695	0.299368
-3.573758	-2.286262	0.525504	0.000718	0.299220
-4.191994	-2.228394	0.530509	0.000833	0.298957
-4.750804	-2.140980	0.535514	0.000937	0.298889
-4.896165	-2.175082	0.540518	0.000964	0.298596
-5.154739	-2.140880	0.545523	0.001012	0.298534
-4.791286	-2.264081	0.550528	0.000944	0.298257
-5.080346	-2.234372	0.555533	0.000998	0.298147
-5.545656	-2.187764	0.560538	0.001085	0.297963
-5.842659	-2.167805	0.565542	0.001140	0.297798
-6.295393	-2.119403	0.570547	0.001224	0.297634
-6.268334	-2.159808	0.575552	0.001219	0.297461
-7.220750	-2.013931	0.580557	0.001396	0.297329
-7.268317	-2.037498	0.585562	0.001405	0.297173
-7.162359	-2.089839	0.590566	0.001385	0.297012
-7.206442	-2.109713	0.595571	0.001393	0.296876
-7.374503	-2.112511	0.600576	0.001424	0.296714
-7.514035	-2.107437	0.605581	0.001450	0.296616
-7.678449	-2.126462	0.610586	0.001481	0.296377
-7.909548	-2.096179	0.615590	0.001524	0.296320
-8.283563	-2.079210	0.620595	0.001593	0.296071
-8.125323	-2.112226	0.625600	0.001564	0.296051
-8.360126	-2.133208	0.630605	0.001608	0.295740
-8.320151	-2.139831	0.635610	0.001600	0.295743
-8.424692	-2.167712	0.640614	0.001620	0.295514
-8.832022	-2.097306	0.645619	0.001695	0.295497
-8.951367	-2.131804	0.650624	0.001717	0.295222
-9.140454	-2.111522	0.655629	0.001753	0.295153
-9.258144	-2.134265	0.660634	0.001774	0.294937
-9.446664	-2.120721	0.665638	0.001809	0.294835
-9.518969	-2.140588	0.670643	0.001823	0.294674
-9.315191	-2.212306	0.675648	0.001785	0.294504
-9.643463	-2.173440	0.680653	0.001846	0.294402
-10.234149	-2.103043	0.685658	0.001956	0.294220
-10.017930	-2.147902	0.690662	0.001916	0.294193
-10.526147	-2.119523	0.695667	0.002010	0.293879
-10.412666	-2.137645	0.700672	0.001989	0.293891
-10.565066	-2.165007	0.705677	0.002017	0.293620
-10.703482	-2.149405	0.710682	0.002043	0.293574
-10.928719	-2.148697	0.715686	0.002085	0.293376
-11.039911	-2.154870	0.720691	0.002105	0.293246
-10.882011	-2.203043	0.725696	0.002076	0.293150
-11.544299	-2.120693	0.730701	0.002199	0.292962
-11.499441	-2.134192	0.735706	0.002191	0.292936
-11.668288	-2.166887	0.740710	0.002222	0.292623
-11.670589	-2.168576	0.745715	0.002223	0.292613
-12.087013	-2.138640	0.750720	0.002300	0.292387
-12.230805	-2.129067	0.755725	0.002327	0.292305
-12.207124	-2.158871	0.760730	0.002322	0.292180
-12.856010	-2.079048	0.765734	0.002443	0.291991
-12.604547	-2.127541	0.770739	0.002396	0.291977
-12.584777	-2.185062	0.775744	0.002392	0.291710
-13.417717	-2.034810	0.780749	0.002547	0.291705
-13.739313	-2.005993	0.785754	0.002607	0.291558
-13.254219	-2.133432	0.790758	0.002517	0.291364
-13.476511	-2.094773	0.795763	0.002558	0.291355
-13.561748	-2.136253	0.800768	0.002574	0.291072
-13.629552	-2.128261	0.805773	0.002587	0.291051
-13.653400	-2.156532	0.810778	0.002591	0.290889
-14.146688	-2.097184	0.815782	0.002683	0.290739
-14.225843	-2.083623	0.820787	0.002697	0.290735
-14.040791	-2.166474	0.825792	0.002663	0.290490
-14.300352	-2.119859	0.830797	0.002711	0.290488
-14.336693	-2.154618	0.835802	0.002718	0.290282
-14.424888	-2.166807	0.840806	0.002734	0.290141
-14.484472	-2.170296	0.845811	0.002745	0.290070
-15.124862	-2.102043	0.850816	0.002864	0.289830
-14.973631	-2.131009	0.855821	0.002836	0.289823
-15.003704	-2.169507	0.860826	0.002842	0.289604
-15.624636	-2.074780	0.865830	0.002957	0.289513
-15.521224	-2.103490	0.870835	0.002938	0.289464
-15.410685	-2.173726	0.875840	0.002917	0.289214
-15.828508	-2.097756	0.880845	0.002995	0.289214
-16.136020	-2.084358	0.885850	0.003052	0.289002
-15.869248	-2.157974	0.890854	0.003002	0.288876
-16.016872	-2.136914	0.895859	0.003030	0.288848
-16.371794	-2.129955	0.900864	0.003096	0.288559
-16.569170	-2.093632	0.905869	0.003133	0.288562
-16.378967	-2.158676	0.910874	0.003097	0.288409
-16.892170	-2.097992	0.915878	0.003193	0.288246
-17.246523	-2.034503	0.920883	0.003258	0.288242
-16.942294	-2.136313	0.925888	0.003202	0.288008
-17.191273	-2.102151	0.930893	0.003248	0.287953
-17.511957	-2.060456	0.935898	0.003308	0.287870
-17.738253	-2.068078	0.940902	0.003350	0.287625
-17.547957	-2.105377	0.945907	0.003314	0.287611
-17.497679	-2.147976	0.950912	0.003305	0.287443
-17.980425	-2.089637	0.955917	0.003395	0.287295
-17.739062	-2.132371	0.960922	0.003350	0.287302
-17.659432	-2.209587	0.965926	0.003335	0.286986
-18.224713	-2.110891	0.970931	0.003440	0.286965
-17.922944	-2.189295	0.975936	0.003384	0.286847
-18.559099	-2.105141	0.980941	0.003502	0.286688
-18.771606	-2.066729	0.985946	0.003542	0.286688
-18.739982	-2.123934	0.990950	0.003536	0.286428
-18.830538	-2.123862	0.995955	0.003552	0.286345
-18.927056	-2.117820	1.000960	0.003570	0.286288
-19.195571	-2.117692	1.005965	0.003620	0.286042
-19.349386	-2.088804	1.010970	0.003649	0.286047
-19.039516	-2.179895	1.015974	0.003591	0.285871
-19.968837	-2.039747	1.020979	0.003764	0.285726
-19.806385	-2.067010	1.025984	0.003734	0.285737
-19.773236	-2.114776	1.030989	0.003728	0.285526
-20.224624	-2.043128	1.035994	0.003811	0.285474
-20.398140	-2.012388	1.040998	0.003844	0.285470
-20.298318	-2.096989	1.046003	0.003825	0.285133
-19.982058	-2.153416	1.051008	0.003766	0.285139
-20.687985	-2.047412	1.056013	0.003898	0.285026
-20.777156	-2.072554	1.061018	0.003914	0.284816
-20.669325	-2.089565	1.066022	0.003894	0.284830
-21.257706	-2.026522	1.071027	0.004003	0.284607
-21.182822	-2.061452	1.076032	0.003989	0.284498
-21.226705	-2.052275	1.081037	0.003997	0.284505
-21.682427	-2.018351	1.086042	0.004082	0.284256
-21.561484	-2.048281	1.091046	0.004060	0.284216
-21.553666	-2.055608	1.096051	0.004058	0.284186
-21.634902	-2.102314	1.101056	0.004073	0.283873
-21.759763	-2.082190	1.106061	0.004096	0.283860
-22.063040	-2.045711	1.111066	0.004153	0.283766
-22.008584	-2.095651	1.116070	0.004143	0.283562
-22.238923	-2.055762	1.121075	0.004185	0.283552
-22.327340	-2.075612	1.126080	0.004202	0.283369
-22.486569	-2.073603	1.131085	0.004231	0.283231
-22.786843	-2.019144	1.136090	0.004287	0.283231
-22.626938	-2.093582	1.141094	0.004257	0.282999
-22.940879	-2.047468	1.146099	0.004316	0.282944
-22.726804	-2.093284	1.151104	0.004276	0.282909
-23.228046	-2.061159	1.156109	0.004369	0.282607
-23.231458	-2.061749	1.161114	0.004370	0.282601
-23.391860	-2.050238	1.166118	0.004400	0.282511
-23.873707	-2.003661	1.171123	0.004489	0.282301
-23.786200	-2.016644	1.176128	0.004473	0.282316
-24.157666	-1.977644	1.181133	0.004542	0.282170
-24.386305	-1.972798	1.186138	0.004584	0.281982
-24.696160	-1.911265	1.191142	0.004642	0.282009
-24.704834	-1.935333	1.196147	0.004644	0.281878
-24.717199	-1.967660	1.201152	0.004646	0.281700
-24.843980	-1.945386	1.206157	0.004669	0.281697
-25.127360	-1.914307	1.211162	0.004722	0.281592
-24.892882	-2.001784	1.216166	0.004678	0.281362
-25.402825	-1.906824	1.221171	0.004773	0.281374
-25.335409	-1.939600	1.226176	0.004761	0.281268
-25.579207	-1.935394	1.231181	0.004806	0.281062
-25.550315	-1.938343	1.236186	0.004800	0.281074
-25.620987	-1.945602	1.241190	0.004814	0.280971
-26.100655	-1.903991	1.246195	0.004903	0.280736
-25.255053	-2.057411	1.251200	0.004745	0.280738
-25.386623	-2.057440	1.256205	0.004770	0.280615
-25.753136	-2.015207	1.261210	0.004838	0.280489
-25.300426	-2.097072	1.266214	0.004754	0.280492
-26.120297	-2.005610	1.271219	0.004906	0.280195
-26.272104	-1.985026	1.276224	0.004934	0.280159
-26.053112	-2.032507	1.281229	0.004894	0.280120
-26.637200	-1.979535	1.286234	0.005002	0.279845
-26.648107	-1.977578	1.291238	0.005004	0.279845
-27.039017	-1.918852	1.296243	0.005077	0.279781
-26.907911	-1.991280	1.301248	0.005052	0.279530
-26.934468	-1.988405	1.306253	0.005057	0.279520
-26.958856	-2.008059	1.311258	0.005062	0.279396
-27.544250	-1.928491	1.316262	0.005171	0.279257
-27.602013	-1.920957	1.321267	0.005181	0.279242
-27.961707	-1.884532	1.326272	0.005248	0.279092
-27.892267	-1.932113	1.331277	0.005235	0.278911
-27.519123	-2.002065	1.336282	0.005166	0.278900
-27.766332	-1.992870	1.341286	0.005212	0.278715
-28.281135	-1.924303	1.346291	0.005308	0.278585
-28.383455	-1.901547	1.351296	0.005326	0.278607
-28.288205	-1.965546	1.356301	0.005309	0.278365
-28.454308	-1.954916	1.361306	0.005340	0.278263
-27.822797	-2.069480	1.366310	0.005222	0.278265
-28.505576	-2.001211	1.371315	0.005349	0.277975
-28.600217	-1.985009	1.376320	0.005367	0.277970
-28.419641	-2.039013	1.381325	0.005333	0.277860
-28.856676	-2.003614	1.386330	0.005414	0.277630
-29.155162	-1.945586	1.391334	0.005470	0.277650
-28.958307	-2.019215	1.396339	0.005433	0.277453
-29.386626	-1.964500	1.401344	0.005513	0.277333
-29.328393	-1.976562	1.406349	0.005502	0.277325
-29.537137	-1.993017	1.411354	0.005541	0.277041
-29.367250	-2.032083	1.416358	0.005509	0.276999
-29.382984	-2.039514	1.421363	0.005512	0.276945
-29.832344	-2.002554	1.426368	0.005595	0.276712
-29.855575	-1.999501	1.431373	0.005600	0.276706
-29.623398	-2.076752	1.436378	0.005556	0.276523
-30.149261	-2.008932	1.441382	0.005654	0.276378
-30.652343	-1.916962	1.446387	0.005748	0.276381
-30.410169	-2.008143	1.451392	0.005703	0.276134
-30.440405	-2.016967	1.456397	0.005708	0.276059
-30.652924	-1.982466	1.461402	0.005748	0.276038
-30.779530	-2.010242	1.466406	0.005771	0.275771
-30.618357	-2.044591	1.471411	0.005741	0.275745
-31.535575	-1.891316	1.476416	0.005912	0.275675
-31.301730	-1.966040	1.481421	0.005868	0.275506
-31.085496	-2.005638	1.486426	0.005828	0.275505
-31.483356	-1.974616	1.491430	0.005902	0.275288
-32.160743	-1.873208	1.496435	0.006028	0.275174
-31.027238	-2.081882	1.501440	0.005817	0.275160
-31.283975	-2.093451	1.506445	0.005865	0.274854
-32.102305	-1.946501	1.511450	0.006017	0.274845
-31.761775	-2.028553	1.516454	0.005953	0.274739
-31.758960	-2.073335	1.521459	0.005953	0.274506
-31.704649	-2.083779	1.526464	0.005943	0.274503
-32.168253	-2.043535	1.531469	0.006029	0.274271
-32.414520	-2.005735	1.536474	0.006075	0.274234
-32.188588	-2.063442	1.541478	0.006033	0.274147
-32.851846	-1.992426	1.546483	0.006156	0.273885
-32.655682	-2.027817	1.551488	0.006119	0.273887
-32.753518	-2.045316	1.556493	0.006138	0.273701
-33.361429	-1.956490	1.561498	0.006251	0.273586
-33.308131	-1.963787	1.566502	0.006241	0.273599
-33.102263	-2.062032	1.571507	0.006202	0.273278
-33.310103	-2.029902	1.576512	0.006241	0.273248
-33.318625	-2.046943	1.581517	0.006243	0.273150
-33.322465	-2.082455	1.586522	0.006243	0.272958
-33.457198	-2.054333	1.591526	0.006268	0.272978
-34.003351	-2.010900	1.596531	0.006370	0.272681
-33.649967	-2.086531	1.601536	0.006304	0.272621
-33.552893	-2.123155	1.606541	0.006286	0.272521
-34.194252	-2.047573	1.611546	0.006405	0.272303
-33.866369	-2.105540	1.616550	0.006344	0.272312
-33.877490	-2.156484	1.621555	0.006346	0.272031
-34.259957	-2.095757	1.626560	0.006417	0.271984
-34.433586	-2.085311	1.631565	0.006449	0.271872
-34.467075	-2.113460	1.636570	0.006456	0.271690
-34.381227	-2.127774	1.641574	0.006440	0.271697
-35.037020	-2.071101	1.646579	0.006562	0.271364
-34.928785	-2.091284	1.651584	0.006541	0.271361
-34.886780	-2.124236	1.656589	0.006534	0.271227
-35.293562	-2.083349	1.661594	0.006609	0.271050
-35.564121	-2.030610	1.666598	0.006660	0.271069
-35.867423	-2.031874	1.671603	0.006716	0.270768
-35.665523	-2.072445	1.676608	0.006678	0.270748
-35.686827	-2.086378	1.681613	0.006682	0.270653
-35.901228	-2.079359	1.686618	0.006722	0.270482
-35.754389	-2.103150	1.691622	0.006695	0.270498
-36.309055	-2.060336	1.696627	0.006798	0.270187
-36.714007	-1.993956	1.701632	0.006873	0.270149
-36.418080	-2.062744	1.706637	0.006818	0.270069
-37.012035	-1.999717	1.711642	0.006929	0.269828
-36.924316	-2.013513	1.716646	0.006912	0.269840
-37.131386	-2.012399	1.721651	0.006951	0.269644
-37.473343	-1.974425	1.726656	0.007014	0.269514
-37.486663	-1.973504	1.731661	0.007017	0.269506
-37.623640	-1.993123	1.736666	0.007042	0.269267
-37.199789	-2.078212	1.741670	0.006963	0.269225
-37.708039	-2.001225	1.746675	0.007058	0.269142
-38.177268	-1.961291	1.751680	0.007145	0.268898
-37.543603	-2.079249	1.756685	0.007027	0.268884
-38.034603	-2.026242	1.761690	0.007118	0.268688
-38.190598	-2.018034	1.766694	0.007147	0.268580
-38.614911	-1.940476	1.771699	0.007226	0.268583
-38.323594	-2.047083	1.776704	0.007172	0.268294
-38.620561	-2.000171	1.781709	0.007227	0.268256
-38.472178	-2.044120	1.786714	0.007199	0.268164
-38.582911	-2.059732	1.791718	0.007220	0.267972
-39.248221	-1.939567	1.796723	0.007344	0.267967
-39.273813	-1.972846	1.801728	0.007348	0.267763
-39.028255	-2.042828	1.806733	0.007303	0.267626
-39.153057	-2.020959	1.811738	0.007326	0.267622
-39.400455	-2.032360	1.816742	0.007372	0.267317
-39.470534	-2.022079	1.821747	0.007385	0.267304
-39.668108	-2.007827	1.826752	0.007422	0.267187
-40.148717	-1.955566	1.831757	0.007511	0.266996
-40.056436	-1.975771	1.836762	0.007494	0.266978
-39.657206	-2.081062	1.841766	0.007419	0.266801
-40.434686	-1.958478	1.846771	0.007564	0.266699
-40.444713	-1.957023	1.851776	0.007566	0.266698
-40.338049	-2.037222	1.856781	0.007546	0.266368
-40.557646	-1.999689	1.861786	0.007587	0.266355
-40.512678	-2.029559	1.866790	0.007578	0.266237
-40.891108	-1.994067	1.871795	0.007649	0.266056
-40.716135	-2.024559	1.876800	0.007616	0.266064
-41.067347	-2.009027	1.881805	0.007681	0.265801
-41.217424	-1.994641	1.886810	0.007709	0.265731
-40.907640	-2.059101	1.891814	0.007652	0.265687
-41.331291	-2.022859	1.896819	0.007730	0.265465
-41.343383	-2.018913	1.901824	0.007733	0.265475
-41.505877	-2.027225	1.906829	0.007763	0.265268
-41.907673	-1.979351	1.911834	0.007837	0.265131
-41.634339	-2.030498	1.916838	0.007787	0.265124
-42.407744	-1.945539	1.921843	0.007930	0.264820
-42.239841	-1.975277	1.926848	0.007899	0.264824
-42.242631	-1.994451	1.931853	0.007900	0.264717
-42.267279	-2.033676	1.936858	0.007904	0.264478
-41.791477	-2.118653	1.941862	0.007816	0.264487
-42.104242	-2.108824	1.946867	0.007874	0.264230
-42.585194	-2.026011	1.951872	0.007963	0.264204
-42.381433	-2.089422	1.956877	0.007925	0.264060
-42.843079	-2.043280	1.961882	0.008011	0.263853
-43.073136	-1.997922	1.966886	0.008054	0.263873
-43.179980	-2.030092	1.971891	0.008074	0.263590
-43.274747	-2.018954	1.976896	0.008091	0.263556
-43.328820	-2.027086	1.981901	0.008101	0.263458
-44.022011	-1.940534	1.986906	0.008230	0.263241
-43.568408	-2.021186	1.991910	0.008146	0.263251
-43.689993	-2.037048	1.996915	0.008168	0.263043
-44.059599	-1.985659	2.001920	0.008237	0.262956

-44.631731	-1.940511	2.011917	0.008343	0.262632
-44.738054	-1.938562	2.021914	0.008363	0.262537
-44.839363	-1.961803	2.031910	0.008382	0.262307
-44.931589	-1.964657	2.041907	0.008399	0.262200
-45.137263	-1.967941	2.051904	0.008437	0.261975
-44.948563	-2.003452	2.061901	0.008402	0.261970
-45.250211	-1.996944	2.071898	0.008458	0.261703
-45.418889	-1.968945	2.081894	0.008489	0.261689
-45.305994	-1.989902	2.091891	0.008468	0.261687
-45.345647	-2.004200	2.101888	0.008475	0.261569
-45.507249	-2.015639	2.111885	0.008505	0.261343
-45.616191	-1.995031	2.121882	0.008525	0.261348
-45.919264	-1.938447	2.131878	0.008582	0.261357
-45.288019	-2.056084	2.141875	0.008464	0.261342
-45.463276	-2.023267	2.151872	0.008496	0.261348
-45.363963	-2.041929	2.161869	0.008478	0.261345
-45.695269	-1.982223	2.171866	0.008539	0.261343
-45.642381	-1.991474	2.181862	0.008529	0.261346
-45.450600	-2.026366	2.191859	0.008494	0.261346
-45.617700	-1.995886	2.201856	0.008525	0.261348
-45.369846	-2.042008	2.211853	0.008478	0.261343
-45.472424	-1.993042	2.221850	0.008497	0.261511
-45.134347	-2.025333	2.231846	0.008434	0.261674
-45.040618	-2.042557	2.241843	0.008417	0.261673
-45.092914	-2.032708	2.251840	0.008426	0.261676
-44.974327	-2.054481	2.261837	0.008404	0.261675
-45.031171	-2.003385	2.271834	0.008414	0.261902
-44.824943	-2.030699	2.281830	0.008376	0.261959
-44.683723	-2.056731	2.291827	0.008349	0.261957
-44.881518	-1.988487	2.301824	0.008386	0.262136
-44.449811	-2.039141	2.311821	0.008306	0.262291
-44.574577	-2.017966	2.321818	0.008329	0.262283
-44.102113	-2.055163	2.331814	0.008241	0.262553
-44.532350	-1.966387	2.341811	0.008321	0.262612
-44.211378	-1.997278	2.351808	0.008261	0.262764
-44.054012	-1.992297	2.361805	0.008231	0.262950
-44.100252	-1.965477	2.371802	0.008240	0.263052
-43.828174	-1.980193	2.381798	0.008189	0.263244
-44.291164	-1.868926	2.391795	0.008275	0.263394
-43.990771	-1.888498	2.401792	0.008219	0.263587
-43.736846	-1.895520	2.411789	0.008172	0.263803
-43.598443	-1.907187	2.421786	0.008146	0.263878
-43.305418	-1.896940	2.431782	0.008091	0.264227
-43.233966	-1.891617	2.441779	0.008077	0.264328
-42.668895	-1.962141	2.451776	0.007972	0.264505
-42.584508	-1.940770	2.461773	0.007956	0.264707
-42.560871	-1.923110	2.471770	0.007952	0.264828
-42.097433	-1.950448	2.481766	0.007865	0.265140
-41.990138	-1.951727	2.491763	0.007845	0.265240
-41.377857	-2.019378	2.501760	0.007731	0.265480
-41.753714	-1.918442	2.511757	0.007801	0.265658
-41.707129	-1.903235	2.521754	0.007792	0.265788
-40.982150	-1.985647	2.531750	0.007657	0.266058
-40.700836	-2.010452	2.541747	0.007605	0.266202
-40.403046	-2.035634	2.551744	0.007549	0.266360
-40.526046	-1.958593	2.561741	0.007572	0.266658
-40.149577	-2.004710	2.571738	0.007502	0.266780
-39.740271	-2.043430	2.581734	0.007425	0.266974
-39.807677	-1.986801	2.591731	0.007438	0.267216
-40.223777	-1.872851	2.601728	0.007515	0.267424
-39.478862	-1.969132	2.611725	0.007376	0.267637
-38.948916	-2.016447	2.621722	0.007277	0.267903
-38.545334	-2.066816	2.631718	0.007202	0.268028
-38.729290	-1.989746	2.641715	0.007236	0.268264
-38.148996	-2.052734	2.651712	0.007128	0.268494
-38.357374	-1.986814	2.661709	0.007167	0.268646
-37.585419	-2.084756	2.671706	0.007023	0.268876
-37.559270	-2.045624	2.681702	0.007018	0.269112
-37.133371	-2.098887	2.691699	0.006938	0.269243
-36.831982	-2.106944	2.701696	0.006882	0.269495
-36.518140	-2.131837	2.711693	0.006824	0.269669
-36.436665	-2.118789	2.721690	0.006808	0.269819
-36.422472	-2.064386	2.731686	0.006806	0.270125
-36.177106	-2.076572	2.741683	0.006760	0.270300
-35.734426	-2.122208	2.751680	0.006677	0.270487
-35.660531	-2.090610	2.761677	0.006663	0.270729
-35.535859	-2.082987	2.771674	0.006640	0.270892
-35.224757	-2.109380	2.781670	0.006582	0.271054
-35.055408	-2.083082	2.791667	0.006550	0.271359
-34.895752	-2.076730	2.801664	0.006520	0.271549
-35.018851	-2.017300	2.811661	0.006543	0.271747
-34.503583	-2.066852	2.821658	0.006447	0.271983
-34.340084	-2.047203	2.831654	0.006416	0.272246
-34.271157	-2.021358	2.841651	0.006404	0.272451
-34.045270	-2.020038	2.851648	0.006361	0.272677
-33.624380	-2.041790	2.861645	0.006283	0.272968
-33.425870	-2.037580	2.871642	0.006246	0.273183
-33.575289	-1.968030	2.881638	0.006273	0.273408
-32.780052	-2.076548	2.891635	0.006125	0.273600
-32.837708	-2.010798	2.901632	0.006136	0.273893
-32.729940	-1.981535	2.911629	0.006116	0.274151
-32.004778	-2.074883	2.921626	0.005981	0.274355
-32.043206	-2.031807	2.931622	0.005988	0.274546
-31.797858	-2.019332	2.941619	0.005942	0.274848
-31.492599	-2.027686	2.951616	0.005885	0.275097
-31.187173	-2.043551	2.961613	0.005828	0.275306
-30.961573	-2.043757	2.971610	0.005786	0.275522
-30.996614	-1.995070	2.981606	0.005792	0.275745
-30.355051	-2.063640	2.991603	0.005672	0.275998
-30.761306	-1.947288	3.001600	0.005748	0.276221
-30.207694	-2.004345	3.011597	0.005645	0.276450
-30.038867	-1.986524	3.021594	0.005613	0.276705
-30.036257	-1.932596	3.031590	0.005612	0.276990
-29.872680	-1.910851	3.041587	0.005582	0.277260
-29.883816	-1.859449	3.051584	0.005584	0.277518
-29.493384	-1.878643	3.061581	0.005511	0.277789
-28.970562	-1.926167	3.071578	0.005413	0.278037
-29.206648	-1.834039	3.081574	0.005457	0.278294
-28.354884	-1.929624	3.091571	0.005299	0.278603
-28.407336	-1.874160	3.101568	0.005308	0.278842
-28.311572	-1.838533	3.111565	0.005290	0.279118
-27.431560	-1.956377	3.121562	0.005126	0.279337
-27.195704	-1.960919	3.131558	0.005082	0.279537
-26.201167	-2.084465	3.141555	0.004897	0.279834
-26.225246	-2.044171	3.151552	0.004901	0.280020
-25.983711	-2.050599	3.161549	0.004856	0.280215
-25.809295	-2.029391	3.171546	0.004824	0.280488
-25.901223	-1.971345	3.181542	0.004841	0.280702
-25.751021	-1.957222	3.191539	0.004812	0.280917
-25.654133	-1.928629	3.201536	0.004794	0.281155
-25.041375	-2.000521	3.211533	0.004680	0.281359
-25.082287	-1.928557	3.221530	0.004688	0.281692
-24.569337	-1.980253	3.231526	0.004592	0.281906
-24.392402	-1.970563	3.241523	0.004559	0.282121
-24.234090	-1.953913	3.251520	0.004529	0.282355
-23.870684	-1.966159	3.261517	0.004461	0.282632
-23.798572	-1.923723	3.271514	0.004448	0.282917
-23.599107	-1.916715	3.281510	0.004411	0.283139
-23.261262	-1.935499	3.291507	0.004348	0.283357
-22.902008	-1.956055	3.301504	0.004281	0.283586
-22.726695	-1.927928	3.311501	0.004248	0.283893
-22.449921	-1.929463	3.321498	0.004196	0.284142
-21.850212	-2.001025	3.331494	0.004084	0.284334
-21.438395	-2.040444	3.341491	0.004008	0.284515
-21.441163	-1.976980	3.351488	0.004008	0.284836
-21.110771	-1.993689	3.361485	0.003946	0.285057
-21.043945	-1.964975	3.371482	0.003934	0.285265
-20.223943	-2.072185	3.381478	0.003781	0.285478
-20.015209	-2.065203	3.391475	0.003742	0.285706
-19.684781	-2.092184	3.401472	0.003680	0.285874
-19.518016	-2.087799	3.411469	0.003649	0.286050
-19.707480	-1.992196	3.421466	0.003684	0.286360
-18.940098	-2.092233	3.431462	0.003541	0.286560
-18.808613	-2.080750	3.441459	0.003517	0.286740
-18.709210	-2.051276	3.451456	0.003498	0.286980
-18.141577	-2.107296	3.461453	0.003392	0.287219
-18.248691	-2.052520	3.471450	0.003412	0.287397
-17.796918	-2.092606	3.481446	0.003328	0.287610
-17.630111	-2.061708	3.491443	0.003297	0.287918
-17.447024	-2.059657	3.501440	0.003262	0.288096
-17.521883	-2.006668	3.511437	0.003276	0.288295
-17.269684	-1.996425	3.521434	0.003229	0.288577
-16.575000	-2.074278	3.531430	0.003100	0.288820
-16.942904	-1.964280	3.541427	0.003168	0.289037
-16.197962	-2.059964	3.551424	0.003029	0.289236
-15.684251	-2.102351	3.561421	0.002933	0.289492
-15.620996	-2.073536	3.571418	0.002921	0.289694
-15.392265	-2.077546	3.581414	0.002879	0.289882
-15.215547	-2.057388	3.591411	0.002846	0.290144
-14.599463	-2.116283	3.601408	0.002731	0.290409
-14.857805	-2.036086	3.611405	0.002779	0.290576
-14.465765	-2.074175	3.621402	0.002706	0.290741
-14.243485	-2.053401	3.631398	0.002664	0.291046
-14.040347	-2.051286	3.641395	0.002626	0.291241
-13.775495	-2.059811	3.651392	0.002577	0.291438
-13.502036	-2.056860	3.661389	0.002526	0.291700
-13.247252	-2.054328	3.671386	0.002478	0.291943
-12.921157	-2.074575	3.681382	0.002417	0.292137
-12.484012	-2.118979	3.691379	0.002336	0.292312
-12.033016	-2.138542	3.701376	0.002252	0.292621
-12.082276	-2.092021	3.711373	0.002261	0.292807
-11.585038	-2.149428	3.721370	0.002168	0.292971
-11.356601	-2.134852	3.731366	0.002125	0.293249
-11.042390	-2.158266	3.741363	0.002067	0.293415
-10.769445	-2.172575	3.751360	0.002016	0.293590
-10.847246	-2.099654	3.761357	0.002030	0.293880
-10.787209	-2.065852	3.771354	0.002019	0.294101
-10.415311	-2.095893	3.781350	0.001949	0.294286
-10.411554	-2.048228	3.791347	0.001949	0.294525
-10.076149	-2.051690	3.801344	0.001886	0.294808
-9.705780	-2.078628	3.811341	0.001817	0.295006
-9.463472	-2.084080	3.821338	0.001772	0.295196
-9.082547	-2.091421	3.831334	0.001701	0.295500
-8.936726	-2.082954	3.841331	0.001673	0.295672
-8.769992	-2.075827	3.851328	0.001642	0.295856
-8.416802	-2.097294	3.861325	0.001576	0.296065
-8.159302	-2.086757	3.871322	0.001528	0.296346
-7.988963	-2.077272	3.881318	0.001496	0.296544
-7.804988	-2.068579	3.891315	0.001462	0.296750
-7.892586	-1.999598	3.901312	0.001478	0.297009
-7.317843	-2.050497	3.911309	0.001371	0.297271
-6.967356	-2.076083	3.921306	0.001306	0.297457
-6.989725	-2.027746	3.931302	0.001310	0.297673
-6.614405	-2.032964	3.941299	0.001240	0.297979
-6.866670	-1.938035	3.951296	0.001286	0.298218
-6.207926	-2.014016	3.961293	0.001164	0.298431
-5.846409	-2.038560	3.971290	0.001096	0.298631
-5.485338	-2.050721	3.981286	0.001029	0.298891
-4.804916	-2.121286	3.991283	0.000902	0.299148
-4.678397	-2.112137	4.001280	0.000878	0.299304
-4.430886	-2.115373	4.011277	0.000832	0.299506
-4.288422	-2.084410	4.021274	0.000805	0.299782
-4.504790	-2.002962	4.031270	0.000846	0.299985
-4.437903	-1.964625	4.041267	0.000833	0.300229
-3.987515	-1.988567	4.051264	0.000749	0.300509
-3.656323	-2.008784	4.061261	0.000687	0.300702
-3.399299	-2.016057	4.071258	0.000639	0.300892
-3.130495	-2.021862	4.081254	0.000589	0.301100
-3.195112	-1.954337	4.091251	0.000601	0.301368
-3.131766	-1.904058	4.101248	0.000589	0.301665
-3.018694	-1.878764	4.111245	0.000568	0.301886
-2.810381	-1.866820	4.121242	0.000529	0.302125
-2.819080	-1.809209	4.131238	0.000530	0.302394
-2.576739	-1.796775	4.141235	0.000485	0.302664
-2.509713	-1.743799	4.151232	0.000472	0.302976
-2.674278	-1.653426	4.161229	0.000503	0.303266
-2.675333	-1.590216	4.171226	0.000503	0.303567
-2.022792	-1.648888	4.181222	0.000381	0.303853
-2.049099	-1.578983	4.191219	0.000386	0.304163
-1.753695	-1.574689	4.201216	0.000331	0.304439
-1.703355	-1.520194	4.211213	0.000321	0.304742
-2.097821	-1.377884	4.221210	0.000395	0.305078
-1.524098	-1.410758	4.231206	0.000288	0.305417
-1.565982	-1.341232	4.241203	0.000295	0.305711
-1.686984	-1.248616	4.251200	0.000318	0.306045
-1.575216	-1.191925	4.261197	0.000297	0.306410
-1.765261	-1.075720	4.271194	0.000332	0.306796
-1.695839	-1.013170	4.281190	0.000319	0.307150
-1.475203	-0.976977	4.291187	0.000277	0.307510
-1.206949	-0.942636	4.301184	0.000227	0.307901
-1.123405	-0.875343	4.311181	0.000212	0.308289
-0.847471	-0.840426	4.321178	0.000160	0.308689
-1.170113	-0.696416	4.331174	0.000220	0.309089
-0.777376	-0.691103	4.341171	0.000147	0.309448
-0.439733	-0.657605	4.351168	0.000084	0.309892
-0.390409	-0.579607	4.361165	0.000074	0.310298
-0.549855	-0.469943	4.371162	0.000104	0.310675
-0.211442	-0.441937	4.381158	0.000041	0.311092
-0.316819	-0.328714	4.391155	0.000060	0.311530
-0.224249	-0.258218	4.401152	0.000043	0.311936
-0.464985	-0.105015	4.411149	0.000087	0.312443
-0.429641	-0.017326	4.421146	0.000080	0.312880
-0.521389	0.110447	4.431142	0.000097	0.313393
0.000000	0.104776	4.441139	0.000000	0.313805

-0.338022	0.446301	4.446144	0.000063	0.315094
0.041532	0.940019	4.451149	-0.000008	0.317667
0.676026	1.683479	4.456154	-0.000127	0.321554
1.053359	2.767066	4.461158	-0.000198	0.326696
2.008001	4.044275	4.466163	-0.000377	0.333058
2.467081	5.709395	4.471168	-0.000463	0.340568
4.066553	7.477745	4.476173	-0.000762	0.349203
5.660479	9.560150	4.481178	-0.001061	0.358892
7.352472	11.945827	4.486182	-0.001377	0.369585
9.071544	14.663393	4.491187	-0.001699	0.381256
10.501757	17.771108	4.496192	-0.001968	0.393822
11.943349	21.222555	4.501197	-0.002238	0.407229
13.910102	24.933353	4.506202	-0.002607	0.421425
16.050823	28.968728	4.511206	-0.003008	0.436338
17.951053	33.414732	4.516211	-0.003365	0.451933
19.724784	38.244368	4.521216	-0.003699	0.468122
21.639437	43.408616	4.526221	-0.004058	0.484843
23.384587	48.971460	4.531226	-0.004387	0.502066
24.875028	54.924187	4.536230	-0.004669	0.519673
26.744590	61.146650	4.541235	-0.005021	0.537612
28.058695	67.797862	4.546240	-0.005270	0.555826
29.868587	74.680118	4.551245	-0.005611	0.574267
31.494461	81.908920	4.556250	-0.005919	0.592897
32.814169	89.472266	4.561254	-0.006170	0.611619
34.377436	97.269794	4.566259	-0.006466	0.630421
35.674911	105.354498	4.571264	-0.006713	0.649211
37.235079	113.644501	4.576269	-0.007009	0.668016
38.658324	122.150822	4.581274	-0.007279	0.686710
39.961376	130.870843	4.586278	-0.007528	0.705300
41.158747	139.786504	4.591283	-0.007757	0.723765
42.424643	148.834133	4.596288	-0.007998	0.742050
43.114910	158.124821	4.601293	-0.008133	0.760162
44.267858	167.424988	4.606298	-0.008354	0.778022
45.184644	176.857361	4.611302	-0.008531	0.795644
46.306168	186.338966	4.616307	-0.008746	0.813035
46.610887	196.026654	4.621312	-0.008809	0.830168
47.635524	205.605216	4.626317	-0.009006	0.846985
48.457079	215.245247	4.631322	-0.009165	0.863517
49.001316	224.944080	4.636326	-0.009273	0.879754
49.934011	234.587792	4.641331	-0.009453	0.895718
50.964688	244.198061	4.646336	-0.009651	0.911375
51.651452	253.858803	4.651341	-0.009786	0.926752
52.402491	263.483036	4.656346	-0.009932	0.941839
52.826899	273.138126	4.661350	-0.010017	0.956647
53.302145	282.757666	4.666355	-0.010112	0.971190
53.992285	292.284822	4.671360	-0.010247	0.985437
54.423567	301.824613	4.676365	-0.010333	0.999434
55.128371	311.252894	4.681370	-0.010471	1.013146
55.366109	320.704085	4.686374	-0.010521	1.026593
57.754671	329.741587	4.691379	-0.010972	1.039809
68.127830	337.486077	4.696384	-0.012908	1.052981
69.610032	346.827566	4.701389	-0.013191	1.066064
70.632074	356.185777	4.706394	-0.013387	1.078904
71.705761	365.466875	4.711398	-0.013593	1.091501
72.665380	374.720204	4.716403	-0.013778	1.103892
73.289392	383.967575	4.721408	-0.013900	1.116063
74.173090	393.111657	4.726413	-0.014071	1.128026
74.943562	402.224861	4.731418	-0.014220	1.139800
75.542832	411.325724	4.736422	-0.014338	1.151401
76.723708	420.249766	4.741427	-0.014564	1.162790
76.951046	429.292670	4.746432	-0.014612	1.174013
77.742859	438.188021	4.751437	-0.014765	1.185067
78.400645	447.067606	4.756442	-0.014893	1.195973
79.208956	455.848890	4.761446	-0.015050	1.206692
79.911624	464.659785	4.766451	-0.015186	1.217331
80.222460	473.475304	4.771456	-0.015250	1.227804
81.259464	482.125297	4.776461	-0.015449	1.238139
81.783467	490.840365	4.781466	-0.015552	1.248362
82.182017	499.545000	4.786470	-0.015632	1.258466
83.214199	508.120548	4.791475	-0.015830	1.268465
83.832659	516.729348	4.796480	-0.015951	1.278343
84.758555	525.261678	4.801485	-0.016129	1.288117
85.487396	533.832945	4.806490	-0.016270	1.297824
86.189411	542.381002	4.811494	-0.016407	1.307428
86.525976	551.044408	4.816499	-0.016475	1.317021
87.063245	559.522794	4.821504	-0.016581	1.326379
87.468638	568.042591	4.826509	-0.016662	1.335693
88.087391	576.477569	4.831514	-0.016782	1.344889
88.393246	584.976051	4.836518	-0.016845	1.354034
89.337113	593.351630	4.841523	-0.017026	1.363101
89.936223	601.768158	4.846528	-0.017143	1.372089
90.425037	610.187155	4.851533	-0.017240	1.381003
91.498466	618.514541	4.856538	-0.017445	1.389865
92.063564	626.912578	4.861542	-0.017556	1.398656
92.409941	635.336009	4.866547	-0.017626	1.407380
92.955591	643.695374	4.871552	-0.017733	1.416019
93.458253	652.076204	4.876557	-0.017832	1.424620
93.956902	660.454763	4.881562	-0.017931	1.433166
94.281361	668.800485	4.886566	-0.017997	1.441600
94.515942	677.188972	4.891571	-0.018046	1.450012
94.774127	685.554882	4.896576	-0.018099	1.458357
95.122120	693.879826	4.901581	-0.018170	1.466629
96.446069	702.069137	4.906586	-0.018422	1.474878
97.000789	710.346583	4.911590	-0.018530	1.483044
97.572889	718.652783	4.916595	-0.018642	1.491196
97.719062	727.013541	4.921600	-0.018675	1.499288
98.329607	735.280548	4.926605	-0.018794	1.507320
99.360275	743.469153	4.931610	-0.018992	1.515300
99.534792	751.795172	4.936614	-0.019030	1.523235
100.374817	760.033628	4.941619	-0.019191	1.531149
101.043490	768.280120	4.946624	-0.019321	1.539003
101.648726	776.544645	4.951629	-0.019440	1.546824
102.154797	784.819817	4.956634	-0.019539	1.554601
102.891626	793.020943	4.961638	-0.019682	1.562305
103.493858	801.281057	4.966643	-0.019799	1.570005
104.023559	809.526483	4.971648	-0.019903	1.577643
104.279470	817.816312	4.976653	-0.019957	1.585244
104.708562	826.095443	4.981658	-0.020042	1.592824
105.269454	834.286175	4.986662	-0.020152	1.600308
105.861256	842.519164	4.991667	-0.020267	1.607799
106.542100	850.714596	4.996672	-0.020400	1.615234
106.523418	859.042125	5.001677	-0.020402	1.622653
107.291557	867.222062	5.006682	-0.020550	1.630019
107.907525	875.416278	5.011686	-0.020670	1.637343
108.731435	883.558268	5.016691	-0.020829	1.644617
108.880490	891.844160	5.021696	-0.020862	1.651890
109.215952	900.055377	5.026701	-0.020930	1.659092
109.843288	908.229514	5.031706	-0.021052	1.666272
110.485645	916.399045	5.036710	-0.021177	1.673418
110.442295	924.686294	5.041715	-0.021175	1.680541
111.148288	932.818380	5.046720	-0.021311	1.687603
111.831062	940.977093	5.051725	-0.021444	1.694655
112.263215	949.180961	5.056730	-0.021530	1.701682
112.818259	957.356178	5.061734	-0.021639	1.708673
113.459356	965.532420	5.066739	-0.021763	1.715647
113.840024	973.722761	5.071744	-0.021840	1.722569
114.317964	981.898791	5.076749	-0.021934	1.729465
114.916734	990.068312	5.081754	-0.022051	1.736344
115.251363	998.259375	5.086758	-0.022119	1.743179
115.322436	1006.517887	5.091763	-0.022137	1.750008
115.596590	1014.707553	5.096768	-0.022194	1.756781
116.709279	1022.735105	5.101773	-0.022406	1.763502
117.177943	1030.909853	5.106778	-0.022499	1.770235
117.099029	1039.179987	5.111782	-0.022490	1.776951
118.382895	1047.204604	5.116787	-0.022734	1.783615
118.977932	1055.370313	5.121792	-0.022850	1.790280
119.338579	1063.579219	5.126797	-0.022923	1.796926
119.351448	1071.805188	5.131802	-0.022931	1.803518
119.992186	1079.892985	5.136806	-0.023055	1.810054
120.216659	1088.096584	5.141811	-0.023102	1.816606
120.739541	1096.211265	5.146816	-0.023205	1.823101
121.117991	1104.374763	5.151821	-0.023281	1.829594
121.732530	1112.500016	5.156826	-0.023401	1.836062
122.377511	1120.599386	5.161830	-0.023526	1.842491
123.037908	1128.740116	5.166835	-0.023655	1.848931
123.338757	1136.904104	5.171840	-0.023716	1.855324
123.827466	1145.044342	5.176845	-0.023812	1.861698
124.468474	1153.174647	5.181850	-0.023937	1.868061
124.878000	1161.318019	5.186854	-0.024019	1.874386
125.611234	1169.408643	5.191859	-0.024160	1.880686
125.922288	1177.568701	5.196864	-0.024224	1.886968
126.380062	1185.722204	5.201869	-0.024314	1.893242
126.638069	1193.895999	5.206874	-0.024368	1.899488
126.619764	1202.072775	5.211878	-0.024370	1.905683
127.194054	1210.196681	5.216883	-0.024482	1.911886
127.742149	1218.297292	5.221888	-0.024590	1.918048
127.460671	1226.514571	5.226893	-0.024543	1.924184
128.126252	1234.589229	5.231898	-0.024672	1.930301
128.370734	1242.731122	5.236902	-0.024723	1.936401
128.832439	1250.839428	5.241907	-0.024814	1.942481
128.947545	1259.013587	5.246912	-0.024841	1.948552
129.494384	1267.068795	5.251917	-0.024948	1.954564
129.777530	1275.185980	5.256922	-0.025006	1.960574
130.159748	1283.283229	5.261926	-0.025083	1.966562
130.513880	1291.414846	5.266931	-0.025154	1.972554
130.808280	1299.542547	5.271936	-0.025214	1.978518
130.948810	1307.676165	5.276941	-0.025246	1.984452
131.521881	1315.759096	5.281946	-0.025358	1.990378
132.304909	1323.777373	5.286950	-0.025509	1.996262
132.721916	1331.894462	5.291955	-0.025592	2.002161
132.849709	1340.066718	5.296960	-0.025621	2.008050
133.219327	1348.182462	5.301965	-0.025695	2.013908
133.637057	1356.279815	5.306970	-0.025778	2.019741
133.969463	1364.387269	5.311974	-0.025845	2.025555
134.185827	1372.564959	5.316979	-0.025891	2.031390
134.841973	1380.599229	5.321984	-0.026019	2.037152
134.993869	1388.715088	5.326989	-0.026052	2.042903
135.551889	1396.809399	5.331994	-0.026161	2.048665
135.927967	1404.909711	5.336998	-0.026237	2.054396
136.408596	1412.996625	5.342003	-0.026332	2.060113
136.803506	1421.087005	5.347008	-0.026411	2.065807
137.217408	1429.200174	5.352013	-0.026493	2.071503
137.399462	1437.348830	5.357018	-0.026532	2.077184
137.800860	1445.404435	5.362022	-0.026612	2.082808
138.058957	1453.544687	5.367027	-0.026666	2.088460
138.255996	1461.682332	5.372032	-0.026708	2.094090
138.714310	1469.741467	5.377037	-0.026798	2.099676
139.156881	1477.837499	5.382042	-0.026886	2.105271
139.524128	1485.941913	5.387046	-0.026960	2.110849
139.659910	1494.099811	5.392051	-0.026991	2.116426
139.779298	1502.195782	5.397056	-0.027018	2.121945
139.940884	1510.297850	5.402061	-0.027054	2.127457
140.048317	1518.430052	5.407066	-0.027079	2.132970
140.421029	1526.466386	5.412070	-0.027154	2.138431
141.235096	1534.460440	5.417075	-0.027310	2.143891
141.443255	1542.590617	5.422080	-0.027355	2.149370
141.456378	1550.733099	5.427085	-0.027362	2.154825
142.058020	1558.763138	5.432090	-0.027480	2.160248
142.159294	1566.866049	5.437094	-0.027504	2.165657
142.780344	1574.935162	5.442099	-0.027625	2.171080
143.124893	1583.012582	5.447104	-0.027694	2.176468
143.601410	1591.065706	5.452109	-0.027788	2.181839
143.942775	1599.181047	5.457114	-0.027857	2.187226
144.079064	1607.306187	5.462118	-0.027888	2.192586
144.316286	1615.411514	5.467123	-0.027938	2.197930
144.413144	1623.496063	5.472128	-0.027961	2.203234
144.669837	1631.596189	5.477133	-0.028014	2.208550
145.296120	1639.625848	5.482138	-0.028136	2.213841
145.634096	1647.691178	5.487142	-0.028204	2.219117
145.912837	1655.783117	5.492147	-0.028262	2.224391
146.127408	1663.892897	5.497152	-0.028307	2.229659
146.258645	1671.990667	5.502157	-0.028337	2.234899
146.807071	1680.041643	5.507162	-0.028444	2.240134
147.186609	1688.085221	5.512166	-0.028520	2.245337
147.474771	1696.191264	5.517171	-0.028579	2.250560
147.950430	1704.242474	5.522176	-0.028673	2.255752
148.228041	1712.339040	5.527181	-0.028730	2.260944
148.363529	1720.461006	5.532186	-0.028761	2.266127
148.699174	1728.560007	5.537190	-0.028828	2.271301
149.277039	1736.609502	5.542195	-0.028941	2.276453
149.444503	1744.682536	5.547200	-0.028978	2.281573
149.763218	1752.723370	5.552205	-0.029042	2.286674
150.197430	1760.778556	5.557210	-0.029129	2.291782
150.345075	1768.874020	5.562214	-0.029161	2.296880
150.761401	1776.942231	5.567219	-0.029244	2.301972
151.096560	1785.023067	5.572224	-0.029312	2.307054
151.505533	1793.088504	5.577229	-0.029393	2.312121
151.633930	1801.185684	5.582234	-0.029423	2.317173
151.916887	1809.240661	5.587238	-0.029481	2.322201
152.236030	1817.323717	5.592243	-0.029545	2.327238
152.438001	1825.418086	5.597248	-0.029588	2.332262
152.682191	1833.482504	5.602253	-0.029639	2.337259
153.047504	1841.559488	5.607258	-0.029713	2.342264
153.187722	1849.639962	5.612262	-0.029744	2.347242
153.527639	1857.719923	5.617267	-0.029813	2.352225
153.905435	1865.774570	5.622272	-0.029888	2.357185
154.402151	1873.782701	5.627277	-0.029986	2.362116
154.623080	1881.876091	5.632282	-0.030033	2.367066
154.833337	1889.953595	5.637286	-0.030077	2.371995
155.358430	1897.997751	5.642291	-0.030180	2.376920
155.346086	1906.118369	5.647296	-0.030183	2.381836
155.594615	1914.181804	5.652301	-0.030235	2.386729
156.006269	1922.241296	5.657306	-0.030317	2.391623
156.113613	1930.327859	5.662310	-0.030342	2.396498
156.507880	1938.365913	5.667315	-0.030421	2.401357
156.819835	1946.433121	5.672320	-0.030484	2.406218
156.947171	1954.530339	5.677325	-0.030513	2.411071
157.257997	1962.601906	5.682330	-0.030576	2.415914
157.274217	1970.679111	5.687334	-0.030585	2.420728
157.660142	1978.716572	5.692339	-0.030662	2.425537
157.833177	1986.822281	5.697344	-0.030699	2.430361
158.053234	1994.899184	5.702349	-0.030746	2.435161
158.309883	2002.947933	5.707354	-0.030799	2.439939
158.496693	2010.972884	5.712358	-0.030839	2.444687
158.925658	2019.026386	5.717363	-0.030924	2.449462
159.222298	2027.083058	5.722368	-0.030985	2.454219
159.634892	2035.117088	5.727373	-0.031067	2.458962
159.796324	2043.191982	5.732378	-0.031102	2.463701
159.754810	2051.300669	5.737382	-0.031100	2.468435
160.457360	2059.295841	5.742387	-0.031236	2.473150
160.646723	2067.369460	5.747392	-0.031277	2.477863
160.875389	2075.404477	5.752397	-0.031324	2.482547
161.135980	2083.494855	5.757402	-0.031378	2.487257
161.475910	2091.537193	5.762406	-0.031447	2.491937
161.638082	2099.651320	5.767411	-0.031482	2.496635
161.884062	2107.705700	5.772416	-0.031534	2.501297
162.160439	2115.747154	5.777421	-0.031590	2.505944
162.443740	2123.838463	5.782426	-0.031648	2.510612
162.343483	2131.937747	5.787430	-0.031635	2.515247
162.804843	2139.950049	5.792435	-0.031726	2.519866
163.138420	2147.970057	5.797440	-0.031794	2.524471
163.279641	2156.033299	5.802445	-0.031825	2.529078
163.801249	2164.074165	5.807450	-0.031928	2.533692
164.048316	2172.140018	5.812454	-0.031979	2.538292
163.789811	2180.275929	5.817459	-0.031936	2.542886
164.371720	2188.255173	5.822464	-0.032050	2.547444
164.751275	2196.308721	5.827469	-0.032126	2.552021
164.870048	2204.400880	5.832474	-0.032153	2.556593
164.987228	2212.439255	5.837478	-0.032180	2.561126
165.190822	2220.500408	5.842483	-0.032224	2.565670
165.413501	2228.599186	5.847488	-0.032270	2.570229
165.841842	2236.595121	5.852493	-0.032355	2.574737
166.109426	2244.667378	5.857498	-0.032411	2.579267
166.571967	2252.667992	5.862502	-0.032502	2.583764
166.607695	2260.811414	5.867507	-0.032514	2.588302
166.823683	2268.943033	5.872512	-0.032560	2.592838
167.192659	2276.942798	5.877517	-0.032634	2.597304
167.098142	2285.030118	5.882522	-0.032621	2.601779
166.678553	2293.140805	5.887526	-0.032549	2.606236
167.686858	2301.040157	5.892531	-0.032742	2.610667
167.558737	2309.177526	5.897536	-0.032723	2.615144
167.849525	2317.146913	5.902541	-0.032782	2.619549
168.617206	2325.122679	5.907546	-0.032931	2.623984
169.013680	2333.155269	5.912550	-0.033010	2.628416
169.165784	2341.275460	5.917555	-0.033043	2.632872
169.091691	2349.351009	5.922560	-0.033035	2.637281
169.758692	2357.304268	5.927565	-0.033164	2.641666
170.320038	2365.346475	5.932570	-0.033274	2.646084
169.906773	2373.521588	5.937574	-0.033203	2.650502
170.490577	2381.520781	5.942579	-0.033317	2.654884
170.710502	2389.568037	5.947584	-0.033363	2.659261
170.808234	2397.627564	5.952589	-0.033386	2.663628
170.979106	2405.733619	5.957594	-0.033424	2.668019
171.220212	2413.769784	5.962598	-0.033474	2.672369
171.504614	2421.808668	5.967603	-0.033532	2.676716
171.955874	2429.824693	5.972608	-0.033621	2.681055
171.950654	2437.874799	5.977613	-0.033626	2.685376
172.635128	2445.873018	5.982618	-0.033758	2.689706
172.556329	2453.975708	5.987622	-0.033749	2.694036
172.526996	2462.084797	5.992627	-0.033749	2.698365
172.679174	2470.135071	5.997632	-0.033783	2.702668
172.591834	2478.196775	6.002637	-0.033772	2.706954
173.363374	2486.170262	6.007642	-0.033921	2.711242
173.101685	2494.283963	6.012646	-0.033877	2.715532
173.629056	2502.246223	6.017651	-0.033981	2.719784
173.933203	2510.265256	6.022656	-0.034043	2.724046
174.078483	2518.343926	6.027661	-0.034075	2.728323
174.620478	2526.387172	6.032666	-0.034181	2.732599
174.682867	2534.454509	6.037670	-0.034198	2.736851
175.035442	2542.465856	6.042675	-0.034269	2.741085
175.569592	2550.482407	6.047680	-0.034374	2.745326
175.830225	2558.553218	6.052685	-0.034428	2.749573
176.082018	2566.672347	6.057690	-0.034480	2.753837
176.020082	2574.739829	6.062694	-0.034474	2.758048
176.464380	2582.724232	6.067699	-0.034562	2.762241
176.683565	2590.765680	6.072704	-0.034608	2.766443
176.724834	2598.823102	6.077709	-0.034621	2.770637
176.838379	2606.926948	6.082714	-0.034647	2.774852
176.528375	2615.015972	6.087718	-0.034595	2.779027
177.231636	2622.931411	6.092723	-0.034731	2.783168
177.492547	2631.008904	6.097728	-0.034785	2.787360
177.842486	2639.009587	6.102733	-0.034856	2.791511
178.047478	2647.082997	6.107738	-0.034899	2.795684
178.212787	2655.113131	6.112742	-0.034935	2.799827
178.493244	2663.156417	6.117747	-0.034993	2.803977
178.745835	2671.219293	6.122752	-0.035045	2.808129
178.765782	2679.287156	6.127757	-0.035054	2.812264
178.896008	2687.370600	6.132762	-0.035084	2.816407
179.164956	2695.367387	6.137766	-0.035139	2.820508
179.605335	2703.356138	6.142771	-0.035226	2.824609
179.856856	2711.444198	6.147776	-0.035278	2.828744
179.673100	2719.537298	6.152781	-0.035249	2.832849
179.881811	2727.569802	6.157786	-0.035294	2.836941
180.373743	2735.537743	6.162790	-0.035391	2.841011
180.717710	2743.564592	6.167795	-0.035460	2.845095
180.663790	2751.662335	6.172800	-0.035455	2.849187
180.897347	2759.680670	6.177805	-0.035504	2.853249
181.331524	2767.731047	6.182810	-0.035590	2.857334
181.376862	2775.785990	6.187814	-0.035604	2.861392
181.650574	2783.814000	6.192819	-0.035660	2.865444
182.101264	2791.839660	6.197824	-0.035749	2.869499
182.027789	2799.903316	6.202829	-0.035741	2.873538
182.451647	2807.941354	6.207834	-0.035825	2.877586
182.439281	2816.000857	6.212838	-0.035828	2.881615
182.956771	2824.009390	6.217843	-0.035930	2.885642
182.824158	2832.097569	6.222848	-0.035910	2.889667
182.814546	2840.148625	6.227853	-0.035914	2.893675
183.203193	2848.194446	6.232858	-0.035992	2.897696
183.211196	2856.242691	6.237862	-0.035998	2.901693
183.372160	2864.264149	6.242867	-0.036034	2.905678
183.752834	2872.305011	6.247872	-0.036110	2.909681
183.873912	2880.382285	6.252877	-0.036138	2.913681
184.093617	2888.424965	6.257882	-0.036184	2.917664
184.257349	2896.415277	6.262886	-0.036220	2.921613
184.529510	2904.426052	6.267891	-0.036276	2.925572
184.839258	2912.457653	6.272896	-0.036339	2.929538
184.878822	2920.523150	6.277901	-0.036351	2.933501
185.185469	2928.565045	6.282906	-0.036414	2.937461
185.246017	2936.601029	6.287910	-0.036430	2.941400
185.030311	2944.683278	6.292915	-0.036396	2.945341
185.103047	2952.732465	6.297920	-0.036414	2.949276
185.358044	2960.744319	6.302925	-0.036467	2.953198
185.787444	2968.726107	6.307930	-0.036552	2.957109
186.109844	2976.761835	6.312934	-0.036618	2.961035
185.946685	2984.812398	6.317939	-0.036593	2.964938
186.376286	2992.834185	6.322944	-0.036678	2.968852
186.241409	3000.895791	6.327949	-0.036658	2.972751
186.625724	3008.966574	6.332954	-0.036735	2.976677
186.633120	3016.990057	6.337958	-0.036742	2.980555
186.843049	3025.015094	6.342963	-0.036786	2.984439
186.881962	3033.109308	6.347968	-0.036799	2.988342
187.216850	3041.095350	6.352973	-0.036866	2.992204
187.401381	3049.161315	6.357978	-0.036906	2.996091
187.219881	3057.208745	6.362982	-0.036877	2.999945
187.650009	3065.150877	6.367987	-0.036963	3.003776
188.028577	3073.213257	6.372992	-0.037039	3.007656
188.154941	3081.239967	6.377997	-0.037067	3.011502
188.310409	3089.334740	6.383002	-0.037102	3.015376
188.773781	3097.296006	6.388006	-0.037193	3.019197
188.633888	3105.376107	6.393011	-0.037173	3.023040
188.550259	3113.477544	6.398016	-0.037162	3.026891
188.786012	3121.493755	6.403021	-0.037212	3.030712
188.896324	3129.567000	6.408026	-0.037237	3.034549
188.631269	3137.605648	6.413030	-0.037193	3.038346
189.324454	3145.518001	6.418035	-0.037328	3.042127
189.470215	3153.575221	6.423040	-0.037360	3.045944
189.591059	3161.622084	6.428045	-0.037388	3.049750
189.809835	3169.679445	6.433050	-0.037434	3.053561
189.877843	3177.720922	6.438054	-0.037452	3.057352
189.975239	3185.797919	6.443059	-0.037475	3.061157
190.042254	3193.823689	6.448064	-0.037493	3.064932
190.228287	3201.849726	6.453069	-0.037533	3.068707
190.574696	3209.897158	6.458074	-0.037603	3.072496
190.662795	3217.950678	6.463078	-0.037625	3.076271
190.921080	3225.936478	6.468083	-0.037678	3.080017
191.399942	3233.884709	6.473088	-0.037772	3.083752
191.752044	3241.918795	6.478093	-0.037843	3.087516
191.931592	3249.989940	6.483098	-0.037882	3.091285
191.814912	3258.091921	6.488102	-0.037866	3.095049
191.819378	3266.114046	6.493107	-0.037872	3.098777
192.305595	3274.094082	6.498112	-0.037968	3.102504
192.412150	3282.144129	6.503117	-0.037993	3.106241
192.709322	3290.187290	6.508122	-0.038053	3.109980
192.679423	3298.240988	6.513126	-0.038053	3.113703
193.193044	3306.213540	6.518131	-0.038154	3.117410
193.650816	3314.266485	6.523136	-0.038245	3.121146
193.695525	3322.269226	6.528141	-0.038258	3.124836
193.976834	3330.323514	6.533146	-0.038316	3.128556
194.023099	3338.398202	6.538150	-0.038330	3.132271
194.297760	3346.450800	6.543155	-0.038386	3.135981
194.332703	3354.507742	6.548160	-0.038398	3.139678
194.851829	3362.452961	6.553165	-0.038500	3.143341
194.530177	3370.602671	6.558170	-0.038445	3.147055
194.542908	3378.677379	6.563174	-0.038453	3.150746
194.622818	3386.652944	6.568179	-0.038473	3.154390
195.247916	3394.620840	6.573184	-0.038595	3.158051
195.362980	3402.634945	6.578189	-0.038622	3.161706
195.421442	3410.712724	6.583194	-0.038638	3.165384
195.531199	3418.746074	6.588198	-0.038664	3.169038
195.636355	3426.769250	6.593203	-0.038688	3.172684
196.007342	3434.808064	6.598208	-0.038763	3.176345
196.015751	3442.815212	6.603213	-0.038770	3.179971
196.361885	3450.825496	6.608218	-0.038839	3.183609
196.071976	3458.966525	6.613222	-0.038791	3.187274
195.957929	3467.001392	6.618227	-0.038775	3.190894
196.155525	3475.009566	6.623232	-0.038817	3.194512
196.509835	3482.966656	6.628237	-0.038888	3.198110
196.182795	3491.087619	6.633242	-0.038833	3.201748
196.828465	3499.023750	6.638246	-0.038958	3.205341
196.629454	3507.111644	6.643251	-0.038926	3.208961
197.065151	3515.128123	6.648256	-0.039013	3.212573
197.246092	3523.134298	6.653261	-0.039052	3.216164
197.741611	3531.162750	6.658266	-0.039149	3.219776
197.857591	3539.169549	6.663270	-0.039176	3.223357
198.098193	3547.200055	6.668275	-0.039226	3.226950
198.604979	3555.246583	6.673280	-0.039326	3.230558
198.699877	3563.269854	6.678285	-0.039349	3.234133
198.932884	3571.299524	6.683290	-0.039398	3.237713
199.291873	3579.312239	6.688294	-0.039470	3.241288
199.790100	3587.266647	6.693299	-0.039568	3.244838
199.871358	3595.351000	6.698304	-0.039588	3.248424
200.017663	3603.406475	6.703309	-0.039621	3.251996
200.194915	3611.489888	6.708314	-0.039659	3.255578
200.139550	3619.558782	6.713318	-0.039654	3.259140
200.181634	3627.562970	6.718323	-0.039667	3.262673
200.520318	3635.587232	6.723328	-0.039736	3.266224
200.771849	3643.590183	6.728333	-0.039788	3.269758
200.597161	3651.689729	6.733338	-0.039761	3.273313
200.913114	3659.666582	6.738342	-0.039825	3.276830
201.349396	3667.658142	6.743347	-0.039911	3.280355
201.817377	3675.634934	6.748352	-0.040004	3.283870
201.593785	3683.736151	6.753357	-0.039967	3.287409
201.689123	3691.869586	6.758362	-0.039990	3.290970
201.937798	3699.809122	6.763366	-0.040042	3.294450
201.881919	3707.856559	6.768371	-0.040037	3.297960
202.654284	3715.841363	6.773376	-0.040186	3.301472
202.752543	3723.851177	6.778381	-0.040210	3.304965
202.806692	3731.930238	6.783386	-0.040225	3.308482
202.865673	3740.013181	6.788390	-0.040241	3.311997
202.931465	3748.055209	6.793395	-0.040259	3.315492
203.162995	3756.057685	6.798400	-0.040307	3.318971
203.078481	3764.056738	6.803405	-0.040297	3.322434
203.558424	3772.058896	6.808410	-0.040391	3.325916
203.734682	3780.067261	6.813414	-0.040429	3.329385
203.699540	3788.136960	6.818419	-0.040428	3.332869
204.126665	3796.184724	6.823424	-0.040513	3.336357
204.268066	3804.159286	6.828429	-0.040545	3.339800
204.009516	3812.270534	6.833434	-0.040502	3.343282
204.435395	3820.255395	6.838438	-0.040586	3.346732
204.652670	3828.299868	6.843443	-0.040632	3.350197
205.216239	3836.268375	6.848448	-0.040742	3.353638
204.670846	3844.371371	6.853453	-0.040646	3.357092
204.518588	3852.458868	6.858458	-0.040623	3.360550
205.419820	3860.320680	6.863462	-0.040796	3.363948
205.674531	3868.369450	6.868467	-0.040849	3.367397
205.961016	3876.449436	6.873472	-0.040908	3.370858
205.931579	3884.476030	6.878477	-0.040907	3.374281
206.035002	3892.499961	6.883482	-0.040932	3.377704
206.285860	3900.549396	6.888486	-0.040984	3.381140
206.579462	3908.519713	6.893491	-0.041044	3.384540
206.733672	3916.588157	6.898496	-0.041078	3.387973
207.054895	3924.612217	6.903501	-0.041143	3.391390
207.130538	3932.714248	6.908506	-0.041163	3.394828
207.063546	3940.755628	6.913510	-0.041155	3.398231
207.026422	3948.755244	6.918515	-0.041154	3.401614
207.371115	3956.735418	6.923520	-0.041223	3.405000
207.652689	3964.743871	6.928525	-0.041281	3.408391
207.839979	3972.826204	6.933530	-0.041321	3.411808
207.845844	3980.856499	6.938534	-0.041327	3.415192
208.087653	3988.834020	6.943539	-0.041378	3.418559
208.670348	3996.854655	6.948544	-0.041492	3.421953
208.817241	4004.835446	6.953549	-0.041524	3.425311
209.014315	4012.925607	6.958554	-0.041566	3.428714
209.000808	4021.015467	6.963558	-0.041569	3.432106
209.115893	4029.023548	6.968563	-0.041596	3.435464
209.411750	4036.985649	6.973568	-0.041656	3.438807
209.638913	4045.019629	6.978573	-0.041704	3.442173
209.790530	4053.080569	6.983578	-0.041737	3.445545
209.874961	4061.096656	6.988582	-0.041758	3.448893
209.817090	4069.178036	6.993587	-0.041753	3.452260
210.147697	4077.174532	6.998592	-0.041820	3.455601
209.942791	4085.191405	7.003597	-0.041787	3.458930
210.652220	4093.167251	7.008602	-0.041924	3.462269
210.825120	4101.243915	7.013606	-0.041962	3.465629
210.802607	4109.260871	7.018611	-0.041963	3.468954
211.189060	4117.293678	7.023616	-0.042040	3.472296
211.434496	4125.286264	7.028621	-0.042091	3.475613
211.785107	4133.271292	7.033626	-0.042162	3.478928
211.984552	4141.316384	7.038630	-0.042204	3.482259
212.407645	4149.314932	7.043635	-0.042288	3.485575
212.712236	4157.356582	7.048640	-0.042350	3.488902
212.741835	4165.406136	7.053645	-0.042361	3.492220
212.537565	4173.544303	7.058650	-0.042328	3.495563
212.953969	4181.478087	7.063654	-0.042411	3.498840
213.141878	4189.518288	7.068659	-0.042451	3.502149
213.134723	4197.555816	7.073664	-0.042455	3.505448
213.294885	4205.604415	7.078669	-0.042490	3.508754
213.336150	4213.677710	7.083674	-0.042503	3.512063
213.431350	4221.671215	7.088678	-0.042526	3.515338
213.966056	4229.588765	7.093683	-0.042631	3.518593
214.066644	4237.681759	7.098688	-0.042655	3.521903
214.305276	4245.661419	7.103693	-0.042705	3.525167
214.182135	4253.767992	7.108698	-0.042687	3.528469
214.597265	4261.755080	7.113702	-0.042770	3.531737
214.953443	4269.773528	7.118707	-0.042842	3.535011
215.270981	4277.798738	7.123712	-0.042906	3.538285
215.394998	4285.837269	7.128717	-0.042934	3.541555
215.285156	4293.872084	7.133722	-0.042919	3.544812
215.286337	4301.915720	7.138726	-0.042925	3.548074
215.401155	4309.985031	7.143731	-0.042951	3.551347
215.859972	4318.005425	7.148736	-0.043042	3.554608
216.094943	4325.967844	7.153741	-0.043091	3.557835
216.245137	4334.005136	7.158746	-0.043124	3.561087
216.246876	4342.001543	7.163750	-0.043130	3.564315
216.446687	4350.009565	7.168755	-0.043172	3.567550
216.611196	4358.058630	7.173760	-0.043208	3.570798
216.724477	4366.073189	7.178765	-0.043235	3.574028
216.740257	4374.122578	7.183770	-0.043243	3.577266
217.160583	4382.106968	7.188774	-0.043327	3.580487
217.260706	4390.100907	7.193779	-0.043351	3.583699
217.789803	4398.146392	7.198784	-0.043454	3.586942
217.787489	4406.185936	7.203789	-0.043459	3.590164
217.859963	4414.249783	7.208794	-0.043478	3.593394
217.991376	4422.271277	7.213798	-0.043508	3.596607
218.098917	4430.256442	7.218803	-0.043533	3.599801
218.487068	4438.286768	7.223808	-0.043611	3.603019
218.527894	4446.320987	7.228813	-0.043624	3.606225
218.775819	4454.355055	7.233818	-0.043675	3.609435
218.953611	4462.388966	7.238822	-0.043713	3.612639
218.976492	4470.430389	7.243827	-0.043723	3.615839
219.427706	4478.414840	7.248832	-0.043812	3.619026
219.557412	4486.444774	7.253837	-0.043842	3.622219
219.428530	4494.537536	7.258842	-0.043823	3.625427
219.721039	4502.528269	7.263846	-0.043883	3.628603
219.540155	4510.598009	7.268851	-0.043854	3.631794
219.938839	4518.620611	7.273856	-0.043934	3.634981
220.363766	4526.525338	7.278861	-0.044018	3.638118
220.809290	4534.563696	7.283866	-0.044107	3.641306
220.752278	4542.579350	7.288870	-0.044101	3.644469
220.782060	4550.640146	7.293875	-0.044112	3.647648
221.131731	4558.698860	7.298880	-0.044183	3.650833
221.199407	4566.674375	7.303885	-0.044200	3.653975
221.523005	4574.719796	7.308890	-0.044266	3.657149
221.741029	4582.733663	7.313894	-0.044312	3.660304
221.777925	4590.730622	7.318899	-0.044324	3.663445
221.927878	4598.814162	7.323904	-0.044357	3.666620
221.944698	4606.820810	7.328909	-0.044366	3.669759
222.274616	4614.826978	7.333914	-0.044432	3.672904
222.337587	4622.904113	7.338918	-0.044449	3.676066
222.602694	4630.819321	7.343923	-0.044504	3.679168
222.837098	4638.884167	7.348928	-0.044553	3.682324
223.008716	4646.877924	7.353933	-0.044590	3.685449
222.715410	4654.979207	7.358938	-0.044541	3.688600
223.250153	4662.983561	7.363942	-0.044646	3.691733
223.107980	4671.033745	7.368947	-0.044625	3.694863
223.485049	4679.041861	7.373952	-0.044700	3.697988
223.306996	4687.118547	7.378957	-0.044672	3.701122
223.569335	4695.061333	7.383962	-0.044726	3.704213
223.767562	4703.155260	7.388966	-0.044769	3.707359
223.610755	4711.209844	7.393971	-0.044745	3.710477
223.650147	4719.264486	7.398976	-0.044757	3.713598
223.949247	4727.243259	7.403981	-0.044818	3.716693
224.236916	4735.202119	7.408986	-0.044877	3.719778
224.135696	4743.220957	7.413990	-0.044864	3.722874
224.526218	4751.202639	7.418995	-0.044942	3.725965
225.117999	4759.190838	7.424000	-0.045057	3.729061
224.964582	4767.287533	7.429005	-0.045034	3.732177
225.282297	4775.321983	7.434010	-0.045098	3.735279
225.393882	4783.364530	7.439014	-0.045124	3.738376
225.443560	4791.369893	7.444019	-0.045139	3.741455
225.975640	4799.348968	7.449024	-0.045243	3.744533
225.877455	4807.406527	7.454029	-0.045230	3.747622
226.083938	4815.454319	7.459034	-0.045274	3.750713
226.217113	4823.466279	7.464038	-0.045304	3.753786
226.449768	4831.446678	7.469043	-0.045353	3.756847
226.801960	4839.458721	7.474048	-0.045424	3.759921
226.692497	4847.482365	7.479053	-0.045408	3.762985
226.682783	4855.562607	7.484058	-0.045412	3.766070
226.991757	4863.557277	7.489062	-0.045475	3.769128
227.205659	4871.566220	7.494067	-0.045520	3.772187
227.219868	4879.637779	7.499072	-0.045528	3.775262
227.545704	4887.620081	7.504077	-0.045594	3.778308
227.685533	4895.646882	7.509082	-0.045625	3.781364
227.780882	4903.657539	7.514086	-0.045648	3.784410
228.170946	4911.672843	7.519091	-0.045726	3.787463
228.155993	4919.760211	7.524096	-0.045729	3.790531
228.488869	4927.707430	7.529101	-0.045796	3.793552
228.551680	4935.747841	7.534106	-0.045813	3.796599
228.668416	4943.785662	7.539110	-0.045840	3.799644
229.138197	4951.742330	7.544115	-0.045933	3.802664
229.374911	4959.813142	7.549120	-0.045982	3.805719
229.399028	4967.808339	7.554125	-0.045992	3.808738
229.744599	4975.863282	7.559130	-0.046062	3.811785
229.557242	4983.911431	7.564134	-0.046032	3.814814
229.984248	4991.873378	7.569139	-0.046117	3.817823
230.062959	5000.019533	7.574144	-0.046137	3.820891
230.024088	5007.941779	7.579149	-0.046135	3.823869
230.446791	5016.003099	7.584154	-0.046219	3.826908
230.675365	5023.996871	7.589158	-0.046267	3.829914
230.794700	5032.033468	7.594163	-0.046294	3.832932
230.990383	5040.105279	7.599168	-0.046336	3.835962
231.186937	5048.018419	7.604173	-0.046378	3.838931
231.433880	5056.093371	7.609178	-0.046429	3.841958
231.376978	5064.129924	7.614182	-0.046424	3.844963
231.570027	5072.131446	7.619187	-0.046465	3.847957
231.733994	5080.222950	7.624192	-0.046501	3.850982
231.787584	5088.173254	7.629197	-0.046516	3.853949
232.139921	5096.218888	7.634202	-0.046587	3.856956
232.312278	5104.263695	7.639206	-0.046624	3.859957
232.386652	5112.241583	7.644211	-0.046643	3.862928
232.351863	5120.330126	7.649216	-0.046642	3.865936
232.518967	5128.273981	7.654221	-0.046679	3.868892
232.789174	5136.401487	7.659226	-0.046734	3.871916
232.803361	5144.471655	7.664230	-0.046742	3.874911
232.970954	5152.410573	7.669235	-0.046779	3.877858
233.278209	5160.387395	7.674240	-0.046841	3.880820
233.312974	5168.349405	7.679245	-0.046853	3.883768
233.546519	5176.389997	7.684250	-0.046902	3.886748
233.847467	5184.424676	7.689254	-0.046963	3.889724
233.994314	5192.407371	7.694259	-0.046996	3.892675
234.141109	5200.487588	7.699264	-0.047028	3.895661
234.300444	5208.442969	7.704269	-0.047063	3.898598
234.587967	5216.503348	7.709274	-0.047122	3.901574
234.707351	5224.488429	7.714278	-0.047150	3.904517
234.680994	5232.555416	7.719283	-0.047150	3.907485
234.802961	5240.595867	7.724288	-0.047178	3.910443
235.306281	5248.536036	7.729293	-0.047277	3.913370
235.490079	5256.628009	7.734298	-0.047317	3.916345
235.607194	5264.587611	7.739302	-0.047344	3.919267
235.375847	5272.666379	7.744307	-0.047306	3.922224
235.820741	5280.607763	7.749312	-0.047394	3.925141
236.142358	5288.635166	7.754317	-0.047459	3.928086
236.210847	5296.729919	7.759322	-0.047477	3.931048
235.871974	5304.803522	7.764326	-0.047419	3.933992
236.148403	5312.792645	7.769331	-0.047476	3.936914
236.784894	5320.761335	7.774336	-0.047600	3.939834
237.005659	5328.792950	7.779341	-0.047646	3.942767
237.029430	5336.804852	7.784346	-0.047656	3.945687
237.371710	5344.856878	7.789350	-0.047725	3.948625
237.510071	5352.906654	7.794355	-0.047756	3.951556
237.557654	5360.919014	7.799360	-0.047770	3.954470
237.474047	5368.943146	7.804365	-0.047760	3.957384
237.704117	5376.951197	7.809370	-0.047808	3.960295
237.475780	5384.985874	7.814374	-0.047771	3.963205
237.766313	5392.957113	7.819379	-0.047830	3.966100
238.287017	5400.983100	7.824384	-0.047933	3.969016
238.008465	5409.068167	7.829389	-0.047886	3.971938
238.267785	5417.064904	7.834394	-0.047940	3.974835
238.537400	5425.047205	7.839398	-0.047995	3.977724
238.228172	5433.131520	7.844403	-0.047943	3.980638
238.467677	5441.093343	7.849408	-0.047993	3.983516
238.731578	5449.098806	7.854413	-0.048047	3.986408
239.107544	5457.115123	7.859418	-0.048122	3.989303
238.952006	5465.218819	7.864422	-0.048099	3.992218
239.383683	5473.148879	7.869427	-0.048184	3.995079
239.778781	5481.177781	7.874432	-0.048263	3.997973
239.791102	5489.227612	7.879437	-0.048271	4.000866
239.855497	5497.212068	7.884442	-0.048288	4.003733
239.822278	5505.286155	7.889446	-0.048287	4.006630
240.026904	5513.243273	7.894451	-0.048331	4.009486
239.876489	5521.335415	7.899456	-0.048308	4.012383
240.052316	5529.324629	7.904461	-0.048346	4.015246
240.210026	5537.332700	7.909466	-0.048381	4.018113
240.748434	5545.360219	7.914470	-0.048486	4.020992
240.742799	5553.308023	7.919475	-0.048490	4.023831
240.792903	5561.423336	7.924480	-0.048505	4.026729
240.739016	5569.399614	7.929485	-0.048500	4.029574
241.009341	5577.470867	7.934490	-0.048556	4.032455
241.406295	5585.515918	7.939494	-0.048635	4.035327
241.262717	5593.503773	7.944499	-0.048614	4.038168
241.655622	5601.522899	7.949504	-0.048692	4.041027
241.777413	5609.456450	7.954509	-0.048720	4.043849
241.661113	5617.539959	7.959514	-0.048704	4.046719
241.797037	5625.559793	7.964518	-0.048734	4.049568
241.932910	5633.549241	7.969523	-0.048765	4.052404
242.041405	5641.591383	7.974528	-0.048790	4.055256
242.356794	5649.601878	7.979533	-0.048854	4.058098
242.463899	5657.652003	7.984538	-0.048880	4.060949
242.609855	5665.612540	7.989542	-0.048912	4.063767
242.879797	5673.651017	7.994547	-0.048968	4.066612
243.018067	5681.681512	7.999552	-0.048999	4.069451
242.926926	5689.755029	8.004557	-0.048987	4.072299
243.318905	5697.709772	8.009562	-0.049065	4.075111
243.614690	5705.767341	8.014566	-0.049126	4.077955
243.604886	5713.768333	8.019571	-0.049129	4.080773
243.793608	5721.770866	8.024576	-0.049170	4.083593
244.035832	5729.831806	8.029581	-0.049220	4.086431
244.118646	5737.823420	8.034586	-0.049241	4.089242
244.285056	5745.928219	8.039590	-0.049277	4.092091
244.340158	5753.880552	8.044595	-0.049293	4.094883
244.698594	5761.920140	8.049600	-0.049365	4.097708
244.680644	5769.928406	8.054605	-0.049367	4.100515
244.614911	5777.928073	8.059610	-0.049360	4.103316
245.028786	5785.996546	8.064614	-0.049442	4.106146
244.940524	5793.988530	8.069619	-0.049431	4.108940
245.302141	5802.040068	8.074624	-0.049503	4.111759
245.536246	5809.987989	8.079629	-0.049552	4.114539
245.795342	5818.003909	8.084634	-0.049606	4.117341
245.867037	5826.043632	8.089638	-0.049624	4.120146
246.039677	5834.014978	8.094643	-0.049662	4.122927
246.281976	5842.076892	8.099648	-0.049712	4.125739
246.346191	5850.090415	8.104653	-0.049730	4.128529
246.430329	5858.145421	8.109658	-0.049751	4.131332
246.757278	5866.131799	8.114662	-0.049817	4.134113
246.709917	5874.144500	8.119667	-0.049813	4.136896
246.814745	5882.208890	8.124672	-0.049838	4.139697
246.885368	5890.195487	8.129677	-0.049856	4.142469
246.961466	5898.197169	8.134682	-0.049876	4.145244
247.232790	5906.237401	8.139686	-0.049932	4.148033
247.259598	5914.250010	8.144691	-0.049942	4.150808
247.412139	5922.275005	8.149696	-0.049976	4.153586
247.673028	5930.265263	8.154701	-0.050029	4.156352
247.803117	5938.223345	8.159706	-0.050059	4.159104
247.970700	5946.344553	8.164710	-0.050096	4.161910
247.869694	5954.287526	8.169715	-0.050082	4.164650
247.826155	5962.398420	8.174720	-0.050079	4.167446
248.113400	5970.388510	8.179725	-0.050138	4.170203
248.293844	5978.390605	8.184730	-0.050177	4.172961
248.281555	5986.473083	8.189734	-0.050180	4.175743
248.366276	5994.384032	8.194739	-0.050201	4.178464
248.794420	6002.492390	8.199744	-0.050286	4.181256
248.761351	6010.449030	8.204749	-0.050285	4.183989
248.746691	6018.527592	8.209754	-0.050288	4.186761
249.076090	6026.592162	8.214758	-0.050354	4.189532
249.066380	6034.573817	8.219763	-0.050358	4.192267
249.210817	6042.646514	8.224768	-0.050390	4.195034
249.415626	6050.611226	8.229773	-0.050433	4.197763
249.565068	6058.601368	8.234778	-0.050466	4.200499
249.682016	6066.578711	8.239782	-0.050493	4.203227
250.004331	6074.586325	8.244787	-0.050559	4.205967
249.903311	6082.645583	8.249792	-0.050545	4.208717
250.417760	6090.654673	8.254797	-0.050646	4.211456
250.574471	6098.626160	8.259802	-0.050681	4.214176
250.810868	6106.727622	8.264806	-0.050730	4.216939
250.870741	6114.709170	8.269811	-0.050747	4.219658
251.071343	6122.730752	8.274816	-0.050789	4.222390
251.262295	6130.724875	8.279821	-0.050830	4.225111
251.154756	6138.782591	8.284826	-0.050815	4.227848
251.256063	6146.842457	8.289830	-0.050840	4.230587
251.288575	6154.826986	8.294835	-0.050851	4.233297
251.760090	6162.849665	8.299840	-0.050944	4.236024
251.933987	6170.798665	8.304845	-0.050982	4.238720
252.076232	6178.876407	8.309850	-0.051013	4.241458
252.465583	6186.841035	8.314854	-0.051091	4.244159
252.371031	6194.893276	8.319859	-0.051079	4.246882
252.439680	6202.965028	8.324864	-0.051097	4.249612
252.941526	6210.952042	8.329869	-0.051196	4.252316
253.195300	6218.931546	8.334874	-0.051248	4.255013
252.981767	6227.025656	8.339878	-0.051214	4.257742
253.159613	6234.991826	8.344883	-0.051252	4.260430
253.316461	6242.998945	8.349888	-0.051287	4.263131
253.503551	6251.018662	8.354893	-0.051327	4.265834
253.343920	6259.041689	8.359898	-0.051302	4.268533
253.704584	6267.111162	8.364902	-0.051375	4.271251
253.730020	6275.096260	8.369907	-0.051385	4.273935
253.853358	6283.104024	8.374912	-0.051413	4.276627
254.026319	6291.073612	8.379917	-0.051451	4.279304
254.316293	6299.084962	8.384922	-0.051510	4.281995
254.358306	6307.116865	8.389926	-0.051523	4.284689
254.618706	6315.127216	8.394931	-0.051577	4.287375
254.817394	6323.141629	8.399936	-0.051619	4.290061
254.900129	6331.185822	8.404941	-0.051640	4.292754
255.087518	6339.247172	8.409946	-0.051680	4.295452
255.272600	6347.249271	8.414950	-0.051720	4.298129
255.309266	6355.281962	8.419955	-0.051732	4.300813
255.354698	6363.197849	8.424960	-0.051745	4.303456
255.541849	6371.297371	8.429965	-0.051786	4.306160
255.668062	6379.254759	8.434970	-0.051814	4.308814
255.777820	6387.355315	8.439974	-0.051840	4.311514
255.954996	6395.228542	8.444979	-0.051878	4.314138
256.084797	6403.373429	8.449984	-0.051908	4.316849
256.099611	6411.339601	8.454989	-0.051916	4.319499
256.005156	6419.371719	8.459994	-0.051904	4.322168
256.329856	6427.364307	8.464998	-0.051969	4.324826
256.362285	6435.417275	8.470003	-0.051981	4.327499
256.553517	6443.421394	8.475008	-0.052022	4.330157
256.623421	6451.448587	8.480013	-0.052040	4.332819
256.811658	6459.432609	8.485018	-0.052080	4.335466
257.089233	6467.468456	8.490022	-0.052137	4.338129
257.169831	6475.479207	8.495027	-0.052158	4.340781
257.345995	6483.499216	8.500032	-0.052196	4.343435
257.420365	6491.560642	8.505037	-0.052215	4.346100
257.346433	6499.515217	8.510042	-0.052206	4.348728
257.712081	6507.597676	8.515046	-0.052280	4.351399
257.919224	6515.599013	8.520051	-0.052324	4.354040
257.989449	6523.632128	8.525056	-0.052342	4.356690
258.098335	6531.592523	8.530061	-0.052367	4.359314
258.187630	6539.603726	8.535066	-0.052389	4.361953
258.342039	6547.611722	8.540070	-0.052423	4.364589
258.381761	6555.631927	8.545075	-0.052436	4.367228
258.652777	6563.648110	8.550080	-0.052492	4.369865
258.653502	6571.724584	8.555085	-0.052497	4.372518
258.729812	6579.688296	8.560090	-0.052517	4.375134
259.024816	6587.744439	8.565095	-0.052577	4.377779
259.241374	6595.675830	8.570099	-0.052623	4.380382
259.424922	6603.727072	8.575104	-0.052662	4.383022
259.479218	6611.707763	8.580109	-0.052677	4.385636
259.609131	6619.783270	8.585114	-0.052707	4.388280
259.906926	6627.880318	8.590119	-0.052768	4.390931
259.466399	6635.857900	8.595123	-0.052691	4.393537
259.812682	6643.889238	8.600128	-0.052761	4.396163
260.116545	6651.846995	8.605133	-0.052823	4.398764
260.023820	6659.923616	8.610138	-0.052811	4.401399
259.822544	6667.943971	8.615143	-0.052778	4.404014
260.374995	6675.919023	8.620147	-0.052887	4.406617
260.707207	6683.898434	8.625152	-0.052954	4.409218
260.770060	6692.001937	8.630157	-0.052971	4.411857
260.532835	6699.971018	8.635162	-0.052932	4.414449
261.046541	6707.990323	8.640167	-0.053033	4.417060
261.228918	6715.941865	8.645171	-0.053072	4.419645
261.350648	6724.042504	8.650176	-0.053100	4.422277
261.345586	6732.073335	8.655181	-0.053104	4.424884
261.270149	6740.165989	8.660186	-0.053096	4.427509
261.612011	6748.195419	8.665191	-0.053165	4.430114
261.418363	6756.199500	8.670195	-0.053134	4.432707
261.732651	6764.210087	8.675200	-0.053198	4.435303
262.045821	6772.181135	8.680205	-0.053261	4.437884
262.366473	6780.214759	8.685210	-0.053326	4.440484
262.450387	6788.229137	8.690215	-0.053347	4.443076
262.551682	6796.232484	8.695219	-0.053371	4.445662
262.682920	6804.243924	8.700224	-0.053401	4.448249
262.692394	6812.373326	8.705229	-0.053408	4.450873
262.695986	6820.282014	8.710234	-0.053414	4.453424
262.596091	6828.379005	8.715239	-0.053401	4.456033
262.947528	6836.322525	8.720243	-0.053471	4.458594
262.996753	6844.434435	8.725248	-0.053486	4.461205
263.368972	6852.316252	8.730253	-0.053560	4.463743
263.350387	6860.400785	8.735258	-0.053562	4.466343
264.087355	6868.382778	8.740263	-0.053705	4.468912
264.166481	6876.454997	8.745267	-0.053725	4.471505
264.129918	6884.421712	8.750272	-0.053723	4.474062
264.359808	6892.466134	8.755277	-0.053771	4.476644
264.612042	6900.399089	8.760282	-0.053824	4.479189
264.720251	6908.530610	8.765287	-0.053849	4.481795
264.659146	6916.442974	8.770291	-0.053843	4.484329
264.930989	6924.544653	8.775296	-0.053899	4.486923
265.080522	6932.516067	8.780301	-0.053932	4.489474
265.195482	6940.582389	8.785306	-0.053959	4.492053
265.369909	6948.582279	8.790311	-0.053997	4.494610
265.361413	6956.598864	8.795315	-0.054000	4.497170
265.372689	6964.595317	8.800320	-0.054008	4.499723
265.711149	6972.638378	8.805325	-0.054076	4.502289
265.838860	6980.594639	8.810330	-0.054105	4.504826
265.914114	6988.717781	8.815335	-0.054124	4.507415
266.080419	6996.650403	8.820339	-0.054161	4.509941
266.307673	7004.677132	8.825344	-0.054208	4.512497
266.503934	7012.636198	8.830349	-0.054250	4.515029
266.560175	7020.675026	8.835354	-0.054266	4.517585
266.548245	7028.722118	8.840359	-0.054269	4.520141
266.731105	7036.670415	8.845363	-0.054308	4.522666
266.797566	7044.715953	8.850368	-0.054326	4.525219
266.692688	7052.784548	8.855373	-0.054312	4.527778
266.928831	7060.771525	8.860378	-0.054361	4.530311
267.166399	7068.815300	8.865383	-0.054410	4.532860
267.361934	7076.809862	8.870387	-0.054452	4.535392
267.328920	7084.818027	8.875392	-0.054451	4.537926
267.462883	7092.851840	8.880397	-0.054481	4.540467
267.426854	7100.830490	8.885402	-0.054480	4.542989
267.749293	7108.877632	8.890407	-0.054545	4.545532
267.974127	7116.847176	8.895411	-0.054592	4.548049
268.126397	7124.904967	8.900416	-0.054626	4.550592
268.333962	7132.875784	8.905421	-0.054670	4.553107
268.354270	7140.963558	8.910426	-0.054679	4.555656
268.485838	7148.933082	8.915431	-0.054709	4.558167
268.435742	7156.993742	8.920435	-0.054705	4.560705
268.599053	7164.951110	8.925440	-0.054741	4.563210
268.469492	7173.028233	8.930445	-0.054722	4.565750
268.715415	7180.982984	8.935450	-0.054773	4.568251
268.700810	7189.098056	8.940455	-0.054775	4.570800
268.762834	7197.049066	8.945459	-0.054792	4.573297
269.102590	7205.051422	8.950464	-0.054861	4.575809
269.022171	7213.048003	8.955469	-0.054851	4.578317
269.099636	7221.085844	8.960474	-0.054871	4.580837
269.267293	7229.073793	8.965479	-0.054907	4.583339
269.573493	7237.127229	8.970483	-0.054970	4.585862
269.784929	7245.174770	8.975488	-0.055014	4.588381
270.206648	7253.172796	8.980493	-0.055098	4.590883
270.057546	7261.174270	8.985498	-0.055076	4.593384
270.057687	7269.208310	8.990503	-0.055081	4.595894
270.003379	7277.185001	8.995507	-0.055076	4.598385
270.140103	7285.223177	9.000512	-0.055107	4.600894
270.269030	7293.213776	9.005517	-0.055136	4.603386
270.520210	7301.223285	9.010522	-0.055188	4.605883
270.589399	7309.237962	9.015527	-0.055206	4.608381
270.629512	7317.229051	9.020531	-0.055219	4.610869
270.945483	7325.282703	9.025536	-0.055283	4.613376
270.935029	7333.334932	9.030541	-0.055287	4.615881
270.403529	7341.345971	9.035546	-0.055193	4.618371
270.950637	7349.357944	9.040551	-0.055300	4.620861
270.973788	7357.292448	9.045555	-0.055310	4.623325
271.232995	7365.314101	9.050560	-0.055363	4.625816
271.614352	7373.384187	9.055565	-0.055440	4.628319
271.872526	7381.386552	9.060570	-0.055493	4.630801
271.920145	7389.388696	9.065575	-0.055507	4.633281
271.910347	7397.440628	9.070579	-0.055511	4.635774
271.867994	7405.422300	9.075584	-0.055508	4.638245
271.932737	7413.464594	9.080589	-0.055525	4.640733
272.290863	7421.353339	9.085594	-0.055597	4.643173
272.373711	7429.492194	9.090599	-0.055618	4.645688
272.465841	7437.464636	9.095603	-0.055640	4.648151
272.732711	7445.527221	9.100608	-0.055695	4.650640
272.685190	7453.518466	9.105613	-0.055692	4.653106
272.785963	7461.536183	9.110618	-0.055716	4.655579
273.051292	7469.537939	9.115623	-0.055771	4.658045
273.066840	7477.593680	9.120627	-0.055779	4.660527
273.346622	7485.545298	9.125632	-0.055836	4.662975
273.527409	7493.606694	9.130637	-0.055875	4.665456
273.650657	7501.588145	9.135642	-0.055903	4.667910
273.833622	7509.678543	9.140647	-0.055943	4.670397
274.118576	7517.709415	9.145651	-0.056001	4.672865
274.150855	7525.700586	9.150656	-0.056012	4.675319
273.984226	7533.672270	9.155661	-0.055987	4.677765
274.384560	7541.634791	9.160666	-0.056066	4.680208
274.547696	7549.702020	9.165671	-0.056102	4.682681
274.603875	7557.683678	9.170675	-0.056118	4.685127
274.803774	7565.763675	9.175680	-0.056160	4.687601
274.620474	7573.805243	9.180685	-0.056132	4.690063
274.488398	7581.777619	9.185690	-0.056112	4.692502
274.569138	7589.875221	9.190695	-0.056133	4.694978
274.645475	7597.801377	9.195699	-0.056152	4.697401
274.617796	7605.789593	9.200704	-0.056152	4.699841
275.102626	7613.810327	9.205709	-0.056248	4.702289
275.191901	7621.789983	9.210714	-0.056270	4.704724
275.559729	7629.878307	9.215719	-0.056343	4.707190
275.521065	7637.876150	9.220723	-0.056341	4.709628
275.675063	7645.911748	9.225728	-0.056375	4.712076
275.837188	7653.885994	9.230733	-0.056411	4.714504
275.916453	7661.940993	9.235738	-0.056431	4.716956
276.179220	7669.903579	9.240743	-0.056485	4.719377
276.378661	7677.979951	9.245747	-0.056528	4.721832
276.579757	7685.912633	9.250752	-0.056570	4.724243
276.397933	7694.048909	9.255757	-0.056542	4.726714
276.274348	7701.975728	9.260762	-0.056524	4.729120
276.741140	7710.090093	9.265767	-0.056616	4.731582
276.729895	7718.016518	9.270771	-0.056619	4.733985
276.665216	7726.104287	9.275776	-0.056613	4.736437
277.119009	7734.077896	9.280781	-0.056702	4.738851
277.027986	7742.132620	9.285786	-0.056691	4.741290
277.247196	7750.069733	9.290791	-0.056737	4.743691
277.480175	7758.099847	9.295795	-0.056786	4.746120
277.480966	7766.112882	9.300800	-0.056791	4.748542
277.517534	7774.240869	9.305805	-0.056803	4.750998
277.460764	7782.187280	9.310810	-0.056798	4.753398
277.801350	7790.236988	9.315815	-0.056867	4.755827
277.942611	7798.206558	9.320819	-0.056898	4.758231
277.808165	7806.242187	9.325824	-0.056878	4.760654
278.218005	7814.258425	9.330829	-0.056960	4.763069
277.832473	7822.272115	9.335834	-0.056894	4.765484
277.985334	7830.318281	9.340839	-0.056927	4.767906
277.947717	7838.331624	9.345843	-0.056926	4.770317
278.613019	7846.272354	9.350848	-0.057055	4.772704
278.683669	7854.356186	9.355853	-0.057073	4.775133
278.617701	7862.348291	9.360858	-0.057066	4.777535
278.714449	7870.408370	9.365863	-0.057089	4.779955
279.217223	7878.354867	9.370867	-0.057188	4.782339
279.357582	7886.379945	9.375872	-0.057220	4.784746
279.113627	7894.490576	9.380877	-0.057180	4.787178
279.067523	7902.451020	9.385882	-0.057176	4.789564
279.082281	7910.538047	9.390887	-0.057184	4.791987
279.066944	7918.443192	9.395891	-0.057187	4.794353
279.790718	7926.459553	9.400896	-0.057327	4.796750
279.699997	7934.525339	9.405901	-0.057315	4.799163
279.500148	7942.527052	9.410906	-0.057283	4.801555
279.729511	7950.467659	9.415911	-0.057331	4.803927
280.093600	7958.561319	9.420915	-0.057404	4.806343
280.010639	7966.535602	9.425920	-0.057394	4.808723
280.115791	7974.627064	9.430925	-0.057419	4.811137
280.855058	7982.521062	9.435930	-0.057562	4.813488
280.759899	7990.133125	9.440935	-0.057549	4.815757
280.907587	7994.791876	9.445939	-0.057580	4.817145

280.968850	7997.278842	9.450944	-0.057593	4.817885
281.185957	7998.570988	9.455949	-0.057634	4.818269
281.266935	7998.980876	9.460954	-0.057650	4.818391
281.547947	8000.166009	9.465959	-0.057703	4.818743
281.528292	8000.173100	9.470963	-0.057699	4.818745
281.313328	8000.217521	9.475968	-0.057659	4.818759
281.616419	8000.184726	9.480973	-0.057716	4.818748
281.522159	8000.159406	9.485978	-0.057698	4.818741
281.493387	8000.173718	9.490983	-0.057693	4.818745
281.447192	8000.196194	9.495987	-0.057685	4.818752
281.767676	8000.201366	9.500992	-0.057744	4.818753
282.074780	8000.189592	9.505997	-0.057802	4.818748
281.995764	8000.172854	9.511002	-0.057787	4.818743
282.115355	8000.208994	9.516007	-0.057809	4.818753
282.349871	8000.142816	9.521011	-0.057853	4.818733
282.024919	8000.174290	9.526016	-0.057793	4.818743
281.812911	8000.197781	9.531021	-0.057753	4.818751
282.250281	8000.176148	9.536026	-0.057835	4.818743
282.266118	8000.229827	9.541031	-0.057838	4.818759
282.441964	8000.174428	9.546035	-0.057870	4.818742
282.626199	8000.162123	9.551040	-0.057905	4.818738
282.730527	8000.165566	9.556045	-0.057924	4.818738
282.436001	8000.186946	9.561050	-0.057870	4.818746
282.634135	8000.208370	9.566055	-0.057907	4.818751
282.438807	8000.189088	9.571059	-0.057870	4.818746
282.613505	8000.207065	9.576064	-0.057903	4.818751
282.890134	8000.196997	9.581069	-0.057954	4.818747
282.791718	8000.191542	9.586074	-0.057936	4.818746
282.942654	8000.194536	9.591079	-0.057964	4.818746
282.640097	8000.167584	9.596083	-0.057908	4.818739
283.006187	8000.167054	9.601088	-0.057976	4.818738
283.096777	8000.188144	9.606093	-0.057993	4.818743
282.884572	8000.178080	9.611098	-0.057954	4.818741
283.088318	8000.190141	9.616103	-0.057992	4.818744
283.414223	8000.166029	9.621107	-0.058052	4.818736
283.240897	8000.193161	9.626112	-0.058020	4.818744
283.141085	8000.189785	9.631117	-0.058002	4.818744
283.123360	8000.191658	9.636122	-0.057999	4.818744
283.312600	8000.194097	9.641127	-0.058034	4.818744
282.936796	8000.166202	9.646131	-0.057964	4.818738
283.166509	8000.199566	9.651136	-0.058007	4.818747
282.973276	8000.218054	9.656141	-0.057971	4.818753
282.815258	8000.220220	9.661146	-0.057941	4.818754
283.100851	8000.216559	9.666151	-0.057995	4.818752
283.366768	8000.183288	9.671155	-0.058044	4.818741
283.323424	8000.206849	9.676160	-0.058036	4.818748
283.319182	8000.188975	9.681165	-0.058036	4.818743
283.117294	8000.172753	9.686170	-0.057998	4.818739
283.644997	8000.180594	9.691175	-0.058096	4.818739
283.436785	8000.174775	9.696179	-0.058058	4.818738
283.374805	8000.208581	9.701184	-0.058046	4.818748
283.796173	8000.200377	9.706189	-0.058125	4.818744
283.416875	8000.190259	9.711194	-0.058054	4.818743
283.825042	8000.211242	9.716199	-0.058130	4.818748
283.789348	8000.189818	9.721203	-0.058124	4.818741
283.917494	8000.214538	9.726208	-0.058148	4.818748
283.788746	8000.214982	9.731213	-0.058124	4.818749
283.648462	8000.195358	9.736218	-0.058098	4.818743
283.873360	8000.189868	9.741223	-0.058140	4.818741
283.758836	8000.183157	9.746227	-0.058118	4.818739
283.626014	8000.209761	9.751232	-0.058094	4.818748
283.852981	8000.204298	9.756237	-0.058136	4.818745
283.772669	8000.161330	9.761242	-0.058121	4.818733
283.713112	8000.236059	9.766247	-0.058110	4.818755
283.427686	8000.232391	9.771251	-0.058057	4.818755
283.850403	8000.183313	9.776256	-0.058136	4.818739
283.983053	8000.186073	9.781261	-0.058160	4.818739
283.865509	8000.174080	9.786266	-0.058139	4.818736
284.123496	8000.205714	9.791271	-0.058187	4.818745
283.917122	8000.198868	9.796275	-0.058148	4.818743
283.827888	8000.227082	9.801280	-0.058132	4.818752
283.619351	8000.224403	9.806285	-0.058093	4.818752
283.727984	8000.195400	9.811290	-0.058113	4.818743
283.854341	8000.222193	9.816295	-0.058137	4.818751
284.212622	8000.199548	9.821299	-0.058204	4.818743
284.182165	8000.193918	9.826304	-0.058198	4.818741
284.049410	8000.208990	9.831309	-0.058173	4.818746
284.166756	8000.190583	9.836314	-0.058195	4.818740
284.308071	8000.202891	9.841319	-0.058222	4.818743
284.144505	8000.180870	9.846323	-0.058191	4.818737
283.976149	8000.210162	9.851328	-0.058160	4.818747
284.160435	8000.220926	9.856333	-0.058195	4.818749
283.945928	8000.209782	9.861338	-0.058155	4.818747
283.870461	8000.264385	9.866343	-0.058141	4.818763
284.110391	8000.193035	9.871347	-0.058185	4.818741
284.023442	8000.197163	9.876352	-0.058169	4.818743
284.117934	8000.188947	9.881357	-0.058187	4.818740
283.994052	8000.198891	9.886362	-0.058164	4.818743
284.319723	8000.204135	9.891367	-0.058225	4.818743
284.262534	8000.201306	9.896371	-0.058214	4.818743
284.534350	8000.189082	9.901376	-0.058265	4.818738
284.482748	8000.229313	9.906381	-0.058255	4.818750
284.225317	8000.198744	9.911386	-0.058207	4.818742
284.228784	8000.223957	9.916391	-0.058208	4.818750
284.321501	8000.213621	9.921395	-0.058225	4.818746
284.500400	8000.199152	9.926400	-0.058259	4.818741
284.404345	8000.237763	9.931405	-0.058241	4.818753
284.315779	8000.187349	9.936410	-0.058224	4.818738
284.135171	8000.229065	9.941415	-0.058191	4.818752
283.772224	8000.232787	9.946419	-0.058123	4.818754
284.155479	8000.208366	9.951424	-0.058195	4.818745
284.095812	8000.254784	9.956429	-0.058184	4.818759
284.423516	8000.218115	9.961434	-0.058245	4.818747
284.485789	8000.208437	9.966439	-0.058257	4.818744
284.366123	8000.196416	9.971443	-0.058234	4.818741
284.616950	8000.170291	9.976448	-0.058281	4.818732
284.648354	8000.185379	9.981453	-0.058287	4.818737
284.721522	8000.191568	9.986458	-0.058301	4.818738
285.003924	8000.216178	9.991463	-0.058353	4.818744
284.801592	8000.162201	9.996467	-0.058316	4.818729
284.603351	8000.174332	10.001472	-0.058279	4.818733
285.003000	8000.188918	10.006477	-0.058353	4.818736
284.660177	8000.199188	10.011482	-0.058290	4.818741
284.802317	8000.230381	10.016487	-0.058316	4.818749
284.833384	8000.206670	10.021491	-0.058322	4.818742
284.971371	8000.204257	10.026496	-0.058348	4.818741
284.936884	8000.204866	10.031501	-0.058341	4.818741
284.920303	8000.179492	10.036506	-0.058338	4.818734
285.130606	8000.189544	10.041511	-0.058378	4.818736
284.982093	8000.185539	10.046515	-0.058350	4.818735
284.899393	8000.196013	10.051520	-0.058335	4.818739
285.008807	8000.205814	10.056525	-0.058355	4.818741
285.110170	8000.195590	10.061530	-0.058374	4.818738
284.899497	8000.219095	10.066535	-0.058335	4.818746
284.816559	8000.192867	10.071539	-0.058319	4.818738
284.931407	8000.199593	10.076544	-0.058341	4.818740
285.067466	8000.194010	10.081549	-0.058366	4.818738
284.715372	8000.188433	10.086554	-0.058301	4.818737
285.130143	8000.238863	10.091559	-0.058378	4.818751
284.967602	8000.215805	10.096563	-0.058348	4.818744
284.788773	8000.228186	10.101568	-0.058315	4.818749
284.850897	8000.223747	10.106573	-0.058326	4.818747
284.951750	8000.201983	10.111578	-0.058345	4.818740
284.824767	8000.237051	10.116583	-0.058322	4.818751
284.555891	8000.250370	10.121587	-0.058272	4.818756
285.123192	8000.225174	10.126592	-0.058377	4.818747
284.888448	8000.254660	10.131597	-0.058334	4.818756
284.937111	8000.203914	10.136602	-0.058343	4.818741
284.692527	8000.222788	10.141607	-0.058297	4.818748
285.036474	8000.193669	10.146611	-0.058361	4.818738
284.760782	8000.231016	10.151616	-0.058310	4.818750
284.816656	8000.238031	10.156621	-0.058321	4.818752
284.758635	8000.211075	10.161626	-0.058310	4.818744
284.919657	8000.221541	10.166631	-0.058340	4.818746
285.153437	8000.185761	10.171635	-0.058383	4.818735
284.972113	8000.207546	10.176640	-0.058350	4.818742
284.875843	8000.225184	10.181645	-0.058332	4.818748
284.639172	8000.206414	10.186650	-0.058288	4.818743
285.125359	8000.234697	10.191655	-0.058379	4.818749
284.945913	8000.198839	10.196659	-0.058345	4.818739
284.469168	8000.237791	10.201664	-0.058256	4.818753
284.998653	8000.245661	10.206669	-0.058355	4.818753
285.144833	8000.193026	10.211674	-0.058382	4.818737
285.193489	8000.218821	10.216679	-0.058392	4.818744
284.415493	8000.257040	10.221683	-0.058247	4.818759
284.493609	8000.264341	10.226688	-0.058261	4.818761
284.643548	8000.290391	10.231693	-0.058289	4.818768
284.536099	8000.253363	10.236698	-0.058269	4.818757
284.601226	8000.281467	10.241703	-0.058282	4.818765
284.962429	8000.247328	10.246707	-0.058349	4.818754
284.851708	8000.239616	10.251712	-0.058328	4.818752
284.378914	8000.310074	10.256717	-0.058240	4.818775
284.159930	8000.297823	10.261722	-0.058200	4.818772
284.196633	8000.318221	10.266727	-0.058207	4.818778
284.491155	8000.255962	10.271731	-0.058261	4.818758
284.365425	8000.284754	10.276736	-0.058238	4.818767
284.800460	8000.256807	10.281741	-0.058319	4.818757
284.321137	8000.291533	10.286746	-0.058230	4.818769
284.085508	8000.341977	10.291751	-0.058186	4.818785
284.450373	8000.294254	10.296755	-0.058254	4.818770
284.285640	8000.269071	10.301760	-0.058224	4.818763
284.375575	8000.342579	10.306765	-0.058240	4.818784
284.451431	8000.247098	10.311770	-0.058255	4.818756
284.844681	8000.263699	10.316775	-0.058328	4.818759
284.176685	8000.348420	10.321779	-0.058204	4.818787
284.552237	8000.264137	10.326784	-0.058274	4.818760
284.833842	8000.284543	10.331789	-0.058326	4.818765
285.221637	8000.220340	10.336794	-0.058398	4.818745
285.058924	8000.246559	10.341799	-0.058368	4.818753
285.028902	8000.251419	10.346803	-0.058363	4.818755
284.863266	8000.229369	10.351808	-0.058332	4.818749
285.085489	8000.239575	10.356813	-0.058373	4.818751
285.153027	8000.222624	10.361818	-0.058386	4.818746
284.810630	8000.268548	10.366823	-0.058322	4.818761
284.778947	8000.283872	10.371827	-0.058316	4.818765
285.103997	8000.241928	10.376832	-0.058377	4.818752
285.225666	8000.283343	10.381837	-0.058400	4.818763
285.221783	8000.260230	10.386842	-0.058399	4.818757
285.245434	8000.252151	10.391847	-0.058403	4.818754
285.614899	8000.245380	10.396851	-0.058472	4.818751
285.727717	8000.233207	10.401856	-0.058493	4.818747
285.680055	8000.217918	10.406861	-0.058485	4.818742
285.492180	8000.210260	10.411866	-0.058450	4.818741
285.460477	8000.268574	10.416871	-0.058444	4.818758
284.987447	8000.286602	10.421875	-0.058356	4.818765
285.073290	8000.271984	10.426880	-0.058372	4.818761
285.441059	8000.263095	10.431885	-0.058440	4.818757
285.361742	8000.227476	10.436890	-0.058426	4.818746
285.118968	8000.268392	10.441895	-0.058381	4.818759
285.003832	8000.279496	10.446899	-0.058359	4.818763
285.431639	8000.235730	10.451904	-0.058439	4.818748
285.282485	8000.325034	10.456909	-0.058411	4.818776
285.043848	8000.276879	10.461914	-0.058367	4.818762
285.714641	8000.241485	10.466919	-0.058492	4.818749
285.433655	8000.264084	10.471923	-0.058440	4.818757
285.181466	8000.255598	10.476928	-0.058393	4.818755
285.721198	8000.262554	10.481933	-0.058493	4.818755
285.536594	8000.218239	10.486938	-0.058459	4.818743
285.313065	8000.232141	10.491943	-0.058417	4.818748
285.213930	8000.267567	10.496947	-0.058399	4.818759
285.464395	8000.247730	10.501952	-0.058446	4.818752
285.268946	8000.263042	10.506957	-0.058409	4.818757
284.790241	8000.308259	10.511962	-0.058320	4.818773
285.134548	8000.295921	10.516967	-0.058385	4.818768
285.001826	8000.301556	10.521971	-0.058360	4.818770
284.977209	8000.266643	10.526976	-0.058355	4.818759
285.179221	8000.310141	10.531981	-0.058393	4.818772
285.106176	8000.211693	10.536986	-0.058379	4.818743
285.393156	8000.238460	10.541991	-0.058433	4.818749
285.524232	8000.211843	10.546995	-0.058457	4.818741
285.690243	8000.219228	10.552000	-0.058488	4.818743
285.627263	8000.239392	10.557005	-0.058477	4.818749
285.497753	8000.217806	10.562010	-0.058453	4.818743
285.344097	8000.246239	10.567015	-0.058424	4.818752
285.692098	8000.233950	10.572019	-0.058489	4.818747
285.110133	8000.245332	10.577024	-0.058381	4.818753
284.990716	8000.319292	10.582029	-0.058359	4.818775
285.217555	8000.305442	10.587034	-0.058401	4.818770
285.584955	8000.259849	10.592039	-0.058469	4.818755
285.636891	8000.246892	10.597043	-0.058479	4.818751
285.842307	8000.201310	10.602048	-0.058517	4.818737
285.511736	8000.258919	10.607053	-0.058456	4.818755
285.545652	8000.192255	10.612058	-0.058462	4.818735
285.505393	8000.232634	10.617063	-0.058455	4.818747
285.596651	8000.220183	10.622067	-0.058472	4.818743
285.447706	8000.227706	10.627072	-0.058444	4.818746
285.637235	8000.244831	10.632077	-0.058480	4.818750
285.776033	8000.220410	10.637082	-0.058505	4.818743
285.344509	8000.266234	10.642087	-0.058425	4.818758
285.393999	8000.285749	10.647091	-0.058434	4.818763
285.813881	8000.215668	10.652096	-0.058513	4.818741
285.734466	8000.260785	10.657101	-0.058498	4.818755
285.732096	8000.202041	10.662106	-0.058498	4.818737
285.505108	8000.260985	10.667111	-0.058455	4.818756
285.612007	8000.256075	10.672115	-0.058475	4.818754
285.001220	8000.260796	10.677120	-0.058362	4.818758
285.365952	8000.273885	10.682125	-0.058430	4.818760
285.305085	8000.288834	10.687130	-0.058418	4.818765
285.428814	8000.288335	10.692135	-0.058442	4.818764
285.567440	8000.275446	10.697139	-0.058467	4.818760
285.635583	8000.235435	10.702144	-0.058480	4.818748
285.541399	8000.270925	10.707149	-0.058463	4.818758
285.618501	8000.231030	10.712154	-0.058477	4.818746
285.872326	8000.261566	10.717159	-0.058524	4.818754
285.699907	8000.261447	10.722163	-0.058492	4.818755
285.806077	8000.225072	10.727168	-0.058512	4.818744
285.687569	8000.279122	10.732173	-0.058490	4.818760
285.599013	8000.255966	10.737178	-0.058474	4.818754
285.141531	8000.307747	10.742183	-0.058389	4.818771
285.531219	8000.279218	10.747187	-0.058461	4.818761
285.557685	8000.237622	10.752192	-0.058466	4.818748
285.784373	8000.244741	10.757197	-0.058509	4.818750
285.342285	8000.254779	10.762202	-0.058426	4.818754
284.956103	8000.332643	10.767207	-0.058355	4.818779
285.539412	8000.284589	10.772211	-0.058463	4.818763
285.560218	8000.273327	10.777216	-0.058467	4.818759
285.589634	8000.287342	10.782221	-0.058473	4.818763
285.893311	8000.236735	10.787226	-0.058529	4.818747
285.761906	8000.292716	10.792231	-0.058505	4.818764
285.840575	8000.284297	10.797235	-0.058520	4.818761
285.843437	8000.235057	10.802240	-0.058520	4.818747
285.645543	8000.282842	10.807245	-0.058483	4.818762
285.454182	8000.260459	10.812250	-0.058448	4.818756
285.346680	8000.313602	10.817255	-0.058428	4.818772
285.883394	8000.247124	10.822259	-0.058528	4.818750
285.793154	8000.233383	10.827264	-0.058511	4.818746
285.825128	8000.272595	10.832269	-0.058517	4.818758
286.274277	8000.164096	10.837274	-0.058601	4.818724
286.320839	8000.197205	10.842279	-0.058610	4.818733
286.201156	8000.219784	10.847283	-0.058587	4.818741
286.073309	8000.262180	10.852288	-0.058564	4.818754
286.132933	8000.253516	10.857293	-0.058575	4.818751
285.937154	8000.213251	10.862298	-0.058538	4.818740
285.948724	8000.251151	10.867303	-0.058541	4.818751
286.294687	8000.207380	10.872307	-0.058605	4.818737
286.087709	8000.238271	10.877312	-0.058567	4.818747
286.296904	8000.243068	10.882317	-0.058606	4.818747
286.287031	8000.194713	10.887322	-0.058604	4.818733
286.100595	8000.224820	10.892327	-0.058569	4.818743
286.313843	8000.224426	10.897331	-0.058609	4.818742
286.327391	8000.236139	10.902336	-0.058612	4.818745
286.288582	8000.244032	10.907341	-0.058604	4.818748
286.156947	8000.223467	10.912346	-0.058580	4.818742
286.166476	8000.245613	10.917351	-0.058582	4.818748
286.272078	8000.221814	10.922355	-0.058602	4.818741
286.204930	8000.160138	10.927360	-0.058589	4.818723
285.916833	8000.230877	10.932365	-0.058536	4.818745
286.135069	8000.220062	10.937370	-0.058576	4.818741
286.290466	8000.221020	10.942375	-0.058605	4.818741
286.122778	8000.224107	10.947379	-0.058574	4.818742
286.141997	8000.209679	10.952384	-0.058578	4.818738
286.133860	8000.256763	10.957389	-0.058576	4.818752
286.155239	8000.194131	10.962394	-0.058580	4.818733
286.158770	8000.223540	10.967399	-0.058581	4.818742
286.502956	8000.238465	10.972403	-0.058645	4.818745
286.284759	8000.240900	10.977408	-0.058605	4.818747
286.330779	8000.234158	10.982413	-0.058613	4.818744
286.122972	8000.239873	10.987418	-0.058575	4.818747
286.287226	8000.225217	10.992423	-0.058605	4.818742
286.400015	8000.221432	10.997427	-0.058626	4.818740
286.035700	8000.234568	11.002432	-0.058559	4.818746
286.337252	8000.259429	11.007437	-0.058615	4.818752
285.975614	8000.241143	11.012442	-0.058547	4.818748
285.907479	8000.244463	11.017447	-0.058535	4.818749
285.934077	8000.269976	11.022451	-0.058540	4.818757
285.895782	8000.243273	11.027456	-0.058533	4.818749
285.906824	8000.267536	11.032461	-0.058535	4.818756
286.098016	8000.251130	11.037466	-0.058571	4.818750
286.245364	8000.261422	11.042471	-0.058598	4.818753
286.048929	8000.311322	11.047475	-0.058562	4.818768
286.181038	8000.221806	11.052480	-0.058586	4.818741
286.286355	8000.287129	11.057485	-0.058606	4.818760
286.357942	8000.220949	11.062490	-0.058619	4.818740
286.242807	8000.239392	11.067495	-0.058598	4.818746
286.490381	8000.244684	11.072499	-0.058644	4.818747
286.546201	8000.229679	11.077504	-0.058655	4.818742
286.449608	8000.234730	11.082509	-0.058637	4.818744
286.236371	8000.242473	11.087514	-0.058597	4.818747
286.273908	8000.249252	11.092519	-0.058604	4.818749
286.455758	8000.274668	11.097523	-0.058638	4.818756
286.033789	8000.277623	11.102528	-0.058560	4.818758
286.542813	8000.263216	11.107533	-0.058654	4.818752
286.431720	8000.234527	11.112538	-0.058634	4.818744
286.339152	8000.264795	11.117543	-0.058617	4.818753
286.583275	8000.215518	11.122547	-0.058662	4.818738
286.448976	8000.207501	11.127552	-0.058637	4.818736
286.330463	8000.262599	11.132557	-0.058615	4.818753
286.368840	8000.238982	11.137562	-0.058622	4.818746
286.814984	8000.240542	11.142567	-0.058705	4.818744
286.873157	8000.204597	11.147571	-0.058716	4.818733
286.443398	8000.225276	11.152576	-0.058636	4.818741
286.614661	8000.251605	11.157581	-0.058668	4.818748
286.320466	8000.245721	11.162586	-0.058614	4.818748
286.208405	8000.239039	11.167591	-0.058593	4.818746
286.547855	8000.229786	11.172595	-0.058656	4.818742
286.463477	8000.225558	11.177600	-0.058640	4.818741
286.553876	8000.241407	11.182605	-0.058657	4.818746
286.452995	8000.191878	11.187610	-0.058639	4.818731
286.568724	8000.223782	11.192615	-0.058660	4.818740
286.883739	8000.212118	11.197619	-0.058719	4.818736
286.622300	8000.233918	11.202624	-0.058670	4.818743
286.749432	8000.249192	11.207629	-0.058694	4.818747
286.656762	8000.218643	11.212634	-0.058677	4.818738
286.780662	8000.213953	11.217639	-0.058700	4.818737
286.727272	8000.218512	11.222643	-0.058690	4.818738
286.825833	8000.222933	11.227648	-0.058709	4.818739
286.842809	8000.235739	11.232653	-0.058712	4.818743
286.676133	8000.211575	11.237658	-0.058681	4.818736
286.705340	8000.225587	11.242663	-0.058686	4.818740
286.731068	8000.222778	11.247667	-0.058691	4.818739
286.421470	8000.224035	11.252672	-0.058634	4.818741
286.714261	8000.237250	11.257677	-0.058688	4.818744
286.667027	8000.241888	11.262682	-0.058679	4.818745
286.659835	8000.206149	11.267687	-0.058678	4.818735
286.491174	8000.224951	11.272691	-0.058647	4.818741
286.421830	8000.221965	11.277696	-0.058634	4.818740
286.694298	8000.225481	11.282701	-0.058685	4.818740
286.459149	8000.228746	11.287706	-0.058641	4.818742
286.377626	8000.276982	11.292711	-0.058626	4.818757
286.193809	8000.299783	11.297715	-0.058592	4.818764
286.471332	8000.221577	11.302720	-0.058644	4.818740
286.586301	8000.253471	11.307725	-0.058665	4.818749
286.417424	8000.214600	11.312730	-0.058634	4.818738
286.738096	8000.226077	11.317735	-0.058693	4.818740
286.893500	8000.224939	11.322739	-0.058722	4.818739
286.861067	8000.215088	11.327744	-0.058716	4.818737
286.903384	8000.240803	11.332749	-0.058724	4.818744
286.779266	8000.205654	11.337754	-0.058701	4.818734
286.860446	8000.243405	11.342759	-0.058717	4.818745
286.816766	8000.235506	11.347763	-0.058708	4.818743
286.696665	8000.205652	11.352768	-0.058686	4.818734
286.628217	8000.230988	11.357773	-0.058673	4.818742
286.678275	8000.237929	11.362778	-0.058683	4.818744
286.937198	8000.211911	11.367783	-0.058731	4.818735
286.894233	8000.247013	11.372787	-0.058723	4.818746
286.770873	8000.234942	11.377792	-0.058700	4.818743
286.928908	8000.230692	11.382797	-0.058730	4.818741
286.838522	8000.206463	11.387802	-0.058713	4.818734
287.010425	8000.229654	11.392807	-0.058745	4.818740
287.019210	8000.217189	11.397811	-0.058747	4.818737
286.787799	8000.215260	11.402816	-0.058704	4.818737
286.758728	8000.225375	11.407821	-0.058698	4.818740
286.928558	8000.197160	11.412826	-0.058730	4.818731
286.749456	8000.220022	11.417831	-0.058697	4.818738
286.760372	8000.220167	11.422835	-0.058699	4.818738
286.639452	8000.207079	11.427840	-0.058676	4.818735
286.765586	8000.238069	11.432845	-0.058700	4.818744
286.836753	8000.209631	11.437850	-0.058713	4.818735
286.649370	8000.233434	11.442855	-0.058679	4.818743
286.661418	8000.254565	11.447859	-0.058681	4.818749
286.763964	8000.205560	11.452864	-0.058700	4.818734
286.949441	8000.227878	11.457869	-0.058735	4.818740
287.184372	8000.222523	11.462874	-0.058778	4.818738
287.084456	8000.233822	11.467879	-0.058760	4.818741
287.039490	8000.234295	11.472883	-0.058752	4.818742
286.965473	8000.203986	11.477888	-0.058738	4.818733
286.979621	8000.238775	11.482893	-0.058741	4.818743
286.851803	8000.205675	11.487898	-0.058717	4.818734
286.887766	8000.197755	11.492903	-0.058724	4.818731
287.101971	8000.230929	11.497907	-0.058764	4.818740
286.902003	8000.227307	11.502912	-0.058726	4.818740
286.834231	8000.231681	11.507917	-0.058714	4.818742
287.047574	8000.204027	11.512922	-0.058754	4.818733
287.083636	8000.198205	11.517927	-0.058760	4.818731
286.955473	8000.218577	11.522931	-0.058737	4.818737
287.010668	8000.195176	11.527936	-0.058747	4.818730
286.947654	8000.224777	11.532941	-0.058735	4.818739
287.102177	8000.198462	11.537946	-0.058764	4.818731
287.036048	8000.212294	11.542951	-0.058752	4.818735
287.165058	8000.222350	11.547955	-0.058776	4.818738
286.982037	8000.219995	11.552960	-0.058742	4.818738
286.951356	8000.233236	11.557965	-0.058736	4.818742
286.913372	8000.214925	11.562970	-0.058729	4.818736
286.901218	8000.234695	11.567975	-0.058727	4.818742
286.911141	8000.219099	11.572979	-0.058729	4.818738
286.830701	8000.175076	11.577984	-0.058714	4.818725
286.846466	8000.219323	11.582989	-0.058717	4.818738
286.934766	8000.183766	11.587994	-0.058734	4.818727
286.736695	8000.207432	11.592999	-0.058697	4.818735
287.010601	8000.226695	11.598003	-0.058748	4.818739
287.046537	8000.196755	11.603008	-0.058755	4.818730
287.168740	8000.213014	11.608013	-0.058777	4.818735
287.013634	8000.214165	11.613018	-0.058749	4.818736
286.982970	8000.252571	11.618023	-0.058743	4.818747
287.048864	8000.218822	11.623027	-0.058755	4.818737
286.837004	8000.215048	11.628032	-0.058716	4.818737
286.999132	8000.246502	11.633037	-0.058746	4.818745
287.137116	8000.200051	11.638042	-0.058772	4.818731
287.011178	8000.205772	11.643047	-0.058748	4.818733
287.111039	8000.228035	11.648051	-0.058767	4.818739
286.998608	8000.177308	11.653056	-0.058746	4.818725
287.082024	8000.197262	11.658061	-0.058762	4.818730
287.199810	8000.202979	11.663066	-0.058784	4.818732
287.172444	8000.190048	11.668071	-0.058779	4.818728
287.251106	8000.198406	11.673075	-0.058794	4.818730
287.064163	8000.201244	11.678080	-0.058759	4.818732
287.039564	8000.265942	11.683085	-0.058754	4.818751
287.285127	8000.202004	11.688090	-0.058800	4.818731
287.134624	8000.205311	11.693095	-0.058772	4.818733
287.224519	8000.230591	11.698099	-0.058789	4.818740
287.335203	8000.206857	11.703104	-0.058810	4.818732
287.178658	8000.237349	11.708109	-0.058781	4.818742
287.084839	8000.191056	11.713114	-0.058763	4.818728
287.211136	8000.212611	11.718119	-0.058787	4.818734
287.365191	8000.230330	11.723123	-0.058815	4.818739
287.129292	8000.223099	11.728128	-0.058772	4.818738
287.410807	8000.239316	11.733133	-0.058824	4.818742
287.297584	8000.205355	11.738138	-0.058803	4.818732
286.919643	8000.241382	11.743143	-0.058733	4.818744
287.101199	8000.223804	11.748147	-0.058767	4.818738
287.147312	8000.220208	11.753152	-0.058775	4.818737
287.005942	8000.241459	11.758157	-0.058749	4.818744
286.851823	8000.222700	11.763162	-0.058720	4.818739
286.814683	8000.240051	11.768167	-0.058714	4.818744
286.930387	8000.226867	11.773171	-0.058735	4.818740
286.631219	8000.227210	11.778176	-0.058679	4.818741
287.010935	8000.240497	11.783181	-0.058750	4.818743
286.971038	8000.207482	11.788186	-0.058743	4.818734
286.861463	8000.223900	11.793191	-0.058723	4.818739
286.937603	8000.226983	11.798195	-0.058737	4.818740
286.640636	8000.234694	11.803200	-0.058682	4.818743
287.165056	8000.222584	11.808205	-0.058779	4.818738
286.925730	8000.221600	11.813210	-0.058735	4.818738
287.392281	8000.223425	11.818215	-0.058822	4.818737
287.611311	8000.217865	11.823219	-0.058863	4.818734
287.264701	8000.187186	11.828224	-0.058798	4.818727
287.338633	8000.237427	11.833229	-0.058812	4.818741
287.267871	8000.205062	11.838234	-0.058799	4.818732
287.240780	8000.218349	11.843239	-0.058794	4.818736
287.331416	8000.241541	11.848243	-0.058811	4.818743
287.246229	8000.236253	11.853248	-0.058795	4.818741
287.086191	8000.246778	11.858253	-0.058765	4.818745
286.801527	8000.220044	11.863258	-0.058712	4.818738
287.193544	8000.229296	11.868263	-0.058785	4.818739
287.129165	8000.259928	11.873267	-0.058773	4.818749
287.047080	8000.251534	11.878272	-0.058758	4.818747
287.114805	8000.278626	11.883277	-0.058771	4.818754
287.388206	8000.240213	11.888282	-0.058822	4.818742
286.987501	8000.230857	11.893287	-0.058747	4.818741
287.093796	8000.271029	11.898291	-0.058767	4.818752
287.146969	8000.233970	11.903296	-0.058777	4.818741
287.213810	8000.244273	11.908301	-0.058790	4.818744
287.216413	8000.231729	11.913306	-0.058790	4.818740
287.036669	8000.213688	11.918311	-0.058757	4.818735
287.423465	8000.262719	11.923315	-0.058829	4.818748
287.234789	8000.221493	11.928320	-0.058794	4.818737
286.993471	8000.258232	11.933325	-0.058749	4.818749
287.102699	8000.223994	11.938330	-0.058769	4.818738
287.126448	8000.225353	11.943335	-0.058774	4.818738
287.209783	8000.261035	11.948339	-0.058789	4.818749
287.103532	8000.226115	11.953344	-0.058770	4.818739
287.120272	8000.246258	11.958349	-0.058773	4.818745
286.830459	8000.230993	11.963354	-0.058719	4.818741
286.763470	8000.243765	11.968359	-0.058707	4.818745
287.136707	8000.244386	11.973363	-0.058776	4.818744
286.767278	8000.243823	11.978368	-0.058707	4.818745
286.983568	8000.287510	11.983373	-0.058748	4.818758
287.337735	8000.242797	11.988378	-0.058814	4.818743
287.508987	8000.227184	11.993383	-0.058846	4.818738
287.427230	8000.237669	11.998387	-0.058831	4.818741
287.315101	8000.227839	12.003392	-0.058810	4.818738
287.484503	8000.232125	12.008397	-0.058841	4.818739
287.270932	8000.230424	12.013402	-0.058802	4.818739
287.321252	8000.230029	12.018407	-0.058811	4.818739
287.508034	8000.238733	12.023411	-0.058846	4.818741
287.402716	8000.228991	12.028416	-0.058826	4.818738
287.589659	8000.243989	12.033421	-0.058861	4.818742
287.663983	8000.234466	12.038426	-0.058875	4.818739
287.481265	8000.235260	12.043431	-0.058841	4.818740
287.251697	8000.260616	12.048435	-0.058799	4.818748
287.576621	8000.224964	12.053440	-0.058859	4.818737
287.629030	8000.234033	12.058445	-0.058869	4.818739
287.266890	8000.209446	12.063450	-0.058802	4.818733
287.242501	8000.221719	12.068455	-0.058797	4.818737
287.445214	8000.236920	12.073459	-0.058835	4.818741
287.277551	8000.225325	12.078464	-0.058804	4.818738
287.277596	8000.225330	12.083469	-0.058804	4.818738
287.451818	8000.184590	12.088474	-0.058836	4.818725
287.402071	8000.211216	12.093479	-0.058827	4.818733
287.394464	8000.241531	12.098483	-0.058826	4.818742
287.668646	8000.182156	12.103488	-0.058877	4.818723
287.657344	8000.190403	12.108493	-0.058875	4.818726
287.580682	8000.234508	12.113498	-0.058861	4.818739
287.485936	8000.213368	12.118503	-0.058843	4.818733
287.671593	8000.244078	12.123507	-0.058878	4.818742
287.429484	8000.207406	12.128512	-0.058833	4.818732
287.334944	8000.247086	12.133517	-0.058815	4.818744
287.208742	8000.268532	12.138522	-0.058792	4.818751
287.296006	8000.289584	12.143527	-0.058808	4.818757
287.461327	8000.277041	12.148531	-0.058839	4.818753
287.285594	8000.250662	12.153536	-0.058806	4.818745
287.141399	8000.278167	12.158541	-0.058779	4.818754
287.273921	8000.257861	12.163546	-0.058804	4.818748
287.018462	8000.232552	12.168551	-0.058757	4.818741
287.303097	8000.278169	12.173555	-0.058810	4.818753
287.117322	8000.231738	12.178560	-0.058775	4.818740
287.037809	8000.282097	12.183565	-0.058760	4.818756
287.566863	8000.233349	12.188570	-0.058859	4.818739
287.763936	8000.228554	12.193575	-0.058896	4.818737
287.636896	8000.257329	12.198579	-0.058872	4.818746
287.786767	8000.220469	12.203584	-0.058900	4.818734
287.740648	8000.273357	12.208589	-0.058892	4.818750
287.854437	8000.223448	12.213594	-0.058913	4.818735
287.533382	8000.219312	12.218599	-0.058853	4.818735
287.496760	8000.238768	12.223603	-0.058846	4.818741
287.520925	8000.203432	12.228608	-0.058851	4.818730
287.526301	8000.237060	12.233613	-0.058852	4.818740
287.301672	8000.243606	12.238618	-0.058810	4.818743
287.683044	8000.225459	12.243623	-0.058881	4.818736
287.557222	8000.273124	12.248627	-0.058858	4.818751
287.273936	8000.211805	12.253632	-0.058805	4.818734
287.521646	8000.238071	12.258637	-0.058852	4.818741
287.517982	8000.242223	12.263642	-0.058851	4.818742
287.649554	8000.231341	12.268647	-0.058875	4.818738
287.737572	8000.238772	12.273651	-0.058892	4.818740
287.508489	8000.230580	12.278656	-0.058849	4.818738
287.468644	8000.257333	12.283661	-0.058842	4.818747
287.593527	8000.233782	12.288666	-0.058865	4.818739
287.692670	8000.206754	12.293671	-0.058884	4.818731
287.493900	8000.257673	12.298675	-0.058847	4.818747
287.545002	8000.198567	12.303680	-0.058856	4.818729
287.460547	8000.223697	12.308685	-0.058841	4.818737
287.364948	8000.244489	12.313690	-0.058823	4.818743
287.441034	8000.240232	12.318695	-0.058837	4.818742
287.657064	8000.253508	12.323699	-0.058878	4.818745
287.576412	8000.239889	12.328704	-0.058863	4.818741
287.643742	8000.237616	12.333709	-0.058875	4.818740
287.545721	8000.216434	12.338714	-0.058857	4.818734
287.574769	8000.201084	12.343719	-0.058863	4.818729
287.792800	8000.218580	12.348723	-0.058903	4.818734
287.777155	8000.195314	12.353728	-0.058900	4.818727
287.738130	8000.227321	12.358733	-0.058893	4.818737
287.759855	8000.238092	12.363738	-0.058897	4.818740
287.622034	8000.218493	12.368743	-0.058872	4.818734
287.656332	8000.267175	12.373747	-0.058878	4.818749
287.720263	8000.195652	12.378752	-0.058890	4.818727
287.741183	8000.256744	12.383757	-0.058894	4.818745
287.776947	8000.223655	12.388762	-0.058901	4.818735
287.724945	8000.220891	12.393767	-0.058891	4.818735
287.986700	8000.246292	12.398771	-0.058940	4.818741
287.794674	8000.234383	12.403776	-0.058904	4.818738
287.782234	8000.253101	12.408781	-0.058902	4.818744
287.708978	8000.244821	12.413786	-0.058888	4.818742
287.737471	8000.215832	12.418791	-0.058894	4.818733
287.825475	8000.234798	12.423795	-0.058910	4.818738
287.592849	8000.198248	12.428800	-0.058867	4.818728
287.656155	8000.237866	12.433805	-0.058879	4.818740
287.579176	8000.237927	12.438810	-0.058865	4.818740
287.774441	8000.233109	12.443815	-0.058901	4.818738
287.884754	8000.255508	12.448819	-0.058922	4.818744
287.642958	8000.204159	12.453824	-0.058877	4.818730
287.838015	8000.228699	12.458829	-0.058913	4.818737
287.785456	8000.228026	12.463834	-0.058903	4.818737
287.628581	8000.202939	12.468839	-0.058874	4.818730
287.842322	8000.248692	12.473843	-0.058914	4.818743
287.618854	8000.208065	12.478848	-0.058872	4.818731
287.633810	8000.236574	12.483853	-0.058875	4.818740
287.638134	8000.218809	12.488858	-0.058876	4.818734
287.400817	8000.257696	12.493863	-0.058832	4.818747
287.697654	8000.237411	12.498867	-0.058887	4.818740
287.452513	8000.191263	12.503872	-0.058842	4.818727
287.661488	8000.206545	12.508877	-0.058881	4.818731
287.707137	8000.200847	12.513882	-0.058889	4.818729
287.639087	8000.247160	12.518887	-0.058877	4.818743
287.671410	8000.246532	12.523891	-0.058883	4.818743
287.854009	8000.230017	12.528896	-0.058917	4.818737
287.880663	8000.232463	12.533901	-0.058922	4.818738
287.733298	8000.214838	12.538906	-0.058895	4.818733
287.705812	8000.198759	12.543911	-0.058889	4.818728
288.045321	8000.232503	12.548915	-0.058953	4.818737
287.802165	8000.217837	12.553920	-0.058908	4.818733
287.799165	8000.249260	12.558925	-0.058907	4.818743
287.928442	8000.227863	12.563930	-0.058931	4.818736
287.699922	8000.200803	12.568935	-0.058889	4.818729
287.777668	8000.261579	12.573939	-0.058903	4.818747
287.628169	8000.225053	12.578944	-0.058876	4.818736
287.564751	8000.265134	12.583949	-0.058864	4.818748
287.745165	8000.244396	12.588954	-0.058897	4.818742
287.704093	8000.217657	12.593959	-0.058890	4.818734
287.970053	8000.261986	12.598963	-0.058939	4.818746
287.792498	8000.194688	12.603968	-0.058906	4.818727
287.842702	8000.242526	12.608973	-0.058916	4.818741
287.981520	8000.242224	12.613978	-0.058942	4.818740
287.867633	8000.240760	12.618983	-0.058921	4.818740
287.866402	8000.253331	12.623987	-0.058920	4.818744
287.917002	8000.233017	12.628992	-0.058930	4.818738
287.857067	8000.251123	12.633997	-0.058919	4.818743
287.713434	8000.237741	12.639002	-0.058892	4.818740
287.567103	8000.224324	12.644007	-0.058865	4.818736
287.701856	8000.270106	12.649011	-0.058890	4.818749
287.576173	8000.225498	12.654016	-0.058867	4.818737
287.760777	8000.227883	12.659021	-0.058901	4.818737
287.689704	8000.239554	12.664026	-0.058888	4.818740
287.828924	8000.206751	12.669031	-0.058914	4.818730
287.799771	8000.232594	12.674035	-0.058909	4.818738
287.742775	8000.197260	12.679040	-0.058898	4.818728
287.731045	8000.252688	12.684045	-0.058896	4.818744
287.848201	8000.243718	12.689050	-0.058918	4.818741
287.635359	8000.221054	12.694055	-0.058878	4.818735
287.956214	8000.239877	12.699059	-0.058938	4.818739
287.611479	8000.250116	12.704064	-0.058874	4.818744
287.613090	8000.229169	12.709069	-0.058874	4.818738
287.643397	8000.243196	12.714074	-0.058880	4.818742
287.791319	8000.231477	12.719079	-0.058908	4.818738
288.009100	8000.253165	12.724083	-0.058948	4.818743
287.888231	8000.218055	12.729088	-0.058926	4.818733
287.839506	8000.252035	12.734093	-0.058917	4.818743
287.845710	8000.236391	12.739098	-0.058918	4.818739
287.729392	8000.210778	12.744103	-0.058896	4.818732
287.892319	8000.216029	12.749107	-0.058927	4.818733
287.693684	8000.206132	12.754112	-0.058890	4.818730
287.940037	8000.253354	12.759117	-0.058936	4.818743
287.905611	8000.221457	12.764122	-0.058930	4.818734
287.985601	8000.209910	12.769127	-0.058945	4.818730
287.922634	8000.270969	12.774131	-0.058933	4.818749
287.685798	8000.246947	12.779136	-0.058889	4.818743
288.053060	8000.263223	12.784141	-0.058957	4.818746
287.761331	8000.248979	12.789146	-0.058903	4.818743
287.696982	8000.233473	12.794151	-0.058891	4.818738
287.801035	8000.277812	12.799155	-0.058911	4.818751
287.608315	8000.247019	12.804160	-0.058875	4.818743
287.496382	8000.241386	12.809165	-0.058854	4.818742
287.516463	8000.250038	12.814170	-0.058858	4.818744
287.676634	8000.226942	12.819175	-0.058888	4.818737
287.878937	8000.247381	12.824179	-0.058925	4.818742
287.707297	8000.204278	12.829184	-0.058893	4.818730
287.972232	8000.211893	12.834189	-0.058943	4.818731
287.927988	8000.208181	12.839194	-0.058935	4.818730
287.772077	8000.207224	12.844199	-0.058906	4.818730
288.024342	8000.241939	12.849203	-0.058953	4.818740
287.984444	8000.201583	12.854208	-0.058945	4.818728
287.946086	8000.237793	12.859213	-0.058938	4.818739
287.903935	8000.242497	12.864218	-0.058931	4.818740
287.648054	8000.225570	12.869223	-0.058883	4.818736
288.008727	8000.253295	12.874227	-0.058950	4.818743
287.881870	8000.229643	12.879232	-0.058927	4.818737
287.982867	8000.234096	12.884237	-0.058946	4.818738
287.832262	8000.221672	12.889242	-0.058918	4.818734
287.684499	8000.175731	12.894247	-0.058890	4.818721
288.022995	8000.222044	12.899251	-0.058953	4.818734
287.852573	8000.205170	12.904256	-0.058922	4.818729
287.906466	8000.232084	12.909261	-0.058932	4.818737
287.879180	8000.241174	12.914266	-0.058927	4.818740
287.897716	8000.242466	12.919271	-0.058930	4.818740
287.987452	8000.245725	12.924275	-0.058947	4.818741
287.737697	8000.215245	12.929280	-0.058900	4.818733
287.876496	8000.220186	12.934285	-0.058926	4.818734
288.125328	8000.232837	12.939290	-0.058973	4.818737
287.993422	8000.237431	12.944295	-0.058948	4.818738
288.095886	8000.241903	12.949299	-0.058967	4.818739
287.910194	8000.216444	12.954304	-0.058933	4.818733
287.899923	8000.244628	12.959309	-0.058931	4.818741
287.877316	8000.226515	12.964314	-0.058927	4.818736
287.837031	8000.259554	12.969319	-0.058919	4.818746
288.046894	8000.245488	12.974323	-0.058959	4.818741
287.794150	8000.230699	12.979328	-0.058912	4.818737
287.805921	8000.248681	12.984333	-0.058914	4.818743
287.925412	8000.238692	12.989338	-0.058936	4.818739
287.977917	8000.227839	12.994343	-0.058946	4.818736
288.027476	8000.257843	12.999347	-0.058955	4.818744
288.044954	8000.217178	13.004352	-0.058959	4.818732
288.076089	8000.249042	13.009357	-0.058965	4.818742
287.667523	8000.217563	13.014362	-0.058888	4.818734
287.908596	8000.223822	13.019367	-0.058933	4.818735
288.105847	8000.250488	13.024371	-0.058970	4.818742
288.100419	8000.234694	13.029376	-0.058969	4.818737
287.938509	8000.240998	13.034381	-0.058939	4.818740
288.106851	8000.241077	13.039386	-0.058971	4.818739
287.973204	8000.234115	13.044391	-0.058946	4.818738
287.836720	8000.236553	13.049395	-0.058920	4.818739
287.831554	8000.220763	13.054400	-0.058920	4.818734
288.057172	8000.241503	13.059405	-0.058962	4.818739
287.972412	8000.234123	13.064410	-0.058946	4.818738
287.881735	8000.225617	13.069415	-0.058929	4.818735
288.021219	8000.229518	13.074419	-0.058955	4.818736
287.750322	8000.243855	13.079424	-0.058905	4.818741
287.728630	8000.241482	13.084429	-0.058901	4.818741
287.890645	8000.253014	13.089434	-0.058931	4.818743
287.747800	8000.216573	13.094439	-0.058904	4.818733
287.512817	8000.239761	13.099443	-0.058861	4.818741
287.995189	8000.212432	13.104448	-0.058951	4.818731
287.857463	8000.218000	13.109453	-0.058925	4.818733
287.660010	8000.252159	13.114458	-0.058888	4.818744
287.844083	8000.218885	13.119463	-0.058923	4.818733
287.985161	8000.268944	13.124467	-0.058949	4.818748
287.788261	8000.249632	13.129472	-0.058912	4.818743
287.820548	8000.266830	13.134477	-0.058919	4.818748
287.907365	8000.265857	13.139482	-0.058935	4.818747
287.626980	8000.273780	13.144487	-0.058883	4.818751
287.778551	8000.305100	13.149491	-0.058911	4.818759
287.757023	8000.240863	13.154496	-0.058907	4.818740
287.670386	8000.253382	13.159501	-0.058891	4.818744
287.538816	8000.259030	13.164506	-0.058866	4.818747
287.586954	8000.253363	13.169511	-0.058876	4.818745
287.654380	8000.290938	13.174515	-0.058888	4.818756
287.891059	8000.227934	13.179520	-0.058932	4.818736
287.847389	8000.247298	13.184525	-0.058924	4.818742
288.082758	8000.251387	13.189530	-0.058968	4.818742
287.729769	8000.232159	13.194535	-0.058902	4.818738
287.768893	8000.249445	13.199539	-0.058910	4.818743
287.935076	8000.200212	13.204544	-0.058941	4.818728
287.769110	8000.257846	13.209549	-0.058910	4.818745
287.886534	8000.239441	13.214554	-0.058932	4.818739
287.863731	8000.232860	13.219559	-0.058928	4.818738
287.875750	8000.269720	13.224563	-0.058930	4.818748
287.909391	8000.236604	13.229568	-0.058936	4.818738
287.951026	8000.247631	13.234573	-0.058944	4.818742
288.021012	8000.234907	13.239578	-0.058957	4.818738
287.775234	8000.243276	13.244583	-0.058912	4.818741
287.862781	8000.250701	13.249587	-0.058928	4.818743
287.732120	8000.236437	13.254592	-0.058904	4.818739
287.604091	8000.248422	13.259597	-0.058880	4.818743
288.039381	8000.244604	13.264602	-0.058961	4.818740
287.949309	8000.213037	13.269607	-0.058944	4.818731
287.935707	8000.242227	13.274611	-0.058942	4.818740
288.040702	8000.204788	13.279616	-0.058961	4.818728
287.981190	8000.221851	13.284621	-0.058950	4.818734
288.137940	8000.247995	13.289626	-0.058980	4.818741
287.842745	8000.235803	13.294631	-0.058925	4.818738
287.739968	8000.263842	13.299635	-0.058906	4.818747
287.614322	8000.268518	13.304640	-0.058882	4.818749
287.908463	8000.262879	13.309645	-0.058937	4.818746
287.850570	8000.258991	13.314650	-0.058926	4.818745
287.527820	8000.245396	13.319655	-0.058866	4.818743
287.922999	8000.249448	13.324659	-0.058940	4.818742
287.894701	8000.233359	13.329664	-0.058935	4.818738
287.613952	8000.270637	13.334669	-0.058883	4.818750
287.636396	8000.292951	13.339674	-0.058887	4.818756
287.832142	8000.262974	13.344679	-0.058923	4.818747
287.885673	8000.258426	13.349683	-0.058933	4.818745
288.028470	8000.214135	13.354688	-0.058960	4.818731
288.178076	8000.245429	13.359693	-0.058988	4.818740
288.238281	8000.250405	13.364698	-0.058999	4.818741
287.924189	8000.218046	13.369703	-0.058941	4.818733
287.972743	8000.273204	13.374707	-0.058950	4.818749
288.021377	8000.245523	13.379712	-0.058959	4.818741
287.821765	8000.230370	13.384717	-0.058922	4.818737
288.026812	8000.267623	13.389722	-0.058960	4.818747
287.596270	8000.227471	13.394727	-0.058880	4.818737
287.764196	8000.278925	13.399731	-0.058912	4.818752
287.537740	8000.268669	13.404736	-0.058869	4.818749
287.765177	8000.248538	13.409741	-0.058912	4.818743
288.010294	8000.274772	13.414746	-0.058958	4.818749
287.644942	8000.239656	13.419751	-0.058890	4.818740
287.815830	8000.260739	13.424755	-0.058921	4.818746
287.827936	8000.250413	13.429760	-0.058924	4.818743
287.643356	8000.281592	13.434765	-0.058889	4.818753
287.486234	8000.297396	13.439770	-0.058860	4.818758
287.847755	8000.262217	13.444775	-0.058928	4.818746
287.904693	8000.272393	13.449779	-0.058938	4.818749
287.848400	8000.245457	13.454784	-0.058928	4.818741
288.201780	8000.245825	13.459789	-0.058994	4.818740
288.161399	8000.261038	13.464794	-0.058986	4.818745
287.932251	8000.233969	13.469799	-0.058944	4.818738
288.047856	8000.263776	13.474803	-0.058965	4.818746
288.013131	8000.235021	13.479808	-0.058959	4.818738
287.695156	8000.264479	13.484813	-0.058900	4.818748
287.905799	8000.267201	13.489818	-0.058939	4.818748
287.966558	8000.233385	13.494823	-0.058950	4.818737
288.064309	8000.274497	13.499827	-0.058969	4.818749
288.055613	8000.241883	13.504832	-0.058967	4.818739
288.192707	8000.262531	13.509837	-0.058993	4.818745
288.119443	8000.249007	13.514842	-0.058979	4.818741
288.140994	8000.227269	13.519847	-0.058983	4.818735
288.196316	8000.250008	13.524851	-0.058994	4.818741
288.100783	8000.214176	13.529856	-0.058976	4.818731
287.925605	8000.253865	13.534861	-0.058943	4.818743
288.134584	8000.268099	13.539866	-0.058982	4.818747
287.985295	8000.246255	13.544871	-0.058955	4.818741
288.094691	8000.261302	13.549875	-0.058975	4.818745
287.721815	8000.257546	13.554880	-0.058906	4.818745
287.899498	8000.253551	13.559885	-0.058939	4.818743
288.135509	8000.276523	13.564890	-0.058983	4.818749
288.106472	8000.232112	13.569895	-0.058977	4.818736
288.208708	8000.249164	13.574899	-0.058997	4.818741
288.154636	8000.239033	13.579904	-0.058987	4.818738
287.971476	8000.238773	13.584909	-0.058952	4.818739
287.829727	8000.293573	13.589914	-0.058926	4.818756
287.714074	8000.250142	13.594919	-0.058905	4.818743
287.700887	8000.280385	13.599923	-0.058902	4.818752
287.544127	8000.282563	13.604928	-0.058873	4.818753
287.808270	8000.247176	13.609933	-0.058922	4.818742
287.910196	8000.263175	13.614938	-0.058941	4.818746
287.595013	8000.250726	13.619943	-0.058883	4.818744
287.676198	8000.264361	13.624947	-0.058898	4.818748
288.088490	8000.237177	13.629952	-0.058975	4.818738
288.082396	8000.239200	13.634957	-0.058974	4.818738
288.123052	8000.260700	13.639962	-0.058981	4.818745
288.155662	8000.252737	13.644967	-0.058988	4.818742
288.161145	8000.270638	13.649971	-0.058989	4.818748
288.067447	8000.242171	13.654976	-0.058971	4.818739
288.050427	8000.267122	13.659981	-0.058968	4.818747
288.090818	8000.259259	13.664986	-0.058976	4.818744
288.018005	8000.266713	13.669991	-0.058962	4.818747
288.153471	8000.273707	13.674995	-0.058988	4.818748
288.025240	8000.231163	13.680000	-0.058964	4.818736
288.098745	8000.238407	13.685005	-0.058977	4.818738
288.141460	8000.285101	13.690010	-0.058986	4.818752
287.969168	8000.218919	13.695015	-0.058953	4.818733
287.811682	8000.286099	13.700019	-0.058924	4.818753
287.815433	8000.259937	13.705024	-0.058925	4.818746
287.803634	8000.275518	13.710029	-0.058923	4.818750
287.941425	8000.261571	13.715034	-0.058949	4.818746
287.894625	8000.254680	13.720039	-0.058940	4.818744
287.892371	8000.252558	13.725043	-0.058940	4.818743
287.882479	8000.254533	13.730048	-0.058938	4.818744
287.925044	8000.239357	13.735053	-0.058946	4.818739
287.947145	8000.270056	13.740058	-0.058950	4.818748
288.077813	8000.232948	13.745063	-0.058974	4.818737
288.280186	8000.248146	13.750067	-0.059012	4.818740
288.113384	8000.237610	13.755072	-0.058981	4.818738
288.283958	8000.258690	13.760077	-0.059013	4.818743
288.320016	8000.261257	13.765082	-0.059020	4.818744
288.344938	8000.234319	13.770087	-0.059024	4.818736
288.441039	8000.275410	13.775091	-0.059042	4.818748
288.469303	8000.236981	13.780096	-0.059048	4.818736
288.395526	8000.220305	13.785101	-0.059034	4.818732
288.522163	8000.227186	13.790106	-0.059058	4.818733
288.299104	8000.219070	13.795111	-0.059016	4.818732
288.492245	8000.237295	13.800115	-0.059052	4.818736
288.243277	8000.221505	13.805120	-0.059006	4.818733
288.136614	8000.236911	13.810125	-0.058986	4.818738
288.183720	8000.286807	13.815130	-0.058995	4.818752
288.284259	8000.219949	13.820135	-0.059014	4.818732
288.117190	8000.255548	13.825139	-0.058983	4.818743
288.249638	8000.248873	13.830144	-0.059007	4.818741
288.261058	8000.232247	13.835149	-0.059010	4.818736
288.406648	8000.250907	13.840154	-0.059037	4.818741
288.228495	8000.249662	13.845159	-0.059004	4.818741
288.499228	8000.262597	13.850163	-0.059054	4.818744
288.475460	8000.224545	13.855168	-0.059050	4.818733
288.202816	8000.236761	13.860173	-0.058999	4.818737
288.142147	8000.240177	13.865178	-0.058988	4.818738
288.186534	8000.220831	13.870183	-0.058996	4.818733
288.156177	8000.261339	13.875187	-0.058991	4.818745
288.293963	8000.219080	13.880192	-0.059016	4.818732
287.997918	8000.247772	13.885197	-0.058961	4.818741
288.303137	8000.250665	13.890202	-0.059018	4.818741
287.983762	8000.238161	13.895207	-0.058959	4.818738
288.129702	8000.284089	13.900211	-0.058986	4.818752
288.220398	8000.260097	13.905216	-0.059003	4.818744
288.121417	8000.266165	13.910221	-0.058985	4.818746
288.245139	8000.222676	13.915226	-0.059008	4.818733
288.303890	8000.216098	13.920231	-0.059019	4.818731
288.378112	8000.243275	13.925235	-0.059033	4.818738
288.371231	8000.215927	13.930240	-0.059031	4.818730
288.341228	8000.230225	13.935245	-0.059026	4.818735
288.294808	8000.264235	13.940250	-0.059017	4.818745
288.163546	8000.226894	13.945255	-0.058993	4.818734
288.256652	8000.248022	13.950259	-0.059010	4.818740
288.506339	8000.240762	13.955264	-0.059057	4.818737
288.095911	8000.232326	13.960269	-0.058981	4.818736
288.360267	8000.248324	13.965274	-0.059030	4.818740
288.395907	8000.213136	13.970279	-0.059037	4.818729
288.375966	8000.256924	13.975283	-0.059033	4.818743
288.458978	8000.272680	13.980288	-0.059048	4.818747
288.589434	8000.251299	13.985293	-0.059073	4.818740
288.406451	8000.267817	13.990298	-0.059039	4.818746
288.380507	8000.207717	13.995303	-0.059034	4.818728
288.476599	8000.228884	14.000307	-0.059052	4.818734
288.244976	8000.242678	14.005312	-0.059009	4.818739
288.344094	8000.245010	14.010317	-0.059027	4.818739
288.517394	8000.280806	14.015322	-0.059060	4.818749
288.576850	8000.237536	14.020327	-0.059071	4.818736
288.412699	8000.255346	14.025331	-0.059040	4.818742
288.603776	8000.234747	14.030336	-0.059076	4.818735
288.594883	8000.235685	14.035341	-0.059074	4.818735
288.606575	8000.253667	14.040346	-0.059077	4.818741
288.401086	8000.233194	14.045351	-0.059038	4.818735
288.506333	8000.258674	14.050355	-0.059058	4.818743
288.535357	8000.242275	14.055360	-0.059064	4.818738
288.353257	8000.246222	14.060365	-0.059030	4.818739
288.300385	8000.267565	14.065370	-0.059020	4.818746
288.494559	8000.244908	14.070375	-0.059056	4.818738
288.463832	8000.286460	14.075379	-0.059051	4.818751
288.470906	8000.246709	14.080384	-0.059052	4.818739
288.224110	8000.254016	14.085389	-0.059006	4.818742
288.283538	8000.278905	14.090394	-0.059017	4.818749
288.495514	8000.237603	14.095399	-0.059057	4.818736
288.514216	8000.266161	14.100403	-0.059060	4.818745
288.490915	8000.259573	14.105408	-0.059056	4.818743
288.663149	8000.255508	14.110413	-0.059088	4.818741
288.564074	8000.258429	14.115418	-0.059070	4.818742
288.642252	8000.240567	14.120423	-0.059084	4.818737
288.453624	8000.275887	14.125427	-0.059049	4.818748
288.383719	8000.238289	14.130432	-0.059036	4.818737
288.077715	8000.260561	14.135437	-0.058979	4.818745
288.443449	8000.264235	14.140442	-0.059048	4.818744
288.303214	8000.245653	14.145447	-0.059022	4.818739
288.197593	8000.292530	14.150451	-0.059002	4.818754
288.553322	8000.273006	14.155456	-0.059068	4.818747
288.435133	8000.243174	14.160461	-0.059046	4.818738
288.484117	8000.235421	14.165466	-0.059055	4.818736
288.531503	8000.234989	14.170471	-0.059064	4.818735
288.423100	8000.246178	14.175475	-0.059044	4.818739
288.527731	8000.252775	14.180480	-0.059064	4.818741
288.466055	8000.251984	14.185485	-0.059052	4.818741
288.467077	8000.271925	14.190490	-0.059053	4.818747
288.601740	8000.261084	14.195495	-0.059078	4.818743
288.320559	8000.272141	14.200499	-0.059026	4.818747
288.578047	8000.236669	14.205504	-0.059073	4.818736
288.522333	8000.239101	14.210509	-0.059063	4.818737
288.572850	8000.272264	14.215514	-0.059073	4.818746
288.403546	8000.235480	14.220519	-0.059041	4.818736
288.673250	8000.243159	14.225523	-0.059091	4.818737
288.362928	8000.233916	14.230528	-0.059034	4.818736
288.314188	8000.204980	14.235533	-0.059025	4.818727
288.568576	8000.254405	14.240538	-0.059072	4.818741
288.509720	8000.226386	14.245543	-0.059061	4.818733
288.488702	8000.233460	14.250547	-0.059057	4.818735
288.533593	8000.242432	14.255552	-0.059066	4.818738
288.635976	8000.217543	14.260557	-0.059085	4.818730
288.368757	8000.266530	14.265562	-0.059035	4.818745
288.260363	8000.252553	14.270567	-0.059015	4.818742
288.500382	8000.275577	14.275571	-0.059060	4.818748
288.519912	8000.254862	14.280576	-0.059064	4.818741
288.396180	8000.229152	14.285581	-0.059041	4.818734
288.486577	8000.260732	14.290586	-0.059058	4.818743
288.414854	8000.226256	14.295591	-0.059044	4.818733
288.244013	8000.254466	14.300595	-0.059013	4.818742
288.438299	8000.229713	14.305600	-0.059049	4.818734
288.385123	8000.233226	14.310605	-0.059039	4.818735
288.337767	8000.257786	14.315610	-0.059030	4.818743
288.387883	8000.225930	14.320615	-0.059040	4.818733
288.456062	8000.227863	14.325619	-0.059052	4.818733
288.505141	8000.237938	14.330624	-0.059062	4.818736
288.417284	8000.202205	14.335629	-0.059045	4.818726
288.687988	8000.238209	14.340634	-0.059096	4.818736
288.636791	8000.237553	14.345639	-0.059086	4.818736
288.577227	8000.269296	14.350643	-0.059075	4.818745
288.707258	8000.264687	14.355648	-0.059100	4.818743
288.410997	8000.257723	14.360653	-0.059044	4.818743
288.469070	8000.280497	14.365658	-0.059055	4.818749
288.267083	8000.240146	14.370663	-0.059018	4.818738
288.489531	8000.260847	14.375667	-0.059059	4.818743
288.449690	8000.241462	14.380672	-0.059052	4.818738
288.293031	8000.244689	14.385677	-0.059023	4.818739
288.457132	8000.281414	14.390682	-0.059053	4.818749
288.452997	8000.247810	14.395687	-0.059053	4.818739
288.542281	8000.253161	14.400691	-0.059069	4.818741
288.666394	8000.240086	14.405696	-0.059093	4.818736
288.629707	8000.255347	14.410701	-0.059086	4.818741
288.587552	8000.261099	14.415706	-0.059078	4.818743
288.529028	8000.227841	14.420711	-0.059067	4.818733
288.498562	8000.247376	14.425715	-0.059062	4.818739
288.602537	8000.246625	14.430720	-0.059081	4.818738
288.523172	8000.217293	14.435725	-0.059066	4.818730
288.489208	8000.255658	14.440730	-0.059060	4.818742
288.452519	8000.241557	14.445735	-0.059053	4.818738
288.553110	7999.194288	14.450739	-0.059071	4.818425

288.570296	7996.138315	14.455744	-0.059073	4.817515
288.563853	7990.618628	14.460749	-0.059068	4.815871
288.486857	7984.036648	14.465754	-0.059049	4.813910
288.484689	7976.809101	14.470759	-0.059044	4.811756
288.360990	7969.154218	14.475763	-0.059016	4.809473
288.510740	7961.457127	14.480768	-0.059039	4.807176
288.136858	7953.439652	14.485773	-0.058964	4.804784
288.494292	7945.619758	14.490778	-0.059026	4.802447
288.458255	7937.597469	14.495783	-0.059014	4.800050
288.268643	7929.627603	14.500787	-0.058974	4.797668
288.330501	7921.630107	14.505792	-0.058980	4.795276
287.912822	7913.648093	14.510797	-0.058897	4.792888
288.227686	7905.595645	14.515802	-0.058951	4.790476
288.086974	7897.576778	14.520807	-0.058919	4.788074
288.171890	7889.608042	14.525811	-0.058930	4.785686
288.080120	7881.588404	14.530816	-0.058908	4.783281
287.909599	7873.598077	14.535821	-0.058871	4.780885
287.867604	7865.571476	14.540826	-0.058858	4.778475
288.100385	7857.609745	14.545831	-0.058896	4.776083
287.934818	7849.514235	14.550835	-0.058860	4.773651
287.940991	7841.580212	14.555840	-0.058856	4.771266
287.988233	7833.514588	14.560845	-0.058860	4.768840
288.027878	7825.560859	14.565850	-0.058862	4.766446
287.965763	7817.519031	14.570855	-0.058845	4.764025
287.758389	7809.631393	14.575859	-0.058801	4.761650
287.807502	7801.562411	14.580864	-0.058805	4.759218
287.768595	7793.581723	14.585869	-0.058793	4.756811
288.065332	7785.543542	14.590874	-0.058843	4.754386
287.997849	7777.613126	14.595879	-0.058825	4.751992
287.951947	7769.505003	14.600883	-0.058812	4.749543
287.596639	7761.540398	14.605888	-0.058740	4.747138
287.788851	7753.492916	14.610893	-0.058771	4.744704
287.920747	7745.582207	14.615898	-0.058790	4.742311
287.515369	7737.484222	14.620903	-0.058710	4.739861
287.624351	7729.525801	14.625907	-0.058725	4.737452
287.953901	7721.543905	14.630912	-0.058781	4.735033
287.678624	7713.565452	14.635917	-0.058725	4.732615
287.763756	7705.520193	14.640922	-0.058735	4.730175
287.759928	7697.532058	14.645927	-0.058730	4.727752
287.787092	7689.491644	14.650931	-0.058729	4.725311
287.634105	7681.559271	14.655936	-0.058696	4.722902
287.675232	7673.518996	14.660941	-0.058698	4.720459
287.802423	7665.553099	14.665946	-0.058717	4.718037
287.436197	7657.556144	14.670951	-0.058644	4.715605
287.415893	7649.537300	14.675955	-0.058635	4.713164
287.541543	7641.577569	14.680960	-0.058653	4.710740
287.474621	7633.539159	14.685965	-0.058635	4.708291
287.444451	7625.547089	14.690970	-0.058625	4.705855
287.264105	7617.519742	14.695975	-0.058586	4.703407
287.315420	7609.540410	14.700979	-0.058590	4.700972
287.538395	7601.536111	14.705984	-0.058627	4.698529
287.355622	7593.528528	14.710989	-0.058587	4.696083
287.522042	7585.499642	14.715994	-0.058613	4.693629
287.124781	7577.567302	14.720999	-0.058534	4.691204
286.918442	7569.511152	14.726003	-0.058491	4.688739
287.373286	7561.562803	14.731008	-0.058570	4.686306
287.262949	7553.473534	14.736013	-0.058544	4.683829
287.073269	7545.605408	14.741018	-0.058504	4.681418
287.247537	7537.460030	14.746023	-0.058531	4.678921
287.154763	7529.569869	14.751027	-0.058509	4.676500
286.954906	7521.533178	14.756032	-0.058466	4.674034
286.765860	7513.498795	14.761037	-0.058426	4.671567
287.011373	7505.454917	14.766042	-0.058467	4.669096
286.976454	7497.479990	14.771047	-0.058455	4.666644
287.108835	7489.400778	14.776051	-0.058474	4.664159
287.009383	7481.539767	14.781056	-0.058451	4.661740
286.834142	7473.453757	14.786061	-0.058413	4.659251
286.878413	7465.518041	14.791066	-0.058416	4.656806
286.644551	7457.481228	14.796071	-0.058367	4.654329
286.820463	7449.479994	14.801075	-0.058395	4.651862
286.774570	7441.414293	14.806080	-0.058381	4.649374
286.745676	7433.446952	14.811085	-0.058371	4.646914
286.881418	7425.402840	14.816090	-0.058391	4.644430
286.881277	7417.469202	14.821095	-0.058386	4.641978
286.675533	7409.430018	14.826099	-0.058342	4.639492
286.851585	7401.523766	14.831104	-0.058370	4.637046
286.820970	7393.419309	14.836109	-0.058359	4.634538
286.852764	7385.463257	14.841114	-0.058360	4.632074
286.820714	7377.431996	14.846119	-0.058349	4.629585
286.815054	7369.428167	14.851123	-0.058342	4.627104
286.784971	7361.433736	14.856128	-0.058332	4.624624
286.769438	7353.436532	14.861133	-0.058324	4.622142
286.766880	7345.392339	14.866138	-0.058318	4.619644
286.331100	7337.529668	14.871143	-0.058232	4.617201
286.448054	7329.352217	14.876147	-0.058248	4.614659
286.661686	7321.434783	14.881152	-0.058283	4.612197
286.726477	7313.392674	14.886157	-0.058290	4.609694
286.495352	7305.449298	14.891162	-0.058242	4.607221
286.364718	7297.395660	14.896167	-0.058212	4.604711
286.188566	7289.479842	14.901171	-0.058174	4.602244
286.396039	7281.458539	14.906176	-0.058208	4.599742
286.374838	7273.463602	14.911181	-0.058199	4.597248
286.312809	7265.442232	14.916186	-0.058182	4.594743
286.047979	7257.413308	14.921191	-0.058128	4.592235
285.984568	7249.359861	14.926195	-0.058111	4.589717
286.236407	7241.454856	14.931200	-0.058152	4.587246
286.006297	7233.371214	14.936205	-0.058104	4.584716
286.146156	7225.393649	14.941210	-0.058125	4.582219
285.768753	7217.371701	14.946215	-0.058050	4.579705
286.062272	7209.414856	14.951219	-0.058099	4.577212
286.182084	7201.363828	14.956224	-0.058116	4.574687
285.864340	7193.392721	14.961229	-0.058052	4.572186
286.044018	7185.371019	14.966234	-0.058080	4.569668
286.145597	7177.387014	14.971239	-0.058094	4.567160
285.829087	7169.347809	14.976243	-0.058030	4.564633
286.171926	7161.431388	14.981248	-0.058089	4.562144
285.867405	7153.380232	14.986253	-0.058027	4.559611
285.917969	7145.428078	14.991258	-0.058031	4.557107
286.021084	7137.312397	14.996263	-0.058045	4.554551
286.024436	7129.353581	15.001267	-0.058041	4.552043
286.119945	7121.292477	15.006272	-0.058053	4.549502
285.973348	7113.316072	15.011277	-0.058021	4.546985
286.078098	7105.294491	15.016282	-0.058035	4.544453
285.856366	7097.377109	15.021287	-0.057989	4.541951
285.885603	7089.320661	15.026291	-0.057989	4.539405
285.921271	7081.425611	15.031296	-0.057991	4.536909
285.873579	7073.342338	15.036301	-0.057977	4.534351
285.553968	7065.365878	15.041306	-0.057912	4.531825
285.528908	7057.335896	15.046311	-0.057902	4.529282
285.627336	7049.346618	15.051315	-0.057915	4.526750
285.821316	7041.273192	15.056320	-0.057946	4.524191
285.555200	7033.364527	15.061325	-0.057892	4.521681
285.800823	7025.296602	15.066330	-0.057932	4.519120
285.799454	7017.346886	15.071335	-0.057927	4.516595
285.429427	7009.298663	15.076339	-0.057853	4.514036
285.577312	7001.400472	15.081344	-0.057875	4.511525
285.419410	6993.308056	15.086349	-0.057841	4.508950
285.695574	6985.286842	15.091354	-0.057887	4.506397
285.254339	6977.268778	15.096359	-0.057800	4.503842
285.356326	6969.310596	15.101363	-0.057813	4.501306
285.551022	6961.256881	15.106368	-0.057844	4.498738
285.492574	6953.252905	15.111373	-0.057828	4.496184
285.533914	6945.286464	15.116378	-0.057831	4.493641
285.602612	6937.250894	15.121383	-0.057839	4.491074
285.355484	6929.224010	15.126387	-0.057787	4.488508
285.437563	6921.250174	15.131392	-0.057798	4.485958
285.294466	6913.261432	15.136397	-0.057766	4.483401
285.512283	6905.293851	15.141402	-0.057801	4.480851
285.408788	6897.285470	15.146407	-0.057777	4.478285
285.486272	6889.269461	15.151411	-0.057786	4.475716
285.684402	6881.237832	15.156416	-0.057818	4.473141
285.507197	6873.211288	15.161421	-0.057780	4.470564
285.416455	6865.227071	15.166426	-0.057758	4.468000
285.333764	6857.240562	15.171431	-0.057737	4.465434
285.206952	6849.247695	15.176435	-0.057708	4.462864
285.253876	6841.280146	15.181440	-0.057712	4.460301
285.301787	6833.232780	15.186445	-0.057716	4.457712
285.373281	6825.221697	15.191450	-0.057724	4.455132
284.993015	6817.254303	15.196455	-0.057648	4.452563
285.002224	6809.178976	15.201459	-0.057644	4.449960
285.105573	6801.243283	15.206464	-0.057659	4.447400
285.101632	6793.160128	15.211469	-0.057653	4.444791
285.032558	6785.265452	15.216474	-0.057635	4.442241
285.005426	6777.228802	15.221479	-0.057624	4.439644
284.839086	6769.271620	15.226483	-0.057588	4.437070
284.875121	6761.211485	15.231488	-0.057590	4.434463
284.867767	6753.242641	15.236493	-0.057583	4.431883
285.003803	6745.174768	15.241498	-0.057603	4.429270
284.993561	6737.215308	15.246503	-0.057596	4.426691
284.532829	6729.138615	15.251507	-0.057505	4.424069
284.843782	6721.253040	15.256512	-0.057558	4.421512
284.744806	6713.136179	15.261517	-0.057535	4.418876
284.708605	6705.243058	15.266522	-0.057523	4.416312
284.792124	6697.216929	15.271527	-0.057533	4.413703
284.624876	6689.272211	15.276531	-0.057497	4.411118
284.612109	6681.150906	15.281536	-0.057489	4.408475
284.574237	6673.166275	15.286541	-0.057477	4.405875
284.776529	6665.165436	15.291546	-0.057510	4.403269
284.715925	6657.223237	15.296551	-0.057493	4.400680
284.588560	6649.245925	15.301555	-0.057464	4.398076
284.646011	6641.264920	15.306560	-0.057470	4.395472
284.518301	6633.258921	15.311565	-0.057441	4.392856
284.678715	6625.239464	15.316570	-0.057466	4.390236
284.832391	6617.251601	15.321575	-0.057489	4.387625
284.654684	6609.196144	15.326579	-0.057451	4.384989
284.613372	6601.288613	15.331584	-0.057438	4.382400
284.395298	6593.261847	15.336589	-0.057392	4.379769
284.338141	6585.367967	15.341594	-0.057377	4.377181
284.245591	6577.293981	15.346599	-0.057354	4.374532
284.268821	6569.314667	15.351603	-0.057353	4.371914
284.652701	6561.237178	15.356608	-0.057420	4.369264
284.485026	6553.242183	15.361613	-0.057383	4.366636
284.444299	6545.279623	15.366618	-0.057371	4.364018
284.314125	6537.378906	15.371623	-0.057341	4.361418
284.402496	6529.306378	15.376627	-0.057353	4.358761
284.139987	6521.400287	15.381632	-0.057299	4.356155
284.202363	6513.239631	15.386637	-0.057305	4.353466
284.198498	6505.224668	15.391642	-0.057299	4.350823
284.162562	6497.225743	15.396647	-0.057287	4.348184
284.079613	6489.200669	15.401651	-0.057267	4.345533
284.040452	6481.255065	15.406656	-0.057254	4.342908
283.932151	6473.257415	15.411661	-0.057229	4.340263
283.719777	6465.331376	15.416666	-0.057184	4.337640
284.045123	6457.255637	15.421671	-0.057240	4.334970
284.256197	6449.215837	15.426675	-0.057274	4.332309
284.214456	6441.243686	15.431680	-0.057261	4.329667
283.935478	6433.274829	15.436685	-0.057204	4.327022
283.957631	6425.251636	15.441690	-0.057203	4.324360
283.701477	6417.310959	15.446695	-0.057150	4.321722
283.693940	6409.259895	15.451699	-0.057143	4.319047
283.882682	6401.328010	15.456704	-0.057173	4.316412
283.990855	6393.249104	15.461709	-0.057188	4.313726
283.795088	6385.286305	15.466714	-0.057147	4.311074
283.953400	6377.231058	15.471719	-0.057171	4.308393
284.043881	6369.191938	15.476723	-0.057183	4.305715
283.647920	6361.270026	15.481728	-0.057104	4.303070
283.506446	6353.221879	15.486733	-0.057072	4.300384
283.787047	6345.220655	15.491738	-0.057120	4.297715
283.628625	6337.246574	15.496743	-0.057085	4.295050
283.348264	6329.268735	15.501747	-0.057028	4.292380
283.276417	6321.223014	15.506752	-0.057009	4.289689
283.410308	6313.228857	15.511757	-0.057029	4.287014
283.046411	6305.240590	15.516762	-0.056956	4.284336
283.240834	6297.257501	15.521767	-0.056987	4.281662
283.151561	6289.205506	15.526771	-0.056965	4.278961
283.566041	6281.254874	15.531776	-0.057037	4.276298
283.366488	6273.213364	15.536781	-0.056995	4.273596
283.604204	6265.211690	15.541786	-0.057034	4.270910
283.485993	6257.208669	15.546791	-0.057007	4.268219
283.456429	6249.178449	15.551795	-0.056996	4.265517
283.532452	6241.220675	15.556800	-0.057005	4.262839
283.513096	6233.192885	15.561805	-0.056996	4.260135
283.443520	6225.239320	15.566810	-0.056978	4.257454
283.342626	6217.221412	15.571815	-0.056954	4.254749
283.475608	6209.180260	15.576819	-0.056974	4.252037
283.659913	6201.161106	15.581824	-0.057003	4.249331
283.299598	6193.182253	15.586829	-0.056931	4.246632
283.278310	6185.175035	15.591834	-0.056922	4.243924
283.216950	6177.254454	15.596839	-0.056905	4.241244
283.132428	6169.192128	15.601843	-0.056884	4.238514
283.164120	6161.235479	15.606848	-0.056885	4.235819
283.070759	6153.198550	15.611853	-0.056863	4.233094
283.135591	6145.167303	15.616858	-0.056869	4.230371
283.116722	6137.165053	15.621863	-0.056861	4.227654
282.988309	6129.202752	15.626867	-0.056832	4.224949
283.060163	6121.230824	15.631872	-0.056840	4.222240
283.127077	6113.173289	15.636877	-0.056847	4.219501
283.179920	6105.214068	15.641882	-0.056852	4.216794
283.070953	6097.152565	15.646887	-0.056827	4.214047
283.087916	6089.167284	15.651891	-0.056825	4.211327
283.145872	6081.214166	15.656896	-0.056830	4.208616
283.172432	6073.159266	15.661901	-0.056830	4.205868
282.968616	6065.197893	15.666906	-0.056787	4.203148
282.681248	6057.223601	15.671911	-0.056728	4.200421
282.852354	6049.210580	15.676915	-0.056755	4.197684
282.912499	6041.208376	15.681920	-0.056761	4.194947
282.667587	6033.139895	15.686925	-0.056710	4.192183
282.484610	6025.115689	15.691930	-0.056671	4.189432
282.870904	6017.134233	15.696935	-0.056738	4.186701
282.515634	6009.128482	15.701939	-0.056666	4.183952
282.298356	6001.256030	15.706944	-0.056621	4.181247
282.287487	5993.168737	15.711949	-0.056614	4.178470
282.370375	5985.203358	15.716954	-0.056624	4.175734
282.672139	5977.150872	15.721959	-0.056675	4.172969
282.599090	5969.164357	15.726963	-0.056656	4.170220
282.513836	5961.228913	15.731968	-0.056635	4.167486
282.565622	5953.129740	15.736973	-0.056640	4.164697
282.535310	5945.230913	15.741978	-0.056629	4.161973
282.493589	5937.215571	15.746983	-0.056616	4.159207
282.418487	5929.246606	15.751987	-0.056597	4.156455
282.506376	5921.221751	15.756992	-0.056608	4.153684
282.281615	5913.241964	15.761997	-0.056561	4.150923
282.227626	5905.198881	15.767002	-0.056546	4.148140
282.014716	5897.238489	15.772007	-0.056501	4.145381
282.150079	5889.198112	15.777011	-0.056521	4.142598
282.267142	5881.243930	15.782016	-0.056538	4.139843
281.939168	5873.239281	15.787021	-0.056472	4.137062
281.999742	5865.189129	15.792026	-0.056478	4.134269
282.207939	5857.230306	15.797031	-0.056511	4.131507
282.255521	5849.179744	15.802035	-0.056515	4.128710
282.225025	5841.221153	15.807040	-0.056504	4.125942
282.015590	5833.218501	15.812045	-0.056460	4.123154
282.107171	5825.231801	15.817050	-0.056472	4.120374
282.091342	5817.236837	15.822055	-0.056464	4.117587
282.131729	5809.198507	15.827059	-0.056466	4.114785
282.112876	5801.221692	15.832064	-0.056458	4.112001
282.022221	5793.160254	15.837069	-0.056436	4.109184
281.789180	5785.203066	15.842074	-0.056387	4.106400
281.953148	5777.163745	15.847079	-0.056412	4.103592
281.923648	5769.204707	15.852083	-0.056402	4.100806
281.644840	5761.262278	15.857088	-0.056345	4.098021
281.645044	5753.199794	15.862093	-0.056340	4.095196
281.675662	5745.227949	15.867098	-0.056340	4.092401
281.548018	5737.203240	15.872103	-0.056311	4.089583
281.366647	5729.191713	15.877107	-0.056272	4.086768
281.545059	5721.157268	15.882112	-0.056300	4.083947
281.870964	5713.191282	15.887117	-0.056356	4.081151
281.849664	5705.194868	15.892122	-0.056347	4.078337
281.649486	5697.212535	15.897127	-0.056304	4.075524
281.551540	5689.205721	15.902131	-0.056281	4.072701
281.490344	5681.208228	15.907136	-0.056265	4.069881
281.827889	5673.187506	15.912141	-0.056322	4.067056
281.496923	5665.176618	15.917146	-0.056255	4.064222
281.553210	5657.243718	15.922151	-0.056261	4.061420
281.114258	5649.247142	15.927155	-0.056174	4.058586
281.410102	5641.276804	15.932160	-0.056224	4.055771
281.228443	5633.235230	15.937165	-0.056185	4.052921
281.452195	5625.166355	15.942170	-0.056221	4.050065
281.378233	5617.230836	15.947175	-0.056202	4.047250
281.260576	5609.174419	15.952179	-0.056175	4.044390
281.235635	5601.275151	15.957184	-0.056166	4.041585
281.003237	5593.276602	15.962189	-0.056117	4.038739
281.399100	5585.233246	15.967194	-0.056186	4.035886
281.177992	5577.235033	15.972199	-0.056139	4.033036
281.037115	5569.166140	15.977203	-0.056108	4.030161
281.194584	5561.246971	15.982208	-0.056132	4.027342
281.150082	5553.180718	15.987213	-0.056119	4.024465
280.934595	5545.268149	15.992218	-0.056074	4.021638
280.920702	5537.236459	15.997223	-0.056066	4.018770
280.880684	5529.251043	16.002227	-0.056053	4.015915
280.803891	5521.248622	16.007232	-0.056034	4.013053
281.031397	5513.192214	16.012237	-0.056071	4.010173
280.862720	5505.281449	16.017242	-0.056034	4.007338
280.771851	5497.228956	16.022247	-0.056012	4.004451
280.698336	5489.255457	16.027251	-0.055994	4.001590
280.852423	5481.284589	16.032256	-0.056017	3.998732
281.087616	5473.285034	16.037261	-0.056056	3.995863
280.826739	5465.294316	16.042266	-0.056002	3.992987
280.631668	5457.275034	16.047271	-0.055961	3.990099
280.794758	5449.246762	16.052275	-0.055986	3.987213
281.089059	5441.216078	16.057280	-0.056035	3.984325
280.768955	5433.313113	16.062285	-0.055971	3.981471
280.798224	5425.300060	16.067290	-0.055971	3.978582
280.735978	5417.318111	16.072295	-0.055954	3.975699
280.821239	5409.273298	16.077299	-0.055965	3.972795
280.906788	5401.236051	16.082304	-0.055976	3.969891
280.436493	5393.286895	16.087309	-0.055883	3.967007
280.261783	5385.288320	16.092314	-0.055845	3.964108
280.236442	5377.338950	16.097319	-0.055835	3.961228
280.273913	5369.257904	16.102323	-0.055837	3.958299
280.157921	5361.317095	16.107328	-0.055811	3.955416
280.091147	5353.281626	16.112333	-0.055793	3.952497
280.363238	5345.211541	16.117338	-0.055838	3.949570
280.357640	5337.250042	16.122343	-0.055832	3.946675
280.331906	5329.218247	16.127347	-0.055822	3.943752
280.434493	5321.268036	16.132352	-0.055836	3.940858
280.439754	5313.243060	16.137357	-0.055832	3.937934
280.162739	5305.304705	16.142362	-0.055775	3.935034
280.449868	5297.249506	16.147367	-0.055824	3.932099
280.182168	5289.239691	16.152371	-0.055769	3.929169
280.161232	5281.326237	16.157376	-0.055760	3.926276
280.212489	5273.258664	16.162381	-0.055764	3.923326
280.025217	5265.316419	16.167386	-0.055724	3.920415
280.235250	5257.349547	16.172391	-0.055758	3.917501
279.854913	5249.297614	16.177395	-0.055682	3.914541
280.185346	5241.265552	16.182400	-0.055738	3.911601
280.271024	5233.266223	16.187405	-0.055749	3.908666
280.150384	5225.313790	16.192410	-0.055722	3.905741
280.094288	5217.348581	16.197415	-0.055706	3.902811
280.095174	5209.323514	16.202419	-0.055701	3.899858
280.194730	5201.378783	16.207424	-0.055714	3.896934
280.046159	5193.322373	16.212429	-0.055682	3.893962
280.052367	5185.318640	16.217434	-0.055678	3.891010
280.001432	5177.346133	16.222439	-0.055663	3.888067
280.104541	5169.306920	16.227443	-0.055677	3.885099
279.803722	5161.410312	16.232448	-0.055616	3.882174
279.765177	5153.363391	16.237453	-0.055604	3.879196
279.793084	5145.425147	16.242458	-0.055604	3.876258
279.785206	5137.344165	16.247463	-0.055597	3.873263
279.682233	5129.216749	16.252467	-0.055573	3.870247
279.454498	5121.300428	16.257472	-0.055525	3.867305
279.546196	5113.272887	16.262477	-0.055537	3.864326
279.510302	5105.321769	16.267482	-0.055525	3.861370
279.583366	5097.348701	16.272487	-0.055534	3.858406
279.567947	5089.318915	16.277491	-0.055526	3.855416
279.499392	5081.388074	16.282496	-0.055508	3.852460
279.652568	5073.310721	16.287501	-0.055531	3.849452
279.744223	5065.347752	16.292506	-0.055543	3.846483
279.693941	5057.360725	16.297511	-0.055529	3.843500
279.852092	5049.329321	16.302515	-0.055553	3.840502
279.990517	5041.357021	16.307520	-0.055573	3.837524
280.088612	5033.320688	16.312525	-0.055587	3.834518
279.733034	5025.388239	16.317530	-0.055515	3.831539
279.774071	5017.373676	16.322535	-0.055518	3.828536
279.363432	5009.386424	16.327539	-0.055436	3.825530
279.691398	5001.385679	16.332544	-0.055492	3.822534
279.638122	4993.355748	16.337549	-0.055477	3.819516
279.303370	4985.431255	16.342554	-0.055410	3.816528
278.986218	4977.433278	16.347559	-0.055345	3.813511
279.045485	4969.390029	16.352563	-0.055351	3.810483
279.218047	4961.395134	16.357568	-0.055378	3.807473
279.298960	4953.312793	16.362573	-0.055388	3.804426
279.174706	4945.442015	16.367578	-0.055360	3.801452
279.342298	4937.400186	16.372583	-0.055386	3.798417
279.402965	4929.398515	16.377587	-0.055392	3.795393
279.230740	4921.483516	16.382592	-0.055355	3.792394
278.994218	4913.413211	16.387597	-0.055306	3.789332
278.867607	4905.422589	16.392602	-0.055277	3.786300
278.788070	4897.425630	16.397607	-0.055257	3.783264
278.342311	4889.494959	16.402611	-0.055169	3.780243
278.902554	4881.470939	16.407616	-0.055268	3.777207
279.006301	4873.398887	16.412621	-0.055282	3.774140
278.552860	4865.484867	16.417626	-0.055193	3.771118
279.009086	4857.410994	16.422631	-0.055272	3.768053
278.961863	4849.381108	16.427635	-0.055258	3.764991
278.898721	4841.490492	16.432640	-0.055242	3.761980
278.900664	4833.440246	16.437645	-0.055237	3.758906
278.923789	4825.528355	16.442650	-0.055236	3.755883
278.836594	4817.526266	16.447655	-0.055215	3.752821
278.933851	4809.437358	16.452659	-0.055227	3.749727
279.031706	4801.484585	16.457664	-0.055241	3.746683
278.844748	4793.482584	16.462669	-0.055201	3.743611
278.806901	4785.520674	16.467674	-0.055188	3.740555
278.538887	4777.577831	16.472679	-0.055133	3.737498
278.645977	4769.479090	16.477683	-0.055148	3.734389
278.739956	4761.495818	16.482688	-0.055160	3.731320
278.834568	4753.481746	16.487693	-0.055173	3.728238
278.848688	4745.455266	16.492698	-0.055170	3.725146
278.529386	4737.562679	16.497703	-0.055106	3.722094
278.255029	4729.545967	16.502707	-0.055050	3.718993
278.312118	4721.608586	16.507712	-0.055055	3.715929
278.263812	4713.513606	16.512717	-0.055041	3.712799
278.225640	4705.472394	16.517722	-0.055029	3.709687
278.270836	4697.504901	16.522727	-0.055032	3.706603
277.980096	4689.527946	16.527731	-0.054973	3.703504
277.943192	4681.551155	16.532736	-0.054961	3.700409
278.145221	4673.490953	16.537741	-0.054993	3.697285
278.153769	4665.492360	16.542746	-0.054990	3.694178
278.066159	4657.564016	16.547751	-0.054968	3.691093
278.014139	4649.542090	16.552755	-0.054953	3.687970
278.162494	4641.517297	16.557760	-0.054976	3.684848
278.199075	4633.570949	16.562765	-0.054977	3.681751
277.856154	4625.592575	16.567770	-0.054908	3.678629
278.243453	4617.585980	16.572775	-0.054975	3.675513
278.130379	4609.559912	16.577779	-0.054949	3.672373
277.715798	4601.591184	16.582784	-0.054867	3.669245
277.743062	4593.634598	16.587789	-0.054867	3.666131
277.587721	4585.633781	16.592794	-0.054833	3.662992
277.582020	4577.656492	16.597799	-0.054827	3.659863
277.212571	4569.637589	16.602803	-0.054753	3.656706
277.542705	4561.638572	16.607808	-0.054809	3.653572
277.876316	4553.581740	16.612813	-0.054866	3.650414
277.665083	4545.628928	16.617818	-0.054821	3.647278
277.692750	4537.617000	16.622823	-0.054821	3.644124
277.721020	4529.634918	16.627827	-0.054822	3.640978
278.012395	4521.646517	16.632832	-0.054871	3.637834
277.861580	4513.677522	16.637837	-0.054837	3.634683
277.967899	4505.656821	16.642842	-0.054852	3.631516
277.950440	4497.655911	16.647847	-0.054844	3.628351
277.815412	4489.652335	16.652851	-0.054813	3.625178
277.769551	4481.704518	16.657856	-0.054800	3.622028
277.730288	4473.675827	16.662861	-0.054787	3.618842
277.237277	4465.742203	16.667866	-0.054690	3.615679
277.227260	4457.748385	16.672871	-0.054683	3.612502
277.476735	4449.605337	16.677875	-0.054725	3.609271
277.687191	4441.629921	16.682880	-0.054759	3.606103
277.330431	4433.713230	16.687885	-0.054687	3.602939
277.346775	4425.725336	16.692890	-0.054685	3.599755
277.205842	4417.792081	16.697895	-0.054654	3.596585
276.905468	4409.753460	16.702899	-0.054593	3.593365
277.171956	4401.719959	16.707904	-0.054637	3.590161
277.414617	4393.712443	16.712909	-0.054677	3.586964
276.999252	4385.728284	16.717914	-0.054595	3.583754
277.486272	4377.711282	16.722919	-0.054680	3.580555
277.022208	4369.763157	16.727923	-0.054589	3.577352
277.286963	4361.745860	16.732928	-0.054633	3.574140
276.779504	4353.845828	16.737933	-0.054533	3.570950
276.927149	4345.746942	16.742938	-0.054555	3.567696
276.996698	4337.767464	16.747943	-0.054563	3.564485
276.790262	4329.843969	16.752947	-0.054520	3.561285
277.042739	4321.816194	16.757952	-0.054561	3.558055
276.566628	4313.882091	16.762957	-0.054468	3.554837
276.364867	4305.827857	16.767962	-0.054425	3.551575
276.645537	4297.791961	16.772967	-0.054472	3.548333
276.679608	4289.739078	16.777971	-0.054473	3.545074
276.687954	4281.835721	16.782976	-0.054470	3.541871
276.395467	4273.856582	16.787981	-0.054410	3.538626
276.530208	4265.821841	16.792986	-0.054430	3.535368
276.748830	4257.818655	16.797991	-0.054466	3.532123
276.723509	4249.773433	16.802995	-0.054456	3.528850
276.526421	4241.866367	16.808000	-0.054414	3.525624
276.662646	4233.863984	16.813005	-0.054434	3.522368
276.368634	4225.886609	16.818010	-0.054374	3.519105
276.243553	4217.937893	16.823015	-0.054346	3.515855
276.121755	4209.889416	16.828019	-0.054318	3.512563
276.334932	4201.870154	16.833024	-0.054353	3.509290
276.118929	4193.902935	16.838029	-0.054307	3.506021
275.918088	4185.900163	16.843034	-0.054265	3.502735
276.347311	4177.898992	16.848039	-0.054339	3.499467
276.252052	4169.910451	16.853043	-0.054317	3.496184
275.797428	4161.997681	16.858048	-0.054227	3.492918
275.325318	4154.035513	16.863053	-0.054134	3.489627
275.581875	4145.980093	16.868058	-0.054176	3.486319
275.854884	4137.932394	16.873063	-0.054222	3.483012
276.113564	4129.913800	16.878067	-0.054265	3.479713
276.060653	4121.959652	16.883072	-0.054250	3.476427
276.121568	4113.932090	16.888077	-0.054256	3.473111
276.001011	4105.978220	16.893082	-0.054229	3.469817
276.403315	4097.950918	16.898087	-0.054298	3.466507
276.046312	4089.969037	16.903091	-0.054227	3.463186
276.032351	4082.001492	16.908096	-0.054219	3.459880
276.102572	4074.017380	16.913101	-0.054227	3.456567
276.071535	4066.025953	16.918106	-0.054216	3.453245
275.411626	4058.126346	16.923111	-0.054088	3.449935
275.163063	4050.105471	16.928115	-0.054037	3.446586
275.241693	4042.069148	16.933120	-0.054046	3.443239
275.301259	4034.075094	16.938125	-0.054052	3.439905
275.304610	4026.094194	16.943130	-0.054048	3.436572
275.461480	4018.076883	16.948135	-0.054072	3.433225
275.465538	4010.051020	16.953139	-0.054067	3.429867
275.453238	4002.088026	16.958144	-0.054060	3.426531
275.231131	3994.105773	16.963149	-0.054013	3.423176
275.295861	3986.088714	16.968154	-0.054020	3.419813
275.485910	3978.127613	16.973159	-0.054050	3.416475
275.417932	3970.114416	16.978163	-0.054033	3.413103
275.456113	3962.122412	16.983168	-0.054035	3.409740
275.194586	3954.152640	16.988173	-0.053981	3.406372
275.658787	3946.068404	16.993178	-0.054062	3.402979
275.544948	3938.133742	16.998183	-0.054036	3.399624
275.666645	3930.158023	17.003187	-0.054053	3.396258
275.586220	3922.152909	17.008192	-0.054033	3.392868
275.478737	3914.146373	17.013197	-0.054008	3.389474
275.296378	3906.192640	17.018202	-0.053969	3.386095
274.789588	3898.273472	17.023207	-0.053869	3.382716
274.657746	3890.258026	17.028211	-0.053840	3.379307
274.950742	3882.218299	17.033216	-0.053889	3.375899
275.264454	3874.165694	17.038221	-0.053942	3.372483
275.260124	3866.156128	17.043226	-0.053936	3.369071
275.322437	3858.238129	17.048231	-0.053943	3.365696
275.007974	3850.265258	17.053235	-0.053879	3.362281
274.952071	3842.275050	17.058240	-0.053864	3.358864
274.856696	3834.319813	17.063245	-0.053841	3.355457
275.145514	3826.253614	17.068250	-0.053889	3.352014
274.795908	3818.306513	17.073255	-0.053819	3.348594
275.163771	3810.231519	17.078259	-0.053882	3.345143
275.337645	3802.295934	17.083264	-0.053910	3.341741
274.999368	3794.345634	17.088269	-0.053842	3.338310
275.007273	3786.328631	17.093274	-0.053838	3.334859
275.032218	3778.368375	17.098279	-0.053837	3.331430
274.819493	3770.347851	17.103283	-0.053793	3.327963
274.960800	3762.338033	17.108288	-0.053814	3.324510
274.756379	3754.437549	17.113293	-0.053771	3.321087
274.840224	3746.393159	17.118298	-0.053781	3.317610
275.126220	3738.407377	17.123303	-0.053829	3.314162
274.929013	3730.399316	17.128307	-0.053787	3.310682
274.777388	3722.429434	17.133312	-0.053754	3.307217
274.852452	3714.416524	17.138317	-0.053763	3.303739
274.921655	3706.401076	17.143322	-0.053770	3.300255
274.309900	3698.538550	17.148327	-0.053652	3.296808
274.362282	3690.471391	17.153331	-0.053656	3.293294
274.112216	3682.505586	17.158336	-0.053604	3.289808
274.252219	3674.486847	17.163341	-0.053625	3.286311
274.579205	3666.466525	17.168346	-0.053681	3.282817
274.707454	3658.497845	17.173351	-0.053700	3.279334
273.877591	3650.614628	17.178355	-0.053540	3.275846
273.941819	3642.591348	17.183360	-0.053547	3.272329
274.548208	3634.496562	17.188365	-0.053655	3.268799
274.122744	3626.583451	17.193370	-0.053570	3.265303
274.436457	3618.590363	17.198375	-0.053624	3.261798
273.997035	3610.622850	17.203379	-0.053537	3.258270
274.561978	3602.543418	17.208384	-0.053637	3.254730
274.526369	3594.563385	17.213389	-0.053625	3.251206
274.220628	3586.606087	17.218394	-0.053563	3.247676
274.343416	3578.603183	17.223399	-0.053581	3.244140
274.167302	3570.654025	17.228403	-0.053543	3.240611
274.321118	3562.640940	17.233408	-0.053566	3.237064
274.285752	3554.666418	17.238413	-0.053554	3.233523
274.011856	3546.682549	17.243418	-0.053498	3.229963
273.963610	3538.712829	17.248423	-0.053484	3.226415
273.826658	3530.682587	17.253427	-0.053454	3.222833
274.229757	3522.637811	17.258432	-0.053523	3.219263
273.918866	3514.744813	17.263437	-0.053460	3.215726
273.890984	3506.712752	17.268442	-0.053450	3.212136
274.031320	3498.711203	17.273447	-0.053471	3.208562
273.947078	3490.703877	17.278451	-0.053450	3.204972
273.918555	3482.750300	17.283456	-0.053440	3.201404
274.374656	3474.742128	17.288461	-0.053520	3.197829
274.139750	3466.771359	17.293466	-0.053471	3.194237
273.663495	3458.893412	17.298471	-0.053377	3.190672
273.308231	3450.878360	17.303475	-0.053306	3.187046
273.767021	3442.798214	17.308480	-0.053386	3.183423
273.739412	3434.830467	17.313485	-0.053376	3.179825
273.563012	3426.880772	17.318490	-0.053338	3.176224
274.092912	3418.813097	17.323495	-0.053431	3.172598
273.463068	3410.886764	17.328499	-0.053309	3.168979
273.448970	3402.891384	17.333504	-0.053301	3.165353
273.869204	3394.876142	17.338509	-0.053374	3.161732
273.664245	3386.912351	17.343514	-0.053331	3.158103
273.156551	3379.026836	17.348519	-0.053231	3.154492
273.019020	3371.020107	17.353523	-0.053200	3.150838
273.388372	3362.953950	17.358528	-0.053264	3.147176
273.397019	3354.941758	17.363533	-0.053260	3.143517
273.626630	3346.912777	17.368538	-0.053298	3.139857
273.533168	3339.009833	17.373543	-0.053276	3.136236
273.478475	3330.988264	17.378547	-0.053260	3.132557
273.586511	3322.955756	17.383552	-0.053275	3.128877
273.330191	3315.077924	17.388557	-0.053222	3.125247
272.978226	3307.130795	17.393562	-0.053152	3.121576
273.027738	3299.127645	17.398567	-0.053156	3.117893
273.261048	3291.067304	17.403571	-0.053194	3.114189
273.307075	3283.086774	17.408576	-0.053197	3.110508
273.297220	3275.099050	17.413581	-0.053190	3.106817
272.889880	3267.164577	17.418586	-0.053109	3.103127
273.237625	3259.126521	17.423591	-0.053169	3.099421
273.409196	3251.138074	17.428595	-0.053196	3.095725
272.924692	3243.221404	17.433600	-0.053101	3.092026
273.056506	3235.199685	17.438605	-0.053120	3.088304
272.621975	3227.257046	17.443610	-0.053034	3.084587
272.557132	3219.321044	17.448615	-0.053017	3.080886
272.943410	3211.231802	17.453619	-0.053083	3.077131
273.298708	3203.191505	17.458624	-0.053144	3.073393
272.848059	3195.258092	17.463629	-0.053055	3.069661
273.072220	3187.199402	17.468634	-0.053092	3.065899
273.039069	3179.235746	17.473639	-0.053081	3.062164
272.711558	3171.323043	17.478643	-0.053015	3.058434
272.609245	3163.336303	17.483648	-0.052990	3.054676
272.890012	3155.310214	17.488653	-0.053038	3.050913
272.801765	3147.331775	17.493658	-0.053016	3.047150
272.781843	3139.360717	17.498663	-0.053007	3.043389
272.450114	3131.418347	17.503667	-0.052940	3.039622
272.476273	3123.440479	17.508672	-0.052940	3.035851
272.197454	3115.486159	17.513677	-0.052883	3.032071
272.218104	3107.450432	17.518682	-0.052882	3.028263
272.522940	3099.433568	17.523687	-0.052933	3.024473
272.425106	3091.477088	17.528691	-0.052910	3.020687
272.405317	3083.490887	17.533696	-0.052901	3.016886
272.493869	3075.516353	17.538701	-0.052912	3.013091
272.418725	3067.484212	17.543706	-0.052893	3.009256
272.424892	3059.537296	17.548711	-0.052889	3.005460
272.294921	3051.563416	17.553715	-0.052860	3.001640
272.405861	3043.577239	17.558720	-0.052875	2.997822
271.834525	3035.693829	17.563725	-0.052764	2.994013
271.693431	3027.686819	17.568730	-0.052733	2.990161
272.177788	3019.637203	17.573735	-0.052818	2.986317
271.944888	3011.654895	17.578739	-0.052769	2.982463
271.700915	3003.699761	17.583744	-0.052719	2.978616
272.007833	2995.679293	17.588749	-0.052771	2.974762
272.189569	2987.630966	17.593754	-0.052799	2.970882
271.821725	2979.722348	17.598759	-0.052726	2.967037
272.213022	2971.666291	17.603763	-0.052793	2.963155
272.252846	2963.706461	17.608768	-0.052796	2.959295
272.215023	2955.797583	17.613773	-0.052783	2.955452
271.999139	2947.788895	17.618778	-0.052738	2.951545
272.297188	2939.794872	17.623783	-0.052788	2.947668
271.899925	2931.848449	17.628787	-0.052709	2.943772
271.904108	2923.876954	17.633792	-0.052705	2.939880
272.074773	2915.892584	17.638797	-0.052732	2.935985
271.633503	2907.951781	17.643802	-0.052644	2.932073
271.483521	2899.961635	17.648807	-0.052611	2.928148
271.390256	2891.949951	17.653811	-0.052589	2.924210
271.448190	2883.988201	17.658816	-0.052594	2.920299
271.131689	2876.073591	17.663821	-0.052530	2.916386
270.621591	2868.081806	17.668826	-0.052430	2.912419
270.788696	2860.014348	17.673831	-0.052456	2.908446
270.934312	2852.001252	17.678835	-0.052478	2.904494
270.850416	2844.044819	17.683840	-0.052457	2.900552
270.977042	2836.037898	17.688845	-0.052476	2.896590
270.528926	2828.114520	17.693850	-0.052387	2.892633
270.796792	2820.069022	17.698855	-0.052432	2.888650
270.724505	2812.096595	17.703859	-0.052413	2.884678
271.045569	2804.121502	17.708864	-0.052468	2.880722
270.947112	2796.193331	17.713869	-0.052445	2.876760
270.708057	2788.202765	17.718874	-0.052395	2.872754
270.815489	2780.208515	17.723879	-0.052410	2.868760
270.679395	2772.224975	17.728883	-0.052379	2.864751
270.412125	2764.331639	17.733888	-0.052325	2.860775
270.845227	2756.255392	17.738893	-0.052400	2.856741
270.977144	2748.226546	17.743898	-0.052419	2.852709
270.439840	2740.350490	17.748903	-0.052314	2.848709
270.459676	2732.337912	17.753907	-0.052313	2.844666
270.724039	2724.342617	17.758912	-0.052357	2.840641
270.497165	2716.427280	17.763917	-0.052310	2.836622
270.350024	2708.434082	17.768922	-0.052277	2.832563
269.911442	2700.518600	17.773927	-0.052190	2.828520
269.992785	2692.477912	17.778931	-0.052200	2.824438
270.250716	2684.456569	17.783936	-0.052243	2.820370
270.387412	2676.461926	17.788941	-0.052263	2.816303
270.661228	2668.453063	17.793946	-0.052309	2.812231
270.057061	2660.593106	17.798951	-0.052192	2.808177
269.972791	2652.578872	17.803955	-0.052171	2.804069
270.191630	2644.588537	17.808960	-0.052206	2.799986
270.294418	2636.618433	17.813965	-0.052220	2.795899
270.080949	2628.653246	17.818970	-0.052176	2.791791
270.289905	2620.649784	17.823975	-0.052209	2.787682
270.332899	2612.652687	17.828979	-0.052212	2.783560
270.378691	2604.671912	17.833984	-0.052216	2.779441
270.232267	2596.743073	17.838989	-0.052183	2.775331
270.236785	2588.743210	17.843994	-0.052179	2.771187
270.529512	2580.742898	17.848999	-0.052228	2.767055
270.478400	2572.775857	17.854003	-0.052214	2.762912
270.463139	2564.835726	17.859008	-0.052206	2.758779
270.414700	2556.891086	17.864013	-0.052191	2.754636
270.213195	2548.868443	17.869018	-0.052149	2.750437
270.269395	2540.893112	17.874023	-0.052154	2.746271
270.389655	2532.878702	17.879027	-0.052171	2.742083
270.421771	2524.913181	17.884032	-0.052172	2.737909
270.143663	2516.995144	17.889037	-0.052115	2.733733
269.896217	2509.044161	17.894042	-0.052064	2.729536
269.748785	2501.096496	17.899047	-0.052032	2.725340
269.583478	2493.143788	17.904051	-0.051996	2.721134
269.179907	2485.218005	17.909056	-0.051915	2.716921
269.716016	2477.135345	17.914061	-0.052010	2.712678
269.404627	2469.167459	17.919066	-0.051947	2.708435
269.763861	2461.132809	17.924071	-0.052009	2.704193
269.676097	2453.203484	17.929075	-0.051987	2.699971
269.648171	2445.244192	17.934080	-0.051977	2.695731
269.724998	2437.243752	17.939085	-0.051986	2.691468
269.295570	2429.317618	17.944090	-0.051901	2.687206
269.564535	2421.332490	17.949095	-0.051946	2.682951
269.718765	2413.320924	17.954099	-0.051970	2.678668
269.541517	2405.381254	17.959104	-0.051931	2.674395
269.532608	2397.422710	17.964109	-0.051925	2.670115
269.244999	2389.442214	17.969114	-0.051866	2.665799
269.196849	2381.489890	17.974119	-0.051852	2.661506
269.021991	2373.511174	17.979123	-0.051814	2.657184
268.941958	2365.551133	17.984128	-0.051794	2.652871
269.010251	2357.548917	17.989133	-0.051802	2.648539
269.108281	2349.531077	17.994138	-0.051815	2.644192
269.176964	2341.604569	17.999143	-0.051822	2.639887
268.621023	2333.723822	18.004147	-0.051714	2.635557
268.549723	2325.731196	18.009152	-0.051695	2.631191
268.708412	2317.718095	18.014157	-0.051720	2.626823
268.631780	2309.744725	18.019162	-0.051700	2.622453
268.575326	2301.784442	18.024167	-0.051685	2.618084
268.577187	2293.795249	18.029171	-0.051680	2.613697
268.494392	2285.845951	18.034176	-0.051660	2.609317
269.050885	2277.770379	18.039181	-0.051758	2.604906
268.732538	2269.881963	18.044186	-0.051694	2.600529
268.955495	2261.912641	18.049191	-0.051730	2.596138
269.093477	2253.842634	18.054195	-0.051750	2.591678
268.887746	2245.859626	18.059200	-0.051707	2.587234
269.138399	2237.866975	18.064205	-0.051749	2.582809
268.552515	2230.030509	18.069210	-0.051634	2.578405
268.736681	2222.029004	18.074215	-0.051664	2.573956
268.908413	2214.024373	18.079219	-0.051690	2.569496
268.939193	2206.058429	18.084224	-0.051691	2.565040
269.080617	2198.112793	18.089229	-0.051712	2.560596
268.916385	2190.174597	18.094234	-0.051677	2.556126
268.828952	2182.248051	18.099239	-0.051655	2.551660
268.800090	2174.264003	18.104243	-0.051645	2.547159
268.575858	2166.320231	18.109248	-0.051598	2.542658
268.727053	2158.337219	18.114253	-0.051621	2.538154
268.401488	2150.422695	18.119258	-0.051555	2.533646
268.379649	2142.438002	18.124263	-0.051546	2.529112
268.110107	2134.512743	18.129267	-0.051491	2.524586
268.674624	2126.427605	18.134272	-0.051590	2.520022
268.488042	2118.542729	18.139277	-0.051551	2.515509
268.142332	2110.590152	18.144282	-0.051481	2.510937
268.194319	2102.598496	18.149287	-0.051486	2.506364
267.942162	2094.653563	18.154291	-0.051434	2.501786
267.966420	2086.665109	18.159296	-0.051433	2.497196
267.510849	2078.805570	18.164301	-0.051343	2.492635
267.725402	2070.729978	18.169306	-0.051378	2.487992
268.061995	2062.726755	18.174311	-0.051435	2.483391
267.912881	2054.810603	18.179315	-0.051403	2.478796
268.016736	2046.827676	18.184320	-0.051417	2.474172
267.965373	2038.895266	18.189325	-0.051402	2.469557
267.456145	2030.976574	18.194330	-0.051302	2.464907
267.749955	2022.981318	18.199335	-0.051352	2.460264
268.011930	2014.964605	18.204339	-0.051395	2.455598
268.061389	2007.006459	18.209344	-0.051399	2.450941
267.852859	1999.089806	18.214349	-0.051356	2.446279
267.835114	1991.125703	18.219354	-0.051347	2.441596
267.709501	1983.216869	18.224359	-0.051319	2.436927
268.009138	1975.165847	18.229363	-0.051369	2.432199
267.741184	1967.221064	18.234368	-0.051314	2.427480
268.331520	1959.154677	18.239373	-0.051419	2.422748
267.685963	1951.323939	18.244378	-0.051294	2.418048
267.889444	1943.335118	18.249383	-0.051326	2.413312
267.911008	1935.360267	18.254387	-0.051325	2.408561
267.856606	1927.405298	18.259392	-0.051310	2.403807
267.971942	1919.473035	18.264397	-0.051326	2.399070
267.671663	1911.564328	18.269402	-0.051265	2.394304
268.006597	1903.578565	18.274407	-0.051323	2.389534
267.847436	1895.606433	18.279411	-0.051288	2.384722
267.679710	1887.693267	18.284416	-0.051252	2.379936
267.695898	1879.734888	18.289421	-0.051249	2.375128
267.817122	1871.722256	18.294426	-0.051267	2.370285
267.431566	1863.844171	18.299431	-0.051190	2.365473
267.570116	1855.866110	18.304435	-0.051211	2.360633
267.389045	1847.941084	18.309440	-0.051172	2.355790
267.484309	1839.964983	18.314445	-0.051184	2.350928
267.100327	1832.033911	18.319450	-0.051108	2.346043
266.864314	1824.117469	18.324455	-0.051059	2.341170
266.895117	1816.115207	18.329459	-0.051059	2.336256
267.023013	1808.127353	18.334464	-0.051078	2.331348
267.457214	1800.103882	18.339469	-0.051154	2.326435
266.861694	1792.251228	18.344474	-0.051038	2.321529
266.823640	1784.326119	18.349479	-0.051026	2.316615
266.979935	1776.353173	18.354483	-0.051050	2.311678
266.740778	1768.406781	18.359488	-0.051000	2.306713
266.619788	1760.486847	18.364493	-0.050972	2.301763
266.406998	1752.544806	18.369498	-0.050928	2.296781
266.741410	1744.521003	18.374503	-0.050985	2.291785
266.689962	1736.567925	18.379507	-0.050970	2.286789
266.150954	1728.721968	18.384512	-0.050865	2.281806
266.560049	1720.708088	18.389517	-0.050936	2.276790
266.448193	1712.731005	18.394522	-0.050910	2.271740
266.457792	1704.754061	18.399527	-0.050906	2.266689
266.581683	1696.780155	18.404531	-0.050924	2.261639
266.144539	1688.918037	18.409536	-0.050838	2.256600
266.210168	1680.958177	18.414541	-0.050845	2.251531
265.860396	1673.020939	18.419546	-0.050775	2.246428
266.069081	1665.042360	18.424551	-0.050808	2.241338
265.802926	1657.145059	18.429555	-0.050754	2.236245
265.857276	1649.174294	18.434560	-0.050759	2.231122
266.052993	1641.180830	18.439565	-0.050790	2.225985
265.622816	1633.304089	18.444570	-0.050705	2.220855
266.127371	1625.254825	18.449575	-0.050794	2.215687
266.774815	1617.219361	18.454579	-0.050909	2.210529
266.416397	1609.357347	18.459584	-0.050837	2.205379
265.808192	1601.558448	18.464589	-0.050719	2.200236
265.773764	1593.600140	18.469594	-0.050707	2.195029
266.114853	1585.584958	18.474599	-0.050766	2.189807
265.831262	1577.669286	18.479603	-0.050708	2.184580
266.197014	1569.658605	18.484608	-0.050771	2.179338
266.055934	1561.782268	18.489613	-0.050740	2.174125
265.866587	1553.834034	18.494618	-0.050699	2.168848
265.779896	1545.919946	18.499623	-0.050678	2.163589
265.801324	1537.984087	18.504627	-0.050677	2.158314
265.884292	1530.017830	18.509632	-0.050687	2.153012
265.812106	1522.106489	18.514637	-0.050669	2.147718
265.585966	1514.191001	18.519642	-0.050621	2.142393
265.732943	1506.238309	18.524647	-0.050644	2.137066
265.826730	1498.272470	18.529651	-0.050656	2.131712
265.851757	1490.318706	18.534656	-0.050655	2.126346
265.773513	1482.424117	18.539661	-0.050636	2.120997
265.715226	1474.508672	18.544666	-0.050620	2.115621
265.520982	1466.567078	18.549671	-0.050579	2.110201
265.812033	1458.544185	18.554675	-0.050628	2.104759
265.998302	1450.593071	18.559680	-0.050657	2.099342
265.826488	1442.717664	18.564685	-0.050620	2.093927
265.565642	1434.815379	18.569690	-0.050567	2.088470
265.491832	1426.881489	18.574695	-0.050548	2.082997
265.499678	1418.978436	18.579699	-0.050544	2.077538
265.178415	1411.084673	18.584704	-0.050479	2.072038
265.712842	1403.041057	18.589709	-0.050573	2.066506
265.511692	1395.149150	18.594714	-0.050531	2.060990
265.745377	1387.191355	18.599719	-0.050569	2.055458
265.903584	1379.240950	18.604723	-0.050594	2.049908
265.550044	1371.377363	18.609728	-0.050523	2.044352
265.587823	1363.485183	18.614733	-0.050525	2.038800
265.240272	1355.594530	18.619738	-0.050455	2.033194
265.373413	1347.627670	18.624743	-0.050475	2.027570
265.304448	1339.701748	18.629747	-0.050457	2.021937
265.350460	1331.755479	18.634752	-0.050460	2.016286
265.182014	1323.868519	18.639757	-0.050424	2.010639
265.185814	1315.908951	18.644762	-0.050419	2.004942
265.358266	1307.983124	18.649767	-0.050446	1.999272
265.221310	1300.103667	18.654771	-0.050416	1.993585
265.170890	1292.163894	18.659776	-0.050401	1.987848
265.036526	1284.277474	18.664781	-0.050371	1.982124
264.867978	1276.367296	18.669786	-0.050335	1.976362
265.321797	1268.375026	18.674791	-0.050414	1.970591
265.340582	1260.460592	18.679795	-0.050412	1.964813
264.899372	1252.637239	18.684800	-0.050325	1.959034
264.943925	1244.710966	18.689805	-0.050328	1.953216
264.586040	1236.838620	18.694810	-0.050257	1.947375
264.304559	1228.948689	18.699815	-0.050199	1.941512
264.715388	1220.926093	18.704819	-0.050271	1.935611
264.415738	1213.039845	18.709824	-0.050210	1.929713
264.104507	1205.176755	18.714829	-0.050147	1.923813
263.930367	1197.277444	18.719834	-0.050109	1.917883
264.125513	1189.327309	18.724839	-0.050140	1.911938
263.870660	1181.434070	18.729843	-0.050088	1.905967
263.808795	1173.523175	18.734848	-0.050071	1.899985
263.403497	1165.679047	18.739853	-0.049991	1.893995
264.100608	1157.600405	18.744858	-0.050115	1.887936
264.047113	1149.715466	18.749863	-0.050100	1.881918
264.281953	1141.786803	18.754867	-0.050139	1.875881
264.224175	1133.898172	18.759872	-0.050123	1.869821
264.343301	1125.983309	18.764877	-0.050140	1.863741
264.126308	1118.111626	18.769882	-0.050095	1.857636
264.081270	1110.235925	18.774887	-0.050081	1.851527
264.459331	1102.241329	18.779891	-0.050146	1.845357
264.304284	1094.388598	18.784896	-0.050113	1.839212
264.336709	1086.521736	18.789901	-0.050114	1.833058
264.223540	1078.627713	18.794906	-0.050087	1.826845
263.921245	1070.793811	18.799911	-0.050026	1.820635
263.717046	1062.934433	18.804915	-0.049983	1.814395
263.791957	1054.994939	18.809920	-0.049992	1.808104
263.842683	1047.101589	18.814925	-0.049996	1.801825
263.358821	1039.286178	18.819930	-0.049901	1.795520
263.273206	1031.378934	18.824935	-0.049880	1.789169
263.250581	1023.461715	18.829939	-0.049871	1.782795
263.101621	1015.576477	18.834944	-0.049838	1.776408
263.313305	1007.647022	18.839949	-0.049872	1.770008
263.314797	999.740558	18.844954	-0.049867	1.763576
263.460325	991.842432	18.849959	-0.049889	1.757147
262.759443	984.099810	18.854963	-0.049754	1.750712
262.921614	976.154585	18.859968	-0.049779	1.744198
263.153266	968.246219	18.864973	-0.049817	1.737699
262.586505	960.462876	18.869978	-0.049707	1.731176
262.592489	952.552844	18.874983	-0.049703	1.724597
262.878922	944.629452	18.879987	-0.049751	1.718019
262.680702	936.776162	18.884992	-0.049709	1.711410
262.726815	928.883244	18.889997	-0.049712	1.704775
262.758758	921.004383	18.895002	-0.049713	1.698123
262.383089	913.198113	18.900007	-0.049638	1.691453
262.306343	905.316977	18.905011	-0.049619	1.684732
262.379526	897.444582	18.910016	-0.049627	1.678012
262.492035	889.563933	18.915021	-0.049643	1.671264
262.661072	881.633083	18.920026	-0.049670	1.664453
262.969212	873.742888	18.925031	-0.049722	1.657668
263.035147	865.890281	18.930035	-0.049729	1.650855
262.704867	858.095062	18.935040	-0.049663	1.644008
262.463773	850.305702	18.940045	-0.049613	1.637150
262.208366	842.443632	18.945050	-0.049560	1.630197
262.358004	834.538714	18.950055	-0.049583	1.623234
262.314523	826.689538	18.955059	-0.049570	1.616262
262.393268	818.814881	18.960064	-0.049579	1.609256
262.716271	810.929656	18.965069	-0.049634	1.602244
262.338814	803.155175	18.970074	-0.049559	1.595200
262.129848	795.363181	18.975079	-0.049515	1.588133
262.593809	787.414750	18.980083	-0.049597	1.580991
262.380702	779.623083	18.985088	-0.049552	1.573860
262.263377	771.816158	18.990093	-0.049525	1.566697
262.165249	763.996146	18.995098	-0.049502	1.559491
262.405368	756.131121	19.000103	-0.049541	1.552262
262.228633	748.314558	19.005107	-0.049503	1.544980
262.248653	740.481250	19.010112	-0.049502	1.537678
262.325237	732.647574	19.015117	-0.049511	1.530350
262.008333	724.870727	19.020122	-0.049447	1.522980
262.153315	717.031239	19.025127	-0.049469	1.515585
262.471114	709.158105	19.030131	-0.049523	1.508150
261.882925	701.441540	19.035136	-0.049409	1.500685
262.217123	693.583885	19.040141	-0.049466	1.493193
262.075824	685.777785	19.045146	-0.049435	1.485637
261.688619	678.071251	19.050151	-0.049358	1.478101
261.212066	670.308244	19.055155	-0.049264	1.470456
261.418272	662.424353	19.060160	-0.049297	1.462762
261.625583	654.591347	19.065165	-0.049331	1.455079
261.392320	646.817298	19.070170	-0.049282	1.447340
260.940925	639.112104	19.075175	-0.049193	1.439594
261.127965	631.277395	19.080179	-0.049223	1.431780
261.118782	623.464367	19.085184	-0.049216	1.423914
261.088212	615.683802	19.090189	-0.049206	1.416032
261.207823	607.862537	19.095194	-0.049223	1.408091
261.597980	600.034872	19.100199	-0.049291	1.400144
261.284826	592.339182	19.105203	-0.049227	1.392168
261.067963	584.580470	19.110208	-0.049182	1.384096
261.363474	576.772848	19.115213	-0.049232	1.376015
261.423543	568.986836	19.120218	-0.049238	1.367868
261.275158	561.266583	19.125223	-0.049206	1.359705
261.105228	553.556727	19.130227	-0.049169	1.351500
260.792854	545.847891	19.135232	-0.049106	1.343220
260.927992	538.081389	19.140237	-0.049126	1.334907
260.878360	530.335131	19.145242	-0.049112	1.326531
260.971882	522.602514	19.150247	-0.049124	1.318142
260.847885	514.830583	19.155251	-0.049096	1.309617
260.458334	507.128247	19.160256	-0.049019	1.301063
260.404277	499.426275	19.165261	-0.049004	1.292515
260.387399	491.693529	19.170266	-0.048995	1.283883
260.196507	484.022001	19.175271	-0.048955	1.275229
259.932891	476.349895	19.180275	-0.048901	1.266501
259.621696	468.700634	19.185280	-0.048838	1.257729
259.897721	460.936390	19.190285	-0.048885	1.248877
259.950717	453.210385	19.195290	-0.048889	1.239963
259.898723	445.547780	19.200295	-0.048875	1.231037
259.951575	437.840462	19.205299	-0.048880	1.222015
259.494784	430.247231	19.210304	-0.048790	1.212958
259.634826	422.546709	19.215309	-0.048811	1.203825
259.899888	414.838022	19.220314	-0.048855	1.194639
259.902096	407.183771	19.225319	-0.048851	1.185394
259.457829	399.635143	19.230323	-0.048763	1.176111
259.684411	391.932667	19.235328	-0.048800	1.166707
259.448192	384.366875	19.240333	-0.048752	1.157297
259.265342	376.740637	19.245338	-0.048713	1.147746
258.923012	369.177063	19.250343	-0.048644	1.138159
258.737212	361.585166	19.255347	-0.048605	1.128489
258.746910	353.961786	19.260352	-0.048601	1.118738
258.637843	346.400257	19.265357	-0.048576	1.108954
258.418154	338.834850	19.270362	-0.048530	1.099054
258.352039	331.262142	19.275367	-0.048513	1.089089
258.403945	323.682856	19.280371	-0.048518	1.079050
258.220639	316.149271	19.285376	-0.048479	1.068924
258.261480	308.594955	19.290381	-0.048482	1.058725
258.172681	301.058885	19.295386	-0.048460	1.048421
257.994232	293.574722	19.300391	-0.048422	1.038065
258.385879	285.987580	19.305395	-0.048490	1.027599
258.179681	278.527339	19.310400	-0.048447	1.017059
258.195324	271.046476	19.315405	-0.048445	1.006433
258.086866	263.595432	19.320410	-0.048420	0.995706
257.880513	256.149791	19.325415	-0.048377	0.984845
257.908310	248.692018	19.330419	-0.048378	0.973905
257.786559	241.273727	19.335424	-0.048350	0.962860
257.627634	233.900175	19.340429	-0.048316	0.951745
257.327184	226.542215	19.345434	-0.048255	0.940485
257.556949	219.112711	19.350439	-0.048293	0.929121
257.344972	211.791858	19.355443	-0.048249	0.917666
257.010883	204.493542	19.360448	-0.048182	0.906067
257.167307	197.127499	19.365453	-0.048206	0.894347
256.709015	189.888492	19.370458	-0.048116	0.882503
256.448056	182.654443	19.375463	-0.048063	0.870562
256.262582	175.403770	19.380467	-0.048024	0.858450
255.974986	168.190446	19.385472	-0.047966	0.846197
255.732272	161.005914	19.390477	-0.047916	0.833827
255.115058	153.879706	19.395482	-0.047797	0.821257
254.552792	146.788312	19.400487	-0.047687	0.808571
254.387226	139.650308	19.405491	-0.047652	0.795724
253.492106	132.657354	19.410496	-0.047481	0.782695
253.249409	125.587669	19.415501	-0.047431	0.769519
252.503640	118.633721	19.420506	-0.047288	0.756162
251.629224	111.728213	19.425511	-0.047120	0.742614
251.130220	104.780905	19.430515	-0.047023	0.728864
250.681289	97.868674	19.435520	-0.046935	0.714937
250.036534	91.036482	19.440525	-0.046811	0.700825
249.120454	84.283119	19.445530	-0.046636	0.686487
248.636239	77.668807	19.450535	-0.046541	0.672304